Method for manufacturing ABS resin containing biogenic organic matter

A stepwise heating process with specific material ratios in an extrusion molding machine addresses viscosity issues in ABS resin blends, enabling stable and efficient production of pellets from bamboo powder and talc mixed with ABS resin.

JP2024163480APending Publication Date: 2024-11-22UNION IND CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023079108
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-12
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The extrusion molding of ABS resin mixed with biologically derived organic powders like bamboo powder and inorganic talc powder faces challenges due to differences in viscosity and physical properties, leading to brittle strands and production inefficiencies.

Method used

A method involving a stepwise heating process in an extrusion molding machine with specific temperature settings and material ratios, including at least 40-50% ABS resin, 2-14% biologically derived organic powder, and 28-38% inorganic powder, ensures smooth extrusion by using a screw to knead and melt the mixture, followed by cooling and cutting into pellets.

Benefits of technology

This method allows for stable and continuous extrusion of rod-shaped strands that can be cut into pellets, preventing breakage and enhancing production efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024163480000001_ABST
    Figure 2024163480000001_ABST
Patent Text Reader

Abstract

To provide a method for manufacturing ABS resin blended with biologically derived organic matter that can be smoothly extruded by using an extrusion molding machine, in which biologically derived organic matter powder such as bamboo powder and inorganic matter powder such as talc are blended into ABS resin.SOLUTION: A mixed resin powder containing 40 to 50 wt.% of ABS resin powder, 2 to 14 wt.% of biologically derived organic powder, and 28 to 38 wt.% of inorganic powder, and an extrusion molding machine 10 are prepared. An MVR (cm3 / 10 min) of ABS resin is set to 4 to 6. The mixed resin powder fed into a cylinder 30 is conveyed by a screw 40 in a conveying direction, and a heating temperature of the cylinder 30 is divided into four or more stages, with the heating temperature of a first stage being 100°C or higher, and from a second stage onwards the heating temperature is increased or maintained in stages, with the heating temperature of a final stage being 230°C or higher. A strand (molded product) S extruded in a rod shape from a die 60 is solidified by cooling, and then cut into pellets.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing ABS resin containing organic matter of biological origin, which is suitable for use in the production of ABS resin containing organic matter of biological origin, such as bamboo powder. [Background technology]

[0002] Bamboo has antibacterial properties, and for this reason, various molded products are made from synthetic resins containing bamboo powder. To enhance the antibacterial properties of bamboo, molded products are also made by mixing highly antibacterial dolomite (lime) powder and scallop shell powder in addition to the bamboo powder.

[0003] Conventionally, polyolefin-based synthetic resins (such as polypropylene) and biodegradable resins have been used as the synthetic resins constituting the above-mentioned molded products.

[0004] On the other hand, it is desirable to use ABS resin as a synthetic resin. ABS resin has a relatively high heat resistance, is resistant to external impacts (it has impact resistance similar to rubber), is easy to process (it can be molded using various molding methods such as injection molding and extrusion molding, can be cut, bonded, and welded, and can also be subjected to various surface treatments such as plating and painting), and has a high design potential (it has excellent surface gloss and colorability). [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Utility Model Registration No. 3158617 Summary of the Invention [Problem to be solved by the invention]

[0006] However, when attempting to use an extrusion molding machine to mix large amounts of biological organic powder such as bamboo powder and inorganic talc powder with ABS resin, extrude the molten material into a rod shape (spaghetti-like), and then cut it into small pieces after cooling to produce pellets, the viscosity and physical properties of the molten ABS resin, which contains biological organic and inorganic substances, are significantly different from the viscosity and physical properties when pellets are made from ABS resin alone, making it difficult to mold the material under the conventional molding conditions for ABS resin alone.

[0007] For example, because a large amount of the above-mentioned bamboo powder and talc powder is added in addition to ABS resin, there were various problems, such as the rod-shaped extruded molded product (hereinafter referred to as "strand") being brittle and breaking apart, and the rod-shaped molded product not being extruded at a stable speed. If the strand breaks, it takes time to repair, which reduces production efficiency. In addition, in the case of ABS resin, extrusion molding is more difficult than extrusion molding of a polyolefin synthetic resin mixed with bamboo powder.

[0008] The present invention has been made in consideration of the above-mentioned points, and its purpose is to provide a method for producing ABS resin containing bio-organic matter, which can smoothly and reliably extrude and mold, using an extrusion molding machine, a bio-organic matter mixed resin powder obtained by kneading ABS resin with a bio-organic matter powder such as bamboo powder and an inorganic matter powder such as talc. [Means for solving the problem]

[0009] The method for producing a bio-derived organic ABS resin according to the present invention comprises preparing a bio-derived organic mixed resin powder obtained by mixing at least 40 to 50% by weight of ABS resin, 2 to 14% by weight of a bio-derived organic powder, and 28 to 38% by weight of an inorganic powder, and an extrusion molding machine having at least a cylinder for introducing the bio-derived organic mixed resin powder, a screw rotatably inserted into the cylinder for conveying the bio-derived organic mixed resin powder while kneading it, a plurality of heating means for gradually heating the cylinder in the conveying direction of the bio-derived organic mixed resin powder to melt the ABS resin in the bio-derived organic mixed resin powder, and a die connected to the tip of the cylinder for forming and extruding the molten and kneaded resin melted and kneaded by the screw and the heating means into a desired shape, and 3 The present invention is characterized in that the heating temperature of the cylinder is divided into four or more stages in the conveying direction of the mixed resin powder fed into the cylinder by the screw, the heating temperature of the cylinder is 100°C or higher in the first stage, and the heating temperature is increased or maintained stepwise from the second stage onwards, and the heating temperature of the final stage is 230°C or higher, and the mixed resin powder fed into the cylinder is melted and kneaded by the stepwise heating and the rotation of the screw, and then extrusion-molded from the die. According to the present invention, it is possible to smoothly and reliably extrude a bio-organic mixed resin powder obtained by mixing ABS resin with a bio-organic powder and an inorganic powder in the above-mentioned mixing ratio. In particular, when a strand is extruded from a die into a thin rod shape, it is possible to prevent the strand from being brittle and breaking, or from being unable to be extruded at a stable speed.

[0010] In addition to the above characteristics, the present invention is characterized in that the heating by the heating means is performed in stages at temperatures of 110°C, 220°C, 230°C, 230°C, and 235°C, starting from the first stage in the conveying direction. By using the heating step of the present invention, it becomes possible to carry out extrusion molding of a molded product smoothly and reliably.

[0011] In addition to the above features, the present invention is characterized in that the biological organic powder is bamboo powder. According to the present invention, by using bamboo powder as the biological organic powder, it is possible to provide the molded product with antibacterial effects and ethylene gas adsorption effects.

[0012] In addition to the above features, the present invention is characterized in that the inorganic powder is talc powder.

[0013] In addition to the above features, the present invention is characterized in that a rod-shaped molded product (strand) is continuously extruded from the die, solidified by cooling, and then cut into pellets. Effect of the Invention

[0014] According to the present invention, it is possible to smoothly and reliably extrude a powder of a bio-derived organic mixed resin obtained by kneading ABS resin with a powder of a bio-derived organic material and a powder of an inorganic material using an extruder. [Brief description of the drawings]

[0015] [Figure 1] This is a flow diagram showing an example of a process for producing pellets of ABS resin containing bamboo powder, etc. [Diagram 2] FIG. 1 is a schematic overall perspective view of an extrusion molding machine 10. [Diagram 3] 1 is a schematic cross-sectional view of a main portion of an extrusion molding machine 10. FIG. [Figure 4] FIG. 2 is a diagram showing the test results when bamboo-mixed resin powder was extruded using an extrusion molding machine 10. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0016] Hereinafter, an embodiment of the present invention will be described in detail with reference to the drawings. Figure 1 is a flow diagram showing an example of a manufacturing process for ABS resin pellets containing bamboo powder as a biological organic powder. As shown in the figure, to manufacture ABS resin pellets containing bamboo powder, first, ABS resin pellets, bamboo powder, talc powder, lime or shell powder, and additive powder are prepared (steps 1-1, 1-2, 1-3, 1-4, 1-5).

[0017] The ABS resin used was in pellet form.

[0018] The bamboo powder used was made by grinding bamboo into a powder with an average particle size of about 200 μm (or less).

[0019] Talc is an inorganic mineral called talc, and is a smooth material. Its chemical name is magnesium silicate hydrate (Mg3Si4O 10 Talc is a substance that has the lowest hardness (Mohs hardness 1) of any inorganic mineral, has excellent heat resistance, and is also chemically stable.

[0020] The lime used was, for example, calcined dolomite, which was powdered to an average particle size of about 200 μm (or less). Calcined dolomite has high antibacterial properties and the ability to suppress the generation of dioxins when incinerated.

[0021] As the shell, for example, scallop shell powder was used. Scallop shells baked at high temperature were used, which were then powdered to an average particle size of about 200 μm (or less). Scallop shell powder has strong antibacterial properties. Although the antibacterial properties are weaker, in some cases, unbaked scallop shell powder may be used.

[0022] The range of mixing ratios of each raw material is as follows: ABS resin powder 40~50% by weight Bamboo powder 2~14% by weight Talc powder 28-38% by weight Lime or shell powder 2-14% by weight Additives: Small amount

[0023] The specific blending ratios of the raw materials in this embodiment (sample No. 1 described below) were as follows: ABS resin powder 45% by weight Bamboo powder 8% by weight Talc powder 33% by weight Dolomite powder 8% by weight Additives 6% by weight

[0024] Next, the bamboo mixed resin powder obtained by mixing the raw materials is put into the hopper 20 of the extrusion molding machine 10 described below and kneaded (Step 2).

[0025] Next, the bamboo-mixed resin powder kneaded in the hopper 20 is introduced into the cylinder 30 of the extrusion molding machine 10 described below, where it is heated, melted, kneaded, and extruded into a thin rod shape (step 3).

[0026] Next, the strands S, which are the extruded rod-shaped products, are cooled and solidified by cooling means 70, which will be described below (step 4).

[0027] Next, the cooled and solidified strand S is cut into short pieces by a cutter of a pelletizer 80 described below, thereby obtaining pelletized molding material 100 (step 5).

[0028] FIG. 2 is a schematic perspective view of the entire extrusion molding machine 10, and FIG. As shown in these figures, the extrusion molding machine 10 is equipped with a hopper 20 into which the bamboo mixed resin powder is input, a cylinder 30 into which the bamboo mixed resin powder is introduced from the hopper 20, a screw 40 rotatably stored within the cylinder 30 and transports the bamboo mixed resin powder while kneading it, multiple (five) heating means 50-1, 2, 3, 4, 5 which gradually heat the cylinder 30 in the direction in which the bamboo mixed resin powder is transported to melt the ABS resin in the bamboo mixed resin powder, a die 60 connected to the tip of the cylinder 30 and forms the molten material melted and kneaded by the heating means 50-1, 2, 3, 4, 5 into the desired shape (rod shape in this example) and extrudes it, a cooling means 70 which cools the multiple strands S (four in this example) formed and extruded by the die 60, and a pelletizer 80 which finely cuts the strands S cooled by the cooling means 70 into pellets.

[0029] The extruder 10 is a single-screw extruder using only one screw 40. The heating means 50-1, 2, 3, 4, 5 are attached in series to the outer circumference of the cylinder 30 in the longitudinal direction. Each of the heating means 50-1, 2, 3, 4, 5 can independently heat the cylinder 30 at a desired set temperature. The die 60 is a device for continuously forming rod-shaped strands S by passing a molten material through a plurality of small circular holes. The cooling means 70 is composed of a water tank filled with cooling water (not shown), and the strands S extruded from the die 60 are cooled and solidified by immersing them in the water in the water tank. The pelletizer 80 is a device for cutting the cooled strands S into pellets.

[0030] When extrusion molding of bamboo-mixed resin powder was performed using the extrusion molding machine 10 configured as described above, it was confirmed that, depending on the heating temperature by the heating means 50-1, 2, 3, 4, 5 and the fluidity of the ABS resin when molten, smooth extrusion molding was not possible, and the produced pellets were burned, foamed, or brittle.

[0031] The inventors of the present application have tested various extrusion molding conditions, such as the heating temperatures of the heating means 50-1, 2, 3, 4, and 50-5 and the fluidity of the ABS resin when melted, and have found the optimal conditions, which will be described below.

[0032] FIG. 4 is a diagram showing the results when bamboo-mixed resin powder was extruded by the extruder 10 under various conditions.

[0033] The inventors of this application initially thought that since the bamboo mixed resin powder contains more than half of the materials other than ABS resin, there was a risk that the viscosity would become too high if it was mixed with molten ABS resin, so they conducted tests using ABS resin with a low viscosity when molten (MVR = 20). Here, MVR stands for melt volume rate, a value in the ISO (JIS) standard that indicates the fluidity of thermoplastic resin when molten, and it is measured by the amount of resin extruded per 10 minutes from a die of a specified diameter installed at the bottom of the cylinder under the constant temperature and load conditions specified in the standard. As shown in sample No. 4, a bamboo-mixed resin powder consisting of 45 parts by weight of ABS resin with an MVR of 20, 8 parts by weight of bamboo powder, 33 parts by weight of talc, 8 parts by weight of lime, and 6 parts by weight of other additives not shown in the figure was added from the hopper 20, and while rotating the screw 40, the temperatures of the heating means 50-1, 2, 3, 4, 5 were set to 100°C, 160°C, 185°C, 190°C, and 190°C, respectively, to heat, melt, and knead the material, and a rod-shaped strand S was extruded from the die 60.

[0034] At this time, the strand S had a smooth surface, but was not extruded smoothly (it came out quickly and then stopped), and when it was passed through the cooling water of the cooling means 70, it hardened immediately and became brittle.

[0035] In order to solve the above problems, the heating temperature was increased, and as shown in sample No. 3, the temperatures of heating means 50-1, 2, 3, 4, and 5 were set to 100°C, 170°C, 195°C, 200°C, and 205°C, respectively, to heat, melt, and knead the material, and then a strand S was extruded from a die 60.

[0036] At this time, the strand S was not smoothly extruded from the nozzle hole of the die 60 (it came out quickly and then stopped). As a result, the extruded strand S was torn off, and even when introduced into the pelletizer 80, uniform pellets could not be produced.

[0037] In order to achieve smooth extrusion of a molded product, as shown in sample No. 2, the blending ratio of ABS resin was increased to 48 parts by weight, and the heating temperature was further increased overall, with the temperatures of heating means 50-1, 2, 3, 4, and 5 being set to 165°C, 190°C, 200°C, 200°C, and 190°C, respectively, for heating, melting, and kneading, and strand S was extruded from die 60.

[0038] At this time, the strand S was not brittle and could be cut by the pelletizer 80. However, the smooth extrusion of the strand S from the nozzle hole of the die 60 was still not good (it came out quickly and then stopped).

[0039] In the above tests, the ratio of ABS resin in the bamboo mixed resin powder was set to less than half, so tests were repeated using a resin with good fluidity when melted (a resin with a low MVR). However, we changed our thinking and decided to use a resin with low fluidity when melted, and instead conduct tests under conditions where the heating temperature was further increased. We also returned the ratio of the materials used to the same as in sample No. 4.

[0040] That is, as shown in sample No. 1, the MVR of the ABS resin was set to 5, while the heating temperatures of the heating means 50-1, 2, 3, 4, and 5 were further increased to 110°C, 220°C, 230°C, 230°C, and 235°C, respectively, for heating, melting, and kneading, and the strand S was extruded from the die 60.

[0041] At this time, the strand S was strong, the strand S was easily extruded from the nozzle hole of the die 60, and the strand S was smoothly cut by the pelletizer 80, allowing the production of uniform pellets.

[0042] From the above test results, it was found that the heating conditions when extrusion molding bamboo mixed resin powder (ABS resin powder: 45% by weight, bamboo powder: 8% by weight, talc powder: 33% by weight, lime powder: 8% by weight, additives: 6% by weight) are preferably such that the heating temperature of the cylinder 30 is divided into five stages in the conveying direction in which the bamboo mixed resin powder is conveyed by the screw 40, and the powder is melted and kneaded in stages by heating means 50-1, 2, 3, 4, 5, from the first stage to 110°C, 220°C, 230°C, 230°C, and 235°C, respectively.

[0043] In the above test, bamboo was used as the biological organic matter, but similar results were obtained with various other biological organic matter, such as wheat bran, coffee grounds, shell ginger, and wood such as cedar and cypress.

[0044] In the above test, lime was used, but instead of (or together with) powdered shells may be used. As the shells, scallop shells are particularly preferred because they have antibacterial properties.

[0045] In the above test, the blending ratio of the bio-organic mixed resin powder was 45% by weight of ABS resin powder, 8% by weight of bamboo powder, 33% by weight of talc powder, 8% by weight of lime powder, and 6% by weight of additives, but there is a certain range for this blending ratio, and it is considered that the same results as the above embodiment can be obtained if the blending ratio is at least 40-50% by weight of ABS resin powder, 2-14% by weight of bio-organic powder, and 28-38% by weight of inorganic powder. It is also considered that the same results as the above embodiment can be obtained if the blending ratio of lime powder (or shell powder) is 1-12% by weight.

[0046] In the above test, the heating temperatures of heating means 50-1, 2, 3, 4, 5 were set to 110°C, 220°C, 230°C, 230°C, 235°C, respectively, from the first stage. However, it is considered that there is a certain width within this temperature range, and if the heating temperature in the first stage is set to 100°C or higher, and the heating temperature is increased or maintained stepwise from the second stage onwards, and the heating temperature in the final stage is set to 230°C or higher, it is considered that results similar to those of the above embodiment can be obtained.

[0047] In addition, in the above test, the MVR (cm 3 / 10 min) was set to 5, but it is believed that if it is set to 4 to 6, the same results as in the above embodiment will be obtained.

[0048] In the above test, the heating means 50-1, 2, 3, 4, 5 were in five stages, but it is considered that if there are at least four stages or more, the same results as in the above embodiment will be obtained.

[0049] Although the embodiment of the present invention has been described above, the present invention is not limited to the above embodiment, and various modifications are possible within the scope of the claims and the technical ideas described in the specification and drawings. Any shape, structure, or material not directly described in the specification and drawings is within the scope of the technical ideas of the present invention as long as it has the functions and effects of the present invention. For example, the extrusion molding machine 10 used in the above embodiment produces pellets by installing a pelletizer 80 after producing strands S using a die 60 and a cooling means 70, but a cutting method in which the resin extruded from the die is immediately cut on the spot may be used.

[0050] In addition, the embodiments described above and shown in each drawing can be combined with each other as long as there is no contradiction in the purpose, configuration, etc. In addition, even a part of the description in the above description and the description in each drawing can be an independent embodiment, and the embodiment of the present invention is not limited to one embodiment that combines the description in the above description and each drawing. [Explanation of symbols]

[0051] 10 Extrusion molding machine 20 Hopper 30 Cylinder 40 Screw 50(50-1,2,3,4,5) Heating means 60 Dice 70 Cooling means 80 Pelletizer 100 Molding material (pellets) S Strand

Claims

1. a bio-derived organic mixed resin powder obtained by mixing at least 40 to 50% by weight of ABS resin, 2 to 14% by weight of a bio-derived organic powder, and 28 to 38% by weight of an inorganic powder; an extrusion molding machine having at least a cylinder for introducing the biological organic mixed resin powder, a screw rotatably inserted into the cylinder for conveying the biological organic mixed resin powder while kneading it, a plurality of heating means for gradually heating the cylinder in the conveying direction of the biological organic mixed resin powder to melt the ABS resin in the biological organic mixed resin powder, and a die connected to the tip of the cylinder for forming and extruding the molten and kneaded resin melted and kneaded by the screw and the heating means into a desired shape; Prepare The MVR (cm) of the ABS resin constituting the mixed resin powder 3 / 10 min) is 4 to 6, The heating temperature of the cylinder is divided into four or more stages in the conveying direction of the mixed resin powder fed into the cylinder by the screw, the heating temperature of the cylinder being 100° C. or higher in the first stage, and the heating temperature is increased or maintained in stages from the second stage onwards, until the heating temperature of the final stage is 230° C. or higher; A method for producing ABS resin containing biological organic matter, characterized in that the mixed resin powder fed into the cylinder is melted and kneaded by the stepwise heating and rotation of the screw, and then extruded through the die.

2. A method for producing the ABS resin containing the biological organic matter according to claim 1, A method for producing an ABS resin containing biological organic matter, characterized in that the heating by the heating means is carried out in stages at 110°C, 220°C, 230°C, 230°C, and 235°C, starting from the first stage in the conveying direction.

3. A method for producing the ABS resin containing the biological organic matter according to claim 1, A method for producing ABS resin containing biological organic matter, characterized in that the biological organic matter powder is bamboo powder.

4. A method for producing the ABS resin containing the biological organic matter according to claim 1 or 3, The method for producing an ABS resin containing a biologically derived organic substance, wherein the inorganic powder is talc powder.

5. A method for producing the ABS resin containing the biological organic matter according to claim 1, A method for producing an ABS resin containing biological organic matter, characterized in that a molded product is continuously extruded in a rod shape from the die, solidified by cooling, and then cut into pellets.

Citation Information

Patent Citations

  • Molded products and manufacturing equipment using bamboo

    JP3158617U