Manufacturing method for press-molded product
A two-stage press-forming method with adjusted holding forces addresses the challenge of suppressing wrinkles and cracks in complex press-formed products, particularly for aluminum alloys, ensuring high dimensional accuracy and stability.
Patent Information
- Application Number
- JP2023079397
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-12
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2043-05-12
AI Technical Summary
Existing methods for manufacturing press-formed products with complex shapes, such as automobile door inners, face challenges in suppressing both wrinkles and cracks, particularly with materials like high-tensile steel or aluminum plates, due to inadequate control of the holding force during the forming process.
A two-stage press-forming method using a mold with a die, holder, and pad, where the holding force is adjusted between stages to suppress wrinkles and cracks, with a higher force in the initial stage and a lower force in the final stage, to stabilize the intermediate and completed shapes.
This approach enables the production of press-formed products with high dimensional accuracy and complex shapes, effectively suppressing wrinkles and cracks, especially for materials with low formability like aluminum alloys, by optimizing the holding force throughout the forming process.
Smart Images

Figure 2024163622000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for manufacturing a press-molded product. [Background technology]
[0002] For press-formed products with complex shapes, such as side door inners or back door inners for automobiles, metal sheets such as high-tensile steel sheets or aluminum sheets are often used from the viewpoint of strength and weight. However, such metal sheets have lower formability than mild steel sheets, and wrinkles and cracks become a problem during press forming.
[0003] Patent Document 1 discloses a method for manufacturing a panel-shaped molded product, which includes a step of molding an intermediate molded product and a step of molding the intermediate molded product into a final panel-shaped molded product. This two-stage molding process is used to mold shapes that are difficult to mold, such as stepped parts. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Patent No. 6662142 Summary of the Invention [Problem to be solved by the invention]
[0005] In press molding, a molding condition that affects wrinkles and cracks is the holding force that holds the peripheral portion of the metal sheet. Such holding of the peripheral portion of the metal sheet is also called wrinkle suppression. In wrinkle suppression, a large holding force that does not cause wrinkles may cause cracks, and a small holding force that does not cause cracks may cause wrinkles. Patent Document 1 does not mention such holding force, and there is room for improvement in terms of suppressing wrinkles and cracks by adjusting the holding force.
[0006] An object of the present invention is to suppress both wrinkles and cracks in a manufacturing method for a press-molded product. [Means for solving the problem]
[0007] The present invention provides a method for manufacturing a press-molded product, which includes the steps of preparing a mold including a die, a holder, a pad, and a punch, and a sheet material which is a flat metal plate, performing wrinkle suppression by clamping the peripheral portion of the sheet material with a first holding force using the die and the holder, performing a first press molding in which the sheet material is molded into an intermediate shape by clamping it with the pad and the punch, and performing a second press molding in which the sheet material molded into the intermediate shape is molded into a finished shape as a press-molded product by clamping it with the pad, the punch, and the die, and reducing the first holding force to a second holding force which is lower than the first holding force during the molding process of the sheet material.
[0008] According to this configuration, a press-formed product having a complex shape can be manufactured with high dimensional accuracy by at least two-stage press forming including a first press forming and a second press forming, and both wrinkles and cracks can be suppressed by lowering the holding force of the blank holder during the forming process. Specifically, in the early stage of forming, wrinkles can be suppressed by performing blank holding with a relatively high first holding force, and cracks can be suppressed by performing blank holding with a relatively low second holding force in the later stage of forming.
[0009] The plate may be made of an aluminum alloy.
[0010] According to this configuration, both wrinkles and cracks can be suppressed for a material with low formability (i.e., a material that is difficult to form) such as an aluminum alloy. The aluminum alloy may be a 4000 series, 5000 series, or 6000 series.
[0011] The blank holding during the first press molding may be performed with the first holding force, and the blank holding during the second press molding may be performed with the second holding force.
[0012] According to this configuration, by maintaining a relatively high holding force (first holding force) in the first press molding in the early stage of molding when wrinkles are likely to occur, wrinkles in the intermediate shape can be suppressed and the intermediate molded product can be stably manufactured. Also, by maintaining a relatively low holding force (second holding force) in the second press molding in the later stage of molding when cracks are likely to occur, both wrinkles and cracks in the finished shape can be suppressed and the press molded product can be stably manufactured.
[0013] The intermediate shape may include at least one step shape, and the completed shape may include more steps than the intermediate shape.
[0014] According to this configuration, a press-formed product having a multi-step shape, in which problems such as wrinkles and cracks are likely to become apparent, can be produced while suppressing both wrinkles and cracks. In addition, since the step shape is formed by dividing it into the first press molding and the second press molding, the press-formed product having a multi-step shape can be produced with high dimensional accuracy. Effect of the Invention
[0015] According to the present invention, in a manufacturing method for a press-molded product, both wrinkles and cracks can be suppressed. [Brief description of the drawings]
[0016] [Figure 1] FIG. [Diagram 2] FIG. [Diagram 3] 3 is a cross-sectional view showing a first step of a method for manufacturing a press-molded product according to one embodiment. FIG. [Figure 4] FIG. 4 is a cross-sectional view showing a second step of the method for manufacturing a press-molded product according to the embodiment. [Diagram 5] FIG. 4 is a cross-sectional view showing a third step of the method for manufacturing a press-molded product according to the embodiment. [Figure 6] 13 is a graph showing changes in the holding force of the wrinkle holder. [Figure 7] FIG. 7 is an enlarged view of a portion indicated by a dashed circle VII in the press-molded product in FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0017] Hereinafter, an embodiment of the present invention will be described with reference to the accompanying drawings.
[0018] In the method for manufacturing a press-formed product according to one embodiment of the present invention, a press-formed product having a complex shape such as an inner side door or an inner back door of an automobile is manufactured. In particular, a press-formed product having high dimensional accuracy is manufactured by a two-stage press molding including a first press molding and a second press molding, while suppressing both wrinkles and cracks.
[0019] With reference to FIG. 1, a press-molded product 1 having a multi-stage shape is manufactured by the manufacturing method of the press-molded product of this embodiment. The press-molded product 1 has an upper stage 2 including a horizontal upper surface, a middle stage 3 including a horizontal surface one step lower than the upper stage 2, and a lower stage 4 including a horizontal surface one step lower than the middle stage 3. The upper stage 2 and the middle stage 3 are connected by a first vertical wall 5 extending in a substantially vertical direction, and the middle stage 3 and the lower stage 4 are connected by a second vertical wall 6 extending in a substantially vertical direction. From the lower stage 4, a third vertical wall 7 extends substantially vertically downward. From the lower end of the third vertical wall 7, a flange portion 8 extends horizontally outward. That is, the press-molded product 1 has a step shape with three steps rising from the flange portion 8.
[0020] A bead portion 9 having a convex shape is provided on the flange portion 8. The bead portion 9 is provided in an annular shape along the third vertical wall portion 7. The flange portion 8 and the bead portion 9 may be removed later if they are not required as a finished product.
[0021] The structure of the mold 100 used in this embodiment will be described with reference to FIG.
[0022] The die 100 includes a punch 110, a holder 120, a die 130, and a pad 140. A plate material 1, which is a flat metal plate, is press-molded by the die 100 to form a press-molded product 1 (see FIG. 1). Note that although the shapes before and after molding are different, the plate material 1 and the press-molded product 1 are the same member, so the same reference numerals are used for them.
[0023] In this embodiment, the plate material 1 is made of an aluminum alloy of the 6000 series. Alternatively, the plate material 1 may be made of an aluminum alloy of the 4000 series or 5000 series, or may be made of mild steel or high tensile steel, or may be made of other metals.
[0024] Punch 110 has convex portions 111-113 having three-stage convex shapes corresponding to the upper stage 2, first vertical wall portion 5, middle stage 3, second vertical wall portion 6, lower stage portion 4, and third vertical wall portion 7 of press-molded product 1 (see FIG. 1).
[0025] The holder 120 has a flat portion 121 having a flat shape corresponding to the flange portion 8 of the press-formed product 1, and a convex portion 122 having a convex shape corresponding to the bead portion 9 of the press-formed product 1 (see FIG. 1).
[0026] The die 130 has a flat portion 131 having a flat shape corresponding to the flange portion 8 of the press-molded product 1, and a concave portion 132 having a shape complementary to the convex portion 122 of the holder 120. The die 130 also has a stair portion 133 having a stair shape complementary to the convex portions 112, 113 of the punch 110.
[0027] The pad 140 has a stepped portion 141 having a stepped shape complementary to the protrusions 111 and 112 of the punch 110 .
[0028] Each step of the method for producing a press-molded product according to this embodiment will be described with reference to Figures 3 to 5. Note that Figures 3 to 5 are schematic diagrams, and there may be slight inconsistencies in shape between these diagrams and other diagrams.
[0029] 3, in a first step of the manufacturing method for a press-molded product of this embodiment, wrinkle suppression is performed by clamping the peripheral portion 10 of the sheet material 1 between a holder 120 and a die 130. In the wrinkle suppression, a holding force (first holding force) is applied to the sheet material 1, and a flange portion 8 (see FIG. 1) and a bead portion 9 (see FIG. 1) are formed in the sheet material 1. By adjusting the holding force, the amount of material flowing inward into the bead portion 9 can be adjusted. The amount of material flowing in is a factor that greatly affects wrinkles and cracks.
[0030] 4, in a second step of the manufacturing method for a press-molded product of the present embodiment, as a first press molding, the plate material 1 is sandwiched between a punch 110 and a pad 140 to form an upper stage 2, a first vertical wall 5, and a middle stage 3. That is, the plate material 1 is molded into an intermediate shape including at least one stepped shape.
[0031] 5, in a third step of the manufacturing method for a press-molded product of the present embodiment, the sheet material 1 is sandwiched between a punch 110 and a die 130 as a second press molding to form a second vertical wall portion 6, a lower step portion 4, and a third vertical wall portion 7. That is, the sheet material 1 is molded into a finished shape including a step shape with more steps than the intermediate shape.
[0032] The change in the holding force will be described with reference to FIG.
[0033] 6, the horizontal axis represents the amount of movement (stroke) D [mm] of the die 100, and the vertical axis represents the holding force F [kN]. When the stroke is equal to or shorter than D1 [mm], the first press molding is performed, and when the stroke is equal to or longer than D2 [mm], the second press molding is performed.
[0034] Referring to the graph, in the first press molding where the stroke is before D1 [mm], the holding force (first holding force) is maintained at F1 [kN]. In the process of transition of the stroke from D1 [mm] to D2 [mm], the holding force gradually decreases from F1 [kN] to F2 [kN]. Then, in the second press molding where the stroke is after D2 [mm], the holding force (second holding force) is maintained at F2 [kN].
[0035] In this embodiment, as described above, the holding force of the wrinkle suppressor is reduced during the forming process of the plate material 1. More specifically, the wrinkle suppression during the first press forming is performed with a first holding force F1, and the wrinkle suppression during the second press forming is performed with a second holding force F2. For example, when manufacturing a press-formed product 1 having a height of about several tens of millimeters, a holding force of about several hundred kilonewtons may be applied, and the second holding force F2 may be 60% or less of the first holding force F1.
[0036] The effectiveness of the manufacturing method of the press-formed product of this embodiment will be described from the viewpoint of the sheet thickness reduction rate with reference to Fig. 7 and the following Table 1. Also, the effectiveness of the manufacturing method of the press-formed product of this embodiment will be described from the viewpoint of the minimum principal stress with reference to Fig. 7 and the following Table 2.
[0037] In the analysis, the material of the plate material 1 was set to 6000 series aluminum alloy. The dimensions of the plate material 1 were set to a rectangle of 600 [mm] × 500 [mm] and a thickness of 1.0 [mm], and the pad load was set to 103.7 [kN], and a forming simulation was performed using the finite element method.
[0038] Table 1 below shows the pass / fail results of the sheet thickness reduction rate and crack evaluation in the regions R1, R2, and R3 shown in FIG. 7. The sheet thickness reduction rate is an evaluation index in which the risk of cracking increases as the sheet thickness reduction rate increases. Here, a large sheet thickness reduction rate is judged to be a high risk of cracking, and the pass / fail evaluation is set to "x", whereas a small sheet thickness reduction rate is judged to be a low risk of cracking, and the pass / fail evaluation is set to "o". Note that the judgment threshold value of the sheet thickness reduction rate for pass / fail evaluation is omitted here in detail, but may be set based on sensory evaluation or may be appropriately set according to the simulation conditions, etc. Table 1 shows the manufacturing method of the press-formed product of this embodiment (when the holding force is reduced during the forming process of the sheet material 1 as shown in FIG. 6), a first comparative example different from this embodiment in which the holding force is constant at 240 [kN], and a second comparative example different from this embodiment in which the holding force is constant at 140 [kN]. The first and second comparative examples are substantially the same as this embodiment except for the holding force.
[0039] [Table 1]
[0040] In the first comparative example, the thickness reduction rate is large in the regions R1, R2, and R3, and there is a high risk of cracks occurring (pass / fail evaluation: fail "x"). In the second comparative example, the thickness reduction rate is small in the regions R1, R2, and R3, and there are no other parts with a large thickness reduction rate, and there is a low risk of cracks occurring (pass / fail evaluation: pass "o"). In this embodiment, as in the second comparative example, the thickness reduction rate is small in the regions R1, R2, and R3, and there are no other parts with a large thickness reduction rate, and there is a low risk of cracks occurring (pass / fail evaluation: pass "o"). Therefore, it was confirmed that the manufacturing method of the press-molded product of this embodiment is effective in terms of suppressing cracks.
[0041] Table 2 below shows the minimum principal stress [GPa] in the region R4 shown in FIG. 7 and the pass / fail evaluation for wrinkles caused by the minimum principal stress. The minimum principal stress is an evaluation index that expresses compression as a negative number, and the risk of wrinkles increases as the value is small (large as an absolute value). Here, when the minimum principal stress is small, the risk of wrinkles is judged to be high, and the pass / fail evaluation is set to "x", and when the minimum principal stress is large, the risk of wrinkles is judged to be low, and the pass / fail evaluation is set to "o". Note that the judgment threshold value of the minimum principal stress for pass / fail evaluation is omitted here in detail, but may be set based on a sensory evaluation or may be appropriately set according to the simulation conditions, etc. Table 2 shows the manufacturing method of the press-formed product of this embodiment (when the holding force is reduced during the forming process of the plate material 1 as shown in FIG. 6), a first comparative example different from this embodiment in which the holding force is constant at 240 [kN], and a second comparative example different from this embodiment in which the holding force is constant at 140 [kN]. The first and second comparative examples are substantially the same as this embodiment except for the holding force.
[0042] [Table 2]
[0043] In the second comparative example, the minimum principal stress is small in region R4, and there is a high risk of wrinkles occurring (pass / fail evaluation: fail "x"). In the first comparative example, the minimum principal stress is large in region R4, and there are no other parts with small minimum principal stresses, and there is a low risk of wrinkles occurring (pass / fail evaluation: pass "o"). In this embodiment, as in the first comparative example, the minimum principal stress is large in region R4, and there are no other parts with small minimum principal stresses, and there is a low risk of wrinkles occurring (pass / fail evaluation: pass "o"). Therefore, it was confirmed that the manufacturing method of the press-molded product of this embodiment is effective in terms of suppressing wrinkles.
[0044] According to the manufacturing method of the press-molded product of this embodiment, the following advantageous effects are obtained.
[0045] By performing at least two press molding steps including the first press molding and the second press molding, a press-molded product 1 having a complex shape can be manufactured with high dimensional accuracy, and both wrinkles and cracks can be suppressed by lowering the holding force of the blank holder during the molding process. Specifically, in the early stage of molding, wrinkles can be suppressed by performing blank holder with a relatively high first holding force, and in the later stage of molding, cracks can be suppressed by performing blank holder with a relatively low second holding force.
[0046] In addition, both wrinkles and cracks can be suppressed for materials with low formability (i.e., materials that are difficult to form) such as aluminum alloys.
[0047] Moreover, wrinkle suppression during the first press molding is performed with the first holding force, and wrinkle suppression during the second press molding is performed with the second holding force. Therefore, by maintaining a relatively high holding force (first holding force) in the first press molding in the early stages of molding when wrinkles are likely to occur, wrinkles in the intermediate shape can be suppressed and the intermediate molded product can be stably manufactured. Furthermore, by maintaining a relatively low holding force (second holding force) in the second press molding in the later stages of molding when cracks are likely to occur, both wrinkles and cracks in the finished shape can be suppressed and the press molded product can be stably manufactured.
[0048] In addition, the press-formed product 1 having a multi-step shape, in which problems such as wrinkles and cracks are likely to become apparent, can be realized while suppressing both wrinkles and cracks. In addition, since the step shape is formed by separately performing the first press molding and the second press molding, the press-formed product 1 having a multi-step shape can be manufactured with high dimensional accuracy.
[0049] The present invention includes the following aspects. (Aspect 1) A die including a die, a holder, a pad, and a punch, and a plate material that is a flat metal plate are prepared; performing a blank suppression by clamping a peripheral portion of the plate material with a first holding force between the die and the holder; A first press molding is performed in which the plate material is sandwiched between the pad and the punch to form an intermediate shape; A second press molding is performed in which the plate material formed into an intermediate shape is sandwiched between the pad, the punch, and the die to form the plate material into a finished shape as a press-formed product. Including, The method for manufacturing a press-molded product further comprises reducing the first holding force to a second holding force lower than the first holding force during a forming process of the plate material. (Aspect 2) 2. The method for producing a press-molded product according to claim 1, wherein the plate material is made of an aluminum alloy. (Aspect 3) 3. The method for manufacturing a press-molded product according to claim 1, wherein the blank holding during the first press molding is performed with the first holding force, and the blank holding during the second press molding is performed with the second holding force. (Aspect 4) The intermediate shape includes at least one step shape, Aspects 4. The method for producing a press-molded product according to any one of aspects 1 to 3, wherein the finished shape includes a step shape having more steps than the intermediate shape.
[0050] Although the specific embodiment of the present invention has been described above, the present invention is not limited to the above embodiment, and various modifications can be made within the scope of the present invention. For example, the shape of the press-molded product 1 is not particularly limited and can be any shape. [Explanation of symbols]
[0051] 1. Press-molded products (sheet materials) 2 Upper section 3 Middle section 4 Lower section 5 First vertical wall section 6 Second vertical wall section 7 Third vertical wall section 8 Flange 9 Bead section 10 Periphery 11,12 Press-molded products 100 Molds 110 Punch 111~113 Convex 120 Holder 121 Flat area 122 Convex stripe 130 Dice 131 Flat area 132 Concave section 133 Stairs 134 Bottom surface 140 Pad 141 Stairs 142 Bottom surface
Claims
1. A die including a die, a holder, a pad, and a punch, and a plate material that is a flat metal plate are prepared; performing a blank suppression by clamping a peripheral portion of the plate material with a first holding force between the die and the holder; A first press molding is performed in which the plate material is sandwiched between the pad and the punch to form the plate material into an intermediate shape; A second press molding is performed in which the plate material formed into an intermediate shape is sandwiched between the pad, the punch, and the die to form the plate material into a finished shape as a press-formed product. Including, A method for manufacturing a press-molded product, comprising: reducing the first holding force to a second holding force lower than the first holding force during a molding process of the plate material.
2. The method for manufacturing a press-formed product according to claim 1 , wherein the plate material is made of an aluminum alloy.
3. The method for manufacturing a press-formed product according to claim 1 or 2, wherein the blank holding during the first press molding is performed with the first holding force, and the blank holding during the second press molding is performed with the second holding force.
4. The intermediate shape includes at least one step shape, The method for manufacturing a press-formed product according to claim 1 or 2, wherein the finished shape includes a step shape having more steps than the intermediate shape.
Citation Information
Patent Citations
Drawing die
JP1993023751A
Apparatus and method for press work
JP2008100239A
Press molding apparatus
JP2012218061A
Manufacturing method of panel-like formed product
JP2017170506A
Press molding method and press molding device for automobile outer plate panel
JP2022069887A