System and method for piercing via in material with permeability
A laser drilling method with controlled parameters forms high-quality vias in glass substrates efficiently, addressing inefficiencies in existing methods by achieving rapid, uniform via formation without etching.
Patent Information
- Application Number
- JP2024134762
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2018-10-08
- Filing Date
- 2024-08-13
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2039-10-02
AI Technical Summary
Existing laser drilling methods for forming high-quality holes in glass substrates are inefficient, requiring high capital investment, slow processing times, and often necessitate additional etching processes, leading to non-uniform thickness and difficulty in achieving precise via formation rates.
A laser drilling process using a focused laser pulse beam with a Gaussian energy distribution, transparent to the substrate, and a high pulse repetition rate forms through vias with controlled parameters to minimize etching, achieving uniform thickness and rapid via formation without additional processing.
The process enables high-speed, high-quality via formation in glass substrates with uniform diameter and morphology, reducing production costs and time, and eliminating the need for post-drilling etching.
Smart Images

Figure 2024164063000001_ABST
Abstract
Description
Related Applications
[0001] This application claims the benefit of U.S. Provisional Patent Application No. 62 / 742,694, filed October 8, 2018, which is incorporated by reference in its entirety. Background
[0002] I.Technical field FIELD OF THE DISCLOSURE Embodiments of the present invention relate generally to processing substrates, and more particularly to laser drilling vias, such as through vias, in substrates.
[0003] II. Description of Related Art Thin glass with precisely formed holes is gaining attention for electronics applications. The holes are filled with conductive material and are used to transmit electrical signals from one component to another. This allows for precise connections of central processing units, memory chips, image processing units, or other electronic components. For such applications, substrates with metallized holes inside are typically called "interposers." Compared to currently used interposer materials such as fiber-reinforced polymers or silicon, glass has many advantageous properties. Glass can be formed thin and smooth in large sheets without the need for polishing, and it is stiffer and more dimensionally stable than organic alternatives. Glass is a much better electrical insulator than silicon, and is more dimensionally stable (thermally and rigidly) than organic options. Glass can be matched to different thermal expansion coefficients to control stack warpage in integrated circuits.
[0004] A variety of hole formation methods can be used to form holes in glass, such as hot pressing, lithography of optically machinable glass, discharge drilling, powder blasting, and various laser drilling processes. The challenge with any of these techniques is generally to form holes of sufficient quality (low crack rate, adequate size and roundness) at a high enough via formation rate (holes / second), which ultimately impacts cost. For example, hot pressing of glass can be difficult to form holes with small enough dimensions (approximately 100 microns or less). Discharge drilling can be difficult to address tight hole pitches (i.e., distance between holes less than approximately 50 microns). Laser drilling of holes using beam trepanning can be slow (e.g., approximately 1 hole / second). Excimer laser processing and optically machinable glass can have large initial capital costs.
[0005] Previously, laser drilling processes have been developed that produce particularly high quality holes. For example, UV nanosecond lasers can be used in a percussion drilling process to create pilot holes (each about 10 microns in diameter) in a glass part using multiple (e.g., hundreds) of laser pulses per hole. The part is then etched in acid to enlarge the pilot holes to achieve the target dimensions. The etched holes are then metallized, a redistribution layer is added for fan-out of electrical signals, and the part is diced into smaller pieces to produce functional interposers. However, laser drilling with UV nanosecond lasers is a time-consuming process, and percussion drilling (i.e., successive pulses at the same location) can require hundreds of pulses to drill a single hole to the desired depth. The capital costs to build a precision laser drilling platform can be substantial (approaching $1 million per unit), so the speed of hole formation is a key parameter in the overall production cost of an interposer. Also, etching the glass parts makes it difficult to ensure that different glass parts have substantially the same thickness after etching.
[0006] Other conventional laser drilling processes include single-shot laser processes that use a single laser pulse with a Bessel beam profile to modify a glass part regardless of where the vias are required, and then etch the part with acid to form the vias. While this process can be used to produce up to 5000 vias per second (200 μs per via), it still requires etching, which, as mentioned above, can make it difficult to achieve a uniform thickness of the glass part in the finished product. Furthermore, laser pulses with a Bessel beam profile are difficult to deflect at high speeds using conventional beam steering methods (e.g., galvanometer mirrors, etc.). Thus, the time required to form a pattern of relatively sparse vias is typically much slower than 5000 vias per second.
[0007] In Karimelahi, Samira, Ladan Abolghasemi, and Peter R. Herman, "Rapid micromachining of high aspect ratio holes in fused silica glass by high repetition rate picosecond laser," Applied Physics A 114.1 (2014), pp. 91-111, a thorough study revealed that high aspect ratio vias could be produced in glass using IR and green ultrafast lasers and Gaussian focal spots, but that the vias were of poor quality or required a subsequent etching step. Thus, there is a need for a method of laser drilling materials such as glass that minimizes or eliminates the problems mentioned above. Abstract
[0008] One embodiment may be characterized as an article of manufacture that includes a substrate having a plurality of laser-drilled through holes extending continuously from a first side of the substrate to a second side of the substrate opposite the first side of the substrate, the plurality of laser-drilled through holes having a diameter of 10 μm or greater and a spacing between adjacent etched through holes of 30 μm or greater, the plurality of laser-drilled through holes including an opening at the first side, an opening at the second side, and a waist located between the opening at the first side and the opening at the second side, a diameter of the waist being 75% or greater of a diameter of the opening at the first side or the opening at the second side, and a difference between a diameter of the opening at the first side and a diameter of the opening at the second side being 3.5 μm or less.
[0009] Another embodiment may be characterized as a method for forming a through via in a substrate, comprising: providing a substrate having a first side and a second side opposite the first side; irradiating the substrate with a focused laser pulse beam through the first side and subsequently through the second side of the substrate for a drilling period of less than 100 μs; the focused laser pulse beam having a wavelength at which the substrate is at least substantially transparent; an optical intensity of the focused laser pulse beam at the substrate is less than an optical breakdown intensity of the substrate; the focused laser pulse beam having a Gaussian energy distribution; the focused laser pulse beam having a pulse repetition rate greater than 5 MHz; and laser pulses in the focused laser pulse beam having a pulse width greater than 200 fs.
[0010] Another embodiment may be characterized as a method for forming a through via in a substrate, comprising: providing a substrate having a thickness in a range of 30 μm to 150 μm and having a first side and a second side opposite the first side; irradiating the substrate with a focused laser pulse beam through the first side of the substrate and thereafter through the second side of the substrate, the focused laser pulse beam having a wavelength at which the substrate is at least substantially transparent, an optical intensity of the focused laser pulse beam at the substrate being less than an optical breakdown intensity of the substrate, the focused laser pulse beam having a Gaussian energy distribution, the focused laser pulse beam having a pulse repetition rate, a peak optical intensity at the substrate, and an average power at the substrate that produces a cumulative heating effect, laser pulses in the focused laser pulse beam having a pulse width, and the peak optical intensity, the pulse repetition rate, the average power, and the pulse width selected such that the through via is formed in less than 40 μs.
[0011] Yet another embodiment may be characterized as a method for forming a through via in a substrate, comprising: providing a substrate having a first side and a second side opposite the first side; irradiating the substrate with a focused laser pulse beam through the first side of the substrate and thereafter through the second side of the substrate, the focused laser pulse beam having a wavelength at which the substrate is at least substantially transparent, a beam waist of the focused laser pulse beam being closer to the second side of the substrate than to the first side of the substrate, the focused laser pulse beam melting an area of the substrate proximate the second side of the substrate to create a melt zone in the substrate, the focused laser pulse beam propagating toward the first side, and characterized by a pulse repetition rate, a peak light intensity at the substrate, and an average power at the substrate sufficient to vaporize or evaporate material of the substrate located within the melt zone. [Brief description of the drawings]
[0012] [Figure 1]FIG. 1 illustrates an exemplary laser processing system for performing a laser drilling process. [Figure 2-3] 2 and 3 are photographs showing through vias drilled in an exemplary glass substrate using a laser drilling process according to one embodiment. [Figure 4] FIG. 4 is a graph illustrating experimental results of a laser drilling process on a glass substrate in one embodiment. [Figure 5-8] 5-8 are photographs of cut glass substrates that have been processed according to embodiments described herein to form through vias. Detailed Description
[0013] Examples of embodiments are described herein with reference to the accompanying drawings. Unless expressly stated otherwise, in the drawings, the sizes and locations of components, features, elements, etc., and distances therebetween are not necessarily to scale and have been exaggerated for clarity. Like numbers refer to like elements throughout the drawings. Thus, the same or similar numbers may be described with reference to other drawings even if they are not mentioned or described in the corresponding drawing. Also, elements that are not numbered may be described with reference to other drawings.
[0014] The terms used herein are for the purpose of describing particular exemplary embodiments only and are not intended to be limiting. Unless otherwise defined, all terms (including technical and scientific terms) used herein have the same meaning as commonly understood by one of ordinary skill in the art. As used herein, the singular is intended to include the plural unless the content clearly indicates otherwise. Furthermore, it should be understood that the terms "comprises" and / or "comprising", when used herein, specify the presence of stated features, integers, steps, operations, elements, and / or components, but do not exclude the presence or addition of one or more other features, integers, steps, operations, elements, components, and / or groups thereof. Unless otherwise indicated, when a range of values is listed, the range includes the upper and lower limits as well as any subranges between the upper and lower limits of the range. Unless otherwise indicated, terms such as "first" and "second" are only used to distinguish elements from one another. For example, one node can be referred to as a "first node" and similarly another node can be referred to as a "second node" or vice versa.
[0015] Unless otherwise indicated, terms such as "about," "around," "approximately," and the like, mean that amounts, sizes, formulations, parameters, and other quantities and characteristics are not and need not be exact, but may be approximate and / or larger or smaller, as appropriate, or to reflect tolerances, conversion factors, rounding, measurement errors, and the like, and other factors known to those of skill in the art. Spatially relative terms such as "below," "lower," "lower side," "upper," and "above" may be used herein for ease of description in describing the relationship of an element or feature to another element or feature, as depicted in the figures. It should be understood that the spatially relative terms are intended to include different orientations in addition to those depicted in the figures. For example, an element described as being "below" or "below" another element or feature would be oriented "above" the other element or feature if the object in the figure were inverted. Thus, the exemplary term "below" may include both an upper and lower orientation. If the object is otherwise oriented (e.g., rotated 90 degrees or at another orientation), the spatially relative descriptors used herein may be interpreted accordingly.
[0016] It will be appreciated that many different forms, embodiments, and combinations are possible without departing from the spirit and teachings of the present disclosure, and that the disclosure should not be construed as limited to the example embodiments set forth herein, but rather, these examples and embodiments are provided so that this disclosure will be complete and all-inclusive, and will fully convey the scope of the disclosure to those skilled in the art.
[0017] In embodiments described herein, a laser drilling process for drilling through vias in a substrate involves irradiating the substrate with a beam of laser pulses such that the beam of laser pulses is transmitted through a first side of the substrate and propagates through the substrate toward a second side of the substrate opposite the first side. Typically, the laser pulse beam is focused to have a beam waist located on or near the second side (inside or outside the substrate).
[0018] In some embodiments, the substrate is provided as an article of glass (e.g., borosilicate glass, aluminoborosilicate glass, aluminosilicate glass, alkali lead silicate glass, alkali alkaline earth silicate glass, germanium oxide glass, quartz glass, etc.), synthetic quartz, glass ceramic (e.g., lithium-aluminum-silicate), ceramic, sapphire, semiconductor material (e.g., Si, SiGe, GaAs, GaN, SiC, etc.), etc., or any combination thereof. Thus, the article may be provided as a glass interposer, silicon interposer, semiconductor wafer, semiconductor die, substrate (e.g., for display screens, wafer mounting or other semiconductor mounting, display panel mounting, MEMS or sensor devices, etc.), etc., or any combination thereof. In some embodiments, the substrate is provided as an article (e.g., having a thickness in the range of 30 μm (or thereabouts) to 150 μm (or thereabouts)). However, it should be understood that the thickness of the substrate may be less than 30 μm or may be greater than 150 μm, depending on the particular product embodied by the substrate.
[0019] Typically, the laser pulse beam irradiated to the substrate has a wavelength at which the substrate is substantially transparent. As used herein, a substrate is considered to be "substantially transparent" to the wavelength of the laser pulse beam if the absorption of the laser pulse beam by the substrate at that wavelength is less than about 20% (e.g., less than about 15%, less than about 10%, less than about 5%, less than about 1%) per mm of material depth. Thus, depending on the material forming the substrate, the laser pulse beam may have a wavelength in the ultraviolet, visible, or infrared regions of the electromagnetic spectrum. For example, in an embodiment, when the substrate is a product made of glass, quartz, or sapphire, the laser pulse beam may have a wavelength in the range of 300 nm (or thereabouts) to 1064 nm (or thereabouts).
[0020] As described in more detail below, the laser drilling process can be characterized by parameters including pulse wavelength, pulse width, pulse energy, pulse repetition rate, peak light intensity at the substrate, drilling duration (i.e., the time the laser pulse is applied to a particular location on the substrate to form a through via), and average power of the laser pulse beam at the substrate. Typically, the laser pulse beam that is ultimately applied to the substrate during the laser drilling process has a Gaussian energy profile. Using a laser pulse beam with a Gaussian energy profile allows the laser pulse beam to be rapidly deflected using conventional beam steering techniques (e.g., galvanometer mirrors, fast steering mirrors, rotating polygon mirrors, acousto-optic deflectors, electro-optic deflectors, etc.) to form through vias in the substrate. Depending on the diameter of the via required, a percussion drilling process can be used (e.g., when forming vias having diameters in the range of 1 μm to 100 μm, e.g., 10 μm, 20 μm, 30 μm, 50 μm, etc.) or the beam can be deflected (e.g., as described above) to form vias of similar or larger diameters. Because the beam can be deflected rapidly, even relatively sparse patterns of through vias can be formed with high throughput compared to that achieved with conventional laser drilling processes. Finally, the laser drilling processes described herein do not require an acid etch process to obtain through vias with acceptable diameters or surface morphology.
[0021] The laser drilling process can also be characterized by a parameter referred to herein as "z-range." The z-range is the range of distances between the second surface of the substrate and the beam waist of the laser pulse beam that forms a through via in the substrate during the laser drilling process. The inventors have discovered that the z-range depends at least in part on the other parameters of the laser drilling process described above. For example, for a given pulse wavelength, pulse width, and pulse repetition rate, and above threshold drilling duration and average power at the substrate, the z-range has been discovered to vary as a function of the drilling duration and average power at the substrate during the laser drilling process. Identifying values of the laser drilling process parameters (e.g., drilling duration and average power at the substrate for a given pulse wavelength, pulse width, and pulse repetition rate) that result in a sufficiently large z-range can be challenging. This is because substrates typically do not have a perfectly uniform thickness (i.e., thickness variability can occur on the order of about 10 μm or more) and / or are not perfectly flat when the laser drilling process is being performed (i.e., some waviness can occur on the substrate on the order of about 10 μm or more), and the thickness of one substrate may differ from the thickness of another substrate. If the z-range does not accommodate the variations in substrate thickness and flatness, the laser drilling process cannot reliably form through vias.
[0022] After drilling, the through vias can be coated and / or filled with conductive materials. For example, through vias can be formed in a substrate, such as a glass interposer, and coated and / or filled with conductive materials (e.g., copper, aluminum, gold, silver, lead, tin, indium tin oxide, etc., or any combination or alloy thereof). The process used to metallize the interior of the through vias can be, for example, electrolytic plating, electroless plating, physical vapor deposition, or other vapor deposition coating methods. The through vias can also be coated with catalytic materials, such as platinum, palladium, titanium dioxide, or other materials that promote chemical reactions inside the holes. Alternatively, the through vias can be coated with chemical functionalization to change the wetting properties of the surface or allow attachment of biomolecules and used for biochemical analysis. Such chemical functionalization can be silanization of the glass surface of the through vias and / or additional attachment of specific proteins, antibodies, or other biologically specific molecules designed to promote attachment of biomolecules for the desired application.
[0023] In general, the laser pulse beam can be characterized by parameters such as pulse repetition rate, pulse energy, and pulse width. The pulse energy and pulse width are selected such that when the laser pulse beam is focused, the beam waist is at an offset distance away from the second surface of the substrate, and each laser pulse in the focused laser pulse beam strikes an area of the substrate (i.e., corresponding to the spot size of the laser pulse at that area of the substrate) with a peak optical intensity lower than the optical breakdown intensity of the substrate. Furthermore, the pulse repetition rate of the laser pulse beam is selected to be sufficiently high (e.g., considering the peak optical intensity of each laser pulse striking an area of the substrate) such that the irradiated area of the substrate can accumulate heat during an initial period (e.g., also referred to herein as the "incubation period"). Heating of the substrate during the incubation period is primarily initiated by multiphoton absorption by the substrate material. Absorption of the laser pulses during the incubation period can also occur at point defects in the substrate that can create defect states for optical absorption between the conduction band and the valence band.
[0024] At the end of the incubation period, the irradiated regions of the substrate (which may be, for example, on or near the second side of the substrate, on or near the first side of the substrate, or a combination thereof) accumulate a sufficient amount of heat to locally increase the temperature of the substrate, reduce its band gap energy, and allow the irradiated regions of the substrate to transition to a state in which they can melt and ultimately evaporate. It is believed that the band gap of the substrate material narrows as a result of thermal ionization, i.e., the gradual overlay of band gaps at high temperatures due to electronic vibrational states of molecules. It is also believed that impact ionization and cascade ionization may also occur within the hot regions of the substrate, causing an increase in carrier density that may also contribute to enhanced laser absorption. The regions of the substrate that become melted during the laser drilling process may be characterized as "melt zones." As soon as the absorption of the laser pulse increases significantly at the edges or boundaries or interfaces of the hot regions in the substrate, the melt zones grow progressively toward the first side (i.e., in the opposite direction to the propagation of the laser pulse beam from the scan lens 110). In addition, it has been found that at very high temperatures inside the substrate (i.e., above 3000°C), thermally ionized free electrons can cause impact ionization and cascade ionization, even without the contribution of multiphoton absorption, and the absorption of the laser pulse can be greatly increased. As the temperature in the melting zone increases beyond the vaporization / boiling point of the substrate material, a large vapor pressure is created that can eventually push the molten substrate material out of the via (at least primarily through the second surface) to create a through via. Thus, for an additional period immediately following the incubation period (e.g., also referred to herein as the "removal period"), the focused laser pulse beam may remain on the irradiated region of the substrate to heat and melt the irradiated region of the substrate, and evaporate (through the entire thickness of the substrate) to form a through via. The entire period from the start of the incubation period to the end of the removal period is referred to herein as the "drilling period".
[0025] In view of the above, it should be clear that the laser drilling process described herein depends heavily on the heat accumulation dynamics of the substrate (when irradiated by the focused laser pulse beam). Thus, the laser pulse beam may be generated and focused by any method known in the art to generate a focused laser pulse beam. Each laser pulse in the focused laser pulse beam has a peak power and peak optical intensity at the substrate sufficient to heat (but not ablate, crack, or damage) the substrate. The laser pulse beam is further generated by any method known in the art to generate laser pulses with sufficient peak power to prevent the substrate from substantially cooling between laser pulses (e.g., to allow the substrate to accumulate heat during the incubation period and continue to accumulate heat during the removal period, as described above), at a pulse repetition rate sufficient to prevent cooling. However, the peak power, peak optical intensity, and pulse repetition rate of the focused laser pulse beam should also be selected to prevent the substrate from accumulating heat too quickly. If heat accumulates too quickly, undesirable phenomena such as cracks appearing in areas of the substrate not exposed to the laser pulse beam or molten material erupting outside the substrate can occur.
[0026] In one embodiment, the laser pulse beam generated and focused to impinge on the substrate to perform the laser drilling process described herein has a wavelength of 1.27·10 11 W / cm 2The laser pulse beam may be characterized as having a pulse repetition rate of 30 MHz and a peak power at the substrate of about 78 kW (e.g., determined by pulse energy and pulse width as known in the art) to irradiate the substrate with a peak light intensity (e.g., determined by peak power and spot size at the substrate as known in the art) of (or thereabouts). It should be understood that the laser pulse beam may have a pulse repetition rate higher than 30 MHz or lower than 30 MHz, and the peak power of the laser pulse beam at the substrate may be maintained or adjusted if necessary (e.g., by adjusting the pulse width or pulse energy of the laser pulses in the laser pulse beam) to compensate for changes in the pulse repetition rate. Similarly, the peak light intensity at the substrate may be maintained or adjusted if necessary (e.g., by adjusting the pulse width, pulse energy, or spot size at the second side of the substrate) to compensate for changes in the pulse repetition rate, if necessary. The pulse repetition rate, peak power, pulse width, or pulse energy of the laser pulses in the laser pulse beam may be constant or may vary during the drilling period. Typically, lasers capable of generating laser pulse beams with sufficiently high pulse repetition rates and peak powers to perform the laser drilling process are QCW lasers capable of generating laser pulses with pulse widths ranging from 200 fs (or thereabouts) to 50 ps (or thereabouts). For example, the laser pulses can have pulse widths of 200 fs, 400 fs, 800 fs, 1 ps, 2 ps, 5 ps, 10 ps, 20 ps, 25 ps, 30 ps, 40 ps, 45 ps, 50 ps, etc., or any value between these values.
[0027] Thus, to perform the laser drilling processes described herein, the pulse repetition rate of the laser pulse beam may range from 5 MHz (or thereabouts) to 5 GHz (or thereabouts), with the peak power of the laser pulse beam and peak light intensity at the substrate, if necessary, being adjusted if necessary to compensate for changes in the pulse repetition rate. In one embodiment, the pulse repetition rate may range from 5 MHz (or thereabouts) to 500 MHz (or thereabouts). In other embodiments, the pulse repetition rate may range from 25 MHz (or thereabouts) to 40 MHz (or thereabouts), 150 MHz (or thereabouts) to 180 MHz (or thereabouts).
[0028] Depending on one or more factors such as the thickness of the substrate, the pulse repetition rate of the laser pulse beam, the pulse energy of the laser pulses in the laser pulse beam, the pulse width of the laser pulses in the laser pulse beam, the peak power at the substrate, the light intensity at the substrate, the perforation duration may range from 5 μs (or thereabouts) to 120 μs (or thereabouts), in certain embodiments, it may be advantageous for the perforation duration to be 50 μs (or thereabouts) or less, 30 μs (or thereabouts) or less, 20 μs (or thereabouts) or less, 15 μs (or thereabouts) or less, 10 μs (or thereabouts) or less, etc., or a value between any of these values.
[0029] When the beam waist of the focused laser pulse beam is outside the substrate near the second side, absorption of the laser energy occurs at the interface between the second side of the substrate and the surrounding environment (i.e., air). This interface helps to lower the ablation threshold at which the laser energy in the laser pulse beam begins to couple to the substrate. The relatively high peak intensity helps to eliminate the need for an absorbing coating on the second side of the substrate. From experiments performed by the inventors, it appears that there is an initial incubation period during which the focused laser pulse beam does not damage the substrate.
[0030] In one embodiment, the first side of the substrate is cleaned to remove (or reduce the amount of) contaminants on the first side that would absorb the energy in the laser pulse beam. Experiments performed by the inventors have shown that when a laser energy beam is passed over a portion of the first side that has not been cleaned, the through vias formed in the substrate tend to have a relatively large opening at the first side and a relatively small opening at the second side. When a laser energy beam is passed over a portion of the first side that has been suitably cleaned, the through vias formed in the substrate tend to have openings of approximately the same diameter at the first and second sides (e.g., within the range of 2 μm to 5 μm, respectively).
[0031] Thus, removal of material from the substrate during the laser drilling process appears to involve a combination of melting and ablation of the substrate material, and the material removal rate is surprisingly high compared to conventional laser drilling processes, even though the laser pulse beam has a relatively low average power. Indeed, the laser drilling process described herein exhibits a significant improvement in via formation rate compared to conventional laser drilling processes. Experiments performed by the inventors on optically transparent glass substrates with a thickness of 100 μm or less (i.e., performing the laser drilling process described herein by a percussion drilling method) show that through vias having a diameter of about 10 μm can be reliably formed in 15 μs (or thereabouts). Experiments performed by the inventors on optically transparent glass substrates with a thickness of 50 μm or less (i.e., performing the laser drilling process described herein by a percussion drilling method) show that through vias having a diameter of about 10 μm can be reliably formed in only 5 μs (or thereabouts) and can be reliably formed in 15 μs (or thereabouts). In contrast to the laser drilling processes of the embodiments described herein, conventional laser drilling processes performed on optically transparent glass substrates using laser pulses having pulse widths of less than 10 picoseconds at transparent wavelengths rely on nonlinear absorption and tend to require several times longer to form a single through via than the time required to form a single through via with the laser drilling processes described herein.
[0032] 1 shows an exemplary laser processing system for performing the laser drilling process described in the above embodiments. Referring to FIG. 1, the laser processing system 100 includes a laser 102, a beam expander 104, a beam modulator 106, a beam scanner 108, a scan lens 110, and a stage 112.
[0033] The laser 102 can be any suitable laser capable of generating a laser pulse beam having the above characteristics (e.g., a QCW laser capable of generating a laser pulse beam having the above characteristics). For example, the laser 102 can be configured to generate a laser pulse beam with an average power of 100 W (or thereabouts), a wavelength of 515 nm (or thereabouts, e.g., 532 nm), a pulse width in the range of 20 ps (or thereabouts) to 40 ps (or thereabouts), and a pulse repetition rate in the range of 25 MHz (or thereabouts) to 40 MHz (or thereabouts). In one embodiment, the laser pulses have a pulse width of 28 ps (or thereabouts) and a pulse repetition rate of 30 MHz (or thereabouts).
[0034] The beam expander 104 may be any suitable device capable of expanding the incident beam from a first beam size (e.g., diameter of 2 mm or thereabouts) to a second beam size (e.g., diameter of 4.5 mm or thereabouts). In one embodiment, the beam expander may be a motorized variable beam expander.
[0035] The beam modulator 106 may be any suitable device capable of selectively attenuating (e.g., partially attenuating, fully attenuating, or not attenuating) the laser energy beam. In one embodiment, the beam modulator 106 may be an acousto-optic (AO) modulator (AOM) or an AO deflector (AOD).
[0036] Beam scanner 108 may be any suitable device (or devices) capable of deflecting an incident laser pulse beam (e.g., within a one-dimensional scan region, within a two-dimensional scan region, etc.) Thus, beam scanner 108 may include one or more galvanometer mirrors, one or more fast steering mirrors, one or more deformable mirrors, one or more AODs, a rotating polygon mirror, etc., or any combination thereof.
[0037] The scan lens 110 can be any suitable device (or devices) capable of focusing an incident laser pulse beam to generate a focused laser pulse beam. In one embodiment, the scan lens 110 is a telecentric scan lens. In another embodiment, the scan lens 110 has a focal length of 100 mm (or thereabouts) and a numerical aperture (NA) of about 0.5 or less. In one embodiment, the scan lens 110 can focus the laser pulse beam to generate a beam waist (e.g., at the focal plane of the scan lens 110) having a diameter in the range of 10 μm (or thereabouts) to 13 μm (or thereabouts), e.g., in the range of 11 μm to 12 μm.
[0038] The stage 112 may be any suitable device (or devices) capable of supporting and moving the substrate (e.g., identified as 114) described above. In one embodiment, the stage 112 is configured to linearly move the substrate 114 along one axis, two axes, the like, or any combination thereof. In general, the substrate 114 may be characterized as including a first side (e.g., facing the scan lens 110) and a second side opposite the first side (e.g., facing away from the scan lens 110). The stage 112 is configured to support the substrate 114 such that the second side of the substrate 114 does not contact an underlying structure, such as the stage 112. As used herein, the first side of the substrate 114 may also be referred to as the "front side" of the substrate 114, and the second side of the substrate 114 may also be referred to as the "back side" of the substrate 114.
[0039] In one embodiment, stage 112 supports substrate 114 such that the focal plane of scan lens 110 is located outside of substrate 114 (i.e., below the second side of substrate 114). The distance between the second side of substrate 114 and the focal plane of scan lens 110 (i.e., the "offset distance" discussed above) is set such that the focused laser pulse beam illuminates an area of the substrate with a peak intensity that is less than the optical breakdown strength of the substrate while still producing through vias in the substrate as discussed above. It will be appreciated that the offset distance may be determined experimentally or calculated (e.g., based on parameters of the laser drilling process, based on the material of the substrate, or the like, or any combination thereof).
[0040] The system 100 may further include one or more other components that polarize, reflect, expand, focus, etc., the laser pulse beam propagating from the laser 102 to the scan lens 110 (e.g., along the dotted line exemplarily shown in FIG. 1). Examples of such components include a half-wave plate 116, a pair of relay lenses 118, and a number of folding mirrors (e.g., folding mirror 120). In one embodiment, the pair of relay lenses are arranged and configured to expand the laser pulse beam as output from the beam modulator 106 (e.g., double the beam size of the laser pulse beam as output from the beam modulator 106). Thus, when the laser pulse beam as output from the beam modulator 106 has the second beam size of 4.5 mm (or thereabouts) as described above, the laser pulse beam output from the pair of relay lenses can be characterized as having a third beam size of 9 mm (or thereabouts).
[0041] 2 and 3 are photographs taken from a first side and a second side, respectively, of through vias drilled in a 50 μm thick glass substrate (i.e., a substrate made of AF 32® manufactured by SCHOTT) using the above-described laser drilling process using the above-described laser processing system 100. The glass substrate was uncoated in the sense that no absorbing coating was formed on either side, and the average power of the laser pulse beam at the substrate (i.e., after being reflected, propagated, or diffracted by the above-described components of the laser processing system 100) ranged from 66 W (or thereabouts) to 67 W (or thereabouts). The diameter of the through vias at the first side (shown in FIG. 2) was 9.5 μm to 10.1 μm, and the diameter of the through vias at the second side (shown in FIG. 3) was 9 μm.
[0042] 4 is a graph showing the results of an experiment in which the above-described laser drilling process was performed on a 50 μm thick glass substrate (i.e., an uncoated substrate made of AF 32® manufactured by SCHOTT). In this experiment, the average power of the laser pulse beam at the substrate was varied from 25 W (or thereabouts) to 67 W (or thereabouts), and the drilling duration at each position of the substrate where a via was to be formed was varied from 5 μs to 120 μs in 5 μs intervals. The points in the graph represent the actual data points obtained from each experiment, and the contour boundaries were obtained from the experimentally obtained data using the statistical analysis software JPM produced by SAS INSTITUTE.
[0043] As shown in FIG. 4, experiments performed by the inventors showed that a laser drilling process with an average power of 25 W and a drilling duration of 120 μs did not damage the substrate at all and did not form through vias. Similarly, the same was true for average power / drilling duration combinations of 25 W / 40 μs, 30 W / 40 μs, 35 W / 40 μs, 40 W / 30 μs, 40 W / 20 μs, 40 W / 10 μs, and 50 W / 10 μs. With an average power of 67 W and a drilling duration of 5 μs, through vias were formed in the substrate when the z offset was 0.05 mm, but no through vias were formed when the z offset was greater than 0.05 mm. Thus, with an average power of 66 W (or thereabouts) to 67 W (or thereabouts) and a drilling duration of 5 μs, the z range of the laser drilling process is 0.05 mm. It has been found that the z-range of the laser drilling process can be expanded by increasing the average power at the substrate and / or by increasing the drilling duration at each drilling location, as shown in FIG. 4. For example, by increasing the drilling duration from 40 μs to 120 μs (at an average power of 30 W), through vias can be formed with a z-offset of 0.075 mm. Similarly, with an average power of 40 W and a drilling duration of 40 μs, through vias were formed in the substrate at a z-offset of 0.075 mm (however, no through vias were formed when the z-offset was greater than 0.075 mm). Importantly, it has been discovered that through vias formed with a drilling duration of 15 μs can be formed with a z-offset of 0.2 mm or more (at or about) when the average power at the workpiece is in the range of 66 W (at or about) to 67 W (at or about). Thus, at an average power of 66 W (or thereabouts) to 67 W (or thereabouts) and a drilling duration of 15 μs, the z-range of the laser drilling process is greater than 0.2 mm. In many cases, the z-range desirably accommodates variations in substrate thickness or flatness, allowing rapid and reliable formation of through vias through the substrate.
[0044] 5-8 are cross-sectional photographs of 50 μm (FIGS. 5 and 7) or 100 μm (FIGS. 6 and 8) thick glass substrates (i.e., glass substrates made from AF 32® manufactured by SCHOTT) that were processed to form through vias (e.g., using the laser processing system 100 and the laser drilling process described above). Each via was formed with a drilling duration of 15 μs. No absorbing coating was formed on either side of the glass substrate. The average power of the laser pulse beam at the substrate (i.e., after being reflected, transmitted, or diffracted by the above-mentioned components of the laser processing system 100) was 67 W (or thereabouts) to 69 W (or thereabouts). In FIGS. 5-8, the roughness of the edges at the cross-sectional plane is due to the fragility of the glass material to the mechanical grinding method used to cut the substrate. Thus, the diameters identified in FIGS. 5-8 may have been smaller than the annotated diameters before cutting. The main purpose of Figures 5-8 is to show how straight the sidewalls of the through vias are and how uniform the diameter of the through vias is throughout the entire thickness of the substrate.
[0045] From the above, it can be appreciated that the laser pulse beam can be scanned (e.g., by the beam scanner 108) to form multiple through vias. In the laser drilling process described herein, the minimum via-to-via pitch (i.e., the distance between nearest adjacent vias) is generally limited by the diameter of the "splash zone" around the opening of each through via in the second side of the substrate. In general, the splash zone is the area where molten material ejects from the substrate during the formation of the through vias around the opening in the second side. In one embodiment, the laser drilling process described above produces a splash zone of about 30 μm in diameter. Thus, the via-to-via pitch can be 30 μm (or thereabouts) or more.
[0046] The above is a description of embodiments and examples of the present invention and is not to be construed as limiting thereof. Although several specific embodiments and examples have been described with reference to the drawings, those skilled in the art will readily recognize that many modifications to the disclosed embodiments and examples and other embodiments are possible without significantly departing from the novel teachings and advantages of the present invention.
[0047] For example, although through vias have been described having openings of approximately 10 μm diameter at the first and second sides of substrates having thicknesses of either 50 μm or 100 μm, it will be understood that through vias having similar sized openings may be formed in substrates having thicknesses of less than 50 μm, between 50 μm and 100 μm, or greater than 100 μm. Furthermore, by using a scan lens 110 having an NA higher than 0.5, through vias having smaller radius openings at the first and second sides can be obtained.
[0048] In another example, although the laser system 100 is described above as including a laser 102 capable of generating a laser pulse beam at a wavelength of 515 nm (or thereabouts), it will be understood that laser pulses at wavelengths other than 515 nm (or thereabouts) can be used to achieve the laser drilling process described in the above embodiment, depending on one or more other factors such as the average power at the substrate, the pulse width, the pulse repetition rate, the material forming the substrate, etc. For example, if the laser pulse beam has a pulse repetition rate as described above, and further, the average power of the laser pulse beam at the substrate is 100 W (or thereabouts) or more (e.g., 110 W, 120 W, 130 W, etc., or a value between any of these values), a laser pulse beam at a wavelength in the near infrared region of the electromagnetic spectrum (e.g., 1030 nm, 1064 nm, etc.) can be used to achieve the laser drilling process described above. At wavelengths in the near infrared region, the laser pulses in the laser pulse beam can have the pulse widths described above. However, it should be noted that the selection of the pulse width can affect the length of the drilling period. In general, it has been found that for a given average power and pulse repetition rate, a laser pulse beam having a relatively short pulse width (e.g., 10 ps or thereabouts) can form a through via in a shorter drilling period than a laser pulse beam having a relatively long pulse width (e.g., 30 ps or thereabouts).
[0049] In another example, although the laser drilling process is described above as eliminating the need for an absorbing coating on the second side of the substrate, it will be appreciated that the second side of the substrate may be coated or treated with a material that is more absorptive to the laser pulse beam than the substrate or a material that alters the substrate's absorptivity for the laser pulses (e.g., at or near its second side).
[0050] In another example, if desired, a thermal annealing process may be performed on the substrate after the laser drilling process is performed to form the through vias, in which case the thermal annealing treatment may act to relieve internal stresses in the substrate caused by solidification of molten material ejected into the splash zone during the laser drilling process.
[0051] Accordingly, all such modifications are intended to be included within the scope of the present invention as defined in the claims. For example, one of ordinary skill in the art will understand that the subject matter of any sentence, paragraph, example or embodiment may be combined with any or all of the subject matter of any other sentence, paragraph, example or embodiment, except where such combinations would be mutually exclusive. Thus, the scope of the present invention should be determined by the following claims and any equivalents of such claims that are to be included therein.
Claims
1. a substrate having a plurality of laser-drilled through holes extending continuously from a first surface of the substrate to a second surface of the substrate opposite the first surface of the substrate; the plurality of laser-drilled through holes having a diameter of 10 μm or greater; The spacing between adjacent etched through holes is 30 μm or more; the plurality of laser-drilled through holes include an opening in the first surface, an opening in the second surface, and a waist located between the opening in the first surface and the opening in the second surface; a diameter of the waist is 75% or more of a diameter of the opening in the first surface or the opening in the second surface; a difference between a diameter of the opening on the first surface and a diameter of the opening on the second surface is 3.5 μm or less; product.
2. 10. The article of claim 1, wherein the substrate is transparent to at least one wavelength in the range of 390 nm to 700 nm.
3. The article of claim 1 , wherein the substrate is glass.
4. The article of claim 1 , wherein the substrate has a thickness in the range of 50 μm to 100 μm.
5. 2. The article of claim 1, wherein the diameter of the waist is greater than or equal to 80% of the diameter of the opening in the first surface or the opening in the second surface.
6. The article of manufacture of claim 1 , wherein the plurality of laser-drilled holes contain a conductive material.
7. 1. A method for forming a through via in a substrate, comprising: providing a substrate having a first surface and a second surface opposite the first surface; irradiating the substrate with a focused laser pulse beam at a position passing through the first side of the substrate and subsequently at a position passing through the second side of the substrate for a drilling period of less than 100 μs; the focused laser pulse beam has a wavelength through which the substrate is at least substantially transparent; the optical intensity of the focused laser pulse beam at the substrate is less than the optical breakdown intensity of the substrate; the focused laser pulse beam has a Gaussian energy distribution; the focused laser pulse beam has a pulse repetition rate greater than 5 MHz; The laser pulses in the focused laser pulse beam have a pulse width longer than 200 fs. method.
8. The method of claim 7 , wherein the substrate is at least substantially transparent to at least one wavelength in the ultraviolet, visible, or infrared regions of the electromagnetic spectrum.
9. The method of claim 8 , wherein the substrate is at least substantially transparent to at least one wavelength in the visible region of the electromagnetic spectrum.
10. The method of claim 8 , wherein the substrate is at least substantially transparent to at least one wavelength in the infrared region of the electromagnetic spectrum.
11. The method of claim 7 , wherein the substrate is glass.
12. The method of claim 7 , wherein the substrate is sapphire.
13. The method of claim 7 , wherein the substrate is a silicon die.
14. The method of claim 7 , wherein the substrate is a GaN die.
15. 8. The method of claim 7, wherein the focused laser pulse beam has a pulse repetition rate greater than 25 MHz.
16. 16. The method of claim 15, wherein the focused laser pulse beam has a pulse repetition rate greater than 40 MHz.
17. 17. The method of claim 16, wherein the focused laser pulse beam has a pulse repetition rate greater than 300 MHz.
18. 20. The method of claim 17, wherein the focused laser pulse beam has a pulse repetition rate greater than 500 MHz.
19. 17. The method of claim 16, wherein the laser pulses in the focused laser pulse beam have a pulse width shorter than 50 ps.
20. 1. A method for forming a through via in a substrate, comprising: providing a substrate having a thickness in the range of 30 μm to 150 μm and having a first surface and a second surface opposite the first surface; irradiating the substrate with a focused laser pulse beam through the first surface of the substrate and thereafter through the second surface of the substrate; the focused laser pulse beam has a wavelength through which the substrate is at least substantially transparent; the optical intensity of the focused laser pulse beam at the substrate is less than the optical breakdown intensity of the substrate; the focused laser pulse beam has a Gaussian energy distribution; the focused laser pulse beam has a pulse repetition rate, a peak light intensity at the substrate, and an average power at the substrate that produces a cumulative heating effect; a laser pulse in the focused laser pulse beam having a pulse width; the peak light intensity, the pulse repetition rate, the average power, and the pulse width are selected such that the through via is formed in less than 40 μs. method.
21. 21. The method of claim 20, wherein the peak light intensity, the pulse repetition rate, the average power, and the pulse width are selected such that the through via is formed in less than 30 μs.
22. 22. The method of claim 21, wherein the peak light intensity, the pulse repetition rate, the average power, and the pulse width are selected such that the through via is formed in less than 20 μs.
23. 23. The method of claim 22, wherein the peak light intensity, the pulse repetition rate, the average power, and the pulse width are selected such that the through via is formed in less than 10 μs.
24. 22. The method of claim 21, wherein the peak light intensity, the pulse repetition rate, the average power, and the pulse width are selected such that the through via is formed in a time within a range of 5 μs to 15 μs.
25. 1. A method for forming a through via in a substrate, comprising: providing a substrate having a first surface and a second surface opposite the first surface; irradiating the substrate with a focused laser pulse beam through the first surface of the substrate and thereafter through the second surface of the substrate; the focused laser pulse beam has a wavelength through which the substrate is at least substantially transparent, and a beam waist of the focused laser pulse beam is closer to the second side of the substrate than to the first side of the substrate; The focused laser pulse beam Melting a region of the substrate proximate the second surface to create a melt zone within the substrate; Propagating the molten zone towards the first surface; Vaporizing or evaporating material of the substrate located within the melt zone. a pulse repetition rate sufficient for the laser to reach a desired wavelength, a peak optical intensity at the substrate, and an average power at the substrate; method.
Citation Information
Patent Citations
Method and apparatus for laser-machining silicon by filamentation of burst ultrafast laser pulse
JP2015110248A
Method and system for scribing and chemically etching brittle materials
JP2018509298A
Cited By
FORMING SYSTEM AND FORMING PROCESS
DE102025137075A1