Substrate processing method and substrate processing apparatus

The substrate processing method uses laser-induced modified layers to efficiently thin and edge-trim semiconductor wafers, addressing the inefficiencies and costs of conventional grinding methods while ensuring high-quality results.

JP2024163275AActive Publication Date: 2024-11-21TOKYO ELECTRON LTD
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
JP2024157335
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2018-12-21
Filing Date
2024-09-11
Publication Date
2024-11-21
Estimated Expiration
2039-12-09

AI Technical Summary

Technical Problem

Conventional methods for thinning semiconductor wafers and edge trimming require frequent replacement of grinding tools, use large amounts of grinding water, and incur significant running costs due to waste water treatment, while also risking wafer damage from sharp edges.

Method used

A substrate processing method involving laser irradiation to form peripheral and internal modified layers in a polymerized substrate, allowing for precise removal of the wafer edge and thinning without the need for grinding, reducing consumables and water usage.

Benefits of technology

The method efficiently performs wafer thinning and edge trimming with reduced maintenance and running costs, ensuring high-quality processing by minimizing wafer damage and environmental impact.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024163275000001_ABST
    Figure 2024163275000001_ABST
Patent Text Reader

Abstract

To form a peripheral modification layer in an appropriate position in a polymerized substrate where substrates are bonded together.SOLUTION: A substrate processing method for processing a substrate has a step for holding a second substrate in a polymerized substrate in which the first and second substrates are bonded, and a step for irradiating the boundary between the periphery and the center of a removal target inside the first substrate with a laser beam for the periphery to form a periphery modification layer, and the polymerized substrate has a bonded area where the surface of the first substrate and the surface of the second substrate are bonded and an unbonded area that is the area radially outside the outer edge of the bonded area, and in forming the peripheral modification layer, the laser beam for the periphery is irradiated so that the distance between the peripheral modification layer and the outer edge of the bonded area is within 500 μm.SELECTED DRAWING: Figure 4
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a substrate processing method and a substrate processing apparatus. [Background technology]

[0002] Patent Document 1 discloses a method for manufacturing a stacked semiconductor device. In this manufacturing method, two or more semiconductor wafers are stacked to manufacture a stacked semiconductor device. At this time, each semiconductor wafer is stacked on another semiconductor wafer, and then the back surface of the semiconductor wafer is ground to a desired thickness.

[0003] Patent Document 2 discloses a method of grinding the peripheral edge of a semiconductor wafer into a substantially L-shape by rotating a disk-shaped grinding tool having abrasive grains on its outer periphery and bringing at least the outer periphery of the grinding tool into linear contact with the semiconductor wafer. The semiconductor wafer is made by bonding two silicon wafers together. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2012-69736 A [Patent Document 2] Japanese Patent Application Publication No. 9-216152 Summary of the Invention [Problem to be solved by the invention]

[0005] The technology according to the present disclosure forms a peripheral modification layer at an appropriate position in a laminated substrate in which substrates are bonded together. [Means for solving the problem]

[0006] One aspect of the present disclosure is a substrate processing method for processing a substrate, comprising: holding the second substrate in a laminated substrate in which a first substrate and a second substrate are bonded; and irradiating a peripheral laser beam into the inside of the first substrate along a boundary between a peripheral portion to be removed and a central portion to form a peripheral modified layer, wherein the laminated substrate has a bonded region where a surface of the first substrate and a surface of the second substrate are bonded, and an unbonded region that is a region radially outward from an outer end of the bonded region, and in forming the peripheral modified layer, the peripheral laser beam is irradiated so that a distance between the peripheral modified layer and the outer end of the bonded region is within 500 μm. Effect of the Invention

[0007] According to the present disclosure, a peripheral modification layer can be formed at an appropriate position in a laminated substrate in which substrates are bonded together. [Brief description of the drawings]

[0008] [Figure 1] 1 is a plan view showing a schematic configuration of a wafer processing system according to an embodiment of the present invention; [Diagram 2] FIG. 2 is a side view showing an outline of a configuration of an overlapping wafer. [Diagram 3] FIG. 2 is a side view showing an outline of a configuration of a portion of the overlapping wafer. [Figure 4] FIG. 2 is a plan view showing the outline of the configuration of the reformer. [Diagram 5] FIG. 2 is a side view showing the outline of the configuration of a reformer. [Figure 6] FIG. 2 is a plan view showing an outline of the configuration of a peripheral edge removing device. [Figure 7] FIG. 2 is a side view showing an outline of the configuration of the edge removing device. [Figure 8] FIG. 2 is a vertical cross-sectional view showing an outline of the configuration of a transfer arm. [Figure 9] FIG. 2 is a flow diagram showing main steps of wafer processing according to the first embodiment. [Figure 10] 1A to 1C are explanatory views of main steps of wafer processing according to a first embodiment. [Figure 11]FIG. 2 is an explanatory diagram of main steps of the modification treatment. [Figure 12] 1A to 1C are explanatory views showing a state in which a peripheral modified layer is formed on a processing wafer. [Figure 13] 10 is an explanatory diagram showing a state in which a peripheral modified layer is formed on a processing wafer. FIG. [Figure 14] 1A to 1C are explanatory views showing a state in which divided modified layers are formed on a processing wafer. [Figure 15] 10 is an explanatory diagram showing a state in which divided modified layers are formed on a processing wafer. FIG. [Figure 16] 1A to 1C are explanatory diagrams showing a state in which an internal surface modification layer is formed on a processing wafer. [Figure 17] 1A to 1C are explanatory diagrams showing a state in which an internal surface modification layer is formed on a processing wafer. [Figure 18] FIG. 11 is an explanatory diagram showing a state in which a peripheral portion is removed. [Figure 19] FIG. 13 is an explanatory diagram showing a state in which the back surface wafer is separated from the processing wafer. [Figure 20] FIG. 11 is a side view showing an outline of the configuration of a peripheral edge removing device according to another embodiment. [Figure 21] FIG. 11 is a plan view showing the outline of the configuration of a reformer according to another embodiment. [Figure 22] FIG. 11 is a plan view showing the outline of the configuration of a reformer according to another embodiment. [Figure 23] 6A to 6C are explanatory views of main steps of wafer processing according to a modified example of the first embodiment. [Figure 24] FIG. 11 is a flow diagram showing main steps of a wafer processing according to a second embodiment. [Diagram 25] 10A to 10C are explanatory views of main steps of a wafer processing according to a second embodiment. [Figure 26] 13 is an explanatory view showing a state in which the back surface wafer is separated from the processing wafer in the second embodiment. FIG. [Figure 27] FIG. 2 is a side view showing an outline of the configuration of a removal and separation device. [Figure 28] FIG. 11 is a flow diagram showing main steps of a wafer processing according to a third embodiment. [Figure 29]11A to 11C are explanatory views of main steps of wafer processing according to a third embodiment. [Diagram 30] FIG. 11 is a vertical cross-sectional view showing an outline of the configuration of a transfer arm according to another embodiment. [Diagram 31] 13 is a longitudinal sectional view showing the outline of the configuration of the peripheral portion of an attraction plate according to another embodiment. FIG. [Diagram 32] 13 is an explanatory diagram showing a state in which a peripheral portion is removed in a transfer arm according to another embodiment. FIG. [Diagram 33] FIG. 11 is a plan view showing the outline of the configuration of a reformer according to another embodiment. [Diagram 34] 10A to 10C are explanatory views showing a state in which a peripheral modified layer is formed on a processing wafer in another embodiment. [Diagram 35] 10A to 10C are explanatory views showing a state in which an internal surface modification layer is formed on a processing wafer in another embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] In the manufacturing process of semiconductor devices, for example, as disclosed in Patent Document 1, a semiconductor wafer (hereinafter referred to as "wafer") having a plurality of electronic circuits and other devices formed on its surface is thinned by grinding the back surface of the wafer.

[0010] The grinding process of the back surface of the wafer is performed, for example, by rotating the wafer and the grinding wheel while the grinding wheel is in contact with the back surface and then lowering the grinding wheel. In such a case, the grinding wheel wears out and needs to be replaced periodically. In addition, grinding water is used in the grinding process, and waste liquid treatment is also required. For this reason, the conventional wafer thinning process is expensive to run.

[0011] In addition, the peripheral edge of the wafer is usually chamfered, but when the back surface of the wafer is ground as described above, the peripheral edge of the wafer becomes sharp (so-called knife-edge shape). This can cause chipping at the peripheral edge of the wafer, which can damage the wafer. Therefore, so-called edge trimming is performed to remove the peripheral edge of the wafer before grinding.

[0012] The end face grinding device described in the above-mentioned Patent Document 2 is a device that performs this edge trimming. However, in this end face grinding device, since edge trimming is performed by grinding, the grinding wheel wears out and needs to be replaced periodically. In addition, a large amount of grinding water is used, and waste liquid treatment is also required. For this reason, conventional edge trimming requires high running costs.

[0013] The technology disclosed herein efficiently performs pre-processing for wafer thinning and edge trimming. Hereinafter, a wafer processing system as a substrate processing apparatus and a wafer processing method as a substrate processing method according to the present embodiment will be described with reference to the drawings. In this specification and the drawings, elements having substantially the same functional configurations are denoted by the same reference numerals, and duplicated descriptions will be omitted.

[0014] First, the configuration of a wafer processing system according to this embodiment will be described.

[0015] In the wafer processing system 1, a predetermined process is performed on an overlapped wafer T, which is an overlapped substrate in which a process wafer W as a first substrate and a support wafer S as a second substrate are bonded together, as shown in Figures 2 and 3. In the wafer processing system 1, a peripheral portion We of the process wafer W is removed, and the process wafer W is further thinned. Hereinafter, the surface of the process wafer W bonded to the support wafer S is referred to as the front surface Wa, and the surface opposite to the front surface Wa is referred to as the back surface Wb. Similarly, the surface of the support wafer S bonded to the process wafer W is referred to as the front surface Sa, and the surface opposite to the front surface Sa is referred to as the back surface Sb.

[0016] The processing wafer W is a semiconductor wafer such as a silicon wafer, and has a device layer (not shown) including a plurality of devices formed on its surface Wa. An oxide film F, such as a SiO2 film (TEOS film), is further formed on the device layer. The peripheral portion We of the processing wafer W is chamfered, and the cross section of the peripheral portion We becomes thinner toward its tip. The peripheral portion We is a portion to be removed in edge trimming, and is, for example, in the range of 1 mm to 5 mm in the radial direction from the outer end of the processing wafer W.

[0017] In order to avoid complication of the drawing, the oxide film F is omitted in Fig. 2. Similarly, in other drawings used in the following description, the oxide film F may be omitted in some cases.

[0018] The support wafer S is a wafer that supports the process wafer W, and is, for example, a silicon wafer. An oxide film (not shown) is formed on the surface Sa of the support wafer S. The support wafer S also functions as a protective material that protects devices on the surface Wa of the process wafer W. When multiple devices are formed on the surface Sa of the support wafer S, a device layer (not shown) is formed on the surface Sa in the same manner as the process wafer W.

[0019] Here, if the processing wafer W and the support wafer S are bonded at the peripheral portion We of the processing wafer W, there is a risk that the peripheral portion We cannot be properly removed. Therefore, at the interface between the processing wafer W and the support wafer S, a bonding region Aa where the oxide film F and the surface Sa of the support wafer S are bonded, and an unbonded region Ab which is an area radially outside the bonding region Aa are formed. The presence of the unbonded region Ab in this way allows the peripheral portion We to be properly removed. Note that, as will be described in detail later, it is preferable that the outer end of the bonding region Aa is positioned slightly radially outside the inner end of the peripheral portion We to be removed.

[0020] 1, the wafer processing system 1 has a configuration in which a loading / unloading station 2 and a processing station 3 are integrally connected. The loading / unloading station 2 loads / unloads a cassette Ct capable of accommodating a plurality of overlapped wafers T, for example, between the outside and the loading / unloading station 2. The processing station 3 includes various processing devices that perform predetermined processing on the overlapped wafers T.

[0021] The loading / unloading station 2 is provided with a cassette mounting table 10. In the illustrated example, a plurality of cassettes Ct, for example, three cassettes Ct, can be freely mounted in a line in the Y-axis direction on the cassette mounting table 10. The number of cassettes Ct mounted on the cassette mounting table 10 is not limited to the present embodiment and can be determined arbitrarily.

[0022] In the carry-in / out station 2, a wafer transfer device 20 is provided adjacent to the cassette mounting table 10 on the X-axis negative side of the cassette mounting table 10. The wafer transfer device 20 is configured to be movable on a transfer path 21 extending in the Y-axis direction. The wafer transfer device 20 has, for example, two transfer arms 22, 22 for holding and transferring the overlapped wafer T. Each transfer arm 22 is configured to be movable in the horizontal direction, the vertical direction, around the horizontal axis, and around the vertical axis. The configuration of the transfer arm 22 is not limited to this embodiment, and may have any configuration. The wafer transfer device 20 is configured to be able to transfer the overlapped wafer T to the cassette Ct on the cassette mounting table 10 and a transition device 30 described later.

[0023] In the carry-in / out station 2, a transition device 30 for transferring the overlapped wafer T is provided adjacent to the wafer transfer device 20 on the negative X-axis direction side of the wafer transfer device 20.

[0024] For example, three processing blocks G1 to G3 are provided in the processing station 3. The first processing block G1, the second processing block G2, and the third processing block G3 are arranged in this order from the positive side of the X-axis (the load / unload station 2 side) to the negative side.

[0025] The first processing block G1 is provided with an etching device 40, a cleaning device 41, and a wafer transport device 50. The etching device 40 and the cleaning device 41 are arranged in a stacked manner. The number and arrangement of the etching devices 40 and the cleaning devices 41 are not limited to this. For example, the etching devices 40 and the cleaning devices 41 may each extend in the X-axis direction and be placed in parallel in a plan view. Furthermore, the etching devices 40 and the cleaning devices 41 may each be stacked.

[0026] The etching device 40 etches the back surface Wb of the processing wafer W ground by the processing device 80 described later. For example, a chemical solution (etchant) is supplied to the back surface Wb to wet-etch the back surface Wb. For example, HF, HNO3, H3PO4, TMAH, Choline, KOH, etc. are used as the chemical solution.

[0027] The cleaning device 41 cleans the back surface Wb of the processing wafer W ground by the processing device 80 described below. For example, a brush is brought into contact with the back surface Wb to scrub the back surface Wb. Note that a pressurized cleaning liquid may be used to clean the back surface Wb. The cleaning device 41 may also be configured to clean the back surface Sb of the support wafer S as well as the back surface Wb of the processing wafer W.

[0028] The wafer transport device 50 is disposed, for example, on the negative side of the Y axis with respect to the etching device 40 and the cleaning device 41. The wafer transport device 50 has, for example, two transport arms 51, 51 that hold and transport the overlapped wafer T. Each transport arm 51 is configured to be movable horizontally, vertically, around a horizontal axis, and around a vertical axis. Note that the configuration of the transport arm 51 is not limited to this embodiment, and any configuration may be used. The wafer transport device 50 is configured to be able to transport the overlapped wafer T to the transition device 30, the etching device 40, the cleaning device 41, and a modification device 60 described later.

[0029] The second processing block G2 is provided with a modifying device 60, an edge removing device 61, and a wafer transport device 70. The modifying device 60 and the edge removing device 61 are arranged in a stacked manner. Note that the number and arrangement of the modifying devices 60 and the edge removing devices 61 are not limited to this.

[0030] The modifying device 60 irradiates the inside of the processing wafer W with laser light to form a peripheral modified layer, a divided modified layer, and an inner surface modified layer. A specific configuration of the modifying device 60 will be described later.

[0031] The edge removing device 61 removes the edge portion We of the processing wafer W, starting from the edge modified layer formed by the modifying device 60. The specific configuration of the edge removing device 61 will be described later.

[0032] The wafer transport device 70 is disposed, for example, on the Y-axis positive side with respect to the modification device 60 and the edge removal device 61. The wafer transport device 70 has, for example, two transport arms 71, 71 that hold and transport the overlapped wafer T. Each transport arm 71 is supported by an articulated arm member 72 and configured to be movable horizontally, vertically, around a horizontal axis, and around a vertical axis. The specific configuration of the transport arm 71 will be described later. The wafer transport device 70 is configured to be able to transport the overlapped wafer T to the cleaning device 41, the modification device 60, the edge removal device 61, and a processing device 80 described later.

[0033] The third processing block G3 is provided with a processing device 80. The number and arrangement of the processing devices 80 are not limited to those in this embodiment, and a plurality of processing devices 80 may be arranged arbitrarily.

[0034] The processing device 80 grinds the back surface Wb of the processing wafer W. Then, in the back surface Wb on which the internal surface modification layer is formed, the internal surface modification layer is removed, and further the peripheral modification layer is removed. Specifically, the processing device 80 rotates the processing wafer W and the grinding wheel (not shown) while the back surface Wb of the processing wafer W held by the chuck 81 is in contact with the grinding wheel (not shown), and grinds the back surface Wb. In this embodiment, the chuck 81 and the grinding wheel (not shown) constitute a processing unit. In addition, a known grinding device (polishing device) is used for the processing device 80, and for example, a device described in JP 2010-69601 A is used.

[0035] The above-described wafer processing system 1 is provided with a control device 90. The control device 90 is, for example, a computer, and has a program storage unit (not shown). The program storage unit stores a program for controlling the processing of the laminated wafer T in the wafer processing system 1. The program storage unit also stores a program for controlling the operation of the drive systems of the above-described various processing devices and transport devices, and for realizing the substrate processing described below in the wafer processing system 1. The above-described program may be recorded in a computer-readable storage medium H and installed in the control device 90 from the storage medium H.

[0036] Next, the above-mentioned reformer 60 will be described. Fig. 4 is a plan view showing an outline of the configuration of the reformer 60. Fig. 5 is a side view showing an outline of the configuration of the reformer 60.

[0037] The modification device 60 has a chuck 100 as a substrate holding part that holds the overlapped wafer T on the upper surface. The chuck 100 holds the support wafer S by suction with the process wafer W on the upper side and the support wafer S on the lower side. The chuck 100 is supported by a slider table 102 via an air bearing 101. A rotating part 103 is provided on the lower surface side of the slider table 102. The rotating part 103 has a built-in motor as a driving source. The chuck 100 is configured to be rotatable around a vertical axis by the rotating part 103 via the air bearing 101. The slider table 102 is configured to be movable along a rail 105 that is provided on a base 106 and extends in the Y-axis direction by a horizontal moving part 104 provided on the lower surface side of the slider table 102. The driving source of the horizontal moving part 104 is not particularly limited, but a linear motor is used, for example.

[0038] A laser head 110 is provided above the chuck 100. The laser head 110 has a lens 111. The lens 111 is a cylindrical member provided on the lower surface of the laser head 110, and irradiates the processing wafer W held by the chuck 100 with laser light. In this embodiment, the peripheral modification unit and the internal surface modification unit have a common laser head 110.

[0039] The laser head 110 further includes an LCOS (Liquid Crystal on Silicon) (not shown). The LCOS is a spatial light modulator that modulates and outputs the laser light. Specifically, the LCOS can control the focal position and phase of the laser light, and can adjust the shape and number (number of branches) of the laser light irradiated onto the processing wafer W.

[0040] The laser head 110 focuses and irradiates a predetermined position inside the processing wafer W with high-frequency pulsed laser light oscillated from a laser light oscillator (not shown) and having a wavelength that is transparent to the processing wafer W. As a result, the portion inside the processing wafer W where the laser light is focused is modified, and a peripheral modified layer, a divided modified layer, and an internal surface modified layer are formed.

[0041] The laser head 110 is supported by a support member 120. The laser head 110 is configured to be movable up and down by an elevating mechanism 130 along a rail 121 extending in the vertical direction. The laser head 110 is also configured to be movable in the Y-axis direction by a moving mechanism 131. The elevating mechanism 130 and the moving mechanism 131 are each supported by a support column 132.

[0042] A macro camera 140 and a micro camera 150 are provided above the chuck 100 on the Y-axis positive side of the laser head 110. For example, the macro camera 140 and the micro camera 150 are integrally configured, and the macro camera 140 is disposed on the Y-axis positive side of the micro camera 150. The macro camera 140 and the micro camera 150 are configured to be able to move up and down by an elevating mechanism 160, and further configured to be able to move in the Y-axis direction by a moving mechanism 161.

[0043] The macro camera 140 captures an image of the outer edge of the processing wafer W (polymerized wafer T). The macro camera 140 includes, for example, a coaxial lens, emits visible light, for example, red light, and receives reflected light from an object. For example, the imaging magnification of the macro camera 140 is 2x.

[0044] The micro camera 150 captures an image of the peripheral portion of the processing wafer W, and captures an image of the boundary between the bonded area Aa and the unbonded area Ab. The micro camera 150 is equipped with, for example, a coaxial lens, irradiates infrared light (IR light), and receives reflected light from an object. For example, the imaging magnification of the micro camera 150 is 10 times, the field of view is about 1 / 5 of that of the macro camera 140, and the pixel size is about 1 / 5 of that of the macro camera 140.

[0045] Next, the above-mentioned peripheral edge removing device 61 will be described. Fig. 6 is a plan view showing an outline of the configuration of the peripheral edge removing device 61. Fig. 7 is a side view showing an outline of the configuration of the peripheral edge removing device 61.

[0046] The edge removing device 61 has a chuck 170 as another substrate holding part that holds the overlapped wafer T on the upper surface. The chuck 170 adsorbs and holds the support wafer S in a state in which the process wafer W is arranged on the upper side and the support wafer S is arranged on the lower side. The chuck 170 is configured to be rotatable about a vertical axis by a rotation mechanism 171.

[0047] A pad 180 is provided above the chuck 170 as a peripheral edge removal unit that holds and transfers the peripheral edge We of the processing wafer W. A suction mechanism (not shown), such as a vacuum pump, is connected to the pad 180, and the pad 180 holds the peripheral edge We by suction on its lower surface. The pad 180 is provided with a lifting mechanism 181 that lifts and lowers the pad 180 in the vertical direction, and a moving mechanism 182 that moves the pad 180 in the horizontal direction (X-axis direction and Y-axis direction).

[0048] A detection unit 190 is provided above the chuck 170 to check whether the peripheral portion We has been removed from the processing wafer W. The detection unit 190 detects the presence or absence of the peripheral portion We in the processing wafer W held by the chuck 170 and from which the peripheral portion We has been removed. The detection unit 190 uses, for example, a sensor. The sensor is, for example, a line-type laser displacement meter, and detects the presence or absence of the peripheral portion We by irradiating a laser onto the peripheral portion of the overlapped wafer T (processing wafer W) and measuring the thickness of the overlapped wafer T. Note that the method of detecting the presence or absence of the peripheral portion We by the detection unit 190 is not limited to this. For example, the detection unit 190 may use, for example, a line camera to detect the presence or absence of the peripheral portion We by capturing an image of the overlapped wafer T (processing wafer W).

[0049] A recovery section (not shown) that recovers the peripheral edge portion We transferred by the pad 180 is provided below the chuck 170. The recovery section receives and recovers the peripheral edge portion We that is sucked and held by the pad 180.

[0050] Next, a description will be given of the transfer arm 71 of the above-mentioned wafer transfer device 70. Fig. 8 is a vertical cross-sectional view showing an outline of the configuration of the transfer arm 71.

[0051] The transfer arm 71 serving as a substrate separating section and a transfer section has a disk-shaped suction plate 200 having a diameter larger than the overlapped wafer T. A holder 210 for holding a central portion Wc of the processing wafer W is provided on the lower surface of the suction plate 200.

[0052] A suction pipe 211 that sucks the central portion Wc is connected to the holding portion 210, and the suction pipe 211 is connected to a suction mechanism 212 such as a vacuum pump. A pressure sensor 213 that measures the suction pressure is provided on the suction pipe 211. The pressure sensor 213 may have any configuration, but may be, for example, a diaphragm-type pressure gauge.

[0053] A rotation mechanism 220 that rotates the attraction plate 200 about a vertical axis is provided on the upper surface of the attraction plate 200. The rotation mechanism 220 is supported by a support member 221. In addition, the support member 221 (rotation mechanism 220) is supported by an arm member 72.

[0054] Next, a description will be given of wafer processing according to a first embodiment, which is performed using the wafer processing system 1 configured as above. Fig. 9 is a flow diagram showing main steps of the wafer processing. Fig. 10 is an explanatory diagram of the main steps of the wafer processing. In this embodiment, the processing wafer W and the support wafer S are bonded in a bonding device (not shown) outside the wafer processing system 1 to form an overlapped wafer T in advance.

[0055] First, a cassette Ct containing a plurality of overlapped wafers T as shown in FIG.

[0056] Next, the overlapped wafer T in the cassette Ct is taken out by the wafer transfer device 20 and transferred to the transition device 30. Next, the overlapped wafer T in the transition device 30 is taken out by the wafer transfer device 50 and transferred to the modification device 60. In the modification device 60, a peripheral modified layer M1 and a divided modified layer M2 are sequentially formed inside the processing wafer W as shown in FIG. 10(b) (steps A1 and A2 in FIG. 9), and further, an internal surface modified layer M3 is formed as shown in FIG. 10(c) (step A3 in FIG. 9). The peripheral modified layer M1 is a base point for removing the peripheral portion We in the edge trim. The divided modified layer M2 is a base point for dividing the peripheral portion We to be removed into small pieces. The internal surface modified layer M3 is a base point for thinning the processing wafer W.

[0057] 11A to 11C are explanatory diagrams of main steps of the modification process in the modifying device 60. First, as shown in Fig. 11A, the chuck 100 (slider table 102) is moved to the carry-in / out position P1. Then, the overlapped wafer T is carried in from the wafer transfer device 50 and held by the chuck 100.

[0058] 11(b), the chuck 100 is moved to the macro alignment position P2. The macro alignment position P2 is a position where the macro camera 140 can capture an image of the outer edge of the processing wafer W.

[0059] Next, images of the outer end portion of the process wafer W in the circumferential direction of 360 degrees are captured by the macro camera 140. The captured images are output from the macro camera 140 to the control device 90.

[0060] The control device 90 calculates a first eccentricity between the center Cc of the chuck 100 and the center Cw of the processing wafer W from the image of the macro camera 140. Furthermore, the control device 90 calculates the movement amount of the chuck 100 based on the first eccentricity so as to correct the Y-axis component of the first eccentricity. The chuck 100 moves in the Y-axis direction based on this calculated movement amount, and moves the chuck 100 to the micro-alignment position P3 as shown in FIG. 11(c). The micro-alignment position P3 is a position where the micro camera 150 can capture an image of the peripheral portion of the processing wafer W. Here, since the field of view of the micro camera 150 is approximately 1 / 5 of that of the macro camera 140 as described above, if the Y-axis component of the first eccentricity is not corrected, the peripheral portion of the processing wafer W may not be included in the angle of view of the micro camera 150 and may not be captured by the micro camera 150. Therefore, it can be said that the correction of the Y-axis component based on the first eccentricity is for moving the chuck 100 to the micro-alignment position P3.

[0061] Next, the micro camera 150 captures an image of the boundary between the bonded region Aa and the unbonded region Ab in the circumferential direction of 360 degrees of the process wafer W. The captured image is output from the micro camera 150 to the control device 90.

[0062] The control device 90 calculates a second eccentricity between the center Cc of the chuck 100 and the center Ca of the bonding region Aa from the image of the micro camera 150. Furthermore, the control device 90 determines the position of the chuck 100 with respect to the peripheral modified layer M1 based on the second eccentricity so that the center of the bonding region Aa coincides with the center of the chuck 100. As described above, the unbonded region Ab is formed before bonding the processing wafer W and the support wafer S, but the center of this unbonded region Ab (the center Ca of the bonding region Aa) may be misaligned with the center of the processing wafer W. In this regard, the misalignment of the unbonded region Ab is corrected by adjusting the position of the chuck 100 with respect to the peripheral modified layer M1 based on the second eccentricity as in this embodiment.

[0063] Next, as shown in Fig. 11(d), the chuck 100 is moved to the modification position P4. The modification position P4 is a position where the laser head 110 irradiates the processing wafer W with laser light to form the peripheral modified layer M1. In this embodiment, the modification position P4 is the same as the micro-alignment position P3.

[0064] Next, as shown in Figures 12 and 13, a laser beam L1 (laser beam L1 for peripheral edge) is irradiated from the laser head 110 to form a peripheral modified layer M1 at the boundary between the peripheral portion We and the central portion Wc of the processing wafer W (step A1 in Figure 9). The shape and number of the laser beam L1 are adjusted by LCOS. Specifically, the focal position and phase of the laser beam L1 are controlled to adjust the shape so as to form the peripheral modified layer M1 described below. In this embodiment, the number of laser beams L1 is one.

[0065] The peripheral modified layer M1 formed by the laser light L1 extends in the thickness direction and has a vertically long aspect ratio. The lower end of the peripheral modified layer M1 is located above the target surface (dotted line in FIG. 12) of the processed wafer W after thinning. In other words, the distance H1 between the lower end of the peripheral modified layer M1 and the front surface Wa of the processed wafer W is greater than the target thickness H2 of the processed wafer W after thinning. In this case, the peripheral modified layer M1 does not remain on the processed wafer W after thinning. Note that inside the processed wafer W, a crack C1 develops from the peripheral modified layer M1 and reaches the front surface Wa and back surface Wb.

[0066] The peripheral modified layer M1 is formed radially inward from the outer end of the bonding area Aa. When the peripheral modified layer M1 is formed by the laser light L1 from the laser head 110, even if the peripheral modified layer M1 is formed shifted from the outer end of the bonding area Aa due to, for example, a processing error, the peripheral modified layer M1 can be prevented from being formed radially outward from the outer end of the bonding area Aa. Here, if the peripheral modified layer M1 is formed radially outward from the outer end of the bonding area Aa, the processing wafer W will be in a floating state with respect to the support wafer S after the peripheral portion We is removed. In this regard, in the present embodiment, such a state of the processing wafer W can be reliably prevented.

[0067] As a result of intensive research, the inventors have confirmed that the peripheral portion We can be appropriately removed when the distance D between the peripheral modification layer M1 and the outer end of the bonding region Aa is sufficiently small. This distance D is preferably within 500 μm, and more preferably within 50 μm.

[0068] Here, as described above, the control device 90 determines the position of the chuck 100 based on the second eccentricity. In step A1, the chuck 100 is rotated by the rotation unit 103 and moved in the Y-axis direction by the horizontal movement unit 104 in accordance with the determined position of the chuck 100 so that the center of the joining area Aa coincides with the center of the chuck 100. At this time, the rotation of the chuck 100 and the movement in the Y-axis direction are synchronized. By performing complete synchronization control in this manner, the movement of the chuck 100 can be made to appropriately follow the determined position with little error.

[0069] Then, while rotating and moving the chuck 100 (processing wafer W) in this manner, the laser head 110 irradiates the inside of the processing wafer W with laser light L1. That is, the peripheral modified layer M1 is formed while correcting the second eccentricity amount. In this way, the peripheral modified layer M1 is formed in an annular shape concentric with the bonding area Aa. That is, the distance D between the peripheral modified layer M1 and the outer end of the bonding area Aa shown in FIG. 12 can be made constant. Therefore, in the peripheral removal device 61, the peripheral portion We can be appropriately removed from the peripheral modified layer M1 as a base point.

[0070] In this example, when the second eccentricity amount has an X-axis component, the X-axis component is corrected by rotating the chuck 100 while moving the chuck 100 in the Y-axis direction. On the other hand, when the second eccentricity amount does not have an X-axis component, it is sufficient to only move the chuck 100 in the Y-axis direction without rotating it.

[0071] Next, the laser head 110 is moved in the Y-axis direction, and as shown in Figs. 14 and 15, the laser head 110 irradiates the laser light L2 (division laser light L2) to form divided modified layers M2 on the radially outer side of the peripheral modified layer M1 (step A2 in Fig. 9). At this time, the laser light irradiated from the laser head 110 is switched from the laser light L1 to the laser light L2 by the LCOS, and the shape and number of the laser light L2 are adjusted. Specifically, the focal position and phase of the laser light L2 are controlled to adjust the shape so as to form the divided modified layers M2 described below. In this embodiment, the number of laser lights L2 is one.

[0072] The divided modified layer M2 also extends in the thickness direction like the peripheral modified layer M1, and has a vertically long aspect ratio. In this embodiment, the divided modified layer M2 is formed to the same height as the peripheral modified layer M1. In addition, a crack C2 advances from the divided modified layer M2 and reaches the front surface Wa and the back surface Wb.

[0073] In addition, by forming multiple divided modified layers M2 and cracks C2 at a pitch of several μm in the radial direction, one line of divided modified layers M2 extending radially outward from the peripheral modified layer M1 is formed as shown in FIG. 15. In the illustrated example, the divided modified layers M2 in the radially extending line are formed in eight places, but the number of divided modified layers M2 is arbitrary. If the divided modified layers M2 are formed in at least two places, the peripheral portion We can be removed. In this case, when removing the peripheral portion We in the edge trim, the peripheral portion We is divided into multiple pieces by the divided modified layers M2 while being separated with the annular peripheral modified layer M1 as a base point. In this way, the peripheral portion We to be removed is divided into small pieces, making it easier to remove.

[0074] In the present embodiment, the laser head 110 is moved in the Y-axis direction when forming the divided modified layers M2, but the chuck 100 may be moved in the Y-axis direction.

[0075] Next, as shown in Figs. 16 and 17, a laser beam L3 (internal surface laser beam L3) is irradiated from the laser head 110 to form an internal surface modification layer M3 along the surface direction (step A3 in Fig. 9). At this time, the laser beam irradiated from the laser head 110 is switched from the laser beam L2 to the laser beam L3 by the LCOS, and the shape and number of the laser beam L3 are adjusted. Specifically, the focal position and phase of the laser beam L3 are controlled to adjust the shape so as to form the internal surface modification layer M3 described later. In this embodiment, the number of laser beams L3 is one. The black arrow in Fig. 17 indicates the rotation direction of the chuck 100, and the same applies in the following description.

[0076] The lower end of the internal surface modification layer M3 is located slightly above the target surface (dotted line in FIG. 16) of the thinned processed wafer W. That is, the distance H3 between the lower end of the internal surface modification layer M3 and the surface Wa of the processed wafer W is slightly larger than the target thickness H2 of the thinned processed wafer W. Note that, inside the processed wafer W, a crack C3 propagates from the internal surface modification layer M3 in the surface direction.

[0077] In step A3, the chuck 100 (processing wafer W) is rotated, and the laser head 110 is moved in the Y-axis direction from the outer periphery to the center of the processing wafer W, while irradiating the inside of the processing wafer W with laser light L3 from the laser head 110. Then, an internal surface modification layer M3 is formed in a spiral shape from the outside to the inside within the surface of the processing wafer W.

[0078] In the present embodiment, the laser head 110 is moved in the Y-axis direction when forming the inner surface modified layer M3, but the chuck 100 may be moved in the Y-axis direction.

[0079] 11(e), the chuck 100 is moved to the carry-in / out position P1, and the overlapped wafer T is then carried out by the wafer transfer device .

[0080] As described above, in the modification device 60, the peripheral modified layer M1 in step A1 and the internal surface modified layer M3 in step A3 are formed in this order. If the internal surface modified layer M3 is formed before the peripheral modified layer M1, the processing wafer W may expand or warp. For example, when the internal surface modified layer M3 is formed, a crack C3 is formed in the surface direction of the processing wafer W. Then, stress is applied to the crack C3, and the processing wafer W expands in the surface direction. If the magnitude of this expansion differs depending on the surface direction position of the processing wafer W, separation of the processing wafer W may progress locally. In such a case, the height of the processing wafer W becomes non-uniform in the surface, and warping occurs. If the processing wafer W expands or warps in this way, the peripheral modified layer M1 cannot be formed at an appropriate position. As a result, the peripheral portion We cannot be properly removed, and quality cannot be ensured. In this respect, in this embodiment, the peripheral modified layer M1 and the internal surface modified layer M3 are formed in this order, and the expansion and warping of the processing wafer W can be suppressed.

[0081] Next, the overlapped wafer T is transported by the wafer transport device 70 to the edge removing device 61. In the edge removing device 61, the edge We of the processing wafer W is removed from the edge modified layer M1 as shown in FIG. 10(d) (step A4 in FIG. 9). In step A4, the pad 180 is lowered by the lifting mechanism 181 as shown in FIG. 18 to suction-hold the edge We, and then the pad 180 is further raised. Then, the edge We held by the pad 180 is separated from the processing wafer W from the edge modified layer M1 as the base point. At this time, the edge We is separated into small pieces from the divided modified layer M2 as the base point. The removed edge We is collected from the pad 180 to a collection section (not shown).

[0082] Next, the overlapped wafer T is transported to the processing device 80 by the wafer transport device 70. In the processing device 80, first, when the overlapped wafer T is transferred from the transport arm 71 to the chuck 81, the back surface Wb side of the processing wafer W (hereinafter, referred to as the back surface wafer Wb1) is separated from the inner surface modified layer M3 as shown in FIG. 10(e) (step A5 in FIG. 9).

[0083] In step A5, as shown in FIG. 19(a), the suction plate 200 of the transport arm 71 suction-holds the processing wafer W, while the chuck 81 suction-holds the support wafer S. Then, the suction plate 200 is rotated, and the back surface wafer Wb1 is cut at the inner surface modification layer M3. Thereafter, as shown in FIG. 19(b), the suction plate 200 is raised while suction-holding the back surface wafer Wb1, to separate the back surface wafer Wb1 from the processing wafer W. At this time, the presence or absence of the back surface wafer Wb1 can be detected by measuring the pressure for sucking the back surface wafer Wb1 with the pressure sensor 213, and it can be confirmed whether or not the back surface wafer Wb1 has been separated from the processing wafer W. Note that, if the back surface wafer Wb1 can be separated by simply raising the suction plate 200 as shown in FIG. 19(b), the rotation of the suction plate 200 shown in FIG. 19(a) may be omitted. The separated back surface wafer Wb1 is collected outside the wafer processing system 1.

[0084] 10(f), the back surface Wb of the process wafer W held by the chuck 81 is ground to remove the inner surface modified layer M3 and the peripheral modified layer M1 remaining on the back surface Wb (step A6 in FIG. 9). In step A6, the process wafer W and the grinding wheel are rotated while the grinding wheel is in contact with the back surface Wb to grind the back surface Wb. Thereafter, the back surface Wb of the process wafer W may be cleaned with a cleaning liquid using a cleaning liquid nozzle (not shown).

[0085] Next, the overlapped wafer T is transferred to the cleaning device 41 by the wafer transfer device 70. In the cleaning device 41, the back surface Wb, which is the ground surface of the processing wafer W, is scrubbed and cleaned (step A7 in FIG. 9). Note that in the cleaning device 41, the back surface Sb of the supporting wafer S may be cleaned together with the back surface Wb of the processing wafer W.

[0086] Next, the overlapped wafer T is transported by the wafer transport device 50 to the etching device 40. In the etching device 40, the back surface Wb of the processing wafer W is wet-etched with a chemical solution (step A8 in FIG. 9). Grinding marks may be formed on the back surface Wb ground by the above-mentioned processing device 80. In this step A8, the grinding marks can be removed by wet etching, and the back surface Wb can be smoothed.

[0087] Thereafter, the laminated wafer T on which all the processes have been performed is transferred by the wafer transfer device 50 to the transition device 30, and further transferred by the wafer transfer device 20 to the cassette Ct on the cassette mounting table 10. In this manner, a series of wafer processes in the wafer processing system 1 is completed.

[0088] According to the above embodiment, the edge portion We is removed from the peripheral modified layer M1 as a base point to perform edge trimming, and the back surface wafer Wb1 is separated from the inner surface modified layer M3 as a base point to perform thinning of the processing wafer W. The laser head 110 used to form the peripheral modified layer M1 and the inner surface modified layer M3 is less likely to deteriorate over time, and fewer consumables are required, so that the frequency of maintenance can be reduced. In addition, since this is a dry process using a laser, grinding water and wastewater treatment are not required. This makes it possible to reduce running costs. Therefore, it is possible to reduce running costs compared to conventional edge trimming by grinding and thinning by grinding.

[0089] In this embodiment, the back surface Wb is ground in step A6, but this grinding only requires removing the inner surface modified layer M3 and the peripheral modified layer M1, and the amount of grinding is small, about several tens of μm. In contrast, when the back surface Wb is ground to thin the processing wafer W as in the conventional method, the amount of grinding is large, for example, 700 μm or more, and the degree of wear of the grinding wheel is large. Therefore, in this embodiment, the frequency of maintenance can be reduced.

[0090] Moreover, according to this embodiment, the peripheral modified layer M1 and the internal surface modified layer M3 are formed in this order inside the processing wafer W. As described above, if the internal surface modified layer M3 is formed first, the processing wafer W may expand or warp, but this embodiment can suppress the expansion and warp of the processing wafer W. As a result, the peripheral portion We can be appropriately removed, and quality can be ensured.

[0091] Moreover, according to this embodiment, the shape of the laser beams L1 to L3 is adjusted using one laser head 110, so that the peripheral modified layer M1, the divided modified layer M2, and the internal surface modified layer M3 can be formed. That is, even if the direction in which the modified layer extends or the required processing quality is different, the appropriate shape of the laser beam can be selected using one laser head 110. And, since a modified layer of any shape can be formed in this way, the degree of freedom for forming the modified layer is improved. Also, the occupation area (footprint) of the device can be reduced, and space saving can be realized. Furthermore, since the device configuration is simplified, the device cost can be reduced. Thus, in this embodiment, the thinning process and the pre-processing of the edge trim of the processing wafer W can be efficiently performed.

[0092] In the above embodiment, the laser beams L1 to L3 of different shapes are irradiated by one laser head 110, but it is preferable that the laser head 110 is calibrated before the overlapped wafer T to be processed is carried into the modifying apparatus 60. More specifically, it is preferable to calibrate the laser head 110 before the overlapped wafer T is held by the chuck 100. In this case, it is not necessary to calibrate the laser head 110 during the modification process of one processing wafer W, and the time required to switch the laser beams L1 to L3 can be shortened. As a result, the throughput of the wafer processing can be improved.

[0093] In the above embodiment, when forming the peripheral modified layer M1, one laser beam L1 is irradiated from the laser head 110 to the inside of the processing wafer W, but multiple laser beams L1 may be irradiated. In such a case, the time required to form the peripheral modified layer M1 can be shortened, and the throughput of the wafer processing can be further improved. Similarly, when forming the internal surface modified layer M3, one laser beam L3 is irradiated from the laser head 110 to the inside of the processing wafer W, but multiple laser beams L3 may be irradiated. In such a case, the time required to form the internal surface modified layer M3 can be shortened, and the throughput of the wafer processing can be further improved.

[0094] In the above embodiment, the peripheral edge We is removed using the pad 180 in the peripheral edge removing device 61, and the processing wafer W is separated using the transfer arm 71 in the processing device 80. However, the removal of the peripheral edge We and the transfer arm 71 may be performed in the same device. For example, as shown in FIG. 20, the peripheral edge removing device 61 further includes an adsorption plate 230 as a substrate separating unit above the chuck 170. The adsorption plate 230 has the same configuration as the adsorption plate 200 of the transfer arm 71, and has a disk shape with a larger diameter than the laminated wafer T. A suction mechanism (not shown), such as a vacuum pump, is connected to the adsorption plate 230, and the adsorption plate 230 adsorbs and holds the back surface Wb of the processing wafer W on its lower surface. The adsorption plate 230 includes a lifting mechanism 231 for lifting the adsorption plate 230 in the vertical direction, and a rotation mechanism 232 for rotating the adsorption plate 230 around a vertical axis.

[0095] In this case, after removing the peripheral portion We by the pad 180 in step A4, the processing wafer W is separated by the suction plate 230 in step A5. In step A5, the back surface Wb of the processing wafer W is suction-held by the suction plate 230. Then, the suction plate 230 is rotated to cut the back surface wafer Wb1 at the inner surface modification layer M3. Thereafter, while the suction plate 230 suction-holds the back surface wafer Wb1, the suction plate 230 is raised to separate the back surface wafer Wb1 from the processing wafer W. Note that if the back surface wafer Wb1 can be separated by simply raising the suction plate 230, the rotation of the suction plate 230 may be omitted.

[0096] The suction plate 230 may suction-hold the central portion Wc and the peripheral portion We of the processing wafer W separately. Specifically, for example, a central holding portion (not shown) for holding the central portion Wc and a peripheral holding portion (not shown) for holding the peripheral portion We may be provided on the lower surface of the suction plate 230. Separate suction mechanisms (not shown) are connected to the central holding portion and the peripheral holding portion, respectively, and the central holding portion and the peripheral holding portion can be switched to suction-hold the central portion Wc and the peripheral portion We separately. In this case, the removal of the peripheral portion We in step A4 and the separation of the processing wafer W in step A5 are each performed by the suction plate 230. In this example, the pad 180, the lifting mechanism 181, and the moving mechanism 182 are omitted.

[0097] In this embodiment, it is also possible to appropriately remove the peripheral portion We of the processing wafer W and separate the processing wafer W. Moreover, since these can be performed in the same apparatus, it is possible to improve the throughput of the wafer processing.

[0098] In this embodiment, the peripheral modified layer M1 and the internal surface modified layer M3 are formed in this order inside the processing wafer W. However, when the internal surface modified layer M3 is formed, the processing wafer W may expand. In such a case, the peripheral portion We may peel off due to the expansion of the processing wafer W, and the peeled peripheral portion We may adversely affect the drive system, such as the rotating unit 103 and the horizontal moving unit 104, in the modifying device 60. Therefore, it is preferable to take measures to prevent the peripheral portion We from peeling off. For example, the following two measures are considered as the measures.

[0099] The first measure to prevent the peeling of the peripheral portion We is a method of physically holding the peripheral portion We. For example, as shown in FIG. 21, a plurality of cylindrical peripheral holding parts 240 that contact the outer end of the processing wafer W may be provided. Alternatively, as shown in FIG. 22, a plurality of rectangular parallelepiped peripheral holding parts 241 that contact the outer end of the processing wafer W may be provided. Each of these peripheral holding parts 240, 241 is configured to be freely movable in the vertical and horizontal directions by a moving mechanism (not shown). Although the peripheral holding parts 240, 241 have a difference in whether they make point contact or line contact with the processing wafer W, in either case, they can prevent the peeling of the peripheral portion We. Note that the peripheral holding parts 240, 241 only need to be in contact with the outer end of the processing wafer W when the inner surface modification layer M3 is formed, and may be retreated from the processing wafer W otherwise.

[0100] The second measure to prevent peeling of the peripheral portion We is to cause the crack C1 formed from the peripheral modified layer M1 in the thickness direction of the processing wafer W to propagate only to the front surface Wa. By adjusting the shape of the laser light L1 irradiated from the laser head 110, the crack C1 is caused to propagate only to the front surface Wa and not to reach the back surface Wb, as shown in FIG. 23(a). Similarly, when forming the divided modified layer M2, the crack C2 is also caused to propagate only to the front surface Wa and not to reach the back surface Wb. In such a case, even if the internal surface modified layer M3 is subsequently formed as shown in FIG. 23(b), the peripheral portion We will not peel off from the processing wafer W.

[0101] Next, a wafer processing according to the second embodiment will be described. Fig. 24 is a flow diagram showing main steps of the wafer processing. Fig. 25 is an explanatory diagram of the main steps of the wafer processing.

[0102] In the first embodiment, the removal of the peripheral portion We and the separation of the processing wafer W are performed separately, but in the second embodiment, these are performed simultaneously. The removal of the peripheral portion We and the separation of the processing wafer W are performed, for example, in the processing device 80, using a transfer arm 71 as a removal and separation unit. Note that the transfer arm 71 in this embodiment holds the entire processing wafer W, that is, the central portion Wc and the peripheral portion We. Also, since the removal of the peripheral portion We is performed using the transfer arm 71 in this manner, the peripheral removal device 61 may be omitted in the wafer processing system 1 of this embodiment.

[0103] In the wafer processing according to the second embodiment, first, the overlapped wafer T shown in Fig. 25(a) is transported to the modifying apparatus 60. In the modifying apparatus 60, a peripheral modified layer M10 (step B1 in Fig. 24) is formed on the processing wafer W as shown in Fig. 25(b), and further, an inner surface modified layer M30 (step B2 in Fig. 24) is formed as shown in Fig. 25(c).

[0104] Here, the method for forming the peripheral modified layer M10 in step B1 is the same as that in step A1, except that, whereas the crack C1 in the peripheral modified layer M1 shown in Fig. 10(b) progresses to the front surface Wa and the back surface Wb, the crack C10 from the peripheral modified layer M10 progresses only to the front surface Wa and does not reach the back surface Wb.

[0105] The method for forming the inner surface modified layer M30 in step B2 is the same as that in step A3. However, while the crack C3 in the inner surface modified layer M3 shown in FIG. 10(c) progresses in the surface direction to the outer edge of the processing wafer W, the crack C30 from the inner surface modified layer M30 progresses only to the inside of the peripheral modified layer M10.

[0106] Next, the overlapped wafer T is transported to the processing device 80 by the wafer transport device 70. In the processing device 80, first, when the overlapped wafer T is transferred from the transport arm 71 to the chuck 81, the back surface Wb side of the processing wafer W (hereinafter, referred to as the back surface wafer Wb2) is separated based on the peripheral modified layer M10 and the inner surface modified layer M30 as shown in FIG. 25(d) (step B3 in FIG. 24).

[0107] In step B3, as shown in Fig. 26(a), the suction plate 200 of the transfer arm 71 suction-holds the processing wafer W, while the chuck 81 suction-holds the support wafer S. Then, the suction plate 200 is rotated to cut the back surface wafer Wb2 at the boundary between the peripheral modified layer M10 and the internal surface modified layer M30. Thereafter, as shown in Fig. 26(b), while the suction plate 200 suction-holds the back surface wafer Wb2, the suction plate 200 is raised to separate the back surface wafer Wb2 from the processing wafer W. Thus, in step B3, the back surface wafer Wb2 is separated together with the peripheral portion We, that is, removal of the peripheral portion We and separation of the processing wafer W are performed simultaneously.

[0108] 25(e), the back surface Wb of the process wafer W is ground (Step B4 in FIG. 24), followed by cleaning of the back surface Wb in the cleaning device 41 (Step B5 in FIG. 24) and wet etching of the back surface Wb in the etching device 40 (Step B6 in FIG. 24). In this manner, a series of wafer processing steps in the wafer processing system 1 is completed.

[0109] In this embodiment, the peripheral modified layer M10 and the internal surface modified layer M30 are formed in this order inside the processing wafer W, and the same effects as those of the first embodiment can be obtained. Moreover, since cracks from the peripheral modified layer M10 do not reach the back surface Wb, the peripheral portion We is not peeled off due to the expansion of the processing wafer W when the internal surface modified layer M30 is formed. In order to more reliably prevent the peripheral portion We from peeling off, peripheral holding parts 240 and 241 may be provided as shown in FIG. 21 or FIG. 22.

[0110] In the above embodiment, the removal of the peripheral edge We and the separation of the processing wafer W are performed using the transfer arm 71, but they may be performed using a separate device. For example, the wafer processing system 1 may be provided with a removal / separation device 300 shown in FIG. 27 instead of the peripheral edge removing device 61.

[0111] The removal / separation apparatus 300 has a chuck 310 as another substrate holding unit that holds the overlapped wafer T on the upper surface. The chuck 310 adsorbs and holds the support wafer S with the process wafer W on the upper side and the support wafer S on the lower side. The chuck 310 is configured to be rotatable about a vertical axis by a rotation mechanism 311.

[0112] An adsorption plate 320 serving as a removal and separation unit is provided above the chuck 310. The adsorption plate 320 has a configuration similar to that of the adsorption plate 200 of the transfer arm 71, and has a disk shape with a diameter larger than that of the laminated wafers T. A suction mechanism (not shown), such as a vacuum pump, is connected to the adsorption plate 320, and the adsorption plate 320 adsorbs and holds the back surface Wb of the processing wafer W on its lower surface. The adsorption plate 320 is provided with a lifting mechanism 321 that lifts and lowers the adsorption plate 320 in the vertical direction, and a rotation mechanism 322 that rotates the adsorption plate 320 around a vertical axis.

[0113] In this case, the back surface Wb of the processing wafer W is adsorbed and held by the adsorption plate 320. Then, the adsorption plate 320 is rotated to cut the back surface wafer Wb2 at the boundary between the peripheral modified layer M10 and the internal surface modified layer M30. Thereafter, while the adsorption plate 320 is adsorbing and holding the back surface wafer Wb2, the adsorption plate 320 is raised to separate the back surface wafer Wb2 from the processing wafer W. The removal and separation apparatus 300 of this embodiment can also appropriately remove the peripheral portion We of the processing wafer W and separate the processing wafer W.

[0114] Next, a wafer processing according to the third embodiment will be described. Fig. 28 is a flow diagram showing main steps of the wafer processing. Fig. 29 is an explanatory diagram of the main steps of the wafer processing.

[0115] In the first embodiment, the peripheral portion We is removed after the internal surface modification layer M3 is formed, but in the third embodiment, the peripheral portion We is removed and then the internal surface modification layer M31 is formed. That is, in the third embodiment, the peripheral modification layer M11 is formed, the peripheral portion We is removed, and the internal surface modification layer M31 is formed in this order. The peripheral modification layer M11 and the internal surface modification layer M31 are each performed in the modification device 60, but if the peripheral portion We is removed outside the modification device 60, the throughput decreases. Therefore, in this embodiment, the peripheral portion We is removed inside the modification device 60 using a transfer arm 71 as a peripheral removal unit. Since the peripheral portion We is removed using the transfer arm 71 in this way, the peripheral removal device 61 may be omitted in the wafer processing system 1 of this embodiment. The transfer arm 71 also functions as a substrate separation unit as described later.

[0116] 30, the transfer arm 71 has a disk-shaped suction plate 400 having a diameter larger than the processing wafer W. On the lower surface of the suction plate 400, a center holding part 410 for holding a center portion Wc of the processing wafer W and a peripheral holding part 420 for holding a peripheral portion We of the processing wafer W are provided.

[0117] A suction pipe 411 that sucks the central portion Wc is connected to the central holding portion 410, and the suction pipe 411 is connected to a central suction mechanism 412 such as a vacuum pump. A central pressure sensor 413 that measures the suction pressure is provided on the suction pipe 411. The central pressure sensor 413 may have any configuration, but may be, for example, a diaphragm-type pressure gauge.

[0118] A suction pipe 421 for sucking the peripheral part We is connected to the peripheral holding part 420, and the suction pipe 421 is in communication with a peripheral suction mechanism 422 such as a vacuum pump. A peripheral pressure sensor 423 for measuring the suction pressure is provided on the suction pipe 421. The peripheral pressure sensor 423 may have any configuration, but may be, for example, a diaphragm-type pressure gauge.

[0119] 31, a recess 400a is formed in the peripheral portion of the suction plate 400 where the peripheral holding portion 420 is provided, the recess 400a being recessed above the central holding portion 410. As will be described later, the peripheral portion We is pushed up and removed by the peripheral removing portion 440, and the recess 400a ensures a space into which the peripheral portion We is pushed up.

[0120] With this configuration, the central holding part 410 and the peripheral holding part 420 can individually suck and hold the central part Wc and the peripheral part We. In addition, the central pressure sensor 413 and the peripheral pressure sensor 423 can individually measure the pressure sucking the central part Wc and the pressure sucking the peripheral part We.

[0121] A rotation mechanism 430 that rotates the attraction plate 400 about a vertical axis is provided on the upper surface of the attraction plate 400. The rotation mechanism 430 is supported by a support member 431. In addition, the support member 431 (rotation mechanism 430) is supported by an arm member 72.

[0122] A plurality of peripheral edge removing portions 440 are provided on the sides of the attraction plate 400 along the circumferential direction of the attraction plate 400. Each peripheral edge removing portion 440 has a wedge roller 441 and a support roller 442.

[0123] The wedge roller 441 has a wedge shape with a pointed tip in a side view. The wedge roller 441 is inserted into the interface between the process wafer W and the support wafer S from the outer ends of the process wafer W and the support wafer S. Then, the inserted wedge roller 441 pushes up the peripheral edge portion We, and the peripheral edge portion We is separated and removed from the process wafer W.

[0124] The support roller 442 passes through the center of the wedge roller 441 and supports the wedge roller 441. The support roller 442 is configured to be freely movable in the horizontal direction by a moving mechanism (not shown), and the movement of the support roller 442 causes the wedge roller 441 to move as well. The support roller 442 is configured to be freely rotatable about a vertical axis, and the rotation of the support roller 442 causes the wedge roller 441 to rotate as well. In this embodiment, a so-called free roller that rotates in response to the rotation of the chuck 100, as described later, is used as the support roller 442. However, the support roller 442 may be actively rotated by a rotation mechanism (not shown).

[0125] A rotating shaft 443 is provided on the upper surface of the support roller 442, and the rotating shaft 443 is supported by a moving mechanism 444. The moving mechanism 444 is provided on the outer periphery of the upper surface of the support member 431. The moving mechanism 444 is, for example, an air cylinder, and can move the wedge roller 441 and the support roller 442 in the horizontal direction via the rotating shaft 443.

[0126] In the wafer processing according to the third embodiment, first, the overlapped wafer T shown in Fig. 29(a) is transported to the modifying apparatus 60. In the modifying apparatus 60, a peripheral modified layer M11 and divided modified layers M21 are sequentially formed on the processing wafer W as shown in Fig. 29(b) (steps C1 and C2 in Fig. 28). Note that the method of forming the peripheral modified layer M11 in step C1 is the same as step A1, and the method of forming the divided modified layers M21 in step C2 is the same as step A2.

[0127] Next, the transfer arm 71 of the wafer transfer device 70 enters the inside of the modifying device 60, and the peripheral edge portion We is removed as shown in FIG. 29(c) (Step C3 in FIG. 28).

[0128] In step C3, first, the back surface Wb of the processing wafer W is suction-held by the suction plate 400 of the transfer arm 71. Then, as shown in FIG. 32(a), the wedge roller 441 is moved toward the overlapping wafer T, and the wedge roller 441 is brought into contact with the interface between the processing wafer W and the support wafer S. At this time, the suction plate 400 is rotated, and the wedge roller 441 is also rotated in the opposite direction in plan view. Next, as shown in FIG. 32(b), while rotating the suction plate 400, the wedge roller 441 is further moved and inserted into the interface between the processing wafer W and the support wafer S. Then, the peripheral portion We is pushed up, separated from the processing wafer W, and suction-held by the peripheral edge holder 420.

[0129] Thereafter, the transport arm 71 withdraws from the reformer 60 while the peripheral edge holding portion 420 suction-holds the peripheral edge We and the multiple wedge rollers 441 hold the peripheral edge We. Then, the peripheral edge We is collected in a collection portion (not shown) provided outside the reformer 60.

[0130] When removing the peripheral portion We, the central pressure sensor 413 and the peripheral pressure sensor 423 measure the pressure for sucking the central portion Wc and the pressure for sucking the peripheral portion We, respectively. If the peripheral portion We is properly removed, the pressure for sucking the central portion Wc is zero, and the pressure for sucking the peripheral portion We is a predetermined pressure. On the other hand, if the peripheral portion We is not properly removed, for example, the pressure for sucking the peripheral portion We is zero. By measuring the suction pressure with the central pressure sensor 413 and the peripheral pressure sensor 423 in this manner, the presence or absence of the peripheral portion We on the processing wafer W can be detected, and it can be confirmed whether the peripheral portion We has been removed from the processing wafer W.

[0131] Next, in the reforming device 60, an inner surface modified layer M31 is formed as shown in Fig. 29(d) (Step C4 in Fig. 28). Note that the method of forming the inner surface modified layer M31 in Step C4 is the same as in Step A3.

[0132] Next, the overlapped wafer T is transported to the processing device 80 by the wafer transport device 70. In the processing device 80, first, when the overlapped wafer T is transferred from the transport arm 71 to the chuck 81, the back surface Wb side of the processing wafer W (hereinafter, referred to as the back surface wafer Wb3) is separated from the inner surface modification layer M31 as a base point as shown in FIG. 29(e) (step C5 in FIG. 28). The method of separating the processing wafer W in step C5 is the same as that in step A5. Furthermore, the separation of the processing wafer W is not limited to the method using the transport arm 71, and may be performed using, for example, an apparatus similar to the edge removing apparatus 61 shown in FIG. 20.

[0133] 29(f), the back surface Wb of the process wafer W is ground (Step C6 in FIG. 28), followed by cleaning of the back surface Wb in the cleaning apparatus 41 (Step C7 in FIG. 28) and wet etching of the back surface Wb in the etching apparatus 40 (Step C8 in FIG. 28). In this manner, a series of wafer processing steps in the wafer processing system 1 is completed.

[0134] In this embodiment, the peripheral modified layer M11 and the internal surface modified layer M31 are formed in this order inside the processing wafer W, and the same effects as those of the first embodiment can be obtained. Moreover, the formation of the peripheral modified layer M11 in step C1, the removal of the peripheral portion We in step C3, and the formation of the internal surface modified layer M31 in step C4 are performed in a single modifying apparatus 60, so that the throughput of the wafer processing can be maintained. Note that, in this embodiment, the removal of the peripheral portion We in step C3 is performed in the modifying apparatus 60, but of course it may be performed in a separate apparatus.

[0135] Next, another embodiment of the reforming device 60 will be described. In the above embodiment, the reforming device 60 is provided with one laser head 110, but as shown in FIG. 33, a plurality of laser heads, for example, two laser heads 110 and 500, may be provided. In this embodiment, for convenience of explanation, the laser head 110 is referred to as the first laser head 110, and the laser head 500 is referred to as the second laser head 500. Note that the number of laser heads is not limited to this embodiment. In addition, in FIG. 33, in order to avoid complexity of the illustration, the macro camera 140 and the micro camera 150 are omitted.

[0136] The second laser head 500 is provided on the Y-axis positive side of the first laser head 110. The configuration of the second laser head 500 is similar to the configuration of the first laser head 110. That is, the second laser head 500 has a lens 501 and an LCOS (not shown).

[0137] The support configuration of the second laser head 500 is similar to that of the first laser head 110. That is, the second laser head 500 is supported by a support member 510, a rail 511, an elevating mechanism 520, and a moving mechanism 521. The second laser head 500 is configured to be freely movable up and down and to be freely movable in the Y-axis direction.

[0138] In such a case, for example, when forming the peripheral modified layer M1 in the first embodiment, the first laser head 110 and the second laser head 500 are arranged on a concentric circle at the outer periphery of the processing wafer W as shown in FIG. 34. Then, while rotating the processing wafer W, the first laser head 110 irradiates the laser light L12 and the second laser head 500 irradiates the laser light L13. Then, the peripheral modified layer M12 is formed by the laser light L12, and the peripheral modified layer M13 is formed by the laser light L13. The peripheral modified layers M12 and M13 are each formed on half the circumference of the processing wafer W, and the peripheral modified layer M1 is formed in an annular shape by combining these peripheral modified layers M12 and M13. That is, in this embodiment, when forming the peripheral modified layer M1, it is only necessary to rotate the processing wafer W by 180 degrees. Therefore, the time required to form the peripheral modified layer M1 can be shortened, and as a result, the throughput of the wafer processing can be further improved.

[0139] In the above example, the laser beam L12 from the first laser head 110 and the laser beam L13 from the second laser head 500 are irradiated to the same depth inside the processing wafer W, and the peripheral modified layer M12 and the peripheral modified layer M13 are formed to the same depth. However, the laser beam L12 and the laser beam L13 may be irradiated to different depths, and the peripheral modified layer M12 and the peripheral modified layer M13 may be formed to different depths.

[0140] In addition, when forming the internal surface modification layer M3, the first laser head 110 and the second laser head 500 are arranged on a concentric circle at the outer periphery of the processing wafer W as shown in FIG. 35. Then, the processing wafer W is rotated, and the first laser head 110 and the second laser head 500 are moved in the Y-axis direction from the outer periphery to the center of the processing wafer W. That is, the first laser head 110 is moved in the Y-axis positive direction, and the second laser head 500 is moved in the Y-axis negative direction. During the rotation of the processing wafer W and the movement of the laser heads 110 and 500, the first laser head 110 irradiates the inside of the processing wafer W with laser light L32, and the second laser head 500 irradiates the inside of the processing wafer W with laser light L33. Then, the internal surface modification layer M32 is formed by the laser light L32, and the internal surface modification layer M33 is formed by the laser light L33. The inner surface modification layers M32 and M33 are each formed in a spiral shape, and the inner surface modification layer M3 is formed on the entire surface of the processing wafer W. By simultaneously forming the inner surface modification layers M32 and M33 in this manner, the time required to form the inner surface modification layer M3 can be shortened, and as a result, the throughput of the wafer processing can be further improved.

[0141] In the above embodiment, the divided modified layer M2 is formed by using the laser head 110 used in forming the other peripheral modified layer M1 and internal surface modified layer M3 in the modifying device 60, but a separate laser head (not shown) may be used. Furthermore, in the modifying device 60, the peripheral modified layer M1, the divided modified layer M2, and the internal surface modified layer M3 may each be formed by using a separate laser head (not shown).

[0142] For example, in the above embodiment, the unbonded region Ab is formed at the interface between the process wafer W and the support wafer S before bonding, but the unbonded region Ab may be formed after bonding. For example, it is also possible to form the unbonded region Ab by irradiating the outer periphery of the oxide film F with laser light after bonding to reduce the bonding strength.

[0143] The embodiments disclosed herein should be considered as illustrative and not restrictive in all respects. The above-described embodiments may be omitted, substituted, or modified in various forms without departing from the scope and spirit of the appended claims. [Explanation of symbols]

[0144] 1. Wafer Processing System 60 Reformer 100 Chuck 110 Laser Head S Support Wafer T Polymer Wafer W Processing Wafer

Claims

1. A substrate processing method for processing a substrate, comprising the steps of: Holding the second substrate in a laminated substrate in which the first substrate and the second substrate are bonded together; irradiating the inside of the first substrate with a peripheral laser light along a boundary between a peripheral portion and a central portion to be removed, thereby forming a peripheral modified layer; The laminated substrate has a bonding region where a surface of the first substrate and a surface of the second substrate are bonded to each other, and an unbonded region which is a region radially outward from an outer end of the bonding region, A substrate processing method, comprising: irradiating the peripheral laser light such that a distance between the peripheral modified layer and the outer end of the bonding region is within 500 μm when forming the peripheral modified layer.

2. 2. The substrate processing method according to claim 1, wherein in forming the peripheral modified layer, the peripheral laser light is irradiated so that a distance between the peripheral modified layer and the outer end of the bonding region is within 50 μm.

3. The substrate processing method according to claim 1 , further comprising: acquiring an image by using an imaging section to image a boundary between the bonded region and the unbonded region of the laminated substrate.

4. The substrate processing method according to claim 3 , further comprising correcting, from the image, a deviation between a position where the peripheral modified layer is formed and the outer end of the bonding region.

5. holding the second substrate on the laminated substrate by a substrate holder configured to be rotatable around an axis perpendicular to the laminated substrate; calculating an amount of eccentricity between a rotation center of the substrate holder and a center of the bonding area from the image; The substrate processing method according to claim 4 , further comprising: correcting the misalignment by adjusting a relative position between a position where the peripheral modified layer is formed and the outer end of the bonding region based on the amount of eccentricity.

6. The substrate processing method according to claim 5 , wherein the substrate holding unit has a movement mechanism, and the relative position between the position where the peripheral modified layer is formed and the outer end of the bonding region is adjusted by the movement mechanism.

7. The imaging unit includes a micro camera that captures an image of a boundary between the bonded region and the unbonded region in the laminated substrate to obtain the image, and a macro camera that captures an image of an outer edge of the laminated substrate; capturing an image of the outer edge of the laminated substrate with the macro camera to obtain a second image; calculating a second eccentricity amount between a center of the substrate holding part and a center of the laminated substrate from the second image; The substrate processing method according to claim 6 , further comprising: determining a position at which the micro camera can capture an image of the boundary between the bonded region and the unbonded region of the laminated substrate based on the second amount of eccentricity.

8. A substrate processing apparatus for processing a substrate, a substrate holder that holds the second substrate in a laminated substrate formed by bonding a first substrate and a second substrate; a modification device that irradiates a peripheral laser beam along a boundary between a peripheral portion and a central portion to be removed inside the first substrate of the laminated substrate held by the substrate holding part to form a peripheral modified layer; The laminated substrate has a bonding region where a surface of the first substrate and a surface of the second substrate are bonded to each other, and an unbonded region which is a region radially outside the bonding region, The modification device is configured to irradiate the peripheral laser light so that the distance between the peripheral modified layer and an outer end of the bonding region is within 500 μm.

9. The substrate processing apparatus according to claim 8 , wherein the modifying device is configured to irradiate the peripheral laser light so that a distance between the peripheral modified layer and an outer end of the bonding region is within 50 μm.

10. The substrate processing apparatus according to claim 9 , further comprising an imaging unit configured to be able to obtain an image by imaging a boundary between the bonded region and the unbonded region in the laminated substrate.

11. The substrate processing apparatus according to claim 10 , further comprising a control unit that executes control including correcting, from the image, a deviation between a position where the peripheral modified layer is formed and the outer end of the bonding region.

12. The control unit is holding the second substrate on the laminated substrate by the substrate holding unit configured to be rotatable around an axis perpendicular to the laminated substrate; calculating an amount of eccentricity between a rotation center of the substrate holder and a center of the bonding area from the image; The substrate processing apparatus according to claim 11 , further comprising: correcting the misalignment by adjusting a relative position between a position where the peripheral modified layer is formed and the outer end of the bonding region based on the amount of eccentricity.

13. The substrate holder has a moving mechanism, The control unit is The substrate processing apparatus according to claim 12 , further comprising a control unit configured to adjust, by the moving mechanism, the relative position between the position where the peripheral modified layer is formed and the outer end of the bonding region.

14. The imaging unit includes: A micro camera configured to be able to acquire the image by capturing an image of a boundary between the bonded region and the unbonded region in the laminated substrate, and a macro camera capturing an image of an outer edge of the laminated substrate, The control unit is capturing an image of the outer edge of the laminated substrate with the macro camera to obtain a second image; calculating a second eccentricity amount between a center of the substrate holding part and a center of the laminated substrate from the second image; The substrate processing apparatus according to claim 13 , further comprising: determining a position at which the micro camera can capture an image of the boundary between the bonded region and the unbonded region of the laminated substrate based on the second amount of eccentricity.

Citation Information

Patent Citations

  • Method of processing wafer

    JP2004111606A

  • Method of grinding wafer

    JP2006108532A

  • Method for manufacturing semiconductor device

    JP2011171647A

  • Method of manufacturing lamination device

    JP2016004835A

  • Wafer thinning method and apparatus

    JP2016519433A