Method for manufacturing non-coated type printing paper and non-coated type printing paper

JP2024166517AInactive Publication Date: 2024-11-29MITSUBISHI PAPER MILLS LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023082665
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-19
Publication Date
2024-11-29
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Benefits of technology

【0011】 本発明により、白色顔料を含む塗工層を有しない非塗工紙でありながら、角度75度に設定したISO2813:1994/Cor 1:1997に準じて求められる75度光沢が10%以上23%以下であり、インクジェット印刷機に対する印刷適性を有する非塗工紙タイプの印刷用紙の製造方法を提供することができる。さらに、本発明により、前記製造方法によって、オフセット印刷機だけでなく、デジタル印刷機に対する印刷適性、特に、インクジェット印刷機に対する印刷適性を有する非塗工紙タイプの印刷用紙を提供することができる。

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024166517000001
    Figure 2024166517000001
Patent Text Reader

Abstract

To provide a method for manufacturing non-coated type printing paper which is non-coated paper having no coated layer, has 75-degree glossiness of 10% or more and 23% or less and has printability to an inkjet printer.SOLUTION: A method for manufacturing non-coated type printing paper includes the steps of preparing paper stock containing cellulose pulp and calcium carbonate, papermaking the paper stock, size pressing the paper obtained in the paper making step using a size pressing liquid containing a surface size agent and one or two or more kinds of compounds selected from the group consisting of a cationic resin and a water-soluble polyvalent cation salt, and super calendering the paper after the size pressing, wherein a numeric value R (R=[smoothness after super calendering]÷[smoothness before super calendering]) determined by the following expression from Bekk smoothness is 3.6 or more and 12.2 or less, and Bekk smoothness after the super calendering is 175 seconds or more and 370 seconds or less.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing uncoated printing paper that does not have a coating layer containing a white pigment, and in particular to a method for producing uncoated printing paper suitable for inkjet printing machines, which are a type of digital printing machine, and also to uncoated printing paper produced by the method. [Background technology]

[0002] Printing machines for producing commercial printed matter include digital printing machines or on-demand printing machines (hereinafter collectively referred to as "digital printing machines") capable of handling variable information. A representative example is an inkjet printing machine that uses an inkjet recording method. Inkjet printing machines already exist under names such as TruepressJet (registered trademark) from SCREEN Graphic Solutions, MJP series from Miyakoshi, Prosper (registered trademark) and VERSAMARK (registered trademark) from Kodak, and JetPress (registered trademark) from Fujifilm.

[0003] Although it depends on the printing conditions, inkjet printers have color printing speeds several tens of times faster than general home and SOHO inkjet printers and large-format inkjet printers, with printing speeds of 60 m / min or more, and even faster speeds exceeding 100 m / min. For this reason, inkjet printers are distinguished from general home and SOHO inkjet printers and large-format inkjet printers.

[0004] Many of the printing machines on the market for producing commercial printed materials are still offset printing machines, which existed before the advent of digital printing machines. In other words, the printing machines on the market for producing commercial printed materials are a mixture of digital printing machines, such as inkjet printing machines, and offset printing machines. Therefore, printing paper needs to be suitable for printing on both types of printing machines.

[0005] A method for producing uncoated printing paper that has the same gloss as light-weight coated paper (LWC paper) is known (see, for example, Patent Document 1). The printing paper obtained by the method described in Patent Document 1 is called "supercalender paper." Recently, in Europe and the United States, supercalender paper is used as printing paper for offset printing machines or gravure printing machines for commercial printing applications such as magazines, advertising flyers, and catalogs. Supercalender paper has intermediate quality between conventional uncoated paper and LWC paper. However, the supercalender paper described in Patent Document 1 has a white paper gloss of 30% or more, which is somewhat high gloss. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2008-274517 A Summary of the Invention [Problem to be solved by the invention]

[0007] The present invention provides a method for producing uncoated printing paper having a weak gloss like LWC paper, which is an uncoated paper that does not have a coating layer containing a white pigment, but has a 75-degree gloss of 10% or more and 23% or less as required in accordance with ISO2813:1994 / Cor 1:1997 "Paints and varnishes-Determination of specular gloss of non-metallic paint films at 20 degrees, 60 degrees, and 85 degrees,-Technical corrigendum 1" set at an angle of 75 degrees, and is printable not only with offset printing machines but also with digital printing machines, and in particular with inkjet printing machines. Furthermore, the manufacturing method of the present invention provides uncoated printing paper with low gloss, like LWC paper, which has printability not only for offset printing machines but also for digital printing machines, and in particular for inkjet printing machines. [Means for solving the problem]

[0008] The above problems can be solved by the present invention described below.

[0009] [1] A method for producing a paper stock containing cellulose pulp and calcium carbonate as main components, a papermaking process using the paper stock, a size press process using a size press liquid containing a surface sizing agent and one or more compounds selected from the group consisting of a cationic resin and a water-soluble polyvalent cation salt, and a supercalender process for the paper after the size press process, The value R calculated from the Bekk smoothness (seconds) calculated according to ISO5627:1995 "Paper and board-Determination of smoothness (Bekk method)" before and after the supercalendering process by the following formula is 3.6 or more and 12.2 or less, R= (Bekk smoothness after supercalendering (sec))÷ (Bekk smoothness before supercalendering (sec)) and a Bekk smoothness (seconds) after the supercalendering, as determined in accordance with ISO 5627:1995, of 175 (seconds) or more and 370 (seconds) or less.

[0010] [2] Uncoated printing paper manufactured by the manufacturing method described in [1] above and having a 75 degree gloss of 10% to 23% as determined in accordance with ISO 2813:1994 / Cor 1:1997 with an angle of 75 degrees. Effect of the Invention

[0011] The present invention can provide a method for producing uncoated printing paper that is uncoated but does not have a coating layer containing a white pigment, has a 75 degree gloss of 10% to 23% as determined in accordance with ISO2813:1994 / Cor 1:1997 set at an angle of 75 degrees, and is printable on inkjet printers. Furthermore, the present invention can provide an uncoated printing paper that is printable not only on offset printers but also on digital printers, particularly on inkjet printers, by the above production method. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] The uncoated printing paper of the present invention will be described in detail below. As used herein, "inkjet printing" refers to printing using an inkjet printer. Also, "uncoated type" refers to printing paper in which, when the cross section of the printing paper is magnified and observed under an electron microscope, a coating layer containing a white pigment, unlike that observed in coated paper, cannot be visually recognized.

[0013] The method for producing uncoated printing paper includes the steps of preparing a stock containing cellulose pulp and calcium carbonate as main components, making the stock, size pressing the paper obtained in the making step using a size press liquid, and supercalendering the paper after the size press treatment.Furthermore, the value R calculated by the following formula from the Bekk smoothness (sec) calculated in accordance with ISO5627:1995 before and after the supercalendering is 3.6 or more and 12.2 or less, R= (Bekk smoothness after supercalendering (sec))÷ (Bekk smoothness before supercalendering (sec)) Furthermore, the Bekk smoothness (seconds) determined in accordance with ISO 5627:1995 after the supercalendering is 175 seconds or more and 370 seconds or less.

[0014] The stock used in the papermaking process contains cellulose pulp and calcium carbonate as the main components. In the present invention, the term "main components" means that the total of cellulose pulp and calcium carbonate accounts for 60% by mass or more of the mass of the resulting paper.

[0015] The step of preparing the stock is a method conventionally known in the papermaking field, in which cellulose pulp and calcium carbonate, and various additives are mixed as necessary. In some embodiments, the step of preparing the stock is a method of mixing calcium carbonate and, as necessary, various additives conventionally known in the papermaking field, with a slurry of disintegrated and beaten cellulose pulp in water. Examples of the additives include fillers other than calcium carbonate, filler dispersants, internal sizing agents, fixing agents, retention aids, thickeners, flow improvers, defoamers, foam inhibitors, release agents, foaming agents, penetrating agents, coloring dyes, coloring pigments, fluorescent whitening agents, ultraviolet absorbers, antioxidants, preservatives, mold inhibitors, water-resistant agents, paper strength agents, and paper strength enhancers.

[0016] The cellulose pulp is one or more selected from the group consisting of wood pulp and non-wood pulp conventionally known in the papermaking field. Examples of wood pulp include chemical pulps such as Leaf Bleached Kraft Pulp (LBKP) and Needle Bleached Kraft Pulp (NBKP), mechanical pulps such as Groundwood Pulp (GP), Pressure GroundWood pulp (PGW), Refiner Mechanical Pulp (RMP), ThermoMechanical Pulp (TMP), ChemiThermoMechanical Pulp (CTMP), and ChemiMechanical Pulp (CMP), semi-chemical pulps such as ChemiGroundwood Pulp (CGP), waste paper pulps such as DeInked Pulp (DIP), and pulp obtained by disintegrating spoilage generated in paper mills. Non-wood pulp is pulp made of non-wood fibers conventionally known in the papermaking field. Examples of raw materials for non-wood fibers include woody bast such as paper mulberry, mitsumata, and gampi, herbaceous bast such as flax, hemp, and kenaf, leaf fibers such as Manila hemp, abaca, and sisal, grasses such as rice straw, wheat straw, sugarcane bagasse, bamboo, and esparto, and seed hairs such as cotton and linter.

[0017] Calcium carbonate is a type of filler. The paper stock contains one or more calcium carbonates selected from the group consisting of light calcium carbonate and heavy calcium carbonate. In addition to calcium carbonate, the paper stock may contain various fillers conventionally known in the papermaking field, such as talc and kaolin. In some embodiments, the content of calcium carbonate in the paper stock is 60% by mass or more based on the total filler including calcium carbonate in the paper stock, because the printability of the produced printing paper for an inkjet printer is improved.

[0018] The step of making a paper stock is a method of making paper from the paper stock using a papermaking method conventionally known in the papermaking field, and may be any of acidic papermaking, neutral papermaking, and alkaline papermaking. In some embodiments, the step of making a paper stock is a method of making paper using a papermaking machine. The papermaking machine is conventionally known in the papermaking field. Examples of the papermaking machine include a Fourdrinier papermaking machine, a twin-wire papermaking machine, a combination papermaking machine, a cylinder papermaking machine, and a Yankee papermaking machine.

[0019] The size press processing step using the size press liquid is a size press processing method conventionally known in the papermaking field. In some embodiments, the size press processing step using the size press liquid is a size press processing method using a size press processing device. Examples of the size press processing device include an inclined size press, a horizontal size press, a rod metering size press, a roll metering size press, and a blade metering size press as a film transfer method, a shim sizer, an opti sizer, a speed sizer, and a film press as a rod metering size press, and a gate roll coater as a roll metering size press. Examples of other size press processing devices include a bill blade coater, a twin blade coater, a velbapa coater, a tab size press, and a calendar size press.

[0020] The size press liquid contains one or more members selected from the group consisting of cationic resins and water-soluble polyvalent cation salts. In some embodiments, the size press liquid contains one or more selected from the group consisting of cationic resins and does not contain a water-soluble polyvalent cation salt, because this improves the ink drying property in terms of printability with an inkjet printer. In some embodiments, the size press liquid contains one or more selected from the group consisting of water-soluble polyvalent cation salts and does not contain a cationic resin, because this improves ink fixation in terms of printability with an inkjet printer.

[0021] The cationic resin is a cationic polymer or cationic oligomer, and is conventionally known in the field of inkjet printing. In some embodiments, the cationic resin is a polymer or oligomer containing primary to tertiary amines or quaternary ammonium salts that are easily proton-coordinated and dissociate when dissolved in water to exhibit cationicity. Examples of the cationic resin include compounds such as polyethyleneimine, polyvinylpyridine, polyamine sulfone, polydialkylaminoethyl methacrylate, polydialkylaminoethyl acrylate, polydialkylaminoethyl methacrylamide, polydialkylaminoethyl acrylamide, polyepoxyamine, polyamine and modified polyamine, polyamide and modified polyamide, polyamidoamine, dicyandiamide-formaldehyde condensate, polyvinylamine, and polyallylamine, and their hydrochlorides, as well as copolymers of polydiallyldimethylammonium chloride and diallyldimethylammonium chloride with acrylamide, polydiallylmethylamine hydrochloride, and polycondensates of aliphatic monoamines or aliphatic polyamines with epihalohydrin compounds, such as dimethylamine epichlorohydrin polycondensates and diethylenetriamine epichlorohydrin polycondensates. In some embodiments, the cationic resin is a polycondensate of an aliphatic monoamine or aliphatic polyamine and an epihalohydrin compound. This is because it has some effect on improving not only the printability of the inkjet printer but also the strength of the printing paper. In at least one embodiment, the cationic resin is a dimethylamine epichlorohydrin polycondensate. This is because it is advantageous in terms of material cost and is commercially available.

[0022] The water-soluble polyvalent cation salt is a water-soluble salt containing a metal polyvalent cation. The water-soluble polyvalent ion salt is a salt that contains a metal polyvalent cation and can be dissolved in water at 20°C to a final concentration of 1% by mass or more. The metal polyvalent cation is, for example, a divalent cation such as magnesium, calcium, strontium, barium, nickel, zinc, copper, iron, cobalt, tin, manganese, etc.; a trivalent cation such as aluminum, iron, chromium, etc.; or a tetravalent cation such as titanium, zirconium, etc.; and a complex ion thereof. The anion that forms a salt with the metal polyvalent cation may be either an inorganic acid or an organic acid, and is not particularly limited. Examples of inorganic acids include hydrochloric acid, nitric acid, phosphoric acid, sulfuric acid, boric acid, and hydrofluoric acid. Examples of organic acids include formic acid, acetic acid, lactic acid, citric acid, oxalic acid, succinic acid, and organic sulfonic acid. However, aluminum sulfate, which has been conventionally known as a fixing agent for internal sizing agents, is excluded from the water-soluble polyvalent cation salts. In some embodiments, the water-soluble polyvalent cation salt has a metal polyvalent cation of calcium. In at least one embodiment, the water-soluble polyvalent cation salt is one or more selected from the group consisting of calcium chloride, calcium formate, calcium nitrate, and calcium acetate. The reason for this is that printability on a digital printer such as an inkjet printer is improved.

[0023] In some embodiments, in the step of performing a size press treatment using a size press liquid containing one or more compounds selected from the group consisting of a cationic resin and a water-soluble polyvalent cation salt, the total amount of the compound selected from the cationic resin and the water-soluble polyvalent cation salt applied is 0.5 g / m2 or less in terms of dry solid content per side of the paper. 2 More than 2g / m 2 The reason is that the printability of the ink is improved when used with a digital printer such as an inkjet printer.

[0024] The size press fluid contains a surface sizing agent that is conventionally known in the papermaking art. In some embodiments, the size press liquid contains one or more surface sizing agents conventionally known in the papermaking field, such as acrylamide polymers, acrylic polymers, styrene-acrylic acid copolymers, styrene-methacrylic acid copolymers, acrylonitrile-vinyl formal-acrylic acid ester copolymers, styrene-maleic acid copolymers, olefin-maleic acid copolymers, various polyvinyl alcohols, various modified polyvinyl alcohols, starches, and carboxyethyl cellulose. In some embodiments, the surface sizing agent is one or more selected from the group consisting of various polyvinyl alcohols and various modified polyvinyl alcohols, and starches, because this improves printability on digital printers such as inkjet printers.

[0025] In some embodiments, in the step of performing size press treatment using a size press liquid containing a surface sizing agent, the total amount of surface sizing agents conventionally known in the papermaking field to be applied is 0.4 g / m2 in terms of dry solid content per one side of the paper. 2 More than 1.5g / m 2 The reason is that the printability of the ink is improved when used with a digital printer such as an inkjet printer.

[0026] The step of subjecting the paper made after the size press treatment step to supercalendering is a method of performing calendering using a supercalender device conventionally known in the papermaking field. Supercalendering is a type of finishing process that occurs after the papermaking step, and is a method of imparting smoothness and gloss to the paper made. The supercalender device is a machine with multiple roll stages, and is generally installed independently of the papermaking machine, and pressurizes, heats and / or rubs the paper by passing it between multiple metal rolls or between a metal roll and an elastic roll. In some embodiments, the supercalender has 6 to 12 roll nips in the number of roll stages, because this makes it easier to adjust the final Bekk smoothness of the printing paper, which will be described later.

[0027] The printing paper has a Bekk smoothness of 175 (seconds) or more and 370 (seconds) or less after the supercalendering process. Furthermore, the printing paper has a value R of 3.6 or more and 12.2 or less, calculated from the Bekk smoothness (seconds) before and after the supercalendering process using the above formula. The Bekk smoothness is calculated in accordance with ISO5627:1995. This allows the printing paper to have printability on digital printers, particularly inkjet printers, while also achieving a 75-degree gloss of 10% or more and 23% or less, calculated in accordance with ISO2813:1994 / Cor 1:1997, which is set at an angle of 75 degrees.

[0028] Bekk smoothness is measured by pressing a smooth plate against the paper surface with a certain force, letting air flow between the smooth plate and the paper surface, and measuring the time it takes for a certain amount of air to flow, based on the principle that air flows more easily in the case of paper with poor smoothness. The longer the measurement time, the smoother the paper. The actual measurement of Bekk smoothness is not based only on the above principle. This is because it includes air passing through the inside of the surface layer of the paper. Therefore, the measurement of Bekk smoothness is the time it takes for air to pass through both the gap formed between the smooth plate and the paper surface and the gap inside the surface layer of the paper. In other words, the inventors have found that Bekk smoothness is a value that indirectly represents the fine condition of the paper surface of the printing paper. When the Bekk smoothness (seconds) of the printing paper after the supercalendering process is within the above range, the uncoated printing paper can obtain printability for digital printers, particularly printability for inkjet printers, and a weak gloss like that of LWC paper. When the value is less than 175 seconds, printability for digital printers, particularly printability for inkjet printers, is deteriorated in terms of the sharpness of the printed image. When the value is more than 370 seconds, printability for digital printers, particularly printability for inkjet printers, is deteriorated in terms of the ink absorbency of the printed image. Furthermore, when the value is less than 175, the printing paper that has been subjected to a size press process using a size press liquid containing one or more compounds selected from the group consisting of a cationic resin and a water-soluble polyvalent cation salt may have poor offset printability. The printing paper has a value R of 3.6 or more and 12.2 or less, calculated by the above formula from the Bekk smoothness (seconds) calculated according to ISO5627:1995 before and after supercalendering. If the value R of the printing paper is less than 3.6, the printability of the printing paper for digital printers, particularly inkjet printers, is deteriorated in terms of the sharpness of the printed image. If the value R of the printing paper is more than 12.2, the printability of the printing paper for digital printers, particularly inkjet printers, is deteriorated in terms of the ink absorbency of the printed image.

[0029] The uncoated printing paper of the present invention can be obtained by a manufacturing method including the steps of preparing a stock containing cellulose pulp and calcium carbonate as main components, papermaking the stock, size-pressing the paper obtained in the papermaking step with a size-press liquid containing a surface sizing agent and one or more compounds selected from the group consisting of cationic resins and water-soluble polyvalent cation salts, and supercalendering the paper after the size-pressing step, and the value R calculated by the above formula from the Bekk smoothness (seconds) calculated in accordance with ISO5627:1995 before and after the supercalendering is 3.6 to 12.2, and the Bekk smoothness (seconds) calculated in accordance with ISO5627:1995 after the supercalendering is 175 to 370 seconds. The uncoated printing paper obtained by the above manufacturing method has a 75 degree gloss of 10% to 23% as determined according to ISO2813:1994 / Cor 1:1997 with the angle set at 75 degrees. This is a weak gloss like that of LWC paper.

[0030] The smoothness of printing paper is a physical quantity conventionally known in the papermaking field, and can be adjusted by those skilled in the art by the conditions of the manufacturing method. In the papermaking machine and supercalendering device, for example, the conditions of the press zone, the conditions of the drying zone, and the conditions of the supercalendering process can be mentioned. In each condition, for example, increasing the press pressure in the press zone, reducing the heat amount in the drying zone, and increasing the press pressure and / or the number of press stages in the supercalendering process tend to increase the smoothness of the printing paper.

[0031] In some embodiments different from the present invention, the method for producing uncoated printing paper may use a size press liquid that does not necessarily contain one or more compounds selected from the group consisting of cationic resins and water-soluble polyvalent cation salts in the "step of performing size press treatment on the paper obtained in the paper-making step using a size press liquid containing a surface sizing agent and one or more compounds selected from the group consisting of cationic resins and water-soluble polyvalent cation salts" even if the paper lacks printability for digital printers, particularly inkjet printers, so long as there is no problem in terms of practical print quality that matches the application. That is, in some embodiments different from the present invention, the method for producing uncoated printing paper may replace the "step of performing size press treatment on the paper obtained in the paper-making step using a size press liquid containing a surface sizing agent" with "step of performing size press treatment on the paper obtained in the paper-making step using a size press liquid containing a surface sizing agent". In some embodiments different from the present invention, the uncoated printing paper can be obtained by a manufacturing method including the steps of preparing a stock containing cellulose pulp and calcium carbonate as main components, making the stock, subjecting the paper obtained in the making step to a size press treatment using a size press liquid containing a surface sizing agent, and subjecting the paper obtained after the size press treatment to a supercalendering. The value R calculated by the above formula from the Bekk smoothness (seconds) calculated according to ISO5627:1995 before and after the supercalendering is 3.6 to 12.2, and the Bekk smoothness (seconds) calculated according to ISO5627:1995 after the supercalendering is 175 to 370. The printing paper obtained by the manufacturing method has a 75 degree gloss of 10% to 23% at an angle of 75 degrees, calculated according to ISO2813:1994 / Cor 1:1997. This is a low gloss like LWC paper. EXAMPLES

[0032] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples as long as it does not deviate from the gist of the invention. Furthermore, the parts by mass shown in the examples indicate the value of the dry solid content or the value of the substantial component, unless otherwise specified. Furthermore, the amount of the size press applied is the value of the dry solid content.

[0033] (Process for preparing paper material) The process for preparing a paper stock containing cellulose pulp and calcium carbonate as main components is as follows. To a cellulose pulp slurry consisting of 1,000 parts by mass of LBKP with a freeness of 400 mlcsf, 220 parts by mass of calcium carbonate (light calcium carbonate, Okutama Kogyo Co., Ltd., Tamapearl (registered trademark) TP-121SA) as a filler, 1 part by mass of an alkyl ketene dimer type internal sizing agent, 10 parts by mass of a paper strength agent (cationized starch), 9 parts by mass of a fixing agent (aluminum sulfate), and a retention aid (acrylic acid-based resin) were added and mixed.

[0034] (The process of making paper stock) The papermaking process is as follows: The paper stock obtained as described above was made into paper using a fourdrinier paper machine, and the paper was made into a paper having a basis weight of 75 g / m 2 As a result, paper was obtained.

[0035] (A process of size pressing using a size press liquid) The size press process using the size press liquid was as follows. A gate roll coater was used as the size press processing device. In the size press processing, a surface sizing agent (polyvinyl alcohol having a saponification degree of 98 to 99 mol% and a polymerization degree of 300 to 1700) was applied to both sides of the obtained paper at a rate of 0.6 g / m2 per side of the paper. 2and one or more compounds selected from the group consisting of cationic resins and water-soluble polyvalent cation salts, such as calcium chloride (referred to as "calcium chloride" in Table 1), dimethylamine epichlorohydrin polycondensate (referred to as "DMAEPI" in Table 1), magnesium chloride (referred to as "magnesium chloride" in Table 1), or modified polyamine (referred to as "MPA" in Table 1), at a concentration of 1 g / m 2 The compounds selected from the group consisting of cationic resins and water-soluble polyvalent cation salts are shown in Table 1.

[0036] In Comparative Example 5, water not containing a surface sizing agent and a compound selected from the group consisting of a cationic resin and a water-soluble polyvalent cation salt was used as the size press liquid.

[0037] (Super calendar processing process) The paper after the size press treatment was subjected to a supercalender treatment as follows. The paper after size press processing in the size press processing device was subjected to supercalendering in a supercalendering device combining offline metal rolls and elastic rolls, with 12 nip stages, a metal roll temperature of 40°C, and appropriate adjustment of the nip pressure of each stage. During the supercalendering process, the Bekk smoothness was measured before and after the supercalendering process in accordance with ISO5627:1995. The printing paper has a value R of 3.6 or more and 12.2 or less, calculated from the Bekk smoothness (sec) before and after the supercalendering process using the above formula. The Bekk smoothness is calculated in accordance with ISO5627:1995. Before and after the supercalendering process, the Bekk smoothness (seconds) was measured in accordance with ISO5627:1995, and the value R was calculated using the above formula. The values ​​are shown in Table 1.

[0038] In Comparative Example 6, the super calendar device was replaced with a soft nip calendar device to carry out the calendaring process.

[0039] By carrying out each of the above steps, the uncoated printing papers shown in Table 1 were obtained.

[0040] [Table 1]

[0041] (Glossy) The gloss of uncoated printing paper was measured using a Murakami Color Research Laboratory Co., Ltd. digital gloss meter GM-26D model, with the incident-reflection angle set at 75 degrees, according to ISO2813:1994 / Cor 1:1997, with the angle set at 75 degrees.

[0042] (Compared to LWC paper) The obtained uncoated printing papers were observed using a commercially available LWC paper (Mitsubishi Paper Mills, Margaree Light) as a standard, and were subjected to a sensory evaluation according to the following criteria. A: I feel it is similar to LWC paper. B: I don't think it is similar to LWC paper.

[0043] (Printability for offset printing machines) A sheet-fed offset printing machine (Mitsubishi Heavy Industries, Dia 3H-4) was used to print four colors on one side of the printing paper using lithographic offset process inks. For printing, a 4 cm x 4 cm image of each color was randomly arranged. The printed image was visually observed and evaluated according to the following criteria. In the present invention, uncoated printing paper is considered to be suitable for printing on an offset printing machine if it is rated A or B. A: Good usable quality. B: Although inferior to A above, it is still of usable quality. C: The quality is not practical.

[0044] (Printability for inkjet printers) The inkjet printer used was a Fujifilm Jet Press 540W (printing speed: 100 m / min). The printed image was a 2 cm x 2 cm square image with a total of seven solid color patterns, consisting of the single colors black, cyan, magenta, and yellow, and the double colors (red, green, and blue) made with the other three ink colors excluding black, arranged in a horizontal row with no gaps. The prints were visually evaluated from the viewpoints of ink absorption, sharpness, color development, fixation, color vividness, uniformity, image visibility on the back side of the printed surface (the less visible the better), etc. In this invention, uncoated printing paper is considered to have printability for inkjet printers if it is rated A or B. A: Good usable quality. B: Although inferior to A above, it is still of usable quality. C: The quality is not practical.

[0045] The results are shown in Table 1.

[0046] From Table 1, it can be seen that the uncoated printing paper produced by the production method according to the present invention has printability for offset printing machines and inkjet printing machines, which are representative of digital printing machines, and is an uncoated paper that does not have a coating layer containing a white pigment, but has a 75 degree gloss of 10% to 23% as determined in accordance with ISO2813:1994 / Cor 1:1997 set at an angle of 75 degrees. On the other hand, it can be seen that the uncoated printing paper produced by a production method not corresponding to the present invention is an uncoated paper that does not have a coating layer containing a white pigment, but has a 75 degree gloss of 10% to 23% as determined in accordance with ISO2813:1994 / Cor 1:1997 set at an angle of 75 degrees, and does not satisfy at least one of the printability for offset printing and the printability for inkjet printing machines.

Claims

1. The method comprises the steps of preparing a stock containing cellulose pulp and calcium carbonate as main components, papermaking the stock, subjecting the paper obtained in the papermaking step to a size press treatment using a size press liquid containing a surface sizing agent and one or more compounds selected from the group consisting of a cationic resin and a water-soluble polyvalent cation salt, and subjecting the paper obtained after the size press treatment step to a supercalender treatment, The value R calculated by the following formula from the Bekk smoothness (seconds) calculated in accordance with ISO 5627:1995 before and after the supercalendering is 3.6 or more and 12.2 or less, R = (Bekk smoothness after supercalendering (sec))÷ (Bekk smoothness (sec) before supercalendering) and a Bekk smoothness (seconds) after the supercalendering, as determined in accordance with ISO 5627:1995, of 175 seconds or more and 370 seconds or less.

2. 2. An uncoated printing paper produced by the method according to claim 1, which has a 75 degree gloss of 10% to 23% as determined in accordance with ISO 2813:1994 / Cor 1:1997 with an angle of 75 degrees.

Citation Information

Patent Citations

  • Method for producing printing paper

    JP2008274517A