Polypropylene-based resin composition, polypropylene-based non-stretched film, packaging material, and package
A polypropylene resin composition with controlled luminescence and molecular weight addresses odor issues in packaging materials by minimizing resin deterioration, achieving reduced odor and improved heat seal strength and impact resistance.
Patent Information
- Application Number
- JP2024146426
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2024-08-28
- Publication Date
- 2024-11-21
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing polypropylene-based packaging materials emit odors during retort processing due to decomposition of polypropylene and antioxidants, and existing odor suppression methods are costly and impractical.
A polypropylene resin composition comprising 60 to 70 parts by weight of a propylene homopolymer and 30 to 40 parts by weight of an ethylene propylene random copolymer, with controlled luminescence and molecular weight to minimize resin deterioration and odor, ensuring excellent heat seal strength and impact resistance.
The resin composition results in a polypropylene unstretched film with reduced odor emission, enhanced heat seal strength, and improved impact resistance, suitable for packaging materials and packages.
Smart Images

Figure 2024163131000001 
Figure 2024163131000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a polypropylene-based resin composition having low odor, heat seal strength and impact resistance by controlling the degree of degradation and molecular weight of polypropylene, and also to a polypropylene-based non-oriented film, packaging material and package using the polypropylene-based resin composition. [Background technology]
[0002] Polypropylene resins, which are thermoplastic resins, have excellent properties such as rigidity and heat resistance, and are therefore widely used in the packaging field, including food packaging, textile packaging, pharmaceutical packaging, etc. For packaging materials for retort foods, which can be heated and sterilized after filling to extend the expiration date, polypropylene non-oriented films are often used because of their excellent heat resistance.
[0003] Retort foods can emit a unique odor. This odor occurs when the food is heated for a long period of time during retort processing, which causes odorous components to be released from both the contents and the packaging material. Methods proposed to suppress odors include kneading an adsorbent into the film (Patent Document 1), mixing an adsorbent into the print layer (Patent Document 2), and mixing an adsorbent into the adhesive layer (Patent Document 3). These methods are capable of adsorbing odors originating from the contents and the packaging material, but are difficult to put into practical use due to the high cost of the adsorbent.
[0004] The odors from packaging materials are caused by low molecular weight components that are generated by the decomposition of polypropylene due to heat and shear during processing of the packaging material, and phenols that are generated by the decomposition of antioxidants used as additives, which are transferred from the film to the contents during retort processing. In order to suppress odors from packaging materials, it is preferable to perform molding processing while suppressing the decomposition of polypropylene and antioxidants. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2019-177521 A [Patent Document 2] JP 2019-182536 A [Patent Document 3] JP 2017-94533 A Summary of the Invention [Problem to be solved by the invention]
[0006] The present invention has been made in consideration of the above problems, and aims to provide a polypropylene-based non-oriented film that has little odor derived from the packaging material during retort treatment and is excellent in heat seal strength and impact resistance, a packaging material using said film, and a package using said packaging material. Another aim of the present invention is to provide a polypropylene-based resin composition for providing said polypropylene-based non-oriented film. [Means for solving the problem]
[0007] One aspect of the present invention for solving the above problems is a polypropylene-based resin composition comprising 60 to 70 parts by weight of a propylene homopolymer and 30 to 40 parts by weight of an ethylene-propylene random copolymer, the composition having an amount of luminescence measured by a chemiluminescence method of 300,000 or less and a weight average molecular weight of 600,000 or more and 700,000 or less. Effect of the Invention
[0008] According to the present invention, it is possible to provide a polypropylene-based non-oriented film that has little odor derived from the packaging material during retort treatment and is excellent in heat seal strength and impact resistance, a packaging material using the film, and a package using the packaging material. It is also possible to provide a polypropylene-based resin composition for providing the polypropylene-based non-oriented film. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] The polypropylene resin composition of the present invention will be described in detail below.
[0010] [Resin composition characteristics] The polypropylene resin composition of the present invention must satisfy the following properties (a) to (c). (a) It consists of 60 to 70 parts by weight of a propylene homopolymer and 30 to 40 parts by weight of an ethylene propylene random copolymer. (b) The luminescence intensity measured by chemiluminescence is 300,000 or less. (c) The weight average molecular weight (Mw) measured by gel permeation chromatography (GPC) is 600,000 or more and 700,000 or less.
[0011] [Luminescence measurement using chemiluminescence method] A chemiluminescence analyzer (CLA) is used to measure the amount of luminescence by the chemiluminescence method. The CLA is a device used to measure chemiluminescence described in JIS K7351, and can detect weak chemiluminescence emitted when the electrons of a carbonyl group change from an excited state to a ground state, and can evaluate the deterioration of the resin. In the case of propylene homopolymers and ethylene-propylene random copolymers, resin deterioration progresses due to shearing during molding processing, and carbonyl groups are generated, and chemiluminescence is confirmed by the CLA. If the amount of luminescence measured by the CLA is small, it indicates that the heat and shear stress applied to the resin during molding processing is small, and resin deterioration is small. It can also be seen that the decomposition of the antioxidant is suppressed. Therefore, if a polypropylene-based resin composition with a small amount of CLA luminescence is used, the generation of low-molecular-weight components and the decomposition of the antioxidant are suppressed, and a polypropylene-based non-oriented film with excellent low odor can be obtained. It is desirable that the amount of CLA luminescence is 300,000 or less. The polypropylene-based non-oriented film will be described later.
[0012] [Weight average molecular weight] The weight average molecular weight is a value that depends on the degree of polymerization of the monomer, and a larger value indicates that more monomers are polymerized. It is known that the weight average molecular weight affects the resin viscosity, rigidity, and heat resistance. If the weight average molecular weight of a polypropylene resin composition is 600,000 or less, the rigidity and heat resistance are low, and the impact resistance and heat seal strength after retort are reduced. If the weight average molecular weight is 700,000 or more, the resin viscosity is high, which increases the load on the resin molding machine and deteriorates the molding processability.
[0013] [Propylene homopolymer] Propylene homopolymer is a polymer polymerized using propylene as a raw material. The polymerization method of the propylene homopolymer used in the present invention is not particularly limited, and a polymerized product polymerized by a known method may be used. The polymerization catalyst may be a Ziegler-Natta catalyst, a metallocene catalyst, or other catalyst. The raw material propylene may be polymerized in a state dissolved in a solvent, in a liquid state, or in a gaseous state. The propylene homopolymer used in the present invention may be one type alone or two or more types may be mixed and used.
[0014] [Ethylene propylene random copolymer] Ethylene propylene random copolymer is polymerized using ethylene and propylene as raw materials. The ethylene propylene random copolymer is a polymer obtained by polymerization of ethylene and propylene structures with no regularity in the arrangement thereof. The polymerization method for the ethylene propylene random copolymer used in the present invention is not particularly limited, and a copolymer obtained by polymerization using a known method may be used. The polymerization catalyst may be a Ziegler-Natta catalyst, a metallocene catalyst, or other catalyst. The raw materials ethylene and propylene may be polymerized in a state dissolved in a solvent, in a liquid state, or in a gaseous state. The ethylene propylene random copolymer used in the present invention is not particularly limited in terms of the ratio of ethylene structures to propylene structures. In addition, the ethylene propylene random copolymer may be used alone or in a mixture of two or more types.
[0015] In order to improve the processability when molding a polypropylene-based non-oriented film and the suitability when using the film, known additives such as antioxidants, antistatic agents, neutralizing agents, nucleating agents, antiblocking agents, slip agents, etc. can be added to the ethylene propylene random copolymer as necessary within a range that does not impair the effects of the present invention.
[0016] The method of mixing the propylene homopolymer and the ethylene-propylene random copolymer of the present invention is not particularly limited, and known methods can be used. For example, a method of mixing in a pellet state called dry blending, or a method of mixing by melt kneading and granulating using a general mixer such as a single screw extruder, a twin screw extruder, or a multi-screw extruder, can be used. When considering workability, the method of using dry blending or a twin screw extruder is particularly preferred.
[0017] The type of twin screw extruder is not particularly limited, and may be a co-rotating twin screw extruder or a counter-rotating twin screw extruder. The screw shape is not particularly limited, and may be a full flight screw or a kneading disk type. A known method for removing low molecular weight components from the extruder may also be used. For example, a method of devolatilization using a vent cylinder or a method of adding water or a supercritical fluid may be used. These methods may be used in combination.
[0018] Next, the polypropylene-based non-oriented film will be described. The thickness of the polypropylene-based non-oriented film is not particularly limited as long as it is within the range that can be used as a packaging film, but if the thickness is too thick, it will be a cost disadvantage. Therefore, it is preferable that the thickness is in the range of 100 μm or less.
[0019] The method for thermoforming the polypropylene-based non-oriented film of the present invention is not particularly limited, and known methods can be used. For example, a melt-kneading method using a general mixer such as a single-screw extruder, a twin-screw extruder, or a multi-screw extruder, or a method in which each component is dissolved or dispersed and mixed, and then the solvent is removed by heating, can be used. In consideration of workability, it is particularly preferable to use a single-screw extruder or a twin-screw extruder. When a single-screw extruder is used, a full-flight screw, a screw with a mixing element, a barrier flight screw, a fluted screw, etc. can be used without any particular limitation. The twin-screw kneading device is not particularly limited to a co-rotating twin-screw extruder or a counter-rotating twin-screw extruder, and the screw shape is not particularly limited to a full-flight screw or a kneading disk type.
[0020] In the above method, a polypropylene-based non-oriented film can be produced by melting the polypropylene in a single-screw extruder or twin-screw extruder or the like, and then passing the melt through a feed block or a multi-manifold to form a film using a T-die.
[0021] Furthermore, the polypropylene-based non-oriented film of the present invention can be subjected to a surface modification treatment to appropriately improve suitability for post-processing, if necessary. For example, the printing property when the film is used alone can be improved. In order to improve printability and lamination suitability during lamination, it is possible to perform a surface modification treatment on the surface that comes into contact with other substrates. As the surface modification treatment, a method of expressing functional groups by oxidizing the film surface, such as corona discharge treatment, plasma treatment, and flame treatment, or a method of modifying the surface by a wet process, such as coating an easy-adhesion layer, can be suitably used.
[0022] The polypropylene-based non-oriented film may be used alone or may be laminated with other substrates to be used as a packaging material. Specifically, at least one substrate selected from biaxially oriented polyamide film (ONy), biaxially oriented polyester film (PET), printed paper, and metal foil (AL foil) is laminated on the polypropylene-based non-oriented film of the present invention to form a packaging material. Representative configurations of these are PET / AL foil / polypropylene-based non-oriented film, PET / ONy / AL foil / polypropylene-based non-oriented film, PET / AL foil / ONy / polypropylene-based non-oriented film, and ONy / polypropylene-based non-oriented film. The manufacturing method of the packaging material can be suitably adopted as a normal dry lamination method in which a substrate is bonded to the polypropylene-based non-oriented film using an adhesive, but a method of directly extrusion laminating the polypropylene-based non-oriented film can also be adopted as necessary.
[0023] The laminate structure of these packaging materials must be selected appropriately based on the required characteristics of the packaging material, such as barrier properties that meet the shelf life of the packaged food, size and impact resistance to accommodate the weight of the contents, visibility of the contents, etc.
[0024] These packaging materials can be used to make packages such as flat bags, three-sided bags, palm-shaped bags, gusseted bags, standing pouches, pouches with spouts, and pouches with beaks, with a polypropylene-based non-oriented film as a sealing material, and the bag making style is not particularly limited.
[0025] As described above, by using the polypropylene-based resin composition according to this embodiment, the amount of chemiluminescence measured by CLA can be suppressed, and by mixing and forming a film of the resin composition so as to have an appropriate molecular weight distribution, it is possible to produce polypropylene-based non-oriented films, packaging materials, and packages that suppress the odor specific to retort and have excellent heat seal strength and impact resistance. EXAMPLES
[0026] Examples of the present invention will be described in detail below, but the present invention is not limited to only the following examples.
[0027] Two types of propylene homopolymers were prepared. As propylene homopolymer A, a commercially available propylene homopolymer having MFR (230°C, 2.16kg) = 3.0g / 10min and Mw = 596,000 measured by a method conforming to ISO1133 was used. As propylene homopolymer B, a commercially available propylene homopolymer having MFR (230°C, 2.16kg) = 0.5g / 10min and Mw = 987,000 was used. Two types of ethylene propylene random copolymers were prepared. As ethylene propylene random copolymer A, a commercially available ethylene propylene random copolymer having MFR (230°C, 2.16kg) = 0.6g / 10min and Mw = 765,000 was used. As the ethylene propylene random copolymer B, a commercially available ethylene propylene random copolymer having MFR (230° C., 2.16 kg)=8.0 g / 10 min and Mw=354,000 was used.
[0028] Next, chemiluminescence measurement and molecular weight distribution measurement were performed to evaluate the resin characteristics, which will be explained.
[0029] [Chemiluminescence measurement] The chemiluminescence measurement was carried out under the following conditions. Equipment: Chemiluminescence analyzer CLA-FS4 (Tohoku Electronics Industry Co., Ltd.) Sample chamber temperature: 150℃ Purge gas: Nitrogen gas Measurement time: 5 min Gate time: 0.1 sec Sample size: 0.2g
[0030] [Molecular weight distribution measurement] The molecular weight distribution measurement was carried out under the following conditions. Equipment: HLC-8321GPC / HT type high temperature gel permeation chromatograph (Tosoh Corporation) Column / Temperature: TSKgel GMH6-HT x 2 + TSKgel GMH6-HTL x 2 pieces, 7.5mm x 300mm (Tosoh Corporation) / 140℃ Mobile phase: o-dichlorobenzene (stabilizer: 0.025 wt% BHT included) Flow rate: 1.0mL / min Injection volume: 0.4mL Detector: Differential refractometer (RI) Column calibration: Monodisperse PS (TSKgel standard polystyrene; manufactured by Tosoh Corporation) Molecular weight calibration: relative calibration method (PS conversion) Analysis software: Empower3 (manufactured by Nihon Waters Co., Ltd.)
[0031] Example 1 A polypropylene resin composition obtained by dry blending 65 parts by weight of propylene homopolymer A and 35 parts by weight of ethylene propylene random copolymer A so that the CLA emission amount was 99,297 and Mw was 657,219 was used.
[0032] The above-described propylene raw material was supplied to a single screw extruder whose temperature was adjusted to 230°C, and melt extrusion was performed. Cooling water at 20°C was supplied to the cooling roll, and the film-forming speed was adjusted to 15 m / min and the thickness was adjusted to 60 μm, thereby producing the polypropylene-based unstretched film of Example 1.
[0033] The packaging material of Example 1 was produced by dry laminating a 12 μm-thick biaxially oriented PET film, a 7 μm-thick AL foil, a 15 μm-thick biaxially oriented polyamide film, and the above-mentioned polypropylene-based unoriented film in that order using a urethane-based adhesive.
[0034] Example 2 65 parts by weight of propylene homopolymer A and 35 parts by weight of ethylene propylene random copolymer A were fed to a twin-screw extruder with a screw diameter of 42 mm, which was adjusted to a temperature of 230°C, a screw speed of 300 rpm, a resin output rate of 40 kg / h, and supercritical carbon dioxide was injected at an injection rate of 2.4 kg / h. A polypropylene-based resin composition obtained by blending the two components so that the CLA emission was 134,131 and the Mw was 656,509 was used.
[0035] In the same manner as in Example 1, a polypropylene-based non-oriented film and a packaging material of Example 2 were produced.
[0036] Example 3 65 parts by weight of propylene homopolymer A and 35 parts by weight of ethylene propylene random copolymer A were fed to a twin-screw extruder with a screw diameter of 26.5 mm, the temperature of which was adjusted to 230°C, the screw speed was set to 300 rpm, the resin output rate was set to 20 kg / h, and supercritical carbon dioxide was injected into the extruder at an injection rate of 1.2 kg / h. The CLA emission was 210,048, M A polypropylene resin composition obtained by blending so that w was 676,829 was used.
[0037] In the same manner as in Example 1, a polypropylene-based non-oriented film and a packaging material of Example 3 were produced.
[0038] Comparative Example 1 65 parts by weight of propylene homopolymer A and 35 parts by weight of ethylene propylene random copolymer A were fed to a twin-screw extruder with a screw diameter of 26.5 mm, which was adjusted to a temperature of 230° C., a screw rotation speed of 300 rpm, and a resin output rate of 20 kg / h. A polypropylene resin composition obtained by blending the components so that the CLA emission amount was 345,579 and the Mw was 497,953 was used.
[0039] In the same manner as in Example 1, a polypropylene-based non-oriented film and a packaging material of Comparative Example 1 were produced.
[0040] Comparative Example 2 65 parts by weight of propylene homopolymer A and 35 parts by weight of ethylene propylene random copolymer A were fed to a twin-screw extruder with a screw diameter of 42 mm, which was adjusted to a temperature of 230° C., a screw rotation speed of 300 rpm, and a resin output rate of 40 kg / h. A polypropylene resin composition obtained by blending the components so that the CLA emission amount was 1,251,796 and the Mw was 252,005 was used.
[0041] In the same manner as in Example 1, a polypropylene-based non-oriented film and a packaging material of Comparative Example 2 were produced.
[0042] Comparative Example 3 A polypropylene-based resin composition was used, which was prepared by dry-blending 65 parts by weight of propylene homopolymer A and 35 parts by weight of ethylene-propylene random copolymer B so that the CLA emission amount was 101,267 and the Mw was 483,062.
[0043] In the same manner as in Example 1, a polypropylene-based non-oriented film and a packaging material of Comparative Example 3 were produced.
[0044] Comparative Example 4 65 parts by weight of propylene homopolymer A and 35 parts by weight of ethylene propylene random copolymer B were fed to a twin-screw extruder with a screw diameter of 42 mm, which was adjusted to a temperature of 230°C, a screw speed of 300 rpm, a resin output rate of 40 kg / h, and supercritical carbon dioxide was injected into the extruder at an injection rate of 2.4 kg / h. A polypropylene-based resin composition obtained by blending the components so that the CLA emission was 167,028 and the Mw was 472,550 was used.
[0045] In the same manner as in Example 1, a polypropylene-based non-oriented film and a packaging material of Comparative Example 4 were produced.
[0046] Comparative Example 5 65 parts by weight of propylene homopolymer A and 35 parts by weight of ethylene propylene random copolymer B were fed to a twin-screw extruder with a screw diameter of 26.5 mm, which was adjusted to a temperature of 230°C, with a screw rotation speed of 300 rpm and a resin output rate of 20 kg / h, and with supercritical carbon dioxide injected into the extruder at a rate of 1.2 kg / h. The CLA emission was 176,541, M A polypropylene resin composition obtained by blending so that w was 469,066 was used.
[0047] In the same manner as in Example 1, a polypropylene-based non-oriented film and a packaging material of Comparative Example 5 were produced.
[0048] Comparative Example 6 65 parts by weight of propylene homopolymer A and 35 parts by weight of ethylene propylene random copolymer B were fed to a twin-screw extruder with a screw diameter of 26.5 mm, which was adjusted to a temperature of 230° C., a screw rotation speed of 300 rpm, and a resin output rate of 20 kg / h. A polypropylene resin composition obtained by blending the components so that the CLA emission amount was 393,786 and the Mw was 366,000 was used.
[0049] In the same manner as in Example 1, a polypropylene-based non-oriented film and a packaging material of Comparative Example 6 were produced.
[0050] Comparative Example 7 65 parts by weight of propylene homopolymer A and 35 parts by weight of ethylene propylene random copolymer B were fed to a twin-screw extruder with a screw diameter of 42 mm, which was adjusted to a temperature of 230° C., a screw rotation speed of 300 rpm, and a resin output rate of 40 kg / h. A polypropylene resin composition obtained by blending the components was used, with a CLA emission of 1,203,760 and Mw of 236,046.
[0051] In the same manner as in Example 1, a polypropylene-based non-oriented film and a packaging material of Comparative Example 7 were produced.
[0052] Comparative Example 8 A polypropylene resin composition was used, which was prepared by dry blending 65 parts by weight of propylene homopolymer B and 35 parts by weight of ethylene propylene random copolymer A so that the CLA emission amount was 98,354 and Mw was 911,124.
[0053] An attempt was made to produce a polypropylene-based unstretched film of Comparative Example 8 in the same production method as in Example 1, but molding was not possible because the upper limit of the operable torque of the extruder was exceeded. Comparative Example 9
[0054] A polypropylene resin composition was used, which was prepared by dry blending 65 parts by weight of propylene homopolymer B and 35 parts by weight of ethylene propylene random copolymer B so that the CLA emission amount was 104,874 and the Mw was 731,851.
[0055] An attempt was made to produce a polypropylene-based unstretched film of Comparative Example 9 in the same production method as in Example 1, but molding was not possible because the upper limit of the operable torque of the extruder was exceeded.
[0056] Examples 1 to 3 and Comparative Examples 1 to 9 are summarized in Table 1.
[0057] [Table 1]
[0058] [Odor evaluation] An odor evaluation was carried out for each of the packaging materials produced in Examples 1 to 3 and Comparative Examples 1 to 7. Each packaging material was heat-sealed for 1 second at 200°C, 0.15 MPa, and a seal width of 5 mm to produce a three-sided bag, and 200 mL of water was poured into it, and one unsealed side was heat-sealed under the same conditions to produce a package with inner dimensions of 130 mm x 160 mm. This was subjected to a retort treatment at 130°C for 40 minutes, and if the water contained had no odor and was safe to drink, it was rated as good (◯); The water in the container had an unpleasant odor and was unsuitable for drinking, and was therefore rated as defective (X).
[0059] [Heat seal strength evaluation] Heat seal strength evaluation was carried out for each of the packaging materials produced in Examples 1 to 3 and Comparative Examples 1 to 7. The conditions for the heat seal strength evaluation were as follows. Equipment: Tensile testing machine AGS-500NX (manufactured by Shimadzu Corporation) Test speed: 300mm / min Sample dimensions: 15mm width x 80mm
[0060] A sample (pre-retort sample) was prepared by heat-sealing the packaging material at 200°C, 0.15 MPa, and a seal width of 5 mm for 1 second. A three-sided bag was also prepared by sealing under the same conditions, and 200 mL of water was poured into it, and one unsealed side was heat-sealed under the same conditions to prepare a package with inner dimensions of 130 mm x 160 mm. This package was retorted at 130°C for 40 minutes to prepare a sample (post-retort sample). These two types of samples were cut to the above sample dimensions and measurements were performed. Those with a heat seal strength of 50 N / 15 mm or more both before and after retort were judged to have good heat seal strength, and those with a heat seal strength of less than 50 N / 15 mm at least either before or after retort were judged to have bad heat seal strength.
[0061] [Impact resistance evaluation] Impact resistance evaluation was carried out for each of the polypropylene-based unstretched films produced in Examples 1 to 3 and Comparative Examples 1 to 7. The conditions for the impact resistance evaluation were as follows. Equipment: Film impact tester with thermostatic chamber (Toyo Seiki Seisakusho Co., Ltd.) Temperature: -5℃ Bullet size: 1 / 2 inch Measurement load: 1.5J Sample dimensions: 100mm wide x 2000mm
[0062] The impact resistance was judged to be good when the measured value was divided by the sample thickness and was 8 J / mm or more, and to be poor when the value was less than 8 J / mm.
[0063] In Examples 1 to 3 and Comparative Examples 1 to 9, those in which the results of the odor evaluation, heat seal strength evaluation, and impact resistance evaluation were all good were evaluated as "◯", and those in which the results were poor in any one of the evaluations or in which a polypropylene-based unstretched film could not be produced were evaluated as "X".
[0064] The results of the above-mentioned evaluations performed on Examples 1 to 3 and Comparative Examples 1 to 9 are shown in Table 2.
[0065] [Table 2]
[0066] Examples 1 to 3 met all of the above-mentioned criteria, and were excellent in low odor, heat sealability, and impact resistance.
[0067] In Comparative Examples 1 and 2, the CLA luminescence amount exceeds 300,000, the weight average molecular weight is less than 600,000, and the low odor and heat seal strength after retort are poor, making them difficult to put into practical use.
[0068] In the case of Comparative Examples 3 to 5, the weight average molecular weight is less than 600,000, and the heat seal strength and impact resistance after retort are insufficient, making it difficult to put them to practical use.
[0069] In Comparative Examples 6 to 7, the CLA luminescence amount exceeds 300,000, the weight average molecular weight is less than 600,000, and the low odor, heat seal strength and impact resistance are poor, making them difficult to put into practical use.
[0070] In Comparative Examples 8 to 9, the weight average molecular weight exceeds 700,000, and the resin viscosity is high, resulting in a torque value exceeding the operable range of the extruder, which makes it impossible to operate the extruder and therefore impossible to mold a film. [Industrial Applicability]
[0071] INDUSTRIAL APPLICABILITY The present invention is useful for a polypropylene-based non-oriented film, a packaging material, a packaging body, and a polypropylene-based resin composition for providing these, which are low in odor and excellent in heat seal strength and impact resistance.
Claims
1. It is composed of 60 to 70 parts by weight of a propylene homopolymer and 30 to 40 parts by weight of an ethylene-propylene random copolymer, The amount of light emitted as measured by a chemiluminescence method is 300,000 or less, A polypropylene-based resin composition having a weight average molecular weight of 600,000 or more and 700,000 or less.
2. A polypropylene-based non-oriented film using the polypropylene-based resin composition according to claim 1.
3. A packaging material comprising the non-oriented polypropylene film according to claim 2 and at least one substrate layer selected from the group consisting of biaxially oriented polyamide film, biaxially oriented polyester film, printing paper, and metal foil.
4. A package comprising the packaging material according to claim 3.
Citation Information
Patent Citations
Polypropylene composition of which early stage of crystal structure formation is controlled
JP1996217929A
Polypropylene sheet for ptp
JP2003277556A
Semicrystalline propylene polymer composition for making biaxially oriented polypropylene film
JP2004500452A
Polypropylene-based sealant film for contraction molding
JP2018176690A
Resin composition and manufacturing method, and molded body thereof