toner
The toner formulation with polyester resin and hydrotalcite particles addresses paper discharge adhesion in high-speed continuous printing by maintaining charge stability and release properties, ensuring stable image quality and low-temperature fixability.
Patent Information
- Application Number
- JP2023082478
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-18
- Publication Date
- 2024-11-28
AI Technical Summary
Toner used in electrophotographic devices experiences paper discharge adhesion when printing solid images on both sides continuously at high speed, particularly due to heat and pressure causing image areas to adhere to each other or the paper.
A toner formulation comprising polyester resin with a specific structure and hydrotalcite particles as an external additive, where fluorine and aluminum are present inside the hydrotalcite, with a controlled F/Al ratio, to prevent adhesion by maintaining charge stability and release properties.
The toner effectively reduces paper discharge adhesion even in various environments, ensuring stable image quality during high-speed continuous printing on both sides without impairing low-temperature fixability.
Smart Images

Figure 2024165895000011 
Figure 2024165895000001 
Figure 2024165895000002
Abstract
Description
[Technical field]
[0001] FIELD This disclosure relates to toners for use in imaging processes such as electrophotography. [Background technology]
[0002] In recent years, electrophotographic image forming apparatuses such as copying machines and printers have been improved in terms of speed and life span, and there is a demand for toners that can provide stable image quality even during continuous printing at high speeds. In light of this, many toners have been proposed that contain hydrotalcite compounds as external additives, which contain multiple types of metal ions and thus can stably maintain the chargeability and transferability of the toner. For example, Patent Document 1 discloses a toner that contains at least a hydrotalcite compound as an external additive and can reduce fluctuations in image quality even during long-term continuous use. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2019-045578 A Summary of the Invention [Problem to be solved by the invention]
[0004] However, the inventors of the present invention have found that when solid images with a large toner load are continuously printed on both sides at high speed using the toner described in Patent Document 1, discharged paper tends to stick. It is believed that the heat and pressure of the paper causes image areas to stick to each other or image areas to paper to stick to each other as the paper is piled up on the discharge tray while still hot.
[0005] The present disclosure is directed to a toner that is less likely to cause discharge adhesion even when solid images are continuously printed on both sides at high speed in various environments. [Means for solving the problem]
[0006] The present disclosure relates to a toner having toner particles containing a binder resin and an external additive, The binder resin contains a polyester resin, The polyester resin contains a structure represented by the following formula (1) in an amount of 10.0 to 30.0% by mass, The external additive contains hydrotalcite particles, In a line analysis in a STEM-EDS mapping analysis of the toner, fluorine and aluminum are present inside the hydrotalcite particles, The toner has a ratio value F / Al of the atomic concentration of fluorine to aluminum in the hydrotalcite particles, which is obtained from main component mapping of the hydrotalcite particles by STEM-EDS mapping analysis of the toner, of 0.01 to 0.60. [ka] Effect of the Invention
[0007] According to the present disclosure, even when solid images are continuously printed on both sides at high speed in various environments, the paper can be discharged. It is possible to obtain a toner that is less susceptible to adhesion. [Brief description of the drawings]
[0008] [Figure 1] Schematic diagram of EDS line analysis in STEM-EDS mapping analysis DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] The present disclosure will be described in more detail below with reference to embodiments thereof, but is not limited thereto. In addition, the description of "XX or more and YY or less" or "XX to YY" representing a numerical range means a numerical range including a lower limit and an upper limit as endpoints, unless otherwise specified. When a numerical range is described in stages, the upper limit and the lower limit of each numerical range can be arbitrarily combined.
[0010] The present disclosure relates to a toner having toner particles containing a binder resin and an external additive, The binder resin contains a polyester resin, The polyester resin contains a structure represented by the following formula (1) in an amount of 10.0 to 30.0% by mass, The external additive contains hydrotalcite particles, In a line analysis in a STEM-EDS mapping analysis of the toner, fluorine and aluminum are present inside the hydrotalcite particles, The toner has a ratio value F / Al of the atomic concentration of fluorine to aluminum in the hydrotalcite particles, which is obtained from main component mapping of the hydrotalcite particles by STEM-EDS mapping analysis of the toner, of 0.01 to 0.60. [ka]
[0011] The toner makes it difficult for discharged paper to adhere to the paper even when solid images are continuously printed on both sides at high speed in various environments such as a normal temperature and normal humidity environment, a high temperature and high humidity environment, etc. The present inventors consider the mechanism by which such an effect is obtained as follows. One of the means for suppressing paper discharge adhesion is to use a binder resin that does not easily melt the toner due to heat. However, in recent years, there has been a high demand for energy saving in electrophotography, and toner that can be fixed at a lower temperature is required. Therefore, with the above-mentioned binder resin, there is a trade-off between paper discharge adhesion and low-temperature fixability. In other words, in order to suppress paper discharge adhesion without impairing low-temperature fixability, it is considered necessary for the toner to melt quickly in response to heat during fixing and to suppress adhesion by some method during paper discharge.
[0012] The structure represented by formula (1) contained in polyester resin has an electron-rich carbonyl structure. On the other hand, hydrotalcite particles contain divalent or trivalent electron-deficient metal ions. Since the length of the ethylene group in the structure represented by formula (1) is suitable for chelate coordination, it is believed that it can easily coordinate to the metal ions in the hydrotalcite particles.
[0013] For this reason, the hydrotalcite particles as an external additive interact with the structure of the toner particles shown in formula (1), making them less likely to migrate from the toner particle surface during the image formation process, with some remaining on the toner surface in the printed image area. Furthermore, the hydrotalcite particles contain fluorine inside, such as between layers, and it is believed that the fluorine parts that are partially exposed through the image formation process exhibit releasability to the overlapping paper and its image area after paper ejection, thereby suppressing paper ejection adhesion.
[0014] The toner particles contain a polyester resin as a binder resin. The polyester resin contains the structure represented by formula (1) in an amount of 10.0 to 30.0 mass % based on the mass of the polyester resin. The polyester resin preferably contains the structure represented by formula (1) in an amount of 15.0 to 25.0 mass %. When the polyester resin contains 10.0% by mass or more of the structure represented by formula (1), some hydrotalcite particles can remain on the toner surface even after paper discharge, which results in the effect of suppressing paper discharge adhesion. On the other hand, when the content of the structure represented by formula (1) is 30.0% by mass or less, paper discharge adhesion can be suppressed, and a toner having excellent heat-resistant storage stability can be obtained.
[0015] The structure represented by formula (1) is, for example, a structure obtained by condensation polymerization of ethylene glycol in a polyester resin. To obtain a polyester resin containing the structure represented by formula (1), ethylene glycol may be used as a monomer during resin synthesis, or a recycled PET oligomer produced by recycling may be used. The carboxylic acid monomer is not particularly limited, but it is preferable to use terephthalic acid, isophthalic acid, succinic acid, adipic acid, fumaric acid, trimellitic acid, etc.
[0016] In the case of a structure in which methanediol or propanediol is condensed, rather than the structure represented by formula (1), it is considered that the structure is difficult to chelate with the metal ions in the hydrotalcite particles, and therefore adhesion during discharge cannot be suppressed.
[0017] The toner contains hydrotalcite particles as an external additive. The hydrotalcite particles may be those represented by the following structural formula (2): 2+ y M 3+ x (OH)2A n- (x / n) ·mH2O formula (2) where 0 <x≦0.5、y=1-x、m≧0である。 M 2+ , and M 3+ represent divalent and trivalent metals, respectively. M 2+ is preferably at least one divalent metal ion selected from the group consisting of Mg, Zn, Ca, Ba, Ni, Sr, Cu, and Fe.
[0018] Hydrotalcite particles are M 3+ The structure represented by formula (1) is easily coordinated to aluminum, so the hydrotalcite particles are more likely to remain on the toner in the image area after paper ejection, and the effect of suppressing paper ejection adhesion works efficiently. In addition to aluminum, the hydrotalcite particles also contain other M 3+The oxide may contain at least one trivalent metal ion selected from the group consisting of B, Ga, Fe, Co, and In.
[0019] A n- is an anion with a valence of n, and the hydrotalcite particles contain at least F - Hydrotalcite particles can easily introduce fluoride ions between layers (intercalation) through anion exchange. In addition to fluorine, other A n- CO3 2- , O.H. - , Cl - , I - , Br - , SO4 2- , HCO3 - , CH3COO - , and NO3 - It may contain at least one anion selected from the group consisting of:
[0020] The hydrotalcite particles contain, for example, fluorine, magnesium and aluminum. 2+ It is preferable that the hydrotalcite particles contain at least Mg as a fluorine atom. It is also preferable that the hydrotalcite particles contain magnesium in addition to fluorine and aluminum.
[0021] Specific examples of hydrotalcite particles include: Mg 4.3 Al2(OH) 12.6 CO3·mH2O, Mg 8.6 Al4(OH)2 5.2 F2CO3·mH2O, Mg 12 Al4(OH) 32 Examples include F2CO3·mH2O. The hydrotalcite particles may be a solid solution containing a plurality of different elements, and may also contain a trace amount of a monovalent metal.
[0022] The value of the atomic number concentration ratio of fluorine to aluminum, F / Al (element ratio), in the hydrotalcite particles obtained from the main component mapping of the hydrotalcite particles by STEM-EDS mapping analysis of the toner should be 0.01 to 0.60. When the element ratio of fluorine to aluminum, F / Al, is 0.01 or more, the hydrotalcite particles can sufficiently contain the fluorine necessary for suppressing paper discharge adhesion. Also, when F / Al is 0.60 or less, the strongly negative fluoride ions can easily coordinate to aluminum in the structure represented by formula (1) without canceling the charge of the aluminum ions, and paper discharge adhesion can be suppressed. F / Al is preferably 0.02 to 0.30, more preferably 0.07 to 0.20.
[0023] In the line analysis in the STEM-EDS mapping analysis of the toner, fluorine and aluminum must be present inside the hydrotalcite particles. Thereby, it can be confirmed that fluorine is intercalated between the layers of the layered structure of the hydrotalcite particles.
[0024] The value of the atomic number concentration ratio of magnesium to aluminum, Mg / Al, in the hydrotalcite particles obtained from the main component mapping of the hydrotalcite particles by STEM-EDS mapping analysis of the toner is preferably 1.5 to 4.0, more preferably 1.6 to 3.8, and even more preferably 2.1 to 3.8. F / Al and Mg / Al can be controlled by adjusting the amount of raw materials during the production of hydrotalcite.
[0025] Also, the hydrotalcite particles preferably have water in their molecules, and in formula (2), it is more preferably 0.1 < m < 0.6.
[0026] The hydrotalcite particles may be hydrophobized with a surface treatment agent. As the surface treatment agent, higher fatty acids, coupling agents, esters, and oils such as silicone oil can be used. Among them, higher fatty acids are preferably used, and specific examples thereof include stearic acid, oleic acid, and lauric acid.
[0027] The number average particle diameter of the primary particles of the hydrotalcite particles is preferably 30 to 1200 nm, more preferably 60 to 1000 nm, and even more preferably 100 to 800 nm. When the number average particle diameter of the hydrotalcite particles is 60 nm or more, a sufficient distance between papers can be secured, and adhesion during discharge can be further suppressed.
[0028] On the other hand, when the number-average particle diameter of the primary particles of the hydrotalcite particles is 1000 nm or less, the number of hydrotalcite particles per unit mass tends to be sufficient to maintain the charge amount of the toner constant throughout durable use while more sufficiently inhibiting adhesion to discharged paper. In addition, the hydrotalcite particles are less likely to migrate from the toner during the image formation process, the charge amount of the toner is kept constant throughout durable use, and a sufficient amount of hydrotalcite particles tends to remain on the toner in the image area in order to suppress adhesion to discharged paper.
[0029] When the content of the hydrotalcite particles in the toner based on mass is represented as b (mass %), b may be 0.025 to 0.900 mass %, and is preferably 0.050 to 0.500 mass %, and more preferably 0.100 to 0.400 mass %. By setting the content b of the hydrotalcite particles to 0.050% by mass or more, the charge amount of the toner is kept constant throughout durable use, and a sufficient amount of the hydrotalcite particles can remain on the image to suppress adhesion at discharge. On the other hand, by setting the content b of the hydrotalcite particles to 0.500% by mass or less, excessive charging of the toner can be prevented, and image defects such as fogging can be suppressed. The content of the hydrotalcite particles can be quantified using a calibration curve prepared from a standard sample by using fluorescent X-ray analysis. The content b can be controlled by changing the amount of the hydrotalcite particles added to the toner particles.
[0030] The mass-based content of the toner having the structure represented by formula (1) is represented by a (mass %), where a and b preferably satisfy the following formula (3). 4.0≦a / b≦100.0 (3) When the value of a / b is within the range of formula (3), the metal ions in the hydrotalcite particles are efficiently oriented in the structure represented by formula (1), and tend to remain on the toner surface even after fixing, so that adhesion during discharge can be further suppressed. a / b is preferably 5.0 to 55.0. The content a is preferably from 1.400 to 5.700 mass %, and more preferably from 1.500 to 4.200 mass %.
[0031] The polyester resin preferably contains a structure corresponding to a propylene oxide adduct of bisphenol A (preferably a 1.0-5.0 mol adduct, more preferably a 1.0-3.0 mol adduct) and a structure corresponding to an ethylene oxide adduct of bisphenol A (preferably a 1.0-5.0 mol adduct, more preferably a 1.0-3.0 mol adduct).
[0032] In the polyester resin, when the content of the structure corresponding to a propylene oxide adduct of bisphenol A is c (mass%) and the content of the structure corresponding to an ethylene oxide adduct of bisphenol A is d (mass%), c and d may satisfy the following formula (4') and preferably satisfy the following formula (4). 3.0≦c / d≦25.0 (4´) 5.0≦c / d≦20.0 (4)
[0033] When the value of c / d is within the range of the formula (4), adhesion during discharge can be more sufficiently suppressed, and low-temperature fixability and heat-resistant storage stability can be more satisfactorily achieved. c / d is more preferably 6.0 to 12.0. The content c is preferably 30.0 to 60.0 mass %, more preferably 40.0 to 52.0 mass %. The content d is preferably 1.0 to 15.0 mass %, more preferably 2.0 to 10.0 mass %.
[0034] The structure corresponding to the propylene oxide adduct of bisphenol A and the structure corresponding to the ethylene oxide adduct of bisphenol A are structures obtained by condensation polymerization of the propylene oxide adduct or ethylene oxide adduct of bisphenol A, and are represented by the following formula (A). [ka]
[0035] In formula (A), R is an ethylene or propylene group, x and y are each an integer of 0 or more, and the average value of x+y is 0 to 10 (preferably 1.0 to 5.0, more preferably 1.0~3.0).
[0036] The method for producing the toner is not particularly limited, and known methods such as a suspension polymerization method, a dissolution suspension method, an emulsion aggregation method, and a pulverization method can be used. A production method using an emulsion aggregation method is preferred. That is, the toner particles are preferably emulsion aggregation toner particles.
[0037] This is preferable from the viewpoint of ease of production, including the fact that a surfactant is generally used in the toner formation process. In the production of toner by the emulsion aggregation method, the components to be contained can be mixed as emulsion particles and aggregated to form a toner, so that it is easy to introduce the necessary components and to design and produce a highly functional toner. In addition, since the toner produced by the emulsion aggregation method is nearly spherical and has a uniform size, the hydrotalcite particles can be uniformly added to the toner in the external addition process, so that there is less bias in the hydrotalcite particles present in the image area after fixing, and the suppression of adhesion at discharge can be more effectively achieved.
[0038] It is preferable that the toner contains compound A and compound B which are eluted in methanol when the toner is subjected to an elution treatment under the elution condition A described below. Dissolution condition A: At 25° C., 10 times the mass of the toner is used in methanol (JIS K8891 equivalent), and the toner is stirred for 10 hours at a rotor speed of 200 rpm using a stirring device.
[0039] In addition, when the supernatant obtained by centrifuging the eluate in which Compound A and Compound B were eluted in methanol under the following centrifugation condition A was analyzed by liquid chromatography ESI / MS under the following analysis condition A, The compound A contained in the supernatant is ionized as a cation and detected, The compound B contained in the supernatant is preferably detected as an anion. Centrifugation condition A: Rotation is performed for 30 minutes at 25° C., a rotation radius of 10.1 cm, and a rotation speed of 3,500 rpm. Analysis condition A: Sheath Gas: 10 (arb. unit.), Aux Gas: 5 (arb. unit.), spray voltage: 5 kV, capillary temperature: 275°C. Ionized substances are detected as cations under the conditions of capillary voltage: 35 V, tube lens voltage: 110 V, and ionized substances are detected as anions under the conditions of capillary voltage: -35 V, tube lens voltage: -110 V.
[0040] Compound A and compound B, which can be extracted into methanol and ionized, are highly polar components that exist near the surface and play a role in supporting the charging properties of the toner. The fact that compound A was detected on the cation side and compound B on the anion side in ESI / MS analysis indicates that some compounds have a tendency to have positive charging properties and others have a tendency to have negative charging properties.
[0041] By containing compound A and compound B in the toner, both positive and negative components are present, which means that the negative components tend to cause negative charging, and the positive components tend to cause leakage. The structure shown in formula (1) has high polarity and is easy to charge. The presence of compound A and compound B, which play a role in supporting the charging characteristics, near the toner surface stabilizes the retention of negative charge, and prevents overcharging of the toner due to leakage from the positive components.
[0042] As a result, the toner in the image area is prevented from electrostatically attracting the overlapping paper after discharge more strongly than the releasing effect of the hydrotalcite particles due to overcharging, and as a result, discharge adhesion is more easily suppressed. Also, image problems such as fogging caused by charge-up due to overcharging are more easily suppressed. By containing compound A and compound B, adverse effects such as discharge adhesion and image problems are reduced. The noise can be suppressed better.
[0043] In order to incorporate Compound A into the toner, it is preferable to use a material that does not bond to the binder resin of the toner and exists independently, for example, a surfactant having a repeating structure of ethylene oxide.
[0044] Preferably, compound A includes at least one compound selected from the group consisting of polyoxyethylene lauryl ether, polyoxyethylene hexadecyl ether, polyoxyethylene nonylphenyl ether, polyoxyethylene dodecyl ether, polyoxyethylene sorbitan monooleate ether, polyoxyethylene styryl phenyl ether, polyoxyethylene (2) lauryl ether sodium sulfate, polyoxyethylene lauryl ether sodium acetate, and the like.
[0045] Compound A is preferably at least one compound selected from the group consisting of an ethylene oxide adduct of a linear aliphatic alcohol having 8 to 16 carbon atoms (more preferably 10 to 14) and sodium polyoxyethylene lauryl ether acetate, and is more preferably an ethylene oxide adduct of lauryl alcohol.
[0046] There is no particular limitation on the method of addition, but for example, when a toner is produced by an emulsion aggregation method, Compound A may be added in any step of preparing a colorant dispersion, a release agent dispersion, a resin particle dispersion, or the like, or in a step of washing the toner. Compound A is preferably added when preparing each dispersion, such as a colorant dispersion, a release agent dispersion, or a resin particle dispersion. Compound A is also preferably added to a mixture when preparing these aggregated particles (i.e., in a dispersion step).
[0047] In order to incorporate compound B into the toner, it is preferable to use a material that does not bind to the binder resin of the toner and exists independently. For example, an anionic surfactant can be preferably used. Compound B is preferably at least one compound selected from the group consisting of aliphatic soaps such as sodium stearate and sodium laurate, sodium lauryl sulfate, (linear or branched) sodium dodecylbenzenesulfonate, and sodium polyoxyethylene (2) lauryl ether sulfate. Compound B is preferably linear or branched sodium dodecylbenzenesulfonate.
[0048] There is no particular limitation on the method of addition, but for example, when a toner is manufactured by an emulsion aggregation method, the above-mentioned compound may be added in any step of preparing a colorant dispersion, a release agent dispersion, a resin particle dispersion, or the like, or in a step of washing the toner. It is preferable to add compound B when preparing each dispersion, such as a colorant dispersion, a release agent dispersion, or a resin particle dispersion. It is also preferable to add compound B to the mixture when preparing these aggregated particles (i.e., in the dispersion step).
[0049] Each component constituting the toner and the method for producing the toner will be described in more detail. <Binding resin> The toner particles have a binder resin. Examples of the binder resin include polyester resin, vinyl resin, and other binder resins such as the following resins or polymers: styrene acrylic resin, polyester resin, epoxy resin, polyurethane resin, polyamide resin, cellulose resin, polyether resin, mixed resins or composite resins thereof. The binder resin includes a polyester resin. The binder resin may further include a styrene-acrylic resin or the like. The binder resin may include a hybrid resin of a polyester resin and a styrene-acrylic resin. It is more preferable that the binder resin is a polyester resin.
[0050] The polyester resin can be obtained by combining suitable compounds selected from polyvalent carboxylic acids, polyols, hydroxycarboxylic acids, etc., and synthesizing them using a conventionally known method such as an ester exchange method or a polycondensation method.
[0051] Polycarboxylic acids are compounds containing two or more carboxy groups in one molecule. Among them, dicarboxylic acids are compounds containing two carboxy groups in one molecule and are preferably used.
[0052] Examples of dicarboxylic acids include oxalic acid, succinic acid, glutaric acid, maleic acid, adipic acid, β-methyladipic acid, azelaic acid, sebacic acid, nonanedicarboxylic acid, decanedicarboxylic acid, undecanedicarboxylic acid, dodecanedicarboxylic acid, fumaric acid, citraconic acid, diglycolic acid, cyclohexane-3,5-diene-1,2-carboxylic acid, hexahydroterephthalic acid, malonic acid, pimelic acid, suberic acid, phthalic acid, isophthalic acid, terephthalic acid, tetrachlorophthalic acid, chlorophthalic acid, nitrophthalic acid, p-carboxyphenylacetic acid, p-phenylenediacetic acid, m-phenylenediacetic acid, o-phenylenediacetic acid, diphenylacetic acid, diphenyl-p,p'-dicarboxylic acid, naphthalene-1,4-dicarboxylic acid, naphthalene-1,5-dicarboxylic acid, naphthalene-2,6-dicarboxylic acid, anthracenedicarboxylic acid, and cyclohexanedicarboxylic acid.
[0053] Examples of polyvalent carboxylic acids other than dicarboxylic acids include trimellitic acid, trimesic acid, pyromellitic acid, naphthalene tricarboxylic acid, naphthalene tetracarboxylic acid, pyrene tricarboxylic acid, pyrene tetracarboxylic acid, itaconic acid, glutaconic acid, n-dodecyl succinic acid, n-dodecenyl succinic acid, isododecyl succinic acid, isododecenyl succinic acid, n-octyl succinic acid, n-octenyl succinic acid, etc. These may be used alone or in combination of two or more.
[0054] A polyol is a compound containing two or more hydroxyl groups in one molecule. Among them, a diol is a compound containing two hydroxyl groups in one molecule, and is preferably used. Specifically, ethylene glycol, diethylene glycol, triethylene glycol, 1,2-propylene glycol, 1,3-propylene glycol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,7-heptanediol, 1,8-octanediol, 1,9-nonanediol, 1,10-decanediol, 1,11-undecanediol, 1,12-dodecanediol, 1,13-tridecanediol, 1,14-tetradecanediol, 1,18-octadecanediol, 1,14-eicosanediol, didecanediol, tetra ... Examples of suitable bisphenols include propylene glycol, polyethylene glycol, polypropylene glycol, polytetramethylene ether glycol, 1,4-cyclohexanediol, 1,4-cyclohexanedimethanol, 1,4-butenediol, neopentyl glycol, 1,4-cyclohexanediol, polytetramethylene glycol, hydrogenated bisphenol A, bisphenol A, bisphenol F, bisphenol S, and alkylene oxide (ethylene oxide, propylene oxide, butylene oxide, etc.) adducts of the above bisphenols.
[0055] Among these, preferred are alkylene glycols having 2 to 12 carbon atoms and alkylene oxide adducts of bisphenols, and particularly preferred are alkylene oxide adducts of bisphenols and their combined use with alkylene glycols having 2 to 12 carbon atoms.
[0056] Examples of trivalent or higher polyols include glycerin, trimethylolethane, trimethylolpropane, pentaerythritol, hexamethylolmelamine, hexaethylolmelamine, tetramethylolbenzoguanamine, tetraethylolbenzoguanamine, Examples of the polyphenols include sorbitol, trisphenol PA, phenol novolac, cresol novolac, and alkylene oxide adducts of the above-mentioned polyphenols having a valence of three or more. These may be used alone or in combination of two or more. The polyester resin may also be a polyester resin containing a urea group. It is preferable that the carboxyl group at the terminal of the polyester resin is not capped.
[0057] More preferably, the polyester resin is a condensation polymer of a monomer mixture containing an alkylene oxide adduct of ethylene glycol and bisphenol A (the average number of moles added is preferably 1 to 5 mol), and terephthalic acid. The polyester resin is preferably an amorphous polyester resin. The monomer mixture may contain isophthalic acid, trimellitic acid, etc.
[0058] The binder resin may contain a polyester resin. The binder resin may be a hybrid resin of a polyester resin and a styrene-acrylic resin. The binder resin preferably contains a polyester resin or a hybrid resin of a polyester resin and a styrene-acrylic resin. The content of the polyester resin in the binder resin is preferably 60 to 100% by mass, more preferably 70 to 100% by mass, and further preferably 75 to 100% by mass.
[0059] Examples of the styrene-acrylic resin include homopolymers made of the following polymerizable monomers, copolymers obtained by combining two or more of these, and mixtures thereof. Styrenic monomers such as styrene, α-methylstyrene, β-methylstyrene, o-methylstyrene, m-methylstyrene, p-methylstyrene, 2,4-dimethylstyrene, pn-butylstyrene, p-tert-butylstyrene, pn-hexylstyrene, pn-octylstyrene, pn-nonylstyrene, pn-decylstyrene, pn-dodecylstyrene, p-methoxystyrene and p-phenylstyrene; (Meth)acrylic monomers such as methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, iso-propyl (meth)acrylate, n-butyl (meth)acrylate, iso-butyl (meth)acrylate, tert-butyl (meth)acrylate, n-amyl (meth)acrylate, n-hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, n-octyl (meth)acrylate, n-nonyl (meth)acrylate, cyclohexyl (meth)acrylate, benzyl (meth)acrylate, dimethyl phosphate ethyl (meth)acrylate, diethyl phosphate ethyl (meth)acrylate, dibutyl phosphate ethyl (meth)acrylate and 2-benzoyloxyethyl (meth)acrylate, (meth)acrylonitrile, 2-hydroxyethyl (meth)acrylate, (meth)acrylic acid, maleic acid; Vinyl ether monomers such as vinyl methyl ether and vinyl isobutyl ether; vinyl ketone monomers such as vinyl methyl ketone, vinyl ethyl ketone and vinyl isopropenyl ketone; Polyolefins such as ethylene, propylene, and butadiene.
[0060] The styrene acrylic resin may contain a polyfunctional polymerizable monomer as required. Examples of the polyfunctional polymerizable monomer include diethylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, tetraethylene glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, neopentyl glycol di(meth)acrylate, tripropylene glycol di(meth)acrylate, polypropylene glycol di(meth)acrylate, 2,2'-bis(4-((meth)acryloxydiethoxy)phenyl)propane, trimethylolpropane tri(meth)acrylate, and tetramethylolmethane. Examples include tetra(meth)acrylate, divinylbenzene, divinylnaphthalene, and divinyl ether. In order to control the degree of polymerization, it is also possible to further add a known chain transfer agent and polymerization inhibitor.
[0061] The styrene-acrylic resin is preferably a polymer of a monomer containing styrene and n-butyl acrylate. To obtain a hybrid resin, a monomer capable of reacting with a polyester resin may be used. For example, mono-n-butyl maleate, maleic acid, (meth)acrylic acid, etc. may be used.
[0062] Examples of the polymerization initiator for obtaining the styrene-acrylic resin include organic peroxide-based initiators and azo-based polymerization initiators. Examples of the organic peroxide initiator include benzoyl peroxide, lauroyl peroxide, di-α-cumyl peroxide, 2,5-dimethyl-2,5-bis(benzoylperoxy)hexane, bis(4-t-butylcyclohexyl)peroxydicarbonate, 1,1-bis(t-butylperoxy)cyclododecane, t-butylperoxymaleic acid, bis(t-butylperoxy)isophthalate, methyl ethyl ketone peroxide, tert-butylperoxy-2-ethylhexanoate, diisopropyl peroxycarbonate, cumene hydroperoxide, 2,4-dichlorobenzoyl peroxide, and tert-butylperoxypivalate.
[0063] Examples of the azo polymerization initiator include 2,2'-azobis-(2,4-dimethylvaleronitrile), 2,2'-azobisisobutyronitrile, 1,1'-azobis(cyclohexane-1-carbonitrile), 2,2'-azobis-4-methoxy-2,4-dimethylvaleronitrile, azobismethylbutyronitrile, and 2,2'-azobis-(methyl isobutyrate).
[0064] Furthermore, a redox initiator, which is a combination of an oxidizing substance and a reducing substance, can also be used as the polymerization initiator. Oxidizing substances include inorganic peroxides such as hydrogen peroxide, persulfates (sodium, potassium and ammonium salts) and oxidizing metal salts such as tetravalent cerium salts. Examples of reducing substances include reducing metal salts (divalent iron salts, monovalent copper salts, and trivalent chromium salts), ammonia, lower amines (amines having from 1 to 6 carbon atoms, such as methylamine and ethylamine), amino compounds such as hydroxylamine, reducing sulfur compounds such as sodium thiosulfate, sodium hydrosulfite, sodium hydrogensulfite, sodium sulfite, and sodium formaldehyde sulfoxylate, lower alcohols (having from 1 to 6 carbon atoms), ascorbic acid or a salt thereof, and lower aldehydes (having from 1 to 6 carbon atoms).
[0065] The polymerization initiator is selected with reference to its 10-hour half-life temperature and is used alone or in combination. The amount of polymerization initiator added varies depending on the desired degree of polymerization, but is generally 0.5 to 20.0 parts by mass per 100.0 parts by mass of polymerizable monomer.
[0066] The binder resin may contain a crystalline polyester, for example, a condensation polymer of an aliphatic diol and an aliphatic dicarboxylic acid. It is preferably a condensation polymer of an aliphatic diol having 2 to 12 carbon atoms and an aliphatic dicarboxylic acid having 2 to 12 carbon atoms. Examples of the aliphatic diol having 2 to 12 carbon atoms include the following compounds: 1,2-ethanediol, 1,3-propanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,7-heptanediol, 1,8-octanediol, 1,9-nonanediol, 1,10-hexanediol, ... 1,11-undecanediol, 1,12-dodecanediol, etc.
[0067] Aliphatic diols having a double bond can also be used, such as the following compounds: 2-butene-1,4-diol, 3-hexene-1,6-diol, and 4-octene-1,8-diol.
[0068] Examples of aliphatic dicarboxylic acids having 2 to 12 carbon atoms include the following compounds: oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, 1,9-nonanedicarboxylic acid, 1,10-decanedicarboxylic acid, 1,11-undecanedicarboxylic acid, 1,12-dodecanedicarboxylic acid, lower alkyl esters and acid anhydrides of these aliphatic dicarboxylic acids.
[0069] Among these, sebacic acid, adipic acid, 1,10-decanedicarboxylic acid, and lower alkyl esters and acid anhydrides thereof are preferred. These may be used alone or in combination of two or more.
[0070] Aromatic dicarboxylic acids can also be used. Examples of aromatic dicarboxylic acids include the following compounds: terephthalic acid, isophthalic acid, 2,6-naphthalenedicarboxylic acid, and 4,4'-biphenyldicarboxylic acid. Among these, terephthalic acid is preferred because of its ease of availability and the ease of forming a polymer with a low melting point.
[0071] A dicarboxylic acid having a double bond can also be used. The dicarboxylic acid having a double bond can be preferably used to suppress hot offset during fixing, since the double bond can be utilized to crosslink the entire resin. Such dicarboxylic acids include fumaric acid, maleic acid, 3-hexenedioic acid, and 3-octenedioic acid. In addition, lower alkyl esters and acid anhydrides thereof are also included. Among these, fumaric acid and maleic acid are more preferred.
[0072] The method for producing the crystalline polyester is not particularly limited, and the crystalline polyester can be produced by a general polyester polymerization method in which a dicarboxylic acid component and a diol component are reacted. For example, the crystalline polyester can be produced by a direct polycondensation method or an ester exchange method, which are selected depending on the type of monomer.
[0073] The content of the crystalline polyester is preferably 1.0 parts by mass or more and 30.0 parts by mass or less, and more preferably 3.0 parts by mass or more and 25.0 parts by mass or less, relative to 100 parts by mass of the binder resin.
[0074] The peak temperature of the maximum endothermic peak of the crystalline polyester measured using a differential scanning calorimeter (DSC) is preferably 50.0° C. or more and 100.0° C. or less, and from the viewpoint of low-temperature fixability, more preferably 60.0° C. or more and 90.0° C. or less.
[0075] The molecular weight of the binder resin is preferably such that the peak molecular weight Mp is 5000 or more and 100000 or less, and more preferably such that the peak molecular weight Mp is 10000 or more and 40000 or less. The glass transition temperature Tg of the binder resin is preferably 40° C. or more and 70° C. or less.
[0076] <Crosslinking agent> In order to control the molecular weight of the binder resin constituting the toner particles, a crosslinking agent may be added during polymerization of the polymerizable monomer. For example, ethylene glycol dimethacrylate, ethylene glycol diacrylate, diethylene glycol dimethacrylate, diethylene glycol diacrylate, triethylene glycol diacrylate, ethylene glycol dimethacrylate, triethylene glycol diacrylate, neopentyl glycol dimethacrylate, neopentyl glycol diacrylate, divinylbenzene, bis(4-acryloxypolyethoxyphenyl)propane, ethylene glycol diacrylate, 1,3-butylene glycol diacrylate, 1,4-butanediol diacrylate, 1,5-pentanediol diacrylate, 1,6-hexanediol diacrylate, neopentyl glycol diacrylate, diethylene glycol diacrylate, triethylene glycol diacrylate, tetraethylene glycol diacrylate, polyethylene glycol #200, #400, #600 diacrylates, dipropylene glycol diacrylate, polypropylene glycol diacrylate, polyester type diacrylate (MANDA Nippon Kayaku), and the above acrylates are methacrylated. Something that has been converted into a relate. The amount of the crosslinking agent added is preferably 0.001 parts by mass or more and 15,000 parts by mass or less based on 100 parts by mass of the polymerizable monomer.
[0077] <Release agent> The toner may contain a known wax as a releasing agent. Specific examples include petroleum waxes such as paraffin wax, microcrystalline wax, and petrolatum and their derivatives, montan wax and its derivatives, hydrocarbon waxes produced by the Fischer-Tropsch process and their derivatives, polyolefin waxes such as polyethylene and polypropylene and their derivatives, and natural waxes such as carnauba wax and candelilla wax and their derivatives. Derivatives also include oxides, block copolymers with vinyl monomers, and graft modified products. Other examples include alcohols such as higher aliphatic alcohols, fatty acids such as stearic acid and palmitic acid or their acid amides, esters and ketones, hydrogenated castor oil and its derivatives, vegetable waxes and animal waxes. These can be used alone or in combination.
[0078] Among these, polyolefin, Fischer-Tropsch hydrocarbon wax, or petroleum wax is preferably used since it tends to improve the developing property and transfer property. Note that these waxes may contain an antioxidant within a range that does not affect the properties of the toner. From the viewpoint of phase separation with respect to the binder resin or crystallization temperature, preferred examples include higher fatty acid esters such as behenyl behenate and dibehenyl sebacate. Ester waxes as plasticizers, which will be described later, can also be used preferably.
[0079] The content of the release agent is preferably 1.0 part by mass or more and 30.0 parts by mass or less with respect to 100.0 parts by mass of the binder resin. The melting point of the release agent is preferably from 30° C. to 120° C., more preferably from 60° C. to 100° C. By using a release agent having a melting point of from 30° C. to 120° C., the release effect is efficiently exerted and a wider fixing area is secured.
[0080] <Plasticizer> In order to improve the sharp melting property of the toner, it is preferable to use a crystalline plasticizer. The plasticizer is not particularly limited, and any of the known plasticizers used in toners such as those described below can be used. Esters of monohydric alcohols and aliphatic carboxylic acids, such as behenyl behenate, stearyl stearate, and palmityl palmitate, or esters of monohydric carboxylic acids and aliphatic alcohols; esters of dihydric alcohols and aliphatic carboxylic acids, such as ethylene glycol distearate, dibehenyl sebacate, and hexanediol dibehenate, or esters of dihydric carboxylic acids and aliphatic alcohols; esters of trihydric alcohols and aliphatic carboxylic acids, such as glycerol tribehenate, or esters of trihydric carboxylic acids and aliphatic alcohols. esters of tetrahydric alcohols and aliphatic carboxylic acids, such as pentaerythritol tetrastearate and pentaerythritol tetrapalmitate, or esters of tetrahydric carboxylic acids and aliphatic alcohols; esters of hexahydric alcohols and aliphatic carboxylic acids, such as dipentaerythritol hexastearate and dipentaerythritol hexapalmitate, or esters of hexahydric carboxylic acids and aliphatic alcohols; esters of polyhydric alcohols and aliphatic carboxylic acids, such as polyglycerin behenate, or esters of polyhydric carboxylic acids and aliphatic alcohols; and natural ester waxes, such as carnauba wax and rice wax. These may be used alone or in combination.
[0081] <Coloring agent> The toner particles may contain a colorant. Known pigments and dyes can be used as the colorant. Pigments are preferred as the colorant because they have excellent weather resistance. Examples of cyan colorants include copper phthalocyanine compounds and derivatives thereof, anthraquinone compounds, and basic dye lake compounds. Specific examples include: CI Pigment Blue 1, 7, 15, 15:1, 15:2, 15:3, 15:4, 60, 62 and 66. Examples of magenta colorants include condensed azo compounds, diketopyrrolopyrrole compounds, anthraquinone compounds, quinacridone compounds, basic dye lake compounds, naphthol compounds, benzimidazolone compounds, thioindigo compounds, and perylene compounds. Specific examples include: CI Pigment Red 2, 3, 5, 6, 7, 23, 48:2, 48:3, 48:4, 57:1, 81:1, 122, 144, 146, 150, 166, 169, 177, 184, 185, 202, 206, 220, 221 and 254, and CI Pigment Violet 19.
[0082] Examples of yellow colorants include condensed azo compounds, isoindolinone compounds, anthraquinone compounds, azo metal complexes, methine compounds, and allylamide compounds. Specific examples include: CI Pigment Yellow 12, 13, 14, 15, 17, 62, 74, 83, 93, 94, 95, 97, 109, 110, 111, 120, 127, 128, 129, 147, 151, 154, 155, 168, 174, 175, 176, 180, 181, 185, 191 and 194. Examples of black colorants include those toned to black using the above yellow, magenta and cyan colorants, as well as carbon black. These colorants can be used alone or in mixtures, or further in the form of a solid solution. The colorant is preferably used in an amount of 1.0 part by mass or more and 20.0 parts by mass or less with respect to 100.0 parts by mass of the binder resin.
[0083] <Charge control agents and charge control resins> The toner particles may contain a charge control agent or a charge control resin. Any known charge control agent can be used as the charge control agent, and a charge control agent that has a high triboelectric charging speed and can stably maintain a constant triboelectric charge amount is particularly preferred. Furthermore, when the toner particles are produced by a suspension polymerization method, a charge control agent that has low polymerization inhibition and is substantially free of solubilized matter in an aqueous medium is particularly preferred.
[0084] Examples of toners that control the toner to be negatively charged include monoazo metal compounds, acetylacetone metal compounds, aromatic oxycarboxylic acids, aromatic dicarboxylic acids, oxycarboxylic and dicarboxylic acid-based metal compounds, aromatic oxycarboxylic acids, aromatic mono- and polycarboxylic acids and their metal salts, anhydrides, esters, phenol derivatives such as bisphenol, urea derivatives, metal-containing salicylic acid-based compounds, metal-containing naphthoic acid-based compounds, boron compounds, quaternary ammonium salts, calixarenes, and charge control resins.
[0085] The charge control resin may be a polymer or copolymer having a sulfonic acid group, a sulfonate group, or a sulfonate ester group. As the polymer having a sulfonic acid group, a sulfonate group, or a sulfonate ester group, a polymer containing a sulfonic acid group-containing acrylamide monomer or a sulfonate group-containing methacrylamide monomer in a copolymerization ratio of 2% by mass or more is preferable, and a polymer containing a sulfonic acid group-containing methacrylamide monomer in a copolymerization ratio of 5% by mass or more is more preferable.
[0086] The charge control resin preferably has a glass transition temperature (Tg) of 35° C. or more and 90° C. or less, a peak molecular weight (Mp) of 10,000 or more and 30,000 or less, and a weight average molecular weight (Mw) of 25,000 or more and 50,000 or less. When used, it is possible to impart preferable triboelectric charging characteristics without affecting the thermal characteristics required for the toner particles. Furthermore, when the charge control resin contains a sulfonic acid group, for example, the dispersibility of the charge control resin itself in the polymerizable monomer composition and the dispersibility of the colorant are improved, and the coloring power, transparency, and triboelectric charging characteristics can be further improved. These charge control agents or charge control resins may be added alone or in combination of two or more kinds. The amount of the charge control agent or charge control resin added is preferably 0.01 parts by mass or more and 20.0 parts by mass or less, and more preferably 0.5 parts by mass or more and 10.0 parts by mass or less, relative to 100.0 parts by mass of the binder resin.
[0087] <Method of manufacturing toner particles> The toner particles contain a binder resin. The toner particles may have a core particle containing a binder resin and a shell on the surface of the core particle. The method for producing the toner particles is not particularly limited and may be a known method, such as a kneading and grinding method or a wet production method. From the viewpoints of uniform particle size, shape controllability, and ease of obtaining toner particles with a core-shell structure, a wet production method is preferred. Examples of the wet production method include a suspension polymerization method, a dissolution suspension method, an emulsion polymerization aggregation method, and an emulsion aggregation method, and the emulsion aggregation method is more preferred from the viewpoint of ease of controlling the shape of the toner particles. In other words, the toner particles are preferably emulsion aggregation toner particles.
[0088] In the emulsion aggregation method, first, a dispersion liquid of each material such as binder resin particles and colorant is prepared. The obtained dispersion liquid of each material is dispersed and mixed by adding a dispersion stabilizer as necessary. Then, an aggregating agent is added to aggregate the particles to the desired toner particle size, and then or simultaneously with the aggregation, the resin particles are fused together. If necessary, the shape is controlled by heat to form toner particles.
[0089] The method for producing the toner preferably includes the following steps. (1) A dispersion and mixing step of preparing a binder resin particle dispersion (or a colorant particle dispersion, if necessary) containing a binder resin and mixing the particles to obtain a mixed dispersion; (2) an aggregation step of aggregating the binder resin fine particles (and colorant fine particles, if necessary) contained in the obtained mixed dispersion to form aggregates; and (3) a fusion step of heating the aggregates to fuse them together to form fused particles; The resulting fused particles can be cooled to obtain toner particles.
[0090] After the step (3), the following steps (4) and / or (5) may be included. (4) An annealing step of heating and holding the fused particles at a temperature equal to or higher than the crystallization temperature or glass transition temperature of the binder resin. (5) A step of cooling the fused particles at a cooling rate of 0.1° C. / sec or more to obtain toner particles.
[0091] Here, the binder resin particles can be composite particles formed of a plurality of layers, each of which is made of two or more layers of resins with different compositions. For example, they can be manufactured by emulsion polymerization, mini-emulsion polymerization, phase inversion emulsification, or a combination of several manufacturing methods. When an internal additive is contained in the toner particles, the resin particles may contain the internal additive, or a dispersion of internal additive particles consisting of only the internal additive may be separately prepared, and the internal additive particles may be aggregated together with the resin particles when the internal additive particles are aggregated. In addition, resin particles with different compositions can be added at different times during aggregation and aggregated to produce toner particles with different layer configurations. After the resin particles containing the binder resin are aggregated to form a core portion, the resin particles containing the shell resin can be added at different times and aggregated to form a shell portion.
[0092] The toner particles may have a shell. The resin for the shell may be the same as or different from the binder resin. The resin for the shell is, for example, a polyester resin having a structure represented by formula (1). The amount of the resin for the shell (shell content) is preferably 1.0 to 10.0 parts by mass, more preferably 2.0 to 7.0 parts by mass, based on 100 parts by mass of the binder resin contained in the core particles.
[0093] In this case, the method for producing the toner preferably includes the following steps. (1) A dispersion and mixing step of preparing a binder resin particle dispersion (or a colorant particle dispersion, if necessary) containing a binder resin and mixing the particles to obtain a mixed dispersion; (2) an aggregation step of aggregating the binder resin fine particles (and colorant fine particles, if necessary) contained in the obtained mixed dispersion to form aggregates; (3) a shell formation step of further adding resin fine particles containing a resin for a shell to the dispersion containing the aggregates to aggregate them and form aggregates having a shell; and (4) a fusion step of heating the aggregates to fuse them together to form fused particles;
[0094] In addition, during the step (4) or after the steps (1) to (4), the following step (5) is carried out: (5) A spheronization step in which the agglomerates are heated at a higher temperature. It is preferred that the compound has the formula:
[0095] After the step (5), the following steps (6) and (7) may be included: (6) An annealing step of heating and holding the fused particles at a temperature equal to or higher than the crystallization temperature or glass transition temperature of the binder resin. (7) A step of cooling the fused particles at a cooling rate of 0.1° C. / sec or more to obtain toner particles.
[0096] The following can be used as the dispersion stabilizer. As the surfactant, a known cationic surfactant, anionic surfactant, or nonionic surfactant can be used. Examples of inorganic dispersion stabilizers include tricalcium phosphate, magnesium phosphate, zinc phosphate, aluminum phosphate, calcium carbonate, magnesium carbonate, calcium hydroxide, magnesium hydroxide, aluminum hydroxide, calcium metasilicate, calcium sulfate, barium sulfate, bentonite, silica, and alumina. Examples of the organic dispersion stabilizer include polyvinyl alcohol, gelatin, methyl cellulose, methylhydroxypropyl cellulose, ethyl cellulose, sodium salt of carboxymethyl cellulose, and starch.
[0097] As the flocculant, in addition to surfactants having a polarity opposite to that of the surfactants used in the above-mentioned dispersion stabilizer, inorganic salts and inorganic metal salts having a valence of two or more can be suitably used. In particular, inorganic metal salts can control the flocculation property and the toner charge property by ionizing polyvalent metal elements in an aqueous medium. It is preferable because it is easy to use. Specific examples of preferred inorganic metal salts include metal salts such as calcium chloride, calcium nitrate, barium chloride, magnesium chloride, zinc chloride, iron chloride, aluminum chloride, and aluminum sulfate, as well as inorganic metal salt polymers such as polyiron chloride, polyaluminum chloride, polyaluminum hydroxide, and calcium polysulfide. Among these, aluminum salts and their polymers are particularly preferred. In general, in order to obtain a sharper particle size distribution, the valence of the inorganic metal salt is preferably divalent rather than monovalent, and more preferably trivalent or more than divalent, and even if the valence is the same, inorganic metal salt polymers are more suitable.
[0098] From the viewpoint of high definition and high resolution of images, the weight average particle size (D4) of the toner particles is preferably 3.0 μm or more and 10.0 μm or less. Also, from the viewpoint of the balance between developability, transferability and cleaning ability, the average circularity of the toner particles is preferably 0.95 or more and 0.98 or less.
[0099] <Toner manufacturing method> The toner contains hydrotalcite particles as an external additive. If necessary, other external additives may be added. Examples of other external additives include inorganic oxide particles such as silica particles, alumina particles, and titanium oxide particles, inorganic stearic acid compound particles such as aluminum stearate particles and zinc stearate particles, and inorganic titanic acid compound particles such as strontium titanate and zinc titanate. These may be used alone or in combination of two or more. Preferably, the external additive further contains silica particles.
[0100] These inorganic particles are preferably gloss-treated with a silane coupling agent, a titanium coupling agent, a higher fatty acid, a silicone oil, etc., to improve heat resistance and storage stability and environmental stability. The BET specific surface area of the external additive is 10 m 2 / g or more 450m 2 It is preferable that the molecular weight is not more than 1 / g.
[0101] The BET specific surface area can be determined by a low-temperature gas adsorption method using a dynamic constant pressure method according to the BET method (preferably the BET multipoint method). For example, a specific surface area measuring device (product name: Gemini 2375 Ver. 5.0, manufactured by Shimadzu Corporation) is used to adsorb nitrogen gas onto the surface of a sample, and the BET multipoint method is used to measure the BET specific surface area (m2 / g).
[0102] The total content of these various external additives is preferably 0.05 parts by mass or more and 5 parts by mass or less, more preferably 0.1 parts by mass or more and 3 parts by mass or less, and even more preferably 1.0 parts by mass or more and 3.0 parts by mass or less, relative to 100 parts by mass of the toner particles. Also, various external additives may be used in combination.
[0103] The mixer for adding the external additive to the toner particles is not particularly limited, and any known mixer can be used, regardless of whether it is a dry or wet type. Examples include FM Mixer (manufactured by Nippon Coke & Engineering Co., Ltd.), Super Mixer (manufactured by Kawata Corporation), Nobilta (manufactured by Hosokawa Micron Corporation), and Hybridizer (manufactured by Nara Machinery Co., Ltd.). In order to control the coating state of the external additive, the toner can be prepared by adjusting the rotation speed, processing time, and water temperature and amount of water in the jacket of the external addition device.
[0104] In addition, sieving devices used to sift out coarse particles after external addition include Ultrasonic (manufactured by Koei Sangyo Co., Ltd.); Resonaseave, Gyroshifter (Tokuju Kogyo Co., Ltd.); Vibrasonic System (manufactured by Dalton Co., Ltd.); Soniclean (manufactured by Shinto Kogyo Co., Ltd.); Turbo Screener (manufactured by Turbo Kogyo Co., Ltd.); Microshifter (manufactured by Makino Sangyo Co., Ltd.), etc.
[0105] The methods for measuring the physical properties of the toner and each material will be described below. <Identification of resin components by nuclear magnetic resonance spectroscopy (NMR) and measurement method for the content of the structure represented by formula (1) in the polyester resin, and the contents a, c, and d> 1 mL of deuterated chloroform is added to 20 mg of toner, and the NMR spectrum of the protons of the dissolved resin is measured. From the obtained NMR spectrum, the molar ratio and mass ratio of each monomer are calculated, and the content of the constituent monomer units of the resin, such as polyester resin, can be obtained. For example, as a monomer of polyester resin, a peak derived from terephthalic acid appears around 8.0 ppm, a peak of the structure shown in formula (1) (derived from ethylene glycol) appears around 4.7 ppm, a peak derived from bisphenol appears around 6.8 ppm, and a peak derived from styrene appears around 7.1 ppm, so the molar ratio and weight ratio of each monomer can be calculated based on the integral ratio of the peaks of each monomer that constitutes the resin. In addition, by measuring the mass of the insoluble portion of the toner that did not dissolve in chloroform, the content a (%), and contents c and d of the structure represented by formula (1) in the toner can be calculated. NMR device: JEOL RESONANCE ECX500 Observed nucleus: Proton Measurement mode: Single pulse Base peak: TMS
[0106] <Method for identifying hydrotalcite particles> The hydrotalcite particles, which are an external additive, can be identified by a combination of shape observation using a scanning electron microscope (SEM) and elemental analysis using energy dispersive X-ray analysis (EDS). Using a scanning electron microscope "S-4800" (product name; manufactured by Hitachi), the toner is observed at a maximum magnification of 50,000 times. The focus is adjusted to the surface of the toner particles, and the external additive to be identified is observed. An EDS analysis is performed on the external additive to be identified, and the hydrotalcite particles can be identified from the type of element peak. When element peaks observed include an element peak of at least one metal selected from the group consisting of Mg, Zn, Ca, Ba, Ni, Sr, Cu, and Fe, which are metals that can constitute hydrotalcite particles, and an element peak of at least one metal selected from the group consisting of Al, B, Ga, Fe, Co, and In, the presence of hydrotalcite particles containing the two types of metals can be inferred. A specimen of the hydrotalcite particles estimated by EDS analysis is prepared separately, and its shape is observed by SEM and analyzed by EDS. The analysis results of the specimen are compared to the analysis results of the particles to be identified to see if they match, and it is determined whether or not they are hydrotalcite particles.
[0107] <Method for measuring the element ratio of hydrotalcite particles> The element ratios of hydrotalcite particles are measured by EDS mapping of the toner using a scanning transmission electron microscope (STEM). In EDS mapping measurements, spectrum data is obtained for each pixel in the analysis area. By using a silicon drift detector with a large detection element area, EDS mapping can be measured with high sensitivity. By performing statistical analysis on the spectral data for each pixel obtained by EDS mapping measurement, it is possible to obtain a principal component mapping that extracts pixels with similar spectra, making it possible to map specific components.
[0108] The observation sample is prepared according to the following procedure. 0.5 g of toner was weighed out and placed in a cylindrical mold with a diameter of 8 mm, and left to stand for 2 minutes under a load of 40 kN using a Newton press to prepare cylindrical toner pellets with a diameter of 8 mm and a thickness of approximately 1 mm. A thin section having a thickness of 200 nm is prepared from the toner pellet using an ultramicrotome (Leica, FC7).
[0109] The STEM-EDS analysis is carried out using the following equipment and conditions. Scanning transmission electron microscope: JEM-2800 manufactured by JEOL Ltd. EDS detector: JED-2300T Dry SD100GV detector (detector area: 100 mm 2 ) EDS analyzer: Thermo Fisher Scientific NORAN System 7
[0110] [Conditions for STEM-EDS] STEM accelerating voltage: 200kV ·Magnification: 20,000x Probe size 1nm STEM image size: 1024 x 1024 pixels (EDS element mapping images are acquired at the same position.) EDS mapping size: 256 x 256 pixels, Dwell Time: 30 μs, Integration count: 100 frames The ratio of each element in the hydrotalcite particles is calculated based on the multivariate analysis as follows.
[0111] The EDS mapping is obtained by the STEM-EDS analysis device. Next, the collected spectral mapping data is subjected to multivariate analysis using the COMPASS (PCA) mode in the measurement command of the NORAN System 7 described above, and a principal component map image is extracted. In this case, the setting values are as follows: Kernel size: 3×3 Quantitative map setting: High (slow) Filter Fit Type: High Precision (Slow) At the same time, this operation calculates the area ratio of each extracted principal component in the EDS measurement field of view. Quantitative analysis is performed on the EDS spectrum of each obtained principal component mapping by the Cliff-Lorimer method.
[0112] The toner particle portion and the hydrotalcite particles are distinguished based on the quantitative analysis results of the obtained STEM-EDS main component mapping. The particles can be identified as hydrotalcite particles based on the particle size, shape, content of polyvalent metals such as aluminum and magnesium, and the amount ratio thereof. Moreover, whether or not fluorine and aluminum are present inside the hydrotalcite particles can be determined by the following means.
[0113] (Method for analyzing fluorine and aluminum in hydrotalcite particles) Based on the mapping data obtained by the above-mentioned method using STEM-EDS mapping analysis, the fluorine and aluminum in the hydrotalcite particles are analyzed. Specifically, EDS line analysis is performed in the normal direction to the outer periphery of the hydrotalcite particle, and the fluorine and aluminum present inside the particle are analyzed. A schematic diagram of the line analysis is shown in Figure 1(a). For a toner particle 1 and a hydrotalcite particle 3 adjacent to a toner particle 2, a line analysis is performed in the normal direction to the outer periphery of the hydrotalcite particle 3, i.e., in the direction of 5. Note that 4 indicates the boundary of the toner particle. The area in the acquired STEM image where hydrotalcite particles exist is selected using the rectangular selection tool, and line analysis is performed under the following conditions. Line analysis conditions STEM magnification: 800,000x Line length: 200nm Line width: 30 nm Number of line divisions: 100 points (intensity measurement every 2 nm)
[0114] When the elemental peak intensity of fluorine or aluminum in the EDS spectrum of the hydrotalcite particle is 1.5 times or more the background intensity, and when the elemental peak intensity of fluorine or aluminum at both ends of the hydrotalcite particle in the line analysis (points a and b in FIG. 1(a)) does not exceed 3.0 times the peak intensity at point c, the element is determined to be contained inside the hydrotalcite particle. Point c is the midpoint of the line segment ab (i.e., the midpoint of the both ends). Examples of X-ray intensities of fluorine and aluminum obtained by line analysis are shown in Figures 1(b) and 1(c). When hydrotalcite particles contain fluorine and aluminum inside, the graph of X-ray intensity normalized by peak intensity shows a shape as shown in Figure 1(b). When hydrotalcite particles contain fluorine derived from a surface treatment agent, the graph of X-ray intensity normalized by peak intensity has peaks near the points a and b at both ends of the fluorine graph, as shown in Figure 1(c). By checking the X-ray intensities derived from fluorine and aluminum in the line analysis, it can be confirmed that the hydrotalcite particles contain fluorine and aluminum inside.
[0115] (Calculation method of the ratio of the atomic concentration of fluorine to aluminum in hydrotalcite particles (element ratio) F / Al) The atomic concentration ratio (element ratio) F / Al of fluorine to aluminum in the hydrotalcite particles obtained from the main component mapping derived from the hydrotalcite particles by the above-mentioned STEM-EDS mapping analysis is obtained in multiple fields of view, and the arithmetic average is taken for 100 or more relevant particles to obtain the atomic concentration ratio (element ratio) F / Al of fluorine to aluminum in the hydrotalcite particles.
[0116] (Method of calculating the ratio of the atomic concentration of magnesium to aluminum in hydrotalcite particles (element ratio) Mg / Al) The same method as for calculating the atomic concentration ratio (element ratio) F / Al of fluorine to aluminum in the hydrotalcite particles described above is performed for magnesium and aluminum to calculate the atomic concentration ratio (element ratio) Mg / Al of magnesium to aluminum in the hydrotalcite particles.
[0117] <Method for measuring number average particle size of primary particles of hydrotalcite particles> The number-average particle size of hydrotalcite particles is measured using a combination of a scanning electron microscope "S-4800" (product name; manufactured by Hitachi) and elemental analysis by energy dispersive X-ray analysis (EDS). The toner to which external additives have been added is observed, and the hydrotalcite particles are photographed at a field of view magnified up to 200,000 times. From the photographed image, hydrotalcite particles are selected, and the major axis of the primary particles of 100 hydrotalcite particles is measured at random to determine the number-average particle size. The observation magnification is adjusted appropriately depending on the size of the external additive. Here, particles that appear as a single grain upon observation are determined to be primary particles.
[0118] <Method for measuring the mass content b (%) of hydrotalcite particles in toner> The mass-based content b (%) of hydrotalcite particles in the toner can be quantified using a calibration curve created from a standard sample by fluorescent X-ray analysis. The fluorescent X-ray measurement of each element conforms to JIS K 0119-1969, specifically as follows. The measurement equipment used was the wavelength dispersive X-ray fluorescence analyzer "Axios" (PANalytic A 300 nm laser scanner (manufactured by PANalytical) and the accompanying dedicated software "SuperQ ver.4.0F" (manufactured by PANalytical) for setting measurement conditions and analyzing measurement data are used. Rh is used as the anode of the X-ray tube, the measurement atmosphere is vacuum, the measurement diameter (collimator mask diameter) is 27 mm, and the measurement time is 10 seconds. A proportional counter (PC) is used to measure light elements, and a scintillation counter (SC) is used to measure heavy elements.
[0119] The measurement sample is prepared by putting 4 g of toner into a dedicated aluminum ring for pressing, flattening it, and pressing it at 20 MPa for 60 seconds using a tablet press to form pellets with a thickness of 2 mm and a diameter of 39 mm. The tablet press used is the "BRE-32" manufactured by Mayekawa Test Machinery Co., Ltd.
[0120] Measurements are performed under the above conditions, and elements are identified based on the peak positions of the obtained X-rays, and their concentrations are calculated from the counting rate (unit: cps), which is the number of X-ray photons per unit time. A separately prepared sample of hydrotalcite particles is added to 100 parts by mass of toner particles so that the amount is 0.10 parts by mass, and the mixture is thoroughly mixed using a coffee mill. Similarly, 0.20 parts by mass and 0.50 parts by mass of hydrotalcite particles are mixed with the toner particles, respectively, to prepare samples for the calibration curve.
[0121] For each sample, the count rate (unit: cps) derived from the metal elements in the hydrotalcite is measured. In this case, the acceleration voltage and current value of the X-ray generator are 24 kV and 100 mA, respectively. A linear calibration curve is obtained by plotting the obtained X-ray count rate on the vertical axis and the amount of hydrotalcite particles added in each calibration curve sample on the horizontal axis. Next, the toner to be analyzed is pelletized as described above using a tablet molding compressor, and the counting rate derived from the metal elements in the hydrotalcite is measured. Then, the mass-based content b (%) of the hydrotalcite particles in the toner is calculated from the calibration curve.
[0122] <Method for confirming that compound A is contained and that compound A is detected as a cation and compound B is detected as an anion> The method of confirming that the compound A and the compound B are contained may be a method using liquid chromatography ESI / MS (electrospray ionization mass spectrometry), 1 Known analytical methods such as H nuclear magnetic resonance spectroscopy can be used. In the present disclosure, an analytical method using liquid chromatography ESI / MS is used. The analytical method is described below. The sample is prepared by using a toner under the dissolution condition A described below, and then separated into a solid content and a supernatant liquid under the centrifugation condition A. The supernatant obtained by the above adjustment is supplied to the liquid chromatograph ESI / MS analyzer described below, and ESI / MS analysis is carried out under analysis condition A.
[0123] Dissolution condition A: At 25°C, 10 times the mass of methanol (JISK8891 equivalent) is used for 10 g of toner, and a multi-stirrer (KSS-8; AS ONE Corporation) is used as the stirring device, and stirring is performed for 10 hours at 200 rpm. A triangle rotor (001.440; AS ONE Corporation) with total length x side length: 40 x 14 mm is used for stirring.
[0124] Centrifugation condition A: Rotation is performed for 30 minutes at 25° C., a rotation radius of 10.1 cm, and a rotation speed of 3500 rpm. As the centrifugation device, a centrifuge (H-9R; manufactured by Kokusan Co., Ltd.) can be used.
[0125] Measurement device: Ultimate3000 (Thermo Fisher Scientific) Mass spectrometer: LCQ Fleet (manufactured by Thermo Fisher Scientific) Analysis condition A: Under the following conditions, ionized materials are detected as cations under the capillary voltage of 35 V and tube lens voltage of 110 V, and ionized materials are detected as anions under the capillary voltage of -35 V and tube lens voltage of -110 V, and MS spectra of the cations and anions are obtained. Ionization method: Electrospray Ionization (ESI) Sheath Gas: 10 (arb. unit.) Aux Gas: 5 (arb. unit.) Spray voltage: 5kV Capillary temperature: 275℃ Mobile phase: Methanol (JISK8891 standard equivalent) Column: Not used (no stationary phase) Flow rate: 1ml / min Injection volume: 10μl Chromatogram detector: UV detector MS acquisition time: 5min MS measurement range: 50-1500 m / z
[0126] <Method of measuring weight average particle size (D4) of toner> The weight-average particle size (D4) of the toner is calculated as follows. The measurement device used is a precision particle size distribution measurement device using the narrow hole electrical resistance method, "Coulter Counter Multisizer 3" (registered trademark, manufactured by Beckman Coulter, Inc.), equipped with a 100 μm aperture tube. The measurement conditions are set and the measurement data is analyzed using the accompanying dedicated software "Beckman Coulter Multisizer 3 Version 3.51" (manufactured by Beckman Coulter, Inc.). The measurement is performed with an effective measurement channel count of 25,000 channels. The electrolyte solution used for the measurement is prepared by dissolving special grade sodium chloride in ion-exchanged water to a concentration of approximately 1% by mass, for example, "ISOTON II" (manufactured by Beckman Coulter). Before carrying out the measurements and analyses, the dedicated software is set up as follows. In the "Change standard measurement method (SOMME)" screen of the dedicated software, set the total count number in the control mode to 50,000 particles, the number of measurements to 1, and the Kd value to the value obtained using "Standard particle 10.0 μm" (Beckman Coulter). Press the "Threshold / Noise level measurement button" to automatically set the threshold and noise level. In addition, set the current to 1600 μA, the gain to 2, the electrolyte to ISOTON II, and check "Flush aperture tube after measurement." In the "Pulse to particle size conversion setting" screen of the dedicated software, the bin interval is set to logarithmic particle size, the particle size bin is set to 256 particle size bins, and the particle size range is set to 2 μm to 60 μm. The specific measurement method is as follows.
[0127] (1) Pour about 200 ml of the electrolyte solution into a 250 ml round-bottom glass beaker made exclusively for the Multisizer 3, set it on the sample stand, and stir the stirrer rod counterclockwise at 24 revolutions per second. Then, remove dirt and air bubbles from inside the aperture tube using the "Aperture Tube Flush" function of the dedicated software. (2) About 30 ml of the electrolyte solution is placed in a 100 ml flat-bottom glass beaker, and about 0.3 ml of a dilution of "Contaminon N" (a 10% aqueous solution of a pH 7 neutral detergent for cleaning precision measuring instruments made of a nonionic surfactant, anionic surfactant, and organic builder, manufactured by Wako Pure Chemical Industries, Ltd.) diluted about three times by mass with ion-exchanged water is added as a dispersant. (3) Two oscillators with an oscillation frequency of 50 kHz are built in with a phase difference of 180 degrees, and An ultrasonic disperser "Ultrasonic Dispersion System Tetra150" (manufactured by Nikkaki Bios Co., Ltd.) with a target output of 120 W is prepared. Approximately 3.3 L of ion-exchanged water is placed in the water tank of the ultrasonic disperser, and approximately 2 ml of Contaminon N is added to this water tank. (4) The beaker from (2) is set in the beaker fixing hole of the ultrasonic disperser, and the ultrasonic disperser is operated. Then, the height position of the beaker is adjusted so that the resonance state of the liquid surface of the electrolyte solution in the beaker is maximized. (5) While the electrolyte solution in the beaker in (4) is irradiated with ultrasonic waves, about 10 mg of toner is added little by little to the electrolyte solution and dispersed. Then, ultrasonic dispersion treatment is continued for another 60 seconds. During ultrasonic dispersion, the water temperature in the water tank is appropriately adjusted to be 10°C or higher and 40°C or lower. (6) Using a pipette, the electrolytic solution (5) in which the toner is dispersed is dropped into the round-bottom beaker (1) placed in the sample stand, and the measurement concentration is adjusted to about 5%. Then, measurements are continued until the number of particles measured reaches 50,000. (7) The measurement data is analyzed using the dedicated software that comes with the device, and the weight-average particle size (D4) is calculated. Note that when the dedicated software is set to Graph / Volume%, the "Average diameter" on the "Analysis / Volume Statistics (Arithmetic Mean)" screen is the weight-average particle size (D4).
[0128] <Method for measuring average circularity> The average circularity of the toner particles is measured using a flow type particle image analyzer "FPIA-3000" (manufactured by Sysmex Corporation) under the measurement and analysis conditions during the calibration process. The specific measurement method is as follows. First, about 20 ml of ion-exchanged water from which impurities such as solids have been removed is placed in a glass container. About 0.2 ml of a dilution of "Contaminon N" (a 10% aqueous solution of a neutral detergent for cleaning precision measuring instruments with a pH of 7, consisting of a nonionic surfactant, an anionic surfactant, and an organic builder, manufactured by Wako Pure Chemical Industries, Ltd.) diluted about three times by mass with ion-exchanged water is added to the container. About 0.02 g of the measurement sample is further added, and the dispersion treatment is performed for 2 minutes using an ultrasonic disperser to obtain a dispersion liquid for measurement. At that time, the dispersion liquid is appropriately cooled so that the temperature is 10°C or higher and 40°C or lower. As the ultrasonic disperser, a tabletop ultrasonic cleaner disperser (e.g., "VS-150" (manufactured by Vervoclear Co., Ltd.) with an oscillation frequency of 50 kHz and an electrical output of 150 W is used, a predetermined amount of ion-exchanged water is placed in the water tank, and about 2 ml of the Contaminon N is added to the water tank.
[0129] For the measurement, the flow type particle image analyzer equipped with "UPlanApro" (magnification 10x, numerical aperture 0.40) was used as the objective lens, and particle sheath "PSE-900A" (manufactured by Sysmex Corporation) was used as the sheath liquid. The dispersion liquid prepared according to the above procedure was introduced into the flow type particle image analyzer, and 3000 toner particles were measured in HPF measurement mode and total count mode. Then, the binarization threshold during particle analysis was set to 85%, and the analyzed particle diameter was limited to a circle equivalent diameter of 1.985 μm or more and less than 39.69 μm, and the average circularity of the toner particles was obtained.
[0130] Before starting the measurement, standard latex particles (e.g., Duke Science Automatic focus adjustment is performed using "RESEARCH AND TEST PARTICLES Latex Microsphere Suspensions 5200A" manufactured by tific (diluted with ion-exchanged water). After that, it is preferable to perform focus adjustment every 2 hours from the start of measurement.
[0131] In the examples of the present application, a flow-type particle image analyzer was used that had been calibrated by Sysmex Corp. and had a calibration certificate issued by Sysmex Corp. Measurements were performed under the same measurement and analysis conditions as when the calibration certificate was received, except that the particle diameters analyzed were limited to a circle-equivalent diameter of 1.985 μm or more and less than 39.69 μm. EXAMPLES
[0132] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is in no way limited thereto. "Parts" used in the examples are by weight unless otherwise specified.
[0133] An example of toner production will now be described. <Production Example of Polyester Resin 1> A reaction vessel equipped with a stirrer, a thermometer, a nitrogen inlet tube, a dehydration tube, and a pressure reducing device was charged with 8.8 parts of ethylene glycol, 45.0 parts of a propylene oxide 2.2 mol adduct of bisphenol A, 4.7 parts of an ethylene oxide 2.2 mol adduct of bisphenol A, 34.3 parts of terephthalic acid, and 0.9 parts of isophthalic acid, and heated to a temperature of 130°C while stirring. Then, 0.52 parts of di(2-ethylhexanoate)tin was added as an esterification catalyst relative to 100.0 parts of the total amount of the monomers, and the temperature was raised to 200°C, and condensation polymerization was performed until the desired molecular weight was obtained. Furthermore, 6.3 parts of trimellitic anhydride were added to obtain an amorphous polyester resin 1. The composition and physical properties of the obtained polyester resin are shown in Table 1.
[0134] <Production example of binder resin 1> Polyester resin 1: 75 parts by mass, vinyl monomers: styrene: 18 parts by mass, n-butyl acrylate: 6.5 parts by mass, mono n-butyl maleate: 0.5 parts by mass, paraffin wax (Mn 450, Mw 520, main peak molecular weight 500, DSC peak temperature 75.0 ° C): 2 parts by mass, and initiator: 2,5-dimethyl-2,5-bis (t-butylperoxy) hexyne-3 (10-hour half-life temperature 128 ° C): 0.08 parts by mass were mixed. This vinyl monomer / polyester resin mixture was polymerized at 120 ° C for 20 hours until the polymerization conversion rate of the vinyl monomer reached 98%, and then the temperature was further raised to 150 ° C and maintained for 5 hours to polymerize the unreacted vinyl monomer, and binder resin 1 was obtained.
[0135] <Production Examples of Polyester Resins 2 to 11> Polyester resins 2 to 11 were obtained in the same manner as in Production Example of Polyester resin 1, except that the amounts of ethylene glycol, 2.2 mol propylene oxide adduct of bisphenol A, and 2.2 mol ethylene oxide adduct of bisphenol A were changed to the amounts shown in Table 1. The compositions and physical properties of the obtained polyester resins 2 to 11 are shown in Table 1.
[0136] [Table 1]
[0137] <Production Example of Polyester Resin 12> In the manufacturing example of polyester resin 1, ethylene glycol was changed to methanediol. Amorphous polyester resin 12 was obtained in the same manner except for the above.
[0138] <Production Example of Polyester Resin 13> Amorphous polyester resin 13 was obtained in the same manner as in Production Example of polyester resin 1, except that ethylene glycol was changed to propanediol.
[0139] <Preparation of Polyester Resin Particle Dispersion 1> Polyester resin 1: 200 parts Ion-exchanged water: 500 parts The above materials were placed in a stainless steel container, heated to 95°C in a hot bath, and melted, and then 0.1 mol / L sodium bicarbonate was added while thoroughly stirring at 7800 rpm using a homogenizer (IKA: Ultra Turrax T50) to make the pH greater than 7.0. Thereafter, a mixed solution of 3 parts of sodium dodecylbenzenesulfonate and 297 parts of ion-exchanged water was gradually added dropwise to emulsify and disperse the mixture, thereby obtaining polyester resin particle dispersion 1. The particle size distribution of this polyester resin particle dispersion 1 was measured using a particle size measuring device (LA-960V2, manufactured by Horiba, Ltd.), and the number average particle size of the polyester resin particles was 0.25 μm, and no coarse particles exceeding 1 μm were observed.
[0140] <Preparation of Resin Particle Dispersion 2> Binder resin 1: 200 parts Ion-exchanged water: 500 parts The above materials were placed in a stainless steel container, heated to 95°C in a hot bath, and melted, and then 0.1 mol / L sodium bicarbonate was added while thoroughly stirring at 7,800 rpm using a homogenizer (IKA: Ultra Turrax T50) to make the pH greater than 7.0. After that, a mixed solution of 3 parts of sodium dodecylbenzenesulfonate and 297 parts of ion-exchanged water was gradually added dropwise to emulsify and disperse the mixture, thereby obtaining resin particle dispersion 2. The particle size distribution of this resin particle dispersion 2 was measured using a particle size measuring device (LA-960V2, manufactured by Horiba, Ltd.), and the number average particle size of the resin particles was 0.25 μm, and no coarse particles exceeding 1 μm were observed.
[0141] <Preparation of Polyester Resin Particle Dispersions 2 to 13> Polyester resin particle dispersions 2 to 13 were obtained in the same manner as in preparation of polyester resin particle dispersion 1, except that polyester resin 1 was changed to polyester resins 2 to 13.
[0142] <Preparation example of wax particle dispersion> -Ion-exchanged water 500 parts Wax (hydrocarbon wax; maximum endothermic peak temperature 77°C) 250 parts The above materials were placed in a stainless steel container, heated to 95°C in a hot bath, and melted. While thoroughly stirring at 7,800 rpm using a homogenizer (IKA Ultra Turrax T50), 0.1 mol / L sodium bicarbonate was added to adjust the pH to greater than 7.0. Thereafter, a mixed solution of 5 parts of sodium dodecylbenzenesulfonate and 245 parts of ion-exchanged water was gradually added dropwise to emulsify and disperse the wax particles. The particle size distribution of the wax particles contained in this wax particle dispersion was measured using a particle size measuring device (LA-960V2, manufactured by Horiba, Ltd.), and the number-average particle size of the wax particles contained was 0.35 μm, and no coarse particles exceeding 1 μm were observed.
[0143] <Preparation example of colorant particle dispersion> Carbon black 100 parts Sodium dodecylbenzenesulfonate 5 parts -Ion-exchanged water 400 parts The above was mixed and dispersed using a sand grinder mill to obtain a colorant particle dispersion. The particle size distribution of the colorant particles contained in this colorant particle dispersion was measured using a particle size measuring device (LA-960V2, manufactured by Horiba, Ltd.), and the number-average particle size of the colorant particles contained was 0.2 μm, and no coarse particles exceeding 1 μm were observed.
[0144] <Production Example of Toner Particle 1> Polyester resin particle dispersion 1: 500 parts Colorant particle dispersion: 50 parts Wax particle dispersion: 50 parts Sodium dodecylbenzenesulfonate: 5 parts Fatty alcohol alkylene oxide adduct (fatty alcohol type: lauryl alcohol, fatty alcohol parts: 190 parts, ethylene oxide parts: 310 parts) 5 parts A reactor (1-liter flask, anchor blade with baffles) was charged with polyester resin particle dispersion 1, wax particle dispersion, sodium dodecylbenzenesulfonate, and aliphatic alcohol alkylene oxide adduct, and mixed uniformly. Meanwhile, a colorant particle dispersion was mixed uniformly in a 500 mL beaker, and this was gradually added to the reactor while stirring to obtain a mixed dispersion. 0.5 parts of aluminum sulfate aqueous solution (solid content) was added dropwise while stirring the obtained mixed dispersion to form aggregated particles. After the dropwise addition was completed, the system was replaced with nitrogen and the mixture was kept at 50°C for 1 hour and then at 55°C for another 1 hour. The temperature was then raised and kept at 90°C for 30 minutes. The temperature was then lowered to 63°C and kept at that temperature for 3 hours to form fused particles. The reaction at this time was carried out in a nitrogen atmosphere. After the specified time had elapsed, the mixture was cooled to room temperature at a rate of 0.5°C per minute. After cooling, the reaction product was subjected to solid-liquid separation under a pressure of 0.4 MPa in a 10 L pressure filter to obtain a toner cake. Thereafter, ion-exchanged water was added to the pressure filter until it was filled with water, and the mixture was washed under a pressure of 0.4 MPa. The mixture was further washed in the same manner for a total of three times. After that, the mixture was subjected to solid-liquid separation under a pressure of 0.4 MPa, and then fluidized bed drying was performed at 45°C to obtain toner particles 1 having a weight average particle size (D4) of 6.8 μm and an average circularity of 0.96.
[0145] <Production Example of Toner Particle 2> Toner particles 2 were obtained in the same manner as in the production example of toner particles 1, except that polyester resin particle dispersion liquid 1 was changed to resin particle dispersion liquid 2.
[0146] <Production Example of Toner Particle 3> Polyester resin 1: 100.0 parts Wax (behenyl behenate, melting point: 72.1°C): 6.0 parts Carbon black Nipex35 (Orion Engineered Carbons): 10 parts Monoazo dye iron complex (T-77, manufactured by Hodogaya Chemical Co., Ltd.): 2.0 parts The above materials were mixed in a Henschel mixer (FM-75, manufactured by Mitsui Mining Co., Ltd.) at a rotation speed of 20 s. -1After mixing for 5 minutes, the mixture was kneaded in a twin-screw kneader (PCM-30, manufactured by Ikegai Corporation) set at a temperature of 130°C. The kneaded mixture was cooled to 25°C and coarsely crushed to 1 mm or less in a hammer mill to obtain a coarsely crushed product. The coarsely crushed product was finely crushed in a mechanical crusher (T-250, manufactured by Turbo Kogyo Co., Ltd.). The product was classified using a multi-division classifier utilizing the Coanda effect to obtain toner particles 3 having a weight average particle size (D4) of 7.5 μm.
[0147] <Production Example of Toner Particle 4> Toner particles 4 were obtained in the same manner as in the production example of toner particles 1, except that the aliphatic alcohol alkylene oxide adduct was changed to sodium dodecylbenzenesulfonate.
[0148] <Production Examples of Toner Particles 5 to 16> In the production example of toner particles 1, polyester resin particle dispersion liquid 1 is Toner particles 5 to 16 were obtained in the same manner except that the child dispersions 2 to 13 were used instead. The relationship between the toner particles, the resin particle dispersion liquid used, and the type of resin is shown in Table 1-2. [Table 1-2]
[0149] <Production Example of Hydrotalcite Particle 1> Hydrotalcite particles 1 were produced as follows. A mixed aqueous solution of 1.03 mol / L magnesium chloride and 0.239 mol / L aluminum sulfate (Liquid A), a 0.753 mol / L aqueous solution of sodium carbonate (Liquid B), and a 3.39 mol / L aqueous solution of sodium hydroxide (Liquid C) were prepared. Next, liquid A, liquid B, and liquid C were poured into the reaction tank using a metering pump at a flow rate that gave a volume ratio of liquid A:liquid B of 4.5:1, and the pH value of the reaction solution was maintained in the range of 9.3 to 9.6 with liquid C, and the reaction temperature was 40°C to generate a precipitate. After filtration and washing, the precipitate was re-emulsified in ion-exchanged water to obtain a raw material hydrotalcite slurry. The hydrotalcite in the obtained hydrotalcite slurry had a concentration of 5.6 mass%. The obtained hydrotalcite slurry was vacuum dried overnight at 40°C. NaF was dissolved in ion-exchanged water to a concentration of 100mg / L, and a solution was prepared by adjusting the pH to 7.0 using 1mol / L HCl or 1mol / L NaOH, to which the dried hydrotalcite was added to a concentration of 0.1% (w / v%). The mixture was stirred at a constant speed for 48 hours using a magnetic stirrer to prevent precipitation. The mixture was then filtered through a membrane filter with a pore size of 0.5μm and washed with ion-exchanged water. The obtained hydrotalcite was vacuum dried overnight at 40°C, and then crushed. The composition and physical properties of the obtained hydrotalcite particles 1 are shown in Table 2.
[0150] <Production Examples of Hydrotalcite Particles 2 to 6> Hydrotalcite particles 2 to 6 were obtained in the same manner as in the production example of hydrotalcite particles 1, except that the concentrations of the A liquid, the B liquid and the NaF aqueous solution were appropriately adjusted. The compositions and physical properties of the nanoparticles 2 to 6 are shown in Table 2.
[0151] <Production Example of Hydrotalcite Particle 7> Hydrotalcite particles 7 were obtained in the same manner as in Production Example of Hydrotalcite Particles 1, except that ion-exchanged water was used instead of the NaF aqueous solution in Production Example of Hydrotalcite Particles 1. The composition and physical properties of the obtained hydrotalcite particles 7 are shown in Table 2.
[0152] [Table 2] The number average particle size indicates the number average particle size of primary particles.
[0153] <Toner 1 Manufacturing Example> Toner particles 1 (100.0 parts) obtained above, hydrotalcite particles 1 (0.310 parts) and silica particles 1 (RX200: primary average particle size 12 nm, HMDS treatment, manufactured by Nippon Aerosil Co., Ltd.) (1.5 parts) were externally added and mixed using FM10C (manufactured by Nippon Coke and Engineering Co., Ltd.). The external addition conditions were as follows: the lower blade was set to A0 blade, the gap with the deflector wall was set to 20 mm, the amount of toner particles charged was 2.0 kg, and the rotation speed was 66.6 s. -1 The external addition time was 10 minutes, and the cooling water temperature was 20°C and the flow rate was 10 L / min. Thereafter, the mixture was sieved through a mesh having an opening of 200 μm to obtain Toner 1. The physical properties of Toner 1 thus obtained are shown in Table 4.
[0154] <Production Examples of Toners 2 to 31> Toners 2 to 31 were obtained in the same manner as in the production example of toner 1, except that the type of toner particles, the type of hydrotalcite particles and the amount added were changed as shown in Table 3. The physical properties of toners 2 to 31 obtained are shown in Table 3. When the hydrotalcite particles were subjected to line analysis by the above-mentioned method, it was confirmed that fluorine and aluminum were present inside the hydrotalcite particles in toners 1 to 24, 26 and 28 to 31. Furthermore, when the hydrotalcite particles of each of the obtained toners were analyzed for F / Al, Mg / Al and number average particle size by the method described above, the same results as shown in Table 2 were obtained. Furthermore, when the content ratio of the structure represented by formula (1), the content c and the content d in the polyester resin were measured by the method described above using each of the obtained toners, the same results as shown in Table 1 were obtained. Toners 1, 2, and 5 to 31 contain compound A and compound B that dissolve in methanol, and when analyzed under analysis condition A, compound A was detected as ionized as a cation, and compound B was detected as ionized as an anion. In toner 3, compounds A and B were not detected, and in toner 4, compound B was detected as ionized as an anion, but compound A was not detected.
[0155] [Table 3] The amount of hydrotalcite added indicates the amount (parts by mass) of hydrotalcite particles added relative to 100.0 parts by mass of toner particles.
[0156] The obtained toner was subjected to the following evaluations. <Image evaluation> Image evaluation was performed using a commercially available color laser printer (HP LaserJet Enterprise Color M555dn, manufactured by HP) that had been partially modified so that it could operate with only one color process cartridge installed. The toner was removed from the black cartridge and replaced with 100 g of the toner to be evaluated, and evaluation was performed.
[0157] [Method for evaluating adhesion of discharged paper] By changing the gear and software of the evaluation machine, the process speed was set to 410 mm / sec and the fixing temperature to 200°C. Under the above conditions, the toner loading amount was 0.45 mg / cm 2 Print a full solid image in continuous double-sided mode and measure it on the evaluation paper. A Canon color laser copier paper (A4: 81.4 g / m 2 While changing the number of sheets of the paper (hereinafter, unless otherwise specified, it is assumed that this paper is used), the paper discharge adhesion rank (NN rank and HH rank) was evaluated in a normal temperature and humidity environment NN (25°C / 50% RH) and a high temperature and high humidity environment HH (30°C / 80% RH; the same applies below). In order to reproduce the temperature rise caused by heat during continuous printing, 50 images were printed first and the printed images were removed from the paper output tray. After that, a specified number of images for evaluation were printed and left on the paper output tray for one minute, after which the bottommost paper (the first printed sheet) of the stack was checked for defects due to adhesion of the image area. Evaluation criteria A: No loss of image area with a load of 400 sheets. B: When the number of sheets loaded is between 250 and 400, loss of the image area occurs. C: When the number of sheets loaded is between 100 and 250, loss of the image area occurs. D: When the number of sheets loaded was less than 100, damage to the image area occurred.
[0158] [Fog] For the purpose of testing the charging property of the toner, fogging in a high temperature and high humidity environment was evaluated by the following method. In a high temperature and high humidity environment, 1,000 images with a print rate of 1.0% were printed per day with a 2 second intermittent time for every two images, for a total of 2,000 images. After printing 2,000 images, the drum fog was taped off and collected for evaluation. The fog density was measured using a reflection densitometer (REFLECTOMETER MODEL TC-6DS, manufactured by TOKYO DENSHOKU CORP.). The fog density (%) was calculated as (Ds-Dr) where Ds is the minimum reflection density of the white background of the tape portion and Dr is the average reflection density of the paper of the taped portion. Measurements were performed using three types of filters: green, amber, and blue, and the minimum value was taken as the fog density. In this evaluation method, if the chargeability of the toner decreases, the fog density on the drum increases. The fog density was evaluated according to the following criteria: C or higher was considered to be good. Evaluation criteria A: Fog density less than 0.5% B: Fog density 0.5% or more and less than 1.5% C: Fog density 1.5% or more and less than 3.0% D: Fog density 3.0% or more
[0159] [Evaluation method for low-temperature fixability (reduction rate of density due to rubbing)] The rate of decrease in rubbing density was measured by removing the fixing device of the above-mentioned evaluation machine from the outside, modifying the fixing device so that the temperature could be arbitrarily set, and using an external fixing device with a process speed of 410 mm / sec. Using the above device, the toner amount per unit area was set to 0.5 mg / cm under normal temperature and humidity conditions. 2 The unfixed image, set at 4.9 kPa (50 g / cm), was passed through the fixing unit, the temperature of which was adjusted to 180° C. The resulting fixed image was fixed at 4.9 kPa (50 g / cm 2The image was rubbed with Silbon paper under a load of 1000 g (1.0 kg), and the image density was evaluated based on the decrease (%) in image density before and after rubbing. Evaluation criteria A: The decrease in image density is less than 5.0%. B: The decrease rate of image density is 5.0% or more and less than 10.0%. C: The decrease rate of image density is 10.0% or more and less than 15.0%. D: The decrease in image density is 15.0% or more.
[0160] [Method for evaluating heat resistance storage stability] 5 g of each toner was placed in a 50 mL resin cup and left for 72 hours at a temperature of 50° C. and a humidity of 10% RH or at a temperature of 55° C. and a humidity of 10% RH. The toner was checked for the presence or absence of agglomerates and ranked according to the temperature range. Evaluation criteria A: No clumps formed B: Slight clumps formed, crumbles when lightly pressed with fingers C: Agglomerates form, but do not crumble when lightly pressed with fingers D: Completely aggregated
[0161] [Examples 1 to 24] In Examples 1 to 24, the above evaluations were carried out using toners 1 to 24, respectively. The evaluation results are shown in Table 4.
[0162] [Table 4]
[0163] [Comparative Examples 1 to 7] In Comparative Examples 1 to 7, the above evaluations were carried out using toners 25 to 31, respectively. The evaluation results are shown in Table 4.
[0164] The present disclosure relates to the following configurations. (Configuration 1) A toner having toner particles containing a binder resin and an external additive, The binder resin contains a polyester resin, The polyester resin contains a structure represented by the following formula (1) in an amount of 10.0 to 30.0% by mass, The external additive contains hydrotalcite particles, In a line analysis in a STEM-EDS mapping analysis of the toner, fluorine and aluminum are present inside the hydrotalcite particles, the ratio F / Al of the atomic concentration of fluorine to aluminum in the hydrotalcite particles, which is obtained from main component mapping of the hydrotalcite particles by STEM-EDS mapping analysis of the toner, is 0.01 to 0.60. TIFF2024165895000009.tif20153(Configuration 2) The toner according to configuration 1, wherein the polyester resin contains the structure represented by formula (1) in an amount of 15.0 to 25.0% by mass. (Configuration 3) 3. The toner according to configuration 1 or 2, wherein the number average particle size of primary particles of the hydrotalcite particles is 60 to 1000 nm. (Configuration 4) The toner according to any one of configurations 1 to 3, wherein when the content of the hydrotalcite particles in the toner based on the mass is designated as b (mass %), the b is 0.050 to 0.500 mass %. (Configuration 5) When the content of the structure represented by the formula (1) in the toner based on mass is a (mass%) and the content of the hydrotalcite particles in the toner based on mass is b (mass%), The toner according to any one of configurations 1 to 4, wherein a and b satisfy the following formula (3): 4.0≦a / b≦100.0 (3) (Configuration 6) The polyester resin contains a structure corresponding to a propylene oxide adduct of bisphenol A and a structure corresponding to an ethylene oxide adduct of bisphenol A, In the polyester resin, when the content of the structure corresponding to the propylene oxide adduct of bisphenol A is c (mass%) and the content of the structure corresponding to the ethylene oxide adduct of bisphenol A is d (mass%), The toner according to any one of configurations 1 to 5, wherein c and d satisfy the following formula (4): 5.0≦c / d≦20.0 (4) (Configuration 7) The toner according to any one of configurations 1 to 6, wherein the content of the structure represented by formula (1) in the toner based on mass is a (mass %), and a is 1.400 to 5.700 mass %. (Configuration 8) The toner according to any one of Configurations 1 to 7, wherein the hydrotalcite particles contain magnesium in addition to the fluorine and aluminum. (Configuration 9) The toner according to any one of configurations 1 to 8, wherein the content of the polyester resin in the binder resin is 60 to 100% by mass. (Configuration 10) 10. The toner according to any one of configurations 1 to 9, wherein the toner particles are emulsion aggregation toner particles. (Configuration 11) The toner contains compound A and compound B which are eluted in methanol when the toner is subjected to an elution treatment under the following elution condition A, The supernatant obtained by centrifuging the eluate in which the compound A and the compound B were eluted in the methanol under the following centrifugation condition A was analyzed by liquid chromatography ESI / MS under the following analysis condition A. The compound A contained in the supernatant is ionized as a cation and detected, 11. The toner according to any one of configurations 1 to 10, wherein the compound B contained in the supernatant is detected as an anion. Dissolution condition A: At 25° C., 10 times the mass of the toner is used in methanol (JIS K8891 equivalent), and the toner is stirred for 10 hours at a rotor speed of 200 rpm using a stirring device. Centrifugation condition A: Rotation is performed for 30 minutes at 25° C., a rotation radius of 10.1 cm, and a rotation speed of 3,500 rpm. Analysis condition A: Sheath Gas: 10 (arb. unit.), Aux Gas: 5 (arb. unit.), spray voltage: 5 kV, capillary temperature: 275°C. Ionized substances are detected as cations under the conditions of capillary voltage: 35 V, tube lens voltage: 110 V, and ionized substances are detected as anions under the conditions of capillary voltage: -35 V, tube lens voltage: -110 V. (Configuration 12) The compound A is at least one compound selected from the group consisting of an ethylene oxide adduct of a linear aliphatic alcohol having 8 to 16 carbon atoms and sodium polyoxyethylene lauryl ether acetate, 12. The toner according to claim 11, wherein the compound B is linear or branched sodium dodecylbenzenesulfonate. [Explanation of symbols]
[0165] 1: toner particle 1, 2: toner particle 2, 3: hydrotalcite particle, 4: boundary of toner particle, 5: analysis direction of line analysis
Claims
1. A toner having toner particles containing a binder resin and an external additive, The binder resin contains a polyester resin, The polyester resin contains 10.0 to 30.0 mass % of a structure represented by the following formula (1), The external additive contains hydrotalcite particles, In a line analysis in a STEM-EDS mapping analysis of the toner, fluorine and aluminum are present inside the hydrotalcite particles, the ratio F / Al of the atomic concentration of fluorine to aluminum in the hydrotalcite particles, which is obtained from main component mapping of the hydrotalcite particles by STEM-EDS mapping analysis of the toner, is 0.01 to 0.
60.
2. 2. The toner according to claim 1, wherein the polyester resin contains the structure represented by the formula (1) in an amount of 15.0 to 25.0% by mass.
3. 2. The toner according to claim 1, wherein the number average particle size of the primary particles of the hydrotalcite particles is 60 to 1000 nm.
4. 4. The toner according to claim 1, wherein the content of the hydrotalcite particles in the toner based on the mass is defined as b (mass %), and the b is 0.050 to 0.500 mass %.
5. When the content of the structure represented by the formula (1) in the toner based on the mass basis is a (mass %) and the content of the hydrotalcite particles in the toner based on the mass basis is b (mass %), The toner according to any one of claims 1 to 3, wherein a and b satisfy the following formula (3): 4.0≦a / b≦100.0 (3)
6. The polyester resin contains a structure corresponding to a propylene oxide adduct of bisphenol A and a structure corresponding to an ethylene oxide adduct of bisphenol A, In the polyester resin, when the content of the structure corresponding to the propylene oxide adduct of bisphenol A is c (mass%) and the content of the structure corresponding to the ethylene oxide adduct of bisphenol A is d (mass%), The toner according to any one of claims 1 to 3, wherein c and d satisfy the following formula (4): 5.0≦c / d≦20.0 (4)
7. The toner according to any one of claims 1 to 3, wherein the content of the structure represented by formula (1) in the toner based on mass is a (mass %), and a is 1.400 to 5.700 mass %.
8. 4. The toner according to claim 1, wherein the hydrotalcite particles contain magnesium in addition to the fluorine and aluminum.
9. The content of the polyester resin in the binder resin is 60 to 100% by mass. The toner according to any one of claims 1 to 3.
10. The toner of any one of claims 1 to 3, wherein the toner particles are emulsion aggregation toner particles.
11. The toner contains compound A and compound B which are soluble in methanol when the toner is subjected to an elution treatment under the following elution condition A, The supernatant obtained by centrifuging the eluate in which the compound A and the compound B were eluted in methanol under the following centrifugation condition A was analyzed by liquid chromatography ESI / MS under the following analysis condition A. The compound A contained in the supernatant is ionized as a cation and detected, 4. The toner according to claim 1, wherein the compound B contained in the supernatant is detected as an anion. Dissolution condition A: At 25° C., methanol (equivalent to JIS K8891 standard) in an amount 10 times the mass of the toner is used, and the toner is stirred for 10 hours at a rotor speed of 200 rpm using a stirring device. Centrifugation condition A: Rotation was performed at 25° C., a rotation radius of 10.1 cm, and a rotation speed of 3,500 rpm for 30 minutes. Analysis condition A: Sheath gas: 10 (arb. unit), Aux gas: 5 (arb. unit), spray voltage: 5 kV, capillary temperature: 275° C., ionized substances are detected as cations under the conditions of capillary voltage: 35 V, tube lens voltage: 110 V, and ionized substances are detected as anions under the conditions of capillary voltage: −35 V, tube lens voltage: −110 V.
12. The compound A is at least one compound selected from the group consisting of an ethylene oxide adduct of a linear aliphatic alcohol having 8 to 16 carbon atoms and sodium polyoxyethylene lauryl ether acetate, The toner according to claim 11, wherein the compound B is linear or branched sodium dodecylbenzenesulfonate.
Citation Information
Patent Citations
Toner
JP2019045578A