Processing method of refractory brick

The method of freezing and thawing refractory bricks with adhering slag effectively separates deposits while preserving brick integrity, enhancing recycling efficiency and yield.

JP2024163760AActive Publication Date: 2024-11-22JFE STEEL CORP
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2023079631
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-12
Publication Date
2024-11-22
Estimated Expiration
2043-05-12

AI Technical Summary

Technical Problem

Existing methods for recycling refractory bricks are inefficient and reduce the yield due to manual hammering and water-jet cleaning devices that scrape both deposits and the base material, leading to reduced durability and high costs.

Method used

A method involving soaking refractory bricks with water and repeatedly freezing and thawing to create gaps between the bricks and adhering slag, allowing easy peeling without damaging the bricks.

Benefits of technology

Effectively separates slag from refractory bricks while maintaining high yield, achieving a slag content of 2.7% or less and a refractory brick yield of 90% or more.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024163760000001_ABST
    Figure 2024163760000001_ABST
Patent Text Reader

Abstract

To provide a processing method of a refractory brick capable of effectively separating a slag deposited on a surface of a refractory brick while maintaining yield of the refractory brick.SOLUTION: In a processing method of a refractory brick with its surface deposited with a slag, a slag is separated from the refractory brick after allowing the refractory brick to take in water, followed by repeating freeze and thaw multiple times.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for treating refractory bricks. [Background technology]

[0002] In recent years, as part of efforts to improve recycling efficiency in steelmaking, it has been proposed to reuse refractory bricks used in the ironmaking process. Refractory bricks include torpedo bricks and converter bricks.

[0003] Generally, iron and slag adhere to the working surface of a refractory brick (the surface that comes into contact with molten steel and slag) through the pores in the refractory, and mortar may adhere to some other surfaces. When recycling such refractory bricks, if the above-mentioned adhesions are mixed in, the durability of the recycled product as a refractory material is significantly reduced and it becomes unusable. Therefore, when recycling refractory bricks, it is necessary to remove the above-mentioned adhesions such as slag.

[0004] The current method of recycling refractory bricks involves manually striking each refractory brick to separate the slag adhering to the surface, and then crushing the bricks. This method allows only a portion of the refractory bricks to be reused, and is not fully satisfactory in terms of work efficiency and running costs. Therefore, in order to efficiently recycle refractory bricks, it is desirable to automate the separation of slag and other adhering matter from the surface of refractory bricks in large quantities.

[0005] In response to this, for example, Patent Document 1 proposes a water jet type scraping device that performs scraping (processing to remove material adhering to the surface) by spraying water from a jet nozzle onto a workpiece being transported. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2001-009390 A Summary of the Invention [Problem to be solved by the invention]

[0007] However, in the device described in the above-mentioned Patent Document 1, the high-speed water spray not only scrapes the surface but also scrapes the base material itself. In other words, the above-mentioned device has a problem of reducing the yield.

[0008] The present invention has been made in consideration of the above circumstances, and an object of the present invention is to provide a method for treating refractory bricks, which is capable of effectively separating slag adhering to the surfaces of the refractory bricks while ensuring the yield of the refractory bricks. [Means for solving the problem]

[0009] As a result of intensive research by the inventors to solve the above-mentioned problems, they discovered that by soaking refractory bricks in water and repeatedly freezing and thawing them multiple times, gaps are formed between the refractory bricks and the slag, making the slag easier to peel off, which led to the present invention.

[0010] The gist and configuration of the present invention are as follows.

[0011] [1] A method for treating refractory bricks having slag attached to their surfaces, comprising the steps of: A method for treating a refractory brick, comprising the steps of: introducing water into the refractory brick; and then repeatedly freezing and thawing the refractory brick a number of times to remove slag from the refractory brick.

[0012] [2] The method for treating a refractory brick according to [1], wherein the freezing temperature is -20°C or lower.

[0013] [3] The method for treating a refractory brick according to [1] or [2], wherein the total processing time of the repeated freezing and thawing is 1 hour or longer.

[0014] [4] The method for treating a refractory brick according to any one of [1] to [3], wherein the number of repetitions of the freezing and thawing is four or more. Effect of the Invention

[0015] According to the method for treating refractory bricks of the present invention, it is possible to effectively separate slag adhering to the surfaces of the refractory bricks while ensuring the yield of the refractory bricks. [Brief description of the drawings]

[0016] [Figure 1] FIG. 2 is a schematic diagram of a processing flow according to one embodiment of the processing method of the present invention. [Diagram 2] FIG. 2 is a schematic diagram showing an effect of the processing method of the present invention. [Diagram 3] 1 is a graph in which the crushing strength and slag content of slag remaining on the surface of refractory bricks after treatment in the examples are plotted in relation to the time (number of repetitions) of freezing and thawing treatment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0017] Hereinafter, a method for treating a refractory brick according to one embodiment of the present invention (sometimes referred to as the "treatment method of the present embodiment") will be described. Note that the following description shows one embodiment or a preferred aspect of the present invention, and does not limit the present invention in any way.

[0018] The treatment method of this embodiment is a method for treating refractory bricks having slag adhering to their surfaces, and is characterized in that water is introduced into the refractory bricks, and then freezing and thawing are repeated multiple times to separate the slag from the refractory bricks.

[0019] More specifically, the treatment method of this embodiment includes a step of taking in water into a refractory brick having slag adhering to its surface (hereinafter, sometimes referred to as a "refractory brick with slag") (water taking in step), then a step of freezing the refractory brick (freezing step), and then a step of thawing the refractory brick (thawing step), and requires repeating the above-mentioned freezing step and thawing step multiple times.

[0020] 1 is a schematic diagram of a process flow according to this embodiment. Each step will be described in detail below with reference to FIG.

[0021] (Water intake process) In the water intake step, water 5 is taken into the refractory brick 1 with the slag 2 attached thereto, as shown in FIG. 1(A). This water intake step is performed to make the slag 2 easy to peel off in the following freezing step and drying step. In addition, in this water intake step, it is preferable that moisture penetrates between the refractory brick 1 and the surface-adhering slag 2 in order to make the slag 2 easy to peel off, as described above. As a specific method, it is preferable that the water intake step is performed by immersing the refractory brick 1 with the slag 2 attached thereto in water 5 stored in a water tank 4, as shown in FIG. 1(A). In this case, the immersion time is preferably 8 seconds or more in order to obtain the desired effect, and is preferably 20 seconds or less in terms of processing efficiency. In addition, the method of spraying water onto the surface of the refractory bricks, for example with a spray, may result in little or no penetration of water between the refractory bricks 1 and the surface-adhering slag 2 (i.e., the water may not be absorbed into the refractory bricks).

[0022] (freezing process) Next, in the freezing step, as shown in FIG. 1B, the refractory bricks 1 with the slag 2 after the water intake step are frozen using a freezer 6 or the like. In this freezing step, the water 5 that has permeated between the refractory bricks 1 and the surface-adhering slag 2 freezes to become ice 5', and the volume of the ice expands. From the viewpoint of finally making it easier for the slag 2 to peel off from the refractory bricks 1, the freezing temperature is preferably -15°C or lower, more preferably -20°C or lower, and even more preferably -25°C or lower. On the other hand, from the viewpoint of sufficiently causing volume expansion of the water (avoiding quick freezing), the freezing temperature is preferably -30°C or higher, and more preferably -28°C or higher. The freezing time is not particularly limited, but can be about 10 to 30 minutes.

[0023] (Thaw process) Next, in the thawing step, the refractory brick 1 with the slag 2 after the freezing step is thawed. The thawing is preferably performed by natural thawing as shown in Fig. 1(C). In the case of natural thawing, the time required for thawing is about 5 to 15 minutes.

[0024] (Repeated freezing and thawing) In the treatment method of this embodiment, the above-mentioned freezing and thawing must be repeated multiple times. By repeating the freezing and thawing steps multiple times, the water 5 that has penetrated between the refractory brick 1 and the surface-adhered slag 2 turns into ice 5' each time, causing repeated volume expansion (see FIG. 2). Furthermore, by repeating the freezing and thawing steps multiple times, the strength of the slag 2 that has adhered to the surface of the refractory brick 1 decreases. As a result, the slag 2 becomes easy to peel off from the refractory brick 1 (so-called freeze peeling). In this way, the slag 2 that has adhered to the surface of the refractory brick 1 can be effectively peeled off. Specifically, according to the treatment method of this embodiment, it is also possible to achieve a slag content of 2.7 mass% or less (a target value set based on the requirements of a specific recycling destination) of the refractory brick.

[0025] The timing for transition from the thawing process to the freezing process can be the time when the ice on the surface of the refractory bricks 1 melts and turns back into water.

[0026] The total processing time of the repeated freezing and thawing is not particularly limited, but is preferably 1 hour or more. In this case, the slag adhering to the surface of the refractory brick can be more effectively peeled off. From the same viewpoint, the total processing time of the repeated freezing and thawing is more preferably 3 hours or more, and even more preferably 4 hours or more. On the other hand, the total processing time is preferably 7 hours or less, since an excessively long processing time will saturate the amount of slag peeled off.

[0027] A certain degree of effect can be achieved if the freezing and thawing is repeated multiple times (two or more times), but it is particularly preferable that the freezing and thawing is repeated four or more times. In this case, the slag adhering to the surface of the refractory brick can be peeled off more effectively. From the same viewpoint, it is more preferable that the freezing and thawing is repeated six or more times, and even more preferable that the freezing and thawing is repeated nine or more times. On the other hand, since an excessively high number of times leads to a saturation of the amount of slag peeled off, it is preferable that the number of times is 14 or less.

[0028] (sieving process) In the treatment method of this embodiment, after the repeated freezing and thawing steps, the treated material (refractory bricks 1 and slag 2) can be passed through a sieve 8 and separated into a plurality of different fractions for recovery, as shown in (D) of Fig. 1. For example, by using a sieve 8 with a mesh size of 40 mm, refractory bricks 1 with a size of 40 mm or more remain on the sieve 8, making it possible to separate the refractory bricks 1 from other substances, including the peeled slag 2, which falls below the sieve 8, and thus to recover the treated refractory bricks 1.

[0029] In addition, the treatment method of this embodiment has the advantages that it is not necessary to crush or grind the refractory bricks, so that the labor required for crushing is saved, the refractory bricks 1 can be easily separated from the peeled slag 2, and the yield of the refractory bricks 1 during the sieving can be ensured. Specifically, according to the treatment method of this embodiment, it is possible to achieve a yield of 90% or more of the refractory bricks. EXAMPLES

[0030] The present invention will now be described in more detail with reference to examples, although the present invention is not limited to the following examples.

[0031] In the following, the peeling ability of slag adhering to the surface of refractory bricks was compared by changing the freezing and thawing processing time (number of repetitions) and the freezing temperature.

[0032] (1) Evaluation of freezing and thawing processing time (number of repetitions) A refractory brick with slag (slag content: about 16% by mass) was prepared and immersed in water for about 10 seconds. Next, freezing (freezing temperature: -20°C, freezing time: 20 minutes) and thawing (natural thawing, thawing time: 10 minutes) were combined into one set (total of 30 minutes), and freezing and thawing (repeated) were performed by changing one set at a time between 0 sets (no freezing) and 14 sets (total of 7 hours) (total of 15 cases). The crushing strength (MPa) of the slag remaining on the surface of the refractory brick after each example of freezing and thawing (repeated) was measured using a rebound hammer. In addition, the slag content (mass%) of the refractory brick after each example of freezing and thawing (repeated) was measured using a rebound hammer. A graph plotting these results is shown in Figure 3. In each example, the yield of the refractory brick was nearly 100%.

[0033] Figure 3 shows that the strength of the surface slag decreases the more times the freezing and thawing is repeated, and that by repeating freezing and thawing sufficiently, the slag adhering to the surface undergoes freeze-peeling and can eventually be completely detached from the refractory brick.

[0034] (2) Freezing temperature evaluation A refractory brick with slag (slag content: about 16% by mass) was prepared and immersed in water for about 10 seconds. Next, the freezing temperature was changed to -5°C, -10°C, -15°C, -20°C, -25°C, and -30°C, and a combination of freezing (freezing time: 20 minutes) and thawing (natural thawing, thawing time: 10 minutes) was counted as one set (total of 30 minutes), and up to 20 sets of freezing and thawing (total of 10 hours) were performed (total of 6 cases). In each example, the time when the slag content of the refractory bricks became 2.7 mass% or less (a target value set based on the requirements of a specific recycling destination) was considered to be the completion of freezing and peeling. This time is shown in Table 1. In each example, the yield of the refractory bricks was almost 100%.

[0035] [Table 1]

[0036] From Table 1, it can be seen that when the freezing temperature was -25°C, the slag content of the refractory bricks was reduced to the target value in the shortest time. When the freezing temperature was -30°C, the time to complete freezing and peeling took a little longer, but this is thought to be because the temperature was lowered too much, causing rapid freezing, which made it difficult for the volume expansion of the water to proceed.

[0037] As described above, the method for treating refractory bricks of the present invention can effectively separate the slag adhering to the surface of the refractory bricks while ensuring the yield of the refractory bricks. In particular, the present invention is expected to achieve a slag content of 2.7 mass% or less remaining in the refractory bricks and a refractory brick yield of 90% or more, which could not be achieved by conventional methods. [Explanation of symbols]

[0038] 1: Refractory bricks 2: Slug 4: Aquarium 5:Water 5': Ice 6: Freezer 8: Sieve

Claims

1. A method for treating refractory bricks having slag attached to their surfaces, comprising the steps of: A method for treating a refractory brick, comprising the steps of: introducing water into the refractory brick; and then repeatedly freezing and thawing the refractory brick a number of times to remove slag from the refractory brick.

2. 2. The method for treating a refractory brick according to claim 1, wherein the freezing temperature is −20° C. or lower.

3. 3. The method for treating a refractory brick according to claim 1 or 2, wherein a total treatment time for the repeated freezing and thawing is one hour or more.

4. 3. The method for treating a refractory brick according to claim 1, wherein the number of times the freezing and thawing is repeated is four or more.

Citation Information

Patent Citations

  • Production process of cement concrete recycled aggregate

    CN113105135A

  • Method for removing ceramic mold for shell mold

    JP2000288689A

  • Selection method of used refractory, and selector of used refractory

    JP2016168562A

  • Sorting and recovering method and facility for valuable substance from waste material

    JP2019089007A

  • Manufacturing method of recycled coarse aggregate

    JP2019151536A