Substrate for gas barrier film, gas barrier film, laminate, and packaging material
The base material for gas barrier films, with controlled thermal strain and a specific layer structure, addresses the issue of property deterioration during heat treatment, ensuring stable and effective barrier performance.
Patent Information
- Application Number
- JP2023081281
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-17
- Publication Date
- 2024-11-28
AI Technical Summary
Existing gas barrier films experience deterioration in barrier properties due to dimensional changes during production, particularly when subjected to heat treatment, which can lead to cracking and reduced effectiveness.
A base material for gas barrier films is developed with a thermal strain difference of 0.005 or less between maximum and minimum values, using a specific layer structure comprising a base material, a gas barrier layer, and optionally an inorganic oxide layer, to maintain stability and prevent deterioration during production processes.
The solution ensures that the gas barrier film maintains its properties even after heat treatment, providing excellent barrier performance and resistance to cracking, suitable for high-temperature applications.
Smart Images

Figure 2024165250000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a substrate for a gas barrier film, and a gas barrier film, a laminate, and a packaging material using the substrate for a gas barrier film. [Background technology]
[0002] Packaging materials used for packaging food, medicine, etc. are required to have the property of preventing the intrusion of gases (water vapor, oxygen, etc.) that denature the contents, in order to prevent deterioration or spoilage of the contents and to maintain their function and quality. For this reason, film materials with gas barrier properties (gas barrier films) are used for these packaging materials.
[0003] Known gas barrier films include those in which a coating layer (gas barrier layer) made of a material having gas barrier properties is provided on the surface of a resin substrate (see, for example, Patent Document 1). Patent Document 1 discloses an outer packaging material for vacuum insulation material in which a heat-sealable film is layered on this gas barrier film. Patent Document 1 focuses on the dimensional change of the manufactured outer packaging material in the usage environment (high temperature and high humidity environment) so that the manufactured outer packaging material can prevent gas transmission over a long period of time (i.e., maintain gas barrier properties).Then, by keeping the dimensional change rate of the outer packaging material within a specified range after being kept in a high temperature and high humidity environment that simulates the usage environment for a long period of time (e.g., 2 hours), it is possible to suppress the occurrence of cracks in the gas barrier film in the usage environment and maintain the barrier properties. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2017-150565 A Summary of the Invention [Problem to be solved by the invention]
[0005] However, the inventors have found through their investigations that the barrier properties of a gas barrier film after production are affected by dimensional changes in the substrate during production of the gas barrier film. The inventors have focused in particular on the effect of heat during production of the gas barrier film on the substrate, and have completed the invention.
[0006] The present invention has been made in view of the above circumstances, and has an object to provide a substrate for a gas barrier film whose barrier properties are resistant to deterioration even when subjected to a heat treatment during the production of the gas barrier film. Another object of the present invention is to provide a gas barrier film, a laminate and a packaging material using the gas barrier film substrate. [Means for solving the problem]
[0007] One aspect of the present invention includes, for example, the following embodiment. [1] A substrate for a gas barrier film, which is used in a gas barrier film having a substrate and a gas barrier layer in this order, A substrate having a difference between maximum and minimum thermal distortion values of 0.005 or less as measured as follows: [Thermal strain measurement method] A sample with a dimension of 4 mm in the MD direction and 25 mm in the TD direction is taken from the substrate. At this time, the center of each sample in the TD direction is adjusted to a position 50 mm + 100 mm × N (N is an integer of 1 or more) from one end of the substrate in the TD direction, and multiple samples are taken over the entire width of the substrate in the TD direction. Then, each sample is subjected to a thermal history of heating from 20 to 100 ° C and cooling from 100 to 20 ° C while applying a tension of 30 mN in the TD direction, and a thermomechanical analysis is performed. Then, the difference between the maximum and minimum thermal strains in the TD direction of each sample is calculated. [2] The substrate for gas barrier films according to [1], which is a polyolefin-based resin film, a polyester-based resin film, or a polyamide-based resin film. [3] The substrate for gas barrier films according to [1] or [2], wherein the gas barrier layer comprises, from the substrate side, an undercoat layer and a gas barrier coating layer; an inorganic oxide layer and a gas barrier coating layer; or an undercoat layer, an inorganic oxide layer and a gas barrier coating layer, in this order. [4] The substrate for gas barrier films according to [3], wherein the underlayer has a thickness of 0.01 to 1 μm. [5] The gas barrier film substrate according to [3] or [4], wherein the undercoat layer contains an organic polymer as a main component, and the organic polymer contains at least one of a polyacrylic resin, a polyol resin, a polyurethane resin, and a polyamide resin. [6] The substrate for gas barrier films according to any one of [3] to [5], wherein the inorganic oxide layer has a thickness of 1 to 200 nm. [7] The substrate for a gas barrier film according to any one of [3] to [6], wherein the inorganic oxide layer contains aluminum oxide or silicon oxide. [8] The substrate for gas barrier films according to any one of [3] to [7], wherein the gas barrier coating layer has a thickness of 0.05 to 1 μm. [9] The substrate for gas barrier films according to any one of [3] to [8], wherein the gas barrier coating layer is a cured product of a raw material for forming the gas barrier coating layer, the raw material comprising at least one of a metal alkoxide and a hydrolysate of a metal alkoxide, and a water-soluble polymer.
[10] The substrate for gas barrier films according to [9], wherein the raw material for forming the gas barrier coating layer contains at least one of a silane coupling agent and a hydrolysate of a silane coupling agent.
[11] The substrate for gas barrier films according to any one of [3] to [8], wherein the gas barrier coating layer contains a polyvalent metal salt of a carboxylic acid which is a reaction product between a carboxy group of a polycarboxylic acid polymer and a polyvalent metal compound.
[12] The substrate for gas barrier films according to any one of [3] to [8], wherein the gas barrier coating layer is a cured product of a raw material for forming the gas barrier coating layer, the raw material including a polyvinyl alcohol resin, a polyurethane resin and a silane compound.
[13] A gas barrier film comprising the substrate for gas barrier films according to any one of [1] to
[12] and a gas barrier layer, in this order.
[14] A gas barrier film according to
[13] , a heat seal layer formed on the gas barrier layer of the gas barrier film; A laminate comprising:
[15] The laminate according to
[14] , wherein the gas barrier film substrate and the heat sealable layer contain polypropylene as main components.
[16] The laminate according to
[15] , wherein the polypropylene content is 90% by mass or more.
[17] A packaging material formed from the laminate according to any one of
[14] to
[16] . Effect of the Invention
[0008] According to the present invention, it is possible to provide a substrate for a gas barrier film, the barrier properties of which are not easily deteriorated even when subjected to a heat treatment during the production of the gas barrier film. Furthermore, according to the present invention, it is possible to provide a gas barrier film, a laminate, and a packaging material using the substrate for a gas barrier film. [Brief description of the drawings]
[0009] [Figure 1] FIG. 1 is a schematic cross-sectional view of a gas barrier film according to one embodiment of the present invention. [Diagram 2] FIG. 2 is a schematic diagram showing a method for collecting a sample from a substrate. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] <Gas barrier film> Hereinafter, one embodiment of the present invention will be described with reference to FIG. 1 is a schematic cross-sectional view of a gas barrier film 1 according to this embodiment. The gas barrier film 1 includes a resin-containing gas barrier film substrate 10 (hereinafter, may be simply referred to as "substrate") and a gas barrier layer 50. The gas barrier layer 50 includes an underlayer 20, an inorganic oxide layer 30, and a gas barrier coating layer 40.
[0011] 1, an underlayer 20 is formed on a substrate 10. An inorganic oxide layer 30 is formed on the underlayer 20. A gas barrier coating layer 40 is formed on the inorganic oxide layer 30. In the gas barrier film according to this embodiment, it is not necessary to provide either the underlayer 20 or the inorganic oxide layer 30. In this case, the inorganic oxide layer 30 may be formed on the substrate 10, or the gas barrier coating layer 40 may be formed on the underlayer 20. That is, the gas barrier layer may include, from the substrate 10 side, the underlayer 20 and the gas barrier coating layer 40, the inorganic oxide layer 30 and the gas barrier coating layer 40, or the underlayer 20, the inorganic oxide layer 30 and the gas barrier coating layer 40, in this order.
[0012] (base material) Examples of the resin constituting the substrate 10 include olefin-based resins such as polyethylene, polypropylene, polymers of olefins having 2 to 10 carbon atoms, and propylene-ethylene copolymers; polyester-based resins such as polyethylene terephthalate, polybutylene terephthalate, and polyethylene naphthalate; polyamide-based resins such as aliphatic polyamides such as nylon 6 and nylon 66, and aromatic polyamides such as polymetaxylylene adipamide; vinyl-based resins such as polystyrene, polyvinyl acetate, ethylene-vinyl acetate copolymer, polyvinyl alcohol, and ethylene-vinyl alcohol copolymer; acrylic-based resins such as homopolymers or copolymers of (meth)acrylic monomers such as polymethyl methacrylate and polyacrylonitrile; cellophane; and engineering plastics such as polycarbonate and polyimide. One of these resins may be used alone, or two or more may be used in combination.
[0013] The substrate 10 may be a single-layer film made of a single resin, or a single-layer or laminate film made of multiple resins, i.e., the substrate 10 may be a single layer or two or more layers. As the substrate 10, a polyolefin resin film (particularly, a polypropylene film), a polyester resin film (particularly, a polyethylene terephthalate film), a polyamide resin film (particularly, a nylon film), or the like is preferable.
[0014] The substrate 10 may be an unstretched film or a stretched film such as uniaxially stretched or biaxially stretched. From the viewpoint of excellent water vapor barrier properties, a stretched polypropylene (OPP) film is particularly preferable as the substrate 10. The OPP film may be at least one type of polymer selected from homopolymer, random copolymer, and block copolymer processed into a film. A homopolymer is a polypropylene consisting of only propylene alone. A random copolymer is a polypropylene in which the main monomer propylene and a small amount of a comonomer different from propylene are randomly copolymerized to form a homogeneous phase. A block copolymer is a polypropylene in which the main monomer propylene and the above comonomer are copolymerized in blocks or polymerized into a rubber-like form to form a heterogeneous phase. When the substrate 10 contains OPP, the OPP may be one layer or two or more layers.
[0015] In the substrate 10, the first surface 10a on which the underlayer 20 or the inorganic oxide layer 30 is formed may be subjected to a surface treatment such as a chemical treatment, a solvent treatment, a corona treatment, a low-temperature plasma treatment, an ozone treatment, etc. This can improve the adhesion between the underlayer 20 or the inorganic oxide layer 30 formed on the first surface 10a.
[0016] The substrate 10 may contain additives such as a filler, an antiblocking agent (hereinafter sometimes referred to as an "AB agent"), an antistatic agent, a plasticizer, a lubricant, an antioxidant, etc. These additives may be used alone or in combination of two or more kinds.
[0017] The AB agent is a solid particle such as an organic particle or an inorganic particle. Examples of the organic particles include polymethyl methacrylate particles, polystyrene particles, and polyamide particles. These organic particles are obtained, for example, by emulsion polymerization or suspension polymerization. Examples of the inorganic particles include particles of silica, zeolite, talc, kaolinite, and feldspar. Any one of these AB agents may be used alone, or two or more of them may be used in combination.
[0018] When the substrate 10 contains an AB agent, the first surface 10a has unevenness resulting from the AB agent. That is, some of the AB agent particles protrude from the first surface 10a, reducing the contact area when the substrate is wound into a roll. As a result, blocking is suppressed, and the blocking resistance of the substrate 10 can be improved.
[0019] From the above viewpoint, it is preferable that the substrate 10 contains an AB agent. On the other hand, if large convex portions are formed on the first surface 10a of the substrate 10, defects that become paths for gas permeation are likely to occur in the undercoat layer 20, inorganic oxide layer 30, gas barrier coating layer 40, etc. formed thereon, which may reduce the oxygen barrier properties of the gas barrier film 1. In consideration of this point, as well as the appearance, transparency, possibility of the AB agent falling off, and anti-blocking performance of the gas barrier film 1, it is preferable that the average particle size of the AB agent is, for example, 0.1 to 5 μm. The average particle size of the AB agent is a weight average diameter measured by the Coulter method.
[0020] When the substrate 10 contains an AB agent, the AB agent may be dispersed in the resin material before curing. The AB agent particles located near the surface of the substrate 10 may be covered by the resin or may be exposed. The content of the AB agent may be 0.05 parts by mass or more and 0.5 parts by mass or less with respect to 100 parts by mass of the resin constituting the substrate 10. When the content of the AB agent is 0.05 parts by mass or more, the processing characteristics of the film that is the raw material of the substrate 10 are easily improved. When the content of the AB agent is 0.5 parts by mass or less, the deterioration of the oxygen barrier property of the gas barrier film 1 is easily suppressed.
[0021] There is no particular limit to the thickness of the substrate 10, and it can be appropriately determined according to the price and application, taking into consideration the suitability as a packaging material and the suitability for laminating other layers (coatings). The thickness of the substrate 10 is preferably 3 to 200 μm, more preferably 5 to 120 μm, further preferably 6 to 100 μm, and particularly preferably 10 to 30 μm, from a practical standpoint.
[0022] (Gas barrier layer: Base layer) The underlayer 20 contains an organic polymer. The content of the organic polymer in the underlayer 20 may be, for example, 70% by mass or more, or 80% by mass or more. Examples of the organic polymer include polyacrylic resin, polyester resin, polycarbonate resin, polyurethane resin, polyamide resin, polyolefin resin, polyimide resin, melamine resin, and phenol resin. Considering the hot water resistance of the adhesive strength between the substrate 10 and the inorganic oxide layer 30 or the gas barrier coating layer 40, it is preferable that the underlayer 20 contains at least one of the above polyacrylic resin, polyol resin, polyurethane resin, and polyamide resin (or a reaction product of these organic polymers). The underlayer 20 may contain a silane coupling agent, an organic titanate, a modified silicone oil, or the like.
[0023] The organic polymer used in the undercoat layer 20 may be an organic polymer having a urethane bond produced by the reaction of a polyol having two or more hydroxyl groups at the polymer end with an isocyanate compound, or an organic polymer containing a reaction product of a polyol having two or more hydroxyl groups at the polymer end with an organic silane compound such as a silane coupling agent or a hydrolyzate thereof. Either one of these may be used, or both may be used.
[0024] The polyols include, for example, at least one selected from acrylic polyol, polyvinyl acetal, polystyrene polyol, polyurethane polyol, etc. The acrylic polyol may be obtained by polymerizing an acrylic acid derivative monomer, or may be obtained by copolymerizing an acrylic acid derivative monomer with another monomer. Examples of the acrylic acid derivative monomer include ethyl methacrylate, hydroxyethyl methacrylate, hydroxypropyl methacrylate, and hydroxybutyl methacrylate. Examples of the monomer to be copolymerized with the acrylic acid derivative monomer include styrene, etc. The isocyanate compound has the effect of increasing the adhesion between the substrate 10 and the inorganic oxide layer 30 or the gas barrier coating layer 40 by forming a urethane bond by reacting with the polyol. That is, the isocyanate compound functions as a crosslinking agent or a curing agent. Examples of the isocyanate compound include monomers such as aromatic tolylene diisocyanate (TDI), diphenylmethane diisocyanate (MDI), aliphatic xylene diisocyanate (XDI), hexamethylene diisocyanate (HMDI), and isophorone diisocyanate (IPDI), their polymers, and their derivatives. The above-mentioned isocyanate compounds may be used alone or in combination of two or more. Examples of silane coupling agents include vinyltrimethoxysilane, γ-chloropropylmethyldimethoxysilane, γ-chloropropyltrimethoxysilane, glycidoxypropyltrimethoxysilane, γ-methacryloxypropyltrimethoxysilane, and γ-methacryloxypropylmethyldimethoxysilane. The organic silane compound may be a hydrolyzate of these silane coupling agents. The organic silane compound may contain one of the above-mentioned silane coupling agents and their hydrolyzates alone, or two or more of them in combination.
[0025] The undercoat layer 20 can be formed using a mixed solution in which the above-mentioned components are mixed in an organic solvent at any ratio. The mixed solution may contain, for example, a curing accelerator such as a tertiary amine, an imidazole derivative, a metal salt compound of a carboxylic acid, a quaternary ammonium salt, or a quaternary phosphonium salt; an antioxidant such as a phenol-based, sulfur-based, or phosphite-based antioxidant; a leveling agent; a flow control agent; a catalyst; a crosslinking reaction accelerator; a filler; and the like. The mixed liquid can be arranged in a layer on the substrate 10 by using a known printing method such as offset printing, gravure printing, or silk screen printing, or a known coating method such as roll coating, knife edge coating, or gravure coating. After the mixture is arranged, the underlayer 20 can be formed by heating the mixture to, for example, 50°C to 200°C.
[0026] There is no particular limit to the thickness of the undercoat layer 20, and it can be, for example, 0.005 to 5 μm. The thickness can be appropriately determined depending on the application or the desired characteristics. The thickness of the undercoat layer 20 is preferably 0.01 to 1 μm, and more preferably 0.01 to 0.5 μm. If the thickness of the undercoat layer 20 is 0.01 μm or more, sufficient adhesion strength between the substrate 10 and the inorganic oxide layer 30 or the gas barrier coating layer 40 is obtained, and the oxygen barrier property is also good. If the thickness of the undercoat layer 20 is 1 μm or less, it is easy to form a uniform coating surface, and the drying load and manufacturing costs can be suppressed.
[0027] (Gas barrier layer: inorganic oxide layer) Examples of inorganic oxides constituting the inorganic oxide layer 30 include aluminum oxide, silicon oxide, magnesium oxide, titanium oxide, tin oxide, zinc oxide, and indium oxide. In particular, aluminum oxide and silicon oxide are preferred because they are highly productive and have excellent oxygen barrier properties and water vapor barrier properties in heat resistance and moist heat resistance. The inorganic oxide layer 30 may be formed of one type of inorganic oxide, or may be formed of two or more types of inorganic oxides selected appropriately.
[0028] The thickness of the inorganic oxide layer 30 can be 1 to 200 nm. If the thickness is 1 nm or more, excellent oxygen barrier property and water vapor barrier property can be obtained. If the thickness is 200 nm or less, the manufacturing cost can be kept low, cracks due to external forces such as bending and pulling are unlikely to occur, and deterioration of the barrier property can be suppressed. The inorganic oxide layer 30 can be formed by a known film formation method such as vacuum deposition, sputtering, ion plating, or plasma chemical vapor deposition (CVD).
[0029] (Gas barrier layer: gas barrier coating layer) The gas barrier coating layer 40 may be a known gas barrier coating layer formed by a wet coating method. The gas barrier coating layer 40 is obtained by forming a coating film made of a coating agent on the underlayer 20 or the inorganic oxide layer 30 by a wet coating method, and drying the coating film. In this specification, the term "coating film" refers to a wet film, and the terms "coating film" and "coating layer" refer to a dry film.
[0030] The gas barrier coating layer 40 may be a coating (hereinafter, sometimes referred to as an "organic-inorganic composite coating") that is a cured product of a raw material for forming the gas barrier coating layer, which contains at least one of a metal alkoxide and its hydrolysate, and a water-soluble polymer. Furthermore, it is preferable that the raw material for forming the gas barrier coating layer further contains at least one of a silane coupling agent and its hydrolysate.
[0031] Examples of metal alkoxides and their hydrolysates contained in the organic-inorganic composite coating include those represented by the general formula M(OR), such as tetraethoxysilane [Si(OC2H5)4] and triisopropoxyaluminum [Al(OC3H7)3]. n and hydrolysates thereof. One of these may be contained alone, or two or more of them may be contained in combination.
[0032] The total content of at least one of the metal alkoxide and hydrolysate thereof in the organic-inorganic composite coating is, for example, 40 to 70 mass%. From the viewpoint of further reducing oxygen permeability, the lower limit of the total content of at least one of the metal alkoxide and hydrolysate thereof in the organic-inorganic composite coating may be 50 mass%. From the same viewpoint, the upper limit of the total content of at least one of the metal alkoxide and hydrolysate thereof in the organic-inorganic composite coating may be 65 mass%.
[0033] The water-soluble polymer contained in the organic-inorganic composite coating is not particularly limited, and examples thereof include polyvinyl alcohol-based and acrylic polyol-based polymers, and polysaccharides such as starch, methyl cellulose, and carboxymethyl cellulose. From the viewpoint of further improving the oxygen gas barrier property, it is preferable to include a polyvinyl alcohol-based polymer. The number average molecular weight of the water-soluble polymer is, for example, 40,000 to 180,000.
[0034] A water-soluble polymer such as polyvinyl alcohol can be obtained by, for example, saponifying polyvinyl acetate (including partial saponification). This water-soluble polymer may have several tens of percent of acetate groups remaining, or may have only a few percent of acetate groups remaining.
[0035] The content of the water-soluble polymer in the organic-inorganic composite coating is, for example, 15 to 50 mass %. If the content of the water-soluble polymer is 20 to 45 mass %, the oxygen permeability of the organic-inorganic composite coating can be further reduced, which is preferable.
[0036] The silane coupling agent and its hydrolysate contained in the organic-inorganic composite coating film may be a silane coupling agent having an organic functional group. Such silane coupling agents and their hydrolysates may be ethyltrimethoxysilane, vinyltrimethoxysilane, γ-chloropropylmethyldimethoxysilane, γ-chloropropyltrimethoxysilane, glycidoxypropyltrimethoxysilane, γ-methacryloxypropyltrimethoxysilane, γ-methacryloxypropylmethyldimethoxysilane, and their hydrolysates. One of these may be contained alone, or two or more may be contained in combination.
[0037] At least one of the silane coupling agent and its hydrolysate is preferably used with an epoxy group as an organic functional group. Examples of the silane coupling agent with an epoxy group include γ-glycidoxypropyltrimethoxysilane and β-(3,4-epoxycyclohexyl)ethyltrimethoxysilane. The silane coupling agent with an epoxy group and its hydrolysate may have an organic functional group different from the epoxy group, such as a vinyl group, an amino group, a methacryl group or a ureido group.
[0038] The silane coupling agent having an organic functional group and its hydrolysate can further improve the oxygen barrier property of the gas barrier coating layer 40 and the adhesion to the underlayer 20 or the inorganic oxide layer 30 through the interaction between the organic functional group and the hydroxyl group of the water-soluble polymer. In particular, the epoxy group of the silane coupling agent and its hydrolysate can improve the adhesion of the gas barrier coating layer 40 to the underlayer 20 or the inorganic oxide layer 30 through the interaction between the hydroxyl group of the polyvinyl alcohol.
[0039] The total content of the silane coupling agent and / or hydrolysate thereof in the organic-inorganic composite coating is, for example, 1 to 15 mass %. If the total content of the silane coupling agent and / or hydrolysate thereof is 2 to 12 mass %, the oxygen permeability of the organic-inorganic composite coating can be further reduced, which is preferable.
[0040] The organic-inorganic composite coating may contain a crystalline inorganic layered compound having a layered structure. Examples of the inorganic layered compound include clay minerals such as kaolinite, smectite, and mica. These may be used alone or in combination of two or more. The particle size of the inorganic layered compound is, for example, 0.1 to 10 μm. The aspect ratio of the inorganic layered compound is, for example, 50 to 5000.
[0041] As the inorganic layered compound, a clay mineral of the smectite group is preferable because a coating film having excellent oxygen barrier properties and adhesive strength can be formed by the infiltration (intercalation) of a water-soluble polymer between layers of the layered structure. Specific examples of the clay mineral of the smectite group include montmorillonite, hectorite, saponite, water-swellable synthetic mica, etc.
[0042] Another preferred example of the gas barrier coating layer 40 is a coating containing a polyvalent metal salt of carboxylic acid, which is a reaction product between a carboxy group of a polycarboxylic acid polymer (A) and a polyvalent metal compound (B) (polycarboxylic acid polyvalent metal salt coating). The polycarboxylic acid polyvalent metal salt coating may be formed by applying a coating agent in which a polycarboxylic acid polymer (A) and a polyvalent metal compound (B) are mixed and then heating and drying, or by applying a coating agent mainly composed of a polycarboxylic acid polymer (A) and drying to form an A coating, applying a coating agent mainly composed of a polyvalent metal compound (B) on top of that and drying to form a B coating, and then allowing a crosslinking reaction to occur between the A / B layers.
[0043] A polycarboxylic acid polymer is a polymer of a carboxylic acid monomer having two or more carboxyl groups in the molecule. Examples of polycarboxylic acid polymers include (co)polymers of ethylenically unsaturated carboxylic acids; copolymers of ethylenically unsaturated carboxylic acids and other ethylenically unsaturated monomers; and acidic polysaccharides having a carboxyl group in the molecule, such as alginic acid, carboxymethylcellulose, and pectin. Examples of ethylenically unsaturated carboxylic acids include acrylic acid, methacrylic acid, itaconic acid, maleic acid, fumaric acid, and crotonic acid. Examples of ethylenically unsaturated monomers copolymerizable with ethylenically unsaturated carboxylic acids include saturated carboxylic acid vinyl esters such as ethylene, propylene, and vinyl acetate, alkyl acrylates, alkyl methacrylates, alkyl itaconates, vinyl chloride, vinylidene chloride, styrene, acrylamide, and acrylonitrile. These polycarboxylic acid polymers may be used alone or in combination of two or more.
[0044] Among the above, from the viewpoint of the gas barrier properties of the resulting gas barrier film 1, a polymer containing a structural unit derived from at least one polymerizable monomer selected from the group consisting of acrylic acid, maleic acid, methacrylic acid, itaconic acid, fumaric acid, and crotonic acid is preferred, and a polymer containing a structural unit derived from at least one polymerizable monomer selected from the group consisting of acrylic acid, maleic acid, methacrylic acid, and itaconic acid is particularly preferred. In the polymer, the proportion of the structural unit derived from at least one polymerizable monomer selected from the group consisting of acrylic acid, maleic acid, methacrylic acid, and itaconic acid is preferably 80 mol% or more, more preferably 90 mol% or more (however, the total of all structural units constituting the polymer is 100 mol%). The polymer may be a homopolymer or a copolymer. When the polymer is a copolymer containing structural units other than the above structural units, examples of the other structural units include structural units derived from ethylenically unsaturated monomers copolymerizable with the above-mentioned ethylenically unsaturated carboxylic acid.
[0045] The number average molecular weight of the polycarboxylic acid polymer is preferably within the range of 2,000 to 10,000,000, more preferably 5,000 to 1,000,000. If the number average molecular weight is less than 2,000, the resulting gas barrier film is unlikely to achieve sufficient water resistance, and moisture may cause the gas barrier properties and transparency to deteriorate, or whitening may occur. On the other hand, if the number average molecular weight exceeds 10,000,000, the viscosity of the coating agent when forming the gas barrier coating layer 40 may increase, and the coatability may be impaired. The number average molecular weight is a polystyrene-equivalent number average molecular weight determined by gel permeation chromatography (GPC).
[0046] In the case where a coating agent mainly composed of a polycarboxylic acid polymer is applied and dried to form an A-coating, and then a coating agent mainly composed of a polyvalent metal compound is applied and dried to form a B-coating, the polycarboxylic acid polymer may have a part of its carboxyl groups neutralized in advance with a basic compound. By neutralizing a part of the carboxyl groups of the polycarboxylic acid polymer in advance, the water resistance and heat resistance of the A-coating can be further improved. As the basic compound, at least one basic compound selected from the group consisting of a polyvalent metal compound, a monovalent metal compound, and ammonia is preferable. As the polyvalent metal compound, the compounds exemplified in the description of the polyvalent metal compound described later can be used. As the monovalent metal compound, for example, sodium hydroxide, potassium hydroxide, etc. can be mentioned.
[0047] Various additives can be added to the coating agent containing a polycarboxylic acid polymer as the main component, as long as the additives do not impair the barrier performance. Examples of such additives include crosslinking agents, curing agents, leveling agents, defoamers, antiblocking agents, antistatic agents, dispersants, surfactants, softeners, stabilizers, film-forming agents, thickeners, etc.
[0048] The solvent used in the coating agent mainly composed of a polycarboxylic acid polymer is preferably an aqueous medium. Examples of the aqueous medium include water, water-soluble or hydrophilic organic solvents, or mixtures thereof. The aqueous medium usually contains water or water as the main component. The content of water in the aqueous medium is preferably 70% by mass or more, more preferably 80% by mass or more. Examples of the water-soluble or hydrophilic organic solvent include alcohols such as methanol, ethanol, and isopropanol, ketones such as acetone and methyl ethyl ketone, ethers such as tetrahydrofuran, cellosolves, carbitols, and nitriles such as acetonitrile.
[0049] The polyvalent metal compound is not particularly limited as long as it is a compound that reacts with the carboxyl group of the polycarboxylic acid polymer to form a polyvalent metal salt of polycarboxylic acid, and examples thereof include zinc oxide particles, magnesium oxide particles, magnesium methoxide, copper oxide, calcium carbonate, etc. These may be used alone or in combination. From the viewpoint of the oxygen barrier property of the gas barrier coating layer 40, zinc oxide is preferred.
[0050] Zinc oxide is an inorganic material having ultraviolet absorbing ability. The average particle size of the zinc oxide particles is not particularly limited, but from the viewpoints of gas barrier properties, transparency, and coating suitability, the average particle size is preferably 5 μm or less, more preferably 1 μm or less, and particularly preferably 0.1 μm or less.
[0051] When a coating agent containing a polyvalent metal compound as a main component is applied and dried to form a film, various additives may be contained in addition to zinc oxide particles as necessary within a range that does not impair the effects of the present invention. Examples of such additives include resins soluble or dispersible in the solvent used in the coating agent, dispersants soluble or dispersible in the solvent, surfactants, softeners, stabilizers, film-forming agents, thickeners, etc. Among the above, it is preferable to contain a resin that is soluble or dispersible in a solvent. This improves the applicability and film-forming property of the coating agent. Examples of such resins include alkyd resins, melamine resins, acrylic resins, urethane resins, polyester resins, phenolic resins, amino resins, fluorine resins, epoxy resins, and isocyanate resins.
[0052] It is also preferable to include a dispersant that is soluble or dispersible in the solvent. This improves the dispersibility of the polyvalent metal compound. As the dispersant, an anionic surfactant or a nonionic surfactant can be used. As the surfactant, various surfactants such as (poly)carboxylate, alkyl sulfate, alkylbenzene sulfonate, alkylnaphthalene sulfonate, alkylsulfosuccinate, alkyldiphenylether disulfonate, alkylphosphate, aromatic phosphate, polyoxyethylene alkyl ether, polyoxyethylene alkylphenol ether, polyoxyethylene alkyl ester, alkylallyl sulfate, polyoxyethylene alkylphosphate, sorbitan alkyl ester, glycerin fatty acid ester, sorbitan fatty acid ester, sucrose fatty acid ester, polyethylene glycol fatty acid ester, polyoxyethylene sorbitan alkyl ester, polyoxyethylene alkylallyl ether, polyoxyethylene derivative, polyoxyethylene sorbitol fatty acid ester, polyoxy fatty acid ester, and polyoxyethylene alkylamine can be mentioned. These surfactants may be used alone or in combination of two or more.
[0053] When an additive is contained in a coating agent mainly composed of a polyvalent metal compound, the mass ratio of the polyvalent metal compound to the additive (polyvalent metal compound:additive) is preferably within the range of 30:70 to 99:1, and more preferably within the range of 50:50 to 98:2.
[0054] Examples of the solvent for the coating agent include water, methyl alcohol, ethyl alcohol, isopropyl alcohol, n-propyl alcohol, n-butyl alcohol, n-pentyl alcohol, dimethyl sulfoxide, dimethylformamide, dimethylacetamide, toluene, hexane, heptane, cyclohexane, acetone, methyl ethyl ketone, diethyl ether, dioxane, tetrahydrofuran, ethyl acetate, and butyl acetate. These solvents may be used alone or in combination of two or more. Among these, from the viewpoint of coating property, methyl alcohol, ethyl alcohol, isopropyl alcohol, toluene, ethyl acetate, methyl ethyl ketone, and water are preferred. From the viewpoint of manufacturability, methyl alcohol, ethyl alcohol, isopropyl alcohol, and water are preferred.
[0055] When a coating agent in which a polycarboxylic acid polymer (A) and a polyvalent metal compound (B) are mixed is applied and dried to form a polycarboxylic acid polyvalent metal salt coating, a coating agent in which the polycarboxylic acid polymer (A), the polyvalent metal compound (B), water or alcohol as a solvent, a resin or dispersant that can be dissolved or dispersed in the solvent, and additives as necessary can be used. By applying and drying this coating agent by a known coating method, a polycarboxylic acid polyvalent metal salt coating can be formed. Examples of the coating method include casting, dipping, roll coating, gravure coating, screen printing, reverse coating, spray coating, kit coating, die coating, metalling bar coating, chamber doctor combined coating, curtain coating, and the like.
[0056] The gas barrier coating layer 40 may contain a polyurethane resin from the viewpoint of bending resistance and gas barrier properties. That is, the gas barrier coating layer 40 may be a cured product (polyurethane resin coating) of a raw material for forming the gas barrier coating layer, which contains a polyvinyl alcohol resin, a polyurethane resin, and a silane compound. The polyurethane resin may be an aqueous polyurethane resin. The aqueous polyurethane resin includes an acid group-containing polyurethane resin and a polyamine compound. By using the aqueous polyurethane resin, it is easy to impart flexibility and gas barrier properties, especially oxygen barrier properties, to the gas barrier coating layer. In the aqueous polyurethane resin, the acid group of the acid group-containing polyurethane resin is bonded to a polyamine compound as a crosslinking agent, thereby exhibiting gas barrier properties. The bond between the acid group of the acid group-containing polyurethane resin and the polyamine compound may be an ionic bond (e.g., an ionic bond between a carboxyl group and a tertiary amino group) or a covalent bond (e.g., an amide bond).
[0057] The acid group-containing polyurethane resin constituting the aqueous polyurethane resin has anionic properties and self-emulsifying properties due to the presence of acid groups, and is also called anionic self-emulsifying polyurethane resin. The acid group of the acid group-containing polyurethane resin can be bonded to the amino group (primary amino group, secondary amino group, tertiary amino group, etc.) of the polyamine compound constituting the aqueous polyurethane resin. Examples of the acid group include a carboxyl group and a sulfonic acid group. The acid group can usually be neutralized by a neutralizing agent (base) and may form a salt with a base. The acid group may be located at the end or side chain of the acid group-containing polyurethane resin, but is preferably located at least on the side chain.
[0058] The acid value of the acid group-containing polyurethane resin can be selected within a range in which the acid group-containing polyurethane resin is water-dispersible, and is usually 5 to 100 mgKOH / g, preferably 10 to 70 mgKOH / g, and more preferably 15 to 60 mgKOH / g. If the acid value of the acid group-containing polyurethane resin is less than the lower limit of the above range, the water dispersibility of the acid group-containing polyurethane resin becomes insufficient, which may lead to a decrease in the uniform dispersion of the aqueous polyurethane resin and other materials and a decrease in the dispersion stability of the coating agent. If the acid value of the acid group-containing polyurethane resin exceeds the upper limit of the above range, the water resistance and gas barrier properties of the gas barrier coating layer 40 may be decreased. By setting the acid value of the acid group-containing polyurethane resin within the above range, it is easy to avoid a decrease in the dispersion stability, and a decrease in the water resistance and gas barrier properties. The acid value of the acid group-containing polyurethane resin can be measured by a method according to JIS K 0070.
[0059] The number average molecular weight of the acid group-containing polyurethane resin can be appropriately selected, but is preferably 800 to 1,000,000, more preferably 800 to 200,000, and even more preferably 800 to 100,000. If the number average molecular weight of the acid group-containing polyurethane resin exceeds the upper limit of the above range, the viscosity of the coating agent increases, which is not preferable. If the number average molecular weight of the acid group-containing polyurethane resin is less than the lower limit of the above range, the gas barrier properties of the gas barrier coating layer may be insufficient. The number average molecular weight of the acid group-containing polyurethane resin is a value calculated in terms of standard polystyrene measured by gel permeation chromatography (GPC).
[0060] The acid group-containing polyurethane resin may be crystalline in order to enhance the gas barrier property. The glass transition temperature of the acid group-containing polyurethane resin is preferably 100°C or higher, more preferably 110°C or higher, and even more preferably 120°C or higher. If the glass transition temperature of the acid group-containing polyurethane resin is less than 100°C, the gas barrier property of the gas barrier coating layer may be insufficient. The glass transition temperature of the acid group-containing polyurethane resin is typically 200°C or lower, further 180°C or lower, and even 150°C or lower. It is practically unlikely that the glass transition temperature of the acid group-containing polyurethane resin that satisfies the preferred ranges of each of the above items will be higher than the upper limit value. Therefore, the glass transition temperature of the acid group-containing polyurethane resin is preferably 100°C to 200°C, more preferably 110°C to 180°C, and even more preferably 120°C to 150°C. The glass transition temperature of the acid group-containing polyurethane resin is measured by differential scanning calorimetry (DSC).
[0061] The polyamine compound constituting the aqueous polyurethane resin is a compound having two or more basic nitrogen atoms. The basic nitrogen atom is a nitrogen atom that can be bonded to the acid group of the acid group-containing polyurethane resin, and examples thereof include nitrogen atoms in amino groups such as primary amino groups, secondary amino groups, and tertiary amino groups. The polyamine compound is not particularly limited as long as it can be bonded to the acid group of the acid group-containing polyurethane resin and improve the gas barrier property, and various compounds having two or more basic nitrogen atoms can be used. The polyamine compound is preferably a polyamine compound having two or more amino groups of at least one type selected from the group consisting of primary amino groups, secondary amino groups, and tertiary amino groups.
[0062] Specific examples of polyamine compounds include alkylenediamines, polyalkylenepolyamines, silicon compounds having multiple basic nitrogen atoms, etc. Examples of alkylenediamines include alkylenediamines having 2 to 10 carbon atoms, such as ethylenediamine, 1,2-propylenediamine, 1,3-propylenediamine, 1,4-butanediamine, and 1,6-hexamethylenediamine. Examples of polyalkylenepolyamines include tetraalkylenepolyamines. Examples of silicon compounds having multiple basic nitrogen atoms (including nitrogen atoms such as amino groups) include silane coupling agents having multiple basic nitrogen atoms, such as 2-[N-(2-aminoethyl)amino]ethyltrimethoxysilane and 3-[N-(2-aminoethyl)amino]propyltriethoxysilane.
[0063] In the aqueous polyurethane resin, the content of the polyamine compound is preferably such that the molar ratio of the acid groups of the acid group-containing polyurethane resin to the basic nitrogen atoms of the polyamine compound (acid groups / basic nitrogen atoms) is 10 / 1 to 0.1 / 1, more preferably 5 / 1 to 0.2 / 1. When the acid group / basic nitrogen atom ratio is within the above range, the crosslinking reaction between the acid groups of the acid group-containing polyurethane and the polyamine compound occurs appropriately, and the gas barrier coating layer exhibits excellent oxygen barrier properties.
[0064] The aqueous polyurethane resin is usually used in the form of a dispersion in an aqueous medium (aqueous dispersion). Examples of the aqueous medium include water, water-soluble or hydrophilic organic solvents, or mixtures thereof. Examples of the water-soluble or hydrophilic organic solvent include alcohols such as methanol, ethanol, and isopropanol; ketones such as acetone and methyl ethyl ketone; ethers such as tetrahydrofuran; cellosolves; carbitols; and nitriles such as acetonitrile. The aqueous medium is preferably water or one containing water as a main component. The content of water in the aqueous medium is preferably 70% by mass or more, more preferably 80% by mass or more. The aqueous medium may or may not contain a neutralizing agent (base) that neutralizes the acid group of the acid group-containing polyurethane resin. Usually, a neutralizing agent is included.
[0065] In the aqueous dispersion of the aqueous polyurethane resin, the average particle size of the dispersed particles (polyurethane resin particles) is not particularly limited, and is preferably 20 to 500 nm, more preferably 25 to 300 nm, and even more preferably 30 to 200 nm. If the average particle size of the dispersed particles exceeds the upper limit of the above range, the uniform dispersion of the dispersed particles and other materials and the dispersion stability of the coating agent may decrease, and the gas barrier properties of the gas barrier coating layer formed from the coating agent may become insufficient. If the average particle size of the dispersed particles is less than the lower limit of the above range, the effect of further improving the dispersion stability of the coating agent and the gas barrier properties of the gas barrier coating layer formed from the coating agent cannot be expected. In addition, it is practically difficult to obtain such a dispersion. The average particle size of the dispersed particles can be measured using a concentrated particle size analyzer (FPAR-10 manufactured by Otsuka Electronics Co., Ltd.) using a dispersion with a solid content concentration of 0.03 to 0.3 mass%.
[0066] The aqueous polyurethane resin may be a commercially available one, or may be one produced by a known production method. Examples of commercially available ones include Takelac WPB-341 manufactured by Mitsui Chemicals, Inc. and Hydran HW350 manufactured by DIC Corporation. The production method of the aqueous polyurethane resin is not particularly limited, and a normal aqueous polyurethane resin technology such as an acetone method or a prepolymer method is used. In the urethanization reaction, a urethanization catalyst such as an amine catalyst, a tin catalyst, or a lead catalyst may be used as necessary. For example, in an inert organic solvent such as a ketone such as acetone, an ether such as tetrahydrofuran, or a nitrile such as acetonitrile, a polyisocyanate compound, a polyhydroxy acid, and, if necessary, at least one of a polyol component and a chain extender component are reacted to prepare an acid group-containing polyurethane resin. More specifically, a polyisocyanate compound, a polyhydroxy acid, and a polyol component are reacted in an inert organic solvent (particularly, a hydrophilic or water-soluble organic solvent) to generate a prepolymer having an isocyanate group at the end, which is neutralized with a neutralizing agent and dissolved or dispersed in an aqueous medium, and then a chain extender component is added and reacted, and the organic solvent is removed to prepare an aqueous dispersion of an acid group-containing polyurethane resin. A polyamine compound is added to the aqueous dispersion of an acid group-containing polyurethane resin thus obtained, and the aqueous polyurethane resin in the form of an aqueous dispersion can be prepared by heating as necessary. When heating, the heating temperature is preferably 30°C to 60°C.
[0067] When forming a polyurethane resin film, the amount of polyurethane resin in the polyurethane resin film forming raw material may be 0.9 to 4.0 parts by mass per 1 part by mass of the polyvinyl alcohol resin from the viewpoint of bending resistance and gas barrier property, preferably 1.1 to 3.0 parts by mass, more preferably 1.2 to 2.5 parts by mass.
[0068] The thickness of the gas barrier coating layer 40 is set according to the required oxygen barrier properties, and can be, for example, 0.05 to 5 μm. The thickness of the gas barrier coating layer 40 is preferably 0.05 to 1 μm, and more preferably 0.1 to 0.5 μm. If the thickness of the gas barrier coating layer 40 is 0.05 μm or more, sufficient oxygen barrier properties are easily obtained. If the thickness of the gas barrier coating layer 40 is 1 μm or less, it is easy to form a uniform coating surface, and drying load and production costs can be suppressed.
[0069] A gas barrier film having the above-mentioned organic / inorganic composite coating, polycarboxylic acid polyvalent metal salt coating, polyurethane resin coating, or the like as the gas barrier coating layer 40 exhibits excellent oxygen barrier properties even when subjected to boiling treatment or retort sterilization treatment.
[0070] Incidentally, when forming a gas barrier layer on the substrate, the substrate is exposed to heat during a drying process or the like. Depending on the substrate, partial sagging may occur due to the heat, and depending on how such sagging occurs, coating unevenness and cracks in the gas barrier layer (inorganic oxide layer) are likely to occur. As a result, there is a problem that it is difficult to obtain sufficient barrier properties as a gas barrier film. The inventors have conducted extensive research into this point and have found that the degree of the sagging of the substrate that occurs during the formation of the gas barrier layer can be grasped in advance by thoroughly analyzing the thermal strain in the TD direction of the substrate using a thermomechanical analyzer (TMA) and observing the local difference in the thermal strain (the difference between the maximum and minimum values of the thermal strain). In other words, it has been found that a substrate with a large difference between the maximum and minimum values of the thermal strain (the difference between the strain at a point where the shrinkage due to heat is large and that at a point where the shrinkage is small) is likely to sag due to heat during the formation of the gas barrier layer.
[0071] From the above findings, in this embodiment, a substrate for gas barrier film is used for a gas barrier film having a substrate and a gas barrier layer in this order, and the difference between the maximum and minimum values of thermal strain measured as follows is 0.005 or less. By using such a substrate, it is possible to sufficiently suppress the occurrence of partial slack due to heat applied when forming a gas barrier layer on the substrate. This makes it possible to obtain a gas barrier film with excellent barrier properties. That is, it can be said that the substrate for gas barrier film is a substrate (base roll) suitable for obtaining a gas barrier film with excellent barrier properties. From this viewpoint, the difference between the maximum and minimum values of thermal strain is preferably 0.003 or less, more preferably 0.002 or less, and even more preferably 0.001 or less. The lower limit of the difference between the maximum and minimum values of thermal strain is not particularly limited, but the smaller the difference, the less likely slack occurs, so it can be set to 0.
[0072] [Thermal strain measurement method] A sample having a dimension of 4 mm in the MD (machine direction) and a dimension of 25 mm in the TD (transverse direction) is taken from the substrate. At this time, the center of each sample in the TD (transverse direction) is adjusted to a position of 50 mm + 100 mm × N from one end of the substrate in the TD direction, and a plurality of samples are taken for the entire width of the substrate in the TD direction. N is an integer of 1 or more, and the upper limit of N can be appropriately adjusted according to the width W of the substrate. From the viewpoint of the width W (length in the TD direction) of a general substrate original roll, for example, N may be an integer of 5 or more, 10 or more, or 15 or more, or may be an integer of 30 or less. Then, a thermal history of heating from 20 to 100 ° C. and cooling from 100 to 20 ° C. is given to each sample under a tension of 30 mN in the TD direction, and a thermomechanical analysis is performed. Then, the difference between the maximum and minimum thermal strains in the TD direction of each sample is calculated.
[0073] Fig. 2 is a schematic diagram showing how to take samples from a substrate. As shown in the figure, multiple samples are taken across the entire width W of the substrate in the TD direction, i.e., a total of 1+N samples, sample No. 0 to sample No. N. Samples are taken while avoiding both ends E (width: 37.5 mm) in the TD direction of the substrate. If the TD direction of the sample to be taken overlaps with the ends E, that sample is not taken, and the previous sample is treated as sample No. N and collection is terminated.
[0074] The above measurement method focuses on the drying process during the formation of the gas barrier coating layer (after coating), performs thermomechanical analysis of the substrate in a temperature range (20 to 100°C) simulating the inside of a coater drying furnace, and identifies the difference between the maximum and minimum values of thermal strain in the TD direction that is permissible from the viewpoint of maintaining the barrier properties. The heating rate during heating and the cooling rate during cooling are not particularly limited, but can be, for example, about 10°C / min. The thermal strain in the TD direction of each sample is the value (unitless) obtained by dividing the amount of change in the sample by the original length of the sample.
[0075] <Laminates and packaging materials> When a heat seal layer (thermal adhesive layer) is provided on the gas barrier layer of the gas barrier film 1 having the above basic structure, a laminate applicable to packaging materials is obtained. That is, the laminate of this embodiment includes the above gas barrier film and a thermal adhesive layer formed on the gas barrier layer of the gas barrier film. Moreover, by preparing one or more sheets of the above laminate, and heat sealing the edges by facing each other, a packaging material using the gas barrier film 1 can be formed. That is, the packaging material of this embodiment is formed from the above laminate. Since such a packaging material uses a base material in which the difference between the maximum and minimum values of thermal strain is 0.005 or less, it can exhibit suitable barrier properties even when subjected to high-temperature treatment such as boiling or retorting. Moreover, since the above gas barrier film 1 is formed without using a metal foil or a metal vapor deposition film, it has transparency that allows the contents to be visually recognized, and is also excellent in bending resistance and stretching resistance.
[0076] The heat-sealing layer can be, for example, a CPP film (unstretched polypropylene film) having a thickness of about 40 to 200 μm. The heat-sealing layer can be laminated on the gas barrier film by a known dry lamination method, extrusion lamination method, or the like, using a known adhesive such as a polyurethane-based, polyester-based, or polyether-based adhesive. By making both the base material 10 and the heat-sealing layer from polypropylene, the polypropylene content in the laminate and packaging material can be 90 mass % or more. This makes the laminate and packaging material a so-called mono-material material, improving the recyclability.
[0077] <Method of manufacturing gas barrier film> An example of a method for producing the gas barrier film 1 will be described below. The method for producing the gas barrier film includes the steps of: A step of measuring the difference between the maximum and minimum values of thermal strain of the substrate as follows, and selecting a substrate A having a difference between the maximum and minimum values of 0.005 or less and a substrate B having a difference between the maximum and minimum values of 0.005 or more; A heat treatment process (optional, however) of heat-treating the substrate B to produce substrate A having a difference between the maximum and minimum values of thermal strain of 0.005 or less; The method includes a gas barrier layer forming step of forming, on the substrate A, an underlayer and a gas barrier coating layer, an inorganic oxide layer and a gas barrier coating layer, or an underlayer, an inorganic oxide layer and a gas barrier coating layer in this order. [Thermal strain measurement method] A sample with a dimension of 4 mm in the MD direction and 25 mm in the TD direction is taken from the substrate. At this time, the center of each sample in the TD direction is adjusted to a position 50 mm + 100 mm × N (N is an integer of 1 or more) from one end of the substrate in the TD direction, and multiple samples are taken over the entire width of the substrate in the TD direction. Then, each sample is subjected to a thermal history of heating from 20 to 100 ° C and cooling from 100 to 20 ° C while applying a tension of 30 mN in the TD direction, and a thermomechanical analysis is performed. Then, the difference between the maximum and minimum thermal strains in the TD direction of each sample is calculated.
[0078] The cause of the difference between the maximum and minimum values of thermal strain (shrinkage variation) in the TD direction of the substrate is assumed to be temperature unevenness in the TD direction during substrate film formation (stretching, heat setting). If there is unevenness in the heat setting temperature, there will be partial differences in the degree of shrinkage when the substrate shrinks due to heat during subsequent drying. Therefore, before sending the substrate to the gas barrier layer formation process, the difference between the maximum and minimum values of thermal strain of the substrate is measured, and a substrate with a difference of 0.005 or less is selected. For substrates with a difference of more than 0.005, a heat treatment is performed to eliminate the temperature unevenness during substrate film formation, and the difference can be made 0.005 or less. The heat treatment temperature at this time is preferably set to a temperature equal to or higher than the heat setting temperature during substrate film formation and within a range equal to or lower than the melting point of the substrate. A gas barrier layer formation process is performed on a substrate selected or prepared by heat treatment, in which the difference between the maximum and minimum values of thermal strain is 0.005 or less, to produce a gas barrier film with excellent barrier properties.
[0079] The underlayer 20 may be formed, for example, by applying a coating agent to the first surface 10a of the substrate 10 by a wet coating method to form a coating film, and then drying the coating film (to remove the solvent). The coating agent can be applied by a known wet coating method, such as roll coating, gravure coating, reverse coating, die coating, screen printing, and spray coating. The method for drying the coating film made of the coating agent can be a known drying method such as hot air drying, heat roll drying, infrared irradiation, etc. The drying temperature for the coating film can be, for example, 50 to 200° C. The drying time varies depending on the thickness of the coating film, the drying temperature, etc., but can be, for example, 1 second to 5 minutes.
[0080] The inorganic oxide layer 30 can be formed on the first surface 10a of the substrate 10 or on the underlayer 20 by using the above-mentioned vacuum deposition method, sputtering method, ion plating method, plasma chemical vapor deposition (CVD) method, or the like.
[0081] The gas barrier coating layer 40 can be formed, for example, by applying a coating agent onto the underlayer 20 or the inorganic oxide layer 30 by a wet coating method to form a coating film, and then drying the coating film (removing the solvent). The coating agent can be applied and dried in the same manner as described in the step of forming the underlayer 20. The gas barrier coating layer 40 can be formed by a single application and drying step, or by multiple applications and drying steps using the same or different coating agents.
[0082] The above steps complete the gas barrier film 1. The gas barrier film 1 may further include a printed layer, a protective layer, a light-shielding layer, an adhesive layer, a heat-sealable heat fusion layer, and other functional layers, as required. EXAMPLES
[0083] The present invention will be described in more detail with reference to the following examples, but the present invention is not limited to these examples.
[0084] <Preparation of the substrate> As a substrate, a biaxially oriented polypropylene film (VPH2011 manufactured by AJPlast) having a thickness of 20 μm and having a first surface subjected to a corona treatment was prepared. The difference between the maximum and minimum values of thermal strain of this substrate was measured as follows, and was found to be 0.0208 (Comparative Example 2). This substrate was then placed in an oven and heated under the temperature conditions shown in Table 1, and the difference between the maximum and minimum values of thermal strain was measured again. Substrates with a difference of 0.005 or less were selected as substrates corresponding to the examples, and substrates with a difference of more than 0.005 were selected as substrates corresponding to the comparative examples. [Thermal strain measurement method] A sample with a dimension of 4 mm in the MD direction and a dimension of 25 mm in the TD direction was taken from the substrate. At this time, the center of each sample in the TD direction was adjusted to a position of 50 mm + 100 mm × 19 from one end of the substrate in the TD direction, and 20 samples were taken from the entire width of the substrate in the TD direction. Then, each sample was subjected to a thermal history of heating from 20 to 100 ° C. and cooling from 100 to 20 ° C. with a tension of 30 mN in the TD direction, and a thermomechanical analysis was performed. A thermal analysis system TA7000 series manufactured by Hitachi High-Tech Science Corporation was used as the thermomechanical analysis device. The difference between the maximum and minimum thermal strains in the TD direction of each sample was calculated.
[0085] <Preparation of gas barrier film> Mixture A prepared by the procedure described below was applied to the first surface of the substrate of each example using a gravure printing machine to form a coating film, and the coating film was then dried in an oven at 80°C for 10 seconds to form a 0.1 μm-thick undercoat layer. (Preparation procedure for mixed solution A) Acrylic polyol was Acrydic CL-1000 (DIC Corporation), and the isocyanate compound was TDI type curing agent Coronate 2030 (Tosoh Corporation). The acrylic polyol and the isocyanate compound were mixed in a solids weight ratio of 6:4, and the solids content was adjusted to 2 mass% using a dilution solvent (ethyl acetate).
[0086] Next, a mixed material containing two or more of silicon metal, silicon monoxide, and silicon dioxide was evaporated using a vacuum deposition apparatus using an electron beam heating method to form an inorganic oxide layer made of silicon oxide having a thickness of 30 nm on the underlayer.
[0087] Next, mixed solution B prepared by the procedure described below was applied onto the inorganic oxide layer using a bar coater to form a coating film, and then dried in a 100°C oven for 10 seconds to form a gas barrier coating layer with a thickness of 0.3 μm. (Preparation procedure for mixed solution B) The following liquids a, b, and c were mixed in a compounding ratio (wt%) of 70:20:10. Solution A: A hydrolysis solution with a solid content of 5 wt% (SiO2 equivalent) obtained by adding 72.1 g of hydrochloric acid (0.1N) to 17.9 g of tetraethoxysilane (hereinafter referred to as TEOS) and 10 g of methanol and stirring for 30 minutes. Liquid B: 5 wt% water / methanol solution of polyvinyl alcohol (water / methanol weight ratio = 95 / 5). Liquid c: Hydrochloric acid (1N) was gradually added to β-(3,4-epoxycyclohexyl)ethyltrimethoxysilane and isopropyl alcohol (IPA solution), and the solution was stirred for 30 minutes to hydrolyze, then hydrolyzed in a 1 / 1 water / IPA solution to adjust the solid content to 5 wt% (calculated as R2Si(OH)3).
[0088] In this manner, a gas barrier film using the substrate of each example was obtained.
[0089] <Preparation of laminates and packaging materials> A 60 μm thick CPP film (Toray Film Processing Co., Ltd., Torayfan ZK93KM) was attached to the gas barrier coating layer of each gas barrier film using an adhesive to provide a heat-sealed layer. As the adhesive, a two-liquid curing adhesive Takelac A620 (base agent) / Takenate A65 (curing agent) manufactured by Mitsui Chemicals Polyurethane was used, and dry laminated using a multi-coater TM-MC manufactured by HIRANO TECSEED and cured at 40° C. for 3 days. As a result, a laminate according to each example was obtained. The polypropylene content of each laminate according to each example was 90% by mass or more.
[0090] From each laminate, an A5-sized film corresponding to each location in the TD direction where the thermomechanical analysis was performed was cut out, and an A5-sized four-sided sealed pouch (packaging material) was produced by placing the heat-sealing layers opposite each other and sealing the peripheral portions.
[0091] <Oxygen permeability measurement> Each pouch obtained as described above was filled with 200 ml of tap water, sealed, and subjected to heat sterilization treatment (retort treatment) in hot water at 121° C. for 30 minutes. After retort treatment, samples were cut out from each pouch and measured for oxygen permeability (cc / (m)) using an oxygen permeability measuring device (product name: OXTRAN-2 / 20, manufactured by MOCON) under an atmosphere of 23°C and 50% RH (relative humidity). 2 The oxygen permeability was measured for each pouch (corresponding to each location in the TD direction where the thermomechanical analysis was performed), and the average value was calculated. The results are shown in Table 1.
[0092] [Table 1] [Explanation of symbols]
[0093] Reference Signs List 1: gas barrier film, 10: substrate, 10a: first surface, 20: undercoat layer, 30: inorganic oxide layer, 40: gas barrier coating layer, 50: gas barrier layer.
Claims
1. A substrate for a gas barrier film, which is used in a gas barrier film having a substrate and a gas barrier layer in this order, A substrate having a difference between the maximum and minimum values of thermal distortion measured as follows of 0.005 or less. [Thermal strain measurement method] A sample having a dimension of 4 mm in the MD direction and a dimension of 25 mm in the TD direction is taken from the substrate. At this time, the center of each sample in the TD direction is adjusted to be 50 mm + 100 mm × N (N is an integer of 1 or more) from one end of the substrate in the TD direction, and multiple samples are taken over the entire width of the substrate in the TD direction. Then, each sample is subjected to a thermal history of heating from 20 to 100 ° C. and cooling from 100 to 20 ° C. with a tension of 30 mN applied in the TD direction, and a thermomechanical analysis is performed. Then, the difference between the maximum and minimum thermal strains in the TD direction of each sample is calculated.
2. 2. The substrate for gas barrier films according to claim 1, which is a polyolefin-based resin film, a polyester-based resin film, or a polyamide-based resin film.
3. 2. The substrate for gas barrier films according to claim 1, wherein the gas barrier layer comprises, from the substrate side, an undercoat layer and a gas barrier coating layer; an inorganic oxide layer and a gas barrier coating layer; or an undercoat layer, an inorganic oxide layer and a gas barrier coating layer in this order.
4. The gas barrier film substrate according to claim 3, wherein the undercoat layer has a thickness of 0.01 to 1 μm.
5. 5. The gas barrier film substrate according to claim 4, wherein the undercoat layer contains an organic polymer as a main component, and the organic polymer contains at least one of a polyacrylic resin, a polyol resin, a polyurethane resin, and a polyamide resin.
6. The gas barrier film substrate according to any one of claims 3 to 5, wherein the inorganic oxide layer has a thickness of 1 to 200 nm.
7. The substrate for gas barrier films according to any one of claims 3 to 5, wherein the inorganic oxide layer contains aluminum oxide or silicon oxide.
8. The gas barrier film substrate according to any one of claims 3 to 5, wherein the gas barrier coating layer has a thickness of 0.05 to 1 µm.
9. The gas barrier film substrate according to any one of claims 3 to 5, wherein the gas barrier coating layer is a cured product of a raw material for forming the gas barrier coating layer, the raw material comprising at least one of a metal alkoxide and a hydrolyzate of a metal alkoxide, and a water-soluble polymer.
10. The substrate for a gas barrier film according to claim 9 , wherein the raw material for forming the gas barrier coating layer contains at least one of a silane coupling agent and a hydrolysate of a silane coupling agent.
11. The gas barrier film substrate according to any one of claims 3 to 5, wherein the gas barrier coating layer contains a polyvalent metal salt of a carboxylic acid which is a reaction product between a carboxy group of a polycarboxylic acid polymer and a polyvalent metal compound.
12. The gas barrier film substrate according to any one of claims 3 to 5, wherein the gas barrier coating layer is a cured product of a gas barrier coating layer forming raw material containing a polyvinyl alcohol resin, a polyurethane resin and a silane compound.
13. A gas barrier film comprising the substrate for gas barrier films according to claim 1 or 2 and a gas barrier layer in this order.
14. The gas barrier film according to claim 13; a heat seal layer formed on the gas barrier layer of the gas barrier film; A laminate comprising:
15. The laminate according to claim 14 , wherein the gas barrier film substrate and the heat seal layer contain polypropylene as a main component.
16. The laminate according to claim 15, wherein the polypropylene content is 90% by mass or more.
17. A packaging material formed from the laminate of claim 14.
Citation Information
Patent Citations
Vacuum insulation material outer packaging material, vacuum insulation material, and apparatus with vacuum insulation material
JP2017150565A