Adhesive composition, adhesive sheet, laminate and display comprising the laminate
The adhesive composition, featuring a specific acrylic polymer and curing agent, addresses adhesion and durability issues in optical displays by enhancing adhesion and resistance to heat and light, while using biologically derived materials to reduce petroleum use.
Patent Information
- Application Number
- JP2023079379
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-12
- Publication Date
- 2024-11-22
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing adhesives for optical displays face challenges in maintaining adhesion to both high-polar and low-polar adherends, heat resistance, wet heat whitening resistance, outgas resistance, light resistance, and impact resistance, particularly under high-temperature conditions, with a need for improved durability and reduced petroleum resource consumption.
An adhesive composition comprising an acrylic polymer with specific monomer ratios and a curing agent, optionally with a silane coupling agent, to enhance adhesion, heat resistance, and resistance to whitening and outgassing, while using biologically derived materials.
The adhesive composition demonstrates excellent adhesion, heat resistance, wet heat whitening resistance, outgassing resistance, and light resistance, maintaining adhesive strength even after heat aging, and reduces petroleum consumption.
Smart Images

Figure 2024163615000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a pressure-sensitive adhesive composition, a pressure-sensitive adhesive sheet, a laminate, and a display including the laminate. [Background technology]
[0002] Adhesive sheets having an adhesive layer formed from an adhesive are easy to handle and are therefore used in a wide range of fields such as label applications, medical applications, etc. Among them, adhesives used in applications where long-term use is expected, such as marking films, window films, automotive parts, optical displays, etc., require durability such as heat resistance, moist heat resistance, weather resistance, light resistance, and impact resistance, and in recent years, active research has been conducted on improving the durability of adhesives.
[0003] Various optical displays, such as liquid crystal displays (LCDs) and organic electroluminescence displays (OLEDs), are widely used as display devices. In addition to being used as display devices, optical displays are also used as input devices such as touch panels. A cover panel is installed on the touch panel to protect the surface. Usually, the components that make up these optical displays are bonded together via an adhesive layer.
[0004] As mentioned above, adhesives for optical displays, which are expected to be used for a long time, are required to have high durability, such as not lifting or peeling off from the adherend in high temperature / high humidity environments (peel resistance), not discoloring the adhesive layer itself to white (humid heat whitening resistance), and not discoloring the adhesive layer itself to yellow (yellowing resistance).In addition to the above durability, adhesives used to fasten cover panels made of transparent plastic materials such as polycarbonate (PC) and polymethyl methacrylate (PMMA) are required to not cause appearance defects due to gases generated from the transparent plastic (outgassing resistance).
[0005] In terms of durability, displays are required to have high durability, especially for in-vehicle applications. In particular, due to the recent revolutionary advances in information technology such as the fifth generation mobile communication system (5G), Internet of Things (IoT), and artificial intelligence (AI), the development of automobiles equipped with electric equipment and vehicles equipped with external displays has progressed, and the required performance has become even stricter, requiring heat resistance at higher temperatures such as 120°C (previously around 85-105°C). Therefore, it has been a major challenge to develop an adhesive that satisfies all of the heat resistance at higher temperatures and the continued requirements for humidity and heat whitening resistance and outgassing resistance. In addition, compared to displays that are used in a fixed manner such as computer monitors and televisions, displays are more susceptible to impact and external force during handling, and there is a continuous need for lighter weight and thinner thickness, so impact resistance is required even in adhesive layers with a low coating amount.
[0006] Many studies have been conducted so far to satisfy the durability required for adhesives for displays. For example, the adhesive described in Patent Document 1 uses an acrylic adhesive obtained by copolymerizing a hydroxyl group-containing acrylic ester and a nitrogen-containing acrylic ester in order to impart resistance to moist heat whitening and outgassing, but the heat resistance and light resistance at 120°C are insufficient. In addition, the adhesive described in Patent Document 2 uses an acrylic adhesive obtained by copolymerizing an acrylic acid alkyl ester having 4 to 8 carbon atoms and N-(2-hydroxyethyl)acrylamide as monomers in order to suppress display unevenness, but the heat resistance, moist heat whitening resistance, outgassing resistance, and adhesion at 120°C are insufficient.
[0007] On the other hand, Patent Document 3 discloses an optical pressure-sensitive adhesive sheet that suppresses the generation of bubbles even in a high-temperature environment and exhibits excellent adhesion to an adherend, and Examples 1 to 4 describe a pressure-sensitive adhesive composition that is a mixture of an acrylic polymer obtained by copolymerizing a monomer mixture containing 25 to 30 parts by weight of 4-hydroxybutyl acrylate (4HBA) in 100 parts by weight of a monomer component, a high Tg acrylic polymer, a crosslinking compound, and a photopolymerization initiator. However, such a pressure-sensitive adhesive composition containing an acrylic polymer having a large amount of hydroxyl groups has a problem that it has insufficient adhesion to adherends with low polarity such as cycloolefin polymers, although it exhibits good adhesion to adherends with high polarity such as glass surfaces.
[0008] Furthermore, in recent years, the demand for displays has fluctuated rapidly, and there are increasing cases where the displays are stored in the form of adhesive sheets for long periods of time. Even if all of the required quality described above is met, there is a concern that the adhesive strength may decrease due to exposure to high temperature environments for long periods of time, depending on the adhesive composition.
[0009] In addition to the increasing demands for performance and the handling of adhesives, the depletion of petroleum resources and the emission of carbon dioxide from the combustion of petroleum-derived products are becoming issues in the industries in which adhesive sheets are used. Therefore, attempts are being made to conserve petroleum resources by using bio-derived materials instead of petroleum-derived materials in various industries, starting with the packaging materials field, as well as in the optical and semiconductor fields.
[0010] In a pressure-sensitive adhesive mainly composed of an acrylic polymer, a method for increasing the ratio of biologically derived materials includes a method for obtaining an acrylic polymer by copolymerizing a monomer mixture containing a linear alkyl alcohol produced from a living organism and a (meth)acrylic acid alkyl ester monomer obtained by esterifying (meth)acrylic acid. Since linear alcohols derived from living organisms are currently distributed at a relatively low cost and in stable quantities, they can be used industrially. For example, Patent Document 4 discloses a pressure-sensitive adhesive obtained by copolymerizing a monomer mixture containing a biomass-derived acrylate having an alkyl group with 12 to 24 carbon atoms, but the conditions for the heat resistance retention test are low temperature and short time, and the durability under high temperature conditions is insufficient. [Prior art documents] [Patent documents]
[0011] [Patent Document 1] JP 2017-106000 A [Patent Document 2] JP 2007-264092 A [Patent Document 3] Patent Publication No. 2022-069221 [Patent Document 4] JP 2020-105308 A Summary of the Invention [Problem to be solved by the invention]
[0012] The problem that the present invention aims to solve is to provide an adhesive that has adhesion to high-polarity and low-polarity adherends, heat resistance, moist heat whitening resistance, outgassing resistance, light resistance, impact resistance, and a sufficient pot life after mixing with a curing agent, and to provide an adhesive sheet and laminate that have sufficient adhesion even after thermal aging using the same, and a display that includes the laminate. [Means for solving the problem]
[0013] As a result of extensive investigations, the present inventors have found that the problems of the present invention can be solved in the following aspect, and have thus completed the present invention. That is, the present invention provides a pressure-sensitive adhesive composition comprising an acrylic polymer (A) and a curing agent (B), The acrylic polymer (A) is a copolymer of a monomer mixture containing the following monomer (a1), monomer (a2), and at least one of monomer (a3-1) and monomer (a3-2): A pressure-sensitive adhesive composition comprising, based on 100 mass% of a monomer mixture, 5 to 50 mass% of monomer (a1), 30 to 80 mass% of monomer (a2), and 2 to 20 mass% of monomer (a3). (a1) (Meth)acrylic acid alkyl ester monomer having an alkyl group having 1 to 4 carbon atoms (a2) (Meth)acrylic acid alkyl ester monomer having a linear alkyl group having 8 to 18 carbon atoms (a3) Monomer (a3-1) having a carboxy group and monomer (a3-2) having a hydroxy group
[0014] The present invention also relates to the above pressure-sensitive adhesive composition, wherein the curing agent (B) contains an epoxy-based curing agent.
[0015] The present invention also relates to the above pressure-sensitive adhesive composition, further comprising a silane coupling agent (C).
[0016] The present invention also relates to the above pressure-sensitive adhesive composition, wherein the content of the hydroxyl group-containing monomer (a3-2) is 10 mass % or less based on 100 mass % of the monomer mixture constituting the acrylic polymer.
[0017] The present invention also relates to the above pressure-sensitive adhesive composition, wherein the content of the nitrogen atom-containing monomer is 10 mass % or less in 100 mass % of the monomer mixture constituting the acrylic polymer.
[0018] The present invention also relates to a pressure-sensitive adhesive sheet comprising a pressure-sensitive adhesive layer made of the pressure-sensitive adhesive composition.
[0019] The present invention also relates to a laminate comprising the above pressure-sensitive adhesive sheet and a light-transmitting substrate.
[0020] The present invention also relates to a display comprising the above laminate, a polarizing plate, and an optical element. Effect of the Invention
[0021] The present invention makes it possible to provide an adhesive that combines adhesion to high-polarity and low-polarity adherends, heat resistance, resistance to moist heat whitening, outgassing resistance, light resistance, impact resistance, and a sufficient pot life after mixing with a curing agent, as well as an adhesive sheet and laminate that retain sufficient adhesion even after thermal aging using the same, and a display that includes the laminate. [Brief description of the drawings]
[0022] [Figure 1] 1 is a schematic cross-sectional view partially showing a laminate of the present invention. [Diagram 2] FIG. 1 is a schematic cross-sectional view partially illustrating a display, which is an example of the use of the laminate of the present invention. [Diagram 3] 1 is a schematic cross-sectional view partially illustrating a pressure-sensitive adhesive sheet of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0023] The pressure-sensitive adhesive, pressure-sensitive adhesive sheet, laminate and display of the present invention will be described below, but the present invention is not limited thereto. In this specification, the term "(meth)acrylic acid ester" includes acrylic acid ester and methacrylic acid ester, and the term "(meth)acryloxy group" includes acryloxy group and methacryloxy group. The term "monomer" refers to a monomer having an ethylenically unsaturated group. In addition, in this specification, a numerical range specified by "~" includes the numerical values written before and after "~" as the range of the lower and upper limits. Furthermore, "film" and "sheet" are not distinguished by thickness. In other words, in this specification, a "sheet" includes a thin film-like material, and a "film" includes a thick sheet-like material. Furthermore, the adherend refers to a counterpart to which the pressure-sensitive adhesive layer of the pressure-sensitive adhesive sheet is attached. Unless otherwise noted, the various components appearing in this specification may be used independently as a single type or as a combination of two or more types.
[0024] <<Adhesive composition>> The pressure-sensitive adhesive composition of the present invention contains an acrylic polymer (A) and a curing agent (B).
[0025] <Acrylic polymer (A)> The acrylic polymer (A) is a copolymer of a monomer mixture containing monomer (a1), monomer (a2), and at least one of monomer (a3-1) and monomer (a3-2) described below, and is characterized in that it contains 5 to 50 mass% of (a1), 30 to 80 mass% of (a2), and 2 to 20 mass% or less of monomer (a3) based on 100 mass% of the monomer mixture.
[0026] [Monomer (a1)] (a1) is a (meth)acrylic acid alkyl ester monomer having an alkyl group having 1 to 4 carbon atoms. However, in this specification, a (meth)acrylic acid ester monomer having a carboxy group or a hydroxy group is considered to be monomer (a3) even if it has an alkyl group having 1 to 4 carbon atoms, and a (meth)acrylic acid ester monomer having a functional group other than a carboxy group or a hydroxy group, such as a nitrogen atom, is considered to be an other monomer.
[0027] The content of (a1) is 5 to 50 mass% in 100 mass% of the monomer mixture, preferably 17 to 47 mass%, more preferably 22 to 42 mass%, and most preferably 27 to 37 mass%. If the content of (a1) is less than 5 mass%, the cohesive strength of the adhesive layer decreases, resulting in insufficient adhesive strength, heat resistance, and light resistance. If the content of (a1) is more than 50 mass%, the tack of the adhesive layer decreases, resulting in insufficient adhesive strength, heat resistance, and light resistance.
[0028] Examples of the monomer (a1) include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, butyl (meth)acrylate, etc. Among them, in terms of adhesive strength and heat resistance, methyl (meth)acrylate and ethyl (meth)acrylate are preferred, and methyl (meth)acrylate is more preferred.
[0029] [Monomer (a2)] (a2) is a (meth)acrylic acid alkyl ester monomer having a linear alkyl group with 8 to 18 carbon atoms. Since (meth)acrylic acid alkyl ester monomers with such a carbon number are available as biologically derived materials, the proportion of biologically derived materials can be increased by using these. In addition, the polarity of the entire adhesive layer can be reduced, so that the adhesive strength to an adherend with low polarity can be increased. In addition, since the alkyl group is linear, it can be partially crystallized in the adhesive layer, thereby increasing heat resistance.
[0030] Examples of monomer (a2) include normal octyl (meth)acrylate, normal nonyl (meth)acrylate, normal decyl (meth)acrylate, normal undecyl (meth)acrylate, normal dodecyl (meth)acrylate, normal tridecyl (meth)acrylate, normal tetradecyl (meth)acrylate, normal pentadecyl (meth)acrylate, normal hexadecyl (meth)acrylate, normal heptadecyl (meth)acrylate, and normal octadecyl (meth)acrylate.
[0031] The content of (a2) is 30-80% by mass, preferably 37-67% by mass, more preferably 42-62% by mass, and most preferably 47-57% by mass, based on 100% by mass of the monomer mixture. If the content of (a2) is less than 30% by mass, sufficient biological material cannot be used for the adhesive or adhesive layer, and the adhesive strength to low-polarity adherends is insufficient, making it impossible to use the adhesive for attachment to such adherends. If the content of (a2) is more than 80% by mass, the cohesive strength of the adhesive layer decreases, resulting in insufficient adhesive strength, heat resistance, and light resistance.
[0032] In 100% by mass of (a2), the content of (meth)acrylic acid alkyl ester monomers having a linear alkyl group having 12 to 14 carbon atoms is preferably 30% by mass or more, more preferably 50% by mass or more, and even more preferably 70% by mass or more. By setting the content at such a ratio, high adhesive strength is easily obtained regardless of the polarity of the adherend.
[0033] In 100% by mass of (a2), the content of methacrylate is preferably 35% by mass or more, more preferably 45% by mass or more, and even more preferably 55% by mass or more. In terms of adhesive strength and heat resistance, a higher content of methacrylate is preferable, and the content of methacrylate in 100% by mass of (a2) may be 100% by mass.
[0034] [Monomer (a3)] (a3) is a monomer (a3-1) having a carboxy group and a monomer (a3-2) having a hydroxy group. (a3) may contain both the monomer (a3-1) having a carboxy group and the monomer (a3-2) having a hydroxy group, or may contain only one of them, but it is preferable to contain the monomer (a3-1) having a carboxy group. By containing the monomer (a3-1) having a carboxy group, the cohesive strength of the adhesive layer is increased, and the adhesive strength and heat resistance are easily increased, and impact resistance can be increased.
[0035] The content of (a3) is 2 to 20% by mass, preferably more than 7.5% by mass and 19% by mass or less, and more preferably 8 to 12% by mass, based on 100% by mass of the monomer mixture. By making it 2% by mass or more, it is possible to ensure resistance to moist heat, and by making it 20% by mass or less, it is possible to reduce outgassing and further to ensure a sufficient pot life after mixing with a curing agent.
[0036] The monomer (a3-1) having a carboxy group is not limited as long as it has a carboxy group in the molecule, and specific examples thereof include (meth)acrylic acid, p-carboxybenzyl acrylate, β-carboxyethyl acrylate, maleic acid, monoethyl maleic acid, itaconic acid, citraconic acid, and fumaric acid. Of these, (meth)acrylic acid is preferred from the viewpoint of adhesive strength, and acrylic acid is more preferred.
[0037] The content of the monomer (a3-1) having a carboxy group in 100% by mass of the monomer mixture is preferably more than 7.5% by mass and not more than 16% by mass, more preferably more than 7.5% by mass and not more than 12% by mass, and even more preferably 8 to 10% by mass. By exceeding 7.5% by mass, impact resistance can be ensured, and by making it not more than 16% by mass, outgassing can be reduced, adhesive strength to a low-polarity adherend can be ensured, and furthermore, a sufficient pot life after mixing with a curing agent can be ensured.
[0038] The monomer (a3-2) having a hydroxy group is not limited as long as it is a monomer having a hydroxy group in the molecule, and specific examples thereof include 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, and 4-hydroxybutyl (meth)acrylate. Of these, 2-hydroxyethyl (meth)acrylate and 4-hydroxybutyl (meth)acrylate are preferred from the viewpoints of adhesive strength and resistance to moist heat.
[0039] The content of the hydroxyl group-containing monomer (a3-2) in 100% by mass of the monomer mixture is preferably 10% by mass or less, more preferably 5% by mass or less, and most preferably 2% by mass or less. By making the hydroxyl group-containing monomer 10% by mass or less, the adhesive strength to adherends with low polarity is ensured, and the reaction between the hydroxyl group and the carboxyl group of (a3) is less likely to occur during thermal aging of the adhesive sheet, making it easier to avoid a decrease in adhesive strength.
[0040] [Nitrogen-containing monomers] The monomer mixture constituting the acrylic polymer (A) may further contain a nitrogen atom-containing monomer. As such a monomer, a monomer having a polymerizable functional group with an unsaturated double bond such as a (meth)acryloyl group or a vinyl group and a nitrogen atom may be used without any particular limitation. Among such monomers, a monomer having a cyclic structure is preferred, and a monomer having a nitrogen atom in the cyclic structure is more preferred.
[0041] Examples of the nitrogen atom-containing monomer include N-vinyl lactams, cyclic amides such as vinylpyridine, vinylpyrimidine, vinylpiperazine, vinylpyrazine, vinylpyrrole, vinylimidazole, vinyloxazole, vinylmorpholine, and (meth)acryloylmorpholine, N-vinyl carboxylic acid amides such as N-vinylformamide and N-vinylacetamide, acrylonitrile, acrylamide, and N,N-dimethylacrylamide. N-vinyl lactams are monomers having a cyclic lactam ring, and examples thereof include N-vinyl-2-pyrrolidone, N-vinyl-2-piperidone, N-vinyl-ε-caprolactam, and compounds having a structure in which one or more of these hydrogen atoms are substituted with a substituent. Examples of the substituent include an alkyl group having 1 to 20 carbon atoms, an alkyl group having 2 to 20 carbon atoms, an aryl group having 6 to 20 carbon atoms, an alkoxy group having 1 to 20 carbon atoms, a carboxy ester group having 3 to 20 carbon atoms, and an amino group having 1 to 20 carbon atoms, but do not include acidic groups such as a hydroxy group, a carboxylic acid (salt) group, a sulfonic acid (salt) group, or a hypophosphorous acid (salt) group. Among these, cyclic amides and N-vinyl lactams are preferred, and N-vinyl lactams are more preferred.
[0042] The content of the nitrogen atom-containing monomer is preferably 5% by mass or less, more preferably 2% by mass or less, based on 100% by mass of the monomer mixture. By setting the content to 5% by mass or less, it becomes easier to improve heat yellowing resistance and light yellowing resistance.
[0043] [Other monomers] The monomer mixture constituting the acrylic polymer (A) may contain other monomers as optional components in addition to the above (a1) to (a3) and the nitrogen atom-containing monomer. Examples include (meth)acrylic acid alkyl ester monomers having an alicyclic structure, (meth)acrylic acid alkyl ester monomers having a branched alkyl group, alkoxy-based (meth)acrylic acid esters such as methoxyethyl acrylate, vinyl-based monomers such as vinyl acetate and styrene, and monomers having a glycidyl group such as glycidyl (meth)acrylate. The content of other monomers is preferably 15% by mass or less, more preferably 10% by mass or less, and most preferably 5% by mass or less, based on 100% by mass of the monomer mixture.
[0044] (Production of acrylic polymer (A)) The acrylic polymer (A) can be produced by polymerizing the above-mentioned monomer mixture. The polymerization can be carried out by known polymerization methods such as solution polymerization, bulk polymerization, emulsion polymerization, and suspension polymerization, but solution polymerization is preferred. The solvent used in the solution polymerization is preferably, for example, acetone, methyl acetate, ethyl acetate, toluene, xylene, anisole, methyl ethyl ketone, cyclohexanone, etc. The polymerization temperature is preferably a boiling point reaction at 60 to 120°C. The polymerization time is preferably about 5 to 12 hours.
[0045] The polymerization initiator used in the polymerization is preferably a radical polymerization initiator, and the radical polymerization initiator is generally a peroxide or an azo compound. Examples of the peroxide include dialkyl peroxides such as di-t-butyl peroxide, dicumyl peroxide, t-butylcumyl peroxide, α,α'-bis(t-butylperoxy-m-isopropyl)benzene, and 2,5-di(t-butylperoxy)hexyne-3; Peroxyesters such as t-butyl peroxybenzoate, t-butyl peroxyacetate, and 2,5-dimethyl-2,5-di(benzoylperoxy)hexane; ketone peroxides such as cyclohexanone peroxide, 3,3,5-trimethylcyclohexanone peroxide, and methylcyclohexanone peroxide; Peroxyketals such as 2,2-bis(4,4-di-t-butylperoxycyclohexyl)propane, 1,1-bis(t-butylperoxy)3,3,5-trimethylcyclohexane, 1,1-bis(t-butylperoxy)cyclohexane, and n-butyl-4,4-bis(t-butylperoxy)valerate; Hydroperoxides such as cumene hydroperoxide, diisopropylbenzene hydroperoxide, and 2,5-dimethylcyclohexane-2,5-dihydroperoxide; Diacyl peroxides such as benzoyl peroxide, decanoyl peroxide, lauroyl peroxide, and 2,4-dichlorobenzoyl peroxide; Examples include peroxydicarbonates such as bis(t-butylcyclohexyl) peroxydicarbonate.
[0046] Examples of the azo compound include 2,2'-azobisbutyronitrile such as 2,2'-azobisisobutyronitrile (abbreviation: AIBN) and 2,2'-azobis(2-methylbutyronitrile); 2,2'-azobisvaleronitrile such as 2,2'-azobis(4-methoxy-2,4-dimethylvaleronitrile) and 2,2'-azobis(2,4-dimethylvaleronitrile); 2,2'-azobispropionitriles such as 2,2'-azobis(2-hydroxymethylpropionitrile); Examples include 1,1'-azobis-1-alkanenitriles such as 1,1'-azobis(cyclohexane-1-carbonitrile).
[0047] The polymerization initiator is preferably used in an amount of 0.01 to 10 parts by mass, more preferably 0.1 to 2 parts by mass, based on 100 parts by mass of the monomer mixture.
[0048] (Weight average molecular weight (Mw)) The weight average molecular weight of the acrylic polymer (A) is preferably 500,000 to 1,500,000, more preferably 600,000 to 1,200,000. By setting the weight average molecular weight within the above range, peel resistance, outgas resistance, and light resistance in high temperature / high humidity environments are further improved. The weight average molecular weight is a polystyrene-equivalent value measured by gel permeation chromatography (GPC).
[0049] <Hardening agent (B)> The adhesive composition of the present invention contains a curing agent (B). The curing agent to be blended into the adhesive is preferably one that reacts with the carboxyl group and / or hydroxyl group of the monomer (a3) by heat or the like to form a bond. The blending of the curing agent improves the cohesive strength of the adhesive layer, and improves the adhesive strength, heat resistance, and light resistance.
[0050] The curing agent can be selected from known curing agents such as epoxy-based curing agents, isocyanate-based curing agents, oxazoline-based curing agents, aziridine-based curing agents, carbodiimide-based curing agents, metal chelate-based curing agents, and melamine-based curing agents, taking into consideration the reactivity with the functional groups of the polymer in the adhesive. From the viewpoints of adhesive strength, light resistance, and impact resistance, it is preferable to include an epoxy-based curing agent.
[0051] Examples of epoxy-based curing agents include N,N,N',N'-tetraglycidyl-m-xylylenediamine, tetraglycidyl-3,3'-diaminodiphenylsulfone, tetraglycidyldiaminodiphenylmethane, 1,3-bis(N,N'-diglycidylaminomethyl)cyclohexane, N,N,N',N'-tetraglycidylaminophenylmethane (the above are examples of tetrafunctional epoxy compounds), glycerin diglycidyl ether, 1,6-hexanediol diglycidyl ether, etc., and these can be appropriately selected one or more. From the viewpoint of adhesive strength and heat resistance, it is preferable that the tetrafunctional epoxy compound is contained in 50% by mass or more of 100% by mass of the curing agent (B). When an epoxy-based curing agent is used, it is preferably contained in an amount of 0.05 to 0.4 parts by mass, more preferably 0.1 to 0.3 parts by mass, relative to 100 parts by mass of the acrylic polymer (A) in the adhesive composition. When the content is 0.05 parts by mass or more, the cohesive strength is further improved, and when it is 0.4 parts by mass or less, it becomes easier to achieve both cohesive strength and flexibility, making it easier to obtain sufficient adhesive strength, heat resistance, and light resistance.
[0052] The isocyanate-based curing agent is an isocyanate having two or more isocyanate groups. For example, aromatic polyisocyanates, aliphatic polyisocyanates, araliphatic polyisocyanates, alicyclic polyisocyanates, and their biuret forms, nurate forms, and adduct forms are preferred as isocyanates, and from the viewpoint of yellowing resistance, aliphatic polyisocyanates, alicyclic polyisocyanates, and their biuret forms, nurate forms, and adduct forms are more preferred. When an isocyanate-based curing agent is used, it is preferably contained in an amount of 1 to 5 parts by mass, more preferably 2 to 4 parts by mass, per 100 parts by mass of the acrylic polymer (A) in the adhesive composition. When the content is 1 part by mass or more, the cohesive strength is further improved, and when it is 5 parts by mass or less, it is easy to achieve both cohesive strength and flexibility, so that sufficient adhesive strength, heat resistance, and light resistance are easily obtained.
[0053] The biuret form is a self-condensation product having a biuret bond formed by self-condensation of an isocyanate monomer, for example, a biuret form of hexamethylene diisocyanate.
[0054] The nurate form is a trimer of an isocyanate monomer, such as a trimer of hexamethylene diisocyanate, a trimer of isophorone diisocyanate, or a trimer of tolylene diisocyanate.
[0055] The adduct is a bifunctional or higher isocyanate compound obtained by reacting an isocyanate monomer with a bifunctional or higher low-molecular active hydrogen-containing compound. Examples of the adduct include a compound obtained by reacting trimethylolpropane with hexamethylene diisocyanate, a compound obtained by reacting trimethylolpropane with tolylene diisocyanate, a compound obtained by reacting trimethylolpropane with xylylene diisocyanate, a compound obtained by reacting trimethylolpropane with isophorone diisocyanate, and a compound obtained by reacting 1,6-hexanediol with hexamethylene diisocyanate.
[0056] The isocyanate compound is preferably a trifunctional isocyanate compound from the viewpoint of forming a sufficient crosslinked structure. The isocyanate compound is more preferably an adduct or nurate, which is a reaction product between an isocyanate monomer and a trifunctional low molecular weight active hydrogen-containing compound. The isocyanate compound is preferably a trimethylolpropane adduct of hexamethylene diisocyanate, a nurate of hexamethylene diisocyanate, a trimethylolpropane adduct of tolylene diisocyanate, a nurate of tolylene diisocyanate, a trimethylolpropane adduct of isophorone diisocyanate, or a nurate of isophorone diisocyanate, and more preferably a trimethylolpropane adduct of hexamethylene diisocyanate, a trimethylolpropane adduct of tolylene diisocyanate, or a trimethylolpropane adduct of isophorone diisocyanate.
[0057] The oxazoline-based curing agent has two or more oxazoline groups in the molecule, and may be a low molecular weight compound or a polymer. Examples of the low molecular weight compound oxazoline-based curing agent include 2-vinyl-2-oxazoline, 2-vinyl-4-methyl-2-oxazoline, 2-vinyl-5-methyl-2-oxazoline, 2-isopropenyl-2-oxazoline, 2-isopropenyl-4-methyl-2-oxazoline, 2-isopropenyl-5-ethyl-2-oxazoline, 2,2'-bis-(2-oxazoline), 2,2'-methylene-bis-(2-oxazoline), 2,2'-ethylene-bis-(2-oxazoline), 2,2'-trimethylene-bis-(2-oxazoline), and 2,2'-tetramethylene-bis-(2-oxazoline). , 2,2'-hexamethylene-bis-(2-oxazoline), 2,2'-octamethylene-bis-(2-oxazoline), 2,2'-ethylene-bis-(4,4'-dimethyl-2-oxazoline), 2,2'-p-phenylene-bis-(2-oxazoline), 2,2'-m-phenylene-bis-(2-oxazoline), 2,2'-m-phenylene-bis-(4,4'-dimethyl-2-oxazoline), 2,2'-(1,3-phenylene)-bis-(2-oxazoline), bis-(2-oxazolinylcyclohexane)sulfide, bis-(2-oxazolinylnorbornane)sulfide, etc. Examples of oxazoline-based curing agents for polymers include polymers that contain addition-polymerizable oxazoline as an essential component. Examples of the addition-polymerizable oxazoline include 2-vinyl-2-oxazoline, 2-vinyl-4-methyl-2-oxazoline, 2-vinyl-5-methyl-2-oxazoline, 2-isopropenyl-2-oxazoline, 2-isopropenyl-4-methyl-2-oxazoline, 2-isopropenyl-5-methyl-2-oxazoline, and 2-isopropenyl-5-ethyl-2-oxazoline. When an oxazoline-based curing agent is used, it is preferable to include 3 to 10 parts by mass per 100 parts by mass of the acrylic polymer (A) in the adhesive composition. When the content is 3 parts by mass or more, the cohesive strength is further improved, and when it is 10 parts by mass or less, it is easy to achieve both cohesive strength and flexibility, so that sufficient adhesive strength, heat resistance, and light resistance are easily obtained.
[0058] Examples of the aziridine-based curing agent include N,N'-diphenylmethane-4,4'-bis(1-aziridinecarboxite), tris-2,4,6-(1-aziridinyl)-1,3,5-triazine, and 4,4'-bis(ethyleneiminocarbonylamino)diphenylmethane. When an aziridine-based curing agent is used, it is preferable to include 1 to 5 parts by mass per 100 parts by mass of the acrylic polymer (A) in the adhesive composition. When the content is 1 part by mass or more, the cohesive strength is further improved, and when it is 5 parts by mass or less, it is easy to achieve both cohesive strength and flexibility, so that sufficient adhesive strength, heat resistance, and light resistance are easily obtained.
[0059] The carbodiimide compound is preferably a high molecular weight polycarbodiimide produced by decarboxylation condensation reaction of a diisocyanate compound in the presence of a carbodiimide catalyst. The commercially available high molecular weight polycarbodiimide is preferably the Carbodilite series of Nisshinbo Industries. Among them, Carbodilite V-03, 07, and 09 are preferable because they have excellent compatibility with organic solvents. When a carbodiimide-based curing agent is used, it is preferable to include 0.1 to 3 parts by mass per 100 parts by mass of the acrylic polymer (A) in the adhesive composition. When the content is 0.1 parts by mass or more, the cohesive strength is further improved, and when it is 3 parts by mass or less, it is easy to achieve both cohesive strength and flexibility, so that sufficient adhesive strength, heat resistance, and light resistance are easily obtained.
[0060] The metal chelate is preferably a coordination compound of a polyvalent metal such as aluminum, iron, copper, zinc, tin, titanium, nickel, antimony, magnesium, vanadium, chromium, and zirconium with acetylacetone or ethyl acetoacetate. Examples of the metal chelate include aluminum ethyl acetoacetate diisopropylate, aluminum tris acetylacetonate, aluminum bis ethyl acetoacetate monoacetylacetonate, and aluminum alkyl acetoacetate diisopropylate. When a metal chelate is used, it is preferably contained in an amount of 0.1 to 0.5 parts by mass, more preferably 0.2 to 0.4 parts by mass, per 100 parts by mass of the acrylic polymer (A) in the adhesive composition. When the content is 0.1 parts by mass or more, the cohesive strength is further improved, and when the content is 0.5 parts by mass or less, it is easy to achieve both cohesive strength and flexibility, so that sufficient adhesive strength, heat resistance, and light resistance are easily obtained.
[0061] Representative examples of the melamine-based curing agent include fully alkyl etherified melamine resins, methylol group-type melamine resins, and imino group-type melamine resins having imino groups in part. When a melamine-based curing agent is used, it is preferable to include 0.1 to 10 parts by mass per 100 parts by mass of the acrylic polymer (A) in the adhesive composition. When the content is 0.1 parts by mass or more, the cohesive strength is further improved, and when the content is 10 parts by mass or less, it is easy to achieve both cohesive strength and flexibility, so that sufficient adhesive strength, heat resistance, and light resistance are easily obtained.
[0062] <Silane coupling agent (C)> The pressure-sensitive adhesive composition of the present invention preferably contains a silane coupling agent (C). By containing the silane coupling agent (C), it is possible to improve the adhesive strength, heat resistance, wet heat whitening resistance, and light resistance. The silane coupling agent (C) is preferably contained in an amount of 0.05 to 1 part by mass, more preferably 0.1 to 0.5 parts by mass, per 100 parts by mass of the acrylic polymer (A). By containing the silane coupling agent (C) in an amount of 0.05 to 1 part by mass, it becomes easy to achieve both heat resistance, outgassing resistance, and light resistance.
[0063] Examples of the silane coupling agent (C) include an alkoxysilane compound having a (meth)acryloxy group, an alkoxysilane compound having a vinyl group, an alkoxysilane compound having an amino group, an alkoxysilane compound having a mercapto group, and an alkoxysilane compound having an epoxy group. Specific examples of commercially available products include KBM-403 (3-glycidoxypropyltrimethoxysilane), KBE-403 (3-glycidoxypropyltriethoxysilane), KBM-303 (2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane) (all manufactured by Shin-Etsu Chemical Co., Ltd.), BYK-325N (polyether-modified polymethylalkylsiloxane) (manufactured by BYK Japan KK), and the like.
[0064] Examples of chlorinated polyolefins include chlorinated polypropylene, acid-modified chlorinated polypropylene, acrylic-modified chlorinated polypropylene, chlorinated polyethylene, and chlorinated ethylene-vinyl acetate copolymer. From the viewpoints of good compatibility with acrylic polymers and the like and effective reduction in polarity, chlorinated polypropylene and chlorinated ethylene-vinyl acetate copolymer are preferred. Specific examples of commercially available products include Superchlorine 390S (chlorinated polypropylene, chlorine content 36%) and Superchlorine BX (chlorinated EVA, chlorine content 18%) (both manufactured by Nippon Paper Industries Co., Ltd.).
[0065] Adhesive sheet The pressure-sensitive adhesive sheet comprises a pressure-sensitive adhesive layer made of the pressure-sensitive adhesive composition of the present invention.
[0066] The pressure-sensitive adhesive sheet of the present invention preferably has a configuration in which a release film is attached to at least one side of the pressure-sensitive adhesive layer. Specifically, the pressure-sensitive adhesive sheet has a configuration in which release films are formed on both sides of the pressure-sensitive adhesive layer, or a release film is formed on one side of the pressure-sensitive adhesive layer and a light-transmitting substrate is provided on the other side of the pressure-sensitive adhesive, and the pressure-sensitive adhesive layer is formed from the pressure-sensitive adhesive composition of the present invention.
[0067] <Release film> The release film is not particularly limited, but a transparent plastic substrate can be suitably used. Examples of the material of the transparent plastic substrate include polyester such as polyethylene terephthalate (PET), acrylic resin such as polymethyl methacrylate (PMMA), polycarbonate, triacetyl cellulose, polysulfone, polyarylate, polycycloolefin, and other plastic materials. The plastic materials can be used alone or in combination of two or more kinds.
[0068] As the release film, among the above-mentioned transparent plastic substrates, a transparent plastic substrate having excellent heat resistance, i.e., a transparent plastic substrate in which deformation is suppressed or prevented under severe conditions such as high temperature, high temperature and high humidity, etc. As the transparent plastic substrate, a PET film or sheet is particularly suitable.
[0069] The thickness of the transparent plastic substrate is not particularly limited, and is, for example, preferably from 10 to 200 μm, and more preferably from 25 to 150 μm.
[0070] The pressure-sensitive adhesive sheet of the present invention has excellent adhesion, heat resistance, wet heat whitening resistance, outgas resistance, and light resistance to high polarity and low polarity adherends, and is therefore suitable as a pressure-sensitive adhesive for forming optical display members such as display devices such as LCDs and OLEDs and input devices such as touch panels, and for bonding these members together. The optical members are not particularly limited, and include PET films, COP films, polarizing plates, retardation plates, elliptical polarizing plates, optical compensation films, brightness improvement films, infrared / electromagnetic wave cut films, front anti-reflection films, surface protection films, films having an ITO (indium tin oxide) layer, films having a zinc oxide (ZnO) layer, films obtained by coating or printing metal nanoparticles, films obtained by coating or printing a dispersion containing carbon nanotubes, films obtained by coating or printing a dispersion containing graphene, films obtained by coating or printing a dispersion containing conductive polymers, metal plates formed of SUS, metal meshes, and further laminates thereof.
[0071] In coating the adhesive composition, a suitable liquid medium can be added to adjust the viscosity.Specific examples of the solvent include hydrocarbon solvents such as toluene, xylene, hexane, and heptane; ester solvents such as ethyl acetate and butyl acetate; ketone solvents such as acetone and methyl ethyl ketone; halogenated hydrocarbon solvents such as dichloromethane and chloroform; ether solvents such as diethyl ether, methoxytoluene, and dioxane, and other hydrocarbon solvents.However, water and alcohol should be used with caution because they may cause reaction inhibition between the acrylic polymer (A) and the isocyanate curing agent (B).
[0072] The coating method is not particularly limited, and various coating methods can be used, such as a Mayer bar, applicator, brush, spray, roller, gravure coater, die coater, lip coater, comma coater, knife coater, reverse coater, spin coater, etc. In addition, the drying and curing method is not particularly limited, and examples thereof include hot air drying, infrared rays, reduced pressure methods, and active energy rays, but hot air or steam heating at 60 to 180°C is preferred from the viewpoint of outgassing resistance.
[0073] The thickness of the pressure-sensitive adhesive layer is preferably from 2 to 1000 μm, more preferably from 5 to 500 μm. The pressure-sensitive adhesive layer may be in the form of either a single layer or a laminate of two or more layers.
[0074] <Laminate> The laminate includes a light-transmitting substrate and a pressure-sensitive adhesive layer, and the pressure-sensitive adhesive layer is formed using the pressure-sensitive adhesive sheet of the present invention. Specifically, for example, the release film is peeled off from the pressure-sensitive adhesive sheet of the present invention, and the pressure-sensitive adhesive layer is attached to the light-transmitting substrate to form the laminate. The laminate of the present invention has a structure of, for example, a light-transmitting substrate / a pressure-sensitive adhesive layer / a polarizing plate. In this case, it is preferable to provide the light-transmitting substrate, the pressure-sensitive adhesive layer, and the polarizing plate in this order. This makes it possible to obtain a laminate with excellent transparency.
[0075] <Light transparent base material> A transparent plastic substrate is used as the light-transmitting substrate. Examples of the material of such a light-transmitting substrate include acrylic resins such as polyethylene terephthalate (PET), polyethylene naphthalate, and polymethyl methacrylate (PMMA), and plastic materials such as polycarbonate (PC), polycycloolefin (COP), polyimide, polyphenylene ether, polysulfone, polyethersulfone, polystyrene, and polypropylene. In particular, PET film or PC is preferable, and PC is more preferable in terms of durability. The plastic materials can be used alone or in combination of two or more kinds. The light-transmitting substrate may be subjected to an appropriate surface treatment, for example, a physical treatment such as a corona discharge treatment or a plasma treatment, or a chemical treatment such as an undercoat treatment.
[0076] An example of a schematic cross-sectional view partially showing the laminate of the present invention is shown in Fig. 1. In Fig. 1, 3 is a light-transmitting substrate (cover panel), 1 is a pressure-sensitive adhesive layer, and 4 is a polarizing plate.
[0077] In the laminate shown in FIG. 1, a light-transmitting substrate (cover panel) is attached to a polarizing plate via a pressure-sensitive adhesive layer.
[0078] <Production of Laminate> The laminate can be manufactured, for example, by peeling off the release film from an adhesive sheet having a release film on both sides of the adhesive layer, and attaching the adhesive layer to an adherend such as a light-transmitting flexible substrate or a polarizing plate to form a laminate. Alternatively, the release film can be peeled off from an adhesive sheet having a release film on one side of the adhesive layer and a light-transmitting substrate on the other side, and attaching the adhesive layer to an adherend such as a light-transmitting flexible substrate or a polarizing plate to form a laminate. Furthermore, after forming the adhesive layer directly on the light-transmitting flexible substrate, the adhesive layer can be attached to an adherend or an adhesive layer of another adhesive sheet to form a laminate.
[0079] "display" The display comprises the laminate of the present invention, a polarizing plate, and an optical element, and thereby has excellent visibility. The optical element is not particularly limited, and examples thereof include a liquid crystal element and an organic EL element.
[0080] Fig. 2 shows an example of a schematic cross-sectional view partially illustrating a display, which is an example of the use of the pressure-sensitive adhesive sheet of the present invention. In Fig. 2, 3 is a light-transmitting substrate (cover panel), 1 is a pressure-sensitive adhesive layer 1, 4 is a polarizing plate, 5 is a pressure-sensitive adhesive layer 2, 6 is a barrier layer such as silicon nitride, 7 is an organic EL layer, 8 is a support such as polyimide, and 9 is an organic EL cell. Note that the configuration of the display is not limited to that shown in Fig. 2.
[0081] In the display shown in Fig. 2, a light-transmitting substrate (cover panel) is attached to a polarizing plate via the pressure-sensitive adhesive layer (pressure-sensitive adhesive layer 1) of the present invention, and is further attached to an organic EL cell via a pressure-sensitive adhesive layer for polarizing plate (pressure-sensitive adhesive layer 2). Thus, the pressure-sensitive adhesive sheet of the present invention can be used in a form in which a transparent pressure-sensitive adhesive layer formed from the pressure-sensitive adhesive is attached to a light-transmitting substrate (cover panel) and a polarizing plate, and the laminate is further attached to an organic EL cell via a pressure-sensitive adhesive layer for polarizing plate. For example, in FIG. 2, the pressure-sensitive adhesive layer of the present invention can be used as either pressure-sensitive adhesive layer 1 or pressure-sensitive adhesive layer 2. In general, when comparing pressure-sensitive adhesive layer 1 and pressure-sensitive adhesive layer 2, the pressure-sensitive adhesive layer 1 has higher quality requirements, and since the pressure-sensitive adhesive of the present invention has good adhesion and bonding properties to the substrate, it is preferably used for pressure-sensitive adhesive layer 1. In this case, the pressure-sensitive adhesive for forming pressure-sensitive adhesive layer 2 may be the pressure-sensitive adhesive of the present invention or a conventionally known pressure-sensitive adhesive.
[0082] There are no particular limitations on the uses of the displays, but examples include OLED televisions, OLED smartphones, OLED tablets, and OLED smartwatches. EXAMPLES
[0083] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples. In the examples, unless otherwise specified, "parts" means "parts by mass" and "%" means "% by mass". The blending amounts in the tables are parts by mass, and the amounts other than the solvent are calculated as non-volatile contents. The blanks in the tables indicate that no blending was performed. The method for measuring the weight average molecular weight of the acrylic polymer is as follows.
[0084] <Measurement of weight average molecular weight (Mw)> Weight average molecular weight (Mw) was measured by gel permeation chromatography (GPC). Shimadzu Corporation's GPC device: LC-GPC system "Prominence" was used. Tosoh Corporation's TSKgel α-M was used as the column, and two columns were connected in series. N,N-dimethylformamide (DMF) was used as the eluent, and measurements were performed at 40°C. Mw was determined by conversion using polystyrene with a known Mw as the standard substance.
[0085] <Production example of acrylic polymer> (Acrylic polymer (A-1)) Using a reaction apparatus equipped with a stirrer, reflux condenser, nitrogen inlet, thermometer, and dropping tube, 34 parts of methyl acrylate (MA) as monomer (a1), 24 parts of dodecyl acrylate (DDA) and 31 parts of dodecyl methacrylate (DDMA) as monomer (a2), 9 parts of acrylic acid (AA) as monomer (a3), 2 parts of 2-ethylhexyl acrylate (2EHA) as other monomers, half of the above monomer mixtures, 0.2 parts of azobisisobutyronitrile as an initiator, and 60 parts of ethyl acetate as a solvent were charged into a reaction vessel, and the remaining half of the monomer mixture, 60 parts of ethyl acetate, and 0.2 parts of azobisisobutyronitrile were added and mixed, and the solution was dropped from the dropping tube over about 2 hours, and polymerized for 6 hours at about 80 ° C. under a nitrogen atmosphere. After the reaction was completed, it was cooled and diluted with ethyl acetate to obtain an acrylic polymer solution (A-1) with a non-volatile content of 30%. The weight average molecular weight (Mw) of the obtained acrylic polymer is shown in Table 1.
[0086] (Acrylic polymers (A-2 to A-45, A'-1 to A'-6)) Acrylic polymers (A-2 to A-45, A'-1 to A'-6) were synthesized in the same manner as for the production of acrylic polymer (A-1), except that the compositions and amounts (parts by mass) were changed to those shown in Tables 1 to 4. The weight average molecular weights of the obtained acrylic polymers are shown in Tables 1 to 4.
[0087] [Table 1]
[0088] [Table 2]
[0089] [Table 3]
[0090] [Table 4]
[0091] The abbreviations are as follows: [Monomer (a1)] MA: Methyl acrylate (alkyl group carbon number 1) MMA: Methyl methacrylate (alkyl group carbon number 1) EA: Ethyl acrylate (alkyl group carbon number: 2) BMA: n-butyl methacrylate (alkyl group carbon number: 4) [Monomer (a2)] OA: normal octyl acrylate (alkyl group carbon number: 8) OMA: normal octyl methacrylate (alkyl group carbon number: 8) DA: normal decyl acrylate (alkyl group carbon number: 10) DMA: normal decyl methacrylate (alkyl group carbon number: 10) DDA: normal dodecyl acrylate (alkyl group carbon number: 12) DDMA: normal dodecyl methacrylate (alkyl group carbon number 12) TrDA: normal tridecyl acrylate (alkyl group carbon number: 13) TrDMA: normal tridecyl methacrylate (alkyl group carbon number: 13) TeDA: normal tetradecyl acrylate (alkyl group carbon number 14) TeDMA: normal tetradecyl acrylate (alkyl group carbon number 14) HDA: normal hexadecyl acrylate (alkyl group carbon number 16) HDMA: normal hexadecyl methacrylate (alkyl group carbon number 16) ODA: normal octadecyl acrylate (alkyl group carbon number: 18) ODMA: normal octadecyl methacrylate (alkyl group carbon number 18) [Monomer (a3)] AA: Acrylic acid MAA: Methacrylic acid HEA: Hydroxyethyl acrylate 4HBA: 4-Hydroxy n-butyl acrylate [Other monomers] 2EHA: 2-Ethylhexyl acrylate iDA: Isodecyl acrylate iDMA: Isodecyl methacrylate IBXA: Isobornyl acrylate THFA: Tetrahydrofurfuryl acrylate NVP: n-vinyl-2-pyrrolidone NVCL: n-vinyl-ε-caprolactam ACMO: Acryloylmorpholine AAm: Acrylamide
[0092] The materials used in the examples and comparative examples are listed below. <Hardening agent (B)> B-1: "TETRAD-X" (N,N,N',N'-tetraglycidyl-m-xylylenediamine manufactured by Mitsubishi Gas Chemical Co., Inc.) B-2: "TG3DAS" (Tetraglycidyl-3,3'-diaminodiphenyl sulfone, manufactured by Mitsui Fine Chemicals, Inc.) B-3: "Sumiepoxy ELM-434" (Sumitomo Chemical Co., Ltd., tetraglycidyldiaminodiphenylmethane) B-4: "Sumiepoxy ELM100" (Sumitomo Chemical Co., Ltd., N-[2-methyl-4-(oxiranylmethoxy)phenyl]-N-(oxiranylmethyl)oxiranemethanamine) B-5: "Denacol EX-313" (Glycerol poly(di, tri)glycidyl ether, manufactured by Nagase Chemical Co., Ltd.) B-6: "GAN" (N,N-diglycidylaniline manufactured by Nippon Kayaku Co., Ltd.) B-7: "Coronate L" (manufactured by Tosoh Corporation, an adduct of trimethylolpropane and tolylene diisocyanate) B-8: "Aluminum Chelate A" (Kawaken Fine Chemicals Co., Ltd., aluminum tris(acetylacetonate))
[0093] <Silane coupling agent (C)> KBE-403: (3-glycidoxypropyltriethoxysilane, manufactured by Shin-Etsu Chemical Co., Ltd.) KBM-303: ([2-(3,4-epoxycyclohexyl)ethyl]trimethoxysilane, manufactured by Shin-Etsu Chemical Co., Ltd.)
[0094] <Example 1> A pressure-sensitive adhesive composition was obtained by blending 100 parts of the acrylic polymer (A-1) with 0.25 parts of (B-1) "TETRAD-X" (N,N,N',N'-tetraglycidyl-m-xylylenediamine, manufactured by Mitsubishi Gas Chemical Company, Inc.) as the curing agent (B) and 0.1 parts of KBE-403 (3-glycidoxypropyltriethoxysilane, manufactured by Shin-Etsu Chemical Co., Ltd.) as the silane coupling agent (C). The obtained adhesive composition was coated using a comma coater onto a 38 μm thick release liner (SP-PET-O1-BU: manufactured by Mitsui Chemicals Tocello) as a release sheet so that the thickness after drying would be 100 μm. After drying at 110°C for 3 minutes, a 75 μm thick release liner (SP-PET-O3-B3: manufactured by Mitsui Chemicals Tocello) as a release sheet was bonded to the adhesive layer and aged in this state at 23°C for 7 days to obtain an adhesive sheet.
[0095] <Examples 2 to 66 and Comparative Examples 1 to 6> As shown in Tables 5 and 6, pressure-sensitive adhesive compositions and pressure-sensitive adhesive sheets were obtained in the same manner as in Example 1, except that the types and amounts of the acrylic polymer, curing agent, and silane coupling agent were changed.
[0096] [Table 5]
[0097] [Table 6]
[0098] {Physical properties and evaluation of pressure-sensitive adhesive composition and pressure-sensitive adhesive sheet} The adhesive strength, heat resistance (peeling, yellowing), humidity and heat whitening resistance, outgassing resistance, light resistance (peeling, yellowing), usable time after addition of a curing agent, adhesive strength after thermal aging of the adhesive sheet, and impact resistance of the adhesive composition and adhesive sheet of the present invention were evaluated by the following methods. The results are shown in Tables 7 and 8.
[0099] <Adhesion to glass> The 38 μm release liner of the obtained adhesive sheet was peeled off, and the adhesive layer was attached to a PET film substrate (Toyobo Co., Ltd., Cosmoshine A-4360, thickness 100 μm), and cut to a size of 25 mm wide x 100 mm long to prepare a test adhesive sheet. The other 75 μm release liner of this test adhesive sheet was peeled off, and the adhesive layer was attached to a glass plate in an atmosphere of 23°C and 50% relative humidity (50% RH), and further pressed with a roll in accordance with JIS Z-0237. After 24 hours from pressing, the peel strength (peel angle 180°, peel speed 300 mm / min; unit N / 25 mm width) was measured using a tensile tester (Tensilon: Orientec Co., Ltd.). [Evaluation criteria] ◎: Peel strength is 25N / 25mm or more. Excellent. ○: Peel strength is 21N / 25mm or more and less than 25N / 25mm. Good. △: Peel strength is 18N / 25mm or more and less than 21N / 25mm. Fairly good. ▲: Peel strength is 15N / 25mm or more and less than 18N / 25mm. Practical use is possible. ×: Peel strength is less than 15N / 25mm. Not practical.
[0100] <Adhesion to low polarity films> The 38 μm release liner of the obtained adhesive sheet was peeled off, and the adhesive layer was attached to a PET film (Toyobo Co., Ltd., Cosmoshine A-4360, thickness 100 μm) as a substrate, and cut into a size of 25 mm wide x 100 mm long to prepare a test adhesive sheet. The other 75 μm release liner of this test adhesive sheet was peeled off, and the adhesive layer was attached to a 50 μm thick cycloolefin film in an atmosphere of 23 ° C - relative humidity 50% (50% RH), and further pressed with a roll according to JIS Z-0237. After 24 hours from pressing, the peel strength (peel angle 180 °, peel speed 300 mm / min; unit N / 25 mm width) was measured with a tensile tester (Tensilon: Orientec Co., Ltd.). [Evaluation Criteria] ◎: Peel strength is 20N / 25mm or more. Excellent. ○: Peel strength is 17N / 25mm or more and less than 20N / 25mm. Good. △: Peel strength is 14N / 25mm or more and less than 17N / 25mm. Fairly good. ▲: Peel strength is 12N / 25mm or more and less than 14N / 25mm. Practical use is possible. ×: Peel strength is less than 12N / 25mm. Not practical.
[0101] <Heat resistance (peeling)> The 38 μm release liner of the obtained adhesive sheet was peeled off, and the adhesive layer was attached to a 0.5 mm thick polycarbonate (PC) plate (Iupilon NF2000: manufactured by Mitsubishi Gas Chemical Co., Ltd.) using a laminator in an atmosphere of 23 ° C-50% RH. Next, the other 75 μm release liner of the adhesive sheet was peeled off, and the adhesive layer was attached to a glass plate using a laminator as described above. The test piece was prepared by applying a pressure of 0.5 MPa and holding it for 20 minutes in an atmosphere of 50 ° C, and laminated in the order of PC plate / adhesive layer / glass plate, and was left in an environment of 120 ° C for 1000 hours. The test piece was cooled at 23 ° C-50% RH for 24 hours, and then the degree of peeling of the test piece was visually evaluated. [Evaluation Criteria] ◎: Peeling area is less than 5% of the whole. Excellent. ○: Peeling area is 5% or more and less than 15% of the whole area. Good. △: Peeling area is 15% or more and less than 30% of the total area. Fairly good. ▲: Peeling area is 30% or more and less than 50% of the total area. Practical use is possible. ×: Peeling area is 50% or more of the whole. Not practical.
[0102] <Light resistance (yellowing)> The 38 μm release liner of the obtained adhesive sheet was peeled off, and the adhesive layer was attached to a glass plate using a laminator in an atmosphere of 23 ° C-50% RH. Next, the other 75 μm release liner of the adhesive sheet was peeled off, and the adhesive layer was attached to a glass plate using a laminator as described above. The test piece was prepared by applying a pressure of 0.5 MPa to the glass plate / adhesive layer / glass plate and holding it for 20 minutes in an atmosphere of 50 ° C., and was left for 1000 hours in an environment of 120 ° C. After cooling it for 1 hour at 23 ° C.-50% RH, the b * value was measured, and the difference Δb * from the b * value before the heat resistance test was calculated. The b * value was measured using a spectrophotometer SE6000 manufactured by Nippon Denshoku Kogyo Co., Ltd. under conditions of D65 light source and viewing angle 2 °. [Evaluation Criteria] ◎: Δb* is less than 0.8. Excellent. ○: Δb* is 0.8 or more and less than 1.3. Good. △: Δb* is 1.3 or more and less than 2.0. Fairly good. ▲: Δb* is 2.0 or more and less than 3.0. Practical use is possible. ×: Δb* is 3.0 or more. Not practical.
[0103] <Wet and heat whitening resistance (glass composition)> The 38 μm release liner of the obtained adhesive sheet was peeled off, and the adhesive layer was laminated to a glass plate using a laminator in an atmosphere of 23 ° C-50% RH. Next, the other 75 μm release liner of the adhesive sheet was peeled off, and the adhesive layer was laminated to a glass plate using a laminator as described above. The laminate was held for 20 minutes under a pressure of 0.5 MPa in an atmosphere of 50 ° C to prepare a test piece in which the glass plate / adhesive layer / glass plate were laminated in this order, and the test piece was left in an environment of 85 ° C-85% RH for 1000 hours. The test piece was cooled at 23 ° C-50% RH for 1 hour, and then the haze was measured. The haze was measured using a Turbidimeter NDH5000W manufactured by Nippon Denshoku Kogyo Co., Ltd. [Evaluation Criteria] ◎: Haze is less than 1.0. Excellent. ○: Haze is 1.0 or more and less than 2.0. Good. △: Haze is 2.0 or more and less than 3.5. Fairly good. ▲: Haze is 3.5 or more and less than 5.0. Practical use is possible. ×: Haze is 5.0 or more. Not practical.
[0104] <Resistance to moist heat whitening (PC composition)> The 38 μm release liner of the obtained adhesive sheet was peeled off, and the adhesive layer was attached to a PET film (Toyobo Co., Ltd., A-4300, thickness 100 μm), and cut to a size of 40 mm wide x 60 mm long to prepare a test adhesive sheet. Next, the other 75 μm release liner of the test adhesive sheet was peeled off, and it was attached to a 0.5 mm thick polycarbonate (PC) plate (Iupilon NF2000: Mitsubishi Gas Chemical Co., Ltd.). It was held for 20 minutes under a pressure of 0.5 MPa in an atmosphere of 50 ° C. to prepare a test piece in which the PET film / adhesive layer / PC plate were laminated in this order, and left in an environment of 85 ° C.-85% RH for 240 hours. It was cooled at 23 ° C.-50% RH for 1 hour, and then the HAZE was measured. The HAZE was measured using a Turbidimeter NDH5000W manufactured by Nippon Denshoku Kogyo Co., Ltd. [Evaluation Criteria] ◎: Haze is less than 1.5. Excellent. ○: Haze is 1.5 or more and less than 2.5. Good. △: Haze is 2.5 or more and less than 4.0. Fairly good. ▲: Haze is between 4.0 and 5.5. Practical use is possible. ×: Haze is 5.5 or more. Not practical.
[0105] <Outgassing resistance> Test pieces were prepared in the same manner as in the evaluation of heat and humidity whitening resistance (PC composition), and then left in an environment of 85°C and 85% RH for 72 hours. After leaving it in an atmosphere of 23°C and 50% RH for 1 hour, the appearance of the test pieces was visually observed. [Evaluation Criteria] ◎: No bubbles or floating. Excellent. ◯: There are very few air bubbles or lifted adhesive layers (1 to less than 5 air bubbles, and the lifted area is less than 3% of the total). Good. △: There are a few air bubbles or lifting of the adhesive layer (5 to less than 15 air bubbles, and the lifting area is 3% to less than 5% of the total). Fairly good. ▲: Air bubbles or lifted adhesive layer are found (15 to less than 30 air bubbles, and lifted area is 5 to less than 10% of the total). Practical use is possible. ×: There are many air bubbles or raised areas of the adhesive layer (30 or more air bubbles, or 10% or more of the raised area). Not suitable for practical use.
[0106] <Light resistance (peeling)> A coating liquid was prepared by mixing 100 parts of a surface protective coating agent (YL454UR, acrylic varnish, manufactured by Toyo Ink Mfg. Co., Ltd.) with 10 parts of D-172N as a curing agent, and applying the mixture to a 0.5 mm thick polycarbonate (PC) plate (Iupilon NF2000, manufactured by Mitsubishi Gas Chemical Co., Ltd.) using a bar coater. The plate was then aged at 40°C for 72 hours to prepare a PC plate having a surface protective layer. Test pieces were prepared in the same manner as in the evaluation of heat resistance (peeling), except that the PC plate having the above-mentioned surface protective layer was used instead of Iupilon NF2000, and then the test pieces were subjected to a test using a Q-Lab xenon weather resistance tester at a black panel temperature of 83°C and an illuminance of 60 W / m 2 The specimen was exposed to light for 500 hours under the above conditions. After cooling for 24 hours at 23°C and 50% RH, the degree of peeling of the specimen was visually evaluated. [Evaluation Criteria] ◎: Peeling area is less than 5% of the whole. Excellent. ○: Peeling area is 5% or more and less than 15% of the whole area. Good. △: Peeling area is 15% or more and less than 25% of the total area. Fairly good. ▲: Peeling area is between 25% and 50% of the total area. Practical use is possible. ×: Peeling area is 50% or more of the whole. Not practical.
[0107] <Light resistance (yellowing)> After preparing test pieces using the same procedure as for the evaluation of heat resistance (yellowing), they were tested using a Q-Lab xenon weathering tester at a black panel temperature of 63°C and an illuminance of 85W / m 2 The sample was exposed to light for 1000 hours under these conditions. After cooling for 1 hour at 23℃-50%RH, the b* value was measured and the difference Δb* from the b* value before the lightfastness test was calculated. The b* value was measured using a Nippon Denshoku Industries Co., Ltd. SE6000 spectrophotometer under conditions of a D65 light source and a viewing angle of 2°. [Evaluation Criteria] ◎: Δb* is less than 1.0. Excellent. ○: Δb* is 1.0 or more and less than 2.0. Good. △: Δb* is 2.0 or more and less than 3.5. Fairly good. ▲: Δb* is 3.5 or more and less than 5.0. Practical use is possible. ×: Δb* is 5.0 or more. Not practical.
[0108] <Pot life after adding hardener> The viscosity of the adhesive composition immediately after mixing with the curing agent in a 25°C atmosphere was measured using a Brookfield viscometer (rotor: 3, rotation speed: 12 rpm, measurement time: 1 minute, unit: mPa s). The adhesive composition was left in a 25°C atmosphere for 12 hours, and the viscosity was measured in the same manner as above. The rate of change in viscosity before and after leaving the adhesive composition was calculated, and the pot life was evaluated according to the following criteria. The rate of change in viscosity is expressed by Equation 1, where Va is the viscosity immediately after mixing the curing agent, and Vb is the viscosity after leaving it in an atmosphere at 25°C for 12 hours. (Formula 1) Viscosity change rate = (Vb - Va) / Va x 100 ◎: Viscosity change is less than 20% (Excellent) ○: Viscosity change is 20% or more but less than 40% (good) △: Viscosity change is 40% or more but less than 70% (fairly good). ▲: Viscosity change is 70% or more but less than 100% (practical). ×: Viscosity change of 100% or more. (Not practical)
[0109] <Adhesive sheet adhesive strength after heat aging> The obtained adhesive sheet was left in an environment of 80°C for 720 hours, and then left in an atmosphere of 23°C-50%RH for 24 hours. Thereafter, the 38μm release liner of the adhesive sheet was peeled off, and the adhesive layer was attached to a substrate PET film (Toyobo Co., Ltd., Cosmoshine A-4360, thickness 100μm), and cut into a size of 25mm wide x 100mm long to prepare a test adhesive sheet. The other 75μm release liner of this test adhesive sheet was peeled off, and the adhesive layer was attached to a glass plate in an atmosphere of 23°C-50%RH, and further pressed with a roll in accordance with JIS Z-0237. After 24 hours from pressing, the peel strength (peel angle 180°, peel speed 300mm / min; unit N / 25mm width) was measured using a tensile tester (Tensilon: Orientec Co., Ltd.). [Evaluation criteria] ◎: Peel strength is 23N / 25mm or more. Excellent. ○: Peel strength is 20N / 25mm or more and less than 23N / 25mm. Good. △: Peel strength is 16N / 25mm or more and less than 20N / 25mm. Fairly good. ▲: Peel strength is 13N / 25mm or more and less than 16N / 25mm. Practical use is possible. ×: Peel strength is less than 13N / 25mm. Not practical.
[0110] <Impact resistance test> The 38 μm release liner of the obtained adhesive sheet was peeled off, and the adhesive layer was attached to a PET film (Toyobo Co., Ltd., Cosmoshine A-4360, thickness 50 μm) as a substrate, and cut into a size of 100 mm wide x 200 mm long to prepare a test adhesive sheet. The other 75 μm release liner of this test adhesive sheet was peeled off, and the adhesive layer was attached to a 30 μm thick glass plate in an atmosphere of 23 ° C.-50% RH, and cut into a width of 70 mm x length of 150 mm using a super cutter to prepare a test laminate. 24 hours after attachment, in an atmosphere of 23 ° C. and 50% RH relative humidity, the evaluation pen was held so that the pen tip was located at a height of 10 cm from the outermost surface of the PET film of the test laminate and the pen tip was facing downward, and the evaluation pen was dropped from that position. A pen with a mass of 5.4 g and a pen tip diameter of 0.75 mm was used as the evaluation pen. After the evaluation pen was dropped, the test laminate was observed under an optical microscope (Keyence, VHK-8000) with a 20x eyepiece and evaluated according to the following criteria. ◎: No cracks on the PET film or glass plate ○: No cracks in the PET film, cracks in the glass plate ×: Cracks in the PET film and glass plate
[0111] [Table 7]
[0112] [Table 8]
[0113] As shown in Tables 7 and 8, the adhesive composition of the present invention had excellent results in terms of adhesive strength, heat resistance, moist heat whitening resistance, outgassing resistance, light resistance, pot life after mixing with a curing agent, adhesive strength of the adhesive sheet after heat aging, and impact resistance. On the other hand, the adhesive composition of the comparative example did not satisfy all of the adhesive strength, heat resistance, moist heat whitening resistance, outgassing resistance, light resistance, pot life after mixing with a curing agent, adhesive strength of the adhesive sheet after heat aging, and impact resistance. From these results, it can be said that the pressure-sensitive adhesive composition of the present invention can be suitably used for bonding optical members. [Explanation of symbols]
[0114] The symbols in Figures 1, 2 and 3 are explained below. 1 Adhesive layer 1 2 Release film 3 Film substrate (cover panel) 4. Polarizing Plate 5 Adhesive layer 2 6 Barrier Layer 7 Organic EL layer 8 Support 9 Organic EL Cell
Claims
1. A pressure-sensitive adhesive composition comprising an acrylic polymer (A) and a curing agent (B), The acrylic polymer (A) is a copolymer of a monomer mixture containing the following monomer (a1), monomer (a2), and at least one of monomer (a3-1) and monomer (a3-2): A pressure-sensitive adhesive composition comprising, based on 100 mass% of a monomer mixture, 5 to 50 mass% of monomer (a1), 30 to 80 mass% of monomer (a2), and 2 to 20 mass% of monomer (a3). (a1) (Meth)acrylic acid alkyl ester monomer having an alkyl group having 1 to 4 carbon atoms (a2) (meth)acrylic acid alkyl ester monomer having a linear alkyl group having 8 to 18 carbon atoms (a3) Monomer (a3-1) having a carboxy group and monomer (a3-2) having a hydroxy group
2. The pressure-sensitive adhesive composition according to claim 1, characterized in that the monomer mixture contains more than 7.5 mass% and not more than 16 mass% of a monomer (a3-1) having a carboxy group, based on 100 mass% of the monomer mixture.
3. 2. The pressure-sensitive adhesive composition according to claim 1, wherein the curing agent (B) comprises an epoxy-based curing agent.
4. The pressure-sensitive adhesive composition according to claim 1, further comprising a silane coupling agent (C).
5. 2. The pressure-sensitive adhesive composition according to claim 1, wherein the content of the hydroxyl group-containing monomer (a3-2) is 10 mass% or less in 100 mass% of the monomer mixture constituting the acrylic polymer.
6. 2. The pressure-sensitive adhesive composition according to claim 1, wherein the content of the nitrogen atom-containing monomer is 10 mass % or less based on 100 mass % of the monomer mixture constituting the acrylic polymer.
7. A pressure-sensitive adhesive sheet comprising a pressure-sensitive adhesive layer comprising the pressure-sensitive adhesive composition according to any one of claims 1 to 6.
8. A laminate comprising a pressure-sensitive adhesive layer made of the pressure-sensitive adhesive composition according to any one of claims 1 to 6 and a light-transmitting substrate.
9. A display comprising the laminate according to claim 8, a polarizing plate, and an optical element.
Citation Information
Patent Citations
Optical adhesive, optical film with binder and image display device
JP2007264092A
Adhesive composition and adhesive sheet
JP2017106000A
Adhesive composition
JP2020105308A
Adhesive composition and adhesive sheet
JP2022069221A
Cited By
Adhesive composition, adhesive layer, laminate, optical member, and optical device
WO2026191651A1