Steel material and mold

The optimized steel composition addresses heat checks and cracks in large molds by enhancing thermal conductivity and microstructure refinement, ensuring durability and manufacturability while maintaining high hardness and impact resistance.

JP2024165785AInactive Publication Date: 2024-11-28DAIDO STEEL CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023082279
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-18
Publication Date
2024-11-28
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing steel materials for large molds are prone to heat checks and large cracks due to slow cooling rates and thermal stress, which compromise manufacturability and durability, with no steel material effectively balancing hardness, impact resistance, and machinability.

Method used

A steel composition with optimized amounts of C, V, Mn, Cr, Mo, Si, and N, along with controlled ratios and limits, to enhance pinning particles, thermal conductivity, and microstructure refinement, reducing retained austenite and transformation heat generation, thereby improving heat check resistance and crack prevention.

Benefits of technology

The optimized steel material achieves high hardness, impact value, and machinability, effectively preventing heat checks and large cracks in molds exceeding 2000 kg, with extended creep rupture time and improved manufacturability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024165785000001_ABST
    Figure 2024165785000001_ABST
Patent Text Reader

Abstract

To provide: a steel material which is applicable to both a hardening and tempering (HT) casting plan and a pre-hardening (PH) casting plan, and enables manufacture of a mold excellent in durability (heat check resistance and / or large crack resistance) without remarkably impairing manufacturability (SA property and / or machinability); and a mold manufactured of the steel material.SOLUTION: A steel material comprises 0.23≤C≤0.39 mass%, 0.03≤V≤0.30 mass%, 6.60≤Mn+Cr≤7.40 mass%, Mn / Cr≤0.150, Mn≥0.60 mass%, Cr≤6.60 mass%, Cu+Ni≤0.84 mass%, 0.01≤Si≤0.40 mass%, 2.00≤Mo≤3.50 mass%, 0.001≤Al≤0.080 mass%, and 0.003≤N≤0.040 mass%, with the balance being Fe and inevitable impurities. A mold is manufactured of such a steel material, and has a mass of 2000 kg or more.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a steel material and a mold, and more particularly to a steel material suitable for manufacturing a mold having a large mass and size, and a mold using the same. [Background technology]

[0002] Since dies are repeatedly subjected to stress and heat during use, the steel materials for dies are required to have excellent properties such as hardness, impact resistance, heat check resistance, abrasion resistance, etc. For this reason, various proposals have been made for steel materials having such properties. For example, Patent Document 1 discloses a hot work tool steel containing predetermined amounts of C, Si, Mn, Cr, Mo, and V, with the balance being Fe and unavoidable impurities.

[0003] There are two methods for manufacturing dies: quenching and tempering (HT) and pre-hardening (PH). The HT method is a method for imparting the necessary hardness and toughness to dies "after" machining. On the other hand, the PH method is a method for imparting the necessary hardness and toughness to dies "before" machining.

[0004] Whether the HT method or the PH method is used to manufacture dies, the larger the size of the die, the more likely it is that heat checking and large cracks will occur. This is thought to be because the larger the size of the die, the slower the cooling rate during quenching, which reduces the high-temperature strength and toughness of the steel. Another reason is that the larger the size of the die, the greater the thermal stress and mechanical stress acting on the die during use.

[0005] On the other hand, steel materials that are less susceptible to heat checking and large cracking generally have low manufacturability (SA property, machinability). Furthermore, there have been no examples of steel materials that can suppress heat checking and large cracking without significantly impairing manufacturability, even when applied to large-sized dies. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2011-001572 A Summary of the Invention [Problem to be solved by the invention]

[0007] The problem that the present invention aims to solve is to provide a steel material that can be used to manufacture dies having excellent durability (heat check resistance and / or large crack resistance) without significantly impairing manufacturability (SA property and / or machinability). [Means for solving the problem]

[0008] In order to solve the above problems, the steel material according to the present invention comprises: 0.23≦C≦0.39mass%, 0.03≦V≦0.30mass%, 6.60≦Mn+Cr≦7.40mass%, Mn / Cr≦0.150, Mn≧0.60mass%, Cr≦6.60mass%, Cu+Ni≦0.84mass%, 0.01≦Si≦0.40mass%, 2.00≦Mo≦3.50mass%, 0.001≦Al≦0.080mass%, and 0.003≦N≦0.040mass% The balance consists of Fe and unavoidable impurities.

[0009] The die according to the present invention is manufactured from the steel material according to the present invention and has a mass of 2000 kg or more. Effect of the Invention

[0010] The present invention optimizes the amounts of Si and Mo in low-Si, high-Mo steel material, so that large cracks and heat checks can be suppressed even when the steel material has a large mass or size. [Brief description of the drawings]

[0011] [Figure 1] FIG. 1 is a schematic diagram of the effects obtained by increasing Mo and decreasing Si. [Diagram 2] FIG. 2 is a diagram showing the ranges of Mn and Cr contents for obtaining a steel material having excellent SA properties and hardenability. [Diagram 3] FIG. 4 is a graph showing the relationship between the amount of retained austenite and the amount of Mo. [Figure 4] FIG. 1 is a graph showing the relationship between creep rupture time and Mo content. [Diagram 5] FIG. 1 is a graph showing the relationship between fracture toughness and the Si content.

[0012] [Figure 6] FIG. 2 is a graph showing the relationship between high-temperature tensile strength and the Si content. [Figure 7] FIG. 1 is a graph showing the relationship between softening resistance and Si content. [Figure 8] FIG. 1 is a graph showing the relationship between the critical cooling rate for pearlite precipitation and the Si content. [Figure 9] FIG. 13 is a diagram showing a change in temperature at the center of a block during rapid cooling. [Figure 10] FIG. 13 is a diagram showing a hardening simulation of a 12.5 ton block of SKD61.

[0013] An embodiment of the present invention will be described in detail below. [1. Steel materials] [1.1. Composition] [1.1.1. Main constituent elements] The steel material according to the present invention contains the following elements, with the balance being Fe and unavoidable impurities. The types of added elements, their component ranges, and the reasons for their limitations are as follows:

[0014] (1) 0.23≦C≦0.39mass%: Fine particles (carbides, carbonitrides) with a diameter of 0.5 μm or less function as "pinning particles" that suppress the growth of austenite grains during quenching heating. If the amount of C is too small, the amount of pinning particles will be insufficient during quenching heating. As a result, the grains will become coarse, and the steel properties such as impact value, fracture toughness value, and ductility may deteriorate. Also, if the C content is too low, the martensitic transformation start temperature (Ms point) becomes excessively high, which results in high hardenability but a decrease in impact value.

[0015] Furthermore, if the amount of C is too small, it is difficult to obtain a hardness of 45HRC or more by tempering at 560 to 600°C. To ensure high heat check resistance, a hardness of 45HRC or more is necessary. Also, if the amount of C is too small, the softening resistance decreases. Therefore, even if a hardness of 45HRC or more is obtained after quenching and tempering, the hardness may decrease during use as a mold, and the tensile strength at high temperatures may decrease. If this happens, it will no longer be possible to satisfy (2) and (3) in Table 1 described below. Therefore, the C content must be 0.23 mass% or more, preferably 0.25 mass% or more, and more preferably 0.27 mass% or more.

[0016] On the other hand, if the amount of C is excessive, coarse carbides and carbonitrides may crystallize during casting. These become "inclusions" that reduce the impact value. For this reason, (4) in Table 1 described below is required. It is difficult to dissolve and eliminate coarse inclusions through heat treatment (homogenization heat treatment, normalizing, spheroidizing annealing). Coarse inclusions often do not dissolve completely and remain even after quenching and tempering. Coarse inclusions dissolve during homogenization heat treatment and become smaller in size, but are still observed with a diameter exceeding 5 μm. Inclusions that do not dissolve completely and remain can become the starting point of fracture, causing a decrease in impact value and fatigue strength.

[0017] Furthermore, when an ingot is formed into a block or bar-shaped steel material by hot working, if the cooling rate after hot working is slow, the impact value may decrease. This phenomenon becomes clear when the amount of C is excessive. The cause is carbides and carbonitrides that precipitate at the austenite grain boundaries during cooling after hot working. Like the crystallized particles mentioned above, these precipitates become "foreign matter" that lower the impact value. For this reason, (4) in Table 1, which will be described later, is required. These precipitates do not dissolve completely even with various heat treatments after hot working, and ultimately remain in the quenched and tempered structure. The precipitates are not large, less than 10 μm, but multiple precipitates are distributed in a dotted line with a gap between them, forming a necklace-like structure. The "diameter of the necklace (the maximum length of the area where multiple precipitates are distributed in a dotted line with a gap between them)" corresponds to the coarse austenite grain size after hot working. The size of these coarse prior austenite grains becomes the fracture surface unit, so the impact value and fracture toughness deteriorate. Therefore, the C content must be 0.39 mass% or less, preferably 0.38 mass% or less, and more preferably 0.37 mass% or less.

[0018] (2) 0.03≦V≦0.30mass%: V bonds with C and / or N in the steel to form carbides, carbonitrides, and / or nitrides. All of these function as pinning particles. See (5) in Table 1, which will be described later. Therefore, if the amount of V is too small, the amount of pinning particles will be insufficient during quenching heating. Also, if the amount of V is too small, the degree of secondary hardening during tempering will be small. As a result, when tempered at 560 to 600°C, it will be difficult to obtain a hardness of 45HRC or more. In addition, since the softening resistance will decrease, even if a hardness of 45HRC or more can be obtained by quenching and tempering, the hardness will decrease during use as a mold, and the high-temperature tensile strength may decrease. See (2) in Table 1 below. Therefore, the amount of V must be 0.03 mass% or more, preferably 0.05 mass% or more, and more preferably 0.07 mass% or more.

[0019] On the other hand, if the amount of V is excessive, the amount of coarse inclusions increases. As mentioned above, "inclusions" are crystallized substances that crystallize during casting or precipitates that precipitate during cooling after hot working. For this reason, (4) in Table 1, which will be described later, is required. Therefore, the amount of V must be 0.30 mass% or less, preferably 0.29 mass% or less, and more preferably 0.28 mass% or less.

[0020] (3) 6.60≦Mn+Cr≦7.40mass%: Both Mn and Cr affect hardenability. If the Mn+Cr content is too small, hardenability is insufficient. As a result, the impact value may decrease significantly, particularly inside a large mold (in an area where the hardening rate is slow). Therefore, the Mn+Cr content must be 6.60 mass% or more. The Mn+Cr content is preferably 6.65 mass% or more, and more preferably 6.70 mass% or more.

[0021] On the other hand, if the Mn+Cr content is excessive, the thermal conductivity drops significantly. As a result, the heat check resistance is deteriorated due to the increase in thermal stress. Therefore, the Mn+Cr content must be 7.40 mass% or less. The Mn+Cr content is preferably 7.35 mass% or less, and more preferably 7.30 mass% or less.

[0022] (4) Mn / Cr≦0.150: The ratio of the mass of Mn to the mass of Cr contained in the steel (Mn / Cr) affects the SA property. If the Mn / Cr ratio is too large, the SA property deteriorates. c3 In order to soften the steel to 98HRB or less in SA at a heating temperature exceeding the above point, the cooling rate must be less than 10°C / H. As a result, the SA process becomes longer and productivity decreases. In addition, when the crystal grains are coarse, SA defects are likely to occur when the Mn / Cr ratio is high. SA also plays a role in avoiding austenite memory, which will be described later. Therefore, if SA defects occur, it may become difficult to refine the grains during quenching. Therefore, the Mn / Cr ratio must be 0.150 or less, preferably 0.148 or less, and more preferably 0.145 or less.

[0023] (5) Mn≧0.60mass%: Mn affects hardenability. If the Mn content is too low, the hardenability deteriorates. In order to ensure hardenability when the Mn content is low, it is necessary to increase the Cr content. However, if the Cr content is excessive, the following problems may become apparent. Therefore, the Mn content must be 0.60 mass% or more, preferably 0.62 mass% or more, and more preferably 0.65 mass% or more.

[0024] (6)Cr≦6.60mass%: If the Cr content is excessive, the softening resistance decreases. That is, the surface of the die that is in contact with the molten metal during use as a die casting die becomes hot, and the surface of the die that is heated to a high temperature becomes easily softened. If the high-temperature strength decreases due to softening, the heat check resistance also deteriorates. In addition, the softening of the area exceeding the maximum hardness becomes noticeable, making it difficult to adjust the tempered hardness. This is because the hardness is sensitive to fluctuations in the furnace temperature.

[0025] Moreover, if the Cr content is excessive, the thermal conductivity decreases, which results in an increase in thermal stress and a deterioration in heat check resistance. Furthermore, when the Si content is 0.50 mass% or less, if the Cr content is increased, the machinability decreases significantly. Therefore, the Cr content must be 6.60 mass% or less, preferably 6.55 mass% or less, and more preferably 6.50 mass% or less. As described above, the refinement of the structure can be achieved by optimizing the Mn+Cr content, Mn / Cr, Mn content, and Cr content (see (5) in Table 1 and FIG. 2, which will be described later).

[0026] (7) Cu+Ni≦0.84mass%: As described above, in the present invention, the SA property, hardenability, and softening resistance are ensured by the balance of Cr and Mn (Cr amount, Mn amount, Mn+Cr amount, Mn / Cr ratio). In contrast, both Cu and Ni have the effect of increasing hardenability, but deteriorate the SA property. Furthermore, Cu and Ni do not have a significant effect on softening resistance, but rather have a noticeable adverse effect on the SA property. Also, when the amount of Cu is greater than that of Ni, the hot workability deteriorates. Therefore, the total amount of Cu and Ni is specified, and the upper limit of the total amount is specified to be within a range in which the effect on the hardenability and SA property is small.

[0027] Therefore, the Cu+Ni content must be 0.84 mass% or less. Since the Mn+Cr content required to ensure hardenability is 6.60 mass% or more, it is clear that if the Cu+Ni content is 0.84 mass% or less, it will not have a significant effect on hardenability. The Cu+Ni content is preferably 0.78 mass% or less, and more preferably 0.72 mass% or less.

[0028] (8) 0.01≦Si≦0.40mass%: If the amount of Si is too small, the machinability is reduced, making it difficult to machine large dies stably on an industrial scale. In particular, since the steel material of the present invention is intended for the manufacture of large dies, a large amount of material is cut, and good machinability is required. Therefore, the amount of Si must be 0.01 mass% or more. The amount of Si is preferably 0.03 mass% or more, and more preferably 0.05 mass% or more.

[0029] On the other hand, when the amount of Si is excessive, the number of coarse foreign matters may increase. This tendency is remarkable when the amount of C, V, and N is large. Also, pearlite is likely to precipitate during cooling after quenching. Furthermore, when the amount of Si is excessive, the decrease in thermal conductivity is remarkable. Therefore, the amount of Si must be 0.40 mass% or less. The amount of Si is preferably 0.37 mass% or less, and more preferably 0.35 mass% or less.

[0030] (9) 2.00≦Mo≦3.50mass%: If the Mo content is too small, pearlite is likely to precipitate during cooling after quenching. In addition, the degree of secondary hardening during tempering is reduced. Therefore, if the Mo content is too small, it is difficult to obtain a hardness of 45HRC or more when tempered at 560 to 600°C. In addition, softening resistance and high-temperature strength are insufficient, and heat check resistance may deteriorate. Furthermore, when the quenching rate is low, the amount of retained austenite increases. In addition, if the Mo content is too small, the creep strength also decreases. Therefore, the Mo content must be 2.00 mass% or more. The Mo content is preferably 2.05 mass% or more, and more preferably 2.10 mass% or more.

[0031] On the other hand, if the Mo content is excessive, the machinability decreases. In particular, when the Si content is small and the Mo content is excessive, the decrease in machinability is significant. Furthermore, if the Mo content is excessive, the fracture toughness may decrease. This tendency becomes evident when the Si content is large. Therefore, the Mo content must be 3.50 mass% or less. The Mo content is preferably 3.40 mass% or less, and more preferably 3.25 mass% or less.

[0032] (10) 0.001≦Al≦0.080mass%: The steel material according to the present invention has a significantly lower amount of C and V than the existing hot die steel (SKD61). Therefore, the amount of V-based carbides, carbonitrides, and nitrides that become pinning particles during quenching heating is smaller than that of SKD61. Therefore, in the present invention, AlN particles are also used in combination to suppress the growth of austenite grains. See (5) in Table 1 described later.

[0033] If the amount of Al is too small, it becomes difficult to reduce oxygen during refining, and oxides increase, which may result in a decrease in impact value. Also, if the amount of Al is too small, the amount of AlN that becomes pinning particles will be insufficient. As a result, austenite grains will become coarse during quenching heating, which may result in a decrease in impact value, fracture toughness, and / or ductility. Therefore, the amount of Al must be 0.001 mass% or more. The amount of Al is preferably 0.002 mass% or more, and more preferably 0.003 mass% or more.

[0034] On the other hand, if the amount of Al is excessive, the number of coarse alumina particles increases, and the impact value and fatigue strength may decrease. Also, the thermal conductivity may decrease, and the heat check resistance may deteriorate. Therefore, the amount of Al must be 0.080 mass% or less. The amount of Al is preferably 0.070 mass% or less, and more preferably 0.060 mass% or less. When Ca is added to improve machinability, the amount of Al is very important in optimizing the morphology of the compound.

[0035] (11) 0.003≦N≦0.040mass%: The steel material according to the present invention has a significantly smaller amount of C and V than existing hot die steel (SKD61). Therefore, the amount of V-based carbides that become pinning particles during quenching heating is smaller than that of SKD61. Therefore, in the present invention, N is added to increase the amount of V-based carbides, carbonitrides, and nitrides that become pinning particles, thereby suppressing the growth of austenite crystal grains. By adding N, AlN can also be used as pinning particles. See (5) in Table 1 described later.

[0036] If the amount of N is too small, the amount of AlN that serves as pinning particles will be insufficient. As a result, the austenite grains will become coarse during quenching heating, and the impact value, fracture toughness value, and / or ductility may decrease. Also, if the amount of N is too small, the amount of V-based carbonitrides and nitrides, which are also pinning particles, may also be insufficient. Therefore, the amount of N needs to be 0.003 mass% or more. The amount of N is preferably 0.004 mass% or more, and more preferably 0.005 mass% or more.

[0037] On the other hand, in order to add an amount of N that exceeds the amount that can be adjusted by normal refining, it is necessary to actively add N using dedicated equipment, which increases the material cost. In addition, if the amount of N is excessive, coarse crystallized products may increase. See (4) in Table 1 described later. This tendency becomes apparent when the amount of C, Si, and V is large. Furthermore, if the amount of N is excessive, coarse AlN may become excessively large, and the impact value may decrease. Therefore, the amount of N needs to be 0.040 mass% or less. The amount of N is preferably 0.038 mass% or less, and more preferably 0.036 mass% or less.

[0038] (12) Inevitable impurities: The steel material according to the present invention may contain unavoidable impurities. The elements that may be contained as impurities in the steel material according to the present invention and the contents thereof are as follows. P≦0.03mass%, S≦0.006mass%, O≦0.006mass%, W≦0.30mass%, Co≦0.30mass%, B≦0.0002mass%, Nb≦0.004mass%, Ta≦0.004mass%, Ti≦0.004mass%, Zr≦0.004mass%, Ca≦0.0005mass%, Se≦0.03mass%, Te≦0.005mass%, Bi≦0.01mass%, Pb≦0.03mass%, Mg≦0.02mass%.

[0039] In the present invention, the term "content" refers to the "average element content in the steel material" including areas with high segregation, areas with low segregation, and areas with average segregation. The method for evaluating the element content is as follows: (a) A method in which a predetermined mass of steel (preferably 1 gram or more per element to be analyzed) is dissolved in acid and analyzed; (b) A method of irradiating the surface of steel with X-rays etc.

[0040] [1.1.2. Sub-constituent elements] The steel material according to the present invention may further contain one or more of the following elements in addition to the above-mentioned main constituent elements and unavoidable impurities. The types of added elements, their component ranges, and the reasons for their limitations are as follows:

[0041] [A. Group A] (13)0.30 <W≦2.00mass%: The steel material according to the present invention has a smaller amount of C and V than conventional hot work die steels, and therefore may have insufficient strength depending on the application. In such cases, it is effective to add W to increase the strength. To obtain such an effect, the W content is preferably more than 0.30 mass%. The W content is more preferably 0.80 mass% or more.

[0042] On the other hand, if the W content is excessive, the material cost increases. In addition, segregation may become apparent, which may lead to deterioration of mechanical properties and increase in anisotropy. Therefore, the W content is preferably 2.00 mass% or less. The W content is more preferably 1.50 mass% or less.

[0043] (14)0.30 <Co≦1.00mass%: Co, like W, has the effect of improving strength. Therefore, when the strength is insufficient, it is effective to add Co to increase the strength. To obtain such an effect, the Co content is preferably more than 0.30 mass%. The Co content is more preferably 0.50 mass% or more.

[0044] On the other hand, if the amount of Co is excessive, the material cost increases. In addition, segregation may become apparent, which may lead to deterioration of mechanical properties and increase in anisotropy. Therefore, the amount of Co is preferably 1.00 mass% or less. The amount of Co is more preferably 0.90 mass% or less. The steel material according to the present invention may contain either Co or W, or may contain both.

[0045] [B. Group B] (15)0.0002 <B≦0.0080mass%: When the amount of P in steel is relatively high, P that segregates at the grain boundaries reduces the grain boundary strength and the impact value decreases. Adding B is effective in improving grain boundary strength. To improve grain boundary strength, B must exist alone (without forming a compound) in the steel. If B forms BN, the effect of adding B is lost. Therefore, when B is added to steel containing N in order to improve grain boundary strength, N must be combined with an element other than B.

[0046] Specifically, it is preferable to combine N with nitride-forming elements such as Ti, Zr, and Nb, which easily form nitrides. Although these elements are effective even when contained at the impurity level, when the amount is insufficient, it is preferable to add an amount exceeding the impurity level. In addition, BN has the effect of improving the machinability of steel. Therefore, when adding B for the purpose of improving machinability, it is not necessary to actively add nitride-forming elements to the steel.

[0047] In order to obtain the above-mentioned effects, the B content is preferably 0.0002 mass% or more, more preferably 0.0003 mass% or more, and even more preferably 0.0004 mass% or more. On the other hand, adding more B than necessary does not make a difference in effect and is of no practical benefit. Moreover, an excessive B content increases the cost of the steel material. Therefore, the B content is preferably 0.0080 mass% or less. The B content is more preferably 0.0075 mass% or less, and even more preferably 0.0070 mass% or less.

[0048] [C. Group C] (16)0.006 <S≦0.180mass%: (17)0.0005 <Ca≦0.0500mass%: (18)0.03 <Se≦0.50mass%: (19)0.005 <Te≦0.100mass%: (20)0.01 <Bi≦0.50mass%: (21)0.03 <Pb≦0.50mass%:

[0049] In the steel material according to the present invention, the addition of a free-cutting element is effective in improving the machinability. Specific examples of the free-cutting elements include S, Ca, Se, Te, Bi, and Pb. The steel material according to the present invention may contain any one of these free-cutting elements, or may contain two or more of them.

[0050] In order to obtain sufficient free-cutting properties, the content of each free-cutting element is preferably greater than the respective lower limit values ​​given above. On the other hand, if the free-cutting element content is excessive, the steel is more likely to crack during hot working. Also, if the free-cutting element content is excessive, the impact value, fatigue strength, heat check resistance, etc. may decrease. Therefore, the content of each free-cutting element is preferably equal to or less than the upper limit value mentioned above.

[0051] [D. Group D] (22)0.004 <Nb≦0.100mass%: (23)0.004 <Ta≦0.100mass%: (24)0.004 <Ti≦0.100mass%: (25)0.004 <Zr≦0.100mass%:

[0052] The steel material according to the present invention may contain an element that forms carbonitride other than V and Al to increase the amount of carbides, carbonitrides, and / or nitrides. Specific examples of the carbonitride-forming elements include Nb, Ta, Ti, and Zr. The steel material according to the present invention may contain any one of these carbonitride-forming elements, or may contain two or more of them.

[0053] In order to suppress excessive grain growth of austenite grains, the content of each carbonitride-forming element is preferably higher than the above-mentioned lower limit. On the other hand, if the content of the carbonitride-forming elements is excessive, carbides, carbonitrides, and / or nitrides are crystallized in a coarse state during casting. The coarse crystallized particles do not disappear during homogenization heat treatment, SA, and quenching, but remain as foreign matter, causing a decrease in impact value and fatigue strength. Therefore, the content of each carbonitride-forming element is preferably equal to or less than the upper limit value described above.

[0054] [1.2. Steel characteristics] 1.2.1. Mass and size The steel material according to the present invention has a small amount of C and V, and an optimized amount of Mn and Cr, and is therefore less susceptible to large inclusions and to a slow cooling rate and a slow quenching rate after hot working. In other words, even if the steel material according to the present invention is large in mass and size, it can achieve a high level of compatibility in five properties, namely, SA property, machinability, impact value, heat check resistance, and softening resistance.

[0055] For example, by optimizing the composition and manufacturing conditions of a steel material, it is possible to obtain a steel material that has a mass of 3000 kg or more in addition to achieving a practical level for all of the above five characteristics. By further optimizing the composition and manufacturing conditions of the steel material, it is possible to produce a steel material with a mass of 4000 kg or more, or even 5000 kg or more.

[0056] In addition, by optimizing the composition and manufacturing conditions of the steel material, in addition to having the above characteristics, the minimum size (Lmin By further optimizing the composition and manufacturing conditions of the steel material, it is possible to obtain a steel material with a L min It is also possible to manufacture steel materials with a thickness of 350 mm or more, or 400 mm or more. Here, the "vertical dimension (L1)", "horizontal dimension (L2)", and "height dimension (L3)" refer to the lengths of the three sides of the rectangular parallelepiped with the smallest volume that circumscribes the steel material.

[0057] 1.2.2. Hardness In the present invention, "hardness of steel material" means (a) A test piece was cut from near the center of the cross section of the steel material that had been subjected to SA (the area with the slowest solidification rate). (b) Rockwell B scale hardness measured at room temperature using the test piece This refers to.

[0058] For example, if the steel material is a block material of a [mm] × b [mm] × c [mm] (a≦b≦c, a≧300 mm), a first blank of a size of a [mm] × b [mm] × d [mm] is cut out from the end face in the c-axis direction. d is not particularly limited, but is preferably 30 to 70 mm. Next, a second material with e [mm] × f [mm] × d [mm] is cut out from approximately the center of the ab surface of the first material. The values ​​of e and f are not particularly limited, but e = 90 to 120 mm and f = 130 to 160 mm are preferable. Furthermore, a test piece for hardness measurement is cut out from the second material, and the hardness is measured using this.

[0059] When the steel material according to the present invention is subjected to SA under suitable conditions, the hardness of the steel material is appropriately reduced, making it possible to machine it. When the composition and manufacturing conditions of the steel material (particularly the SA conditions) are optimized, the hardness at room temperature becomes 98HRB or less. When the composition and / or manufacturing conditions of the steel material are further optimized, the hardness at room temperature becomes 97HRB or less, or 96HRB or less.

[0060] [1.2.3. Impact value] In the present invention, the "impact value of steel" means (a) A square bar (12 mm x 12 mm x 55 mm) was cut from near the center of the cross section of the steel material that had been subjected to SA (the area with the slowest solidification rate). (b) The square bar is heat treated to temper it to 44.5 to 45.5 HRC, (c) preparing an impact test specimen from the tempered square bar; (d) Impact value obtained by conducting an impact test at 15 to 35°C This refers to.

[0061] The cutting position of the square bar is the same as that of the test piece for hardness measurement, that is, the square bar is cut out from the second material described above.

[0062] "Heat treatment" for tempering square bars is, (a) After holding the square bar at 970°C for 2 hours, it is cooled from 970°C to 500°C at 6°C / min, from 500°C to 180°C at 0.5°C / min, and from 180°C to below 100°C at any desired cooling rate. (b) Then, heat treatment is performed at least once, with one cycle of heating to a temperature range of 560°C to 600°C and cooling to below 100°C. This refers to processing.

[0063] The "impact test piece" is a test piece conforming to JIS Z2242 (10 mm x 10 mm x 50 mm, arc radius of the notch tip: 1 mm, notch depth: 2 mm, cross-sectional area of ​​the test piece at the bottom of the notch: 0.8 cm 2 ) Impact value (J / cm 2 ) is the absorbed energy [J] relative to the cross-sectional area (0.8 [cm 2 ]) Average impact value (J / cm 2 )" refers to the average impact value of 10 or more (preferably 10 to 20) impact test pieces. "Low impact value rate (%)" refers to the percentage of impact test pieces with an impact value of 20 [J / cm 2 [0] is the percentage of the number (n) of impact test pieces (= n × 100 / n0) that is less than

[0064] In the steel material according to the present invention, by optimizing the composition and manufacturing conditions, a steel material can be obtained that exhibits a high impact value despite its large size and has a small variation in the impact value. Specifically, by optimizing the composition and manufacturing conditions, the average impact value is 25 [J / cm 2 ] or more and a low impact value rate of 30% or less can be obtained. Further optimization of the composition and manufacturing conditions resulted in an average impact value of 26 [J / cm 2 ] or more, or 27 [J / cm 2 ]That's all. Furthermore, by further optimizing the composition and manufacturing conditions, the low impact value rate can be reduced to 20% or less, or even 10% or less.

[0065] [1.2.4. Prior austenite grain size] The "prior austenite grain size" of steel is (a) Prepare an impact test piece or a test piece heat-treated under the same conditions; (b) Etching the test piece to reveal prior austenite grain boundaries, or by identifying prior austenite grain boundaries through crystal orientation analysis; (c) Observe the test piece at a magnification such that 50 or more grains are included in one field of view, and calculate the circle equivalent diameter of each prior austenite grain included in the field of view. This refers to the value obtained by The "average prior austenite grain size" is defined as a grain size with a total area of ​​0.5 mm 2 This refers to the average grain size of all prior austenite grains contained in one or more fields of view that is equal to or greater than this value.

[0066] Since the steel material according to the present invention contains a relatively large amount of pinning particles, the austenite grains are less likely to coarsen during quenching heating. When the composition and manufacturing conditions of the steel material are optimized, the average prior austenite grain size becomes 150 μm or less. When the composition and manufacturing conditions of the steel material are further optimized, the average prior austenite grain size becomes 135 μm or less, or 120 μm or less.

[0067] [2. Mold] The die according to the present invention is made of the steel material according to the present invention and has the following characteristics.

[0068] 2.1. Mass and size The mold of the present invention may have a mass of 2000 kg or more. By further optimizing the composition and manufacturing conditions of the mold, it is possible to manufacture a mold having a mass of 3000 kg or more, or even 4000 kg or more.

[0069] In addition, when the composition of the mold and the manufacturing conditions are optimized, in addition to having the above characteristics, the minimum dimension (L' min By further optimizing the composition and manufacturing conditions of the mold, it is possible to obtain a mold having an L' of 250 mm or more. min It is also possible to manufacture dies having a diameter of 300 mm or more, or 350 mm or more. Here, "vertical dimension (L'1)," "horizontal dimension (L'2)," and "height dimension (L'3)" refer to the lengths of the three sides of the rectangular prism with the smallest volume that circumscribes the mold, respectively.

[0070] 2.2. Hardness In the present invention, the "hardness of the mold" means (a) A test piece is cut from the surface of the mold. (b) Rockwell C scale hardness measured at room temperature using the test piece This refers to. Alternatively, the surface of the mold may be evaluated on the Rockwell C scale using a portable hardness tester (hardness tester). Also, the hardness (e.g., Shore hardness) evaluated by the portable hardness tester (hardness tester) may be converted to Rockwell C scale hardness.

[0071] The mold according to the present invention can obtain high hardness even if the mass and size are relatively large. When the composition and manufacturing conditions of the mold are optimized, the hardness at room temperature is 38 to 48 HRC for the HT method. When the composition and manufacturing conditions of the mold are further optimized, the hardness at room temperature is 39 to 49 HRC, or 40 to 50 HRC. In the case of the PH method, the hardness at room temperature is 35 to 45HRC. If the composition of the mold and the manufacturing conditions are further optimized, the hardness at room temperature will be 34 to 44HRC or 33 to 43HRC.

[0072] [3. Steel manufacturing method] The method for producing a steel material according to the present invention comprises the steps of: (a) a first step of melting raw materials mixed to obtain a predetermined composition, refining the molten metal, and casting the molten metal into a mold; (b) a second step of homogenizing the ingot; (c) the third step of hot working the ingot after the homogenization heat treatment; It is equipped with:

[0073] For steel materials for HT method, after the third process, (d) a fourth step of normalizing the raw material after hot working, if necessary; (e) a fifth step of tempering the raw material as necessary; (f) the sixth step of performing spheroidizing annealing (SA) of the raw material; It is equipped with:

[0074] On the other hand, in the case of steel for the PH method, after the third process, (d) a fourth step of normalizing the raw material after hot working, if necessary; (e) a fifth step of tempering the raw material as necessary; (f) a sixth step of performing spheroidizing annealing (SA) of the raw material as necessary; (g) the seventh step of quenching and tempering the raw material as necessary; It is equipped with:

[0075] The sixth step is essential for steel materials used in the HT method. The SA treatment is used to refine the material to a hardness that allows machining. On the other hand, for dies used in the PH method, the SA treatment is performed as necessary. In the present invention, "spheroidizing annealing (SA)" means (a) Steel is placed in a furnace at A c3 Point -10℃~A c3 By heating the steel to a temperature of +50°C (hereinafter referred to as the "SA treatment temperature"), "carbides are dispersed in the austenite phase and the ferrite phase is very little or completely absent" and (b) Applying the slow cooling method or constant temperature holding method to steel materials having the above structure This refers to processing.

[0076] The SA treatment temperature depends on the composition of the steel material, but is often between 830 and 950°C. Whether the slow cooling method or the constant temperature holding method is used, the hardness of the steel material after SA is approximately 98HRB or less (approximately 240Hv or less), and it is in a soft state that allows easy rough processing (machining into the rough shape of a die by machining).

[0077] [4. Effect] [4.1. Background] In recent years, the size of castings has increased, and the die-casting dies used to manufacture these castings have also become larger. The reasons for this increase in size of castings are as follows: (a) The individual castings are getting larger; or (b) Parts that were previously manufactured by assembling multiple castings are now being cast in an integrated state. This is the reason.

[0078] For large die-casting dies, the weight of the die is 2000 kg or more, and the weight of the material used to manufacture the die is 3000 kg or more. The steel material used for large die-casting dies is required to be easy to cut (high machinability), to be resistant to cracks on the die surface (heat check), and to be resistant to large cracks. Large cracks are cracks that reach deep inside the mold, and the time when they occur marks the end of the mold's life. On the mold surface, heat checking can cause large cracks, so it is necessary to prevent both large cracks and heat checking.

[0079] In the present invention, in order to prevent large cracks, the C and V contents are reduced and the Mn and Cr contents are increased compared to existing steels. Furthermore, the components are further optimized based on the following three new perspectives. (a) Reduction of retained austenite by increasing Mo (b) Extension of creep rupture time by increasing Mo (c) Suppression of transformation heat by using low silicon The above three points are important for large molds weighing 2000 kg or more, but they were not recognized as issues for conventional molds, most of which were weighing less than 2000 kg. FIG. 1 shows a schematic diagram of the effects obtained by increasing Mo and decreasing Si.

[0080] [4.2. How to prevent major cracks] [4.2.1. Reduction of retained austenite] The retained austenite in the quenched structure transforms into martensite by sub-zero treatment. However, when steel containing retained austenite is tempered, the retained austenite transforms into bainite at high temperatures (>Ms point + 120°C). The coarse bainite structure transformed at high temperatures has a negative effect on impact value and fracture toughness.

[0081] In the past, it was believed that retained austenite would transform into martensite by tempering. Therefore, it was believed that even if retained austenite was present, there would be no problem with properties such as toughness if the steel was tempered. In contrast, in the present invention, it was discovered that tempered retained austenite transforms into bainite at high temperatures, and it was concluded that controlling the amount of retained austenite is important for preventing large cracks.

[0082] The amount of retained austenite increases as the quenching speed decreases. Therefore, the larger the size of the die-casting die, the more retained austenite there is. With the recent trend toward larger die-casting dies, it is expected that it will become important to reduce the amount of retained austenite as much as possible. The steel material according to the present invention is characterized in that the Mo content is increased compared to existing steels in order to reduce the amount of retained austenite.

[0083] [4.2.2. Extension of creep rupture time] In addition to impact value and fracture toughness, creep strength is expected to become important for large die casting dies. In die casting, solidification of large castings takes a long time, which leads to a long mold closing time. During the mold closing, the die is subjected to high loads at high temperatures with little fluctuation. This load can cause creep deformation, which can lead to large cracks in the die. The steel material according to the present invention is characterized in that the Mo content is increased compared to existing steels in order to extend the creep rupture time.

[0084] [4.2.3. Suppression of transformation heat] When austenite transforms into another phase, the crystal structure and thermal properties change, generating heat. This is called transformation heat. Transformation heat makes it difficult to lower the temperature of the steel material during quenching. Even during cooling, temperature increases and stagnation may occur. This tendency is particularly noticeable on the inside of large die-casting dies.

[0085] Transformation heat generation has a negative effect on the structure and properties. The reason is that diffusion-type transformation continues while the temperature rises or stagnates due to transformation heat generation. For example, in the case of bainite transformation with large transformation heat generation, the transformation proceeds at a higher temperature than in the case of small transformation heat generation. Therefore, it is difficult to obtain a fine structure. The steel material according to the present invention is characterized in that the Si content is reduced compared to existing steels in order to suppress transformation heat.

[0086] [4.2.4. Effect of low V and high Mo] In order to obtain a hardness of 45HRC or more, conventional steels such as SKD61 often have a content of 0.50≦V≦1.20mass% and 1.00≦Mo≦2.00mass%. When a heat check of a mold is welded and repaired with a bar or wire made from such steel, V-based carbides and carbonitrides crystallize in the weld. This is because the weld repair material solidifies from a molten state, and is the same phenomenon as crystallization during casting. The crystallized particles that crystallize during welding are smaller than those that crystallize during casting, but they can cause large cracks.

[0087] In contrast, the steel material according to the present invention has low V and high Mo (V≦0.30 mass%, 2.00 mass%≦Mo). Therefore, when this steel material is made into a bar, wire, or powder and used for welding repair or additive manufacturing, the above problems do not occur. This is because the V content is low. Moreover, the high Mo content makes it possible to stably obtain a hardness of 45HRC or more.

[0088] [4.3. Optimization of ingredients] The optimization of the components to suppress heat checking, prevent large cracks, improve SA properties, and improve machinability is described in detail below. Table 1 shows the effects of adjusting the elements in terms of suppressing heat checking and preventing large cracks.

[0089] [Table 1]

[0090] [4.3.1. Suppression of heat checks] The prevention of heat checking is an effect that can be achieved by reducing thermal fatigue, which requires lowering the thermal stress generated in the die and at the same time increasing the die's resistance to thermal stress.

[0091] In order to reduce thermal stress, it is effective to increase the thermal conductivity of the steel material. In the present invention, the thermal conductivity is increased by the following method. (a) Reduce the amount of Si. (b) The amounts of Mn and Cr are not increased excessively.

[0092] In order to increase the resistance, it is effective to increase the high-temperature tensile strength and softening resistance. In the present invention, the high-temperature tensile strength and softening resistance are increased by the following method. (a) Reduce the amount of Si. (b) Increase the amount of Mo. (c) The amount of Cr is not excessively increased.

[0093] [4.3.2. Prevention of large cracks] Prevention of large cracks is an effect achieved by suppressing the initiation and progression of cracks. In order to suppress the initiation and progression of cracks, it is necessary to increase the impact value, fracture toughness, and resistance to high temperature and long-term loads. To increase the impact value and fracture toughness, it is effective to reduce coarse inclusions and at the same time make the structure finer. In the present invention, the term "coarse foreign matter" refers to large particles having a size exceeding 0.5 μm that are detrimental to the impact value and fracture toughness. Coarse foreign matter is roughly divided into the following two types depending on its origin. (4a) Crystallization during ingot solidification: Size is approximately 5 to 150 μm (4b) Precipitates formed after hot working: Size is approximately 0.5-10 μm

[0094] In the present invention, the amount of coarse foreign matter is reduced by the following method. (a) Reduce the amounts of C and V. (b) Do not increase the amount of Si or N excessively. The C and V contents were adjusted because many of the foreign matter contains C or V. The Si and N contents were adjusted because they affect the amount of foreign matter and are also constituent elements of the foreign matter.

[0095] The refinement of the structure was achieved by optimizing the following six factors (a) to (f). In addition, (a) and (b) show the refinement of austenite grains during quenching heating. (c)(d)(e) suppression of phase transformation behavior during quenching and cooling; (f) shows the structure after quenching. This is regarding.

[0096] (a) Austenite memory during quenching heating: "Austenite memory" refers to the phenomenon that the position of austenite grain boundaries during quenching heating (> Ac3 point) is almost the same as the position of prior austenite grain boundaries before heating (< Ac1 point). That is, the prior austenite grain size hardly changes before and after quenching. When the prior austenite grains before quenching are coarse, they hardly refine during quenching heating, and the prior austenite grains of the quenched material remain as coarse as before quenching.

[0097] Austenite memory is likely to occur when bainite or martensite exists in SA materials. For example, it is the case where the untransformed austenite remaining at the time of furnace discharging by the slow cooling method or the isothermal holding method becomes bainite or martensite by rapid cooling after furnace discharging. That is, austenite memory is likely to occur in steel materials with "high hardenability but poor SA property". In order to avoid austenite memory, mainly, the Mn / Cr ratio, Ni content, and Cu content were optimized to ensure SA property while maintaining high hardenability.

[0098] (b) Pinning particles dispersed in austenite during quenching: During quenching heating, the fine austenite grains obtained by avoiding austenite memory are likely to coarsen during holding at the heating temperature. The pinning particles present during quenching suppress the coarsening of austenite grains. In the present invention, mainly, the C content, V content, Al content, and N content were optimized to optimize the amount of pinning particles. Preferred particles dispersed in the quenched structure are small particles with a size of 0.5 μm or less, at most 1 μm or less. The size is the length measured in the direction in which the length of the particle is maximized.

[0099] (c) Pearlite precipitation during quenching cooling: When pearlite precipitates during quenching and cooling, the quenched structure is in a state where pearlite is dispersed in the parent phase of bainite or martensite. Since pearlite is coarser and has lower strength than the parent phase, it can cause large cracks during use of the die. In the present invention, the amounts of Si, Mn, and Mo are mainly optimized to suppress the precipitation of pearlite.

[0100] (d) Low temperature hardenability capable of producing martensite or bainite transformed at low temperatures: The higher the hardenability in the low temperature range, the more the formation of coarse bainite is suppressed. In the present invention, the Mn+Cr content is mainly optimized in order to improve the hardenability in the low temperature range.

[0101] (e) Heat generation during transformation into bainite and martensite: In particular, in large steel products, the smaller the transformation heat generation, the finer the structure after quenching. In the present invention, the Si content is mainly optimized in order to suppress the transformation heat generation.

[0102] (f) Amount of retained austenite in hardened structure: The retained austenite in the quenched structure is transformed into coarse bainite at high temperatures by tempering. In a structure in which coarse bainite regions exist, cracks tend to grow. In the present invention, the amount of Mo is mainly optimized in order to reduce the amount of retained austenite.

[0103] "To withstand high temperature and long-term load" means to extend the creep rupture time. In other words, it is necessary that the material is resistant to rupture even if a high load is applied to the material at high temperature for a long period of time with little fluctuation. In the present invention, the Mo content is mainly optimized to extend the creep rupture time.

[0104] [4.3.3. SA property] It is preferable that the steel material used in the HT method has excellent SA properties. When the hardenability is increased by increasing the amount of Mn, Ni, or Cu, the SA properties deteriorate. Since the steel material according to the present invention also needs high hardenability, good SA properties are ensured by the following method. (a) Do not increase Mn excessively. (b) Optimize the Mn / Cr ratio. (c) Lower the upper limits of Ni and Cr. In addition, improved SA properties can avoid the austenite memory phenomenon that occurs during quenching and heating, which also contributes to grain refinement.

[0105] 4.3.4. Machinability It is preferable that both the steel material used in the HT scheme and the steel material used in the PH scheme have excellent machinability. If the amount of Si is reduced to suppress heat checking, the machinability will deteriorate. Since it is also necessary to suppress heat checking in the steel material according to the present invention, the following method was used to ensure machinability that allows industrial cutting. (a) The amount of Si is not reduced excessively. (b) The Cr and Mo contents should not be increased excessively. EXAMPLES

[0106] [1. Various verification tests] [1.1. Suitable range of Mn and Cr contents] [1.1.1. Overview] In large die-casting dies, the hardening speed is slow. In particular, inside the die, the cooling rate from 500°C to 180°C can be 1.5°C / min or less. Even under these conditions, high hardenability is required to transform into martensite or bainite at low temperatures (≦Ms point + 120°C) to create a fine structure.

[0107] Increasing the Mn and Cr contents improves hardenability, but increasing the Mn content reduces SA properties. In particular, high SA properties are required for steel materials used in HT processes. Therefore, in the present invention, hardenability was investigated with respect to the Mn content and the Mn+Cr content, and SA properties were investigated with respect to the Mn / Cr ratio, aiming to achieve both hardenability and SA properties. Furthermore, softening resistance (Cr content) was also taken into consideration when determining the preferred range.

[0108] [1.1.2. Sample preparation and test methods] The composition of the steel (mass%) was 0.32C-0.34Si-0.08Cu-0.11Ni-2.16Mo-0.18V-0.028Al-0.011N, and the Mn and Cr contents were systematically changed. The steel was cast into an ingot weighing 150 kg. The ingot was subjected to homogenization heat treatment, hot working, normalizing, tempering, and SA.

[0109] The obtained steel materials were used to evaluate the SA properties. That is, a test piece for evaluating SA properties measuring 12 mm x 12 mm x 20 mm was prepared from the steel material after the SA. This test piece was subjected to a vacuum heat treatment simulating the "hot working - normalizing - tempering - spheroidizing annealing" process in the manufacturing process of large mold materials, and the SA properties were evaluated. Note that in this verification, normalizing and tempering were performed, but these processes may be omitted.

[0110] The details of the vacuum processing step are as follows. First, the test piece was placed in a vacuum and held at 1240℃ for 0.5 hours. This was a treatment to reproduce the coarse crystal grains of hot-worked material. After holding at 1240℃ for 0.5 hours, nitrogen gas was introduced into the furnace and the nitrogen gas was pressurized to cause forced convection, and the test piece was cooled to below 100℃.

[0111] The test piece was then placed in a vacuum and held at 1020℃ for 1 hour, simulating normalizing. After holding at 1020℃ for 1 hour, nitrogen gas was introduced into the furnace, and the nitrogen gas was pressurized to create a forced convection, and the test piece was cooled to below 100℃. The test pieces were then placed in a vacuum and held at 680°C for 6 hours, simulating tempering. After holding at 680°C for 6 hours, nitrogen gas was introduced into the furnace, and the nitrogen gas was pressurized to create a forced convection, cooling the test pieces to below 100°C.

[0112] Finally, SA was performed. That is, the test piece was kept at 900°C for 1H in a vacuum. After that, it was cooled to 600°C at 15°C / H while still in the vacuum. After that, nitrogen gas was introduced into the furnace, and the nitrogen gas was pressurized to cause forced convection, and the test piece was cooled to below 100°C.

[0113] In addition, the hardenability was evaluated using the obtained steel material. That is, ten square bars of 12 mm x 12 mm x 55 mm were made from the round bars in the SA state. These square bars were held at 970°C for 2 hours in a vacuum, and then quenched. The cooling rate during quenching was 6°C / min from 970°C to 500°C, and 0.5°C / min from 500°C to 180°C.

[0114] The above quenching process is one example assuming the slowest cooling rate inside when quenching a large mold weighing 2000 kg or more. The cooling rate from 180°C to 100°C was not specifically controlled because the cooling rate below 180°C does not have much effect on the impact value. Next, the square bars were tempered by holding them at 590°C for 2H and then cooling them to 100°C or lower. Furthermore, tempering was added. That is, the square bar was held at 560° C. to 600° C. for a predetermined time, and then cooled to 100° C. or less. This treatment was carried out one or more times, and the square bar was tempered to 44.5 to 45.5 HRC.

[0115] Impact test specimens were prepared from square bars tempered to 44.5 to 45.5 HRC. The shape of the impact test specimen conformed to JIS Z2242 (10 mm × 10 mm × 50 mm, arc radius at the tip of the notch: 1 mm, notch depth: 2 mm, cross-sectional area of ​​the test specimen at the bottom of the notch: 0.8 cm2). 2 Using the obtained impact test pieces, an impact test was carried out at 15 to 35°C. The impact value was used for the evaluation. The impact value [J / cm 2 ]" is the absorbed energy [J] at the cross-sectional area of ​​0.8 cm2 below the notch bottom of the test specimen. 2 This is the average value of 10 pieces.

[0116] [1.1.3. Results] Figure 2 shows the range of Mn and Cr content required to obtain steel with excellent SA and hardenability. The hatched area in Figure 2 shows the area where the hardness after SA is 98HRB or less and the impact value after quenching and tempering is 25J / cm. 2 This represents a region where the softening resistance is high.

[0117] [1.2. Suitable Mo content (1): Amount of retained austenite] [1.2.1. Sample preparation and test method] The composition (mass%) of the steel was 0.32C-0.28Si-0.81Mn-0.11Cu-0.23Ni-6.22Cr-0.22V-0.017Al-0.012N, and the amount of Mo was varied in the range of 0.51mass% to 3.06mass%. These steels were cast into ingots of 150 kg. The obtained ingots were subjected to homogenization heat treatment, hot working, normalizing, tempering, and SA.

[0118] A round bar with a diameter of 12 mm and a length of 50 mm was prepared from the material after SA (a rectangular material with a cross section of 40 mm x 65 mm). The cooling process for quenching the round bar to 970°C was divided into two types. The first process involves heating at 970°C for 2 hours, followed by cooling at 100°C / min to 500°C and 20°C / min from 500°C to 180°C. The second process involves heating at 970°C for 2 hours, followed by cooling at 6°C / min to 500°C and 0.5°C / min from 500°C to 180°C. The cooling rate of 500°C or less simulates the center of a mold. 20°C / min (first process) simulates the hardening of a small mold weighing about 5 kg. 0.5°C / min (second process) simulates the hardening of a large mold weighing more than 2000 kg. Test pieces were cut from the above hardened round bar, and the amount of retained austenite was measured.

[0119] [1.2.2. Results] Figure 3 shows the relationship between the amount of retained austenite and the amount of Mo. When the cooling rate was 20°C / min, the amount of retained austenite was small, at about 5%, and the effect of the amount of Mo was also small. On the other hand, when the cooling rate was 0.5°C / min, the amount of retained austenite was large. In particular, when the Mo content was small, the amount of retained austenite reached 20%. Furthermore, when the Mo content was 2 mass% or more, the amount of retained austenite was significantly reduced even when the cooling rate was 0.5°C / min. In other words, when targeting large dies with slow quenching rates, it was found that in order to reduce the amount of retained austenite, the Mo content should be set to 2.00 mass% or more.

[0120] [1.3. Suitable Mo content (2): Creep rupture time] [1.3.1. Sample preparation and test method] The material after SA was prepared in the same manner as in [1.2.1.]. A round bar with a diameter of 18 mm and a length of 100 mm was prepared from the material after SA. The round bar was heated at 970°C for 2 hours, and then quenched by cooling down to 500°C at 6°C / min, and then from 500°C to 180°C at 0.5°C / min. It was then allowed to cool to below 100°C, after which it was tempered multiple times at 560°C to 600°C, and tempered to 45HRC. A creep test specimen with a total length of 70 mm, a diameter of the parallel part of 6 mm, and a length of the parallel part of 30 mm was prepared from the round bar after the tempering. A load of 1000 MPa was applied to this test specimen at 500°C, and the judgment time was evaluated.

[0121] [1.3.2. Results] The relationship between creep rupture time and Mo content is shown in Figure 4. The higher the Mo content, the longer the creep rupture time. Moreover, when the Mo content was approximately 2.0 mass% or more, a stable long rupture time was achieved. In other words, in cases where a high load continues to act for a long period of time at high temperatures with little fluctuation, such as in die-casting dies for producing large castings, it was found that a Mo content of 2.00 mass% or more is sufficient to prevent destruction.

[0122] [1.4. Suitable Si content (1): Fracture toughness] [1.4.1. Sample preparation and test methods] The composition (mass%) of the steel material was 0.34C-0.86Mn-6.33Cr-0.22V-0.018Al-0.011N, and the Mo content was 1.21mass% or 2.83mass%. The Si content was changed in the range of 0.05mass% to 0.96mass%. These steel materials were cast into ingots of 150 kg. The obtained ingots were subjected to homogenization heat treatment, hot working, normalizing, tempering, and SA.

[0123] Plates with a height of 13 mm, width of 62 mm, and length of 65 mm were made from the material after SA (a rectangular material with a cross section of 40 mm x 65 mm). The plate was heated at 970°C for 2 hours, and then quenched by cooling at 6°C / min to 500°C, and then at 0.5°C / min from 500°C to 180°C. It was then allowed to cool naturally until it reached 100°C or below, after which it was tempered multiple times at 560°C to 600°C and tempered to 43HRC. A fracture toughness test piece having a thickness of 12.5 mm, a width of 61 mm, and a length of 64 mm was prepared from the tempered plate material. The fracture toughness of this test piece was measured at room temperature.

[0124] [1.4.2. Results] The relationship between fracture toughness and the Si content is shown in Figure 5. When the Si content was 0.96 mass%, increasing the Mo content from 1.21 mass% to 2.83 mass% reduced the fracture toughness. Although not shown, it is known that the fracture toughness is extremely reduced when the Mo content is 3.5 mass% or more.

[0125] On the other hand, even when the Mo content was 2.83 mass%, the fracture toughness increased when the Si content was reduced. In particular, when the Mo content was 2.83 mass%, and the Si content was 0.40 mass% or less, the fracture toughness value became equivalent to that of the test piece with a Mo content of 1.21 mass%. In other words, when targeting large dies with slower quenching rates and increasing the Mo content from the standpoint of the amount of retained austenite and creep strength, it was found that fracture toughness can be ensured by keeping the Si content at 0.40 mass% or less.

[0126] [1.5. Suitable Si content (2): High-temperature tensile strength] [1.5.1. Sample preparation and test methods] The material after SA was prepared in the same manner as in [1.4.1.]. A round bar with a diameter of 18 mm and a length of 105 mm was prepared from the material after SA. The round bar was heated at 970°C for 2 hours, and then quenched by cooling at 6°C / min to 500°C, and then at 0.5°C / min from 500°C to 180°C. It was then allowed to cool naturally until it reached 100°C or below, after which it was tempered multiple times at 560°C to 600°C, and tempered to 45HRC. A tensile test piece with a total length of 100 mm, a diameter of the parallel part of 8 mm, and a length of the parallel part of 40 mm was prepared from the round bar after the tempering. A tensile test was performed at 600°C using this test piece.

[0127] [1.5.2. Results] Figure 6 shows the relationship between high-temperature tensile strength and Si content. It was found that the lower the Si content, the higher the high-temperature tensile strength. It was found that a stable high-temperature tensile strength can be achieved when the Si content is approximately 0.4 mass% or less. Furthermore, it was found that even when the Mo content is high, the high-temperature tensile strength can be increased by reducing the Si content. In other words, when increasing the Mo content, it was found that the high-temperature tensile strength can be effectively increased by simultaneously reducing the Si content (Si≦0.40 mass%).

[0128] [1.6. Suitable Si content (3): Softening resistance] [1.6.1. Sample preparation and test methods] The material after SA was prepared in the same manner as in [1.4.1.]. A block of 11 mm height, 12 mm width, and 20 mm length was prepared from the material after SA. The block was heated at 970°C for 2 hours, and then quenched by cooling down to 500°C at 6°C / min, and from 500°C to 180°C at 3°C / min. It was then allowed to cool naturally until it reached 100°C or below, after which it was tempered multiple times at 560°C to 600°C and tempered to 45HRC. The cooling rate of 3°C / min below 500°C is assumed to be for the surface of a large mold weighing more than 2000 kg. Since the surface of the mold is where softening becomes an issue, we simulated quenching of the surface.

[0129] The tempered block material was heated to 580℃ in a vacuum furnace, held at 580℃ for 10 hours, and then cooled to room temperature. It took about 1 hour to cool from 580℃ to 150℃. At room temperature, the initial HRC hardness and the HRC hardness after heat treatment (H) were measured. The difference between the HRC hardness after heat treatment (H) and the initial HRC hardness (45HRC), ΔHRC (=H-45), was calculated and used as an index of softening resistance.

[0130] [1.6.2. Results] Figure 7 shows the relationship between softening resistance (ΔHRC) and the Si content. It was found that the lower the Si content, the smaller the absolute value of ΔHRC, i.e., the higher the softening resistance. It was found that a stable high softening resistance can be ensured when the Si content is approximately 0.4 mass% or less. Furthermore, it was found that softening resistance can be increased by reducing the Si content, even when the Mo content is high. In other words, when increasing the Mo content, it is possible to effectively increase softening resistance by simultaneously reducing the Si content (Si≦0.40 mass%). In addition, 0.96Si-1.21Mo in Fig. 7 is SKD61. The steel according to the present invention has lower C and V than SKD61, and in particular, the V content is low at 0.22 mass%, but the softening resistance is improved by using a low Si and high Mo system. The validity of low V and high Mo was confirmed.

[0131] It is known that reducing the amount of silicon, a solid solution strengthening element, reduces strength at room temperature. On the other hand, it has been found that reducing the amount of silicon increases high-temperature tensile strength and softening resistance. The reason for this is that reducing the silicon content suppresses the coarsening of carbides at high temperatures (the region between 450°C and Ac1 point).

[0132] [1.7. Suitable Si content (4): Preventing pearlite precipitation] [1.7.1. Sample preparation and test methods] The material after SA was prepared in the same manner as in [1.4.1.]. Test pieces with a diameter of 4 mm and a length of 10 mm were prepared from the material after SA. The test pieces were cooled uniformly from 970°C to below 100°C. The cooling rate was varied. The dimensional change of the test pieces during cooling was measured, and an attempt was made to detect expansion due to pearlite transformation. After cooling to room temperature, the structure was observed to confirm whether pearlite had precipitated. The critical cooling rate for pearlite precipitation was determined by the above procedure. In order to suppress pearlite precipitation, the lower the critical cooling rate, the better. The reason is that pearlite is less likely to precipitate even if cooled slowly, so this is suitable for large dies with slow quenching rates.

[0133] [1.7.2. Results] Figure 8 shows the relationship between the critical cooling rate for pearlite precipitation and the Si content. It was found that the lower the Si content, the smaller the critical cooling rate. It was found that a stable, small critical cooling rate can be ensured when the Si content is approximately 0.4 mass% or less. Furthermore, it was found that the critical cooling rate can be reduced by reducing the Si content, even when the Mo content is large.

[0134] When increasing the Mo content for large dies or steels for large dies in this way from the viewpoint of the amount of retained austenite and creep strength, the critical cooling rate can be effectively reduced by simultaneously reducing the Si content (Si≦0.40 mass%), that is, the precipitation of pearlite can be suppressed.

[0135] [1.8. Suitable Si content (5): transformation heat generation] [1.8.1. Sample preparation and test methods] The composition (mass%) of the steel was 0.35C-0.83Mn-0.07Cu-0.12Ni-6.28Cr-2.26Mo-0.24V-0.019Al-0.012N, and the Si content was 0.05mass% or 1.83mass%. These steels were cast into 10-ton ingots. The obtained ingots were subjected to homogenization heat treatment, hot working, normalizing, tempering, and SA.

[0136] A block with a height of 400 mm, width of 400 mm, length of 800 mm, and mass of approximately 1 ton was made from the steel after SA. A thermocouple was inserted into the center of the block to measure the temperature during vacuum quenching. Vacuum quenching was performed by heating the block to 970°C in a vacuum, introducing nitrogen gas into the furnace, pressurizing it to 10 Bar, and forcing the nitrogen gas into the furnace.

[0137] [1.8.2. Results] Figure 9 shows the temperature transition at the center of the block during rapid cooling. Stagnation and rise in temperature due to transformation heat (indicated by arrows in Figure 9) was confirmed. The amount of transformation heat also decreased as the Si content decreased. Meanwhile, the average cooling rate from 450°C to 200°C was approximately 3°C / min, regardless of the Si content in the block.

[0138] [1.9. Suitable Si content (6): Effect of transformation heat on impact strength] [1.9.1. Sample preparation and test methods] Impact value and fracture toughness are greatly affected by the cooling rate from temperature Ts to temperature Tf at 500°C or less. Ts and Tf vary depending on the steel type, but preliminary studies have shown that Ts = 450°C and Tf = 200°C for both of the two steel types evaluated. For this reason, the average cooling rate from 450°C to 200°C was evaluated. The region from Ts to Tf is the temperature range in which bainite transformation and martensitic transformation occur.

[0139] The vacuum-hardened block produced in [1.8.1.] was tempered multiple times at 560-600℃ to a hardness of 47HRC. When the structure near the center of the block after hardening was checked, no pearlite was found to have precipitated. This was because the cooling rate in the pearlite transformation region from 800℃ to 600℃ exceeded 5℃ / min. An impact test piece was prepared from the center of the block after the tempering. The test piece had dimensions of 10 mm square, length: 55 mm, notch bottom radius: 1 mm, and notch depth: 2 mm. The impact value at room temperature was measured using the obtained impact test piece.

[0140] [1.9.2. Results] When the Si content is 1.83 mass%, the impact value is 19 J / cm 2 On the other hand, when the Si content was 0.05 mass%, the impact value was 34 J / cm 2 It was. The block is not very large, weighing about 1 ton, and the hardening speed is high due to the powerful cooling of 10 Bar. In addition, the steel material evaluated has high hardenability (high Mn + Cr content). For these reasons, it is believed that the impact value of the 0.05% Si material was high. On the other hand, the 1.83% Si material had a lower impact value, even though the quenching speed and hardenability were almost the same as those of the 0.05% Si material.

[0141] From the above results, it was found that even if the average cooling rate in the bainite transformation region is the same, the impact value of steel with small transformation heat generation is higher than that of steel with large transformation heat generation. It is thought that the effect of transformation heat generation becomes more significant in large dies that are difficult to cool. Therefore, it was found that in order to stably obtain high impact values ​​with large dies, it is necessary not only to improve hardenability but also to suppress transformation heat generation.

[0142] [1.10. Simulation of transformation heat in a large mold] Test method In the HT method for hardening a large die, and in the PH method for hardening a large die steel, the delay in cooling due to transformation heat becomes apparent. This phenomenon, which is difficult to conduct experiments, was estimated by simulation. The subject was the hardening of a large mold steel material in the PH method. The steel material was SKD61. The size of the steel material was thickness: 700mm, width: 1000mm, length: 2300mm, and the mass of the steel material was approximately 12.5 tons. Vacuum hardening of this steel material from 1030℃ (nitrogen gas pressure: 10 Bar) was simulated.

[0143] [1.10.2. Results” Fig. 10 shows a hardening simulation of a 12.5 ton block of SKD61. A significant delay in cooling due to transformation heat was predicted around 400°C. If existing steel is applied to a large mold, in addition to low hardenability, large transformation heat will occur, so the impact value is expected to be very low.

[0144] [2. Verification tests of phenomena that actually occur in molds: Examples 1-16, Comparative Examples 1-6] [2.1. Overview] The object of the present invention is to "provide a steel material for dies with good manufacturability, and to provide a die with a long life made from the steel material." "Manufacturability" refers to SA property and machinability. "Long life" refers to the fact that heat checking is unlikely to occur and large cracks do not occur. Another problem that the present invention aims to solve is to "achieve the above even when the mass and size of the steel material are both large."

[0145] The following tests verify SA properties, machinability, heat check, large cracks, impact value, creep rupture time, and amount of retained austenite. A heat treatment process simulating a large mold weighing over 2000 kg is applied to a small piece of material. This allows us to verify the phenomena that actually occur in a large mold efficiently and accurately without using large pieces of material that are expensive and take a long time to manufacture.

[0146] 2.2. Sample preparation [2.2.1. Preparation of round bar material] Table 2 shows the compositions of the 22 types of steel (Examples 1 to 16 and Comparative Examples 1 to 6) used in the verification. Comparative Example 1 is SKD61. Comparative Examples 2 to 4 are commercially available steels that are improved versions of SKD61. Comparative Example 5 is a steel with lower C and Mo contents (C=0.17 mass%, Mo=0.51 mass%) than the steel according to the present invention. Comparative Example 6 is a steel with a higher V content (V=0.48 mass%) than the steel according to the present invention.

[0147] The steel types in Table 2 were each cast into 150 kg ingots, and through the first process of the HT plan, round bar material in an SA state with a diameter of 82 mm and a length of approximately 2,900 mm was produced. The SA process was carried out under appropriate conditions according to the composition of the steel. The heating temperature for SA was 920°C for Comparative Example 1, 880°C for Comparative Examples 2 to 4, 900°C for Comparative Examples 5 to 6, and 900°C for Examples 1 to 16. After holding at the above heating temperatures for 2H, the steel was cooled to 650°C at a rate of 10°C / H. Then, the steel was removed from the heat treatment furnace and allowed to cool.

[0148] [Table 2]

[0149] 2.2.2. Preparation of test specimens The following test pieces were prepared from the above round bar. (A) SA property: Test piece A, 12 mm x 12 mm x 20 mm (B) Machinability: Test piece B, 25mm x 50mm x 200mm (C) Heat check and rapid crack growth: φ72mm×50mm test piece C (D) Impact value: 11mm x 11mm x 55mm test piece D (E) Creep rupture time: φ18mm×100mm test piece E (F) Amount of retained austenite: φ10mm×20mm test piece F Test pieces C, D, and E were subjected to various evaluations after being heat-treated to 45HRC and machined to the specified shape. The other test pieces were subjected to various evaluations as they were.

[0150] [2.2.3. Test piece conditioning] Tempering was performed in a vacuum furnace. Test pieces C, D, and E were heated at the quenching temperature for 2 hours, then cooled to 500°C at 6°C / min, and quenched by cooling from 500°C to 180°C at 0.5°C / min. Test pieces C, D, and E were removed from the furnace when the temperature was below 180°C, and allowed to cool to below 100°C. The quenching temperature for Comparative Examples 1 to 4 was 1030°C, and for the others it was 970°C. After quenching, the test pieces were tempered to 45HRC by multiple tempering at 560 to 600°C.

[0151] 2.2.4. Machining of test specimens Specimens tempered to 45HRC were machined into shapes for characterization. A cylindrical specimen C2 with an approximate diameter of 70 mm and a diameter of 50 mm was prepared from specimen C. A V-notch was provided on one end of the cylinder. The notch depth was 1 mm, the notch opening angle was 120°, and the R of the notch tip was 0.4 mm. An impact test piece D2 measuring approximately 10 mm x 10 mm x 55 mm was prepared from the test piece D. A U-notch was provided in the center of the longitudinal direction. The notch depth was 2.0 mm, and the R of the notch tip was 1.0 mm. From test piece E, a creep test piece E2 was prepared, having a total length of 70 mm, a diameter of the parallel part of 6 mm, and a length of the parallel part of 30 mm.

[0152] [2.3. Test Method and Results] [2.3.1. Evaluation of SA] Using test piece A in the SA state, an experiment was conducted to simulate the manufacturing process from the hot working process in the "first step of the HT plan."

[0153] A vacuum furnace was used for the heat treatment. In order to simulate the coarse austenite grains that form during hot working, test piece A was heated to 1240°C for 2 hours. In order to simulate the grain boundary precipitation of carbides and other substances during cooling after hot working, the specimen was cooled from 1240°C to 650°C at a rate of 1°C / min. Nitrogen gas was introduced into the furnace for accelerated cooling below 650°C. The phenomenon simulated by this heat treatment is the grain boundary precipitation of coarse austenite grains and carbides, etc., and other conditions do not necessarily correspond to actual hot working processes.

[0154] After heat treatment simulating the hot working process, the normalizing and tempering processes were carried out, and then SA was carried out. The heating temperature for SA was the same as that used for producing the round bar material. Meanwhile, the cooling rate from the heating temperature for SA was set to 23°C / H. Softening to 98HRB or less at this high cooling rate is industrially essential in terms of productivity and cost. After holding at the specified temperature for 2 hours, the specimens were cooled to 650°C at a rate of 23°C / H, and accelerated cooling was performed below 650°C by introducing nitrogen gas into the furnace. After SA, the Rockwell B scale hardness was measured. For Comparative Example 4, the Rockwell C scale hardness was also measured.

[0155] Table 3 shows the hardness after SA. "S" indicates that the hardness after SA is 98HRB or less (good SA property), "D" indicates that the hardness after SA is more than 98HRB (poor SA property).

[0156] If untransformed austenite remains when the temperature reaches 650℃, the austenite will transform into martensite or bainite during the subsequent accelerated cooling, resulting in a hardness of over 98HRB. Such steel is considered to have poor SA properties. In Comparative Example 4, the Rockwell B scale hardness was rated D and the Rockwell C scale hardness was 29HRC. This is believed to be due to the high Mn / Cr ratio of 0.204. On the other hand, the other steel types that satisfied Mn / Cr≦0.150 had Rockwell B scale hardness of 98HRB or less and showed good SA properties.

[0157] [Table 3]

[0158] 2.3.2. Machinability evaluation Test piece B was cut. The cutting distance until the wear of the cutting tool reached 0.1 mm was taken as the tool life. The tool life corresponds to the machinability when rough machining a die material in SA state. A long cutting distance indicates a long tool life and good machinability.

[0159] Table 4 shows the cutting distance [m]. Table 4 also shows the ratio of the cutting distance of each steel material (hereinafter, also referred to as "relative cutting distance") when the cutting distance of SKD61 (Comparative Example 1) of 36.4 m is taken as 100%. "S" indicates that the relative cutting distance is 90% or more. "A" indicates that the relative cutting distance is 75% or more but less than 90%. "B" indicates that the relative cutting distance is 50% or more but less than 75%. "C" indicates that the relative cutting distance is 33% or more but less than 50%. "D" indicates that the relative cutting distance is less than 33%.

[0160] SKD61 (Comparative Example 1) had very good machinability. On the other hand, the steel grades rated D had machinability equivalent to less than 1 / 3 of that of SDK61, and are therefore not industrially acceptable. The 22 steel types evaluated did not include any steel types that were judged as D. It is known that machinability deteriorates when the Si content is low. Since the 22 steel types did not include any steel types with a Si content of less than 0.01 mass%, there were no steel types that were judged as D.

[0161] Although Examples 6 and 9 were rated C, they had industrially acceptable machinability. The Si content of Example 6 was 0.01 mass%, and that of Example 9 was 0.02 mass%. The Si content of Example 10 was 0.05 mass%, and the machinability was rated B. From the above results, it can be said that there are almost no problems with machinability if the Si content is 0.03 mass% or more. Since Examples 15 and 16 contain free-cutting components, their machinability was rated A or higher.

[0162] [Table 4]

[0163] [2.3.3. Heat Check Evaluation] A thermal cycle was applied to test piece C2, and the progression of the heat check that occurred was evaluated. The end face with the notch was repeatedly heated to 580°C using high frequency waves and cooled to 90°C using water jets. A combination of heating and cooling was considered one cycle. This evaluation simulated heating by molten metal in a die-casting mold and cooling by jetting mold release agent. The notch was modeled after a sharp corner on the mold surface that would become a stress concentration area.

[0164] Test piece C2, which had been subjected to 10 to 10,000 thermal cycles, was cut in the center and the crack at the bottom of the notch, i.e., the depth of the heat check, was measured. A graph was created with the number of thermal cycles on the horizontal axis and the crack depth on the vertical axis, and the number of thermal cycles at which the crack depth was 0.2 mm was determined by interpolation. A crack depth of 0.2 mm is the condition at which the transfer of cracks to the casting begins to become evident during die casting, and cracks begin to appear in penetrant testing. A large number of thermal cycles at which a crack depth of 0.2 mm is reached indicates that the occurrence and progression of heat checks is slow, and that heat check resistance is good.

[0165] Table 5 shows the number of cycles until the crack depth reached 0.2 mm. Table 5 also shows the percentage of the number of cycles for each steel material when 228 cycles for SKD61 (Comparative Example 1) is taken as 100% (hereinafter, this is also referred to as "relative number of cycles A"). "S" indicates that the relative cycle number A is greater than 190%; "A" indicates that the relative cycle number A is greater than 160% and less than or equal to 190%; "B" indicates that the relative cycle number A is greater than 130% and less than or equal to 160%; "C" indicates that the relative cycle number A is greater than 105% and less than or equal to 130%; "D" indicates that the relative cycle number A is 105% or less.

[0166] SKD61 (Comparative Example 1) had poor heat check resistance and was judged as D. On the other hand, the improved steels of SKD61 (Comparative Examples 2 to 4) had improved heat check resistance and were judged as B to C. Comparative Example 5 had poor heat check resistance and was judged as D. This is thought to be because the C content was smaller than that of the steel according to the present invention, and the Mo content was also smaller, so that the test piece surface softened significantly when heated to 580°C when the heat cycle was applied, and the reduced strength made heat checks more likely to occur.

[0167] The heat check resistance of Examples 15 and 16 was rated C, which was lower than that of the other Examples. This is believed to be because the compounds of the free-cutting components accelerated the initiation and propagation of cracks. The other examples had good heat check resistance, rated at B or higher. In particular, the three steel types of Examples 6, 9, and 10 had a Si content of 0.05 mass% or less, so their heat check resistance was rated S, indicating that they stably exhibited heat check resistance that was about 2 to 3 times that of SKD61. Furthermore, the examples with Si = 0.10 to 0.24 mass% were rated A, indicating that they exhibited heat check resistance nearly twice that of SKD61.

[0168] [Table 5]

[0169] [2.3.4. Evaluation of major cracks] In die-casting dies, once a crack has progressed to a certain depth, the rate of progression rapidly increases, leading to large cracks. A similar phenomenon was confirmed in the thermal cycle test described above. In a graph with the number of thermal cycles on the horizontal axis and the crack depth on the vertical axis, the slope of the graph changes suddenly at a certain number of thermal cycles. In the case of die-casting dies, this is a phenomenon that can lead to large cracks. The number of thermal cycles at which the slope of the graph changes suddenly was determined by interpolation, and this was used as an index of large cracks. A larger number of thermal cycles at which the slope of the graph changes suddenly indicates that it is less likely to lead to large cracks.

[0170] Table 6 shows the number of thermal cycles at which cracks begin to grow rapidly. Table 6 also shows the percentage of the number of cycles for each steel material (hereinafter, also referred to as "relative number of cycles B"), with 284 cycles for SKD61 (Comparative Example 1) taken as 100%. "S" indicates that the relative cycle number B is greater than 900%; "A" indicates that the relative cycle number B is more than 600% and less than or equal to 900%. "B" indicates that the relative cycle number B is more than 300% and less than or equal to 600%; "C" indicates that the relative cycle number B is more than 150% and less than or equal to 300%; "D" indicates that the relative cycle number B is 150% or less.

[0171] When a large mold is made with SKD61 (Comparative Example 1), the mold is prone to large cracks. In fact, the number of heat cycles for SKD61 is small at 284 cycles, which is a small increase from the 228 cycles in Table 5. This corresponds to the short time from when the heat check begins to be transferred to the casting to when large cracks occur. Comparative Example 2 has a 39% improvement in the relative cycle number B compared to SKD61 (Comparative Example 1), but considering that the variation in mold life due to large cracks is about 50%, this is not a significant improvement.

[0172] If the number of thermal cycles at which large cracks occur is stably around double, that is, the relative number of cycles B is 150 to 300%, it is judged to be a clear improvement effect. This condition was specified as judgment C. Examples 1 to 16 all exceeded judgment C and were judged to be judgment B or higher. Moreover, only Example 15 was judged to be judged B. The other examples were judged A or higher, and the number of thermal cycles at which large cracks occur was stably six times or more compared to SKD61. In particular, the number of thermal cycles for the examples judged S exceeded 10 times that of SKD61. Examples 1 to 16 suppress the rapid progression of cracks due to low thermal stress due to high thermal conductivity and fine structure due to high hardenability. Comparative Example 5, which was judged as D in Table 5, was judged as A for large cracks. This is thought to be because although the heat check resistance was poor due to the large softening, the progress of the cracks was suppressed due to the high thermal conductivity and high hardenability.

[0173] [Table 6]

[0174] [2.3.5. Evaluation of impact value] The impact value, which is sensitive to the presence or absence of foreign matter and the density of the structure, makes it easy to determine whether the components, manufacturing method, or heat treatment are appropriate. In fact, molds with long life have high impact values. For this reason, the impact value is sometimes specified as an acceptance condition for mold steels and molds. The impact test was carried out at room temperature using test piece D2. The absorbed energy [J] was calculated based on the cross-sectional area of ​​the notch (0.8 [cm 2 ] is the shock value.

[0175] The evaluation was done by averaging 10 test pieces for each steel type. The results are shown in Table 7. The absolute value of the impact value is more important than the ratio for a certain steel type. "S" is an impact value of 30 [J / cm 2 ] represents being beyond "A" is an impact value of 25 [J / cm 2 ]Super 30[J / cm 2 ] or less, "B" is an impact value of 23 [J / cm 2 ]Super 25[J / cm 2 ] or less, "C" is an impact value of 20 [J / cm 2 ]Super 23[J / cm 2 ] or less, "D" is an impact value of 20 [J / cm 2 ] or less.

[0176] Impact value is 20 [J / cm 2 ] or less, large cracks are likely to occur during use as a die. The impact value required for a die casting die is 25 [J / cm 2 The impact value is 30 [J / cm 2

[0043] The risk of large cracks is extremely low. In all of Examples 1 to 16, the impact value was graded B or higher.

[0177] Comparative Example 5 is a steel having a smaller amount of C and Mo than the steel material according to the present invention, and the impact value was judged to be C. Comparative Example 5 has a V content of 0.30 mass% or less, so there is little foreign matter, and a Mn+Cr content of 6.70 mass% or more, so the hardenability is also good. However, Comparative Example 5 has a small amount of C and a high transformation point, so the structure is coarse. Therefore, the impact value of Comparative Example 5 is insufficient.

[0178] Comparative Example 6 is a steel having a larger V content than the steel material according to the present invention, and the impact value was judged to be D. Comparative Example 6 has a Mn+Cr content of 6.70 mass% or more, and has high hardenability. However, Comparative Example 6 has a V content exceeding 0.30 mass%, and contains a large amount of foreign matter, so good hardenability cannot be achieved.

[0179] The impact values ​​of Comparative Examples 1 to 4 were judged to be D. This is because (a) The V content exceeds 0.30 mass% and there is a lot of foreign matter, and (b) The Mn + Cr content was less than 6.70 mass%, which resulted in poor hardenability and a coarse structure. It is thought that. In particular, SKD61 (Comparative Example 1) had the highest V content and the lowest Mn + Cr content, resulting in an impact value of 10 [J / cm 2 ] was a very low value.

[0180] [Table 7]

[0181] [2.3.6. Evaluation of creep rupture time] A creep test was carried out at 500°C using test piece E2. The load was 1000 MPa. Each steel type was evaluated using the average value of three test pieces. The results are shown in Table 8. Table 8 also shows the percentage of creep judgment time (hereinafter also referred to as "relative rupture time") for each steel material when 1.7H for SKD61 (Comparative Example 1) is taken as 100%. In Table 8, "S" indicates that the relative time to failure is greater than 300%. "A" indicates that the relative break time is more than 250% and less than or equal to 300%. "B" indicates that the relative break time is more than 200% and less than or equal to 250%; "C" indicates that the relative break time is more than 150% and less than or equal to 200%; "D" indicates that the relative time to failure is 150% or less.

[0182] The fracture time of SKD61 (Comparative Example 1) was short at 17 hours. In large molds, in addition to the tendency for cracks to grow rapidly (see Table 6) and the low impact value (see Table 7), it can also be said that it is prone to large cracks from the creep viewpoint. Comparative Example 2 was an improved version of SKD61, but had a rupture time equivalent to that of SKD61. Comparative Example 5 had a rupture time of only 65% ​​of that of SKD61.

[0183] If the fracture time is consistently nearly twice that of SKD61, i.e., 1.5 times or more, it is judged to have a clear improvement effect. This condition was specified as judgment C. Steel products whose fracture time is consistently more than twice that of SKD61 were specified as judgment B. Steel products whose fracture time is nearly three times that of SKD61, i.e., 2.5 times or more, show a significant improvement effect and were specified as judgment A. Furthermore, steel products whose fracture time is more than three times that of SKD61 were specified as judgment S.

[0184] All of Examples 1 to 16 exceeded the grade B and were graded at or above grade A. Moreover, only Examples 13 and 16 were graded A. All of the other Examples were graded S. The creep rupture time increases with increasing Mo content. None of the 22 steel types examined this time had a Mo content in the range of 1.25 to 2.00 mass%, so neither criteria B nor C were applicable.

[0185] [Table 8]

[0186] [2.3.7. Evaluation of retained austenite] Test piece F was heated at the quenching temperature for 15 minutes, then cooled to 500°C at 6°C / min, and cooled from 500°C to 180°C at 0.5°C / min. After that, it was removed from the furnace and allowed to cool. The quenching temperature for Comparative Examples 1 to 4 was 1030°C, and the rest were 970°C. After quenching, test piece F was cut in half near the center in the longitudinal direction, and the amount of retained austenite was measured on the cut surface with a diameter of 10 mm.

[0187] Table 9 shows the amount of retained austenite. There was a tendency that the worse the hardenability and the smaller the Mo content, the more the retained austenite. The amount of retained austenite in Comparative Examples 1 to 5 was 16% or more. In Comparative Example 6, the Mn+Cr content was 6.70 mass% or more, which gave high hardenability, and the Mo content was 2.00 mass% or more, so the amount of retained austenite was small at 13%. In contrast, the amount of retained austenite in Examples 1 to 16 was 16% or less.

[0188] [Table 9]

[0189] [2.3.9. Summary of Examples] The six properties are listed in Table 10. Comparative Example 1 (SKD61) had extremely high SA and machinability, and therefore was the most efficient for manufacturing dies. On the other hand, its performance as a die, such as heat checking, was insufficient. Comparative Examples 2 to 4, which are improved steels of SKD61, are steels with lower machinability than SKD61 and improved heat check resistance. However, they did not have the performance to stably prevent large cracks. Comparative Examples 5 and 6 have some elements different from the steel material of the present invention. Therefore, they could not exhibit sufficient performance in terms of heat checking and large cracks.

[0190] In contrast, Examples 1 to 16 were excellent in all properties, and the amount of retained austenite, which affects the impact value and creep rupture time, was small. That is, it was found that the steel material according to the present invention makes it easy to manufacture materials for dies and dies, and that dies manufactured from this steel have a long life.

[0191] [Table 10]

[0192] Although the embodiment of the present invention has been described in detail above, the present invention is not limited to the above embodiment, and various modifications are possible without departing from the gist of the present invention. [Industrial Applicability]

[0193] The steel material according to the present invention can be used as dies and parts thereof for use in various manufacturing methods such as casting, forging, hot stamping, extrusion, injection molding, and blow molding. Since the steel material according to the present invention has a low C and V content, when it is used in the form of powder, bar stock, or wire stock for additive manufacturing or welding repair, cracks in the molded object or welded joints can be avoided.

Claims

1. 0.23≦C≦0.39mass%, 0.03≦V≦0.30mass%, 6.60≦Mn+Cr≦7.40mass%, Mn / Cr≦0.150, Mn≧0.60mass%, Cr≦6.60mass%, Cu+Ni≦0.84mass%, 0.01≦Si≦0.40 mass%, 2.00≦Mo≦3.50mass%, 0.001≦Al≦0.080 mass%, and 0.003≦N≦0.040mass% The remainder of the steel material is Fe and unavoidable impurities.

2. The steel material according to claim 1, further comprising one or more groups selected from the following groups A to D: Group A: 0.30<W≦2.00 mass%, and 0.30<Co≦1.00mass% One or two types selected from Group B: 0.0002<B≦0.0080mass% Group C: 0.006<S≦0.180mass%, 0.0005<Ca≦0.0500mass%, 0.03<Se≦0.50mass%, 0.005<Te≦0.100mass%, 0.01<Bi≦0.50 mass%, and 0.03<Pb≦0.50mass% One or more selected from Group D: 0.004<Nb≦0.100mass%, 0.004<Ta≦0.100mass%, 0.004<Ti≦0.100 mass%, and 0.004<Zr≦0.100mass% One or more selected from

3. The mass is 3000 kg or more, Vertical dimension (L 1 ), horizontal dimension (L 2 ), and the height dimension (L 3 ) the smallest dimension (L min ) is 300 mm or more The steel material according to claim 1 or 2.

4. A die manufactured from the steel material according to claim 1 and having a mass of 2000 kg or more.

Citation Information

Patent Citations

  • Tool steel for hot work and steel product using the same

    JP2011001572A