Catalyst for exhaust gas purification

By employing an alumina-ceria-zirconia composite oxide with low Ce concentration and pyrochlore type ceria-zirconia composite oxide in the Rh coating layer, the catalyst enhances both exhaust gas purification and OSC performance, especially at low temperatures.

JP2024165417AActive Publication Date: 2024-11-28TOYOTA JIDOSHA KK
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2023081601
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-17
Publication Date
2024-11-28
Estimated Expiration
2043-05-17

AI Technical Summary

Technical Problem

Conventional exhaust gas purification catalysts face challenges in achieving both high exhaust gas purification performance and oxygen storage capacity (OSC) performance, particularly under low-temperature conditions, due to the interaction of Rh with OSC materials.

Method used

The use of an alumina-ceria-zirconia composite oxide with low Ce concentration and a pyrochlore type ceria-zirconia composite oxide in the Rh coating layer addresses this issue, enhancing both purification and OSC performance.

Benefits of technology

The catalyst achieves improved exhaust gas purification and OSC performance, particularly at low temperatures, by optimizing the interaction between Rh and the composite oxides.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024165417000001_ABST
    Figure 2024165417000001_ABST
Patent Text Reader

Abstract

To provide a catalyst for exhaust gas purification that combines exhaust purifying performance with OSC performance.SOLUTION: A catalyst for exhaust gas purification includes a substrate and a catalyst coat layer formed on the substrate. The catalyst coat layer includes a Pd coat layer containing Pd and an Rh coat layer containing Rh. The Rh coat layer includes alumina-ceria-zirconia complex oxide with a ceria content of less than 20 wt.% and pyrochlore type ceria-zirconia complex oxide.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an exhaust gas purifying catalyst. [Background technology]

[0002] In recent years, while exhaust gas regulations have become stricter, there is a demand to reduce the amount of precious metals used in exhaust gas purification catalysts from the perspective of resource risks. In order to make effective use of precious metals, oxygen storage capacity (OSC) materials are used, which mitigate atmospheric fluctuations and maintain the activity of the precious metals. Here, when Rh is used as a catalytic metal, if the OSC material and Rh are used in close proximity, the OSC function is exerted at low temperatures, but the state change of the precious metal is delayed, and there is a risk of a decrease in purification activity.

[0003] In response to this, for example, in Patent Document 1, an Al2O3-ZrO2 composite oxide and an Al2O3-CeO2-ZrO2 composite oxide are used in the upstream catalyst layer, and Rh is supported on the Al2O3-ZrO2 composite oxide, thereby improving the purification activity and achieving both exhaust gas purification performance and OSC performance.

[0004] In the future, with the introduction of the proposed Euro 7 exhaust gas regulations, OSC performance at low temperatures will become even more important, and there will be a demand for exhaust gas purification catalysts that can maintain purification activity while using OSC materials. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2017-189745 A Summary of the Invention [Problem to be solved by the invention]

[0006] As described above, in conventional exhaust gas purification catalysts, further improvement in compatibility between exhaust gas purification performance and OSC performance has been required. Therefore, an object of the present invention is to provide an exhaust gas purification catalyst that achieves both exhaust gas purification performance and OSC performance. [Means for solving the problem]

[0007] The present inventors discovered that by combining an alumina-ceria-zirconia composite oxide with a low Ce concentration and a pyrochlore-type ceria-zirconia composite oxide in a Rh coating layer, it is possible to achieve both exhaust gas purification performance and OSC performance, and completed the present invention.

[0008] That is, the gist of the present invention is as follows. (1) A catalyst for purifying exhaust gas, comprising a substrate and a catalytic coating layer formed on the substrate, the catalytic coating layer comprising a Pd coating layer containing Pd and a Rh coating layer containing Rh, the Rh coating layer comprising an alumina-ceria-zirconia-based composite oxide having a ceria content of less than 20% by weight, and a pyrochlore-type ceria-zirconia-based composite oxide. Effect of the Invention

[0009] According to the present invention, it is possible to provide an exhaust gas purification catalyst that achieves both exhaust gas purification performance and OSC performance. [Brief description of the drawings]

[0010] [Figure 1] 1 is a schematic cross-sectional view showing one embodiment of an exhaust gas purifying catalyst of the present invention. [Diagram 2] 1 is a table and a graph showing the difference in performance depending on the composition of the Rh layer in an embodiment. [Diagram 3] 1 is a table and a graph showing the difference in performance depending on the CeO2 content of ACZ in the examples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] Preferred embodiments of the present invention will now be described in detail.

[0012] FIG. 1 is a schematic cross-sectional view showing one embodiment of the exhaust gas purification catalyst (hereinafter also referred to as catalyst) of the present invention. As shown in FIG. 1, the exhaust gas purification catalyst 10 has a substrate 11 and a catalyst coating layer 12 formed on the substrate 11. The catalyst coating layer 12 has a Pd coating layer 13 containing Pd and a Rh coating layer 14 containing Rh, and preferably has a two-layer structure consisting of these layers. In the catalyst coating layer, the arrangement of layers is not particularly limited, but preferably, the Pd coating layer is the lower layer and the Rh coating layer is the upper layer. The coating width of the Pd coating layer is usually in the range of 20% to 100% (preferably 30% to 50%) of the total length of the substrate from the end face, and the coating width of the Rh coating layer is usually in the range of 20% to 100% (preferably 70% to 90%) of the total length of the substrate from the end face on the opposite side to the Pd coating layer.

[0013] The Pd coating layer preferably contains, in addition to Pd as a catalytic metal, a metal oxide (e.g., alumina (Al2O3), alumina-ceria (CeO2)-zirconia (ZrO2) composite oxide) and an alkaline earth metal element (e.g., barium). In the Pd coating layer, the Pd content is usually 0.1 g / L to 10 g / L relative to the volume of the substrate.

[0014] The Rh coating layer contains, in addition to Rh as a catalytic metal, an alumina-ceria-zirconia composite oxide (hereinafter also referred to as ACZ composite oxide) and a pyrochlore-type ceria-zirconia composite oxide (hereinafter also referred to as pyrochlore-type CZ composite oxide. It can also be expressed as pyrochlore-type ZC composite oxide.) The Rh content is usually 0.01 g / L to 5 g / L with respect to the volume of the substrate.

[0015] From the viewpoint of high low-temperature purification activity of the catalyst, the ACZ composite oxide contained in the Rh coating layer has a ceria content of less than 20% by weight, preferably 15% by weight or less, based on the composite oxide. Rh is preferably supported on the ACZ composite oxide.

[0016] In the ACZ composite oxide contained in the Rh coating layer, the alumina content is usually 40% by weight to 70% by weight, and the zirconia content is usually 10% by weight to 30% by weight. The ACZ composite oxide may contain other metal oxides (e.g., Nd2O3, La2O3, Y2O3, etc.) in addition to alumina, ceria, and zirconia, and the total content of the other metal oxides is usually 10% by weight or less.

[0017] The content of the ACZ composite oxide in the Rh coating layer is usually 100 g / L to 140 g / L relative to the volume of the base material.

[0018] In pyrochlore-type CZ composite oxides, a crystalline phase (pyrochlore phase) having a pyrochlore-type ordered array structure of cerium ions and zirconium ions is formed. In addition to ceria and zirconia, pyrochlore-type CZ composite oxides can also contain other metal oxides (e.g., PrO 11 The total content of other metal oxides is usually 5% by weight or less. The cerium ions and zirconium ions may be partially substituted with additional elements such as praseodymium. In the pyrochlore type CZ composite oxide, the ceria content is usually 30% by weight to 70% by weight, and the zirconia content is usually 30% by weight to 70% by weight.

[0019] The content of the pyrochlore-type CZ composite oxide in the Rh coating layer is usually 10 g / L to 25 g / L (preferably 12 g / L to 20 g / L) relative to the volume of the base material.

[0020] In the catalyst of the present invention, the use of an ACZ composite oxide with a low Ce concentration (ceria content less than 20 wt %) in the Rh coating layer suppresses the decrease in Rh activity caused by Ce, while the use of a pyrochlore-type CZ composite oxide improves the OSC performance, thereby achieving a high level of both exhaust gas purification performance and OSC performance.

[0021] The catalyst of the present invention can be prepared by coating a substrate with a slurry containing the components of each layer of the catalyst coating layer by a method known to those skilled in the art. EXAMPLES

[0022] The present invention will be described in more detail below with reference to examples, although the technical scope of the present invention is not limited to these examples.

[0023] <Preparation of catalyst> Raw materials used Material 1 (Al2O3): La2O3 composite Al2O3 (La2O3: 1% by weight) Material 2 (ACZ): ACZ composite oxide (Al2O3: 62% by weight / CeO2: 10% by weight / ZrO2: 22% by weight / Nd2O3: 2% by weight / La2O3: 2% by weight / Y2O3: 2% by weight) Material 3 (ACZ): ACZ composite oxide (Al2O3: 57% by weight / CeO2: 12% by weight / ZrO2: 25% by weight / Nd2O3: 2% by weight / La2O3: 2% by weight / Y2O3: 2% by weight) Material 4 (ACZ): ACZ composite oxide (Al2O3: 30% by weight / CeO2: 20% by weight / ZrO2: 44% by weight / Nd2O3: 2% by weight / La2O3: 2% by weight / Y2O3: 2% by weight) Material 5 (ACZ): ACZ composite oxide (Al2O3: 25% by weight / CeO2: 23% by weight / ZrO2: 46% by weight / Nd2O3: 2% by weight / La2O3: 2% by weight / Y2O3: 2% by weight) Material 6 (ACZ): ACZ composite oxide (Al2O3: 15% by weight / CeO2: 30% by weight / ZrO2: 49% by weight / Nd2O3: 2% by weight / La2O3: 2% by weight / Y2O3: 2% by weight) Material 7 (AZ): Al2O3-ZrO2 composite oxide (Al2O3: 30% by weight / ZrO2: 60% by weight / La2O3: 5% by weight / Y2O3: 5% by weight) Material 8 (pyrochlore-type CZ): CZ composite oxide (prepared in the same manner as Pr-doped pyrochlore CZ described in the examples of JP 2018-38999 A; CeO2: 51.5 wt% / ZrO2: 45.5 wt% / PrO 11:3% by weight) Material 9 (Ba): Ba sulfate Material 10 (Rh): Nitric acid Rh aqueous solution (Rh concentration: 2.75% by weight) Material 11 (Pd): Pd nitrate aqueous solution (Rh concentration: 8.40% by weight) Base material: 875cc (600 cells hexagonal, wall thickness 2mil, total length 105mm) cordierite honeycomb base material

[0024] Comparative Example 1 First, Pd nitrate (material 11) and ACZ (material 4) were added to distilled water while stirring, and then dried and fired to prepare Pd / ACZ in which Pd was supported on ACZ. Pd / ACZ, Al2O3 (material 1), Ba sulfate (material 9), and Al2O3-based binder were added to distilled water while stirring to prepare slurry 1. Next, the prepared slurry 1 was poured into the end face of the substrate, and unnecessary parts were blown away with a blower to coat the material on the substrate wall. At that time, the coating material was prepared so that the coating layer was 6g / L-zone as Pd for material 11, 50g / L-zone for material 1, 100g / L-zone for material 4, and 15g / L-zone for material 9 relative to the substrate volume. The coating width was adjusted to 40% of the substrate total length. Finally, the moisture was removed in a dryer maintained at 120°C for 2 hours, and then the material was fired in an electric furnace at 500°C for 2 hours to prepare the first coating layer (lower Pd layer).

[0025] Next, Rh nitrate (material 10) and AZ (material 7) were added to distilled water while stirring, and this was dried and fired to prepare Rh / AZ in which Rh was supported on AZ. Rh / AZ, Al2O3 (material 1), ACZ (material 4), and an Al2O3-based binder were added to distilled water while stirring to prepare a suspended slurry 2. This was poured into the substrate coated with slurry 1 from the end face opposite to the end face coated with slurry 1, and unnecessary parts were blown away with a blower to coat the material on the substrate wall. At that time, the coating material was prepared so that the coating layer was 0.40 g / L-zone as Rh for material 10, 35 g / L-zone for material 1, 100 g / L-zone for material 4, and 30 g / L-zone for material 7 relative to the substrate volume. The coating width was adjusted to 80% of the substrate total length. Finally, the moisture was removed in a dryer maintained at 120°C for 2 hours, and then the catalyst was baked in an electric furnace at 500°C for 2 hours to prepare the second coating layer (upper Rh layer), resulting in the preparation of a catalyst with two coating layers.

[0026] The catalysts of Examples 1 to 3 and Comparative Examples 2 to 7 were prepared by changing the materials, compositions, and Rh-supporting positions in slurry 2 for forming the upper Rh layer, as shown in Tables 1-1 and 1-2. The configurations of the catalysts of Examples 1 to 3 and Comparative Examples 1 to 7 are shown in the following Tables 1-1 and 1-2.

[0027] [Table 1]

[0028] <Durability test> A durability test was carried out for each catalyst prepared using an actual engine. Specifically, each catalyst was attached to the exhaust system of a V8 engine, and the durability test was carried out by repeatedly flowing exhaust gases in stoichiometric and lean atmospheres for a certain period of time (ratio of 3:1) at a catalyst bed temperature of 950°C for 50 hours.

[0029] <Performance evaluation> For each catalyst that underwent durability testing, a performance evaluation was carried out using an actual engine. Specifically, each catalyst was installed in the exhaust system of an L-type 4-cylinder engine, and OSC performance evaluation and NOx-T50 evaluation were carried out under the following conditions.

[0030] OSC performance evaluation The oxygen absorption and release capacity was measured by supplying exhaust gas with an air-fuel ratio (A / F) of 14.1-15.1 and 600°C, and repeating this in short cycles. The higher the value, the better it can absorb A / F fluctuations in the engine exhaust gas, keeping the atmosphere inside the catalyst close to stoichiometric, and maintaining high purification performance.

[0031] NOx-T50 evaluation Exhaust gas with an air-fuel ratio (A / F) of 14.4 was supplied, and the temperature was raised at Ga = 35g / s and 20℃ / min, the NOx purification rate was measured, and the NOx purification activity was evaluated based on the temperature at which the NOx purification rate reached 50% (NOx-T50). The smaller the NOx-T50 value, the better the low-temperature purification activity.

[0032] The evaluation results of the catalysts of Examples 1 to 3 and Comparative Examples 1 to 7 are shown in Figures 2 and 3. Figure 2 shows the performance difference depending on the composition of the Rh layer. Figure 3 shows the performance difference depending on the CeO2 content of ACZ.

[0033] As shown in Fig. 2, the catalyst of Example 1 supported Rh on ACZ with a low ceria content (low Ce concentration) and combined with pyrochlore-type CZ with excellent OSC performance, and thus achieved a high balance between low-temperature purification activity and OSC performance compared to the catalysts of Comparative Examples 1 to 3 with different Rh layer compositions. Note that, compared to Comparative Example 1, which used a conventional material combination and Rh-supported position, Comparative Example 2, in which Rh was also supported on ACZ, showed a decrease in low-temperature purification activity. Moreover, Comparative Example 3, which used only ACZ with a low ceria content, showed good low-temperature purification activity, but a significant decrease in OSC performance.

[0034] In Figure 3, the amount of Ce contained in each catalyst was constant, so there was no significant difference in the OSC performance of each catalyst. However, since the Ce utilization efficiency decreases as the Ce concentration increases, the OSC performance slightly decreased as the ceria (CeO2) content of ACZ increased. On the other hand, the low-temperature purification activity was better with a lower ceria content. In particular, when the ceria content was less than 20 wt%, the low-temperature purification activity was significantly higher. This is presumably because the Ce amount in each catalyst was constant, so the lower the Ce concentration, the wider the support field and the fewer the contact points between Rh and Ce. [Explanation of symbols]

[0035] 10: exhaust gas purification catalyst, 11: substrate, 12: catalyst coating layer, 13: Pd coating layer, 14: Rh coating layer

Claims

[Claim 1] A catalyst for purifying exhaust gas, comprising a substrate and a catalyst coating layer formed on the substrate, the catalyst coating layer has a Pd coating layer containing Pd and a Rh coating layer containing Rh, the Rh coating layer contains an alumina-ceria-zirconia-based composite oxide having a ceria content of less than 20% by weight, and a pyrochlore-type ceria-zirconia-based composite oxide; Catalyst for purifying exhaust gas.

Citation Information

Patent Citations

  • Exhaust purifying catalyst

    JP2012086199A

  • Catalyst carrier for exhaust gases and exhaust gas purification catalyst

    JP2014100614A

  • Exhaust gas purification catalyst

    JP2016112489A

  • Exhaust gas purification catalyst

    JP2018038999A

  • Exhaust gas purifying catalyst, exhaust gas purifying apparatus using same, and exhaust gas purifying method

    WO2010064497A1