Porous silica alumina particle
By optimizing the synthesis of porous silica alumina particles with controlled surface area and pore volume, the developed method addresses the limitations of conventional methods, resulting in materials with improved catalytic and insulating properties.
Patent Information
- Application Number
- JP2024152838
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2024-09-05
- Publication Date
- 2024-11-28
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Conventional methods for producing porous silica alumina particles result in materials with relatively small specific surface areas and pore volumes, limiting their effectiveness in applications such as catalysts and insulation.
The development of porous silica alumina particles with a specific surface area of 400-600 m²/g and a pore volume of 1.25-2.00 ml/g, achieved through controlled synthesis processes involving the mixing and aging of pseudo-boehmite alumina and silica hydrogel solutions, followed by careful washing and drying to minimize impurities.
The resulting particles exhibit enhanced specific surface area and pore volume, providing improved catalytic performance and heat insulation properties, suitable for applications requiring high reactivity and stability.
Smart Images

Figure 2024166231000001
Abstract
Description
[Technical field]
[0001] The present invention relates to porous silica-alumina particles having a high specific surface area and a high pore volume. [Background technology]
[0002] Methods for preparing silica-alumina compositions are well known in the art, and representative methods include the neutralization reaction method and the pH swing method.
[0003] As the neutralization reaction (coprecipitation method, cogelation method) method, as described in Patent Documents 1 to 4, there is a preparation method in which a silica hydrogel and a solution of a metal salt are mixed to produce amorphous silica-alumina that contains the metal salt uniformly inside.
[0004] In addition, the pH swing method (immersion method) includes a preparation method that enables the production of amorphous silica-alumina in a single vessel by changing the pH of the reaction mixture, thereby precipitating silica and alumina, as described in Patent Documents 5 and 6. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Special Publication No. 27-3989 [Patent Document 2] Special Publication No. 31-1862 [Patent Document 3] Special Publication No. 30-5963 [Patent Document 4] Special Publication No. 32-413 [Patent Document 5] Special Publication No. 2010-537808 [Patent Document 6] Special Publication No. 2016-502971 Summary of the Invention [Problem to be solved by the invention]
[0006] However, in the prior art, the porous silica-alumina obtained by the preparation methods described in Patent Documents 1 to 6 has a relatively small specific surface area, i.e., 400 m 2 The problem was that the α-to-β-sigma ratio tended to be much smaller than α-to-β / g.
[0007] Furthermore, there is a problem that the pore volume tends to be smaller than 1.0 ml / g.
[0008] An object of the present invention is to provide porous silica-alumina particles having a high specific surface area and a high pore volume. [Means for solving the problem]
[0009] Under such technical background, the inventors conducted intensive research to solve the above problems, and as a result, discovered that it is possible to obtain porous silica-alumina particles having a high specific surface area and a high pore volume, and thus developed the present invention. The present invention, which has been developed to solve the above problems and achieve the above objects, is as follows. That is, the present invention is an amorphous porous silica-alumina particle, The specific surface area SA measured by the BET method is 400 to 600 m 2 / g range, The pore volume PV measured by the BJH method is in the range of 1.25 to 2.00 ml / g. The average pore diameter PD measured by the BJH method is in the range of 8 to 20 nm. The present invention provides porous silica-alumina particles, characterized in that the mass ratio of silica to alumina is in the range of 2 / 98 to 70 / 30.
[0010] In addition, the porous silica-alumina particles according to the present invention further contain an alkali metal ion (M + ) to M 2 A more preferable solution would be to have an O content of 0.1% by mass or less and a residual amount of inorganic acid ions of 1.0% by mass or less. Effect of the Invention
[0011] The present invention can provide porous silica-alumina particles having a high specific surface area and a large pore volume.
[0012] The porous silica-alumina particles according to the present invention have excellent heat insulating properties and can be used in a wide range of applications. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] Preferred embodiments of the present invention will now be described in detail. [Porous silica alumina particles] The porous silica-alumina particles of the present invention (hereinafter, also simply referred to as "silica-alumina particles") are made of silica (SiO 2 ) and alumina (Al 2 O 3 ) and are composed of oxides with a high specific surface area and high pore volume.
[0014] The porous silica-alumina particles of the present invention are amorphous. Therefore, zeolite, which is crystalline silica-alumina, is not included in the silica-alumina of the present invention. Whether the silica-alumina of the present invention is amorphous can be judged from the X-ray diffraction pattern. Specifically, if the X-ray diffraction pattern obtained by X-ray diffraction measurement of the silica-alumina of the present invention does not show a diffraction peak with a full width at half maximum of less than 1.0° in the range of 5°≦2θ≦50°, the silica-alumina of the present invention can be judged to be amorphous.
[0015] The silica-alumina particles obtained in the present invention have a silica to alumina ratio S / A of SiO 2 and Al 2 O 3The mass ratio S / A calculated by S / A is in the range of 2 / 98 to 70 / 30, preferably in the range of 5 / 95 to 65 / 35. If the alumina ratio is lower than S / A:70 / 30, the solid acid amount tends to decrease, and when the particles are used as a cracking catalyst, etc., the required cracking rate cannot be obtained. On the other hand, if the silica ratio is lower than S / A:2 / 98, the specific surface area SA tends to decrease.
[0016] The specific surface area SA of the resulting silica-alumina particles measured by the BET method is 400 to 600 m 2 / g, preferably 420 to 550 m 2 The reason for setting the lower limit is that when used as a cracking catalyst, it is advantageous for the specific surface area SA to be moderately high in terms of contact and reactivity with hydrocarbons. 2 If it exceeds 1 / g, the pore diameter PD becomes too small and is smaller than the molecular size of the hydrocarbon reactants, which cannot diffuse within the pores and may not result in an effective reaction.
[0017] Furthermore, the pore volume PV according to the BJH method is in the range of 1.25 to 2.00 ml / g, preferably in the range of 1.30 to 1.90 ml / g. If the pore volume PV is less than 1.25 ml / g, there will be fewer effective reaction sites with hydrocarbon molecules. On the other hand, if the pore volume PV exceeds 2.00 ml / g, the crushing strength or abrasion strength of the molded product will be weakened when used as a cracking catalyst, and powdering may occur when packed in a reactor, making it impossible to operate the reactor.
[0018] The average pore diameter PD measured by the BJH method is in the range of 8 to 20 nm (80 to 100 Å), and preferably in the range of 10 to 18 nm (100 to 180 Å). The reason for setting a lower limit is that if the average pore diameter PD is too small, there will be many pores smaller than the molecular size of the reactant hydrocarbon, and the reactants will not be able to diffuse in the pores, which may prevent effective reaction from occurring. On the other hand, the reason for setting an upper limit is that the specific surface area will decrease, resulting in a decrease in the active sites for the decomposition reaction.
[0019] The silica alumina particles of the present application are also characterized by having a small remaining amount of cationic and anionic impurity ion components. Examples of the residual cations include alkali metal ions such as residual sodium ions and potassium ions. The amount of these alkali metal ions (M + ) is 0.1% by mass or less, preferably 0.05% by mass or less in terms of M 2 O conversion. Furthermore, the remaining amount of inorganic acid ions such as sulfate ions and nitrate ions is 1.0% by mass or less, preferably 0.5% by mass or less. By reducing the impurity ion components, poisoning of the solid acid sites and the active metal is suppressed.
[0020] [Method for producing porous silica alumina particles] <Step of obtaining a pseudo-boehmite alumina hydrate aqueous solution> <<a-1. Preparation step>> Methods for preparing pseudo-boehmite alumina particles are widely known. Among them, a method of neutralizing an aluminum salt and / or an aluminate solution to form a precipitate of pseudo-boehmite alumina particles is preferred. As the aluminum salt, any aluminum salt such as aluminum sulfate, aluminum chloride, and aluminum nitrate can be used. Also, as the aluminate, any one such as sodium aluminate and potassium aluminate can be used. The neutralization reaction can be carried out by any of the following methods: adding an alkaline aqueous solution such as sodium hydroxide, potassium hydroxide, or aqueous ammonia to an aqueous solution of an aluminum salt; adding an aqueous solution of an acid such as sulfuric acid, hydrochloric acid, or nitric acid to an aqueous solution of an aluminate; or mixing an aqueous solution of an aluminum salt and an aqueous solution of an aluminate. However, from the perspective of production cost, a method of mixing an aqueous solution of an aluminum salt and an aqueous solution of an aluminate to obtain an aqueous solution of pseudo-boehmite alumina hydrate is preferred.
[0021] <<a-2. Aging step>> After mixing the two liquids to carry out the neutralization reaction, in order to promote the reaction to pseudo-boehmite alumina hydrate (hereinafter, also referred to as "aging"), by adjusting the pH of the solution in the range of 7.0 to 10.0 and the temperature in the range of 30 to 70 °C, the reaction can be promoted and pseudo-boehmite alumina hydrate can be obtained. When the pH exceeds 10.0, a baylite phase with a small specific surface area is generated, so the activity of the finally produced catalyst may decrease. Also, when the pH is lower than 7.0, the pore volume of the finally obtained pseudo-boehmite alumina particles tends to decrease, and it may become difficult to produce pseudo-boehmite alumina particles suitable for the catalyst.
[0022] The aging temperature is desirably in the range of 30 to 70 °C. When the temperature is 30 °C or lower, the particles tend to strongly aggregate, and the pore volume of the powder obtained through the aging and drying process may become small. Also, when the temperature is 70 °C or higher, baylite is likely to precipitate, which is not preferable. The aging time is desirably in the range of 5 minutes to 120 minutes, preferably 10 to 100 minutes, and more preferably 10 to 90 minutes. If it is outside this range, the pore volume of the finally obtained pseudo-boehmite alumina particles may be 0.8 cc / g or less, and it may not be possible to use them as pseudo-boehmite alumina particles for the catalyst. Although there is no particular limitation on the aging time, from the perspective of production efficiency, within 120 minutes is preferable. If the aging time is too long, the specific surface area of the finally obtained pseudo-boehmite alumina particles tends to become small.
[0023] <b. Step of obtaining silica hydrogel aqueous solution> The method for preparing silica hydrogel is widely known. Among them, during the preparation, the pH is adjusted by adjusting the supply rates of the silicate aqueous solution and the acid, and the SiO 2 concentration can be controlled by using a silicic acid aqueous solution and an acid with a pre-calculated specified concentration. The reaction can obtain a silica hydrogel solution by supplying a silicate aqueous solution and an acid while stirring in a reactor maintained at 10 to 100 °C, preferably 20 to 95 °C.
[0024] Those that can be used as the silicate may be any of sodium silicate No. 1, No. 2, No. 3, potassium silicate, other soluble silicates, and diatomaceous earth.
[0025] As the acid, inorganic acids such as sulfuric acid, nitric acid, hydrochloric acid, and phosphoric acid, or organic acids such as formic acid may be used, but inorganic acids are preferred.
[0026] The concentration of the silicate to be supplied is 30% by mass or less, preferably 10% by mass or less in terms of SiO 2 conversion. The lower limit of the silicate concentration is not particularly provided. However, for example, if it is supplied at 5% by mass or more, it is preferable because a large-volume mixing container or a large amount of water is not required to adjust the required amount of SiO 2 On the other hand, the reason for setting the upper limit is that due to the gelation caused by the neutralization with the inorganic acid, the stirrer becomes overloaded due to the influence of the strong gel-like substance and stops or sufficient stirring cannot be performed.
[0027] According to the above adjustment method, an aqueous solution of silica hydrogel having a specific surface area in the range of 190 to 600 m 2 / g can be easily obtained.
[0028] <c. Step of obtaining an aqueous solution of silica-alumina mixture> (Mix the pseudo-boehmite alumina hydrate aqueous solution and the silica hydrogel aqueous solution to obtain an aqueous solution of a silica-alumina particle mixture.) An aqueous solution of pseudo-boehmite alumina hydrate adjusted to a solid content concentration of 1 to 5% by mass and an aqueous solution of silica hydrogel adjusted to a solid content concentration of 5 to 10% by mass are mixed, and further adjusted to a range of pH 7.0 to 10.0, more preferably a range of pH 8.0 to 9.0, and aged at a temperature in the range of 40 to 60 °C for 10 minutes to 2 hours to obtain an aqueous solution of a silica-alumina mixture. When mixing these two liquids, the silica hydrogel aqueous solution may be added to the pseudo-boehmite alumina hydrate aqueous solution, or the pseudo-boehmite alumina hydrate aqueous solution may be added to the silica hydrogel aqueous solution.
[0029] <d. First washing step> After filtering the aqueous solution of the silica-alumina mixture obtained in the step c, a silica-alumina mixture cake 1 is obtained. The mixture cake 1 is transferred to a washing container and washed with water at 50 to 70 °C to remove unreacted raw materials, impurity ions, etc., and a silica-alumina mixture cake 1 is obtained.
[0030] The temperature of the washing water is preferably in the range of 50 to 70 °C, which is higher than room temperature, in order to improve the removal efficiency of unreacted raw materials, impurity ions, etc. The amount of water at 50 to 70 °C used here is preferably about 35 times the mass of the silica-alumina particles theoretically obtained for washing.
[0031] <e. Step of obtaining a silica-alumina gel slurry> After dispersing the silica-alumina mixture cake 1 obtained in the step d in water, the pH is adjusted to a range of 8.0 to 12.0, more preferably pH 8.5 to 11.5, at a temperature of 30 to 50 °C, and then heated to 80 °C or higher and stirred for 1 to 20 hours, more preferably 1 to 15 hours, to promote the reaction from the silica-alumina mixture to the silica-alumina gel and obtain a silica-alumina gel slurry. Here, in the heating at 80 °C or higher, since it is for the purpose of promoting and completing the aging of the silica-alumina gel, it may be carried out at normal pressure or under pressurized conditions such as an autoclave. By carrying out under pressurized conditions, there is an advantage that the treatment time can be shortened.
[0032] <f. First drying step> The silica-alumina gel slurry obtained in the step e is dried to obtain silica-alumina particles 1.
[0033] To obtain silica-alumina particles 1 by drying, spray drying or other commonly used drying devices can be used. The drying temperature is not particularly limited, but if the temperature is too high, it is not preferable because of the phase transition from pseudo-boehmite alumina to gamma-alumina. For this reason, the inlet temperature is preferably 500 °C or lower and the outlet temperature is preferably 200 °C or lower, that is, it is preferably dried in the range of an inlet temperature of 300 to 500 °C and an outlet temperature of 130 to 200 °C.
[0034] <g. Second washing step> The silica-alumina particles 1 obtained in the step f are suspended again and stirred, then filtered off and washed to obtain silica-alumina particle cake 2.
[0035] In order to reduce the residual alkali metal ion concentration of the silica-alumina particles 1 obtained in the step f, it is preferable to use a suspension having a temperature in the range of 40 to 70°C. Further, it is preferable to perform filtration on the suspension with an aqueous solution containing a water-soluble acidic substance. Examples of the water-soluble acidic substance used here include ammonium sulfate, ammonium nitrate, ammonium chloride, and the like.
[0036] Furthermore, after filtration, in order to remove residual salts and the like, washing and filtration are performed with warm water or the like containing a water-soluble basic substance to obtain silica-alumina particle cake 2. The temperature of the washing water is preferably in the range of 50 to 70°C, which is higher than room temperature, in order to improve the removal efficiency of unreacted raw materials, impurity ions, and the like. Examples of the water-soluble basic substance used here include aqueous ammonia, hydroxide salts, carbonates, and hydrogen carbonates (the salts referred to here mean alkali metal salts and alkaline earth metal salts).
[0037] <h. Second drying step> The drying of the silica-alumina particle cake 2 after filtration obtained in the step g is performed by the drying method described in the step f to obtain the target silica-alumina particles 2.
[0038] Also, depending on the remaining amount of impurities such as impurity ions, after the step g, the steps f and / or g may be performed again as necessary.
Examples
[0039] Hereinafter, the present invention will be specifically described by way of examples, but the present invention is not limited to these examples in any way.
[0040] <Measurement method or evaluation method> The measurement and evaluation methods used in the examples are as follows.
[0041] (Each element, compound and metal component (Si, Al, Na, SO 4 2- ) content measurement method) 3 g of the measurement sample was placed in a 30 ml zirconia bowl with a lid, heated (200°C, 20 min), and then calcined (700°C, 5 min). 2 O 2 2g of HO and 1g of NaOH were added and melted for 15 minutes. 2 SO 4 After dissolving in 25 ml of ethanol and 200 ml of water, the mixture was diluted to 500 ml with pure water to prepare a sample. The content of each component in the obtained sample was measured on an oxide-equivalent mass basis using an inductively coupled plasma (ICP) optical emission spectrometer (Shimadzu Corporation, ICPS-8100, analysis software ICPS-8000).
[0042] (Method of measuring pore volume PV and average pore diameter PD) The pore volume PV and average pore diameter PD were measured using a BELSORP-mini Ver2.5.6 manufactured by Microtrack-Bell Corporation. Specifically, the sample was heat-treated at 500°C for 2 hours while being evacuated to a vacuum, and nitrogen gas was adsorbed onto the sample. 0 The pore volume PV (ml / g) and average pore diameter PD (nm) were calculated from the desorption isotherm (p = 0.99).
[0043] (Method of measuring specific surface area SA) To measure the specific surface area SA, about 30 mL of the measurement sample was placed in a magnetic crucible (B-2 type), heated at 500°C for 2 hours, and then cooled to room temperature in a desiccator to obtain a measurement sample. Next, 1 g of this sample was taken and the specific surface area SA (m 2 / g) was measured by the BET method.
[0044] (Method of measuring average particle size) The particle size distribution of the catalysts in the examples was measured using a laser diffraction / scattering particle size distribution analyzer (LA-300) manufactured by Horiba, Ltd. Specifically, the sample was placed in a solvent (water) so that the light transmittance was in the range of 70 to 95%, and measurements were performed under the following conditions: circulation rate: 2.8 L / min, ultrasonic irradiation: 3 minutes, and repetition number: 30 times. From the obtained particle size distribution, the median diameter (D50) was adopted as the average particle diameter.
[0045] (Method of measuring ignition loss (hereinafter simply referred to as "ignition loss")) The catalyst sample was calcined at 1000°C for 1 hour, and the mass loss was calculated from the amount of mass loss due to calcination.
[0046] (X-ray diffraction measurement conditions) X-ray diffraction of silica alumina particles was measured using MiniFlex manufactured by Rigaku Corp. The measurement conditions were as follows: operation axis 2θ / θ, CuKα was used as the radiation source, voltage 40 kV, current 15 mA, starting angle: 2θ = 5° to ending angle: 2θ = 50°, sampling width 0.020°, and scan speed 10.000° / min. The criterion for determining whether a material is amorphous is that it does not exhibit a diffraction peak with a full width at half maximum of less than 1.0° in the range of 5°≦2θ≦50°.
[0047] [Example 1] (Step a) Step of obtaining an aqueous solution of pseudoboehmite alumina hydrate 60 kg of water was placed in a 200 L steam jacketed stainless steel tank, and 24 g of a 25% by weight aqueous solution of sodium gluconate was added while stirring. 2 O 3 :22.6% by mass, Na 2 0: 885 g of a 17.3 mass% aqueous solution of sodium aluminate was added, followed by 1408 g of a 24 mass% aqueous solution of aluminum sulfate over a period of 2 minutes to prepare a pseudoboehmite alumina seed slurry with a pH of 7.2. 2 O 3 :22.6% by mass, Na 2O: A 17.3% by mass aqueous solution of sodium aluminate was added dropwise at a flow rate of 275 ml / min, and a 23.6% by mass solution of aluminum sulfate was added dropwise at a flow rate of 488 ml / min, respectively, for 20 minutes while maintaining the temperature at 60°C. The pH of the finished slurry was 7.2. After stirring for 5 minutes, the Al 2 O 3 :22.6% by mass, Na 2 O: The pH was adjusted to 8.8 with 642 g of a 17.3 mass % aqueous solution of sodium aluminate, and stirring was continued at 60° C. for 2 hours to prepare an aqueous solution of pseudoboehmite alumina hydrate.
[0048] (Step b) Step of obtaining an aqueous silica hydrogel solution 4.72 kg of 25% by mass sulfuric acid and 2.0 kg of pure water were placed in a 40 L plastic tank and adjusted to 30°C. This sulfuric acid solution was stirred while being cooled to 45°C to obtain 8.5% by mass SiO 2 Concentration, SiO 2 / Na 2 A sodium silicate solution with an O molar ratio of 3.2 was added dropwise at a flow rate of 0.56 kg / min for 45 minutes, and then the flow rate was reduced to 0.1 kg / min and the sodium silicate solution was added dropwise for 30 minutes until the pH reached 4.0. After the addition was completed, stirring was continued for 165 minutes to obtain an aqueous silica hydrogel solution. 400 ml of 15% aqueous ammonia was added to this silica hydrogel, and the pH was adjusted to 7.0 and the mixture was aged for 1 hour.
[0049] (Step c) Step of obtaining an aqueous silica-alumina mixture solution 78,191 g of the pseudoboehmite alumina hydrate aqueous solution and 893 g of the silica hydrogel aqueous solution were mixed by stirring, and then the pH was adjusted to 8.8 with 15 mass % ammonia water and aged at a temperature of 40 to 60°C for 10 minutes to obtain a silica alumina mixture aqueous solution.
[0050] (Step d) First cleaning step The silica-alumina mixture aqueous solution obtained in the step c was filtered, and the filtered silica-alumina mixture cake 1a was washed with 105 L of water at 60°C to remove sulfate ions and sodium ions. (The impurity content at this stage was Na on a dry basis.) 2The O equivalent concentration is 0.1 mass%, and the SO 4 2- The concentration was 2.1% by mass.
[0051] (Step e) Step of obtaining silica alumina gel slurry 7 kg of 60°C hot pure water was added to 23.0 kg of the silica-alumina mixture cake 1a obtained in the step d, and the silica-alumina concentration was adjusted to 10% by mass, and then the mixture was stirred to form a slurry. The temperature of this slurry was 45°C and the pH was 8.7. 1.8 L of 15% by mass ammonia water was added to this slurry to adjust the pH to 10.8, and the slurry was transferred to a 50 L sealed tank equipped with a steam jacket and aged at 95°C for 10 hours.
[0052] (Step f).First drying step The aged slurry obtained in the step e was homogenized in an emulsifier and then dried at an inlet temperature of 300° C. and an outlet temperature of 150° C. in a spray dryer to obtain silica alumina particles 1a having an average particle size of 70 μm.
[0053] (Step g) Second cleaning step 300g of the silica-alumina particles 1a obtained in the step f was suspended in 3000g of ammonium sulfate at 60°C with a concentration of 10% by mass on a dry basis, stirred for 20 minutes, and then subjected to solid-liquid separation using a vacuum filter. The cake remaining after the solid-liquid separation was resuspended by pouring 3000g of warm pure water at 60°C. The pH was then adjusted to 8.8 using 15% by mass of ammonia water, and stirred for 20 minutes. The mixture was then subjected to solid-liquid separation using a vacuum filter to obtain a silica-alumina mixed cake 2a.
[0054] (Step h).Second drying step The silica-alumina particle cake 2a obtained from the filter was taken out into a stainless steel tray and dried overnight at 130° C. to obtain the target silica-alumina particles I. The chemical composition analysis and physical properties are shown in Table 1.
[0055] [Example 2] (Process a~c) In the same manner as in Example 1, a pseudoboehmite alumina hydrate aqueous solution and a silica hydrogel aqueous solution were obtained, and Al 2 O3 Converted to 2400g, SiO 2 After weighing out 600 g of the slurry on a converted basis, the slurry was stirred and mixed, adjusted to pH 8.8 with 15% by mass of ammonia water, and aged for 10 minutes. (Step d) This mixed slurry was filtered and washed in the same manner as in Example 1. (The impurity content at this stage was Na on a dry basis.) 2 O: 0.9% by mass, SO 4 2- : 1.7% by mass.) (Steps e~h) The subsequent treatment was carried out in the same manner as in Example 1 to obtain the desired silica-alumina particles II.
[0056] [Example 3] (Process a~c) In the same manner as in Example 1, a pseudoboehmite alumina hydrate aqueous solution and a silica hydrogel aqueous solution were obtained, and Al 2 O 3 Conversion standard: 1800g, SiO 2 After weighing out 1200 g of the slurry on a converted basis, the slurry was stirred and mixed, adjusted to pH 8.8 with 15% by mass of ammonia water, and aged for 10 minutes. (Step d) This mixed slurry was filtered and washed in the same manner as in Example 1. (The impurity content at this stage was Na on a dry basis.) 2 O: 1.8% by mass, SO 4 2- : 1.1% by mass.) (Steps e~h) The subsequent treatment was carried out in the same manner as in Example 1 to obtain the desired silica-alumina particles III.
[0057] [Example 4] (Process a~c) In the same manner as in Example 1, a pseudoboehmite alumina hydrate aqueous solution and a silica hydrogel aqueous solution were obtained, and Al 2 O 3 Conversion standard is 1200g, SiO 2 After weighing out 1,800 g of the slurry on a converted basis, the slurry was stirred and mixed, adjusted to pH 8.8 with 15% by mass of ammonia water, and aged for 10 minutes. (Step d) The mixed slurry was subjected to solid-liquid separation using a vacuum filter in the same manner as in Example 1, and then washed with warm pure water. (The impurity content at this stage was 1.0% on a dry basis.) 2 O: 2.7% by mass, SO 4 2- : 0.8% by mass.) (Steps e~h) The subsequent treatment was carried out in the same manner as in Example 1 to obtain the desired silica-alumina particles IV.
[0058] [Example 5] (Process a~c) In the same manner as in Example 1, a pseudoboehmite alumina hydrate aqueous solution and a silica hydrogel aqueous solution were obtained, and Al 2 O 3 Conversion standard is 1200g, SiO 2 After weighing out 1,800 g of the slurry on a converted basis, the slurry was stirred and mixed, adjusted to pH 8.8 with 15% by mass of ammonia water, and aged for 10 minutes. (Step d) This mixed slurry was filtered and washed in the same manner as in Example 1. (The impurity content at this stage was Na on a dry basis.) 2 O: 0.6% by mass, SO 4 2- : 3.2% by mass.) (Steps e~h) The subsequent treatment was carried out in the same manner as in Example 1, and the desired silica-alumina particles V were obtained.
[0059] [Comparative Example 1] *Method that does not use pseudoboehmite alumina (Process a'~c') 4.72 kg of 25% by mass sulfuric acid and 2.0 kg of pure water were placed in a 40 L resin tank and adjusted to 30° C. While stirring this sulfuric acid solution, 8.5% by mass SiO 2 Concentration, SiO 2 / Na 2A sodium silicate solution having a molar ratio of 3.2 was added dropwise at a flow rate of 0.56 kg / min for 45 minutes, and then the flow rate was reduced to 0.1 kg / min and the sodium silicate solution was added dropwise for 30 minutes until the pH reached 4.0. After the dropwise addition, stirring was continued for 165 minutes to obtain a silica hydrogel. 500 ml of 15% by mass ammonia water was added to this silica hydrogel to adjust the pH to 7.0 and matured for 1 hour. The weight of the finished silica hydrogel was 35.54 kg, and half of it was transferred to a 50 L steam jacketed tank and 1 kg of pure water was added. After that, 8.45 kg of 23.6% by mass aluminum sulfate solution was added with stirring for 5 minutes while maintaining the slurry temperature in the tank at 45°C, and the pH after the addition was 2.96. Next, 22.6% by mass Al 2 O 3 Concentration, 17.3 mass%Na 2 5.31 kg of 0 concentration sodium aluminate solution was added over 3 minutes, the pH was adjusted to 7.0, and stirring was continued at 45°C for 2 hours. (Process d~h) Thereafter, the silica-alumina mixture slurry was treated in the same manner as in Example 1 to obtain silica-alumina particles VI.
[0060] [Comparative Example 2] (Process a'~c') 35.54 kg of silica hydrogel was prepared in the same manner as in Comparative Example 1. 31.1 kg of this silica hydrogel was weighed and transferred to a 50 L steam jacketed tank, and 1 kg of pure water was added. Then, while maintaining the slurry temperature in the tank at 45°C, 4.22 kg of 23.6% by mass aluminum sulfate solution was added with stirring over a period of 5 minutes. The pH after the addition was 3.50. Next, Al 2 O 3 :22.6% by mass, Na 2 O: 2.66 kg of a 17.3 mass % sodium aluminate solution was added over 3 minutes, and the pH was adjusted to 6.9, followed by continued stirring at 45° C. for 2 hours. (Process d~h) This silica-alumina mixture slurry was treated in the same manner as in Example 1 to obtain silica-alumina particles VII.
[0061] The component composition, loss on ignition LOI, pore volume PV, average pore diameter PD, and specific surface area SA of Samples No. I to VII prepared as above are summarized in Table 1. The results of X-ray diffraction measurements of Samples No. I to VII confirmed that they were amorphous silica-alumina particles. Samples No. I to V had sufficient pore volume PV and specific surface area SA, but Samples No. VI and VII had small average pore diameter PD and poor pore volume PV.
[0062] [Table 1] [Industrial Applicability]
[0063] The porous silica-alumina particles according to the present invention have a high pore volume and a high specific surface area, so that they are expected to have heat insulating properties.In addition to the above physical properties, since they are composed of silica-alumina and have solid acidity, they can be used as a catalyst for petroleum refining, an optical material, or as an additive for cosmetics, resin fillers, and surface coating materials (for the purpose of optical scattering, refractive index adjustment, etc.), etc.
Claims
1. Amorphous porous silica-alumina particles, The specific surface area SA measured by the BET method is 400 to 600 m 2 / g, The pore volume PV measured by the BJH method is in the range of 1.25 to 2.00 ml / g, The average pore diameter PD measured by the BJH method is in the range of 8 to 20 nm, Porous silica-alumina particles, characterized in that the mass ratio of silica to alumina is in the range of 2 / 98 to 70 / 30.
2. In addition, alkali metal ions (M + ) to M 2 Contains 0.1% by mass or less in terms of O, 2. The porous silica-alumina particles according to claim 1, characterized in that the amount of residual inorganic acid ions is 1.0 mass % or less.
Citation Information
Patent Citations
JP1952-003989B
JP1955-005963B
JP1956-001862B
JP1957-000413B
Aromatic hydrogenation catalyst and method for manufacturing and using the catalyst.
JP2010537808A