Rhenium-tungsten wire rod and thermo couple using the same, medical needle, probe pin and rhenium-tungsten wire for electron tube heater
The controlled Re and K content in Re-W wire rods address non-uniformity issues, ensuring stable thermoelectromotive force and mechanical properties, enhancing the performance and yield of thermocouples and medical needles.
Patent Information
- Application Number
- JP2024149029
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-03-09
- Filing Date
- 2024-08-30
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2042-03-03
AI Technical Summary
Existing Re-W wire rods exhibit non-uniformity due to the presence of σ-phase segregated phases, leading to variations in Re content and thermoelectromotive force, which affects temperature measurement accuracy and wire integrity, particularly in high-temperature applications like thermocouples and medical needles.
A Re-W wire rod with controlled Re content (1-30 wt%) and a coefficient of variation (CV) of 0.10 or less, along with controlled K content (30-90 wtppm), ensuring homogeneous distribution and reduced σ-phase formation, thereby stabilizing thermoelectromotive force and mechanical properties.
The solution enhances the stability and accuracy of thermocouples by minimizing Re content variations, improving yield and reducing wire breakage, while maintaining consistent mechanical properties for medical needles and other applications.
Smart Images

Figure 2024164257000001_ABST
Abstract
Description
[Technical field]
[0001] The embodiments described below relate to a tungsten rhenium wire rod and a thermocouple using the same. [Background technology]
[0002] Various tungsten (W) wires have been used in the past as cathode heaters for TV electron guns, filament materials for lighting in automobile lamps and home appliances, high-temperature structural members, contact materials, and materials for discharge electrodes. Among these, tungsten alloy (Re-W) wires containing a certain amount of rhenium (Re) improve the electrical resistance characteristics and wear resistance of W wires and are widely used in probe pins for semiconductor inspection. In addition, they improve the high-temperature strength and ductility after recrystallization of W wires and are widely used in heaters for electron tubes, filament materials for vibration-resistant light bulbs, thermocouples, etc. In addition, due to the solid solution strengthening of Re, the strength and rigidity at room temperature are higher than stainless steel wires and W wires, so they are also used in medical needles. (Patent Document 2) Figure 1 shows a schematic diagram of an example of temperature measurement using a thermocouple. Thermocouples are temperature sensors that utilize the thermoelectromotive force produced by combining two dissimilar metals. They have been the most widely used in industry for many years due to their simple structure and ability to be used over a wide temperature range, from low to high, by selecting the right material. Figure 2 shows some examples of thermocouple types according to the JIS standard (see JIS C1602). Thermocouples used at high temperatures include platinum-rhodium alloy-based B, S, and R thermocouples, and Re-W-based C thermocouples. C thermocouples are particularly commonly used in non-oxidizing atmospheres above approximately 1500°C.
[0003] For example, sintered metals and sintered ceramics are molded by mixing raw powder and wax as a binder, and then heat-treating the molded product in a vacuum atmosphere below 1000°C to remove the wax. Then, heat-treating the molded product at 1600-2000°C to sinter it, and a C thermocouple is used to measure the temperature at 1600-2000°C. For example, in a pressure sintering (HP) furnace or a hot isostatic pressing (HIP) device, the temperature inside the pressure vessel is as high as about 2000°C in a gas pressure atmosphere. In optical temperature measurement using a radiation thermometer or the like, it is necessary to make an opening to directly observe the radiation light in the furnace chamber, which reduces the strength of the pressure vessel. In addition, the opening in the vessel also causes heat loss. For this reason, it is very difficult to apply and the device is expensive. Therefore, in HP furnaces and HIP devices that are subject to the High Pressure Gas Safety Act, a C thermocouple is used to measure the temperature.
[0004] In recent years, the use of ceramics with high properties such as silicon nitride has expanded to include insulating heat dissipation substrates for power semiconductor modules and LED mounting, bearing balls for wind power generators and vehicle engines, and industrial equipment parts such as vehicle components and semiconductor manufacturing equipment. These ceramics are produced using the above-mentioned heat treatment equipment, and in order to maintain high properties and produce with good yield, it is very important to manage the temperature profile of the heat treatment. For this reason, it is very important that the temperature measurement accuracy is maintained within and between production lots of thermocouples.
[0005] When using a thermocouple, a calibration process is required to determine the relationship between the value indicated by the thermocouple and the actual temperature. Calibration methods can be broadly divided into fixed-point method and comparative method. The fixed-point method is a method in which an accurate temperature value is given at a fixed temperature point to perform calibration, while the comparative method is a method in which the temperature of an arbitrarily determined thermostatic chamber is measured with a standard thermocouple (reference line) and the error with the thermocouple being calibrated, measured at the same time, is determined to perform calibration. For C thermocouples, the comparative method is generally used because they measure temperatures above 1500°C.
[0006] It is said that the relationship between temperature and thermoelectromotive force of thermocouples used at high temperatures will not change unless any inhomogeneity occurs in any part of the wires that make up the thermocouple. Here, inhomogeneity means "change in thermoelectromotive force per 1°C temperature difference" (see Non-Patent Document 1). In other words, if a part having this inhomogeneity (inhomogeneous part) exists in the wire and a temperature gradient occurs in that part, the detected thermoelectromotive force will show a different value compared to a thermocouple of wires that does not have an inhomogeneous part. For example, even if the above-mentioned calibration is performed, there is a high possibility that the thermal gradient in the actual device cannot be reproduced, and there is a possibility that a temperature deviation from the calibration will occur. Also, if many parts of the wire have inhomogeneous parts, the difference from the reference line will be too large, and the product may not be able to be calibrated.
[0007] On the other hand, medical needles are formed into their shape by cutting a wire to a desired length and performing press processing and bending processing. During press processing and bending processing, stress is applied to the cut wire, so it is required that cracks are unlikely to occur and that no cracks occur at the bent portion. In addition, medical needles are used for suturing during surgery. In order to suppress fluctuations in needle behavior, such as needle bending caused by the force applied during suturing, it is preferable that the tensile strength is high and has little variation. In order to prevent a decrease in yield due to cracks and breaks during needle processing and to obtain needles of stable quality, it is necessary that the cut wires are homogeneous, that is, the wires used are homogeneous.
[0008] The main cause of the inhomogeneity is the variation in the wire material. For example, Re-W is usually manufactured by powder metallurgy, in which W powder and Re powder are mixed, molded, and sintered. Since the sintering of Re-W proceeds by solid-phase diffusion, it is impossible to diffuse and homogenize (solid-solve) Re in the W matrix depending on the particle size distribution of each powder, the mixing state of the powder, and the molding and sintering conditions. As a result, a phase region with a locally high Re composition ratio (a segregation phase of the σ phase) may be generated. The generation of a segregation phase of the σ phase means that there are also parts where the Re composition ratio is lower than the average. When a sintered body with such a variation in Re composition is processed into a bar or wire, inhomogeneity occurs due to the variation in the Re amount in the cross section in the processing direction (axial direction) and in the cross section perpendicular to the axial direction (radial direction). Regarding the σ-phase segregation phase, for example, if the σ-phase segregation phase is unevenly distributed in one area, wire breakage is likely to occur during wire drawing. Therefore, there is a Re-W wire in which the σ-phase segregation phase has a maximum grain size of 10 μm or less and is dispersed over a wide range (see Patent Document 1). [Prior art documents] [Patent documents]
[0009] [Patent Document 1] Japanese Patent No. 4256126 [Patent Document 2] Japanese Patent No. 5766833 [Non-patent literature]
[0010] [Non-Patent Document 1] Yoshio Monma and 5 others, "Causes of Degradation and Variation of PR Thermocouples Used in Long-Term Creep Tests," Tetsu-to-Hagane, 1989, No. 75, No. 4, pp. 665-672 Summary of the Invention [Problem to be solved by the invention]
[0011] The method described in Patent Document 1 aims to suppress the σ-phase segregation phase to a level where it will not break during wire drawing by miniaturizing the region of its existence below a certain size and dispersing it over a wide area, rather than distributing it in a specific region, and therefore tolerates the presence of fine σ-phase segregation phases. However, even if the σ-phase segregation phase exists homogeneously, if the proportion of the phase in a certain volume changes, there is a possibility that a variation in the Re content (change in material) will occur in the axial cross section or radial cross section, resulting in the generation of inhomogeneous parts.
[0012] Figure 3 shows an example of the amount of Re in the W matrix when a σ-phase segregation phase is present in a 26% Re-W wire. The results of semi-quantitative analysis using EPMA (accelerating voltage 15.0 kV, probe current 5.0×E -8 From the image (A, beam diameter 1μm or less), it can be seen that the inclusions are σ phases. The σ phase is harder than the matrix, so it exists in the form of inclusions like this. The amount of Re in the matrix varies in the area near this σ phase. In this way, the presence of the σ phase causes the amount of Re in the surrounding area to vary (inhomogeneity). [Means for solving the problem]
[0013] In order to solve the above problems, the rhenium tungsten wire rod according to the embodiment is a wire rod made of a tungsten alloy containing 1 wt% or more and less than 30 wt% of rhenium, with the remainder being made of tungsten and inevitable impurities. In two radial cross sections of the wire rod body, the rhenium content is less than 30 wt% in a measurement area of a unit area of 1 μm diameter at a total of 17 points, including 16 intersections between four equally spaced concentric circles and two perpendicular diameters, and the center. The rhenium content has a coefficient of variation of 0.10 or less in semi-quantitative analysis using EPMA. According to an embodiment, a wire rod is provided which is made of a tungsten alloy containing 1 wt% or more and less than 30 wt%, potassium (K) 90 wtppm or less, and the remainder being tungsten and inevitable impurities. In two radial cross sections of the wire rod body, the rhenium content is less than 30 wt% in a measurement area of a unit area of 1 μm diameter at a total of 17 points, including 16 intersections between four equally spaced concentric circles and two perpendicular diameters, and the center. The rhenium content has a coefficient of variation of 0.10 or less in semi-quantitative analysis using EPMA. Furthermore, according to the embodiment, a thermocouple using the tungsten rhenium wire rod according to the embodiment is provided. According to an embodiment, there is provided a wire rod made of a tungsten alloy containing 1 wt% or more and less than 30 wt% of rhenium, with the balance being tungsten and unavoidable impurities. The standard deviation of the tensile strength of the wire rod is 35 N / mm 2 The following is the result. According to an embodiment, a wire rod is provided that is made of a tungsten alloy containing 1 wt% or more and less than 30 wt%, 90 wtppm or less of potassium (K), and the balance being tungsten and unavoidable impurities. The standard deviation of the tensile strength of the wire rod is 35 N / mm 2 The following is the result. Furthermore, according to the embodiment, there are provided a thermocouple, a probe pin, a medical needle, and a ReW wire for an electron tube heater, each including the rhenium tungsten wire rod of the embodiment. [Brief description of the drawings]
[0014] [Figure 1] Schematic diagram of a thermocouple temperature measurement system. [Diagram 2] A table showing types of thermocouples. [Diagram 3] A diagram showing inclusions (σ phase) present in a ReW matrix and the results of semi-quantitative analysis (an example of a conventional material). [Figure 4] Schematic diagram of radial cross section and surface layer of a sample. [Diagram 5] Schematic diagram of Re content measurement points. [Figure 6] Schematic diagram of particle size distribution. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] Hereinafter, the rhenium tungsten wire rod of the embodiment will be described with reference to the drawings. Hereinafter, the rhenium tungsten wire rod may be referred to as a ReW wire rod. Note that the drawings are schematic, and for example, the dimensional ratio of each part is not limited to the drawings.
[0016] FIG. 4 shows an example of a radial cross section of a sample taken from a ReW wire rod. In the radial cross section, the rhenium tungsten wire rod body is indicated by C. FIG. 4 also shows an enlarged view of the portion indicated by A in the radial cross section of the rhenium tungsten wire rod outer periphery. As shown in the enlarged view of FIG. 4, a surface mixture layer B is formed on the outer periphery of the rhenium tungsten wire rod body C. The surface mixture layer B contains W, O, and C as constituent elements. The diameter of the wire rod is preferably 0.1 mm or more and 5.0 mm or less so that it can be used as various thermocouples and wires for wire drawing. For example, when used for thermocouples, if the wire diameter is less than 0.1 mm, it is prone to breakage due to evaporation loss during high-temperature use, and has a short life. If the wire diameter exceeds 5.0 mm, the temperature of the object cannot be accurately measured due to the heat capacity of the thermocouple itself. A more preferable range is 0.2 mm or more and 3.5 mm or less. ReW wire rods are processed to a thickness of 0.1 mm to 5.0 mm through a forging (swaging: SW) process and a subsequent wire drawing (drawing: DW) process. SW and DW wire rods have a mixture layer on the surface. The mixture contains W, O, and C as constituent elements, and is removed, for example, through an electrolytic process, when the rod is manufactured. The main body excluding this mixture is used as the sample. The sampling position is arbitrary, but in consideration of the product yield and to evaluate the variation, it is desirable to sample two or more separate positions within a single wire rod. The front and rear ends of a single ReW wire rod have parts where the conditions are unstable, for example, when the DW device is started and stopped. These parts are not included in the sampling. The length of the unstable part varies depending on the layout and size of the device.
[0017] Measurements may be performed on any cross section of the sample taken, but a radial cross section as shown in FIG. 4 is preferred because of the ease of sample processing. Observation becomes easier by embedding the sample in resin and polishing and etching it as necessary. For the obtained measurement surface, as shown in FIG. 5, for example, the intersections (16 points) of the four equally spaced concentric circles 2 to 5 with the X-axis and Y-axis, and the center point 1 are used to quantify the amount of Re in a 1 μm diameter area at a total of 17 points in the radial cross section of the rhenium tungsten rod body C, using an EPMA (electron probe microanalyzer). The measurement points are illustrative, and any point may be measured, but this point is preferable for measuring the entire cross section without bias. In addition, the radial cross section to be measured is not an arbitrary one point of the rod, but an arbitrary two or more points separated from each other are used.
[0018] In the embodiment, the ReW wire rod body has a rhenium content of less than 30 wt% in any measurement area with a unit area of 1 μm in diameter. A Re content of 30 wt% or more exceeds the average addition amount. This indicates that sufficient diffusion of Re or W is not performed in the sintering process, and there is variation in the Re content in the axial cross-sectional direction and radial cross-sectional direction. The variation in the Re content causes inhomogeneity, and may cause variation in thermoelectromotive force depending on the position in the ReW wire rod.
[0019] Next, the average value (Ave), standard deviation (Sd), and coefficient of variation (CV) calculated by Sd / Ave are calculated for the obtained Re content data. CV indicates the ratio of the magnitude of data variation to the average, and can be used to compare the variation regardless of whether the Re ratio of the ReW wire rod is high or low.
[0020] The CV of the rhenium content of the ReW wire rod of the embodiment is preferably 0.10 or less. More preferably, it is 0.05 or less. When the CV is greater than 0.10, for example, even if no σ-phase segregation phase is present, it indicates that the Re content varies in the axial cross-sectional direction or the radial cross-sectional direction. The variation in the Re content causes inhomogeneity, and may cause the thermoelectromotive force to vary depending on the position in the ReW wire rod.
[0021] The amount of Re contained in the ReW wire rod of the embodiment is preferably 1 wt% or more and less than 30 wt%, and more preferably 2 wt% or more and 28 wt% or less. The amount of Re is a value analyzed by inductively coupled plasma-optical emission spectrometry (ICP-OES), which is suitable for evaluating constituent elements, rather than inductively coupled plasma-mass spectrometry (ICP-MS), which is suitable for evaluating trace impurities. Re improves the elongation of W at high temperatures and improves its workability. It also increases strength through solid solution strengthening. However, when the content is less than 1 wt%, the effect is insufficient. For example, when used as a material for probe pins, the completed probe pins will deform more with frequency of use, causing contact failure and reducing the inspection accuracy of semiconductors. When the Re content is greater than about 28 wt%, it exceeds the solid solution limit with W, causing a σ-phase segregation phase, which makes it easier for inhomogeneous parts to occur in the wire rod. The occurrence of inhomogeneous parts causes variations in thermoelectromotive force and strength. By setting the Re content at 1 wt% or more and less than 30 wt%, or 2 wt% or more and 28 wt% or less, for example, a thermocouple using this embodiment as a constituent material and a thermocouple using the positive conductor and the negative conductor (the positive conductor means the positive conductor, and the negative conductor means the negative conductor) and a ReW wire for a probe pin using this embodiment as a material can be manufactured with a good yield while ensuring the thermoelectromotive force characteristics (stability) and mechanical characteristics (strength and abrasion resistance).
[0022] The ReW wire rod of the embodiment may contain 30wtppm to 90wtppm of K as a dopant. By containing K, the tensile strength and creep strength at high temperatures are improved by the doping effect. If the K content is less than 30wtppm, the doping effect is insufficient. If it exceeds 90wtppm, the workability may decrease, and the yield may be significantly reduced. By containing 30wtppm to 90wtppm of K as a dopant, for example, a thermocouple using the present embodiment as a constituent material for the + side conductor and the - side conductor, or a ReW wire for an electron tube heater using the present embodiment as a material, can be manufactured with a high yield while maintaining high-temperature properties (prevention of breakage and deformation when used at high temperatures).
[0023] The standard deviation of the tensile strength of the ReW wire rod of the embodiment is 35 N / mm 2 The standard deviation of the tensile strength of the ReW wire rod can be reduced to 35 N / mm. By reducing the variation in tensile strength, the processing stability of the ReW wire rod can be improved, which is expected to improve the yield of products using the ReW wire rod (e.g., thermocouples, probe pins, medical needles). In addition, the stable tensile strength improves the quality of medical needles when used as a material for medical needles. The ReW wire rod of the embodiment has a standard deviation of 35 N / mm 2 If the wire rod has a diameter of 0.1 mm or more and 5.0 mm or less, better processing stability can be obtained. Tensile strength is measured using a universal tension and compression tester. Since the load varies depending on the wire diameter, the load cell of the universal tension and compression tester may be changed or different equipment may be used depending on the wire diameter. For example, Shimadzu AG-I 5kN or Minebea LTS 500N may be used. The test piece is chucked with a flat plate via non-slip sandpaper, and both ends are fixed to the device. The tensile test is performed with a gauge length of 50 mm and at a speed of 10 mm / min. If the fracture is not between the gauges, remeasurement is performed.
[0024] According to this embodiment, a ReW wire rod can be realized that is free from material variation (inhomogeneous parts) and contributes greatly to improving the stability of thermoelectromotive force, and can be applied to high-temperature thermocouple applications. It can also be applied to ReW wire applications for probe pins. The ReW wire rod is not limited to one with a circular cross section, and may have a cross section of a shape other than a circle, such as an ellipse or a polygon.
[0025] Next, a method for producing the ReW wire rod according to the present embodiment will be described. The method for producing the ReW wire rod is not particularly limited, but the following method can be given as an example.
[0026] W powder and Re powder are mixed so that the Re content is 1 wt% or more and less than 30 wt%. Although there is no particular limitation on the mixing method, a method in which the powder is made into a slurry using water or an alcohol-based solution and mixed is particularly preferred because it produces a powder with good dispersibility. In addition, in order to ensure the homogeneity of the powder lot, it is even more preferred to dry the above-mentioned slurry and then mix the same powder lot together in a dry state.
[0027] The Re powder to be mixed preferably has an average particle size of less than 8 μm. The particle size distribution preferably has an SD value of less than 11 μm. Figure 6 shows an explanatory diagram of particle size distribution. The horizontal axis is particle size (μm), the left vertical axis is frequency (%), and the right vertical axis is cumulative (%). The SD value is calculated by SD = (d (84%) - d (16%)) / 2, where d (84%) is the cumulative 84% particle size, and d (16%) is the cumulative 16% particle size, and is a guide to the distribution width of the measured particle size. The particle size distribution is measured by the laser diffraction method. The amount of powder used for one measurement is the amount recommended for the measuring device. Generally, 0.02 g is recommended. The measurement sample is thoroughly stirred before measurement and then weighed.
[0028] The W powder is either pure W powder excluding unavoidable impurities, or doped W powder containing an amount of K considering the yield to wire rod. The W powder preferably has an average particle size of less than 16 μm. The particle size distribution preferably has an SD value of less than 13 μm. If the average particle size and particle size distribution of the Re powder and W powder are above the above range, the diffusion distance of the Re atoms or W atoms to become homogeneous increases, making it easier to generate the σ phase.
[0029] The ratio of the average grain size of Re to the average grain size of W is preferably 0.4 to 2.0. If the ratio of the average grain size of Re to the average grain size of W is smaller than 0.4 or larger than 2.0, the diffusion distance of Re atoms to the center of the W grains or the diffusion distance of W atoms to the center of the Re grains becomes large, which may make it easier for the σ phase to occur.
[0030] Next, the mixed powder is put into a predetermined mold and press molded. The pressing pressure at this time is preferably 150 MPa or more. The molded body may be pre-sintered at 1200 to 1400°C in a hydrogen furnace to facilitate handling. The obtained molded body is sintered in a hydrogen atmosphere, an inert gas atmosphere such as argon, or in a vacuum. The sintering temperature is preferably 2500°C or more. If the temperature is less than 2500°C, the diffusion of Re atoms and W atoms during sintering does not proceed sufficiently. The upper limit of the sintering temperature is 3400°C (below the melting point of W, 3422°C).
[0031] The relative density of the sintered body is preferably 90% or more. The relative density after sintering is the relative density (%) to the true density, and the relative density (%) to the true density is expressed as [sintered body density / true density] x 100%. In addition, the ratio of the density of the lowest part of a single sintered body, for example the lower end in electric current sintering, to the overall average density of the same sintered body is preferably 0.98 or more. By making the relative density of the sintered body 90% or more and the ratio of the density of the lowest part to the overall average density of the same sintered body 0.98 or more, the fluctuation of the Re content can be suppressed.
[0032] The sintered body obtained in the main sintering step is subjected to a first SW process. The first SW process is preferably carried out at a heating temperature of 1300 to 1600° C. The reduction rate of the cross-sectional area (area reduction rate) in one heat treatment (one heat) is preferably 5 to 15%.
[0033] Instead of the first SW process, rolling may be performed. The rolling is preferably performed at a heating temperature of 1200 to 1600°C. The reduction in area per heat is preferably 40 to 75%. As the rolling machine, a two-way roller rolling machine, a four-way roller rolling machine, a die roll rolling machine, or the like can be used. The rolling can significantly increase the manufacturing efficiency. The first SW process and rolling may be combined.
[0034] The second SW process is carried out on the sintered body (ReW bar material) that has been subjected to the first SW process, rolling process, or a combination of these processes. The second SW process is preferably carried out at a heating temperature of 1200 to 1500°C. The area reduction rate in one heating (one heat) is preferably about 5 to 20%.
[0035] The ReW bar that has been through the second SW process is then subjected to a recrystallization process. The recrystallization process can be carried out, for example, using a high-frequency heating device in a hydrogen atmosphere, an inert gas atmosphere such as argon, or in a vacuum at a processing temperature in the range of 1800 to 2600°C.
[0036] The ReW bar that has completed the recrystallization treatment is subjected to a third SW process. The third SW process is preferably performed at a heating temperature of 1200 to 1500°C. The area reduction rate in one heat is preferably about 10 to 30%. The third SW process is performed until the ReW bar has a diameter that can be drawn (preferably a diameter of 2 to 4 mm).
[0037] The ReW bar material that has completed the third SW process is subjected to DW processing, which involves repeatedly applying a lubricant to the surface, drying the lubricant, heating to a workable temperature, and drawing using a drawing die, in order to enable smooth wire drawing (DW) processing. It is preferable to use a C-based lubricant with excellent heat resistance as the lubricant. The processing temperature is preferably 1100°C or lower. The processing temperature is set according to the wire diameter to be DWed. The reduction in area per die is preferably 10 to 35%. An annealing process or a surface polishing process (e.g., an electrolytic process) may be added during the DW process as necessary.
[0038] The appropriate amount of SW or DW finished ReW wire rod is processed through necessary processes such as heat treatment and surface polishing to create a thermocouple material. After this, thermocouples are manufactured with the specified combination. (Example) In Examples 1 to 4, sintered bodies were produced under the above processing conditions. In Example 5 and Comparative Example 1, sintered bodies were produced using conventional Re powder and W powder sizes. In Example 6 and Comparative Example 2, sintered bodies were produced using conventional W powder sizes. Table 1 shows the analysis results for each example. Re and K were analyzed using inductively coupled plasma-optical emission spectrometry (ICP-OES) rather than inductively coupled plasma-mass spectrometry (ICP-MS). The lower detection limit for K is 5 wtppm, and cases where the analysis value was below 5 wtppm without addition are indicated with "-".
[0039] [Table 1]
[0040] Each sintered body was processed to a diameter of 0.5 mm by the above-mentioned processing step. In Examples 2 and 4 and Comparative Example 2, the diameters were separately processed to 5.0 mm and 0.1 mm. After processing was completed, samples were taken from both ends of each wire rod by the above-mentioned method, and 17 points per size x 2 samples = 34 points in total were measured using an EPMA (JXA-8100 manufactured by JEOL Ltd., magnification 1000 times, acceleration voltage 15.0 kV, irradiation current 5.0 x E-8 A) was used to analyze the Re content in an area with a diameter of 1 μm. Next, CV was calculated from the analysis values. The evaluation results are shown in Table 2. The Re content is represented by "○" if "less than 30 wt% at all measurement points" and "×" if "30 wt% or more at one point." The diagonal lines in the table indicate sizes for which samples were not produced. Additionally, if K was not added and the analysis value was below 5 wtppm, it is indicated by "-".
[0041] [Table 2]
[0042] Next, thermocouples were produced through a prescribed process using wire rods processed to a diameter of 0.5 mm in combinations of prototypes 1 to 8 shown in Table 3. Prototype 2 was also produced with a diameter of 0.1 mm (prototype 2-2) and a diameter of 5 mm (prototype 2-3). Two pieces of material were sampled from each end. Four thermocouples were produced for each combination, with the positions not overlapping (front-front, front-back, back-front, back-back). Here, one end of one wire rod is the front, and the other end of the same wire rod is the back. For example, front-front indicates a combination of the front of one wire rod and the front of the other wire rod. For each prototype, the thermocouple was placed in an electric furnace together with a calibrated platinum-rhodium thermocouple, and the thermoelectromotive force was measured using the system shown in Figure 1 at a temperature where the platinum-rhodium thermocouple indicated 1600°C, and the temperature was calculated (JISC1602). The temperature measurement system shown in FIG. 1 includes a thermocouple positive (+) conductor and a thermocouple negative (-) conductor, a temperature measurement junction, a reference junction, a measuring instrument, and a compensation conductor. The temperature measurement junction is formed by welding the tip of the thermocouple positive conductor to the tip of the thermocouple negative conductor. The thermocouple positive conductor and the thermocouple negative conductor are each connected to a reference junction. The reference junction and the measuring instrument are connected by a compensation conductor. Table 3 shows the maximum and minimum differences (Max-Min) of the temperatures obtained using each prototype. As can be seen from the table, the ReW wire rod according to the embodiment suppresses the Re variation of the main body, and suppresses the temperature variation of the thermocouple using the same wire rod. In contrast, the comparative example does not suppress the Re variation, and the temperature variation of the thermocouple using the same wire rod is large. Therefore, the yield is greatly improved when the embodiment is used as a thermocouple.
[0043] [Table 3]
[0044] In addition, the tensile strength was compared between Example 4 with a diameter of 0.5 mm and Comparative Example 2 with a diameter of 0.5 mm. 20 samples of tensile pieces were taken evenly from the entire length. A universal tensile compression tester (AG-I 5kN manufactured by Shimadzu Corporation) was used for the test. The test pieces were chucked with a flat plate via sandpaper to prevent slipping, and both ends were fixed to the device. The gauge length was 50 mm, and the tensile test was performed at a speed of 10 mm / min. The results are shown in Table 4. There was no difference in the average tensile strength, but the standard deviation, which indicates the variation, is much smaller in Example 4 than in Comparative Example 2. Therefore, the stability of conditions when processing the Example as a material is greatly improved, which contributes to improving the yield. In addition, the standard deviation of the tensile strength for the other Examples was 35 N / mm 2 The results were as follows. The stability of conditions when processing the example material is greatly improved, which contributes to improving yields. When this wire rod is cut into multiple pieces to produce medical needles, needles with stable tensile strength can be obtained.
[0045] [Table 4]
[0046] Although some embodiments of the present invention have been illustrated above, these embodiments are presented as examples and are not intended to limit the scope of the invention. These novel embodiments can be implemented in various other forms, and various omissions, substitutions, modifications, etc. can be made without departing from the gist of the invention. Modifications of these embodiments are included in the scope and gist of the invention, and are included in the scope of the invention and its equivalents described in the claims. In addition, the above-mentioned embodiments can be implemented in combination with each other. The invention as originally claimed in the present application is set forth below. [1] A tungsten rhenium wire rod made of a tungsten alloy containing rhenium, in which the rhenium content is less than 30 wt% in any measurement area of a unit area of 1 μm in diameter in the rod body. [2] The rhenium tungsten wire rod according to [1], wherein the rhenium content has a coefficient of variation of 0.10 or less in semi-quantitative analysis using EPMA. [3] The rhenium tungsten wire rod according to any one of [1] and [2], wherein the rhenium content is 1 wt% or more and less than 30 wt%. [4] The rhenium tungsten wire rod according to any one of [1] and [2], wherein the rhenium content is 2 wt% or more and 28 wt% or less. [5] The tungsten alloy has a potassium (K) content of 30 wtppm or more and 90 wtppm or less. [1] to [4]. [6] The tungsten rhenium wire rod according to any one of [1] to [5], wherein the diameter of the wire rod is 0.1 mm or more and 5.0 mm or less. [7] The standard deviation of the tensile strength of the wire rod is 35 N / mm 2 The rhenium tungsten wire rod according to [6], [8] A thermocouple using the rhenium tungsten wire rod described in any one of [1] to [7]. [Explanation of symbols]
[0047] A…Outer periphery of rhenium tungsten rod B…Surface mixture layer C…Rhenium tungsten rod and wire body 1...Center point of radial cross section 2,3,4,5...Concentric circles in radial cross section X, Y: X-axis and Y-axis of radial cross section
Claims
1. A wire rod made of a tungsten alloy containing 1 wt% or more and less than 30 wt% of rhenium, with the remainder being tungsten and unavoidable impurities, The standard deviation of the tensile strength of the wire rod is 35 N / mm 2 The following is a rhenium tungsten wire rod.
2. A wire rod made of a tungsten alloy containing 1 wt% or more and less than 30 wt% of rhenium, 90 wtppm or less of potassium (K), and the remainder being tungsten and unavoidable impurities, The standard deviation of the tensile strength of the wire rod is 35 N / mm 2 The following is a rhenium tungsten wire rod.
3. 3. The tungsten rhenium wire rod according to claim 1, wherein the rhenium content is 2 wt % or more and 28 wt % or less.
4. The tungsten rhenium wire rod according to claim 2, wherein the tungsten alloy has a potassium (K) content of 30 wtppm or more and 90 wtppm or less.
5. 5. The tungsten rhenium wire rod according to claim 1, wherein the diameter of the wire rod is 0.1 mm or more and 5.0 mm or less.
6. A thermocouple using the tungsten rhenium wire rod according to any one of claims 1 to 5.
7. A medical needle using the tungsten rhenium wire rod according to any one of claims 1 to 5.
8. A probe pin using the tungsten rhenium wire rod according to any one of claims 1 to 5.
9. A ReW wire for an electron tube heater, comprising the rhenium tungsten wire rod according to any one of claims 1 to 5.
Citation Information
Patent Citations
W3Re-W25Re thermocouple material and preparation method of thermocouple
CN102586663A
Device for heating sample to high temperature
JP1983104150A
Rhenium-tungsten wire, probe pin and inspection instrument provided with the probe pin
JP2002356732A
Rhenium-tungsten wire, process for producing same, and medical needle comprising same
WO2010100808A1
Mixed assembling production system
JP1982066833A