Flame-retardant resin composition, method for producing flame-retardant resin composition, flame-retardant resin molded article, flame-retardant resin housing and electronic apparatus
A flame-retardant resin composition using polysaccharide-phosphate reaction products with small particle sizes addresses the challenge of combining toughness, elasticity, and low environmental impact, improving flame retardancy and reducing combustion residues.
Patent Information
- Application Number
- JP2023078952
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-12
- Publication Date
- 2024-11-22
AI Technical Summary
Existing flame-retardant resin compositions face challenges in achieving both toughness and elasticity while maintaining a low environmental impact, particularly when using metal hydrates and phosphorus-based flame retardants, which compromise strength and produce combustion residues during thermal recycling.
A flame-retardant resin composition containing thermoplastic resin and particles formed by reacting polysaccharides with compounds having phosphate groups, with an average primary particle size of 1 to 1000 nm, promoting carbonization and improving flame retardancy without halogen-based additives.
The composition achieves both toughness and elasticity with reduced environmental impact by enhancing flame retardancy through a uniform carbonized layer, minimizing the need for additional flame retardants and reducing combustion residues.
Smart Images

Figure 2024163406000006 
Figure 2024163406000001 
Figure 2024163406000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a flame-retardant resin composition, a method for producing the flame-retardant resin composition, a flame-retardant resin molded product, a flame-retardant resin housing, and an electronic device. More specifically, the present invention relates to a flame-retardant resin composition that has both toughness and elasticity and has a low environmental impact. [Background technology]
[0002] From the viewpoint of reducing the environmental burden, the use of resin compositions composed of biomass-derived materials is being promoted. In addition, using biomass-derived materials as the main raw material is called "bio-based." The higher the bio-based mass content, the better, and a resin composition with a bio-based mass content of 100% is the most preferable. After using such a resin composition as a material, energy can be obtained without increasing carbon dioxide emissions and with a small amount of combustion residue when finally thermally recycled. In addition, it makes it less likely to cause marine plastic problems and eliminates the cost of biodegrading resin materials.
[0003] Development and production of bio-based resin materials is expanding. When using bio-based resin materials for electronic device housings, flame retardants must be added to impart flame retardancy. Among flame retardants, high-performance halogen-based flame retardants and antimony compounds, which are often used as auxiliary agents, have a high environmental impact and are being sought to be eliminated. On the other hand, metal hydrates and phosphorus-based flame retardants have a low environmental impact. However, because their flame retardant effect is weak, it is necessary to increase their content in the resin material, but increasing their content has the problem of reducing the strength (toughness and elasticity) of the resin material. In other words, it is difficult to achieve both flame retardancy and strength in a resin material with a low environmental impact. In addition, metal hydrates have the problem of generating combustion residues that need to be discharged during thermal recycling.
[0004] Patent Document 1 discloses a technology for a flame-retardant resin composition containing, as a flame retardant, a phosphorus-containing polysaccharide obtained by adding a phosphoric acid ester to the side chain of a natural polysaccharide. However, the demand for impact strength of flame-retardant resin compositions is increasing, and further improvements are needed. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2010-31230 A Summary of the Invention [Problem to be solved by the invention]
[0006] The present invention has been made in consideration of the above problems and circumstances, and an object of the present invention is to provide a flame-retardant resin composition which combines toughness and elasticity and has a low environmental impact, a method for producing a flame-retardant resin composition, a flame-retardant resin molded product, a flame-retardant resin housing, and an electronic device. [Means for solving the problem]
[0007] In order to solve the above problems, the present inventors have investigated the causes of the above problems and have found that in a flame-retardant resin composition containing at least a thermoplastic resin and particles, the particles contain a reaction product of a polysaccharide and a compound having a phosphate group, and the average primary particle size of the particles is within the range of 1 to 1000 nm, thereby providing both toughness and elasticity and reducing the environmental load, thereby arriving at the present invention. That is, the above-mentioned problems of the present invention are solved by the following means.
[0008] 1. A flame-retardant resin composition containing at least a thermoplastic resin and particles, the particles contain a reaction product of a polysaccharide and a compound having a phosphate group; The average primary particle size of the particles is within the range of 1 to 1000 nm. A flame-retardant resin composition comprising:
[0009] 2. The polysaccharide is an acidic polysaccharide. 2. The flame-retardant resin composition according to claim 1,
[0010] 3. The polysaccharide is a basic polysaccharide. 2. The flame-retardant resin composition according to claim 1,
[0011] 4. The reaction product has at least an acidic functional group, a salt of the acidic functional group, or a group derived from the acidic functional group on an atom constituting the sugar skeleton. 3. The flame-retardant resin composition according to claim 1 or 2,
[0012] 5. The acidic functional group is a phosphate group. 5. The flame-retardant resin composition according to claim 4.
[0013] 6. The softening point of the thermoplastic resin is 200°C or lower. 4. The flame-retardant resin composition according to any one of claims 1 to 3,
[0014] 7. The number average molecular weight of the polysaccharide is within the range of 1,000 to 1,000,000. 3. The flame-retardant resin composition according to claim 1 or 2,
[0015] 8. A method for producing the flame-retardant resin composition according to any one of items 1 to 3, comprising: A step of dissolving the polysaccharide in the compound having a phosphate group and reacting the polysaccharide in the solution; and and adding the reaction product to an organic solvent to precipitate the reaction product. A method for producing a flame-retardant resin composition comprising the steps of:
[0016] 9. A flame-retardant resin molded product, characterized in that it is formed using the flame-retardant resin composition according to any one of items 1 to 3.
[0017] 10. A flame-retardant resin housing comprising the flame-retardant resin molded product according to item 9.
[0018] 11. An electronic device comprising the flame-retardant resin molded article according to item 9. Effect of the Invention
[0019] According to the above-mentioned means of the present invention, it is possible to provide a flame-retardant resin composition which combines toughness and elasticity and has a low environmental impact, a method for producing a flame-retardant resin composition, a flame-retardant resin molded product, a flame-retardant resin housing, and an electronic device.
[0020] Although the mechanism by which the effects of the present invention are manifested or the mechanism by which the effects of the present invention are acted upon has not been clearly understood, it is speculated as follows.
[0021] Polysaccharides, which have many hydroxyl groups in the molecule, are biomass-derived materials. Polysaccharides are prone to dehydration reactions at high temperatures, and when burned, they are prone to form a carbonized layer that inhibits continued combustion due to their heat insulating and gas barrier properties. In particular, when an acid catalyst having an acidic functional group or the like is brought into close proximity with a polysaccharide molecule, carbonization is promoted, so that the addition of a specific amount of polysaccharide can impart flame retardancy to a resin composition. However, the amount of polysaccharide added must be sufficient to obtain sufficient flame retardancy, and it is believed that a large amount of polysaccharide added would cause stress concentration points to occur, resulting in a decrease in impact strength.
[0022] Most commercial polysaccharides have a large particle size of about 10 μm or more, and are strong. Therefore, when kneaded with resin, polysaccharides are difficult to divide, and the polysaccharides are contained in the resin composition with large particle size. In this case, the total area of the interface between the polysaccharide and the matrix resin becomes relatively small, which is insufficient in terms of strength. In particular, when the polysaccharide content is high, contact points are generated between the polysaccharide particles. These contact points are likely to concentrate stress, and are considered to be one of the causes of the occurrence of stress concentration points. In other words, it is considered that the small total area of the interface between the polysaccharide and the resin makes it easy for the interface to peel off, and the impact strength and bending strength are likely to decrease.
[0023] A method for suppressing the occurrence of contact points includes a method of reducing the number of contact points between polysaccharide particles. That is, a method of adding an additive having a plasticizing effect such as a compatibilizer to uniformly mix the resin and polysaccharide is included. However, when a compatibilizer or the like is added, the bending strength of the resin composition is likely to decrease due to the plasticizing effect.
[0024] The resin composition of the present invention contains a reaction product of a polysaccharide and a compound having a phosphoric acid group (phosphoric acid). That is, it is believed that carbonization by a dehydration condensation reaction is promoted by bringing the polysaccharide and the acid catalyst into close proximity, and that the flame retardancy can be improved. In addition, it is believed that the phosphoric acid incorporated in the polysaccharide molecule is dehydrated during combustion and incorporated into the crosslinks, strengthening the carbonized layer and improving the impact strength. Furthermore, since the flame retardancy can be improved without containing halogen, the environmental load can be reduced. In addition, since the amount of phosphorus-based flame retardants, metal hydrates, etc. used in combination can be reduced by improving the flame retardancy, the decrease in impact strength caused by the combined use of these flame retardants can be suppressed.
[0025] Then, the particles containing this reaction product are made to have a small particle size. Specifically, the average primary particle size is made to be within the range of 1 to 1000 nm. This is believed to reduce unevenness in the carbonized layer, that is, improve the uniformity of the carbonized layer, and further improve the flame retardancy. By making the particle size small, the same level of flame retardancy can be exhibited with a small amount compared to a large particle size, so the content in the resin composition can be reduced. In addition, by making the particle size small, the total interface area between the polysaccharide and the resin is significantly increased, and peeling at the interface can be suppressed, and it is believed that impact strength and bending strength can be improved.
[0026] In other words, the resin composition of the present invention is believed to be able to resolve the trilemma of flame retardancy, toughness (impact strength), and elasticity (flexural strength) while using materials that do not contain halogens and have a high bio-based content. [Brief description of the drawings]
[0027] [Figure 1] FIG. 1 is a schematic perspective view of a large-sized copying machine as an example of application of the flame-retardant resin molded article of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0028] The flame-retardant resin composition of the present invention is a flame-retardant resin composition containing at least a thermoplastic resin and particles, the particles containing a reaction product of a polysaccharide and a compound having a phosphate group, and the particles have an average primary particle size within the range of 1 to 1000 nm. This feature is a technical feature common to or corresponding to the following embodiments.
[0029] In an embodiment of the present invention, the polysaccharide is preferably an acidic polysaccharide from the viewpoint of improving flame retardancy, since the formation of char is promoted by a dehydration condensation reaction during combustion, and the resulting carbonized layer insulates against heat and blocks the diffusion of combustible gases.
[0030] In an embodiment of the present invention, the polysaccharide is preferably a basic polysaccharide from the viewpoint of improving flame retardancy, since the formation of char is promoted by a dehydration condensation reaction during combustion, and the resulting carbonized layer insulates against heat and blocks the diffusion of combustible gases.
[0031] In an embodiment of the present invention, the formation of char is promoted by a dehydration condensation reaction during combustion, and the resulting carbonized layer insulates against heat and blocks the diffusion of combustible gases, so that from the viewpoint of improving flame retardancy, it is preferable that the reaction product has at least an acidic functional group, a salt of the acidic functional group, or a group derived from the acidic functional group on the atoms constituting the sugar skeleton.
[0032] In an embodiment of the present invention, the formation of char is promoted by a dehydration condensation reaction during combustion, and the resulting carbonized layer insulates against heat and blocks the diffusion of combustible gases, so that the acidic functional group is preferably the phosphate group from the viewpoint of improving flame retardancy.
[0033] In an embodiment of the present invention, from the viewpoint of ease of molding, the softening point of the thermoplastic resin is preferably 200° C. or lower.
[0034] In an embodiment of the present invention, from the viewpoint of achieving excellent flame retardancy, toughness, and elasticity, the number average molecular weight of the polysaccharide is preferably within the range of 1,000 to 1,000,000.
[0035] The method for producing a flame-retardant resin composition of the present invention is a method for producing the flame-retardant resin composition, characterized in that it comprises a step of dissolving the polysaccharide in a compound having a phosphate group and reacting the polysaccharide in the liquid, and a step of adding the polysaccharide to an organic solvent to precipitate the reaction product.
[0036] The flame-retardant resin molded article of the present invention is characterized in that it is formed using the flame-retardant resin composition. The flame-retardant resin housing of the present invention is characterized by including the flame-retardant resin molded product described above. The electronic device of the present invention is characterized by comprising the flame-retardant resin molded product.
[0037] The present invention, its components, and embodiments for carrying out the present invention will be described in detail below. In this application, the symbol "to" is used to mean that the numerical values before and after the symbol "to" are included as the lower and upper limits.
[0038] 1. Overview of flame-retardant resin compositions The flame-retardant resin composition of the present invention is a flame-retardant resin composition containing at least a thermoplastic resin and particles, the particles containing a reaction product of a polysaccharide and a compound having a phosphate group, and the particles have an average primary particle size within the range of 1 to 1000 nm.
[0039] "Flame retardancy" is a type of heat resistance, and refers to the property of burning slowly but continuing to burn to a certain extent. Specifically, it means meeting the pass criteria in the UL94 standard established by the U.S. Underwriters Laboratories (UL), more specifically, meeting the pass criteria in UL94HB in the UL94 test (combustion test for plastic materials for equipment parts). In addition, it is preferable to meet the V-2 criteria in UL94V, more preferably the V-1 criteria, and even more preferably the V-0 criteria.
[0040] "Combustion" refers to an oxidation reaction accompanied by the generation of light and heat, and three elements are required for combustion: a combustible material, an oxygen source, and an ignition source. When resin (a combustible material) is ignited (an ignition source), the following phenomena A to C are repeated, and the combustion continues. a) High temperatures cause resin (a combustible material) to melt and decompose, generating large amounts of flammable gas. a) In a high temperature environment, flammable gases become radicals and accelerate chemical reactions with oxygen in the air (oxygen source), generating a considerable amount of light and heat. C) The heat generated maintains the high temperature, causing the resin to continue decomposing.
[0041] Therefore, combustion can be stopped by lowering the temperature, cutting off the supply of oxygen, or removing the flammable gas. Furthermore, by designing a resin so that such a phenomenon occurs when it is ignited, it is possible to impart flame retardancy to the resin.
[0042] Specifically, for example, water vapor is generated from inside the resin to lower the temperature, i.e., cooling is performed by absorbing a large amount of heat. A large amount of non-flammable gas is generated from inside the resin to lower the oxygen concentration and cut off the supply of oxygen. A barrier layer is formed by carbonizing the surface of the resin to cut off the supply of oxygen. The "barrier layer" is also called "char" or "carbonized layer."
[0043] In the present invention, it is believed that the resin composition contains polysaccharides, which can cause the above phenomenon and provide flame retardancy. It is also believed that the flame retardancy can be improved by containing polysaccharides in the form of a reaction product with a compound having a phosphoric acid group. In other words, it is believed that the flame retardancy of polysaccharides and the flame retardancy of phosphorus can be synergistically achieved by containing polysaccharides in the form of a reaction product with a compound having a phosphoric acid group. Furthermore, it is believed that the uniformity of the carbonized layer can be improved and the flame retardancy can be further improved by setting the average primary particle size of the particles containing this reaction product to be within the range of 1 to 1000 nm.
[0044] The resin composition can also be used as housings or parts for electronic devices by molding it into an appropriate form and shape.
[0045] 2. Composition of flame-retardant resin composition The flame-retardant resin composition of the present invention contains at least a thermoplastic resin and particles, and may further contain other flame retardants, etc., as necessary.
[0046] Each material constituting the flame-retardant resin composition will be described below. From the viewpoint of reducing the environmental load, the material used in the flame-retardant resin composition of the present invention is preferably a biomass material, but materials other than biomass materials may also be used.
[0047] The materials that make up the flame-retardant resin composition can be analyzed by energy dispersive X-ray spectroscopy (EDS), which irradiates a sample with an electron beam and detects the characteristic X-rays emitted from the atoms contained in the sample with a semiconductor detector, and the type and content of the elements contained in the sample can be determined from the energy level and intensity.
[0048] Whether or not a flame-retardant resin composition contains a halogen flame retardant or an antimony flame retardant can be analyzed by wavelength dispersive X-ray spectroscopy (WDS).
[0049] The bio-based mass content refers to the content (mass%) of biomass materials in all raw materials, and can be calculated in accordance with ISO 16620-4. The bio-based mass content of the flame-retardant resin composition can be calculated from the raw materials. It can also be measured by radiocarbon analysis or elemental analysis.
[0050] In the present invention, the reaction product of the polysaccharide and the compound having a phosphate group is contained in the flame-retardant resin composition in the form of particles having an average primary particle size in the range of 1 to 1000 nm. The particles may be composed of only the reaction product, or may be composed of the reaction product and other components. Hereinafter, the particles are also referred to as "polysaccharide-containing nanoparticles."
[0051] (1) Polysaccharide-containing nanoparticles The polysaccharide-containing nanoparticles according to the present invention contain a reaction product between a polysaccharide and a compound having a phosphate group, and have an average primary particle size within the range of 1 to 1000 nm.
[0052] In the present invention, the "reaction product of a polysaccharide and a compound having a phosphate group" refers to the entire compound finally obtained by reacting a polysaccharide with a compound having a phosphate group. Hereinafter, the reaction product of a polysaccharide and a compound having a phosphate group may also be simply referred to as the "reaction product".
[0053] The reaction products are believed to include polysaccharides into which phosphate groups have been introduced, salts of polysaccharides and compounds having phosphate groups, unreacted polysaccharides and compounds having phosphate groups, and the like. The polysaccharides having phosphate groups introduced therein may be phosphate esters obtained by reacting hydroxyl groups of the polysaccharides with phosphate groups, compounds obtained by reacting functional groups other than hydroxyl groups of the polysaccharides with phosphate groups, and acid anhydrides consisting of carboxyl groups and phosphate groups. As the salt of a polysaccharide with a compound having a phosphate group, a salt formed between a basic functional group of the polysaccharide and a phosphate group is considered.
[0054] From the viewpoints of flame retardancy, toughness and elasticity, the content of the polysaccharide-containing nanoparticles is preferably within the range of 5 to 50 mass %, and more preferably within the range of 10 to 35 mass %, relative to the total mass of the flame-retardant resin composition.
[0055] (1.1) Structure of polysaccharide-containing nanoparticles The polysaccharides and the reaction products of the polysaccharides and the compounds having a phosphate group will be described in turn.
[0056] (1.1.1) Polysaccharides In the present invention, the term "polysaccharide" refers to a substance formed by dehydration condensation of a large number of monosaccharides through glycosidic bonds, and is a general term for such substances. The type of monosaccharide that is the structural unit of a polysaccharide may be one type alone or two or more types may be used in combination.
[0057] In the present invention, "monosaccharide" refers to a sugar that cannot be hydrolyzed any further, and is a general term for such sugars. As for the structure, it is a chain polyhydroxy compound having an aldehyde group or a ketone group, and usually exists in a cyclic form in which the molecule is hemiacetalized. The monosaccharide is preferably a five-carbon sugar (pentose) or a six-carbon sugar (hexose), and more preferably a six-carbon sugar. In addition, in the present invention, "sugar skeleton" refers to the skeleton structure of a monosaccharide.
[0058] The degree of polymerization of the polysaccharide is preferably within the range of 50 to 20,000, more preferably within the range of 200 to 1,500, and further preferably within the range of 200 to 1,100.
[0059] The molecular weight of the polysaccharide is preferably within a range of 10,000 to 250,000, and more preferably within a range of 20,000 to 80,000, in terms of the weight average molecular weight based on polystyrene standards as determined by gel permeation chromatography (GPC).
[0060] The polysaccharide may be an acidic polysaccharide, a basic polysaccharide, or a neutral polysaccharide. In the present invention, a polysaccharide having an acidic functional group or the like in the molecule is referred to as an "acidic polysaccharide". A polysaccharide having a basic functional group or the like but not an acidic functional group or the like is referred to as a "basic polysaccharide". A polysaccharide having neither an acidic functional group or the like nor a basic functional group or the like is referred to as a "neutral polysaccharide". In other words, a polysaccharide having both an acidic functional group or the like and a basic functional group or the like corresponds to an acidic polysaccharide. The acidic functional group and the basic functional group do not include the hydroxyl group contained in the polysaccharide.
[0061] (1.1.1.1) Acidic polysaccharides In the present invention, polysaccharides having an acidic functional group, a salt of an acidic functional group, or a group derived from an acidic functional group are also referred to as "acidic polysaccharides". In the present invention, acidic functional groups, salts of acidic functional groups, and groups derived from acidic functional groups are also collectively referred to as "acidic functional groups, etc." An acidic polysaccharide molecule may have one type of acidic functional group, etc., or two or more types.
[0062] It is believed that the flame retardancy is further improved when the polysaccharide is an acidic polysaccharide. Although the mechanism of its expression or action is not clear, acidic polysaccharides have acidic functional groups, etc., and therefore, protons (H + ) is easily released. In addition, the distance between the proton and the hydroxyl group contained in the polysaccharide is relatively short. Therefore, it is considered that the dehydration condensation reaction is further promoted. In addition, it is considered that the temperature of the resin can be lowered by generating water vapor.
[0063] In the present invention, "acidic" means "to function as an acid", and "to function as an acid" means to function as an acceptor that receives an electron pair involved in a bond (Lewis definition). The function includes the addition of a proton (H + ) donor (Brønsted definition).
[0064] For example, when the type of monosaccharide that serves as a structural unit of a polysaccharide is only one type (A), the sugar skeleton corresponds to the skeleton structure of monosaccharide A. In this case, it is preferable that the atoms constituting the skeleton structure of monosaccharide A have an acidic functional group, a salt of an acidic functional group, or a group derived from an acidic functional group.
[0065] When the polysaccharide has two types of monosaccharides (A and B) as its constituent units, the sugar backbone corresponds to the backbone structures of monosaccharides A and B. In this case, it is preferable that either the backbone structure of monosaccharide A or monosaccharide B has an acidic functional group, a salt of an acidic functional group, or a group derived from an acidic functional group on a constituent atom.
[0066] Similarly, when the polysaccharide has three or more kinds of monosaccharides as its structural units, the saccharide skeleton corresponds to the skeleton structure of each monosaccharide. It is preferable that any of the skeleton structures of each monosaccharide has an acidic functional group, a salt of an acidic functional group, or a group derived from an acidic functional group on a constituent atom. It should be noted that the polysaccharide does not necessarily have to have a structure having repeating units.
[0067] In the present invention, since it is preferable to use a biomass material, it is preferable to use a natural polysaccharide as the polysaccharide. However, the polysaccharide according to the present invention is not limited to those of natural origin. In addition, the polysaccharide may be a natural polysaccharide that has been partially modified. Specifically, an acidic functional group or the like may be introduced into a polysaccharide that does not have an acidic functional group or the like, and the polysaccharide may be made into a derivative as necessary.
[0068] Polysaccharide derivatives include compounds in which atoms at certain sites are replaced with different atoms or substituents, specifically compounds in which hydrogen atoms in polysaccharides are replaced with substituents such as halogen groups (halogen atoms) or hydrocarbon groups. Further, compounds obtained by binding the polysaccharide to other compounds or other molecules via functional groups are also included, specifically, ester derivatives, ether derivatives, etc. obtained by reacting hydroxyl groups in the polysaccharide with compounds having functional groups reactive with hydroxyl groups, and crosslinked polysaccharides described later are also included.
[0069] Examples of the acidic functional group include a carboxy group (-COOH) and a sulfo group (-SO 3 H), thiocarboxy group (-CSOH), sulfino group (-SO 2 H), sulfeno group (-SOH), phospho group (-OP(=O)(OH) 2 ), phosphono group (-P(=O)(OH) 2 ), borono group (-B(OH) 2 Among them, from the viewpoint of flame retardancy, a carboxy group or a sulfo group is preferable. The acidic functional group is an acidic functional group having a sulfo group, for example, an acidic functional group in which a sulfo group is bonded to an oxygen atom (-O-SO 3 H).
[0070] Examples of salts of acidic functional groups include salts with alkali metals such as Li, Na, and K, salts with alkaline earth metals such as Mg, Ca, Sr, and Ba, and alkyl ammonium salts. 4 N + -", and each R is independently a hydrogen atom or an alkyl group having 1 to 3 carbon atoms, provided that at least one of the four Rs is an alkyl group.
[0071] Among them, a salt with a divalent or higher cation is preferable. By using a salt with a divalent or higher cation, a crosslinked structure is formed within or between molecules, resulting in a rigid structure. In addition, the heat resistance is dramatically improved, deformation of the resin composition can be prevented during melt kneading or molding, and the impact resistance and appearance are excellent.
[0072] From the viewpoint of achieving even better flame retardancy, the total number of acidic functional groups, etc. per monosaccharide unit in the acidic polysaccharide is preferably within the range of 0.20 to 1.50, more preferably within the range of 0.60 to 1.20, and even more preferably within the range of 0.60 to 1.00. Hereinafter, the total number of acidic functional groups, etc. per monosaccharide unit in the acidic polysaccharide is also simply referred to as the "number of acidic functional groups."
[0073] By setting the number of acidic functional groups to 0.20 or more, a dehydration condensation reaction is easily caused, and flame retardancy can be improved. Also, by setting the number of acidic functional groups to 1.50 or less, a decrease in dispersibility of the acidic polysaccharide in the resin composition can be suppressed, so that a carbonized layer can be formed uniformly on the surface of the resin composition, and flame retardancy can be improved.
[0074] The acidic polysaccharides may be used alone or in combination of two or more. When two or more acidic polysaccharides are used in combination, it is preferable that the number of acidic functional groups of the entire acidic polysaccharides is within the above range. However, the number of acidic functional groups of each of the combined acidic polysaccharides does not necessarily have to be within the above range. It is sufficient to select each acidic polysaccharide so that the number of acidic functional groups in the entire acidic polysaccharide obtained by combining them is within the above range.
[0075] In other words, when the acidic polysaccharide is a combination of two or more kinds of acidic polysaccharides, the number of acidic functional groups of each of the combined acidic polysaccharides does not necessarily have to be within the range of 0.20 to 1.50. The individual acidic polysaccharides may be selected so that the number of acidic functional groups of the combined acidic polysaccharide as a whole is within the range of 0.20 to 1.50. The number of acidic functional groups can be adjusted by appropriately introducing or separating the acidic functional groups, etc.
[0076] From the viewpoint of reducing the environmental load, the acidic polysaccharide is preferably a naturally occurring acidic polysaccharide. In addition, the number of acidic functional groups may be adjusted to a suitable number by appropriately introducing or separating acidic functional groups into or from the naturally occurring polysaccharide.
[0077] Examples of monosaccharides having an acidic functional group, specifically, monosaccharides having a carboxy group, include uronic acids such as glucuronic acid, iduronic acid, mannuronic acid, and galacturonic acid, etc. Examples of monosaccharides having a sulfooxy group include galactose-3-sulfate, etc. Examples of monosaccharides having both an acidic functional group and a basic functional group include muramic acid, N-acetylglucosamine-4-sulfate, N-acetylgalactosamine-4-sulfate, neuraminic acid, and N-acetylneuraminic acid. Examples of monosaccharides having a salt of an acidic functional group include salts of these. Examples of monosaccharides having a group derived from an acidic functional group include derivatives of these.
[0078] The type of monosaccharide that is the constituent unit of the polysaccharide is not particularly limited, but when there are two or more types of monosaccharides, it is preferable that at least one of them is the above-mentioned monosaccharide. The other monosaccharides may or may not correspond to the above-mentioned monosaccharides.
[0079] Other neutral monosaccharides not corresponding to the above monosaccharides include, for example, ribose, arabinose, xylose, lyxose, xylulose, ribulose, deoxyribose, glucose, mannose, galactose, fructose, sorbose, tagatose, fucose, fuculose, rhamnose, etc.
[0080] The other monosaccharide may be a monosaccharide having a basic functional group, etc. Examples of the monosaccharide having a basic functional group include glucosamine, galactosamine, mannosamine, etc. Examples of the monosaccharide having a salt of a basic functional group include salts of these, and examples of the monosaccharide having a group derived from a basic functional group include derivatives of these.
[0081] Examples of the derivatives include N-substituted products or salts with inorganic salts such as sulfuric acid, and organic acids such as acetic acid. Among these, N-substituted products with organic acids are preferred, and N-acyl substituted products are more preferred.
[0082] Examples of the N-acyl substitution product include N-formyl substitution product, N-acetyl substitution product, N-propionyl substitution product, N-butyryl substitution product, N-isobutyryl substitution product, N-valeryl substitution product, N-isovaleryl substitution product, N-pivaloyl substitution product, etc. Among them, N-acetyl substitution product is preferable, and examples of the N-acetyl substitution product include N-acetylglucosamine, N-acetylgalactosamine, N-acetylmannosamine, etc.
[0083] Examples of acidic polysaccharides composed of the above monosaccharides include pectin, alginic acid, propylene glycol alginate, carboxymethylcellulose, xanthan gum, gum arabic, karaya gum, psyllium, xylan, arabic acid, tragacanthic acid, khava gum, linseed acid, cellulose acid, lichenin uronic acid, gellan gum, rhamsan gum, welan gum, carrageenan, glycosaminoglycans (e.g., hyaluronic acid, chondroitin-4-sulfate, chondroitin-6-sulfate, dermatan sulfate, keratin sulfate, and heparin) and their salts.
[0084] Among these, from the viewpoint of being natural acidic polysaccharides, alginic acid, alginates, carrageenan, pectin, xanthan gum, or gellan gum is preferred, and further, from the viewpoint of improving flame retardancy and impact resistance, calcium alginate is more preferred.
[0085] The number of acidic functional groups per monosaccharide unit in an acidic polysaccharide can be determined from the molecular structural formula or by measurement and calculation using a neutralization titration method. The molecular structural formulas of alginic acid and carrageenan and a method for calculating the number of acidic functional groups from the molecular structural formulas will be described below.
[0086] For example, the molecular structure of alginic acid is shown in the following formula (A). As shown in formula (A), the acidic functional group of alginic acid is a carboxyl group (-COOH). From the molecular structure in formula (A), the number of acidic functional groups of alginic acid can be determined to be 1.00.
[0087] [ka]
[0088] For example, there are three types of carrageenan: κ-carrageenan, whose molecular structure is represented by the following formula (C1), ι-carrageenan, whose molecular structure is represented by the following formula (C2), and λ-carrageenan, whose molecular structure is represented by the following formula (C3). As shown in formulas (C1) to (C3), the acidic functional group possessed by carrageenan is a sulfo group, more specifically, an acidic functional group in which a sulfo group is bonded to an oxygen atom (-O-SO 3 In the formulae (C1) to (C3), the acidic functional group is in an ionized state (-OSO 3 -) is listed.
[0089] From the molecular structure in formula (C1), the number of acidic functional groups of κ-carrageenan can be 0.50, and from the molecular structure in formula (C2), the number of acidic functional groups of ι-carrageenan can be 1.00. In formula (C3), typically, R is H (30%) or SO 3 -(70%), and from the molecular structure in formula (C3), the number of acidic functional groups of λ-carrageenan can be determined to be 1.35.
[0090] [ka]
[0091] When the acidic polysaccharide is a combination of two or more kinds of acidic polysaccharides, the number of acidic functional groups can be calculated from the number of acidic functional groups per monosaccharide unit in each acidic polysaccharide and the molar ratio using the following formulas (1) and (2). Formula (1): Number of acidic functional groups = A 1 ×R 1 +A 2 ×R 2 +B 3 ×R 3 +…A n ×R n Formula (2):R n =B n / (B 1 +B 2 +B 3 +…B n )
[0092] However, the symbols are as follows: An: number of acidic functional groups per monosaccharide unit in each acidic polysaccharide Bn: The number of moles per monosaccharide unit in each acidic polysaccharide (calculated by dividing the mass of each acidic polysaccharide by the average molecular weight of the monosaccharide) Rn: mole ratio per monosaccharide unit in each acidic polysaccharide Here, n corresponds to the number of types of acidic polysaccharides.
[0093] The number of acidic functional groups can also be determined by the following method. When determining the number of acidic functional groups of the acidic polysaccharide contained in the flame-retardant resin composition, first, the acidic polysaccharide is extracted from the flame-retardant resin composition by an appropriate method. The molecular structure of the extracted acidic polysaccharide is identified by thermogravimetric analysis, infrared spectroscopy (IR), or the like.
[0094] [Method for measuring the number of acidic functional groups] The number of acidic functional groups per monosaccharide unit in acidic polysaccharides can be measured, for example, by neutralization titration. In the measurement by neutralization titration, about 1 g of the extracted acidic polysaccharide is precisely weighed out, made into a slurry, and treated with a strongly acidic ion exchange resin. Next, a 0.1 mol / L aqueous solution of sodium hydroxide is added, and the change in pH is observed to obtain a titration curve. The number of moles of sodium hydroxide required from the start of the titration to the inflection point of the titration curve is equal to the number of moles of the acid of the acidic polysaccharide used in the titration. The number of acidic functional groups per monosaccharide unit can be calculated from the number of moles of the acid obtained and the molecular structure.
[0095] In addition, in the case of carboxymethyl cellulose, the number of acidic functional groups can be calculated by measuring the degree of substitution of the carboxymethyl group. Carboxymethyl cellulose is an acidic polysaccharide obtained by introducing carboxymethyl groups into cellulose. The number of acidic functional groups of carboxymethyl cellulose can be adjusted to a suitable range by adjusting the production conditions.
[0096] Carboxymethyl cellulose can be produced by a known production method, specifically, the method described in JP 2000-34301 A, which includes a step of reacting cellulose with an alkali at a temperature range of 20 to 50° C. to produce alkali cellulose, and a step of reacting alkali cellulose with monochloroacetic acid to produce carboxymethyl cellulose.
[0097] Alternatively, it can be produced by another method, for example, the method described in JP 2012-12553 A, in which cellulose, an alkaline agent, and a monohaloacetic acid or a salt thereof are mixed together, and then the mixture is heated within a range of 40 to 90° C. to cause a reaction.
[0098] In either method, the number of acidic functional groups in the resulting carboxymethyl cellulose can be adjusted by adjusting the amount of monochloroacetic acid or monohaloacetic acid added to cellulose.
[0099] The structural formula of carboxymethylcellulose can be represented, for example, by the following general formula (CMC): In formula (CMC), each R is independently H or CH 2 COOH. For example, when averaged within a molecule, 0.2 to 1.5 of the R in the formula (CMC) are CH 2 By adjusting the structure so that the monomer unit is COOH, it is possible to obtain carboxymethyl cellulose having superior flame retardancy.
[0100] [ka]
[0101] Examples of acidic polysaccharides in which acidic functional groups or the like have been introduced into cellulose include, in addition to carboxymethyl cellulose, carboxyalkyl cellulose (e.g., having a carbon number in the range of 2 to 3), sulfoethyl cellulose, hydroxypropyl methyl cellulose acetate succinate, etc. In addition, in the present invention, acidic polysaccharides in which acidic functional groups or the like have been introduced into polysaccharides other than cellulose that do not have acidic functional groups or the like, such as starch, agarose, guar gum, etc., can also be used.
[0102] [Method for measuring the degree of substitution of carboxymethyl groups] In the case of carboxymethyl cellulose, the number of acidic functional groups can be calculated by measuring the degree of substitution of the carboxymethyl group. The method is shown below. The number of acidic functional groups of other acidic polysaccharides can also be calculated by referring to the following method.
[0103] The degree of substitution of the carboxymethyl group can be calculated by measuring the amount of a base such as sodium hydroxide required to neutralize the carboxymethyl cellulose in the sample. If the carboxymethyl ether group is in the form of a salt, it is converted to carboxymethyl cellulose before the measurement.
[0104] (Conversion to carboxymethyl cellulose) Accurately weigh out approximately 2.0 g of the sample and place it in a 300 mL Erlenmeyer flask with a stopper. Add 100 mL of nitric acid methanol (a solution of 1000 mL of methanol and 100 mL of special-grade concentrated nitric acid) to the Erlenmeyer flask. Shake the mixture at room temperature for 3 hours to convert the carboxymethylcellulose salt into carboxymethylcellulose.
[0105] (Measurement of the degree of substitution of carboxymethyl cellulose) Weigh out approximately 1.5 g of completely dried carboxymethylcellulose and place it in a 300 mL Erlenmeyer flask with a stopper. Wet the carboxymethylcellulose with 15 mL of 80% methanol. Then, add 100 mL of 0.1 N sodium hydroxide (NaOH) solution to the Erlenmeyer flask and shake at room temperature for 3 hours. This solution is diluted with 0.1 N sulfuric acid (H 2 SO 4 ) to back-titrate the excess NaOH.
[0106] The degree of substitution of carboxymethyl cellulose is calculated using the following formulas (i) and (ii). Formula (i): A = (100 × f 1 -a×f 2 ) / mass of sample (g) Formula (ii): Degree of substitution = (162×A) / (10000-58×A)
[0107] However, the symbols and values are as follows: A: The amount (mL) of 0.1 N sodium hydroxide solution required to neutralize 1 g of sample (bone-dried carboxymethylcellulose) a: Titration volume of 0.1N sulfuric acid (mL) f 1 : Factor of 0.1N sodium hydroxide solution f 2 : Factor of 0.1N sulfuric acid 100: Amount of 0.1N sodium hydroxide solution used (mL) 162: Anhydroglucose (C 6 H 10 O 5 ) molecular weight 58:CH 2 The difference in molecular weight between COOH (molecular weight 59) and H (molecular weight 1)
[0108] The molecular weight of the acidic polysaccharide is preferably within the range of 1,000 to 1,000,000, more preferably within the range of 1,000 to 800,000, in terms of the number average molecular weight based on polystyrene standards determined by gel permeation chromatography (GPC). By having a number average molecular weight of 1,000 or more, strength can be imparted to the flame-retardant resin composition. In addition, by having a number average molecular weight of 1,000,000 or less, the hydroxyl group and the phosphate group of the polysaccharide molecule are adjacent to each other, thereby obtaining sufficient flame retardancy.
[0109] The acidic polysaccharides used may be commercially available products. Commercially available acidic polysaccharides include, for example, "Kimica Acid SA" (alginic acid, manufactured by Kimica), "Snow Algin SAW-80" (calcium alginate, manufactured by Kimica), "Kimica Algin I-3G" (sodium alginate, manufactured by Kimica), "Carrageenan WG-108" (carrageenan, manufactured by Sansho), "Pectin, citrus-derived" (pectin, manufactured by Fujifilm Wako Pure Chemical Industries), "Xanthan Gum" (xanthan gum, manufactured by Tokyo Chemical Industry Co., Ltd.), "Gellan Gum" (gellan gum, manufactured by Fujifilm Wako Pure Chemical Industries), and "Aqualon (registered trademark) CMC" (carboxymethylcellulose, manufactured by ASHland).
[0110] (1.1.1.2) Basic polysaccharides In the present invention, among polysaccharides having a basic functional group, a salt of a basic functional group, or a group derived from a basic functional group, those not corresponding to acidic polysaccharides are also referred to as "basic polysaccharides". In the present invention, basic functional groups, salts of basic functional groups, and groups derived from basic functional groups are also collectively referred to as "basic functional groups, etc." A basic polysaccharide molecule may have one type of basic functional group, etc., or two or more types.
[0111] It is believed that the flame retardancy is further improved by using a basic polysaccharide as the polysaccharide. Although the mechanism of expression or action of this effect has not been clarified, it is believed that the presence of basic functional groups, etc., inhibits combustion due to the inert gas generated during combustion and promotes the dehydration condensation reaction.
[0112] Examples of monosaccharides having a basic functional group include glucosamine, galactosamine, mannosamine, etc. Examples of monosaccharides having a salt of a basic functional group include salts of these, and examples of monosaccharides having a group derived from a basic functional group include derivatives of these.
[0113] Examples of the derivatives include N-substituted products or salts with inorganic salts such as sulfuric acid, and organic acids such as acetic acid. Among these, N-substituted products with organic acids are preferred, and the above-mentioned N-acyl substituted products are more preferred.
[0114] When the basic polysaccharide has two or more kinds of monosaccharides as its constituent units, it is preferable that at least one of them is a monosaccharide having a basic functional group, etc. The other monosaccharides may or may not fall under the category of monosaccharides having a basic functional group, etc. Examples of other monosaccharides not falling under the category of monosaccharides having a basic functional group, etc. include the neutral monosaccharides.
[0115] Examples of basic polysaccharides composed of monosaccharides having the above-mentioned basic functional groups include chitosan and chitin.
[0116] (1.1.1.3) Neutral polysaccharide In the present invention, a polysaccharide that does not have either an acidic functional group or a basic functional group is also referred to as a "neutral polysaccharide". Examples of monosaccharides that serve as constituent units of neutral polysaccharides include the above-mentioned neutral monosaccharides. Examples of neutral polysaccharides include cellulose, tamarind seed gum, guar gum, locust bean gum, starch, and pullulan.
[0117] (1.1.2) Reaction products of polysaccharides with compounds having phosphate groups In the present invention, the "reaction product of a polysaccharide with a compound having a phosphate group" refers to the entire compound finally obtained by reacting a polysaccharide with a compound having a phosphate group.
[0118] The mechanism by which phosphorus exerts its flame retardant properties or its action mechanism has not been clarified, but it is speculated as follows. During combustion, phosphorus combines with oxygen and water in the air to produce phosphoric acid, which then mixes with the carbonized polysaccharides to form char, which forms an insulating layer and thus inhibits combustion.
[0119] In the present invention, the polysaccharide is used as a reaction product of the polysaccharide and a compound having a phosphate group. In other words, in the polysaccharide-containing nanoparticles, the polysaccharide and the phosphate group are relatively close to each other. Therefore, it is considered that a synergistic effect of flame retardancy due to phosphorus and polysaccharide is obtained.
[0120] (1.1.2.1) Compounds containing a phosphate group The compound having a phosphate group is not particularly limited as long as it can adjust the particle size to within the range of 1 to 1000 nm in the production of polysaccharide-containing nanoparticles described below.
[0121] Examples of compounds having a phosphoric acid group include phosphoric acid and its salts, phosphorous acid and its salts, dehydrated condensed phosphoric acid and its salts, and anhydrous phosphoric acid (diphosphorus pentoxide). Phosphoric acid of various purities can be used, for example, 100% phosphoric acid (orthophosphoric acid) or 85% phosphoric acid. However, as described above, it is preferable to use a high purity, since it is preferable to carry out the reaction without using a solvent. Examples of phosphorous acid include 99% phosphorous acid (phosphonic acid). Dehydrated condensed phosphoric acid is phosphoric acid in which two or more molecules are condensed by a dehydration reaction, and examples of such as pyrophosphoric acid and polyphosphoric acid can be mentioned.
[0122] Examples of phosphates, phosphites, and dehydrated condensed phosphates include lithium salts, sodium salts, potassium salts, and ammonium salts of phosphoric acid, phosphorous acid, or dehydrated condensed phosphoric acid. These can be neutralized to various degrees. Among them, from the viewpoint of high efficiency of introduction of phosphate groups, phosphoric acid, sodium salts of phosphoric acid, potassium salts of phosphoric acid, and ammonium salts of phosphoric acid are preferred, and phosphoric acid, sodium dihydrogen phosphate, disodium hydrogen phosphate, and ammonium dihydrogen phosphate are more preferred.
[0123] (1.1.2.2) Reaction products As will be described in detail later, the polysaccharide is dissolved in a compound having a phosphate group and reacted with the compound. The reaction products are believed to include polysaccharides into which phosphate groups have been introduced, salts of polysaccharides and compounds having phosphate groups, unreacted polysaccharides and compounds having phosphate groups, and the like.
[0124] Examples of polysaccharides having phosphate groups introduced therein include phosphate esters obtained by reacting hydroxyl groups of polysaccharides with phosphate groups. Examples of other compounds include compounds obtained by reacting functional groups other than hydroxyl groups of polysaccharides with phosphate groups. Specifically, examples of such compounds include acid anhydrides obtained by reacting carboxyl groups of polysaccharides with phosphate groups.
[0125] From the viewpoint of facilitating the reaction between the acidic functional group and the polysaccharide during combustion, it is preferable that the reaction product has at least an acidic functional group, a salt of the acidic functional group, or a group derived from the acidic functional group on the atoms constituting the sugar skeleton. In addition, when the acidic functional group is a phosphate group, phosphorus and the polysaccharide can easily react with each other.
[0126] Examples of salts of polysaccharides with compounds having a phosphate group include salts formed between a basic functional group of the polysaccharide and a phosphate group. From the viewpoint of bringing the polysaccharide and the phosphate group into close proximity, it is preferable that the reaction product contains a larger amount of the polysaccharide into which a phosphate group has been introduced, or a salt of the polysaccharide and a compound having a phosphate group.
[0127] (1.2) Average primary particle size of polysaccharide-containing nanoparticles The average primary particle size of the polysaccharide-containing nanoparticles according to the present invention is preferably within the range of 1 to 1000 nm, more preferably within the range of 5 to 1000 nm, and even more preferably within the range of 10 to 500 nm. By being within the above range, the uniformity of the char layer formed during combustion is improved.
[0128] The average primary particle size of the polysaccharide-containing nanoparticles can be measured by the following method. A sample of the flame-retardant resin composition is prepared. A scanning electron microscope (SEM) "JSM-7401F" (manufactured by JEOL Ltd.) set at 1000x magnification is used to take a photograph, and the photographic image is captured by a scanner. Then, an image processing and analyzing device "LUZEX (registered trademark) AP" (manufactured by Nireco Corporation) is used to binarize the polysaccharide-containing nanoparticles in the photographic image. 100 polysaccharide-containing nanoparticles are randomly selected, and their Feret's diameters in the horizontal direction are calculated, and the average value is taken as the average primary particle size. Instead of the SEM, a transmission electron microscope (TEM) may be used.
[0129] (2)Thermoplastic resin The flame-retardant resin composition of the present invention contains a thermoplastic resin. By containing a thermoplastic resin, the composition can be molded into a desired shape using a known melt-kneading method, and is easy to handle.
[0130] From the viewpoint of reducing the environmental load, the resin according to the present invention is preferably a biomass resin, but the present invention can also be applied to resins other than biomass resins. Also, a biomass resin and a resin other than biomass resin may be used in combination.
[0131] The content of the thermoplastic resin is preferably within a range of 30 to 95 mass %, more preferably within a range of 40 to 90 mass %, and even more preferably within a range of 50 to 80 mass %, relative to the total mass of the flame-retardant resin composition.
[0132] The type of thermoplastic resin is not particularly limited, but from the viewpoints of being able to suppress decomposition of polysaccharides and of achieving excellent strength and appearance in addition to flame retardancy, it is preferable that the softening point of the resin is 200° C. or lower.
[0133] In the present invention, the "softening point" refers to the temperature at which a material begins to soften and deform due to an increase in temperature. Specifically, the softening point refers to the temperature measured by a method in accordance with "JIS K 2207 6.4 Softening Point Test Method (Ring and Ball Method)".
[0134] Examples of thermoplastic resins include styrene-based resins, polycarbonates, aromatic polyesters, polyphenylene sulfite, olefin-based resins, polyamideimides, polyetheretherketones, polyethersulfones, polyimides, vinyl chloride-based resins, polyamides, polyacetals, acrylic-based resins, polystyrene-based thermoplastic elastomers, polyolefin-based thermoplastic elastomers, polyurethane-based thermoplastic elastomers, 1,2-polybutadiene-based thermoplastic elastomers, ethylene-vinyl acetate copolymer-based thermoplastic elastomers, fluororubber-based thermoplastic elastomers, and chlorinated polyethylene-based thermoplastic elastomers. These may be used alone or in combination of two or more.
[0135] In addition, a thermoplastic biomass resin may be used as the thermoplastic resin. Examples of the thermoplastic biomass resin include polypropylene, aliphatic polyester, polyamino acid, polyvinyl alcohol, polyalkylene glycol, and copolymers containing these. In addition, a thermoplastic biomass resin may be combined with a resin other than the thermoplastic biomass resin to provide a thermoplastic resin having the advantages of both.
[0136] Examples of styrene-based resins include polystyrene, syndiotactic polystyrene, acrylonitrile-styrene copolymers (AS resins), and acrylonitrile-butadiene-styrene copolymers (ABS resins).
[0137] Examples of aromatic polyesters include aromatic polyesters having a structure in which an aromatic dicarboxylic acid or its ester derivative component is linked to a diol component such as an aliphatic diol or an alicyclic diol by an ester reaction.Specific examples include polyethylene terephthalate, polypropylene terephthalate, polybutylene terephthalate, polyethylene naphthalate, polybutylene naphthalate, polyethylene-1,2-bis(phenoxy)ethane-4,4'-dicarboxylate, and copolymer polyesters such as polyethylene isophthalate / terephthalate, polybutylene terephthalate / isophthalate, and polybutylene terephthalate / decane dicarboxylate.
[0138] Examples of the aliphatic polyester include polyoxyacids, which are copolymers of oxyacids, and polycondensates of aliphatic diols and aliphatic dicarboxylic acids. Examples of the polyoxyacids include poly-L-lactic acid (PLLA), poly-D-lactic acid (PDLA), random copolymers of L-lactic acid and D-lactic acid, polylactic acids such as stereocomplexes of L-lactic acid and D-lactic acid, polycaprolactone, polyhydroxybutyric acid, and polyhydroxyvaleric acid. Examples of the polycondensates of aliphatic diols and aliphatic dicarboxylic acids include polyethylene succinate, polybutylene succinate (PBS), and polybutylene adipate.
[0139] From the viewpoint of strength and ease of handling, the thermoplastic resin is preferably a resin having an aromatic ring. Examples of the resin having an aromatic ring include styrene-based resins, polycarbonates, and aromatic polyesters, and among these, styrene-based resins are preferred.
[0140] Commercially available thermoplastic resins include "Panlite (registered trademark)" (polycarbonate, manufactured by Teijin Chemicals), "Duranex (registered trademark)" (polybutylene terephthalate, manufactured by Polyplastics), "Clapet (registered trademark)" (polyethylene terephthalate, manufactured by Kuraray), "Aramin" (polyamide, manufactured by Toray), "Lacia (registered trademark)" (polylactic acid, manufactured by Mitsui Chemicals), and "Terramac (registered trademark)" (polylactic acid, manufactured by Unitika Ltd.).
[0141] Commercially available styrene-based resins include "CLEAREN (registered trademark)" (SBC resin: styrene-butadiene copolymer, manufactured by Denki Kagaku Kogyo Co., Ltd.), "ASAFLEX (registered trademark)" (SBC resin, manufactured by Asahi Kasei Chemicals Corporation), "Styrolux (registered trademark)" (SBC resin, manufactured by BASF), "PSJ (registered trademark)-Polystyrene" (styrene-based resin, manufactured by PS Japan Co., Ltd.), and "TOYOLAC (registered trademark)" (ABS resin, manufactured by Toray Industries, Inc.). In addition, examples of commercially available mixed resins containing styrene-based resins include "Multilon (registered trademark)" (a mixed resin of polycarbonate / ABS resin, manufactured by Teijin Limited).
[0142] (3) Other flame retardants The flame-retardant resin composition of the present invention may contain other flame retardants besides the polysaccharide-containing nanoparticles, as long as the effect of the present invention is not impaired. In the present invention, since the flame retardancy of the polysaccharide-containing nanoparticles is very high, even if other flame retardants are contained, the content thereof can be reduced.
[0143] Examples of other flame retardants include polysaccharides other than polysaccharide-containing nanoparticles, phosphorus-based flame retardants, metal hydroxides, intumescent flame retardants, etc. Among these, phosphorus-based flame retardants are preferred from the viewpoint of increasing the flame retardancy of the polysaccharide-containing nanoparticles and from the viewpoint of low content of petroleum resources.
[0144] The content of the phosphorus-based flame retardant is preferably within a range of 5 to 20 mass %, more preferably within a range of 5 to 10 mass %, based on the total mass of the flame-retardant resin composition. By being within the above range, the obtained molded product can have both high flame retardancy and high strength.
[0145] Examples of phosphorus-based flame retardants include phosphazene compounds, phosphates, phosphoric acid esters, polyphosphates, phosphinates, phosphinic acid esters, phosphonates, and phosphonic acid esters. These may be used alone or in combination of two or more.
[0146] (4) Other additives The flame-retardant resin composition of the present invention may contain other additives depending on the purpose, provided that the effects of the present invention are not impaired.
[0147] Examples of additives include antioxidants, fillers, crystal nucleating agents, etc. The content of the additives is preferably within a range of 0 to 30% by mass, and more preferably within a range of 0 to 20% by mass, based on the total mass of the flame-retardant resin composition.
[0148] 3. Method for producing flame-retardant resin composition The method for producing a flame-retardant resin composition of the present invention is a method for producing the above-mentioned flame-retardant resin composition, characterized in that it comprises a step of dissolving the polysaccharide in the compound having a phosphate group and reacting the polysaccharide in the liquid, and a step of adding the polysaccharide to an organic solvent to precipitate the reaction product.
[0149] (3.1) Method for preparing polysaccharide-containing nanoparticles The method for producing the polysaccharide-containing nanoparticles according to the present invention is not particularly limited, but as described above, it is extremely difficult to obtain nano-sized particles using conventional techniques. Therefore, it is preferable to have a step of dissolving the polysaccharide in a compound having a phosphate group and reacting it in the liquid, and a step of adding it to an organic solvent to precipitate the reaction product.
[0150] The mechanism by which nano-sized particles are obtained or the mechanism of action is not clear, but is speculated as follows.
[0151] For example, the phosphorus-containing polysaccharide used in Patent Document 1 is subjected to a phosphoric esterification reaction using a solvent, and precipitated in water. Specifically, a cellulose derivative is dissolved in a solvent, and a reaction reagent is added dropwise thereto. The resulting reaction solution is added dropwise to distilled water to precipitate the reaction product.
[0152] On the other hand, the polysaccharide-containing nanoparticles according to the present invention are precipitated by reacting a polysaccharide with a compound having a phosphate group without using a solvent and adding the reactant to an organic solvent. Specifically, the polysaccharide is dissolved in a compound having a phosphate group and reacted in the solution. In the solution, the higher the concentration of the polysaccharide, the better. The resulting reaction solution is then dropped into a large amount of well-stirred organic solvent to precipitate the reactant.
[0153] In order to obtain nanoparticles as the final particles, it is necessary to generate and precipitate the reaction product, remove the solvent, wash, isolate, etc., while suppressing aggregation. In particular, polysaccharides have a high affinity for water because they have many polar groups such as hydroxyl groups, and therefore easily incorporate water molecules. Furthermore, when polysaccharides incorporate water molecules, they tend to become soft and easily aggregate.
[0154] Therefore, by not using a solvent in the step of generating the reaction product, the solvent remains in the resulting particles, which can prevent the particles from aggregating. Also, by not using water in the step of precipitating the reaction product, it is believed that the particles can be prevented from aggregating.
[0155] The polysaccharide-containing nanoparticles can be prepared by the following procedure, but is not limited thereto. 1) A step of dissolving polysaccharides in a compound having a phosphate group and reacting them in the solution 2) A process in which the reaction product is precipitated by adding it to an organic solvent. 3) A process of washing the precipitated reaction product. 4) Drying the reaction product
[0156] In the step 1), in order not to use a solvent, it is preferable that the polysaccharide and the compound having a phosphate group are combined in such a way that the polysaccharide is soluble in the compound having a phosphate group.
[0157] In the step 2), from the viewpoint of suppressing aggregation of particles, it is preferable to precipitate the reaction product by adding it to an organic solvent.
[0158] As an example of a method for producing polysaccharide-containing nanoparticles according to the present invention, a method for producing particles containing a reaction product of carboxymethyl cellulose and phosphoric acid will be described.
[0159] Carboxymethylcellulose (1 part by mass) is added to stirred phosphoric acid (3 parts by mass) and heated to 100°C. As the temperature rises, carboxymethylcellulose dissolves in phosphoric acid. This reaction solution is heated and stirred at 100°C for 8 hours to allow the reaction to proceed. After the reaction is completed, this reaction solution is thoroughly cooled to room temperature. The cooled reaction solution is poured into ethanol (10 parts by mass) with thorough stirring to precipitate crystals. The precipitated crystals are filtered, pure water (10 parts by mass) is added, and the mixture is stirred at room temperature. The crystals are filtered from this mixture and washed with ethanol. The crystals are dried in a dryer at 60°C overnight to obtain colored crystals (1 part by mass).
[0160] In this preparation method, the combination of carboxymethyl cellulose and phosphoric acid allows the carboxymethyl cellulose to be dissolved in phosphoric acid without using a solvent, and the solution is heated to cause the carboxymethyl cellulose and phosphoric acid to react with each other.
[0161] After that, the reaction liquid is poured into ethanol to precipitate crystals, thereby suppressing the incorporation of water molecules into the interior of the reaction product particles. Also, components that are easily soluble in water can be incorporated into the interior of the particles. In other words, salts of polysaccharides and compounds having phosphate groups can also be incorporated into the interior of the particles. Then, by washing the precipitated crystals with pure water, some of the components that are easily soluble in water and present on the surface of the particles are removed. The particles are washed with ethanol and dried.
[0162] The resulting particles are aggregates of nano-sized particles. However, these aggregates are relatively easy to disintegrate, and can be disintegrated to nano-sized particles by kneading with a thermoplastic resin. The degree of disintegration varies depending on the type of thermoplastic resin and the melt-kneading conditions, and can be adjusted appropriately. In other words, the size of the particles can be adjusted by the type of thermoplastic resin and the melt-kneading conditions.
[0163] (3.2) Mixing of materials The method of mixing the polysaccharide-containing nanoparticles, the thermoplastic resin and other additives to produce the flame-retardant resin composition is not particularly limited. Among them, it is preferable to use the melt-kneading method from the viewpoint of being able to disintegrate the polysaccharide-containing nanoparticles and adjust them to a desired particle size. The melt-kneading method can be a known method. Hereinafter, a method for producing the flame-retardant resin composition of the present invention using the melt-kneading method will be described.
[0164] Examples of the melt-kneading method include a method in which the thermoplastic resin, the polysaccharide-containing nanoparticles, and other additives are premixed using various mixers such as a tumbler or a high-speed mixer known as a Henschel mixer, and then melt-kneaded using a kneading device such as a Banbury mixer, a roll, a plastograph, a single-screw extruder, a twin-screw extruder, or a kneader.
[0165] Among them, from the viewpoint of production efficiency, it is preferable to use an extruder, and it is more preferable to use a twin-screw extruder. The material is melt-kneaded using the extruder, and the kneaded product is extruded in a strand shape, and then the kneaded product can be processed into a shape such as pellets or flakes.
[0166] It is preferable to thoroughly dry each material before premixing in which the materials are mixed in advance. The drying temperature is not particularly limited, but is preferably within the range of 60 to 120°C. The drying time is not particularly limited, but is preferably within the range of 2 to 6 hours. In addition, from the viewpoint of facilitating the drying, it is preferable to dry under reduced pressure. The above drying may be performed after premixing.
[0167] The melt-kneading temperature is not particularly limited, but is preferably selected appropriately depending on the type of resin used, and is preferably within the range of 150 to 280°C. Here, the melt-kneading temperature corresponds to the cylinder temperature in a kneading device such as a twin-screw extruder. In addition, the cylinder temperature refers to the highest cylinder temperature when multiple temperatures are set in the cylinder of the kneading device. The kneading pressure is not particularly limited, but is preferably within the range of 1 to 20 MPa.
[0168] When an extruder is used for melt kneading, the screw rotation speed is not particularly limited, but is preferably within the range of 100 to 500 rpm.
[0169] The discharge rate from the kneading device is not particularly limited, but from the viewpoint of sufficient melt-kneading, it is preferably within the range of 10 to 100 kg / hr, and more preferably within the range of 20 to 70 kg / hr.
[0170] The kneaded product melt-kneaded by the kneading device in the above-mentioned method is preferably cooled after being extruded from the kneading device. The cooling method is not particularly limited, and examples thereof include a method of immersing the kneaded product in water within a range of 0 to 60°C to cool it with water, a method of cooling it with gas within a range of -40 to 60°C, and a method of contacting it with a metal within a range of -40 to 60°C.
[0171] The form and shape of the flame-retardant resin composition of the present invention is not particularly limited, and may be, for example, a solid such as powder, granules, tablets, pellets, flakes, or fibers, or a liquid.
[0172] 4. Flame-retardant resin molded products The flame-retardant resin molded article of the present invention is characterized in that it is formed using the above-mentioned flame-retardant resin composition. The flame-retardant resin molded article of the present invention is formed using the above-mentioned flame-retardant resin composition, so that the resin molded article can be imparted with flame retardancy and can also have sufficient toughness and elasticity.
[0173] The flame-retardant resin molded article of the present invention can be obtained by melting and molding the above-mentioned flame-retardant resin composition in various molding machines. The molding method can be appropriately selected depending on the shape and application of the molded article, and examples thereof include injection molding, extrusion molding, compression molding, blow molding, calendar molding, inflation molding, etc. In addition, a sheet-like or film-like molded article obtained by extrusion molding, calendar molding, etc. may be subjected to secondary molding such as vacuum forming or pressure molding.
[0174] The flame-retardant resin molded article is not particularly limited, and examples thereof include parts in the fields of home appliances and automobiles (electrical and electronic parts, electrical components, exterior parts, interior parts, etc.), various packaging materials, household goods, office supplies, piping, agricultural materials, etc.
[0175] 5. Flame-retardant resin housings and electronic devices A flame-retardant resin housing of the present invention includes the above-mentioned flame-retardant resin molded article. Also, an electronic device of the present invention is equipped with the above-mentioned flame-retardant resin molded article. That is, the flame-retardant resin molded article may be used as a housing for accommodating an electronic device or as a component in an electronic device or the like. In the present invention, the term "electronic device" refers to an electrical product that utilizes electronic engineering technology.
[0176] The article to be housed in the flame-retardant resin casing of the present invention is not particularly limited, but it is preferable to house an electronic device, etc. In addition, the flame-retardant resin casing of the present invention can also be applied to casings that are generally preferably made of flame-retardant resin.
[0177] Examples of electronic devices include, but are not limited to, computers, scanners, copiers, printers, facsimile machines, office automation equipment such as multifunction machines called MFPs (Multi Function Peripherals) that combine the functions of these devices, and digital printing systems for commercial printing.
[0178] A specific example of an electronic device of the present invention is shown in Fig. 1. Fig. 1 is a schematic perspective view of a large-sized copying machine 10 having the flame-retardant resin molded article of the present invention as an exterior part. As shown in Fig. 1, the large-sized copying machine 10 is exteriorly covered with exterior parts G1 to G9. The flame-retardant resin molded article of the present invention can be used for such exterior parts. EXAMPLES
[0179] The present invention will be described in detail below with reference to examples, but the present invention is not limited thereto. In the examples, the terms "parts" and "%" are used, but they represent "parts by mass" or "% by mass" unless otherwise specified. In the following examples, operations were carried out at room temperature (25° C.) unless otherwise specified.
[0180] 1. Preparation of resin composition (1) Preparation of polysaccharide-containing particles (1.1) Preparation of polysaccharide-containing particles A1 Carboxymethylcellulose (1 part by mass) was added to stirred phosphoric acid (3 parts by mass) and heated to 100°C. As the temperature increased, the carboxymethylcellulose dissolved in the phosphoric acid. This reaction solution was heated and stirred at 100°C for 8 hours to allow the reaction to proceed. After the reaction was completed, this reaction solution was thoroughly cooled to room temperature. The cooled reaction solution was poured into ethanol (10 parts by mass) with thorough stirring to precipitate crystals. The precipitated crystals were filtered, and pure water (10 parts by mass) was added and stirred at room temperature. The crystals were filtered from this mixture and washed with ethanol. The crystals were dried in a dryer at 60°C overnight, and then colored crystals (1 part by mass) of polysaccharide-containing particles A1 were obtained. The carboxymethyl cellulose used was manufactured by Kimika Co., Ltd. and had a number average molecular weight of 750,000.
[0181] (1.2) Preparation of polysaccharide-containing particles A2 Polysaccharide-containing particles A2 were prepared in the same manner as in the preparation of polysaccharide-containing particles A1, except that the number average molecular weight of carboxymethylcellulose was changed to 450.
[0182] (1.3) Preparation of polysaccharide-containing particles A3 Polysaccharide-containing particles A3 were prepared in the same manner as in the preparation of polysaccharide-containing particles A1, except that the amount of ethanol used in precipitating the crystals was changed to 3 parts by mass.
[0183] (1.4) Preparation of polysaccharide-containing particles A4 Polysaccharide-containing particles A4 were prepared in the same manner as in the preparation of polysaccharide-containing particles A1, except that the number average molecular weight of carboxymethylcellulose was changed to 1.8 million.
[0184] (1.5) Preparation of polysaccharide-containing particles A5 Polysaccharide-containing particles A5 were prepared in the same manner as in the preparation of polysaccharide-containing particles A1, except that the number average molecular weight of carboxymethylcellulose was changed to 1,000.
[0185] (1.6) Preparation of polysaccharide-containing particles A6 Polysaccharide-containing particles A6 were prepared in the same manner as in the preparation of polysaccharide-containing particles A1, except that the number average molecular weight of carboxymethylcellulose was changed to 1,000,000.
[0186] (1.7) Preparation of polysaccharide-containing particles A7 In the preparation of the polysaccharide-containing particles A1, the carboxymethyl cellulose (acidic polysaccharide) was changed to iota-carrageenan (acidic polysaccharide) having a number-average molecular weight of 750,000. Except for this, the polysaccharide-containing particles A7 were prepared in the same manner.
[0187] (1.8) Preparation of polysaccharide-containing particles B1 In the preparation of the polysaccharide-containing particles A1, the carboxymethyl cellulose was changed to chitosan (basic polysaccharide) having a number average molecular weight of 750,000. Except for this, the polysaccharide-containing particles B1 were prepared in the same manner.
[0188] (1.9) Preparation of polysaccharide-containing particles C1 Polysaccharide-containing particles C1 were produced in the same manner as in the production of polysaccharide-containing particles A1, except that carboxymethyl cellulose was changed to cellulose (neutral polysaccharide) having a number average molecular weight of 750,000.
[0189] (2) Preparation of resin compositions 1 to 17 As a pre-drying before kneading, the thermoplastic resin, the polysaccharide-containing particles, and the phosphorus-based flame retardant were each dried at 80°C for 4 hours. Then, the components were weighed out at the component ratios (mass%) shown in Table I and dry-blended. Next, the mixture obtained by dry blending was supplied from the raw material supply port (hopper) of a twin-screw extrusion kneader "Thermo Scientific HAAKE Rheomex PTW 16 OS Twin-screw Extruder" (manufactured by Thermo Fisher Scientific Co., Ltd.). Then, melt-kneading was performed under the conditions of a cylinder temperature of 180°C and a screw rotation speed of 400 rpm. The molten resin after kneading was cooled and then pelletized with a pelletizer to obtain resin compositions 1 to 17.
[0190] The thermoplastic resins and phosphorus-based flame retardants used are as follows: PC(50): Polycarbonate with a bio-based mass content of 50% by mass PC(60): Polycarbonate with a bio-based mass content of 60% by mass PLA: Polylactic acid ABS: Acrylonitrile-butadiene-styrene copolymer PA-6: Nylon 6 (softening point 225°C) Phosphorus-based flame retardant: Aromatic condensed phosphate ester flame retardant "PX-200" (manufactured by Daihachi Chemical Industry Co., Ltd.)
[0191] Table I below shows the composition and bio-based mass content of the resin composition. For the polysaccharide-containing particles Cf1, the carboxymethyl cellulose used in the preparation of the polysaccharide-containing particles A1 was used as it was. The "-" in the table indicates that the corresponding ingredient is not contained. "Resin ratio" in the table refers to the content [mass %] of the corresponding component relative to the total mass of the thermoplastic resin. The "Bio-based mass content" in the table was calculated in accordance with ISO 16620-4.
[0192] [Table 1]
[0193] 2. Measurement
[0194] (1) Detection of bromine (Br), chlorine (Cl), and antimony (Sb) The obtained pellets were crushed and compression molded to prepare samples, which were then subjected to semi-quantitative analysis using a wavelength dispersive X-ray fluorescence analyzer (WDX) "ZSX PrimusIV" (manufactured by Rigaku Corporation).
[0195] (2) Average primary particle size of polysaccharide-containing particles The fracture surface of the resin composition obtained after the evaluation of impact strength described later was used as a sample. The fracture surface was photographed using a scanning electron microscope (SEM) "JSM-7401F" (manufactured by JEOL Ltd.) set at 1000x magnification, and the photographic image was captured by a scanner. Then, the polysaccharide-containing nanoparticles in the photographic image were binarized using an image processing and analysis device "LUZEX (registered trademark) AP" (manufactured by Nireco Corporation). 100 polysaccharide-containing nanoparticles were randomly selected, and their Feret's diameters in the horizontal direction were calculated, and the average value was taken as the average primary particle size.
[0196] 3. Evaluation (1) Flame retardancy Each of the obtained pellet-like resin compositions was dried at 80° C. for 4 hours. Then, using an injection molding machine "Babyplast" (manufactured by Rambaldi), molding was performed at a cylinder temperature of 180° C. and a mold temperature of 50° C. to obtain a rectangular test piece having a length of 125 mm, a width of 13 mm, and a thickness of 1.6 mm.
[0197] The obtained test pieces were conditioned for 48 hours in a temperature-controlled room at 23°C and 50% humidity. Then, a flame retardancy test was conducted in accordance with the UL94 test (combustion test for plastic materials for equipment parts) established by Underwriters Laboratories (UL) in the United States. The test method used was the UL94V test method, and the flame retardancy was evaluated according to the following criteria. A to AAA were deemed to be acceptable for practical use.
[0198] AAA:V-0 (passed) AA:V-1 (passed) A:V-2 (passed) B: Nonstandard
[0199] (2) Impact strength Each of the obtained pellet-like resin compositions was dried at 80° C. for 4 hours. Then, using an injection molding machine "Babyplast" (manufactured by Rambaldi), the resin was molded at a cylinder temperature of 180° C. and a mold temperature of 50° C. to obtain a test piece having a length of 80 mm, a width of 10 mm, and a thickness of 4 mm. Test pieces were molded by 15 consecutive shots, after which 10 shots were discarded. The Izod impact strength of the obtained 15 test pieces was measured in accordance with JIS K7110:1999, and evaluated according to the following criteria. A to AA were deemed to be acceptable for practical use.
[0200] AA: 10kJ / m 2 That's all. A: 8kJ / m 2 More than 10kJ / m 2 is less than. B: 8kJ / m 2 is less than.
[0201] (3) Bending strength Each of the obtained pellet-like resin compositions was dried at 80° C. for 4 hours. Then, using an injection molding machine “J55ELII” (manufactured by Japan Steel Works, Ltd.), molding was performed at a cylinder temperature of 180° C. and a mold temperature of 50° C. to obtain a test piece having a length of 80 mm, a width of 10 mm, and a thickness of 4 mm.
[0202] Test pieces were molded by 15 consecutive shots, with 10 shots being discarded. The flexural strength variation XTS [%] of the obtained 15 test pieces was calculated using the following formula and evaluated according to the following criteria. A to AAA were deemed to be acceptable for practical use. (Formula)XTS[%]=(TR max -TR min ) / (TR av ) x 100 In the above formula, TR max TR indicates the maximum bending strength [MPa] of 15 molded products. min TR indicates the minimum bending strength [MPa] of 15 molded products. av indicates the average bending strength [MPa] of 15 molded products. The bending strength of the molded products is a value measured in accordance with JIS K7171:2022.
[0203] AAA:TR av is 20 MPa or more and XTS is less than 0.5%. AA:TR av is 20 MPa or more, and XTS is 0.5% or more and less than 5%. A:TR av is 20 MPa or more, and XTS is 5% or more and less than 15%. B: TRav is less than 20 MPa, or XTS is 15% or more.
[0204] The measurement results and evaluation results are shown in Table II below. In the table, "None" in "Br, Cl, Sb detected" indicates that none of Br, Cl, or Sb was detected. For resin composition 12, the molding temperature (cylinder temperature) was relatively high at 200° C., and the polysaccharide-containing nanoparticles were burned and deformed, so the particle size could not be measured. In order to obtain an average primary particle size of the polysaccharide-containing particles as shown in Table II, the composition of the various materials was changed as shown in Table I, and the kneading time was also appropriately changed.
[0205] [Table 2]
[0206] From the above evaluation results, it is apparent that the flame-retardant resin composition of the present invention is excellent in flame retardancy, impact strength and flexural strength.
[0207] A comparison of resin compositions 1, and 15 to 17 shows that the flame retardancy is improved by using an acidic polysaccharide or a basic polysaccharide as the polysaccharide.
[0208] Comparison of resin compositions 1, 6, and 9 to 11 shows that the number average molecular weight of the acidic polysaccharide (carboxymethyl cellulose) is within the range of 1,000 to 1,000,000, resulting in excellent flame retardancy, impact strength, and flexural strength. [Explanation of symbols]
[0209] 10 Large-format copy machine G1~G9 Exterior parts
Claims
1. A flame-retardant resin composition containing at least a thermoplastic resin and particles, the particles contain a reaction product of a polysaccharide and a compound having a phosphate group; The average primary particle size of the particles is within the range of 1 to 1000 nm. A flame-retardant resin composition comprising:
2. The polysaccharide is an acidic polysaccharide. The flame-retardant resin composition according to claim 1 .
3. The polysaccharide is a basic polysaccharide. The flame-retardant resin composition according to claim 1 .
4. The reaction product has at least an acidic functional group, a salt of the acidic functional group, or a group derived from the acidic functional group on an atom constituting the sugar skeleton.
3. The flame-retardant resin composition according to claim 1 or 2.
5. The acidic functional group is a phosphate group.
5. The flame-retardant resin composition according to claim 4.
6. The softening point of the thermoplastic resin is 200° C. or less. The flame-retardant resin composition according to any one of claims 1 to 3.
7. The number average molecular weight of the polysaccharide is within the range of 1,000 to 1,000,000.
3. The flame-retardant resin composition according to claim 1 or 2.
8. A method for producing the flame-retardant resin composition according to any one of claims 1 to 3, comprising the steps of: A step of dissolving the polysaccharide in the compound having a phosphate group and reacting the polysaccharide in the solution; and and adding the reaction product to an organic solvent to precipitate the reaction product. A method for producing a flame-retardant resin composition comprising the steps of:
9. A flame-retardant resin molded product, which is formed using the flame-retardant resin composition according to any one of claims 1 to 3.
10. A flame-retardant resin housing comprising the flame-retardant resin molded product according to claim 9.
11. 10. An electronic device comprising the flame-retardant resin molded article according to claim 9.
Citation Information
Patent Citations
Flame-retardant resin composition and molded article
JP2010031230A
Cited By
Preparation process of organic fireproof flame retardant
CN120248219A