Succinic anhydride group-containing cyclic organosiloxane, addition-curable silicone composition comprising succinic anhydride group-containing cyclic organosiloxane, and use of them

The succinic anhydride group-containing cyclic organosiloxane enhances adhesion in addition-curing silicone compositions, addressing the adhesion issues with metals and plastics, ensuring a smooth and non-yellowing cured product.

JP2024166203AActive Publication Date: 2024-11-28MOMENTIVE PERFORMANCE MATERIALS JAPAN LLC
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2024135598
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2024-08-15
Publication Date
2024-11-28
Estimated Expiration
2040-04-09

AI Technical Summary

Technical Problem

Existing addition-curing silicone adhesive compositions fail to provide sufficient adhesion to metals such as aluminum and engineering plastics like PPS, PBT, and PET, and do not maintain a good appearance after curing.

Method used

A succinic anhydride group-containing cyclic organosiloxane is used in an addition-curing silicone composition, combined with a platinum-based catalyst and optionally polyorganohydrogensiloxane, to enhance adhesion to various substrates, ensuring a cured product with good appearance and adhesion properties.

Benefits of technology

The composition exhibits excellent adhesion to metals and engineering plastics, maintaining a smooth surface and preventing yellowing even after further heating, with improved cohesive failure rates and shear adhesive strength.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024166203000001
    Figure 2024166203000001
  • Figure 2024166203000002
    Figure 2024166203000002
  • Figure 2024166203000003
    Figure 2024166203000003
Patent Text Reader

Abstract

To provide: a cyclic organosiloxane that can be used as an adhesive aid for an addition-curable silicone composition to form a cured product with good appearance and excellent adhesion to various substrates; and an addition-curable silicone composition comprising the same.SOLUTION: The present invention relates to: a succinic anhydride group-containing cyclic organosiloxane (where the succinic anhydride group-containing cyclic organosiloxane has, in its molecule, one or more succinic anhydride groups, and one or more hydrogen atoms directly bonded to silicon atoms); an addition-curable silicone composition which comprises the succinic anhydride group-containing cyclic organosiloxane; and adhesive aids and adhesives based on them.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a succinic anhydride group-containing cyclic organosiloxane, an addition-curable silicone composition containing said succinic anhydride group-containing cyclic organosiloxane, and uses thereof. [Background technology]

[0002] The addition-curing silicone adhesive composition cures at room temperature or, if necessary, by heating to develop adhesion to various adherends. Addition-type silicones are used as adhesives and potting agents for in-vehicle electronic components. In addition, in order to improve adhesion to substrates, adhesive assistants are used. Patent Document 1 proposes an organosilicon compound that contains a hydrosilyl group (a hydrogen atom directly bonded to a silicon atom) and has bisphenol A in its skeleton as an adhesive assistant for fluorine-containing adhesives. Patent Document 2 also proposes a cyclic organosiloxane having a hydrolyzable silyl group and two or more succinic anhydride groups as an adhesive assistant for organosiloxane compositions. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2002-114793 A [Patent Document 2] JP 2013-32498 A Summary of the Invention [Problem to be solved by the invention]

[0004] There is an increasing demand for the use of addition-curing silicone adhesive compositions to bond metals such as aluminum and aluminum die-casting, and engineering plastics such as PPS, PBT, and PET. According to the findings of the present inventors, the adhesive assistants described in Patent Documents 1 and 2 do not function adequately as adhesive assistants. That is, the silicone compositions containing the adhesive assistants described in Patent Documents 1 and 2 have the problem of insufficient adhesion to various engineering plastics including PPS and metals.

[0005] The present invention has an object to provide a cyclic organosiloxane that functions as an adhesion promoter that has excellent adhesion to various substrates and gives cured products with good appearance. Another object of the present invention is to provide an addition-curable silicone composition that contains the cyclic organosiloxane and that gives cured products with excellent adhesion to various substrates and good appearance. [Means for solving the problem]

[0006] The present invention relates to the following [1] to [5]. [1] A cyclic organosiloxane containing a succinic anhydride group represented by the following general formula (1): [ka] (In the formula, R 1 are independently a monovalent hydrocarbon group containing no fluorine atoms, R 2 are each independently a divalent hydrocarbon group having 2 to 10 carbon atoms, a is an integer of 0 or 1 or more, b is an integer equal to or greater than 1; c is an integer equal to or greater than 1, provided that a+b+c is an integer greater than or equal to 3) [2] The succinic anhydride group-containing cyclic organosiloxane of [1], wherein a+b+c is an integer of 3 to 8. [3] An adhesive agent using the succinic anhydride group-containing cyclic organosiloxane of [1] or [2]. [4] (A) a polyorganosiloxane having two or more alkenyl groups bonded to silicon atoms in the molecule; (C) a platinum-based catalyst; and (D) the succinic anhydride group-containing cyclic organosiloxane of [1] or [2]; and optionally, (B) a polyorganohydrogensiloxane having three or more hydrogen atoms directly bonded to silicon atoms in the molecule. [5] An adhesive using the addition-curing silicone composition of [4]. Effect of the Invention

[0007] The present invention provides a cyclic organosiloxane that functions as an adhesion promoter that provides a cured product with excellent adhesion to various substrates and good appearance. The present invention also provides an addition-curable silicone composition that contains the cyclic organosiloxane and has excellent adhesion to various substrates. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0008] [Terminology definition] The structural units of siloxane compounds are sometimes described by the following abbreviations (hereinafter, these structural units are referred to as "M units" and "D units" respectively). H (sometimes called "units"). M :Si(CH3)3O 1 / 2 M H :SiH(CH3)2O 1 / 2 M Vi :Si(CH=CH2)(CH3)2O 1 / 2 D :Si(CH3)2O 2 / 2 D H :SiH(CH3)O 2 / 2 D Vi :Si(CH=CH2)(CH3)O 2 / 2 T :Si(CH3)O3 / 2 Q :SiO 4 / 2 (tetrafunctional)

[0009] In this specification, specific examples of groups are as follows. Examples of the monovalent hydrocarbon group include an alkyl group, a cycloalkyl group, an aryl group, an aralkyl group, and an alkenyl group. Examples of the monovalent hydrocarbon group having no aliphatic unsaturated bond include the above-mentioned monovalent hydrocarbon groups other than the alkenyl group.

[0010] The alkyl group is a straight-chain or branched group having 1 to 18 carbon atoms, and examples thereof include a methyl group, an ethyl group, a propyl group, a butyl group, a pentyl group, a hexyl group, an octyl group, a decyl group, a dodecyl group, a hexadecyl group, and an octadecyl group. The cycloalkyl group is a monocyclic or polycyclic group having 3 to 20 carbon atoms, and examples thereof include a cyclopentyl group and a cyclohexyl group. The aryl group is an aromatic group containing a monocyclic or polycyclic group having 6 to 20 carbon atoms, and examples thereof include a phenyl group and a naphthyl group. The aralkyl group is an alkyl group substituted with an aryl group, and examples thereof include a 2-phenylethyl group and a 2-phenylpropyl group. The alkenyl group is a straight-chain or branched group having 2 to 6 carbon atoms, and examples thereof include a vinyl group, an allyl group, a 3-butenyl group, and a 5-hexenyl group. The monovalent hydrocarbon group may be unsubstituted or substituted with a substituent. Examples of the substituent include halogen atoms such as fluorine, chlorine, and bromine; and cyano groups. Examples of the monovalent hydrocarbon group substituted with a halogen atom include a chloromethyl group, a chlorophenyl group, and a 3,3,3-trifluoropropyl group. Examples of the monovalent hydrocarbon group substituted with a cyano group include a 2-cyanoethyl group.

[0011] Examples of the monovalent hydrocarbon group not containing a fluorine atom include the above-mentioned monovalent hydrocarbon groups which are unsubstituted or substituted with the above-mentioned substituents (excluding fluorine atoms).

[0012] The divalent hydrocarbon group is a group obtained by removing a hydrogen atom from the above-mentioned monovalent hydrocarbon group, and examples of the divalent hydrocarbon group include an alkylene group, a cycloalkylene group, an arylene group, an aralkylene group, and an alkenylene group. The alkylene group is a straight-chain or branched group having 1 to 18 carbon atoms, and examples thereof include a methylene group, an ethylene group, a trimethylene group, a 2-methylethylene group, and a tetramethylene group. The divalent hydrocarbon group may be unsubstituted or substituted with the above-mentioned substituents, but preferably does not contain a fluorine atom.

[0013] [Succinic anhydride group-containing cyclic organosiloxane] The succinic anhydride group-containing cyclic organosiloxane (hereinafter also referred to as "cyclic organosiloxane") is represented by the following general formula (1). [ka] (In the formula, R 1 , R 2 , a, b and c are as defined above.

[0014] The succinic anhydride group-containing cyclic organosiloxane functions as an adhesion promoter for addition curing silicone compositions that provide a cured product with excellent adhesion to various substrates and good appearance, particularly under curing conditions of 150°C for 1 hour or 100°C for 2 hours. The succinic anhydride group-containing cyclic organosiloxane also functions as an adhesion promoter that provides a cured product with good appearance, particularly under curing conditions of 150°C for 1 hour. That is, the cured product of the addition curing silicone composition containing the adhesive aid made of the succinic anhydride group-containing cyclic organosiloxane has a smooth surface and does not exude liquid to the surface. The succinic anhydride group-containing cyclic organosiloxane also functions as an adhesion promoter that provides a cured product with good appearance even after heating. That is, even when the cured product of the addition curing silicone composition containing the adhesive aid made of the succinic anhydride group-containing cyclic organosiloxane is further heated, it has an appearance with reduced yellowing.

[0015] The succinic anhydride group-containing cyclic organosiloxane may be a random copolymer, a block copolymer, or a combination thereof. In formula (1), a to c indicate the number of units defined by a to c. In formula (1), the units defined by a to c may be the same or different.

[0016] R 1 R is independently a monovalent hydrocarbon group that does not contain a fluorine atom. 1 is preferably an alkyl group not containing a fluorine atom, more preferably an unsubstituted alkyl group, further preferably an unsubstituted alkyl group having 1 to 4 carbon atoms, and particularly preferably a methyl group.

[0017] R 2 R is independently a divalent hydrocarbon group having 2 to 10 carbon atoms. 2 is preferably an alkylene group, and particularly preferably an ethylene group, a trimethylene group, or a 2-methylethylene group.

[0018] a is an integer of 0 or equal to or greater than 1. In terms of ease of synthesis and handling, a is preferably 0 or an integer of 1 to 3, and particularly preferably 0 or an integer of 1 to 2.

[0019] b is an integer of 1 or more. When b is an integer of 1 or more, the succinic anhydride group-containing cyclic organosiloxane has a hydrosilyl group (hydrogen atom directly bonded to silicon atom) participating in the addition reaction. b is preferably an integer of 1 to 5, particularly preferably an integer of 1 to 3, because it acts as a bridge between the silicone composition and various members to be bonded as a component that imparts adhesiveness, and in some cases, the cyclic organosiloxane component alone serves as a crosslinking point of the silicone composition. When b is 0, there is no bridging effect, and the adhesiveness is poor. That is, such a cyclic organosiloxane-containing silicone composition has poor function as an adhesive aid. On the other hand, a silicone composition containing a succinic anhydride group-containing cyclic organosiloxane in which b is an integer of 5 or less can obtain a cured product with excellent rubber elasticity.

[0020] c is an integer of 1 or more. When c is an integer of 1 or more, the cyclic organosiloxane contains a succinic anhydride group. c is preferably an integer of 1 to 3, particularly preferably an integer of 1 to 2, from the viewpoint of the effect on storage stability due to compatibility with the silicone composition and adhesion to various members. When c is 0, adhesion is poor. That is, such a cyclic organosiloxane-containing cyclic organosiloxane has poor function as an adhesive aid. In addition, a composition containing a succinic anhydride group-containing cyclic organosiloxane in which c is 3 or less can give a cured product with improved heat resistance, appropriate hardness, and good adhesion to various members.

[0021] In addition, a+b+c is an integer of 3 or more. When a+b+c is an integer of 3 or more, the main skeleton becomes a cyclic organosiloxane. From the viewpoint of ease of synthesis, a+b+c is preferably an integer of 3 to 8, and particularly preferably an integer of 3 to 6. That is, when a+b+c is an integer of 3 or more, D, which can be a raw material, a D H 8-a The cyclic compound itself is easy to synthesize. When a+b+c is an integer of 8 or less, the raw material D a D H 8-a When isolating the target compound (Da D H 8-a This makes it easy to separate and purify the cyclic organosiloxane with high purity.

[0022] (Uses of succinic anhydride group-containing cyclic organosiloxane) The succinic anhydride group-containing cyclic organosiloxane can be used as an adhesion promoter to improve the adhesion of addition-curable silicone compositions, which are described below.

[0023] (Method for Producing Succinic Anhydride Group-Containing Cyclic Organosiloxane) The succinic anhydride group-containing cyclic organosiloxane can be prepared by utilizing a method known to those skilled in the art or a similar method. The method for producing the succinic anhydride group-containing cyclic organosiloxane includes a method of reacting a cyclic siloxane having two or more hydrogen atoms directly bonded to a silicon atom with a succinic anhydride having an unsaturated bond to obtain a siloxane having a structure represented by general formula (1). Those skilled in the art can appropriately select the reaction conditions, purification method, etc. From the viewpoint of easily obtaining a product with high purity, and from the viewpoint of facilitating the synthesis and purification of the raw material, which is a cyclic compound containing hydrogen atoms directly bonded to silicon atoms, a method for producing a cyclic organosiloxane containing succinic anhydride groups is preferred, in which a is 2, b is 1, c is 1, and a+b+c is 4, a cyclic siloxane is used which has four-membered rings and two hydrogen atoms directly bonded to silicon atoms, in which a is 2, b is 1, c is 1, and a+b+c is 4, a cyclic siloxane is used which has three hydrogen atoms directly bonded to silicon atoms, in which a is 1 and a+b+c is 4, or a cyclic siloxane is used which has four hydrogen atoms directly bonded to silicon atoms, in which a is 0 and a+b+c is 4.

[0024] [Addition-curable silicone composition] The addition curing type silicone composition (hereinafter, simply referred to as "silicone composition") contains the above-mentioned succinic anhydride group-containing cyclic organosiloxane. Since the silicone composition contains the succinic anhydride group-containing cyclic organosiloxane, it can achieve excellent adhesion to various substrates, particularly metals (aluminum, aluminum die cast, etc.) and engineering plastics (polybutylene terephthalate resin (PBT resin), polyphenylene sulfide resin (PPS resin), polyethylene terephthalate resin (PET resin), etc.).

[0025] The silicone composition is not particularly limited as long as it is a silicone composition capable of forming a crosslinked structure by utilizing an addition reaction between an alkenyl group bonded to a silicon atom and a hydrogen atom directly bonded to a silicon atom. Specifically, the silicone composition comprises the following components: (A) a polyorganosiloxane having two or more alkenyl groups bonded to silicon atoms in the molecule; (C) a platinum-based catalyst; and (D) the succinic anhydride group-containing cyclic organosiloxane; and optionally containing (B) a polyorganohydrogensiloxane having three or more hydrogen atoms directly bonded to silicon atoms in the molecule (excluding component (D)).

[0026] In this specification, "(A) a polyorganosiloxane having two or more silicon-bonded alkenyl groups in the molecule" is also referred to as "component (A)". The same applies to "(C) a platinum-based catalyst" and the like.

[0027] In a silicone composition containing components (A), (C), and (D), and optionally containing component (B), an addition-curable silicone composition can be produced depending on the number of hydrosilyl groups in component (D) (i.e., b) and the number of alkenyl groups in component (A). Specifically, this is as follows: (i) When the number of alkenyl groups in component (A) is 2 or more, the silicone composition can be made into an addition-curable silicone composition by further containing component (B). In this case, the value of b in component (D) can be 1 or more. (ii) When the number of alkenyl groups in component (A) exceeds 2, an addition-curable silicone composition can be made by including component (D) in which the value of b is 2 or greater. In this case, the silicone composition may further include component (B), or may include component (D) in which the value of b is 1. (iii) When the number of alkenyl groups in component (A) is 2, an addition-curable silicone composition can be obtained by including component (D) in which the value of b is 3 or greater. In this case, the silicone composition may further include component (B), and may also include component (D) in which the value of b is 1 or 2. Such a silicone composition may be the following first, second or third silicone composition.

[0028] (First silicone composition) The first silicone composition contains a cyclic organosiloxane containing a succinic anhydride group, in which b is an integer of 1. In this case, the first silicone composition contains (A1) a polyorganosiloxane having two or more alkenyl groups bonded to silicon atoms in the molecule; (B) a polyorganohydrogensiloxane having three or more hydrogen atoms directly bonded to silicon atoms in the molecule; (C) a platinum-based catalyst; and (D1) a cyclic organosiloxane containing a succinic anhydride group, in which b is an integer of 1.

[0029] In the first silicone composition, component (B) has three or more hydrogen atoms directly bonded to silicon atoms in the molecule, so a cured product can be formed by a crosslinking reaction between components (A1) and (B) even if b in component (D1) is an integer of 1. The first silicone composition may also contain (D) a cyclic organosiloxane containing a succinic anhydride group, in which b is an integer of 2 or more.

[0030] (Second Silicone Composition) The second silicone composition contains a cyclic organosiloxane containing a succinic anhydride group, in which b is an integer of 2. In this case, the second silicone composition contains (A2) a polyorganosiloxane having more than two alkenyl groups bonded to silicon atoms in the molecule; (C) a platinum-based catalyst; and (D2) a cyclic organosiloxane containing a succinic anhydride group, in which b is an integer of 2.

[0031] The second silicone composition can form a cured product by a crosslinking reaction even when b is an integer of 2, because the number of alkenyl groups bonded to silicon atoms in component (A2) in the molecule is more than 2. The second silicone composition may further contain (D) a cyclic organosiloxane containing a succinic anhydride group, in which b is an integer of 1 or 3 or more. The second silicone composition may further contain (B) a polyorganohydrogensiloxane having three or more hydrogen atoms bonded directly to silicon atoms in the molecule.

[0032] (Third Silicone Composition) The third silicone composition contains a cyclic organosiloxane containing a succinic anhydride group, in which b is an integer of 3 or greater. In this case, the third silicone composition contains (A1) a polyorganosiloxane having two or more alkenyl groups bonded to silicon atoms in the molecule; (C) a platinum catalyst; and (D3) a cyclic organosiloxane containing a succinic anhydride group, in which b is an integer of 3 or greater.

[0033] The third silicone composition can form a cured product by a crosslinking reaction between the (A1) and (D3) components, since the number of hydrogen atoms directly bonded to silicon atoms in the (D3) component is 3 or more per molecule. The third silicone composition may also contain (D) a cyclic organosiloxane containing a succinic anhydride group, in which b is 1 or 2. The third silicone composition may also contain (B) a polyorganohydrogensiloxane having 3 or more hydrogen atoms directly bonded to silicon atoms per molecule.

[0034] The components contained in the first, second or third silicone composition are as follows. <(A1) Polyorganosiloxane having two or more alkenyl groups bonded to silicon atoms in the molecule> (A1) Polyorganosiloxane having two or more alkenyl groups bonded to silicon atoms in the molecule (hereinafter also referred to as "(A1) alkenyl group-containing polyorganosiloxane") is a component that serves as the base polymer in the silicone composition. A network structure is formed in the cured product of the silicone composition by addition reaction between the alkenyl group of component (A1) and the hydrosilyl group (hydrogen atom directly bonded to silicon atom) of component (B) or (D). There are no particular limitations on component (A1) as long as it is capable of forming the network structure together with component (B) and / or component (D). Component (A) is typically represented by the general formula (I): (R 11 ) e (R 12 ) f SiO (4-e-f) / 2 (I) (In the formula, R 11 is an alkenyl group, R 12 is a monovalent hydrocarbon group having no aliphatic unsaturated bonds, e is an integer from 1 to 3; f is an integer from 0 to 2, with the proviso that e+f is an integer from 1 to 3. In (A1), the number of alkenyl groups bonded to silicon atoms is preferably 2 to 100, and more preferably 2 to 50, in the molecule.

[0035] R 11 From the viewpoints of ease of synthesis and of the fluidity of the silicone composition before curing, R is preferably a vinyl group. e is preferably 1 from the viewpoint of ease of synthesis. 12is preferably a methyl group or a phenyl group, and particularly preferably a methyl group, from the viewpoints of ease of synthesis and excellent balance of properties such as mechanical strength and fluidity before curing. In addition, from the viewpoint of being able to control the fluidity and thixotropy when applying the silicone composition before curing to a substrate, a polyorganosiloxane having only methyl groups and a polysiloxane having phenyl groups and methyl groups can be used in combination.

[0036] The organic group bonded to the silicon atom of the other siloxane unit in the component (A1) is, for example, a monovalent hydrocarbon group that does not have an aliphatic unsaturated bond. 12 For the same reasons as above, a methyl group or a phenyl group is preferred, and a methyl group is particularly preferred.

[0037] R 11 may be present either at the terminals or in the middle of the molecular chain of component (A1), or may be present at both.

[0038] The siloxane skeleton of the component (A1) can be linear or branched, that is, the component (A) can be a linear polyorganosiloxane (A1-1) or a branched polyorganosiloxane (A1-2).

[0039] (A1-1) As the linear polyorganosiloxane, both ends are RSiO 1 / 2 Blocked in units, intermediate unit is R 12 2SiO 2 / 2 The unit is a linear polyorganosiloxane (where R is R 11 or R 12 and R 11 is an alkenyl group, R 12 is a monovalent hydrocarbon group that does not have an aliphatic unsaturated bond and has two or more R 11 (Containing RSiO in component (A1-1) 1 / 2 The unit is R. 11 R 12 2SiO 1 / 2 Units, R 11 2R 12SiO 1 / 2 Unit or R 11 3SiO 1 / 2 The unit is preferably R 11 R 12 2SiO 1 / 2 It is particularly preferred that the unit is a unit.

[0040] (A1-2) Branched polyorganosiloxane has SiO as an essential unit. 4 / 2 Units and RSiO 1 / 2 Including units, as well as RSiO as an arbitrary unit 2 / 2 Units and / or RSiO 3 / 2 In particular, the branched polyorganosiloxanes include those containing the units R 11 or R 12 However, in R, there are two or more R per molecule. 11 In order to act as crosslinking points in the curing reaction, at least three R per molecule are R 11 and the remainder is R 12 From the viewpoint of providing the cured product of the silicone composition with excellent mechanical strength, it is preferable that RSiO 1 / 2 Units and SiO 4 / 2 The molar ratio of the units is preferably within the range of 1:0.8 to 1:3, and the resin is a solid or viscous semi-solid resin at room temperature.

[0041] In the (A1-2) component, R 11 is R3SiO 1 / 2 It may also exist as a unit R, RSiO unit or RSiO 3 / 2 It may also exist as the unit R.

[0042] The viscosity of the (A1) component at 23°C is preferably 0.1 to 500 Pa·s, more preferably 0.3 to 300 Pa·s, and particularly preferably 0.5 to 200 Pa·s. When the viscosity of the (A1) component is in the above range, the adhesiveness to various substrates can be efficiently improved, the silicone composition in the uncured state exhibits good fluidity and excellent workability during casting and potting, and the cured product of the silicone composition exhibits excellent mechanical strength, appropriate elasticity and hardness. In addition, in order to further improve the adhesiveness even at room temperature, it is preferable that the viscosity of the (A1) component is high. Here, when the (A1) component is a combination of two or more types, the viscosity of the (A1) component means the viscosity of the mixed alkenyl group-containing polyorganosiloxane. In this specification, the viscosity is a value measured using a rotational viscometer in accordance with JIS K 6249, with the spindle number and rotation speed appropriately set, under conditions of 23°C.

[0043] The component (A1) may be one type or a combination of two or more types. For example, the component (A1) may be two or more types of linear alkenyl-containing polyorganosiloxanes (A1-1), or may be a mixture of one or more types of linear alkenyl-containing polyorganosiloxanes (A1-1) and one or more types of branched alkenyl-containing polyorganosiloxanes (A1-2).

[0044] The (A1) component has both ends terminated with R. 11 R 12 2SiO 1 / 2 Blocked in units, intermediate unit is R 12 2SiO 2 / 2 A linear polyorganosiloxane having a viscosity of 0.1 to 500 Pa s at 23°C (in each of the above formulas, R represents R 11 or R 12 and R 11 is an alkenyl group, R 12 is a monovalent hydrocarbon group that does not have an aliphatic unsaturated bond and has two or more R 11 ) and SiO as an essential unit 4 / 2 Units and RSiO 1 / 2Including units and optional units RSiO 2 / 2 Units and RSiO 3 / 2 Branched polyorganosiloxanes containing units (R is R 11 or R 12 However, in R, at least three R per molecule are R 11 and the remainder is R 12 In addition, the component (A1) is preferably a combination of vi It is particularly preferred that the polyorganosiloxane is a linear polyorganosiloxane that is blocked with D units (dimethylvinylsiloxane units) and has intermediate units consisting only of D units (dimethylsiloxane units).

[0045] Component (A1) is not a component that corresponds to component (D). Component (A) preferably does not have any adhesion-imparting functional groups other than silicon-bonded alkenyl groups. In addition, component (A1) particularly preferably does not have one or more groups selected from epoxy groups, silicon-bonded alkoxy groups, and silicon-bonded hydrogen atoms.

[0046] <(A2) Polyorganosiloxane having more than two alkenyl groups bonded to silicon atoms in the molecule> (A2) polyorganosiloxane having more than two alkenyl groups bonded to silicon atoms in the molecule is as described above for component (A1), including preferred examples, except that it has more than two alkenyl groups bonded to silicon atoms in the molecule. Component (A2) may be a mixture of a polyorganosiloxane having three or more alkenyl groups bonded to silicon atoms in the molecule and a polyorganosiloxane having two alkenyl groups bonded to silicon atoms in the molecule.

[0047] <(B) Polyorganohydrogensiloxane having three or more hydrogen atoms directly bonded to silicon atoms in the molecule> The polyorganohydrogensiloxane (B) having three or more hydrogen atoms directly bonded to silicon atoms in the molecule (excluding component (D)) (hereinafter also referred to as "polyorganohydrogensiloxane (B)") is not particularly limited as long as it functions as a crosslinking agent for component (A).

[0048] The component (B) is typically represented by the general formula (II): (R 13 ) g H h SiO (4-g-h) / 2 (II) (In the formula, R 13 is a monovalent hydrocarbon group having no aliphatic unsaturated bonds, g is an integer from 0 to 2; h is an integer from 1 to 3, with the proviso that g+h is an integer from 1 to 3. The molecule has three or more units represented by the following formula:

[0049] R 13 is preferably a methyl group from the viewpoint of ease of synthesis, and h is preferably 1 from the viewpoint of ease of synthesis.

[0050] From the viewpoint of ease of synthesis, it is preferable that component (B) has 3 or more siloxane units. Moreover, from the viewpoints of not volatilizing even when heated to a curing temperature, and having excellent fluidity and being easily mixed with component (A), the number of siloxane units in component (B) is preferably 6 to 200, and particularly preferably 10 to 150.

[0051] The siloxane skeleton in component (B) may be linear, branched, or cyclic, with linear being preferred.

[0052] The component (B) is a compound (B1) having two ends each independently represented by R 14 3SiO 1 / 2 It is blocked by units, and the intermediate unit is R 14 2SiO 2 / 2 A linear polyorganohydrogensiloxane consisting of only units, and (B2)R14 3SiO 1 / 2 Units and SiO 4 / 2 Polyorganohydrogensiloxane (in each of the above formulas, R 14 are each independently a hydrogen atom or a monovalent hydrocarbon group having no aliphatic unsaturated bonds, provided that R 14 In the case of the component (B1) and the component (B2), it is preferable that at least three of R 14 3SiO 1 / 2 The unit is HR. 15 2SiO 1 / 2 Units and R 15 3SiO 1 / 2 The units are listed as R 14 2SiO 2 / 2 The unit is HR. 15 SiO 2 / 2 Units and R 15 2SiO 2 / 2 Units (in the above formulas, R 15 is a monovalent hydrocarbon group having no aliphatic unsaturated bonds.) In the case of component (B1), the hydrogen atom bonded to the silicon atom may be present at the terminal or in the middle unit, but is preferably present in the middle unit.

[0053] The (B) component is a siloxane having a chain length of 100 nm and a length of 100 nm, both ends of which are blocked with M units (trimethylsiloxane units) and the middle unit is D. H (B1-2) a linear polymethylhydrogensiloxane consisting only of units (methylhydrogensiloxane units), (B1-3) a linear polymethylhydrogensiloxane consisting only of units (methylhydrogensiloxane units), (B1-4) a linear polymethylhydrogensiloxane consisting only of units (methylhydrogensiloxane units), (B1-5) a linear polymethylhydrogensiloxane consisting only of units (methylhydrogensiloxane units), (B1-6) a linear polymethylhydrogensiloxane consisting only of units (methylhydrogensiloxane units), (B1-7) a linear polymethylhydrogensiloxane consisting only of units (methylhydrogensiloxane units), (B1-8) a linear polymethylhydrogensiloxane consisting only of units (methylhydrogensiloxane units), H (B1-3) a linear polymethylhydrogensiloxane consisting only of units (methylhydrogensiloxane units) and having 0.1 to 3.0 moles of methylhydrogensiloxane units per mole of dimethylsiloxane units; H It is blocked with a dimethylhydrogensiloxane unit, and the intermediate unit is D H(B1-4) Linear polymethylhydrogensiloxane consisting only of units (methylhydrogensiloxane units), H The intermediate units are D units (dimethylsiloxane units) and D H linear polymethylhydrogensiloxanes consisting only of units (methylhydrogensiloxane units) and having 0.1 to 3.0 moles of methylhydrogensiloxane units per mole of dimethylsiloxane units, and (B2-1) M H unit (dimethylhydrogensiloxane unit) and Q unit (SiO 2 / 2 More preferred is a polymethylhydrogensiloxane consisting only of (B-1) and (B-2) components. The component (B) may be one type or a combination of two or more types.

[0054] Component (B) is not a component corresponding to component (D) and preferably does not have a succinic anhydride group. Also, component (B) preferably does not have an ester bond and / or does not have one or more groups selected from an aliphatic unsaturated hydrocarbon group, an epoxy group, and an alkoxy group bonded to a silicon atom.

[0055] <(C) Platinum-based catalyst> (C) The platinum catalyst is a catalyst for promoting the addition reaction between alkenyl groups and hydrosilyl groups in the silicone composition.

[0056] Examples of component (C) include platinum compounds such as chloroplatinic acid, reaction products of chloroplatinic acid and alcohols (for example, Lamoreaux's catalyst (platinum-octanol complex, U.S. Pat. No. 3,220,972)), platinum-olefin complexes, platinum-vinylsiloxane complexes, platinum-ketone complexes, and platinum-phosphine complexes. Of these, the reaction products of chloroplatinic acid and alcohols and platinum-vinylsiloxane complexes are preferred because of their good catalytic activity, and are appropriately selected depending on the purpose of use. The component (C) may be one type or a combination of two or more types.

[0057] <(D) Succinic anhydride group-containing cyclic organosiloxane> (D) Succinic anhydride group-containing cyclic organosiloxanes include the following (D1), (D2), and (D3) depending on the number b. (D1) A cyclic organosiloxane containing a succinic anhydride group, in which b is an integer of 1. (D2) A cyclic organosiloxane containing a succinic anhydride group, wherein b is an integer of 2. (D3) A cyclic organosiloxane containing a succinic anhydride group, in which b is an integer of 3 or more. The components (D1), (D2) and (D3) are as described above, including preferred embodiments, except that the number b is different. The components (D) may each be one type or a combination of two or more types.

[0058] <(E) Further Ingredients> The silicone composition may contain (E) an additional component other than the components (A) to (D) to the extent that the effects of the present invention are not impaired. Such components include (E1) an inorganic filler, (E2) a reaction inhibitor, and (E3) various additives. Each of the (E) additional components may be one type or a combination of two or more types.

[0059] <<(E1) Inorganic filler>> The silicone composition contains (E1) inorganic filler, which gives the cured product of the silicone composition high mechanical strength. (E1) inorganic filler includes reinforcing fillers such as fumed silica, calcined silica, silica aerogel, precipitated silica, and fumed titanium oxide; and non-reinforcing fillers such as diatomaceous earth, ground silica, aluminum oxide, zinc oxide, titanium oxide, aluminosilicate, calcium carbonate, calcium carbonate, magnesium carbonate, zinc carbonate, calcium silicate, talc, and ferric oxide, which are selected according to extrusion workability and the physical properties required for the cured product of the silicone composition. (E1) inorganic filler is preferably a reinforcing filler, more preferably silica such as fumed silica, calcined silica, silica aerogel, and precipitated silica, and particularly preferably fumed silica.

[0060] (E1) When the inorganic filler is fumed silica, the BET specific surface area of ​​the inorganic filler is 50 to 500 m 2 / g, and 80 to 400m 2 / g is more preferable, and 100 to 300m 2 It is particularly preferred that the molecular weight is / g.

[0061] The inorganic filler (E1) may be treated with a surface treatment agent, such as organoalkoxysilane, organohalosilane, siloxane oligomers, or organosilazane.

[0062] <<(E2) Reaction inhibitor>> The (E2) reaction inhibitor is a component that inhibits the curing reaction rate of the silicone composition, thereby contributing to improving the balance between ease of handling and the development of adhesiveness and the curing rate. Examples of the (E2) reaction inhibitor include isocyanurates that have an aliphatic unsaturated hydrocarbon group and do not have an alkoxy group bonded to a silicon atom, such as triallyl isocyanurate, diallyl methyl isocyanurate, diallyl ethyl isocyanurate, tributenyl isocyanurate, and diallyl phenyl isocyanurate; organic compounds that have a polar group in the molecule, such as diallyl maleate; organic compounds that have an unsaturated bond, such as acetylene alcohols and derivatives thereof, such as 3,5-dimethyl-1-hexyn-3-ol; and the like.

[0063] <<(E3) Various Additives>> Depending on the purpose, the silicone composition may further contain (E3) various additives such as (E3-1) an adhesion imparting agent, (E3-2) a polyorganohydrogensiloxane having two hydrogen atoms directly bonded to silicon atoms, an organic solvent, an inorganic pigment, an organic pigment, a thixotropy imparting agent, a viscosity modifier for improving extrusion workability, an ultraviolet protection agent, an antifungal agent, a heat resistance improving agent, a flame retardant, etc. Each of the various additives (E3) may be a single type or a combination of two or more types.

[0064] The adhesion promoter (E3-1) has two or more adhesion-imparting functional groups selected from an aliphatic unsaturated hydrocarbon group, an epoxy group, a polar group such as a carbonyl group or an isocyanuric group, an alkoxy group bonded to a silicon atom, and a hydrogen atom bonded directly to a silicon atom. The component (E3-1) is a component that imparts adhesion to various substrates to the composition, and can be appropriately selected from known adhesion promoters that can be applied to silicone compositions. However, the adhesion promoter (E3-1) is not the components (A) to (D), the component (E2), or the component (E3-2) described below.

[0065] The polyorganohydrogensiloxane (E3-2) having two hydrogen atoms directly bonded to silicon atoms is as described above for component (B) except that there are two hydrogen atoms directly bonded to silicon atoms. H A linear polymethylhydrogensiloxane in which the intermediate units are blocked with D units (dimethylhydrogensiloxane units) is preferred. The component (E3-2) is not a component corresponding to the component (D) and preferably does not have a succinic anhydride group. In addition, the component (E3-2) preferably does not have an ester bond and / or does not have one or more groups selected from an aliphatic unsaturated hydrocarbon group, an epoxy group, and an alkoxy group bonded to a silicon atom.

[0066] [Content] The content of each component in the silicone composition is preferably as follows. There are no particular limitations on the contents of components (B) and (D) as long as they are sufficient to cure the silicone composition. A The number of hydrogen atoms directly bonded to silicon atoms in component (B) relative to B and the number of hydrogen atoms directly bonded to silicon atoms in component (D), H D The ratio of the sum of {(H B +H D ) / Vi A The amount of {(H B +H D ) / Vi A When {(H B +H D ) / Vi A} is (H D / Vi A ) The content of the component (D) is the same as that of the above {(HB +H D ) / Vi A In addition to satisfying the above condition, the content of component (D) is more preferably 0.1 to 20 parts by mass, even more preferably 0.5 to 10 parts by mass, and particularly preferably 1 to 5 parts by mass, per 100 parts by mass of component (A). When the content of component (D) is 0.1 part by mass or more, per 100 parts by mass of component (A), the adhesion to various members is further improved, and when it is 20 parts by mass or less, the adhesion can be efficiently improved and the heat resistance can be improved.

[0067] The content of component (C) is a catalytic amount relative to the total amount of the silicone composition. Specifically, the content of component (C) is preferably 0.1 to 1,000 mass ppm, and particularly preferably 0.5 to 200 mass ppm, calculated as platinum metal atom, relative to 100 parts by mass of the total composition. When the content of component (C) is within the above range, the curability is sufficient.

[0068] The content of the (E1) inorganic filler is preferably 0.1 to 60 parts by mass, and particularly preferably 1 to 45 parts by mass, per 100 parts by mass of the (A) component. Such a content provides excellent extrusion workability and provides the obtained cured product with excellent mechanical strength. The content of the surface treatment agent can be appropriately determined depending on the specific surface area of ​​the (E1) inorganic filler and the degree of surface treatment.

[0069] The content of the reaction inhibitor (E2) is preferably 0.001 to 20 parts by mass, and particularly preferably 0.01 to 10 parts by mass, per 100 parts by mass of the component (A). Within this range, the effect of the reaction inhibitor can be efficiently exerted.

[0070] There are no particular limitations on the amount of the additional component (E) other than the components (E1) and (E2), so long as it does not impair the intended use of the silicone composition.

[0071] (Method of producing silicone composition) The silicone composition can be produced by uniformly kneading the essential components (A), (C), and (D), as well as the optional components (B) and / or (E) using a mixing means such as a universal kneader or kneader.

[0072] (Preferred embodiment of the composition) For stable long-term storage, the components (B) and (D) may be appropriately distributed and stored in two or more containers, with component (C) being stored in a separate container, and then mixed immediately before use.

[0073] (Uses of silicone compositions) The silicone composition has excellent adhesive properties to a variety of substrates and can therefore be used as an adhesive for a variety of substrates.

[0074] <Adhesion method> The silicone composition can be attached to the object to be bonded by a method such as injection, dripping, casting, casting, extrusion from a container, or integral molding such as transfer molding or injection molding, and cured, thereby simultaneously bonding the silicone composition to the object to be bonded. The curing conditions (i.e., heating temperature and heating time) can be appropriately adjusted according to the heat resistance temperature of the member to which the silicone composition is applied. From the viewpoint of the heat resistance and operability of the member to be bonded, the heating temperature is preferably 80 to 180°C, more preferably 80 to 150°C, and particularly preferably more than 100°C and 150°C or less. From the viewpoint of the simplicity of the curing process, the heating time is preferably 1 minute to 24 hours, more preferably 1 minute to 12 hours, and particularly preferably 1 minute to 8 hours.

[0075] The material of the object to be bonded is not particularly limited, and examples include metals such as aluminum, magnesium, nickel, iron, copper, etc., or alloys thereof (e.g., aluminum die casting), and polymers such as ABS (acrylonitrile butadiene styrene resin), polycarbonate resin, PBT (polybutylene terephthalate resin), PPS (polyphenylene sulfide resin), etc.

[0076] (Application) The composition can be used for mounting or sealing automotive and electrical / electronic parts, bonding semiconductors or general-purpose plastics, etc. Specifically, the composition can be used as a sealing material or potting material for automotive parts. EXAMPLES

[0077] The present invention will be described in more detail below with reference to examples and comparative examples. In these examples, the parts indicate parts by mass, and the viscosity indicates the viscosity at 23° C. The present invention is not limited to these examples.

[0078] (Ingredients used) The components used in the examples and comparative examples are as follows.

[0079] (A) Alkenyl-containing polyorganosiloxane A mixture of A-1 and A-2 (amount of alkenyl groups bonded to silicon atoms: 0.25 mmol / g). A-1:A-2=75:25 (weight ratio). A-1: Both ends are M v A linear polymethylvinylsiloxane having a viscosity of 100 Pa s at 23°C, with intermediate units consisting only of D units. A-2: M unit, D vi It consists of only units and Q units, and the molar unit ratio is M6D vi Branched polymethylvinylsiloxane represented by Q8 (weight average molecular weight 5,000, average of about 5 vinyl groups per molecule) The weight average molecular weight is a value calculated in terms of styrene measured by GPC (gel permeation chromatography). The device used for measuring the weight average molecular weight is a Nihon Waters RI (differential refractometer) Model 2414 (mobile phase toluene).

[0080] (B) Polyorganohydrogensiloxane B: Both ends are blocked with M units, and the middle unit is D and D HA linear polymethylhydrogensiloxane consisting only of units, with a viscosity of 20 mPa·s at 23°C (the amount of hydrogen atoms directly bonded to silicon atoms is 8.8 mmol / g).

[0081] (C) Platinum catalyst C: Platinum-octanol complex (a complex containing 4.0% platinum by weight obtained by heating chloroplatinic acid with octanol)

[0082] (D) Succinic anhydride group-containing cyclic organosiloxane The succinic anhydride group-containing cyclic siloxane shown below was used.

[0083] [ka]

[0084] [ka]

[0085] [ka]

[0086] [Example 1 of Synthesis] Synthesis of (D-1) In a 500 ml flask equipped with a nitrogen gas inlet tube and a condenser, 42 g of toluene, 190.7 g (0.749 mol) of 2,2,4,6,8-pentamethyl-cyclotetrasiloxane, and 0.1 g of alumina-supported platinum catalyst were charged, and the mixture was heated to 120°C while stirring under a nitrogen gas flow. 17.5 g (0.125 mol) of allylsuccinic anhydride (Tokyo Chemical Industry Co., Ltd.) was added dropwise over about 1 hour. Then, the mixture was reacted at 120°C for 12 hours to obtain a reaction solution. The reaction solution obtained was cooled to room temperature (23°C), and activated carbon was added to adsorb the alumina-supported platinum catalyst, after which the activated carbon was removed by filtration. Next, the reaction solution obtained was heat stripped under reduced pressure to remove toluene and unreacted components, and 47.7 g of the desired cyclic siloxane compound was obtained. The yield was 97%.1 Analysis by H-NMR revealed the following, confirming that it was the target compound.

[0087] [ka]

[0088] [Synthesis Example 2] Synthesis of (D-2) In a 1L flask equipped with a nitrogen gas inlet tube and a condenser, 83.8g of toluene, 381g (1.584mol) of 2,4,6,8-tetramethyl-cyclotetrasiloxane, and 1.6g of alumina-supported platinum catalyst were charged, and the temperature was raised to 120°C while stirring under a nitrogen gas flow. 37g (0.264mol) of allylsuccinic anhydride (Tokyo Chemical Industry Co., Ltd.) was added dropwise over about 1 hour. Then, the mixture was reacted at 120°C for 34 hours to obtain a reaction solution. The reaction solution obtained was cooled to room temperature (23°C), and activated carbon was added to adsorb the alumina-supported platinum catalyst, after which the activated carbon was removed by filtration. Next, the reaction solution obtained was heat stripped under reduced pressure to remove toluene and unreacted components, and 91.2g of the target cyclic siloxane compound was obtained. The yield was 91%. 1 Analysis by H-NMR revealed the following, confirming that it was the target compound.

[0089] [ka]

[0090] [Example 3 of Synthesis] Synthesis of (D-3) In a 300 ml flask equipped with a nitrogen gas inlet tube and a condenser, 50 g of toluene, 45 g (0.187 mol) of 2,4,6,8-tetramethyl-cyclotetrasiloxane, and 1.2 g of alumina-supported platinum catalyst were charged, and the mixture was heated to 120°C while stirring under a nitrogen gas flow. 52.4 g (0.374 mol) of allylsuccinic anhydride (Tokyo Chemical Industry Co., Ltd.) was added dropwise over about 1 hour. Then, the mixture was reacted at 120°C for 6 hours to obtain a reaction solution. The reaction solution obtained was cooled to room temperature (23°C), and activated carbon was added to adsorb the alumina-supported platinum catalyst, after which the activated carbon was removed by filtration. Next, the reaction solution obtained was heat stripped under reduced pressure to remove toluene and unreacted components, and 92.2 g of the target cyclic siloxane compound was obtained. The yield was 95%. 1 Analysis by H-NMR revealed the following, confirming that it was the target compound.

[0091] [ka]

[0092] (D') Compound for comparison The following compounds were used. Here, (D'-6) was [3-(trimethoxysilyl)propyl]succinic anhydride manufactured by Tokyo Chemical Industry Co., Ltd.

[0093] [ka]

[0094] [ka]

[0095] [ka]

[0096] [ka]

[0097] [ka]

[0098] [ka]

[0099] [ka]

[0100] [Comparative Synthesis Example 1] Synthesis of (D'-1) In a 5L flask equipped with a nitrogen gas inlet tube and a condenser, 440g of toluene, 1991.9g (7.42mol) of 2,2,4,6,6,8-hexamethyl-cyclotetrasiloxane, and 17.7g of alumina-supported platinum catalyst were charged, and the mixture was heated to 120°C while stirring under a nitrogen stream. 1100g (7.42mol) of vinyltrimethoxysilane was added dropwise over about 1 hour. The mixture was allowed to react at 120°C for about 3 hours. The resulting reaction solution was cooled to room temperature (23°C), and the alumina-supported platinum catalyst was removed by filtration. The resulting reaction solution was heat stripped under reduced pressure to remove toluene and unreacted components. The reaction product was then distilled under reduced pressure to obtain 400g of the desired cyclic siloxane compound. The yield was 13%. 1 Analysis by H-NMR revealed the following, confirming that it was the target compound.

[0101] [ka]

[0102] [Comparative Synthesis Example 2] Synthesis of (D'-2) In a 300 ml flask equipped with a nitrogen gas inlet tube and a condenser, 66 g (0.471 mol) of allylsuccinic anhydride (Tokyo Chemical Industry Co., Ltd.), 50 g of toluene, and 2.1 g of alumina-supported platinum catalyst were charged, and the temperature was raised to 120°C while stirring under a nitrogen stream. 55 g (0.205 mol) of 2,2,4,6,6,8-hexamethyl-cyclotetrasiloxane was added dropwise over about 2 hours. The reaction was allowed to proceed at 120°C for about 13 hours. The resulting reaction solution was cooled to room temperature (23°C), and activated carbon was added to adsorb the alumina-supported platinum catalyst, after which the activated carbon was removed by filtration. The resulting reaction solution was heat stripped under reduced pressure to remove toluene and unreacted components, and 110.5 g of the target cyclic siloxane compound was obtained. The yield was 98%. 1 Analysis by H-NMR revealed the following, confirming that it was the target compound.

[0103] [ka]

[0104] [Comparative Synthesis Example 3] Synthesis of (D'-3) In a 500 ml flask equipped with a nitrogen gas inlet tube and a condenser, 42 g of toluene, 190.7 g (0.749 mol) of 2,2,4,6,8-pentamethyl-cyclotetrasiloxane, and 0.1 g of alumina-supported platinum catalyst were charged, and the temperature was raised to 120°C while stirring under a nitrogen gas flow. 17.5 g (0.125 mol) of allylsuccinic anhydride (Tokyo Chemical Industry Co., Ltd.) was added dropwise over about 1 hour. Then, the mixture was reacted at 120°C for 12 hours to obtain a reaction solution. The reaction solution obtained was cooled to room temperature (23°C), and activated carbon was added to adsorb the alumina-supported platinum catalyst, after which the activated carbon was removed by filtration. Next, the reaction solution obtained was heat stripped under reduced pressure to remove toluene and unreacted components, and 50 g of reaction product was obtained.

[0105] Next, 50g of toluene, 68.3g (0.461mol) of vinyltrimethoxysilane, and 1.5g of alumina-supported platinum catalyst were charged into a 500ml flask equipped with a nitrogen gas inlet tube and a condenser, and the temperature was raised to 120°C while stirring under a nitrogen stream. 49.5g (0.125mol) of the above reactant was dropped over about 2 hours. Then, the reaction was carried out at 120°C for 10 hours to obtain a reaction solution. The reaction solution obtained was cooled to room temperature (23°C), and activated carbon was added to adsorb the alumina-supported platinum catalyst, and the activated carbon was removed by filtration. The reaction solution obtained was heat stripped under reduced pressure to remove toluene and unreacted components, and 84.8g of the target cyclic siloxane compound was obtained. The yield was 98%. 1 Analysis by H-NMR revealed the following, confirming that it was the target compound.

[0106] [ka]

[0107] [Comparative Synthesis Example 4] Synthesis of (D'-4) In a 300 ml flask equipped with a nitrogen gas inlet tube and a condenser, 39 g (0.162 mol) of 2,4,6,8-tetramethyl-cyclotetrasiloxane, 40 g of toluene, and 1 g of alumina-supported platinum catalyst were charged, and the temperature was raised to 120°C while stirring under a nitrogen stream. 45.45 g (0.324 mol) of allylsuccinic anhydride (Tokyo Chemical Industry Co., Ltd.) was added dropwise over about 1 hour. The mixture was allowed to react at 120°C for about 5 hours. Furthermore, 96.2 g (0.649 mol) of vinyltrimethoxysilane was added dropwise over about 3 hours. The mixture was allowed to react at 120°C for 16 hours to obtain a reaction solution. The reaction solution obtained was cooled to room temperature (23°C), activated carbon was added to adsorb the alumina-supported platinum catalyst, and the activated carbon was removed by filtration. The resulting reaction solution was heat stripped under reduced pressure to remove toluene and unreacted components, yielding 127.6 g of the target cyclic siloxane compound in a yield of 96%. 1 Analysis by H-NMR revealed the following, confirming that it was the target compound.

[0108] [ka]

[0109] [Comparative Synthesis Example 5] Synthesis of (D'-5) In a 200 ml flask equipped with a nitrogen gas inlet tube and a condenser, 38.8 g (0.161 mol) of 2,4,6,8-tetramethyl-cyclotetrasiloxane and 0.8 g of alumina-supported platinum catalyst were charged, and the temperature was raised to 120°C while stirring under a nitrogen stream. 23.9 g (0.161 mol) of vinyltrimethoxysilane was added dropwise over about 1 hour. Furthermore, 45.2 g (0.322 mol) of allylsuccinic anhydride (Tokyo Chemical Industry Co., Ltd.) was added dropwise over about 2 hours. The reaction was carried out at 120°C for 24 hours to obtain a reaction solution. The reaction solution obtained was cooled to room temperature (23°C), activated carbon was added to adsorb the alumina-supported platinum catalyst, and the activated carbon was removed by filtration to obtain 64.3 g of the target cyclic siloxane compound. The yield was 60%. 1 Analysis by H-NMR revealed the following, confirming that it was the target compound.

[0110] [ka]

[0111] [Comparative Synthesis Example 6] Synthesis of (D'-7) In a 200 ml flask equipped with a nitrogen gas inlet tube and a condenser, 41 g (0.17 mol) of 2,4,6,8-tetramethyl-cyclotetrasiloxane was added with 1,3-divinyl-1,1,3,3-tetramethyldisiloxane complex of platinum so that the platinum metal concentration was 2.5 ppm, and reacted with 10 g (0.032 mol) of bisphenol A bisallyl ether. Unreacted 2,4,6,8-tetramethylcyclotetrasiloxane was removed by stripping to obtain 21 g of the desired cyclic siloxane compound. 1 Analysis by H-NMR revealed the following, confirming that it was the target compound.

[0112] [ka]

[0113] (E1) Inorganic filler E1-1: Quartz powder (Crystallite VX-S, manufactured by Tatsumori Co., Ltd.)

[0114] (E2) Reaction inhibitor E2-1: Triallyl isocyanurate E2-2: 3,5-dimethyl-1-hexyn-3-ol

[0115] Example 1 (1) Preparation of base polymer (1) In the composition shown in Table 1, (A) alkenyl group-containing polyorganosiloxane and (E1) inorganic filler (E1-1) were placed in a universal mixer and stirred for 3 hours under reduced pressure at 150° C. After cooling to room temperature (23° C.), (E2) reaction inhibitors (E2-1 and E2-2) and (C) platinum catalyst were added and stirred for 15 minutes to prepare base polymer (1). (2) Preparation of addition-curable silicone composition In the compositions shown in Tables 2 to 4, (B) polyorganohydrogensiloxane and / or (D) succinic anhydride group-containing cyclic organosiloxane or (D') comparative compound was added to base polymer (1) and stirred to prepare addition-curable silicone compositions.

[0116] [Table 1] (C) is an amount that gives a platinum content of 12 ppm in the base polymer.

[0117] (Evaluation method) <Hardness> The addition-curable silicone composition was poured into a 6 mm thick Teflon (registered trademark) coated metal mold, covered with a similarly Teflon (registered trademark) coated metal lid, and cured in a hot air circulating dryer at 150°C for 1 hour. After cooling to room temperature (23°C), measurements were performed in accordance with JIS K6249.

[0118] <Whether or not discoloration (yellow) occurs> The cured product used in the above "hardness" measurement was further heated in a hot air circulation dryer at 150°C for 72 hours, and the appearance (degree of yellowing) was observed and the presence and degree of discoloration (yellowing) was evaluated according to the following criteria. ◎: No change from the initial stage ○: Slight yellowing was observed compared to the initial state. ×: Yellowing was clearly observed

[0119] <Surface condition> The addition-curing silicone composition was poured into a 2 mm thick Teflon (registered trademark) coated metal mold and cured in a hot air circulating dryer at 150°C for 1 hour. After cooling to room temperature (23°C) and 24 hours later, the surface condition was observed. Good: The surface was smooth and no liquid was seeping out when palpated. Bleeding: Liquid seeps out onto the cured surface.

[0120] <Shear adhesive strength> The details of the test were in accordance with JIS K 6249. The silicone composition was applied to one end of the test piece and spread evenly, and then the other end of the test piece was attached to obtain a test piece so that the adhesive thickness was 1 mm, the width direction was 25 mm, and the length direction (overlap) was 10 mm. The test piece was placed in an oven adjusted to the temperature of the curing conditions while fixed with a jig, and cured in a hot air circulation dryer under the conditions of "150°C for 1 hour" or "100°C for 2 hours", and cooled to room temperature (23°C) to obtain a test piece. The test piece was measured with a tensile tester at a tensile speed of 10 mm / min, and the "tensile shear adhesive strength" (MPa) was obtained.

[0121] <Cohesive failure rate> The cohesive failure rate is the percentage of silicone layers that break without peeling at the interface of the opposing adherends in a shear bond strength test. A cohesive failure rate of 100% indicates that the adhesive strength (adhesion) is adequately maintained. After measuring the shear bond strength as described in "shear bond strength" above, the area of ​​the silicone layer bonded to each adherend was divided by the coating area to obtain the cohesive failure rate (area %).

[0122] <Adhesion test> The silicone composition was applied to a specified member to a thickness of 2 mm, and cured at 100°C for 2 hours. A cut was made with a knife at the interface between the member and the cured silicone composition, and the member was pulled in a 180° direction. The adhesion state was checked, and the adhesion was evaluated according to the following criteria. ◎: Cohesive failure △: Cohesive failure and interfacial peeling were mixed ×: Interfacial peeling

[0123] The results are summarized in Tables 2, 3, and 4. B +H D ) / Vi A " varies depending on the presence or absence of the (B), (D) and (D') components. That is, in Example 1, "(H B +H D ) / Vi A " is "H D / Vi A " In Example 2 and the like, "(H B +H D ) / Vi A " is "(H B +H D ) / Vi A " In Comparative Example 1, "(H B +H D ) / Vi A " is "H B / Vi A " In Comparative Example 2, etc., "(H B +H D ) / Vi A " is "(H B +H D’ ) / Vi A". In addition, the value of "D unit (a)" in the (D) component and the (D') component means the number of D units per structural formula. The same applies to other groups, etc.

[0124] [Table 2]

[0125] [Table 3]

[0126] [Table 4]

[0127] The abbreviations in the table are as follows: Aluminum: A1050P (JIS H 4000): Pure aluminum with an aluminum purity of 99.5% or more Aluminum die casting: ADC-12 (JIS H 5302:2006): Al-Si-Cu alloy PBT: Polybutylene terephthalate resin (Polyplastics, Duranex 2002) PPS: Polyphenylene sulfide resin (Tosoh, Sasteel GS-40%)

[0128] As is clear from Tables 2 to 4, the silicone compositions of the examples showed excellent adhesion to various substrates under the curing conditions of 150°C for 1 hour or 100°C for 2 hours. In addition, the silicone compositions of the examples gave cured products with good appearances under the curing conditions of 150°C for 1 hour, and the cured products were further heated at 150°C for 72 hours, and yellowing was suppressed. Furthermore, the adhesive assistant of the examples was able to improve the adhesion to various substrates by curing the silicone composition under the curing conditions of 150°C for 1 hour or 100°C for 2 hours. In particular, the silicone composition containing the adhesive assistant of the examples was particularly excellent in the cohesive failure rate to PPS, aluminum, and aluminum die cast under the curing conditions of 100°C for 2 hours, and the shear adhesive strength to PBT under the curing conditions of 100°C for 2 hours. Therefore, it can be seen that the succinic anhydride group-containing cyclic organosiloxane represented by the general formula (1) is excellent as an adhesive assistant.

[0129] Comparing Example 3 with Example 6, when c was 1, the adhesion to various substrates was superior to that when c was 2 (particularly, the shear adhesive strength and cohesive failure rate to PPS cured at 100°C for 2 hours, and the shear adhesive strength to PBT cured at 150°C for 1 hour).

[0130] On the other hand, the compositions of Comparative Examples 1 to 8 did not contain (D), and therefore the compositions of Comparative Examples 1 to 8 had poor adhesion to various substrates or did not give cured products with good appearances. In particular, the compositions of Comparative Examples 1 to 8 had poor cohesive failure rates for PPS, aluminum, and aluminum die-cast when cured at 100°C for 2 hours, and poor shear adhesive strength to aluminum when cured at 100°C for 2 hours. The composition of Comparative Example 1 contained only the crosslinking agent (Component (B)) as a component having a hydrogen atom directly bonded to a silicon atom, and therefore the composition of Comparative Example 1 had poor adhesion. The composition of Comparative Example 2 contained a cyclic organosiloxane containing a hydrogen atom directly bonded to a silicon atom and not containing a succinic anhydride group as an adhesion promoter, and therefore the composition of Comparative Example 2 had poor adhesion. The composition of Comparative Example 3 contains a succinic anhydride group-containing cyclic organosiloxane as an adhesive aid, which does not have a hydrosilyl group and has two succinic anhydride groups. Therefore, the cured product of the composition containing the adhesive aid of Comparative Example 3 was confirmed to bleed under the curing condition of 150°C for 1 hour. In addition, the cured product of the composition containing the adhesive aid of Comparative Example 3 had poor adhesion. The composition of Comparative Example 4 contains a succinic anhydride group-containing cyclic organosiloxane that does not have a hydrosilyl group as an adhesive promoter. Therefore, bleeding was observed in the cured product of the composition containing the adhesive promoter of Comparative Example 4 under the curing condition of 150°C for 1 hour. In addition, the cured product of the composition containing the adhesive promoter of Comparative Example 4 was particularly poor in shear adhesive strength under the curing condition of 100°C for 2 hours. The composition of Comparative Example 5 contains a succinic anhydride group-containing cyclic organosiloxane having two succinic anhydride groups as an adhesive promoter. Therefore, bleeding was observed in the cured product of the composition containing the adhesive promoter of Comparative Example 5 under the curing condition of 150°C for 1 hour. The cured product of the composition containing the adhesive promoter of Comparative Example 5 was particularly poor in shear adhesive strength under the curing condition of 100°C for 2 hours. The composition of Comparative Example 7 contains a succinic anhydride group-containing silane compound as an adhesive aid that does not have a hydrosilyl group and does not have a cyclic siloxane structure. Therefore, bleeding was confirmed in the cured product of the composition containing the adhesive aid of Comparative Example 7. In addition, the cured product of the composition containing the adhesive aid of Comparative Example 7 had poor adhesion to various substrates. The composition of Comparative Example 8 contains, as an adhesive promoter, an organosilicon compound that contains a hydrosilyl group and has bisphenol A in its skeleton. Therefore, the cured product of the composition containing the adhesive promoter of Comparative Example 8 had poor shear adhesive strength to various substrates (especially aluminum). Furthermore, the compositions of Comparative Examples 3 and 5 to 8 were cured at 150°C for 1 hour, and after further heating at 150°C for 72 hours, the cured products showed significant yellowing and had poor appearances after heating.

Claims

1. A succinic anhydride group-containing cyclic organosiloxane represented by the following general formula (1): [C22] (In the formula, R 1 are independently a monovalent hydrocarbon group containing no fluorine atoms, R 2 are independently a divalent hydrocarbon group having 2 to 10 carbon atoms, a is 0 or an integer of 1 or more; b is an integer of 1 or more; c is an integer of 1 or more, provided that a+b+c is an integer of 3 or more.

2. 2. The succinic anhydride group-containing cyclic organosiloxane according to claim 1, wherein a+b+c is an integer of 3 to 8.

3. 3. An adhesion promoter comprising the succinic anhydride group-containing cyclic organosiloxane according to claim 1 or 2.

4. (A) a polyorganosiloxane having two or more alkenyl groups bonded to silicon atoms in the molecule; (C) a platinum-based catalyst; and (D) the succinic anhydride group-containing cyclic organosiloxane according to claim 1 or 2; and optionally, (B) a polyorganohydrogensiloxane having three or more hydrogen atoms directly bonded to silicon atoms in the molecule.

5. An adhesive comprising the addition-curable silicone composition according to claim 4.

Citation Information

Patent Citations

  • Organosilicon compound

    JP2002114793A

  • Succinic anhydride group-containing cyclic organosiloxane, method for producing the same, organosiloxane composition, and thermosetting resin composition

    JP2013032498A