Gallium nitride single crystal substrate

The manufacturing method for gallium nitride single crystal substrates, involving germanium doping and controlled growth conditions, effectively reduces dislocations with large strain fields, enhancing device characteristics by minimizing etch pits and improving substrate quality.

JP2024163495APending Publication Date: 2024-11-22SUMITOMO CHEM CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023079178
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-12
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

Existing gallium nitride single crystal substrates face challenges in accurately identifying and reducing dislocations that adversely affect device characteristics, as etch pit size is influenced by strain fields and impurities, making it difficult to determine dislocation type and impact on device performance.

Method used

A manufacturing method for gallium nitride single crystal substrates involves growing a first layer with a high concentration of germanium doping in the inclined interface region, followed by a second layer with controlled growth conditions to reduce dislocations with large strain fields, resulting in a substrate with a low density of etch pits exceeding 4a in diameter.

Benefits of technology

The method significantly reduces dislocations with large strain fields, leading to improved device characteristics by minimizing etch pits and enhancing the abundance ratio of dislocations with small strain fields, thereby improving the quality of devices fabricated on these substrates.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024163495000001_ABST
    Figure 2024163495000001_ABST
Patent Text Reader

Abstract

To improve property of a device fabricated on a gallium nitride single crystal substrate.SOLUTION: A gallium nitride single crystal substrate has a diameter of 50 mm or more and in which a low index crystal plane nearest to a principal surface is a (0001) plane, where an etch pit formed when the principal surface is subjected to etching with an alkaline etchant has a density of less than 1×106 cm-2 and, when a diameter of a first peak that appears on a side of the smallest diameter of the peaks appearing in a histogram of a diameter of an etch pit represents a, the sum total of etch pits of which diameter exceeds 4a is 1 / 1000 or less of the number of etch pits constituting the first peak.SELECTED DRAWING: Figure 5
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a gallium nitride single crystal substrate. [Background technology]

[0002] For example, Patent Document 1 describes a process for preparing a base substrate made of a single crystal of a Group III nitride semiconductor, having a mirror-finished primary surface, with the crystal plane with the lowest index closest to the primary surface being the (0001) plane, and epitaxially growing a single crystal of a Group III nitride semiconductor having a top surface with the (0001) plane exposed directly on the primary surface of the base substrate, thereby generating a plurality of recesses on the top surface composed of inclined interfaces other than the (0001) plane, and gradually expanding the inclined interfaces toward the top surface of the base substrate, thereby forming a (0001)-oriented inclined interface. The disclosed method for manufacturing a gallium nitride single crystal substrate includes a first step of growing a first layer having a surface composed only of inclined interfaces by eliminating the (0001) plane from the top surface, and a second step of epitaxially growing a single crystal of a Group III nitride semiconductor on the first layer, eliminating the inclined interfaces, and growing a second layer having a mirror-finished surface, wherein in the first step, a plurality of recesses are generated in the top surface of the single crystal and the (0001) plane is eliminated, thereby forming a plurality of valleys and a plurality of peaks on the surface of the first layer. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2020-33211 A Summary of the Invention [Problem to be solved by the invention]

[0004] An object of the present invention is to improve the characteristics of devices fabricated on a gallium nitride single crystal substrate. [Means for solving the problem]

[0005] According to one aspect of the present invention, A gallium nitride single crystal substrate having a diameter of 50 mm or more and a low-index crystal plane closest to the primary surface being the (0001) plane, The density of etch pits formed when etching the main surface with an alkaline etching solution is 1×10 6 cm -2 is less than The present invention provides a gallium nitride single crystal substrate, in which when the diameter of a first peak appearing on the smallest diameter side among peaks appearing in a histogram of etch pit diameters is taken as a, the total number of etch pits having a diameter exceeding 4a is 1 / 1000 or less of the number of etch pits constituting the first peak. Effect of the Invention

[0006] According to the present invention, it is possible to improve the characteristics of devices fabricated on a gallium nitride single crystal substrate. [Brief description of the drawings]

[0007] [Figure 1] FIG. 1 is a flowchart showing a method for producing a gallium nitride single crystal substrate according to one embodiment of the present invention. [Diagram 2] 2(a) to 2(c) are schematic cross-sectional views showing a part of a method for producing a gallium nitride single crystal substrate according to one embodiment of the present invention. [Diagram 3] 3(a) and (b) are schematic cross-sectional views showing a part of a method for producing a gallium nitride single crystal substrate according to one embodiment of the present invention. [Figure 4] 4(a) and (b) are schematic cross-sectional views showing a part of a method for producing a gallium nitride single crystal substrate according to one embodiment of the present invention. [Diagram 5] FIG. 5 is an SEM image showing an example of an etch pit formed on the primary surface of a gallium nitride single crystal substrate according to one embodiment of the present invention. [Figure 6] FIG. 6(a) is a histogram of etch pit diameters according to Example 1, and FIG. 6(b) is an enlarged view of FIG. 6(a) in the vertical direction. [Figure 7]FIG. 7(a) is a histogram of etch pit diameters according to Example 2, and FIG. 7(b) is an enlarged view of FIG. 7(a) in the vertical direction. [Figure 8] FIG. 8(a) is a histogram of etch pit diameters according to the comparative example, and FIG. 8(b) is an enlargement of FIG. 8(a) in the vertical direction. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0008] <Inventor's findings> First, the findings of the inventors will be described.

[0009] It is known that when etching is performed on the c-plane of a gallium nitride (GaN) single crystal substrate using, for example, an alkaline etching solution, etch pits corresponding to dislocations are formed. A method for identifying the type of dislocation (edge, mixed, screw) based on the size (diameter) of the etch pit is also known to those skilled in the art, but this method is not necessarily universally applicable. The size of the etch pit formed by alkaline etching corresponds to the magnitude of distortion of the crystal lattice around the dislocation core. Therefore, the size of the etch pit is determined not only by the type of dislocation, but also by the impurities trapped in the dislocation, the precipitates on the dislocation, and the distance from other nearby dislocations.

[0010] For the reasons mentioned above, it is difficult to specify the type of dislocation (edge, mixed, screw) based on the size of the etch pit, but it can be said that dislocations that form large etch pits also have a large strain field around the dislocation core. Dislocations with large strain fields are likely to have a large Burgers vector, and such dislocations tend to become micropipe defects with hollow cores, which can become anomalous diffusion paths for impurities. The inventors have found that dislocations with large strain fields adversely affect the characteristics of devices fabricated on gallium nitride single crystal substrates.

[0011] The size of the etch pit also depends greatly on the etching conditions. For this reason, it is meaningless to discuss the absolute value of the size of the etch pit. However, among the several types of etch pits with different sizes detected by etching, the smallest etch pit is highly likely to correspond to an edge dislocation with the smallest strain field around the dislocation core. Therefore, the inventors have found a technology to grasp the presence or absence of dislocation defects that adversely affect the characteristics of a device fabricated on a gallium nitride single crystal substrate by examining a histogram of the etch pit diameters, taking the diameter of the smallest peak among the peaks appearing in this histogram as a standard, and examining the diameters and numbers of other etch pits. Then, when the diameter of the standard etch pit is a, an etch pit with a diameter exceeding 4a corresponds to a dislocation that has accumulated the above-mentioned large strain, and it has been found that such dislocations are highly likely to adversely affect the device characteristics.

[0012] Furthermore, the inventors have conducted extensive research into methods for reducing (or eliminating) dislocations that have accumulated large strains as described above. As a result, they have discovered that by doping the inclined interface growth region with a high concentration of germanium (Ge) in the step of growing the substrate using an inclined interface as the growth surface as described in Patent Document 1 (the first step described below), it is possible to manufacture a gallium nitride single crystal substrate that is substantially free of large etch pits with a diameter exceeding 4a when etched with an alkaline etching solution (i.e., substantially free of dislocations that have accumulated large strains that are likely to adversely affect device characteristics).

[0013] <One embodiment of the present invention> Hereinafter, an embodiment of the present invention will be described with reference to the drawings.

[0014] (1) Method for manufacturing gallium nitride single crystal substrate A method for producing a gallium nitride single crystal substrate according to this embodiment will be described with reference to Figs. 1 to 4. Fig. 1 is a flow chart showing a method for producing a gallium nitride single crystal substrate according to this embodiment. Figs. 2(a) to (c), Figs. 3(a) and (b), and Figs. 4(a) and (b) are schematic cross-sectional views showing a part of the method for producing a gallium nitride single crystal substrate according to this embodiment. In Fig. 3(b), the thin solid line s indicates a crystal plane during growth, and in Figs. 2(c), 3(a) and (b), 4(a) and (b), the dotted lines indicate dislocations.

[0015] As shown in FIG. 1, the method for manufacturing a gallium nitride single crystal substrate according to this embodiment includes, for example, a base substrate preparation step S100, a first step S200, a second step S300, a slicing step S400, and a polishing step S500.

[0016] (S100: Base board preparation process) 2(a), in the base substrate preparation step S100, a base substrate 10 made of gallium nitride single crystal is prepared. In the base substrate preparation step S100 of this embodiment, a commercially available gallium nitride single crystal substrate (not a template, but a free-standing substrate) can be used as the base substrate 10. Alternatively, the base substrate 10 made of gallium nitride single crystal may be produced by the VAS (Void-Assisted Separation) method described in Patent Document 1. The base substrate 10 may be Ge-doped, Si-doped, or undoped, but is preferably a Ge-doped GaN layer, which can reduce the difference in Ge concentration between the base substrate 10 and the first layer 30 described below.

[0017] In the following, in a GaN crystal having a wurtzite structure, <0001> The axis is called the "c-axis" and the (0001) plane is called the "c-plane". The (0001) plane is sometimes called the "+c-plane (gallium polar plane)" and the (000-1) plane is sometimes called the "-c-plane (nitrogen (N) polar plane)". The <1-100> axis is called the "m-axis" and the {1-100} plane is called the "m-plane". The m-axis may also be written as the <10-10> axis. The <11-20> axis is called the "a-axis" and the {11-20} plane is called the "a-plane".

[0018] (S200: 1st process (1st layer growth process)) 2(b), a single crystal of GaN having a top surface 30u with an exposed c-plane 30c is directly epitaxially grown on the primary surface 10s of the base substrate 10 prepared in the base substrate preparation step S100 by supplying GaCl gas and NH3 gas to the heated base substrate 10, for example, by the HVPE method, thereby growing the first layer 30.

[0019] At this time, a plurality of recesses 30p surrounded by inclined interfaces 30i other than the c-plane are generated on the top surface 30u of the single crystal, and the inclined interfaces 30i are gradually enlarged and the c-planes 30c are gradually reduced toward the upper side of the main surface 10s of the base substrate 10. This causes the c-planes 30c to disappear from the top surface 30u. As a result, a first layer 30 whose surface is composed only of the inclined interfaces 30i is grown, as shown in FIG. 2(c).

[0020] That is, in the first step S200, the first layer 30 is three-dimensionally grown as a single crystal, so as to intentionally roughen the main surface 10s of the base substrate 10.

[0021] In the first step S200, the first layer 30 is grown under, for example, predetermined first growth conditions. In the first growth conditions of this embodiment, for example, the growth temperature in the first step S200 is set lower than the growth temperature in the second step S300 described below. Specifically, the growth temperature in the first step S200 is set to, for example, 980°C or higher and 1,020°C or lower, preferably 1,000°C or higher and 1,020°C or lower.

[0022] As a first growth condition of this embodiment, for example, the ratio of the supply rate of NH3 gas as the nitriding gas to the supply rate of GaCl gas as the Group III source gas in the first step S200 (hereinafter also referred to as "V / III ratio") may be set to be larger than the V / III ratio in the second step S300 described later. Specifically, the V / III ratio in the first step S200 is set to, for example, 2 to 20, preferably 2 to 15.

[0023] In this embodiment, under the first growth conditions, the first layer 30 (particularly, the inclined interface growth region 70 described later) is doped with a high concentration of Ge. This reduces dislocations that have accumulated large strain on the surface of the second layer 40 described later, and effectively increases the proportion of dislocations with small strain fields. Ge doping is performed using, for example, tetrachlorogermane (GeCl4) gas. GeCl4 gas is supplied, for example, from a cylinder, or by placing a source container in a thermostatic chamber maintained at about 5°C and bubbling GeCl4 in a liquid state using a carrier gas. Either H2 gas or N2 gas, or both, can be used as the carrier gas. In either case, the flow rate of GeCl4 gas is controlled by a mass flow controller so that the partial pressure of the GeCl4 gas is 0.3 to 30 Pa, and the Ge concentration in the first layer 30 (particularly, the inclined interface growth region 70) is increased to 3×10 18 ~9×10 20 cm -3 It is preferable to appropriately adjust the amount of

[0024] Other conditions among the first growth conditions in this embodiment are, for example, as follows. Growth pressure: 90 to 105 kPa, preferably 90 to 95 kPa GaCl gas partial pressure: 1.5~15kPa N2 gas flow rate / H2 gas flow rate: 0~1 Partial pressure of GeCl4 gas: 0.3 to 30 Pa

[0025] Here, the first step S200 of this embodiment is classified into two steps, for example, based on the morphology of the first layer 30 during growth. Specifically, the first step S200 of this embodiment includes, for example, an inclined interface expansion step S220 and an inclined interface maintenance step S240. Through these steps, the first layer 30 includes, for example, an inclined interface expansion layer 32 and an inclined interface maintenance layer 34.

[0026] (S220: Inclined interface expansion process) First, as shown in FIG. 2(b), the gradient interface expansion layer 32 of the first layer 30 made of single crystal GaN is epitaxially grown directly on the primary surface 10s of the base substrate 10 under the first growth conditions described above.

[0027] In the initial stage of growth of the inclined interface spreading layer 32, the inclined interface spreading layer 32 grows in the normal direction (direction along the c-axis) of the main surface 10s of the base substrate 10, with the c-plane 30c as the growth plane.

[0028] By gradually growing the inclined interface expansion layer 32 under the first growth conditions, as shown in FIG. 2(b), a plurality of recesses 30p consisting of inclined interfaces 30i other than the c-plane are generated on the top surface 30u where the c-plane 30c is exposed of the inclined interface expansion layer 32. The plurality of recesses 30p consisting of inclined interfaces 30i other than the c-plane are formed randomly on the top surface 30u. This forms an inclined interface expansion layer 32 in which the c-plane 30c and the inclined interfaces 30i other than the c-plane are mixed on the surface.

[0029] The term "inclined interface 30i" means a growth interface inclined with respect to the c-plane 30c, and includes low-index facets other than the c-plane, high-index facets other than the c-plane, or inclined faces that cannot be expressed by a plane index. Examples of facets other than the c-plane include {11-2m} and {1-10n}, where m and n are integers other than 0.

[0030] By further growing the inclined interface expansion layer 32 under the first growth conditions, as shown in Fig. 2(b), in the inclined interface expansion layer 32, the inclined interfaces 30i other than the c-plane are gradually enlarged and the c-plane 30c is gradually reduced toward the upper side of the underlying substrate 10. Note that at this time, the inclination angle of the inclined interfaces 30i with respect to the main surface 10s of the underlying substrate 10 gradually decreases toward the upper side of the underlying substrate 10. As a result, most of the inclined interfaces 30i eventually become {11-2m} planes where m ≥ 3.

[0031] As the inclined interface spreading layer 32 is further grown, the c-plane 30c of the inclined interface spreading layer 32 disappears from the top surface 30u, and the surface of the inclined interface spreading layer 32 is composed only of the inclined interface 30i, as shown in Fig. 2(c). This results in the formation of a mountain range-like inclined interface spreading layer 32 in which pyramids are continuously bonded.

[0032] In this embodiment, in the initial stage of growth of the inclined interface expansion layer 32, the inclined interface expansion layer 32 is grown to a predetermined thickness on the main surface 10s of the base substrate 10 using the c-plane 30c as the growth surface without generating the inclined interface 30i, and then an inclined interface 30i other than the c-plane is generated on the surface of the inclined interface expansion layer 32. As a result, the multiple valleys 30v are formed at positions above and away from the main surface 10s of the base substrate 10. In this case, when a Ge-doped base substrate 10 is used, the Ge concentration difference between the base substrate 10 and the region grown using the c-plane 30c as the growth surface is, for example, 1×10 18 cm -3 It is preferable to adjust the following:

[0033] Due to the above-described growth process of the inclined interface expansion layer 32, dislocations are bent and propagated as follows. Specifically, as shown in FIG. 2(c), a plurality of dislocations extending in the direction along the c-axis in the base substrate 10 are propagated from the base substrate 10 toward the direction along the c-axis of the inclined interface expansion layer 32. In the region of the inclined interface expansion layer 32 that has grown with the c-plane 30c as the growth plane, dislocations are propagated from the base substrate 10 toward the direction along the c-axis of the inclined interface expansion layer 32. However, when the inclined interface expands and the growth plane of the dislocations propagating in the direction along the c-axis changes to the inclined interface 30i, the dislocations are bent and propagated toward a direction substantially perpendicular to the inclined interface 30i. That is, the dislocations are bent and propagated in a direction inclined with respect to the c-axis. As a result, in the steps following the inclined interface expansion step S220, the dislocations are locally collected at substantially the center of the plurality of recesses 30p formed by the inclined interfaces 30i. Among the dislocations gathered at approximately the center of the recess 30p, those having opposite Burgers vectors disappear when they meet. Some of the dislocations form dislocation loops and are suppressed from propagating in the direction along the c-axis. As a result, the dislocation density on the surface of the second layer 40 described below can be reduced. On the other hand, dislocations that do not meet with other dislocations continue to propagate as they are, while some dislocations meet with other dislocations and progress while forming an even larger Burgers vector.

[0034] At this time, in the inclined interface expansion layer 32, based on the difference in the growth surface during the growth process, a first c-plane growth region 60 grown using the c-plane 30c as the growth surface, and an inclined interface growth region 70 (gray part in the figure) grown using an inclined interface 30i other than the c-plane as the growth surface are formed.

[0035] At this time, in the first c-plane growth region 60, a recess 60a is formed at a position where the inclined interface 30i occurs, and a protrusion 60b is formed at a position where the c-plane 30c disappears. In addition, in the first c-plane growth region 60, a pair of inclined portions 60i are formed on both sides of the protrusion 60b as a locus of intersections between the c-plane 30c and the inclined interface 30i.

[0036] (S240: Inclined interface maintenance process) After the c-plane 30c has disappeared from the surface of the inclined interface spreading layer 32, the growth of the first layer 30 is continued over a predetermined thickness while maintaining the state in which the surface is composed only of the inclined interface 30i, as shown in Fig. 3(a). In this way, an inclined interface maintaining layer 34 having no c-plane and only the inclined interface 30i on its surface is formed on the inclined interface spreading layer 32. By forming the inclined interface maintaining layer 34, the c-plane 30c can be reliably eliminated over the entire surface of the first layer 30.

[0037] At this time, the growth conditions in the inclined interface maintaining step S240 are maintained at the above-mentioned first growth conditions, similar to the inclined interface expanding step S220. This allows the inclined interface maintaining layer 34 to grow using only the inclined interface 30i as a growth surface.

[0038] In addition, at this time, by growing the inclined interface maintaining layer 34 under the first growth conditions with the inclined interface 30i as the growth surface, as described above, the dislocations that have propagated while bending in a direction inclined with respect to the c-axis at the position where the inclined interface 30i is exposed in the inclined interface expansion layer 32 continue to propagate in the same direction in the inclined interface maintaining layer 34.

[0039] At this time, the inclined interface maintaining layer 34 grows using the inclined interface 30i as a growth surface, so that the entire inclined interface maintaining layer 34 becomes a part of the inclined interface growth region 70.

[0040] The inclined interface growth region 70 is more likely to incorporate oxygen than the first c-plane growth region 60. Therefore, the oxygen concentration in the inclined interface growth region 70 is higher than that in the first c-plane growth region 60. The oxygen incorporated in the inclined interface growth region 70 is, for example, oxygen unintentionally mixed into the HVPE apparatus, or oxygen released from a member (such as a quartz member) constituting the HVPE apparatus. When oxygen is incorporated into the inclined interface growth region 70, the lattice constant increases, and the crystal is deformed to the convex side. The c-plane shape of a GaN substrate manufactured by the VAS method is generally curved in a concave shape. When a GaN substrate manufactured by the VAS method is used as the base substrate 10, the c-plane shape, which was initially concave, gradually deforms to the convex side as the inclined interface growth region 70 grows thick, and approaches a flat surface, so that the c-axis distribution becomes smaller. This allows the radius of curvature of the c-plane 40c of the main growth layer 44 described later to be increased.

[0041] The oxygen concentration in the first c-plane growth region 60 is, for example, 5×10 16 cm -3 Less than or equal to 3×10 16 cm -3 On the other hand, the oxygen concentration in the inclined interface growth region 70 is, for example, 3×10 18 cm -3 5×10 or more 19 cm -3 The following is the result.

[0042] Here, by doping the inclined interface growth region 70 with Ge at a high concentration, dislocations that have accumulated large strains can be reduced on the surface of the second layer 40 described later. Ge has an effect of preventing the movement of dislocations (pinning effect), and also has the property that the larger the strain field of a dislocation, the more likely it is that impurities will be collected at the dislocation core due to the Cotterell effect. As described above, in the recess 30p, dislocations that have formed a large Burgers vector by gathering together collected dislocations are present. By doping the inclined interface 30i (particularly the inclined interface growth region 70) with Ge at a high concentration, among the collected dislocations, dislocations with particularly large strain fields are pinned by Ge. Since the progression of the pinned dislocations to other slip planes is hindered, it becomes difficult to maintain the propagation in the same form, and the probability that the dislocations will decompose into two or more dislocations and proceed in order to maintain the propagation increases. Since each decomposed dislocation has a smaller strain field than before, the presence ratio of dislocations with small strain fields on the surface of the second layer 40 can be increased. Although the number of dislocations increases by decomposing dislocations with large strain fields, the absolute number of dislocations with large strain fields is originally small, so the number of dislocations increased by the above decomposition is negligibly small compared to the number of dislocations that are reduced by being gathered at approximately the center of the recess 30p of the inclined interface 30i. This makes it possible to selectively reduce dislocations with large strain fields that adversely affect device characteristics.

[0043] Compared to the first c-plane growth region 60 grown using the c-plane 30c as a growth surface, the inclined interface growth region 70 grown using the inclined interface 30i other than the c-plane as a growth surface is more likely to incorporate Ge as well as oxygen. Therefore, if doping with Ge begins at the timing when the inclined interface 30i is formed, the Ge concentration of the inclined interface 30i becomes higher than that of the c-plane 30c. Furthermore, in the inclined interface 30i, dislocations bend in a direction inclined to the c-axis and are gathered at approximately the center of the recess 30p, so that by doping with Ge at the timing when the inclined interface 30i is formed, dislocations with large strain fields can be effectively reduced.

[0044] The Ge concentration in the inclined interface growth region 70 is 3×10 18 ~9×10 20 cm -3The O concentration and Ge concentration of the inclined interface growth region 70 can be measured by, for example, secondary ion mass spectrometry (SIMS). The effect of increasing the proportion of dislocations with small strain fields is seen when the Ge concentration of the inclined interface growth region 70 is 5×10 18 cm -3 It becomes noticeable when it exceeds 5×10 19 cm -3 The Ge concentration in the inclined interface growth region 70 is 5×10 21 cm -3 If the temperature exceeds this range, the crystals will grow abnormally (for example, polycrystallization will occur).

[0045] By the above-described first step S200, the first layer 30 having the gradient interface enlarging layer 32 and the gradient interface maintaining layer 34 is formed.

[0046] In the first step S200 of this embodiment, it is preferable that the height from the main surface 10s of the base substrate 10 to the top 30t of the first layer 30 (the maximum height in the thickness direction of the first layer 30, hereinafter also referred to as the thickness of the first layer 30) is, for example, 0.5 mm or more and 3 mm or less. If the thickness of the first layer 30 is less than 0.5 mm, the effect of increasing the abundance ratio of small dislocations in the strain field on the surface of the second layer 40 may not be sufficiently obtained. In contrast, by making the thickness of the first layer 30 0.5 mm or more, the effect of increasing the abundance ratio of small dislocations in the strain field can be sufficiently obtained. On the other hand, if the thickness of the first layer 30 exceeds 3 mm, the effect of increasing the abundance ratio of small dislocations in the strain field on the surface of the second layer 40 is likely to be saturated, which is disadvantageous in terms of production costs. In contrast, by making the thickness of the first layer 30 3 mm or less, the effect of increasing the abundance ratio of small dislocations in the strain field can be efficiently obtained.

[0047] (S300: 2nd process (2nd layer growth process)) After the first layer 30 with the c-plane 30c eliminated has been grown, a single crystal of GaN is further epitaxially grown on the first layer 30, as shown in FIG. 3(b) and FIG. 4(a).

[0048] At this time, the inclined interface 40i is gradually reduced and the c-plane 40c is gradually expanded upwardly on the main surface 10s of the base substrate 10. This causes the inclined interface 30i formed on the surface of the first layer 30 to disappear. As a result, the second layer 40 having a mirror-finished surface is grown.

[0049] In the second step S300, the second layer 40 is grown under, for example, predetermined second growth conditions. As the second growth conditions in this embodiment, the growth temperature in the second step S300 is, for example, higher than the growth temperature in the first step S200. Specifically, the growth temperature in the second step S300 is, for example, 990°C or higher and 1,120°C or lower, preferably 1,020°C or higher and 1,100°C or lower.

[0050] As the second growth condition of this embodiment, the V / III ratio in the second step S300 may be adjusted. For example, the V / III ratio in the second step S300 may be smaller than the V / III ratio in the first step S200. Specifically, the V / III ratio in the second step S300 is set to, for example, 1 or more and 10 or less, preferably 1 or more and 5 or less.

[0051] The second step S300 of this embodiment is classified into two steps, for example, based on the morphology of the second layer 40 during growth. Specifically, the second step S300 of this embodiment includes, for example, a c-plane expansion step S320 and a main growth step S340. Through these steps, the second layer 40 includes, for example, a c-plane expansion layer 42 and a main growth layer 44.

[0052] Other conditions among the second growth conditions in this embodiment are, for example, as follows. Growth pressure: 90 to 105 kPa, preferably 90 to 95 kPa GaCl gas partial pressure: 1.5~15kPa N2 gas flow rate / H2 gas flow rate: 1~20

[0053] (S320: c-plane expansion process) As shown in FIG. 3(b), a c-plane expansion layer 42 of a second layer 40 made of a single crystal of GaN is epitaxially grown on the first layer 30 under the above-mentioned second growth conditions.

[0054] At this time, as one moves upward in the first layer 30, the c-plane 40c is enlarged, while the inclined interface 40i other than the c-plane is reduced.

[0055] Specifically, by growth under the second growth conditions, the c-plane expansion layer 42 grows from the inclined interface 30i of the inclined interface maintaining layer 34 in a direction perpendicular to the c-axis (i.e., in a longitudinal or lateral direction) with the inclined interface 40i as the growth plane. As the c-plane expansion layer 42 is grown in the lateral direction, the c-plane 40c of the c-plane expansion layer 42 begins to be exposed again above the top portion 30t of the inclined interface maintaining layer 34. This results in the formation of the c-plane expansion layer 42 in which the c-plane 40c and the inclined interface 40i other than the c-plane are mixed on the surface.

[0056] When the c-plane expansion layer 42 is further grown laterally, the c-plane 40c gradually expands and the inclined interfaces 40i of the c-plane expansion layer 42 gradually shrink. As a result, the recesses 30p formed by the multiple inclined interfaces 30i on the surface of the first layer 30 are gradually filled.

[0057] Thereafter, when the c-plane extension layer 42 is further grown, the inclined interfaces 40i of the c-plane extension layer 42 disappear completely, and the recesses 30p formed by the multiple inclined interfaces 30i are completely filled in the surface of the first layer 30. As a result, the surface of the c-plane extension layer 42 becomes a mirror surface (flat surface) formed only by the c-plane 40c.

[0058] At this time, dislocations are locally collected during the growth process of the first layer 30 and the c-plane extension layer 42, so that the dislocation density can be reduced. Specifically, dislocations that have propagated while bending in a direction inclined to the c-axis in the first layer 30 continue to propagate in the same direction in the c-plane extension layer 42. As a result, dislocations are locally collected at the meeting point of the adjacent inclined interfaces 40i, approximately above the center between the pair of apexes 30t, in the c-plane extension layer 42. Among the multiple dislocations collected at the meeting point of the adjacent inclined interfaces 40i in the c-plane extension layer 42, dislocations having mutually opposite Burgers vectors disappear when they meet. In addition, some of the multiple dislocations collected at the meeting point of the adjacent inclined interfaces 40i form loops, and are suppressed from propagating in a direction along the c-axis (i.e., toward the surface side of the c-plane extension layer 42). The other part of the dislocations collected at the meeting part of the adjacent inclined interfaces 40i in the c-plane extension layer 42 changes its propagation direction again from the direction inclined with respect to the c-axis to the direction along the c-axis, and propagates to the surface side of the second layer 40. By eliminating some of the dislocations in this way or suppressing the propagation of some of the dislocations to the surface side of the c-plane extension layer 42, the dislocation density on the surface of the second layer 40 can be reduced. Furthermore, by collecting the dislocations locally, a low dislocation density region can be formed above the part of the second layer 40 where the dislocations propagate in the direction inclined with respect to the c-axis.

[0059] Here, in the c-plane expansion step S320, it is preferable to dope the second layer 40 (particularly the c-plane expansion layer 42) with Ge at a high concentration. During the growth of the inclined interface 40i in the c-plane expansion layer 42, the increase in dislocations accumulating large strains in the c-plane 40c of the second layer 40 can be suppressed by doping Ge at a high concentration similar to the inclined interface growth region 70. Furthermore, during the growth of the inclined interface 40i, the increase in dislocations accumulating large strains can be further reduced by doping Ge at a high concentration. When doping the c-plane expansion layer 42 with Ge, it may be doped at the same concentration as the Ge doped in the inclined interface growth region 70, or it may be doped at a different concentration. When doping at a concentration different from that of the inclined interface growth region 70, it is preferable to continuously change the Ge concentration during the growth of the second layer 40. At this time, it is preferable to adjust the partial pressure of GeCl4 gas in the range of 0.3 to 40 Pa.

[0060] At this time, in the c-plane expansion layer 42, the c-plane 40c gradually expands, and a second c-plane growth region 80 (described later) that grows using the c-plane 40c as a growth surface is formed while gradually expanding toward the top in the thickness direction.

[0061] In the c-plane expansion process S320, the surface of the c-plane expansion layer 42 becomes a mirror surface composed only of the c-plane 40c, so that the height in the thickness direction of the c-plane expansion layer 42 (maximum height in the thickness direction) is, for example, greater than or equal to the height from the valley 30v to the top 30t of the inclined interface maintaining layer 34.

[0062] (S340: Main growth process (c-plane growth process)) When the inclined interface 40i disappears in the c-plane expansion layer 42 and the surface becomes a mirror finish, as shown in Fig. 4(a), a main growth layer 44 is formed on the c-plane expansion layer 42 to a predetermined thickness with the c-plane 40c as the growth surface. This forms a main growth layer 44 that does not have the inclined interface 40i and has only the c-plane 40c on its surface.

[0063] At this time, the growth conditions in the main growth step S340 are maintained at the above-mentioned second growth conditions, similar to the c-plane expansion step S320. This allows the main growth layer 44 to be grown by step flow growth using the c-plane 40c as the growth surface.

[0064] In this growth step S340, GaCl gas, NH3 gas, and dichlorosilane (SiH2Cl2) gas as an n-type dopant gas may be supplied to the base substrate 10 heated to a predetermined growth temperature to epitaxially grow a silicon (Si)-doped GaN layer as the second layer 40, or GeCl4 gas or the like may be supplied as an n-type dopant gas instead of SiH2Cl2 gas to epitaxially grow a Ge-doped GaN layer. Note that a GaN layer doped with iron (Fe), manganese (Mn), carbon (C), or the like may be epitaxially grown as the second layer 40.

[0065] When the second layer 40 is doped with Ge in the main growth step S340, it may be doped at the same concentration as the Ge doped in the c-plane expansion layer 42 in the c-plane expansion step S320, or may be doped at a different concentration. When doping at a concentration different from that in the c-plane expansion step S320, it is preferable to continuously change the Ge concentration during growth in the main growth step S340. At this time, it is preferable to adjust the partial pressure of GeCl4 gas in the range of 0.3 to 50 Pa. Also, when doping with a dopant other than Ge (e.g., Si) in the main growth step S340, it is preferable to gradually reduce the Ge concentration during growth in the main growth step S340, and gradually increase the concentration of the dopant other than Ge after the Ge concentration reaches the lower limit of detection by SIMS.

[0066] At this time, oxygen is taken into the inclined interface growth region 70, which elongates the crystal lattice and reduces the c-axis distribution of the second layer 40, so that the radius of curvature of the c-plane 40c of the main growth layer 44 grown thereon can be made larger than the radius of curvature of the c-plane 10c of the base substrate 10. This makes it possible to make the variation in the off-angle of the c-axis of the main growth layer 44 relative to the normal to the surface smaller than the variation in the off-angle of the c-axis 10ca relative to the normal to the main surface 10s of the base substrate 10.

[0067] At this time, the main growth layer 44 is grown using only the c-plane 40c as the growth surface without exposing the inclined interface 40i, so that the entire main growth layer 44 becomes a second c-plane growth region 80, which will be described later.

[0068] In the main growth step S340, the thickness of the main growth layer 44 is set to, for example, 300 μm or more and 10 mm or less. By setting the thickness of the main growth layer 44 to 300 μm or more, at least one substrate 50 can be sliced ​​from the main growth layer 44 in the slicing step S400 described below. On the other hand, by setting the thickness of the main growth layer 44 to 10 mm or less, the final thickness is set to 650 μm, and when slicing substrates 50 having a thickness of 700 μm from the main growth layer 44, at least ten substrates 50 can be obtained even taking into account a kerf loss of about 200 μm.

[0069] The above-described second step S300 forms the second layer 40 having the c-plane expansion layer 42 and the main growth layer 44. As a result, the stacked structure 90 of the present embodiment is formed.

[0070] The above first step S200 to second step S300 are performed consecutively in the same chamber without exposing the base substrate 10 to the atmosphere. This makes it possible to prevent an unintended high oxygen concentration region (a region having an oxygen concentration excessively higher than that of the inclined interface growth region 70) from being formed at the interface between the first layer 30 and the second layer 40.

[0071] (S400: Slicing process) 4(b), for example, the main growth layer 44 is sliced ​​by a wire saw along a cutting plane approximately parallel to the surface of the main growth layer 44. This forms at least one gallium nitride single crystal substrate 50 (also referred to as substrate 50) as an as-sliced ​​substrate. At this time, the thickness of the substrate 50 is set to, for example, 300 μm or more and 700 μm or less.

[0072] At this time, for the reasons described above, the radius of curvature of the c-plane 50c of the substrate 50 cut out from the main growth layer 44 becomes larger than the radius of curvature of the c-plane 10c of the underlying substrate 10. This makes it possible to make the variation in the off-angle θ of the c-axis 50ca relative to the normal to the main surface 50s of the substrate 50 (the maximum and minimum difference in the off-angle θ within the substrate plane) smaller than the variation in the off-angle of the c-axis 10ca of the underlying substrate 10.

[0073] (S500: Polishing process) Next, a polishing device is used to polish both sides of the substrate 50. At this time, the final thickness of the substrate 50 is set to, for example, 250 μm or more and 650 μm or less.

[0074] Through the above steps, the substrate 50 according to this embodiment is manufactured.

[0075] (Fabrication process of semiconductor laminate and fabrication process of semiconductor device) Once the substrate 50 is manufactured, for example, a semiconductor functional layer made of a group III nitride semiconductor may be epitaxially grown on the substrate 50 to manufacture a semiconductor laminate. Once the semiconductor laminate is manufactured, electrodes and the like may be formed on the semiconductor laminate, and the semiconductor laminate may be diced to cut out chips of a predetermined size. In this manner, a semiconductor device may be manufactured. By reducing dislocations that have accumulated large strains on the surface of the substrate 50, the characteristics of the semiconductor device (device) manufactured on the substrate 50 can be improved.

[0076] (2) Gallium nitride single crystal substrate (free-standing nitride semiconductor substrate, nitride crystal substrate) Next, the gallium nitride single crystal substrate 50 according to this embodiment will be described.

[0077] In this embodiment, the substrate 50 obtained by the above-described manufacturing method is a free-standing substrate made of single crystal GaN.

[0078] The diameter of the substrate 50 is, for example, 50 mm or more, and the thickness of the substrate 50 is, for example, 300 μm or more and 1 mm or less.

[0079] The conductivity of the substrate 50 is not particularly limited. However, when the substrate 50 is used to manufacture a semiconductor device as a vertical Schottky barrier diode (SBD), the substrate 50 is, for example, an n-type, the n-type impurity in the substrate 50 is, for example, Si or germanium (Ge), and the n-type impurity concentration in the substrate 50 is, for example, 1.0×10 18 cm -3 Above 1.0×10 20 cm -3 The following is the result.

[0080] The substrate 50 has, for example, a primary surface 50s which serves as an epitaxial growth surface. In this embodiment, the low-index crystal plane closest to the primary surface 50s is, for example, a c-plane 50c.

[0081] The main surface 50s of the substrate 50 is, for example, mirror-finished, and the root-mean-square roughness RMS of the main surface 50s of the substrate 50 is, for example, less than 1 nm.

[0082] Furthermore, in this embodiment, the impurity concentration in the substrate 50 obtained by the above-mentioned manufacturing method is lower than that of a substrate obtained by the flux method or ammonothermal method.

[0083] Specifically, the hydrogen concentration in the substrate 50 is, for example, 1×10 17 cm -3 Less than 5 x 10 16 cm -3 The following is the result.

[0084] In this embodiment, the substrate 50 is formed by slicing the main growth layer 44 grown using the c-plane 40c as the growth surface, and therefore does not include the inclined interface growth region 70 grown using the inclined interface 30i or the inclined interface 40i as the growth surface. In other words, the entire substrate 50 is composed of a low oxygen concentration region.

[0085] Specifically, the oxygen concentration in the substrate 50 is, for example, 5×10 16 cm -3 Less than or equal to 3×10 16 cm -3 The following is the result.

[0086] (Curving of the c-plane and variation in off-angle) In this embodiment, the radius of curvature of c-face 50c of substrate 50 is greater than, for example, the radius of curvature of c-face 10c of base substrate 10 used in the method of manufacturing substrate 50 described above.

[0087] Specifically, the radius of curvature of the c-face 50c of the substrate 50 is, for example, 23 m or more, preferably 30 m or more, and more preferably 40 m or more.

[0088] In this embodiment, the upper limit of the radius of curvature of c-face 50c of substrate 50 is not particularly limited, since the larger the better. When c-face 50c of substrate 50 is substantially flat, the radius of curvature of c-face 50c may be considered to be infinite.

[0089] In this embodiment, the large radius of curvature of the c-plane 50c of the substrate 50 allows the variation in the off-angle θ of the c-axis 50ca relative to the normal to the main surface 50s of the substrate 50 to be smaller than the variation in the off-angle of the c-axis 10ca of the base substrate 10.

[0090] Specifically, when an X-ray rocking curve measurement is performed on the (0002) surface of the substrate 50 and the off-angle θ of the c-axis 50ca relative to the normal to the main surface 50s is measured based on the diffraction peak angle of the (0002) surface, the variation calculated as the maximum and minimum difference in the magnitude of the off-angle θ within a diameter of 29.6 mm from the center of the main surface 50s is, for example, 0.075° or less, preferably 0.057° or less, and more preferably 0.043° or less.

[0091] In this embodiment, the lower limit of the variation in the off-angle θ of the c-axis 50ca of the substrate 50 is not particularly limited, since the smaller the better. When the c-plane 50c of the substrate 50 is substantially flat, the variation in the off-angle θ of the c-axis 50ca of the substrate 50 may be considered to be 0°.

[0092] Furthermore, in this embodiment, the curvature of the c-plane 50c is isotropically small with respect to the main surface 50s of the substrate 50, so that the radius of curvature of the c-plane 50c has little directional dependency.

[0093] Specifically, the difference between the radius of curvature of c-face 50c in the direction along the a-axis obtained by the above-mentioned measurement method and the radius of curvature of c-face 50c in the direction along the m-axis is, for example, 50% or less, and preferably 20% or less, of the larger of these radii of curvature.

[0094] (dislocation density) In this embodiment, the above-described manufacturing method reduces the dislocation density in the surface of second layer 40 below the dislocation density in main surface 10s of base substrate 10. As a result, dislocations are also reduced in main surface 50s of substrate 50 formed by slicing second layer 40.

[0095] When the substrate 50 is manufactured using the base substrate 10 made of high-purity GaN single crystal produced by the VAS method, there are few non-radiative centers caused by foreign matter or point defects in the substrate 50. Therefore, 95% or more (preferably 99% or more) of the dark spots observed when observing the main surface of the substrate 50 of the present application with a multiphoton excitation microscope or the like correspond to dislocations rather than non-radiative centers caused by foreign matter or point defects. The "multiphoton excitation microscope" is sometimes called a two-photon excitation fluorescence microscope.

[0096] In this embodiment, no regions with particularly high dislocation density due to dislocation concentration are formed, and regions with low dislocation density are formed uniformly. Specifically, in this embodiment, when the main surface 50s of the substrate 50 is observed with a multiphoton excitation microscope in a field of view of 250 μm square and the dislocation density is calculated from the dark spot density, the dislocation density is 1×10 6 cm -2 There is no region exceeding 5×10 5 cm -2 The area where this is less than 100% accounts for 80% or more of the main surface 50s, preferably 90% or more, and more preferably 95% or more.

[0097] In other words, in this embodiment, the dislocation density averaged over the entire main surface 50s of the substrate 50 is, for example, 1×10 6 cm -2 less than 5.5 x 10 5 cm -2 More preferably, it is less than 3×10 5 cm -2 The following is the result.

[0098] (Etch pit histogram) When the main surface 50s of the substrate 50 is etched with an alkaline etching solution, etch pits are formed as shown in FIG. 5. In this embodiment, the substrate 50 is immersed in a molten liquid (temperature 470°C) obtained by mixing potassium hydroxide (KOH) and sodium hydroxide (NaOH) at a ratio of 1:1 for 20 minutes to perform etching. The main surface 50s of the substrate 50 after etching is observed using an SEM, the diameter of each etch pit is calculated by image analysis, and a histogram of the etch pit diameters is created from the obtained data on the diameters of the etch pits. The diameter of the etch pits may be the maximum diameter of each etch pit region subjected to image analysis, or may be the diameter equivalent to a circle. In this embodiment, the diameter of the peak (hereinafter also referred to as the first peak) appearing on the smallest side of the peaks appearing in the histogram of the diameters of the etch pits is standardized as a, and the class (step width) of the horizontal axis is set to 0.1a steps. The vertical axis is the number (frequency) of etch pits in the measurement region.

[0099] The density of etch pits (number per unit area) formed when the main surface 50s of the substrate 50 of this embodiment is etched under the above-mentioned conditions corresponds approximately to the dislocation density. The size of the etch pits can be changed by adjusting the etching conditions, but if they are present at too high a density, adjacent etch pits will overlap, making it difficult to measure the diameter of the etch pits. Therefore, in order to perform meaningful measurements, the density of the etch pits should be less than 1×10 6 cm -2 Preferably, less than 5.5×10 5 cm -2 Less than 3 × 10 5 cm -2 It is preferable that the density of etch pits and the diameter of etch pits are not more than 1 mm. 2 It is preferable to measure from the above areas.

[0100] In the substrate 50 of this embodiment, when the diameter of the first peak is a, the total number (total number) of etch pits having a diameter exceeding 4a is 1 / 1000 or less of the number of etch pits constituting the first peak. This can be said in other words that there are substantially no etch pits having a diameter exceeding 4a, but since large etch pits may be formed due to scratches or foreign matter on the substrate 50, it is expressed as 1 / 1000 or less. It can be said that such a substrate 50 is substantially free of dislocations that have accumulated large strains that deteriorate the device characteristics. Therefore, the characteristics of devices fabricated on the substrate 50 can be improved.

[0101] In the substrate 50 of this embodiment, the total number of etch pits having a diameter of 2a or more is preferably 1 / 10 or less, and more preferably 1 / 100 or less, of the number of etch pits constituting the first peak. Since etch pits having a diameter of 2a or more may correspond to dislocations that affect the device characteristics of the substrate 50, the characteristics of devices fabricated on the substrate 50 can be further improved by making the total number of etch pits having a diameter of 2a or more 1 / 10 or less (more preferably 1 / 100 or less) of the number of etch pits constituting the first peak.

[0102] In the substrate 50 of this embodiment, the number of etch pits constituting the first peak is preferably 50% or more (more preferably 70% or more) of the total. As described above, in the first step S200, the proportion of small dislocations in the strain field is increased by doping Ge at a high concentration in the inclined interface growth region 70, so that the number of etch pits constituting the first peak can be increased. Since small dislocations in the strain field do not have a significant effect on the device characteristics of the substrate 50, a high proportion of etch pits constituting the first peak means that the characteristics of the device fabricated on the substrate 50 are good.

[0103] In the substrate 50 of this embodiment, when the frequency of the first peak is A, the number of peaks appearing in the diameter histogram with a frequency of A / 10 or more, including the first peak, is preferably two. It can be said that the number of peaks appearing in the etch pit histogram corresponds to the number of constituent types of dislocation defects corresponding to the etch pits. A crystal in which many peaks are observed is a crystal that has not only simple edge and mixed dislocations, but also a large variety of impurities and point defects that are combined with them in a complex manner, that is, a crystal that is likely to have many impurity levels and defect levels, and has a large variation in characteristics when a device is fabricated, in other words, a crystal that is likely to have a low device yield. In contrast, a crystal that has two peaks appearing in the histogram with a frequency of A / 10 or more, including the first peak, suggests that the dislocations present in the crystal are only two types, simple edge dislocations and mixed dislocations, that is, a crystal that has a small variation in characteristics when a device is fabricated and has a good device yield. In addition, the substrate 50 of this embodiment has a second peak with a diameter in the range of more than a and less than 2a, and the number of etch pits constituting the second peak is preferably smaller than the number of etch pits constituting the first peak. The fact that the diameter of the etch pits constituting the second peak is in the range of more than a and less than 2a means that it is highly likely that they correspond to simple mixed dislocations, and the fact that the number of etch pits constituting the second peak is small, in other words, the number of etch pits constituting the first peak is large indicates that the dislocations in the crystal are mainly composed of dislocations with little distortion around the dislocation core. These characteristics mean that the characteristics of devices fabricated on the substrate 50 are good.

[0104] <Other embodiments> Although the embodiment of the present invention has been specifically described above, the present invention is not limited to the above embodiment, and various modifications can be made without departing from the spirit and scope of the present invention.

[0105] In the above-described embodiments, the case has been described in which the base substrate 10 is a commercially available gallium nitride single crystal substrate or a GaN freestanding substrate fabricated by the VAS method. However, the base substrate 10 is not limited to a GaN freestanding substrate fabricated by the VAS method and may be, for example, a GaN freestanding substrate fabricated by another method.

[0106] In the above embodiment, the case where the substrate 50 is mainly n-type has been described, but the substrate 50 may be p-type or semi-insulating. For example, when the substrate 50 is used to manufacture a semiconductor device as a high electron mobility transistor (HEMT), the substrate 50 is preferably semi-insulating.

[0107] In the above embodiment, in the first step S200, the case where the growth temperature is mainly adjusted as the first growth condition has been described. However, it is also possible to adjust a growth condition other than the growth temperature, or to adjust the growth temperature in combination with a growth condition other than the growth temperature.

[0108] In the above embodiment, in the second step S300, the case where the growth temperature is mainly adjusted as the second growth condition has been described. However, it is also possible to adjust a growth condition other than the growth temperature, or to adjust the growth temperature in combination with a growth condition other than the growth temperature.

[0109] In the above embodiment, the growth conditions in the inclined interface maintaining step S240 are maintained at the above-mentioned first growth conditions, similar to the inclined interface expanding step S220. However, as long as the growth conditions in the inclined interface maintaining step S240 satisfy the first growth conditions, the growth conditions in the inclined interface maintaining step S240 may be different from the growth conditions in the inclined interface expanding step S220.

[0110] In the above embodiment, the growth conditions in the main growth process S340 are maintained at the above-mentioned second growth conditions, similar to the c-plane expansion process S320, as described above. However, as long as the growth conditions in the main growth process S340 satisfy the second growth conditions, the growth conditions in the main growth process S340 may be different from the growth conditions in the c-plane expansion process S320.

[0111] In the above embodiment, the case where the main growth layer 44 is sliced ​​using a wire saw in the slicing step S400 has been described, but for example, an outer circumferential blade slicer, an inner circumferential blade slicer, an electric discharge machine, or the like may also be used.

[0112] In the above embodiment, the manufacturing process is terminated after the substrate 50 is manufactured. However, the substrate 50 may be used as the base substrate 10, and steps S200 to S500 may be performed again. This allows the substrate 50 to be obtained with a further reduced dislocation density. Furthermore, the substrate 50 may be obtained with a further reduced variation in the off-angle θ of the c-axis 50ca. Furthermore, the substrate 50 may be obtained with a further reduced dislocation caused by accumulated large strain. Furthermore, steps S200 to S500 using the substrate 50 as the base substrate 10 may be set as one cycle, and the cycle may be repeated multiple times. This allows the dislocation density of the substrate 50 to be gradually reduced according to the number of times the cycle is repeated. Furthermore, the variation in the off-angle θ of the c-axis 50ca in the substrate 50 may be gradually reduced according to the number of times the cycle is repeated. Furthermore, the substrate 50 may be obtained with a reduced dislocation caused by accumulated large strain according to the number of times the cycle is repeated. EXAMPLES

[0113] Next, examples of the present invention will be described. These examples are merely examples of the present invention, and the present invention is not limited to these examples.

[0114] (1) Preparation of gallium nitride single crystal substrate Gallium nitride single crystal substrates of Example 1, Example 2, and Comparative Example were produced as follows.

[0115] [Preparation conditions for gallium nitride single crystal substrate in Example 1] (Base substrate) Material: GaN Preparation method: VAS method Diameter: 2 inches Thickness: 400μm The closest low-index crystal plane to the main plane: c-plane No pattern processing such as mask layer is required on the main surface. RMS roughness of main surface: 2nm Off-angle of the main surface: 0.4° in the m direction FWHM of (10-10) plane diffraction in XRC measurement: 100 arcsec (1st layer) Material: GaN Growth method: HVPE method First growth condition: The growth temperature was set to 980° C. or more and 1,020° C. or less, and the V / III ratio was set to 2 or more and 20 or less. In addition, Ge was doped into the inclined interface growth region under the following conditions. Ge doping method: GeCl4 gas Partial pressure of GeCl4 gas: 0.35 Pa Ge concentration in the gradient interface growth region: 5×10 18 cm -3 Thickness from the main surface of the base substrate to the surface of the first layer: 1 mm (2nd layer) Material: GaN Growth method: HVPE method Second growth condition: The growth temperature was 1,050° C. or more and 1,080° C. or less, and the V / III ratio was 2 or more and 5 or less. Ge was not doped in the c-plane expansion step S320, but was doped in the main growth step S340 so as to achieve the following c-plane Ge concentration. Thickness from the main surface of the base substrate to the surface of the second layer: 2 mm Ge concentration on c-plane: 3×10 19 cm -3 In addition, when the Ge concentration of each layer changes from the first layer to the second layer, the Ge doping amount is gradually increased or decreased so that the Ge concentration difference between the layers is 1×10 18 cm -3 It was adjusted as follows: (Slicing conditions) Gallium nitride single crystal substrate thickness: 400μm Kerf loss: 200μm

[0116] [Preparation conditions for gallium nitride single crystal substrate in Example 2] (Base substrate) Same as Example 1. (1st layer) Ge concentration in the gradient interface growth region: 5×10 19 cm -3 Other than the above, the same as in Example 1. (2nd layer) In the c-plane expansion step S320, the Ge concentration of the inclined interface 40i is 5×10 19 cm -3 Ge was doped so that Other than the above, the same as in Example 1. (Slicing conditions) Same as Example 1.

[0117] [Conditions for producing gallium nitride single crystal substrates for comparison] (Base substrate) Same as Example 1. (1st layer) Same as Example 1 except that Ge doping was not performed. (2nd layer) Same as Example 1. (Slicing conditions) Same as Example 1.

[0118] (2) Evaluation of etch pit histogram The main surfaces of the gallium nitride single crystal substrates of Example 1, Example 2, and Comparative Example were etched with an alkaline etching solution under the following conditions to form etch pits. Etching solution: Alkaline solution consisting of 500g KOH and 500g NaOH Melt temperature: 470℃ Soaking time: 20 minutes

[0119] The main surface of the gallium nitride single crystal substrate on which etch pits were formed was observed using a SEM (SU5000, manufactured by Hitachi High-Tech Corporation). The measurement field of view was 127 μm × 95.3 μm (magnification 1000 times), and the etch pits were measured by image analysis of an image (1143 μm × 1048 μm) combining 9 horizontal × 11 vertical (total of 99) SEM images. Specifically, the image was binarized using image processing software (Image J), ​​the etch pit area was filled in, and the larger of the width and height of the etch pit area was calculated as the diameter of the etch pit. When filling in the etch pit area, areas showing small dust particles and linear pit areas caused by processing scratches were removed.

[0120] From the obtained data on the diameters of the etch pits, a histogram of the diameters of the etch pits was created. In this example, the diameter of the smallest peak (first peak) among the peaks appearing in the histogram of the diameters of the etch pits was normalized as 1, and the horizontal axis was divided into classes in increments of 0.1.

[0121] 6(a) and (b) show histograms of Example 1, 7(a) and (b) show histograms of Example 2, and 8(a) and (b) show histograms of the comparative example. In Figs. 6(a), (b), 7(a), (b), and 8(a), (b), the horizontal axis shows the normalized etch pit diameter, and the vertical axis shows the number (frequency) of etch pits in the measurement area. Note that Figs. 6(b), 7(b), and 8(b) are enlarged views of the histograms of Figs. 6(a), 7(a), and 8(a) in the vertical axis (frequency) direction. Table 1 also shows the number of etch pits constituting the first peak, the number of etch pits with a diameter of less than 2, the number of etch pits with a diameter of 2 to less than 4, and the number of etch pits with a diameter of 4 or more, all of which were observed in the histograms of Example 1, Example 2, and the comparative example.

[0122] [Table 1]

[0123] As shown in Figures 8(a) and 8(b) and Table 1, in the substrate of Comparative Example in which Ge was not doped in the first layer (inclined interface growth region), a small number of etch pits with a diameter exceeding 4 were measured. In contrast, as shown in Figures 6(a) and 6(b), Figures 7(a) and 7(b) and Table 1, in the substrates of Example 1 and Example 2 in which Ge was doped at a high concentration in the inclined interface growth region, substantially no etch pits with a diameter exceeding 4 were measured (the total number of etch pits with a diameter exceeding 4 was 1 / 1000 or less of the number of etch pits constituting the first peak).

[0124] From the above, it was confirmed that by doping the first layer (inclined interface growth region) with a high concentration of Ge, when the diameter of the first peak in a histogram of etch pit diameters is taken as a, the total number of etch pits with a diameter exceeding 4a can be reduced (can be reduced to 1 / 1000 or less of the number of etch pits constituting the first peak). In other words, the gallium nitride single crystal substrates of Examples 1 and 2 can be said to be substantially free of dislocations that have accumulated large strains that would lead to deterioration of device characteristics, and therefore device characteristics can be improved.

[0125] Also, as shown in Table 1, in the substrate of Example 1, the number of etch pits constituting the first peak was 3890, and the total number of etch pits with a diameter of 2 or more was 352. That is, in the substrate of Example 1, it was confirmed that the total number of etch pits with a diameter of 2 or more was 1 / 10 or less of the number of etch pits constituting the first peak. In the substrate of Example 2, the number of etch pits constituting the first peak was 3582, and the total number of etch pits with a diameter of 2 or more was 22. That is, in the substrate of Example 2, it was confirmed that the total number of etch pits with a diameter of 2 or more was 1 / 100 or less of the number of etch pits constituting the first peak. On the other hand, in the substrate of the comparative example, the total number of etch pits constituting the first peak was 4192, and the total number of etch pits with a diameter of 2 or more was 435.

[0126] Furthermore, the number of etch pits constituting the first peak was 59% of the total in the substrate of Example 1, and the number of etch pits constituting the first peak was 64% of the total in the substrate of Example 2. In other words, it was confirmed that the number of etch pits constituting the first peak was 50% or more of the total in the substrates of Examples 1 and 2.

[0127] Furthermore, from Figures 6(a) and 7(a), it was confirmed that in the substrates of Examples 1 and 2, when the frequency of the first peak is A, there are two peaks, including the first peak, that appear in the diameter histogram and have a frequency of A / 10 or more.

[0128] Furthermore, from Figures 6(a) and 7(a), it was confirmed that the substrates of Examples 1 and 2 had a second peak in the diameter range of more than 1 and less than 2, and the number of etch pits constituting the second peak was smaller than the number of etch pits constituting the first peak.

[0129] <Preferred embodiment of the present invention> Preferred aspects of the present invention will be described below.

[0130] (Appendix 1) A gallium nitride single crystal substrate having a diameter of 50 mm or more and a low-index crystal plane closest to the primary surface being the (0001) plane, The density of etch pits formed when etching the main surface with an alkaline etching solution is 1×10 6 cm -2 is less than A gallium nitride single crystal substrate, in which, when the diameter of a first peak appearing on the smallest diameter side among peaks appearing in a histogram of etch pit diameters is defined as a, the total number of etch pits having a diameter exceeding 4a is 1 / 1000 or less of the number of etch pits constituting the first peak.

[0131] (Appendix 2) 2. The gallium nitride single crystal substrate according to claim 1, wherein the total number of etch pits having a diameter of 2a or more is 1 / 10 or less of the number of etch pits constituting the first peak. More preferably, the total number of etch pits having a diameter of 2a or more is 1 / 100 or less of the number of etch pits constituting the first peak.

[0132] (Appendix 3) 2. The gallium nitride single crystal substrate according to claim 1, wherein the number of etch pits constituting the first peak is 50% or more of the total. More preferably, the number of etch pits constituting the first peak is 70% or more of the total.

[0133] (Appendix 4) 2. The gallium nitride single crystal substrate according to claim 1, wherein when the frequency of the first peak is A, there are two peaks appearing in the histogram having a frequency of A / 10 or more, including the first peak.

[0134] (Appendix 5) 2. The gallium nitride single crystal substrate of claim 1, having a second peak in a diameter range greater than a and less than 2a, wherein the number of etch pits constituting the second peak is smaller than the number of etch pits constituting the first peak.

[0135] (Appendix 6) The etch pit density and histogram are 2 6. A gallium nitride single crystal substrate according to any one of claims 1 to 5, wherein the measurement is performed from the above-mentioned region. [Explanation of symbols]

[0136] 10. Underlying Substrate 30 1st layer 32 Gradient interface expansion layer 34 Gradient interface maintenance layer 40 2nd layer 42 c-plane expansion layer 44 growth layer 50 Gallium nitride single crystal substrate (substrate) 60 1st c-plane growth region 70 Inclined interface growth region 80 2nd c-plane growth region 90 Laminated Structure

Claims

1. A gallium nitride single crystal substrate having a diameter of 50 mm or more and a low-index crystal plane closest to a primary surface being a (0001) plane, The density of etch pits formed when etching the main surface with an alkaline etching solution is 1×10 6 cm -2 is less than A gallium nitride single crystal substrate, in which, when the diameter of a first peak appearing on the smallest diameter side among the peaks appearing in a histogram of the diameters of the etch pits is defined as a, the total number of etch pits having a diameter exceeding 4a is 1 / 1000 or less of the number of etch pits constituting the first peak.

2. 2. The gallium nitride single crystal substrate according to claim 1, wherein the total number of etch pits having a diameter of 2a or more is 1 / 10 or less of the number of etch pits constituting said first peak.

3. 2. The gallium nitride single crystal substrate according to claim 1, wherein the number of etch pits constituting said first peak is 50% or more of the total.

4. 2. The gallium nitride single crystal substrate according to claim 1, wherein when the frequency of said first peak is A, there are two peaks appearing in said histogram having a frequency of A / 10 or more, including said first peak.

5. 2. The gallium nitride single crystal substrate according to claim 1, having a second peak in a diameter range greater than a and less than 2a, and the number of etch pits constituting said second peak is smaller than the number of etch pits constituting said first peak.

6. The etch pit density and histogram are 2 The gallium nitride single crystal substrate according to claim 1 , wherein the measurement is performed from the above-mentioned region.

Citation Information

Patent Citations

  • AlxGayIn1-x-yN CRYSTAL SUBSTRATE, SEMICONDUCTOR DEVICE AND ITS MANUFACTURING METHOD

    JP2007161536A

  • Nitride semiconductor substrate manufacturing method, nitride semiconductor substrate, and laminate structure body

    JP2020033211A