Semiconductor device

The semiconductor device addresses oxygen vacancy and defect issues in oxide semiconductor channels by using a metal oxide layer and insulating layers that release oxygen during heat treatment, enhancing mobility and stability.

JP2024163588APending Publication Date: 2024-11-22JAPAN DISPLAY INC
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2023079338
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-12
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

Existing semiconductor devices using oxide semiconductors for channels face issues with oxygen vacancies and defects in the insulating layer, leading to abnormal device characteristics and fluctuations in reliability, as supplying oxygen to the oxide semiconductor layer is hindered by defects in the insulating layer and insufficient oxygen content.

Method used

A semiconductor device configuration with a gate electrode, gate insulating layers, a metal oxide layer containing aluminum, an oxide semiconductor layer with a polycrystalline structure, and insulating layers is employed, where the insulating layers release oxygen during heat treatment to repair oxygen vacancies and reduce defects, enhancing oxygen supply to the oxide semiconductor layer.

Benefits of technology

This configuration achieves higher linear mobility and stability in the semiconductor device by minimizing the impact of defects and optimizing oxygen supply, resulting in improved electrical characteristics.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024163588000001_ABST
    Figure 2024163588000001_ABST
Patent Text Reader

Abstract

To provide a semiconductor device with high mobility.SOLUTION: A semiconductor device includes: a gate electrode; a gate insulating layer on the gate electrode; a metal oxide layer mainly containing aluminum on the gate insulating layer; an oxide semiconductor layer with a polycrystal structure on the metal oxide layer; a source electrode and a drain electrode in contact with the oxide semiconductor layer from above the oxide semiconductor layer; and an insulating layer on the source electrode and the drain electrode. In an Id-Vg characteristic of the semiconductor device, when a voltage to be supplied to the gate electrode is Vg, a threshold voltage of the semiconductor device is Vth, and an electrostatic capacitance of the gate insulating layer held between the gate electrode and the oxide semiconductor layer is Cox, the linear mobility is over 20 cm2 / Vs when (Vg-Vth)×Cox=5×10-7C / cm2.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] An embodiment of the present invention relates to a semiconductor device, and more particularly to a semiconductor device using an oxide semiconductor as a channel. [Background technology]

[0002] In recent years, development of semiconductor devices using oxide semiconductors for the channel instead of amorphous silicon, low-temperature polysilicon, and single crystal silicon has been progressing (for example, Patent Documents 1 to 6). A semiconductor device using an oxide semiconductor for the channel can be formed with a simple structure and a low-temperature process, similar to a semiconductor device using amorphous silicon for the channel. It is known that a semiconductor device using an oxide semiconductor for the channel has a higher mobility than a semiconductor device using amorphous silicon for the channel.

[0003] In order to stably operate a semiconductor device using an oxide semiconductor for a channel, it is important to supply oxygen to the oxide semiconductor layer in the manufacturing process and reduce oxygen vacancies formed in the oxide semiconductor layer. As one method for supplying oxygen to the oxide semiconductor layer, for example, a technique has been disclosed in which an insulating layer covering the oxide semiconductor layer is formed under conditions in which the insulating layer contains more oxygen. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2021-141338 A [Patent Document 2] JP 2014-099601 A [Patent Document 3] Patent Publication No. 2021-153196 [Patent Document 4] JP 2018-006730 A [Patent Document 5] JP 2016-184771 A [Patent Document 6] Patent Publication No. 2021-108405 Summary of the Invention [Problem to be solved by the invention]

[0005] However, an insulating layer formed under conditions containing more oxygen contains many defects. As a result, abnormal characteristics of the semiconductor device or characteristic fluctuations in reliability tests occur, which are thought to be caused by electrons being trapped in the defects. On the other hand, if an insulating layer with fewer defects is used, the amount of oxygen contained in the insulating layer cannot be increased. Therefore, sufficient oxygen cannot be supplied from the insulating layer to the oxide semiconductor layer. Thus, there is a demand for realizing a structure that can repair oxygen vacancies formed in the oxide semiconductor layer while reducing defects in the insulating layer that cause characteristic fluctuations of the semiconductor device.

[0006] An object of one embodiment of the present invention is to realize a semiconductor device having high mobility. [Means for solving the problem]

[0007] A semiconductor device according to one embodiment of the present invention includes a gate electrode, a gate insulating layer on the gate electrode, a metal oxide layer mainly composed of aluminum on the gate insulating layer, an oxide semiconductor layer having a polycrystalline structure on the metal oxide layer, a source electrode and a drain electrode in contact with the oxide semiconductor layer from above the oxide semiconductor layer, and an insulating layer on the source electrode and the drain electrode. In the Id-Vg characteristic of the semiconductor device, when the voltage supplied to the gate electrode is Vg, the threshold voltage of the semiconductor device is Vth, and the capacitance of the gate insulating layer sandwiched between the gate electrode and the oxide semiconductor layer is Cox, the linear mobility is expressed as (Vg-Vth)×Cox=5×10 -7 C / cm 2 When 20cm 2 Exceeds / Vs.

[0008] A semiconductor device according to one embodiment of the present invention includes a gate electrode, a gate insulating layer on the gate electrode, a metal oxide layer mainly composed of aluminum on the gate insulating layer, an oxide semiconductor layer having a polycrystalline structure on the metal oxide layer, a source electrode and a drain electrode in contact with the oxide semiconductor layer from above the oxide semiconductor layer, and an insulating layer on the source electrode and the drain electrode. In the Id-Vg characteristic of the semiconductor device, when the voltage supplied to the gate electrode is Vg, the threshold voltage of the semiconductor device is Vth, and the capacitance of the gate insulating layer sandwiched between the gate electrode and the oxide semiconductor layer is Cox, the linear mobility is expressed as (Vg-Vth)×Cox=1×10 -6 C / cm 2 30cm when 2 Exceeds / Vs.

[0009] A semiconductor device according to one embodiment of the present invention includes a gate electrode, a gate insulating layer on the gate electrode, a metal oxide layer mainly composed of aluminum on the gate insulating layer, an oxide semiconductor layer having a polycrystalline structure on the metal oxide layer, a source electrode and a drain electrode in contact with the oxide semiconductor layer from above the oxide semiconductor layer, and an insulating layer on the source electrode and the drain electrode. In the Id-Vg characteristic of the semiconductor device, when the voltage supplied to the gate electrode is Vg, the threshold voltage of the semiconductor device is Vth, and the capacitance of the gate insulating layer sandwiched between the gate electrode and the oxide semiconductor layer is Cox, the normalized linear mobility normalized by the linear mobility at Vg=Vth is expressed as (Vg-Vth)×Cox=5×10 -7 C / cm 2 When it exceeds 3.0.

[0010] A semiconductor device according to one embodiment of the present invention includes a gate electrode, a gate insulating layer on the gate electrode, a metal oxide layer on the gate insulating layer, an oxide semiconductor layer having a polycrystalline structure on the metal oxide layer, a source electrode and a drain electrode in contact with the oxide semiconductor layer from above the oxide semiconductor layer, and an insulating layer on the source electrode and the drain electrode. In the Id-Vg characteristic of the semiconductor device, when a voltage supplied to the gate electrode is Vg, a threshold voltage of the semiconductor device is Vth, and a capacitance of the gate insulating layer sandwiched between the gate electrode and the oxide semiconductor layer is Cox, a normalized linear mobility normalized by a linear mobility at Vg=Vth is expressed as (Vg-Vth)×Cox=1×10 -6 C / cm 2 When it exceeds 4.0. [Brief description of the drawings]

[0011] [Figure 1] 1 is a cross-sectional view showing an overview of a semiconductor device according to an embodiment of the present invention; [Diagram 2] 1 is a plan view showing an overview of a semiconductor device according to an embodiment of the present invention; [Diagram 3] 1 is a flowchart showing a method for manufacturing a semiconductor device according to an embodiment of the present invention. [Figure 4] 1A to 1C are cross-sectional views showing a method for manufacturing a semiconductor device according to an embodiment of the present invention. [Diagram 5] 1A to 1C are cross-sectional views showing a method for manufacturing a semiconductor device according to an embodiment of the present invention. [Figure 6] 1A to 1C are cross-sectional views showing a method for manufacturing a semiconductor device according to an embodiment of the present invention. [Figure 7] 1A to 1C are cross-sectional views showing a method for manufacturing a semiconductor device according to an embodiment of the present invention. [Figure 8] 1A to 1C are cross-sectional views showing a method for manufacturing a semiconductor device according to an embodiment of the present invention. [Figure 9] 1A to 1C are cross-sectional views showing a method for manufacturing a semiconductor device according to an embodiment of the present invention. [Figure 10]1A to 1C are cross-sectional views showing a method for manufacturing a semiconductor device according to an embodiment of the present invention. [Figure 11] 1 is a plan view showing an overview of a display device according to an embodiment of the present invention; [Figure 12] 1 is a block diagram showing a circuit configuration of a display device according to an embodiment of the present invention; [Figure 13] 1 is a circuit diagram showing a pixel circuit of a display device according to an embodiment of the present invention. [Figure 14] 1 is a cross-sectional view showing an overview of a display device according to an embodiment of the present invention. [Figure 15] 2 is a plan view of a pixel electrode and a common electrode of a display device according to an embodiment of the present invention; [Figure 16] 1 is a circuit diagram showing a pixel circuit of a display device according to an embodiment of the present invention. [Figure 17] 1 is a cross-sectional view showing an overview of a display device according to an embodiment of the present invention. [Figure 18] FIG. 4 is a diagram showing electrical characteristics of a semiconductor device according to an embodiment of the present invention. [Figure 19] FIG. 2 is a diagram showing the linear mobility of a semiconductor device according to an embodiment of the present invention. [Figure 20] FIG. 11 is a diagram showing the gate capacitance dependency of the electrical characteristics of a semiconductor device according to one embodiment of the present invention. [Figure 21] FIG. 11 is a diagram showing the gate capacitance dependency of the electrical characteristics of a semiconductor device according to one embodiment of the present invention. [Figure 22] FIG. 11 is a diagram showing the dependence of the gate capacitance on the linear mobility of a semiconductor device according to an embodiment of the present invention. [Diagram 23] The horizontal axis of FIG. 20 is normalized by the threshold voltage and the gate capacitance. [Figure 24] The horizontal axis of FIG. 21 is normalized by the threshold voltage and the gate capacitance. [Diagram 25] The horizontal axis of FIG. 22 is normalized by the threshold voltage and the gate capacitance. [Figure 26] FIG. 11 is a diagram showing the dependence of normalized linear mobility on gate capacitance in a semiconductor device according to an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] Each embodiment of the present invention will be described below with reference to the drawings. The following disclosure is merely an example. A configuration that a person skilled in the art can easily come up with by appropriately modifying the configuration of the embodiment while maintaining the gist of the invention is naturally included in the scope of the present invention. In order to make the explanation clearer, the drawings may be schematic in terms of the width, thickness, shape, etc. of each part compared to the actual embodiment. However, the illustrated shapes are merely examples and do not limit the interpretation of the present invention. In this specification and each figure, elements similar to those described above with respect to the previous figures may be given the same reference numerals, and detailed explanations may be omitted as appropriate.

[0013] In each embodiment of the present invention, the direction from the substrate toward the oxide semiconductor layer is referred to as "up" or "upper". Conversely, the direction from the oxide semiconductor layer toward the substrate is referred to as "down" or "down". In this way, for convenience of explanation, the terms "up" or "down" are used in the explanation, but for example, the substrate and the oxide semiconductor layer may be arranged so that their vertical relationship is reversed from that shown in the figure. In the following explanation, for example, the expression "oxide semiconductor layer on a substrate" merely describes the vertical relationship between the substrate and the oxide semiconductor layer as described above, and other members may be arranged between the substrate and the oxide semiconductor layer. "Up" or "down" means the stacking order in a structure in which multiple layers are stacked, and when a pixel electrode is expressed as being above a transistor, the transistor and the pixel electrode may not overlap in a planar view. On the other hand, when a pixel electrode is expressed as being vertically above a transistor, the transistor and the pixel electrode may overlap in a planar view.

[0014] In this specification, the terms "film" and "layer" may be used interchangeably in some cases.

[0015] The term "display device" refers to a structure that displays an image using an electro-optical layer. For example, the term display device may refer to a display panel including an electro-optical layer, or may refer to a structure in which other optical members (e.g., a polarizing member, a backlight, a touch panel, etc.) are attached to a display cell. The "electro-optical layer" may include a liquid crystal layer, an electroluminescent (EL) layer, an electrochromic (EC) layer, and an electrophoretic layer, unless technically inconsistent. Therefore, the embodiments described below will be described by taking a liquid crystal display device including a liquid crystal layer and an organic EL display device including an organic EL layer as examples of display devices, but the structure in this embodiment can be applied to display devices including other electro-optical layers as described above.

[0016] In this specification, unless otherwise specified, expressions such as "α includes A, B, or C," "α includes any one of A, B, and C," and "α includes one selected from the group consisting of A, B, and C" do not exclude cases where α includes multiple combinations of A to C. Furthermore, these expressions do not exclude cases where α includes other elements.

[0017] The following embodiments can be combined with each other as long as no technical contradiction occurs.

[0018] [1. First embodiment] A semiconductor device 10 according to one embodiment of the present invention will be described with reference to FIGS.

[0019] [1-1. Configuration of semiconductor device 10] The configuration of a semiconductor device 10 according to one embodiment of the present invention will be described with reference to Figures 1 and 2. Figure 1 is a cross-sectional view showing an overview of the semiconductor device 10 according to one embodiment of the present invention. Figure 2 is a plan view showing an overview of the semiconductor device 10 according to one embodiment of the present invention. The cross-sectional view shown in Figure 1 corresponds to a cross section taken along line A1-A2 shown in Figure 2.

[0020] 1, the semiconductor device 10 is provided above a substrate 100. The semiconductor device 10 includes a gate electrode 105, gate insulating layers 110 and 120, a metal oxide layer 130, an oxide semiconductor layer 140, a source electrode 201, a drain electrode 203, and insulating layers 150 and 160. When the source electrode 201 and the drain electrode 203 are not particularly distinguished from each other, they may be collectively referred to as a source-drain electrode 200. In this embodiment, a bottom-gate type transistor in which the gate electrode 105 is provided below the oxide semiconductor layer 140 will be described as the semiconductor device 10.

[0021] In this embodiment, a bottom-gate transistor is illustrated as the semiconductor device 10, but the semiconductor device 10 is not limited to a bottom-gate transistor. For example, the semiconductor device 10 may be a dual-gate transistor in which gate electrodes are provided both above and below the oxide semiconductor layer 140.

[0022] The gate electrode 105 is provided on the substrate 100. The gate insulating layers 110 and 120 are provided on the substrate 100 and the gate electrode 105. The gate insulating layers 110 and 120 have a laminated structure. The metal oxide layer 130 is provided on the gate insulating layer 120. The oxide semiconductor layer 140 is provided on the metal oxide layer 130. The source electrode 201 and the drain electrode 203 are provided on the oxide semiconductor layer 140. The source electrode 201 and the drain electrode 203 are in contact with the oxide semiconductor layer 140 from above. The insulating layers 150 and 160 are provided on the oxide semiconductor layer 140, the source electrode 201, and the drain electrode 203. The insulating layers 150 and 160 have a laminated structure. The insulating layer 160 is provided on the insulating layer 150. That is, the insulating layers 150 and 160 cover the source electrode 201 and the drain electrode 203. The insulating layer 150 is in contact with the oxide semiconductor layer 140 .

[0023] The oxide semiconductor layer 140 has a polycrystalline structure that transmits light and includes a plurality of crystal grains. Although details will be described later, the oxide semiconductor layer 140 having a polycrystalline structure can be formed by using a polycrystalline oxide semiconductor (Poly-OS) technique. The configuration of the oxide semiconductor layer 140 will be described below, and an oxide semiconductor having a polycrystalline structure may be referred to as Poly-OS.

[0024] The crystal grains contained in the Poly-OS have a crystal grain size of, for example, 0.1 μm or more, 0.3 μm or more, or 0.5 μm or more. The crystal grain size can be obtained by, for example, cross-sectional SEM observation, cross-sectional TEM observation, or an electron backscattered diffraction (EBSD) method.

[0025] As described above, the crystal grains contained in the Poly-OS have a grain size of 0.1 μm or more, and therefore, in the oxide semiconductor layer 140 having a thickness of 10 nm or more and 30 nm or less, there is a region that contains only one crystal grain along the film thickness direction.

[0026] The thickness of the gate insulating layer 110 is, for example, 50 nm to 500 nm, 50 nm to 400 nm, 50 nm to 300 nm, 50 nm to 150 nm, or 50 nm to 100 nm. The thickness of the gate insulating layer 120 is, for example, 10 nm to 200 nm, or 10 nm to 100 nm. The total thickness of the gate insulating layers 110 and 120 is, for example, 100 nm to 700 nm, 100 nm to 500 nm, 100 nm to 400 nm, 100 nm to 250 nm, 100 nm to 200 nm, or 100 nm to 150 nm.

[0027] The thickness of the metal oxide layer 130 is, for example, 1 nm to 10 nm or 1 nm to 5 nm. In this embodiment, aluminum oxide is used as the metal oxide layer 130. Aluminum oxide has high barrier properties against gases such as oxygen and hydrogen. The barrier properties refer to a function of suppressing the permeation of gases such as oxygen and hydrogen through aluminum oxide. In other words, even if gases such as oxygen or hydrogen are released from a layer provided under the aluminum oxide film, the gases do not move to a layer provided above the aluminum oxide film. Or, even if gases such as oxygen or hydrogen are released from a layer provided on the aluminum oxide film, the gases do not move to a layer provided below the aluminum oxide film.

[0028] The oxide semiconductor layer 140 has a thickness of 10 to 50 nm, 10 to 40 nm, or 10 to 30 nm. The insulating layer 150 has a thickness of 50 to 300 nm, 60 to 200 nm, or 70 to 150 nm.

[0029] The wiring 109 is formed in the same layer as the gate electrode 105. That is, the wiring 109 is in contact with the substrate 100 and the gate insulating layer 110, like the gate electrode 105. The wiring 209 is formed in the same layer as the source electrode 201 and the drain electrode 203. That is, the wiring 209 is in contact with the insulating layer 150. In a region overlapping with the wiring 109, a contact hole 111 is provided in the gate insulating layers 110 and 120. The wiring 209 is connected to the wiring 109 through the contact hole 111. The wiring 109 and the wiring 209 function as gate wirings.

[0030] As shown in FIG. 2, in a plan view, the oxide semiconductor layer 140 overlaps with the gate electrode 105. The D1 direction is a direction connecting the source electrode 201 and the drain electrode 203, and the D2 direction is a direction perpendicular to the D1 direction. In the semiconductor device 10, the channel region is a region where the gate electrode 105 and the oxide semiconductor layer 140 overlap, and is a region sandwiched between the source electrode 201 and the drain electrode 203. The channel length L is the length of the channel region in the D1 direction, and corresponds to the length between the source electrode 201 and the drain electrode 203 in the D1 direction. The channel width W is the width of the channel region in the D2 direction, and corresponds to the width of the oxide semiconductor layer 140 in the D2 direction. In a plan view, the region of the oxide semiconductor layer 140 overlapping with the source electrode 201 is the source region, and the region of the oxide semiconductor layer 140 overlapping with the drain electrode 203 is the drain region. That is, the channel region is located between the source region and the drain region.

[0031] In a plan view, the planar pattern of the metal oxide layer 130 is substantially the same as the planar pattern of the oxide semiconductor layer 140. In other words, the end of the metal oxide layer 130 and the end of the oxide semiconductor layer 140 are substantially aligned. With reference to FIGS. 1 and 2 , the lower surface of the oxide semiconductor layer 140 is covered with the metal oxide layer 130. In particular, in the semiconductor device 10 according to this embodiment, the entire lower surface of the oxide semiconductor layer 140 is covered with the metal oxide layer 130.

[0032] The wirings 109 and 209 extend in the D1 direction. In the D2 direction, the width of the wiring 109 is larger than the width of the wiring 209. A contact hole 111 is provided at the end of the wiring 209 on the opposite side in the D1 direction. In FIG. 2, a configuration in which the wiring 109 extends in the D1 direction together with the wiring 209 is illustrated, but the present invention is not limited to this configuration. The wiring 209 may extend in the D1 direction beyond the end of the wiring 109 in the D1 direction. The width of the wiring 109 in the D2 direction may be the same as the width of the wiring 209, or may be smaller than the width of the wiring 209.

[0033] [1-2. Electrical Characteristics of Semiconductor Device 10] The gate capacitance Cox is the electrostatic capacitance of a dielectric (the gate insulating layers 110, 120 and the metal oxide layer 130) provided between the oxide semiconductor layer 140 in a state in which carriers are generated and the gate electrode 105 when a voltage for controlling the semiconductor device 10 to be in an on-state is supplied to the gate electrode 105. Specifically, the gate capacitance Cox is calculated based on the film thicknesses and dielectric constants of the gate insulating layers 110, 120 and the metal oxide layer 130 in the channel region.

[0034] The semiconductor device 10 according to the present embodiment has the above-mentioned configuration, and thus can obtain a higher linear mobility than a semiconductor device (conventional semiconductor device) using a conventional oxide semiconductor (for example, an oxide semiconductor having a composition ratio of In:Ga:Zn:O=1:1:1:4 and an amorphous structure). The linear mobility means the mobility in a linear region in the electrical characteristics of a transistor. The linear mobility in the present embodiment is the mobility calculated from the Id-Vg characteristics of the semiconductor device 10 when the voltage between the source electrode 201 and the drain electrode 203 is 0.1 V. The voltage supplied to the drain electrode 203 when 0 V is supplied to the source electrode 201 is called the drain voltage Vd.

[0035] In the semiconductor device 10, the oxide semiconductor layer 140 functioning as a channel has fewer defects in the film than conventional oxide semiconductors. As a result, the mobility calculated from the electrical characteristics of the semiconductor device 10 according to this embodiment is higher than the mobility calculated from the electrical characteristics of the conventional semiconductor device. In particular, in the conventional semiconductor device, high mobility cannot be obtained when the drain voltage Vd and the gate voltage Vg are low, whereas in the semiconductor device 10 according to this embodiment, high mobility can be obtained even when the drain voltage Vd and the gate voltage Vg are low. The gate voltage Vg is a voltage supplied to the gate electrode 105.

[0036] When the mobility is calculated based on the electrical characteristics (Id-Vg characteristics) of the semiconductor device, the mobility value is affected by the amount of defects formed in the oxide semiconductor layer and the difference in the gate capacitance Cox, and therefore it is difficult to evaluate the difference in mobility due to the physical properties of the oxide semiconductor layer and the structure of the semiconductor layer.

[0037] For example, when defects are formed in the oxide semiconductor layer of a semiconductor device, the amount of defects affects the threshold voltage Vth in the Id-Vg characteristics of the semiconductor device. Specifically, when a voltage is supplied to the gate electrode of the semiconductor device, the defects are filled by charges excited in the channel in a range where the gate voltage Vg is small, and the charges do not contribute to the drain current Id, so that the rise voltage of the Id-Vg characteristics shifts to a higher voltage side than the original rise voltage.

[0038] The threshold voltage Vth is the gate voltage Vg when a current of "channel width W / channel length L×10 nA" flows through the semiconductor device in the Id-Vg characteristics when the drain voltage Vd is 0.1 V.

[0039] Furthermore, the gate capacitance Cox depends on the film thickness of the gate insulating layer and the dielectric constant of the material used for the gate insulating layer. Therefore, even when the same gate voltage Vg is supplied, the larger the gate capacitance Cox, the higher the carrier concentration generated in the channel. Therefore, when comparing mobilities at the same gate voltage, the larger the gate capacitance Cox, the higher the mobility is because more carriers are generated in the channel. In other words, the amount of charge stored in the channel changes depending on the film thickness of the gate insulating layer, so there is a possibility that the mobility cannot be evaluated correctly.

[0040] As described above, in order to reduce the influence of defects formed in the oxide semiconductor layer and the influence of the gate capacitance Cox on the mobility, in this embodiment, the measured Id-Vg characteristics are normalized by the threshold voltage Vth and the gate capacitance Cox. Specifically, in the Id-Vg characteristics, the normalization is performed by converting the horizontal axis from "gate voltage Vg" to "(gate voltage Vg-threshold voltage Vth) x gate capacitance Cox". Note that the gate voltage Vg x gate capacitance Cox corresponds to the amount of charge excited in the channel.

[0041] The linear mobility in the normalized Id-Vg characteristics is (Vg-Vth)×Cox=5×10. -7 C / cm 2 When 20cm 2 / Vs. Furthermore, the linear mobility is (Vg-Vth)×Cox=1×10 -6 C / cm 2 30cm when 2 Exceeds / Vs.

[0042] Furthermore, the normalized linear mobility, where the linear mobility on the horizontal axis is (Vg-Vth)×Cox, is normalized by the linear mobility at Vg=Vth, and is given by (Vg-Vth)×Cox=5×10 -7 C / cm 2 When the normalized linear mobility is (Vg-Vth)×Cox=1×10, the normalized linear mobility exceeds 3.0. -6 C / cm 2 When it exceeds 4.0.

[0043] [1-3. Materials of each component of semiconductor device 10] As the substrate 100, a rigid substrate having light-transmitting properties, such as a glass substrate, a quartz substrate, and a sapphire substrate, is used. When the substrate 100 needs to be flexible, a substrate containing a resin, such as a polyimide substrate, an acrylic substrate, a siloxane substrate, or a fluororesin substrate, is used. When a substrate containing a resin is used as the substrate 100, impurities may be introduced into the resin in order to improve the heat resistance of the substrate 100. In particular, when the semiconductor device 10 is a top-emission display, the substrate 100 does not need to be transparent, and therefore impurities that deteriorate the transparency of the substrate 100 may be used. When the semiconductor device 10 is used in an integrated circuit that is not a display device, a substrate not having light-transmitting properties, such as a semiconductor substrate such as a silicon substrate, a silicon carbide substrate, or a compound semiconductor substrate, or a conductive substrate such as a stainless steel substrate, is used as the substrate 100.

[0044] Common metal materials are used for the gate electrode 105, the source-drain electrodes 200, and the wirings 109, 209. For example, aluminum (Al), titanium (Ti), chromium (Cr), cobalt (Co), nickel (Ni), molybdenum (Mo), hafnium (Hf), tantalum (Ta), tungsten (W), bismuth (Bi), silver (Ag), copper (Cu), and alloys or compounds thereof are used for these members. The above materials may be used as a single layer or a laminated layer for the gate electrode 105, the source-drain electrodes 200, and the wirings 109, 209.

[0045] A general insulating material is used for the gate insulating layers 110 and 120 and the insulating layers 150 and 160. For example, silicon oxide (SiO x ), silicon oxynitride (SiO x N y ), aluminum oxide (AlO x ), aluminum oxide nitride (AlO x N y The gate insulating layer 110 and the insulating layer 160 are made of an inorganic insulating layer containing oxygen, such as silicon nitride (SiN x), silicon oxynitride (SiN x O y ), Aluminum Nitride (AlN x ), aluminum oxide nitride (AlN x O y ) is used. However, the gate insulating layer 110 and the insulating layer 160 may be formed of an inorganic insulating layer containing oxygen as described above. The gate insulating layer 120 and the insulating layer 150 may be formed of an inorganic insulating layer containing nitrogen as described above.

[0046] An insulating layer having a function of releasing oxygen by heat treatment is used as the insulating layer 150. That is, an oxide insulating layer containing excess oxygen is used as the insulating layer 150. The temperature of the heat treatment at which the insulating layer 150 releases oxygen is, for example, 600° C. or less, 500° C. or less, 450° C. or less, or 400° C. or less. That is, the insulating layer 150 releases oxygen at the heat treatment temperature performed in the manufacturing process of the semiconductor device 10 when a glass substrate is used as the substrate 100, for example.

[0047] An insulating layer with few defects is used as the gate insulating layer 120. For example, when the oxygen composition ratio in the gate insulating layer 120 is compared with the oxygen composition ratio in an insulating layer having the same composition as the gate insulating layer 120 (hereinafter referred to as "another insulating layer"), the oxygen composition ratio in the gate insulating layer 120 is closer to the stoichiometric ratio for the insulating layer than the oxygen composition ratio in the other insulating layer. Specifically, silicon oxide (SiO x ), the composition ratio of oxygen in the silicon oxide used as the gate insulating layer 120 is closer to the stoichiometric ratio of silicon oxide than the composition ratio of oxygen in the silicon oxide used as the insulating layer 150. For example, the gate insulating layer 120 may be a layer in which no defects are observed when evaluated by electron spin resonance (ESR).

[0048] The above SiO x N y and AlO x N yis a silicon and aluminum compound that contains a smaller ratio (x>y) of nitrogen (N) than oxygen (O). SiN x O y and AlN x O y are silicon and aluminum compounds that contain a smaller proportion of oxygen than nitrogen (x>y).

[0049] A metal oxide containing aluminum as a main component is used as the metal oxide layer 130. For example, aluminum oxide (AlO x ), aluminum oxide nitride (AlO x N y ) is used. "Metal oxide layer 130 containing aluminum as a main component" means that the ratio of aluminum contained in metal oxide layer 130 is 1% or more of the entire metal oxide layer. The ratio of aluminum contained in metal oxide layer 130 may be 5% or more and 70% or less, 10% or more and 60% or less, or 30% or more and 50% or less of the entire metal oxide layer. The above ratio may be a mass ratio or a weight ratio.

[0050] A metal oxide having semiconductor properties can be used as the oxide semiconductor layer 140. The oxide semiconductor layer 140 has a polycrystalline structure. The oxide semiconductor layer 140 having a polycrystalline structure can be manufactured by using a Poly-OS technique.

[0051] For example, the oxide semiconductor layer 140 may be an oxide semiconductor containing indium (In), gallium (Ga), zinc (Zn), and oxygen (O). For example, the oxide semiconductor layer 140 may be an oxide semiconductor having a composition ratio of In:Ga:Zn:O=1:1:1:4. However, the oxide semiconductor containing In, Ga, Zn, and O used in this embodiment is not limited to the above composition, and an oxide semiconductor having a different composition from the above may be used. For example, an oxide semiconductor layer having a higher In ratio than the above may be used to improve mobility. On the other hand, an oxide semiconductor layer having a higher Ga ratio than the above may be used to increase the band gap and reduce the influence of light irradiation.

[0052] For example, an oxide semiconductor containing two or more metals including indium (In) may be used as the oxide semiconductor layer 140 having a ratio of In larger than the above. In this case, the ratio of indium elements to all metal elements in the oxide semiconductor layer 140 may be 50% or more in atomic ratio. In addition to indium, gallium (Ga), zinc (Zn), aluminum (Al), hafnium (Hf), yttrium (Y), zirconia (Zr), and lanthanoids may be used as the oxide semiconductor layer 140. Elements other than the above may be used as the oxide semiconductor layer 140.

[0053] As the oxide semiconductor layer 140, other elements may be added to an oxide semiconductor containing In, Ga, Zn, and O, and for example, a metal element such as Al or Sn may be added. In addition to the above oxide semiconductors, an oxide semiconductor containing In and Ga (IGO), an oxide semiconductor containing In and Zn (IZO), an oxide semiconductor containing In, Sn, and Zn (ITZO), an oxide semiconductor containing In and W, or the like may be used as the oxide semiconductor layer 140.

[0054] When the ratio of the indium element is high, the oxide semiconductor layer 140 is likely to crystallize. As described above, by using a material in which the ratio of the indium element to all metal elements in the oxide semiconductor layer 140 is 50% or more, the oxide semiconductor layer 140 having a polycrystalline structure can be easily obtained. It is preferable that the oxide semiconductor layer 140 contains gallium as a metal element other than indium. Gallium belongs to the same Group 13 element as indium. Therefore, the crystallinity of the oxide semiconductor layer 140 is not impaired by gallium, and the oxide semiconductor layer 140 has a polycrystalline structure.

[0055] Although a detailed manufacturing method of the oxide semiconductor layer 140 will be described later, the oxide semiconductor layer 140 can be formed by a sputtering method. The composition of the oxide semiconductor layer 140 formed by the sputtering method depends on the composition of a sputtering target. Even if the oxide semiconductor layer 140 has a polycrystalline structure, the composition of the sputtering target and the composition of the oxide semiconductor layer 140 are approximately the same. In this case, the composition of the metal elements of the oxide semiconductor layer 140 can be specified based on the composition of the metal elements of the sputtering target.

[0056] When the oxide semiconductor layer 140 has a polycrystalline structure, the composition of the oxide semiconductor layer may be identified by X-ray diffraction (XRD). Specifically, the composition of the metal elements in the oxide semiconductor layer can be identified based on the crystal structure and lattice constant of the oxide semiconductor layer obtained by XRD. Furthermore, the composition of the metal elements in the oxide semiconductor layer 140 can also be identified by fluorescent X-ray analysis or Electron Probe Micro Analyzer (EPMA) analysis. However, this is not limited because the oxygen element contained in the oxide semiconductor layer 140 changes depending on the process conditions of sputtering, etc.

[0057] [1-4. Manufacturing Method of Semiconductor Device 10] A method for manufacturing the semiconductor device 10 according to one embodiment of the present invention will be described with reference to Figs. 3 to 10. Fig. 3 is a flowchart for explaining a method for manufacturing the semiconductor device 10 according to one embodiment of the present invention. Figs. 4 to 10 are schematic cross-sectional views showing a method for manufacturing the semiconductor device 10 according to one embodiment of the present invention. Each step of the flowchart shown in Fig. 3 will be described in order below.

[0058] 3, a gate electrode 105 is formed on a substrate 100 (see FIG. 4). In the same step, a wiring 109 is formed together with the gate electrode 105. The gate electrode 105 and the wiring 109 are formed by a PVD (Physical Vapor Deposition) method such as a sputtering method or a vacuum deposition method.

[0059] In step S1002 ("GI formation") in FIG. 3, gate insulating layers 110 and 120 are formed on the gate electrode 105 and the wiring 109 (see FIG. 4). The gate insulating layers 110 and 120 are formed by a chemical vapor deposition (CVD) method or a sputtering method. For example, an insulating material containing nitrogen is used for the gate insulating layer 110. This configuration can block impurities diffusing from the substrate 100 toward the oxide semiconductor layer 140. An insulating material containing oxygen is used for the gate insulating layer 120.

[0060] An oxide insulating layer with few defects is used as the gate insulating layer 120. In order to form an oxide insulating layer with few defects as the insulating layer 120, the insulating layer 120 can be formed at a film formation temperature of 350° C. or higher.

[0061] 3, a metal oxide layer 130 (see FIG. 5) is formed on the gate insulating layers 110 and 120. The metal oxide layer 130 is formed by sputtering or atomic layer deposition (ALD).

[0062] A metal oxide containing aluminum as a main component is used as the metal oxide layer 130. For example, aluminum oxide (AlO x ), aluminum oxide nitride (AlO x N y ) or other inorganic insulating layers are used.

[0063] 3, an oxide semiconductor layer 140 is formed on the metal oxide layer 130 (see FIG. 5). The oxide semiconductor layer 140 is formed by sputtering or atomic layer deposition (ALD).

[0064] When the oxide semiconductor layer 140 is crystallized by OS annealing described later, the oxide semiconductor layer 140 is preferably amorphous (a state in which the oxide semiconductor has few crystalline components) after deposition and before OS annealing. In other words, the oxide semiconductor layer 140 is preferably formed under conditions that prevent the oxide semiconductor layer 140 from crystallizing immediately after deposition as much as possible. For example, when the oxide semiconductor layer 140 is formed by a sputtering method, the oxide semiconductor layer 140 is formed while controlling the temperature of the object to be deposited (the substrate 100 and a structure formed thereon).

[0065] When a film is formed on a target object by sputtering, ions generated in the plasma and atoms recoiled from the sputtering target collide with the target object, and the temperature of the target object increases with the film formation process. If the temperature of the target object increases during the film formation process, the oxide semiconductor layer 140 contains crystalline components immediately after the film formation. If the oxide semiconductor layer 140 contains crystalline components, the crystal grain size cannot be increased by the subsequent OS annealing. In order to control the temperature of the target object as described above, for example, the target object is cooled while the film is formed, thereby reducing the crystalline components contained in the oxide semiconductor layer 140.

[0066] For example, the object can be cooled from the surface opposite to the surface on which the film is to be formed so that the temperature of the surface on which the film is to be formed (hereinafter referred to as the "film formation temperature") becomes 100°C or less, 70°C or less, 50°C or less, or 30°C or less. In particular, the film formation temperature of the oxide semiconductor layer 140 in this embodiment is preferably 50°C or less. By forming the oxide semiconductor layer 140 while cooling the substrate 100, it is possible to obtain an oxide semiconductor layer 140 having a small amount of crystalline components immediately after the film formation. In this embodiment, the oxide semiconductor layer 140 is formed at a film formation temperature of 50°C or less, and the OS annealing described later is performed at a heating temperature of 400°C or more.

[0067] In the sputtering process, the oxide semiconductor layer 140 having an amorphous structure is formed under conditions of an oxygen partial pressure of 10% or less. If the oxygen partial pressure is high, the oxide semiconductor layer 140 contains crystalline components immediately after the film formation due to the excess oxygen contained in the oxide semiconductor layer 140. Therefore, it is preferable to form the oxide semiconductor layer 140 under conditions of a low oxygen partial pressure. The oxygen partial pressure is, for example, 1% to 5% or 2% to 4%. Under conditions of an oxygen partial pressure of less than 1%, the distribution of oxygen in the film formation apparatus tends to be non-uniform. As a result, the composition of oxygen in the oxide semiconductor layer is also non-uniform, and an oxide semiconductor layer containing a large amount of crystalline components is formed, or an oxide semiconductor layer that does not crystallize even if a subsequent OS annealing process is performed is formed.

[0068] In step S1005 ("OS pattern formation") of FIG. 3, a pattern of the oxide semiconductor layer 140 is formed (see FIG. 6). A resist mask (not shown) is formed on the oxide semiconductor layer 140, and the oxide semiconductor layer 140 is etched using the resist mask to form the pattern. For etching the oxide semiconductor layer 140, wet etching or dry etching may be used. For wet etching, etching can be performed using an acidic etchant. For example, oxalic acid, PAN, sulfuric acid, hydrogen peroxide solution, or hydrofluoric acid can be used as the etchant. In this way, a patterned oxide semiconductor layer 140 can be formed. Thereafter, the resist mask is removed.

[0069] The formation of the patterned oxide semiconductor layer 140 (that is, patterning of the oxide semiconductor layer 140) is preferably performed before OS annealing. Since the oxide semiconductor layer 140 after OS annealing has high etching resistance, it is difficult to process it by etching.

[0070] In step S1006 ("OS anneal") of FIG. 3, after the patterned oxide semiconductor layer 140 is formed, a heat treatment (OS anneal) is performed on the oxide semiconductor layer 140. In the OS anneal, the substrate 100 on which the oxide semiconductor layer 140 is formed is held at a predetermined temperature for a predetermined time. The predetermined temperature is 300° C. or more and 500° C. or less, or 350° C. or more and 450° C. or less. The holding time at the temperature is 15 minutes or more and 120 minutes or less, or 30 minutes or more and 60 minutes or less. By performing the OS anneal, the oxide semiconductor layer 140 having an amorphous structure is crystallized, and an oxide semiconductor layer 140 having a polycrystalline structure (Poly-OS) is formed.

[0071] In step S1007 ("MO pattern formation") in FIG. 3, the metal oxide layer 130 formed on the entire surface of the substrate 100 is patterned (see FIG. 7). The oxide semiconductor layer 140 that is sufficiently crystallized by the heat treatment has high etching resistance. Therefore, the metal oxide layer 130 can be patterned using the crystallized oxide semiconductor layer 140 as a mask. The metal oxide layer 130 can be etched by wet etching or dry etching. For example, diluted hydrofluoric acid (DHF) is used for wet etching. By etching the metal oxide layer 130 using the oxide semiconductor layer 140 as a mask, a photolithography process can be omitted. The process of patterning the metal oxide layer 130 using the oxide semiconductor layer 140 as a mask may be omitted.

[0072] 3, contact holes 111 are formed in the gate insulating layers 110 and 120 (see FIG. 7). By forming the contact holes, the upper surface of the wiring 109 is exposed. If it is not necessary to connect the wiring 209 and the wiring 109, the process of step S1008 may be omitted.

[0073] 3, the source electrode 201, the drain electrode 203, and the wiring 209 are formed (see FIG. 8). The source electrode 201, the drain electrode 203, and the wiring 209 are formed by a sputtering method, and are formed by a photolithography process and an etching process. The wiring 209 and the wiring 109 are connected via a contact hole 111.

[0074] The source electrode 201, the drain electrode 203, and the wiring 209 may be etched by wet etching or dry etching. For wet etching, an aluminum mixed acid solution or a mixed solution of hydrogen peroxide and ammonia water (H2O2 / NH3 solution) may be used. For dry etching, a gas containing fluorine such as sulfur hexafluoride gas (SF6) or a gas containing chlorine such as chlorine gas (Cl2) may be used.

[0075] Poly-OS has excellent etching resistance. Specifically, the etching rate of the Poly-OS with respect to the etching solution or etching gas used in forming the source electrode 201 and the drain electrode 203 is very small. This means that the Poly-OS is hardly etched by the etching solution or etching gas. Therefore, in the semiconductor device 10, even if a conductive film is directly formed on the oxide semiconductor layer 140 and the source electrode 201 and the drain electrode 203 are formed by patterning the conductive film, the channel region of the oxide semiconductor layer 140 is hardly etched. As a result, the selectivity of conductive materials that can be used for the source electrode 201, the drain electrode 203, and the wiring 209 is improved. For example, even if a conductive film using a stacked structure of MoW, Al, and MoW or a single-layer structure of a MoW alloy is processed by wet etching to form the source electrode 201 and the drain electrode 203, the oxide semiconductor layer 140 can be prevented from being thinned.

[0076] In step S1010 ("SiOx formation") in FIG. 3, an insulating layer 150 is formed on the oxide semiconductor layer 140, the source electrode 201, and the drain electrode 203 (see FIG. 9). It is preferable to use an insulating material containing oxygen for the insulating layer 150. For example, silicon oxide (SiO x ) or silicon oxynitride (SiO x N y ) are used.

[0077] The insulating layer 150 can be formed by using the same film formation method as the gate insulating layers 110 and 120. In order to increase the composition ratio of oxygen in the insulating layer 150, the insulating layer 150 may be formed at a relatively low temperature (for example, a film formation temperature of less than 350° C.). Furthermore, after the insulating layer 150 is formed, a process of implanting oxygen into a part of the insulating layer 150 may be performed.

[0078] 3, a metal oxide layer 190 is deposited (see FIG. 9) on the insulating layer 150. The metal oxide layer 190 is deposited by sputtering or atomic layer deposition (ALD).

[0079] A metal oxide containing aluminum as a main component is used as the metal oxide layer 190. For example, aluminum oxide (AlO x ), aluminum oxide nitride (AlO x N y ) is used. A metal oxide layer containing aluminum as a main component means that the ratio of aluminum contained in the metal oxide layer is 1% or more of the entire metal oxide layer 190. The ratio of aluminum contained in the metal oxide layer 190 may be 5% or more and 70% or less, 10% or more and 60% or less, or 30% or more and 50% or less of the entire metal oxide layer 190. The above ratio may be a mass ratio or a weight ratio.

[0080] The thickness of the metal oxide layer 190 is 1 nm or more and 50 nm or less, preferably 1 nm or more and 30 nm or less. Aluminum oxide is preferably used as the metal oxide layer 190. Aluminum oxide has high barrier properties against gases such as oxygen and hydrogen. Here, the barrier properties refer to a function of suppressing the permeation of gases such as oxygen and hydrogen through aluminum oxide. In other words, it means that gases such as oxygen and hydrogen in a layer provided under the aluminum oxide film are not transferred to a layer provided on the aluminum oxide film. Or, it means that gases such as oxygen and hydrogen in a layer provided on the aluminum oxide film are not transferred to a layer provided under the aluminum oxide film.

[0081] 3 ("oxidation annealing"), a heat treatment is performed on the insulating layer 150 and the metal oxide layer 190 formed on the oxide semiconductor layer 140. Here, the oxidation annealing may be performed at, for example, 300° C. or higher and 450° C. or lower. This allows oxygen released from the insulating layer 150 to be supplied to the oxide semiconductor layer 140. By providing the metal oxide layer 190 so as to cover the substrate 100, it is possible to prevent the oxygen released from the insulating layer 150 from being released to the outside of the metal oxide layer 190.

[0082] During the process from when the oxide semiconductor layer 140 is formed until when the insulating layer 150 is formed on the oxide semiconductor layer 140, many oxygen defects are generated in the oxide semiconductor layer 140. However, by the oxidation annealing in step S1012, oxygen released from the insulating layer 150 is supplied to the oxide semiconductor layer 140, and the oxygen defects are repaired.

[0083] In step S1013 ("MO removal") of Figure 3, the metal oxide layer 190 is removed (see Figure 10). The metal oxide layer 190 can be removed using, for example, dilute hydrofluoric acid (DHF).

[0084] In step S1014 ("SiNx deposition") in FIG. 3, an insulating layer 160 is deposited on the insulating layer 150 (see FIG. 1). It is preferable to use an insulating material containing nitrogen for the insulating layer 160. For example, silicon nitride (SiN x ) or silicon oxynitride (SiN x O y The insulating layer 160 can be formed by a method similar to that for forming the gate insulating layer 110.

[0085] Through the steps described above, the semiconductor device 10 shown in FIG. 1 can be manufactured.

[0086] [2. Second embodiment] A display device using a semiconductor device according to one embodiment of the present invention will be described with reference to Figures 11 to 15. In the embodiment shown below, a configuration in which the semiconductor device 10 described in the first embodiment above is applied to a circuit of a liquid crystal display device will be described.

[0087] [2-1. Overview of the display device 20] Fig. 11 is a plan view showing an overview of a display device according to an embodiment of the present invention. As shown in Fig. 11, the display device 20 has an array substrate 300, a seal part 310, a counter substrate 320, a flexible printed circuit board 330 (FPC 330), and an IC chip 340. The array substrate 300 and the counter substrate 320 are bonded together by the seal part 310. In a liquid crystal region 22 surrounded by the seal part 310, a plurality of pixel circuits 301 are arranged in a matrix. The liquid crystal region 22 is an area that overlaps with a liquid crystal element 311 described later in a plan view.

[0088] The seal area 24 in which the seal portion 310 is provided is the area surrounding the liquid crystal area 22. The FPC 330 is provided in the terminal area 26. The terminal area 26 is an area in which the array substrate 300 is exposed from the counter substrate 320, and is provided outside the seal area 24. The outside of the seal area 24 means the outside of the area in which the seal portion 310 is provided and the area surrounded by the seal portion 310. The IC chip 340 is provided on the FPC 330. The IC chip 340 supplies signals for driving each pixel circuit 301.

[0089] [2-2. Circuit configuration of display device 20] Fig. 12 is a block diagram showing a circuit configuration of a display device according to an embodiment of the present invention. As shown in Fig. 12, a source driver circuit 302 is provided at a position adjacent to the liquid crystal region 22 in which the pixel circuits 301 are arranged in the opposite direction to the D3 direction (column direction), and a gate driver circuit 303 is provided at a position adjacent to the liquid crystal region 22 in the D4 direction and the opposite direction (row direction). The source driver circuit 302 and the gate driver circuit 303 are provided in the above-mentioned sealing region 24. However, the region in which the source driver circuit 302 and the gate driver circuit 303 are provided is not limited to the sealing region 24, and may be any region outside the region in which the pixel circuits 301 are provided.

[0090] A source line 304 extends from the source driver circuit 302 in the D3 direction and is connected to a plurality of pixel circuits 301 arranged in the D3 direction. A gate line 305 extends from the gate driver circuit 303 in the D4 direction and is connected to a plurality of pixel circuits 301 arranged in the D4 direction.

[0091] A terminal portion 306 is provided in the terminal region 26. The terminal portion 306 and the source driver circuit 302 are connected by a connection wiring 307. Similarly, the terminal portion 306 and the gate driver circuit 303 are connected by a connection wiring 307. By connecting the FPC 330 to the terminal portion 306, an external device to which the FPC 330 is connected is connected to the display device 20, and each pixel circuit 301 provided in the display device 20 is driven by a signal from the external device.

[0092] The semiconductor device 10 according to the first embodiment is used as a transistor included in a pixel circuit 301, a source driver circuit 302, and a gate driver circuit 303.

[0093] Pixel circuit 301 of display device 20 Fig. 13 is a circuit diagram showing a pixel circuit of a display device according to an embodiment of the present invention. As shown in Fig. 13, the pixel circuit 301 includes elements such as a semiconductor device 10, a storage capacitor element 350, and a liquid crystal element 311. The semiconductor device 10 has a gate electrode 105, a source electrode 201, and a drain electrode 203. The gate electrode 105 is connected to a gate wiring 305. The source electrode 201 is connected to a source wiring 304. The drain electrode 203 is connected to the storage capacitor element 350 and the liquid crystal element 311. In this embodiment, for convenience of explanation, the electrode indicated by the reference numeral "201" is referred to as a source electrode, and the electrode indicated by the reference numeral "203" is referred to as a drain electrode, but the electrode indicated by the reference numeral "201" may function as a drain electrode, and the electrode indicated by the reference numeral "203" may function as a source electrode.

[0094] [2-4. Cross-sectional structure of the display device 20] Fig. 14 is a cross-sectional view of a display device according to one embodiment of the present invention. As shown in Fig. 14, a display device 20 is a display device using a semiconductor device 10. In this embodiment, a configuration in which the semiconductor device 10 is used in a pixel circuit 301 is illustrated, but the semiconductor device 10 may also be used in a peripheral circuit including a source driver circuit 302 and a gate driver circuit 303. In the following description, the configuration of the semiconductor device 10 is similar to that of the semiconductor device 10 shown in Fig. 1, and therefore description thereof will be omitted.

[0095] An insulating layer 360 is provided on the source electrode 201 and the drain electrode 203. A common electrode 370 is provided on the insulating layer 360, and is shared by a plurality of pixels. An insulating layer 380 is provided on the common electrode 370. Openings 381, 382 are provided in the insulating layers 360, 380. A pixel electrode 390 is provided on the insulating layer 380 and inside the opening 381. The pixel electrode 390 is connected to the drain electrode 203. An electrode 395 is provided on the insulating layer 380 and inside the opening 382. The electrode 395, together with the common electrode 370, constitutes a storage capacitance element 350.

[0096] Fig. 15 is a plan view of a pixel electrode and a common electrode of a display device according to one embodiment of the present invention. As shown in Fig. 15, the common electrode 370 has an overlapping region that overlaps with the pixel electrode 390 in a plan view, and a non-overlapping region that does not overlap with the pixel electrode 390. When a voltage is supplied between the pixel electrode 390 and the common electrode 370, a lateral electric field is formed from the pixel electrode 390 in the overlapping region to the common electrode 370 in the non-overlapping region. This lateral electric field causes liquid crystal molecules contained in the liquid crystal element 311 to operate, thereby determining the grayscale of the pixel.

[0097] [3. Third embodiment] A display device using a semiconductor device according to one embodiment of the present invention will be described with reference to Figures 16 and 17. In this embodiment, a configuration in which the semiconductor device 10 described in the first embodiment is applied to the circuit of an organic EL display device will be described. The outline and circuit configuration of the display device 20 are similar to those shown in Figures 11 and 12, and therefore will not be described.

[0098] 3-1. Pixel circuit 301 of display device 20 FIG. 16 is a circuit diagram showing a pixel circuit of a display device according to an embodiment of the present invention. As shown in FIG. 16, a pixel circuit 301 includes elements such as a driving transistor 11, a selection transistor 12, a holding capacitance element 210, and a light-emitting element DO. The driving transistor 11 and the selection transistor 12 have the same configuration as the semiconductor device 10. The source electrode of the selection transistor 12 is connected to a signal line 211, and the gate electrode of the selection transistor 12 is connected to a gate line 212. The source electrode of the driving transistor 11 is connected to an anode power line 213, and the drain electrode of the driving transistor 11 is connected to one end of the light-emitting element DO. The other end of the light-emitting element DO is connected to a cathode power line 214. The gate electrode of the driving transistor 11 is connected to the drain electrode of the selection transistor 12. The holding capacitance element 210 is connected to the gate electrode and drain electrode of the driving transistor 11. A grayscale signal that determines the light-emitting intensity of the light-emitting element DO is supplied to the signal line 211. A signal that selects a pixel row to which the above grayscale signal is written is supplied to the gate line 212.

[0099] [3-2. Cross-sectional structure of the display device 20] Fig. 17 is a cross-sectional view of a display device according to an embodiment of the present invention. The configuration of the display device 20 shown in Fig. 17 is similar to that of the display device 20 shown in Fig. 14, but the structure above the insulating layer 360 of the display device 20 in Fig. 17 is different from the structure above the insulating layer 360 of the display device 20 in Fig. 14, and the display device 20 in Fig. 17 differs in that the configuration related to the retention capacitance element 350 of the display device 20 in Fig. 14 is not provided. Hereinafter, a description of the configuration of the display device 20 in Fig. 17 that is similar to that of the display device 20 in Fig. 14 will be omitted, and the differences between the two will be described.

[0100] As shown in FIG. 17, the display device 20 has a pixel electrode 390, a light-emitting layer 392, and a common electrode 394 included in the light-emitting element DO above an insulating layer 360. The pixel electrode 390 is provided on the insulating layer 360 and inside an opening 381. An insulating layer 362 is provided on the pixel electrode 390. An opening 363 is provided in the insulating layer 362. The opening 363 corresponds to a light-emitting region. In other words, the insulating layer 362 defines a pixel. The light-emitting layer 392 and the common electrode 394 are provided on the pixel electrode 390 exposed by the opening 363. The pixel electrode 390 and the light-emitting layer 392 are provided individually for each pixel. On the other hand, the common electrode 394 is provided in common to a plurality of pixels. The light-emitting layer 392 is made of different materials depending on the display color of the pixel.

[0101] In the second and third embodiments, the semiconductor device described in the first embodiment is applied to a liquid crystal display device and an organic EL display device, but the semiconductor device may be applied to other display devices (for example, a self-luminous display device other than an organic EL display device or an electronic paper display device). The semiconductor device can be applied to a variety of display devices, from small and medium-sized display devices to large display devices, without any particular limitations. EXAMPLES

[0102] [Electrical Characteristics of Semiconductor Device 10] The electrical characteristics of the semiconductor device 10 according to the embodiment will be described with reference to Figs. 18 to 26. Fig. 18 is a diagram showing the electrical characteristics (Id-Vg characteristics) of the semiconductor device according to one embodiment of the present invention. Each Id-Vg characteristic shown in Fig. 18 is a logarithmic graph in which Id on the vertical axis is displayed in logarithm. The measurement conditions of the electrical characteristics are as follows. Fig. 18 shows the electrical characteristics of the semiconductor device 10 shown in Fig. 1, in which the thicknesses of the gate insulating layers 110, 120 are different.

[0103] [Measurement conditions] ·Size of channel region CH: W / L=6.0μm / 6.0μm Source-drain voltage: 0.1V, 10V Gate voltage: -40V~+40V (characteristic F is -30V~+30V) Measurement environment: Room temperature, dark room

[0104] The six electrical characteristics shown in FIG. 18 are electrical characteristics of the semiconductor device 10 having different thicknesses of the gate insulating layers 110 and 120. That is, the semiconductor device 10 exhibiting these electrical characteristics has different gate capacitances Cox. In this embodiment, silicon nitride is used as the gate insulating layer 110, and silicon oxide is used as the gate insulating layer 120. In the figure, the thicknesses of silicon nitride\silicon oxide are indicated. The thicknesses are, from the upper left to the right of FIG. 18, silicon nitride\silicon oxide=400\100nm (characteristic A), 300\100nm (characteristic B), and 150\100nm (characteristic C). Similarly, the thicknesses are, from the lower left to the right of FIG. 18, silicon nitride\silicon oxide=150\50nm (characteristic D), 100\50nm (characteristic E), and 50\50nm (characteristic F).

[0105] The gate capacitance Cox under each film thickness condition is shown in Fig. 18. The gate capacitance Cox ranges from 1.0e-8 [F / cm 2 ](Characteristic A), 1.3e-8[F / cm 2 ](Characteristic B), 1.9e-8[F / cm 2 ] (characteristic C). Similarly, the gate capacitance Cox increases from the bottom left to the right in FIG. 2 ] (Characteristics D), 3.2e-8[F / cm 2 ](Characteristics E), 4.5e-8[F / cm 2 ] (Characteristic F). The gate capacitance Cox was calculated using a dielectric constant of 6.5 for silicon nitride and a dielectric constant of 4.1 for silicon oxide.

[0106] The solid horizontal lines in each graph in FIG. 18 indicate the drain current Id of 10 -7 [A] and the mobility is 50 [cm 2 / Vs]. The drain current Id changes by one digit per scale. The mobility changes by 10[cm2 / Vs]. The solid vertical lines in each graph in Figure 18 indicate the position on the scale where the gate voltage is 0 [V]. The gate voltage changes in value by 10 [V] for each scale mark.

[0107] In each graph of FIG. 18, the electrical characteristic marked with a left-pointing arrow indicates the Id-Vg characteristic of the semiconductor device 10. Two types of Id-Vg characteristics are displayed in each graph. Of the two types of Id-Vg characteristics, the Id-Vg characteristic with a relatively large current (solid line) is the characteristic when the drain voltage Vd is 10 V, and the Id-Vg characteristic with a relatively small current (dotted line) is the characteristic when the drain voltage Vd is 0.1 V. In each graph of FIG. 18, the electrical characteristic marked with a right-pointing arrow indicates the mobility (linear mobility) of the semiconductor device 10 calculated from the Id-Vg characteristic when the drain voltage Vd is 0.1 V. As shown in FIG. 18, good electrical characteristics without any particular abnormalities were obtained under most conditions, and the linear mobility was 30 [cm 2 / Vs] or higher.

[0108] In addition, in the semiconductor device 10 under the condition of silicon nitride\silicon oxide=50\50 nm, if a voltage higher than +30 V or lower than -30 V is applied to the gate electrode 105, the semiconductor device 10 will be destroyed, so the voltage applied to the gate electrode 105 is -30 V to +30 V.

[0109] Fig. 19 is a diagram showing the linear mobility of a semiconductor device according to one embodiment of the present invention. The linear mobility shown in Fig. 19 is a graph plotting the maximum mobility obtained from the Id-Vg characteristics when the drain voltage Vd shown in Fig. 18 is 0.1 V. The plots indicated by "◯" in Fig. 19 show the mobility of the semiconductor device 10 according to the first embodiment. The plots indicated by "X" show the mobility of a conventional semiconductor device as reference data.

[0110] In the semiconductor device 10 according to the first embodiment, the linear mobility tends to increase as the value of the gate capacitance Cox increases. Under any condition, the linear mobility of the semiconductor device 10 is greater than that of the conventional semiconductor device.

[0111] 20 and 21 are diagrams showing the gate capacitance dependency of the electrical characteristics of the semiconductor device according to one embodiment of the present invention. FIG. 20 is a linear graph in which the drain current Id (vertical axis) is linearly displayed. FIG. 21 is a logarithmic graph in which the drain current Id (vertical axis) is logarithmically displayed. Among the Id-Vg characteristics shown in FIGS. 20 and 21, characteristics A to F shown by solid lines are characteristics of the semiconductor device 10 according to the first embodiment. In FIGS. 20 and 21, characteristics shown by dotted lines are characteristics (conventional characteristics) of a conventional semiconductor device as reference data. As shown in FIGS. 20 and 21, the smaller the film thickness of the gate insulating layers 110 and 120 (the larger the gate capacitance Cox), the steeper the rise of the Id-Vg characteristics and the more current flows.

[0112] Fig. 22 is a diagram showing the dependency of the linear mobility on the gate capacitance of a semiconductor device according to an embodiment of the present invention. As shown in Fig. 22, the linear mobility shows a similar tendency to the drain current Id in the Id-Vg characteristics, and the linear mobility tends to be smaller as the thickness of the gate insulating layers 110, 120 increases, and the linear mobility tends to be larger as the thickness of the gate insulating layers 110, 120 decreases. Under either condition, the linear mobility of the semiconductor device 10 is greater than that of a semiconductor device using a conventional oxide semiconductor.

[0113] However, as described in the first embodiment, the above Id-Vg characteristics are affected by defects formed in the oxide semiconductor layer and by the gate capacitance Cox on the mobility. Therefore, in order to reduce these effects, the above Id-Vg characteristics were normalized by the threshold voltage Vth and the gate capacitance Cox. The results are shown in Figs. 23 to 25. Specifically, the horizontal axis in Figs. 20 to 22 was converted from "gate voltage Vg" to "(gate voltage Vg-threshold voltage Vth) x gate capacitance Cox" to obtain the Id-Vg characteristics and linear mobility shown in Figs. 23 to 25. Characteristics A' to F' in Figs. 23 to 25 correspond to characteristics A to F in Figs. 20 to 22.

[0114] 23 to 25, by performing the above normalization, the influence of the gate capacitance Cox is reduced, and the differences between the characteristics A' to F' in the Id-Vg characteristics and linear mobility are reduced, and the differences between the characteristics A' to F' and the conventional characteristics become significant. As shown in FIG. 25, the linear mobility in the normalized Id-Vg characteristics is (Vg-Vth)×Cox=5×10 for any of the characteristics A' to F'. -7 C / cm 2 When 20cm 2 / Vs, 25cm 2 / Vs, or 30cm 2 / Vs. Furthermore, the linear mobility is (Vg-Vth)×Cox=1×10 -6 C / cm 2 30cm when 2 / Vs or 35cm 2 / Vs. The linear mobility values ​​above are values ​​that cannot be achieved with conventional characteristics.

[0115] 26 is a diagram showing the gate capacitance dependency of normalized linear mobility in a semiconductor device according to one embodiment of the present invention. As described above, normalized linear mobility is the mobility obtained by standardizing the linear mobility with (Vg-Vth)×Cox on the horizontal axis by the linear mobility at Vg=Vth. The normalized linear mobility shown in FIG. 26 shows the same behavior as the linear mobility shown in FIG. 25. The normalized linear mobility is (Vg-Vth)×Cox=5×10 in any of the cases of characteristics A' to F'. -7 C / cm 2 When the normalized linear mobility is greater than 3.0, 3.5, or 4.0, the normalized linear mobility is (Vg-Vth) x Cox = 1 x 10 -6 C / cm 2 The normalized linear mobility exceeds 4.0 or 4.5 when the normalized linear mobility is 1.0 or 1.5 times the normalized linear mobility ...

[0116] As described above, in the semiconductor device 10 of the first embodiment, it is possible to obtain linear mobility and normalized linear mobility that cannot be achieved in conventional semiconductor devices, regardless of the gate capacitance Cox associated with the film thickness of the gate insulating layers 110 and 120.

[0117] The above-described embodiments of the present invention may be combined as appropriate as long as they are not mutually inconsistent. Furthermore, those in which a person skilled in the art appropriately adds or removes components or modifies designs, or adds or omits steps or modifies conditions based on the embodiments, are also included in the scope of the present invention as long as they include the gist of the present invention.

[0118] Even if there are other effects and advantages different from those brought about by the aspects of each of the above-mentioned embodiments, those that are clear from the description in this specification or that can be easily predicted by a person skilled in the art are naturally understood to be brought about by the present invention. [Explanation of symbols]

[0119] 10: semiconductor device, 11: driving transistor, 12: selection transistor, 20: display device, 22: liquid crystal region, 24: sealing region, 26: terminal region, 100: substrate, 105: gate electrode, 109: wiring, 110, 120: gate insulating layer, 111: contact hole, 130: metal oxide layer, 140: oxide semiconductor layer, 150, 160: insulating layer, 190: metal oxide layer, 200: source-drain electrode, 201: source electrode, 203: drain electrode, 209: wiring, 210: storage capacitance element, 211: signal line, 212: gate line, 213: anode power line, 214: cathode power line, 300: array substrate, 301: pixel circuit, 302: source driver circuit, 303: gate driver circuit, 304: source wiring, 305: gate wiring, 306: terminal portion, 307: connection wiring, 310: seal portion, 311: liquid crystal element, 320: opposing substrate, 330: flexible printed circuit board, 340: IC chip, 350: storage capacitance element, 360: insulating layer, 362: insulating layer, 363: opening, 370: common electrode, 380: insulating layer, 381: opening, 382: opening, 390: pixel electrode, 392: light emitting layer, 394: common electrode, 395: electrode, DO: light emitting element

Claims

1. A gate electrode; a gate insulating layer on the gate electrode; an aluminum-based metal oxide layer on the gate insulating layer; an oxide semiconductor layer having a polycrystalline structure on the metal oxide layer; a source electrode and a drain electrode in contact with the oxide semiconductor layer from above the oxide semiconductor layer; an insulating layer on the source electrode and the drain electrode, The Id-Vg characteristics of the semiconductor device are as follows: The voltage supplied to the gate electrode is Vg, The threshold voltage of the semiconductor device is Vth, When the capacitance of the gate insulating layer sandwiched between the gate electrode and the oxide semiconductor layer is Cox, The linear mobility is (Vg-Vth)×Cox=5×10 -7 C / cm 2 When 2 A semiconductor device exceeding / Vs.

2. The linear mobility is (Vg-Vth)×Cox=1×10 -6 C / cm 2 When 30 cm 2 The semiconductor device according to claim 1 , wherein the Vref exceeds Vs.

3. A gate electrode; a gate insulating layer on the gate electrode; an aluminum-based metal oxide layer on the gate insulating layer; an oxide semiconductor layer having a polycrystalline structure on the metal oxide layer; a source electrode and a drain electrode in contact with the oxide semiconductor layer from above the oxide semiconductor layer; an insulating layer on the source electrode and the drain electrode, The Id-Vg characteristics of the semiconductor device are as follows: The voltage supplied to the gate electrode is Vg, The threshold voltage of the semiconductor device is Vth, When the capacitance of the gate insulating layer sandwiched between the gate electrode and the oxide semiconductor layer is Cox, The linear mobility is (Vg-Vth)×Cox=1×10 -6 C / cm 2 When 30 cm 2 A semiconductor device exceeding / Vs.

4. A gate electrode; a gate insulating layer on the gate electrode; an aluminum-based metal oxide layer on the gate insulating layer; an oxide semiconductor layer having a polycrystalline structure on the metal oxide layer; a source electrode and a drain electrode in contact with the oxide semiconductor layer from above the oxide semiconductor layer; an insulating layer on the source electrode and the drain electrode, The Id-Vg characteristics of the semiconductor device are as follows: The voltage supplied to the gate electrode is Vg, The threshold voltage of the semiconductor device is Vth, When the capacitance of the gate insulating layer sandwiched between the gate electrode and the oxide semiconductor layer is Cox, The normalized linear mobility normalized by the linear mobility at Vg=Vth is given by: (Vg-Vth)×Cox=5×10 -7 C / cm 2 When the semiconductor device has a capacitance of 3.0 or more, the capacitance of the semiconductor device exceeds 3.

0.

5. The normalized linear mobility is (Vg-Vth)×Cox=1×10 -6 C / cm 2 The semiconductor device according to claim 4 , wherein the resistance exceeds 4.0 when

6. A gate electrode; a gate insulating layer on the gate electrode; an aluminum-based metal oxide layer on the gate insulating layer; an oxide semiconductor layer having a polycrystalline structure on the metal oxide layer; a source electrode and a drain electrode in contact with the oxide semiconductor layer from above the oxide semiconductor layer; an insulating layer on the source electrode and the drain electrode, The Id-Vg characteristics of the semiconductor device are as follows: The voltage supplied to the gate electrode is Vg, The threshold voltage of the semiconductor device is Vth, When the capacitance of the gate insulating layer sandwiched between the gate electrode and the oxide semiconductor layer is Cox, The normalized linear mobility normalized by the linear mobility at Vg=Vth is given by: (Vg-Vth)×Cox=1×10 -6 C / cm 2 When the semiconductor device has a thermal conductivity of 4.0 or more,

7. With respect to a channel region, which is a region where the gate electrode and the oxide semiconductor layer overlap and is sandwiched between the source electrode and the drain electrode, when a length of the channel region in a first direction connecting the source electrode and the drain electrode is L and a width of the channel region in a second direction perpendicular to the first direction is W, 7. The semiconductor device according to claim 1, wherein Vth is Vg when a current of W / L×10 nA flows through the semiconductor device in the Id-Vg characteristics of the semiconductor device when the voltage between the source electrode and the drain electrode is 0.1 V.

8. 7. The semiconductor device according to claim 1, wherein the linear mobility is determined based on an Id-Vg characteristic of the semiconductor device when a voltage between the source electrode and the drain electrode is 0.1 V.

9. The semiconductor device according to claim 1 , wherein the metal oxide layer includes aluminum oxide.

Citation Information

Patent Citations

  • Multilayer film including oxide semiconductor film and manufacturing method for semiconductor device

    JP2014099601A

  • Semiconductor device

    JP2016184771A

  • Semiconductor device and display device having semiconductor device

    JP2018006730A

  • Semiconductor device manufacturing method

    JP2021108405A

  • Manufacturing method for semiconductor device

    JP2021141338A