Catalyst for use in ammonia decomposition or synthesis reaction
A catalyst using nickel, iron, or cobalt supported on a titanium-barium-zirconium composite oxide addresses the high cost and supply issues of noble metals and rare earth elements, achieving high catalytic activity in ammonia reactions.
Patent Information
- Application Number
- JP2023081637
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-17
- Publication Date
- 2024-11-28
AI Technical Summary
Existing ammonia decomposition and synthesis catalysts rely on expensive noble metals or rare earth elements, which are costly and have uneven supply, and non-noble metal alternatives lack sufficient catalytic activity.
A catalyst structure where nickel, iron, or cobalt is supported on a composite oxide containing titanium, barium, and zirconium, specifically BaTi x Zr 1-x O 3-δ, enhancing catalytic activity without using precious metals or rare earth elements.
The catalyst exhibits high activity in ammonia decomposition and synthesis reactions at lower temperatures, offering a cost-effective and stable solution for hydrogen and ammonia production.
Smart Images

Figure 2024165433000001 
Figure 2024165433000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a catalyst used in an ammonia decomposition or synthesis reaction, and more particularly to a catalyst used in an ammonia decomposition reaction or an ammonia synthesis reaction that is useful for hydrogen production and the like. [Background technology]
[0002] Ammonia has long been produced as a raw material for chemical fertilizers, and in recent years has been attracting attention as a promising hydrogen carrier for the realization of a hydrogen society in the future due to its high hydrogen density per volume. Methods for extracting hydrogen from ammonia include electrolysis and catalytic cracking. The thermal catalytic cracking reaction, which is commonly used to crack ammonia, is an endothermic reaction and is known to proceed at high temperatures of 600°C or higher. In recent years, there has been active development of catalysts that exhibit high activity at lower temperatures, with a view to application to fuel cells.
[0003] Known active metals for ammonia decomposition catalysts include ruthenium, cobalt, nickel, iron, etc. (see, for example, Non-Patent Documents 1 and 2). Among them, ruthenium catalysts are known to exhibit high activity at low temperatures, and Patent Document 1 discloses a method for decomposing ammonia, which is characterized by contacting ammonia or an ammonia-containing gas with a catalyst comprising ruthenium supported on an inorganic carrier under heating, and decomposing the ammonia into nitrogen and hydrogen.
[0004] However, since ruthenium, a precious metal, is expensive compared to cobalt, nickel, and iron, techniques for reducing the amount of ruthenium used are also being considered, and for example, Patent Document 2 discloses an ammonia decomposition catalyst characterized in that ruthenium and a promoter are supported on a support formed of ultrafine particle powder with an average particle size of 1 nm to 50 nm in a required shape. Also, Patent Document 3 discloses an ammonia decomposition catalyst in which ruthenium and a rare earth oxide are supported on a support made of a metal oxide other than rare earth oxide, and the content of the rare earth oxide is 0.1 to 30.0 mass%.
[0005] Patent Document 4 discloses a method for producing hydrogen, which comprises a step of contacting a raw material gas containing ammonia with a catalyst (X) containing at least one element (A) selected from nickel, cobalt, and iron, at least one element (B) selected from strontium and barium, and at least one element (C) selected from lanthanoids excluding lanthanum and cerium, and containing element (B) in an amount of 0.1 mass% to 15 mass% calculated as the oxide of element (B). In contrast to these, Non-Patent Document 3 investigates the ammonia decomposition activity of a catalyst in which Ni is supported on a perovskite oxide such as SrZrO3 or BaZrO3 as a catalyst that does not use a precious metal. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] Japanese Patent Application Publication No. 8-84910 [Patent Document 2] JP 2011-78888 A [Patent Document 3] International Publication No. 2019 / 188219 [Patent Document 4] JP 2016-203052 A [Non-patent literature]
[0007] [Non-Patent Document 1] H Muroyama and 3 others, Applied Catalysis A: General, 2012, Vol. 433, p119-124 [Non-Patent Document 2] L Wang and 4 others, Chemical Communications, 2013, Vol. 49, p3787-3789 [Non-Patent Document 3] K Okura and 4 others, RSC Advances, 2018, Vol. 8, p32102-32110 Summary of the Invention [Problem to be solved by the invention]
[0008] As mentioned above, various ammonia decomposition catalysts have been developed, and technologies using rare earth elements as promoters to reduce the amount of ruthenium used have been considered. However, rare earth elements are expensive, and there is a bias in the countries that produce the ores, which causes problems in terms of cost and stable supply. In addition, the catalysts that do not use precious metals or rare earth elements that have been considered so far have not been sufficient in catalytic activity in ammonia decomposition reactions and synthesis reactions. Therefore, there has been a demand for a catalyst that exhibits high catalytic activity in ammonia decomposition reactions and synthesis reactions without using precious metals or rare earth elements.
[0009] The present invention has been made in consideration of the above-mentioned current situation, and an object of the present invention is to provide a catalyst that exhibits high catalytic activity in ammonia decomposition reactions and synthesis reactions without using expensive precious metals or rare earth elements. [Means for solving the problem]
[0010] The present inventors have conducted various studies on catalysts used in the decomposition or synthesis reaction of ammonia, and have found that by supporting nickel and / or its oxide on a carrier containing a composite oxide (A) containing titanium, barium, and zirconium as constituent elements, a catalyst exhibiting high ammonia decomposition activity can be obtained without using expensive precious metals or rare earth elements. In addition, the inventors have found that the above catalyst also exhibits high activity in the ammonia synthesis reaction, which is the reverse reaction of the ammonia decomposition reaction. Thus, the inventors have come up with the idea of brilliantly solving the above problems and have arrived at the present invention.
[0011] The present invention includes the following catalysts etc. [1] A catalyst having a structure in which at least one selected from the group consisting of nickel, iron, cobalt and oxides thereof is supported on a carrier containing a composite oxide (A) containing titanium, barium and zirconium as constituent elements, and used in the decomposition or synthesis reaction of ammonia. [2] The above-mentioned composite oxide (A) is represented by the following formula (1); BaTi x Zr 1-x O 3-δ (1) (wherein x represents a number satisfying 0.05≦x≦0.9, and δ represents an amount of oxygen deficiency). [3] A method for producing the catalyst according to the above [1] or [2], comprising the steps of supporting at least one selected from the group consisting of nickel, iron, cobalt and oxides thereof on a support containing a composite oxide (A) containing titanium, barium and zirconium as constituent elements, and calcining the supported material obtained in the supporting step. [4] A method for producing hydrogen, comprising a step of decomposing ammonia using the catalyst according to [1] or [2] above. [5] An ammonia production method comprising a step of synthesizing ammonia using the catalyst according to [1] or [2] above. Effect of the Invention
[0012] The catalyst of the present invention has the above-mentioned configuration and exhibits high catalytic activity in ammonia decomposition reactions and synthesis reactions without using precious metals or rare earth elements, and can therefore be suitably used for the production of hydrogen, ammonia, and the like. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] The preferred embodiments of the present invention are specifically described below, but the present invention is not limited to the following description, and can be modified as appropriate within the scope of the present invention. In addition, a combination of two or more of the individual preferred embodiments of the present invention described below also falls within the preferred embodiments of the present invention.
[0014] 1. Catalysts used in the decomposition or synthesis of ammonia The catalyst of the present invention has a structure in which at least one selected from the group consisting of nickel, iron, cobalt and oxides thereof is supported on a carrier containing a composite oxide (A) containing titanium, barium and zirconium as constituent elements, and is used in the decomposition or synthesis reaction of ammonia. In this specification, the term "supported" means that the compound to be supported is supported on the surface of a carrier. The compound to be supported may be partially attached to the surface of the carrier, or may form a layer. It is believed that the carrier in the catalyst contains the composite oxide (A) containing titanium, barium, and zirconium as constituent elements, and by forming a composite oxide of these three elements, the electronic interaction changes and oxygen deficiencies and distortions in the unit lattice occur, making it easier for ammonia, hydrogen, and nitrogen to be adsorbed, thereby contributing to improved catalytic activity. Furthermore, the catalyst of the present invention, by virtue of having the above structure, is able to exhibit catalytic activity even at a lowered reaction temperature.
[0015] The ratios of titanium, barium and zirconium in the composite oxide (A) are not particularly limited, but the ratios (molar ratios) of titanium and zirconium to barium are preferably each 0.1 to 0.9. The composite oxide (A) has the following formula (1); BaTi x Zr 1-x O 3-δ (1) (wherein x represents a number satisfying 0.05≦x≦0.9, and δ represents the amount of oxygen deficiency) is preferable. The above x is a number from 0.05 to 0.9, preferably from 0.05 to 0.8, more preferably from 0.08 to 0.3, and further preferably from 0.1 to 0.2. δ in the above formula (1) represents the amount of oxygen vacancy, and takes different values depending on the composition, temperature, atmosphere, etc., but is a value in the range of 0 to 1.
[0016] The crystal structure of the composite oxide (A) is not particularly limited, and examples thereof include perovskite type, fluorite type, spinel type, etc., with the perovskite type being preferred.
[0017] The amount of nickel and / or its oxide supported in the catalyst is preferably 1 to 60 parts by weight in terms of nickel metal element relative to 100 parts by weight of the entire catalyst. With such a supported amount, the catalyst can have higher catalytic activity. The amount of nickel and / or its oxide supported is more preferably 10 to 50 parts by weight, and further preferably 30 to 45 parts by weight. The amount of iron and / or its oxide supported in the catalyst is preferably 1 to 60 parts by weight, more preferably 10 to 50 parts by weight, and further preferably 30 to 45 parts by weight, calculated as iron metal element. The amount of cobalt and / or its oxide supported in the above catalyst is preferably 1 to 60 parts by weight, more preferably 10 to 50 parts by weight, and further preferably 30 to 45 parts by weight, calculated as the cobalt metal element. When nickel, iron, cobalt and oxides thereof are used in combination in the above catalyst, the total supported amount is preferably 1 to 60 parts by weight, more preferably 10 to 50 parts by weight, and even more preferably 30 to 45 parts by weight, calculated as nickel, iron and cobalt metal elements, per 100 parts by weight of the entire catalyst.
[0018] The form of the catalyst is not particularly limited, and the catalyst may be used as a powder as it is, but it is preferable to use the catalyst as a molded catalyst. Examples of molded catalysts include agglomerates obtained by pressurizing and compressing powder catalysts, compression molded bodies obtained by crushing these agglomerates to an appropriate particle size, tablet molded bodies obtained by compressing and solidifying powder catalysts into a specific shape using a tablet press, spherical molded bodies obtained by coating powder catalysts on spherical carriers or by tumbling granulation, honeycomb molded bodies obtained by coating powder catalysts on honeycomb carriers, and extrusion molded bodies obtained by adding binders to powder catalysts and kneading and extruding them.
[0019] The above-mentioned molded catalyst may be molded with a pore-forming agent and then calcined to form pores. Examples of the pore-forming agent include carboxymethyl cellulose, polystyrene, etc., which are easily removed by calcination.
[0020] 2. Catalyst manufacturing method The catalyst of the present invention can be produced by supporting at least one selected from the group consisting of nickel, iron, cobalt and oxides thereof on a carrier containing a composite oxide (A) containing titanium, barium and zirconium as constituent elements. Preferably, the catalyst is produced by carrying out a step of supporting at least one selected from the group consisting of nickel, iron, cobalt and oxides thereof on a carrier containing a composite oxide (A) containing titanium, barium and zirconium as constituent elements, and a step of calcining the supported material obtained in the supporting step. The method of producing a catalyst including the supporting step and the calcining step is also one aspect of the present invention.
[0021] The method for producing the composite oxide (A) containing titanium, barium and zirconium as constituent elements used in the above-mentioned catalyst production method is not particularly limited, and the composite oxide can be obtained by a commonly used method. Specifically, examples of the method include a method of subjecting a mixture of compounds containing barium, titanium, and zirconium to hydrothermal treatment, and a method of synthesizing the compound by a solid-state reaction.
[0022] The nickel raw material used in the above-mentioned supporting step is not particularly limited as long as it contains nickel element, but examples thereof include compounds such as nickel nitrate (II), nickel chloride, nickel oxide (II), nickel sulfate (II), nickel hydroxide (II), nickel acetate (II), nickel carbonate (II), basic nickel carbonate (II), nickel sulfide (II), tetracarbonyl nickel (0), and nickel perchlorate (II), as well as metallic nickel, and one or more of these can be used. Among these, nickel nitrate and nickel chloride are preferred.
[0023] The iron raw material used in the above-mentioned supporting step is not particularly limited as long as it contains iron element, but includes iron nitrate (II), iron nitrate (III), iron oxide (II), iron oxide (III), iron chloride (II), iron chloride (III), iron hydroxide (II), iron hydroxide (III), iron sulfate (II), iron sulfate (III), iron acetate (II), basic iron acetate (III), iron carbonate (II), iron sulfide (II), iron sulfide (III), iron pentacarbonyl iron (0), iron perchlorate (II), iron perchlorate (III), metallic iron, etc., and one or more of these can be used. Among these, iron nitrate and iron chloride are preferred.
[0024] The cobalt raw material used in the above-mentioned supporting step is not particularly limited as long as it contains the cobalt element, but examples thereof include cobalt nitrate (II), cobalt chloride (II), cobalt oxide (II), cobalt sulfate (II), cobalt hydroxide (II), cobalt acetate (II), cobalt carbonate (II), basic cobalt carbonate (II), cobalt sulfide (II), cobalt octacarbonyl (0), cobalt perchlorate (II), metallic cobalt, etc., and one or more of these can be used. Among these, cobalt nitrate and cobalt chloride are preferred.
[0025] In the supporting step, it is preferable to mix the support with at least one material selected from the group consisting of the nickel raw material, the iron raw material, and the cobalt raw material (hereinafter, also referred to as nickel species, etc.). The above-mentioned supporting step may be a dry mixing or a wet mixing step, but it is more preferable to carry out the wet mixing step since it is possible to more sufficiently support at least one selected from the group consisting of nickel, iron, cobalt and oxides thereof on the support. As the solvent used in the wet mixing, water, alcohol, ketone, ether compound, etc. can be used, with water being preferred.
[0026] When the above-mentioned carrier and nickel species, etc. are mixed using a solvent, it is preferable to dissolve the nickel species, etc. in a solvent to prepare a solution of the nickel species, etc., and then mix it with the carrier. In this way, the nickel species, etc. can be made to exist finer on the carrier surface, and the effective surface area of the nickel species, etc. can be increased.
[0027] When a solvent is used in the step of supporting the nickel seeds or the like on the support, it is preferable to remove the solvent before the calcination step, so that the calcination step can be carried out efficiently. The method for removing the solvent is not particularly limited, but a method of evaporating the solvent is preferred, and a method of heating the mixture is preferred. The heating temperature is preferably 60 to 150°C, more preferably 80 to 130°C. The heating time is preferably from 1 to 30 hours, and more preferably from 5 to 10 hours.
[0028] In the step of calcining the material supported on the carrier, such as nickel seeds, the calcination temperature is preferably 100 to 1000°C, more preferably 200 to 800°C, and even more preferably 200 to 700°C. The firing time is preferably 10 to 300 minutes, and more preferably 30 to 180 minutes.
[0029] The firing can be carried out in an air atmosphere, a reducing atmosphere, an inert atmosphere, or a vacuum atmosphere. The reducing atmosphere can be an atmosphere containing a reducing gas such as hydrogen in an inert gas such as helium, nitrogen, or argon at a ratio of more than 0 to 100 vol%. In addition, a hydride such as sodium borohydride or titanium hydride, or a reducing substance such as carbon or an organic substance may be mixed and fired.
[0030] 3. Hydrogen production methods The catalyst of the present invention can be suitably used in a reaction for producing hydrogen by decomposing ammonia. A method for producing hydrogen, which includes a step of decomposing ammonia using the catalyst of the present invention, also constitutes the present invention. The method for producing hydrogen is preferably a method in which ammonia gas is supplied to the catalyst.
[0031] The method for producing hydrogen preferably includes a step of reducing the catalyst before the ammonia decomposition step, which generates oxygen vacancies in the composite oxide (A), making it easier for ammonia to be adsorbed in the ammonia decomposition step and increasing the catalytic activity. The reduction treatment step is not particularly limited as long as the composite oxide (A) in the catalyst is reduced, but it is preferable to heat in a reducing atmosphere. The reducing gas used in the reduction treatment step includes hydrogen, carbon monoxide, etc. The reducing gas is preferably hydrogen. The heating temperature in the reduction treatment step is not particularly limited, but is preferably 300 to 900°C, more preferably 400 to 800°C, and further preferably 500 to 700°C. The heating time in the reduction treatment step is not particularly limited, but is preferably 1 to 24 hours, more preferably 2 to 12 hours, and further preferably 3 to 10 hours.
[0032] The reaction temperature in the ammonia decomposition reaction is preferably 300 to 700°C, and more preferably 400 to 600°C. The reaction pressure is preferably 0.1 to 0.6 MPa, and more preferably 0.1 to 0.3 MPa.
[0033] 4. Method of producing ammonia The catalyst of the present invention can be suitably used in a reaction for producing ammonia using hydrogen and nitrogen as raw materials. A method for producing ammonia, comprising a step of synthesizing ammonia using such a catalyst of the present invention, also constitutes one aspect of the present invention.
[0034] The ammonia synthesis step is not particularly limited as long as hydrogen and nitrogen are reacted, but the reaction temperature is preferably 300 to 700°C, and more preferably 400 to 600°C. The reaction pressure is preferably 0.1 to 0.6 MPa, and more preferably 0.1 to 0.3 MPa. EXAMPLES
[0035] In order to explain the present invention in detail, specific examples are given below, but the present invention is not limited to these examples. Unless otherwise specified, "%" means "% by weight." The methods for measuring each physical property are as follows.
[0036] <Example 1> 33.7 g of nickel (II) nitrate hexahydrate (manufactured by Fujifilm Wako Pure Chemical Industries Co., Ltd.) and 50.0 g of ion-exchanged water were weighed and placed in an eggplant flask, and after stirring, 10.0 g of perovskite-type barium zirconate titanate (manufactured by Sakai Chemical Industry Co., Ltd., product name "BTZ-8020-01") was weighed and placed in the eggplant flask, and stirred for 30 minutes. After that, it was dried to obtain dry powder 1. The obtained dry powder 1 was placed in an alumina crucible, heated to 700 ° C in the air, held at 700 ° C for 2 hours, and then naturally cooled to room temperature to obtain Example 1 powder.
[0037] <Example 2> 4.2 g of nickel (II) nitrate hexahydrate (manufactured by Fujifilm Wako Pure Chemical Industries Co., Ltd.) and 50.0 g of ion-exchanged water were weighed and placed in an eggplant flask, and after stirring, 10.0 g of perovskite-type barium zirconate titanate (manufactured by Sakai Chemical Industry Co., Ltd., product name "BTZ-8020-01") was weighed and placed in the eggplant flask and stirred for 30 minutes. After that, it was dried to obtain dry powder 2. The obtained dry powder 2 was placed in an alumina crucible, heated to 700 ° C in the air, held at 700 ° C for 2 hours, and then naturally cooled to room temperature to obtain Example 2 powder.
[0038] <Example 3> 32.9 g of cobalt (II) nitrate hexahydrate (manufactured by Fujifilm Wako Pure Chemical Industries Co., Ltd.) and 50.0 g of ion-exchanged water were weighed and placed in an eggplant flask, and after stirring, 10.0 g of perovskite-type barium zirconate titanate (manufactured by Sakai Chemical Industry Co., Ltd., product name "BTZ-8020-01") was weighed and placed in the eggplant flask and stirred for 30 minutes. After that, it was dried to obtain dry powder 3. The obtained dry powder 3 was placed in an alumina crucible, heated to 700 ° C in the air, held at 700 ° C for 2 hours, and then naturally cooled to room temperature to obtain Example 3 powder.
[0039] <Example 4> 30.5 g of iron (II) nitrate nonahydrate (manufactured by Fujifilm Wako Pure Chemical Industries Co., Ltd.) and 50.0 g of ion-exchanged water were weighed and placed in an eggplant flask, and after stirring, 10.0 g of perovskite-type barium zirconate titanate (manufactured by Sakai Chemical Industry Co., Ltd., product name "BTZ-8020-01") was weighed and placed in the eggplant flask and stirred for 30 minutes. After that, it was dried to obtain dry powder 4. The obtained dry powder 4 was placed in an alumina crucible, heated to 700 ° C in the air, held at 700 ° C for 4 hours, and then naturally cooled to room temperature to obtain Example 4 powder.
[0040] <Example 5> 3.8 g of iron (II) nitrate nonahydrate (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) and 25.0 g of ion-exchanged water were weighed and placed in an eggplant flask, and after stirring, 10.0 g of perovskite-type barium zirconate titanate (manufactured by Sakai Chemical Industry Co., Ltd., product name "BTZ-8020-01") was weighed and placed in the eggplant flask and stirred for 30 minutes. After that, it was dried to obtain dry powder 5. The obtained dry powder 5 was placed in an alumina crucible, heated to 700°C in the air, held at 700°C for 4 hours, and then naturally cooled to room temperature to obtain Example 5 powder.
[0041] <Comparative Example 1> 33.7 g of nickel (II) nitrate hexahydrate (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) and 50.0 g of ion-exchanged water were weighed and placed in an eggplant flask and stirred, after which 10.0 g of barium zirconate (manufactured by Kojundo Chemical Laboratory Co., Ltd.) was weighed and placed in the eggplant flask and stirred for 30 minutes. It was then dried to obtain dry powder 6. The obtained dry powder 6 was placed in an alumina crucible, heated to 700°C in the air, held at 700°C for 2 hours, and then naturally cooled to room temperature to obtain Comparative Example 1 powder.
[0042] <Comparative Example 2> 33.7 g of nickel (II) nitrate hexahydrate (manufactured by Fujifilm Wako Pure Chemical Industries Co., Ltd.) and 50.0 g of ion-exchanged water were weighed and placed in an eggplant flask, and then stirred. 10.0 g of barium titanate (manufactured by Sakai Chemical Industry Co., Ltd., product name "BT-01") was weighed and placed in the eggplant flask, and stirred for 30 minutes. Then, it was dried to obtain dry powder 7. The obtained dry powder 7 was placed in an alumina crucible, heated to 700°C in the air, and held at 700°C for 2 hours, and then naturally cooled to room temperature to obtain Comparative Example 2 powder.
[0043] <Comparative Example 3> 3.8 g of iron (II) nitrate nonahydrate (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) and 25.0 g of ion-exchanged water were weighed and placed in an eggplant flask and stirred, after which 10.0 g of barium titanate (manufactured by Sakai Chemical Industry Co., Ltd., product name "BT-01") was weighed and placed in the eggplant flask and stirred for 30 minutes. It was then dried to obtain a dry powder 8. The obtained dry powder 8 was placed in an alumina crucible, heated to 700°C in the air, held at 700°C for 4 hours, and then naturally cooled to room temperature to obtain a powder of Comparative Example 3.
[0044] <Ammonia decomposition activity evaluation> 1.0 g of the powder of Examples 1, 2, 3, 4, and 5 and Comparative Examples 1, 2, and 3 was placed in a mold of φ20 mm, pressed at a pressure of 30 MPa using a press machine, and the obtained pellets were passed through a sieve with an opening of 600 μm to 1.4 mm, and the molded powder on the sieve was collected to obtain a sample for evaluating ammonia decomposition activity. The obtained sample for evaluating ammonia decomposition activity was fixed to the center of a quartz tube with a diameter of φ1 cm and a length of 38 cm, and the quartz tube was set in an infrared furnace. Nitrogen was passed through the quartz tube at normal pressure at 200 ml / min and held for 5 minutes. Next, the temperature was raised to 600 ° C. over 120 minutes while passing hydrogen at 180 ml / min, and held for 2 hours. Thereafter, the temperature was lowered to 550 ° C. over 15 minutes while passing a mixed gas of ammonia at 100 ml / min and nitrogen at 60 ml / min, and held for 15 minutes. The temperature was lowered to 500 ° C. over 15 minutes and held for 15 minutes. The generated gas while maintaining each temperature was blown into a stirred 0.3 M aqueous sulfuric acid solution, and the change in electrical conductivity of the aqueous sulfuric acid solution per 300 seconds was measured using an electrical conductivity meter (portable electrical conductivity meter CM-31P, manufactured by DKK-TOA Corporation). The average change over 15 minutes was calculated, and the ammonia decomposition rate was calculated from a previously measured calibration curve.
[0045] <Ammonia synthesis activity evaluation> 1.0 g of the powders of Example 5 and Comparative Example 3 were placed in a mold of φ20 mm, pressed at a pressure of 30 MPa using a press machine, and the obtained pellets were passed through a sieve with an opening of 600 μm to 1.4 mm, and the molded powder on the sieve was collected to obtain a sample for evaluating ammonia synthesis activity. The obtained sample for evaluating ammonia synthesis activity was fixed to the center of a quartz tube with a diameter of φ1 cm and a length of 38 cm, and the quartz tube was set in an infrared furnace. Nitrogen was passed through the quartz tube at normal pressure at 200 ml / min and held for 5 minutes. Next, the temperature was raised to 600 ° C. over 120 minutes while passing hydrogen at 180 ml / min, and held for 30 minutes. Thereafter, the mixture gas of hydrogen at 180 ml / min and nitrogen at 60 ml / min was passed through the tube and held at 600 ° C. for 30 minutes. The temperature was lowered to 550 ° C. over 20 minutes, and held for 30 minutes. The temperature was lowered to 500 ° C. over 20 minutes, and held for 30 minutes. The generated gas at each temperature was stirred at 2.0×10 -6The solution was blown into an aqueous sulfuric acid solution of M, and the change in electrical conductivity of the aqueous sulfuric acid solution per 300 seconds was measured using an electrical conductivity meter (apparatus name: portable electrical conductivity meter CM-31P, manufactured by DKK-TOA Corporation). The average change over 30 minutes was calculated, and the ammonia generation concentration was calculated from a previously measured calibration curve.
[0046] [Table 1] [Table 2]
[0047] As seen from the above results, by using a carrier containing a composite oxide (A) containing titanium, barium, and zirconium as constituent elements, Examples 1 to 5 showed a significantly improved ammonia decomposition activity compared to Comparative Examples 1 and 2, which used a carrier not containing titanium or zirconium as a constituent element. Moreover, in the carrier containing the composite oxide (A) of Example 1, as compared with the catalysts of Comparative Examples 1 and 2, the cracking activity at low temperatures was significantly improved. Furthermore, from Examples 2 and 5, it was found that the support containing the composite oxide (A) had a cracking activity equivalent to or greater than that of Comparative Examples 1 and 2 in which 40 parts by weight of the metal species was supported, even when the amount of the metal species supported was reduced to 5 parts by weight, and that the catalytic activity per weight of the supported metal species was dramatically improved. In addition, in Example 5, by using a support containing a composite oxide containing titanium, barium, and zirconium as constituent elements, the ammonia synthesis activity was significantly improved compared to Comparative Example 3, which used a support not containing titanium or zirconium as constituent elements. Thus, it has become clear that the catalyst of the present invention exhibits high ammonia decomposition or synthesis activity without using any precious metals or rare earth elements.
Claims
1. A catalyst having a structure in which at least one selected from the group consisting of nickel, iron, cobalt and oxides thereof is supported on a carrier containing a composite oxide (A) containing titanium, barium and zirconium as constituent elements, and which is used in an ammonia decomposition or synthesis reaction.
2. The composite oxide (A) is represented by the following formula (1); Baati x Zr 1-x O 3-δ (1) (In the formula, x represents a number in the range of 0.05≦x≦0.9, and δ represents the amount of oxygen deficiency.) The catalyst according to claim 1, which is a compound represented by the formula:
3. A method for producing the catalyst according to claim 1 or 2, comprising the steps of: The production method includes the steps of supporting at least one selected from the group consisting of nickel, iron, cobalt, and oxides thereof on a support containing a composite oxide (A) containing titanium, barium, and zirconium as constituent elements, and calcining the supported material obtained in the supporting step.
4. A method for producing hydrogen, comprising a step of decomposing ammonia using the catalyst according to claim 1 or 2.
5. A method for producing ammonia, comprising a step of synthesizing ammonia using the catalyst according to claim 1 or 2.
Citation Information
Patent Citations
Method for decomposing ammonia
JP1996084910A
Catalyst for decomposing ammonia
JP2011078888A
Method for producing hydrogen and catalyst for hydrogen production
JP2016203052A
Ammonia decomposition catalyst and method for producing same, and method for producing hydrogen gas
WO2019188219A1
Cited By
Preparation method and application of low-temperature efficient ammonia decomposition hydrogen production catalyst
CN121042074A