Rubber product and method for producing the same

By incorporating a filler that absorbs and localizes ionic liquid within a crosslinked rubber composition, the issue of crosslinking inhibition in fluororubber is addressed, ensuring stable antistatic performance and preventing ionic liquid bleed-out.

JP2024163659AActive Publication Date: 2024-11-22MITSUBISHI CABLE INDUSTRIES LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2023079467
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-12
Publication Date
2024-11-22
Estimated Expiration
2043-05-12

AI Technical Summary

Technical Problem

The blending of ionic liquids with fluororubber inhibits crosslinking in the crosslinked rubber composition, leading to ineffective crosslinking inhibition.

Method used

A rubber product is formed from a crosslinked rubber composition containing fluororubber, an ionic liquid, and a filler that absorbs the ionic liquid, with a higher concentration of the ionic liquid in the filler compared to the fluororubber, allowing the ionic liquid to be localized and reducing its inhibitory effect on crosslinking.

Benefits of technology

Crosslinking inhibition by the ionic liquid is suppressed, enabling stable antistatic performance and preventing bleed-out of the ionic liquid, while maintaining effective crosslinking.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024163659000001
    Figure 2024163659000001
  • Figure 2024163659000002
    Figure 2024163659000002
Patent Text Reader

Abstract

To provide a rubber product that reduces the crosslinking inhibition caused by an ionic liquid in a crosslinked rubber composition, which contains a fluororubber and the ionic liquid.SOLUTION: This rubber product is formed of a crosslinked rubber composition containing a fluororubber, an ionic liquid, and a filler dispersed in the fluororubber and capable of absorbing the ionic liquid. The concentration of the ionic liquid in the filler is higher than the concentration of the ionic liquid in the fluororubber.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a rubber product and a method for producing the same. [Background technology]

[0002] There is a known technique for controlling electrical properties by incorporating an ionic liquid into a cross-linked rubber composition that forms a rubber product. For example, Patent Document 1 discloses a sealing material formed from a cross-linked rubber composition in which an ionic liquid is blended with a fluororubber. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] Patent Publication No. 2022-1642 Summary of the Invention [Problem to be solved by the invention]

[0004] However, when an ionic liquid is blended with a fluororubber, there is a problem in that crosslinking is inhibited by the ionic liquid when an uncrosslinked rubber composition is crosslinked to obtain a crosslinked rubber composition.

[0005] An object of the present invention is to provide a rubber product in which inhibition of crosslinking caused by an ionic liquid in a crosslinked rubber composition comprising a fluororubber and an ionic liquid is suppressed. [Means for solving the problem]

[0006] The present invention relates to a rubber product formed from a crosslinked rubber composition containing a fluororubber, an ionic liquid, and a filler that is dispersed in the fluororubber and can absorb the ionic liquid, wherein the concentration of the ionic liquid in the filler is higher than the concentration of the ionic liquid in the fluororubber.

[0007] The present invention is a method for producing a rubber product, which comprises allowing a filler to absorb an ionic liquid, kneading the filler having absorbed the ionic liquid with a fluororubber to prepare an uncrosslinked rubber composition, and crosslinking the uncrosslinked rubber composition. Effect of the Invention

[0008] According to the present invention, the concentration of the ionic liquid in the filler dispersed in the fluororubber is higher than the concentration of the ionic liquid in the fluororubber, so that inhibition of crosslinking by the ionic liquid can be suppressed. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] The embodiments will be described in detail below.

[0010] The rubber product according to the embodiment is formed of a crosslinked rubber composition X containing a fluororubber, an ionic liquid, and a filler. The fluororubber is a main component of the base rubber. The filler is dispersed in the fluororubber. The filler is capable of absorbing the ionic liquid. The concentration of the ionic liquid in the filler is higher than the concentration of the ionic liquid in the fluororubber.

[0011] According to the rubber product of the embodiment, first, by containing an ionic liquid, a stable antistatic performance can be obtained. In addition, the concentration of the ionic liquid in the filler dispersed in the fluororubber is higher than the concentration of the ionic liquid in the fluororubber, so that the inhibition of crosslinking by the ionic liquid can be suppressed. This is considered to be because the ionic liquid is localized around the filler, so that the effect of the ionic liquid on the fluororubber, which is the main subject of direct crosslinking, is reduced. The distribution state of the ionic liquid in the crosslinked rubber composition X can be analyzed by energy dispersive X-ray spectroscopy (EDS).

[0012] According to the rubber product of the embodiment, the filler absorbs the ionic liquid, thereby suppressing the bleeding out of the ionic liquid. However, in the surface layer of the crosslinked rubber composition X forming the rubber product, the concentration of the ionic liquid is preferably higher from the inside to the surface in order to obtain stable antistatic performance. The distribution state of the ionic liquid in the depth direction of the surface layer of the crosslinked rubber composition X can be analyzed by time-of-flight secondary ion mass spectrometry (TOF-SIMS).

[0013] Examples of fluororubber include tetrafluoroethylene (TFE) polymer (PTFE), vinylidene fluoride (VDF) polymer (PVDF), copolymer of vinylidene fluoride (VDF) and hexafluoropropylene (HFP) (binary FKM), copolymer of vinylidene fluoride (VDF), hexafluoropropylene (HFP) and tetrafluoroethylene (TFE) (ternary FKM), copolymer of tetrafluoroethylene (TFE) and propylene (Pr) (FEP), copolymer of vinylidene fluoride (VDF), propylene (Pr) and tetrafluoroethylene (TFE), and copolymer of vinylidene fluoride (VDF), propylene (Pr) and tetrafluoroethylene (TFE). ), copolymer of ethylene (E) and tetrafluoroethylene (TFE) (ETFE), copolymer of ethylene (E), tetrafluoroethylene (TFE) and perfluoromethylvinylether (PMVE), copolymer of vinylidene fluoride (VDF), tetrafluoroethylene (TFE) and perfluoromethylvinylether (PMVE), copolymer of tetrafluoroethylene (TFE) and perfluoromethylvinylether (PMVE) (FFKM), copolymer of vinylidene fluoride (VDF) and perfluoromethylvinylether (PMVE), etc. The fluororubber preferably contains one or more of these, and more preferably contains a ternary FKM from the viewpoint of obtaining a high suppression effect against crosslinking inhibition by the ionic liquid.

[0014] In the present application, the term "ionic liquid" refers to a salt composed of a cationic component and an anionic component, and has a melting point of 100°C or lower.

[0015] Examples of the cationic components of the ionic liquid include imidazolium-based cations, pyridinium-based cations, aliphatic amine-based cations, pyrazolium-based cations, etc. Examples of the imidazolium-based cations include 1-ethyl-3-methylimidazolium, 1-methyl-3-methylimidazolium, 1-butyl-3-methylimidazolium, 1-hexyl-3-methylimidazolium, 1-octyl-3-methylimidazolium, 1-methyl-2,3-dimethylimidazolium, 1-butyl-2,3-dimethylimidazolium, 1-hexyl-2,3-dimethylimidazolium, 1-octyl-2,3-dimethylimidazolium, etc. Examples of the pyridinium-based cations include 1-octyl-4-methyl-pyridinium, 1-methyl-pyridinium, 1-butyl-pyridinium, 1-hexyl-pyridinium, etc. An example of the aliphatic amine cation is tributylmethylammonium.

[0016] Examples of the anion component include bisfluorosulfonylimide anions, fluorinated sulfonic acid anions, fluorinated carboxylic acid anions, thiocyanate anions, dicyanamide anions, and tetracyanoborate anions. Examples of the bisfluorosulfonylimide anions include bisfluorosulfonylimide, bistrifluoromethanesulfonylimide, and bistrifluorobutanesulfonylimide. Examples of the fluorinated sulfonic acid anions include tetrafluoroborate, hexafluoroborate, and trifluoromethanesulfonate. Examples of the fluorinated carboxylic acid anions include trifluoroacetic acid.

[0017] The ionic liquid preferably contains one or more of these cationic components and one or more of anionic components. The cationic component of the ionic liquid preferably contains an imidazolium-based cation or an aliphatic amine-based cation from the viewpoint of obtaining a high suppression effect against the inhibition of crosslinking by the ionic liquid. From the same viewpoint, the cationic component of the ionic liquid preferably contains 1-butyl-3-methylimidazolium as an imidazolium-based cation, and preferably contains tributylmethylammonium as an aliphatic amine-based cation. From the same viewpoint, the anionic component of the ionic liquid preferably contains a bisfluorosulfonylimide-based anion, and more preferably contains bistrifluoromethanesulfonylimide.

[0018] The content of the ionic liquid in the crosslinked rubber composition X is preferably 0.01 parts by mass or more and 5 parts by mass or less, more preferably 0.1 parts by mass or more and 1 part by mass or less, per 100 parts by mass of the fluororubber, from the viewpoint of obtaining a high suppression effect against the inhibition of crosslinking by the ionic liquid.

[0019] Examples of the filler include resin powders and porous powders that can absorb ionic liquids. Examples of the resin powders that can absorb ionic liquids include fluororesin powders, phenolic resin powders, polyether ether ketone resin (PEEK) powders, and polyimide resin (PI) powders. Examples of the fluororesin powders include polyvinylidene fluoride resin (PVDF) powders. Examples of the porous powders include carbon black, silica, and zeolite. The filler preferably contains one or more of these, and from the viewpoint of obtaining a high suppression effect against crosslinking inhibition by ionic liquids, it is more preferable to contain a resin powder, even more preferable to contain a fluororesin powder, and even more preferable to contain a PVDF powder. Examples of commercially available PVDF powders include the Kynar series manufactured by Arkema.

[0020] The density of the filler is preferably 1 g / cm from the viewpoint of obtaining a high suppression effect against the inhibition of crosslinking by the ionic liquid. 3More than 3g / cm 3 Less than or equal to 1.5 g / cm 3 More than 2g / cm 3 The density of this filler is measured according to ISO1183.

[0021] From the viewpoint of obtaining a high suppression effect against the inhibition of crosslinking by the ionic liquid, the content of the filler in the crosslinked rubber composition X is preferably 1 part by mass or more and 15 parts by mass or less, more preferably 3 parts by mass or more and 10 parts by mass or less, relative to 100 parts by mass of the fluororubber. From the same viewpoint, the ratio of the content of the filler to the content of the ionic liquid in the crosslinked rubber composition X (content of the filler / content of the ionic liquid) is preferably 3 or more and 20 or less, more preferably 5 or more and 15 or less.

[0022] Examples of the crosslinking system of the crosslinked rubber composition X include a peroxide crosslinking system, a polyol crosslinking system, and an amine crosslinking system. Of these, the peroxide crosslinking system is preferred as the crosslinking system of the crosslinked rubber composition X from the viewpoint of obtaining a high suppression effect against the crosslinking inhibition by the ionic liquid. In the case of the peroxide crosslinking system, peroxide as a crosslinking agent is blended into the uncrosslinked rubber composition X' before the crosslinking of the crosslinked rubber composition X.

[0023] Examples of the peroxide crosslinking agent include 1,1-bis(t-butylperoxy)-3,5,5-trimethylcyclohexane, 2,5-dimethylhexane-2,5-dihydroperoxide, di-t-butyl peroxide, t-butylcumyl peroxide, dicumyl peroxide, α,α-bis(t-butylperoxy)-p-diisopropylbenzene, 2,5-dimethyl-2,5-di(t-butylperoxy)hexane, 2,5-dimethyl-2,5-di(t-butylperoxy)-hexyne-3, benzoyl peroxide, t-butylperoxybenzene, t-butylperoxymaleic acid, t-butylperoxyisopropyl carbonate, t-butylperoxybenzoate, etc. The peroxide crosslinking agent preferably contains one or more of these, and more preferably contains 2,5-dimethyl-2,5-di(t-butylperoxy)hexane from the viewpoint of obtaining a high suppression effect against crosslinking inhibition by ionic liquid.

[0024] The amount of peroxide crosslinking agent blended into the uncrosslinked rubber composition X' is preferably 0.5 parts by mass or more and 5 parts by mass or less, more preferably 1 part by mass or more and 3 parts by mass or less, per 100 parts by mass of the fluororubber, from the viewpoint of obtaining a high inhibitory effect against the inhibition of crosslinking by the ionic liquid.

[0025] The crosslinking degree of the crosslinked rubber composition X may be further increased by a crosslinking aid. Examples of the crosslinking aid include triallyl cyanurate, trimethallyl isocyanurate, triallyl isocyanurate, triacrylformal, triallyl trimellitate, N,N'-m-phenylene bismaleimide, dipropargyl terephthalate, diallyl phthalate, tetraallyl terephthalate amide, triallyl phosphate, bismaleimide, fluorinated triallyl isocyanurate (1,3,5-tris(2,3,3-trifluoro-2-propenyl)-1,3,5-triazine, etc.). -2,4,6-trione), tris(diallylamine)-S-triazine, triallyl phosphite, N,N-diallylacrylamide, 1,6-divinyldodecafluorohexane, hexaallyl phosphoramide, N,N,N',N'-tetraallylphthalamide, N,N,N',N'-tetraallylmalonamide, trivinyl isocyanurate, 2,4,6-trivinylmethyltrisiloxane, tri(5-norbornene-2-methylene) cyanurate, triallyl phosphite, etc. are mentioned. The crosslinking aid preferably contains one or more of these, and more preferably contains triallyl isocyanurate from the viewpoint of obtaining a high suppression effect against crosslinking inhibition by ionic liquid. From the same viewpoint, the amount of the crosslinking aid to be blended in the uncrosslinked rubber composition X' is preferably 0.5 parts by mass or more and 10 parts by mass or less, more preferably 3 parts by mass or more and 7 parts by mass or less, based on 100 parts by mass of the fluororubber.

[0026] The crosslinked rubber composition X may contain silicone rubber or the like as a component of the base rubber other than the fluororubber. The crosslinked rubber composition X may also contain rubber compounding agents such as processing aids, plasticizers, processing aids, vulcanization accelerators, and antioxidants.

[0027] The volume resistivity of the crosslinked rubber composition X is preferably 1.0×10 12 Ω cm or less, preferably 1.0×10 11 The volume resistivity is Ω·cm or less. This volume resistivity is measured based on JIS K6271-1:2015.

[0028] Specific examples of the rubber products according to the embodiment include sealing materials such as O-rings.

[0029] Next, a method for producing a rubber product according to the embodiment will be described.

[0030] In the method for producing a rubber product according to the embodiment, first, a filler and an ionic liquid are mixed together to allow the filler to absorb the ionic liquid.

[0031] Next, the fluororubber is masticated using a rubber kneader, and the rubber compounding ingredients containing the filler that has absorbed the ionic liquid and the crosslinking agent are added thereto. In this way, the filler that has absorbed the ionic liquid is kneaded with the fluororubber to prepare an uncrosslinked rubber composition X'. At this time, in the obtained uncrosslinked rubber composition X', a part of the ionic liquid absorbed in the filler flows out and diffuses into the fluororubber.

[0032] The maximum torque value of the uncrosslinked rubber composition X' is preferably 0.5 N·m or more, more preferably 1 N·m or more, which is determined in accordance with JIS K6300-2:2001 based on a vulcanization curve obtained from a Curastometer (registered trademark).

[0033] The uncrosslinked rubber composition X' is then molded into a predetermined shape and crosslinked by holding it at a predetermined temperature and pressure for a predetermined time, thereby obtaining a rubber product according to the embodiment formed from the crosslinked rubber composition X. The obtained rubber product may be subjected to a secondary crosslinking treatment in which it is held in an atmosphere at a predetermined temperature for a predetermined time and / or a radiation crosslinking treatment in which it is irradiated with radiation. EXAMPLES

[0034] (O-ring) The O-rings of the following Examples 1 and 2 and Comparative Example were produced. The constitution of the crosslinked rubber composition forming each is shown in Table 1.

[0035] <Example 1> A fluorine-containing ternary FKM (Technoflon P459, manufactured by SOLVAY) was used as the base rubber. First, 100 parts by mass of this ternary FKM was mixed with 5 parts by mass of a filler PVDF powder (Kynar MG15, manufactured by Arkema, density: 1.78 g / cm3). 3 ) and 0.5 parts by mass of ionic liquid A, 1-butyl-3-methylimidazolium bistrifluoromethanesulfonylimide (BMI-N111, manufactured by Mitsubishi Materials Corporation) were mixed to allow the ionic liquid A to be absorbed into the PVDF powder. Next, 1.5 parts by mass of the crosslinking agent, 2,5-dimethyl-2,5-di(t-butylperoxy)hexane (Perhexa 25B, manufactured by NOF Corp.), and 3 parts by mass of the crosslinking aid, triallyl isocyanurate (TAIC, manufactured by Nippon Kasei Kasei Co., Ltd.), were mixed with 100 parts by mass of the ternary FKM together with the PVDF powder having absorbed the ionic liquid A, and an uncrosslinked rubber composition was prepared by kneading. Then, the uncrosslinked rubber composition was crosslinked by press molding to produce an O-ring formed from the crosslinked rubber composition. This O-ring was designated as Example 1.

[0036] <Example 2> An O-ring having the same configuration as in Example 1 was prepared, except that ionic liquid B, tributylmethylammonium bistrifluoromethanesulfonylimide (FC-4400, manufactured by 3M Japan), was used instead of ionic liquid A, and this was designated as Example 2.

[0037] <Comparative Example> An O-ring having the same configuration as in Example 2, except that ionic liquid B was directly added to the ternary FKM without adding PVDF powder, was produced as a comparative example.

[0038] [Table 1]

[0039] (Test Method and Results) <Maximum torque value> For the unvulcanized rubber compositions used to produce the O-rings of Example 1, Example 2, and the Comparative Example, vulcanization curves were obtained using a curemeter. Then, based on the vulcanization curves, the maximum torque value was determined in accordance with JIS K6300-2:2001. The results are shown in Table 2.

[0040]

Table 2

[0041] According to Table 2, in Example 1 where the PVDF powder absorbed ionic liquid A and Example 2 where the PVDF powder absorbed ionic liquid B, the maximum torque value was high, while in the Comparative Example where no PVDF powder was used, the maximum torque value was very low. This is presumably because in the Comparative Example, crosslinking inhibition by the ionic liquid occurred, while in Examples 1 and 2, crosslinking inhibition by the ionic liquid was suppressed by absorbing the ionic liquid into the PVDF powder.

[0042] <SEM Observation·EDS Analysis> For the O-rings of Example 1, Example 2, and the Comparative Example, circular samples of the crosslinked rubber composition in the form of a thin film with a thickness of about 1 μm were cut out, and the central part, surface layer part, and the intermediate part between them were observed by SEM and analyzed by EDS.

[0043] According to the results of observation and analysis, in Examples 1 and 2, a sea-island structure in which islands of PVDF powder were dispersed in a sea of ternary FKM was observed. Also, it was analyzed that the O concentration and S concentration were higher in the islands of PVDF powder than in the sea of ternary FKM. This is due to bistrifluoromethanesulfonylimide which is the anion component of the ionic liquid, meaning that the ionic liquid is localized and the concentration of the ionic liquid in the PVDF powder is higher than the concentration of the ionic liquid in the ternary FKM. Furthermore, it was analyzed that the F concentration was lower in the islands of PVDF powder than in the sea of ternary FKM. This is consistent with the fact that the F content of the ternary FKM is 68% by mass while the F content of PVDF is 59.4% by mass. On the other hand, in the comparative example, a sea-island structure as in Examples 1 and 2 was not observed, and localization of the O concentration and S concentration was not analyzed either.

[0044] <TOF-SIMS analysis> Regarding the O-ring of Example 1, depth direction analysis of the surface layer of the crosslinked rubber composition was performed by TOF-SIMS.

[0045] According to the depth profile of the analysis results, in the surface layer from the surface of the crosslinked rubber composition to a depth of 18 nm, it was analyzed that the concentration of the ionic liquid increased from the inside to the surface, and the maximum concentration difference was about 10 times.

Industrial Applicability

[0046] The present invention is useful in the technical field of rubber products and their manufacturing methods.

Claims

1. A rubber product formed of a crosslinked rubber composition containing a fluororubber, an ionic liquid, and a filler that is dispersed in the fluororubber and can absorb the ionic liquid, A rubber product, wherein the concentration of the ionic liquid in the filler is higher than the concentration of the ionic liquid in the fluororubber.

2. The rubber product according to claim 1, A rubber product in which the concentration of the ionic liquid increases from the inside to the surface in the surface layer of the crosslinked rubber composition.

3. The rubber product according to claim 1, The rubber product, wherein the fluororubber contains a copolymer of vinylidene fluoride, hexafluoropropylene and tetrafluoroethylene.

4. The rubber product according to claim 1, A rubber product, wherein the cationic component of the ionic liquid contains an imidazolium-based cation or an aliphatic amine-based cation.

5. The rubber product according to claim 1, A rubber product, wherein the anion component of the ionic liquid contains a bisfluorosulfonylimide anion.

6. The rubber product according to claim 1, The rubber product, wherein the filler comprises powder of a vinylidene fluoride polymer.

7. The rubber product according to claim 1, The rubber product is a sealing material.

8. A method for producing a rubber product comprising the steps of: causing a filler to absorb an ionic liquid; kneading the filler having absorbed the ionic liquid with a fluororubber to prepare an uncrosslinked rubber composition; and crosslinking the uncrosslinked rubber composition.

Citation Information

Patent Citations

  • Semiconductive member for image formation, image forming apparatus and method, and process cartridge

    JP2008129481A

  • Partially fluorinated elastomers, a method for producing the same, and a method for using the same

    JP2016516880A

  • Resin particle, composition containing resin particle, panel containing the composition, and electrophoresis display device containing the panel

    JP2018072614A

  • Sealant rubber material and sealant including the same

    JP2019085475A

  • Novel ionic liquids, functionalized particulates, and fluoropolymer composites

    US20110033647A1