Terbium-containing paramagnetic garnet-type transparent ceramic, method for producing the same, and mixed raw materials for the same, as well as magneto-optical device using the same and method for manufacturing the same

A terbium-containing paramagnetic garnet-type transparent ceramic with a specific composition and manufacturing process addresses thermal lensing issues, maintaining beam integrity and transparency at high powers, suitable for high-power laser applications.

JP2024165426APending Publication Date: 2024-11-28SHIN ETSU CHEMICAL CO LTD

Patent Information

Application Number
JP2023081620
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-17
Publication Date
2024-11-28

AI Technical Summary

Technical Problem

Existing paramagnetic garnet-type transparent ceramics used in high-power laser applications suffer from significant thermal lensing effects, leading to beam distortion and reduced manufacturing reproducibility, especially when subjected to high input powers.

Method used

A terbium-containing paramagnetic garnet-type transparent ceramic with a specific composition (Tb1-x-yYxScyAl1-zSczO12) and optimized manufacturing process, including controlled calcination, sintering, and polishing, to minimize thermal lensing and maintain beam integrity at high powers.

Benefits of technology

The ceramic maintains a maximum beam diameter change of 10% or less even at 160 W input power, ensuring high transparency and stability for high-power laser applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024165426000001_ABST
    Figure 2024165426000001_ABST
Patent Text Reader

Abstract

To provide a terbium-containing paramagnetic garnet-type transparent ceramic etc. capable of, even when an incident power of a laser beam having a diameter of 1.6 mm at a wavelength of 1064 nm is raised to 160 W, limiting the maximum change in the diameter of the incident laser beam to 10% or less.SOLUTION: Terbium-containing paramagnetic garnet-type transparent ceramics comprise a sintered compact of a complex oxide represented by a formula (1), where the total light transmittance at a wavelength of 600 nm is 84.8% or more. (Tb1-x-yYxScy)3(Al1-zScz)5O12 (1) (In the formula, 0.35≤x≤0.45, 0<y<0.03, 0.5<1-x-y<0.65, 0.001<z<0.03, 0<y+z<0.06).SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a terbium-containing paramagnetic garnet-type transparent ceramic, a manufacturing method thereof, a raw material mixture therefor, and a magneto-optical device using the same and a manufacturing method thereof, and more particularly to a terbium-containing paramagnetic garnet-type transparent ceramic suitable for constituting a magneto-optical device such as an optical isolator, a manufacturing method thereof, a raw material mixture therefor, and a magneto-optical device using the same and a manufacturing method thereof. [Background technology]

[0002] In recent years, as it has become possible to achieve higher output, the use of laser processing machines using fiber lasers has become increasingly widespread. However, when external light enters the laser light source built into the laser processing machine, the resonance state becomes unstable, causing the oscillation state to become disturbed. In particular, when the oscillated light is reflected by the optical system along the way and returns to the light source, the oscillation state is greatly disturbed. To prevent this, an optical isolator is usually installed in front of the light source.

[0003] An optical isolator consists of a Faraday rotator, a polarizer arranged on the light input side of the Faraday rotator, and an analyzer arranged on the light output side of the Faraday rotator. The Faraday rotator is used by applying a magnetic field parallel to the light's traveling direction. In this case, the polarization line of the light only rotates in a fixed direction whether it moves forward or backward through the Faraday rotator. Furthermore, the Faraday rotator is adjusted to a length that rotates the polarization line of the light exactly 45 degrees. Here, if the polarization planes of the polarizer and the analyzer are shifted 45 degrees in the direction of rotation of the forward light, the polarization of the forward light will be transmitted because it matches the polarizer position and the analyzer position. On the other hand, the polarization of the backward light will rotate 45 degrees in the opposite direction to the deviation angle of the polarization plane of the polarizer, which is shifted 45 degrees from the analyzer position. Then, the polarization plane of the return light at the polarizer position will be shifted 45 degrees - (-45 degrees) = 90 degrees from the polarization plane of the polarizer, and it cannot be transmitted through the polarizer. In this way, it functions as an optical isolator that transmits and emits forward-moving light and blocks backward-moving returning light.

[0004] As a material used as the Faraday rotator constituting the above optical isolator, conventionally, TGG crystal (Tb3Ga5O 12 ) and TSAG crystal ((Tb (3-x) Sc x )Sc2Al3O 12 ) have been known (Japanese Patent Application Laid-Open No. 2011-213552 (Patent Document 1), Japanese Patent Application Laid-Open No. 2002-293693 (Patent Document 2)). TGG crystal is currently widely installed for standard fiber laser devices. On the other hand, the Verdet constant of TSAG crystal is said to be about 1.3 times that of TGG crystal, and this is also a material that would not be strange to be installed in a fiber laser device. However, since Sc is an extremely expensive raw material, its adoption has not progressed from the perspective of manufacturing cost.

[0005] Other than the above, as a Faraday rotator having a larger Verdet constant than TSAG, TAG crystal (Tb3Al5O 12 ) has also been known for a long time. However, since TAG crystal is a decomposition-melting type crystal, there is a restriction that the perovskite phase is first generated at the solid-liquid interface and then the TAG phase is generated. That is, the garnet phase and the perovskite phase of TAG crystal can only be crystal-grown in a state where they are always mixed, and the growth of high-quality and large-sized TAG crystals has not been realized.

[0006] However, recently, International Publication No. 2018 / 193848 (Patent Document 3) discloses a sintered body of a complex oxide represented by the following formula, and a paramagnetic garnet-type transparent ceramic characterized in that the linear transmittance at a wavelength of 1064 nm with an optical path length of 15 mm is 83% or more, (Tb 1-x-y Sc x Ce y )3(Al 1-z Sc z )5O 12 (In the formula, 0 < x < 0.08, 0 ≤ y ≤ 0.01, 0.004 < z < 0.16.) has been disclosed.

[0007] Furthermore, the composition is (Tb x Y 1-x)3Al5O 12 A dense ceramic sintered body with (x = 0.5 to 1.0) has a higher extinction ratio compared to existing TGG crystals (the existing 35 dB is improved to 39.5 dB or more), and the insertion loss can also be reduced (the existing 0.05 dB is improved to 0.01 to 0.05 dB) as disclosed in Non-Patent Document 1.

[0008] Subsequently, Japanese Patent Application Laid-Open No. 2019-199386 (Patent Document 4) discloses a sintered body of a composite oxide represented by the following formula, containing more than 0% by mass and 0.1% by mass or less of SiO2 as a sintering aid, and having a linear transmittance of 83.5% or more at a wavelength of 1064 nm with an optical path length of 25 mm, (Tb 1-x-y Y x Sc y )3(Al 1-z Sc z )5O 12 (where 0.05 ≦ x < 0.45, 0 < y < 0.1, 0.5 < 1 - x - y < 0.95, 0.004 < z < 0.2) was disclosed.

Prior Art Documents

Patent Documents

[0009]

Patent Document 1

Patent Document 2

Patent Document 3

Patent Document 4

Non-Patent Documents

[0010]

Non-Patent Document 1

[0011] In Patent Document 3, the Verdet constant is comparable to that of TAG, and the linear transmittance is improved to be 83% or more even with an optical path length of 15 mm, so it can be said that it has almost reached a practical level. However, although it is not specified in Patent Document 3, when the inventors of the present application actually adjusted a laser beam with a wavelength of 1064 nm to a beam diameter of 1.6 mm and incident it with an incident power of 100 W on a sample that reproduced the working example of the patent document, it became clear that the maximum change in the incident laser beam diameter due to the occurrence of a thermal lens exceeded 15%.

[0012] Moreover, the material disclosed in Non-Patent Document 1 is capable of achieving even lower loss than the material in Patent Document 3 by substituting some of the Tb ions with Y ions, and is a material from which an extremely high quality garnet-type Faraday rotator can be obtained. Specifically, when a 1064 nm laser beam was adjusted to a beam diameter of 1.6 mm and incident power of 100 W was applied to a sample reproducing the material described in Non-Patent Document, it was found that the maximum change in the incident laser beam diameter due to the occurrence of thermal lensing was less than 10%.

[0013] However, the material described in Non-Patent Document 1 has very low manufacturing reproducibility, and when the inventors of the present application actually adjusted laser light with a wavelength of 1,064 nm to a beam diameter of 1.6 mm and applied it with an incident power of 100 W to a sample reproducing the example described in the document, it became clear that there was a very high probability that the maximum change in the incident laser beam diameter due to the occurrence of thermal lensing would exceed 15%.

[0014] The material disclosed in Patent Document 4 is a material that can obtain a high-quality garnet-type Faraday rotator equivalent to that of Non-Patent Document 1 by replacing a part of Tb ions with Y ions as in Non-Patent Document 1. In fact, when a 1064 nm laser beam was adjusted to a beam diameter of 1.6 mm and irradiated with an input power of 100 W on a sample that reproduced the material described in the patent document, the maximum change in the diameter of the incident laser beam due to the occurrence of thermal lenses was less than 10%, similar to Non-Patent Document 1. Furthermore, the manufacturing reproducibility of the material described in Patent Document 4 was also significantly improved.

[0015] Therefore, the incident power was further increased to 160 W output, and the light was irradiated onto samples reproducing the material described in Patent Document 4. In many cases, the maximum change in incident laser beam diameter due to thermal lens generation exceeded 15%. In other words, it can be said that the complex oxide sintered body material for an incident power of 100 W has reached a practical level, but the complex oxide sintered body material for an incident power of 160 W has not yet reached a practical level.

[0016] The present invention has been made in view of the above circumstances, and has an object to provide a terbium-containing paramagnetic garnet-type transparent ceramic which contains at least yttrium, terbium, and aluminum as main components, with the volume molar concentration of terbium being equal to or higher than that of yttrium, and which is capable of suppressing the maximum change in incident laser beam diameter to 10% or less even when the incident power of a laser beam having a wavelength of 1064 nm and a beam diameter of 1.6 mm is increased up to 160 W; a method for producing the same; and a raw material mixture therefor, as well as a magneto-optical device using the same and a method for producing the same. [Means for solving the problem]

[0017] In order to achieve the above object, the present invention provides, as a first aspect, a terbium-containing paramagnetic garnet-type transparent ceramic including a sintered body of a composite oxide containing terbium, yttrium, scandium, and aluminum and represented by the following formula (1): (T 1-x-y Y x Sc y )3(Al 1-z Sc z )5O 12 (1) (In the formula, 0.35≦x≦0.45, 0 <y<0.03、0.5<1-x-y<0.65、0.001<z<0.03、0<y+z<0.06である。) Its total light transmittance at a wavelength of 600 nm is 84.8% or more.

[0018] The terbium-containing paramagnetic garnet-type transparent ceramics of the present invention may further contain SiO2 as a sintering aid in an amount of more than 0 mass % and 0.1 mass % or less.

[0019] The terbium-containing paramagnetic garnet-type transparent ceramic of the present invention may have both optical end faces precision mirror-polished to a length of 14 mm or more, and the average roughness of each of the polished optical end faces is in the range of arithmetic mean height Sa≦0.70 nm or root mean square height Sq≦0.89 nm.

[0020] The total light transmittance of the paramagnetic garnet-type transparent ceramic of the present invention is preferably 84.6% or more at a wavelength of 540 nm and 85.25% or more at a wavelength of 1064 nm.

[0021] A second aspect of the present invention is a magneto-optical material that includes the above-mentioned terbium-containing paramagnetic garnet-type transparent ceramics.

[0022] A third aspect of the present invention is a magneto-optical device comprising the magneto-optical material described above.

[0023] The magneto-optical device of the present invention may be an optical isolator that has the above-mentioned terbium-containing paramagnetic garnet-type transparent ceramic as a Faraday rotator and has polarizing materials in front of and behind the optical axis of the Faraday rotator and can be used in the wavelength range of 0.9 μm or more and 1.1 μm or less.

[0024] In a fourth aspect, the present invention provides a method for producing a terbium-containing paramagnetic garnet-type transparent ceramic including a sintered body of a composite oxide containing terbium, yttrium, scandium, and aluminum and represented by the following formula (1), (T 1-x-y Y x Sc y )3(Al 1-z Sc z )5O 12 (1) (In the formula, 0.35≦x≦0.45, 0 <y<0.03、0.5<1-x-y<0.65、0.001<z<0.03、0<y+z<0.06である。) The present invention relates to a method for producing a sintered body having a relative sintering density of 93.8% or more, ... The method includes the steps of obtaining a sintered body within the following range, further densifying the sintered body by hot isostatic pressing (HIP) until the relative sintered density is 99.9% or more, subjecting the densified sintered body to a decolorizing annealing treatment at a temperature lower than the temperature in the HIP treatment to decolorize the brown color of the densified sintered body derived from the tetravalent terbium, additionally sintering the decolorized sintered body under reduced pressure at a temperature higher than both the sintering temperature and the temperature in the HIP treatment, and subjecting the additionally sintered sintered body to an oxidation annealing treatment at a temperature lower than the temperature in the HIP treatment in an oxygen atmosphere or in the air.

[0025] In the mixed raw material, the weight ratio of the residue that does not pass through a mesh having an opening of 20 μm to the total weight of the mixed raw material is preferably 0.5% or less.

[0026] In a fifth aspect, the present invention provides a mixed raw material for producing a terbium-containing paramagnetic garnet-type transparent ceramic, comprising a sintered body of a composite oxide containing terbium, yttrium, scandium, and aluminum and represented by the following formula (1): (T 1-x-y Y x Sc y )3(Al 1-z Sc z )5O 12 (1) (In the formula, 0.35≦x≦0.45, 0 <y<0.03、0.5<1-x-y<0.65、0.001<z<0.03、0<y+z<0.06である。) In the mixed raw material, the oxides of terbium, yttrium, scandium and aluminum are mixed in an uncompounded state, and the weight ratio of the residue that does not pass through a 20 μm mesh to the total weight of the mixed raw material is 0.5% or less.

[0027] A sixth aspect of the present invention is a method for producing a magneto-optical device, in which the magneto-optical device is formed using the paramagnetic garnet-type transparent ceramic obtained by the above-mentioned method for producing a paramagnetic garnet-type transparent ceramic. Effect of the Invention

[0028] According to the present invention, it is possible to provide a terbium-containing paramagnetic garnet-type transparent ceramic that is truly transparent and fully usable for high-power laser applications, capable of suppressing the maximum change in the diameter of the incident laser beam to 10% or less even when a high-power laser beam such as a laser beam having a wavelength of 1064 nm, a beam diameter of 1.6 mm, and an incident power of 160 W is incident, does not lose its shape of the incident beam, and is fully usable for high-power laser applications. Furthermore, by using the terbium-containing paramagnetic garnet-type transparent ceramic, it is possible to provide a magneto-optical material that can be applied to a high-power laser device, a magneto-optical device such as an optical isolator, and a method for manufacturing a magneto-optical device. [Brief description of the drawings]

[0029] [Figure 1] 1 is a schematic cross-sectional view showing an example of the configuration of an optical isolator using the magneto-optical material according to the present invention as a Faraday rotator. [Diagram 2] 1 is a photograph showing the amount of granules generated when a mixed raw material for the terbium-containing paramagnetic garnet-type transparent ceramic according to the present invention is subjected to a pre-sintering treatment at 900 to 1000° C.; [Diagram 3] Photographs showing the appearances of the sintered body after HIP treatment of Example 3 (a), the sintered body after color removal annealing treatment of Example 3 (b), and the sintered body after HIP treatment of Comparative Example 6 (c). [Figure 4] 1 is a graph showing the total light transmittance of the sintered bodies after oxidation annealing treatment in Example 3, Comparative Example 6, and Comparative Example 7. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0030] [1. Terbium-containing paramagnetic garnet-type transparent ceramics] First, an embodiment of the terbium-containing paramagnetic garnet-type transparent ceramic according to the present invention will be described. The terbium-containing paramagnetic garnet-type transparent ceramic according to the present embodiment includes a sintered body of a composite oxide containing terbium, yttrium, scandium, and aluminum, and represented by the following formula (1): (T 1-x-y Y x Sc y )3(Al 1-z Sc z )5O 12 (1) (In the formula, 0.35≦x≦0.45, 0 <y<0.03、0.5<1-x-y<0.65、0.001<z<0.03、0<y+z<0.06である。) The total light transmittance at a wavelength of 600 nm is 84.8% or more.

[0031] By having the composition of the complex oxide represented by the above formula (1), even when a laser beam having a wavelength of 1064 nm, a beam diameter of 1.6 mm, and an incident power of 160 W is incident, the beam does not collapse.

[0032] In the terbium-containing paramagnetic garnet-type transparent ceramics, it is preferable to further contain SiO2 as a sintering aid in an amount exceeding 0% by mass and not exceeding 0.1% by mass. When SiO2 is contained within this range, the transparency of the resulting paramagnetic garnet-type ceramic sintered body is improved to a level that can withstand practical use and is stable, which is preferable.

[0033] In this embodiment, it is essential that the main components of the 6-coordinate site and the 4-coordinate site in the garnet structure are aluminum (Al). If the main components of these sites can be composed of aluminum, the crystal binding property is improved, and as a result, the average value of dn / dt at 30 °C ± 10 °C at a wavelength of 1064 nm can be reduced. When the ratio of the 6-coordinate site and the 4-coordinate site occupied by this aluminum is 1 - z (0.001 < z < 0.03), the average value of dn / dt at 30 °C ± 10 °C at a wavelength of 1064 nm is 9.0×10 -6 K -1 Can be managed as follows.

[0034] In this embodiment, terbium (Tb) and yttrium (Y) are selected as the main components of the 8-coordinate site, and the concentration of terbium is in the range of 1 - x - y (0.5 < 1 - x - y < 0.65), and the concentration of yttrium is in the range of x (0.35 ≤ x ≤ 0.45). By setting the concentration of terbium within the above range, the Verdet constant at a wavelength of 1064 nm is ensured to be 30 rad / (T·m) or more. Furthermore, by setting the concentrations of terbium and yttrium within the above ranges, the beam does not collapse even when laser light with a wavelength of 1064 nm, a beam diameter of 1.6 mm, and an incident power of 160 W is incident. Note that when each of these two main components simultaneously satisfies the above range, the above two characteristics can be satisfied simultaneously.

[0035] In this embodiment, scandium (Sc) is added within the range of the above formula (1). In the above formula (1), the range of y is 0 < y < 0.03, preferably 0.001 < y < 0.008, and more preferably 0.002 < y < 0.004. When y is within this range, the perovskite-type heterogeneous phase can be reduced to a level where it cannot be detected by X-ray diffraction (XRD) analysis. Furthermore, an excessive decrease in the thermal conductivity due to the homogeneity of the sintered body and grain boundary scattering can be prevented. Also, in the above formula (1), the range of z is 0.001 < z < 0.03, and more preferably 0.002 < z < 0.004. When z is within this range, the perovskite-type heterogeneous phase can be reduced to a level where it cannot be detected by X-ray diffraction (XRD) analysis. Furthermore, an excessive decrease in the thermal conductivity due to the homogeneity of the sintered body and grain boundary scattering can be prevented. By adding scandium in the range where y exceeds 0 and is less than 0.03, and z exceeds 0.001 and is less than 0.03, it becomes possible to stably produce a highly transparent sintered body.

[0036] The terbium-containing paramagnetic garnet-type transparent ceramics of this embodiment contain, as a main component, the components of the composition represented by the above formula (1). Here, "containing as a main component" means containing 90 mass% or more of the complex oxide represented by the above formula (1). The content of the complex oxide represented by the above formula (1) is preferably 99 mass% or more, more preferably 99.9 mass% or more, still more preferably 99.99 mass% or more, and particularly preferably 99.999 mass% or more.

[0037] The terbium-containing paramagnetic garnet-type transparent ceramics of the present embodiment is composed of the above-mentioned main component and the sintering aid as a secondary component, but may further contain other elements. Examples of the other elements include rare earth elements such as lutetium (Lu) and cerium (Ce), and various impurities such as sodium (Na), calcium (Ca), magnesium (Mg), phosphorus (P), tungsten (W), and molybdenum (Mo). The content of the other elements is preferably 10 parts by mass or less, more preferably 0.1 parts by mass or less, and particularly preferably 0.001 parts by mass or less (substantially zero), when the total amount of Tb and Y is 100 parts by mass.

[0038] The terbium-containing paramagnetic garnet-type transparent ceramic of this embodiment has a total light transmittance of 84.8% or more at a wavelength of 600 nm, which indicates that the oxygen vacancies of the sintered body are extremely small. It has been confirmed that if oxygen vacancies exist in the sintered body, absorption due to oxygen vacancies occurs near a wavelength of 600 nm, causing the total light transmittance to fall below 84.8%. In other words, if the total light transmittance at a wavelength of 600 nm is 84.8% or more, this means that absorption due to oxygen vacancies is minimized, and further indicates that the sintered body is truly transparent and practical, in that the shape of the incident beam does not collapse even when a high-power laser beam with a wavelength of 1064 nm, a beam diameter of 1.6 mm, and an incident power of 160 W is incident thereon.

[0039] The terbium-containing paramagnetic garnet-type transparent ceramic of this embodiment preferably has a total light transmittance of 84.8% or more at a wavelength of 540 nm and 85.3% or more at a wavelength of 1064 nm. This indicates that the sintered body is truly transparent, without minute air bubbles of 1 μm or less that would slightly reduce the total light transmittance at a wavelength of 540 nm, and without various defects such as residual distortion that would reduce the total light transmittance at a wavelength of 1064 nm.

[0040] The terbium-containing paramagnetic garnet-type transparent ceramics of this embodiment is processed to have a length of 14 mm or more, and is used as the target magneto-optical material. By making the length 14 mm or more, it is possible to rotate incident light in the wavelength band of 0.9 μm to 1.1 μm by 45 degrees by using a correct magnetic circuit design, which is preferable, although it depends on the configuration and size of the external magnet.

[0041] The optical end faces of the terbium-containing paramagnetic garnet-type transparent ceramic of this embodiment are preferably optically polished so that their average roughness is within the range of arithmetic mean height Sa≦0.70 nm or root mean square height Sq≦0.89 nm. When the average roughness of both optical end faces is within the above range, the laser damage threshold is 10 J / cm even when a high-power laser is incident. 2 At the same time, it is also preferable since unintended scattering loss on the optical surface can be suppressed to an extremely small level.

[0042] [2. Manufacturing method of terbium-containing paramagnetic garnet-type transparent ceramics] Next, an embodiment of a method for producing a terbium-containing paramagnetic garnet-type transparent ceramic according to the present invention will be described. The method for producing the present embodiment includes the steps of mixing oxides of terbium, yttrium, aluminum, and scandium to prepare a mixed raw material, calcining or heating and drying the mixed raw material with a predetermined thermal history, and then molding the mixed raw material to obtain a molded body, degreasing the molded body to obtain a degreased body, and sintering the degreased body under reduced pressure by first maintaining the temperature at a predetermined level to degas the degreased body while maintaining the state in which the degreased body exhibits the brown color derived from the tetravalent terbium, and then raising the temperature to the sintering temperature to sinter the degreased body to obtain a sintered body having a predetermined relative sintered density, densifying the sintered body by hot isostatic pressing (HIP), subjecting the densified sintered body to decolorization annealing to decolorize the brown color derived from the tetravalent terbium, additionally sintering the decolorized sintered body, and subjecting the additionally sintered sintered body to oxidation annealing. Each step will be described below.

[0043] [2-1. Preparation process of mixed raw materials] As the raw materials used in the manufacturing method of this embodiment, for example, oxide powders of terbium, yttrium, scandium, and aluminum can be used. In this case, the purity of the raw materials is preferably 99.9 mass% or more, and particularly preferably 99.99 mass% or more. Co-precipitated oxides of terbium and yttrium can also be used. Then, a predetermined amount of each raw material is weighed and mixed so as to obtain a composite oxide composition represented by the above formula (1) to obtain a mixed raw material. In this specification, the "mixed raw material" refers to a mixture of terbium, yttrium, scandium, and aluminum oxides in an uncombined state.

[0044] Silicon oxide (SiO2) may be added as a sintering aid in an amount of more than 0 mass % and 0.1 mass % or less to this mixed raw material. The mixed raw material is mixed and processed by a wet ball mill, a bead mill, or a jet mill, as appropriate.

[0045] Among the above raw materials, terbium oxide and yttrium oxide, or the coprecipitated oxide of terbium and yttrium, are preferably pre-sintered at 1000° C. or higher. By pre-sintering at 1000° C. or higher in this manner, the BET value of each raw material is increased to 35m 2 / g or less, which is preferable because it prevents ultrafine powder from flying around during handling. In addition, it can also remove the moisture adsorbed in the raw material powder, so the accuracy of weighing the raw material after sintering is improved.

[0046] The mixed raw material (when the oxides of terbium and yttrium are previously calcined, the mixed raw material is mixed with aluminum oxide and scandium oxide) is preferably calcined or heated and dried. The thermal history of the mixed raw material that has been calcined or heated and dried is preferably kept at 950°C or less, more preferably at 920°C or less, and even more preferably at 900°C or less. When the thermal history of the mixed raw material is controlled within the above range, it is possible to reduce the possibility that the rare earth oxide component and the aluminum oxide react and combine to change into a monoclinic phase and / or a perovskite phase and / or a garnet phase, and it is also possible to prevent the highly active aluminum oxide fine powder from undergoing a necking reaction and agglomerating into agglomerates.

[0047] In fact, when the thermal history of the mixed raw material is controlled within the above range, it is possible to suppress the amount of residues that do not pass through a 20 μm mesh, among the gritty, clumps, aggregates, and coarse powders (hereinafter simply referred to as "gritty") derived from reaction compounds and necking aggregates, to 0.5% or less by weight relative to the total weight of the mixed raw material. The lower limit of the thermal history in the calcination treatment or heat drying treatment of the mixed raw material is not particularly limited, but may be, for example, 800° C. or higher.

[0048] In addition, when the mixed raw materials are used as described above, the amount of quasi-lump components that barely pass through a 20 μm mesh is small, and the entire mixed raw material can be maintained in a fine powder state. Therefore, the granules granulated by spray drying or the like have soft, easy-to-crush, smooth, and highly fluid properties, and as a result, the filling and crushing properties during the molding process can be maintained in good condition. If the filling and crushing properties during the molding process are good, unintended voids are unlikely to occur inside the molded body, and the overall molding density is also likely to be increased. Furthermore, when such a molded body is put into the sintering process, it is possible to obtain a highly transparent sintered body with very few remaining bubbles.

[0049] Furthermore, when the mixed raw materials are managed in the above-mentioned state, the reactivity of the mixed raw materials is maintained at a high level, which promotes densification during the sintering process and enables homogeneous sintering all the way to the inside of the sintered body. This makes it possible to obtain a high-quality hetero-phase-free sintered body that is highly transparent and has little compositional unevenness.

[0050] Various organic additives may be added to the mixed raw material for the purpose of improving the quality stability and yield in the subsequent processes. In the present embodiment, these are not particularly limited, and various dispersants, binders, lubricants, plasticizers, etc. can be suitably used. However, it is preferable to select high-purity types of these organic additives that do not contain unnecessary metal ions. In addition, the order of addition of each organic additive needs to be appropriately designed so as not to hinder the management of the properties (particle size distribution, etc.) of the mixed raw material to be produced.

[0051] [2-2. Molding process] In the manufacturing method of this embodiment, a normal press molding process can be suitably used. That is, a very common uniaxial pressing process in which the material is filled into a mold and pressed from a certain direction, or a cold isostatic pressing (CIP) process or a warm isostatic pressing (WIP) process in which the material is sealed and stored in a deformable waterproof container and pressed with hydrostatic pressure can be suitably used. The applied pressure can be appropriately adjusted while checking the relative density of the resulting molded body, and is not particularly limited. For example, the manufacturing cost can be reduced by controlling the pressure within a pressure range of about 300 MPa or less that can be handled by a commercially available CIP device or WIP device. Alternatively, a hot press process, a discharge plasma sintering process, a microwave heating process, etc., in which not only the molding process but also sintering is performed at once during molding, can be suitably used. Furthermore, it is possible to produce a molded body by a casting molding method instead of a press molding method. A molding method such as pressurized casting molding, centrifugal casting molding, and extrusion molding can also be adopted by optimizing the combination of the shape and size of the raw material oxide powder and various organic additives. In order to produce the high-quality terbium-containing paramagnetic garnet-type transparent ceramics of the present invention, it is preferable to make the pressure applied during uniaxial press molding as weak as possible without causing the molded body to collapse.

[0052] [2-3. Degreasing process] In the manufacturing method of this embodiment, a normal degreasing process can be suitably used. That is, it is possible to undergo a temperature-raising degreasing process using a heating furnace. In addition, the type of atmospheric gas at this time is not particularly limited, and air, oxygen, hydrogen, etc. can be suitably used. The degreasing temperature is preferably in a range that is equal to or higher than the temperature at which the organic components of the organic additives added can be sufficiently decomposed and removed, and is suppressed to 900°C or lower. If the temperature of the degreasing process is controlled within the above range, it is preferable because it can prevent unintended thermal shrinkage (a situation in which densification progresses while the adsorbed gas is taken in) in an atmosphere that is not a reduced pressure environment due to heating of the degreased body. It is more preferable to suppress the degreasing temperature to 800°C or lower. The lower limit of the degreasing temperature is not particularly limited, but may be, for example, 300°C or higher.

[0053] [2-4. Sintering process] In the manufacturing method of this embodiment, the sintering process is a process in which the degreased body obtained in the degreasing process is sintered under reduced pressure, and during the heating process, the temperature is temporarily held in a temperature range of 1000°C or less to degas the degreased body while retaining the brown color derived from the tetravalent terbium oxide, and then the temperature is raised to the sintering temperature to obtain a sintered body with a relative sintered density of 93.8% or more, and 97.2% or less.

[0054] The reason for temporarily holding the temperature below 1000°C is to thoroughly discharge adsorbed components such as water vapor and nitrogen from the system before full-scale densification begins, and although this holding (hereinafter also referred to as "holding") makes it possible to efficiently discharge from the system the oxygen gas component that is desorbed in large quantities when the terbium oxide component's Tb4 valence changes to trivalent when heated, it was found that at the same time, oxygen bound to the yttrium oxide is also desorbed, gradually causing oxygen deficiency. It was also found that if the Tb4 valence is completely changed to trivalent, the degree of oxygen deficiency in the yttrium oxide also becomes serious in conjunction with this, and the amount of oxygen deficiency in the entire sintered body becomes so large that the appearance becomes black after the HIP process in the subsequent process.

[0055] Therefore, if the hold temperature for changing Tb4 to Tb3 is controlled to 1000°C or less while desorbing the adsorbed components, a small amount of Tb4 will remain and the sintered body will have a light brown color, but the amount of oxygen vacancies in the yttrium oxide can be suppressed to an extremely low level. As a result, the appearance of the sintered body after the HIP process in the subsequent process can be finished as a light brown (close to orange) sintered body with no blackish tinge, i.e., with very little oxygen vacancy.

[0056] On the other hand, if the hold temperature is set to a temperature exceeding 1000°C, the light brown color will completely disappear, but instead a large amount of oxygen deficiency will occur, so that the appearance of the sintered body after the HIP treatment in the subsequent process will be black. The lower limit of the hold temperature is not particularly limited as long as it is a temperature that can change Tb4 to Tb3, but for example, 850°C or higher is preferable, and 900°C or higher is more preferable. Note that, as for the hold time during which the degassing is performed by holding the degassing temperature at 1000°C or lower, several hours is sufficient, but it is preferable to set it to 8 hours or more in order to sufficiently degas the inside of the degreased body. The upper limit of the hold time is not particularly limited, but it may be, for example, 30 hours or less.

[0057] In the sintering process, the material is once held at the hold temperature to degas it, and then heated to a predetermined sintering temperature. It is essential that the predetermined sintering temperature is set within a temperature range in which the oxides of terbium, yttrium, and scandium combine with aluminum oxide to stably obtain only the garnet phase. It is preferable to heat the transparent ceramic sintered body to a temperature range in which only the garnet phase is produced as quickly as possible after the degassing process is fully completed, since this can minimize the production rate of unintended heterogeneous phases such as monoclinic phases and perovskite phases.

[0058] For example, the predetermined sintering temperature is preferably 1400 to 1780°C, and particularly preferably 1450 to 1700°C. If the sintering temperature is within this range, as described above, it is preferable because densification is promoted while suppressing heterogeneous phase precipitation. In addition, the temperature rise rate from the hold temperature to the sintering temperature is preferably 100°C / hr or more, more preferably 200°C / hr or more, and even more preferably a high-speed temperature rise of 250°C / hr or more. The upper limit of the temperature rise rate is not particularly limited, but may be, for example, 300°C / hr or less.

[0059] In the sintering process, the relative sintered density of the obtained sintered body is controlled to be in the range of 93.8% or more and 97.2% or less. The control of the relative sintered density can be performed by repeating several preliminary experiments. It is more preferable to sinter while controlling the relative sintered density to be in the range of 93.8% or more and 96.5% or less, and it is even more preferable to sinter while controlling the relative sintered density to be in the range of 93.8% or more and 96.0% or less. If the obtained sintered body is controlled within this density range, the residual bubbles inside the sintered body can be made into closed pores, while the sintered grain size can be controlled without being excessively large, so that the closed pores can be firmly crushed in the HIP treatment in the subsequent process, which is preferable.

[0060] The sintering process can be suitably carried out by general heating and sintering methods such as resistance heating and induction heating. The atmosphere during this process is a reduced pressure environment (vacuum). By carrying out the sintering process in a reduced pressure atmosphere, the components such as water vapor and nitrogen adsorbed inside the degreased body can be efficiently volatilized and discharged, and the oxygen gas that is desorbed in large quantities when Tb4 is converted to Tb3 by heating can also be efficiently discharged and volatilized outside the sintered body. The vacuum level is 1×10 -3 If the degree of vacuum is controlled within this range, it is preferable because the sintered body can be uniformly and sufficiently exhausted to the center thereof and the gas desorbed from the degreased body can be sufficiently discharged to the outside of the system.

[0061] [2-5. Hot isostatic pressing (HIP) processing process] In the manufacturing method of this embodiment, after the sintering process, a hot isostatic pressing (HIP) process is performed to densify the sintered body until the relative sintered density is 99.9% or more. If the relative sintered density in the sintering process is properly managed, that is, if the HIP process can be performed in a state where the sintered grain size is not excessively large, the HIP stress is transmitted widely and uniformly from the outer periphery to the center of the sintered body, the closed pores are crushed, and the sintered body is firmly densified. In other words, a substantially ideal sintered body is obtained that has no stress unevenness, no unintended void unevenness, and few remaining small bubbles.

[0062] In the manufacturing method of this embodiment, the conditions are controlled so that the sintered body intentionally has a light brown appearance due to Tb4 residual after HIP treatment. This makes it possible to suppress the occurrence of oxygen deficiency in yttrium oxide, which is easily reduced, and it becomes possible to finish a terbium-containing paramagnetic garnet-type transparent ceramic sintered body with a total light transmittance of 84.8% or more at a wavelength of 600 nm. It has been confirmed that when oxygen deficiency is present in yttrium oxide, absorption due to oxygen deficiency occurs near the wavelength of 600 nm, causing the total light transmittance to fall below 84.8%. In other words, when the total light transmittance at a wavelength of 600 nm is 84.8% or more, it means that absorption due to oxygen deficiency is minimized, and thus it is possible to provide a truly transparent and practical sintered body in which the shape of the incident beam does not collapse even when a high-power laser beam with a wavelength of 1064 nm, a beam diameter of 1.6 mm, and an incident power of 160 W is incident.

[0063] The type of pressurized gas medium used in the HIP treatment can be an inert gas such as argon or nitrogen, or Ar-O2. The pressure applied by the pressurized gas medium is preferably 50 to 300 MPa, more preferably 100 to 300 MPa. If the pressure is less than 50 MPa, the transparency improvement effect may not be obtained, and if the pressure exceeds 300 MPa, even if the pressure is increased, no further improvement in transparency can be obtained, and the load on the device may be excessive, which may damage the device. It is convenient and preferable that the applied pressure is 196 MPa or less, which can be processed by a commercially available HIP device.

[0064] The treatment temperature of the HIP treatment is preferably 1100 to 1780°C, more preferably 1200 to 1730°C. If the treatment temperature exceeds 1780°C, the risk of oxygen vacancies increases, which is not preferable. If the treatment temperature is less than 1100°C, the effect of improving the transparency of the sintered body is hardly obtained. The holding time of the treatment temperature is not particularly limited, but if it is held for too long, the risk of oxygen vacancies increases, which is not preferable. Typically, it is preferably set in the range of 1 to 3 hours.

[0065] The heater material, heat insulating material, and processing vessel for HIP processing are not particularly limited, but graphite, molybdenum (Mo), tungsten (W), and platinum (Pt) can be preferably used, and yttrium oxide and gadolinium oxide can also be preferably used as the processing vessel. In particular, when the processing temperature is 1500°C or lower, platinum can be used as the heater material, heat insulating material, and processing vessel, and the pressurized gas medium can be Ar-O2, which is preferable because it can prevent the occurrence of oxygen deficiency during HIP processing. When the processing temperature exceeds 1500°C, graphite is preferable as the heater material and heat insulating material, but in this case, it is preferable to select graphite, molybdenum, or tungsten as the processing vessel, and further select yttrium oxide or gadolinium oxide as a double vessel inside it, and fill the vessel with an oxygen release material, since this can minimize the amount of oxygen deficiency during HIP processing.

[0066] [2-6. Color removal annealing process] In the manufacturing method of this embodiment, the sintered body after the HIP treatment has a light brown appearance, so in order to bleach it and turn it into a nearly white color, a decolorization annealing process is performed in an oxygen atmosphere or in the air at a temperature equal to or lower than the treatment temperature of the HIP treatment, typically 1200 to 1400°C. If the additional sintering process described below is performed without this process, a large amount of bubbles will remain in the sintered body. The sintered body that has been subjected to the decolorization annealing process can discharge excess oxygen derived from terbium tetravalent to the outside of the system while minimizing oxygen deficiency derived from yttrium oxide, making it possible to obtain a garnet-type oxide sintered body with extremely small defect absorption.

[0067] The time for which the above-mentioned temperature is maintained during the decolorizing annealing treatment does not need to be very long, and typically, a period of 2 hours is sufficient.

[0068] [2-7. Additional sintering process] In the manufacturing method of this embodiment, after the decolorization annealing process, additional sintering is performed under reduced pressure at a temperature that exceeds the sintering temperature and also exceeds the HIP processing temperature. However, if the additional sintering temperature exceeds 1780°C, the risk of oxygen vacancies increases, which is not preferable. This makes it possible to more thoroughly eliminate residual internal distortions and bubbles. The degree of vacuum in the additional sintering process may be the same as that in the sintering process.

[0069] It is preferable to secure a processing time of 8 hours or more for the additional sintering, since it is possible to recover even the residual distortion and residual defects inside the sintered body. Processing time of 10 hours or more is even more preferable. It is preferable to secure a processing time of the additional sintering that is long enough, since it is possible to eliminate the residual distortion and residual bubbles sufficiently and uniformly from the outer periphery to the center of the sintered body. The additional sintering process is an essential process, especially when using garnet-type transparent oxide ceramic materials in an environment where a high-power laser of 160 W or more is incident.

[0070] [2-8. Oxidation annealing process] In the manufacturing method of this embodiment, after the additional sintering process is completed, it is preferable to perform an oxidation annealing process (oxygen deficiency recovery process) in an oxygen atmosphere or in the air at a temperature equal to or lower than the HIP process temperature, typically 1000 to 1500°C, in order to recover oxygen deficiencies in the obtained transparent ceramic sintered body. The oxidation annealing process temperature is more preferably 1300°C or higher and 1450°C or lower. This makes it possible to recover oxygen deficiencies even in a sintered body in which oxygen deficiencies have accumulated due to sintering, HIP process, additional sintering, etc., and to finish the terbium-containing paramagnetic garnet-type transparent ceramics that are colorless, transparent, and free of defect absorption.

[0071] The treatment time of the oxidation annealing treatment is preferably 8 hours or more, more preferably 20 hours or more, and even more preferably 30 hours or more. If the treatment time of the oxidation annealing treatment is sufficiently long, it becomes possible to sufficiently recover even the oxygen vacancies remaining in the center part of the sintered body.

[0072] [2-9. Optical polishing process] In the manufacturing method of this embodiment, it is preferable to optically polish both end faces on the optically utilized axis of the terbium-containing paramagnetic garnet-type transparent ceramics that has undergone the above-mentioned series of steps. In this case, the optical surface precision is preferably λ / 2 or less, and more preferably λ / 8 or less, when the measurement wavelength λ=633 nm. Furthermore, the average roughness of both optical end faces is preferably arithmetic mean height Sa of 0.70 nm or less, and root mean square height Sq of 0.89 nm or less, and more preferably Sa≦0.55 nm and Sq≦0.70 nm, respectively. It is also possible to further reduce optical loss by appropriately forming an anti-reflection film (AR coating film) on the surface that has been optically polished as described above.

[0073] In this manner, a terbium-containing paramagnetic garnet-type transparent ceramic containing a sintered body of a composite oxide containing terbium, yttrium, scandium, and aluminum represented by the above formula (1) and having a total light transmittance of 84.8% or more at a wavelength of 600 nm can be manufactured. In addition, by manufacturing under the above-mentioned manufacturing conditions, it is possible to finish the total light transmittance to a high value of 84.8% or more at a wavelength of 540 nm and 85.3% or more at a wavelength of 1064 nm. This suggests that a truly transparent sintered body is finished without minute bubbles of 1 μm or less that slightly reduce the total light transmittance at a wavelength of 540 nm, and without various defects such as residual distortion that reduce the total light transmittance at a wavelength of 1064 nm. If the total light transmittance can be controlled within the above range, a truly transparent sintered body can be provided in which the shape of the incident beam does not collapse even when a high-power laser beam with a wavelength of 1064 nm, a beam diameter of 1.6 mm, and an incident power of 160 W is incident.

[0074] [3. Magneto-optical material, magneto-optical device, and manufacturing method thereof] Further, an embodiment of the magneto-optical material, the magneto-optical device, and the manufacturing method thereof according to the present invention will be described. The magneto-optical material of this embodiment includes the above-mentioned terbium-containing paramagnetic garnet-type transparent ceramic. The magneto-optical device of this embodiment is constructed using the above-mentioned terbium-containing paramagnetic garnet-type transparent ceramic. Specifically, it is preferable to apply a magnetic field parallel to the optical axis of the above-mentioned terbium-containing paramagnetic garnet-type transparent ceramic, and then set a polarizer and an analyzer so that their optical axes are shifted by 45 degrees from each other to construct and use the magneto-optical device. In particular, the above-mentioned terbium-containing paramagnetic garnet-type transparent ceramic is suitably used as a magneto-optical device, particularly as a Faraday rotator of an optical isolator with a wavelength of 0.9 to 1.1 μm.

[0075] FIG. 1 is a cross-sectional view showing an example of an optical isolator, which is a magneto-optical device including a Faraday rotator made of the paramagnetic garnet-type transparent ceramics according to the present embodiment as an optical element. As shown in FIG. 1, the optical isolator 100 includes a Faraday rotator 110 made of the above-mentioned paramagnetic garnet-type transparent ceramics, a polarizer 120 made of a polarizing material, and an analyzer 130 inside the housing 150. These are arranged in the order of the polarizer 120, the Faraday rotator 110, and the analyzer 130 along the optical axis 112 of the Faraday rotator. The polarized light vibration plane of the polarizer 120 and the polarized light vibration plane of the analyzer 130 are arranged so that the relative angle is 45°. In addition, the optical isolator 100 includes a magnet 140 for applying a magnetic field to the Faraday rotator 110 on at least one of the side surfaces of the Faraday rotator 110 inside the housing 150.

[0076] Such an optical isolator 100 can be suitably used in an industrial fiber laser device (not shown). The optical isolator can prevent the reflected light of the laser light emitted from the laser light source from returning to the light source, causing the oscillation to become unstable. EXAMPLES

[0077] EXAMPLES The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited to these examples.

[0078] [Examples 1 to 2, Comparative Examples 1 to 8] We obtained terbium oxide powder, yttrium oxide powder, and scandium oxide powder manufactured by Shin-Etsu Chemical Co., Ltd., and aluminum oxide powder manufactured by Taimei Chemical Co., Ltd. In addition, we obtained liquid tetraethyl orthosilicate (TEOS) manufactured by Kishida Chemical Co., Ltd. The purity of the powder raw materials was 99.95% by mass or more, and the purity of the liquid raw materials was 99.999% by mass or more.

[0079] Using the above raw materials, the mixing ratio was adjusted to prepare two types of composite oxide raw materials with the final compositions shown in Table 1. The mixing ratio was adjusted by weighing and mixing each oxide powder so that the mole numbers of terbium, yttrium, aluminum, and scandium were the molar ratios of each composition in Table 1. Next, TEOS was weighed and added to each raw material in an amount equivalent to SiO2 in the mass % shown in Table 1.

[0080] [Table 1]

[0081] Then, each composition was dispersed and mixed in ethanol using an alumina ball mill, taking care to prevent each composition from being mixed with the others. The processing time was 15 hours.

[0082] The mixed raw materials were then dried by spray drying, and each mixed raw material was calcined at different calcination temperatures as shown in Table 2, and again, each sample was dispersed and mixed in ethanol using an alumina ball mill, taking care to prevent each sample from being mixed with the others. The processing time was 20 hours. At this time, each raw material slurry after 20 hours of mixing was filtered through a mesh with 20 μm openings, and the weight of the residue (grid) remaining on the mesh was measured and recorded as a percentage of the total weight of the mixed raw materials. These results are summarized in Table 2.

[0083] [Table 2]

[0084] Figure 2 shows a photograph of the amount of junk remaining after Samples 1, 2, and 3 were calcined, mixed and ground in ethanol for 20 hours, and then passed through a mesh with 20 μm openings.

[0085] As shown in Figure 2(c), when the mixed raw material is calcined at 1000°C, a large amount of coarse gravel that cannot pass through a 20μm mesh is generated, and there is also a large amount of coarse powder that can barely pass through a 20μm mesh. As a result, the raw material has a large size unevenness, is very hard, and is extremely difficult to handle. Naturally, even after granulation, the mixed raw material has a worsening hardness unevenness of the granules and a large unevenness in crushability. In addition, if a compact is made using such heterogeneous raw material, it is impossible to prevent uneven stress transmission inside the compact and the occurrence of unintended coarse voids. And when such a heterogeneous compact is sintered, uneven stress, uneven final composition due to voids, and local internal defects will inevitably remain inside the sintered body. On the other hand, when the mixed raw materials were calcined at 950°C, the amount of jellies was significantly reduced, as shown in Figure 2(b), and when the mixed raw materials were calcined at 900°C, almost no jellies were detected, as shown in Figure 2(a).

[0086] Then, the six samples (oxide raw materials) obtained were subjected to uniaxial press molding and CIP molding to obtain nine CIP compacts for each sample. All the obtained compacts were degreased in a muffle furnace at 800°C for three hours to obtain degreased compacts.

[0087] Next, among the above samples, the degreased green bodies of Samples 1, 2, 4, and 5 were divided into three groups of three each. Six of the green bodies of Samples 1 to 6 were processed at a hold temperature of 1000°C for 12 hours during the vacuum sintering process, and three were processed at 1080°C for 12 hours. Furthermore, the six green bodies processed at 1000°C for 12 hours were vacuum sintered at different sintering temperatures as shown in Table 3, so that the density after sintering was adjusted to be different. For Samples 3 and 6, the hold temperature during the temperature rise was fixed at 1000°C for 12 hours, and the sintering was performed at a sintering temperature where the relative sintered density was in the range of 93.8% to 97.2%.

[0088] [Table 3]

[0089] The obtained sintered bodies were placed in a HIP furnace made of a carbon heater and HIP-treated in Ar at 200 MPa, 1600°C, and 3 hours. The relative density of each of the obtained sintered bodies was 99.9% or more. In terms of appearance, the one held at 1000°C was light brown (coloring due to Tb4), while the one held at 1080°C was completely black (massive oxygen vacancy absorption).

[0090] Therefore, the samples of Examples 1 to 4 and Comparative Examples 2, 4, 5, 7, 9, and 10, which had a light brown appearance, were all subjected to a decolorization annealing treatment in an atmospheric heating furnace at 1300° C. for 2 hours to remove the color. The obtained annealed products were all transparent or semi-transparent, that is, decolorized.

[0091] Fig. 3(a) is a photograph showing the appearance of the sintered body after HIP treatment in Example 3, which was light brown in color. Fig. 3(b) is a photograph showing the appearance of the sintered body after further decolorizing annealing treatment at 1300°C for 2 hours in Example 3, which was transparent. On the other hand, Fig. 3(c) is a photograph showing the appearance of the sintered body of Comparative Example 6, which was held at a hold temperature of 1080°C for 12 hours, heated to the sintering temperature, sintered, and then HIP-treated, which was black in color.

[0092] After that, all samples, including the HIP-treated sintered bodies that had turned black, were subjected to additional sintering in a vacuum sintering furnace at a sintering temperature of 1720°C for 15 hours in an attempt to eliminate residual bubbles throughout the entire area, including the center of the sintered body.

[0093] Next, each of the obtained sintered bodies was subjected to oxidation annealing treatment at 1400°C for 40 hours in an atmospheric heating furnace while controlling each lot (Example number, Comparative example number) to sufficiently recover distortion and oxygen deficiency. In this way, a total of 14 types of sintered body sets were prepared, including both Examples and Comparative examples, with a minimum of three sets for each, and a maximum of nine sets for each.

[0094] Subsequently, all of the obtained sintered samples were cut to a length of 20 mm and precision polished. It was confirmed that both optical end faces of all the sintered samples had an optical surface precision of λ / 8 or more (when the measurement wavelength λ=633 nm) and average roughness of arithmetic mean height Sa of 0.70 nm or less and root mean square height Sq of 0.89 nm or less.

[0095] For each of the sintered body samples obtained as described above, the total light transmittance and the forward scattering rate were measured as follows.

[0096] (Method of measuring total light transmittance and forward scattering) The total light transmittance and forward scattering were measured with reference to JIS K7105 (ISO 13468-2:1999) and JIS K7136 (ISO 14782:1999). Measurements were performed at wavelengths of 540 nm, 600 nm, 760 nm, 930 nm, and 1064 nm using a spectrophotometer V-670 manufactured by JASCO Corporation.

[0097] First, to measure the total light transmittance, the spectrophotometer V-670 is irradiated with light dispersed by a spectroscope without a workpiece (sample) set on it, the light is received by an integrating sphere set on the device beforehand, and the collected light is received by a detector. The obtained illuminance is I0, and then the workpiece is set on the device, and this time the dispersed light is incident on the workpiece, and the transmitted light is again collected by an integrating sphere and received by a detector. The obtained illuminance is I, and is calculated using the following formula. Total light transmittance (% / 25mm)=I / I0×100

[0098] Next, to measure forward scattering, the same measurement system is used except that the reflector on the back of the integrating sphere is removed from the state where the workpiece is set. The dispersed light is again incident on the workpiece, and the transmitted light is again collected by the integrating sphere and received by the detector. The obtained illuminance represents the scattered components other than the linear transmitted component, and is called I S was calculated using the following formula: Generally, however, forward scattering is almost flat in the visible range and has no wavelength dependency, so the value at a wavelength of 1064 nm was recorded as the representative value. Forward scattering rate (% / 25mm)=I S / I0×100

[0099] In addition, in order to consider the effects of reproducibility and variation, three or nine samples were measured for each condition, and the average values ​​were calculated to determine the total light transmittance and forward scattering values ​​of each sample. In addition, a beam diameter of 2 mmφ was used regardless of the diameter of the sintered body, and the incident position was adjusted to be approximately the center of the optically effective surface. The above results are summarized in Table 4, and the total light transmittance at wavelengths of 540 nm, 600 nm, 760 nm, 930 nm, and 1064 nm and the forward scattering rate at a wavelength of 1064 nm are shown. In addition, a graph of the total light transmittance of Example 3, Comparative Example 6, and Comparative Example 7 is shown in Figure 4.

[0100] [Table 4]

[0101] From the results in Table 4, it was confirmed that the samples in the groups in which the calcination temperature of the starting mixed raw materials was controlled to 950°C or less when producing the complex oxide sintered body of the present invention, that is, the groups in which the uncompounded raw material ratio was less than half, and further the hold temperature during the heating process was set to 1000°C, and the samples were sintered so that the relative sintered density was less than 98.9%, preferably 97.2% or less, and then subjected to HIP treatment, that is, the samples in Examples 1 to 4, all had a total light transmittance of 84.8% or more at a wavelength of 600 nm, a total light transmittance of 84.6% or more at a wavelength of 540 nm, and a total light transmittance of 85.25% or more at a wavelength of 1064 nm, and were finished into truly transparent terbium-containing paramagnetic garnet-type transparent ceramics with no noticeable absorption in a wide wavelength band.

[0102] On the other hand, in the case of the samples in the group in which the calcination temperature of the mixed raw material was 1000°C (Comparative Examples 5 and 10), the total light transmittance at a wavelength of 600 nm did not reach 84.8%, the total light transmittance at a wavelength of 540 nm did not reach 84.6%, and the total light transmittance at a wavelength of 1064 nm did not reach 85.25%.

[0103] In addition, in the groups in which the calcination temperature of the mixed raw materials was controlled below 950°C, but the hold temperature during the sintering process was set to 1080°C (Comparative Examples 1, 3, 6, and 8), and in which the relative sintered density exceeded 97.2% (Comparative Examples 2, 4, 7, and 9), the total light transmittance at a wavelength of 600 nm did not reach 84.8%, the total light transmittance at a wavelength of 540 nm did not reach 84.6%, and the total light transmittance at a wavelength of 1064 nm did not reach 85.25%.

[0104] Finally, for samples with forward scattering of 0.5% or more (Comparative Examples 2, 4, 5, 7, 9, and 10), the evaluation of high power resistance was abandoned because the scattered light would scatter in all directions when a high-power laser beam with an incident power of 160 W was applied, making the evaluation dangerous. For the other eight groups of Examples 1 to 4 and Comparative Examples 1, 3, 6, and 8, the rate of change in beam diameter was evaluated when a high-power laser beam with an incident power of 160 W was applied after coating both optical end faces with an anti-reflection film for a wavelength of 1064 nm. The evaluation results are shown in Table 5.

[0105] (Beam diameter change rate evaluation) The beam diameter change rate was measured using a collimated CW laser beam made by IPG Co., Ltd. with a wavelength of 1070 nm, an output power of 160 W, and a diameter of 1.6 mm, using a ModeMaster PCM made by Coherent. 2 The beam diameter at the reference plane (full bezel) of the profiler was measured using a beam propagation analyzer. However, since the output power after passing through the sample was very high, the intensity of the laser light was first attenuated to 1 / 1000 or less by a beam separator before being introduced into the beam profiler. The distance between the reference plane (full bezel) of the beam profiler and the sample holder was 1.9 m, and the distance between the reference plane and the collimator was 2.1 m. First, the beam diameter of the original beam was measured, and the value at this time was taken as r0. Next, each of the above samples with a length of 20 mm was placed in the optical path, and the beam diameter of each transmitted light was measured and taken as r. The beam diameter change rate in this invention was calculated as |(1-r / r0)|×100, and 10% or less was evaluated as pass, and more than 10% was evaluated as fail. The evaluation results are shown in Table 5.

[0106] [Table 5]

[0107] From the results in Table 5, in the groups of Examples in which the total light transmittance at a wavelength of 600 nm was 84.8% or more, the total light transmittance at a wavelength of 540 nm was 84.6% or more, and the total light transmittance at a wavelength of 1064 nm was 85.25% or more, the beam diameter change rate when a high-power laser beam with an incident power of 160 W was incident was 10% or less in all cases. On the other hand, in the groups of Comparative Examples 1, 3, 6, and 8 in which the total light transmittance values ​​did not reach these values, the beam diameter change rate when a high-power laser beam with an incident power of 160 W was incident was more than 10%, which deteriorated.

[0108] Although the present invention has been described above using the above-mentioned embodiment, the present invention is not limited to this embodiment, and can be modified within the scope of what a person skilled in the art can imagine, such as other embodiments, additions, modifications, deletions, etc., and any aspect is within the scope of the present invention as long as it achieves the effects of the present invention. [Explanation of symbols]

[0109] 100 Optical isolator 110 Faraday Rotator 120 Polarizer 130 Analyzer 140 Magnet 150 Case

Claims

1. A terbium-containing paramagnetic garnet-type transparent ceramic comprising a sintered body of a composite oxide containing terbium, yttrium, scandium and aluminum and represented by the following formula (1): (Tb 1-x-y Y x S.C. y ) 3 (Al 1-z S.C. z ) 5 O 12 (1) (In the formula, 0.35≦x≦0.45, 0<y<0.03, 0.5<1−x−y<0.65, 0.001<z<0.03, and 0<y+z<0.06.) Terbium-containing paramagnetic garnet-type transparent ceramics having a total light transmittance of 84.8% or more at a wavelength of 600 nm.

2. SiO as a sintering aid 2 2. The terbium-containing paramagnetic garnet-type transparent ceramic according to claim 1, further comprising:

3. 3. The terbium-containing paramagnetic garnet-type transparent ceramic according to claim 1 or 2, wherein both optical end faces are precisely mirror-polished so that the length of the terbium-containing paramagnetic garnet-type transparent ceramic is 14 mm or more, and the average roughness of each of the polished optical end faces is in the range of arithmetic mean height Sa≦0.70 nm or root mean square height Sq≦0.89 nm.

4. 3. The terbium-containing paramagnetic garnet-type transparent ceramic according to claim 1, wherein the paramagnetic garnet-type transparent ceramic has a total light transmittance of 84.6% or more at a wavelength of 540 nm and 85.25% or more at a wavelength of 1064 nm.

5. A magneto-optical material comprising the terbium-containing paramagnetic garnet-type transparent ceramic according to claim 1 or 2.

6. A magneto-optical device comprising the magneto-optical material according to claim 5 .

7. 7. The magneto-optical device according to claim 6, which is an optical isolator having the terbium-containing paramagnetic garnet-type transparent ceramic as a Faraday rotator and having polarizing materials in front of and behind the optical axis of the Faraday rotator and usable in the wavelength range of 0.9 μm to 1.1 μm.

8. A method for producing a terbium-containing paramagnetic garnet-type transparent ceramic including a sintered body of a composite oxide containing terbium, yttrium, scandium, and aluminum and represented by the following formula (1), comprising the steps of: (Tb 1-x-y Y x S.C. y ) 3 (Al 1-z S.C. z ) 5 O 12 (1) (In the formula, 0.35≦x≦0.45, 0<y<0.03, 0.5<1−x−y<0.65, 0.001<z<0.03, and 0<y+z<0.06.) A step of preparing a mixed raw material by mixing terbium oxide and yttrium oxide or a coprecipitated oxide of terbium and yttrium, aluminum oxide, and scandium oxide; A step of calcining or heating and drying the mixed raw material at a thermal history of 950° C. or less and then molding the same to obtain a molded body; A step of degreasing the molded body to obtain a degreased body; a step of sintering the degreased body under reduced pressure, firstly maintaining a hold temperature of 1000° C. or less to degas the degreased body while maintaining a state in which the degreased body exhibits a brown color derived from the tetravalent terbium, and then raising the temperature to a sintering temperature to sinter the degreased body, thereby obtaining a sintered body having a relative sintered density in the range of 93.8% or more and 97.2% or less; a step of further densifying the sintered body by hot isostatic pressing (HIP) until the relative sintered density is 99.9% or more; a step of subjecting the densified sintered body to a decolorization annealing treatment at a temperature lower than the temperature of the HIP treatment, thereby decolorizing the brown color of the densified sintered body due to the tetravalent terbium; additionally sintering the decolorized sintered body under reduced pressure at a temperature higher than both the sintering temperature and the temperature in the HIP treatment; subjecting the additionally sintered sintered body to an oxidation annealing treatment in an oxygen atmosphere or in the air at a temperature lower than that in the HIP treatment; A method for producing a terbium-containing paramagnetic garnet-type transparent ceramic comprising the steps of:

9. 9. The method for producing terbium-containing paramagnetic garnet-type transparent ceramics according to claim 8, wherein the weight ratio of the residue which does not pass through a mesh having an opening of 20 μm to the total weight of the mixed raw material is 0.5% or less.

10. A mixed raw material for producing a terbium-containing paramagnetic garnet-type transparent ceramic, comprising a sintered body of a composite oxide containing terbium, yttrium, scandium, and aluminum and represented by the following formula (1): (Tb 1-x-y Y x S.C. y ) 3 (Al 1-z S.C. z ) 5 O 12 (1) (In the formula, 0.35≦x≦0.45, 0<y<0.03, 0.5<1−x−y<0.65, 0.001<z<0.03, and 0<y+z<0.06.) The mixed raw material is a mixture of oxides of terbium, yttrium, scandium, and aluminum in an uncompounded state, The mixed raw material is a mixed raw material in which the weight ratio of the residue that does not pass through a mesh with 20 μm openings to the total weight of the mixed raw material is 0.5% or less.

11. A method for producing a magneto-optical device, comprising the steps of: forming a magneto-optical device using the paramagnetic garnet-type transparent ceramic obtained by the method for producing a paramagnetic garnet-type transparent ceramic according to claim 8 or 9;

Citation Information

Patent Citations

  • Method for manufacturing transparent ceramics for faraday rotator

    JP2019207340A

  • Garnet-type single crystal, optical isolator, and optical processor

    WO2011132668A1

  • Paramagnetic garnet-based transparent ceramic and method for producing same

    WO2022054515A1

  • Paramagnetic garnet-type transparent ceramic, magneto-optical device, and production method for paramagnetic garnet-type transparent ceramic

    WO2022054596A1

  • Terbium-aluminum-garnet single crystal and method of manufacturing for the same

    JP2002293693A

Cited By

  • Terbium-containing ferromagnetic garnet-type transparent ceramic and magneto-optical device using the same

    JP2025078370A

  • Terbium-containing paramagnetic garnet transparent ceramic and magneto-optic device using same

    WO2025100250A1