Metal oxynitride film
Low-temperature epitaxial growth of metal oxynitride films using controlled nitrogen gas flow and substrate temperatures addresses the stability and reliability issues of amorphous films, enhancing their performance in semiconductor devices.
Patent Information
- Application Number
- JP2024123599
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2018-07-06
- Filing Date
- 2024-07-30
- Publication Date
- 2024-11-22
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing metal oxynitride films used in semiconductor devices are amorphous, have low stability, and require high-temperature treatments for epitaxial growth, which limits their application and reliability.
A method for epitaxially growing metal oxynitride films at low temperatures using a sputtering process with controlled nitrogen gas flow and specific substrate temperatures, eliminating the need for high-temperature treatments.
The method enables the formation of highly crystalline, in-plane oriented metal oxynitride films suitable for semiconductor devices, improving their stability and reliability without the constraints of high-temperature processes.
Smart Images

Figure 2024163913000001_ABST
Abstract
Description
[Technical field]
[0001] One embodiment of the present invention relates to a metal oxynitride film and a method for forming the metal oxynitride film. One embodiment of the present invention is a light-emitting element, a lighting device, a display device, an electronic device, or the like, which uses the metal oxynitride film. The present invention relates to a semiconductor device.
[0002] In this specification and the like, a semiconductor device refers to a device that can function by utilizing semiconductor characteristics. This refers to semiconductor devices in general, including semiconductor elements such as transistors, semiconductor circuits, arithmetic units, and memory devices. The device is one aspect of a semiconductor device. device, lighting device, electro-optical device, power storage device, storage device, semiconductor circuit, imaging device, electronic device etc. may be said to have a semiconductor device.
[0003] Note that one embodiment of the present invention is not limited to the above technical fields. One aspect of the present invention relates to an object, a method, or a manufacturing method. , process, machine, manufacture, or composition of matter (-) [Background technology]
[0004] Metal oxynitrides, which contain metal, oxygen, and nitrogen, are known as pigments and photocatalyst materials. Metal oxynitrides are also attracting attention as semiconductor materials and insulating materials for use in semiconductor devices. In Patent Document 1, a metal oxynitride containing indium, gallium, and zinc is A semiconductor material having the following structure is disclosed:
[0005] In addition, one method for forming a thin film with in-plane orientation (also called a single crystal thin film) is the use of an electron microscope. The epitaxial growth method is known. Here, the in-plane orientation is the horizontal orientation with respect to the substrate. This refers to the regularity of the crystal orientation. In Patent Document 2, a single crystal InGaO3(ZnO)5 thin film is A method for forming the layer by reactive solid phase epitaxy is disclosed. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2015-18929 A [Patent Document 2] JP 2004-103957 A Summary of the Invention [Problem to be solved by the invention]
[0007] The state of the metal oxynitride disclosed in Patent Document 1 is an amorphous state in which the bonds between atoms are disordered. Amorphous metal oxynitrides have voids or low density regions. However, the stability of the metal oxynitride is low. Therefore, the metal oxynitride used in the semiconductor device, etc. It is preferable that the metal oxynitride has high crystallinity. In particular, it is preferable that the metal oxynitride has an in-plane orientation. I wish.
[0008] In addition, in the reactive solid phase epitaxial method disclosed in Patent Document 2, InGaO3( Before the deposition of the ZnO thin film, the substrate is heated to 1000°C or higher. After the deposition, high-temperature treatment such as thermal diffusion treatment at a temperature of 1300° C. or higher is required. In addition, to form a single crystal InGaO3(ZnO)5 thin film, an epitaxial growth was performed on the substrate. Thus, it is necessary to provide a ZnO thin film grown by epitaxy using conventional techniques. There are various constraints on the formation of thin films grown at high temperatures. For example, a low temperature refers to a temperature of 700°C or higher, and a low temperature refers to a temperature of 600°C or lower.
[0009] Therefore, one aspect of the present invention is to form a metal oxynitride film by epitaxial growth at a low temperature. Another object of the present invention is to provide a method for forming a metal oxynitride film. The metal oxynitride film is formed by epitaxial growth without performing high temperature treatment before or after the film formation. Another object of the present invention is to provide a method for epitaxial growth. One of the objects of the present invention is to provide a semiconductor device or the like using a metal oxynitride film formed by .
[0010] The description of these problems does not preclude the existence of other problems. It is not necessary for one embodiment to solve all of these problems. The subject matter will be self-evident from the description, drawings, claims, etc. Other issues can be extracted from the drawings, claims, etc. [Means for solving the problem]
[0011] In one embodiment of the present invention, a gas containing nitrogen gas is introduced onto a single crystal substrate to form an oxide target. The metal oxynitride film is epitaxially grown by sputtering using a The method includes the steps of: forming a metal oxynitride film on a substrate; forming a metal oxynitride film on the substrate; and depositing the metal oxynitride film on the substrate. The temperature is 80°C or higher and 400°C or lower, and the flow rate of nitrogen gas is 50% or higher and 10% or lower of the total flow rate of gas. It is less than 0%.
[0012] In addition, one embodiment of the present invention is a method for producing an oxide film by introducing a gas containing nitrogen gas onto a single crystal substrate. Metal oxynitride is a method of forming a film with in-plane orientation by sputtering using a target. A method for producing a metal oxynitride film, comprising: The temperature of the substrate is between 80°C and 400°C, and the flow rate of nitrogen gas is less than 50% of the total flow rate of gas. The top is less than 100%.
[0013] In the above-mentioned method for producing a metal oxynitride film, the oxide target is made of indium and gallium. It is preferable that the compound contains at least one of the following:
[0014] In the above method for producing a metal oxynitride film, the substrate is made of yttria-stabilized zirconia (YS Z) substrate, and the surface orientation of the substrate is (111). It is preferable that the substrate is an A-plane sapphire substrate, and the surface orientation of the substrate is (110).
[0015] In the above-mentioned method for producing a metal oxynitride film, the crystal structure of the metal oxynitride film is a wurtzite structure. It is preferable that the structure is a
[0016] In the method for producing the metal oxynitride film, a pole measurement is performed on the metal oxynitride film. When this was done, the pole measurement was performed by scanning the φ of the (101) plane of the crystal of the metal oxynitride film. It is preferable that a diffraction peak exhibiting six-fold symmetry is observed.
[0017] In the above-mentioned method for producing a metal oxynitride film, a wide-area reciprocal space map of the metal oxynitride film is In the sample, a first spot and a second spot are observed, and the peak of the first spot is The angle 2θ is 30° or more and 35° or less, and the angle ψ is located near 0°, and the first spot The half-width of the first spot is less than 2°, and the peak of the second spot is between 33° and 37°. .degree. or less, and the angle .psi. is located in the range of 61.degree. to 65.degree., and the half width of the second spot is 2. It is preferable that the angle is less than 100°. Effect of the Invention
[0018] According to one aspect of the present invention, a method for forming a metal oxynitride film by epitaxial growth at low temperature is provided. According to one embodiment of the present invention, a method for forming a metal oxynitride film can be provided. The metal oxynitride film is formed by epitaxial growth without high temperature treatment. According to one aspect of the present invention, a film formed by epitaxial growth can be provided. It is possible to provide a semiconductor device using the metal oxynitride film.
[0019] The description of these effects does not preclude the existence of other effects. An embodiment does not necessarily have all of these effects. Effects other than these are described in the specification. The above will become apparent from the description, drawings, claims, etc. From the above description, it is possible to extract other effects. [Brief description of the drawings]
[0020] [Figure 1] Fig. 1(A) is a diagram illustrating a metal oxynitride film epitaxially grown on a substrate. Fig. 1(B) is a diagram illustrating the crystal planes of the crystals in the metal oxynitride film. Fig. 1(C) is a diagram illustrating the atomic arrangement of the crystals. [Diagram 2] FIG. 2 is a diagram for explaining the range of the atomic ratio of metals constituting the oxide target. [Diagram 3] 3(A) and 3(B) are schematic diagrams illustrating a sputtering apparatus. [Figure 4]Figure 4 shows the experimental setup for wide-area reciprocal space mapping and pole measurements. [Diagram 5] Fig. 5(A) is a diagram for explaining a pole figure, and Fig. 5(B) and Fig. 5(C) are diagrams for explaining the intensity distribution obtained by pole measurement. [Figure 6] 6(A) and 6(B) are diagrams showing configuration examples of a light-emitting element. [Figure 7] 7(A) and 7(B) are diagrams illustrating a lighting device according to one embodiment of the present invention. [Figure 8] 8A to 8C are diagrams showing configuration examples of a display device. [Figure 9] 9A to 9E are diagrams showing configuration examples of electronic devices. [Figure 10] Fig. 10(A) is a diagram showing a wide-area reciprocal space map of Sample 1 of the embodiment, Fig. 10(B) and Fig. 10(C) are diagrams showing wide-area reciprocal space maps obtained by simulation. [Figure 11] 11(A) and 11(B) are diagrams showing the results of pole measurement for Sample 1 of the embodiment. [Figure 12] Fig. 12(A) is a diagram showing a wide-area reciprocal space map of Sample 2 of the embodiment, Fig. 12(B) and Fig. 12(C) are diagrams showing wide-area reciprocal space maps obtained by simulation. [Figure 13] 13(A) and 13(B) are diagrams showing the results of pole measurement for Sample 2 of the embodiment. [Figure 14] Fig. 14(A) is a diagram showing a wide-area reciprocal space map of Example Sample 3. Fig. 14(B) and Fig. 14(C) are diagrams showing wide-area reciprocal space maps obtained by simulation. [Figure 15] 15(A) and 15(B) are diagrams showing the results of pole measurement for Sample 3 of the embodiment. [Figure 16] Fig. 16(A) is a diagram showing a wide-area reciprocal space map of Example Sample 4. Fig. 16(B) and Fig. 16(C) are diagrams showing wide-area reciprocal space maps obtained by simulation. [Figure 17] 17(A) and 17(B) are diagrams showing the results of pole measurement for Sample 4 of the embodiment. [Figure 18] Fig. 18(A) is a diagram showing a wide-area reciprocal space map of Example Sample 5. Fig. 18(B) and Fig. 18(C) are diagrams showing wide-area reciprocal space maps obtained by simulation. [Figure 19] 19(A) and 19(B) are diagrams showing the results of pole measurement for Sample 5 of the embodiment. [Figure 20] Fig. 20(A) is a diagram showing a wide-area reciprocal space map of Example Sample 6. Fig. 20(B) and Fig. 20(C) are diagrams showing wide-area reciprocal space maps obtained by simulation. [Figure 21] 21(A) and 21(B) are diagrams showing the results of pole measurement for Sample 6 of the embodiment. [Figure 22] Fig. 22(A) is a diagram showing a wide-area reciprocal space map of Example Sample 7. Fig. 22(B) and Fig. 22(C) are diagrams showing wide-area reciprocal space maps obtained by simulation. [Figure 23] 23(A) and 23(B) are diagrams showing the results of pole measurement for Sample 7 of the embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0021] Hereinafter, the embodiments will be described with reference to the drawings. It is understood that the present invention can be practiced in many different ways without departing from the spirit and scope of the present invention. It will be readily understood by those skilled in the art that various changes in form and detail may be made. Therefore, the present invention should not be construed as being limited to the description of the following embodiment modes.
[0022] In the drawings, the size, layer thickness, or area may be exaggerated for clarity. Therefore, the drawings are not necessarily limited to the scale. The examples are shown in schematic form, and are not limited to the shapes or values shown in the drawings. For example, In the actual manufacturing process, layers and resist masks are damaged by etching and other processes. However, in order to make it easier to understand, this is not reflected in the diagram. In the drawings, the same parts or parts having similar functions are designated by the same reference numerals in different drawings. In addition, when referring to similar functions, In such cases, the hatch patterns may be the same and no particular reference numbers may be used.
[0023] In addition, the invention is easily understood, particularly in top views (also called "plan views") and perspective views. In order to simplify the description, some of the components may be omitted. The above information may be omitted.
[0024] In addition, in this specification, the terms "above" and "below" that indicate an arrangement are used to refer to the relationship between components. The positional relationship is used for convenience in describing the drawings. The relationship changes accordingly depending on the direction in which each configuration is depicted. The terms are not limited to those described above, and may be rephrased appropriately depending on the situation.
[0025] For example, in the present specification, it is explicitly stated that X and Y are connected. The cases are when X and Y are electrically connected and when X and Y are functionally connected. The case where X and Y are directly connected and the case where X and Y are directly connected are disclosed in the present specification, etc. Therefore, the connection relationship is limited to a specific one, for example, the connection relationship shown in the figure or text. Connections other than those shown in the drawings or text are also disclosed in the drawings or text. Here, X and Y are objects (e.g., devices, elements, circuits, wiring, electrodes, terminals, etc.). , conductive film, layer, etc.).
[0026] In this specification, a transistor includes a gate, a drain, and a source. The drain terminal is a diode that has at least three terminals. Between the drain region or drain electrode and the source (source terminal, source region or source electrode) The channel forming region is formed in the channel. A current can be passed between the source and drain via the channel forming region. In this specification and the like, the channel formation region refers to a region through which current mainly flows.
[0027] In addition, the functions of the source and drain may differ depending on whether transistors of different polarities are used or the circuit In operation, when the direction of the current changes, the positions may be reversed. In the specification, the terms source and drain may be used interchangeably. do.
[0028] In addition, in this specification, the term "insulator" may be replaced with "insulating film" or "insulating layer." In addition, the term "conductor" can be replaced with "conductive film" or "conductive layer." In addition, the term "semiconductor" can be replaced with "semiconductor film" or "semiconductor layer." can.
[0029] In addition, in this specification, "parallel" means that two straight lines are at an angle of -10° or more and 10° or less. Therefore, it includes the case where the angle is between -5° and 5°. "Almost parallel" means that the two straight lines are arranged at an angle of -30° to 30°. "Perpendicular" means that two straight lines are arranged at an angle of 80° to 100°. Therefore, it includes the case where the angle is between 85° and 95°. " refers to a state in which two straight lines are arranged at an angle of 60° or more and 120° or less.
[0030] In this specification, crystal planes are expressed using Miller indices. The direction of the crystal plane arrangement (perpendicular to the crystal plane) is expressed as the bond. This is called the crystal orientation. The crystal orientation is indicated by three integers in square brackets. For example, to indicate a crystal face, (111) and
[0111] when expressing the crystal orientation. -The notation called the Miller-Bravais index is sometimes used. Specifically, the plane index of the hexagonal crystal lattice is expressed as (h kil), where i = -(h + k). The index i is calculated from the values of the index h and the index k. Therefore, in this specification, mirror indexes using three integers are also used for hexagonal crystal planes. It is expressed in numbers (hkl).
[0031] In this specification, the crystal plane appearing on the surface of the single crystal substrate is called the plane orientation of the single crystal substrate. There are cases.
[0032] In this specification, the lattice points in the reciprocal lattice (also called reciprocal lattice points) corresponding to the crystal planes are referred to as For example, the spots observed in the large-area reciprocal space map are The reciprocal lattice point 111 shown corresponds to the crystal plane (111).
[0033] In addition, in the Miller index, when a negative direction is indicated, a bar is placed above the number representing the index. In this specification, for convenience, a minus sign is placed before the number representing the exponent. Equivalent planes include (-111), (1-11), (11-1), etc. In this case, if you write (111), (111) can be expressed as (-111), (1-11), ( 11-1) may also include equivalent aspects.
[0034] (Embodiment 1) In this embodiment, a method for forming a metal oxynitride film according to one embodiment of the present invention will be described. .
[0035] Metal oxynitrides, which contain metal, oxygen, and nitrogen, are used as semiconductor materials and insulating materials in semiconductor devices. Metal oxynitrides used in semiconductor devices have few impurities and defects. Here, the term "high stability" for a metal oxynitride means that the metal oxynitride is a semiconductor. The metal oxynitride is unlikely to react with materials in contact with it due to heat generated by the operation of the device. The crystallinity of the metal oxynitride does not change, and the metal oxynitride is less likely to have defects. By using metal oxynitrides, which have few impurities and defects and are highly stable, in semiconductor devices, The reliability of the semiconductor device can be improved.
[0036] Impurities in a metal oxynitride refer to, for example, anything other than the main component constituting the metal oxynitride. For example, in metal oxynitrides, elements with a concentration of less than 0.1 atomic percent can be considered impurities. The elements include, for example, hydrogen, silicon, boron, phosphorus, carbon, and metal oxynitrides. There are transition metals other than the main component. Also, the defects in metal oxynitrides are lattice defects. For example, there are point defects such as oxygen vacancies and nitrogen vacancies, line defects such as dislocations, and crystal grain boundaries. Defects in metal oxynitrides include void defects such as cavities.
[0037] In addition, from the viewpoint of crystallinity, thin films are classified into in-plane oriented thin films, oriented thin films, and non-oriented thin films (multiple Crystalline thin film, non-crystalline thin film, amorphous thin film, etc. Oriented thin film is a thin film that is A thin film is a film in which at least one crystal axis of the crystal is aligned in a specific direction. In addition, in-plane oriented thin films are thin films in which the three crystal axes of the crystals contained in the thin film are aligned in a specific direction. It is a thin film in a well-ordered state.
[0038] The thin film of metal oxynitride used in semiconductor devices is a thin film of metal oxynitride with orientation. It is preferable that the thin film be an in-plane oriented metal oxynitride thin film. The thin film of the inwardly oriented metal oxynitride has few impurities and defects and has a dense structure. Therefore, by using a thin film of a metal oxynitride having an in-plane orientation in a semiconductor device, the semiconductor device can be This can improve the reliability of the equipment.
[0039] Epitaxial growth is known as a method for forming a thin film with in-plane orientation. In the case of single crystal growth, the crystals that make up the thin film are grown on a single crystal substrate with a certain crystal orientation relationship. It is also possible to grow a single crystal substrate by using the same material as the substrate. The growth of a crystal with the same lattice constant as the crystal that has the same structure is called homoepitaxial growth. In addition, a material different from the substrate is used on the single crystal substrate, or a material different from the substrate is used. The growth of a crystal using a material with a lattice constant different from that of the crystal being grown is called heteroepitaxial. Heteroepitaxial growth is a process where the lattice mismatch with the substrate crystal is small. A layer that relieves lattice distortion (also called a buffer layer) is provided between the substrate and the thin film. This is possible by, for example,
[0040] The epitaxial growth method includes solid phase epitaxial growth (SPE). Liquid Phase Epitaxial Growth (LPE) method Vapor Phase Epitaxial Growth (VPE) There is the Epitaxy method.
[0041] In the SPE method, a thin film is formed on the surface of a substrate, and the thin film is heated by irradiating it with an electron beam or the like. This is a method to change the crystal structure of the thin film to the same crystal structure as the substrate. The PE method is a method in which crystals are precipitated on the substrate surface from a supersaturated solution. VPE is a method of depositing components in the gas phase onto a substrate surface. (PLD:Pulsed Laser Deposition) method, atomic layer deposition (ALD) method :Atomic Layer Deposition) method, molecular beam epitaxial growth ( There are methods such as the Molecular Beam Epitaxy (MBE) method. In an ultra-high vacuum, the elements that make up the target crystal or materials that contain the elements are heated and evaporated. This is a method of depositing crystals on a substrate.
[0042] In the prior art, there are various limitations to epitaxially growing thin films. For example, the thin film is formed at a high temperature, and after the thin film is formed, the thin film is heated at a high temperature (for example, 10 Heat treatment is performed at a temperature of 00°C or higher. Prior to forming the thin film, the substrate surface is flattened. Place one or more buffer layers on the substrate, select a substrate with a similar lattice constant and thermal expansion coefficient, etc. As a method for flattening the substrate surface, for example, a heat treatment is performed on the substrate at a high temperature. etc.
[0043] Therefore, one aspect of the present invention is a method for epitaxially growing a metal oxynitride film at a low temperature. The method for producing an oxynitride film is specifically described as follows. A gas is introduced into the substrate to epitaxially grow a metal oxynitride film by sputtering. In one embodiment of the present invention, the method is to grow the epitaxially to obtain an in-plane orientation. Since this method is a method for forming a film that is epitaxially grown by this method, the film has an in-plane It is an oriented film.
[0044] The crystal structure of the epitaxially grown metal oxynitride film is a hexagonal crystal structure. Of the hexagonal crystal structures, the wurtzite structure is particularly preferred. The wurtzite structure is a cubic crystal structure (e.g., diamond structure, fluorite structure, zinc blende structure). For example, the cubic crystal
[0111] and the wurtzite structure
[0001] have a crystal orientation relationship that allows epitaxial growth. Therefore, the metal oxynitride film having a hexagonal crystal structure can be formed by cubic, hexagonal, etc. Which crystal structure can be easily grown epitaxially on a single crystal substrate? In addition, a material having a crystal structure such as a cubic system or a hexagonal system is etched onto the metal oxynitride film. This makes it easier to achieve epitaxial growth.
[0045] As the substrate for the single crystal, a sapphire substrate, a stabilized zirconia substrate (yttria stabilized Insulating substrates such as zirconia (YSZ) substrates can be used. Metal oxynitrides When the crystal structure is a wurtzite structure, the substrate may be, for example, a substrate having a surface orientation of (111) Alternatively, a YSZ substrate having a (110) surface orientation or an A-plane sapphire substrate having a (110) surface orientation may be used. By using a YSZ substrate or an A-plane sapphire substrate as the substrate, It is easy to form a thin film of metal oxynitride with a crystal of a mineral structure and an in-plane orientation. Silicon, germanium, silicon carbide, gallium nitride, gallium arsenide, indium phosphide Alternatively, a semiconductor substrate made of zinc oxide may be used.
[0046] The difference between the lattice constant of the epitaxially grown thin film and the lattice constant of the substrate (lattice The smaller the lattice mismatch, the better. By reducing the lattice mismatch, the single crystal substrate can be Furthermore, it is possible to facilitate epitaxial growth of thin films.
[0047] One method for evaluating the degree of lattice mismatch is the lattice mismatch ratio. Δa is the lattice constant a of the epitaxially grown thin film crystal e and the lattice constant a of the substrate crystal s This is calculated using the following formula (1).
[0048]
number
[0049] The lattice mismatch between the epitaxially grown metal oxynitride film and the single crystal substrate is 15 % or less, and more preferably 10% or less. This makes it easier to grow the nitride film epitaxially.
[0050] In addition, a metal oxynitride film having a wurtzite crystal structure is formed on a cubic single crystal substrate. In the case of epitaxial growth, for example, the crystal orientation of the substrate surface is
[0111] , The crystal orientation of the metal oxynitride film surface is
[0001] . The crystal orientation of the metal oxide film is different. s The lattice constant of the crystal of the substrate is divided by two The degree of lattice mismatch can be calculated by multiplying the value by two. When a YSZ substrate with a lattice constant of about 0.51 nm in the a-axis direction is used as the crystal substrate, When the YSZ substrate is viewed from the
[0111] direction, the minimum distance between nearest neighbor atoms is approximately 0. Therefore, in consideration of the above-mentioned preferable range of the lattice mismatch, the metal oxynitride The lattice constant of the film crystal in the a-axis direction is preferably 0.31 nm or more and 0.41 nm or less. More preferably, it is greater than or equal to 0.32 nm and less than or equal to 0.40 nm.
[0051] A schematic diagram of a structure including a metal oxynitride film epitaxially grown on a single crystal substrate is shown in FIG. FIG. 1A shows a metal oxynitride film 20 formed on a single crystal substrate 10. FIG. 1(A) is a schematic diagram of a structure in which a metal oxynitride film 20 has a wurtzite structure. The figure shows a case where the wurtzite crystal 30 is formed by the manufacturing method according to one embodiment of the present invention. The c-axis (0001) direction of the crystal 30 of the type structure coincides with the normal direction of the surface of the single crystal substrate 10. In this manner, the metal oxynitride film 20 grows epitaxially. The epitaxially grown film produced by this method is aligned along the c-axis (
[0001] ) direction of the crystals contained in the film. Since the direction of the epitaxial layer coincides with the normal direction of the single crystal substrate surface, the epitaxial layer can be formed by the method according to one embodiment of the present invention. A film grown in a c-axis direction is sometimes called a c-axis epitaxial film.
[0052] The crystal plane of the wurtzite structure will be explained using FIG. 1(B). The typical crystal faces ((001) and (101)) of the ruthenium-type structure are shown in Fig. 1(B). ) is a plane parallel to the surface of the single crystal substrate 10.
[0053] FIG. 1(C) shows the atomic arrangement in the wurtzite structure. The arrangement X1 in FIG. 1(C) is Configuration X1 is the configuration of a metal atom, and configuration X2 is the configuration of an oxygen atom or a nitrogen atom. Configuration X1 may be the configuration of an oxygen atom or a nitrogen atom, and configuration X2 may be the configuration of a metal atom.
[0054] The sputtering target used in the above sputtering method is a zinc-containing oxide target. It is preferable that the alloy is a tantalum alloy, which is made of at least one of indium and gallium, and zinc. It is more preferable that the oxide target contains the following oxide. , zinc oxide target, indium zinc oxide (In-Zn oxide) target, gallium Indium gallium zinc oxide (Ga-Zn oxide) target, Indium gallium zinc oxide (In- In particular, the oxide target may be a Ga-Zn oxide target. Indium gallium zinc oxide targets are used as the target material. The crystal structures of gallium oxide and zinc oxide are both wurtzite structures. By forming a film using a metal target, it is possible to obtain a metal film with a wurtzite structure and in-plane orientation. This makes it easier to form a thin oxynitride film.
[0055] With reference to FIG. 2, the preferable range of the atomic ratio of the metals constituting the oxide target will be described. FIG. 2 shows the indium, gallium, and zinc oxide contained in the oxide target. It should be noted that FIG. 2 does not show the atomic ratio of oxygen. In addition, the atomic ratio of indium, gallium, and zinc contained in the oxide target is The respective terms are [In], [Ga], and [Zn].
[0056] In FIG. 2, the dashed line indicates [In]:[Ga]:[Zn]=(1+α):(1-α):1 The atomic ratio (α is a real number between -1 and 1) of [In]:[Ga]:[Zn] = (1+α):(1-α):2 atomic ratio line, [In]:[Ga]:[Zn] =(1+α):(1-α):3 atomic ratio line, and [In]:[Ga]:[ This represents the line where the atomic ratio of Zn is (1+α):(1-α):4.
[0057] The dashed line indicates the atomic ratio of [In]:[Ga]:[Zn]=4:1:β (β is zero). The line where the atomic ratio of [In]:[Ga]:[Zn]=2:1:β is The line where the atomic ratio of [In]:[Ga]:[Zn]=1:1:β is ]:[Ga]:[Zn]=1:2:β atomic ratio line, and [In]:[Ga This represents the line where the atomic ratio of Zn:β is 1:4:β.
[0058] Region A shown in FIG. 2 is the region of indium, gallium, and zinc contained in the oxide target. The figure shows an example of a preferable range of the atomic ratio of lead. In region A, [In]:[Ga ]:[Zn]=4:2:4.1, and [In]:[Ga]:[Zn]=1:1:1. n-Ga-Zn oxide target, [In]:[Ga]:[Zn]=2:0:1 ([In ]:[Zn]=2:1) and In-Zn oxide targets with [In]:[Ga]: A zinc oxide target with [Zn] = 0:0:1 is included.
[0059] The sputtering target used in the above sputtering method is an oxide target. The oxynitride target is not limited to the above, and may be an oxynitride target. Indium gallium zinc oxynitride (In-Ga-Zn oxynitride) target, Indium gallium Indium oxynitride (In-Ga oxynitride) target, Indium zinc oxynitride (In-Zn oxynitride) A target such as a nitride target can be used.
[0060] The substrate temperature during the formation of the metal oxynitride film is set to be equal to or higher than room temperature (25° C.) and equal to or lower than 500° C. It is preferable that the temperature is 80° C. or higher and 400° C. or lower, and more preferable that the temperature is 100° C. or higher and 250° C. or lower. It is more preferable that the temperature is 500°C or less. The productivity of semiconductor devices and the like using the metal oxynitride film can be improved.
[0061] A gas containing nitrogen gas is introduced into the reaction chamber during the deposition of the metal oxynitride film. For example, the gas is preferably nitrogen gas or a mixture of nitrogen gas and oxygen gas. It is preferable to use a mixed gas of nitrogen gas and a rare gas (argon, helium, etc.). Here, the flow rate of the nitrogen gas is preferably 50% or more and 100% or less of the total flow rate of the gas. By adjusting the flow rate ratio of the nitrogen gas to the flow rate of the gas, the obtained metal oxide The composition of the nitride film can be adjusted.
[0062] By the above-mentioned manufacturing method, a metal oxynitride film can be formed without providing a buffer layer between the substrate and the thin film. It can be grown epitaxially.
[0063] <Sputtering equipment> Next, referring to FIG. 3(A) and FIG. 3(B), the metal oxynitride film according to one embodiment of the present invention will be described. A sputtering apparatus for the manufacturing method will be described. FIG. 3(B) is a cross-sectional view illustrating a film forming chamber 41 of the sputtering apparatus. 1 is a plan view of a magnet unit 54a and a magnet unit 54b.
[0064] The deposition chamber 41 shown in FIG. 3(A) includes a target holder 52a and a target holder 52b. , backing plate 50a, backing plate 50b, and sputtering target The substrate 70a, the sputtering target 70b, the member 58, and the substrate holder 62 are The sputtering target 70a is disposed on the backing plate 50a. In addition, the backing plate 50a is disposed on the target holder 52a. The magnet unit 54a is connected to the backing plate 50a via the sputtering The sputtering target 70b is disposed under the target 70a. The backing plate 50b is disposed on the target holder 50b. The magnet unit 54b is disposed on the backing plate 50. The sputtering target 70b is disposed below the sputtering target 70b via the gap b.
[0065] As shown in FIG. 3(A) and FIG. 3(B), the magnet unit 54a is a magnet. A magnet 54N1, a magnet 54N2, a magnet 54S, a magnet holder 56, In the magnet unit 54a, the magnet 54N1, the magnet The magnet 54N2 and the magnet 54S are disposed on a magnet holder 56. The net 54N1 and the magnet 54N2 are spaced apart from the magnet 54S. The magnet unit 54b has a similar structure to the magnet unit 54a. When the substrate 60 is carried into the film forming chamber 41, the substrate 60 is placed in contact with the substrate holder 62. It will be placed.
[0066] Sputtering target 70a, backing plate 50a and target holder 52a, sputtering target 70b, backing plate 50b and target The holder 52b is separated from the holder 52 by a member 58. The member 58 is an insulating material. However, the member 58 may be a conductor or a semiconductor. The material 58 may be a conductor or semiconductor whose surface is covered with an insulator.
[0067] The target holder 52a and the backing plate 50a are fixed together using screws (bolts, etc.). The target holder 52a is fixed to the backing plate 52b, and is equipotential. The sputtering target 70a is supported by the support 50a. The get holder 52b and the backing plate 50b are fixed together using screws (bolts, etc.). The target holder 52b is attached to the backing plate 50. b serves to support the sputtering target 70b.
[0068] The backing plate 50a has a function of fixing the sputtering target 70a. The backing plate 50b also serves to fix the sputtering target 70b. Possesses the ability.
[0069] In FIG. 3A, magnetic field lines 64a formed by the magnet unit 54a, and magnetic field lines 64b are clearly shown.
[0070] As shown in FIG. 3B, the magnet unit 54a has a rectangular or substantially rectangular shape. a magnet 54N1 of rectangular or approximately rectangular shape, and a magnet 54N2 of rectangular or approximately rectangular shape. The magnet 54S is fixed to a magnet holder 56. Then, the magnet unit 54a is swung left and right as shown by the arrow in FIG. For example, the magnet unit 54a can be set to a frequency of 0.1 Hz to 1 kHz. Vibration with a beat (which can also be called rhythm, beat, pulse, frequency, period, cycle, etc.) Just move it.
[0071] The magnetic field above the sputtering target 70a is increased with the oscillation of the magnet unit 54a. The area with a strong magnetic field becomes a high-density plasma area, and the plasma in the vicinity The sputtering phenomenon of the sputtering target 70a is likely to occur. The same is true for knit 54b.
[0072] In addition, in FIG. 3(A) and FIG. 3(B), an example using a parallel plate type sputtering device is shown. However, the method for forming a metal oxynitride film according to the present embodiment is not limited to this. For example, a metal oxynitride film is formed using a facing target type sputtering device. It may be coated.
[0073] The sputtering method allows for film formation at low temperatures, so it is suitable for the production of semiconductors using the metal oxynitride film. The productivity of semiconductor devices and the like can be improved.
[0074] According to one aspect of the present invention, a method for forming a metal oxynitride film by epitaxial growth at low temperature is provided. According to one embodiment of the present invention, a method for forming a metal oxynitride film can be provided. The metal oxynitride film is formed by epitaxial growth without high temperature treatment. According to one aspect of the present invention, a film formed by epitaxial growth can be provided. A semiconductor device using the metal oxynitride film can be provided. In this manner, the productivity of semiconductor devices and the like using a metal oxynitride film can be improved.
[0075] <Method for evaluating the crystallinity and orientation of thin films> Epitaxial growth can be evaluated during or after thin film deposition, depending on the evaluation method. It can be done.
[0076] As a method for evaluating epitaxial growth during thin film formation, for example, reflected high-energy electron beam Diffraction (RHEED: Reflection High Energy Electron Diffraction), Surface Photoabsorption (SPA) orption) etc.
[0077] In addition, the epitaxial growth (crystallinity and orientation) of the thin film was observed using a transmission electron microscope. Mirror (TEM: Transmission Electron Microscope), Reciprocal space mapping in the X-ray diffraction (XRD) method Wide-angle Reciprocal Space Mapping (WRSM) cal Space Mapping), pole measurement, out-of-plane measurement, It can be evaluated in combination with n-plane measurements.
[0078] The following describes the measurement methods that can be used to evaluate the crystallinity and orientation of thin films. Reveal.
[0079] <Wide-area reciprocal space mapping> Global reciprocal space mapping will now be described.
[0080] Reciprocal space is constructed by the fundamental vectors of reciprocal space (also called reciprocal vectors). The periodicity of the real space is reflected in the reciprocal lattice vector b j Is a real sky Lattice fundamental vector a i and are related by the following formula (2). In formula (2), δ i ,j is the Kronecker delta. That is, the plane defined in the crystal in real space is Treat it as a lattice point in a lattice.
[0081]
number
[0082] The epitaxially grown thin film has a small variation in the crystal orientation of the crystals that compose the thin film. Therefore, the reciprocal lattice space matrix is used for the epitaxially grown thin film. When a spot is acquired, the observed spot intensity is high and the spot width at half maximum is small. On the other hand, for thin films with a large variation in the crystal orientation, i.e., low orientation, the reciprocal lattice When a spatial map is acquired, the observed spots have low intensity and large half-widths. From the above, it is possible to evaluate the crystallinity and orientation of a thin film by obtaining a reciprocal lattice space map. It can be valued.
[0083] Using FIG. 4, we will explain wide-area reciprocal space mapping using an X-ray analysis device. As shown in FIG. 4, the X-ray analysis device is viewed from above, with the X-ray source, the sample The direction in which the X-ray tube, the sample, and the detector are aligned is called the ψ axis. When the analyzer is viewed from above, the direction perpendicular to the ψ axis is the θ axis. The direction perpendicular to the axis is the φ axis. In other words, the φ axis is the direction in which the X-ray analysis device is viewed from above. In addition, the axis referred to as the ψ axis in this specification may be referred to as the χ axis depending on the device. Therefore, the ψ axis can also be called the χ axis. Similarly, in this specification, the θ axis is In some devices, the axis is called the ω axis. Therefore, the θ axis is called the ω axis. It is also possible.
[0084] In wide-area reciprocal space mapping, a two-dimensional detector is used. The detector shown in FIG. 4 has position information in the 2θ and ψ directions on the detection surface. The ctor is modeled after a two-dimensional detector.
[0085] As shown in Fig. 4, the wide-area reciprocal space mapping is performed with a fixed X-ray source. If the sample is to be detected, this is done by activating the sample and the detector. Here, the detector can be tilted in the 2θ direction, and the sample can be The sample can be tilted in the θ, φ, and ψ directions. While tilting the sample stepwise in the ψ direction, 2θ / θ scanning was performed at each ψ position (angle). This allows the measurement to cover a wide range in reciprocal space. It is possible to obtain a wide-area reciprocal space map. In this case, the wide-area reciprocal space mapping is performed by using the X-ray source, the sample and the detector. The X-ray source is driven in the θ direction. In addition, unless otherwise specified, in this specification, the X-ray source is a C Uses uKα radiation (wavelength: 0.15418 nm).
[0086] In order to analyze the intensity distribution appearing in the wide-area reciprocal space map obtained above, Simulation of lattice space map. Simulation of wide area reciprocal space map. For example, the software "SMAP / for Cr" provided by Bruker Japan The software "oss Sectional XRD-RSM" can be used. By inputting the parameters of the crystal structure, lattice constant, and orientation, the corresponding The wide-area reciprocal space map output by the simulation is By comparing the molecular space map with the large-area reciprocal space map obtained by measurement, The intensity distribution appearing in the large-area reciprocal space map obtained by this method can be analyzed.
[0087] When the crystal structure of the metal oxynitride film is a wurtzite structure oriented in (001), the metal In the wide-area reciprocal space map of the oxynitride film, the reciprocal lattice points 002, 101, etc. Here, the peak of the spot corresponding to the reciprocal lattice point 002 is at an angle It is preferable that 2θ is 30° or more and 35° or less, and the angle ψ is located near 0°. The peak of the spot corresponding to the reciprocal lattice point 101 has an angle 2θ of 33° or more and 37° or less. In addition, it is preferable that the angle ψ is located at 61° or more and 65° or less. The half-width of the spot corresponding to the reciprocal lattice point 101 is preferably less than 2°. As a result, the metal oxynitride film is aligned in the c-axis direction of the crystals contained in the metal oxynitride film and in the single crystal This is one of the indicators for determining whether epitaxial growth has occurred so that the normal direction of the substrate surface coincides with that of the It can be said that:
[0088] <Potential measurement> In pole measurement, the position (angle) of the X-ray source and detector is kept constant while the sample is rotated in any direction. This is a method to measure the distribution of diffraction intensity by rotating the detector. In this specification, a two-dimensional detector is used. The angle (2θ) was fixed, and the sample was tilted in the θ and ψ directions. φ direction) to measure lattice planes tilted in all directions. Diffraction obtained by pole measurement The strength of the thin film can be used to evaluate the crystallinity and orientation of the thin film. The detector is not limited to a two-dimensional detector, but may be a zero-dimensional detector.
[0089] The diffraction intensity obtained by the pole measurement will be explained with reference to Figs. 5(A) to 5(C). The diffraction intensity obtained by the pole measurement is expressed as a pole figure. Figure 5(A) shows a pole figure. As shown in Figure 5(A), the center P0 of the polar figure has an angle ψ of 0°, and the circumference P1 has an angle ψ of 90°. Also, from the center P0 of the polar figure to the outer periphery P1 of the polar figure, The straight line extending straight up (shown by the dashed line P0-P2 in Figure 5(A)) has an angle φ 0°, and the line extending from the center P0 of the polar figure to the periphery P1 of the polar figure The angle between the point P0 and the point P3 (shown by the dashed line in FIG. 5A) is the angle φ. In FIG. 5(A), the angle φ is shown to increase when the rotation is counterclockwise. However, this is not limited to this, and depending on the device, the angle φ may become large when rotated clockwise. Also, depending on the range of the ψ scan, the polar figure obtained by the pole measurement may be larger. The angle may not be acquired in the range of 0° to 90°.
[0090] 5(B) and 5(C) show schematic diagrams of the diffraction intensity obtained by pole measurement. In B), a spot-like intensity distribution is observed on concentric circles of angle ψ (circles indicated by dashed lines in the figure). FIG. 5(C) is a schematic diagram of the diffraction intensity when a ring-shaped intensity distribution is observed. FIG. 2 is a schematic diagram of the diffraction intensity when
[0091] For example, the (101) plane of the wurtzite structure has six-fold symmetry. When a pole measurement was performed on a c-axis epitaxial film having a crystal structure, the results shown in Figure 5(B) were As shown in the figure, there are six spot-like intensity distributions (diffraction peaks) on concentric circles at an angle ψ. Therefore, a thin film with a wurtzite crystal structure grows epitaxially along the c-axis. In this case, the φ scan of the (101) plane of the thin film crystal in the pole measurement shows six-fold symmetry. Specifically, a diffraction peak is observed on a concentric circle with an angle ψ of about 62°. Diffraction peaks are observed approximately every 60°.
[0092] On the other hand, when pole measurements are performed on a thin film that is not epitaxially grown, as shown in Figure 5(C), A ring-shaped intensity distribution as shown in Fig. 1 is observed, or no diffraction peak is observed. Therefore, by analyzing the intensity distribution observed in the pole figure measurement, it is possible to evaluate whether the thin film is epitaxially grown.
[0093] In the φ scan of the pole figure measurement with respect to the (111) plane of a single-crystalline YSZ substrate, diffraction peaks showing three-fold symmetry are observed. Specifically, diffraction peaks are observed at intervals of approximately 120° with respect to the angle φ on a concentric circle where the angle ψ is approximately 70°. Also, in the φ scan of the pole figure measurement with respect to the (104) plane of a single-crystalline A-plane sapphire substrate, diffraction peaks showing two-fold symmetry are observed. Specifically, diffraction peaks are observed at intervals of approximately 180° with respect to the angle φ on a concentric circle where the angle ψ is approximately 58°.
[0094] <Out-of-plane measurement and In-plane measurement> In the measurement using the XRD method, there are Out-of-plane measurement and In-plane measurement. The Out-of-plane measurement is a method for evaluating a crystal plane parallel to the surface of the thin film, and the In-plane measurement is a method for evaluating a crystal plane perpendicular to the surface of the thin film. In the Out-of-plane measurement and In-plane measurement, a 0-dimensional detector may be used as the detector.
[0095] As described above, the configurations, methods, etc. shown in the present embodiment can be used in appropriate combination with the configurations, methods, etc. shown in other embodiments and examples.
[0096] (Embodiment 2) In the present embodiment, the use of the epitaxially grown metal oxynitride film shown in the previous embodiment will be described.
[0097] The metal oxynitride film can be used in, for example, light-emitting devices, light-receiving devices, and semiconductor devices. In particular, it can be used for light-emitting elements (also called light-emitting diodes or LEDs).
[0098] 6(A) and 6(B) are used to explain a configuration example of a light-emitting device using the above-mentioned metal oxynitride film. In this embodiment, a light emitting element having a double heterojunction will be described. However, one embodiment of the present invention is not limited thereto, and a light-emitting element having a quantum well junction will be described. A child is also fine.
[0099] 6(A) and 6(B) show a light-emitting element using a metal oxynitride film according to one embodiment of the present invention. As shown in FIG. 6(A) and FIG. 6(B), the light emitting element 100 is a 02, an n-type cladding layer 104, an active layer 106, a p-type cladding layer 108, and an n-type The semiconductor device has a first electrode 110 and a p-type electrode 112 .
[0100] The active layer 106 is sandwiched between an n-type cladding layer 104 and a p-type cladding layer 108. In the active layer 106, electrons and holes combine to emit light. The n-type cladding layer 104, the active layer 106, and the p-type cladding layer 108 are The laminated structure including the doped layer 108 is formed to emit light of red, yellow, green, blue, etc. For example, the laminated structure may include gallium phosphide, gallium arsenide, gallium arsenide, Aluminum-aluminum-arsenide, Aluminum-gallium-indium-phosphide, Ga The following compounds can be used: gallium nitride, indium-gallium nitride compounds, selenium-zinc compounds, etc. can.
[0101] The atomic ratio of metals constituting the metal oxynitride film according to one embodiment of the present invention, By appropriately selecting the flow rate of the nitrogen gas to be introduced, the conductivity (or It is possible to adjust the insulating property, band gap, light transmittance, etc. The higher the gas flow rate, the higher the conductivity of the film tends to be. The nitride film can be formed into an n-type crystalline silicon film shown in FIG. 6(A) by adjusting the conductivity of the metal oxynitride film. It can be used for the lath layer 104 or the n-type electrode 110 shown in FIG. 6(B).
[0102] The metal oxynitride film is used as the n-type electrode 110 and the n-type clad layer shown in FIG. The metal oxynitride film may be used for the n-type electrode 110 and the n-type electrode 112 shown in FIG. When the metal oxynitride film is used for the n-type cladding layer 104, the flow rate of nitrogen gas is adjusted. By forming the n-type electrode 110 and the n-type cladding layer 104 shown in FIG. The above films can be formed continuously.
[0103] Furthermore, the metal oxynitride film is a barrier for epitaxially growing a thin film on the film. Therefore, the n-type metal oxide nitride film formed on the metal oxide nitride film can function as a buffer layer. The crystallinity of the cladding layer 104 or the active layer 106 can be improved. The crystal structure of the nitride film is hexagonal, and in particular, is a wurtzite crystal structure. The n-type cladding layer 104 or the active layer 106 formed on the metal oxynitride film contains gallium. Materials that form the wurtzite crystal structure, such as indium nitride and indium gallium nitride compounds, It is preferable to use
[0104] From the above, the metal oxynitride film is useful as a base (buffer layer) for hexagonal crystal growth. The metal oxide has a function as an n-type electrode or an n-type clad layer. By using a nitride film for the n-type electrode 110 or the n-type cladding layer 104, The n-type cladding layer 104 or the active layer 106 can be easily epitaxially grown. 4 or the crystallinity of the active layer 106 is increased. The characteristics of the material can be improved.
[0105] This embodiment mode can be appropriately combined with other embodiment modes and examples.
[0106] (Embodiment 3) In this embodiment, an example in which the light-emitting element of one embodiment of the present invention is applied to various lighting devices will be described. 7A and 7B are used to explain the structure of the light-emitting element according to one embodiment of the present invention. This makes it possible to manufacture a highly reliable lighting device with good luminous efficiency.
[0107] FIG. 7(A) shows an example of using a light-emitting element as an indoor lighting device. By this, a large-area lighting device 8501 and a lighting device 8502 having a curved surface are formed. Furthermore, a large lighting device 8503 may be installed on the wall of the room. A touch sensor is provided in the lighting device 8501, the lighting device 8502, and the lighting device 8503. , the power may be turned on or off.
[0108] In addition, by using light-emitting elements on the surface of the table, it can function as a table. The lighting device 8504 may be a light source that uses light emitting elements. This makes it possible to provide a lighting device that also functions as furniture.
[0109] In addition, a light-emitting device using a light-emitting element according to one embodiment of the present invention can be used for automobile lighting. For example, lighting can be installed on the dashboard, windshield, ceiling, etc. Cut.
[0110] FIG. 7B shows the appearance of the automobile 7900. The automobile 7900 includes a body 7901, wheels 7902, and a wheelbase 7903. 902, a windshield 7903, lights 7904, fog lights 7905, etc. The light-emitting element of one embodiment of the present invention can be, for example, the light 7904 and the fog light shown in FIG. It can also be used for, for example, side indicators, It can be used as a back lamp, door courtesy lamp, etc.
[0111] In this manner, a lighting device can be obtained by using the light-emitting element of one embodiment of the present invention. The applicable lighting device is not limited to the one shown in this embodiment, but may be any lighting device in any field. It is possible to apply this to optical devices.
[0112] In addition, the structure shown in this embodiment mode may be appropriately combined with structures shown in other embodiment modes and examples. They can be used in combination.
[0113] (Embodiment 4) In this embodiment, a configuration example of a display device using the light-emitting element described in the above embodiment will be described. This will be described with reference to FIG. 8(A) to FIG. 8(C).
[0114] The display device of this embodiment has a function of displaying an image using light-emitting elements. In terms of form, in particular, the light-emitting element is a micro light-emitting diode (hereinafter also referred to as micro LED). An example of using the above formula (described below) will be described.
[0115] By using micro LEDs as display elements, it is possible to reduce the power consumption of display devices. It is also possible to reduce the thickness and weight of the display device. Display devices using EDs have high contrast and a wide viewing angle, which improves display quality. can be done.
[0116] The area of the light-emitting region of the micro LED is 1 mm 2 Less than 10000μ is preferable. m 2 Less than 3000μm is more preferable. 2 Less than 700μm is more preferable. 2 The following is further Preferred.
[0117] FIG. 8A shows a configuration example of a display device 400 using a light-emitting element. The display device 400 includes: The display device includes a pixel portion 401 , a driver circuit 402 , and a driver circuit 403 .
[0118] The pixel section 401 is composed of a plurality of pixels pix. The wiring GL is connected to the driver circuit 402. The wirings SL are connected to the driver circuits 403. A selection signal is supplied to the wirings GL. A video signal is supplied to the wiring SL.
[0119] The driver circuit 402 has a function of supplying a selection signal to the pixel pix. The circuit 402 has a function of supplying a selection signal to the wiring GL. The driver circuit 402 has a function of transmitting a selection signal output from the driver circuit 402 to the pixel pix. The gate side driving circuit can be called a gate driver, and the wiring GL is a selection signal line, a gate It can also be called a line.
[0120] The driver circuit 403 has a function of supplying a video signal to the pixel pix. The circuit 403 has a function of supplying a video signal to the wiring SL. The driver circuit 403 has a function of transmitting a video signal output from the pixel pix. The source side driving circuit can be called a source driver, and the wiring SL is a video signal line, a source It can also be called a line.
[0121] FIG. 8B shows a configuration example of a pixel pix using a light-emitting element as a display element. The pixel pix shown in FIG. 1 includes a transistor Tr31, a transistor Tr32, and a capacitance element C31. , and the light-emitting element LE. Although R32 is an n-channel type, the polarity of the transistor can be changed as appropriate. The light-emitting element described in the above embodiment can be used as the light-emitting element LE.
[0122] The gate of the transistor Tr31 is connected to the wiring GL, and either the source or the drain is The transistor Tr32 has a gate connected to one electrode of the capacitance element C31. The other of the source and drain of the transistor Tr32 is connected to the line SL. One of the drains is connected to the other electrode of the capacitance element C31 and one of the electrodes of the light emitting element LE. The other of the source and drain is connected to a wiring to which a potential Va is supplied. The other electrode of the optical element LE is connected to a wiring to which a potential Vc is supplied. Either the source or drain of Tr31, the gate of transistor Tr32, and the capacitance element The node connected to one electrode of the transistor C31 is called a node N31. One of the source and drain of Tr32, the other electrode of the capacitance element C31, and the light emitting element The node connected to one electrode of the LE is referred to as node N32.
[0123] Here, the case where the potential Va is the high power supply potential and the potential Vc is the low power supply potential will be explained. The potential Va and the potential Vc can be common to a plurality of pixels pix. The capacitance element C31 serves as a storage capacitance for storing the potential of the node N31. It has the following functions.
[0124] The transistor Tr31 has a function of controlling the supply of the potential of the wiring SL to the node N31. Specifically, the potential of the wiring GL is controlled to turn on the transistor Tr31. As a result, the potential of the line SL corresponding to the video signal is supplied to the node N31, and After that, the potential of the wiring GL is controlled to turn off the transistor Tr31. By setting the node N31 in this state, the potential of the node N31 is maintained.
[0125] The source of the transistor Tr32 is turned on and off in response to the voltage between the nodes N31 and N32. The amount of current flowing between the source and drain is controlled, and the light emitting element LE has a brightness according to the amount of current. This allows the gradation of the pixel pix to be controlled. It is preferable that transistor Tr32 be operated in the saturation region.
[0126] Here, the transistors Tr31 and Tr32 may be provided in the same layer. Alternatively, the transistors Tr31 and Tr32 may be provided in the same layer. By placing the transistors Tr31 and Tr32 at the same time, This allows the manufacturing process of the display device to be shortened. By stacking the transistor Tr32, the integration density of the display device can be increased. .
[0127] As shown in FIG. 8B, two transistors (Tr31 and However, one embodiment of the present invention is not limited to this. Alternatively, a pixel pix may have three or more transistors.
[0128] FIG. 8C shows a pixel pix using a light-emitting element as a display element, which is different from FIG. 8B. The pixel pix shown in FIG. r32, a transistor Tr33, a capacitance element C31, and a light-emitting element LE. 8C, the pixel pix shown in FIG. 8B is provided with a transistor Tr3 This pixel has a transistor Tr33 added to monitor the amount of current flowing through .
[0129] The gate of the transistor Tr31 is connected to the wiring GL, and either the source or the drain is The transistor Tr32 has a gate connected to one electrode of the capacitance element C31. The other of the source and drain of the transistor Tr32 is connected to the line SL. One of the drains is connected to the other electrode of the capacitance element C31, one electrode of the light emitting element LE, and the It is connected to either the source or drain of transistor Tr33. The other electrode of the light-emitting element LE is connected to a wiring to which a potential Va is supplied. The gate of transistor Tr33 is connected to the line GL. The other of the source and drain is connected to a monitor line ML. The source or drain of transistor Tr31, the gate of transistor Tr32, and the capacitance The node connected to one electrode of the element C31 is called a node N31. One of the source or drain of the transistor Tr32, the other electrode of the capacitance element C31, the light-emitting element LE and one of the source or drain of the transistor Tr33. The node is assumed to be node N32.
[0130] By performing the above operation for each wiring GL in sequence, the first frame of video is displayed. This can be done.
[0131] In addition, the wiring GL may be selected using either the progressive method or the interlace method. The supply of the video signal to the wiring SL may be performed by sequentially supplying the video signal to the wiring SL. Alternatively, a dot sequential drive may be used to simultaneously supply a video signal to all the wirings SL. Alternatively, a video signal may be supplied to each of the wirings SL in sequence. This is also fine.
[0132] After that, in the second frame period, the image is generated by the same operation as in the first frame period. As a result, the image displayed on the pixel portion 401 is rewritten.
[0133] The semiconductors used for the transistors in the pixels are silicon, germanium, Group 14 elements such as gallium arsenide, compound semiconductors such as gallium arsenide, organic semiconductors, metal oxides, etc. The semiconductor may be a non-single crystal semiconductor (amorphous semiconductor, microcrystalline semiconductor, etc.). The semiconductor may be a solid, polycrystalline semiconductor, or a single crystal semiconductor.
[0134] The transistor in the pixel pix has an amorphous semiconductor, particularly a hydrogenated It is preferable that the material contains amorphous silicon (a-Si:H). Transistors can be easily adapted to larger substrates, making them suitable for use in applications such as 4K2K broadcasting, To simplify the manufacturing process when producing large-screen display devices compatible with 8K4K broadcasting, etc. It is possible.
[0135] In addition, the transistor in the pixel pix has a transistor containing a metal oxide in a channel formation region. An OS transistor can also be used. Compared to transistors using amorphous silicon, the field effect mobility is higher. This eliminates the need for the crystallization process that is required for transistors using crystalline silicon.
[0136] In addition, since the off-state current of the OS transistor is extremely small, When using OS transistors, the pixel pix can hold a video signal for an extremely long period of time. This allows a period in which the image displayed on the pixel portion 401 does not change, or During periods when the change is below a certain level, the frequency of updating the video signal can be set extremely low. The video signal update frequency is, for example, less than once per 0.1 seconds, less than once per second, It can be set to once every 10 seconds or less. When a large number of pixels are provided corresponding to each other, the update of the video signal can be omitted. It is effective to reduce power consumption by using this method.
[0137] This embodiment mode can be appropriately combined with the descriptions of other embodiments and examples. .
[0138] (Embodiment 5) In this embodiment, an electronic device according to one embodiment of the present invention using the display device described in the above embodiment will be described. The following will explain this with reference to the drawings.
[0139] Examples of electronic devices include television sets, desktop or notebook computers, etc. Personal computers, computer monitors, digital signage, pachinko machines In addition to electronic devices with relatively large screens such as large game consoles, digital cameras, Digital video cameras, digital photo frames, mobile phones, portable game consoles, portable information Examples of such devices include information terminals, audio playback devices, etc.
[0140] The electronic device according to one embodiment of the present invention may include an antenna. By doing so, it is possible to display images, information, etc. on the display unit. The display unit can be called a display device. If the device has an antenna and a secondary battery, the antenna may be used for contactless power transmission. .
[0141] The electronic device according to one embodiment of the present invention includes a sensor (force, displacement, position, velocity, acceleration, angular velocity, rotation Numbers, distance, light, liquids, magnetism, temperature, chemicals, sound, time, hardness, electric field, current, voltage, power (including the ability to measure radiation, flow rate, humidity, gradient, vibration, odor or infrared rays) It may have.
[0142] The electronic device according to one embodiment of the present invention can have various functions. Functions for displaying still images, videos, text images, etc. on the display, touch panel function, calendar Functions such as displaying date or time, running various software (programs) a function to read out a program or data recorded on a recording medium; It can have functions etc.
[0143] FIG. 9A shows an example of a television device. A television device 7100 includes a housing 71. A display unit 7000 is built into the housing 71. This shows a configuration that supports 01.
[0144] The display device of one embodiment of the present invention can be applied to the display portion 7000.
[0145] The television device 7100 shown in FIG. 9A is operated by an operation switch provided in a housing 7101. This can be done by a touch panel or a separate remote control 7111. The display unit 7000 may be provided with a touch sensor, and the display unit 7000 may be touched with a finger, a stylus, or the like. The remote control unit 7111 may be operated by the following: The remote control 7111 may have a display unit for displaying information. The channel and volume can be controlled by the display unit 700 or the touch panel. You can control the image displayed on the screen.
[0146] The television device 7100 includes a receiver and a modem. The receiver can receive general television broadcasts. It can also receive wired or By connecting to a wireless communication network, It is also possible to communicate information in both directions (between sender and receiver, or between receivers, etc.).
[0147] FIG. 9B shows a notebook personal computer 7200. The computer 7200 includes a housing 7211, a keyboard 7212, a pointing device, The housing 7211 includes a display unit 7000 and an external connection port 7213. It is included.
[0148] The display device of one embodiment of the present invention can be applied to the display portion 7000.
[0149] Figures 9(C) and (D) show an example of digital signage.
[0150] The digital signage 7300 shown in FIG. 9C includes a housing 7301, a display unit 7000, a screen It also has an LED lamp, operation keys (power switch, or operation It may have a variety of functions, including a power switch, connection terminals, various sensors, a microphone, etc.
[0151] FIG. 9(D) shows a digital signage 7400 attached to a cylindrical pillar 7401. The digital signage 7400 is a display unit 7 provided along the curved surface of a pillar 7401. 000.
[0152] In FIG. 9C and FIG. 9D, the display device of one embodiment of the present invention is applied to the display portion 7000. It is possible.
[0153] The larger the display unit 7000, the more information can be displayed at one time. The wider the display unit 7000 is, the more easily it will catch people's attention, and the more effective it will be for advertising, for example. can.
[0154] By applying a touch panel to the display unit 7000, images or videos can be displayed on the display unit 7000. It is preferable because it not only displays information but also allows users to operate it intuitively. When used to provide information such as traffic information, the user can operate the device intuitively. This can improve accessibility.
[0155] Also, as shown in Figs. 9(C) and (D), the digital signage 7300 or the digital The signage 7400 is a display that is displayed on an information terminal 7311 such as a smartphone carried by a user. It is preferable that the display unit 7411 can be connected to the information terminal 7411 by wireless communication. The advertisement information displayed on the 7000 is displayed on the screen of the information terminal 7311 or the information terminal 7411. In addition, the information terminal 7311 or the information terminal 7411 can be operated. By operating the buttons, the display on the display unit 7000 can be switched.
[0156] In addition, the Digital Signage 7300 or Digital Signage 7400 can be equipped with an information terminal. A game is played using the screen of the information terminal 7311 or the information terminal 7411 as the operation means (controller). This allows an unspecified number of users to participate in the game at the same time and have fun. You can enjoy it.
[0157] The display device according to one aspect of the present invention can be used for an interior or exterior wall of a house or building, or The present invention can be incorporated into the interior or exterior of a vehicle along its curved surface. 1 shows an example of a display device according to an embodiment of the present invention mounted on a vehicle.
[0158] FIG. 9E shows a configuration example of a vehicle equipped with a display unit 5001. The display unit 5001 includes: The display device according to one embodiment of the present invention can be used. The following shows an example in which the 01 is installed in a right-hand drive vehicle, but it is not limited to this and may also be installed in a left-hand drive vehicle. In this case, the left and right arrangements of the configuration shown in Figure 9(E) are interchanged.
[0159] FIG. 9(E) shows a dashboard 5002 arranged around the driver's seat and the passenger seat, The display unit 5001 includes a dash board 5003, a windshield 5004, and the like. The driver is located at a predetermined position of the driver's seat 5002, specifically around the driver, and has a roughly T-shaped FIG. 9(E) shows a plurality of display panels 5007 (display panels 5007a, 5007b, 5007c, 5007d) is formed on the dashboard 5 002, the display unit 5001 may be arranged in multiple locations. good.
[0160] In addition, the plurality of display panels 5007 may be flexible. In this case, the display unit 50 01 can be processed into a complex shape, and the display unit 5001 can be mounted on a dashboard 5002, etc. The structure is provided along the curved surface of the handle, the display of the instrument, the air outlet 5006, etc. It is possible to easily realize a configuration in which the display area of the display unit 5001 is not provided.
[0161] In addition, a plurality of cameras 5005 for capturing images of the rear and lateral areas may be provided outside the vehicle. In the example shown in FIG. 1, a camera 5005 is installed instead of a side mirror. Both a mirror and a camera may be installed.
[0162] The camera 5005 may be a CCD camera or a CMOS camera. In addition to these cameras, an infrared camera may be used in combination. The higher the temperature of the subject, the higher the output level becomes, so it is used to detect or capture living organisms such as people and animals. It can be extracted.
[0163] The image captured by the camera 5005 is displayed on the display panels 5007a, 5007b, and 5007c. , 5007d, or a combination of the two. The camera 5005 captures the rear and side conditions with a wide angle of view. The image is projected onto the display panel 5007, allowing the driver to see the blind spot. This makes it possible to prevent accidents from occurring.
[0164] In addition, a distance image sensor is installed on the roof of the car, and the image obtained by the distance image sensor is The image may be displayed on the display unit 5001. The range image sensor may be an image sensor or a light sensor. LIDAR (Light Detection and Ranging) The image obtained by the image sensor and the distance image sensor can be used. By displaying the obtained image on the display unit 5001, more information can be provided to the driver. This can assist with driving.
[0165] The display unit 5001 displays map information, traffic information, television images, DVD images, etc. For example, the display panels 5007a, 5007b, 5007c, The 5007d can be used as a single display screen to display map information in a large size. The number of display panels 5007 can be increased depending on the images to be displayed.
[0166] In addition, the images displayed on the display panels 5007a, 5007b, 5007c, and 5007d The settings can be freely adjusted according to the driver's preference. For example, TV and DVD images can be The image is displayed on the left display panel 5007d, and map information is displayed on the central display panel 5007b. The instrument cluster is displayed on the right display panel 5007c, and the audio is displayed near the gear shift ( The display can be displayed on the display panel 5007a between the driver's seat and the passenger seat. By combining the display panel 5007, the display unit 5001 has a fail-safe function. For example, if a display panel 5007 breaks down for some reason, However, the display area can be changed and another display panel 5007 can be used for display.
[0167] This embodiment mode can be appropriately combined with the descriptions of other embodiments and examples. . EXAMPLES
[0168] In this embodiment, the crystallinity and the crystallinity of a metal oxynitride film formed by using the method shown in the above embodiment are The results of evaluating the crystal orientation and the crystal orientation are described below. A plurality of samples (samples 1 to 7) formed by the method shown in the above embodiment were prepared. Wide-area reciprocal space mapping, pole measurement, out-of-plane measurement, In -plane measurements were performed.
[0169] <Sample preparation method> First, manufacturing methods of Samples 1 to 7 will be described.
[0170] Samples 1 to 7 were manufactured by the method for manufacturing a metal oxynitride film described in Embodiment 1. Specifically, a single crystal substrate is prepared, and a gas is introduced into a reaction chamber to form an oxide film on the substrate. A metal oxynitride film was formed by sputtering using the target. Before forming a metal oxynitride film on the substrate, the substrate is subjected to air annealing, vacuum annealing, etc. No pretreatment such as annealing was performed. In addition, no heat treatment was performed on the formed metal oxynitride film. Not yet.
[0171] The deposition conditions for the gold oxynitride films common to Samples 1 to 7 were a deposition pressure of 0.4 Pa and The deposition power was set to 200 W, and the distance between the oxide target and the substrate was set to 130 mm.
[0172] The single crystal substrate used to prepare each sample will be described. In the sample 6, a yttria-stabilized zirconia (YSZ) substrate was prepared. The surface orientation of the plate is (111). In addition, the single crystal substrate for sample 7 is A-plane sapphire. A sapphire substrate was prepared. The surface orientation of the A-plane sapphire substrate was (110).
[0173] Next, the oxide targets used in the preparation of each sample will be described. In the samples 1, 5, 6, and 7, the composition ratio was In:Ga:Zn=4:2:4.1. [Atomic ratio] In-Ga-Zn oxide targets were used. The metal oxynitride films of Samples 6 and 7 are In-Ga-Zn oxynitride films. The oxide target for sample 2 was In-Zn oxide with an atomic ratio of In:Zn=2:1. Therefore, the metal oxynitride film of sample 2 is an In-Zn oxynitride film. In addition, zinc oxide was used as the oxide target in Sample 3. The metal oxynitride film is a zinc oxynitride film. An In-Ga-Zn oxide target with an atomic ratio of In:Ga:Zn=1:1:1 was used. Therefore, the metal oxynitride film of Sample 4 is an In-Ga-Zn oxynitride film.
[0174] Next, the gas (also called film-forming gas) introduced into the reaction chamber will be described. , Sample 1, Sample 2, Sample 3, Sample 4, Sample 6, and Sample 7 were heated with nitrogen gas (N2) 45 For the deposition gas of sample 5, nitrogen gas (N2) was used at 45 sccm. A mixed gas of 45 sccm of argon gas (Ar) was used.
[0175] Next, the substrate temperature during the formation of the metal oxynitride film will be described. In the case of samples 4, 5, and 7, the substrate temperature was set to 200° C. In the case of sample 6, The substrate temperature was set to 100°C.
[0176] As described above, samples 1 to 7 were prepared. The processing conditions for each sample are summarized below. As shown in Table 1.
[0177] [Table 1]
[0178] For each of the prepared samples 1 to 7, wide-area reciprocal space mapping and pole measurement were performed. , out-of-plane measurements, in-plane measurements, etc. For mapping, pole measurement, out-of-plane measurement and in-plane measurement The device used was the Bruker Japan X-ray diffraction device D8 DOSCOVER, and the detector was For large-area reciprocal space mapping and pole measurements, the VÅNTEC-500 2D detector For out-of-plane and in-plane measurements, a zero-dimensional detector is used. As will be described later, out-of-plane and in-plane measurements were used. The e measurements are primarily used to determine the lattice constants used as input for the simulation of large-area reciprocal space maps. Therefore, in this embodiment, out-of-plane measurement is performed to estimate the number of Also, illustration of the results of in-plane measurements will be omitted.
[0179] Wide-area reciprocal space mapping is performed by measuring the angle 2θ using a two-dimensional detector (detector in Figure 4). The sample was scanned at each angle ψ and the angle θ was measured. The distance between the sample (in Fig. 4) and the 2D detector (in Fig. 4) is The angle 2θ was set to 40°, and the angle 2θ was set to 20° or more and 60° or less. The range where the angle was 10° or more and 30° or less was recorded at once. The angle ψ was set in the range of 0° to 85° in 5° increments (total of 18 steps). A collimator was used to set the incident X-ray diameter to 0.3 mmφ, and the X-ray source was CuKα radiation (wavelength: 0 The X-ray output was set to 50 kV and 100 mA. The X-ray exposure time was 60 seconds. Wide-area reciprocal space mapping was performed on each sample. A wide-area reciprocal space map was obtained for each sample. In the above equation, the horizontal axis is the angle 2θ [°] and the vertical axis is the angle ψ [°]. The intensity at each point in the map is represented by a bar to the right of the global reciprocal space map. Specifically, the higher the intensity, the darker the color will be, and the lower the intensity, the whiter the color will be. will be done.
[0180] In addition, the simulation of the wide-area reciprocal space map corresponding to each sample was performed using Bruker et al. Pan's software "SMAP / for Cross Sectional XRD- The crystal structure of the metal oxynitride in each sample is a wurtzite structure. The lattice constant is assumed to be out-of-plane, in-plane, and The lattice constants were estimated from the results of scanning other reciprocal lattice points of the same symmetry (and is the space group), and when comparing wide-area reciprocal space maps of crystal structures with different lattice constants, In this case, the position of the peak of the spot that appears on the map (angle 2θ, angle ψ) is observed to be shifted. This may be the case.
[0181] In addition, the wide-area reciprocal space map obtained by the simulation includes the following: All the spots that can be observed in the assumed crystal are shown. Therefore, epitaxial growth The large-area reciprocal space map of the thin film obtained by the simulation and the large-area reciprocal space map obtained by the simulation In this case, the in-plane oriented crystal orientation may differ depending on the angle φ, so the observed spots The timing may vary.
[0182] In this embodiment, the crystal planes and pole measurements corresponding to the reciprocal lattice points observed in the wide-area reciprocal space map are In order to correspond to the crystal plane observed at the fixed angle, the angle φ is adjusted to perform wide-area reciprocal space mapping. Specifically, in the wide-area reciprocal space maps of samples 1 to 6, The (101) plane of the metal oxynitride film and the (111) plane of the substrate of each sample were simultaneously observed. It is advisable to adjust the angle φ so that the reciprocal lattice space can be widely mapped. In the wide-area reciprocal space map, the (101) plane of the metal oxynitride film of sample 7 and the (101) plane of sample 8 are shown. The angle φ was adjusted so that the (104) plane of the substrate of sample 7 could be simultaneously observed. It is a good idea to perform child space mapping.
[0183] Moreover, the results of the pole measurements shown in this embodiment are expressed as pole figures.
[0184] <Evaluation of Sample 1> The wide-area reciprocal space map of sample 1 is shown in FIG. The large-area reciprocal space maps obtained are shown in Figures 10(B) and 10(C). Figure 10(B) shows FIG. 10(C) is a wide-area reciprocal space map corresponding to the single crystal substrate of Sample 1. 1 is a wide-area reciprocal space map corresponding to the crystals of the metal oxynitride film of FIG.
[0185] In FIG. 10(A), multiple spots were observed. 10(B) and 10(C), it can be seen that the angle 2θ is about 35°. The spot with a peak at an angle ψ of about 62° corresponds to the (101) plane of the wurtzite structure. The spot with a peak at an angle 2θ of about 44° and an angle ψ of about 44° corresponds to the Wurtz wave. It can be seen that this corresponds to the (102) plane of the ore-type structure.
[0186] Next, the results of the pole measurement for sample 1 are shown in FIG. 11(A) and FIG. 11(B). 1(A) shows the results for the (111) surface of the single crystal substrate of sample 1, and FIG. 11(B) shows the results for the (111) surface of the single crystal substrate of sample 1. This is the result for the (101) surface of the metal oxynitride film of 1.
[0187] As shown by the solid circle in Fig. 11(A), the spot is placed at three points on a concentric circle with an angle ψ of about 70°. The spot was observed to be a spot-like intensity distribution. The spot was formed of yttria-stabilized zirconia (YSZ). ) is a three-fold symmetric spot originating from the (111) plane. As shown in Fig. 1, a spot-like intensity distribution was observed at six points on a concentric circle with an angle ψ of approximately 62°. In other words, the (101) plane of the metal oxynitride film of Sample 1 has six-fold symmetry. The metal oxynitride film has an in-plane orientation. The angle between the (101) plane and the (101) plane is approximately 62°. It can be seen that the crystals of have a wurtzite structure. B) shows that the metal oxide film of sample 1 does not contain domains in which the crystal orientation is rotated within the film plane. It is clear that this is an axial epitaxial film.
[0188] From the above, it was found that the metal oxynitride film of Sample 1 has a wurtzite structure and grows epitaxially. It can be seen that...
[0189] <Evaluation of Sample 2> The wide-area reciprocal space map of sample 2 is shown in FIG. The wide-area reciprocal space maps obtained are shown in Figures 12(B) and 12(C). Figure 12(B) shows FIG. 12(C) is a wide-area reciprocal space map corresponding to the single crystal substrate of Sample 2. 1 is a wide-area reciprocal space map corresponding to the crystals of the metal oxynitride film of FIG.
[0190] In FIG. 12(A), multiple spots were observed. By comparing the spots shown in Fig. 2(B) and Fig. 12(C), it can be seen that the angle 2θ is about 34°. The spot with a peak at an angle ψ of about 62° corresponds to the (101) plane of the wurtzite structure. The spot with a peak at an angle 2θ of about 44° and an angle ψ of about 44° corresponds to the Wurtz wave. It can be seen that this corresponds to the (102) plane of the ore-type structure.
[0191] Next, the results of the pole measurement for sample 2 are shown in FIG. 13(A) and FIG. 13(B). 3(A) shows the results for the (111) surface of the single crystal substrate of sample 2, and FIG. 13(B) shows the results for the (111) surface of the single crystal substrate of sample 2. The results are for the (101) surface of the metal oxynitride film of 2.
[0192] As shown by the solid circle in Fig. 13(A), the spot is placed at three points on a concentric circle with an angle ψ of about 70°. In addition, as shown by the solid circle in Fig. 13(B), the angle ψ A spot-like intensity distribution was observed at six points on a concentric circle of about 62°. The (101) plane of the metal oxynitride film has six-fold symmetry, and the metal oxynitride film of sample 2 has an in-plane In addition, the (002) and (101) planes of the wurtzite structure are aligned. The angle is about 62°, which indicates that the crystal of the metal oxynitride film of sample 2 is wurtzite. 13(A) and 13(B), the metal structure of sample 2 is The oxide film is a c-axis epitaxial film that does not contain domains in which the crystal orientation is rotated within the film plane. It can be seen that...
[0193] From the above, it was found that the metal oxynitride film of sample 2 has a wurtzite structure and grows epitaxially. It can be seen that...
[0194] <Evaluation of Sample 3> The wide-area reciprocal space map of sample 3 is shown in FIG. The wide-area reciprocal space maps obtained are shown in Figures 14(B) and 14(C). Figure 14(B) shows FIG. 14(C) is a wide-area reciprocal space map corresponding to the single crystal substrate of sample 3. 1 is a wide-area reciprocal space map corresponding to the crystals of the metal oxynitride film of FIG.
[0195] In FIG. 14(A), multiple spots were observed. 4(B) and 14(C), the angle 2θ is about 36°. The spot with a peak at an angle ψ of about 62° corresponds to the (101) plane of the wurtzite structure. The spot with a peak at an angle 2θ of about 47° and an angle ψ of about 42° corresponds to the Wurtz wave. It can be seen that this corresponds to the (102) plane of the ore-type structure.
[0196] Next, the results of the pole measurement for sample 3 are shown in FIG. 15(A) and FIG. 15(B). 5(A) shows the results for the (111) surface of the single crystal substrate of sample 3, and FIG. 15(B) shows the results for the (111) surface of the single crystal substrate of sample 3. This is the result for the (101) surface of the metal oxynitride film of 3.
[0197] As shown by the solid circle in Fig. 15(A), three spots are placed on the concentric circle with an angle of about 70°. In addition, as shown by the solid circle in Fig. 15(B), the angle ψ A spot-like intensity distribution was observed at six points on a concentric circle of about 62°. The (101) plane of the metal oxynitride film has six-fold symmetry, and the metal oxynitride film of sample 3 has an in-plane In addition, the (002) and (101) planes of the wurtzite structure are aligned. The angle is about 62°, which indicates that the crystal of the metal oxynitride film of sample 3 is wurtzite. 15(A) and 15(B), the metal structure of sample 3 is The oxide film is a c-axis epitaxial film that does not contain domains in which the crystal orientation is rotated within the film plane. It can be seen that...
[0198] From the above, it was found that the metal oxynitride film of sample 3 has a wurtzite structure and grows epitaxially. It can be seen that...
[0199] <Evaluation of Sample 4> The wide-area reciprocal space map of sample 4 is shown in Figure 16(A). The wide-area reciprocal space maps obtained are shown in Figures 16(B) and 16(C). Figure 16(B) shows FIG. 16(C) is a wide-area reciprocal space map corresponding to the single crystal substrate of Sample 4. 1 is a wide-area reciprocal space map corresponding to the crystals of the metal oxynitride film of FIG.
[0200] In FIG. 16(A), multiple spots were observed. By comparing the spots shown in Fig. 6(B) and Fig. 16(C), it can be seen that the angle 2θ is about 35°. The spot with a peak at an angle ψ of about 62° corresponds to the (101) plane of the wurtzite structure. The spot with a peak at an angle 2θ of about 44° and an angle ψ of about 44° corresponds to the Wurtz wave. It can be seen that this corresponds to the (102) plane of the ore-type structure.
[0201] Next, the results of the pole measurement for sample 4 are shown in FIG. 17(A) and FIG. 17(B). 7(A) shows the results for the (111) surface of the single crystal substrate of sample 4, and FIG. 17(B) shows the results for the (111) surface of the single crystal substrate of sample 4. This is the result for the (101) surface of the metal oxynitride film of 4.
[0202] As shown by the solid circle in Fig. 17(A), the spot is placed at three points on a concentric circle with an angle ψ of about 70°. In addition, as shown by the solid circle in Fig. 17(B), the angle ψ A spot-like intensity distribution was observed at six points on a concentric circle of about 62°. The (101) plane of the metal oxynitride film has six-fold symmetry, and the metal oxynitride film of sample 4 has an in-plane In addition, the (002) and (101) planes of the wurtzite structure are aligned. The angle is about 62°, which indicates that the crystal of the metal oxynitride film of sample 4 is wurtzite. 17(A) and 17(B), the metal structure of sample 4 is The oxide film is a c-axis epitaxial film that does not contain domains in which the crystal orientation is rotated within the film plane. It can be seen that...
[0203] From the above, it was found that the metal oxynitride film of sample 4 has a wurtzite structure and grows epitaxially. It can be seen that...
[0204] <Evaluation of Sample 5> The wide-area reciprocal space map of sample 5 is shown in FIG. The wide-area reciprocal space maps obtained are shown in Figures 18(B) and 18(C). Figure 18(B) shows FIG. 18(C) is a wide-area reciprocal space map corresponding to the single crystal substrate of Sample 5. 1 is a wide-area reciprocal space map corresponding to the crystals of the metal oxynitride film of FIG.
[0205] In FIG. 18(A), multiple spots were observed. By comparing the spots shown in Fig. 8(B) and Fig. 18(C), it can be seen that the angle 2θ is about 35°. The spot with a peak at an angle ψ of about 62° corresponds to the (101) plane of the wurtzite structure. The spot with a peak at an angle 2θ of about 44° and an angle ψ of about 44° corresponds to the Wurtz wave. It can be seen that this corresponds to the (102) plane of the ore-type structure.
[0206] Next, the results of the pole measurement for sample 5 are shown in FIG. 19(A) and FIG. 19(B). 9(A) shows the results for the (111) surface of the single crystal substrate of sample 5, and FIG. 19(B) shows the results for the (111) surface of the single crystal substrate of sample 5. This is the result for the (101) surface of the metal oxynitride film of No. 5.
[0207] As shown by the solid circle in Fig. 19(A), the spot is placed at three points on a concentric circle with an angle ψ of about 70°. In addition, as shown by the solid circle in Figure 19(B), the angle ψ A spot-like intensity distribution was observed at six points on a concentric circle of about 62°. The (101) plane of the metal oxynitride film has six-fold symmetry, and the metal oxynitride film of sample 5 has an in-plane In addition, the (002) and (101) planes of the wurtzite structure are aligned. The angle is about 62°, which indicates that the crystal of the metal oxynitride film of Sample 5 is wurtzite. 19(A) and 19(B), the metal structure of sample 5 is The oxide film is a c-axis epitaxial film that does not contain domains in which the crystal orientation is rotated within the film plane. It can be seen that...
[0208] From the above, it was found that the metal oxynitride film of Sample 5 has a wurtzite structure and grows epitaxially. It can be seen that...
[0209] <Evaluation of Sample 6> The wide-area reciprocal space map of sample 6 is shown in FIG. The large-area reciprocal space maps obtained are shown in Figures 20(B) and 20(C). FIG. 20(C) is a wide-area reciprocal space map corresponding to the substrate of the single crystal of Sample 6. 1 is a wide-area reciprocal space map corresponding to the crystals of the metal oxynitride film of FIG.
[0210] In FIG. 20(A), multiple spots were observed. 20(B) and 20(C), the angle 2θ is about 35°. The spot with a peak at an angle ψ of about 62° corresponds to the (101) plane of the wurtzite structure. The spot with a peak at an angle 2θ of about 44° and an angle ψ of about 44° corresponds to the Wurtz wave. It can be seen that this corresponds to the (102) plane of the ore-type structure.
[0211] Next, the results of the pole measurement for sample 6 are shown in FIG. 21(A) and FIG. 21(B). 1(A) shows the results for the (111) surface of the single crystal substrate of sample 6, and FIG. 21(B) shows the results for the (111) surface of the single crystal substrate of sample 6. The results are for the (101) surface of the metal oxynitride film of 6.
[0212] As shown by the solid circle in Fig. 21(A), three spots are placed on a concentric circle with an angle ψ of about 70°. In addition, as shown by the solid circle in Figure 21(B), the angle ψ A spot-like intensity distribution was observed at six points on a concentric circle of about 62°. The (101) plane of the metal oxynitride film has six-fold symmetry, and the metal oxynitride film of sample 6 has an in-plane In addition, the (002) and (101) planes of the wurtzite structure are aligned. The angle is about 62°, which indicates that the crystal of the metal oxynitride film of sample 6 is wurtzite. 21(A) and 21(B), the metal structure of sample 6 is The oxide film is a c-axis epitaxial film that does not contain domains in which the crystal orientation is rotated within the film plane. It can be seen that...
[0213] From the above, it was found that the metal oxynitride film of sample 6 has a wurtzite structure and grows epitaxially. It can be seen that...
[0214] <Evaluation of Sample 7> The wide-area reciprocal space map of sample 7 is shown in FIG. The wide-area reciprocal space maps obtained are shown in Figures 22(B) and 22(C). FIG. 22(C) is a wide-area reciprocal space map corresponding to the substrate of the single crystal of Sample 7. 1 is a wide-area reciprocal space map corresponding to the crystals of the metal oxynitride film of FIG.
[0215] In FIG. 22(A), multiple spots were observed. By comparing the spots shown in Fig. 2(B) and Fig. 22(C), it can be seen that the angle 2θ is about 35°. The spot with a peak at an angle ψ of about 62° corresponds to the (101) plane of the wurtzite structure. The spot with a peak at an angle 2θ of about 44° and an angle ψ of about 44° corresponds to the Wurtz wave. It can be seen that this corresponds to the (102) plane of the ore-type structure.
[0216] Next, the results of the pole measurement for sample 7 are shown in FIG. 23(A) and FIG. 23(B). 3(A) shows the results for the (104) surface of the single crystal substrate of sample 7, and FIG. 23(B) shows the results for the (104) surface of the single crystal substrate of sample 7. This is the result for the (101) surface of the metal oxynitride film of No. 7.
[0217] As shown by the solid circle in Figure 23(A), the spot is placed at two points on a concentric circle with an angle of about 58°. A spot-like intensity distribution was observed. The spot originated from the (104) plane of A-plane sapphire. As shown by the solid circle in Figure 23(B), the angle ψ is A spot-like intensity distribution was observed at six points on a concentric circle of about 62°. The (101) plane of the metal oxynitride film has six-fold symmetry, and the metal oxynitride film of sample 7 has an in-plane In addition, the (002) and (101) planes of the wurtzite structure are aligned. The angle is about 62°, which indicates that the crystal of the metal oxynitride film of sample 7 is wurtzite. 23(A) and 23(B), the metal structure of sample 7 is The oxide film is a c-axis epitaxial film that does not contain domains in which the crystal orientation is rotated within the film plane. It can be seen that...
[0218] From the above, it was found that the metal oxynitride film of sample 7 has a wurtzite structure and grows epitaxially. It can be seen that...
[0219] The configurations, methods, etc. shown in the present embodiment may be at least partially implemented in other embodiments described in this specification. The present invention can be implemented in appropriate combination with the embodiments. [Explanation of symbols]
[0220] 10: substrate, 20: metal oxynitride film, 30: crystal, 41: film-forming chamber, 50a: backing plate, 50b: backing plate, 52a: target holder, 52b: target holder, 54a: magnet unit, 54b: magnet unit, 54N1: magnet Net, 54N2: Magnet, 54S: Magnet, 56: Magnet holder, 58: Component, 60: substrate, 62: substrate holder, 64a: magnetic field, 64b: magnetic field, 70a: spa sputtering target, 70b: sputtering target, 100: light emitting element, 102 : substrate, 104: cladding layer, 106: active layer, 108: cladding layer, 110: n-type electrode , 112: p-type electrode, 400: display device, 401: pixel unit, 402: driving circuit, 403: Drive circuit, 5001: display unit, 5002: dashboard, 5003: handle, 500 4: Windshield, 5005: Camera, 5006: Air vent, 5007: Display panel, 5 007a: display panel, 5007b: display panel, 5007c: display panel, 5007d : display panel, 7000: display unit, 7100: television device, 7101: housing, 71 03: Stand, 7111: Remote control unit, 7200: Notebook personal computer 7211: Housing, 7212: Keyboard, 7213: Pointing device, 72 14: External connection port, 7300: Digital signage, 7301: Housing, 7303: PECA, 7311: Information terminal, 7400: Digital signage, 7401: Pillar, 741 1: Information terminal, 7900: Automobile, 7901: Body, 7902: Wheel, 7903: Front glass, 7904: lights, 7905: fog lamps, 8501: lighting equipment, 850 2: Lighting device, 8503: Lighting device, 8504: Lighting device
Claims
[Claim 1] a metal oxynitride film on a yttria-stabilized zirconia (YSZ) substrate having a (111) surface orientation; the metal oxynitride film comprises zinc, indium and gallium; The metal oxynitride film is an in-plane oriented film.
Citation Information
Patent Citations
Thin film luminous element and luminous device
JP1995262801A
ZnO COMPOUND SEMICONDUCTOR LIGHT-EMITTING DEVICE USING A-SURFACE SAPPHIRE SUBSTRATE, AND MANUFACTURING METHOD THEREFOR
JP2001044500A
Semiconductor of oxynitride
JP2009275236A
Substrate for growing wurtzite type crystal and method for manufacturing the same and semiconductor device
JP2010114423A
Method of manufacturing laminate comprising crystalline homologous compound layer, and field effect transistor
JP2011029238A