Titanium suboxide material and method for producing titanium suboxide material

By using titanic acid aggregates mixed with niobium, the method ensures uniform oxygen vacancy introduction in titanium suboxide, addressing conductivity and heat resistance issues, enabling stable performance in heat-treated environments.

JP2024166035APending Publication Date: 2024-11-28SAKAI CHEM IND CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2023189871
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-16
Filing Date
2023-11-07
Publication Date
2024-11-28

AI Technical Summary

Technical Problem

Existing titanium suboxide materials face challenges with insufficient oxygen vacancies, leading to restricted usage environments due to impaired conductivity and dielectric properties during heat treatment, oxidation reactions, and non-uniform crystal phases.

Method used

A method involving titanic acid aggregates as a precursor, mixed with a niobium element, is used to introduce oxygen vacancies uniformly, maintaining the rutile crystal structure and achieving high conductivity and heat resistance by controlling the reduction degree.

Benefits of technology

The resulting titanium suboxide material exhibits high conductivity and heat resistance, suitable for applications like conductive and dielectric fillers, maintaining properties even under heat treatment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024166035000003
    Figure 2024166035000003
  • Figure 2024166035000004
    Figure 2024166035000004
  • Figure 2024166035000005
    Figure 2024166035000005
Patent Text Reader

Abstract

To provide a titanium suboxide having high conductivity and high heat resistance in which the progress of oxidation reaction is suppressed even in a heat treatment.SOLUTION: A titanium suboxide material has a weight change width of 0.30-3.40% in a temperature range of 50-900°C in a thermogravimetric analysis, and a volume resistivity of 1×100-8×103 Ω cm at 25°C when the powder is pressed at a pressure of 63 MPa.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a titanium suboxide material and a method for making the titanium suboxide material. [Background technology]

[0002] Titanium suboxide, which has oxygen deficiencies, is known to have low volume resistivity, i.e., high electrical conductivity, due to the presence of free electrons, and is used as a conductive material. Titanium suboxide is also used as a pigment in cosmetics, etc., because it is black in color. Disclosed examples of conventional titanium suboxides include conductive particles containing titanium oxide as a main constituent, the whiteness, redness, and yellowness of which are within specific ranges, and the amount of oxygen deficiency measured by thermogravimetric analysis being 0.1% by mass or more and 1.5% by mass or less (see Patent Document 1); low-order titanium oxide powder obtained by forming a gas barrier thin film on the surface of low-order titanium oxide particles (see Patent Document 2); black-colored titanium oxide used as a pigment in cosmetics, which is obtained by heating and reducing titanium dioxide powder in an ammonia gas atmosphere at 500 to 1000°C (see Patent Document 3); and colored titanium oxide produced by spraying and supplying titanium alkoxide into a reducing gas atmosphere and carrying out a decomposition and reduction reaction (see Patent Document 4). [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2019-179590 A [Patent Document 2] Japanese Patent Application Publication No. 8-59240 [Patent Document 3] Japanese Patent Application Publication No. 58-180413 [Patent Document 4] Japanese Patent Application Publication No. 4-46016 Summary of the Invention [Problem to be solved by the invention]

[0004] In general, oxygen vacancies are introduced into titanium oxide by reduction and calcination under a high-temperature atmosphere. However, it is not easy to introduce sufficient oxygen vacancies into titanium oxide. 4 -10 6 Titanium suboxide with a volume resistivity of about Ω·cm has only been obtained. In addition, titanium oxide (titanium suboxide) with oxygen deficiency may undergo oxidation reaction in the air and its electrical conductivity may decrease. Furthermore, when titanium suboxide is used as a conductive / dielectric material, one of the embodiments is to use it in a composite with resin. In this case, the resin is heated to about 100 to 300°C and kneaded to plasticize it, and it is assumed that the electrical conductivity and dielectric properties of titanium suboxide are impaired in the process of composite with resin. In addition, the use of titanium suboxide as a heated object in dielectric heating is one of the assumed uses, but titanium suboxide itself, which has a high dielectric constant, is heated by radio waves such as microwaves, and it is assumed that this also impairs the electrical conductivity and dielectric properties of titanium suboxide. Regarding the oxidation reaction of titanium suboxide in the air, Patent Document 1 discloses a conductive titanium oxide that is less affected by the external environment, but it does not show sufficient electrical conductivity and is therefore of low practical use. For these reasons, titanium suboxide has the problem of being subject to limitations on the environments in which it can be used.

[0005] In view of the above-mentioned current situation, an object of the present invention is to provide a titanium suboxide having high electrical conductivity and high heat resistance in which the progress of oxidation reaction is suppressed even when subjected to heat treatment. [Means for solving the problem]

[0006] Based on the above-mentioned known literature and well-known techniques, the inventors hypothesized that the low heat resistance of titanium suboxide depends on the stability of its crystal structure, i.e., the amount of oxygen vacancies. The greater the amount of oxygen vacancies, the more the chemical composition deviates from TiO2, making it impossible to maintain the anatase or rutile crystal structure, which is considered to be the thermodynamically stable crystal structure of titanium oxide, and it is believed that in addition to becoming amorphous, a crystal structure such as the Magneli phase, which is thermodynamically unstable, is formed. Therefore, the researchers came to the conclusion that if it were possible to introduce oxygen vacancies to the extent that the material had sufficient electrical conductivity and dielectric properties while maintaining the rutile crystal structure, it would be possible to obtain a titanium suboxide with excellent heat resistance whose electrical conductivity and dielectric properties would not change even after heat treatment. Here, if the degree of reduction is insufficient, the material will not exhibit sufficient electrical conductivity or dielectric properties, and if the degree of reduction is too strong, the material will have low heat resistance, so it is important to introduce oxygen defects by moderate reduction. Normally, when titanium oxide particles are reduced and fired to obtain titanium suboxide, almost no oxygen defects are introduced up to a certain threshold reduction condition, but if the threshold reduction condition is exceeded, significant oxygen defects accompanied by changes in the crystal structure occur. Therefore, with conventional methods, it was difficult to obtain the desired titanium suboxide while controlling the degree of reduction to the minimum necessary to ensure sufficient electrical conductivity. Furthermore, the preferential reduction reaction on the particle surface leads to the formation of particles with non-uniform crystal phases on the particle surface and inside the particle, which is also a factor in the decrease in heat resistance. The inventors then synthesized a titanium suboxide material by using a precursor material that satisfies the following requirements: 1) using a titanate aggregate as a precursor material, and 2) uniformly mixing niobium element into the titanate aggregate. 1) By using titanic acid aggregates as a precursor material, the reducing gas can penetrate sufficiently deep into the particles, and the entire particle can be uniformly reduced and fired, resulting in a thermodynamically stable material with a uniform rutile crystal structure throughout. As the reduction reaction progresses, the primary particles that make up the aggregates are sintered, and ultimately a titanium suboxide material that maintains the shape of the aggregates is obtained. 2) By uniformly mixing niobium element into the titanate aggregates, the reduction reaction from tetravalent to trivalent titanium element is promoted during reduction firing, and an appropriate amount of oxygen vacancy can be introduced under mild conditions, resulting in a titanium suboxide material with a rutile-type crystal structure that has sufficient electrical conductivity and dielectric properties. Based on the above material design, the inventors investigated titanium suboxide, which has high electrical conductivity and excellent heat resistance, and found that by mixing titanyl sulfate and / or titanium oxychloride with a specified ratio of a niobium-containing compound, acid, and inorganic salts and then hydrolyzing the resulting hydrolyzate by reduction and calcination, a titanium suboxide material having excellent electrical conductivity and excellent heat resistance can be obtained, which led to the completion of the present invention. The titanium suboxide material of the present invention has a lower volume resistivity than the conductive titanium oxide described in Patent Document 1, and exhibits excellent electrical conductivity.

[0007] That is, the present invention is as follows. [1] In thermogravimetric analysis, the weight change range in the temperature range of 50 to 900 °C is 0.30 to 3.40%, and the volume resistivity at 25 °C when the powder is compressed at a pressure of 63 MPa is 1 × 10 0 Ω cm~8×10 3 A titanium suboxide material characterized by a resistivity of Ω·cm.

[0008] [2] The titanium suboxide material according to [1], characterized in that the weight change range of the titanium suboxide material in the temperature range of 50 to 400°C in thermogravimetric analysis is 0 to 1.20%.

[0009] [3] The titanium suboxide material according to [1] or [2], characterized in that it contains niobium.

[0010] [4] The titanium suboxide material according to any one of [1] to [3], characterized in that the titanium suboxide material has a rutile crystal structure.

[0011] [5] Volume-based 90% diameter D in particle size distribution measurement 90 and 10% diameter D 10 Ratio to (D 90 / D 10 ) is less than 3.0.

[0012] [6] The titanium suboxide material according to any one of [1] to [5], characterized in that the median diameter in the particle size distribution is 1.0 to 20 μm.

[0013] [7] A method for producing a titanium suboxide material, comprising: a first step of mixing and hydrolyzing titanyl sulfate and / or titanium oxychloride, a niobium-containing compound, an acid, and an inorganic salt; and a second step of reducing and calcining the hydrolyzate obtained in the first step, wherein the first step uses a niobium-containing compound in an amount such that the amount of niobium contained in the niobium-containing compound is more than 0.5 mol % and not more than 15 mol % per 100 mol % of titanium contained in the titanyl sulfate and / or titanium oxychloride.

[0014] [8] The method for producing a titanium suboxide material according to [7], wherein the second step is a step of reducing and firing the hydrolyzate in an atmosphere having a hydrogen concentration of less than 4 volume %. Effect of the Invention

[0015] The titanium suboxide material of the present invention has high electrical conductivity and excellent heat resistance, and can therefore be suitably used for applications such as conductive fillers and dielectric fillers which are kneaded with resins at high temperatures. [Brief description of the drawings]

[0016] [Figure 1] FIG. 2 shows the results of thermogravimetric analysis of the titanium suboxide material produced in Example 1. [Diagram 2] FIG. 1 shows the results of thermogravimetric analysis of the titanium suboxide material used in Comparative Example 3. [Diagram 3] FIG. 1 shows the results of electron microscope observation (magnifications: 200x, 2000x, and 10,000x) of the titanic acid aggregate obtained in Example 12. [Figure 4] FIG. 1 shows the results of electron microscope observation (magnifications: 200x, 2000x, and 10,000x) of the titanic acid aggregate obtained in Example 13. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0017] A preferred embodiment of the present invention will be described in detail below, but the present invention is not limited to the following description, and can be modified and applied as appropriate within the scope that does not change the gist of the present invention.

[0018] 1. Titanium suboxide materials The titanium suboxide material of the present invention has a weight change range of 0.30 to 3.40% in the temperature range of 50 to 900°C in thermogravimetric analysis, and a volume resistivity of 1×10 at 25°C when the powder is compressed under a pressure of 63 MPa. 0 Ω cm~8×10 3 It is characterized by its resistance to oxygen deficiency of Ω·cm. By evaluating the range of weight change in the relevant temperature range, it is possible to quantitatively evaluate the amount of oxygen vacancy while taking into account the effect of adsorbed water on the surface of titanium suboxide particles. In thermogravimetric analysis, the range of weight change within the temperature range of 50 to 900°C was 0.30 to 3.40%, which means that sufficient oxygen vacancies were formed to exhibit electrical conductivity while maintaining a stable titanium dioxide crystal structure, and is considered to mean that the titanium suboxide has high heat resistance. The range of weight change in the temperature range of 50 to 900°C in the thermogravimetric analysis of the titanium suboxide material of the present invention may be 0.30 to 3.40%, preferably 0.33 to 3.30%, more preferably 0.35 to 3.00%, particularly preferably 0.37 to 2.70%, and most preferably 0.38 to 1.00%. In addition, the titanium suboxide material of the present invention has a volume resistivity of 1×10 at 25° C. when the powder is compressed under a pressure of 63 MPa. 0 Ω cm~8×10 3 It is a highly conductive material with a volume resistivity of 1×10 Ω·cm. 0 Ω cm~8×10 3 Ω cm is sufficient, but 3×10 0 Ω cm~5×10 3 It is preferably 5×10 Ω·cm. 0 Ω cm~1×10 3Ω cm, and more preferably 1×10 1 Ω cm~5×10 2 Ω cm, and particularly preferably 1×10 1 Ω cm~1×10 2 The volume resistivity at 25°C when the titanium suboxide powder is compressed at a pressure of 63 MPa means the volume resistivity of the original titanium suboxide material that has not been heat-treated. Thermogravimetric analysis and volume resistivity measurement of the titanium suboxide material can be carried out by the method described in the Examples below.

[0019] The titanium suboxide material of the present invention preferably has a weight change range of 0 to 1.20% in a temperature range of 50 to 400°C in thermogravimetric analysis. With such a weight change range, no by-products are generated during heating, or even if there are, they are very small, so that a resin composition can be prepared without impairing the electrical conductivity and dielectric properties of the titanium suboxide material. Furthermore, when the titanium suboxide material is kneaded with a resin, the changes in weight and volume associated with the chemical reaction are small, so that a dense resin composition can be prepared. The weight change range in a temperature range of 50 to 400°C is more preferably 0 to 1.00%, even more preferably 0 to 0.50%, and particularly preferably 0 to 0.30%.

[0020] In addition, the titanium suboxide material of the present invention is a material whose dielectric properties can be adjusted according to the application as described later, but when used in an application requiring a material with a high dielectric constant, the dielectric constant at 1 GHz is preferably 20 or more. With such a dielectric constant, the titanium suboxide material of the present invention can be more suitably used in applications such as conductive fillers and dielectric fillers. The dielectric constant at 1 GHz of the titanium suboxide material is more preferably 25 or more, even more preferably 30 or more, particularly preferably 35 or more, and most preferably 40 or more. There is no particular upper limit to the dielectric constant of the titanium suboxide material, but the dielectric constant at 1 GHz is usually 100 or less. The dielectric constant at 1 GHz of the titanium suboxide material referred to here means the dielectric constant at 1 GHz of the original titanium suboxide material that has not been subjected to heat treatment. The dielectric constant of the titanium suboxide material can be measured by the method described in the Examples below.

[0021] The titanium suboxide material of the present invention may contain other elements as long as it is mainly composed of titanium suboxide, and preferably contains niobium element. By containing niobium element, the titanium suboxide material of the present invention can more fully exhibit excellent electrical conductivity properties with a relatively small amount of oxygen deficiency. When the titanium suboxide material of the present invention contains niobium, the content thereof is preferably more than 0.5 mol % and not more than 15 mol %, more preferably 1.0 to 5.0 mol %, and even more preferably 2.0 to 4.0 mol %, relative to 100 mol % of titanium element contained in the titanium suboxide material. The niobium element contained in titanium suboxide materials can be detected and quantified using energy dispersive spectroscopy (EDS).

[0022] The titanium suboxide material of the present invention has a specific surface area of ​​0.1 to 5.0 m 2 / g. With such a specific surface area, the titanium suboxide material has good handling properties. The specific surface area of ​​the titanium suboxide material is more preferably 0.3 to 3.0 m 2 / g, and more preferably 0.5 to 1.0 m 2 / g. The specific surface area of ​​the titanium suboxide material can be measured by the method described in the Examples below.

[0023] The titanium suboxide material of the present invention has a median diameter D 50 It is preferable that the secondary particle diameter represented by the formula (1) is 1.0 to 20 μm. With such a secondary particle diameter, the titanium suboxide material has good handleability. Furthermore, when the titanium suboxide material of the present invention is mixed with a resin for use, it has excellent dispersibility in the resin and is easily composited with the resin. The secondary particle diameter of the titanium suboxide material is more preferably 2.0 to 15 μm, further preferably 3.0 to 12 μm, and particularly preferably 4.0 to 10 μm.

[0024] The titanium suboxide material of the present invention has a volume-based 90% diameter D 90 and 10% diameter D 10 Ratio to (D 90 / D 10 ) of the titanium suboxide material is preferably less than 3.0. If the particle size distribution is narrow, the titanium suboxide material of the present invention will have excellent dispersibility in the resin when mixed with the resin, and will be easily composited with the resin. 90 / D 10 ) is more preferably less than 2.5, and even more preferably less than 2.0. Titanium suboxide material D 50 and (D 90 / D 10 ) can be measured by the method described in the Examples below.

[0025] The titanium suboxide material of the present invention preferably has a rutile crystal structure. When the crystal structure is rutile, oxygen vacancies are introduced while maintaining the stable crystal structure of titanium dioxide. This improves the stability of the titanium suboxide material, making it excellent in heat resistance, and as a result, it is believed that the material maintains excellent electrical conductivity even when exposed to an oxidizing atmosphere. Furthermore, the titanium suboxide material of the present invention may contain titanium suboxide having a rutile crystal structure and titanium suboxide having a crystal structure other than rutile, so long as it satisfies the above-mentioned requirements for the range of weight change in thermogravimetric analysis and the powder volume resistivity. As long as it satisfies the requirements of the titanium suboxide material of the present invention, the content of titanium suboxide having a crystal structure other than rutile is not particularly limited, but it is preferably 50 mass% or less with respect to 100 mass% of the entire titanium suboxide material. It is more preferably 30 mass% or less, and even more preferably 20 mass% or less. The crystal structure of the titanium suboxide material can be confirmed by XRD measurement.

[0026] The titanium suboxide material of the present invention may be kneaded with a resin such as a silicone resin, an acrylic resin, a urethane resin, a styrene resin, a polyimide resin, an epoxy resin, a copolymer block polymer, or a rubber-based material to be used as a resin composition. In this case, the resin composition may contain one or more other components such as an organic solvent, a curing agent, and an additive, as necessary.

[0027] 2. Manufacturing method of titanium suboxide material The present invention also relates to a method for producing a titanium suboxide material, which comprises a first step of mixing and hydrolyzing titanyl sulfate and / or titanium oxychloride, a niobium-containing compound, an acid, and an inorganic salt, and a second step of reducing and calcining the hydrolyzate obtained in the first step, wherein the first step uses a niobium-containing compound in an amount such that the amount of niobium contained in the niobium-containing compound is more than 0.5 mol % and not more than 15 mol % per 100 mol % of titanium contained in the titanyl sulfate and / or titanium oxychloride. By including in the production method a first step of mixing titanyl sulfate and / or titanium oxychloride with a niobium-containing compound, acid, and inorganic salts and hydrolyzing the mixture, it is possible to efficiently synthesize titanate aggregates containing niobium, and by carrying out the reduction and calcination treatment in the second step, it is possible to produce a titanium suboxide material that has a relatively small amount of oxygen deficiency while still having excellent conductivity and dispersibility.

[0028] In the first step, either titanyl sulfate or titanium oxychloride or both may be used as the titanium source. Titanium oxychloride (TiOCl2) is produced by reacting titanium tetrachloride with water, so if an aqueous solution of titanium tetrachloride is used as a titanium source, titanium oxychloride is being used.

[0029] The niobium element-containing compound used in the first step includes ammonium niobium oxalate, niobium pentachloride, niobium pentafluoride, niobium alkoxides, etc., and one or more of these can be used.

[0030] The amount of the niobium-containing compound used in the first step is an amount such that the amount of niobium contained in the niobium-containing compound is more than 0.5 mol % and not more than 15 mol % relative to 100 mol % of titanium contained in titanyl sulfate and / or titanium oxychloride, preferably an amount such that the amount of niobium is 1.0 to 5.0 mol %, and more preferably an amount such that the amount of niobium is 2.0 to 4.0 mol %.

[0031] In the first step, it is preferable to prepare solutions of the niobium element-containing compound and titanyl sulfate and / or titanium oxychloride, and then mix them with an acid and an inorganic salt. Solvents used in preparing the solution of the niobium element-containing compound or the solution of titanyl sulfate and / or titanium oxychloride include water, ethanol, isopropyl alcohol, dilute sulfuric acid, hydrochloric acid, etc., and one or more of these can be used.

[0032] When preparing the solution of the niobium element-containing compound, the concentration of the solution containing the niobium element-containing compound is preferably 1 to 50 mass % in order to mix uniformly with titanium element, more preferably 5 to 45 mass %, and further preferably 10 to 40 mass %.

[0033] When preparing the titanyl sulfate solution, the titanyl sulfate concentration in the titanyl sulfate-containing solution is not particularly limited, but considering the yield of the hydrolyzate and the production efficiency, it is preferably 0.10 to 3.5 mol / L, more preferably 0.50 to 3.0 mol / L, and even more preferably 0.70 to 2.5 mol / L. The concentration of titanium oxychloride in the titanium oxychloride-containing solution is preferably similar to the concentration of titanyl sulfate in the titanyl sulfate-containing solution.

[0034] In the first step, titanyl sulfate and / or titanium oxychloride and / or the niobium element-containing compound may be mixed with a solvent and then heated in order to thoroughly dissolve the titanyl sulfate and / or titanium oxychloride and / or the niobium element-containing compound in the solvent. The heating temperature is preferably 40 to 80° C., and more preferably 50 to 70° C. This allows the titanyl sulfate and / or titanium oxychloride and the niobium element-containing compound to be dissolved and mixed more uniformly before the hydrolysis reaction begins. The titanyl sulfate solution and / or titanium oxychloride solution and the niobium element-containing compound solution may be heated after mixing them with an acid and an inorganic salt.

[0035] In the first step, titanyl sulfate and / or titanium oxychloride, a niobium element-containing compound, an acid, and inorganic salts are mixed to hydrolyze titanyl sulfate and / or titanium oxychloride, and the niobium element-containing compound. Although hydrolysis can be performed using a base instead of an acid, a titanium suboxide material with a narrow particle size distribution can be produced by performing hydrolysis using an acid. The reason for this is considered as follows. That is, by performing hydrolysis using an acid, the hydrolysis of titanyl sulfate and / or titanium oxychloride and the niobium element-containing compound proceeds slowly, and titanic acid is gradually precipitated in the reaction system while niobium element is uniformly coprecipitated. The precipitated titanic acid aggregates are aggregated with each other by van der Waals forces, and titanic acid aggregates having a narrow particle size distribution and a uniform aggregate particle size are formed. Therefore, by firing this under a reducing atmosphere, it is considered that a titanium suboxide material can be produced while maintaining the particle size and particle size distribution of the titanic acid aggregates. In hydrolysis with a base, the hydrolysis rate is too fast to form uniform titanic acid aggregates with a narrow particle size distribution, making it difficult to control. In addition, the neutralization hydrolysis rate of titanyl sulfate or titanium oxychloride is different from that of elemental niobium, making it undesirable from the viewpoint of uniformity of elemental niobium. The acid used in the first step includes sulfuric acid, hydrochloric acid, nitric acid, and the like. In consideration of sufficient hydrolysis and production costs, the amount of acid used in the first step is preferably 1 to 50 mass % relative to 100 mass % of titanyl sulfate and / or titanium oxychloride, more preferably 5 to 40 mass %, and even more preferably 10 to 30 mass %.

[0036] Examples of inorganic salts used in the first step include sodium chloride, ammonium chloride, potassium chloride, ammonium sulfate, etc. By mixing inorganic salts, the finally obtained titanium suboxide material can have a narrow particle size distribution. Among these, sodium chloride is preferred because it is inexpensive and easily available. The amount of the inorganic salt used is preferably 50 to 1000% by mass relative to 100% by mass of titanyl sulfate and / or titanium oxychloride, more preferably 60 to 700% by mass, still more preferably 100 to 600% by mass, and particularly preferably 125 to 500% by mass relative to 100% by mass of titanyl sulfate and / or titanium oxychloride.

[0037] In the first step, the order in which the titanyl sulfate and / or titanium oxychloride, the niobium element-containing compound, the acid, and the inorganic salts are mixed is not particularly limited. From the viewpoint of uniformly mixing titanium element and niobium element, it is preferable to mix the titanyl sulfate and / or titanium oxychloride, the acid, and the inorganic salts, and then add and mix the niobium element-containing compound thereto.

[0038] In the first step, in order to sufficiently advance the hydrolysis, the mixed liquid obtained by mixing titanyl sulfate and / or titanium oxychloride, a niobium element-containing compound, an acid, and inorganic salts may be heated. When the mixed liquid is heated, the heating temperature is preferably 90 to 115°C. More preferably, it is 95 to 110°C. The time for carrying out the hydrolysis in the first step is preferably 0.5 to 6 hours, more preferably 1 to 5 hours, and even more preferably 2 to 3 hours.

[0039] In the above-mentioned method for producing a titanium suboxide material, it is preferable to carry out a step of neutralizing the obtained hydrolyzate after the first step, which makes it possible to more efficiently remove the remaining acids such as sulfuric acid and hydrochloric acid. The basic compound used for neutralization is not particularly limited, and ammonia, sodium hydroxide, sodium carbonate, sodium hydrogen carbonate, potassium hydroxide, etc. can be used. Among these, ammonia, sodium hydroxide, sodium carbonate, and sodium hydrogen carbonate are preferred in that they can prevent the inclusion of alkali metals or alkaline earth metals other than sodium. Ammonia is more preferred. These may be added in a solid or gaseous state, but are usually added as an aqueous solution.

[0040] In the neutralization step, it is preferable to add a basic compound until the pH of the repulp slurry obtained by repulping the hydrolyzate in water in an amount 10 times the mass of the hydrolyzate reaches 7 to 11. It is more preferable to add a basic compound until the pH of the repulp slurry reaches 8 to 10.

[0041] When the neutralization step is carried out, it is preferable to carry out a step of washing the hydrolyzate with water before the neutralization step. This makes it possible to remove unnecessary acids, inorganic salts, etc. contained in the slurry after hydrolysis. The hydrolyzate can be washed with water by passing water through the solid matter separated by filtering the hydrolyzate. It is preferable to wash the hydrolyzate with water until the electrical conductivity of the filtrate is 5000 μS / cm or less, which makes it possible to reduce the amount of basic compound used in the neutralization step. It is more preferable that the electrical conductivity is 3000 μS / cm or less, and even more preferable that it is 1000 μS / cm or less.

[0042] When the neutralization step is carried out, it is preferable to carry out a step of filtering and washing the obtained neutralized product after the neutralization step. This can remove salts generated in the neutralization step and increase the purity of the hydrolyzate. The neutralized product is preferably washed with water until the electrical conductivity of the filtrate is 1000 μS / cm or less, which can sufficiently remove salts generated in the neutralization step. It is more preferable that the electrical conductivity is 500 μS / cm or less, and even more preferable that the electrical conductivity is 100 μS / cm or less.

[0043] In the method for producing the titanium suboxide material, it is preferable to carry out a step of drying the obtained titanate aggregate after the neutralization step (after the filtration and washing steps if a step of filtering and washing the obtained neutralized product is carried out after the neutralization step) and before the second firing step. The method for drying the titanic acid aggregate is not particularly limited, but it is preferably carried out by heating. The heating temperature is preferably 80 to 200° C., and more preferably 100 to 150° C. Drying at such a temperature allows the particles to be sufficiently dried while preventing excessive sintering between the particles.

[0044] In the method for producing the titanium suboxide material, it is preferable to further include a step of classifying the titanic acid aggregates that have been subjected to the drying step. The method for classifying the dried titanic acid aggregate is not particularly limited, but is preferably performed using a sieve. The average opening size of the sieve is preferably 50 to 1000 μm, and more preferably 200 to 500 μm. By passing the titanic acid aggregate through a sieve with such an average opening size, it is possible to sufficiently remove titanic acid aggregates that have formed aggregates of abnormal size and impurities that may be mixed in from outside the reaction system in the first step.

[0045] The hydrolyzate obtained in the first step was degassed at 200°C for 30 minutes and preheated at 200°C for 5 minutes to obtain a specific surface area of ​​100 to 800 m. 2 / g. With such a specific surface area, reduction can be efficiently carried out to the inside of the titanium suboxide particles. The specific surface area of ​​the hydrolyzate is more preferably 200 to 600 m 2 / g, and most preferably 250 to 500m 2 / g. The specific surface area of ​​the hydrolysate can be measured by the method described in the Examples below.

[0046] The atmosphere in which the reduction firing in the second step is carried out is not particularly limited, and examples thereof include a hydrogen (H2) atmosphere, a nitrogen (N2) atmosphere, an argon (Ar) atmosphere, a carbon monoxide (CO) atmosphere, a mixed gas atmosphere of hydrogen and nitrogen and / or argon, carbon monoxide, a mixed gas atmosphere of hydrogen and an inert gas, and an ammonia (NH3) atmosphere. Among these, a hydrogen atmosphere, a nitrogen atmosphere, or a mixed gas atmosphere of hydrogen and nitrogen is preferred because it allows the desired titanium suboxide material to be produced efficiently. Among these, an atmosphere with a hydrogen concentration of 1% by volume or more and less than 20% by volume is preferred. More preferably, the hydrogen concentration is 1% by volume or more and less than 4% by volume. An atmosphere with a hydrogen concentration of less than 4% by volume is highly safe because hydrogen is below the lower explosion limit concentration, and a mixed gas with nitrogen is suitable for industrialization from the viewpoint of cost.

[0047] The temperature at which the reduction firing in the second step is carried out is preferably 500 to 1300°C, more preferably 800 to 1250°C, further preferably 850 to 1200°C, and particularly preferably 900 to 1100°C. The time for which the reduction firing is carried out depends on the conditions of the reducing atmosphere such as the hydrogen concentration, but is preferably 1 to 8 hours after the firing temperature is reached, more preferably 2 to 6 hours, and even more preferably 3 to 5 hours.

[0048] The method for producing a titanium suboxide material of the present invention may include other steps in addition to the steps described above, such as a step of further firing in air after the reduction firing, a step of crushing the titanate aggregates after drying, and a step of classifying the aggregates. EXAMPLES

[0049] In order to explain the present invention in detail, specific examples are given below, but the present invention is not limited to these examples. Unless otherwise specified, "%" and "wt%" mean "weight % (mass %)". The measurement methods for each physical property are as follows.

[0050] <Thermogravimetric analysis> Using a thermogravimetric analyzer (STA7300, Hitachi High-Tech Science), thermogravimetric analysis was performed in air at a flow rate of 200 mL / min under the following conditions: temperature range 50 to 900°C, heating rate 10°C / min, and holding time 30 seconds. (Displacement calculation) From the results of the thermogravimetric analysis, the displacement ranges in the temperature ranges of 50 to 900°C and 50 to 400°C were calculated. The weight of the sample before measurement is W, and the weight change from the lower limit of weight loss to the maximum weight increase in the temperature range of 50 to 900 °C is ΔW 900 The weight change from the lower limit of weight loss to the maximum weight increase in the temperature range of 50 to 400 ° C is ΔW 400 The displacement range (%) in this case is Displacement width (%) = (ΔW 900 / W)×100 or Displacement width (%) = (ΔW400 / W)×100 It is represented by <Volume Resistivity Measurement> Using a low-resistance resistivity meter (Loresta GX MCP-T700, manufactured by Nitto Seiko Analytics), the powder was filled so that the thickness of the sample was in the range of 1.0 to 3.0 mm when pressed at a pressure of 63 MPa, and the volume resistivity at 25°C was measured. <Dielectric Constant Measurement> A network analyzer P9373A (manufactured by Keysight) was connected to a cavity resonator method dielectric constant measurement device (manufactured by AET), and the dielectric constant of the powder packed in a quartz tube was measured. The measurement frequency was set to 1 GHz. <Specific Surface Area Measurement> Using a fully automatic specific surface area measurement device (Macsorb, manufactured by Microtrac), degassing was performed at 200°C for 30 minutes, preheating was performed at 200°C for 5 minutes, and then the specific surface area was measured by adsorption and desorption measurement. <Median Diameter, Particle Size Distribution Measurement> Using a laser diffraction / scattering particle size distribution measurement device (LA-960, manufactured by Horiba), a 0.025% hexametaphosphate aqueous solution was used as the dispersion medium, and the particle size distribution was measured for the sample that was subjected to a 1-minute dispersion treatment with an ultrasonic homogenizer (US-600, manufactured by Nippon Seiki). The median diameter (D 50 ), volume-based 10% diameter (D 10 ), and volume-based 90% diameter (D 90 ) were measured, and the ratio (D 10 ) and D 90 ) was calculated from the numerical values of D 90 / D 10 ). <XRD Measurement> An X-ray diffractometer (D8 ADVANCE, manufactured by Bruker Japan) was used to measure the sample under the following conditions. [XRD Measurement Conditions] Optical system: Convergent beam method X-ray tube: Cu Kα line 2θ angle: 10.0° - 80.0° Tube voltage - tube current: 40 kV - 40 mA Step width: 0.01° Step time: 0.05 s <SEM / EDS Measurement> Using a field emission scanning electron microscope (JSM-7500, manufactured by JEOL Ltd.) and an EDS detector (Ultim Max 170, manufactured by Oxford Instruments), a sample subjected to carbon coating treatment was measured. During the measurement, the acceleration voltage was set to 15.00 kV and the integration count was set to 5 times. Analysis was performed using the Kα1 line for Ti and the Lα1 line for Nb, and the amount of niobium element (mol%) relative to 100 mol% of titanium element was calculated.

[0051] Example 1 To a reaction apparatus equipped with a reflux device, 240 g of titanyl sulfate hydrate (19.9 wt% as Ti), 400 g of sodium chloride, and 40 mL of 98% sulfuric acid were added to 1200 mL of pure water and mixed. The mixed solution was stirred at 200 rpm and heated to a liquid temperature of 80 °C. After heating, it was confirmed that the titanyl sulfate hydrate had dissolved, and a solution prepared by dissolving 17.26 g of ammonium niobium oxalate hydrate (an amount corresponding to 3.0 mol% of Nb relative to Ti in the titanyl sulfate) in 60 mL of pure water was added. The mixed solution was heated and stirred under the condition of 110 °C and refluxed for 3 hours. The obtained slurry was added to a Buchner funnel and subjected to suction filtration, and the obtained solid content was washed with running water using 100 L of pure water. The solid content was repulped in pure water, and an aqueous ammonia solution was added until the pH of the repulped slurry reached about 8 - 9. The slurry after pH adjustment was filtered again and washed with running water so that the conductivity of the filtrate was 100 μS / cm or less. The washed solid content was dried at 100 °C and passed through a 150 μm sieve. The amount of niobium element (mol%) relative to 100 mol% of titanium element, the median diameter, D 90 / D 10 and the specific surface area of the obtained powder were measured. The results are shown in Table 1. The obtained powder was placed in an alumina boat, and hydrogen gas with a concentration of 3.9 vol% using nitrogen gas as a carrier gas was flowed at a flow rate of 300 mL / min, and reduction firing was performed at a temperature of 900 °C for 4 hours. After reduction firing, it was recovered to obtain the titanium suboxide material of Example 1.

[0052] Example 2 In addition to the reduction firing of Example 1, firing was further carried out in air at 400° C. for 4 hours to slightly reduce the amount of oxygen vacancy, thereby obtaining the titanium suboxide material of Example 2. As in Example 1, the amount (mol%) of niobium element relative to 100 mol% of titanium element in the powder before reduction firing, the median diameter, D 90 / D 10 The results are shown in Table 1.

[0053] Example 3 In addition to the reduction and firing of Example 1, firing was further carried out in air at 200° C. for 4 hours to slightly reduce the amount of oxygen vacancy, thereby obtaining the titanium suboxide material of Example 3. As in Example 1, the amount (mol%) of niobium element relative to 100 mol% of titanium element in the powder before reduction firing, the median diameter, D 90 / D 10 The results are shown in Table 1.

[0054] Example 4 A titanium suboxide material of Example 4 was obtained in the same manner as in Example 1, except that the reduction firing temperature was 1000°C. As in Example 1, the amount (mol%) of niobium element relative to 100 mol% of titanium element in the powder before reduction firing, the median diameter, D 90 / D 10 The results are shown in Table 1.

[0055] Example 5 The titanium suboxide material of Example 5 was obtained in the same manner as in Example 1, except that the amount of ammonium niobium oxalate hydrate added in Example 1 was changed to 28.78 g (an amount equivalent to 5.0 mol% of Nb relative to Ti in titanyl sulfate). As in Example 1, the amount (mol%) of niobium element relative to 100 mol% of titanium element in the powder before reduction firing, the median diameter, D 90 / D 10 The results are shown in Table 1.

[0056] Example 6 In a reactor equipped with a reflux device, 60g of titanyl sulfate hydrate (19.9 wt% as Ti), 100g of sodium chloride, and 10mL of 98% sulfuric acid were added to 300mL of pure water and mixed. The mixed solution was stirred at 200 rpm and heated to a liquid temperature of 80°C. After heating, it was confirmed that the titanyl sulfate hydrate had dissolved, and 6.75g of niobium chloride (equivalent to 10.0 mol% as Nb relative to Ti in titanyl sulfate) dissolved in 20mL of 35% hydrochloric acid was added. The mixed solution was heated and stirred at 110°C and refluxed for 3 hours. The obtained slurry was added to a Buchner funnel and subjected to suction filtration, and the obtained solid was washed with 100 L of pure water. The solid was repulped in pure water, and an aqueous ammonia solution was added until the pH of the repulped slurry became about 8 to 9. The pH-adjusted slurry was filtered again, and washed with water so that the conductivity of the filtrate became 100 μS / cm or less. The washed solid was dried at 100°C and passed through a 150 μm sieve. The amount of niobium element (mol%) relative to 100 mol% of titanium element, the median diameter, and D 90 / D 10 The results are shown in Table 1. The obtained powder was placed on an alumina boat, and hydrogen gas with a concentration of 3.9 vol% using nitrogen gas as a carrier gas was passed through at a flow rate of 300 mL / min, and reduction firing was performed for 4 hours at a temperature of 900° C. After reduction firing, the powder was recovered to obtain the titanium suboxide material of Example 6.

[0057] Example 7 The titanium suboxide material of Example 7 was obtained in the same manner as in Example 1, except that the gas used for the reduction and firing in Example 1 was changed from hydrogen gas with a concentration of 3.9 vol% and nitrogen gas as a carrier gas to hydrogen gas with a concentration of 100 vol%. As in Example 1, the amount (mol%) of niobium element relative to 100 mol% of titanium element in the powder before reduction firing, the median diameter, D 90 / D 10 The results are shown in Table 1.

[0058] Example 8 A titanium suboxide material of Example 8 was obtained in the same manner as in Example 1, except that the amount of sodium chloride added in the hydrolysis step was changed to 800 g. As in Example 1, the amount (mol%) of niobium element relative to 100 mol% of titanium element in the powder before reduction firing, the median diameter, D 90 / D 10 The results are shown in Table 1.

[0059] Example 9 A titanium suboxide material of Example 9 was obtained in the same manner as in Example 1, except that the amount of sodium chloride added in the hydrolysis step was changed to 200 g. As in Example 1, the amount (mol%) of niobium element relative to 100 mol% of titanium element in the powder before reduction firing, the median diameter, D 90 / D 10 The results are shown in Table 1.

[0060] Example 10 The titanium suboxide material of Example 10 was obtained in the same manner as in Example 1, except that the inorganic salt added in the hydrolysis step was changed to ammonium chloride and the amount added was changed to 200 g. As in Example 1, the amount (mol%) of niobium element relative to 100 mol% of titanium element in the powder before reduction firing, the median diameter, D 90 / D 10 The results are shown in Table 1.

[0061] Example 11 A titanium suboxide material of Example 11 was obtained in the same manner as in Example 1, except that the reduction firing temperature was changed to 1200°C. As in Example 1, the amount (mol%) of niobium element relative to 100 mol% of titanium element in the powder before reduction firing, the median diameter, D 90 / D 10 The results are shown in Table 1.

[0062] Example 12 Niobium pentachloride (Mitsuwa Chemicals, 44.1 g, equivalent to 3.1 mol% Nb relative to Ti in the titanium tetrachloride aqueous solution) was dissolved in 200 mL of ethanol, and 100 mL of pure water was added to the solution to prepare a niobium chloride solution. In a reaction device equipped with a reflux device, 1000 mL of titanium tetrachloride aqueous solution (Osaka Titanium, 16.7 wt% Ti, specific gravity 1.56 g / mL), the entire amount of the prepared niobium chloride solution, 300 g of sodium chloride, and 100 mL of 95% sulfuric acid were added to 2000 mL of pure water and mixed. The mixed solution was heated and stirred at 110°C and refluxed for 3 hours. The obtained slurry was added to a Buchner funnel and subjected to suction filtration, and the obtained solid was washed with 100 L of pure water. The solid was repulped in pure water, and an aqueous ammonia solution was added until the pH of the repulped slurry became about 8 to 9. The pH-adjusted slurry was filtered again, and washed with water so that the conductivity of the filtrate became 100 μS / cm or less. The washed solid was dried at 100°C and passed through a 150 μm sieve. The amount of niobium element (mol%) relative to 100 mol% of titanium element, the median diameter, and D 90 / D 10 The results are shown in Table 1. The obtained powder was placed on an alumina boat, and hydrogen gas with a concentration of 3.9 vol% using nitrogen gas as a carrier gas was passed through at a flow rate of 300 mL / min, and reduction firing was performed at a temperature of 1000° C. for 4 hours. After reduction and firing, the powder was recovered to obtain the titanium suboxide material of Example 1. The results of observation of the obtained titanium suboxide material using an electron microscope are shown in FIG.

[0063] Example 13 A titanium suboxide material of Example 13 was obtained in the same manner as in Example 12, except that the amount of niobium pentachloride used in Example 12 was changed to 14.7 g (an amount equivalent to 1.2 mol% as Nb relative to Ti in the titanium tetrachloride aqueous solution). The results of observation of the obtained titanium suboxide material with an electron microscope are shown in FIG. As in Example 12, the amount (mol%) of niobium element relative to 100 mol% of titanium element in the powder before reduction and firing, the median diameter, D 90 / D 10The results are shown in Table 1.

[0064] Example 14 28.5 g of titanium suboxide corresponding to Example 12 and 1.5 g of Magneli phase conductive titanium oxide ENETIA (manufactured by Sakai Chemical Industry Co., Ltd.) were weighed and mixed manually in a mortar for 1 hour. The mixed powder was collected to obtain the titanium suboxide material of Example 14.

[0065] Example 15 27.0 g of titanium suboxide corresponding to Example 12 and 3.0 g of Magneli phase conductive titanium oxide ENETIA (manufactured by Sakai Chemical Industry Co., Ltd.) were weighed and mixed manually in a mortar for 1 hour. The mixed powder was collected to obtain the titanium suboxide material of Example 15.

[0066] Example 16 24.0 g of titanium suboxide corresponding to Example 12 and 6.0 g of Magneli phase conductive titanium oxide ENETIA (manufactured by Sakai Chemical Industry Co., Ltd.) were weighed and mixed manually in a mortar for 1 hour. The mixed powder was collected to obtain the titanium suboxide material of Example 16.

[0067] Example 17 21.0 g of titanium suboxide corresponding to Example 12 and 9.0 g of Magneli phase conductive titanium oxide ENETIA (manufactured by Sakai Chemical Industry Co., Ltd.) were weighed and mixed manually in a mortar for 1 hour. The mixed powder was collected to obtain the titanium suboxide material of Example 17.

[0068] Comparative Example 1 A material for Comparative Example 1 was obtained in the same manner as in Example 1, except that instead of the reduction firing in Example 1, firing was performed in air at 900° C. for 4 hours. As in Example 1, the amount of niobium element (mol%) relative to 100 mol% of titanium element in the powder before air sintering, the median diameter, D 90 / D 10 The results are shown in Table 1.

[0069] Comparative Example 2 The material of Comparative Example 2 was obtained in the same manner as in Example 1, except that the amount of ammonium niobium oxalate hydrate added in Example 1 was 2.88 g (an amount equivalent to 0.50 mol % as Nb relative to Ti in titanyl sulfate). As in Example 1, the amount (mol%) of niobium element relative to 100 mol% of titanium element in the powder before reduction firing, the median diameter, D 90 / D 10 The results are shown in Table 1.

[0070] Comparative Example 3 The material of Comparative Example 3 was Magneli phase conductive titanium oxide ENETIA (manufactured by Sakai Chemical Industry Co., Ltd.).

[0071] Comparative Example 4 A mixed aqueous solution containing Ti(SO4)2 and NbF5 was prepared. The concentration of Ti(SO4)2 in the mixed aqueous solution was 15 g / L in terms of Ti. The concentration of NbF5 was 0.29 g / L in terms of Nb. A 6.0 mol / L NaOH aqueous solution was prepared separately from this mixed aqueous solution. 500 mL of NaOH aqueous solution was continuously dropped into the mixed aqueous solution (3000 mL) at a liquid temperature of 60°C. This resulted in the formation of a precipitate in the liquid. The precipitate was isolated by solid-liquid filtration, and then washed with water. The washing was performed until the electrical conductivity of the water after washing was 600 μS / cm or less at 25°C. The washed precipitate was dried at 150°C for 12 hours to remove water. The precipitate was then pulverized with a mill, and the pulverized precipitate was subjected to sintering. The sintering was performed at 1000°C for 4 hours in an atmosphere of 4% hydrogen gas. In this manner, conductive particles made of titanium dioxide with niobium dispersed throughout the particle were obtained. As in Example 1, the amount (mol%) of niobium element relative to 100 mol% of titanium element in the powder before reduction firing, the median diameter, D 90 / D 10 The results are shown in Table 1.

[0072] Comparative Example 5 15.0 g of titanium suboxide corresponding to Example 12 and 15.0 g of Magneli phase conductive titanium oxide ENETIA (manufactured by Sakai Chemical Industry Co., Ltd.) were weighed and mixed manually in a mortar for 1 hour. The mixed powder was collected to obtain the titanium suboxide material of Comparative Example 5.

[0073] [Table 1]

[0074] The median diameter and particle size distribution (D 90 / D 10 ), specific surface area, and weight variation range in the temperature ranges of 50 to 900°C and 50 to 400°C were measured. The volume resistivity and dielectric constant were measured for the materials obtained in Examples 1 to 17 and Comparative Examples 1 to 5 as they were, and for the materials obtained after heat treatment at 200°C, 400°C, and 600°C. The heat treatment was performed by placing the materials in an alumina crucible and heating them in the atmosphere at a specified temperature for 4 hours. The results are shown in Table 2.

[0075] [Table 2]

[0076] As shown in Table 2, it was confirmed that the titanium suboxide material of the present invention has high electrical conductivity and maintains excellent electrical conductivity even after heat treatment up to 400°C. In Examples 1 to 11, titanyl sulfate was used as the titanium source, while in Examples 12 and 13, titanium oxychloride was used instead of titanyl sulfate as the titanium source. In all cases, it was confirmed that a titanium suboxide material was obtained that had high electrical conductivity and maintained excellent electrical conductivity even after heat treatment up to 400°C. Comparative Example 3 showed a relatively low volume resistivity, but the volume resistivity increased by more than 100 times when heat-treated at 200° C. This is believed to be because Comparative Example 3 (1) has a Magneli phase, which is a thermodynamically unstable crystalline phase, and (2) has a large weight change between 50 and 400° C. in thermogravimetric analysis, and easily reacts with the air, resulting in oxygenation, i.e., oxidation, of the oxygen-deficient parts. Figures 1 and 2 show the results of thermogravimetric analysis of the titanium suboxide materials of Example 1 and Comparative Example 3, respectively. In Example 1 of Figure 1, there is almost no weight change up to about 500°C, suggesting that the above-mentioned oxidation reaction is not progressing. In contrast, in Comparative Example 3 of Figure 2, weight change begins at a temperature of about 200°C, suggesting that the above-mentioned oxidation reaction is progressing. Examples 14 to 17 and Comparative Example 5 are obtained by mixing ENETIA, a Magneli phase titanium suboxide, with titanium suboxide obtained by the manufacturing method of a titanium suboxide material of the present invention. The results of Examples 14 to 17 and Comparative Example 5 confirmed that even when the material contains Magneli phase titanium suboxide, as long as the proportion of this is less than a certain percentage, the material has high electrical conductivity, and maintains excellent electrical conductivity even after heat treatment up to 400°C. Comparative Example 4 reproduces the conductive titanium oxide of the example of Patent Document 1, the above-mentioned prior art document, but it had a higher volume resistivity than the example and did not exhibit sufficient conductivity. Comparative Example 4 was synthesized via a hydrolysis step of titanyl sulfate and a niobium element-containing compound with a base, and it is believed that this is because uniform coprecipitation of titanium and niobium did not occur, and efficient reduction of titanium did not proceed during reduction firing. When a resin composition obtained by kneading titanium suboxide with a resin is used as a conductive material, the heating temperature during kneading with the resin is up to about 400°C. Therefore, by using the titanium suboxide material of the present invention, a resin composition for conductive materials having excellent conductivity can be obtained. Furthermore, the conductivity and dielectric constant of the titanium suboxide material of the present invention can be reduced as desired by heating it at 600°C. By reducing the dielectric constant, the titanium suboxide material becomes a material that appropriately suppresses heat generation when irradiated with electromagnetic waves. The dielectric properties of the titanium suboxide material of the present invention can be adjusted by changing the heat treatment temperature, and the dielectric properties can be adjusted according to the application.

Claims

1. In a thermogravimetric analysis, the weight change range in the temperature range of 50 to 900°C is 0.30 to 3.40%, and the volume resistivity at 25°C when the powder is compressed at a pressure of 63 MPa is 1 x 10 0 Ω cm to 8 x 10 3 A titanium suboxide material having a resistivity of Ω·cm.

2. The titanium suboxide material according to claim 1, characterized in that, in thermogravimetric analysis, the weight change range of the titanium suboxide material is 0 to 1.20% in the temperature range of 50 to 400°C.

3. 2. The titanium suboxide material of claim 1, wherein the titanium suboxide material contains elemental niobium.

4. 2. The titanium suboxide material according to claim 1, wherein the titanium suboxide material has a rutile crystal structure.

5. Volume-based 90% diameter D in particle size distribution measurement 90 and volume-based 10% diameter D 10 Ratio to (D 90 / D 10 2. The titanium suboxide material of claim 1, wherein the σ is less than 3.

0.

6. 2. The titanium suboxide material according to claim 1, characterized in that the median diameter in the particle size distribution is 1.0 to 20 μm.

7. A first step of mixing and hydrolyzing titanyl sulfate and / or titanium oxychloride, a niobium element-containing compound, an acid, and inorganic salts; A second step of reducing and baking the hydrolyzate obtained in the first step, A method for producing a titanium suboxide material, characterized in that in the first step, a niobium-containing compound is used in an amount such that the amount of niobium contained in the niobium-containing compound is more than 0.5 mol % and not more than 15 mol % relative to 100 mol % of titanium contained in titanyl sulfate and / or titanium oxychloride.

8. The method for producing a titanium suboxide material according to claim 7, characterized in that the second step is a step of reducing and firing the hydrolyzate in an atmosphere having a hydrogen concentration of less than 4 volume %.

Citation Information

Patent Citations

  • cosmetic

    JP1983180413A

  • Production of colored titanium oxide

    JP1992046016A