Silicon carbide semiconductor device and manufacturing method of them
The SiC semiconductor device with distinct 4H and 3C layers maintains device design freedom and suppresses leakage current by clearly defining the 3C-SiC and 4H-SiC regions, enhancing device performance.
Patent Information
- Application Number
- JP2023080022
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-15
- Publication Date
- 2024-11-27
AI Technical Summary
The boundary between 3C-SiC and 4H-SiC regions in semiconductor devices becomes vague, leading to a reduction in the degree of freedom in device design.
A SiC semiconductor device is designed with a first silicon carbide layer containing 4H structure and a second silicon carbide layer laminated on top containing 3C structure, with a clear boundary defined by interface S, and a manufacturing method that includes forming a drift layer, source extension and contact regions, and a gate electrode structure.
The design suppresses leakage current and maintains device design flexibility by clearly defining the 3C-SiC and 4H-SiC regions, reducing the risk of overestimating margins and maintaining device performance.
Smart Images

Figure 2024164506000001_ABST
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a silicon carbide (SiC) semiconductor device using SiC and a manufacturing method thereof. [Background technology]
[0002] Patent Document 1 discloses a semiconductor device in which an amorphous layer is formed by ion-implanting phosphorus into a hexagonal single crystal silicon carbide substrate, the amorphous layer is recrystallized into cubic single crystal n-type silicon carbide by heat treatment, and an electrode is formed by vapor-depositing nickel on the upper surface of the n-type silicon carbide.
[0003] Patent Document 2 describes a n-type 4H-SiC + The n-type SiC was formed on the first main surface. - In the epitaxial growth layer, + A type source region, + n-type source region + Type 3C-SiC region and p + and a n-type potential clamping region. + Type 3C-SiC region and p + A semiconductor device is disclosed in which a barrier metal film is formed in contact with a type potential fixing region, and a source wiring electrode is formed on the barrier metal film. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2009-49198 A [Patent Document 2] International Publication No. 2017 / 042963 Summary of the Invention [Problem to be solved by the invention]
[0005] If the boundary between the 3C-SiC region and the 4H-SiC region becomes unclear, there is a possibility that the freedom of device design will be reduced.
[0006] In view of the above-mentioned problems, an object of the present disclosure is to provide a SiC semiconductor device in which a reduction in the degree of freedom in device design is suppressed, and a manufacturing method thereof. [Means for solving the problem]
[0007] In order to achieve the above object, one aspect of the present disclosure is a SiC semiconductor device including: a first silicon carbide layer including silicon carbide of a 4H structure; a second silicon carbide layer including silicon carbide of a 3C structure stacked on an upper surface of the first silicon carbide layer; a drift layer of a first conductivity type provided on the first silicon carbide layer; a base region of a second conductivity type provided on an upper surface side of the drift layer in the first silicon carbide layer; a main region of the first conductivity type having a source extension region whose lower surface is in contact with the base region and provided in the first silicon carbide layer, and a source contact region whose lower surface is in contact with the source extension region and provided in the second silicon carbide layer; a gate insulating film provided inside a trench penetrating the main region and the base region; a gate electrode embedded inside the trench with the gate insulating film interposed therebetween; and a main electrode provided in contact with the source contact region.
[0008] In order to achieve the above object, another aspect of the present disclosure is a method for manufacturing a SiC semiconductor device, comprising: forming a first silicon carbide layer including silicon carbide of a 4H structure and including a drift layer of a first conductivity type; stacking a second silicon carbide layer including silicon carbide of a 3C structure on an upper surface of the first silicon carbide layer; forming a base region of a second conductivity type on an upper surface side of the drift layer in the first silicon carbide layer; forming a main region of a first conductivity type having a stacked structure of a source extension region and a source contact region across the first silicon carbide layer and the second silicon carbide layer; forming a trench penetrating the main region and the base region located on a lower surface side of the main region; forming a gate electrode inside the trench via a gate insulating film; and forming a main electrode so as to be in contact with an upper surface of the source contact region, wherein in the step of forming the main region, a source extension region is formed in the first silicon carbide layer and a source contact region is formed in the second silicon carbide layer. Effect of the Invention
[0009] According to the present disclosure, it is possible to provide a SiC semiconductor device in which a reduction in the degree of freedom in device design is suppressed, and a method for manufacturing the same. [Brief description of the drawings]
[0010] [Figure 1] 1 is a schematic plan view showing an example of a SiC semiconductor device according to a first embodiment. [Diagram 2] 2 is a longitudinal sectional view showing a sectional configuration when viewed in section along the AA cutting line in FIG. 1. [Diagram 3] FIG. 3 is an enlarged schematic cross-sectional view of a region B in FIG. [Figure 4] FIG. 4 is a schematic cross-sectional view of a SiC semiconductor device according to a comparative example. [Diagram 5] 1A to 1C are schematic cross-sectional views for illustrating an example of a method for manufacturing the SiC semiconductor device according to the first embodiment. [Figure 6] 6 is a schematic cross-sectional view continuing from FIG. 5 for illustrating an example of the method for manufacturing the SiC semiconductor device according to the first embodiment. FIG. [Figure 7] 7 is a schematic cross-sectional view continuing from FIG. 6 for illustrating the example of the method for manufacturing the SiC semiconductor device according to the first embodiment. FIG. [Figure 8] 8 is a schematic cross-sectional view continuing from FIG. 7 for illustrating an example of the method for manufacturing the SiC semiconductor device according to the first embodiment. FIG. [Figure 9] 9 is a schematic cross-sectional view continuing from FIG. 8 for illustrating the example of the method for manufacturing the SiC semiconductor device according to the first embodiment. FIG. [Figure 10] 10 is a schematic cross-sectional view continuing from FIG. 9 for illustrating an example of the method for manufacturing the SiC semiconductor device according to the first embodiment. FIG. [Figure 11] 11 is a schematic cross-sectional view continuing from FIG. 10 for illustrating the example of the method for manufacturing the SiC semiconductor device according to the first embodiment. FIG. [Figure 12] 12 is a schematic cross-sectional view continuing from FIG. 11 for illustrating the example of the method for manufacturing the SiC semiconductor device according to the first embodiment. FIG. [Figure 13]13 is a schematic cross-sectional view continuing from FIG. 12 for illustrating the example of the method for manufacturing the SiC semiconductor device according to the first embodiment. FIG. [Figure 14] 14 is a schematic cross-sectional view continuing from FIG. 13 for illustrating the example of the method for manufacturing the SiC semiconductor device according to the first embodiment. FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] Hereinafter, a first embodiment of the present disclosure will be described with reference to the drawings. In the description of the drawings, the same or similar parts are denoted with the same or similar reference numerals, and duplicated descriptions will be omitted. However, the drawings are schematic, and the relationship between thickness and planar dimensions, the ratio of thickness of each layer, etc. may differ from the actual ones. In addition, the drawings may include parts with different dimensional relationships and ratios. In addition, the first embodiment shown below is an example of an apparatus and method for embodying the technical idea of the present disclosure, and the technical idea of the present disclosure does not specify the material, shape, structure, arrangement, etc. of the components as described below.
[0012] In this specification, the source region of a metal-oxide semiconductor field-effect transistor (MOSFET) is "one main region (first main region)" that can be selected as the emitter region of an insulated gate bipolar transistor (IGBT). In addition, in a thyristor such as a MOS-controlled static induction thyristor (SI thyristor), the "one main region" can be selected as the cathode region. The drain region of a MOSFET is the "other main region (second main region)" of the semiconductor device that can be selected as the collector region in an IGBT and as the anode region in a thyristor. In this specification, when the term "main region" is used simply, it means either the first main region or the second main region that is appropriate from the technical common sense of a person skilled in the art.
[0013] In addition, the definitions of directions such as up and down in the following description are merely for convenience of explanation and do not limit the technical idea of the present disclosure. For example, if the object is rotated by 90° and observed, up and down are read as left and right, and if it is rotated by 180° and observed, up and down are read in reverse. Also, "upper surface" may be read as "front surface", and "lower surface" may be read as "back surface".
[0014] In the following description, the case where the first conductivity type is n-type and the second conductivity type is p-type will be exemplified. However, the conductivity types may be selected in the reverse relationship, with the first conductivity type being p-type and the second conductivity type being n-type. Also, the + and - attached to n and p mean semiconductor regions with relatively higher or lower impurity concentrations, respectively, compared to the semiconductor regions without the attached + and -. However, even for semiconductor regions with the same n attached, it does not mean that the impurity concentrations of the respective semiconductor regions are exactly the same.
[0015] SiC crystals have crystal polymorphs, and the main ones are cubic 3C, and hexagonal 4H and 6H. The reported values of the bandgap at room temperature are 2.23 eV for 3C-SiC, 3.26 eV for 4H-SiC, and 3.02 eV for 6H-SiC. In the following description, the cases mainly using 4H-SiC and 3C-SiC will be exemplified.
[0016] (First Embodiment) <Structure of SiC Semiconductor Device> The SiC semiconductor device (silicon carbide semiconductor device, semiconductor chip) 100 according to the first embodiment, as shown in FIG. 1, in a plan view, includes, for example, an active portion 101 having a rectangular planar shape, and a breakdown voltage structure portion 102 provided so as to surround the periphery of the active portion 101. Also, the SiC semiconductor device 100 includes, in a plan view, a region 103 provided so as to surround the active portion 101 between the active portion 101 and the breakdown voltage structure portion 102.
[0017] Fig. 2 is a cross-sectional view taken along line AA in Fig. 1. Note that part of active section 101 is omitted in Fig. 2. As shown in Fig. 2, active section 101 includes an active element, region 103 includes ring region 9b, and voltage withstand structure section 102 includes a plurality of electric field relaxation regions 9a (described later) as a termination structure.
[0018] The SiC semiconductor device 100 includes a trench-gate MOSFET as an active element, as shown in Fig. 2. Note that Fig. 2 illustrates a unit cell including an insulated gate electrode structure (7b, 7c) embedded in one trench 7a, but in reality, a large number of such unit cells are periodically arranged.
[0019] The SiC semiconductor device 100 also has a first silicon carbide layer 14 made of silicon carbide and a second silicon carbide layer 15 made of silicon carbide. The first silicon carbide layer 14 mainly contains 4H-SiC. The ratio of 4H-SiC contained in the first silicon carbide layer 14 is, for example, about 70% or more and 100% or less. The second silicon carbide layer 15 is a silicon carbide film laminated on the upper surface of the first silicon carbide layer 14 and contains 3C-SiC. The ratio of 3C-SiC contained in the second silicon carbide layer 15 is, for example, about 10% or more and 100% or less. Hereinafter, 3C-SiC may be referred to as a 3C structure, and 4H-SiC may be referred to as a 4H structure. The film thickness of the second silicon carbide layer 15 is almost uniform within the chip surface of the SiC semiconductor device 100.
[0020] The first silicon carbide layer 14 is provided across the active section 101, the breakdown voltage structure section 102, and the region 103. The second silicon carbide layer 15 is laminated on the upper surface of the first silicon carbide layer 14 across the active section 101, the breakdown voltage structure section 102, and the region 103. The boundary surface between the first silicon carbide layer 14 and the second silicon carbide layer 15 is called the boundary surface S. More specifically, the boundary surface between the upper surface of the first silicon carbide layer 14 and the lower surface of the second silicon carbide layer 15 is called the boundary surface S. The boundary surface S can be confirmed when observing the vertical cross section of the SiC semiconductor device 100. As shown in FIG. 2, the boundary surface S appears linear when viewed in cross section, depending on the surface condition of the upper surface of the first silicon carbide layer 14, for example. Moreover, at least an upper surface side portion (a portion opposite to the first silicon carbide layer 14 side) of the second silicon carbide layer 15 contains 3C-SiC.
[0021] The SiC semiconductor device 100 includes an active section 101, a breakdown voltage structure section 102, and a first conductivity type (n - The drift layer 2 is provided on a first silicon carbide layer 14. The drift layer 2 is formed of an epitaxially grown layer made of SiC such as 4H—SiC. The impurity concentration of the drift layer 2 is, for example, 1×10 15 cm -3 That's it, 5 x 10 16 cm -3 The thickness of the drift layer 2 is, for example, about 1 μm or more and 100 μm or less. The impurity concentration and thickness of the drift layer 2 can be appropriately adjusted according to the withstand voltage specifications and the like.
[0022] A current spreading layer (CSL) 3 of a first conductivity type (n-type) having a higher impurity concentration than the drift layer 2 is selectively provided on the upper surface side of the drift layer 2 across the active portion 101 and the region 103. The current spreading layer 3 is provided on the first silicon carbide layer 14. The lower surface of the current spreading layer 3 is in contact with the upper surface of the drift layer 2. The current spreading layer 3 is formed by, for example, N ion implantation. The impurity concentration of the current spreading layer 3 is, for example, 5×10 16 cm -3 That's it, 5 x 10 17 cm -3It is to be noted that the current diffusion layer 3 does not necessarily have to be provided, and when the current diffusion layer 3 is not provided, the drift layer 2 may be provided up to the region of the current diffusion layer 3.
[0023] In the active portion 101, base regions 5a, 5b of a second conductivity type (p-type) are selectively provided on the upper surface side of the current diffusion layer 3. The base regions 5a, 5b are provided in the first silicon carbide layer 14. The lower surfaces of the base regions 5a, 5b are in contact with the upper surface of the current diffusion layer 3. When the current diffusion layer 3 is not provided, the lower surfaces of the base regions 5a, 5b are in contact with the upper surface of the drift layer 2. The base regions 5a, 5b are, for example, regions made of SiC in which p-type impurities such as aluminum are ion-implanted into the current diffusion layer 3. The base regions 5a, 5b may be formed of epitaxially grown layers made of SiC such as 4H-SiC. The impurity concentration of the base regions 5a, 5b is, for example, 1×10 16 cm -3 That's it, 1×10 18 cm -3 It is about the following.
[0024] In the active portion 101, the upper surface side of the base regions 5a and 5b is provided with a first conductivity type (n + First main regions (source regions) 6a, 6b of n-type (type) are selectively provided. The source regions 6a, 6b are provided across the first silicon carbide layer 14 and the second silicon carbide layer 15. The source regions 6a, 6b are, for example, regions made of SiC into which n-type impurities are ion-implanted in a region across the second silicon carbide layer 15 and the current spreading layer 3. The n-type impurities include, for example, phosphorus (P) or nitrogen (N). The source regions 6a, 6b may include arsenic (As) as the n-type impurity. The impurity concentration of the source regions 6a, 6b is, for example, 2×10 19 cm -3 That's it, 1×10 20 cm -3 It is less than that.
[0025] The source region 6a is the lower layer + The source extension region 61a and the upper layer +The source extension region 61a has a two-layered structure in which the source region 6b is a lower layer and the source contact region 62a is a lower layer. The lower surface of the source extension region 61a is in contact with the upper surface of the base region 5a. The upper surface of the source extension region 61a is in contact with the lower surface of the source contact region 62a. The source region 6b is + The source extension region 61b is a n-type + The source extension region 61b has a two-layered structure in which the source extension region 61b is in contact with the upper surface of the base region 5b and the source contact region 62b is in contact with the lower surface of the source contact region 62b.
[0026] The source extension regions 61a and 61b of the source regions 6a and 6b are provided in the first silicon carbide layer 14, and the source contact regions 62a and 62b are provided in the second silicon carbide layer 15. In other words, the portions of the source regions 6a and 6b provided in the first silicon carbide layer 14 are called the source extension regions 61a and 61b, and the portions of the source regions 6a and 6b provided in the second silicon carbide layer 15 are called the source contact regions 62a and 62b. The source extension region 61a and the source contact region 62a, and the source extension region 61b and the source contact region 62b are defined by a boundary surface S. The source extension regions 61a and 61b do not include the second silicon carbide layer 15. Therefore, the source extension regions 61a and 61b do not include a mixed crystal of 3C-SiC and 4H-SiC, or even if they include a mixed crystal of 3C-SiC and 4H-SiC, the amount is small.
[0027] The source contact regions 62a, 62b include 3C-SiC. The ratio of 3C-SiC included in the source contact regions 62a, 62b is the same as that of the second silicon carbide layer 15, and is, for example, about 10% or more and 100% or less. When the ratio of 3C-SiC is 100%, the source contact regions 62a, 62b and the second silicon carbide layer 15 are made of 3C-SiC. When the ratio of 3C-SiC is less than 100%, the source contact regions 62a, 62b and the second silicon carbide layer 15 may include a mixed crystal of 3C-SiC and 4H-SiC. The source contact regions 62a, 62b are formed from the upper surface to the lower surface of the second silicon carbide layer 15. Therefore, the dimension of the source contact regions 62a, 62b along the depth direction is the same as that of the second silicon carbide layer 15.
[0028] As shown in FIG. 2, a trench 7a is provided penetrating the source regions 6a, 6b and the base regions 5a, 5b from the upper surfaces of the source regions 6a, 6b toward the normal direction (depth direction) of the upper surfaces of the source regions 6a, 6b. The lower surface of the trench 7a reaches the current diffusion layer 3. The width of the trench 7a is, for example, about 1 μm or less. The source region 6a and the base region 5a are in contact with the left side surface of the trench 7a. The source region 6b and the base region 5b are in contact with the right side surface of the trench 7a. The trench 7a may have a planar pattern extending in a stripe shape in the depth direction and the front direction of the paper surface of FIG. 2, or may have a dot-shaped planar pattern.
[0029] A gate insulating film 7b is provided along the bottom surface and both side surfaces of the trench 7a. A gate electrode 7c is embedded inside the trench 7a via the gate insulating film 7b. The gate insulating film 7b and the gate electrode 7c form a trench-gate insulated gate electrode structure (7b, 7c).
[0030] As the gate insulating film 7b, in addition to a silicon oxide film (SiO2 film), a silicon oxynitride (SiON) film, a strontium oxide (SrO) film, a silicon nitride (Si3N4) film, an aluminum oxide (Al2O3) film, a magnesium oxide (MgO) film, an yttrium oxide (Y2O3) film, a hafnium oxide (HfO2) film, a zirconium oxide (ZrO2) film, a tantalum oxide (Ta2O5) film, a bismuth oxide (Bi2O3) film, or a composite film obtained by stacking a plurality of these films can be used. As the material of the gate electrode 7c, for example, a polysilicon layer (doped polysilicon layer) to which p-type impurities or n-type impurities are added at a high impurity concentration, or a high melting point metal such as titanium (Ti), tungsten (W), or nickel (Ni) can be used.
[0031] Inside the current spreading layer 3 and at the bottom of the trench 7a, a second conductivity type (p + The gate bottom protection region 4 is provided in the first silicon carbide layer 14. The upper surface of the gate bottom protection region 4 is in contact with the lower surface of the trench 7a. The upper surface of the gate bottom protection region 4 does not have to be in contact with the lower surface of the trench 7a. The impurity concentration of the gate bottom protection region 4 is, for example, 1×10 17 cm -3 That's it, 1×10 19 cm -3 The gate bottom protection region 4 is, for example, a region made of SiC with p-type impurity ions implanted into the current diffusion layer 3. The gate bottom protection region 4 is electrically connected to the source wiring electrode 12 at a portion not shown, and has the function of depleting when the MOSFET is turned off to relieve the electric field applied to the bottom surface of the trench 7a.
[0032] Buried regions 81a, 81b of a second conductivity type (p-type) are selectively provided on the upper surface side of the current diffusion layer 3 in contact with the base regions 5a, 5b. The buried regions 81a, 81b are provided in the first silicon carbide layer 14. The lower surfaces of the buried regions 81a, 81b are in contact with the current diffusion layer 3. The side surface of the buried region 81a is in contact with the current diffusion layer 3 and the base region 5a, and the side surface of the buried region 81b is in contact with the current diffusion layer 3 and the base region 5b. The buried regions 81a, 81b are, for example, regions made of SiC in which p-type impurities are ion-implanted into the current diffusion layer 3. The impurity concentrations of the buried regions 81a, 81b are, for example, 5×10 17 cm -3 That's it, 1×10 19 cm -3 It is about the following.
[0033] The upper surface side of the buried regions 81a and 81b is provided with p + P-type base contact regions 82a, 82b are selectively provided. The base contact regions 82a, 82b are provided in the second silicon carbide layer 15. The lower surface of the base contact region 82a contacts the upper surface of the buried region 81a, and the side surface of the base contact region 82a contacts the source region 6a. The lower surface of the base contact region 82b contacts the upper surface of the buried region 81b, and the side surface of the base contact region 82b contacts the source region 6b. The base contact region 82a is electrically connected to the base region 5a, and the base contact region 82b is electrically connected to the base region 5b. The base contact regions 82a, 82b are, for example, regions made of SiC obtained by ion-implanting p-type impurities into the second silicon carbide layer 15. The impurity concentrations of the base contact regions 82a, 82b are, for example, 2×10 19 cm -3 That's it, 1×10 20 cm -3 It is less than that.
[0034] The buried regions 81a, 81b and the base contact regions 82a, 82b are regions made of p-type SiC into which p-type impurities are ion-implanted across the second silicon carbide layer 15 and the first silicon carbide layer 14. Of the regions made of p-type SiC, the portions provided in the first silicon carbide layer 14 are called buried regions 81a, 81b, and the portions provided in the second silicon carbide layer 15 are called base contact regions 82a, 82b. The buried region 81a and the base contact region 82a, and the buried region 81b and the base contact region 82b are defined by a boundary surface S. The buried regions 81a, 81b do not include the second silicon carbide layer 15. Therefore, the buried regions 81a, 81b do not include a mixed crystal of 3C-SiC and 4H-SiC, or even if they include a mixed crystal of 3C-SiC and 4H-SiC, the amount is small.
[0035] The base contact regions 82a, 82b contain 3C-SiC. The ratio of 3C-SiC contained in the base contact regions 82a, 82b is the same as that of the second silicon carbide layer 15, and is, for example, about 10% or more and 100% or less. When the ratio of 3C-SiC is 100%, the base contact regions 82a, 82b and the second silicon carbide layer 15 are made of 3C-SiC. When the ratio of 3C-SiC is less than 100%, the base contact regions 82a, 82b and the second silicon carbide layer 15 may contain a mixed crystal of 3C-SiC and 4H-SiC. Since the base contact regions 82a, 82b contain 3C-SiC, the contact resistance with the source electrodes (11, 12) described later can be suppressed. Moreover, the base contact regions 82a, 82b are formed from the upper surface to the lower surface of the second silicon carbide layer 15. Therefore, the dimensions along the depth direction of the base contact regions 82a, 82b are the same as those of the second silicon carbide layer 15 and the source contact regions 62a, 62b.
[0036] FIG. 3 is an enlarged view of region B in FIG. 2. The configurations of the gate electrode 7c and the source region 6a will be described in more detail with reference to FIG. 3. The dimension of the source contact region 62a and the second silicon carbide layer 15 along the depth direction is defined as d1. The dimension d1 is, for example, about 0.2 μm or more and about 0.5 μm or less. The dimension of the source region 6a along the depth direction is defined as d2. The dimension d2 is, for example, about 1 μm. The source contact region 62a contains 3C-SiC, and thus can be in ohmic contact with the source electrodes (11, 12) with low resistance.
[0037] Moreover, the upper surface (upper end) 7d of the gate electrode 7c at the position of its end in contact with the gate insulating film 7b is located deeper than the lower surface (lower end) 62x of the source contact region 62a at the position of its end in contact with the gate insulating film 7b. In other words, the upper surface 7d of the gate electrode 7c at the position of its end in contact with the gate insulating film 7b is located deeper than the boundary surface S. Moreover, the upper surface (upper end) 7d of the gate electrode 7c at the position of its end in contact with the gate insulating film 7b is located shallower than the lower surface of the source extension region 61a, more specifically, the lower surface (lower end) 61x of the source extension region 61a at the position of its end in contact with the gate insulating film 7b.
[0038] The upper surface 7d of the gate electrode 7c at the position where it contacts the gate insulating film 7b may be the uppermost surface of the gate electrode 7c. For example, when the upper surface of the gate electrode 7c as a whole is a downwardly convex curved surface, the upper surface of the central part of the gate electrode 7c may be located deeper than the upper surfaces 7d of the ends of the gate electrode 7c.
[0039] The gate electrode 7c and the source extension region 61a face each other with the gate insulating film 7b therebetween. More specifically, the gate electrode 7c and the first silicon carbide layer 14 face each other with the gate insulating film 7b therebetween. The gate electrode 7c and the source contact region 62a do not face each other with the gate insulating film 7b therebetween. More specifically, the gate electrode 7c and the second silicon carbide layer 15 do not face each other with the gate insulating film 7b therebetween. The source contact region 62a faces the insulating film 10 with the gate insulating film 7b therebetween. More specifically, the second silicon carbide layer 15 faces the insulating film 10 with the gate insulating film 7b therebetween. The amount of depression d0 of the gate electrode 7c from the upper surface of the source contact region 62a is larger than the dimension d1 along the depth direction of the source contact region 62a and the second silicon carbide layer 15 (d1 < d0). The amount of depression d0 of the gate electrode 7c and the position of the upper surface 7d of the position where the gate electrode 7c contacts the gate insulating film 7b can be controlled, for example, by adjusting the etching conditions of the gate electrode 7c. Since the source extension region 61a contains little or no 3C-SiC, it has fewer crystal defects than the source contact region 62a.
[0040] Since the source extension region 61b and the source contact region 62b of the source region 6b shown in FIG. 2 have the same configurations as the source extension region 61a and the source contact region 62a of the source region 6a, respectively, duplicate descriptions are omitted. Also, since the positional relationships between the source extension region 61b and the source contact region 62b of the source region 6b and the gate electrode 7c are the same as the positional relationships between the source extension region 61a and the source contact region 62a of the source region 6a and the gate electrode 7c, respectively, duplicate descriptions are omitted.
[0041] As shown in FIG. 2, in the breakdown voltage structure 102, a plurality of electric field relaxation regions 9a of a second conductivity type (p type) are selectively provided on the upper surface side of the drift layer 2. In the example shown in FIG. 2, three electric field relaxation regions 9a are provided on the upper surface side of the drift layer 2. Although not shown, the electric field relaxation regions 9a are concentric guard rings (field limiting rings) in a plan view. The electric field relaxation regions 9a are separated from each other by the drift layer 2. The lower surfaces of the electric field relaxation regions 9a are in contact with the upper surface of the drift layer 2. The electric field relaxation regions 9a are, for example, regions made of SiC obtained by ion-implanting p-type impurities such as aluminum into the drift layer 2 and the second silicon carbide layer 15.
[0042] The electric field relaxation region 9a is provided across the second silicon carbide layer 15 and the first silicon carbide layer 14 in the depth direction. Of the electric field relaxation region 9a, a portion provided in the first silicon carbide layer 14 is referred to as a first portion 91a, and a portion provided in the second silicon carbide layer 15 is referred to as a second portion 92a. The first portion 91a and the second portion 92a are defined by a boundary surface S. The dimension of the second portion 92a in the depth direction is the same as that of the second silicon carbide layer 15. The first portion 91a is, for example, a p-type whose impurity concentration is approximately the same as that of the buried regions 81a and 81b. The second portion 92a is, for example, a p-type whose impurity concentration is approximately the same as that of the base contact regions 82a and 82b. + It is a type.
[0043] In the breakdown voltage structure 102, the drift layer 2 has a first conductivity type (n +The channel stopper region 6c is provided so as to go around the outer periphery of the breakdown voltage structure 102 in a plan view, and its lower surface is in contact with the upper surface of the drift layer 2. Of the channel stopper region 6c, a portion provided in the first silicon carbide layer 14 is called a first portion 6c1, and a portion provided in the second silicon carbide layer 15 is called a second portion 6c2. The first portion 6c1 and the second portion 6c2 are defined by a boundary surface S. The channel stopper region 6c is, for example, a region made of 3C-SiC obtained by ion-implanting n-type impurities into the drift layer 2 and the second silicon carbide layer 15. The impurity concentrations of the first portion 6c1 and the second portion 6c2 are, for example, approximately the same as the impurity concentrations of the source regions 6a and 6b.
[0044] In region 103, a ring region 9b of a second conductivity type (p-type) is selectively provided on the upper surface side of the drift layer 2. The lower surface of ring region 9b is in contact with the upper surface of the drift layer 2. Ring region 9b is, for example, a region made of SiC into which p-type impurities are ion-implanted into the drift layer 2. Although not shown in the figure, ring region 9b is a ring-shaped portion that surrounds the edge of active portion 101 in a plan view.
[0045] The ring region 9b is provided across the second silicon carbide layer 15 and the first silicon carbide layer 14 in the depth direction. A portion of the ring region 9b provided in the first silicon carbide layer 14 is referred to as a first portion 91b, and a portion of the ring region 9b provided in the second silicon carbide layer 15 is referred to as a second portion 92b. The first portion 91b and the second portion 92b are defined by a boundary surface S. The dimension of the second portion 92b in the depth direction is the same as that of the second silicon carbide layer 15. The first portion 91b is, for example, a p-type whose impurity concentration is approximately the same as that of the buried regions 81a, 81b. The second portion 92b is, for example, a p-type whose impurity concentration is approximately the same as that of the base contact regions 82a, 82b. + It is a type.
[0046] An insulating film 10 is selectively provided on the upper surface of the gate electrode 7c, the upper surface of the region 103, and the upper surface of the breakdown voltage structure 102. In the breakdown voltage structure 102, the insulating film 10 is provided on the upper surface of the electric field relaxation region 9a. More specifically, the insulating film 10 is provided at a position covering the second portion 92a of the electric field relaxation region 9a. The insulating film 10 is composed of a single layer film such as a silicon oxide film (BPSG film) doped with boron (B) and phosphorus (P), a silicon oxide film (PSG film) doped with phosphorus (P), a non-doped silicon oxide film called "NSG" that does not contain phosphorus (P) or boron (B), a silicon oxide film (BSG film) doped with boron (B), a silicon nitride film (Si3N4 film), or a laminated film thereof. The insulating film 10 is provided with contact holes 10a and 10b so as to expose the upper surfaces of the source regions 6a and 6b and the base contact regions 82a and 82b. Furthermore, a contact hole 10c is provided in the insulating film 10 so as to expose the upper surface of the ring region 9b, more specifically, the upper surface of the second portion 92b.
[0047] A first main electrode (source electrode) (11, 12) is provided so as to cover the insulating film 10, the upper surfaces of the source regions 6a, 6b and the base contact regions 82a, 82b exposed from the contact holes 10a, 10b, and the upper surface of the ring region 9b exposed from the contact hole 10c. The source electrodes (11, 12) include a lower barrier metal layer 11 and an upper source wiring electrode 12. For example, the barrier metal layer 11 is made of a metal such as titanium nitride (TiN), titanium (Ti), or a TiN / Ti laminated structure with Ti as the lower layer. The barrier metal layer 11 is in direct contact with the upper surfaces of the source contact regions 62a, 62b and the upper surfaces of the base contact regions 82a, 82b, and is in ohmic contact with the source contact regions 62a, 62b and the base contact regions 82a, 82b with low resistance. The barrier metal layer 11 is in direct contact with the second portion 92b of the ring region 9b and is in ohmic contact with the second portion 92b with low resistance. The electric field relaxation region 9a is not in contact with the barrier metal layer 11 because the upper surface of the second portion 92a is covered with the insulating film 10.
[0048] The source wiring electrode 12 is electrically connected to the source regions 6a and 6b, the base contact regions 82a and 82b, and the ring region 9b via a barrier metal layer 11. The source wiring electrode 12 is provided separately from a gate wiring electrode (not shown) electrically connected to the gate electrode 7c. The source wiring electrode 12 is made of a metal such as aluminum (Al), aluminum-silicon (Al-Si), aluminum-copper (Al-Cu), or copper (Cu).
[0049] The lower surface side of the drift layer 2 is provided with a first conductivity type (n + The drain region 1 is formed of a semiconductor substrate (SiC substrate) made of, for example, 4H—SiC. The impurity concentration of the drain region 1 is, for example, 1×10 18 cm -3 That's it, 3 x 10 20 cm -3 The thickness of the drain region 1 is, for example, about 30 μm or more and 500 μm or less. Between the drift layer 2 and the drain region 1, a layer having a higher impurity concentration than the drift layer 2 and a lower impurity concentration than the drain region 1 is provided. A dislocation conversion layer or a recombination promotion layer, which is an n-type buffer layer with a low impurity concentration, may be provided.
[0050] A second main electrode (drain electrode) 13 is provided on the lower surface side of the drain region 1. As the drain electrode 13, for example, a single layer film made of gold (Au) or a metal film laminated in the order of titanium (Ti), nickel (Ni) and Au from the drain region 1 side can be used, and further a metal film of molybdenum (Mo), tungsten (W) or the like may be laminated on the bottom layer. In addition, nickel silicide (NiSi x A drain contact layer such as a SiO 2 film may be provided.
[0051] During operation of the SiC semiconductor device according to the first embodiment, when the source electrodes (11, 12) are set to earth potential, a positive voltage is applied to the drain electrode 13, and a positive voltage equal to or greater than a threshold is applied to the gate electrode 7c, an inversion layer (channel) is formed on the side of the trench 7a in the base regions 5a, 5b, resulting in an ON state. In the ON state, a current flows from the drain electrode 13 to the source electrode (11, 12) via the drain region 1, the drift layer 2, the current diffusion layer 3, the inversion layer in the base regions 5a, 5b, and the source regions 6a, 6b. On the other hand, when the voltage applied to the gate electrode 7c is less than the threshold, an inversion layer is not formed in the base regions 5a, 5b, resulting in an OFF state, and no current flows from the drain electrode 13 to the source electrode (11, 12).
[0052] According to the SiC semiconductor device of the first embodiment, the source regions 6a, 6b have a two-layer structure of a source extension region 61a and a source contact region 62a, and the upper source extension region 61a in contact with the source electrodes (11, 12) contains 3C-SiC, so that the source contact region 62a can make ohmic contact with the source electrodes (11, 12) with low resistance without forming a silicide layer such as nickel (Ni) silicide. Therefore, problems such as peeling of the silicide layer can be suppressed compared to the case where a silicide layer is formed.
[0053] 4, consider a case where the source region 6x containing 3C-SiC is formed in a single layer structure and faces the gate electrode 7c via the gate insulating film 7b. In this case, since the source region 6x contains 3C-SiC, the source region 6x can make ohmic contact with the source electrode (11, 12). However, since 3C-SiC has more crystal defects and a larger surface unevenness than 4H-SiC, there is a risk that a leakage current i will flow between the gate electrode 7c and the source region 6x.
[0054] In contrast, according to the SiC semiconductor device 100 of the first embodiment, as shown in FIG. 3, the upper surface 7d of the gate electrode 7c at the position where the gate electrode 7c contacts the gate insulating film 7b is made deeper than the boundary surface S between the first silicon carbide layer 14 and the second silicon carbide layer 15 and shallower than the lower surface 61x of the source extension region 61a. As a result, the source extension region 61a provided in the first silicon carbide layer 14 having fewer crystal defects in the source region 6a faces the gate electrode 7c through the gate insulating film 7b, and the source contact region 62a provided in the second silicon carbide layer 15 having more crystal defects in the source region 6a does not face the gate electrode 7c through the gate insulating film 7b. This makes it possible to suppress the generation of a leak current between the source region 6a and the gate electrode 7c.
[0055] In addition, conventionally, an amorphous layer is formed by ion-implanting phosphorus into a hexagonal single crystal silicon carbide substrate, and the amorphous layer is recrystallized into a cubic single crystal n-type silicon carbide by heat treatment. However, when impurities are ion-implanted, the boundary between the region with high impurity concentration and the region with low impurity concentration in SiC is unclear. Therefore, in the SiC after heat treatment, the boundary between the region containing 3C-SiC and the region containing almost no 3C-SiC may become unclear. In addition, a planar type SiC semiconductor device has a gate electrode on the top surface of SiC, but in a trench type SiC semiconductor device, the gate electrode is provided inside the trench along the depth direction (thickness direction). Therefore, it was necessary to separately create a region containing 3C-SiC and a region of 4H-SiC along the depth direction to suppress contact resistance. In general, in the ion implantation of impurities, it is more difficult to control the impurity concentration in the depth direction than the impurity concentration in the lateral direction. More specifically, the impurity concentration in the lateral direction can be controlled by using a mask pattern, for example. On the other hand, since the control of the impurity concentration in the depth direction is achieved by adjusting the dose amount of the impurity and the acceleration energy, the control of the impurity concentration in the depth direction is more difficult than the control of the impurity concentration in the lateral direction. Therefore, in a trench-type SiC semiconductor device, it may not be easy to identify the boundary between the region containing 3C-SiC and the region containing almost no 3C-SiC, and the margin may be estimated to be large in order to suppress the leakage current i, and the drop amount d0 of the gate electrode 7c from the upper surface of the source contact region 62a may be set to be large. In this way, the degree of freedom in device design may be reduced.
[0056] On the other hand, the SiC semiconductor device 100 according to the first embodiment has a stacked structure including a first silicon carbide layer 14 containing silicon carbide with a 4H structure and a second silicon carbide layer 15 laminated on the upper surface of the first silicon carbide layer 14 and made of silicon carbide containing 3C-SiC. Therefore, the boundary between the region containing 3C-SiC and the region mainly composed of silicon carbide with a 4H structure is made clear by the boundary surface S. And in the region deeper than the boundary surface S, it can be seen that it does not contain a mixed crystal of 3C-SiC and 4H-SiC, or even if it contains a mixed crystal of 3C-SiC and 4H-SiC, it is only a small amount. So, the upper surface 7d at the position in contact with the gate insulating film 7b of the gate electrode 7c may be designed to be provided at a position deeper than the boundary surface S. Thereby, the leakage current i can be suppressed without overestimating the margin, and the reduction in the degree of freedom of device design can be suppressed.
[0057] <Manufacturing method of SiC semiconductor device> Next, an example of the manufacturing method of the SiC semiconductor device according to the first embodiment will be described. Note that the manufacturing method of the SiC semiconductor device described below is an example, and it goes without saying that it can be realized by various other manufacturing methods including this modification within the scope of the gist described in the claims.
[0058] First, as shown in FIG. 5, an n-type 4H-SiC semiconductor substrate (SiC substrate) 1 doped with an n-type impurity such as nitrogen (N) is prepared. The upper surface of the SiC substrate 1 has an off-angle of, for example, 3 degrees to 8 degrees from the {0001} plane. Then, an n-type drift layer 2 made of 4H-SiC doped with an n-type impurity such as N and having a lower impurity concentration than the SiC substrate 1 is epitaxially grown on the upper surface of the SiC substrate 1. Thereby, the first silicon carbide layer 14 is obtained. + type of 4H-SiC semiconductor substrate (SiC substrate) 1 doped with an n-type impurity such as nitrogen (N) is prepared. The upper surface of the SiC substrate 1 has an off-angle of, for example, 3 degrees to 8 degrees from the {0001} plane. Then, an n-type drift layer 2 made of 4H-SiC doped with an n-type impurity such as N and having a lower impurity concentration than the SiC substrate 1 is epitaxially grown on the upper surface of the SiC substrate 1. Thereby, the first silicon carbide layer 14 is obtained. - type of 4H-SiC semiconductor substrate (SiC substrate) 1 doped with an n-type impurity such as nitrogen (N) is prepared. The upper surface of the SiC substrate 1 has an off-angle of, for example, 3 degrees to 8 degrees from the {0001} plane. Then, an n-type drift layer 2 made of 4H-SiC doped with an n-type impurity such as N and having a lower impurity concentration than the SiC substrate 1 is epitaxially grown on the upper surface of the SiC substrate 1. Thereby, the first silicon carbide layer 14 is obtained.
[0059] 6, a mask pattern 20 made of a photoresist film is formed on the upper surface of the drift layer 2 by photolithography. Then, using the mask pattern 20 as an ion implantation mask, an n-type current diffusion layer 3 made of 4H—SiC is formed by ion implanting n-type impurities such as nitrogen (N) into the upper part of the drift layer 2. Thereafter, the mask pattern 20 is removed. The mask pattern 20 may be a hard mask pattern made of, for example, an oxide film.
[0060] 7, a mask pattern 21 made of a photoresist film is formed on the upper surface of the drift layer 2. Then, using the mask pattern 21 as an ion implantation mask, p-type impurities such as aluminum (Al) are selectively ion-implanted to selectively form the gate bottom protection region 4. In this case, the aluminum ion implantation is performed at a high acceleration energy of, for example, 780 keV or more and 960 keV or less, since it is an implantation into a deep region. Then, the mask pattern 21 is removed.
[0061] 8, a mask pattern 22 made of a photoresist film is formed on the upper surface of the drift layer 2. Then, using the mask pattern 22 as an ion implantation mask, n-type impurities such as phosphorus (P) and nitrogen (N) are selectively ion-implanted. The dose during ion implantation is, for example, 2×10 15 cm -2 As a result, in the first silicon carbide layer 14, the n + A source extension region 61 of the n-type is selectively formed on the upper surface side of the drift layer 2 in the breakdown voltage structure 102. + The first portion 6c1 of the mold is formed. After that, the mask pattern 22 is removed. The mask pattern 22 may be a hard mask pattern made of, for example, an oxide film.
[0062] Next, as shown in FIG. 9, a mask pattern 23 made of a photoresist film is formed on the upper surface of the drift layer 2. Then, p-type impurities such as aluminum (Al) are selectively ion-implanted using the mask pattern 23 as an ion implantation mask. As a result, as shown in FIG. 9, a base region 5 is selectively formed on the upper surface side of the current diffusion layer 3 in the active portion 101 and on the lower surface side of the source extension region 61. This base region 5 becomes the region with the lowest impurity concentration among the regions formed with the p-type impurities. Then, the mask pattern 23 is removed. The mask pattern 23 may be, for example, a hard mask pattern made of an oxide film.
[0063] 10, in order to form the second silicon carbide layer 15, an amorphous film 15a made of SiC is formed on the upper surface of the first silicon carbide layer 14. The amorphous film 15a is an n-type amorphous film made of SiC doped with an n-type impurity such as N. - The amorphous film 15a is n-type SiC, and the concentration of n-type impurities is approximately the same as that of the drift layer 2. The amorphous film 15a is formed by plasma enhanced CVD (plasma enhanced chemical vapor deposition) or sputtering. The amorphous film 15a is formed by plasma enhanced chemical vapor deposition at a temperature of, for example, 300° C. or higher and 650° C. or lower. The amorphous film 15a is formed by sputtering at a lower temperature than that of plasma enhanced chemical vapor deposition, for example, at room temperature.
[0064] Next, as shown in FIG. 11, a mask pattern 24 made of a photoresist film is formed on the upper surface of the amorphous film 15a. The mask pattern 24 has openings at positions where the source extension region 61 and the first portion 6c1 overlap. Then, using the mask pattern 24 as an ion implantation mask, n-type impurities such as phosphorus (P) and nitrogen (N) are selectively ion-implanted. The dose amount during ion implantation is set to be approximately the same as the dose amount used when the source extension region 61 and the first portion 6c1 were formed. As a result, n-type impurities are implanted into the amorphous film 15a on the upper surface side of the source extension region 61. +A source contact region 62 of n-type is selectively formed on the upper surface side of the first portion 6c1. + A second portion 6c2 of the mold is formed. The source extension region 61 and the source contact region 62 form the source region 6, and the first portion 6c1 and the second portion 6c2 form the channel stopper region 6c. Thereafter, the mask pattern 24 is removed. The mask pattern 24 may be a hard mask pattern made of, for example, an oxide film.
[0065] Next, as shown in FIG. 12, the buried regions 81a, 81b, the base contact regions 82a, 82b, the electric field relaxation region 9a, and the ring region 9b are formed. More specifically, the ion implantation for the process of forming the buried regions 81a, 81b and the base contact regions 82a, 82b and the ion implantation for the process of forming the electric field relaxation region 9a and the ring region 9b are performed simultaneously. First, a mask pattern 25 made of a photoresist film is formed on the upper surface of the amorphous film 15a by using a photolithography technique. The mask pattern 25 may be a hard mask pattern made of, for example, an oxide film. The mask pattern 25 has an opening at a position where the base contact regions 82a, 82b are formed in the active portion 101, an opening at a position where the electric field relaxation region 9a is formed in the voltage resistant structure portion 102, and an opening at a position where the ring region 9b is formed in the region 103.
[0066] Then, using the mask pattern 25 as an ion implantation mask, p-type impurities such as aluminum (Al) are selectively ion-implanted. By performing ion implantation in multiple stages, the impurity concentration on the upper surface side of the SiC is made higher than that at deeper positions. For example, in a region close to the upper surface side of the SiC, the dose is set to, for example, 2×10 15 cm -2The dose is set to be less than about 100 nm. In a deep region away from the upper surface side of the SiC, the dose may be set to be less than the above-mentioned value. As a result, in the first silicon carbide layer 14, buried regions 81a, 81b are formed on the upper surface side of the current spreading layer 3 in the active portion 101 so as to contact the base region 5. Then, base contact regions 82a, 82b are formed in the amorphous film 15a on the upper surface sides of the buried regions 81a, 81b so as to contact the source region 6.
[0067] Also, in the breakdown voltage structure 102, an electric field relaxation region 9a is formed. More specifically, in the first silicon carbide layer 14, a first portion 91a of the electric field relaxation region 9a is formed on the upper surface side of the current diffusion layer 3, and a second portion 92a is formed in the amorphous film 15a on the upper surface side of the first portion 91a. Then, in the region 103, a ring region 9b is formed. More specifically, in the first silicon carbide layer 14, a first portion 91b of the ring region 9b is formed on the upper surface side of the current diffusion layer 3, and a second portion 92b is formed in the amorphous film 15a on the upper surface side of the first portion 91b. Then, the mask pattern 25 is removed.
[0068] Next, an activation annealing (heat treatment) process is performed. In this activation annealing process, for example, activation annealing is performed at a temperature of 1400° C. or higher and 1900° C. or lower to simultaneously activate p-type impurities or n-type impurities ion-implanted into the gate bottom protection region 4, the base region 5, the source region 6, the buried regions 81a, 81b, the base contact regions 82a, 82b, the electric field relaxation region 9a, the ring region 9b, and the like. In addition, the amorphous film 15a is recrystallized by being heat-treated at a temperature of, for example, 1200° C. or higher, and at least a part of it becomes 3C-SiC. Therefore, by performing the above-mentioned activation annealing, the amorphous film 15a can be recrystallized to obtain the second silicon carbide layer 15. That is, it is not necessary to separately perform heat treatment to recrystallize the amorphous film 15a. As a result, at least a part of each of the source contact region 62, base contact regions 82a, 82b, and second portions 92a, 92b, 6c2 formed in the second silicon carbide layer 15 becomes 3C-SiC. The source extension region 61, buried regions 81a, 81b, and first portions 91a, 91b, 6c1 formed in the first silicon carbide layer 14 remain as 4H-SiC even after the activation annealing.
[0069] In this example, a single activation anneal is performed after all the ion implantation steps, but multiple activation anneal may be performed separately after each ion implantation step. The order of the ion implantation steps may be changed in some cases. Before the activation anneal, a cap film made of carbon (C) may be formed, and activation anneal may be performed in a state covered with the cap film, and the cap film may be removed after the activation anneal.
[0070] Next, as shown in FIG. 13, a trench forming process is performed. In this trench forming process, a hard mask pattern made of, for example, an oxide film is formed on the upper surface of the SiC using photolithography, dry etching, CVD, and the like. The hard mask pattern has an opening at a position where the trench is to be formed. Then, using the hard mask pattern as an etching mask, a trench 7a is selectively formed in the depth direction from the upper surface of the source region 6 by dry etching such as reactive ion etching (RIE). Note that a photoresist film may be used as an etching mask instead of the hard mask pattern. The trench 7a penetrates the source region 6 and the base region 5, and further excavates the upper portion of the current diffusion layer 3 to reach the gate bottom protection region 4. The source region 6 is divided into source regions 6a and 6b, and the base region 5 is divided into base regions 5a and 5b. Then, the etching mask is removed.
[0071] Next, a gate insulating film / gate electrode forming process is performed. In this gate insulating film / gate electrode forming process, a gate insulating film 7b is formed on the lower surface and side surface of the trench 7a by CVD technology, high temperature oxidation (HTO) method, thermal oxidation method, or the like. Next, a polysilicon layer (doped polysilicon layer) to which impurities such as phosphorus (P) or boron (B) are added at a high concentration is deposited by CVD technology or the like so as to fill the inside of the trench 7a. Then, a part of the polysilicon layer and a part of the gate insulating film 7b are selectively removed by photolithography technology and dry etching. As a result, as shown in FIG. 13, an insulated gate type electrode structure (7b, 7c) consisting of the gate insulating film 7b and the gate electrode 7c is formed. More specifically, the polysilicon layer is etched back until the upper surface of the gate electrode 7c at a position in contact with the gate insulating film 7b is deeper than the boundary surface S between the second silicon carbide layer 15 and the first silicon carbide layer 14.
[0072] 14, an insulating film 10 is deposited on the upper surface of the SiC by CVD or the like. Then, a portion of the insulating film 10 is selectively removed by photolithography, dry etching or the like to open contact holes 10a, 10b in the insulating film 10, which expose the upper surfaces of the source regions 6a, 6b and the base contact regions 82a, 82b. In addition, a contact hole 10c is opened to expose the upper surface of the ring region 9b. After that, a heat treatment (reflow) may be performed to planarize the insulating film 10.
[0073] Next, a barrier metal layer 11 and a source wiring electrode 12 are sequentially formed by sputtering or deposition to cover the upper and side surfaces of the insulating film 10 and the upper surfaces of the source regions 6a and 6b, the base contact regions 82a and 82b, and the ring region 9b, forming the source electrodes (11, 12) shown in Fig. 2. The barrier metal layer 11 contacts the source regions 6a and 6b, the base contact regions 82a and 82b, and the ring region 9b. The barrier metal layer 11 makes ohmic contact with the source regions 6a and 6b, the base contact regions 82a and 82b, and the ring region 9b with low resistance.
[0074] Next, the SiC substrate 1 is thinned from the lower surface side by grinding, chemical mechanical polishing (CMP), or the like to adjust the thickness, thereby forming the drain region 1. Next, a drain electrode 13 (see FIG. 2) made of gold (Au) or the like is formed on the entire lower surface of the drain region 1 by a sputtering method, a vapor deposition method, or the like. In this manner, the SiC semiconductor device shown in FIG. 2 is completed.
[0075] Conventionally, an amorphous layer has been formed by ion-implanting phosphorus into a hexagonal single crystal silicon carbide substrate, and the amorphous layer has been recrystallized into a cubic single crystal n-type silicon carbide by heat treatment. However, when impurities are ion-implanted, the boundary between the high and low impurity concentration regions in SiC is unclear. Therefore, in the SiC after heat treatment, the boundary between the region containing 3C-SiC and the region containing 4H-SiC may become unclear. In particular, in a trench-type SiC semiconductor device, it is necessary to separately create a region containing 3C-SiC and a region containing 4H-SiC in order to suppress contact resistance along the depth direction, but when 3C-SiC is formed by ion-implanting impurities, the boundary between the region containing 3C-SiC and the region containing almost no 3C-SiC may become unclear. Therefore, in a trench-type SiC semiconductor device, it may not be easy to identify the boundary between the region containing 3C-SiC and the region containing almost no 3C-SiC, and the margin may be estimated to be large in order to suppress the leakage current i, and the amount of depression d0 of the gate electrode 7c from the upper surface of the source contact region 62a may be set large. In this way, the degree of freedom in device design may be reduced.
[0076] In contrast, the manufacturing method of the SiC semiconductor device 100 according to the first embodiment includes a step of forming (preparing) a first silicon carbide layer 14 including silicon carbide of a 4H structure and including a drift layer 2 of a first conductivity type, and a step of stacking a second silicon carbide layer 15 including silicon carbide of a 3C structure on an upper surface of the first silicon carbide layer 14. That is, in the present technology, the first silicon carbide layer 14 is formed by a film formation method, so that the boundary between the region including 3C-SiC and the region mainly consisting of silicon carbide of a 4H structure is made clear by the boundary surface S. It can be seen that the region deeper than the boundary surface S does not include mixed crystals of 3C-SiC and 4H-SiC, or even if it does include mixed crystals of 3C-SiC and 4H-SiC, the amount is small. Therefore, the upper surface 7d of the gate electrode 7c at the position where the gate electrode 7c contacts the gate insulating film 7b can be designed to be located deeper than the boundary surface S. This makes it possible to suppress the leakage current i without overestimating the margin, and prevents a decrease in the degree of freedom in device design.
[0077] Furthermore, when ion implanting impurities into 4H-SiC to make it amorphous and then performing heat treatment to form 3C-SiC (hereinafter referred to as forming 3C-SiC by ion implantation), it was necessary to use expensive equipment. More specifically, in order to make 4H-SiC amorphous, it was necessary to ion implant impurities at a high concentration, which required an increase in the operating time of expensive ion implantation equipment.
[0078] In contrast, in the manufacturing method of the SiC semiconductor device 100 according to the first embodiment, the amorphous film 15a is formed directly on the upper surface of the first silicon carbide layer 14 by plasma enhanced chemical vapor deposition or sputtering, and therefore can be formed using equipment that is less expensive than an ion implantation equipment.
[0079] Furthermore, when forming 3C-SiC by ion implantation, it was necessary to form 4H-SiC in advance in the areas that would later become 3C. And, the formation of 4H-SiC required epitaxial growth at high temperatures, for example, around 1600°C, using a thermal CVD (thermal chemical vapor deposition) device.
[0080] In contrast, in the manufacturing method of the SiC semiconductor device 100 according to the first embodiment, the amorphous film 15a can be formed at a lower temperature than when 3C-SiC is formed by ion implantation. More specifically, the amorphous film 15a can be formed by plasma enhanced chemical vapor deposition at a temperature of, for example, 300° C. or higher and 650° C. or lower. The amorphous film 15a can be formed by sputtering at a lower temperature than when 3C-SiC is formed by plasma enhanced chemical vapor deposition, for example, at room temperature. In this way, in the manufacturing method of the SiC semiconductor device 100 according to the first embodiment, the processing temperature can be lower than when 3C-SiC is formed by ion implantation, so that the manufacturing cost can be reduced. In addition, the amorphous film 15a is recrystallized by heat treatment at a temperature of, for example, 1200° C. or higher, so that it can be recrystallized together when activating the p-type impurity or n-type impurity ion-implanted into SiC. There is no need to separately perform heat treatment to recrystallize the amorphous film 15a, so that the manufacturing cost can be reduced.
[0081] (Modification 1 of the first embodiment) In the manufacturing method of the SiC semiconductor device according to the first embodiment described above, as shown in Fig. 10, in order to form the second silicon carbide layer 15, an amorphous film 15a made of SiC is formed on the upper surface of the first silicon carbide layer 14, and then the amorphous film 15a is recrystallized by heat treatment, but the present technology is not limited to this. In the manufacturing method of the SiC semiconductor device according to the first modification of the first embodiment, in Fig. 10, the second silicon carbide layer 15 containing 3C-SiC may be directly formed on the upper surface of the first silicon carbide layer 14 instead of the amorphous film 15a. In this case, the second silicon carbide layer 15 is formed by a thermal CVD method (thermal chemical vapor deposition method).
[0082] The method for manufacturing a SiC semiconductor device according to the first modification of the first embodiment can achieve the same effects as those of the first embodiment. More specifically, the second silicon carbide layer 15 containing 3C-SiC can be formed by a cheaper device than an ion implantation device. The processing temperature when forming the second silicon carbide layer 15 by thermal CVD is, for example, about 800° C. or higher and 1100° C. or lower, which is higher than the film formation temperature of the amorphous film 15a but is lower than the processing temperature when forming 3C-SiC by ion implantation. Therefore, the manufacturing cost can be reduced compared to the case of forming 3C-SiC by ion implantation. The manufacturing method other than the above is the same as the manufacturing method described in the first embodiment, so the description will be omitted. In the method for manufacturing a SiC semiconductor device according to the first modification of the first embodiment, the second silicon carbide layer 15 containing 3C-SiC is directly formed, so that heat treatment for forming 3C is not required.
[0083] (Other embodiments) As described above, the first embodiment of the present disclosure has been described, but the description and drawings forming a part of this disclosure should not be understood as limiting the present disclosure. Various alternative embodiments, examples and operating techniques will become apparent to those skilled in the art from this disclosure.
[0084] For example, a MOSFET is exemplified as the semiconductor device according to the first embodiment. + Instead of the drain region of type 1, p + The present invention can also be applied to insulated gate bipolar transistors (IGBTs) that have a collector region of a type other than IGBTs. In addition to IGBTs alone, the present invention can also be applied to reverse conducting IGBTs (RC-IGBTs) and reverse blocking insulated gate bipolar transistors (RB-IGBTs).
[0085] In the first embodiment, the electric field buffer region 9a is described as a guard ring, but it may have a JTE structure.
[0086] In addition, the configurations disclosed in the first embodiment can be appropriately combined within a range that does not cause contradictions. As such, the present disclosure naturally includes various embodiments not described here. Therefore, the technical scope of the present disclosure is determined only by the invention-specifying matters related to the scope of the claims that are appropriate from the above description. [Explanation of symbols]
[0087] 1...Drain region (SiC substrate) 2. Drift layer 3...Current diffusion layer 3a,3b…n-type layer 4…Gate bottom protection area 5…Base area 6,6a,6b…Source region 61, 61a, 61b...Source extension area 61x…Bottom side 62, 62a, 62b...Source contact region 6c...Channel stopper area 7a…Trench 7b...Gate insulating film 7c…Gate electrode 7d…Top surface 81a, 81b...Buried area 82a, 82b...base contact region 9a…electric field relaxation region 9b…Ring area 91a,91b,6c1...first part 92a,92b,6c2…Second part 93a...Third part 10...Insulating film 10a, 10b, 10c...Contact holes 11...Barrier metal layer 12...Source wiring electrode 13...Drain electrode 14...First silicon carbide layer 15...Second silicon carbide layer 15a...Amorphous film S…Boundary surface
Claims
1. a first silicon carbide layer including silicon carbide having a 4H structure; a second silicon carbide layer stacked on an upper surface of the first silicon carbide layer and including silicon carbide having a 3C structure; a drift layer of a first conductivity type provided in the first silicon carbide layer; a second conductivity type base region provided on an upper surface side of the drift layer in the first silicon carbide layer; a first conductivity type main region having a source extension region whose lower surface is in contact with the base region and provided in the first silicon carbide layer, and a source contact region whose lower surface is in contact with the source extension region and provided in the second silicon carbide layer; a gate insulating film provided inside a trench penetrating the main region and the base region; a gate electrode embedded inside the trench via the gate insulating film; a main electrode provided in contact with the source contact region; A silicon carbide semiconductor device comprising:
2. 2 . The silicon carbide semiconductor device according to claim 1 , wherein an upper surface of said gate electrode in contact with said gate insulating film is located deeper than a boundary surface between said second silicon carbide layer and said first silicon carbide layer.
3. 3 . The silicon carbide semiconductor device according to claim 1 , wherein said source extension region and said source contact region are defined by a boundary surface between said first silicon carbide layer and said second silicon carbide layer.
4. 3 . The silicon carbide semiconductor device according to claim 1 , wherein an upper surface of said gate electrode in contact with said gate insulating film is located at a position shallower than a lower surface of said source extension region.
5. 3 . The silicon carbide semiconductor device according to claim 1 , wherein the second silicon carbide layer has a thickness of not less than 0.2 μm and not more than 0.5 μm.
6. 3 . The silicon carbide semiconductor device according to claim 1 , wherein a ratio of silicon carbide having a 3C structure contained in said second silicon carbide layer is equal to or greater than 10 percent and equal to or less than 100 percent.
7. a base contact region of a second conductivity type provided in the second silicon carbide layer; 3 . The silicon carbide semiconductor device according to claim 1 , wherein the base contact region has a side surface in contact with the main region, an upper surface in contact with the main electrode, and a dimension along a depth direction thereof is the same as that of the source contact region.
8. an active portion; and a breakdown voltage structure portion provided so as to surround the active portion in a plan view; the second silicon carbide layer is laminated on an upper surface of the first silicon carbide layer across the active portion and the voltage withstanding structure portion; The silicon carbide semiconductor device according to claim 1 , wherein said base region, said main region, and said trench are provided in said active portion.
9. 9 . The silicon carbide semiconductor device according to claim 8 , further comprising: an electric field relaxation region provided in said voltage withstanding structure portion across said second silicon carbide layer and said first silicon carbide layer in a depth direction, said electric field relaxation region being made of silicon carbide of a second conductivity type.
10. forming a first silicon carbide layer including silicon carbide having a 4H structure and including a drift layer of a first conductivity type; laminating a second silicon carbide layer including silicon carbide having a 3C structure on an upper surface of the first silicon carbide layer; forming a second conductivity type base region on an upper surface side of the drift layer in the first silicon carbide layer; forming a first conductivity type main region having a stacked structure of a source extension region and a source contact region across the first silicon carbide layer and the second silicon carbide layer; forming a trench penetrating the main region and the base region located on a lower surface side of the main region; forming a gate electrode on the inner side of the trench via a gate insulating film; forming a master electrode in contact with an upper surface of the source contact region; Including, In the step of forming the main region, the source extension region is formed in the first silicon carbide layer, and the source contact region is formed in the second silicon carbide layer. A method for manufacturing a silicon carbide semiconductor device.
11. 11. The method for manufacturing a silicon carbide semiconductor device according to claim 10, wherein, in the step of forming the gate electrode, an upper surface of the gate electrode in contact with the gate insulating film is provided at a position deeper than a boundary surface between the second silicon carbide layer and the first silicon carbide layer.
12. 12. The method for manufacturing a silicon carbide semiconductor device according to claim 10, wherein the step of laminating the second silicon carbide layer includes the steps of: forming an amorphous film made of silicon carbide on an upper surface of the first silicon carbide layer; and heat-treating the amorphous film.
13. 13. The method for manufacturing a silicon carbide semiconductor device according to claim 12, wherein the amorphous film is formed by plasma enhanced chemical vapor deposition or sputtering.
14. 12. The method for manufacturing a silicon carbide semiconductor device according to claim 10, wherein the step of laminating the second silicon carbide layer includes forming a silicon carbide film containing silicon carbide having a 3C structure on an upper surface of the first silicon carbide layer.
15. The method for manufacturing a silicon carbide semiconductor device according to claim 14 , wherein said second silicon carbide layer is formed by thermal chemical vapor deposition.
16. 12. The method for manufacturing a silicon carbide semiconductor device according to claim 10, wherein said source contact region is formed by ion-implanting an n-type impurity into said second silicon carbide layer.
17. 12. The method for manufacturing a silicon carbide semiconductor device according to claim 10, further comprising the step of: forming a base contact region in contact with said source contact region by ion-implanting a p-type impurity into said second silicon carbide layer.
Citation Information
Patent Citations
Semiconductor device and manufacturing method thereof
JP2009049198A
Semiconductor device, method for manufacturing same, power module, power conversion device, and rail vehicle