Metal sulfide compound carrier and method for producing the same
A sulfide metal compound support, formed by reacting sulfuric acid with a metal on diatomaceous earth, addresses handling issues of sulfuric acid, providing stable and long-lasting oxidizing capabilities for diverse applications.
Patent Information
- Application Number
- JP2023083350
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-19
- Publication Date
- 2024-11-29
AI Technical Summary
Sulfuric acid, while effective as an oxidizing agent, poses handling challenges due to its strong dehydrating effect, heat generation, and potential for burns, making it difficult to use in large quantities with water-containing substances.
A sulfide metal compound support is created by reacting hot concentrated sulfuric acid with a metal and supporting it on diatomaceous earth, which maintains a solid state, ensuring good handling properties and high oxidizing capabilities.
The sulfide metal compound support remains stable at room temperature, allows large-scale use without rapid reactions, exhibits high oxidizing properties, and sustains these properties over time, suitable for various applications including fertilizers, wastewater treatment, and chemical synthesis.
Smart Images

Figure 2024166918000001 
Figure 2024166918000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a metal sulfide compound support that can be used as an oxidizing agent exhibiting high oxidizing properties. [Background technology]
[0002] Sulfuric acid is a liquid chemical substance having strong acidity, and is used as an oxidizing agent (proton donor) in applications such as fertilizer production, mineral processing, petroleum refining, wastewater treatment agents, raw materials for chemical synthesis, and electrolytes for lead-acid batteries, as described in Patent Documents 1 and 2. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2011-246288 A [Patent Document 2] JP 2006-143509 A Summary of the Invention [Problem to be solved by the invention]
[0004] However, sulfuric acid has a strong dehydrating effect and generates heat when added to water, making it difficult to use in large quantities on substances that contain a lot of water. In addition, if it comes into contact with human tissue, it will cause severe acid chemical burns, so it is not necessarily easy to handle.
[0005] An object of the present invention is to provide a metal sulfide compound support which overcomes the problems associated with sulfuric acid as an oxidizing agent described above, is easy to handle since it is a solid at room temperature, and is capable of exhibiting good oxidizing properties (proton donating properties) over a long period of time (i.e., can be used as an oxidizing agent). [Means for solving the problem]
[0006] The present invention, as set forth in claim 1, is directed to a metal sulfide compound support, characterized in that a metal sulfide compound obtained by reacting hot concentrated sulfuric acid with a metal is supported on diatomaceous earth.
[0007] The invention described in claim 2 is the invention described in claim 1, characterized in that the metal is copper.
[0008] The invention described in claim 3 is a manufacturing method for producing a metal sulfide compound by reacting hot concentrated sulfuric acid with a metal and supporting the metal sulfide compound on diatomaceous earth, and is characterized by having the following steps a and b: A mixing and heating process in which 30 to 70 parts by weight of hot concentrated sulfuric acid, 70 to 30 parts by weight of metal powder, and 5 to 50 parts by weight of diatomaceous earth fine powder are mixed and solidified by heating at a temperature of 190 to 210 ° C for a specified time. b. A crushing step of crushing the solidified material obtained by the mixing and heating step into fine powder particles.
[0009] The invention described in claim 4 is characterized in that, in the invention described in claim 3, the mixing and heating step comprises the following steps α to γ: α. A first mixing step in which 30 to 70 parts by weight of hot concentrated sulfuric acid is mixed with 70 to 30 parts by weight of metal powder. β. A heating step of heating the mixed composition mixed in the first mixing step at a temperature of 180 to 220° C. for a predetermined period of time. γ. A second mixing process in which 5 to 50 parts by weight of diatomaceous earth powder is added while stirring to the mixed composition immediately after heating (in a state in which the metal has precipitated and separated from the liquid) and mixed (mixed and solidified). Effect of the Invention
[0010] The metal sulfide compound support according to claim 1 is stable in a solid state at room temperature and does not undergo a sudden reaction even when it comes into contact with other substances, so that it can be used in large quantities at once and has good handling properties. Furthermore, the remaining sulfuric acid component is easily ionized in a solvent such as water and exhibits high oxidation properties, so that it can be used as a strong oxidizing agent. Furthermore, the properties as an oxidizing agent can be sustained for a long period of time. Therefore, the metal sulfide compound support according to claim 1 can be used in a very wide range of applications, such as raw materials for manufacturing fertilizers, wastewater treatment agents, ion exchange resins, batteries, separators, etc., mineral processing, petroleum refining, and chemical synthesis.
[0011] In addition, the metal sulfide compound support described in claim 1 has the metal reacted with sulfuric acid (hot concentrated sulfuric acid) supported on the diatomaceous earth without impairing the electrical conductivity, and therefore exhibits high electrical conductivity (current flow properties), making it suitable for use as a raw material for conductive materials (conductive resins), etc.
[0012] The metal sulfide compound support according to claim 2 has copper supported on diatomaceous earth, and therefore can exhibit extremely high electrical conductivity (galvanic properties).
[0013] According to the method for producing a metal sulfide compound-supported body as set forth in claim 3, a metal sulfide compound-supported body that has good handleability and can exhibit good oxidation properties over a long period of time can be produced easily and inexpensively.
[0014] According to the method for producing a metal sulfide compound support as described in claim 4, it is possible to produce a metal sulfide compound support that has good handleability and can exhibit good oxidation properties over a long period of time more cheaply and very easily. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] The metal sulfide compound support according to the present invention is characterized in that the metal sulfide compound obtained by reacting hot concentrated sulfuric acid with a metal is supported on diatomaceous earth. Hot concentrated sulfuric acid can be obtained by heating concentrated sulfuric acid at a temperature of 290°C to 300°C for about 20 to 40 minutes. In addition, as the metal to be reacted with hot concentrated sulfuric acid, copper, iron, gold, silver, aluminum, etc. can be used alone or in a mixture of two or more kinds. However, if the main component (80 mass% or more of the total metal) is gold or copper, the conductivity of the metal sulfide compound support is very good, which is preferable. Furthermore, if the main component (80 mass% or more of the total metal) is copper, it is particularly preferable because it can be manufactured inexpensively.
[0016] On the other hand, the diatomite used in the present invention is a sediment (sedimentary rock) made of fossilized shells of diatoms, a type of algae, and is so-called diatomite, which is composed mainly of silicon dioxide (SiO2) (more than 90% by mass of the whole is composed of silicon dioxide). As the diatomite, both those that have been subjected to a calcination treatment and those that have not been subjected to a calcination treatment can be used, but the diatomite is preferably used in the form of a fine powder having an average particle size of 1 to 20 μm, since the conductivity of the metal sulfide compound carrier is very good when calcined at a temperature of 700 to 1,500 ° C., impurities in the micropores are eliminated, and the voids are expanded, thereby increasing the absorbency. In addition, it is also possible to use diatomite that has been calcined together with sodium carbonate. In addition, it is preferable to use diatomite produced in Wakkanai, since it does not lose its porous properties even when pulverized to an average particle size of several μm, and a large amount of metal sulfide compound can be supported with a small amount.
[0017] The metal sulfide compound support according to the present invention can be obtained by a production method including the following steps a and b. A mixing and heating process in which 30 to 70 parts by weight of hot concentrated sulfuric acid, 70 to 30 parts by weight of metal powder, and 5 to 50 parts by weight of diatomaceous earth fine powder are mixed and solidified by heating at a temperature of 190 to 210 ° C for a specified time. b. A crushing process in which the solidified material obtained by the mixing and heating process is crushed into fine powder particles.
[0018] In addition, the mixing ratio of hot concentrated sulfuric acid and metal powder in the mixing and heating step a is preferably 30-70 parts by weight: 70-30 parts by weight, since the oxidizing function of the obtained metal sulfide compound support is more durable, and is particularly preferably 40-60 parts by weight: 60-40 parts by weight. On the other hand, the mixing ratio of metal powder and diatomaceous earth in the mixing and heating step a is preferably 70-30 parts by weight: 5-50 parts by weight, since the pulverization in the pulverization step c is easier, and is particularly preferably 60-40 parts by weight: 7-9 parts by weight.
[0019] The heating temperature in the above-mentioned mixing and heating step a is more preferably 190 to 210° C., since the metal sulfide compound-supported body functions as an oxidizing agent for a longer period of time, and is particularly preferably 195 to 205° C. The heating time required in the mixing and heating step a varies depending on the heating temperature, but when the heating temperature is about 180° C., it is preferably about 45 minutes to 1 hour, and when the heating temperature is 190 to 210° C., it is preferably about 20 minutes to 45 minutes.
[0020] In addition, the pulverization in the above-mentioned pulverization step b is preferably performed so that the average particle size of the solidified material obtained in the mixing and heating step a is 1.0 to 100 μm, since this improves the handleability when the metal sulfide compound support is mixed with other materials (synthetic resins, etc.), and it is more preferable to pulverize to 20 to 50 μm. EXAMPLES
[0021] The metal sulfide compound support and the method for producing the same according to the present invention will be described in detail below with reference to examples and comparative examples, but the metal sulfide compound support and the method for producing the same according to the present invention are not limited to the embodiments of the examples, and can be appropriately modified as necessary without departing from the spirit of the present invention. The methods for evaluating the characteristics in the examples and comparative examples are as follows.
[0022] <Oxidation properties> The metal sulfide compound carrier obtained in each Example and the compound obtained in each Comparative Example were added to 100 g of water (deionized water at room temperature) so as to obtain a predetermined addition ratio (10 mass%), and the mixture was stirred for about 10 seconds and then allowed to stand for about 30 minutes. The acidity of the mixture (precipitate) was then evaluated using litmus paper according to the following three-level scale. ○: Red litmus paper turned blue in less than 3 seconds. △: The red litmus paper turned blue in 3 to 10 seconds. ×: Red litmus paper turned blue in 10 seconds or more, or did not turn blue at all.
[0023] <Oxidation function retention> The metal sulfide compound carrier obtained in each Example and the compound obtained in the Comparative Example were each added to 100 g of water (deionized water at room temperature) to a predetermined addition ratio (10 mass%), stirred for about 10 seconds, and then left for about 30 minutes. Thereafter, the metal sulfide compound carrier or compound precipitated from the mixed solution was removed, and the metal sulfide compound carrier or compound was added to a new 100 g of water (deionized water at room temperature) to a predetermined addition ratio (10 mass%), stirred for about 10 seconds, and then left for about 30 minutes. Furthermore, the above-mentioned series of operations of "removal of the precipitate (metal sulfide compound carrier or compound) from the mixed solution → addition to new 100 g of water (deionized water at room temperature) → stirring and leaving" was repeated once again, and the acidity of the mixed solution (precipitate solution) was evaluated using litmus paper on the following three-level scale. ○: Red litmus paper turned blue in less than 3 seconds. △: The red litmus paper turned blue in 3 to 10 seconds. ×: Red litmus paper turned blue in 10 seconds or more, or did not turn blue at all.
[0024] [Example 1] Hot concentrated sulfuric acid was obtained by heating concentrated sulfuric acid at a temperature of 295°C for about 30 minutes. Then, 30 parts by weight of the hot concentrated sulfuric acid was mixed with 50 parts by weight of copper powder (average particle size = about 30 μm) and thoroughly stirred. Thereafter, the mixed composition was heated at a temperature of 200°C for 30 minutes (hot concentrated sulfuric acid turned red), and 8.0 parts by weight of diatomaceous earth fine powder (calcined at a temperature of 800°C and in the form of a fine powder with an average particle size of 10 μm) was added to the mixed composition immediately after heating and mixed to obtain a solidified product.
[0025] Furthermore, the solidified material (soybean-like coarse granules) was cooled at room temperature and then pulverized using a pulverizer to an average particle size of about 10 μm (particle size distribution: 2 to 30 μm), thereby obtaining a fine powder-shaped metal sulfide compound-supported material of Example 1. The oxidation characteristics and oxidation function retention of the obtained metal sulfide compound-supported material of Example 1 were then evaluated by the above-mentioned method. The evaluation results are shown in Table 1 together with the composition of the metal sulfide compound-supported material, etc.
[0026] [Example 2] 50 parts by weight of hot concentrated sulfuric acid obtained in the same manner as in Example 1 and 50 parts by weight of copper powder (average particle size = about 30 μm) were mixed and thoroughly stirred. Then, the mixed composition was heated at a temperature of 200 ° C for 30 minutes (hot concentrated sulfuric acid turned red), and 20.0 parts by weight of diatomaceous earth fine powder (calcined at a temperature of 800 ° C and in the form of a fine powder with an average particle size of 10 μm) was added to the mixed composition immediately after heating and mixed to obtain a solidified product.
[0027] Furthermore, the solidified material (soybean-like coarse granules) was cooled at room temperature and then pulverized using a pulverizer to an average particle size of about 10 μm (particle size distribution: 2-30 μm) to obtain a fine powder-shaped metal sulfide compound-supported material of Example 2. The oxidation characteristics and oxidation function retention of the obtained metal sulfide compound-supported material of Example 2 were evaluated by the same method as in Example 1. The evaluation results are shown in Table 1 together with the composition of the metal sulfide compound-supported material, etc.
[0028] [Example 3] 50 parts by weight of hot concentrated sulfuric acid obtained in the same manner as in Example 1 and 50 parts by weight of copper powder (average particle size = about 30 μm) were mixed and thoroughly stirred. Then, the mixed composition was heated at a temperature of 200 ° C for 30 minutes (hot concentrated sulfuric acid turned red), and 12.5 parts by weight of diatomaceous earth fine powder (calcined at a temperature of 800 ° C and in the form of a fine powder with an average particle size of 10 μm) was added to the mixed composition immediately after heating and mixed to obtain a solidified product.
[0029] Furthermore, the solidified material (soybean-like coarse granules) was cooled at room temperature and then pulverized using a pulverizer to an average particle size of about 10 μm (particle size distribution: 2-30 μm) to obtain a fine powder-shaped metal sulfide compound-supported material of Example 3. The oxidation characteristics and oxidation function retention of the obtained metal sulfide compound-supported material of Example 3 were evaluated by the same method as in Example 1. The evaluation results are shown in Table 1 together with the composition of the metal sulfide compound-supported material, etc.
[0030] [Example 4] 50 parts by weight of hot concentrated sulfuric acid obtained in the same manner as in Example 1, 50 parts by weight of copper powder, and 12.5 parts by weight of fine powder of diatomaceous earth (the same as in Example 1) were mixed under stirring and heated at a temperature of 200°C for 30 minutes. Thereafter, the obtained solidified material (soybean-like coarse granules) was pulverized in the same manner as in Example 1 to an average particle size of about 10 μm (particle size distribution: 2 to 30 μm) to obtain a fine powder-shaped metal sulfide compound support of Example 4. The oxidation characteristics and oxidation function retention of the obtained metal sulfide compound support of Example 4 were evaluated in the same manner as in Example 1. The evaluation results are shown in Table 1 together with the composition of the metal sulfide compound support.
[0031] [Example 5] A fine powder-shaped metal sulfide compound-supported material of Example 5 was obtained by the same method as in Example 1, except that the metal powder mixed with the hot concentrated sulfuric acid was changed to zinc (average particle size = approximately 30 μm). The oxidation characteristics and oxidation function retention of the obtained metal sulfide compound-supported material of Example 5 were evaluated by the same method as in Example 1. The evaluation results are shown in Table 1 together with the composition of the metal sulfide compound-supported material, etc.
[0032] [Example 6] 40 parts by weight of hot concentrated sulfuric acid obtained in the same manner as in Example 1, 50 parts by weight of copper powder, and 25 parts by weight of fine powder of diatomaceous earth (the same as in Example 1) were mixed under stirring and heated at a temperature of 200°C for 30 minutes. Thereafter, the obtained solidified material (soybean-like coarse granules) was pulverized in the same manner as in Example 1 to an average particle size of about 10 μm (particle size distribution: 2 to 30 μm) to obtain a fine powder-shaped metal sulfide compound support of Example 6. The oxidation characteristics and oxidation function retention of the obtained metal sulfide compound support of Example 6 were evaluated in the same manner as in Example 1. The evaluation results are shown in Table 1 together with the composition of the metal sulfide compound support.
[0033] [Comparative Example 1] 50 parts by weight of hydrochloric acid, 50 parts by weight of copper powder, and 12.5 parts by weight of fine powder of diatomaceous earth (the same as in Example 1) were mixed with stirring and heated at a temperature of 200°C for 30 minutes. Thereafter, the mixed composition was pulverized in the same manner as in Example 1 to an average particle size of about 10 μm (particle size distribution: 2 to 30 μm), thereby obtaining a compound (mixed composition) in the form of fine powder of Comparative Example 1. The oxidizing properties and oxidizing function retention of the obtained compound of Comparative Example 1 were evaluated in the same manner as in Example 1. The evaluation results are shown in Table 1 together with the composition of the compound, etc.
[0034] [Table 1]
[0035] It can be seen from Table 1 that the metal sulfide compound supports of Examples 1 to 6 have good oxidation properties and oxidation function durability. In contrast, the compound of Comparative Example 1 (mixed composition) has poor oxidation properties and oxidation function durability. [Industrial Applicability]
[0036] Since the metal sulfide compound support according to the present invention has the excellent effects as described above, it can be suitably used in a wide range of applications, such as raw materials for producing fertilizers, wastewater treatment agents, ion exchange resins, batteries, separators, etc., mineral processing, petroleum refining, and chemical synthesis.
Claims
1. A metal sulfide compound support comprising a metal sulfide compound supported on diatomaceous earth, the metal sulfide compound being obtained by reacting hot concentrated sulfuric acid with a metal.
2. 2. The metal sulfide compound support according to claim 1, wherein the metal is copper.
3. A method for producing a metal sulfide compound, comprising reacting hot concentrated sulfuric acid with a metal and supporting the resulting metal sulfide compound on diatomaceous earth, comprising: A method for producing a metal sulfide compound, comprising the following steps a and b: a. A mixing and heating process in which 30 to 70 parts by weight of hot concentrated sulfuric acid, 70 to 30 parts by weight of metal powder, and 5 to 50 parts by weight of diatomaceous earth fine powder are mixed and solidified by heating at a temperature of 190 to 210°C for a predetermined period of time. b. A crushing step of crushing the solidified material obtained by the mixing and heating step into fine powder particles.
4. The method for producing a metal sulfide compound according to claim 3, characterized in that the mixing and heating step comprises the following steps α to γ: α. A first mixing step of mixing 30 to 70 parts by weight of hot concentrated sulfuric acid with 70 to 30 parts by weight of metal powder. β. A heating step of heating the mixed composition mixed in the first mixing step at a temperature of 180 to 220° C. for a predetermined time. γ. A second mixing step in which 5 to 50 parts by weight of diatomaceous earth fine powder is added and mixed into the mixed composition immediately after heating while stirring.
Citation Information
Patent Citations
Highly water-absorbing granular fertilizer and method for manufacturing the same
JP2006143509A
Method for producing granular fertilizer
JP2011246288A