Resin composition, method for manufacturing resin product and flame retardant master batch
A resin composition with a thermoplastic resin, phosphorus flame retardant, and acid-modified polyolefin resin addresses the need for improved flame retardancy and mechanical strength in resin products, offering high compositional freedom and sustainability benefits.
Patent Information
- Application Number
- JP2023079658
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-12
- Publication Date
- 2024-11-22
AI Technical Summary
Existing resin products require improved flame retardancy and mechanical strength while maintaining a high degree of compositional freedom.
A resin composition comprising a thermoplastic resin, a phosphorus flame retardant, and an acid-modified polyolefin resin with specific molecular weight and acid value ranges, along with a high concentration of phosphorus flame retardant, enhances mechanical strength and dispersibility, allowing for greater compositional flexibility.
The resin composition achieves excellent flame retardancy and mechanical strength, enabling a high degree of freedom in composition and reducing the need for metal products, contributing to industrial innovation and sustainability.
Smart Images

Figure 2024163780000001 
Figure 2024163780000002 
Figure 2024163780000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a resin composition, a method for producing a resin product, and a flame retardant masterbatch. [Background technology]
[0002] Polyolefin resins have excellent mechanical properties (bending properties, tensile properties, etc.), chemical resistance, moldability, etc., and are low in specific gravity and inexpensive, so that molded articles are used in various applications such as machinery, electrical and electronic equipment, office automation equipment, automotive interior and exterior materials, and electric vehicles. In these applications, the molded articles may be required to be flame retardant. For example, molded articles used for housings (frames, casings, exteriors, covers, etc.) of electrical and electronic equipment or office automation equipment, cables, etc., require high flame retardancy.
[0003] The flame retardancy of a resin product can be improved by adding a flame retardant to the resin composition that is the material of the resin product. A resin composition containing such a flame retardant is known to contain a thermoplastic resin (A), a phosphorus-based flame retardant (B), and a copolymer (C) of an α-olefin and an unsaturated carboxylic acid in a specific ratio (see, for example, Patent Document 1). [Prior art documents] [Patent documents]
[0004] [Patent Document 1] International Publication No. 2021 / 241682 Summary of the Invention [Problem to be solved by the invention]
[0005] On the other hand, resin products that require flame retardancy are usually required to exhibit properties other than flame retardancy. Therefore, flame retardant resin products may be required to have a high degree of freedom in their composition. In addition, such flame retardant resin products may be required to have excellent mechanical strength.
[0006] An object of one aspect of the present invention is to provide a technique suitable for increasing the degree of freedom in the composition of flame-retardant resin products having excellent mechanical strength. [Means for solving the problem]
[0007] In order to solve the above problems, a resin composition according to one embodiment of the present invention comprises a thermoplastic resin (A), a phosphorus-based flame retardant (B), and an acid-modified polyolefin-based resin (C), wherein the acid-modified polyolefin-based resin (C) has an acid value of 70 mg KOH / g or less and a weight-average molecular weight of 1,000 or more and 300,000 or less, and the proportion of the phosphorus-based flame retardant (B) is 50 mass% or more.
[0008] In order to solve the above problems, a method for producing a resin product according to one embodiment of the present invention produces a resin product by molding a product resin composition obtained by diluting the above resin composition with a material composition.
[0009] In order to solve the above problems, a flame retardant masterbatch according to one aspect of the present invention is a pellet of the above resin composition. Effect of the Invention
[0010] According to one aspect of the present invention, it is possible to provide a resin composition suitable for increasing the degree of freedom in the composition of a flame-retardant resin product having excellent mechanical strength, a method for producing the resin product, and a flame-retardant masterbatch. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] [Resin composition] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS An embodiment of the present invention will be described in detail below. The resin composition according to the embodiment of the present invention contains a thermoplastic resin (A), a phosphorus-based flame retardant (B), and an acid-modified polyolefin resin (C).
[0012] [Thermoplastic resin (A)] The thermoplastic resin is not particularly limited, and examples thereof include polyolefin resin, polycarbonate resin, polyester resin, acrylonitrile styrene resin, ABS resin, polyamide resin, modified polyphenylene oxide, etc. These may be used alone or in combination of two or more. For example, the thermoplastic resin (A) may be a composite resin of two or more of the above thermoplastic resins.
[0013] The polyolefin resin is not particularly limited, and may be any of the resins described below. The polyester resin is not particularly limited, and may be, for example, polybutylene terephthalate. The polyamide resin is not particularly limited, and may be, for example, nylon 66 and nylon 6. Among them, the present invention is particularly useful when the thermoplastic resin (A) is a polyolefin resin.
[0014] In the present invention, the term "polyolefin resin" refers to a resin in which the proportion of olefin units or cycloolefin units is 90 mol % or more relative to 100 mol % of all constituent units constituting the resin. The proportion of olefin units or cycloolefin units relative to 100 mol % of all constituent units constituting the polyolefin resin is preferably 95 mol % or more, and particularly preferably 98 mol % or more.
[0015] Examples of polyolefin resins include α-olefin polymers such as polyethylene, polypropylene, polybutene, poly(3-methyl-1-butene), poly(3-methyl-1-pentene), and poly(4-methyl-1-pentene); α-olefin copolymers such as ethylene-propylene block or random copolymers, α-olefin-propylene block or random copolymers having 4 or more carbon atoms, ethylene-methyl methacrylate copolymers, and ethylene-vinyl acetate copolymers; and cycloolefin polymers such as polycyclohexene and polycyclopentene. Examples of polyethylene include low-density polyethylene, linear low-density polyethylene, and high-density polyethylene. Examples of polypropylene include isotactic polypropylene, syndiotactic polypropylene, hemiisotactic polypropylene, and stereoblock polypropylene. In the α-olefin-propylene block or random copolymers having 4 or more carbon atoms, examples of the α-olefins having 4 or more carbon atoms include butene, 3-methyl-1-butene, 3-methyl-1-pentene, and 4-methyl-1-pentene. These polyolefin resins may be used alone or in combination of two or more kinds.
[0016] The polyolefin resin preferably contains polypropylene. Polypropylene may be used in combination with other polyolefin resins. For example, as the polyolefin resin, a mixture of polypropylene and other α-olefin polymers such as ethylene-propylene block or random copolymers, and α-olefin-propylene block or random copolymers having 4 or more carbon atoms may be used.
[0017] The polyolefin resin is preferably composed mainly of polypropylene. The proportion of polypropylene in 100% by mass of the polyolefin resin is preferably 50% by mass or more, more preferably 60% by mass or more. From the viewpoint of flame retardancy, it is particularly preferable that 100% by mass of the polyolefin resin is polypropylene.
[0018] The melt mass flow rate (MFR) of the thermoplastic resin (A) is preferably 0.1 g / 10 min or more, more preferably 0.5 g / 10 min or more, while it is preferably 80 g / 10 min or less, more preferably 60 g / 10 min or less. If the MFR of the thermoplastic resin (A) is the lower limit or more, the molding processability is better, and if it is the upper limit or less, the bending property, tensile property, chemical resistance property, etc. are better. The preferable lower limit and upper limit can be appropriately combined (hereinafter the same). The MFR of the thermoplastic resin (A) may be, for example, 0.1 g / 10 min or more and 80 g / 10 min or less, or 0.5 g / 10 min or more and 60 g / 10 min or more. The melt mass flow rate of the thermoplastic resin (A) is measured in accordance with JIS K7210 under the conditions of a temperature of 230 ° C. and a load of 2.16 kg.
[0019] The proportion of the thermoplastic resin (A) relative to the total mass of the present resin composition is preferably 40% by mass or less, more preferably 29% by mass or less, even more preferably 27% by mass or less, and particularly preferably 25% by mass or less, from the viewpoint of increasing the proportion of the phosphorus-based flame retardant (B) in the resin composition, while from the viewpoint of productivity, it is preferably 10% by mass or more, more preferably 15% by mass or more, and even more preferably 18% by mass or more.
[0020] The polypropylene preferably has an MFR of 10 g / 10 min or more, more preferably 20 g / 10 min or more. A polypropylene having high fluidity is suitable for use as a master batch of the resin composition.
[0021] [Phosphorus-based flame retardants (B)] The phosphorus-based flame retardant (B) is a phosphorus compound, i.e., a compound containing a phosphorus atom in the molecule. The phosphorus-based flame retardant (B) exerts a flame retardant effect by forming char when the resin composition is burned. The phosphorus-based flame retardant (B) may be a known one, for example, (poly)phosphate, (poly)phosphate ester, etc. "(Poly)phosphate" refers to a phosphate or polyphosphate. "(Poly)phosphate ester" refers to a phosphate ester or polyphosphate ester. The phosphorus-based flame retardant (B) is preferably a solid at 80°C.
[0022] From the viewpoint of flame retardancy, the phosphorus-based flame retardant (B) is preferably a (poly)phosphate. Examples of the (poly)phosphate include ammonium polyphosphate, melamine polyphosphate, piperazine polyphosphate, piperazine orthophosphate, melamine pyrophosphate, piperazine pyrophosphate, melamine polyphosphate, melamine orthophosphate, calcium phosphate, and magnesium phosphate.
[0023] In addition, in the above examples, compounds in which melamine or piperazine is replaced with other nitrogen compounds can be used in the same manner. Examples of other nitrogen compounds include N,N,N',N'-tetramethyldiaminomethane, ethylenediamine, N,N'-dimethylethylenediamine, N,N'-diethylethylenediamine, N,N-dimethylethylenediamine, N,N-diethylethylenediamine, N,N,N',N'-tetramethylethylenediamine, N,N,N',N'-diethylethylenediamine, 1,2-propanediamine, 1,3-propanediamine, tetramethylethylene ... Ethylenediamine, pentamethylenediamine, hexamethylenediamine, 1,7-diaminoheptane, 1,8-diaminooctane, 1,9-diaminononane, 1,10-diaminodecane, trans-2,5-dimethylpiperazine, 1,4-bis(2-aminoethyl)piperazine, 1,4-bis(3-aminopropyl)piperazine, acetoguanamine, benzoguanamine, acrylguanamine, 2,4-diamino-6-nonyl-1,3,5-trimethylguanamine, Azine, 2,4-diamino-6-hydroxy-1,3,5-triazine, 2-amino-4,6-dihydroxy-1,3,5-triazine, 2,4-diamino-6-methoxy-1,3,5-triazine, 2,4-diamino-6-ethoxy-1,3,5-triazine, 2,4-diamino-6-propoxy-1,3,5-triazine, 2,4-diamino-6-isopropoxy-1,3,5-triazine, 2,4-diamino-6-mercapto-1 ,3,5-triazine, 2-amino-4,6-dimercapto-1,3,5-triazine, ammeline, benzguanamine, acetoguanamine, phthalodiguanamine, melamine cyanurate, melamine pyrophosphate, butylenediguanamine, norbornenediguanamine, methylenediguanamine, ethylenedimelamine, trimethylenedimelamine, tetramethylenedimelamine, hexamethylenedimelamine, and 1,3-hexylenedimelamine. These (poly)phosphates may be used alone or in combination of two or more.
[0024] Among the above, the phosphorus-based flame retardant (B) is preferably a salt of (poly)phosphoric acid and a nitrogen compound (hereinafter also referred to as "compound (B1)"). Compound (B1) is an intumescent flame retardant, and forms a surface expansion layer (intemescent) which is a foamed char when the resin composition is burned. The formation of the surface expansion layer suppresses the diffusion or heat transfer of decomposition products, and excellent flame retardancy is exhibited. Examples of the nitrogen compound in compound (B1) include ammonia, melamine, piperazine, and the other nitrogen compounds described above.
[0025] Commercially available phosphorus-based flame retardants (B) include, for example, Adeka STAB (registered trademark) FP-2100J, FP-2200, and FP-2500S (manufactured by ADEKA Corporation).
[0026] The proportion of the phosphorus-based flame retardant (B) to the total amount of the resin composition is 50% by mass or more. The proportion of 50% by mass or more is suitable from the viewpoint of increasing the flame retardancy of the resin composition and from the viewpoint of fully expressing desired properties other than flame retardancy in the resin composition. Furthermore, the proportion of 50% by mass or more is suitable for using the resin composition as a flame retardant master batch (hereinafter also simply referred to as "master batch") and is suitable for increasing the degree of freedom of composition other than the flame retardant in the resin composition (hereinafter also referred to as "full compound") that is the material of the resin product. In addition, the proportion of 50% by mass or more can express high flame retardancy of the resin product and further increase the mechanical strength (bending strength) when used as a master batch in combination with the acid-modified polyolefin resin (C) described later.
[0027] The proportion of the phosphorus-based flame retardant (B) relative to the total amount of the resin composition is preferably 55% by mass or more, more preferably 60% by mass or more, even more preferably 65% by mass or more, and particularly preferably 70% by mass or more. The proportion may be appropriately determined from the viewpoint of sufficiently dispersing the phosphorus-based flame retardant (B), and may be 90% by mass or less, 85% by mass or less, or 80% by mass or less from such a viewpoint.
[0028] The mass ratio (B / A) of the phosphorus-based flame retardant (B) to the thermoplastic resin (A) is preferably 1.5 times or more, more preferably 2.4 times or more, even more preferably 3.0 times or more, and particularly preferably 4.0 times or more, from the viewpoint of flame retardancy and from the viewpoint of increasing the degree of freedom of composition in a full compound when used as a resin composition or a master batch. On the other hand, from the viewpoint of productivity, the mass ratio (B / A) may be 9.0 times or less.
[0029] [Acid-modified polyolefin resin (C)] The acid-modified polyolefin resin (C) according to the present invention has an acid value of 70 mgKOH / g or less and a weight average molecular weight of 1,000 to 300,000. Such an acid-modified polyolefin resin (C) enhances the dispersibility of the phosphorus-based flame retardant (B) in the thermoplastic resin (A). In addition, by including the acid-modified polyolefin resin (C) in the resin composition, a resin composition containing a high concentration of the phosphorus-based flame retardant (B) can be obtained.
[0030] The weight average molecular weight of the acid-modified polyolefin resin (C) is preferably 1,500 or more, more preferably 3,000 or more, while it is preferably 250,000 or less, more preferably 100,000 or less, even more preferably 50,000 or less, and particularly preferably 40,000 or less. If the weight average molecular weight of the acid-modified polyolefin resin (C) is within the above upper and lower limit ranges, the dispersibility of the phosphorus-based flame retardant (B) is more excellent, and the resin molded product obtained by using the resin composition as a master batch has excellent mechanical strength. The weight average molecular weight of the acid-modified polyolefin resin (C) is a value calculated in terms of standard polystyrene, which is measured by dissolving the acid-modified polyolefin resin (C) in tetrahydrofuran (THF) and performing gel permeation chromatography.
[0031] The upper limit of the acid value of the acid-modified polyolefin resin (C) is preferably 65 mgKOH / g or less, more preferably 62 mgKOH / g or less, and even more preferably 60 mgKOH / g or less. This allows the flame retardancy and mechanical properties (flexural strength) to be sufficiently improved. The lower limit of the acid value is not particularly limited, but is usually 1 mgKOH / g or more, 10 mgKOH / g or more, or 20 mgKOH / g or more. This allows the deterioration of the flame-retardant resin composition to be suppressed.
[0032] The acid value is a value obtained by measuring according to the following procedures (i) to (iii) in accordance with JIS K0070.
[0033] <Method for measuring the acid value of acid-modified resin> (i) Dissolve 1 g of the acid-modified resin in 70 mL of xylene heated to 140°C. (ii) At the same temperature, titration is performed with 0.1 mol / L potassium hydroxide ethanol solution (product name "0.1 mol / L ethanolic potassium hydroxide solution", manufactured by Wako Pure Chemical Industries, Ltd.) using phenolphthalein as an indicator. (iii) Convert the amount of potassium hydroxide required for the titration into mg to calculate the acid value (unit: mgKOH / g).
[0034] In the present invention, "acid-modified polyolefin resin (C)" means a polyolefin having a structure chemically modified by an acidic monomer, such as an unsaturated carboxylic acid-grafted olefin polymer (hereinafter also referred to as "copolymer (C)").
[0035] Commercially available examples of the copolymer (C) include Eumex (registered trademark) 1010 (manufactured by Sanyo Chemical Industries, Ltd.), Admer (registered trademark) BE518 (manufactured by Mitsui Chemicals, Inc.), and Hiwax (registered trademark) 1105A (manufactured by Mitsui Chemicals, Inc.).
[0036] In the resin composition, the ratio of the acid-modified polyolefin resin (C) to the total amount of the resin composition can be appropriately determined from the viewpoint of sufficiently dispersing the phosphorus-based flame retardant (B). From the viewpoint of improving the tensile properties of the resin composition, the ratio is preferably 10% by mass or less, more preferably 5% by mass or less, even more preferably 4.8% by mass or less, and particularly preferably 4.6% by mass or less. Moreover, from the viewpoint of dispersing the phosphorus-based flame retardant (B) well in the resin composition, the ratio is preferably 1% by mass or more, more preferably 2% by mass or more, and even more preferably 3% by mass or more.
[0037] The ratio of the acid-modified polyolefin resin (C) to the total amount of the resin composition being within the above range, when the resin composition is used as a master batch, a resin product having high flame retardancy while maintaining high mechanical strength and high flexural modulus can be obtained. From the above viewpoint, the ratio of the acid-modified polyolefin resin (C) to the phosphorus-based flame retardant (B) in the resin composition may be, for example, 15% by mass or less, 12% by mass or less, 10% by mass or less, 9% by mass or less, 1% by mass or more, 2% by mass or more, 3% by mass or more, or 4% by mass or more.
[0038] The ratio of the total mass of the thermoplastic resin (A), the phosphorus-based flame retardant (B) and the acid-modified polyolefin resin (C) to the total mass of the resin composition according to the present embodiment is not particularly limited, but is preferably high from the viewpoint of increasing the degree of freedom of the composition when used as a master batch. From this viewpoint, the ratio is preferably 90% by mass or more, more preferably 95% by mass or more, and even more preferably 99% by mass or more.
[0039] [Other ingredients] The resin composition according to the present embodiment may further contain other components other than the thermoplastic resin (A), the phosphorus-based flame retardant (B) and the acid-modified polyolefin resin (C) within a range in which the effects of the present invention can be obtained. The other components may be one or more, and the type and amount may be appropriately determined within a range in which both the effects of the present invention and the effects of the other components can be obtained. Examples of the other components include flame retardants and flame retardant assistants other than the phosphorus-based flame retardant (B).
[0040] <Other flame retardants and flame retardant auxiliaries> The other flame retardants or flame retardant auxiliaries are preferably halogen-free organic or inorganic flame retardants or flame retardant auxiliaries, such as triazine ring-containing compounds, silicone flame retardants, metal hydroxides, metal oxides, boric acid compounds, expandable graphite, and fluorine-based drip prevention agents.
[0041] Examples of triazine ring-containing compounds include melamine, ammeline, benzguanamine, acetoguanamine, phthalodiguanamine, melamine cyanurate, butylenediguanamine, norbornenediguanamine, methylenediguanamine, ethylenedimelamine, trimethylenedimelamine, tetramethylenedimelamine, hexamethylenedimelamine, and 1,3-hexylenedimelamine. Examples of silicone flame retardants include silicone oil, silicone rubber, and silicone resin. Examples of metal hydroxides include magnesium hydroxide, aluminum hydroxide, calcium hydroxide, barium hydroxide, zinc hydroxide, and Kismer 5A (registered trademark of magnesium hydroxide manufactured by Kyowa Chemical Industry Co., Ltd.). Examples of metal oxides include inorganic compounds such as zinc oxide, titanium oxide, aluminum oxide, magnesium oxide, titanium dioxide, and hydrotalcite, and surface-treated products thereof. Specific examples of metal oxides include TIPAQUE R-680 (registered trademark of titanium oxide manufactured by Ishihara Sangyo Kaisha), Kyowamag 150 (registered trademark of magnesium oxide manufactured by Kyowa Chemical Industry Co., Ltd.), DHT-4A (hydrotalcite: manufactured by Kyowa Chemical Industry Co., Ltd.), and Alcamizer 4 (registered trademark of zinc-modified hydrotalcite manufactured by Kyowa Chemical Industry Co., Ltd.). Examples of boric acid compounds include zinc borate. Examples of fluorine-based drip prevention agents include polytetrafluoroethylene (PTFE). These flame retardants or flame retardant assistants may be used alone or in combination of two or more.
[0042] In addition to the above, the resin composition may contain additives that are usually used in synthetic resins, such as crosslinking agents, antistatic agents, metal soaps, filling agents, antifogging agents, anti-plateout agents, surface treatment agents, fluorescent agents, antifungal agents, bactericides, foaming agents, metal deactivators, release agents, pigments, processing aids, etc., within the range in which the effects of the present invention can be obtained.
[0043] As described above, the resin composition of the present invention may contain various additives, but when the resin composition is used as a flame retardant master batch, the content of inorganic fillers derived from minerals such as calcium carbonate or talc in the resin composition is preferably 5% by mass or less. In this case, the handleability as a master batch is improved. From the same viewpoint, the content is more preferably 3% by mass or less, further preferably 2% by mass or less, and particularly preferably 1% by mass or less.
[0044] [Method of producing resin composition] Any method can be used to produce the resin composition. For example, the thermoplastic resin (A), the phosphorus-based flame retardant (B), the acid-modified polyolefin resin (C), and other components such as other flame retardants or flame retardant auxiliaries as necessary are thoroughly mixed using a premixing means such as a V-type blender, a Henschel mixer, a mechanochemical device, or an extrusion mixer, and optionally granulated using an extrusion granulator or a briquetting machine, and then melt-kneaded and extruded using a melt kneader. Examples of the melt kneader include twin-screw extruders such as vent-type twin-screw extruders, Banbury mixers, kneading rolls, single-screw extruders, and multi-screw extruders with three or more screws. The temperature during melt kneading is, for example, 170 to 260°C. The form of the resin composition extruded as described above is not limited, but when used as a master batch for a resin product, it is preferably in the form of pellets from the viewpoint of handling and easy kneading with other materials. In this case, the resin composition melt-kneaded as described above may be directly cut and pelletized by a machine such as a pelletizer, or may be cooled to form strands, and then the strands may be cut and pelletized by a machine such as a pelletizer, or a lump of the resin composition separately molded into a body may be crushed and pelletized. Here, the pellet refers to a minute piece of the resin composition having a major axis length of 0.1 to 10 mm, regardless of the production method.
[0045] The resin composition is suitably used for a flame retardant masterbatch for dispersing a phosphorus-based flame retardant (B) in a material resin composition (full compound) for resin products. Since the resin composition contains a sufficiently large amount of the phosphorus-based flame retardant (B), the degree of freedom in the composition of the full compound is further increased. Therefore, it is applicable to the manufacture of various resin products that require flame retardancy.
[0046] [Method for manufacturing resin products] An embodiment of the present invention includes a method for producing a resin product by molding a product resin composition obtained by diluting the above-mentioned resin composition with a material composition to produce a resin product. As described above, the above-mentioned resin composition contains a high concentration of the phosphorus-based flame retardant (B), and therefore is suitably used as a master batch for flame retardants.
[0047] The resin product according to one aspect of the present invention is made of the resin composition according to the present embodiment. The shape of the resin product is not particularly limited, and may be in various shapes such as a resin plate, sheet, film, cable, or irregular shape.
[0048] The resin product can be obtained by molding the above-mentioned resin composition. The molding method is not particularly limited, and examples thereof include extrusion processing, calendar processing, injection molding, rolling, compression molding, blow molding, etc. The temperature at which the resin composition is molded is, for example, 170 to 260°C.
[0049] The material composition contains, for example, a matrix resin and other material components other than the matrix resin and the above-mentioned resin composition.
[0050] [Matrix resin] The above-mentioned thermoplastic resin (A) can be used as the matrix resin. The thermoplastic resin (A) as the matrix resin may be the same as or different from the thermoplastic resin (A) in the above-mentioned resin composition, but it is preferable that the thermoplastic resin (A) as the matrix resin is the same as the thermoplastic resin (A) in the above-mentioned resin composition. The ratio of the matrix resin to the above-mentioned resin composition may be appropriately determined based on the flame retardancy required for the resin product. For example, the ratio may be 100 to 500 mass%.
[0051] From the viewpoint of improving flame retardancy, it is preferable to employ a polyolefin-based resin as the matrix resin from among the above-mentioned thermoplastic resins (A) and to employ a polyolefin-based resin as the thermoplastic resin (A) of the resin composition. [Other material components] The material composition may contain at least one inorganic fiber filler (D) selected from the group consisting of glass fiber and carbon fiber. The inorganic fiber filler (D) may be used alone or in combination of two or more.
[0052] The type of glass fiber is not particularly limited, and any glass fiber such as E glass, C glass, S glass, D glass, etc. The form of the glass fiber is also not particularly limited, and any glass fiber such as chopped strand, roving, yarn, glass wool, etc. can be used, but chopped strand and glass wool are preferred from the viewpoint of workability.
[0053] The type of carbon fiber is not particularly limited, and any carbon fiber such as polyacrylonitrile (PAN)-based carbon fiber, pitch-based carbon fiber, graphite fiber, etc. The form of the carbon fiber is also not particularly limited, and any carbon fiber such as filament, regular tow, large tow, stable yarn, chopped strand, etc. can be used, but chopped strand is preferred from the viewpoint of workability.
[0054] When the material composition contains an inorganic fiber filler (D), the proportion of the inorganic fiber filler (D) relative to the total mass of the material composition is preferably 0.01 mass% or more, more preferably 0.1 mass% or more, and is preferably 50 mass% or less, more preferably 40 mass% or less, more preferably 30 mass% or less, more preferably 25 mass% or less, more preferably 10 mass% or less, even more preferably 5 mass% or less, and particularly preferably 3 mass% or less. If the proportion of the inorganic fiber filler (D) is equal to or more than the lower limit, it is easy to obtain a lip prevention effect and a smoke suppression effect, and if it is equal to or less than the upper limit, the inherent physical properties of the matrix resin are unlikely to be impaired.
[0055] When the material composition contains an inorganic fiber filler (D), it may further contain an interfacial strength improver (E) for the inorganic fiber filler (D). As the interfacial strength improver (E), a polymer having an olefin skeleton (excluding polyolefin resin and copolymer (C)) is preferable from the viewpoint of compatibility with the thermoplastic resin (A) such as polyolefin resin. The interfacial strength is further improved by the compatibility of the olefin skeleton with the polyolefin resin.
[0056] The material composition may contain at least one selected from the group consisting of an antioxidant, an ultraviolet absorber, a light stabilizer, and an antiaging agent.
[0057] Examples of the antioxidant include phenol-based antioxidants, phosphorus-based antioxidants, and thioether-based antioxidants. Examples of the phenol-based antioxidant include 2,6-di-tert-butyl-p-cresol, 2,6-diphenyl-4-octadecyloxyphenol, distearyl (3,5-di-tert-butyl-4-hydroxybenzyl)phosphonate, 1,6-hexamethylenebis[(3,5-di-tert-butyl-4-hydroxyphenyl)propionamide], 4,4'-thiobis(6-tert-butyl-m-cresol), 2,2'-methylenebis(4-methyl-6-tert-butylphenol), 2,2'-methylenebis(4-ethyl-6 -tert-butylphenol), 4,4'-butylidenebis(6-tert-butyl-m-cresol), 2,2'-ethylidenebis(4,6-di-tert-butylphenol), 2,2'-ethylidenebis(4-sec-butyl-6-tert-butylphenol), 1,1,3-tris(2-methyl-4-hydroxy-5-tert-butylphenyl)butane, 1,3,5-tris(2,6-dimethyl-3-hydroxy-4-tert-butylbenzyl)isocyanurate, 1,3,5-tris(3,5-di-tert-butyl-4-hydroxybenzyl)iso Cyanurate, 1,3,5-tris(3,5-ditert-butyl-4-hydroxybenzyl)-2,4,6-trimethylbenzene, 2-tert-butyl-4-methyl-6-(2-acryloyloxy-3-tert-butyl-5-methylbenzyl)phenol, stearyl(3,5-ditert-butyl-4-hydroxyphenyl)propionate, tetrakis[3-(3,5-ditert-butyl-4-hydroxyphenyl)propionate methyl]methane, thiodiethylene glycol bis[(3,5-ditert-butyl-4-hydroxyphenyl) ) propionate], 1,6-hexamethylenebis[(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], bis[3,3-bis(4-hydroxy-3-tert-butylphenyl)butyric acid] glycol ester, bis[2-tert-butyl-4-methyl-6-(2-hydroxy-3-tert-butyl-5-methylbenzyl)phenyl] terephthalate, 1,3,5-tris[(3,5-di-tert-butyl-4-hydroxyphenyl)propionyloxyethyl] isocyanurate, 3,9-bis[1,Examples of the phenol-based antioxidant include 1-dimethyl-2-{(3-tert-butyl-4-hydroxy-5-methylphenyl)propionyloxy}ethyl]-2,4,8,10-tetraoxaspiro[5,5]undecane, triethylene glycol bis[(3-tert-butyl-4-hydroxy-5-methylphenyl)propionate], etc. The content of the phenol-based antioxidant is preferably 0.001 parts by mass or more, more preferably 0.05 parts by mass or more, and more preferably 10 parts by mass or less, more preferably 5 parts by mass or less, based on 100 parts by mass of the synthetic resin component in the full compound.
[0058] Examples of phosphorus-based antioxidants include trisnonylphenyl phosphite, tris[2-tert-butyl-4-(3-tert-butyl-4-hydroxy-5-methylphenylthio)-5-methylphenyl]phosphite, tridecyl phosphite, octyldiphenyl phosphite, di(decyl)monophenyl phosphite, di(tridecyl)pentaerythritol diphosphite, di(nonylphenyl)pentaerythritol diphosphite, bis(2,4-ditert-butylphenyl)phosphite, phenyl)pentaerythritol diphosphite, bis(2,6-ditert-butyl-4-methylphenyl)pentaerythritol diphosphite, bis(2,4,6-tritert-butylphenyl)pentaerythritol diphosphite, bis(2,4-dicumylphenyl)pentaerythritol diphosphite, tetra(tridecyl)isopropylidenediphenol diphosphite, tetra(tridecyl)-4,4'-n-butylidenebis(2-tert-butyl-5-methylphenol) hexa(tridecyl)-1,1,3-tris(2-methyl-4-hydroxy-5-tert-butylphenyl)butane triphosphite, tetrakis(2,4-ditert-butylphenyl)biphenylene diphosphonite, 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide, 2,2'-methylenebis(4,6-tert-butylphenyl)-2-ethylhexyl phosphite, 2,2'-methylenebis(4,6-tert-butylphenyl)-2-ethylhexyl phosphite Examples of suitable antioxidants include 2-ethyl-2-butylpropylene glycol and 2,4,6-tri-tert-butylphenol phosphite, tris(2-[(2,4,8,10-tetrakis-tert-butyldibenzo[d,f][1,3,2]dioxaphosphepin-6-yl)oxy]ethyl)amine, 2-ethyl-2-butylpropylene glycol and 2,4,6-tri-tert-butylphenol phosphite, and tris(2,4-di-tert-butylphenyl)phosphite. The content of the phosphorus-based antioxidant is preferably 0.001 parts by mass or more, more preferably 0.05 parts by mass or more, and more preferably 10 parts by mass or less, and more preferably 5 parts by mass or less, based on 100 parts by mass of the synthetic resin component in the full compound.
[0059] Examples of thioether-based antioxidants include dialkyl thiodipropionates such as dilauryl thiodipropionate, dimyristyl thiodipropionate, and distearyl thiodipropionate, and pentaerythritol tetra(β-alkylthiopropionate esters). The content of the thioether-based antioxidant is preferably 0.001 parts by mass or more, more preferably 0.05 parts by mass or more, and more preferably 10 parts by mass or less, and more preferably 5 parts by mass or less, relative to 100 parts by mass of the synthetic resin component in the full compound.
[0060] Examples of the ultraviolet absorber include 2-hydroxybenzophenones such as 2,4-dihydroxybenzophenone, 2-hydroxy-4-methoxybenzophenone, 2-hydroxy-4-octoxybenzophenone, and 5,5'-methylenebis(2-hydroxy-4-methoxybenzophenone); 2-(2'-hydroxy-5'-methylphenyl)benzotriazole, 2-(2'-hydroxy-3',5'-di-tert-butylphenyl)-5-chlorobenzotriazole, and 2-(2'-hydroxy-3',5'- 2-(2'-hydroxyphenyl)benzotriazoles such as 2-(2'-hydroxy-5'-tert-octylphenyl)benzotriazole, 2-(2'-hydroxy-3',5'-dicumylphenyl)benzotriazole, 2,2'-methylenebis(4-tert-octyl-6-(benzotriazolyl)phenol), and 2-(2'-hydroxy-3'-tert-butyl-5'-carboxyphenyl)benzotriazole; phenylsa Benzoates such as ricinate, resorcinol monobenzoate, 2,4-ditert-butylphenyl-3,5-ditert-butyl-4-hydroxybenzoate, 2,4-ditert-amylphenyl-3,5-ditert-butyl-4-hydroxybenzoate, hexadecyl-3,5-ditert-butyl-4-hydroxybenzoate; substituted oxanilides such as 2-ethyl-2'-ethoxyoxanilide, 2-ethoxy-4'-dodecyloxanilide; ethyl-α-cyano-β,β-diphenylacrylate, methyl cyanoacrylates such as aryl-2-cyano-3-methyl-3-(p-methoxyphenyl)acrylate; and triaryl triazines such as 2-(2-hydroxy-4-octoxyphenyl)-4,6-bis(2,4-di-tert-butylphenyl)-s-triazine, 2-(2-hydroxy-4-methoxyphenyl)-4,6-diphenyl-s-triazine, and 2-(2-hydroxy-4-propoxy-5-methylphenyl)-4,6-bis(2,4-di-tert-butylphenyl)-s-triazine. The content of the ultraviolet absorber is preferably 0.001 parts by mass or more, more preferably 0.05 parts by mass or more, and more preferably 30 parts by mass or less, and more preferably 10 parts by mass or less, relative to 100 parts by mass of the synthetic resin component in the full compound.
[0061] Examples of light stabilizers include 2,2,6,6-tetramethyl-4-piperidyl stearate, 1,2,2,6,6-pentamethyl-4-piperidyl stearate, 2,2,6,6-tetramethyl-4-piperidyl benzoate, bis(2,2,6,6-tetramethyl-4-piperidyl)sebacate, bis(1,2,2,6,6-tetramethyl-4-piperidyl)sebacate, bis(1-octoxy-2,2,6,6-tetramethyl-4-piperidyl)sebacate, and tetrakis(2,2,6,6-tetramethyl-4-piperidyl)-1,2,3,4-butanol. tetracarboxylate, tetrakis(1,2,2,6,6-pentamethyl-4-piperidyl)-1,2,3,4-butanetetracarboxylate, bis(2,2,6,6-tetramethyl-4-piperidyl)·di(tridecyl)-1,2,3,4-butanetetracarboxylate, bis(1,2,2,6,6-pentamethyl-4-piperidyl)·di(tridecyl)-1,2,3,4-butanetetracarboxylate, bis(1,2,2,4,4-pentamethyl-4-piperidyl)-2-butyl-2-(3,5-ditert-butyl-4-hydroxybenzyl )malonate, 1-(2-hydroxyethyl)-2,2,6,6-tetramethyl-4-piperidinol / diethyl succinate polycondensate, 1,6-bis(2,2,6,6-tetramethyl-4-piperidylamino)hexane / 2,4-dichloro-6-morpholino-s-triazine polycondensate, 1,6-bis(2,2,6,6-tetramethyl-4-piperidylamino)hexane / 2,4-dichloro-6-tert-octylamino-s-triazine polycondensate, 1,5,8,12-tetrakis[2,4-bis(N-butyl-N-(2,2,6,6-tetramethyl-4-piperidylamino)hexane / 2,4-dichloro-6-tert-octylamino-s-triazine polycondensate, lysyl)amino)-s-triazin-6-yl]-1,5,8,12-tetraazadodecane, 1,5,8,12-tetrakis[2,4-bis(N-butyl-N-(1,2,2,6,6-pentamethyl-4-piperidyl)amino)-s-triazin-6-yl]-1,5,8-12-tetraazadodecane, 1,6,11-tris[2,4-bis(N-butyl-N-(2,2,6,6-tetramethyl-4-piperidyl)amino)-s-triazin-6-yl]aminoundecane, 1,6,11-tris[2,4-bis(N-butyl-N-(1,2,2,6,Examples of the hindered amine compounds include 6-pentamethyl-4-piperidyl)amino)-s-triazin-6-yl)aminoundecane. The content of the light stabilizer is preferably 0.001 parts by mass or more, more preferably 0.05 parts by mass or more, and is preferably 30 parts by mass or less, more preferably 10 parts by mass or less, based on 100 parts by mass of the synthetic resin component in the full compound.
[0062] The material composition may contain other fillers than the inorganic fiber filler (D). As the other fillers, those in the form of fibers, plates, particles, or powders can be used. Specifically, inorganic fibrous reinforcing materials such as asbestos fibers, metal fibers, potassium titanate whiskers, aluminum borate whiskers, magnesium whiskers, silicon whiskers, wollastonite, sepiolite, asbestos, slag fibers, zonolite, elestadite, gypsum fibers, silica fibers, silica-alumina fibers, zirconia fibers, boron nitride fibers, silicon nitride fibers, and boron fibers, polyester fibers, nylon fibers, acrylic fibers, regenerated cellulose fibers, acetate fibers, kenaf, ramie, cotton, jute, hemp, sisal, flax, linen, and silk can be used. Examples of the fillers include organic fibrous reinforcing materials such as abaca, sugar cane, wood pulp, waste paper, waste paper and wool, and plate-like or granular reinforcing materials such as glass flakes, non-swelling mica, graphite, metal foil, ceramic beads, clay, mica, sericite, zeolite, bentonite, dolomite, kaolin, finely powdered silicic acid, feldspar powder, potassium titanate, silicic balloons, calcium carbonate, magnesium carbonate, barium sulfate, calcium oxide, aluminum oxide, titanium oxide, titanium dioxide, aluminum silicate, gypsum, novaculite, dawsonite and white clay. These fillers may be coated or bundled with a thermoplastic resin such as an ethylene-vinyl acetate copolymer or a thermosetting resin such as an epoxy resin, or may be treated with a coupling agent such as aminosilane and epoxysilane. The content of the other filler is preferably 10 parts by mass or more, and more preferably 20 parts by mass or more, per 100 parts by mass of the synthetic resin component in the full compound, and is preferably 60 parts by mass or less, and more preferably 50 parts by mass or less.
[0063] The material composition may contain a crystal nucleating agent. As the crystal nucleating agent, any of those generally used as crystal nucleating agents for polyolefin resins can be used as appropriate, such as inorganic crystal nucleating agents and organic crystal nucleating agents.
[0064] Specific examples of inorganic crystal nucleating agents include kaolinite, synthetic mica, clay, zeolite, graphite, carbon black, magnesium oxide, titanium oxide, calcium sulfide, boron nitride, calcium carbonate, barium sulfate, aluminum oxide, neodymium oxide, and metal salts such as phenylphosphonate, etc. These inorganic crystal nucleating agents may be modified with an organic substance in order to enhance dispersibility in the composition.
[0065] Specific examples of organic crystal nucleating agents include sodium benzoate, potassium benzoate, lithium benzoate, calcium benzoate, magnesium benzoate, barium benzoate, lithium terephthalate, sodium terephthalate, potassium terephthalate, calcium oxalate, sodium laurate, potassium laurate, sodium myristate, potassium myristate, calcium myristate, sodium octacosanoate, calcium octacosanoate, sodium stearate, potassium stearate, lithium stearate, calcium stearate, magnesium stearate, barium stearate, sodium montanate, calcium montanate, sodium toluate, sodium salicylate, potassium salicylate, salicylic acid Examples of the organic carboxylic acid metal salts include zinc, aluminum dibenzoate, potassium dibenzoate, lithium dibenzoate, sodium β-naphthalate, and sodium cyclohexanecarboxylate; organic sulfonates such as sodium p-toluenesulfonate and sodium sulfoisophthalate; carboxylic acid amides such as stearic acid amide, ethylene bislauric acid amide, palmitic acid amide, hydroxystearic acid amide, erucic acid amide, and trimesic acid tris(t-butylamide); benzylidene sorbitol and derivatives thereof; phosphorus compound metal salts such as sodium 2,2'-methylenebis(4,6-di-t-butylphenyl)phosphate; and sodium 2,2-methylbis(4,6-di-t-butylphenyl).
[0066] The material composition may contain a plasticizer. As the plasticizer, any plasticizer generally used for polyolefin resins may be appropriately used, such as polyester-based plasticizers, glycerin-based plasticizers, polyvalent carboxylate-based plasticizers, polyalkylene glycol-based plasticizers, and epoxy-based plasticizers. These plasticizers may be used alone or in combination of two or more.
[0067] Specific examples of polyester-based plasticizers include polyesters composed of an acid component such as adipic acid, sebacic acid, terephthalic acid, isophthalic acid, naphthalenedicarboxylic acid, diphenyldicarboxylic acid, or rosin, and a diol component such as propylene glycol, 1,3-butanediol, 1,4-butanediol, 1,6-hexanediol, ethylene glycol, or diethylene glycol, or polyesters composed of hydroxycarboxylic acids such as polycaprolactone, etc. These polyesters may be end-capped with a monofunctional carboxylic acid or a monofunctional alcohol, or may be end-capped with an epoxy compound or the like.
[0068] Specific examples of the glycerin-based plasticizer include glycerin monoacetomonolaurate, glycerin diacetomonolaurate, glycerin monoacetomonostearate, glycerin diacetomonooleate, and glycerin monoacetomonomonoacetate.
[0069] Specific examples of polyvalent carboxylate ester plasticizers include phthalates such as dimethyl phthalate, diethyl phthalate, dibutyl phthalate, dioctyl phthalate, diheptyl phthalate, dibenzyl phthalate, and butyl benzyl phthalate; trimellitates such as tributyl trimellitate, trioctyl trimellitate, and trihexyl trimellitate; adipic esters such as diisodecyl adipate, n-octyl-n-decyl adipate, methyl diglycol butyl diglycol adipate, benzyl methyl diglycol adipate, and benzyl butyl diglycol adipate; citric esters such as triethyl acetyl citrate and tributyl acetyl citrate; azelaic esters such as di-2-ethylhexyl azelaate; and sebacate esters such as dibutyl sebacate and di-2-ethylhexyl sebacate.
[0070] Specific examples of polyalkylene glycol plasticizers include polyalkylene glycols such as polyethylene glycol, polypropylene glycol, poly(ethylene oxide-propylene oxide) block and / or random copolymers, polytetramethylene glycol, ethylene oxide addition polymers of bisphenols, propylene oxide addition polymers of bisphenols, and tetrahydrofuran addition polymers of bisphenols, as well as end-blocking compounds such as terminal epoxy-modified compounds, terminal ester-modified compounds, and terminal ether-modified compounds.
[0071] Epoxy plasticizers generally refer to epoxy triglycerides made from alkyl epoxy stearates and soybean oil, but other types of plasticizers, such as epoxy resins made mainly from bisphenol A and epichlorohydrin, can also be used.
[0072] Specific examples of other plasticizers include benzoic acid esters of aliphatic polyols such as neopentyl glycol dibenzoate, diethylene glycol dibenzoate, and triethylene glycol di-2-ethyl butyrate, fatty acid amides such as stearic acid amide, aliphatic carboxylic acid esters such as butyl oleate, oxyacid esters such as methyl acetylricinoleate and butyl acetylricinoleate, pentaerythritol, various sorbitols, polyacrylic acid esters, and paraffins.
[0073] The material composition may contain a fluorine-containing drip-preventing agent. Examples of the fluorine-containing drip-preventing agent include fluorine-containing polymers having fibril-forming ability. Examples of such fluorine-containing polymers include polytetrafluoroethylene (hereinafter also referred to as "PTFE"), tetrafluoroethylene copolymers (e.g., tetrafluoroethylene / hexafluoropropylene copolymers), partially fluorinated polymers as shown in U.S. Pat. No. 4,379,910, and polycarbonate resins produced from fluorinated diphenols. Among these, PTFE is preferred.
[0074] PTFE having fibril-forming ability has an extremely high molecular weight, and shows a tendency to bond PTFE to each other and become fibrous by external action such as shear force. Its molecular weight is preferably 1 million or more, more preferably 2 million or more, in terms of number average molecular weight calculated from standard specific gravity, and is preferably 10 million or less, more preferably 9 million or less. PTFE having fibril-forming ability can be used in the form of an aqueous dispersion in addition to a solid form.
[0075] Examples of commercially available PTFE products having fibril-forming ability include Teflon (registered trademark) 6J manufactured by DuPont-Mitsui Fluorochemicals Co., Ltd., and Polyflon (registered trademark) MPA FA500 and F-201L manufactured by Daikin Industries, Ltd. Examples of commercially available aqueous dispersions of PTFE include Fluon (registered trademark of AGC Corporation) AD-939E manufactured by Asahi ICI Fluoropolymers Co., Ltd., Fluon D-310 and D-210C manufactured by Daikin Industries, Ltd., and Teflon 31JR manufactured by DuPont-Mitsui Fluorochemicals Co., Ltd.
[0076] In order to improve the dispersibility of the fibril-forming PTFE in the full compound and obtain better flame retardancy, mechanical properties, and flexural modulus, it is also possible to use a PTFE mixture in the form of a mixture of the fibril-forming PTFE and other resins. The proportion of PTFE to the total mass of the PTFE mixture is preferably 1% by mass or more, more preferably 5% by mass or more, while it is preferably 60% by mass or less, more preferably 55% by mass or less. When the proportion of PTFE is within this range, good dispersibility of PTFE can be achieved.
[0077] The PTFE mixture can be prepared, for example, by a method of: (1) mixing an aqueous dispersion of PTFE with an aqueous dispersion or solution of another resin and co-precipitating to obtain a co-agglomerated mixture (methods described in JP-A-60-258263, JP-A-63-154744, etc.); (2) mixing an aqueous dispersion of PTFE with dried particles of another resin (method described in JP-A-4-272957); or (3) uniformly mixing an aqueous dispersion of PTFE with a solution of another resin and simultaneously extracting each medium from the mixture. (4) a method of polymerizing a monomer that forms another resin in an aqueous dispersion of PTFE (method described in JP-A-06-220210, JP-A-08-188653, etc.), or (5) a method of uniformly mixing an aqueous dispersion of PTFE with a dispersion of another resin, polymerizing a vinyl monomer in the resulting mixed dispersion, and then obtaining a mixture (method described in JP-A-11-29679, etc.). Commercially available PTFE mixtures include "Metablen (registered trademark) A3000" from Mitsubishi Chemical Corporation and "BLENDEX (registered trademark of Galata Chemicals) B449" from GE Specialty Chemicals.
[0078] The content of the fluorine-containing drip prevention agent is preferably 0.01 parts by mass or more, more preferably 0.05 parts by mass or more, and even more preferably 0.1 parts by mass or more, in terms of the amount of PTFE per 100 parts by mass of the full compound, while it is preferably 1 part by mass or less, more preferably 0.8 parts by mass or less, and even more preferably 0.5 parts by mass or less.
[0079] The material composition may be a collection of the above-mentioned materials, a mixture of the above-mentioned materials, or a melt-kneaded product of the above-mentioned materials. That is, the material composition may be a master batch of the above-mentioned other components with the matrix resin as a dispersion medium.
[0080] [Major effects] The resin composition contains 50% by mass or more of the phosphorus-based flame retardant (B) in a well-dispersed state in the resin composition. Since the resin composition contains a high concentration of the phosphorus-based flame retardant in a well-dispersed state, it can be suitably used as a master batch of the flame retardant in the full compound of a resin product, and it is possible to further increase the degree of freedom of the material composition other than the flame retardant in the full compound.
[0081] When used as a masterbatch, the above-mentioned resin composition is capable of exhibiting excellent flame retardancy in a full compound while adequately maintaining the inherent physical properties (e.g., mechanical strength and flexural modulus) of the matrix resin, as described in Patent Document 1.
[0082] Furthermore, when the resin composition is used as a master batch to produce a resin product, the mechanical properties (flexural strength) of the resin product can be improved while maintaining high flame retardancy. Although the mechanism behind this is not clear, it is believed that the specific acid-modified polyolefin resin (C) improves the dispersibility of the phosphorus-based flame retardant (B) in the resin composition.
[0083] 〔summary〕 As is clear from the above description, the resin composition of the first aspect of the present invention contains a thermoplastic resin (A), a phosphorus-based flame retardant (B), and an acid-modified polyolefin resin (C), and the acid-modified polyolefin resin (C) has an acid value of 70 mgKOH / g or less, a weight average molecular weight of 1,000 to 300,000, and a proportion of the phosphorus-based flame retardant (B) of 50 mass% or more. Since the first aspect can be suitably used for a masterbatch for flame retardants, the first aspect realizes a resin composition suitable for increasing the degree of freedom in the composition of flame-retardant resin products.
[0084] The resin composition according to the second aspect of the present invention is the resin composition according to the first aspect, wherein the acid-modified polyolefin resin (C) is an unsaturated carboxylic acid-grafted olefin polymer. The second aspect is more effective from the viewpoint of increasing the degree of freedom and improving the mechanical properties of the resin product.
[0085] The resin composition according to the third aspect of the present invention is the resin composition according to the first or second aspect, in which the proportion of the phosphorus-based flame retardant (B) is 70 mass% or more. The third aspect is even more effective from the viewpoint of increasing the degree of freedom and improving the mechanical properties of the resin product.
[0086] The resin composition of the fourth aspect of the present invention is any one of the first to third aspects, in which the proportion of the acid-modified polyolefin resin (C) is 10 mass% or less. The fourth aspect is more effective from the viewpoint of increasing the degree of freedom and improving mechanical properties of the resin product.
[0087] The resin composition of the fifth aspect of the present invention is any one of the first to fourth aspects, in which the ratio of the acid-modified polyolefin resin (C) to the phosphorus-based flame retardant (B) is 15 mass% or less. Since the ratio of the phosphorus-based flame retardant (B) is relatively increased in the fifth aspect, it is more effective from the viewpoint of increasing the degree of freedom and improving mechanical properties of the resin product.
[0088] The method for producing a resin product according to the sixth aspect of the present invention comprises the steps of: diluting the resin composition according to any one of the first to fifth aspects with a material composition; molding the product resin composition to produce a resin product. In the sixth aspect, the resin composition according to the above aspect is used as a master batch for a flame retardant, and therefore, according to the sixth aspect, a method for producing a resin product suitable for increasing the degree of freedom in the composition of a flame-retardant resin product is realized.
[0089] A flame retardant masterbatch according to a seventh aspect of the present invention is a pellet of the resin composition according to any one of the first to fifth aspects. The seventh aspect is even more effective in terms of improving the handling properties during use.
[0090] According to the present invention, it is possible to design and manufacture highly flame-retardant resin products with a high degree of freedom. Since the present invention enables the replacement of metal products with lighter resin products, it is expected to contribute to the achievement of, for example, Goal 9 on laying the foundations for industry and technological innovation in the Sustainable Development Goals (SDGs) advocated by the United Nations.
[0091] The present invention is not limited to the above-described embodiments, and various modifications are possible within the scope of the claims. Embodiments obtained by appropriately combining the technical means disclosed in the different embodiments are also included in the technical scope of the present invention. EXAMPLES
[0092] The present invention will be specifically described below with reference to examples. However, the present invention is not limited to the following examples. In the following examples, % is by mass unless otherwise specified. The following items were evaluated.
[0093] (1) Flame retardant (UL94) The resulting molded products (1 / 16-inch test bars) were used to determine flame retardancy through a vertical flame test in accordance with the UL94 standard. "Total burning time" is the total flaming burning time during the burning test. "Maximum burning time" is the maximum burning time per test specimen. "Judgment" is a grade determined by the UL94 standard, which is specified by (1) the burning time of each test specimen after exposure to flame, (2) the total burning time of five specimens, (3) the position at which each test specimen reaches flame, (4) ignition due to dripping, and (5) red heat after the second exposure to flame.
[0094] (2) Flame retardancy (combustion heat generation) (cone calorimeter) The obtained molded body (100 mm x 100 mm x 3 mm test piece) was subjected to radiant heat of 50 kW / m using a Toyo Seiki Co., Ltd. Model: C3 Cone Calorimeter III in accordance with ISO 5660-1 (2002). 2 Maximum heat output (kW / m 2 ), total heat output (MJ / m 2 ), average heat release rate (kW / m2 "Mass after test" refers to the mass of the sample after the test, and "sample remaining rate" refers to the ratio of the sample weight after the test to the sample weight before the test.
[0095] (3) Bending properties The obtained molded product (JIS K7139-A1 dumbbell test piece) was cut to a length of 80 mm, and the bending strength (MPa) was measured in accordance with JIS K7171. The test speed was 2 mm / min.
[0096] The following materials were used as raw materials.
[0097] <Thermoplastic resin (A)> A-1: Polypropylene resin (manufactured by Japan Polypropylene Corporation, "Novatec (registered trademark) SA06GA", melt mass flow rate 60 g / 10 min). A-2: PP compound containing long glass fiber (GF) (manufactured by Japan Polypropylene Corporation, "Funcster (registered trademark) LR24A", (GF = 40%)). A-3: Polypropylene resin (manufactured by Japan Polypropylene Corporation, "Novatec (registered trademark) BC05B", melt mass flow rate 50 g / 10 min).
[0098] <Phosphorus-based flame retardants (B)> Phosphorus-based flame retardant composition (ADEKA CORPORATION, "ADEKA STAB (registered trademark) FP-2500S", containing 50 to 60% piperadine pyrophosphate, 35 to 45% melamine pyrophosphate, and 3 to 6% zinc oxide based on the total mass of the phosphorus-based flame retardant composition).
[0099] <Acid-modified polyolefin (PO) resin (C)> C-1: Maleic anhydride grafted polypropylene resin (acid value 52 mg KOH / g, weight average molecular weight 30,000). C-2: Maleic anhydride grafted polyethylene resin (acid value 3 mg KOH / g, weight average molecular weight 216,000). C-3: Maleic anhydride grafted polyethylene resin (acid value 60 mg KOH / g, weight average molecular weight 1,500).
[0100] Test 1 Example 1 The following components were blended in the amounts shown below and mixed by hand blending. Then, using a φ30 mm co-rotating twin screw extruder (model name "BT-30", manufactured by Plastics Engineering Research Institute Co., Ltd., L / D=30), the mixture was melt-kneaded at a screw rotation speed of 250 rpm and a cylinder temperature of 200°C to obtain a pellet-shaped resin composition 1. Here, "L / D" indicates the ratio of the screw length (L) to the screw diameter (D). Phosphorus-based flame retardant (B) 60% Acid-modified polyolefin resin (C-1) 3.5% Thermoplastic resin (A) A-1 Remainder
[0101] Next, the following components were mixed in the following amounts by hand blending. The resulting mixture was then injection molded using a fully electric injection molding machine "SE100DU" (Sumitomo Heavy Industries, Ltd.) under conditions of a cylinder temperature of 180 to 200°C (180-190-200-200-200°C) and a mold temperature of 80°C to obtain test piece A, which is the aforementioned 1 / 16 inch combustion rod (125 x 13 x 1.6 mm). Test piece A is referred to as resin product 1. Thermoplastic resin (A) A-2 50.0% Thermoplastic resin (A) A-1 8.0% Resin composition 1 42.0%
[0102] Example 2 Resin composition 2 was obtained in the same manner as resin composition 1, except that acid-modified polyolefin resin (C-2) was used instead of acid-modified polyolefin resin (C-1). In addition, test piece A was obtained in the same manner as resin product 1, except that 42.0% of resin composition 2 was used instead of 42.0% of resin composition 1. Test piece A is referred to as resin product 2.
[0103] Example 3 Resin composition 3 was obtained in the same manner as resin composition 1, except that acid-modified polyolefin resin (C-2) was used instead of acid-modified polyolefin resin (C-1). In addition, test piece A was obtained in the same manner as resin product 1, except that 42.0% of resin composition 3 was used instead of 42.0% of resin composition 1. Test piece A is referred to as resin product 3.
[0104] Comparative Example 1 Resin composition 6 was obtained in the same manner as resin composition 1, except that the amount of phosphorus-based flame retardant (B) was changed to 50.0%, thermoplastic resin (A-3) was used instead of thermoplastic resin (A-1), and no acid-modified polyolefin resin was used. In addition, test piece A was obtained in the same manner as resin product 1, except that 50.0% of resin composition 6 was used instead of 42.0% of resin composition 1, and no thermoplastic resin (A-1) was used. Test piece A is referred to as resin product C1.
[0105] The composition of the materials and the MFR measurement results of Resin Compositions 1 to 3 and 6 are shown in Table 1. Table 2 shows the compounding ratios during the production of Resin Products 1 to 3 and C1, and the proportions of each component after production.
[0106] The above-mentioned flame retardancy evaluation of resin products 1 to 3 and C1 was carried out using the above-mentioned test piece A. The results are shown in Table 2.
[0107] [Table 1]
[0108] [Table 2]
[0109] Test 2 Example 4 Thermoplastic resin (A) A-1 50.0% Resin composition 1 50.0% The above components were mixed in the above amounts by hand blending, and injection molded using a fully electric injection molding machine "SE100DU" (Sumitomo Heavy Industries, Ltd.) under conditions of a cylinder temperature of 180 to 200 ° C (180-190-200-200-200 ° C) and a mold temperature of 80 ° C to prepare a JIS K7139-A1 dumbbell test piece. The obtained JIS K7139-A1 dumbbell test piece was cut to a length of 80 mm to obtain test piece B (80 × 10 × 4 mm). The obtained test piece B is referred to as resin product 4.
[0110] Example 5 A test piece B was obtained by producing in the same manner as for the resin product 4, except that the resin composition 2 was used in an amount of 50.0% instead of the resin composition 1. The obtained test piece B is designated as a resin product 5.
[0111] Example 6 A test piece B was obtained by producing in the same manner as for the resin product 4, except that the resin composition 3 was used in an amount of 50.0% instead of the resin composition 1. The obtained test piece B is designated as a resin product 6.
[0112] Comparative Example 2 A test piece B was obtained by producing in the same manner as the resin product 4, except that a 60.0% amount of the resin composition 6 was used instead of the resin composition 1, and the amount of the thermoplastic resin (A-1) was 40.0%. The obtained test piece B is referred to as a resin product C2.
[0113] The bending properties of resin products 4 to 6 and C2 were evaluated using the above-mentioned test piece B. Table 3 shows the composition of the resin product materials and the measurement results.
[0114] [Table 3]
[0115] Test 3 Example 7 Thermoplastic resin (A) A-1 67.0% Resin composition 1 33.0% The above components were mixed in the above amounts by hand blending, and the resulting mixture was injection molded using a fully electric injection molding machine "SE100DU" (Sumitomo Heavy Industries, Ltd.) under conditions of a cylinder temperature of 180 to 200°C (180-190-200-200-200°C) and a mold temperature of 80°C to obtain a test piece C that was a test piece of 100 mm x 100 mm x 3 mm. The obtained test piece C is referred to as resin product 7.
[0116] Example 8 A test piece C was obtained by producing in the same manner as for resin product 7, except that resin composition 2 in an amount of 33.0% was used instead of resin composition 1. The obtained test piece C is designated as resin product 8.
[0117] Example 9 A test piece C was obtained by producing in the same manner as for resin product 7, except that resin composition 3 in an amount of 33.0% was used instead of resin composition 1. The obtained test piece C is designated as resin product 9.
[0118] Example 10 Resin composition 4 was obtained in the same manner as resin composition 1, except that the amount of phosphorus-based flame retardant (B) was changed to 70.0%, and acid-modified polyolefin resin (C-3) was used instead of acid-modified polyolefin resin (C-1). The material composition and MFR measurement results of resin composition 4 are shown in Table 1. In addition, test piece C was obtained in the same manner as resin product 7, except that the amount of thermoplastic resin (A) A-1 was changed to 71.0%, and 29.0% of resin composition 4 was used instead of resin composition 1. The obtained test piece C is referred to as resin product 10.
[0119] Example 11 Resin composition 5 was obtained in the same manner as resin composition 1, except that the amount of phosphorus-based flame retardant (B) was changed to 75.0%, and acid-modified polyolefin resin (C-3) was used instead of acid-modified polyolefin resin (C-1). The material composition and MFR measurement results of resin composition 5 are shown in Table 1. In addition, test piece C was obtained in the same manner as resin product 7, except that the amount of thermoplastic resin (A) A-1 was changed to 73.0%, and 27.0% of resin composition 5 was used instead of resin composition 1. The obtained test piece C is referred to as resin product 11.
[0120] Comparative Example 3 A test piece C was obtained by producing in the same manner as the resin product 7, except that 40.0% of the resin composition 6 was used instead of the resin composition 1, and the amount of the thermoplastic resin (A-1) was 60.0%. The obtained test piece C is referred to as a resin product C3.
[0121] Cone calorimeter evaluation was performed on resin products 7 to 11 and C3 using the above-mentioned test piece C. Table 4 shows the composition of the resin product materials and the measurement results.
[0122] [Table 4]
[0123] [Consideration] As shown in Table 2, resin products 1 to 3 obtained using resin compositions 1 to 3 have excellent flame retardancy equivalent to V-0 of the UL94 standard. Also, as shown in Table 4, resin products 7 to 11 obtained using resin compositions 1 to 5 have a sample residual rate of 30% or more by a cone calorimeter, and have excellent flame retardant properties. Also, resin compositions 1 to 5 have a high content ratio of phosphorus-based flame retardant. Therefore, for example, when resin compositions 1 to 5 are used as a flame retardant master batch, the amount of master batch required to achieve a desired flame retardant concentration in a diluted resin product can be reduced. This increases the degree of freedom in the composition of the resin product, and it is possible to obtain a resin product with a composition ratio that was not previously possible.
[0124] Furthermore, as shown in Table 3, resin products 4 to 6 obtained using resin compositions 1 to 3 have excellent bending strength. This shows that the resin compositions obtained using resin compositions 1 to 3 as masterbatches have excellent mechanical strength (see Table 3). The reason for this is unclear at this stage, but it is believed that the phosphorus-based flame retardant (B) is well dispersed by containing the specific acid-modified polyolefin (C). From the above, it can be seen that the mechanical strength of a resin product can be further increased by using a resin composition containing the phosphorus-based flame retardant (B) and the specific acid-modified polyolefin (C) as a masterbatch. [Industrial Applicability]
[0125] The present invention can be utilized for producing resin products having high flame retardancy and high degree of freedom in composition.
Claims
1. The present invention comprises a thermoplastic resin (A), a phosphorus-based flame retardant (B), and an acid-modified polyolefin resin (C), The acid-modified polyolefin resin (C) has an acid value of 70 mgKOH / g or less and a weight average molecular weight of 1,000 or more and 300,000 or less, The resin composition, wherein the proportion of the phosphorus-based flame retardant (B) is 50 mass% or more.
2. The resin composition according to claim 1, wherein the acid-modified polyolefin resin (C) is an unsaturated carboxylic acid-grafted olefin polymer.
3. The resin composition according to claim 1 , wherein the proportion of the phosphorus-based flame retardant (B) is 70 mass % or more.
4. The resin composition according to claim 1 , wherein the proportion of the acid-modified polyolefin resin (C) is 10 mass % or less.
5. The resin composition according to claim 1, wherein a ratio of the acid-modified polyolefin resin (C) to the phosphorus-based flame retardant (B) is 15 mass % or less.
6. A method for producing a resin product, comprising molding a product resin composition obtained by diluting the resin composition according to any one of claims 1 to 5 with a material composition to produce a resin product.
7. A flame retardant masterbatch, which is a pellet of the resin composition according to any one of claims 1 to 5.
Citation Information
Patent Citations
Flame-retardant resin composition and molded article using the same
JP2015151459A
Rosin-based resin, compatibilizer, resin composition and molding
JP2023056496A
Polyolefin-based resin composition
WO2011158906A1
Resin composition and molded body
WO2021241682A1