Method of applying coating and coating material set
A multi-component reaction-curing paint method with a curing rate regulator containing alcohol addresses the viscosity increase issue in two-component reactive paints, providing a long pot life and effective application in industrial settings.
Patent Information
- Application Number
- JP2023082522
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-18
- Publication Date
- 2024-11-28
AI Technical Summary
Conventional two-component reactive paints experience a rapid increase in viscosity after mixing, making them difficult to apply over extended periods, especially in industrial settings where a longer pot life is required.
A multi-component reaction-curing paint method involving a main agent, curing agent, and a curing rate regulator containing alcohol is used, which suppresses viscosity increase and extends the pot life by controlling the curing rate.
The method achieves a low viscosity increase rate and long pot life, enabling effective application in industrial settings such as decorative film coating, with improved coating properties and extended usability.
Smart Images

Figure 2024165926000001 
Figure 2024165926000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a coating method and a coating set for a multi-component paint. [Background technology]
[0002] There are various types and characteristics of paints, such as lacquer-type paints that dry with one liquid, crosslinkable paints with one liquid, multi-liquid mixed paints that are mixed with two or more liquids when used for painting, powder paints, water-based paints, solvent-based paints, energy ray curing paints, room temperature drying paints, heat drying paints, etc., and they are used according to the usage environment, the object to be painted, and the intended performance. Among these, two-liquid reactive curing paints, which are used by mixing the base agent and the hardener just before painting, are often used as room temperature drying paints for buildings and structures, automobile repair, etc., and it is common to use paints that are adjusted according to the application so that the pot life after mixing is about 1 to 8 hours from the viewpoint of being a paint with good paint workability until the painting on the object is completed after mixing and quickly drying and curing after painting to perform the next stage of painting or to complete the painting.
[0003] Meanwhile, in recent years, methods of protecting and decorating a substrate using a film instead of a paint have also been studied. JP 2002-234077 A (Patent Document 1) describes a coating film laminated inorganic building material obtained by bonding a coating film to the surface of an inorganic building material by heat and / or pressure. Patent Document 1 describes that inorganic building materials generally used have a porous structure and are subjected to various processes, so that it is difficult to form a uniform coating film when coating with a paint, and there are problems such as cracking and peeling of the coating film itself. However, it is described that a method of bonding a coating film to the surface of an inorganic building material by heat and / or pressure can solve the problems that arise when coating with a paint. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2002-234077 A Summary of the Invention [Problem to be solved by the invention]
[0005] However, in the two-component reactive paint of the type in which components A and B are mixed, as disclosed in Example 3 of Patent Document 1, a uniform coating film can be formed when the two components are mixed and applied immediately, but as time passes after mixing, the viscosity of the paint increases due to the progress of the reaction, making application difficult. In particular, in film coating at factories, paint is used for long periods of time, so a longer pot life is required compared to the pot life of two-component reactive paints for buildings and structures. In other words, a two-component reactive paint that has a small rate of increase in viscosity over time after mixing the two components and can be applied well for a long period of time is required, but this was difficult to achieve with conventional technology.
[0006] SUMMARY OF THE PRESENT EMBODIMENT An object of the present invention is to provide a method for applying a paint which has a low rate of viscosity increase after mixing and a long pot life. [Means for solving the problem]
[0007] As a result of intensive research into achieving the above-mentioned object, the present inventors have discovered that when mixing and applying a multi-component reactive curing paint containing (A) a base agent and (B) a curing agent, a coating method can be provided in which the viscosity increase rate of the paint can be suppressed and the pot life is sufficiently long by separately preparing a curing rate regulator containing (C) an alcohol and mixing the two before applying the mixture to a coating medium, thereby providing a coating method which has suppressed the viscosity increase rate of the paint and has sufficiently long pot life, and have thus completed the present invention.
[0008] Therefore, the coating method of the present invention is a method for coating a multi-component reactive curing paint, characterized in that (A) a base agent, (B) a curing agent, and (C) a curing rate regulator containing an alcohol are prepared in advance, and then mixed prior to coating to prepare a coating composition (X), which is then applied to a coating medium.
[0009] Another embodiment of the present invention is a method for applying a multi-component reactive coating composition containing at least (A) a base agent and (B) a curing agent, wherein the base agent (A) contains a curing rate regulator containing (C) an alcohol, and the base agent (A) and the curing agent (B) are mixed prior to application to prepare a coating composition (Y), which is then applied to a coating medium.
[0010] In a preferred embodiment of the coating method of the present invention, the (B) curing agent contains an isocyanate.
[0011] In another preferred embodiment of the coating method of the present invention, after preparation of the coating composition (X), the viscosity increase rate of the coating composition (X) after 4 hours at 23°C is within twice the initial viscosity of the coating composition (X) when mixed with the paint, and the gel fraction of the coating film after drying is 80% or more.
[0012] In another preferred embodiment of the coating method of the present invention, after preparation of the coating composition (Y), the viscosity increase rate of the coating composition (Y) after 4 hours at 23°C is within twice the initial viscosity of the coating composition (Y) when mixed with the coating composition (Y), and the gel fraction of the coating film after drying is 80% or more.
[0013] Another aspect of the present invention is a paint set comprising at least (A) a base resin, (B) a curing agent, and (C) a curing rate regulator containing an alcohol. Effect of the Invention
[0014] According to the present invention, it is possible to provide a coating method that suppresses the rate of increase in viscosity of the coating material after mixing, has a long pot life, and is applicable to factory coating such as decorative film coating, and a coating set that realizes the method. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] The present invention relates to a paint application method and a paint set. The coating method of the present invention is a method for coating a substrate with a paint. In this case, examples of the substrate include, in addition to films, metal substrates such as iron, stainless steel, aluminum, copper, titanium, and alloys thereof, inorganic substrates other than metals such as cement, concrete, gypsum, calcium silicate, calcium carbonate, marble, artificial marble, glass, and ceramics, wood substrates, plastic substrates such as epoxy resin, ABS resin, polycarbonate, polyvinyl chloride, polystyrene, acrylic resin, and in particular polymethyl methacrylate (PMMA), polyethylene terephthalate (PET), and polypropylene (PP), as well as composite substrates combining two or more of these substrates.
[0016] When the substrate is a film, the substrate film layer is preferably composed of a resin film. The resin used in the film is preferably a thermoplastic resin, such as acrylonitrile-butadiene-styrene resin (ABS resin), acrylonitrile-styrene-acrylic acid ester resin, acrylic resin, polyolefin resin such as polypropylene and polyethylene, polycarbonate resin, vinyl chloride resin such as polyvinyl chloride (PVC), polyethylene terephthalate (PET) resin, polyphenylene ether (PPE) resin, etc. Among these, acrylic resin, ABS resin, and PVC resin are particularly preferable. The resin may be used alone or in combination of two or more kinds.
[0017] In the present invention, the substrate may have various shapes, for example, a two-dimensional substrate such as a film, sheet, or plate, or a three-dimensional substrate that is a complex three-dimensional object. The surface of the substrate may be smooth or may have irregularities. In addition, the substrate in the present invention may have a surface previously coated with paint, ink, or the like.
[0018] First, the coating method of the present invention will be described. The coating method of the present invention is a coating method including the following two steps. First process: (A) a base agent, (B) a hardener, and (C) a hardening rate regulator containing alcohol, or (A) a base agent containing an alcohol-containing hardening rate regulator and (B) a hardener are prepared separately and then mixed to form a single paint. The second step is to apply the coating material prepared in the first step onto a substrate.
[0019] In the coating method of the present invention, in addition to the main agent (A) and the hardener (B), a hardening rate regulator containing alcohol (C) is prepared, and the coating material mixed with this is applied, thereby suppressing the increase in viscosity of the coating material, and sufficient pot life can be ensured, for example, when coating in a factory to create a decorative film and forming a coating layer. The main agent (A) and the hardening rate regulator containing alcohol (C) may be prepared separately and mixed before coating, but the main agent (A) and the hardening rate regulator containing alcohol (C) may be mixed in advance and mixed with the hardener (B) before coating. In the present invention, the coating composition prepared by preparing the main agent (A), the hardener (B), and the hardener containing alcohol (C) in advance and mixing them before coating is called coating composition (X), and the coating composition prepared by mixing the main agent (A) and the hardener containing alcohol (C) before coating is called coating composition (Y).
[0020] In the present invention, the coating layer means a coating layer formed by painting, among layers disposed on a substrate.
[0021] In the first step, other components may be prepared and mixed in addition to (A) the base resin, (B) the curing agent, and (C) the alcohol-containing curing rate regulator.
[0022] In the first step, the (A) main agent usually contains a resin. Examples of the resin include acrylic resin, silicone resin, acrylic silicone resin, styrene acrylic copolymer resin, polyester resin, fluororesin, rosin resin, petroleum resin, coumarone resin, phenol resin, urethane resin, melamine resin, urea resin, epoxy resin, cellulose resin, xylene resin, alkyd resin, aliphatic hydrocarbon resin, butyral resin, maleic acid resin, fumaric acid resin, vinyl resin (e.g. vinyl chloride resin), amine resin, ketimine resin, etc. Among these, from the viewpoint of reacting and curing with the (B) curing agent, it is preferable that the resin has at least one functional group selected from the group consisting of a hydroxyl group, a carboxyl group, an epoxy group, an amino group, an amide group, an imide group, and an alkoxymethyl group, and it is particularly preferable that the resin contains a hydroxyl group.
[0023] Examples of the resin containing a hydroxyl group include a hydroxyl group-containing acrylic resin, a hydroxyl group-containing polyester resin, a hydroxyl group-containing polycarbonate resin, a hydroxyl group-containing polyurethane resin, a hydroxyl group-containing epoxy resin, a hydroxyl group-containing alkyd resin, etc. These may be used alone or in combination of two or more.
[0024] In the first step, the curing agent (B) is not particularly limited as long as it is a commonly used curing agent such as isocyanate, carbodiimide, oxazoline, melamine, amine, etc., and a wide variety of conventionally known curing agents can be used, but from the viewpoint of reaction with the hydroxyl group-containing resin, it is more preferable to include at least one selected from isocyanate and carbodiimide. These curing agents (B) start to react when mixed with the main agent (A), and can form a coating film with high crosslink density and excellent physical properties such as water resistance, acid resistance, and alkali resistance. The compounding ratio of the (A) base agent and the (B) curing agent is preferably determined from the equivalent ratio. For example, when the (A) base agent contains a hydroxyl group and the (B) curing agent contains an isocyanate, the equivalent ratio (NCO / OH) is preferably 0.6 to 2.2, more preferably 0.7 to 2.0, and particularly preferably 0.8 to 1.8.
[0025] The alcohol-containing curing rate regulator in the first step (C) has a function of adjusting the curing rate of the base resin (A) and the curing agent (B). In this specification, the alcohol-containing curing rate regulator in the first step (C) is also referred to as the "curing rate regulator of the present invention."
[0026] Examples of the alcohols used in the curing rate regulator of the present invention include monohydric alcohols and polyhydric alcohols.
[0027] A monohydric alcohol is an organic compound having one hydroxyl group in one molecule, and includes linear monohydric alcohols such as methanol, ethanol, n-propanol, n-butanol, n-pentanol, n-hexanol, n-heptanol, n-octanol, n-nonanol, n-decanol, n-undecanol, n-dodecanol (lauryl alcohol), n-tridecanol, n-tetradecanol, n-pentadecanol, n-hexadecanol, n-heptadecanol, n-octadecanol (stearyl alcohol), n-nonadecanol, and eicosanol. Examples of alcohols include branched monohydric alcohols such as isopropanol, isobutanol, sec-butanol, tert-butanol, isopentanol, isohexanol, isoheptanol, isooctanol, 2-ethylhexane-1-ol, isononanol, isodecanol, 5-ethyl-2-nonanol, trimethylnonyl alcohol, 2-hexyldecanol, 3,9-diethyl-6-tridecanol, 2-isoheptylisoundecanol, 2-octyldodecanol, and other branched alkanols (having 5 to 20 carbon atoms).
[0028] The polyhydric alcohol is an organic compound having two or more hydroxyl groups in one molecule, and examples thereof include alkanediols such as ethylene glycol, propylene glycol (1,2- or 1,3-propanediol or a mixture thereof), butylene glycol (1,2-, 1,3-, or 1,4-butanediol or a mixture thereof), 1,5-pentanediol, 1,6-hexanediol, neopentyl glycol, 3-methyl-1,5-pentanediol, 2,2,2-trimethylpentanediol, and 3,3-dimethylolheptane; and examples thereof include diethylene glycol, triethylene glycol, dipropylene glycol, and the like. Examples of the aliphatic polyhydric alcohols include dihydric alcohols such as ether diols such as glycol; trihydric alcohols such as glycerin, trimethylolpropane, and triisopropanolamine; tetrahydric alcohols such as tetramethylolmethane (pentaerythritol) and diglycerin; pentahydric alcohols such as xylitol; hexahydric alcohols such as sorbitol, mannitol, allitol, iditol, dulcitol, altritol, inositol, and dipentaerythritol; heptahydric alcohols such as perseitol; and octahydric alcohols such as sucrose.
[0029] The alcohols are preferably monohydric alcohols or dihydric alcohols, more preferably monohydric alcohols having a molecular weight of 70 to 170, more preferably butanol, isobutanol, isopropanol, propylene glycol monomethyl ether, ethylene glycol monobutyl ether, diethylene glycol monobutyl ether, tert-butanol, etc. Among them, monohydric alcohols having a molecular weight of 80 or less are particularly preferred because they effectively suppress the viscosity increase rate of the coating material and have excellent drying properties and film-forming properties after application.
[0030] The alcohols used in the curing rate regulator of the present invention preferably have a boiling point of 70°C or higher, and more preferably have a boiling point of 80°C or higher but lower than 250°C. In the present invention, the curing rate regulator is used when mixing with the (B) curing agent, and has the effect of slowing down the curing rate of the (A) base agent and the (B) curing agent, and extending the usable time of the paint after mixing. By using a curing rate regulator containing an alcohol with a boiling point of 80°C or higher but lower than 250°C, the curing rate is slowed down, the viscosity increase rate of the paint is suppressed, and after curing, a coating film with a high crosslink density can be formed, similar to when the (C) curing rate regulator is not contained.
[0031] In the first step, it is preferable that the (A) base agent and / or the (B) curing agent contains a solvent component such as an organic solvent. These solvents can be used without limitation as long as they are normally used in paints. The amount of the solvent in the paint is preferably within the range of 10 to 95% by mass, and more preferably within the range of 20 to 90% by mass. The present invention is particularly effective in non-aqueous paints such as weak solvent paints and strong solvent paints.
[0032] In the first step, the (A) base agent and / or the (B) curing agent may contain, as other components, appropriately as necessary, a pigment, a solvent, a dispersant, an antioxidant, an antisettling agent, an antifoaming agent, a silane coupling agent, an adhesion imparting agent, an anti-algae agent, an anti-fungal agent, a preservative, an insecticide, an antibacterial agent, an antiviral agent, an ultraviolet absorber, a radical scavenger, an antistatic agent, a conductivity imparting agent, and the like.
[0033] In the second step, the substrate may be previously coated with paint, ink, or the like, and the coating layer applied onto the substrate may be one layer or two or more layers.
[0034] In the second step, the coating layer provided on the substrate preferably has a thickness of 120 μm or less, more preferably 5 to 80 μm. When the coating layer is made up of multiple layers, the numerical range described here refers to the total thickness of the coating layers. In the second step of the present invention, two or more coating layers may be formed using the same paint, or two or more layers may be formed using different paints.
[0035] In the second step, the coating layer is obtained by applying a paint to the substrate by a known coating means, such as brush coating, roller coating, trowel coating, spatula coating, roll coater coating, flow coater coating, spray coating (e.g., air spray coating, airless spray coating), shower coater coating, dipping coating, etc.
[0036] In the second step, the means for drying the coating layer is not particularly limited, and may be either natural drying at ambient temperature or forced drying using a dryer or the like.
[0037] The coating method of the present invention is particularly effective when the substrate is a film such as a decorative film. In particular, when coating a decorative film using a roll-to-roll method, the decorative film coated with the first layer is once wound into a roll, then the roll is opened again to coat the second layer, and then wound into a roll again. This requires that the paint has a sufficient pot life and excellent drying properties. The coating method of the present invention is suitable for roll-to-roll coating because it ensures a pot life and has excellent drying properties. Here, decoration means providing a design or imparting a different texture. The design means a shape, pattern, or color, or a combination of these.
[0038] In the present invention, when the substrate is a decorative film, the objects to which the film is applied include various articles, and are preferably automobiles and automobile parts, exterior and interior materials for housing, electrical appliances, small items, interior goods, etc. The materials of the objects to which the decorative film is applied are also diverse, and examples of such materials include plastics and metals.
[0039] In the present invention, the decorative film may have a multi-layer structure. Examples of the multilayer structure include adhesive layer / substrate film layer / primer layer / glossy layer / clear layer, clear layer / substrate film layer / primer layer / glossy layer / adhesive layer, adhesive layer / substrate film layer / enamel layer / clear layer, adhesive layer / substrate film layer / primer layer / enamel layer, adhesive layer / substrate film layer / primer layer / enamel layer / clear layer, substrate film layer / adhesive layer / primer layer / glossy layer / clear layer, substrate film layer / adhesive layer / enamel layer, substrate film layer / adhesive layer / enamel layer / clear layer, substrate film layer / adhesive layer / primer layer / enamel layer / clear layer, substrate film layer / adhesive layer / primer layer / enamel layer / clear layer, adhesive layer / molded film layer / primer layer / enamel layer, adhesive layer / molded film layer / primer layer / enamel layer / clear layer, adhesive layer / primer layer / enamel layer, adhesive layer / primer layer / enamel layer / clear layer, adhesive layer / primer layer / enamel layer, adhesive layer / primer layer / enamel layer / clear layer, and those in which the enamel layer or glossy layer is a printed layer.
[0040] As the molding method, coating method and printing method that can be used for producing the film, conventionally known molding methods, coating methods and printing methods can be used. For example, when using a film composed only of a coating film or a film composed only of a printed film, a coating film (single layer or laminate) or a printed film (single layer or laminate) is formed on a support such as polypropylene, and the coating film or the printed film is peeled off from the support to obtain a coated film.
[0041] Examples of molding methods that can be used to produce the film include injection molding, blow molding, extrusion molding, vacuum molding, and pressure molding.
[0042] Examples of coating methods that can be used in producing the film include dipping and coating methods using a coater such as a bar coater, die coater, roll coater, comma coater, knife coater, or gravure coater.
[0043] Examples of printing methods that can be used in producing the film include inkjet (IJ) printing, gravure printing, flexographic printing, and design spray printing.
[0044] The thickness of the coating layer when applied to the film is preferably 250 μm or less, more preferably 10 to 180 μm. If the coating layer is too thick, for example, when a coating layer including a film is provided on a substrate having an uneven shape, it is preferable that the coating layer is not too thick from the viewpoint of setting the coating layer in a state following the unevenness of the substrate. When the coating layer on the film is composed of multiple layers, the numerical range of thickness described here refers to the total thickness of the coating layer.
[0045] The coating layer on the film may be colored or transparent, and may be coated over the entire surface or only partially.
[0046] When the substrate is a decorative film, an adhesive layer may be provided on one surface of the film layer. The decorative film can be attached to an object to be decorated via the adhesive layer.
[0047] The adhesive layer is a layer composed of an adhesive. The adhesive layer and the adhesive may be called a pressure-sensitive adhesive layer and a pressure-sensitive adhesive, respectively. Examples of the adhesive include a urethane adhesive, an acrylic adhesive, an epoxy adhesive, and a rubber adhesive, and among these, an acrylic adhesive is preferred.
[0048] When the substrate of the present invention is a decorative film, from the viewpoint of adhesion of the decorative film to an object, it is preferable that either one of the coating layer obtained by the second step and the adhesive layer provided on the surface of the film layer contains an acrylic resin, and it is even more preferable that both the coating layer and the adhesive layer contain an acrylic resin.
[0049] The thickness of the adhesive layer is preferably 20 to 200 μm.
[0050] The adhesive layer can be formed by applying an adhesive to the surface of the decorative film layer. A film-like adhesive layer can also be attached to the decorative film layer.
[0051] Next, the viscosity increase rate and the gel fraction of the coating film in the coating method of the present invention will be described.
[0052] In a reactive curing paint in which (A) the base agent and (B) the hardener are mixed and applied, the crosslinking reaction proceeds by mixing, so the viscosity of the paint increases, and after application and drying, the crosslinked coating film provides high coating film properties. The gel fraction is used as a measure of the degree of crosslinking of the coating film. When applying the paint to a decorative film on a factory line, the preferred viscosity increase rate is about 2 to 5 times the initial mixing rate, depending on the type of paint, initial viscosity, and coating machine, and the continuous application time is required to be about 4 to 18 hours. In addition, the reaction rate of the paint also depends on the temperature, but assuming that the paint is applied at room temperature to slight heating, it is considered that the paint can be applied during factory production if the viscosity increase rate after mixing (A) the base agent, (B) the hardener, and (C) the hardening rate regulator containing alcohol at 23°C is within 2 times the initial rate after 4 hours, and preferably within 5 times the initial rate after 19 hours.
[0053] The viscosity in the present invention is the viscosity at 10 (1 / s) and 100 (1 / s) measured with a rheometer (e.g., Physical MCR301) of a paint adjusted to 23° C. In applying the paint, it is preferable to adjust both the viscosity during application and the viscosity after application, so it is preferable that the viscosity at 10 (1 / s) and 100 (1 / s) is within twice the original value even after 4 hours.
[0054] The viscosity of the paint in the present invention is not particularly limited, and what is important is that the rate of increase in viscosity of the paint is low up to 8 hours, and particularly up to 19 hours, after mixing of the paint. The initial viscosity is, for example, within the range of 20 to 100 mPa s at 10 (1 / s), and within the range of 20 to 100 mPa s at 100 (1 / s).
[0055] Here, it is preferable that the curing rate regulator containing alcohol (C) adjusts the curing rate so that the curing reaction between the main agent (A) and the curing agent (B) proceeds slowly, but does not deteriorate the physical properties of the coating film formed. Therefore, it is preferable that the gel fraction of the coating film obtained by applying the coating composition (X) and / or the coating composition (Y) is 80% or more when completely cured. Here, the "complete curing of the coating film" in the present invention refers to the time when the coating composition is naturally dried at room temperature or forcedly dried by heating or the like to volatilize the solvent (volatile components), and then aged at 23°C for 6 days. In addition, in the case of roll-to-roll coating, it is preferable that the gel fraction of the coating film before winding up on the roll is 50% or more.
[0056] The gel fraction is an index that indicates the degree of resistance of a coating film to an organic solvent. In this specification, the gel fraction of a coating film refers to the mass ratio of the coating film that remains without dissolving when a 100 mm x 100 mm coating film is immersed in an organic solvent. Specifically, when the mass of the coating film before immersion is M1 and the mass of the coating film after immersion is M2, the gel fraction of the coating film can be calculated from the following formula. Gel fraction (%) = M2 / M1 × 100 Here, immersion refers to immersing the coating film in a mixed solution of toluene and acetone (mass ratio 1:1) of 100 g per 1 g of coating film under reflux for 5 hours. The mass of the coating film after immersion is the mass of the coating film after drying at 105°C for 30 minutes.
[0057] By adjusting the type and amount of (A) base resin, (B) curing agent, and (C) alcohol-containing curing rate regulator, the viscosity increase rate after 19 hours from mixing at 23°C can be kept within 2 times, and the gel fraction after 6 days from coating can be made 80% or more. Specifically, it can be adjusted by appropriately adjusting the glass transition point (Tg) and hydroxyl value of the resin used in the coating material and the functional group content of the curing agent, adjusting the equivalent ratio of (A) base resin and (B) curing agent, adjusting the blending amount of (C) alcohol-containing curing rate regulator, etc. The blending amount of (C) alcohol-containing curing rate regulator is preferably 5 to 30 mass% of the amount of binder resin contained in (A) base resin. When the amount of the alcohol-containing curing rate regulator (C) is large, a high viscosity increase suppression effect and a pot life extension effect can be obtained, but when the amount of the alcohol-containing curing rate regulator (C) is too large, the curing reaction between the base agent (A) and the curing agent (B) is inhibited, the gel fraction of the resulting coating film is reduced, and the coating film properties such as acid resistance and alkali resistance may be reduced. In particular, the action of the alcohol-containing curing rate regulator (C) may deactivate the curing agent (B), resulting in a low gel fraction of the coating film after curing. In addition, when the gel fraction is low, it is likely to be difficult to wind up the coating film using a roll-to-roll method, so that when coating is performed using a roll-to-roll method, it is preferable that the gel fraction of the coating film when completely cured is 80% or more and the gel fraction when wound up is 50% or more.
[0058] The blending amount of the alcohol-containing curing rate regulator (C) relative to the base resin (A) is preferably 3 to 15 mass %.
[0059] Next, the paint set of the present invention will be described.
[0060] The paint set of the present invention contains at least (A) a base agent, (B) a curing agent, and (C) a curing rate regulator containing alcohol. (A) base agent and (C) a curing rate regulator containing alcohol may be prepared separately or may be prepared by mixing them in advance. Since (B) a curing agent reacts with (A) base agent and cures, the paint set of the present invention is a paint set consisting of (A) base agent, (B) a curing agent, and (C) an alcohol, or a paint set consisting of (A) base agent, (C) a curing rate regulator containing alcohol, and (B) a curing agent. The contents of each are as described in the explanation of the coating method above. EXAMPLES
[0061] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples in any way.
[0062] <Paint preparation> The paints of Examples 1 to 25 and Comparative Examples 1 to 6 were prepared according to the following mixing ratios. (A) Main component Main Agent No.1 The materials were mixed in a solid mass ratio of acrylic resin A / polyester resin A / polyester resin B = 70 / 10 / 20 and dispersed by a known method to prepare a paint. Acrylic resin A: solid content 69% by mass, acid value 9.0 mgKOH / g, hydroxyl value 117 mgKOH / g Polyester resin A: solid content 100% by mass, acid value 3.3 mgKOH / g, hydroxyl value 110 mgKOH / g Polyester resin B: solid content 80% by mass, acid value 1.8 mgKOH / g, hydroxyl value 3.5 mgKOH / g Main Agent No.2 The materials were mixed in a solid mass ratio of acrylic resin B / acrylic resin C / polyester resin A = 49 / 21 / 30 and dispersed by a known method to prepare a paint. Acrylic resin B: solid content 50% by mass, acid value 4.0 mgKOH / g, hydroxyl value 0 mgKOH / g Acrylic resin C: solid content 50% by mass, acid value 3.0 mgKOH / g, hydroxyl value 0 mgKOH / g Polyester resin A: solid content 100% by mass, acid value 3.3 mgKOH / g, hydroxyl value 110 mgKOH / g (B) Hardener Hardener No.1 The isocyanate curing agent A and the isocyanate curing agent B were mixed in a solid mass ratio of 50 / 50 to prepare curing agent No. 1. The materials used are as follows: Isocyanate curing agent A: Product name Sumidur N3800, solid content 100% by mass, NCO group content 11.0% by mass, manufactured by Sumika Covestro Urethane Co., Ltd. Isocyanate curing agent B: Product name Sumidur Z4470MPA / X, solid content 100% by mass, NCO group content 11.9% by mass, manufactured by Sumika Covestro Urethane Co., Ltd. Hardener No.2 The materials used for Hardener No. 2 are as follows: Isocyanate curing agent C: Burnock DN-990S, solid content 100% by mass, NCO group content 17.0% by mass, manufactured by DIC Corporation (C) Alcohol-containing hardening rate regulator nBOH: n-butanol, molecular weight 74.12, boiling point 117.7℃, primary alcohol IBOH: Isobutanol, molecular weight 74.12, boiling point 108°C, primary alcohol IPOH: Isopropanol, molecular weight 60.9, boiling point 83°C, secondary alcohol PM: Propylene glycol monomethyl ether, molecular weight 90.12, boiling point 120℃, primary alcohol ·CCB: Ethylene glycol monobutyl ether, molecular weight 111.18, boiling point 171℃, secondary alcohol 2CCB: Diethylene glycol monobutyl ether, molecular weight 162.23, boiling point 230℃, primary alcohol ·tBOH: tert-butanol, molecular weight 74.12, boiling point 83℃, tertiary alcohol (Other solvents) MEK: Methyl ethyl ketone, molecular weight 72.11, boiling point 79.6℃, ketone solvent ·BA: Butyl acetate, 116.16, boiling point 126.1℃, ester solvent
[0063] <Example 1> <Preparation of isolation membrane for gel fraction measurement> Base agent No. 1 and hardener No. 1 were mixed to an equivalent ratio of 1.6, and the hardening speed regulator nBOH was added in the ratio shown in Table 1. This paint was applied to a PP board (150 mm x 70 mm x 2 mm) with a 3-mil applicator, dried at 80°C for 30 minutes, and then aged at 23°C for 6 days to obtain a coated body, which was then peeled off to obtain an isolated film.
[0064] <Preparation of coating specimens for testing coating appearance, acid resistance, alkali resistance, and coating drying properties> Base agent No. 1 and hardener No. 1 were mixed to an equivalent ratio of 1.6, and nBOH was added in the proportions shown in Table 1. The paint was applied to an ABS plate (150 mm x 70 mm x 2 mm) using a 3-mil applicator and dried at 80°C for 30 minutes to obtain a coated body.
[0065] <Examples 2 to 25 and Comparative Examples 1 to 6> For Examples 2 to 25 and Comparative Examples 1 to 6, coated bodies were produced under the conditions shown in Tables 1 or 2 in the same manner as for Example 1.
[0066] <Measurement of viscosity increase rate> The viscosity value measured immediately after preparation of the paint was compared with the viscosity value after standing at 23°C for 4 hours or 19 hours to determine the viscosity increase rate, which is shown in Tables 1 and 2. A rheometer Physical MCR301 (manufactured by Anton Paar) was used to measure the viscosity. When the viscosity increase rate after 4 hours is less than 2.0, and further when the viscosity increase rate after 19 hours is less than 7.0, and particularly when it is less than 5.0, it can be determined that a high pot life extension effect has been obtained. (Evaluation Criteria) Evaluation after 4 hours ◯: Viscosity increase rate ≦2.0 ×: Viscosity increase rate > 2.0 Evaluation after 19 hours Because the preferred range of viscosity increase rates differs between the paints in Tables 1 and 2 due to differences in coating specifications and initial viscosity, the viscosity increase rate was evaluated according to the following criteria for each: ◯ is a viscosity range in which the same coating appearance as the initial one can be obtained under the same conditions as the initial one, △ is a viscosity range in which coating is possible but in which adjustments such as adjustments to the coating amount and coating speed are required, and × is a viscosity range in which coating is difficult. For paints in Table 1 ◯: Viscosity increase rate ≦5.0 △: 5.0<viscosity increase rate≦7.0 ×: Viscosity increase rate > 7.0 For paints in Table 2 ◯: Viscosity increase rate ≦2.0 ×: Viscosity increase rate > 2.0
[0067] <Coating appearance evaluation> After drying at 80° C. for 30 minutes, the coated bodies obtained above were subjected to an evaluation of the coating appearance based on the following criteria. (Evaluation Criteria) ○: No citron peel has developed. ×: A state in which citrus skin has developed.
[0068] <Measurement of gel fraction> The gel fraction of each coating film was measured using the paints of Examples 1 to 12 and Comparative Examples 1 to 3. The coating film was immersed in a mixed solution of 100 g of toluene and acetone (mass ratio 1:1) for 1 g of the isolated film obtained above under reflux for 5 hours, and then dried at 105°C for 30 minutes, and the gel fraction was calculated using the following formula. The results are shown in Table 1. Gel fraction (%) = M2 / M1 × 100 (The mass of the coating film before immersion is M1, and the mass of the coating film after immersion is M2.) (Evaluation Criteria) ○: Gel fraction ≧90.0 △: 80.0≦gel fraction<90.0 ×: Gel fraction <80.0
[0069] <Acid resistance test / Alkaline resistance test> The coated body obtained above, after drying at 80℃ for 30 minutes, was cured at 23℃ for 6 days, and then an acid resistance test and an alkali resistance test were conducted in accordance with the liquid resistance (general method) test method and the drip method of "JIS K 5600-6-1". For the alkali resistance test, a 0.1N aqueous sodium hydroxide solution was used as the test liquid, and the test specimen was placed in a thermostatic chamber maintained at 50±2°C and left for 3 hours, after which the test specimen was rinsed with water and wiped, and the coating surface condition of the test area was visually evaluated according to the following criteria. Similarly, for the acid resistance test, a 0.1N aqueous sulfuric acid solution was used as the test liquid, and the specimen was left for 24 hours under standard conditions (25±2°C, 50±5% RH), after which the test specimen was rinsed with water and wiped, and the coating surface condition of the test area was visually evaluated according to the following criteria. The results are shown in Tables 1 and 2. (Evaluation Criteria) 〇: No change on the coating surface △: Slight discoloration was observed on the coating surface. ×: Discoloration was observed on the coating surface.
[0070] <Coating film drying test> The coated bodies obtained above after drying at 80°C for 30 minutes were tested for dryness to touch in accordance with "JIS K 5600-1-1," and the coating film dryness was evaluated based on the following criteria. (Evaluation Criteria) ○: When you lightly touch the center of the coating surface with your fingertip, your fingertip does not get dirty. △: When the center of the coating surface is lightly touched with a fingertip, the fingertip becomes slightly dirty. ×: When the center of the coating surface is lightly touched with a fingertip, the fingertip becomes dirty.
[0071] [Table 1]
[0072] [Table 2]
Claims
1. A method for applying a multi-component reactive curing coating composition, comprising: preparing (A) a base agent, (B) a curing agent, and (C) a curing rate regulator containing an alcohol; mixing these components before application to prepare a coating composition (X); and applying the resulting coating composition to a coating medium.
2. A method for applying a multi-component reactive coating composition containing at least (A) a base agent and (B) a curing agent, wherein the base agent (A) contains a curing rate regulator containing (C) an alcohol, and the base agent (A) and the curing agent (B) are mixed prior to application to prepare a coating composition (Y), which is then applied to a coating medium.
3. 3. The coating method according to claim 1, wherein the curing agent (B) contains an isocyanate.
4. 2. The coating method according to claim 1, characterized in that after preparation of the coating composition (X), the viscosity increase rate of the coating composition (X) after 4 hours at 23°C is within twice the initial viscosity at the time of mixing the coating composition (X), and the gel fraction of the coating film when completely cured is 80% or more.
5. 3. The coating method according to claim 2, characterized in that after preparation of the coating composition (Y), the viscosity increase rate of the coating composition (Y) after 4 hours at 23°C is within twice the initial viscosity at the time of mixing the coating composition (Y) and the gel fraction of the coating film when completely cured is 80% or more.
6. A paint set comprising at least (A) a base agent, (B) a curing agent, and (C) a curing rate regulator containing an alcohol.
Citation Information
Patent Citations