Anti-corrosive tape

The laminate film and tape, featuring a metal foil and high elastic resin layer, address the durability and maintenance issues of existing anti-corrosion methods by providing enhanced corrosion resistance and durability, ensuring long-term protection for steel materials.

JP2024163159AInactive Publication Date: 2024-11-21MCC ADVANCED MOLDINGS CO LTD
View PDF 16 Cites 0 Cited by

Patent Information

Application Number
JP2024148396
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2024-08-30
Publication Date
2024-11-21
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing anti-corrosion methods for steel materials, such as coatings and films, suffer from insufficient durability, susceptibility to pinholes and cracks, and high maintenance costs, particularly when exposed to outdoor conditions, leading to reduced corrosion resistance and structural integrity.

Method used

A laminate film comprising a metal foil laminated with a high elastic resin layer on one or both sides via an adhesive, and an anti-corrosion tape using a double-sided tape made of acrylic foam impregnated with an acrylic adhesive, providing enhanced corrosion resistance and durability.

Benefits of technology

The laminate film and tape exhibit excellent workability, long-term durability, and resistance to pinholes, cracks, and external stress, effectively preventing rusting and deterioration of steel materials at a lower cost with reduced environmental impact.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024163159000001_ABST
    Figure 2024163159000001_ABST
Patent Text Reader

Abstract

To provide an anti-corrosive laminate film and an anti-corrosive tape for steel, which have excellent workability, are excellent in anti-corrosiveness and long-term durability thereof, and prevent the occurrence of pinholes and cracks against physical external stress.SOLUTION: An anti-corrosive laminate film for steel has a metal foil, and a high elastic resin layer placed on at least one side of the metal foil through an adhesive. An anti-corrosive tape has the anti-corrosive laminate film bonded to a double-sided tape having acryl foam impregnated with an acrylic adhesive.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a corrosion prevention material for steel materials, and more particularly to an anticorrosive laminate film and an anticorrosive tape that are applied to the surface of steel materials used as constituent members of structures, etc. More specifically, the present invention relates to an anticorrosive laminate film and an anticorrosive tape that are suitably used to prevent corrosion of steel materials used in various structures such as buildings, marine structures, steel towers, elevated water tanks, tanks, water gates, bridges, plants, etc. [Background technology]

[0002] There are many different types of steel used as components for buildings, marine structures, steel towers, elevated water tanks, tanks, water gates, bridges, plants, etc., with strength, corrosion resistance, heat resistance, magnetic properties, thermal expansion coefficient, etc. adjusted by the carbon content and heat treatment method depending on the application and purpose.

[0003] If such steel materials are left as they are indoors or outdoors, they will corrode and develop red rust or yellowish-brown floating rust, which not only mars the scenery but also reduces the strength of the structure due to a decrease in thickness caused by corrosion, and in severe cases may even cause damage.

[0004] Conventionally, as a countermeasure against corrosion of such steel materials over time, it has been common to apply a coating having anticorrosive or antirust properties, as disclosed in Patent Document 1.

[0005] On the other hand, Patent Documents 2 and 3 propose imparting corrosion resistance to the surface of a steel material by attaching a waterproof film made of a resin layer or a metal layer to the surface of the steel material via an adhesive.

[0006] For example, Patent Document 2 describes a waterproof adhesive tape in which a substrate made of a material with low water permeability, for example a rubber material such as butyl rubber, or a resin material such as acrylic, silicone, polyethylene, epoxy, or urethane, is coated with an adhesive whose main components are natural rubber, styrene-butadiene rubber, butyl rubber, or acrylic rubber; it is preferable for this waterproof adhesive tape to have a film thickness of 0.1 to 2.0 mm, an adhesive strength of 1 kg·cm or more, and a water absorption rate of 1.0% or less.

[0007] Patent Document 3 describes a method for protecting steel material from corrosion by applying an adhesive to the surface of the steel material and attaching a resin sheet having a fiber layer or metal layer that imparts elasticity to the inside or surface of a resin layer made of polyvinyl chloride.

[0008] Patent Document 4 describes a heavy-duty corrosion-resistant coated steel material having a vapor-deposited base film layer on which an inorganic substance is vapor-deposited.

[0009] Patent Document 5 describes a steel material repair method that includes a step of attaching metal foil to the surface of the steel material so as to cover the corroded portion. [Prior art documents] [Patent documents]

[0010] [Patent Document 1] JP 2004-97945 A [Patent Document 2] JP 2001-81800 A [Patent Document 3] JP 2013-71267 A [Patent Document 4] JP 2005-262787 A [Patent Document 5] JP 2020-33730 A Summary of the Invention [Problem to be solved by the invention]

[0011] The corrosion prevention method using paint as in Patent Document 1 does not provide sufficient corrosion prevention effect, and there are problems in that corrosion easily progresses in places where moisture is likely to accumulate, where salt is likely to adhere, and in corners where the paint film is likely to thin. There are also problems in that the painting cost is high, the service life is limited, and regular repainting is required, resulting in high maintenance costs.

[0012] In the method of attaching a waterproof film consisting of a resin layer or a metal layer to the surface of a steel material via an adhesive as described in Patent Documents 2 and 3, the anticorrosive effect can be enhanced by selecting the resin layer or the metal layer, but when used outdoors, there is a problem that pinholes and cracks are likely to occur when sand, pebbles, etc. collide with the film surface due to wind and rain, and the anticorrosive properties cannot be maintained for a long period of time. If the metal layer is made thicker to prevent pinholes and cracks, the sheet becomes harder, causing problems with application to steel materials. Furthermore, the waterproof resin sheet used as the film substrate has poor adhesion to paints and adhesives, and there is also the problem of peeling.

[0013] The heavy-duty corrosion-resistant coated steel material having an inorganic vapor-deposited base film layer described in Patent Document 4 has improved moisture barrier properties and increased durability compared to resin films, but is prone to pinholes and cracks and is insufficient for maintaining corrosion resistance for a long period of time. In addition, the film strength is insufficient and there is a possibility of damage due to external forces.

[0014] In the method of applying a metal foil to cover a corroded part on a steel surface as described in Patent Document 5, a thin metal foil has insufficient strength and is susceptible to breakage due to external force. A thick metal foil increases the strength, but is too hard, which causes problems in handling and application, and limits the scope of application.

[0015] As described above, various corrosion prevention methods and various corrosion prevention films have been proposed in the past to impart corrosion resistance to steel materials. However, there is a problem that the corrosion resistance of steel materials cannot be maintained for long periods of time, and maintenance is required every time the steel material corrodes. Furthermore, when pebbles or other debris collide with the steel due to wind and rain, pinholes and cracks can form, compromising the barrier properties and making the steel more susceptible to corrosion.

[0016] The present invention has been made in consideration of the above-mentioned situation, and an object of the present invention is to provide a laminate film and anticorrosion tape for corrosion protection of steel materials that are easy to apply, have excellent corrosion resistance and long-term durability, and are also resistant to pinholes and cracks even when subjected to physical external stress. [Means for solving the problem]

[0017] As a result of extensive investigation into the above problems, the present inventors have found that the above problems can be easily solved by employing a specific configuration, and have thus completed the present invention. That is, the gist of the present invention is A laminate film for corrosion prevention of steel materials, comprising a metal foil and a highly elastic resin layer laminated on at least one surface of the metal foil via an adhesive; and a corrosion-prevention tape comprising a double-sided tape made of an acrylic foam impregnated with an acrylic adhesive bonded to the corrosion-prevention laminate film; It resides in. Effect of the Invention

[0018] The present invention provides a laminate film and anticorrosion tape for corrosion protection of steel materials that are excellent in workability, corrosion prevention and its long-term durability, water resistance, and pinhole resistance, and that can be produced inexpensively using a method that places little strain on the environment. By using the anticorrosive laminate film and anticorrosive tape of the present invention, rusting and deterioration of steel materials can be prevented effectively and at low cost, thereby improving the long-term durability and reliability of steel materials used in various structures. [Brief description of the drawings]

[0019] [Figure 1]1 is a schematic cross-sectional view showing an example of an embodiment of the anticorrosive laminate film and anticorrosive tape of the present invention. [Diagram 2] FIG. 2 is a schematic cross-sectional view showing another example of an embodiment of the anticorrosive laminate film and anticorrosive tape of the present invention. [Diagram 3] FIG. 2 is a schematic cross-sectional view showing another example of an embodiment of the anticorrosive laminate film and anticorrosive tape of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0020] Hereinafter, an embodiment of the present invention will be described in detail with reference to FIGS. 1 to 3 showing an example of an embodiment of the anticorrosive laminate film and anticorrosive tape of the present invention, but the present invention is not limited to the following embodiment.

[0021] [Corrosion-resistant laminate film] The anticorrosive laminate film of the present invention is a anticorrosive laminate film for steel materials, and is characterized by having a metal foil and a highly elastic resin layer laminated on at least one side of the metal foil via an adhesive. That is, as shown in Figures 1 to 3, the anticorrosive laminate film 10 (10A to 10C) of the present invention has at least a high elasticity resin layer 1 (1a, 1b), an adhesive layer 2 (2a, 2b, 2c, 2d) which is an adhesive layer, and a metal foil 3, and may further have a low elasticity resin layer 4 (4a, 4b).

[0022] In the present invention, the high elasticity resin layer refers to a layer made of a resin having a relatively high tensile elastic modulus, and the low elasticity resin layer refers to a layer made of a resin having a relatively low tensile elastic modulus. The suitable tensile elastic modulus of each layer is as described below, but the tensile elastic modulus of the high elasticity resin layer used in the same corrosion-resistant laminate film is higher than the tensile elastic modulus of the low elasticity resin layer, and the difference therebetween is preferably 500 MPa or more. In the present invention, the tensile modulus of a resin is a value measured by the method described in the Examples section below, and the maximum value of the in-plane tensile modulus of a resin film (the tensile modulus in either the extrusion direction (longitudinal direction) MD or the width direction (direction perpendicular to the extrusion direction) TD of the film) is defined as the tensile modulus of the resin film.

[0023] <Metal foil> The metal foil 3 is a layer that acts as a barrier to prevent the intrusion of moisture from the outside, and is required to have the following characteristics: no pinholes, high tensile strength as an anticorrosive laminate film, and crack resistance against deformation and stretching due to external forces.

[0024] Corrosion-resistant and inexpensive aluminum, its alloys, stainless steel, etc. are used as the metal foil 3. From the viewpoint of crack resistance, pure Al (aluminum) with a purity of 99% or more, Al-Cu-Mg alloys, Al-Mn alloys, Al-Si alloys, Al-Mg alloys, Al-Mg-Si alloys, Al-Zn-Mg alloys, Al-Fe alloys, etc. can be used. The aluminum content in the Al alloy is preferably 95% by weight or more.

[0025] Among these, the metal foil is preferably an aluminum foil with excellent elongation, and aluminum foil containing 0.1% to 3.0% by weight of iron (alloy number 8000 series) or pure aluminum with a purity of 99% or more (alloy number 1000 series) is preferable. In the above-mentioned aluminum foil containing 0.1% to 3.0% by weight of iron, if the iron content is less than this range, the elongation tends to be insufficient, and if it is more than this range, the metal foil tends to be easily corroded. The preferable iron content of the iron-containing aluminum foil is 0.2% to 1.7% by weight. Furthermore, there are hard aluminum foils and soft aluminum foils as aluminum foils, and soft aluminum foils that have been annealed are preferred because they have flexibility.

[0026] The thickness of the metal foil 3 such as an aluminum foil is preferably from 6 μm to 60 μm, particularly from 9 μm to 25 μm, in order to achieve both a thin film and good barrier properties.

[0027] The aluminum foil may be subjected to a chemical conversion treatment to improve corrosion resistance. In particular, boehmite treatment is preferred because it is inexpensive and harmless, and the contact angle of the treated surface with water after the boehmite treatment is preferably 10° to 90°.

[0028] <High elasticity resin layer> The highly elastic resin layer 1 (1a, 1b) in the present invention is a layer for preventing damage to the metal foil due to external forces such as punctures, reinforcing the metal foil, and preventing damage to the film itself due to external physical stress, and may be a single-layer film or a laminated film of two or more layers.

[0029] The highly elastic resin layer 1 is required to have excellent mechanical strength, excellent protection for the metal foil 3, and barrier properties, and is preferably made of a resin film having a relatively high tensile modulus of elasticity, since this allows the film thickness to be reduced.

[0030] Examples of resins constituting the highly elastic resin layer include polyamide (PA or Ny), polyamideimide (PAI), polyacetal (POM), polyarylate (Par), polycarbonate (PC), polyalkylene terephthalates (PAT) such as polyethylene terephthalate (PET), polybutylene terephthalate (PBT), and polytrimethylene terephthalate (PTT), polyethylene naphthalate (PEN), polybutylene naphthalate (PBN), polymethyl methacrylate (PMMA), polyphenylene oxide (PPE), polyethersulfone (PES), polymethylpentene (TPX), polyoxybenzylene (POB), polyimide (PI), liquid crystalline polyester, polysulfone (PSF), polyphenylene sulfide (PPS), polybisamidotriazole, polyaminobismaleimide, polyetherimide (PEI), polyetheretherketone (PEEK), and the like, or a mixture of two or more of these. Among these, those made of polycarbonate (PC), polybutylene terephthalate (PBT), polyalkylene terephthalate (PAT) such as polyethylene terephthalate (PET), polyethylene naphthalate (PEN), polybutylene naphthalate (PBN), polyamide (PA or Ny), polyphenylene sulfide (PPS), polyamideimide (PAI), and polyimide (PI) are preferable.

[0031] The high elasticity resin layer may be a non-stretched film or a stretched film, but from the viewpoint of mechanical strength and heat resistance, the high elasticity resin layer is preferably made of a stretched film, and more preferably a biaxially stretched film. In particular, those made of a biaxially stretched polyethylene terephthalate film, a biaxially stretched polyethylene naphthalate film, a biaxially stretched polyamide film, or a biaxially stretched polybutylene terephthalate film are preferable because they have a moderately high tensile modulus and are inexpensive.

[0032] Among these, biaxially oriented polyamide films and biaxially oriented polybutylene terephthalate films are more preferable because they also have appropriate flexibility. Furthermore, biaxially oriented polyamide films and biaxially oriented polybutene terephthalate films produced by the tubular method are particularly preferred, with biaxially oriented polyamide films being particularly preferred, in that they have little anisotropy in the film directions (longitudinal and transverse directions).

[0033] The highly elastic resin layer must also play a role in preventing the formation of pinholes and cracks in the metal foil due to deformation caused by external punctures, etc., and must have a certain degree of elasticity and thickness in order to prevent damage to the corrosion-resistant laminate film during installation. From this viewpoint, it is preferable that the tensile modulus of the high-elasticity resin layer is, as a maximum value in the plane of the film (usually either the extrusion direction (longitudinal direction) or the width direction of the film), 1500 MPa or more, particularly 1700 MPa or more, and especially 2000 MPa or more. If the tensile modulus of elasticity of the highly elastic resin layer is less than 1500 MPa, the effect of reinforcing the metal foil tends to be reduced, and pinholes and cracks tend to occur more easily due to external stress.

[0034] There is no particular upper limit to the tensile modulus of the high-elasticity resin layer, but the maximum value in the film plane is preferably 6500 MPa or less. If the tensile modulus is greater than this, the anticorrosive laminate film of the present invention becomes too hard and loses flexibility, so the thickness must be reduced, and pinhole resistance and puncture resistance may deteriorate. In addition, when the anticorrosive laminate film is attached to a corner while being bent, the return force becomes stronger over time, and peeling may occur. The upper limit of the tensile elastic modulus of the highly elastic resin layer is more preferably 5000 MPa or less, and particularly preferably 4500 MPa or less.

[0035] In addition, the thickness of the high elasticity resin layer is preferably 5 μm or more and 50 μm or less. If the thickness of the high elasticity resin layer is thicker than 50 μm, the rigidity of the anticorrosive laminate film of the present invention becomes too high, making it difficult to bend and difficult to attach to the corners of steel materials, making it difficult to install, and the surface density tends to increase and it becomes difficult to reduce the weight. On the other hand, if the thickness of the high elasticity resin layer is thinner than 5 μm, it may affect the puncture resistance. The thickness of the high elasticity resin layer is particularly preferably 8 μm or more and 30 μm or less. Here, the thickness of the high-elasticity resin layer refers to the thickness of each high-elasticity resin layer (per location). Here, one high-elasticity resin layer is a layer that does not include the adhesive layer 2, for example, a layer between adhesive layers, and if one high-elasticity resin layer has a laminated structure of multiple layers, it corresponds to the total thickness of the layers.

[0036] <Adhesive layer> The adhesive layer 2 is a layer for bonding the high elasticity resin layer 1 to the metal foil 3 or the low elasticity resin layer 4 , or the metal foil 3 to the low elasticity resin layer 4 .

[0037] As the adhesive for the adhesive layer 2, when the high adhesion resin layer 1 and the metal foil 3 or the low elasticity resin layer 4, or the metal foil 3 and the low elasticity resin layer 4 are bonded together by a dry lamination method, various adhesives for dry lamination, such as aliphatic polyester-based, aromatic polyester-based, polyethyleneimine-based, polyether-based, cyanoacrylate-based, urethane-based, organic titanium-based, polyether urethane-based, epoxy-based, polyester urethane-based, imide-based, isocyanate-based, polyolefin-based, silicone-based, and acrylic-based adhesives can be used. Among these adhesives, aromatic polyester-based, polyolefin-based and acrylic-based adhesives are preferred because they have excellent weather resistance and water resistance.

[0038] When further moisture resistance or weather resistance is required, an acid-modified resin may be used for the adhesive layer and bonded by a thermal lamination method, or the acid-modified resin may be extruded onto a metal foil or a low-elasticity resin layer or a high-elasticity resin layer by an extrusion lamination method or a sandwich lamination method, and the high-elasticity resin layer and the metal foil or the low-elasticity resin layer may be bonded together.

[0039] The thickness of the adhesive layer is not limited, but for adhesives used in the dry lamination method, it is usually in the range of 1 to 10 μm, and preferably in the range of 3 to 6 μm. In the case of lamination by thermal lamination, extrusion lamination, or sandwich lamination, the thickness of the acid-modified resin layer is usually in the range of 3 to 80 μm, and preferably in the range of 5 to 30 μm.

[0040] <Low elasticity resin layer> When flexibility and solvent resistance are important in anticorrosive laminate film of the present invention in anticipation of the application of paint or adhesive, a flexible low-elasticity resin layer 4 having a low tensile modulus of elasticity, such as polyolefin, may be further laminated thereto. For example, as shown in FIG. 1, by laminating high-elasticity resin layers 1a, 1b having a high tensile elastic modulus and low-elasticity resin layers 4a, 4b having solvent resistance on both sides of a metal foil 3, flexibility can be imparted, workability such as handling can be improved, and resistance to paints and adhesives containing solvents can be improved, which is preferable. As shown in FIG. 3, when a low-elasticity resin layer 4a is provided only on the bonding surface of the metal foil 3 that is to be bonded to the steel material, workability can be improved by imparting flexibility.

[0041] Examples of resins constituting the low elasticity resin layer 4 include polyolefins such as polypropylene, polyethylene (high density, medium density, low density, linear low density), propylene-ethylene block or random copolymers, and acid-modified products thereof, rubber or latex components such as ethylene-propylene copolymer rubber, styrene-butadiene rubber, styrene-butadiene-styrene block copolymers or hydrogenated derivatives thereof, polybutadiene, polyisobutylene, polyvinylidene fluoride (PVDF), polyvinyl fluoride, chlorotrifluoroethylene, ethylene-tetrafluoroethylene copolymer (ETFE), polytetrafluoroethylene (PTFE), hexafluoropropylene, perfluoroalkyl vinyl ether copolymers, acrylic acid alkyl ester copolymers, polyester ester copolymers, polyether ester copolymers, polyether amide copolymers, polyurethane copolymers, vinyl chloride resins, and the like, or mixtures of two or more of these.

[0042] In particular, the low elasticity resin layer 4 is used as necessary for the purpose of imparting impact resistance and weather resistance to protect the high elasticity resin layer from impact and the external environment, and for the purpose of preventing deterioration due to solvents contained in the adhesive when laminating to steel materials. Preferred examples of the low elasticity resin layer 4 include polyolefins such as polypropylene, polyethylene (high density, medium density, low density, linear low density), propylene-ethylene block or random copolymers, and acid-modified products thereof, rubber or latex components such as ethylene-propylene copolymer rubber, styrene-butadiene rubber, styrene-butadiene-styrene block copolymers or hydrogenated derivatives thereof, polybutadiene, and polyisobutylene.

[0043] In the present invention, the low elasticity resin layer 4 can be appropriately selected from polyethylene resins, i.e., those mainly composed of high-density, medium-density, low-density, or linear low-density polyethylene, polyolefin resins mainly composed of random or block polypropylene, and polyolefin resins modified with acid or silane. Among these, preferred are single-layer or laminated structures including a polyethylene resin layer mainly composed of linear low-density polyethylene (LLPE), high-density polyethylene, or medium-density polyethylene, and also preferred are single-layer or laminated structures including a resin layer mainly composed of random polypropylene (R-PP). The term "main component" used herein refers to the component that is contained in the largest amount by weight in a material made by blending a plurality of components.

[0044] In the present invention, the low elasticity resin layer may contain components other than the polyethylene resin, so long as the above conditions are satisfied.

[0045] Polyethylene resin has a lower melting point than polypropylene resin, but it is a polymer whose molecules cross-link when heat is repeatedly applied. When exposed to high temperatures for long periods of time, such as outdoors in the hot sun when the temperature of the steel material rises to 40-80°C, its molecules are less likely to break, and it has better long-term heat resistance than polypropylene resin. Furthermore, polyethylene resin has high melt tension, flexibility, resistance to deformation, resistance to whitening when deformed, and excellent cold resistance. Polyethylene resin also has a higher density than polypropylene resin, and is highly resistant to external moisture and polar solvents contained in adhesives.

[0046] In the present invention, linear low density polyethylene (LLPE) means a copolymer of ethylene and an α-olefin having about 4 to 20 carbon atoms, and specific examples of the branched side chain composed of an α-olefin include various comonomers such as butene-1, hexene-1, 4-methylpentene-1, octene-1, decene-1, tetracene-1, and octadecene-1. Two or more of these α-olefins may be used in combination. In addition, when an α-olefin having about 4 to 20 carbon atoms is used as a comonomer, propylene may be further used as a comonomer.

[0047] Any linear low-density polyethylene (LLPE) can be used as long as it can keep the MFR, density, and tensile modulus within the preferred ranges described below. Among them, linear low-density polyethylene having at least one side chain of butene-1, hexene-1, or octene-1 is preferred because it has appropriate flexibility, and hexene-1 and octene-1 are particularly preferred because they have excellent solvent resistance.

[0048] There are no limitations on the method for producing linear low density polyethylene (LLPE), and any known method for producing polyolefin resins can be used. Generally, however, it is preferable to produce it using a Ziegler catalyst, a metallocene catalyst, or the like.

[0049] The polyethylene resin in the present invention can also contain polyethylene resins other than linear low density polyethylene (LLPE). The polyethylene resins other than linear low density polyethylene (LLPE) are not limited, but specifically include high density polyethylene (HDPE), medium density polyethylene (MDPE), low density polyethylene (LDPE), etc. Here, low density polyethylene (LDPE) does not include the linear low density polyethylene (LLPE), and generally includes what is called high pressure low density polyethylene. The manufacturing method of high density polyethylene (HDPE), medium density polyethylene (MDPE), and low density polyethylene (LDPE) is not limited, and known methods can be adopted, but it is usually preferable to manufacture them using a Ziegler catalyst, a metallocene catalyst, etc.

[0050] Furthermore, in order to prevent the moisture absorption and ultraviolet degradation of the high elasticity resin layer, various additives such as various elastomer components such as olefin-based elastomers such as ethylene-propylene copolymers, ethylene-butene copolymers, propylene-butene copolymers, ethylene-butene-propylene copolymers, and ethylene-propylene-diene copolymers, styrene-based elastomers, polyester-based elastomers, and polyamide-based elastomers, antioxidants, heat stabilizers, various plasticizers, light stabilizers, ultraviolet absorbers, neutralizing agents, lubricants, anti-fogging agents, anti-blocking agents, crosslinking agents, crosslinking assistants, colorants, flame retardants, and dispersants may be added to the low elasticity resin layer, within a range that does not impair the effects of the present invention.

[0051] The low elasticity resin layer in the present invention has a melt flow rate (MFR) of 0.1 g / 10 min to 20 g / 10 min and a density of 0.91 g / cm 3 More than 0.960g / cm 3 Hereinafter, the tensile modulus is preferably 100 MPa or more and 2000 MPa or less. The MFR, density and tensile modulus of the low elasticity resin layer are measured by the methods described in the Examples section below.

[0052] If the MFR of the low elasticity resin layer 5 is greater than 20 g / 10 min, the molecular weight of the polymer will be low, solvent resistance will be reduced, and weather resistance may be poor. The preferred MFR is 10 g / 10 min, more preferably 5 g / 10 min or less, and even more preferably 3 g / 10 min or less. The lower limit of the MFR is 0.1 g / 10 min or more because it is necessary to have a level that does not cause problems in film formation when forming a film by inflation molding, and it is particularly preferable that the MFR is 0.3 g / 10 min or more because high-speed moldability in inflation molding can be maintained.

[0053] In addition, the density of the low-elasticity resin layer is 0.91 g / cm 3 If the density is smaller than this, the solvent resistance and waterproof resistance may be deteriorated. In order to block moisture from the outside and to increase the resistance to solvents, it is preferable that the density of the low elasticity resin layer is relatively high, and the preferable lower limit of the density is 0.918 g / cm. 3 More preferably, 0.920 g / cm 3 More preferably, it is 0.923 g / cm 3 The upper limit of density is 0.960 g / cm3 without impairing flexibility. 3 Below, especially 0.950g / cm 3 Taking into consideration the whitening resistance, the upper limit of the density is more preferably 0.945 g / cm 3 The following is the result. The means for setting the density of the low-elasticity resin layer within the above range is not limited, but examples include optimizing the polyethylene resin used in the low-elasticity resin layer, and, as described above, using polyethylene resin and resins other than polyethylene resin in combination and optimizing the blending ratio thereof.

[0054] The tensile modulus of the low elasticity resin layer is preferably 100 MPa or more, since too much flexibility can easily cause material destruction when an external force such as deformation is applied, and conversely, if it is too hard, it can easily become brittle and easily peel off from the metal foil in contact with it via the adhesive layer, so it is preferably less than 1500 MPa, and more preferably 1300 MPa or less. The tensile modulus of the low elasticity resin layer is particularly preferably 130 MPa or more and 1000 MPa or less, and particularly preferably 180 MPa or more and 900 MPa or less.

[0055] The above-mentioned values ​​of MFR, density, and tensile modulus refer to the properties of the resin constituting the low elasticity resin layer, and in the case where multiple polyethylene resins are used in combination as the polyethylene resin or where a resin other than polyethylene resin is contained, they refer to the values ​​as a resin composition.

[0056] In the present invention, it is particularly preferable to use a layer mainly composed of linear low-density polyethylene as the low-elasticity resin layer and a specific acid-modified polyethylene resin layer as the adhesive layer that is bonded to the high-elasticity resin layer or the metal foil, thereby further improving the solvent resistance and waterproof resistance.

[0057] The low elasticity resin layer may have a multi-layer structure, such as a laminate structure of a layer mainly composed of linear low density polyethylene and a random polypropylene layer or a block polypropylene layer, or a laminate structure of a layer mainly composed of linear low density polyethylene and a layer mainly composed of medium density polyethylene or high density polyethylene, or may further have a multi-layer laminate structure of about 3 to 5 layers.

[0058] The thickness of the low elasticity resin layer is preferably 3 μm or more and 80 μm or less, more preferably 10 μm or more and 70 μm or less, and particularly preferably 12 μm or more and 60 μm or less. If the thickness of the low elasticity resin layer is thinner than the lower limit, the water resistance may be insufficient and the corrosion prevention may be reduced. In addition, the flexibility may be insufficient and the workability may be poor. On the other hand, if the thickness is thicker than the upper limit, the handleability may be deteriorated. Here, the thickness of the low elasticity resin layer refers to the thickness per low elasticity resin layer (per location). Here, one low elasticity resin layer is a layer that does not include the adhesive layer 2, for example, a layer adjacent to the adhesive layer 2, and if one low elasticity resin layer has a laminated structure of multiple layers, it corresponds to the total thickness of the layers.

[0059] The low elasticity resin layer is preferably provided with an uneven surface in order to improve adhesion with a pressure sensitive adhesive when it is applied to a steel material or with an adhesive when it is applied to a high elasticity resin layer. In this case, the surface roughness Ra of the uneven surface is preferably about 0.1 to 1.0 μm, particularly about 0.3 to 0.8 μm. In addition, one or both sides of the low elasticity resin layer may be subjected to a treatment such as corona discharge treatment, plasma treatment, primer treatment, anchor coat treatment, etc., to improve adhesion to pressure-sensitive adhesives or adhesives and paintability when painting is applied. In this case, the contact angle of the treated surface with water is preferably 50° to 95°, and particularly preferably 55° to 90°.

[0060] [Layer structure of anticorrosive laminate film] The anticorrosive laminate film of the present invention may have a high elasticity resin layer, a metal foil, and an adhesive layer for adhering them together, and there are no particular limitations on its layer structure. For example, as shown in Figure 1, an anticorrosive laminate film 10 (10A) can be produced by laminating high elasticity resin layers 1 (1a, 1b) on both sides of a metal foil 3 via adhesive layers 2 (2a, 2b), and further laminating low elasticity resin layers 4 (4a, 4b) on the outside thereof via adhesive layers 2 (2c, 2d), thereby integrating the two.

[0061] Also, as shown in Figure 2, there is an anticorrosive laminate film 10 (10B) in which the low elasticity resin layers 4a, 4b of the anticorrosive laminate film 10A in Figure 1 are omitted, and high elasticity resin layers 1 (1a, 1b) are laminated and integrated on both sides of the metal foil 3 via adhesive layers 2 (2a, 2b).

[0062] Furthermore, as shown in FIG. 3, a high elasticity resin layer 1 (1a) may be laminated on only one side of a metal foil 3 via an adhesive layer 2 (2a), and a low elasticity resin layer 4 (4a) may be laminated on the other side via an adhesive layer 2 (2b) to form an integrated anticorrosion laminate film 10 (10C).

[0063] In addition, in the corrosion-resistant laminate film 10B of Figure 2, a low-elasticity resin layer may be laminated on only one of the high-elasticity resin layers via an adhesive layer to form an integrated film, or a low-elasticity resin layer may be laminated on the high-elasticity resin layer 1a of the corrosion-resistant laminate film 10C of Figure 3 via an adhesive layer to form an integrated film.

[0064] In either case, when a high elasticity resin layer and a low elasticity resin layer are laminated on one side of a metal foil, the layers are laminated in the following order: metal foil / adhesive layer / high elasticity resin layer / adhesive layer / low elasticity resin layer, and it is preferable that the low elasticity resin layer is located on the outer side (surface side) of the high elasticity resin layer.

[0065] In the corrosion-resistant laminate film of the present invention, the high elasticity resin layer, the metal foil, and the low elasticity resin layer may each be within the preferred thickness ranges described above, and there is no particular restriction on their total thickness. However, in order to ensure the necessary thickness of each layer and effectively obtain each function, the lower limit of the total thickness of the corrosion-resistant laminate film of the present invention is preferably 30 μm or more, more preferably 45 μm or more, and particularly preferably 50 μm or more, as this makes it less likely to tear. On the other hand, from the viewpoint of preventing the anticorrosive laminate film from becoming excessively thick and becoming highly rigid, which would impair workability, etc., the upper limit of the total thickness of the anticorrosive laminate film of the present invention is preferably 250 μm or less, and more preferably 200 μm or less.

[0066] <Other processing> The outer surface of the anticorrosive laminate film (the surface opposite to the surface to which the steel material is attached) may be coated with paint (not shown) to enhance the anticorrosive effect. In order to improve wettability with respect to adhesives or glues used for painting or attachment to steel materials, the film may be subjected to a surface treatment so that the contact angle with water is 50° or more and 95° or less. Furthermore, when spraying paint on the outside of the anticorrosive laminate film or applying an adhesive to the inside, solvent resistance is required, so it is preferable to provide a hydrophobic low-elasticity resin layer with excellent solvent resistance, but good surface wettability is also important. Therefore, a primer may be applied, or as described above, the surface of the low-elasticity resin layer may be made uneven, or the outer surface of the anticorrosive laminate film may be subjected to surface treatment such as corona discharge treatment, plasma treatment, or flame treatment to improve adhesion to the adhesive or paint.

[0067] [Manufacturing method of anticorrosive laminate film] There is no particular limitation on the method for producing the anticorrosive laminate film of the present invention, but it is preferable that at least the highly elastic resin layer and the metal foil are laminated by a dry lamination method using an adhesive.

[0068] Alternatively, the high elasticity resin layer and the low elasticity resin layer may be bonded together in advance by a dry lamination method, and then the metal foil may be bonded together by a dry lamination method, or the high elasticity resin layer and the metal foil may be bonded together by a dry lamination method, and then the low elasticity resin layer may be bonded to a low elasticity resin film that has been formed in advance by an inflation molding method (multilayer inflation molding method) by a dry lamination method using an adhesive. Alternatively, a low elasticity resin film may be laminated to a high elasticity resin layer by thermal lamination, or a low elasticity resin may be melted and extruded from a T-die onto the surface of a high elasticity resin layer by extrusion lamination.

[0069] Generally, polypropylene is often used as the resin for the low elasticity resin layer if heat resistance is required, and polypropylene film-formed by extrusion lamination, sand lamination, or cast method is often used to keep costs low. All of these are formed by cooling molten resin extruded from a T-shaped mold (a strip-shaped resin outlet), so differences in physical properties such as tensile strength, elongation, and tensile modulus are likely to occur in the MD and TD directions. On the other hand, when a corrosion-resistant laminate film using such a film as a low elasticity resin layer is applied to a steel material with an adhesive, it is expected that mechanical stress will occur in all directions and that shrinkage will occur due to the solvent contained in the adhesive. For this reason, films that have differences in physical properties such as tensile strength, elongation, and tensile modulus between the MD and TD directions tend to wrinkle easily during application.

[0070] In contrast, films produced by the inflation molding method have the advantage that there is less difference in mechanical properties between the extrusion direction (MD) and the circumferential direction (TD) perpendicular to the extrusion direction, and wrinkles are less likely to occur when handled during construction.

[0071] For these reasons, if heat resistance is not required, it is preferable to use polyethylene, which has excellent solvent resistance and moderate flexibility, as the resin used for the low-elasticity resin layer, and to produce a film by adjusting the blow-up ratio during molding so as to eliminate anisotropy as a corrosion-resistant laminate film, while taking into consideration the balance with the physical properties of the high-elasticity resin layer and making the film.

[0072] In addition, the resin raw material suitable for the inflation molding method must have characteristics such as low MFR, high molecular weight, and high melt tension, and furthermore, the processing temperature during film formation must be low. In this respect, the resin has different characteristics from the resin used in the extrusion lamination method or sandwich lamination method, which is molded at high temperature and requires high MFR and high flowability. For this reason, in the present invention, the low elasticity resin layer is preferably made of a low MFR resin as described above, and these resins have the advantage that film strength can be easily obtained due to their low MFR and high melt tension.

[0073] In the present invention, in order to make better use of the low anisotropy of the film produced by the inflation molding method while imparting various properties required for an anticorrosive laminate film, such as mechanical properties, sealing properties, heat resistance, and formability, attention is focused on the properties of the resin used in the inflation molding method, and preferably a layer having the specific resin and specific physical properties described above is formed, thereby obtaining an anticorrosive laminate film that has excellent adhesion to the metal foil as a barrier layer, can prevent the penetration of moisture, and has excellent solvent resistance.

[0074] [Anti-corrosion tape] The anticorrosive laminate film of the present invention can be used as an anticorrosive tape by protecting it with a release paper or film to which a pressure-sensitive adhesive or adhesive has been applied in advance, or by attaching a so-called double-sided tape, which is a film or sheet-like material impregnated with a pressure-sensitive adhesive, to the anticorrosive laminate film of the present invention. With such a configuration, it is possible to improve the long-term water resistance, durability, and workability of the anticorrosive tape. In this case, it is preferable to use an adhesive having properties such that the adhesive strength is moderately low, particularly at the initial stage of lamination, and that the adhesive strength improves after hardening due to humidity, as an anticorrosive tape and to adhere it to the anticorrosive laminate film of the present invention, which is the anticorrosive substrate. In addition, the anticorrosive laminate film needs to have appropriate elasticity and thickness in order to absorb the uneven surfaces of the adherend, such as steel materials, and to alleviate the stress applied during lamination and the stress from external impact, thereby preventing damage to the anticorrosive laminate film for a long period of time. From this viewpoint, it is preferable to use a double-sided tape having a base material of paper, nonwoven fabric, cotton fabric, polyethylene or acrylic foam impregnated with an acrylic adhesive attached to an anticorrosive laminate film as an anticorrosive tape.

[0075] 1 to 3 show anticorrosive tapes 20 (20A, 20B, 20C) each formed by adhering such double-sided tape 5 and release paper or release film 6 to anticorrosive laminate films 10 (10A, 10B, 10C). As shown in Figs. 1 to 3, the double-sided tape 5 and release paper or release film 6 are provided so that the highly elastic resin layer 1 (1a) is present on the outer surface side of the metal foil 3 in the anticorrosive laminate films 10A to 10C.

[0076] The preferred thickness of the double-sided tape 5 is 0.1 mm or more and 2 mm or less. If it is thicker than this, flexibility may be lost and application may be deteriorated. On the other hand, if it is thinner than this, conformability to the unevenness of the adherend may be deteriorated and adhesive strength may be insufficient. The more preferred thickness of the double-sided tape is 0.15 mm or more and 1.5 mm or less, and particularly preferably 0.25 mm or more and 1.2 mm or less.

[0077] The modulus of elasticity of the double-sided tape should also be appropriately low, and it is preferable to use an adhesive double-sided tape in which an acrylic adhesive is impregnated into an acrylic foam having a tensile modulus of elasticity of 100 MPa or less. EXAMPLES

[0078] The present invention will be described in more detail below with reference to examples. However, the present invention is not limited to the following examples as long as it does not depart from the gist of the present invention.

[0079] [Evaluation method] The materials used in the following examples and comparative examples and the evaluation methods for the produced anticorrosive laminate films and anticorrosive tapes are as follows.

[0080] <Contact angle with water> The contact angle of the sample surface with water was measured using an automatic contact angle meter (product name: DROPMASTER, manufactured by Kyowa Interface Science Co., Ltd.), and the average value of the measured values ​​at five points was used.

[0081] <Tensile modulus> The tensile modulus of elasticity of a resin or resin composition is a value measured on a 15 mm wide rectangular sample at a chuck distance of 100 mm using a Tensilon type tensile tester at 1 mm / min in accordance with ISO1184-1970.

[0082] <MFR(メルトフローレート)> The value was measured at 190℃ and a load of 2.16kgf based on the JISK 7210A method.

[0083] <density> The density was determined by JIS K7112A method (underwater displacement method).

[0084] <Puncture strength> A test piece was prepared by cutting a piece of anticorrosive laminate film to a size of 50 mm x 100 mm. Using an Imada tensile tester, the test piece was fixed between a presser plate with a 20 mm diameter opening in the center and a stand, and a needle with a diameter of 1 mm and a semicircular tip radius of 0.5 mm was pierced at a piercing speed of 50 mm / min to measure the maximum load until the needle penetrated. The average value of three samples was used as the measurement result and was evaluated according to the following criteria. ○: Piercing strength 15N or more △: Puncture strength 10N or more but less than 15N ×: Piercing strength less than 10N

[0085] <Warping> The anticorrosive laminate film was cut into strips measuring 100 mm x 200 mm to prepare test pieces, which were then left in environmental testers at 10°C / 20% and 45°C / 80% for 10 minutes, after which the warping state of the test pieces was observed and evaluated according to the following criteria. ○: The edge of the test piece film is less than 10 mm lifted from the horizontal due to warping. △: The edge of the test piece film is lifted by 10 mm or more but less than 20 mm due to warping from the horizontal. ×: The edge of the test piece film is lifted by 20 mm or more from the horizontal due to warping.

[0086] <Peel strength> The anticorrosion tape was attached to a SUS430 plate that had previously been coated with an isocyanate-based primer, and the 180°C peel strength was measured for each of the samples after they had been left for 24 hours at 23°C, 50% humidity (initial) and after they had been conditioned for 20 hours at 45°C, 75% humidity and then left for 48 hours at 23°C, 50% humidity (after humidity curing), and the humidity curing properties were evaluated. Specifically, test pieces cut into 15 mm wide strips were used from each sample, and the 180° peel strength of the interface between the SUS plate and the adhesive side of the corrosion protection tape was measured using an Orientec tensile testing machine "STA1225" at a tensile speed of 50 mm / min, peeling for 1 cm, and the maximum load during peeling was recorded as the peel strength.

[0087] The peel strength as an anticorrosive tape was judged according to the following criteria based on the measured values ​​of the initial peel strength and the peel strength after humidity curing. ○: The value obtained by dividing the peel strength after humidity curing by the initial peel strength is more than 1.2 times ×: Does not meet the above requirements

[0088] <Overall rating> The overall evaluation was based on the following criteria: ◯: The puncture strength, warpage and peel strength are all evaluated as "◯". △: Any one of the puncture strength, warping, and peel strength is △, but it is still at a practical level. ×: Any one of the puncture strength, warping, and peel strength is marked "×".

[0089] [Physical properties of resin] In the examples and comparative examples, the properties of the resins used in the high elasticity resin layer and the low elasticity resin layer are as shown in Table 1 below.

[0090] [Table 1]

[0091] [Materials of each layer] The constituent materials of each layer used in the production of the anticorrosive laminate film and anticorrosive tape in the Examples and Comparative Examples are as follows.

[0092] <High elasticity resin layer> Ny-15: Biaxially oriented polyamide (Ny) film produced by the tubular method (thickness: 15 μm, tensile modulus: 2300 MPa, surface roughness Ra: 0.04 μm, both sides corona treated) Ny-25: Biaxially oriented polyamide (Ny) film produced by the tubular method (thickness: 25 μm, tensile modulus: 2300 MPa, surface roughness Ra: 0.04 μm, both sides corona treated) PET-25: Biaxially oriented polyethylene terephthalate (PET) film produced by the T-die method (thickness: 25 μm, tensile modulus: 4500 MPa, surface roughness Ra: 0.05 μm, both sides corona treated) PBT-15: Biaxially oriented polybutylene terephthalate (PBT) film produced by the tubular method (thickness: 15 μm, tensile modulus: 2400 MPa, surface roughness Ra: 0.03 μm, double-sided corona treatment product)

[0093] <Metal foil> AL-40: 40μm thick JIS A8079H-O material (soft aluminum foil containing 1.0% iron by weight) with boehmite treatment on both sides The boehmite treatment was carried out by immersing the aluminum foil in boehmite treatment water (deionized water with 0.5% by weight of triethanolamine added) at 95°C for 1 minute to form a boehmite needle crystal film with a thickness of 0.25 μm. The contact angle of the film surface with water was 15°. AL-35: 35μm thick JIS A8021H-O material (soft aluminum foil containing 1.5% iron by weight) with boehmite treatment on both sides The boehmite treatment was carried out by immersing the aluminum foil in boehmite treatment water (deionized water with triethanolamine added at a concentration of 0.5 wt%) at 95°C for 40 seconds to form a boehmite needle crystal film with a thickness of 0.2 μm. The contact angle of the film surface with water was 15°. AL-25: Untreated JIS 1N30H-O material (soft aluminum foil containing 0.4% by weight of iron) with a thickness of 25 μm. The contact angle of the untreated surface with water was 90°. AL-15: Untreated JIS 8021H-O material (soft aluminum foil containing 1.3% by weight of iron) with a thickness of 15 μm. The contact angle of the untreated surface with water was 90°. AL-9: Untreated JIS 8021H-O material (soft aluminum foil containing 1.3% by weight of iron) with a thickness of 9 μm. The contact angle of the untreated surface with water was 90°.

[0094] <Low elasticity resin layer> LLPE-30: A film made by blown film extrusion using a dry blend of 95% LLPE and 5% LDPE (thickness: 30 μm, tensile modulus: 450 MPa, both sides plasma treated, water contact angle of plasma treated surface: 80°) PEE-25: Polyester elastomer (PEE) extruded through a T-die and biaxially stretched film (thickness: 25 μm, tensile modulus: 1300 MPa, surface roughness Ra: 0.05 μm, both sides corona treated)

[0095] <Low elasticity resin layer with adhesive layer> Laminated LLPE-50: A two-layer film made by co-extrusion inflation molding of a dry blend of 95% LLPE and 5% LDPE and acid-modified LLPE (total thickness: 50 μm, acid-modified LLPE layer (adhesive layer) thickness: 20 μm, LLPE layer thickness: 30 μm, tensile modulus of LLPE layer: 450 MPa, LLPE layer side plasma-treated, water contact angle of plasma-treated surface: 80°, surface roughness Ra: 0.3 μm) Laminated LLPE-30: A two-layer film made by co-extrusion inflation molding of a dry blend of 95% LLPE and 5% LDPE and acid-modified LLPE (total thickness: 30 μm, acid-modified LLPE layer (adhesive layer) thickness: 10 μm, LLPE layer thickness: 20 μm, tensile modulus of LLPE layer: 450 MPa, LLPE layer side plasma-treated, water contact angle of plasma-treated surface: 80°, surface roughness Ra: 0.3 μm)

[0096] <Adhesive layer> Adhesive (4): A layer of a two-part dry lamination adhesive made of aromatic polyester and polyisocyanate, applied to a thickness of 4 μm and dried.

[0097] <Double-sided tape> Double-sided tape A: Double-sided tape made of 0.25 mm thick acrylic foam impregnated with acrylic adhesive (3M VHB tape, product name Y4914, tensile modulus: 10 MPa or less) Double-sided tape B: Double-sided tape made of 0.4 mm thick acrylic foam impregnated with acrylic adhesive (3M VHB tape, product name Y4920, tensile modulus: 10 MPa or less)

[0098] [Example 1] As the highly elastic resin layer, Ny-15 was used, and it was attached to both sides of the AL-25 via an adhesive (4) by dry lamination. Next, LLPE-30 was used as a low-elasticity resin layer, and laminated to each Ny-15 surface by dry lamination using an adhesive (4) to obtain a 9-layer multilayer film (total thickness: 131 μm) of anticorrosive laminate film. The anticorrosive laminate film was evaluated for ejection strength and warpage. Double-sided tape A was applied to this to make an anticorrosive tape, and the humidity curing property was evaluated. The results are shown in Table 2.

[0099] [Example 2] As the highly elastic resin layer, Ny-15 was used, and it was attached to both sides of the AL-9 via an adhesive (4) by dry lamination. Next, LLPE-30 was used as a low-elasticity resin layer, and laminated to each Ny-15 surface by dry lamination using an adhesive (4) to obtain a 9-layer multilayer film (total thickness: 115 μm) anticorrosive laminate film. The anticorrosive laminate film was evaluated for ejection strength and warpage. Double-sided tape A was applied to this to make an anticorrosive tape, and the humidity curing property was evaluated. The results are shown in Table 2.

[0100] [Example 3] Ny-15 was used as the highly elastic resin layer, and it was attached to both sides of AL-25 by dry lamination using an adhesive (4) to obtain a five-layered anticorrosive laminate film (total thickness: 63 μm). The anticorrosive laminate film was evaluated for ejection strength and warpage. Double-sided tape B was applied to this to make an anticorrosive tape, and the humidity curing property was evaluated. The results are shown in Table 2.

[0101] [Example 4] Ny-15 was used as the highly elastic resin layer, and it was attached to both sides of AL-9 by dry lamination using an adhesive (4) to obtain a five-layered anticorrosive laminate film (total thickness: 47 μm). The anticorrosive laminate film was evaluated for ejection strength and warpage. Double-sided tape B was applied to this to make an anticorrosive tape, and the humidity curing property was evaluated. The results are shown in Table 2.

[0102] [Example 5] As the highly elastic resin layer, Ny-25 was used, and Ny-25 was attached to one side of AL-25 via an adhesive (4) by dry lamination. The acid-modified LLPE layer side of the laminated LLPE-30 was laminated to the opposite side of the AL-25 (the side not bonded with Ny-25) by thermal lamination to obtain a five-layer multilayer film (total thickness: 84 μm) as a corrosion-resistant laminate film. The anticorrosive laminate film was evaluated for ejection strength and warpage. Double-sided tape B was applied to the laminated LLPE-30 side to create an anticorrosive tape, and the humidity curing properties were evaluated. The results are shown in Table 2.

[0103] [Example 6] As the highly elastic resin layer, Ny-25 was used, and Ny-25 was attached to one side of AL-35 via an adhesive (4) by dry lamination. The acid-modified LLPE layer side of the laminated LLPE-50 was laminated to the opposite side of the AL-35 (the side not bonded with Ny-25) by thermal lamination to obtain a five-layer multilayer film (total thickness: 114 μm) as a corrosion-resistant laminate film. The anticorrosive laminate film was evaluated for ejection strength and warpage. Double-sided tape A was applied to the laminated LLPE-50 side to create an anticorrosive tape, and the humidity curing property was evaluated. The results are shown in Table 2.

[0104] [Example 7] As the highly elastic resin layer, Ny-25 was used, and Ny-25 was attached to one side of AL-40 via an adhesive (4) by dry lamination. The acid-modified LLPE layer side of the laminated LLPE-50 was laminated to the opposite side of the AL-40 (the side not coated with Ny-25) by thermal lamination to obtain a five-layer multilayer film (total thickness: 119 μm) as a corrosion-resistant laminate film. The anticorrosive laminate film was evaluated for ejection strength and warpage. Double-sided tape A was applied to the laminated LLPE-50 side to create an anticorrosive tape, and the humidity curing property was evaluated. The results are shown in Table 2.

[0105] [Example 8] PET-25 was used as the highly elastic resin layer, and was attached to both sides of the AL-15 via an adhesive (4) by dry lamination. Next, LLPE-30 was used as a low-elasticity resin layer, and laminated to each PET-25 surface via an adhesive (4) by dry lamination to obtain a 9-layered anticorrosive laminate film (total thickness: 141 μm). The anticorrosive laminate film was evaluated for ejection strength and warpage. Double-sided tape A was applied to this to make an anticorrosive tape, and the humidity curing property was evaluated. The results are shown in Table 2.

[0106] [Example 9] As the highly elastic resin layer, PBT-15 was used, and it was attached to both sides of the AL-15 via an adhesive (4) by dry lamination. Next, LLPE-30 was used as a low-elasticity resin layer, and laminated to each PBT-15 surface via an adhesive (4) by dry lamination to obtain a 9-layered anticorrosive laminate film (total thickness: 121 μm). The anticorrosive laminate film was evaluated for ejection strength and warpage. Double-sided tape A was applied to this to make an anticorrosive tape, and the humidity curing property was evaluated. The results are shown in Table 2.

[0107] [Example 10] As the highly elastic resin layer, PBT-15 was used, and the PBT-15 was attached to one side of the AL-15 via an adhesive (4) by dry lamination. LLPE-30 was laminated to the opposite surface of AL-15 (the surface not bonded with PBT-15) via an adhesive (4) by dry lamination to obtain a five-layer multilayer film (total thickness: 68 μm) as a corrosion-resistant laminate film. The anticorrosive laminate film was evaluated for ejection strength and warpage. Double-sided tape B was applied to the LLPE-30 side to create an anticorrosive tape, and the humidity curing properties were evaluated. The results are shown in Table 2.

[0108] [Comparative Example 1] Instead of using a high-elasticity resin layer, laminated LLPE-30 was used as a low-elasticity resin layer, and the acid-modified LLPE layer side was bonded to both sides of AL-15 by thermal lamination to obtain a five-layer multilayer film (total thickness: 75 μm) as a corrosion-resistant laminate film. The anticorrosive laminate film was evaluated for ejection strength and warpage. Double-sided tape B was applied to this to make an anticorrosive tape, and the humidity curing property was evaluated. The results are shown in Table 2.

[0109] [Comparative Example 2] Instead of using a high-elasticity resin layer, laminated LLPE-50 was used as a low-elasticity resin layer, and the acid-modified LLPE layer side was bonded to both sides of AL-25 by thermal lamination to obtain a five-layer multilayer film (total thickness: 125 μm) as a corrosion-resistant laminate film. The anticorrosive laminate film was evaluated for ejection strength and warpage. Double-sided tape A was applied to this to make an anticorrosive tape, and the humidity curing property was evaluated. The results are shown in Table 2.

[0110] [Comparative Example 3] The low elasticity resin layer was made of PEE-25, and was attached to one side of the AL-15 via an adhesive (4). Next, laminated LLPE-30 was used as a low-elasticity resin layer, and the acid-modified LLPE layer side was bonded to the opposite side of AL-15 (the side not bonded with PEE-25) by thermal lamination to obtain a five-layer multilayer film (total thickness: 74 μm) as a corrosion-resistant laminate film. The anticorrosive laminate film was evaluated for ejection strength and warpage. Double-sided tape B was applied to the laminated LLPE-30 side to create an anticorrosive tape, and the humidity curing properties were evaluated. The results are shown in Table 2.

[0111] [Table 2]

[0112] [Consideration] From Table 2, we can see the following: In Examples 1 to 4, by attaching polyamide films to both sides of the metal foil as the highly elastic resin layer defined in the present invention, even if the metal foil is thin, the swelling property of the resin due to humidity change is the same on both sides, so that a film that does not warp can be obtained, and an anticorrosive laminate film with very high puncture strength can be obtained. The anticorrosive laminate film has excellent workability without warping under any temperature and humidity working environment, and has high durability and waterproofness. It can be seen that Examples 1 to 4 are particularly high in puncture strength, and the film does not warp under low temperature and low humidity to high temperature and high humidity environments, and has high workability.

[0113] In Examples 5, 6, and 7, a polyamide film was attached to only one side of the metal foil as a highly elastic resin layer, but by making the metal foil thicker, the puncture strength was high and the film did not warp in low temperature and low humidity to high temperature and high humidity environments. However, by making the metal foil thicker, the rigidity increased, and although there were some difficulties in workability and application, it was fully usable as a corrosion prevention laminate film.

[0114] In Examples 8, 9, and 10, a polyethylene terephthalate film or a polybutylene terephthalate film other than a polyamide film was attached to one or both sides of the metal foil as a highly elastic resin layer, and the film did not warp in a low temperature and low humidity to a high temperature and high humidity environment. The puncture strength was inferior to Examples 1 to 4 using a polyamide film, but it was at a level sufficient for practical use as an anticorrosive laminate film.

[0115] In contrast, Comparative Examples 1 and 2, which do not use a highly elastic resin layer, have low puncture strength and are inferior in long-term durability. In Comparative Example 3, a biaxially oriented polyester elastomer film was used as the low elasticity resin layer, but since the tensile modulus was low, the puncture strength was low and durability as an anticorrosive laminate film was not obtained. [Explanation of symbols]

[0116] 1(1a,1b) High elastic resin layer 2(2a,2b,2c,2d) Adhesive layer 3 Metal foil 4(4a,4b) Low elasticity resin layer 5 Double-sided tape 6 Release paper or release film 10(10A, 10B, 10C) Anticorrosive laminate film 20(20A,20B,20C) Anticorrosive tape

Claims

1. A laminate film for corrosion protection of steel materials, comprising a metal foil and a highly elastic resin layer laminated to at least one side of the metal foil via an adhesive.

2. The anticorrosive laminate film according to claim 1, wherein the highly elastic resin layer is made of a biaxially oriented film having a thickness of 5 to 50 μm and a tensile modulus of elasticity of 1500 to 5000 MPa, and the metal foil is an aluminum foil having a thickness of 6 to 60 μm.

3. 3. The anticorrosive laminate film according to claim 2, wherein the biaxially oriented film is a biaxially oriented polyamide film.

4. The anticorrosive laminate film according to any one of claims 1 to 3, further comprising a low elasticity resin layer.

5. 5. The anticorrosive laminate film according to claim 4, further comprising a low elasticity resin layer on a surface of the high elasticity resin layer opposite to the metal foil.

6. The low elasticity resin layer is mainly composed of a polyethylene resin, has an MFR of 0.1 to 20 g / 10 min, and a density of 0.91 to 0.960 g / cm 3 6. The anticorrosive laminate film according to claim 4 or 5, having a tensile modulus of elasticity of 100 MPa or more and less than 1500 MPa.

7. 7. An anticorrosion tape comprising the anticorrosive laminate film according to claim 1 and a double-sided tape attached thereto.

8. 7. An anticorrosion tape comprising the anticorrosive laminate film according to claim 1 and a double-sided tape comprising an acrylic foam impregnated with an acrylic adhesive attached thereto.

Citation Information

Patent Citations

  • Method for preventing corrosion in deteriorated environmental part of steel structure

    JP2001081584A

  • Resin laminated film excellent in stiffness strength and impact resistance

    JP2001277408A

  • Corrosion preventive method of steel structure, corrosion preventive sheet, and corrosion-proof steel structure

    JP2004244652A

  • Covering material of steel structure

    JP2006225573A

  • Heat shrinkable polyolefinic laminated film, heat shrinkable label, and container carrying the label

    JP2006272775A