Method for manufacturing non-coated type printing paper and non-coated type printing paper
A manufacturing method for non-coated paper using cellulose pulp and calcium carbonate, combined with specific treatments, addresses the issue of high gloss in existing papers, enabling printability on both offset and digital printing machines by controlling Cobb water absorption and gloss.
Patent Information
- Application Number
- JP2023082666
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-19
- Publication Date
- 2024-11-29
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing printing papers with high gloss levels are not suitable for both offset and digital printing machines, particularly inkjet printing machines, due to their high gloss and inadequate printability.
A manufacturing method involving a paper stock with cellulose pulp and calcium carbonate, size press treatment using a cationic resin and water-soluble polyvalent cation salt, and supercalendering to achieve a specific range of Cobb water absorption and gloss levels, ensuring suitability for both offset and digital printing machines.
The method produces a non-coated paper with a gloss of 10-23% at 75 degrees, suitable for inkjet printing machines, while maintaining printability for offset machines, by adjusting Cobb water absorption and gloss levels.
Smart Images

Figure 2024166518000001
Abstract
Description
[Technical Field]
[0001] The present invention relates to a method for producing uncoated printing paper that does not have a coating layer containing a white pigment, and in particular to a method for producing uncoated printing paper that is suitable for inkjet printing machines, which are a type of digital printing machine. It also relates to uncoated printing paper produced by the method. [Background technology]
[0002] Among printing presses for producing commercial printed materials, there are digital printing presses or on-demand printing presses (hereinafter collectively referred to as "digital printing presses") that can handle variable information. A representative example is an inkjet printing press that uses an inkjet recording method. Inkjet printing presses already exist under names such as TruepressJet (registered trademark) from SCREEN Graphic Solutions, the MJP series from Miyakoshi, Prosper (registered trademark) and VERSAMARK (registered trademark) from Kodak, and JetPress (registered trademark) from Fujifilm.
[0003] Although it depends on the printing conditions, inkjet printers have color printing speeds several tens of times faster than general home and SOHO inkjet printers and large-format inkjet printers, with printing speeds of 60 m / min or more, and even faster speeds exceeding 100 m / min. For this reason, inkjet printers are distinguished from general home and SOHO inkjet printers and large-format inkjet printers.
[0004] Many of the printing machines on the market for producing commercial printed materials are still offset printing machines, which existed before the advent of digital printing machines. In other words, the printing machines on the market for producing commercial printed materials are a mixture of digital printing machines, typified by inkjet printing machines, and offset printing machines. Therefore, printing paper must be suitable for printing on both types of printing machines.
[0005] A method for manufacturing uncoated printing paper that has the gloss of lightweight coated paper (LWC paper) despite being uncoated is known (see, for example, Patent Document 1). The printing paper obtained by the manufacturing method described in Patent Document 1 is called "supercalender paper." Recently, in Europe and the United States, supercalender paper is used as printing paper for offset printing machines or gravure printing machines for commercial printing applications such as magazines, promotional flyers, and catalogs. Supercalender paper has quality intermediate between conventional uncoated paper and LWC paper. However, the supercalender paper described in Patent Document 1 has a white paper gloss of 30% or more, which is somewhat higher gloss. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] Japanese Patent Application Laid-Open No. 2008-274517 Summary of the Invention [Problem to be solved by the invention]
[0007] The present invention provides a method for producing uncoated printing paper that does not have a coating layer containing a white pigment, but has a 75-degree gloss of 10% to 23% as determined in accordance with ISO2813:1994 / Cor 1:1997 "Paints and varnishes - Determination of specular gloss of non-metallic paint films at 20 degrees, 60 degrees, and 85 degrees - Technical corrigendum 1" set at a 75-degree angle, and is printable not only with offset printing machines but also with digital printing machines, particularly with inkjet printing machines, and that has a low gloss like LWC paper. Furthermore, the manufacturing method of the present invention provides uncoated printing paper with low gloss, such as LWC paper, that is printable not only with offset printing machines but also with digital printing machines, and in particular with inkjet printing machines. [Means for solving the problem]
[0008] The above problems can be solved by the present invention described below.
[0009] [1] A method for producing a paper stock comprising the steps of preparing a paper stock containing cellulose pulp and calcium carbonate as main components, papermaking the paper stock, size-pressing the paper obtained in the papermaking step using a size-press solution containing a surface sizing agent and one or more compounds selected from the group consisting of cationic resins and water-soluble polyvalent cation salts, and supercalendering the paper after the size-pressing step, wherein the supercalendering step determines the Cobb water absorbency (g / m) of the paper at a contact time of 10 seconds as determined in accordance with ISO535:1991 "Paper and board - Determination of water absorptiveness - Cobb method". 2 ) to the basis weight of the paper (g / m 2 ) before and after the supercalendering treatment is 0.050 or more and 0.160 or less, and the Cobb water absorbency (g / m 2 ) to the basis weight of the paper (g / m 2 ) is 1.050 or more and 1.210 or less.
[0010] [2] Uncoated printing paper manufactured by the manufacturing method described in [1] above, with a 75-degree gloss of 10% to 23% as determined in accordance with ISO 2813:1994 / Cor 1:1997, with the angle set at 75 degrees. [Effects of the Invention]
[0011] The present invention provides a method for producing uncoated printing paper that does not have a coating layer containing a white pigment, but has a 75° gloss of 10% to 23% as determined in accordance with ISO 2813:1994 / Cor 1:1997 at a 75° angle, set at 10°. Furthermore, the present invention provides uncoated printing paper that is printable not only with offset printing machines but also with digital printing machines, particularly with inkjet printing machines. DETAILED DESCRIPTION OF THE INVENTION
[0012] The uncoated printing paper of the present invention will be described in detail below. As used herein, "inkjet printing" refers to printing using an inkjet printer. Furthermore, "uncoated type" refers to printing paper in which, when the cross section of the printing paper is magnified and observed under an electron microscope, a coating layer containing a white pigment, as observed in coated paper, cannot be seen.
[0013] The method for producing uncoated printing paper includes the steps of preparing a stock containing cellulose pulp and calcium carbonate as main components, making the stock, subjecting the paper obtained in the making step to a size press treatment using a size press liquid, and subjecting the paper obtained after the size press treatment to a supercalender treatment. In addition, in the method for producing uncoated printing paper, the Cobb water absorbency (g / m) of the paper at a contact time of 10 seconds determined in accordance with ISO 535:1991 is used. 2 ) to the basis weight of the paper (g / m 2 ) before and after the supercalendering treatment is 0.050 or more and 0.160 or less, and the Cobb water absorbency (g / m 2 ) divided by the paper basis weight is 1.050 or more and 1.210 or less.
[0014] The paper stock used in the papermaking process contains cellulose pulp and calcium carbonate as its main components. In the present invention, the term "main components" means that the total of cellulose pulp and calcium carbonate accounts for 60% by mass or more of the mass of the paper to be obtained.
[0015] The stock preparation step is a conventional method known in the papermaking field, in which cellulose pulp, calcium carbonate, and, if necessary, various additives are mixed. In some embodiments, the stock preparation step is a method in which calcium carbonate and, if necessary, various additives conventionally known in the papermaking field are mixed with an aqueous slurry of disintegrated and beaten cellulose pulp. Examples of the additives include fillers other than calcium carbonate, filler dispersants, internal sizing agents, fixing agents, retention aids, thickeners, flow improvers, antifoaming agents, foam suppressors, release agents, foaming agents, penetrating agents, coloring dyes, coloring pigments, fluorescent whitening agents, ultraviolet absorbers, antioxidants, preservatives, mildew inhibitors, water-resistant agents, paper strength agents, and paper strength enhancers.
[0016] The cellulose pulp is one or more selected from the group consisting of wood pulp and non-wood pulp conventionally known in the papermaking field. Examples of wood pulp include chemical pulps such as Leaf Bleached Kraft Pulp (LBKP) and Needle Bleached Kraft Pulp (NBKP), mechanical pulps such as Groundwood Pulp (GP), Pressure Groundwood Pulp (PGW), Refiner Mechanical Pulp (RMP), ThermoMechanical Pulp (TMP), ChemiThermoMechanical Pulp (CTMP), and ChemiMechanical Pulp (CMP), semi-chemical pulps such as ChemiGroundwood Pulp (CGP), waste paper pulp such as DeInked Pulp (DIP), and pulp obtained by disintegrating spoilage generated in paper mills. Non-wood pulp is pulp made of non-wood fibers conventionally known in the papermaking field. Examples of raw materials for non-wood fibers include woody bast such as paper mulberry, Mitsumata, and gampi, herbaceous bast such as flax, hemp, and kenaf, leaf fibers such as Manila hemp, abaca, and sisal, grasses such as rice straw, wheat straw, sugarcane bagasse, bamboo, and esparto, and seed hairs such as cotton and linter.
[0017] Calcium carbonate is a type of filler. The paper stock contains one or more calcium carbonates selected from the group consisting of light calcium carbonate and heavy calcium carbonate. In addition to calcium carbonate, the paper stock may contain various fillers conventionally known in the papermaking field, such as talc and kaolin. In some embodiments, the content of calcium carbonate in the stock is 60% by mass or more based on the total amount of fillers, including calcium carbonate, in the stock, because this improves the printability of the produced printing paper in an inkjet printer.
[0018] The step of making paper stock is a method of producing paper from the paper stock using a papermaking method conventionally known in the papermaking field, and may be any of acidic papermaking, neutral papermaking, and alkaline papermaking. In some embodiments, the step of making paper stock is a method of making paper using a paper machine. The paper machine is conventionally known in the papermaking field. Examples of paper machines include a Fourdrinier paper machine, a twin-wire paper machine, a combination paper machine, a cylinder paper machine, and a Yankee paper machine.
[0019] The step of performing size press treatment using a size press liquid is a size press treatment method conventionally known in the papermaking field. In some embodiments, the step of performing size press treatment using a size press liquid is a size press treatment method using a size press treatment device. Examples of size press treatment devices include an inclined size press, a horizontal size press, and a film transfer type rod metering size press, a roll metering size press, and a blade metering size press. Examples of rod metering size presses include a shim sizer, an Opticizer, a Speed Sizer, and a film press. Examples of roll metering size presses include a gate roll coater. Other size press treatment devices include a bill blade coater, a twin blade coater, a Belbapa coater, a tab size press, and a calendar size press.
[0020] The size press liquid contains one or more members selected from the group consisting of cationic resins and water-soluble polyvalent cation salts. In some embodiments, the size press liquid contains one or more selected from the group consisting of cationic resins and does not contain a water-soluble polyvalent cation salt, because this improves ink drying properties in terms of printability on an inkjet printer. In some embodiments, the size press liquid contains one or more salts selected from the group consisting of water-soluble polyvalent cation salts and does not contain a cationic resin, because this improves ink fixation in terms of printability with an inkjet printer.
[0021] The cationic resin is a cationic polymer or cationic oligomer, and is conventionally known in the field of inkjet printing. In some embodiments, the cationic resin is a polymer or oligomer containing a primary to tertiary amine or a quaternary ammonium salt, which easily coordinates with a proton and dissociates when dissolved in water to exhibit cationic properties. Examples of the cationic resin include polyethyleneimine, polyvinylpyridine, polyamine sulfone, polydialkylaminoethyl methacrylate, polydialkylaminoethyl acrylate, polydialkylaminoethyl methacrylamide, polydialkylaminoethyl acrylamide, polyepoxyamine, polyamine and modified polyamine, polyamide and modified polyamide, polyamidoamine, dicyandiamide-formalin condensate, polyvinylamine, polyallylamine, and other compounds and their hydrochlorides; further, polydiallyldimethylammonium chloride, copolymers of diallyldimethylammonium chloride with acrylamide, polydiallylmethylamine hydrochloride; and polycondensates of aliphatic monoamines or aliphatic polyamines with epihalohydrin compounds, such as dimethylamine epichlorohydrin polycondensates and diethylenetriamine epichlorohydrin polycondensates. In some embodiments, the cationic resin is a polycondensate of an aliphatic monoamine or aliphatic polyamine with an epihalohydrin compound. This is because it not only improves printability in inkjet printers but also has some effect on improving the paper strength of the printing paper. In at least one embodiment, the cationic resin is a dimethylamine epichlorohydrin polycondensate. This is because it is advantageous in terms of material cost and is readily available commercially.
[0022] Water-soluble polyvalent cation salts are water-soluble salts containing metal polyvalent cations. Water-soluble polyvalent ion salts contain metal polyvalent cations and are ultimately soluble in water at 20°C at a concentration of 1% by mass or more. Examples of metal polyvalent cations include divalent cations such as magnesium, calcium, strontium, barium, nickel, zinc, copper, iron, cobalt, tin, and manganese; trivalent cations such as aluminum, iron, and chromium; and tetravalent cations such as titanium and zirconium, as well as complex ions thereof. Anions that form salts with metal polyvalent cations may be either inorganic or organic acids, and are not particularly limited. Examples of inorganic acids include hydrochloric acid, nitric acid, phosphoric acid, sulfuric acid, boric acid, and hydrofluoric acid. Examples of organic acids include formic acid, acetic acid, lactic acid, citric acid, oxalic acid, succinic acid, and organic sulfonic acids. However, aluminum sulfate, which has been known as a fixing agent for internal sizing agents, is excluded from the water-soluble polyvalent cation salts. In some embodiments, the water-soluble polyvalent cation salt has a metal polyvalent cation of calcium. In at least one embodiment, the water-soluble polyvalent cation salt is one or more selected from the group consisting of calcium chloride, calcium formate, calcium nitrate, and calcium acetate. This is because it improves printability in digital printers such as inkjet printers.
[0023] In some embodiments, in the step of performing a size press treatment using a size press liquid containing one or more compounds selected from the group consisting of a cationic resin and a water-soluble polyvalent cation salt, the total amount of the compound selected from the cationic resin and the water-soluble polyvalent cation salt applied is 0.5 g / m in terms of dry solid content per side of the paper. 2 More than 2g / m 2 The reason for this is that the printability on digital printers such as inkjet printers is improved.
[0024] The size press liquid contains a surface sizing agent conventionally known in the papermaking art. In some embodiments, the size press liquid contains one or more surface sizing agents selected from the group consisting of surface sizing agents conventionally known in the papermaking field, such as acrylamide polymers, acrylic polymers, styrene-acrylic acid copolymers, styrene-methacrylic acid copolymers, acrylonitrile-vinyl formal-acrylic ester copolymers, styrene-maleic acid copolymers, olefin-maleic acid copolymers, various polyvinyl alcohols, various modified polyvinyl alcohols, starches, and carboxyethyl cellulose. In some embodiments, the surface sizing agent is one or more selected from the group consisting of various polyvinyl alcohols and various modified polyvinyl alcohols, and starches, because this improves printability on digital printers such as inkjet printers.
[0025] In some embodiments, in the step of performing size press treatment using a size press liquid containing a surface sizing agent, the total amount of surface sizing agents conventionally known in the papermaking field to be applied is 0.4 g / m2 in terms of dry solid content per side of the paper. 2 More than 1.5g / m 2 The reason for this is that the printability on digital printers such as inkjet printers is improved.
[0026] The supercalendering process for the paper made after the size press process is a method of calendering using a supercalender device conventionally known in the papermaking field. Supercalendering is a type of finishing process that occurs after the papermaking process and is a method of imparting smoothness and gloss to the paper made. A supercalender is a machine with multiple roll stages, generally installed independently of the papermaking machine, and performs pressure, heat, and / or friction by passing the paper between multiple metal rolls or between a metal roll and an elastic roll. In some embodiments, the supercalender has 6 to 12 roll nips in terms of roll stages, because this makes it easier to adjust the final Cobb water absorbency (described below) of the printing paper.
[0027] The printing paper is subjected to a supercalendering process to measure the Cobb water absorbency (g / m) at a contact time of 10 seconds after the supercalendering process. 2 ) to the basis weight of the paper (g / m 2 ) is 1.050 or more and 1.210 or less. Furthermore, in the supercalendering process, the printing paper has a Cobb water absorbency (g / m 2 ) to the basis weight of the paper (g / m 2 ) before and after the supercalendering treatment, the difference in the Cobb water absorbency at a contact time of 10 seconds is determined in accordance with ISO535:1991. This allows the printing paper to have printability for digital printing machines, particularly inkjet printing machines, while also achieving a 75-degree gloss of 10% or more and 23% or less, as determined in accordance with ISO2813:1994 / Cor 1:1997, set at an angle of 75 degrees. Here, the Cobb water absorbency (g / m) at a contact time of 10 seconds 2 ) to the basis weight of the paper (g / m 2 The difference between the value before and after the supercalendering treatment, which is obtained by dividing the value by 1 / (2), is the "value before the supercalendering treatment" - "value after the supercalendering treatment".
[0028] Cobb water absorbency is the amount of water absorbed (g / m) when a given area of paper is in contact with water for a given period of time. 2 ) is measured to express water absorbency. When the paper surface has pores with openings of a certain size, water penetrates into the pores, and when the paper surface has dense pores because the openings have been crushed by supercalendering, water penetrates due to capillary action through the dense pores. Water absorption is also affected by the basis weight of the paper. The greater the basis weight of the paper, the greater the water absorption. The inventors have found that when measuring Cobb water absorbency, if the contact time is 10 seconds, the influence of the individual volume of the pores as described above becomes smaller, and the Cobb water absorbency (g / m 2 ) to the basis weight of the paper (g / m 2) is an index that indirectly represents the condition of the paper surface. Cobb water absorbency (g / m) for a contact time of 10 seconds for printing paper after supercalendering 2 ) to the basis weight of the paper (g / m 2 ) is within the above range, uncoated printing paper can achieve printability with digital printers, particularly with inkjet printers, and a weak gloss like that of LWC paper. If the value is less than 1.050, printability with digital printers, particularly with inkjet printers, deteriorates in terms of ink absorbency of the printed image. If the value exceeds 1.210, printability with digital printers, particularly with inkjet printers, deteriorates in terms of sharpness of the printed image. Furthermore, if the value exceeds 1.210, printing paper that has been subjected to a size press treatment using a size press liquid containing one or more compounds selected from the group consisting of a cationic resin and a water-soluble polyvalent cation salt may exhibit poor offset printability. If the difference between the Cobb absorbency after a 10-second contact time divided by the basis weight before and after supercalendering is less than 0.050, the printability of the printing paper for digital printers, particularly inkjet printers, will be impaired in terms of the sharpness of the printed image.If the difference between the Cobb absorbency after a 10-second contact time divided by the basis weight before and after supercalendering is more than 0.160, the printability of the printing paper for digital printers, particularly inkjet printers, will be impaired in terms of the ink absorbency of the printed image.
[0029] The uncoated printing paper of the present invention can be obtained by a manufacturing method comprising the steps of preparing a stock containing cellulose pulp and calcium carbonate as the main components, papermaking the stock, size-pressing the paper obtained in the papermaking step with a size-press solution containing a surface sizing agent and one or more compounds selected from the group consisting of a cationic resin and a water-soluble polyvalent cation salt, and supercalendering the paper after the size-pressing step, in which the difference between the Cobb water absorbency after a 10-second contact time divided by the paper weight before and after supercalendering is between 0.050 and 0.160, and the value of the Cobb water absorbency after supercalendering divided by the paper weight is between 1.050 and 1.210. The uncoated printing paper obtained by this manufacturing method has a 75-degree gloss of 10% to 23% as determined in accordance with ISO2813:1994 / Cor 1:1997, where the angle is set at 75 degrees. This is a weak gloss similar to that of LWC paper.
[0030] The Cobb water absorbency of printing paper is a physical quantity conventionally known in the papermaking field and can be adjusted by those skilled in the art by adjusting the conditions of the manufacturing method. In papermaking machines and supercalendering devices, examples of such adjustments include the concentration and supply amount of the stock supplied, the conditions of the press zone, the conditions of the drying zone, and the conditions of the supercalendering process. Among the various conditions, for example, increasing the stock concentration, increasing the supply amount of the stock, increasing the press pressure in the press zone, reducing the heat amount in the drying zone, and increasing the press pressure and / or number of press stages in the supercalendering process tend to lower the Cobb water absorbency value of the printing paper.
[0031] In some embodiments different from the present invention, in the method for producing uncoated printing paper, in the "step of performing a size press treatment on the paper obtained in the paper-making step using a size press liquid containing a surface sizing agent and one or more compounds selected from the group consisting of a cationic resin and a water-soluble polyvalent cation salt," even if the paper is not suitable for printing in a digital printer, particularly an inkjet printer, as long as there is no problem with practical print quality suitable for the intended use, the size press treatment may be performed using a size press liquid that does not necessarily contain one or more compounds selected from the group consisting of a cationic resin and a water-soluble polyvalent cation salt. That is, in some embodiments different from the present invention, in the method for producing uncoated printing paper, the "step of performing a size press treatment on the paper obtained in the paper-making step using a size press liquid containing a surface sizing agent" may be replaced with a "step of performing a size press treatment on the paper obtained in the paper-making step using a size press liquid containing a surface sizing agent." In some embodiments different from the present invention described above, uncoated printing paper can be obtained by a manufacturing method comprising the steps of preparing a stock containing cellulose pulp and calcium carbonate as the main components, papermaking the stock, size-pressing the paper obtained in the papermaking step using a size-press liquid containing a surface sizing agent, and supercalendering the paper after the size-pressing step. Regarding the supercalendering step, the Cobb water absorbency (g / m) of the paper at a contact time of 10 seconds determined in accordance with ISO 535:1991 is determined. 2 ) to the basis weight of the paper (g / m 2 ) before and after the supercalendering treatment is 0.050 or more and 0.160 or less, and the Cobb water absorbency (g / m 2 ) to the basis weight of the paper (g / m 2) is 1.050 or more and 1.210 or less. The printing paper obtained by the above manufacturing method has a 75-degree gloss of 10% or more and 23% or less, as determined in accordance with ISO2813:1994 / Cor 1:1997, with an angle set at 75 degrees. This is a weak gloss like that of LWC paper. [Example]
[0032] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples as long as it does not depart from the spirit of the invention. Furthermore, parts by mass shown in the examples represent values of dry solid content or substantial component amount unless otherwise specified. Furthermore, the amount of size press applied is a value of dry solid content.
[0033] (Process for preparing paper stock) The process for preparing a paper stock containing cellulose pulp and calcium carbonate as the main components was as follows. To a cellulose pulp slurry consisting of 1,000 parts by mass of LBKP with a freeness of 400 mlcsf, 220 parts by mass of calcium carbonate (light calcium carbonate, Okutama Kogyo Co., Ltd., Tamapearl (registered trademark) TP-121SA) as a filler, 1 part by mass of an alkyl ketene dimer-type internal sizing agent, 10 parts by mass of a paper strength agent (cationized starch), 9 parts by mass of a fixing agent (aluminum sulfate), and a retention aid (acrylic acid-based resin) were added and mixed.
[0034] (Process for making paper stock) The papermaking process was as follows: The paper stock obtained as described above was made into paper using a Fourdrinier paper machine, and the paper was made into a paper with a basis weight of 75.0 g / m 2 Thus, paper was obtained.
[0035] (A process of size pressing using a size pressing liquid) The size press treatment using the size press liquid was carried out as follows. A gate roll coater was used as the size press treatment device. In the size press treatment, a surface sizing agent (polyvinyl alcohol with a saponification degree of 98 to 99 mol% and a polymerization degree of 300 to 1700) was applied to both sides of the obtained paper at a rate of 0.6 g / m per side of the paper. 2 and 1 g / m of calcium chloride (referred to as "calcium chloride" in Table 1), dimethylamine epichlorohydrin polycondensate (referred to as "DMAEPI" in Table 1), magnesium chloride (referred to as "magnesium chloride" in Table 1), or modified polyamine (referred to as "MPA" in Table 1) as one or more compounds selected from the group consisting of cationic resins and water-soluble polyvalent cation salts. 2 The compounds selected from the group consisting of cationic resins and water-soluble polyvalent cation salts are shown in Table 1. The basis weight of the paper was finally 78.2 g / m except for Comparative Example 5. 2 The paper of Comparative Example 5 had a basis weight of 75.0 g / m 2 This becomes:
[0036] In Comparative Example 5, the size press liquid was water that did not contain a surface sizing agent and a compound selected from the group consisting of a cationic resin and a water-soluble polyvalent cation salt.
[0037] (Super calendar processing process) The paper after the size press treatment was subjected to a supercalender treatment as follows. The paper after size press processing in the size press processing device was subjected to supercalendering in a supercalendering device that combines offline metal rolls and elastic rolls, with 12 nip stages, a metal roll temperature of 40°C, and the nip pressure of each stage appropriately adjusted. In the supercalendering treatment, the Cobb water absorbency (g / m) of the paper after a contact time of 10 seconds, as determined in accordance with ISO 535:1991, was measured before and after the supercalendering treatment. 2 The Cobb water absorbency (g / m) of the paper after the supercalendering treatment was measured. 2 ) to the basis weight of the paper (g / m 2) and Cobb water absorbency (g / m 2 ) to the basis weight of the paper (g / m 2 The difference between the values before and after the super calendar treatment was calculated for the values divided by the formula (1) and (2). The values are shown in Table 1.
[0038] In Comparative Example 6, the super calender was replaced with a soft nip calender to carry out the calendering process.
[0039] By carrying out each of the above steps, the uncoated printing papers shown in Table 1 were obtained.
[0040] [Table 1]
[0041] (glossy) The gloss of uncoated printing paper was measured using a digital gloss meter GM-26D from Murakami Color Research Laboratory Co., Ltd., at an incident-reflection angle of 75 degrees, in accordance with ISO2813:1994 / Cor 1:1997, with the angle set to 75 degrees.
[0042] (Compared to LWC paper) The obtained uncoated printing paper was observed using commercially available LWC paper (Mitsubishi Paper Mills, Margary Light) as a standard, and subjected to a sensory evaluation according to the following criteria. A: I feel it is similar to LWC paper. B: I don't feel it is similar to LWC paper.
[0043] (Printability for offset printing machines) Four-color printing was carried out on one side of coated printing paper using a sheet-fed offset printing press (Mitsubishi Heavy Industries, Dia 3H-4) with lithographic offset process inks. A 4 cm x 4 cm image of each color was randomly arranged for printing. The printed image was visually observed and evaluated according to the following criteria. In the present invention, uncoated coated printing paper is considered to be suitable for printing on an offset printing press if it is rated A or B. A: Good quality that can be used in practice. B: Although inferior to A above, it is still of usable quality. C: The quality is not practical.
[0044] (Printability for inkjet printers) The inkjet printer used was a Fujifilm Jet Press 540W (printing speed: 100 m / min). The printed image consisted of seven solid color patterns: black, cyan, magenta, and yellow, plus two-tone colors (red, green, and blue) made with the other three ink colors (excluding black), arranged in a horizontal row with no gaps in a 2 cm x 2 cm square. The printed matter was visually evaluated from the viewpoints of ink absorption, sharpness, color development, fixation, color vividness, uniformity, image visibility on the backside of the printed surface (the less visible the better), etc. In this invention, uncoated printing paper is considered to be suitable for printing on an inkjet printer if it is rated A or B. A: Good quality that can be used in practice. B: Although inferior to A above, it is still of usable quality. C: The quality is not practical.
[0045] The results are shown in Table 1.
[0046] From Table 1, it can be seen that uncoated printing paper produced by the production method of the present invention is printable on offset presses and inkjet presses, which are representative of digital presses, and is uncoated paper that does not have a coating layer containing a white pigment, but has a 75° gloss of 10% to 23% as measured at a 75° angle in accordance with ISO2813:1994 / Cor 1:1997. On the other hand, uncoated printing paper produced by a production method that does not correspond to the present invention is uncoated paper that does not have a coating layer containing a white pigment, but does not have a 75° gloss of 10% to 23% as measured at a 75° angle in accordance with ISO2813:1994 / Cor 1:1997, and does not satisfy at least one of the printability for offset printing and the printability for inkjet presses.
Claims
1. The method comprises the steps of preparing a stock containing cellulose pulp and calcium carbonate as main components, papermaking the stock, subjecting the paper obtained in the papermaking step to a size press treatment using a size press liquid containing a surface sizing agent and one or more compounds selected from the group consisting of a cationic resin and a water-soluble polyvalent cation salt, and subjecting the paper obtained after the size press treatment step to a supercalender treatment, Regarding the supercalendering process, the Cobb water absorbency (g / m) of the paper at a contact time of 10 seconds determined in accordance with ISO 535:1991 is 2 ) to the basis weight (g / m 2 ) before and after the supercalendering is 0.050 to 0.160, and the Cobb water absorbency (g / m 2 ) to the basis weight (g / m 2 ) is 1.050 or more and 1.210 or less.
2. 2. An uncoated printing paper produced by the method according to claim 1, which has a 75 degree gloss of 10% to 23% as determined in accordance with ISO 2813:1994 / Cor 1:1997 with an angle of 75 degrees.
Citation Information
Patent Citations
Method for producing printing paper
JP2008274517A