Hollow spherical particles
Lignin-sugar complexes form stable, biodegradable, and amphipathic hollow spherical particles that address biocompatibility and environmental concerns, offering controlled drug release and enhanced functionality as drug carriers.
Patent Information
- Application Number
- JP2024135203
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2022-06-08
- Filing Date
- 2024-08-14
- Publication Date
- 2024-12-03
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing hollow spherical particles, such as microcapsules and nanocapsules, face issues with biocompatibility, drug encapsulation, cell penetration, surface charge, control of sustained release, manufacturing cost, and structural stability, while petroleum-based materials pose environmental concerns due to microplastic pollution.
Development of hollow spherical particles formed through self-assembled lignin-sugar complexes with α-ether and γ-ester bonds, which are biodegradable, non-toxic, and amphipathic, allowing for easy preparation and enhanced functionality as drug carriers.
The lignin-sugar complexes provide excellent biocompatibility, biodegradability, and amphipathic properties, enabling controlled drug release, positive and negative surface charges, cell penetration, and stability in various environments, while being safer for the environment.
Smart Images

Figure 2024167239000037 
Figure 2024167239000038 
Figure 2024167239000039
Abstract
Description
[Technical field]
[0001] The present invention relates to hollow spherical particles and the like. [Background technology]
[0002] Hollow spherical particles such as microcapsules and nanocapsules are used in a wide range of industries, including pesticides, detergents, fabric softeners, fragrances, cosmetics, pharmaceuticals, latent heat storage materials (PCM), fibers, paints, and adhesives. By encapsulating molecules such as drugs within the particles, it is expected that the drugs can be acted at the appropriate time in space and time, that the drugs can be protected and dispersed or accumulated appropriately, and that the target object can be protected and weather-resistant by coating. The above capsules are widely used around the world, but the capsule materials derived from petroleum are difficult to recover after being released into the environment, and are the source of microplastics in soil, rivers, and oceans, so the development of natural materials with low environmental impact is a challenge. In the pharmaceutical field, drug carriers (so-called drug delivery systems: DDS) are used, such as liposomes, polymer micelles, and metal particles, but there are issues with biocompatibility, drug encapsulation, cell penetration and delivery, control of surface charge, sustained release, manufacturing costs, and structural stability, and high-function, high-added-value drug carriers that solve these issues are required.
[0003] In addition, hollow spherical particles made of organic polymers derived from living organisms are a good platform for encapsulating or coating a variety of functional substances, such as lipids, polymers, proteins, metal nanoparticles, catalysts, magnetic materials, and carbon materials. Applications are expected in a wide range of fields, including environmental remediation by absorbing harmful substances, removal and detoxification of heavy metals, biosensors using optical properties, catalytic functions, control of magnetic materials, energy storage, high performance capacitors, protective coatings, MRI and fluorescent imaging, etc. In addition, by encapsulating capsules made of biological biomass in matrices such as resins, weight reduction and carbon neutrality are expected.
[0004] There have been reports of nanoparticles that use modified industrial lignin instead of petroleum-derived polymers (Non-Patent Document 1), but there are safety concerns due to the use of organic solvents that are harmful to living organisms in the manufacturing process and the presence of harmful aldehydes and sulfur atoms. [Prior art documents] [Non-patent literature]
[0005] [Non-Patent Document 1] M. Lievonen et al. A simple process for lignin nanoparticle preparation, Green Chem. 2016,18, 1416-1422 (https: / / pubs.rsc.org / en / content / articlelanding / 2016 / gc / c5gc01436k) Summary of the Invention [Problem to be solved by the invention]
[0006] The present invention aims to provide hollow spherical particles which are safer and easier to prepare, and preferably hollow spherical particles which are smaller, more stable, and / or have the various effects described in the Background Art, as well as high functionality and high added value as drug carriers, in order to broaden the fields of application. [Means for solving the problem]
[0007] The present inventors have conducted intensive research in view of the above problems, and have found that the above problems can be solved by hollow spherical particles that are self-assembled bodies of lignin-sugar complexes, the lignin-sugar complexes having at least one bond selected from the group consisting of an α-ether bond between lignin and polysaccharide, an α-ester bond between lignin and polysaccharide, and a γ-ester bond between lignin and polysaccharide. The present inventors have conducted further research based on this finding, and have completed the present invention. That is, the present invention encompasses the following aspects.
[0008] That is, the present invention includes the following aspects. Item 1. A hollow spherical particle that is a self-assembled body of a lignin-sugar complex, the lignin-sugar complex having at least one bond between the lignin and a polysaccharide selected from the group consisting of an α-ether bond, an α-ester bond, and a γ-ester bond.
[0009] Item 2. The hollow spherical particle according to any one of the above items, wherein the composition ratio of polysaccharide to lignin in the lignin-sugar complex (the ratio obtained by dividing the number of monomer units of polysaccharide by the number of monomer units of lignin) is 0.1 to 10.
[0010] Item 2A. An oil-in-water (O / W) type emulsion, double emulsion, vesicle, micelle, capsule, lamellar structure, single-layer / multilayer structure, in which the composition ratio of sugar to lignin in the lignin-sugar complex is 1 to 100% (the percentage of the number of sugar monomer units to the number of lignin monomer units).
[0011] Item 2B. A water-in-oil (W / O) type emulsion, double emulsion, vesicle, reverse micelle, capsule, lamellar structure, single-layer / multilayer structure, in which the ratio of sugar to lignin in the lignin-sugar complex is 100% or more (the percentage of the number of sugar monomer units to the number of lignin monomer units).
[0012] Item 2C. A population of hollow spherical particles made of lignin-sugar complexes having an average particle diameter of 200 nm or more, preferably 250 nm or more, more preferably 300 nm or more, and having a positive average zeta potential at pH=7 and room temperature, according to any one of the preceding items.
[0013] Item 2D. A population of hollow spherical particles made of lignin-sugar complexes having an average particle diameter of less than 200 nm, preferably 150 nm or less, and having a negative average zeta potential at pH=7 and room temperature, according to any one of the preceding items.
[0014] Item 3. The hollow spherical particle according to any one of the above items, wherein the lignin-sugar complex has a molecular weight (Mw) of 800 to 10,000 and a polydispersity (Mw / Mn) of 2.5 or less.
[0015] Item 4. The hollow spherical particles according to any one of the preceding items, having a number average particle size of 1 μm or less.
[0016] Item 5. The hollow spherical particle according to any one of the preceding items, which contains an active ingredient.
[0017] Item 6. The hollow spherical particle according to Item 5, wherein the active ingredient is at least one selected from the group consisting of pigments, agricultural chemicals, fertilizers, medicines, cosmetic ingredients, fragrances, fluorescent agents, paints, proteins, antibodies, nucleic acids, vaccines, lipids, hormones, sugars, glycosides, surfactants, adhesives, vitamins, coenzymes, minerals, cells, organelles, low molecular weight compounds, high molecular weight compounds, metal ions, metal nanoparticles, metal complexes, magnetic materials, liposomes, and hydrogels.
[0018] Item 6A. Self-assembled body that exhibits electron donating properties to metal ions in aqueous solution. A self-assembled body that can donate electrons equivalent to 1 μmol or more per 1 mg of weight to gold(III) ions in aqueous solution.
[0019] Item 7. The hollow spherical particle according to any one of the preceding items, which exhibits long-wavelength fluorescence of 450 nm or more.
[0020] Item 8. A drug delivery or introduction agent comprising the hollow spherical particles according to any one of the preceding items.
[0021] Item 9. The drug delivery or introduction agent according to Item 8, wherein the drug is a nucleic acid.
[0022] Item 10. An ultraviolet absorber containing the hollow spherical particles according to any one of the preceding items.
[0023] Item 11. A light resistance imparting agent comprising the hollow spherical particles according to any one of the above items.
[0024] Item 12. An anti-Stokes fluorescent agent comprising the hollow spherical particle according to any one of the preceding items. Effect of the Invention
[0025] According to the present invention, hollow spherical particles that are excellent in biocompatibility, biodegradability, nontoxicity, and amphiphilicity and can be prepared more easily can be provided. Also, according to the present invention, it is possible to provide a particle that can coat a target object or encapsulate and disperse a drug, and provide sustained release that acts at a suitable timing in terms of space and time, positive and negative surface charges, cell penetration and delivery, stability in water and in a vacuum, light resistance, ultraviolet absorption, and selective identification by fluorescent absorption. [Brief description of the drawings]
[0026] [Figure 1-1] 1 is a diagram showing a flow chart of the M-APA method. [Figure 1-2] 1 is a diagram showing a flow chart of the A-APA method. [Diagram 2] This is a diagram showing the microwave irradiation conditions, power, temperature, pressure profile, and specifications of the equipment involved in the separation of lignocellulosic components: Biotage Initiator+ 60 microwave synthesis equipment, stirring speed: 600 rpm, Cooling: On, Absorption: High conditions. [Diagram 3] This is a 2D NMR spectrum of a low-denaturation, high-purity, high-ether content lignin. This is the analysis result of lignin isolated by the M-APA method (microwave treatment at 50℃ for 10 minutes, acetic acid / peracetic acid 1% condition) using eucalyptus as the starting material. [Figure 4] 1 is a drawing showing partial chemical structures of bonds between lignin units and covalent bonds between lignin and hemicellulose. [Diagram 5]The 2D NMR spectrum of the lignin-hemicellulose complex (a,b) and the enlarged views of the interunit bonds and sugar regions (a'-d') are shown. The lignin-hemicellulose complexes obtained by the M-APA method from hardwood (a,b) and softwood (c,d) were analyzed. The circles in the figure indicate LC bonds (ether and ester types). [Figure 6] Synchrofluorescence spectrum of bagasse (sugar cane)-derived APA lignin in the near-infrared wavelength region. This is the result of synchroscan measurement to detect a certain Stokes shift, i.e., detection of fluorescence wavelengths Em that are 80, 90, 150, 160, and 170 nm longer than the excitation wavelength Ex (scanning the excitation wavelength). [Figure 7] The 3D fluorescence spectrum of APA lignin in the near infrared wavelength region is shown. APA lignin obtained by treating APA lignin from Japanese red pine wood flour using the M-APA method (microwave 50℃, 10 min acetic acid + 0.2M hydrogen peroxide conditions) was measured in an 80% acetonitrile solution (concentration 0.1 wt%). [Figure 8] The UV-visible absorption spectra of reagent lignin (Tokyo Kasei TCI alkaline lignin, blue line) and lignin (APA lignin, red line) are shown. [Figure 9] Synchro antifluorescence spectra of lignin solid thin film and lignin-sugar complex solid thin film are shown. The excitation wavelength was scanned to selectively detect anti-Stokes shifted fluorescence shorter than the excitation wavelength, as shown in the antifluorescence spectra (af) and control (g). The anti-Stokes shift is the excitation wavelength minus 50 nm, while spectrum (b) is minus 40 nm. Comparing spectra (b) and (d) and (e) and (f), it is clear that the antifluorescence intensity is higher when peracetic acid is used as an oxidizing agent than when hydrogen peroxide is used. Comparing spectra (b) and (c), it is clear that the antifluorescence intensity of APA lignin is higher than that of lignin-sugar complex. [Figure 10] The ultraviolet absorption spectra of lignin and lignin-hemicellulose complexes are shown. The vertical axis indicates absorbance, and the horizontal axis indicates wavelength (nm). For an explanation of the legend, see Table 7. [Figure 11-1] 1 shows a bright field image of the hollow spherical particles obtained in Reference Test Example 5. [Figure 11-2] 1 shows scanning electron microscope (SEM) photographs of the lignin capsules (a, b) and the lignin-sugar complex capsules (c) obtained in Example 1. [Figure 12-1] 1 shows a fluorescent image of the hollow spherical particles obtained in Reference Test Example 6. [Figure 12-2] The following are micrographs of the lignin-sugar complex capsules encapsulating the fluorescent dye DAPI obtained in Example 1. These are fluorescent micrographs (A1, A2), bright-field micrographs (B1, B2), and SEM images (C1, C2, C3, C4). The fluorescent micrographs show the drug encapsulation. The SEM images show that the hollow spherical particles do not collapse even in a vacuum and can maintain their shape, i.e., the stability of the particle structure. [Figure 13] This shows the relative values of the average particle size of the hollow spherical particles obtained in Example 2. The horizontal axis shows the time elapsed from immediately after the preparation of the hollow spherical particles. [Figure 14] This shows the relative value of the average particle size of the hollow spherical particles obtained in Example 2. The horizontal axis shows the temperature during heating and stirring. [Figure 15] FIG. 1 shows the particle size and zeta potential distribution of eucalyptus lignin capsules (LP, top) and eucalyptus lignin-sugar complex capsules (LHP, bottom) (Example 1). [Figure 16] The 3D fluorescence spectrum of the lignin-sugar complex capsules is shown. The vertical axis is the excitation wavelength (nm) and the horizontal axis is the fluorescence wavelength (nm). [Figure 17] 1 shows the ultraviolet-visible absorption spectrum of the reaction solution (Reference Test Example 3). [Figure 18] The pore passing time and size plot of sub-microparticles obtained by electrical resistance nanopulse method (electrical resistance nanopulse method (qNANO)) are shown (Example 5-2-1). [Figure 19] SPM image results (left) 10.00 μm×10.00 μm analysis results (right) 2.50 μm×2.50 μm analysis results are shown (Example 5-2-2). [Figure 20] SPM 3D solid shape analysis (left) and image analysis (right) show the results of 3D shape analysis (Example 5-2-2). [Figure 21]The results of SPM physical property analysis (left), shape analysis (center), adsorptive force analysis (right), and hardness analysis are shown (Example 5-2-2). [Figure 22] 1 shows the results of 3D real surface view microscopic observation of lignin-sugar complex microparticles (LCC lignin microparticles) (Example 5-2-2). [Figure 23] 1 shows image data of LCC nanoparticles obtained by an interference light microscope (Example 5-2-2). [Figure 24] 1 shows a particle size histogram of LCC nanoparticles by an interference light microscope (Example 5-2-2). [Diagram 25] 4 shows the particle size evaluation results of LCC nanoparticles by DLS (Example 5-2-2). [Figure 26] The results of measuring the zeta potential of lignin microparticles at pH 3 using an electrical resistance nanopulse method (electrical resistance nanopulse method (qNANO)) are shown (Example 5-2-3-1). [Figure 27] The results of measuring the zeta potential of lignin microparticles at pH 5 using an electrical resistance nanopulse method (qNANO) are shown (Example 5-2-3-1). [Figure 28] The results of zeta potential measurement of lignin microparticles at pH 7 using an electrical resistance nanopulse method (qNANO) are shown (Example 5-2-3-1). [Figure 29] The results of measuring the zeta potential of lignin microparticles at pH 9 using an electrical resistance nanopulse method (qNANO) are shown (Example 5-2-3-1). [Diagram 30] The results of zeta potential measurement of p11 lignin microparticles using electrical resistance nanopulse method (qNANO) are shown (Example 5-2-3-1). [Diagram 31] The results of zeta potential measurement of LCC lignin microparticles at pH 3 using an electrical resistance nanopulse method (qNANO) are shown (Example 5-2-3-1). [Diagram 32] The results of zeta potential measurement of LCC lignin microparticles at pH 5 using an electrical resistance nanopulse method (qNANO) are shown (Example 5-2-3-1). [Diagram 33]The results of zeta potential measurement of LCC lignin microparticles at pH 7 using an electrical resistance nanopulse method (qNANO) are shown (Example 5-2-3-1). [Diagram 34] The results of zeta potential measurement of LCC lignin microparticles at pH 9 using an electrical resistance nanopulse method (qNANO) are shown (Example 5-2-3-1). [Diagram 35] The results of zeta potential measurement of pH 11 LCC lignin microparticles using electrical resistance nanopulse method (qNANO) are shown (Example 5-2-3-1). [Diagram 36] The results of measuring the 3D fluorescence excitation spectrum of LCC lignin microparticles are shown (Example 5-2-4). [Figure 37] The results of measuring the 3D fluorescence excitation spectrum of eosin-complexed LCC lignin microparticles are shown (Example 5-2-4). [Figure 38] The particle size evaluation results of diethyl sebacate composite fine particles using DLS are shown (Example 5-2-5). [Figure 39] The results of measuring the fluorescence excitation spectrum of diethyl sebacate composite fine particles are shown (Example 5-2-5). [Diagram 40] 1 shows a photograph of water-in-1-butanol (W / O) type lignin-sugar complex hollow spherical particles (Test Example X). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0027] In this specification, the expressions "contain" and "comprise" include the concepts of "contain", "include", "consist essentially of" and "consist only of".
[0028] In one aspect, the present invention relates to a hollow spherical particle (sometimes referred to as "the hollow spherical particle of the present invention" or "self-assembled body" in the present specification) which is a self-assembled body of a lignin-sugar complex (sometimes referred to as "the lignin-sugar complex of the present invention" in the present specification), the lignin-sugar complex having at least one bond selected from the group consisting of an α-ether bond between lignin and a polysaccharide, an α-ester bond between lignin and a polysaccharide, and a γ-ester bond between lignin and a polysaccharide. The sugar in the lignin-sugar complex in the present specification is derived from a polysaccharide and contains at least one monomer unit as a sugar. This will be explained below.
[0029] 1. Method for isolating lignin-sugar complexes The lignin-sugar complex of the present invention can be obtained by (A) a method for isolating lignin from plant biomass, which includes a step of contacting a solution containing an organic acid and a peracid with the plant biomass (also referred to as the "isolation method of the present invention" in this specification). This will be described below.
[0030] The isolation method of the present invention includes step (A), and therefore can obtain a high-quality (low-condensation) lignin / polysaccharide complex having a high content of β-O-4 ether structures among all the bond types between monolignols.
[0031] The plant biomass is not particularly limited as long as it contains a lignin-sugar complex, and examples thereof include the plant itself and mechanically processed products of the plant.
[0032] Examples of plant bodies include coniferous trees, hardwoods, and non-woody materials. Specific examples of plant bodies include Japanese cedar, pine, spruce, larch, black pine, Abies sachalinensis, Himekomatsu, yew, Japanese yew, fir, Japanese spruce, Japanese yew, Japanese yew, Japanese bead, fir, Japanese cedar, Japanese cedar, Japanese cedar, Japanese cedar, Japanese cedar, Japanese cedar, Japanese cedar, Japanese cedar, Japanese cedar, Japanese cedar, Japanese cedar, Japanese cedar, Japanese cedar, Japanese cedar, Japanese cedar, Japanese cedar, Japanese cedar, Japanese spruce, yellow cedar, Lawson cypress, Douglas fir, Sitka spruce, Radiata pine, Eastern spruce, Eastern white pine, Western larch, Western fir, Western Examples of suitable wood materials include coniferous woods such as hemlock and tamarack; hardwoods such as asbestos, American black cherry, yellow poplar, walnut, birch, zelkova, sycamore, silver cherry, ash, teak, Chinese elm, Chinese maple, oak, beech, hard maple, hickory, pecan, white ash, white oak, white birch, red oak, acacia, and eucalyptus; and non-woody materials such as rice, sugar cane, wheat, corn, pineapple, oil palm, kenaf, cotton, alfalfa, timothy, bamboo, bamboo grass, bamboo, and sugar beet.
[0033] Examples of mechanically processed products of plants include logs, timber, planks, solid wood, wood materials, laminated lumber, laminated veneer lumber, plywood, wood boards, particle boards, fiberboards, wood chips, particulate wood (chips, particles, wood flour, etc.), fibrous wood, compressed materials, crushed materials, etc.
[0034] From the viewpoint of improving the yield, the plant biomass is preferably wood flour. The volume average particle size of the wood flour is, for example, 500 μm or less, preferably 200 μm or less, more preferably 100 μm or less, even more preferably 50 μm or less, and even more preferably 20 μm or less. The lower limit of the average particle size is not particularly limited, and can be, for example, 1 μm, 2 μm, or 5 μm. By using wood flour with a relatively small particle size, a high yield can be achieved without carrying out the following alkali treatment.
[0035] Wood flour can be obtained by pulverizing plant biomass. The pulverization can be carried out according to or in accordance with a known method, for example, using various mills (e.g., ball mill, mixer mill, etc.).
[0036] From the viewpoint of improving the yield, the plant biomass is preferably an alkali-treated product of a plant body or a mechanically processed product thereof. According to the present invention, by using the alkali-treated product, the target product can be obtained efficiently without pulverization (even in the case of a wood chip having a relatively large specific surface area). The alkali-treated product can be obtained by alkali-treating a plant body or a mechanically processed product thereof. The alkali treatment causes loosening of the plant cell wall structure (reduction of intermolecular interactions and cleavage of hydrogen bonds) and also cleaves ester bonds in the molecule, thereby improving the yield. This makes it possible to achieve a high yield without or to a low degree of physical pulverization of the plant biomass, thereby reducing process costs. Furthermore, the yield can be improved by 1.2 to 2 times. In addition, the crystallinity of the cellulose fiber obtained through this alkali treatment does not show a significant decrease in crystallinity due to the fine pulverization treatment, and a clear cellulose Iβ structure is maintained.
[0037] Specifically, the alkali treatment is, for example, (X) A step of contacting a plant body or a mechanically processed product thereof with an alkaline solution. It is preferable that:
[0038] The alkaline solution is not particularly limited as long as it is an alkaline solution to the extent that the above-mentioned object can be achieved. For example, the alkaline solution may be a solution having a pH of 12 to 15. The pH of the solution is preferably 13 to 14. The alkaline solution may be a solution containing, for example, 0.3 to 2 mass % (preferably 0.7 to 1.5 mass %) of an alkali metal hydroxide (e.g., sodium hydroxide, potassium hydroxide, etc.).
[0039] The amount of the alkaline solution used is not particularly limited as long as the alkaline solution is sufficient to achieve the above-mentioned purpose. The amount of the alkaline solution may be, for example, 3 to 20 mL, preferably 5 to 12 mL, per 1 g of the plant body or mechanically processed product thereof.
[0040] The manner in which the plant body or a mechanically processed product thereof is brought into contact with the alkaline solution is not particularly limited. From the standpoint of treatment efficiency and the like, it is preferable to immerse the plant body or a mechanically processed product thereof in the alkaline solution.
[0041] The temperature of the alkaline solution is not particularly limited as long as it is a temperature at which the above-mentioned object can be achieved. The temperature of the alkaline solution can be, for example, 20 to 150° C., preferably 50 to 120° C., and more preferably 80 to 120° C. When heating, the method includes, for example, an internal heating method using microwave heating, an external heating method using an oil bath, etc., and the like, and the internal heating method using microwave heating is preferred.
[0042] The treatment time in step (X) is not particularly limited as long as it is a time that can achieve the above-mentioned object, and is, for example, 5 to 120 minutes, preferably 15 to 60 minutes.
[0043] After step (X), the soluble portion and the insoluble portion are separated, and the insoluble portion can be subjected to step (A) as an alkali-treated product of the plant body or a mechanically processed product thereof.
[0044] The plant biomass may be of one type alone or of two or more types in combination.
[0045] The solution containing an organic acid and a peracid (organic acid-peracid solution) is a solution that contains an organic acid and a peracid and is capable of extracting and solubilizing at least one selected from the group consisting of lignin, hemicellulose, and lignin-sugar complexes, and is not particularly limited in this respect.
[0046] The organic acid is not particularly limited, and examples thereof include acetic acid, formic acid, glyoxylic acid, maleic acid, propionic acid, folic acid, isobutyric acid, valeric acid, isovaleric acid, pyruvic acid, oxalic acid, malonic acid, succinic acid, glutaric acid, ketoglutaric acid, adipic acid, lactic acid, tartaric acid, fumaric acid, oxaloacetic acid, malic acid, isocitrate, citric acid, benzoic acid, phthalic acid, isophthalic acid, terephthalic acid, hemimellitic acid, trimellitic acid, trimesic acid, mellophanic acid, prenitic acid, pyromellitic acid, mellitic acid, methanesulfonic acid, benzenesulfonic acid, p-toluenesulfonic acid, camphorsulfonic acid, p-toluenesulfinic acid, and benzenesulfinic acid. Of these, preferred are acetic acid, formic acid, glyoxylic acid, 3-oxopropanoic acid, 2-methyl-3-oxopropanoic acid, etc., more preferred are acetic acid, formic acid, glyoxylic acid, etc., and particularly preferred is acetic acid.
[0047] The organic acid may be one kind alone or two or more kinds in combination.
[0048] The peracid is not particularly limited as long as it is an acid having a hydroperoxide group (-O-OH), and examples thereof include organic peroxoacids such as percarboxylic acid, persulfuric acid, percarbonic acid, perphosphoric acid, and hypoperhalogen acid. Examples of percarboxylic acid include peracetic acid, performic acid, perbenzoic acid, and metachloroperbenzoic acid, and examples of hypoperhalogen acid include hypoperchloric acid, hypoperbromic acid, and hypoperiodic acid. In addition to the above, examples of peracids include hydrogen peroxide, lithium peroxide, sodium peroxide, potassium peroxide, sodium percarbonate, urea peroxide, sodium perborate, tert-butyl hydroperoxide, cumene hydroperoxide, di-tert-butyl peroxide, dimethyl dioxirane, acetone peroxide, methyl ethyl ketone peroxide, and hexamethylene triperoxide diamine. Among these, preferred are organic peroxyacids, hydrogen peroxide, sodium percarbonate, urea peroxide, sodium perborate, etc., more preferred are percarboxylic acids (particularly peracetic acid), hydrogen peroxide, etc., and particularly preferred is hydroperoxy acid.
[0049] The peracid may be a single type or a combination of two or more types.
[0050] The content of the organic acid in the organic acid-peracid solution is, for example, 5 to 30 mol / L, preferably 8 to 25 mol / L, and more preferably 10 to 20 mol / L. The content of the organic acid in the organic acid-peracid solution is preferably 3 to 10 g, more preferably 4 to 8 g, and even more preferably 5 to 7 g per 1 g of plant biomass to be contacted with the organic acid-peracid solution.
[0051] The content of peracid in the organic acid-peracid solution is, for example, 0.05 to 3 mol / L, preferably 0.08 to 2.5 mol / L, and more preferably 0.1 to 2 mol / L. The content of peracid in the organic acid-peracid solution is preferably 0.03 to 0.1 g, more preferably 0.04 to 0.08 g, and even more preferably 0.05 to 0.07 g per 1 g of plant biomass to be contacted with the organic acid-peracid solution.
[0052] The manner in which the plant biomass is contacted with the organic acid-peracid solution is not particularly limited, but from the standpoint of treatment efficiency and the like, it is preferable to immerse the plant biomass in the organic acid-peracid solution.
[0053] The temperature of the organic acid-peracid solution is not particularly limited as long as it is a temperature at which the lignin-sugar complex can be extracted and solubilized. The temperature of the organic acid-peracid solution is, for example, 60 to 160°C. By using such a temperature, a high-quality (low-condensation) lignin-polysaccharide complex having a high content of β-O-4 type ether structure among all the bond types between monolignols can be obtained. In step (A), a lignin-polysaccharide complex tends to be obtained when the treatment is performed at a high temperature, and a lignin unit tends to be obtained when the treatment is performed at a low temperature. For example, when the starting material is woody biomass, step (A) is performed with an organic acid-peracid solution at 90° C. or less (preferably 40 to 90° C., more preferably 40 to 70° C., and even more preferably 40 to 60° C.), lignin alone is easily obtained selectively, and when step (A) is performed with an organic acid-peracid solution at more than 90° C. and less than 160° C. (preferably 100 to 160° C., more preferably 120 to 160° C.), a complex of lignin and polysaccharide is easily obtained. For example, when the starting material is herbaceous biomass, step (A) is performed with an organic acid-peracid solution at 60° C. or less (preferably 15 to 60° C.), lignin alone is easily obtained selectively, and when step (A) is performed with an organic acid-peracid solution at more than 60° C. and less than 150° C. (preferably 70 to 150° C.), a complex of lignin and polysaccharide is easily obtained. When heating is performed, examples of the method include an internal heating method using microwave heating and an external heating method using an oil bath or the like, and the internal heating method using microwave heating is preferred. Rapid internal heating using microwaves enables efficient pretreatment in a short time.
[0054] The treatment time in step (A) is not particularly limited as long as it is a time that can achieve the above-mentioned object, and is, for example, 1 to 60 minutes, preferably 1 to 30 minutes, and more preferably 5 to 20 minutes.
[0055] In step (A), it is preferable to perform microwave treatment while the biomass is immersed in the solution. This improves the yield of lignin. The conditions of the microwave treatment can be appropriately set, but for example, a commercially available microwave synthesis device can be used to perform the treatment while stirring the solution. The microwave treatment time can be, for example, 1 to 30 minutes, and is preferably about 10 minutes. When microwave treatment is performed in the isolation method of the present invention, irradiation for a relatively short period of time is sufficient, so that it is easy to construct a continuous system in addition to a batch system.
[0056] In step (A), it is preferable to irradiate the plant biomass with microwaves or ultrasound, from the viewpoint of promoting the penetration of the solution into the pores inside the plant cell walls and improving the yield. The irradiation time is the same as above.
[0057] Step (A) may be carried out in a plurality of stages while changing conditions as necessary. For example, it may be carried out while changing the temperature of the solution. In this case, it is preferable that the temperature of the solution is higher in a particular stage than in the next stage. For example, step (A) may include (A1) a step of contacting a plant biomass with a solution containing an organic acid and a peracid at 90° C. or less, and / or (A2) a step of contacting a plant biomass with a solution containing an organic acid and a peracid at a temperature higher than 90° C. and not higher than 160° C. Note that the "plant biomass" in step (A2) includes the insoluble portion obtained in step (A1).
[0058] Lignin alone can be selectively extracted and solubilized in step (A1), and lignin-sugar complexes can be extracted and solubilized in step (A2). Therefore, by carrying out steps (A1) and (A2) in this order, lignin alone and lignin-sugar complexes can be efficiently obtained.
[0059] After step (A), a separation solvent is added as necessary, and then the soluble and insoluble parts are separated. The method for separating the soluble and insoluble parts is not particularly limited, and methods such as decantation, spin-down, and filtration can be adopted. As the separation solvent, lignin and lignin-hemicellulose complex are isolated using various alcohols such as dioxane, ethanol, acetone, acetonitrile, DMSO, DMF, NMI, ethyl acetate, methanol, and butanol, acetic acid, water, and mixed solvents thereof. From the viewpoints of extraction efficiency, selectivity, and environmental load, organic solvents such as acetone, ethanol, and acetonitrile and 10 to 20 v / v% water-mixed organic solvents are preferable.
[0060] In addition, if an extraction solvent (acetic acid-peracetic acid) or separation solvent that does not contain water is used, a highly pure lignin-hemicellulose complex can be obtained. If a water-containing solvent is used, some of the hemicellulose component, which is a polysaccharide, is also obtained at the same time. A catalyst that promotes the hydrolysis reaction in the presence of an acid or alkali can also be used.
[0061] The soluble portion obtained in step (A) contains a lignin-sugar complex. Therefore, the soluble portion can be obtained as the lignin-sugar complex as it is or after other treatments as necessary.
[0062] Other treatments include the following. After step (A), if necessary, the water can be removed by evaporation and / or freeze-drying to obtain the target substance as a dry powder. If desalting is required, the concentrated solution may be extracted with alcohol or acetone, and the solvent may be distilled off. This allows the target substance to be obtained as a dry powder.
[0063] In the case of selectively obtaining a lignin-sugar complex, for example, the lignin-sugar complex can be obtained from the soluble portion obtained in step (A2) by using the insoluble portion obtained in step (A1) as plant biomass.
[0064] According to the present invention, a new method for pretreatment of plant biomass can be provided as a new paper pulp production process that requires low energy and does not produce hazardous waste liquid, is a low-temperature, mild process that cleanly delignifies polysaccharides, and therefore contains fewer inhibitors in the recovered material that are problematic in ethanol fermentation.
[0065] 2. Lignin-sugar complex According to the isolation method of the present invention, it is possible to obtain a lignin-sugar complex having at least one bond selected from the group consisting of an α-ether bond between lignin and a polysaccharide, an α-ester bond between lignin and a polysaccharide, and a γ-ester bond between lignin and a polysaccharide.
[0066] <2-1. Lignin> The lignin of the present invention refers to lignin isolated from biomass (including natural lignin). The bonding patterns of natural lignin are diverse. Representative bonding patterns of natural lignin include the following.
[0067] [ka] The above is called the β-O-4 bond.
[0068] [ka] The above is called resinol (β-β) bond.
[0069] [ka] The above is called a phenylcoumaran (β-5) bond.
[0070] [ka] The above is called a 5-5 bond.
[0071] [ka] The above is called Dibenzodioxin (DBDO 5-5 / 4-O-β) bond.
[0072] [ka] The above is called a 4-O-5 bond.
[0073] [ka] The above is called β-1 bond.
[0074] [ka] The above is called a spirodienone bond.
[0075] In natural lignin, the content of β-O-4 type ether structure is the highest among all bond types between monolignols, although it varies depending on the plant species. For example, the content is said to be 40 to 60% in coniferous trees. In broad-leaved trees, such as eucalyptus, the content is said to be about 45%.
[0076] The lignin of the present invention has a β-O-4 ether structure content of 50% or more, preferably 60% or more, more preferably 65 to 85%, and even more preferably 70 to 80% of all bonding patterns between monolignols.
[0077] The lignin of the present invention has a content (%) of β-O-4 ether structures among all bond types between monolignols, where the content of the lignin contained in the raw biomass is x%, preferably 1.2x% or more, more preferably 1.4x% or more, and even more preferably 1.6x% or more. In the above, the upper limit is preferably 2x%.
[0078] The content of β-O-4 type ether structure among all the bond types between monolignols in lignin is specifically measured as follows. The sample is dissolved in deuterated dimethyl sulfoxide (DMSO-d6) to a concentration of 1-10 wt%, and an NMR spectrum is obtained using a Bruker Avance III 600 MHz NMR device equipped with a cryogenic probe. The content of β-O-4 type ether structure can be estimated from the signal volume on the HSQC (Heteronuclear single-quantum correlation spectroscopy) spectrum. The quantitative value in the two-dimensional NMR method is corrected according to the literature (H. Okamura, H. Nishimura, T. Nagata, T. Kigawa, T. Watanabe and M. Katahira, Accurate and molecular-size-tolerant NMR quantitation of diverse components in solution, Scientific Reports, 6, 21742. 2016) to calculate the accurate content.
[0079] The lignin of the present invention preferably has a composition ratio of biphenyl-type lignin, which is a condensed structure, of 5% or less.
[0080] The lignin of the present invention has a number average molecular weight (Mn) of preferably 0.7 to 9 kDa, more preferably 1 to 5 kDa, and further preferably 1.5 to 4 kDa.
[0081] The lignin of the present invention has a weight average molecular weight (Mw) of preferably 0.8 to 10 kDa, more preferably 1.5 to 8 kDa, and further preferably 2 to 6 kDa.
[0082] In the present invention, the number average molecular weight (Mn) and weight average molecular weight (Mw) of lignin are specifically measured as follows. The molecular weight of lignin can be determined by size exclusion chromatography (SEC), also known as gel permeation chromatography (GPC). The sample is dissolved in a solution of acetic anhydride and a base (such as pyridine) and reacted for 3-6 hours to obtain an acetylated product. This is dissolved in tetrahydrofuran (THF) at a concentration of 2.0 mg / mL and separated by high performance liquid chromatography. The column used is an HZ-M column (Tosoh, 150 mm x 4.6 mm id, 4 μm, three columns connected in series). The analysis is performed by injecting 10 μL of sample, at a column temperature of 40° C., with tetrahydrofuran (THF) as the mobile phase, and at a flow rate of 0.35 mL / min. A mass calibration curve is constructed using standard polystyrene, Tosoh PStQuickC (molecular weight (MW) of 2,110,000, 427,000, 37,900, and 5,970), pinoresinol (MW 352), and vanillin (MW 152) to determine the Mw and Mn of the samples.
[0083] The lignin of the present invention preferably has a polydispersity (Mw / Mn) of 2.5 or less, more preferably 2 or less.
[0084] <2-2. Lignin-sugar complex> The lignin-sugar complex of the present invention refers to a lignin-sugar complex in a state isolated from biomass.
[0085] Polysaccharides include, for example, xylan and mannan, and include glucomannan, galactoglucomannan, glucuronoxylan, and arabinoglucuronoxylan. Hemicellulose is mainly composed of glucomannan in conifers, glucuronoxylan in broad-leaved trees, and arabinoxylan in herbaceous plants. The monomers in the above are xylose, arabinose, glucose, mannose, galactose, and uronic acid. The side chains also contain acetyl and methoxy groups. Hemicellulose in herbaceous plants includes ferulic acid and diferulic acid bound to the arabinose side chain of arabinoxylan.
[0086] The lignin-sugar complex of the present invention is a lignin-sugar complex that can be uniformly dispersed in a separation solvent and is characterized by a polymer structure in which lignin and polysaccharides are copolymerized by covalent bonds. The lignin-sugar complex of the present invention is isolated by cleaving a very small portion (10% or less of the bonds) of the bonds in the hemicellulose main chain of the lignin-sugar complex structure in the plant cell wall through a hydrolysis reaction. By carrying out the hydrolysis reaction under mild conditions, it is possible to suppress overdecomposition, side reactions, and degradation to smaller molecules.
[0087] The lignin-sugar complex of the present invention is characterized by having at least one bond selected from the group consisting of an α-ether bond between lignin and a polysaccharide (LC α-ether bond), an α-ester bond between lignin and a polysaccharide (LC α-ester bond), and a γ-ester bond between lignin and a polysaccharide (LC γ-ester bond).
[0088] In the lignin-saccharide complex of the present invention, the α-ether bond (LC α-ether), which is the copolymerization point between the lignin and the polysaccharide, is preferably concentrated to 1.2 times or more the original bond unit composition ratio of the raw material biomass.
[0089] In biomass, lignin and polysaccharides are also bound by non-covalent bonds. Non-covalent bonds are due to hydrophobic interactions, hydrogen bonds, electrostatic interactions, and entanglement of polymer chains. For this reason, previous studies have not shown clear evidence that lignin and polysaccharides, which are polymers with different properties, form a copolymer complex through covalent bonds in lignin-sugar complexes. In addition, conventional methods for preparing lignin-sugar complexes involve multiple steps, resulting in low yields (less than 5%) and low purity.
[0090] Clear evidence of copolymerization points (covalent bonds) in lignin-hemicellulose copolymers can be confirmed by signal assignment using HSQC, a two-dimensional NMR method (Figures 3 and 4). Further clear evidence can be confirmed by continuous correlation analysis using HMBC and TOCSY-HSQC methods. For more details, please refer to the literature (Nishimura et al., Direct evidence for α ether linkage between lignin and carbohydrates in wood cell walls, Sci Rep 2018) (Nishimura et al., Direct evidence of α ester linkages between lignin and glucuronoxylan that reveal the robust heteropolymeric complex in plant cell walls, Research Square https: / / doi.org / 10.21203 / rs.3.rs-1327348 / v1).
[0091] LCα Ether The C−H correlation signals at the α-position of lignin (LC ether, δH / δC=4.50 ±0.15 ppm / 80.1 ±1 ppm region) originate from the ether bond between the hydroxyl group at the 6th position of a hexose or the 5th position of a pentose (e.g., the 6th position of mannose, glucose, galactose and the 5th position of arabinose) and the α-position (benzyl position) of lignin, and the C−H correlation signals at the 2nd or 3rd position of a hexose or pentose (e.g., the 2nd and 3rd positions of xylose, mannose, glucose, galactose, and arabinose) (LC ether, δH / δC=4.95 ±0.2 ppm / 81.5 ±1.5 ppm region).
[0092] LC α Ester C-H correlation signal at the α-position of lignin (LC α ester, δH / δC=5.88 ±0.15 ppm / 74.0 ±1.5 ppm region) originating from an ester bond between the carboxyl group at the 6-position of glucuronic acid (uronic acid) and the α-position (benzyl position) of lignin.
[0093] LC gamma ester C-H correlation signal at the γ-position of lignin (LC γester, δH / δC=4.0 ±0.15 ppm, 4.4 ±0.15 ppm, / 64.8 ±1.5 ppm region) derived from the ester bond between the carboxyl group at the 6-position of glucuronic acid (uronic acid) and the γ-position of lignin.
[0094] The lignin-sugar complex of the present invention has a characteristic that its solubility in 60 to 80% ethanol (e.g., 60% or 80%) at 25°C is 2 w / v% or more. Therefore, by using the lignin-sugar complex of the present invention, hollow spherical particles described below can be easily obtained without using a solvent harmful to the living body, and hollow spherical particles with high stability can be obtained. The solubility is preferably 4 w / v% or more, more preferably 5 w / v% or more, even more preferably 6 w / v% or more, and even more preferably 7 w / v% or more. The upper limit of the solubility is not particularly limited and can be, for example, 40 w / v%, 30 w / v%, or 25 w / v%.
[0095] The solubility is measured as follows. After stirring and dissolving the sample in 25°C ethanol, the sample is separated into an ethanol-soluble portion and an ethanol-insoluble portion by solid-liquid separation. A 25°C aqueous ethanol solution (1 / 1 = ethanol / water) is added to the ethanol-insoluble portion, which is stirred to dissolve, to obtain an aqueous ethanol soluble portion. The aqueous ethanol soluble portion is mixed with the ethanol soluble portion to obtain a sample solution. The amount of aqueous ethanol added is adjusted so that the ethanol concentration of the sample solution is in the range of 60 to 80%. In the process of obtaining the soluble portion, the sample is dispersed and solubilized by ultrasonic irradiation as necessary. The maximum sample concentration at which the sample solution becomes visually transparent is defined as the "solubility in 60 to 80% ethanol at 25°C".
[0096] In the lignin-sugar complex of the present invention, the composition ratio of sugar to lignin is preferably 0.01-10.
[0097] The lignin-sugar complex of the present invention has a weight average molecular weight (Mw) of preferably 800 to 15,000, more preferably 2,000 to 10,000, and even more preferably 3,000 to 7,000. The lignin-sugar complex of the present invention has a polydispersity (Mw / Mn) of preferably 3.5 or less, more preferably 2.5 or less.
[0098] The method for measuring each of the above parameters is in accordance with the measurement method for lignin of the present invention or the measurement method in the Examples described below.
[0099] 3.Hollow spherical particles The hollow spherical particles of the present invention are not particularly limited as long as they are self-assembled bodies of the lignin-sugar complexes of the present invention and have a hollow spherical shape. Self-assembly occurs easily, and the conditions for self-assembly can be appropriately set. For example, the lignin-sugar complexes of the present invention can be self-assembled in an aqueous solution in which they are dispersed to form hollow spherical particles.
[0100] Specifically, hollow spherical particles can be formed by gradually adding water to a sample dissolved in an organic solvent (such as alcohol) to induce self-assembly. The final water content is about 95%, but once capsules are formed, they become stable in water. Alternatively, capsules can be formed by dissolving a sample in alcohol-containing water and allowing it to evaporate naturally. This allows the formation of capsules with high uniformity on the submicron order.
[0101] Conventional lignin (commercially available industrial kraft lignin) does not exhibit dispersibility or solubility in hydrophilic solvents such as ethanol and water-mixed solvents. The lignin-sugar complex of the present invention exhibits dispersibility and solubility in hydrophilic solvents and water-mixed solvents. Therefore, by using the lignin-sugar complex of the present invention, hollow spherical particles that are safer for living organisms can be obtained.
[0102] The hollow spherical particles of the present invention contain hollow portions, and the number of the hollow portions is not particularly limited. The hollow spherical particles of the present invention can be mononuclear particles having one hollow portion, or polynuclear particles having multiple hollow portions.
[0103] The self-assembled body of the lignin-sugar complex of the present invention exhibits fluorescence in the long wavelength region. Specifically, it exhibits fluorescence in the wavelength region of 400 nm to 700 nm. In addition, in the self-assembled body of the lignin-sugar complex of the present invention, fluorescence that is significantly shifted to shorter wavelengths than the excitation wavelength, so-called anti-Stokes fluorescence, is observed. Anti-Stokes fluorescence is exhibited even when a weaker light source than conventional light sources, such as a xenon lamp, is used as an excitation light source. Therefore, the hollow spherical particles of the present invention can be used as an anti-Stokes fluorescent agent. In this case, for example, the hollow spherical particles of the present invention can be used as anti-Stokes fluorescent paints, inks, and identification agents, and up-conversion / wavelength conversion molecular materials.
[0104] The hollow spherical particles of the present invention are stably dispersed in an aqueous solution, and furthermore, can maintain the above-mentioned fluorescence even after drying into a solid state.
[0105] The hollow spherical particles of the present invention have a number average particle diameter of, for example, 100 μm or less. In a preferred embodiment of the present invention, the hollow spherical particles of the present invention have a number average particle diameter of, for example, 10 nm or more. The number average particle diameter is preferably 30 nm to 30 μm, more preferably 50 nm to 10 μm, even more preferably 60 nm to 1 μm, still more preferably 70 nm to 400 nm, and particularly preferably 80 nm to 300 nm.
[0106] The hollow spherical particles of the present invention can have a high lumen ratio. The lumen ratio of the hollow spherical particles of the present invention is, for example, 60% or more, preferably 70% or more, more preferably 75% or more, and even more preferably 80% or more. The lumen ratio is measured according to the method described in Reference Test Example 6.
[0107] The hollow spherical particles of the present invention can be used, for example, as a carrier for transporting substances by incorporating an active ingredient in the hollow portion. This can also impart resistance to dissolution, compatibility, light resistance, etc. to the active ingredient. A wide range of active ingredients can be selected, including, for example, pesticides, fertilizers, medicines, cosmetic ingredients, fragrances, fluorescent agents, paints (e.g., vanillin, limonene, menthol, etc.), proteins, antibodies, nucleic acids (e.g., oligonucleotides such as DNA and RNA), vaccines, peptides, lipids, hormones, sugars, glycosides, surfactants, ultraviolet absorbers, light scattering agents, adhesives, vitamins, coenzymes, minerals, cells, organelles, low molecular weight compounds (e.g., signaling substances such as pheromones; nitrogen-containing compounds such as alkaloids, monoterpenes, and sesquiterpenes; isoprenoids such as terpenoids; phenylpropanoids, etc.), polymer compounds, metal complexes, liposomes, and hydrogels.
[0108] Specifically, the hollow spherical particles of the present invention can be used as drug carriers (for DDS applications). More specifically, they can be used as organic capsules as drug carriers. They are natural products and are expected to be biocompatible, making them useful as drug carriers. Furthermore, hollow spherical particles with an average particle size of 200 nm or less, preferably 100 nm or less, are expected to have an EPR (Enhanced Permeation and Retention Effect) that allows them to reach and accumulate in tumor tissues without leaking into normal tissues.
[0109] The hollow spherical particles of the present invention can also be used as ultraviolet absorbing capsules to impart light resistance to protect encapsulated compounds from ultraviolet rays. Since the absorption range includes the wavelength ranges of UV-A and UV-B, they are also useful as ultraviolet absorbing materials used in skin care products such as sunscreens. Such ultraviolet absorbing effect is presumed to be due to intermolecular interactions such as π-π stacking of aromatic lignin.
[0110] The hollow spherical particles of the present invention, including cationic particles, have a high affinity with negatively charged cell membranes and are easily taken up into cells. Therefore, they are useful as drug carriers and can be used as drug transport or introduction agents. Furthermore, the hollow spherical particles of the present invention can form ion complexes with negatively charged nucleic acids on the surface of the hollow spherical particles, so they are useful as nucleic acid carriers and can be used as nucleic acid transport or introduction agents. The hollow spherical particles of the present invention can have a positive charge, for example, a zeta potential of 5 to 100 mV, preferably 10 to 80 mV, more preferably 20 to 60 mV, and even more preferably 40 to 60 mV.
[0111] In one embodiment of the present invention, the hollow spherical particles of the present invention are a group of hollow spherical particles made of lignin-saccharide complexes having an average particle size of 200 nm or more, preferably 250 nm or more, more preferably 300 nm or more, and have a positive average zeta potential at pH=7 and room temperature. In another embodiment of the present invention, the hollow spherical particles of the present invention are a group of hollow spherical particles made of lignin-saccharide complexes having an average particle size of 200 nm or less, preferably 150 nm or less, and have a negative average zeta potential at pH=7 and room temperature. The zeta potential can be measured using an electrical resistance nanopulse method. Room temperature is a temperature around 20°C, for example, 20°C.
[0112] The hollow spherical particles of the present invention are positively charged at neutral to acidic pH and can be stably dispersed in water for long periods of time. Furthermore, as shown in Example 3, by making the external environmental pH basic, switching from a positive charge to a negative charge can be achieved with almost no change in particle diameter, and the particles have the function of acting as pH-responsive nanocarriers.
[0113] The hollow spherical particles of the present invention may contain a liquid, a gas, or a solid (such as a metal) enclosed therein, and may be used, for example, as a heat insulator, a compatibilizer, a catalyst, or a sensitizer.
[0114] The form in which the above-mentioned active ingredients, solids, etc. are present is not particularly limited as long as they are in contact with and held by the hollow spherical particles, for example, they may be present in the hollow portion of the hollow spherical particles, they may be held by or attached to a component (lignin) of the hollow spherical particles, or they may be held by or attached to the outer surface of the hollow spherical particles.
[0115] The hollow spherical particles of the present invention exhibit long-wavelength fluorescence. This is due to the formation of so-called J-aggregates, which are conjugated molecules and polymers formed by self-organization of lignin, and long-wavelength fluorescence due to exciplex formation, preferably fluorescence of 450 nm or more, more preferably fluorescence of 480 nm or more, and even more preferably fluorescence of 500 to 600 nm (specifically, for example, Ex 515 nm / Em 535 nm), and large Stokes shift fluorescence of 100 nm or more (for example, Ex 410 nm / Em 670 nm) are observed. Fluorescence in the long-wavelength region is useful for identifying hollow spherical particles. In particular, fluorescence in the near-infrared region of 600 nm or more is called the biological window, and is suitable for selective optical detection without overlap with coexisting components, and for tracking and imaging drug kinetics in the body.
[0116] The hollow spherical particles, which are the self-assembled bodies of the lignin-sugar complex of the present invention, are stable over time and suppressed from association and aggregation, and can maintain their particle diameter more stably. The stability (dispersion retention, structural stability, and temperature stability) of the hollow spherical particles can be evaluated by the rate of change in the average particle diameter 6 weeks after production when measured under the conditions of Example 2. The stability (rate of change in average particle diameter) of the hollow spherical particles is within ±13% after 6 weeks, with respect to the average particle diameter of 100% immediately after production. In particular, the hollow spherical particles have excellent temperature stability, and the rate of change in the average particle diameter is within ±20% (in the range of 10°C to 60°C), preferably within ±5% (in the range of 10°C to 70°C). Therefore, the stability (6 weeks) of the hollow spherical particles of the present invention is within 15% in terms of change, and preferably the thermal stability is within 5%.
[0117] The structural stability can also be evaluated by scanning electron microscope observation. That is, as shown in Example 1 (Figure 11-2), the hollow spherical structure is maintained even in a dry capsule or in a vacuum. The structure is also stable after drug encapsulation, as shown in Example 1 (Figure 12-2). Such shape stability is suitable for efficient formulation, accumulation, transportation, and storage of drug carriers.
[0118] The particle size, surface charge, dispersibility and encapsulation capacity of the above-mentioned active ingredients of the lignin-sugar complex capsules, which are hollow spherical particles of the present invention, can be widely adapted depending on the plant species and part of the raw material biomass.
[0119] This difference is due to the ratio of structural units of lignin (the ratio of aromatic structures with phenylpropane units as the basic skeleton, guaiacyl lignin, syringyl lignin, p-hydroxyphenyl lignin, and flavonoid lignin) and the types of constituent polysaccharides in the constituent lignin-sugar complexes.
[0120] In addition, the particle size, surface charge, dispersibility, and encapsulation capacity of the above-mentioned active ingredients of the lignin-sugar complex capsules, which are hollow spherical particles of the present invention, can be widely adjusted by changing the lignin-sugar composition ratio (the ratio obtained by dividing the number of polysaccharide monomer units by the number of lignin monomer units) in the constituent lignin-sugar complex and by separating the types of polysaccharides.
[0121] Lignin-sugar complexes with different lignin-sugar composition ratios can be easily separated by their differences in solubility in alcohol / water or dioxane / water, etc. They can also be separated by hydrophobic interaction chromatography (method described in the literature (Nishimura et al., Direct evidence for α ether linkage between lignin and carbohydrates in wood cell walls, Sci Rep 2018), Toyopearl HW50 column).
[0122] The polysaccharide component of the lignin-sugar complex is hemicellulose. If it is made from hardwood, it contains a lot of acidic polysaccharides (glucuronoxylan) containing uronic acid, while if it is made from coniferous wood, it contains a lot of neutral polysaccharides (glucomannan). Separation focusing on the polysaccharide component of the lignin-sugar complex can be performed using the ion exchange chromatography method described in the literature (Nishimura et al., Direct evidence for α ether linkage between lignin and carbohydrates in wood cell walls, Sci Rep 2018).
[0123] The hollow spherical particles of the present invention can control the sustained release properties by the action of an enzyme, which is a biocatalyst. As shown in Example 4, the hollow spherical particles carrying a drug can be released by changing or destroying the shape of the hollow spherical particles carrying a drug through the action of a polysaccharide degrading enzyme. Enzymes have activity that is selective under conditions of substrate specificity, pH, and temperature, and the sustained release conditions (pH, temperature, release rate) can be controlled by using enzymes (hydrolases, oxidases) appropriate for the purpose.
[0124] The inclusion and coating of active ingredients such as metal nanoparticles using the lignin-sugar complex of the present invention allows for the improvement of a wide range of functionality. It improves the dispersibility and durability of the particles in water, good dispersibility of the particles in a dry state, and compatibility with matrices including resins. These allow the use of metal nanoparticles in a wide variety of environments, and by providing hydrophobicity to organic solvents, it increases solubility and dispersibility. This is a characteristic required for many industrial applications. These coatings also provide the ability to maintain the chemical stability of the metal nanoparticles or metal ions and control their reactivity. This allows these particles to function as catalysts and sensors. By improving biocompatibility, environmental affinity, photoresponsiveness, and molecular recognition ability, applications such as biomedical applications, environmental remediation, optical devices, and biosensors are possible. By imparting sustained release properties, it becomes possible to control the release of substances or the expression of functions over time, which is particularly useful for drug delivery applications. By improving weather resistance and light resistance, the durability of the encapsulated ingredients and metal ions against the external environment is improved. In addition, control of particle size contributes to improved safety, optimized performance, and improved environmental compatibility and biocompatibility.
[0125] Specifically, the present invention provides the following improvements, modifications, expansion of applications, and performance enhancements of metal nanoparticles. Gold (Au) nanoparticles are used in biomedical applications such as sensors using surface plasmon resonance (SPR), imaging, carriers in drug delivery systems (DDS), target selectivity, and photothermal therapy using photothermal conversion properties by light irradiation. They are also expected to be used as catalysts in organic synthesis reactions, electrode materials for fuel cells, and air and water purification. Silver (Ag) nanoparticles are used as antibacterial agents taking advantage of their antibacterial properties and as conductive inks. Platinum (Pt) nanoparticles are particularly widely used as catalysts in fuel cells and are also used as catalysts in the chemical industry. Palladium (Pd) nanoparticles are particularly useful as catalysts, and are used in carbon-carbon bond formation reactions and hydrogenation reactions, and are promising as hydrogen storage materials. Iron (Fe) nanoparticles are expected to be used as MRI contrast agents, components of magnetic fluids, and for decomposing harmful substances in groundwater. Copper (Cu) nanoparticles are expected to be used as conductive inks and as catalysts for decomposing air pollutants. Nickel (Ni) nanoparticles, taking advantage of their strong magnetic properties, are expected to be applied to data storage, magnetic inks, magnetic fluids, etc. They are also expected to be used as catalysts in hydrogenation reactions and energy conversion. Titanium (Ti) nanoparticles are used as photocatalysts in the form of titanium dioxide (TiO2), and have self-purifying materials and water / air purification functions. Bioimaging and drug delivery are also expected. Zinc (Zn) nanoparticles are expected to be used in solar power generation, LEDs, UV protection agents, cosmetics, etc. Aluminum (Al) nanoparticles are expected to be used in energy generation (rocket propellants, etc.) and as thermal conductive materials. EXAMPLES
[0126] The present invention will be described in detail below based on examples, but the present invention is not limited to these examples.
[0127] Reference Test Example 1. Isolation of lignin, lignin-sugar complex, hemicellulose, cellulose-hemicellulose complex, and celluloseLignin, lignin-sugar complexes, hemicellulose, cellulose-hemicellulose complexes, and cellulose were isolated from biomass by the M-APA method, the A-APA method, or a method for examining the conditions thereof, and the yield and physical properties of the isolated products were measured. The isolation method of the present invention is a production method capable of highly efficiently isolating soluble lignin, lignin-sugar complexes, hemicellulose, cellulose-hemicellulose complexes, and cellulose from natural polymers in biomass, and includes a step (A) of contacting a solution containing an organic acid and a peracid with plant biomass. Specifically, the isolation method was carried out as follows.
[0128] <Reference Test Example 1-1. Preparation of finely ground wood powder> Fine powder (finely ground wood flour) with a volume average particle size of 10 μm (1-100 μm) was prepared from wood flour of broad-leaved trees (eucalyptus or beech), coniferous trees (red pine, cedar, or cypress), or herbaceous plants (bagasse (sugar cane) or bamboo) using a ball mill or bead mill method.
[0129] Here is an example of the preparation method using a ball mill. A planetary ball mill (P-6, Fritsch) was used. 2g of wood flour and 100g of φ3mm zirconia beads were placed in an 80cc agate container and sealed in a twin overpot. The overpot was evacuated for 20 minutes, and then inert nitrogen gas was injected. One cycle consisted of 1 minute of milling and 1 minute 20 seconds of pause, and the treatment was carried out for 180 cycles (total of 3 hours) at 550 rpm. Under these conditions, fine powdered wood flour could be obtained while suppressing oxidation during milling and denaturation due to heating.
[0130] <Reference Test Example 1-2. Preparation of wood flour> 1 g each of wood flour or wood chips (10 mm x 10 mm x 1 mm) from broadleaf trees (eucalyptus or beech), coniferous trees (red pine, cedar, or cypress), or herbaceous plants (bagasse (sugar cane) or bamboo) was placed in the two pots on the left and right of a mixer mill (MM301, manufactured by Retsch), and the milling process was carried out under the conditions of a milling time of 5 minutes and a frequency of 1 / 15 sec, to obtain a powder (wood flour) with a volume average particle size of 0.1 mm.
[0131] <Reference Test Example 1-3. M-APA Method (Milling-Acid-PerAcid Method)> As a starting material, the finely ground wood flour (average particle size 10 μm) obtained in Reference Test Example 1-1 was used. 2 g of finely ground wood flour and 10 mL of an acetic acid-peracetic acid-containing solution (composition: acetic acid 99% 17.4 M, slightly less than 1% peracetic acid 0.14 M, hydrogen peroxide 0.01 M, trace amount of water) were placed in an initiator vial, and microwave irradiation was performed for 10 min using a Biotage Initiator+ 60 microwave synthesis device under the conditions of 50°C, initial power 400 W, and stirring speed 600 rpm. After microwave treatment, the soluble portion was separated by adding 10 mL of separation solvent (acetone) and spinning down (RCF 8000 xg, 5 min). The insoluble portion was extracted with 10 mL of separation solvent (acetone) and washed three times to combine with the soluble portion. This soluble lignin is called acid peroxy acid lignin (APA lignin).
[0132] In the second step, the insoluble portion was subjected to the same extraction procedure but with the microwave heating condition changed to 140°C. The soluble portion was taken as the lignin-hemicellulose complex. The insoluble portion was obtained with cellulose as the main component.
[0133] <Reference Test Example 1-4. A-APA Method (Alkali-Acid-PerAcid Method)> The wood flour (average particle size 0.1 mm) obtained in Reference Test Example 1-2 was used as the starting material. A 0.25M sodium hydroxide solution was prepared (1N diluted 4 times). 2.4 mL of 0.25M sodium hydroxide solution was added to 0.3 g of wood flour, and microwave extraction treatment (100°C, 30 min) was performed. The required amount of alkali is approximately 1 mmol of NaOH per 1 g of wood flour.
[0134] After microwave treatment, the soluble and insoluble parts can be easily separated by decantation, spin down, or filtration. An additional acetone (separation solvent) extraction was performed three times to combine with the soluble part. For the insoluble part, acid peroxy acid lignin (APA lignin) and lignin-hemicellulose complex were obtained as soluble lignin using the same extraction method as the M-APA method in Reference Test Example 1-3. An insoluble part consisting mainly of cellulose was obtained.
[0135] <Reference test example 1-5. Condition consideration> Instead of acetic acid, other organic acids (formic acid, glyoxylic acid) were used to study. Also, instead of peracetic acid, other peracids (hydrogen peroxide) were used to study. When other peracids (hydrogen peroxide) were used, the composition was acetic acid: 12M, hydrogen peroxide concentration: the concentration shown in the table below.
[0136] The contact temperature between the plant biomass or insoluble matter and the organic acid + peracid was changed from room temperature to 180°C. In addition, the heating method used was an external heating method using an oil bath instead of an internal heating method using microwave heating.
[0137] <Reference Test Example 1-6. Analysis and Measurement Method> Lignin, lignin-sugar complexes, and cellulose were analyzed and measured by the following methods.
[0138] <Reference Test Example 1-6-1. Molecular weight (Mn, Mw and polydispersity) measurement method> The molecular weight was determined by size exclusion chromatography (SEC), also known as gel permeation chromatography (GPC). The sample was dissolved in a solution of acetic anhydride and a base (pyridine, etc.) and reacted for 3-6 hours to obtain an acetylated form. This was dissolved in tetrahydrofuran (THF) at a concentration of 2.0 mg / mL and separated by high-performance liquid chromatography (Shimadzu Corporation, high-pressure gradient SEC analysis system). The column used was an HZ-M column (Tosoh 150 mm x 4.6 mm id, 4 μm, three columns connected in series). The analysis was performed by injecting 10 μL of sample, at a column temperature of 40°C, with tetrahydrofuran (THF) as the mobile phase, and at a flow rate of 0.35 mL / min. Mass calibration curves were constructed using standard polystyrene, Tosoh PStQuickC (molecular weights (MW) of 2,110,000, 427,000, 37,900, and 5970), pinoresinol (MW 352), and vanillin (MW 152) to determine the weight average molecular weight (Mw) and number average molecular weight (Mn) of the samples. Polydispersity was calculated as Mw / Mn.
[0139] <Reference Test Example 1-6-2. Calculation method for the composition ratio of molecular bond units> Samples were dissolved in deuterated dimethyl sulfoxide (DMSO-d6) at 1-10 wt%, and NMR spectra were obtained using a Bruker Avance III 600 MHz NMR instrument equipped with a cryogenic probe. The composition ratio of the interunit bond units of lignin was calculated from the signal volume on the HSQC (Heteronuclear single-quantum correlation spectroscopy) spectrum. The composition ratio was calculated as the ratio per 100 lignin aromatic rings. The content of ether-type bond units was estimated from the sum of the integral values of the CH correlation signals at the β-position (δH / δC=4.0 ±0.2 ppm / 85.6 ±1.2 ppm region, δH / δC=4.3 ±0.2 ppm / 83.0 ±0.7 ppm region). Quantitation in the two-dimensional NMR method was performed by correcting using the TAF method described in the literature (Okamura, H. Nishimura, T. Nagata, T. Kigawa, T. Watanabe and M. Katahira, Accurate and molecular-size-tolerant NMR quantitation of diverse components in solution, Scientific Reports, 6, 21742. 2016), to calculate accurate content.
[0140] <Reference Test Example 1-6-3. Calculation method of the composition ratio of lignin and polysaccharides> The sum of the integral values of the CH correlation signals at the anomeric position (1st position) of the polysaccharide was calculated by the NMR method described above, and after correction by the TAF method, it was calculated as a ratio per 100 lignin aromatic rings.
[0141] <Reference Test Example 1-6-4. Calculation method of the composition ratio of lignin-sugar copolymerization points> As mentioned above, the sum of the integrals of the CH correlation signals (LC ether, δH / δC=4.50 ±0.15 ppm / 80.1 ±1 ppm region) and (LC ester, δH / δC=5.88 ±0.15 ppm / 74.0 ±1.5 ppm region) derived from the LCα ether and LCα ester bond units was calculated by 2D HSQC NMR, and after correction by the TAF method, it was calculated as a ratio per 100 lignin aromatic rings. In the case of the A-APA method, some of the ester bonds are hydrolyzed by alkali treatment, but it is also possible to obtain LCα ester type lignin-hemicellulose complexes.
[0142] <Reference Test Example 1-6-5. Calculation method of yield from raw biomass> The obtained components were checked using a pH meter or pH test paper, and peracid test paper (potassium iodide starch paper), and then neutralized and peracid quenched as necessary. Neutralization was performed by adding 1N HCl or 1N NaOH in small amounts. Peracid quenching was performed by dropping 1M sodium sulfite aqueous solution. The organic solvent was removed using an evaporator. Dry powder was then obtained by freeze-drying. If salts were generated by neutralization, the concentrated liquid after the organic solvent was removed was re-extracted with a separation solvent (acetone) for desalting. The solvent was then removed again using an evaporator, and dry powder was obtained by freeze-drying. Each obtained component was weighed, and the yield per raw biomass was calculated.
[0143] <Result> The molecular structure, molecular weight, and yield of the obtained polymer are desirable under the following conditions. The results are shown in Tables 1 to 7.
[0144] Table 1 shows the peracid conditions in the two-stage microwave extraction reaction of the M-APA method and the yields of each component of polymeric lignocellulose (weight %, raw material biomass ratio, raw material is eucalyptus).
[0145] [Table 1]
[0146] Table 2 shows the yields (wt %, ratio to raw material biomass) of each polymeric lignocellulose component of various biomass in the A-APA method two-stage microwave extraction reaction.
[0147] [Table 2]
[0148] Table 3 shows the peracid conditions in the two-stage microwave extraction reaction of the M-APA method and the molecular weights of each component of high molecular weight lignocellulose (acetylated GPC analysis values).
[0149] [Table 3]
[0150] Table 4 shows the yields (wt %, ratio to raw material biomass) of each polymeric lignocellulose component of various biomass in the two-stage microwave extraction reaction of the M-APA method.
[0151] [Table 4] Solvent: Acetic acid (containing 1% peracetic acid, 0.14 mol / L) Microwave extraction conditions: 50°C, 10 min (first stage) to obtain APA lignin soluble portion, 140°C, 10 min (second stage) to obtain lignin hemicellulose complex. Table 5 shows the yields (wt%, ratio of raw material biomass) of each polymeric lignocellulose component of various biomass in the A-APA method one-stage microwave extraction reaction.
[0152] [Table 5]
[0153] Table 6 shows the molecular weights (acetylated GPC analysis values) of each component of polymeric lignocellulose obtained from various biomass by the A-APA method.
[0154] [Table 6]
[0155] As a result of examining the conditions, it was found that when the starting material is woody biomass, a contact temperature of 40 to 90°C with organic acid + peracid is suitable for obtaining soluble lignin, and a contact temperature of 100 to 160°C is suitable for obtaining a lignin-hemicellulose complex. Furthermore, as a result of examining the conditions, it was found that when the starting material is herbaceous biomass, a contact temperature of room temperature to 60°C with organic acid + peracid is suitable for obtaining soluble lignin, and a contact temperature of 70 to 150°C is suitable for obtaining a lignin-hemicellulose complex.
[0156] As a result of examining the conditions, it was found that the heating time by microwave irradiation is 5-30 min, preferably 10 min. The net irradiation time is short. See Figure 2 for the microwave profile, temperature, and pressure data.
[0157] As a result of examining the conditions, it was found that microwave heating had higher yields and selectivity at lower temperatures, shorter times, and with lower energy inputs than the external heating method. In other words, the microwave effects of localized heating, internal heating, electron transfer, and drug penetration promotion were confirmed.
[0158] As a result of examining the conditions, it was found that lignin could be isolated using all three organic acids, acetic acid, formic acid, and glyoxylic acid, but acetic acid was the most suitable in terms of yield, purity, and industrial application.
[0159] The NMR results of Reference Test Example 1-6-2 and Reference Test Example 1-6-3 are shown in Figure 3. Figure 3 shows the analysis results of lignin isolated by the M-APA method (microwave treatment at 50°C for 10 minutes, acetic acid / peracetic acid 1% conditions) using eucalyptus as the starting material. The proportion of bonds between lignocellulose units was quantified by the TAF-NMR method, and the signal derived from lignin was 99% and the signal derived from polysaccharide (hemicellulose) was 1%. The breakdown of the bonds between lignin units was 81% ether-type β-O-4, 5% β-5, 11% β-β, 1% dibenzodioxocine, and 1% others. See Figure 4 for the partial chemical structures of bonds between lignin units and covalent bonds between lignin and hemicellulose.
[0160] The NMR results of Reference Test Example 1-6-4 are shown in Figure 5. Figure 5 shows the analysis results of the lignin-hemicellulose complex isolated by the M-APA method (microwave treatment at 50°C for 10 minutes, acetic acid / peracetic acid 1% conditions) using each plant as the starting material. The LC bonds (ether and ester types) shown by the circles in the figure are the main branched structures that are present in an amount equal to or greater than the abundance ratios of β-5 and β-β bonds, which are the main inter-unit bonds of lignin. The isolated lignin-hemicellulose complex is characterized in particular by having LCα-ester type bonds.
[0161] Reference test example 2. Solubility measurement The solubility of the lignin and lignin-hemicellulose composite obtained by the method of Reference Test Example 1 or a method similar thereto in 60 to 80% ethanol at 25°C was measured. Details of the measured samples are shown in Table 7. The abbreviations in Table 7 are explained as follows. In addition, similar abbreviations are used in some parts of the specification hereafter. PA: Peracetic acid HP: Hydrogen Peroxide 50: MW50 ACTN, microwave 50℃ processing, high-quality polymeric lignin 140: MW50-Mw140 ACTN, second stage of 140°C treatment of residue after microwave 50°C treatment, Lignin hemicellulose complex A50: Acetic acid peracetic acid system, HP PA1%AA Mw50 ACN Microwave 50°C treatment High quality polymeric lignin H50: Acetic acid hydrogen peroxide system, HP 1M hydrogen peroxide Mw50 ACN Microwave 50°C treatment High quality polymeric lignin.
[0162] [Table 7]
[0163] The solubility was measured as follows. After the sample was dissolved by stirring in 25°C ethanol, it was separated into an ethanol-soluble part and an ethanol-insoluble part by solid-liquid separation. A 25°C aqueous ethanol solution (1 / 1 = ethanol / water) was added to the ethanol-insoluble part, and the ethanol-soluble part was obtained by stirring and dissolving. The aqueous ethanol-soluble part was mixed with the ethanol-soluble part to obtain a sample solution. The amount of the aqueous ethanol solution added was adjusted so that the ethanol concentration of the sample solution was in the range of 60 to 80%. In the process of obtaining the soluble part, the sample was dispersed and solubilized by ultrasonic irradiation as necessary. The maximum sample concentration at which the sample solution became transparent to the naked eye was defined as the "solubility in 60 to 80% ethanol at 25°C".
[0164] The results are shown in Table 8. The lignin and lignin-hemicellulose complex obtained by the method of the present invention exhibited solubilities of 8 to 20% in ethanol / water solutions (60 / 40 and 80 / 20 v / v%).
[0165] [Table 8]
[0166] Reference Test Example 4. Preparation and analysis of self-assembled bodies A self-assembled body was prepared using lignin isolated by the M-APA method (microwave treatment at 50°C for 10 minutes, acetic acid-peracetic acid 1% or acetic acid-0.2M hydrogen peroxide conditions) using eucalyptus or bamboo as a starting material, or lignin-sugar complex isolated by the M-APA method (microwave treatment at 140°C for 10 minutes, acetic acid-peracetic acid 1% or acetic acid-0.2M hydrogen peroxide conditions) using eucalyptus as a starting material. Specifically, the procedure was as follows.
[0167] A DMSO solution with a sample concentration of 1-2 wt% was prepared and diluted to 0.01-0.02 wt% with a mixture (1:1 or 2:1) of a separation solvent (acetonitrile or ethanol) and water (or buffer solution) to obtain a sample solution. 0.1-0.2 mL of the sample solution was applied to a slide glass or cover glass, and the solvent was evaporated under atmospheric pressure to obtain a thin-film self-assembled body. Among the above conditions, a high-concentration self-assembled body was obtained by adding an equal amount of water (or buffer solution) to a DMSO solution with a sample concentration of 1 wt% and applying it.
[0168] Next, the optical properties of the obtained self-assembled bodies (lignin solid thin films or lignin-sugar complex solid thin films) and a comparison object (lignin obtained by the APA method (APA lignin)) were analyzed. Specifically, the optical properties were analyzed as follows.
[0169] The following was used for the measurements.
[0170] Ultraviolet-visible absorption spectrum: UV-2700 (Shimadzu Corporation) Fluorescence spectrum: Spectrofluorometer RF-6000 (Shimadzu Corporation) Fluorescence microscope measurement: All-in-one fluorescence microscope BZ-X810 (Keyence) The analysis was performed using the analysis software provided with each device.
[0171] UV-Vis absorption spectrum: Black quartz cell for spectroscopic measurement (optical path length: 10 mm), Fluorescence measurement: A fully transparent synthetic quartz cell (optical path length: 10 mm) and a Starna three-corner quartz cell SF3 were used. For solid samples, a solid measurement unit was used, and the sample applied to the cover glass was sandwiched between quartz plates and fixed for measurement.
[0172] The 3D fluorescence spectrum was measured under the following conditions: excitation wavelength 310-800nm, data interval 5nm, emission wavelength 350-900nm, data interval 1nm, scan speed 12000nm / min, ultraviolet cut filter U310 was attached on the excitation side to reduce the influence of scattered light and multi-order light. The bandwidth was 5nm on the excitation side, 15nm on the emission side, and the sensitivity setting was Low.
[0173] The synchroscan spectrum is a scanning mode in which the excitation and fluorescence spectrometers of the spectrofluorophotometer are scanned simultaneously with a fixed wavelength interval between them. Measurements were performed by varying the wavelength interval between the excitation light and the fluorescence light in the range of -90 nm to 260 nm. When the wavelength interval is negative, that is, fluorescence with a shorter wavelength than the excitation light is detected. In this case, fluorescence due to the anti-Stokes shift can be selectively detected. The scan was set to cover the fluorescence wavelength range of 350-800 nm, with a data interval of 0.1 nm, a scan speed of 600 nm / min, a bandwidth of 15 nm on the excitation side and 20 nm on the emission side, and a sensitivity setting of Low.
[0174] The ultraviolet-visible absorption spectrum was measured using a double monochromator type UV-2700. A wavelength scan (200-900 nm) was performed.
[0175] The results are shown in Figures 6 to 9. Figure 9 shows that the lignin self-assembled body exhibits anti-Stokes fluorescence.
[0176] In addition, a composite with gold was synthesized from the obtained self-assembled body (hollow spherical particles of lignin-sugar complex). An aqueous solution containing the self-assembled body solution and tetrachloroauric (III) acid (Fujifilm Wako Pure Chemical Industries, special grade) was prepared, and the inside of the reaction vessel was replaced with argon gas and then sealed. The solution was irradiated with 28 kHz ultrasound for 10 minutes (Honda Electronics (AS ONE), triple frequency ultrasonic cleaner VS-10III). The solution was filtered through a filter (pluriSelect Life Science, pore size 1 μm), and the filtrate was analyzed with a dynamic light scattering meter (Horiba, SZ-100 Nanoparticle Size Analyzer) and an ultraviolet-visible spectrophotometer (Shimadzu, UV-2700).
[0177] As a result, the particle size distribution of the self-assembled bodies measured by a dynamic light scattering meter showed that the particle size of the gold-composite (Au Composite 5003, solid line) was smaller than that of the self-assembled bodies alone (LCC4936, dashed line). The mode diameters were 143.8 nm and 113.5 nm, respectively.
[0178] An example of the UV-visible absorption spectrum of the solution after stirring is shown in Figure 17. The absorption observed at 530-540 nm can be attributed to the surface plasmon resonance absorption of gold (Creighton et al., J. Chem. Soc. Faraday Trans., Vol. 87, p. 3881, 1991), which indicates that the gold ions were reduced by the reaction with the self-assembled bodies, producing stable gold nanoparticles. The amount of unreduced gold(III) ions in the reaction solution can be quantified as follows (Mizukoshi et al., Analytical Chemistry, Vol. 45, No. 4, p. 327, 1996). A predetermined amount of the self-assembled body solution and an aqueous solution containing tetrachlorogold(III) were reacted for a predetermined time. A saturated aqueous solution of sodium bromide was added to the reaction solution, and the aggregates formed by salting out were separated by filtration, centrifugation, etc. This removed the spectral interference caused by nanoparticles. On the other hand, the unreacted gold ions coordinated with the added bromide ions, and the absorption of tetrabromogold(III) ions appeared around 381 nm. Using a calibration curve prepared in advance, the amount of unreacted gold ions in the reaction solution was colorimetrically quantified. This allowed us to calculate the amount of gold ions reduced and the electrons donated to the gold ions during reduction, and to determine the amount of electrons donated per 1 mg of self-assembled body. For example, 4 μmol of gold ions were consumed by 1.9 mg of self-assembled bodies, which means that 4 × 3 μmol of electrons were donated to the gold ions, meaning that 6.3 μmol of electrons can be donated per 1 mg of self-assembled bodies.
[0179] Reference Test Example 4. Measurement of UV absorbance The ultraviolet absorbance was measured for the lignin and lignin-hemicellulose complex used in Reference Test Example 2. Specifically, the sample was dissolved in ethanol to a concentration of 0.005 w / v%, and the ultraviolet absorption spectrum of the resulting solution (transparent) was measured with a spectrophotometer (Shimadzu Corporation, UV-2700) (optical path length 1 cm, quartz cell).
[0180] The results are shown in Figure 10. It was found that the lignin and lignin-hemicellulose complex obtained by the method of the present invention exhibited a wide range of ultraviolet light absorbency over the UV-A (320 nm to 400 nm) and UV-B (280 nm to 320 nm) wavelength regions.
[0181] Reference Test Example 5. Preparation of hollow spherical particles 1 The lignin used in Reference Test Example 2 was used as a sample to prepare hollow spherical particles as self-assembled bodies. Specifically, the procedure was as follows.
[0182] (1) 20 mg of lignin sample (dry powder) was dissolved in 1.0 mL of DMSO to prepare a 2% w / v lignin solution.
[0183] (2) 0.1 mL of 2% w / v lignin stock solution was added to 0.9 mL of 80% v / v ethanol solution and stirred until uniform.
[0184] (3) The solution was diluted by gradually adding 3 mL of water while stirring. The dilution rate could be changed, and the formation of hollow spherical particles began when the organic solvent concentration was 40% or less, and a stable dispersion state was observed at 5-30%.
[0185] Alternatively, hollow spherical particles were obtained by a method employing the following step (4) instead of the above step (3).
[0186] (4) 1 mL of alcohol-water solvent was gradually added dropwise while stirring. A 30% ethanol solution or a 10% n-butanol solution was used as the alcohol-water solvent. After that, the solution surface was gently sprayed with nitrogen gas, or the solvent was evaporated by air drying, or distilled off under reduced pressure. The formation of hollow spherical particles began when the organic solvent concentration was 40% or less, and a stable dispersion state was observed at 5-30%.
[0187] A bright field image of the obtained hollow spherical particles is shown in Figure 11-1. Relatively large particles (diameter 5 μm or more) and relatively small particles (diameter less than 5 μm) were confirmed.
[0188] In addition, the particle diameter and film thickness of one relatively large particle were measured, and the volume occupied by the hollow spherical particle lumen (lumen ratio) was calculated. Specifically, a Keyence all-in-one fluorescence microscope BZ-X810 was used to capture fluorescence observations with a 100x objective lens in sectioning mode, and the particle diameter and film thickness were measured from the obtained image data using Keyence analysis software. The lumen ratio (unit: %) was calculated using the formula: lumen ratio = (volume of the lumen part of the hollow spherical particle (part excluding the membrane part) / total volume of the hollow spherical particle) x 100. As a result, the particle diameter was 21.1 μm, the film thickness was 635 nm, and the lumen ratio was 83%.
[0189] Reference Test Example 6. Preparation of hollow spherical particles 2 The lignin used in Reference Test Example 2 was used as a sample to prepare hollow spherical particles encapsulating a drug. Specifically, the procedure was as follows.
[0190] A 0.2% w / v lignin solution (in 80% ethanol) was mixed with 1.0 mL of a 0.1% w / v near-infrared fluorescent dye DiR (DiIC18(7)) 80% ethanol solution while stirring. Water or alcohol-water solvent was added dropwise while stirring, and the organic solvent concentration was reduced in the same manner as in Reference Test Example 5 to form hollow spherical particles.
[0191] The image observed by a fluorescence microscope is shown in Figure 12-1. Particles exhibiting near-infrared fluorescence originating from the encapsulated dye were observed.
[0192] Reference Test Example 7. Preparation of hollow spherical particles 3 Hollow spherical particles were prepared using the lignin used in Reference Test Example 2 as a sample. Specifically, the procedure was as follows.
[0193] A 2.5 wt% solution of lignin (derived from eucalyptus) (ethanol 30%) was prepared and stirred to obtain a homogeneous solution, which was used as the stock solution. 200 μL of 50% organic solvent (ethanol, 1-propanol, allyl alcohol, 2-propanol, or 1-butanol) was gradually added to 100 μL of the stock solution while stirring to obtain a homogeneous solution. 1.7 mL of water was gradually added while stirring to obtain a homogeneous solution. The obtained solution (final concentration 0.125 wt% organic solvent 5% (including 0.015% ethanol)) was subjected to measurement of nanoparticles by DLS. DLS measurement was performed using a multi-analyte nanoparticle size measurement system, 2 mL of the sample was placed in a glass disposable cell, and particle size measurement was performed by dynamic light scattering. Each measurement was performed three times, and the average value was calculated. The measurement temperature was 25°C, and the solvent refractive index was 1.33.
[0194] The results are shown in Table 9.
[0195] [Table 9]
[0196] In addition, the same tests as above were conducted using lignins derived from other tree species (red pine, cypress, cedar, beech, and bamboo) (lignins obtained by the same method as in Reference Test Example 2), and similar results were obtained for the average particle size and polydispersity index.
[0197] Example 1. Preparation of hollow spherical particles 4 Hollow spherical particles were prepared using as a sample the lignin or lignin-hemicellulose complex used in Reference Test Example 2. Specifically, the procedure was as follows.
[0198] The lignin-sugar complex or lignin powder was dissolved homogeneously in DMSO to a concentration of 10 w / v % by ultrasonic treatment, and then ethanol / water solutions were added as poor solvents in a stepwise manner with decreasing organic solvent concentration, followed by stirring to obtain a final organic solvent concentration of 30%.
[0199] The particle size and zeta potential of the obtained hollow spherical particles were measured by electrical resistivity nanopulse (qNANO). Using an electrical resistivity nanopulse (qNANO) nanoparticle multianalyzer (Izon Science, Meiwafosis), the size distribution, concentration, and zeta charge of nanoparticles were measured using the principle of TRPS. 35 μL of the particle solution was analyzed using NP200 and NP400 Nanopore at 46-47 mm stretch conditions according to the manufacturer's protocol.
[0200] The particle size of the lignin-hemicellulose composite hollow spherical particles was smaller than that of the lignin hollow spherical particles obtained under the same conditions. Similar results were obtained when the same test was performed using different tree species from which the samples were derived. The results are shown in Table 10.
[0201] [Table 10]
[0202] In addition, the zeta potential measurements showed that the lignin-hemicellulose composite hollow spherical particles were cationic nanoparticles with a high positive zeta potential of 40 to 60 mV.
[0203] The surface charge of the lignin-sugar complex capsules was measured using an electrical resistivity nanopulse method (qNANO) nanoparticle multianalyzer (Izon Science, Meiwafosis).
[0204] [Table 11]
[0205] Table 11 shows the particle size and zeta potential measurement results of eucalyptus-derived lignin capsules (LP) and eucalyptus-derived lignin-sugar complex capsules (LHP).
[0206] In addition, the particle size and zeta potential distribution of the eucalyptus-derived lignin capsule (LP, top) and the eucalyptus-derived lignin-sugar complex capsule (LHP, bottom) are shown in Figure 15. The particle size and zeta potential of each particle were obtained by electrical resistance nanopulse method (qNANO) and plotted.
[0207] Scanning electron microscope (SEM) images were also taken of the hollow spherical particles obtained. 0.2 mL of the solution containing the hollow spherical particles was pretreated with a Nano Percolator (manufactured by JEOL Ltd.), and the hollow spherical particles remaining on the membrane were treated with an Osnium Coater (manufactured by Meiwa Force Systems Co., Ltd.) to form a conductive coating, and then observed with a field emission scanning electron microscope (Hitachi High-Technologies Corporation: S-4800).
[0208] Scanning electron microscope (SEM) images are shown in Figure 11-2. Lignin capsules with particle sizes of 100 nm to 600 nm and lignin-sugar complex capsules with particle sizes of 20 nm to 200 nm were confirmed. The SEM images show that the hollow spherical particles do not collapse even in a vacuum and can maintain their shape, i.e., the stability of the particle structure. Vesicle structures derived from natural molecules such as liposomes and exosomes are difficult to maintain their shape in normal SEM observations that undergo a vacuum drying process, so this structural stability is particularly noteworthy.
[0209] The lignin-sugar complex capsules have the property of being an amphiphilic polymer, and therefore can have a high hydrophilic drug-containing capacity. In fact, in a test similar to that of Reference Test Example 6, the nucleic acid staining fluorescent dye DAPI [4,6-Diamidino-2-phenylindole, dihydrochloride] (manufactured by Dojindo Laboratories, CAS RN: 28718-90-3), chlorophyll as a dye (manufactured by Tokyo Chemical Industry Co., Ltd., CAS RN: 1406-65-1), and iron porphyrin complex hemin as a metal complex (manufactured by Tokyo Chemical Industry Co., Ltd., CAS RN: 16009-13-5) were encapsulated. After the capsules were prepared, they were separated from low molecular weight components by dialysis, and the dye absorption and absorption in the Soret band and Q band regions in the UV-vis spectrum were confirmed, and the drug encapsulation was confirmed by microscopic observation (bright field, fluorescence). The nucleic acid DNA was VIOLAMO DNA ladder marker (As One VIO-1kb), and the protein was Precision Plus protein marker (Biorad #1610377). The DNA was pre-bound with SYBR Green fluorescent dye before use. The drug inclusion was confirmed by UV-vis spectroscopy and fluorescence microscopy in the same manner.
[0210] Figure 12-2 shows fluorescence micrographs (Ex 360 nm, Em 460 nm), bright-field micrographs, and electron micrographs of lignin-sugar complex capsules encapsulating DAPI.
[0211] Fluorescence and bright field microscopy was performed using an all-in-one fluorescence microscope (Keyence BZ-X810). 0.2 mL of the solution containing the DAPI-encapsulated lignin-sugar complex was pretreated with a nanopercolator (JEOL), and the hollow spherical particles remaining on the membrane were treated with an Osnium Coater (Meiwa Force Systems) to form a conductive film, and then observed with a scanning electron microscope (Keyence VE-9800). The accelerating voltage was 8 kV.
[0212] The lignin-sugar complex capsules can exhibit long-wavelength fluorescence. A representative example of a 3D fluorescence spectrum obtained in the same manner as in Reference Test Example 3 is shown in FIG.
[0213] Example 2. Preparation of hollow spherical particles 5 Hollow spherical particles were prepared in the same manner as in Example 1 using the lignin or lignin-hemicellulose complex used in Reference Test Example 2 as a sample.
[0214] The average particle size of the obtained hollow spherical particles was measured in the same manner as in Example 1.
[0215] The stability of lignin hollow spherical particles obtained under the same conditions as the lignin-hemicellulose composite hollow spherical particles was evaluated at a solute concentration of 0.5 w / v%, solvent: 30 v / v% ethanol / water, and room temperature.
[0216] Furthermore, the fine particle solution was heated and stirred, and the average particle size was measured after 0.5 hours had elapsed.
[0217] The particle size stability and temperature stability are shown in Figures 13 and 14. The lignin-hemicellulose composite particles showed excellent dispersion retention over time, structural stability, and temperature stability. Specifically, the dispersion retention and structural stability showed that the rate of change in number average particle size and mode average particle size over a 6-week period was within ±13%, and the temperature stability showed that the rate of change in average particle size over a 10°C to 70°C period was within ±5%.
[0218] Example 3: Experiment on introduction of protein into eucalyptus-derived lignin-sugar complex capsules The lignin-sugar complex capsules can be prepared under mild conditions and are therefore capable of encapsulating biopolymers such as proteins and nucleic acids. Polysaccharides are highly biocompatible and are therefore promising as DDS.
[0219] In general, liposomes and PEG-modified nanocarriers have a negative surface charge, leading to low intracellular uptake efficiency. The lignin-sugar complex capsules showed a high positive surface charge in water (weakly acidic) (zeta potential measurement results, mode average +44 mV, particle size 276 nm). On the other hand, they showed a negative surface charge in basic conditions (50 mM PBS, pH 11) (zeta potential measurement results, mode average -21 mV, particle size 302 nm). These characteristics provide additional functionality as cationic drug carriers (DDS) with high cellular uptake efficiency. Furthermore, they are advantageous for drug delivery and nanocarrier retention in tumor tissues in an acidic environment. They also function as pH-responsive nanocarriers that can switch from positive to negative charge with little change in particle size.
[0220] Example 4. Sustained release of eucalyptus-derived lignin-sugar complex capsules by glycolytic enzymes Bovine serum albumin (Novagen) was used as the protein. Albumin (100 μg / ml) was fluorescently labeled. Fluorescent labeling was performed using WSE-7010 EzLabel FluoroNeo (ATTO). 10 μL of albumin solution (50 μg / ml, 0.5 μg) was added to 200 μL of lignin-sugar complex (0.5 w / v, 35% v / v ethanol solution), and the albumin was encapsulated in a lignin-sugar capsule. The capsule was observed through a filter using a Keyence All-in-One Fluorescence Microscope BZ-X810. Fluorescence microscopy images (equipped with a fluorescent filter for GFP) showed the inclusion of fluorescently labeled protein.
[0221] Next, polysaccharide-degrading enzyme hemicellulase (Hemicellulase Amano 90, Amano Enzyme) was added to a final concentration of 1 mg / mL, and the mixture was incubated at 50 °C for 90 min. The fluorescence was significantly reduced by the enzyme treatment, and it was observed that the labeled protein had leaked out of the lignin-sugar capsule and was gradually released.
[0222] Example 5. Analysis of hollow spherical particles 5-1. Method 5-1-1. Manufacturing of hollow spherical particles Eucalyptus lignin (PA1%AA, MW50, ACTN) and Eucalyptus LCC lignin (PA1%AA, MW50→140, ACTN) were used. First, 10 w / v % of each lignin stock solution was dissolved in DMSO and diluted with DMSO to prepare lignin stock solutions of different concentrations. Five concentrations were prepared: 1.0 w / v%, 2.5 w / v%, 5.0 w / v%, 7.5 w / v%, and 10 w / v%. 10 μL of each lignin solution was prepared in a 1.5 mL tube. Particle size was evaluated using the electrical resistance nanopulse method (qNANO) (NP400). Measurements were performed under conditions of Pressure 5 and Tension 47.01 cm. Samples were also diluted with PBS buffer containing a surfactant. The dilution ratio is shown in the table. 35 μL of the sample dilution solution was applied during measurement.
[0223] 5-1-2. Examination of temperature conditions during organization We investigated the effect of temperature conditions on the particle size and particle concentration of microparticles when forming microparticles by stirring and rotating reaction with organic solvent. The samples used were eucalyptus lignin (PA1%AA, MW50, ACTN) and eucalyptus LCC lignin (PA1%AA, MW50→140, ACTN). 10 w / v % lignin stock solution dissolved in DMOS was dispensed into 1.5 mL tubes in 10 μL portions. 50 μL of EtOH was used for mixing with the lignin / DMSO solution, but 60 μL was prepared for the rotation reaction at high temperatures, taking into account the evaporation of the solvent. The temperature conditions were 10°C, 25°C, 40°C, 55°C, and 70°C. Before the rotation reaction, the lignin stock solution and each EtOH solution were temperature-adjusted using an Eppendorf Thermomixer so that they were the same temperature as during the rotation reaction. The particle size and concentration of the created microparticles were compared by evaluation using electrical resistance nanopulse method (qNANO).
[0224] 5-1-3. Effect of stirring speed on particle size when adding organic solvent The effect of the solution stirring rotation speed conditions during microparticle preparation on the particle size of the microparticles was investigated. The sample used was eucalyptus lignin (PA1%AA, MW50, ACTN). The rotation speed was set at five conditions: 300 rpm, 600 rpm, 900 rpm, 1200 rpm, and 1500 rpm. The particle size of the lignin microparticles was measured using the electrical resistance nanopulse method (qNANO). In addition, the change in particle size was investigated by reacting the microparticles prepared under the rotation reaction conditions of 300 rpm at 1500 rpm. 180 μL of the sample prepared in the 300 rpm mixture was mixed at 25°C and 1500 rpm for 5 minutes (300 to 1500 rpm sample).
[0225] Next, the particle size of the fine particles was evaluated using Eucalyptus LCC lignin (PA1%AA, MW50, ACTN) at four rotation speeds: 300 rpm, 500 rpm, 700 rpm, and 900 rpm. The particle size of the lignin fine particles was also measured using the electrical resistivity nanopulse method (qNANO).
[0226] 5-1-4. Comparison of the effect of centrifugal direction on particle size of microparticles The equipment and rotation direction when mixing the lignin solution with the organic solvent were examined. The effect of vertical and horizontal rotation on the particle size of the lignin microparticles was examined. A 10 w / v% lignin / DMSO solution prepared as in Experimental Method 1-1 and 80 v / v%, 40 v / v%, and 20 v / v% ethanol aqueous solutions were prepared. When mixing the lignin solution and the ethanol aqueous solution, 50 μL of the ethanol aqueous solution was added stepwise starting from the higher concentration, and centrifugation was repeated. For centrifugation, 1000 rpm centrifugation in the X-axis direction using an Eppendorf Themo mixer and 1000 rpm stirring in the X-axis and Y-axis directions using a Lab Serb were used. The obtained lignin microparticles were measured using the electrical resistance nanopulse method (qNANO) of NP400 to measure the particle size.
[0227] 5-1-5. Evaluation of microparticle size under different pH buffer conditions When preparing lignin microparticles, we confirmed whether the particle size and ease of microparticle generation would differ depending on the type of buffer added. The samples used were eucalyptus lignin (PA1%AA, MW50, ACTN) and eucalyptus LCC lignin (PA1%AA, MW50→140, ACTN). Three types of ethanol aqueous solutions were added: 80 v / v%, 40 v / v%, and 20 v / v%, and 50 μL each was prepared for each sample. Ethanol was diluted with each buffer. Buffers were prepared by diluting 1 M MOPS / NaOH buffer (pH 6.4), 1 M PIPES / NaOH buffer (pH 6.2), and 1 M HEPES / NaOH (pH 8.2) to a final concentration of 50 mM. The particle size of the lignin microparticles was evaluated using the electrical resistance nanopulse method (qNANO) of the NP400. In addition, the particle size of LCC lignin microparticles was evaluated by electrical resistance nanopulse method (qNANO) measurements using NP200.
[0228] 5-1-6. Consideration of organic solvent to be added We compared the ease of lignin organization to see how the particle size of the microparticles is affected by the organic solvent used to organize lignin. The samples used were eucalyptus lignin (PA1%AA, MW50, ACTN) and eucalyptus LCC lignin (PA1%AA, MW50→140, ACTN). Lignin organization was carried out under the same conditions as in Experimental Method 1-1. Meanwhile, the organic solvents added were methanol, ethanol, 1-propanol, and 1-buthanol diluted with pure water to 80 v / v%, 40 v / v, and 20 v / v%, respectively. Using the NP400 nanopore, particle size evaluation and concentration difference measurement were performed using electrical resistance nanopulse method (qNANO).
[0229] 5-1-7. Organization of lignin using different resins We investigated whether lignin microparticles could be produced not only from eucalyptus, a broadleaf tree, but also from coniferous trees such as cedar and red pine. Seven types of resins were used: eucalyptus lignin (PA1%AA, MW50, ACTN), eucalyptus LCC lignin (PA1%AA, MW50→140, ACTN), Japanese cedar lignin (H2O23.2%+AA, MW50, 80DOX), Japanese cedar LCC lignin (H2O23.2%+AA, MW50→140, 80DOX), Japanese red pine (H2O23.2%+AA, MW50, ACTN), Japanese red pine LCC lignin (H2O23.2%+AA, MW50→140, ACTN), and bamboo lignin (MS130-5). The particles were micronized and the particle size was evaluated by electrical resistance nanopulse method (qNANO) measurement using NP400.
[0230] [Table 12]
[0231] 5-1-8.Evaluation of fine particles using electrical resistance nanopulse method (electrical resistance nanopulse method (qNANO)) For both NP200 and NP400, the nanopore stretch condition was adjusted to 47 mm. In addition, the voltage was adjusted so that the current value when the buffer was added was approximately 120 nA. First, sample measurement was performed after calibration. The calibration sample used was Mean Dia: 350 nm, Mode Dia: 330 nm, and concentration: 8.4E+11 particles / mL. It was diluted 500-fold with PBS buffer containing surfactant, and 35 μL was applied for measurement. Next, sample measurement was performed. The sample was diluted with PBS buffer, and 35 μL was applied for measurement. Measurement time was within 10 minutes. Clicking was performed when the current value was unstable.
[0232] 5-1-9. Particle size evaluation by dynamic light scattering method Particle size evaluation was performed using a SZ-100 Nanoparticle Size Analyzer (HORIBA). Measurements were performed using a four-sided transmission quartz cell. For sample preparation, the lignin microparticle sample was diluted 100 times with pure water to prepare 2 mL. Measurements were performed in auto mode, and the peak tendency was measured using polydispersion and standard peaks. Measurements were performed three or more times, and the particle size was evaluated by calculating the average value.
[0233] 5-1-10. Particle size evaluation using an interference microscope The particle size of the microparticles was evaluated using a nanoparticle imaging analyzer VIDEO DROP (Meiwafosis). The prepared lignin microparticles were diluted 100 times with pure water and measured. The presence or absence of aggregates was checked on the monitor during measurement. 8 μL of the diluted solution was applied during measurement, and the sample count was measured until it reached 300 or more.
[0234] 5-2.Results 5-2-1. Particle size distribution analysis The analysis results of the particle size and pore passing time for each microparticle are shown in Figure 18. The distribution plotted on the diagonal line indicates that the microparticles have a high degree of sphericity (symmetry).
[0235] 5-2-2. Observation of nanoparticles using a microscope Eucalyptus lignin (PA1%AA, MW50, ACTN) was gradually mixed with an ethanol / water solution to create a poor solvent condition, and lignin microparticles were prepared. A scanning probe microscope SPM-Nanoa (Shimadzu Corporation) was used to observe the shape of the nanoparticles and evaluate their physical properties. The SPM results confirmed that microparticles of less than 100 nm were prepared (Table 13). It was also confirmed that the nanoscale microparticles were spherical in shape (Figure 19). The physical property analysis of the nanoparticles confirmed that the lignin microparticles had a lower affinity with the probe compared to mica, but were relatively soft (Figure 21).
[0236] [Table 13]
[0237] [Table 14]
[0238] Next, LCC lignin nanoparticles prepared from eucalyptus LCC lignin (PA1%AA, MW50→140, ACTN) were observed using a 3D real surface view microscope. The prepared microparticles were dried in a nanopercolator, then osmium coated and observed using a 3D real surface view microscope. Spherical microparticles were observed from the experimental results (Figure 22).
[0239] The particle size of nanoscale LCC lignin microparticles made from Eucalyptus LCC lignin (PA1%AA, MW50→140, ACTN) was evaluated using an interference light microscope and DLS. The experimental results showed that the median diameter was 98 nm and the mode diameter was 105 nm using the interference light microscope, and 90.7 nm and 85.0 nm using DLS, respectively (Table 15). The experimental results using the interference light microscope also confirmed that granular nanoparticles were generated (Figure 23).
[0240] [Table 15]
[0241] 5-2-3. Evaluation of dispersibility of lignin microparticles 5-2-3-1. Zeta potential measurement using electrical resistance nanopulse method (qNANO) Eucalyptus lignin (PA1%AA, MW50, ACTN) and Eucalyptus LCC lignin (PA1%AA, MW50→140, ACTN) were prepared using phosphate buffer at pH 3 to pH 11 in increments of 2, and the zeta potential of the fine particles was measured using the electrical resistance nanopulse method (qNANO) of the NP400. First, calibration was performed. The measured concentration of the calibration was V1P 2,The order was V1P1V2P1V3P1, confirming that the calibration was performed accurately. Furthermore, the calibration particles did not clog the pores, and the particle count was a beautifully proportional line to the measurement time. First, the particle size of the calibration particles was measured. The measurement result showed that the median diameter was 330 nm, confirming that the calibration measurement was performed accurately.
[0242] Zeta potential measurements of lignin microparticles showed that the average absolute value was positive at 30.5 mV under acidic conditions at pH 3, whereas it was negative at -26.6 mV under alkaline conditions at pH 11 (Table 16). Under neutral conditions, microparticles with a particle size of more than 250 nm showed a positive zeta potential, whereas microparticles with a particle size of 300 nm or less were confirmed to be both negatively and positively charged (Figure 28). From this, it was suggested that there may be a correlation between zeta potential and particle size. For LCC lignin microparticles, many positively charged microparticles were observed under all pH conditions (Table 17). At pH 7, microparticles with a particle diameter of 300 nm or less and both positively and negatively charged were observed, similar to lignin microparticles that do not contain polysaccharides (Figure 30). From this point, the plots tended to spread vertically as the pH became more alkaline (Figures 34 and 35).
[0243] [Table 16]
[0244] [Table 17]
[0245] 5-2-3-2. Zeta potential measurement using DLS Eucalyptus lignin (PA 1% AA, MW 50, ACTN) and eucalyptus LCC lignin (PA 1% AA, MW 50→140, ACTN) were prepared using phosphate buffer at pH 2 increments from pH 1 to pH 13, and the zeta potential of the fine particles was measured using DLS. The experimental results showed that the average zeta potential of lignin microparticles became more negative as the pH increased from acidic to alkaline (Table 18). In addition, the most common zeta potentials were positive at 1.67 mV and 1.48 mV at pH 1 and 3, respectively. In addition, multiple zeta potential peaks were observed from neutral conditions, rather than a single peak. On the other hand, the average zeta potential of LCC lignin microparticles was positive at 2.81 mV at acidic pH 1, but was negatively charged at pH 3 to alkaline conditions. In particular, the average zeta potential of -75.6 mV at pH 9 showed a larger absolute zeta potential than lignin microparticles that did not contain polysaccharides (Table 19).
[0246] [Table 18]
[0247] [Table 19]
[0248] From the results of zeta potential measurements using the electrical resistance nanopulse method (qNANO), it was found that the smaller the particle size of the microparticles, the more likely they are to be negatively charged, and that there is a correlation between particle size and zeta potential (Figure 33). Since the particle size analysis ranges differ between the electrical resistance nanopulse method (qNANO) and zeta potential, we assumed that differences in zeta potential occurred, and measured the particle size of LCC lignin microparticles at pH 7 using DLS. As a result, the median size was 113 nm, and the mode particle size was 78.7 nm, which was greater than the mode particle size of 239 nm measured by the electrical resistance nanopulse method (qNANO) (Figure 33), and nanoscale microparticles were observed.
[0249] 5-2-4. Evaluation of particle size persistence of lignin microparticles The degree of change in particle size of lignin microparticles over time was measured. Lignin microparticles were prepared using eucalyptus lignin (PA 1% AA, MW 50, ACTN) and eucalyptus LCC lignin (PA 1% AA, MW 50→140, ACTN) and the degree of change in average particle size and mode particle size over 6 weeks was measured. The particle size of the lignin microparticles at week 0 was shown as 100%, and the experimental results showed the extent to which the particle size was maintained from the following week onwards. For LCC lignin microparticles, the change in average particle size was within 15% even after 6 weeks (Table 20). In addition, the maintenance of the mode particle size after 6 weeks was almost 100% for both lignin microparticles and LCC lignin microparticles (Table 21).
[0250] [Table 20]
[0251] [Table 21]
[0252] [Table 22]
[0253] [Table 23]
[0254] Using Eucalyptus LCC lignin (PA1%AA, MW50→140, ACTN), we prepared microparticles complexed with eosin molecules as a drug model compound for lignin organization. When the fluorescence excitation wavelengths of the prepared eosin complexed microparticles and microparticles without eosin were measured, a shift in the peak wavelength was confirmed (Figures 36 and 37). The peak fluorescence wavelength of the microparticles without eosin was 428 nm and the excitation wavelength was 310 nm, while the peak fluorescence wavelength of the eosin complexed microparticles was 456 nm and the excitation wavelength was 346 nm.
[0255] 5-2-5. Pharmaceutical use combination test Eucalyptus LCC lignin (PA1%AA, MW50→140, ACTN) was combined with diethyl sebacate, which is used in pharmaceuticals and cosmetics, to produce microparticles. Diethyl sebacate is generally used as an emulsifier and to promote the penetration of fat-soluble substances into the stratum corneum and hair. The particle size of the produced microparticles was measured using the electrical resistance nanopulse method (qNANO) and DLS of NP400. Each measurement was performed twice, and the average values are shown in Table 24. The results confirmed that many microparticles of about 300 nm to 400 nm were produced. In addition, the fluorescence excitation spectrum was measured. The experimental results showed that both the fluorescence and excitation wavelengths showed peaks on the long wavelength side compared to the results of the fluorescence excitation spectrum of the microparticles produced from an ethanol aqueous solution (Figure 36). In addition, two peaks were confirmed at a fluorescence wavelength of 450 nm and excitation wavelengths of 279 nm and 370 nm (Figure 39).
[0256] [Table 24]
[0257] 5-2-6.Evaluation of the effect of temperature change on fine particles 5-2-6-1. Particle size evaluation according to temperature change The degree of change in particle size of lignin microparticles due to continuous temperature change was measured. Lignin microparticles were prepared using eucalyptus lignin (PA1%AA, MW50, ACTN) and eucalyptus LCC lignin (PA1%AA, MW50→140, ACTN), and the degree of change in particle size was measured by DLS while increasing the temperature stepwise by 10°C. The experimental results showed that there was no significant change in the particle size of the lignin microparticles even when the temperature was increased after the microparticles were prepared (Table 25). On the other hand, in the case of LCC lignin microparticles, the average particle size became smaller by about 10 nm when the temperature was increased from 20°C to 60°C (Table 26).
[0258] [Table 25]
[0259] [Table 26]
[0260] 5-2-6-2. Zeta potential evaluation by change The change in zeta potential of lignin microparticles due to continuous temperature change was measured. Lignin microparticles were prepared using eucalyptus lignin (PA1%AA, MW50, ACTN), and the zeta potential was continuously measured while increasing the temperature stepwise by 10°C each time. The experimental results showed that the zeta potential value increased as the temperature approached room temperature compared to the low temperature condition (Table 27).
[0261] [Table 27]
[0262] Test Example X. Preparation and analysis of water-in-oil (W / O) and oil-in-water (O / W) self-assemblies Preparation and analysis of water-in-oil (W / O) and oil-in-water (O / W) self-assemblies in lignin-sugar complexes
[0263] The lignin-sugar complex isolated by the A-APA method (microwave treatment at 140°C for 10 minutes, acetic acid-peracetic acid 1% or acetic acid-0.2M hydrogen peroxide conditions) was further dispersed in an aqueous solution, and the insoluble and soluble parts were separated, and the insoluble part was used as the raw material for O / W type and the soluble part was used as the raw material for W / O type. The results of separation using an aqueous solution containing 10% acetic acid are shown in Table 28. The sugar unit content (%) per 100 aromatic rings was calculated from the HSQC NMR spectrum as the ratio of sugar units (calculated from the correlation signal integral value of the anomeric carbon) to aromatic ring units as a percentage.
[0264] [Table 28]
[0265] A 10 wt% aqueous solution of lignin-polysaccharide complex (W / O type) was prepared, and 200 μL of 1-butanol (Fujifilm Wako Pure Chemical Industries, special grade) was added as a separation solvent to 10 μL of the aqueous solution. The addition was performed in the cleaning tank of an ultrasonic cleaner while irradiating ultrasonic waves with a frequency of 28 kHz, and a self-assembled body was obtained. The oil-in-water (O / W) type was prepared in the same manner as described elsewhere.
[0266] The structure of the self-assembled body was measured by a fluorescence microscope (all-in-one fluorescence microscope BZ-X810, manufactured by Keyence). A photograph of the water-in-oil (W / O) type lignin-sugar complex hollow spherical particles derived from red pine is shown in Figure 40.
Claims
1. The hollow spherical particle is a self-assembled body of a lignin-sugar complex, the lignin-sugar complex having at least one bond between the lignin and a polysaccharide selected from the group consisting of an α-ether bond, an α-ester bond, and a γ-ester bond.
2. 2. The hollow spherical particle according to claim 1, wherein the composition ratio of polysaccharide to lignin in the lignin-sugar complex (the ratio obtained by dividing the number of monomer units of polysaccharide by the number of monomer units of lignin) is 0.1 to 10.
3. 2. The hollow spherical particle according to claim 1, wherein the molecular weight (Mw) of the lignin-sugar complex is 2,000 to 10,000 and the polydispersity (Mw / Mn) is 2.5 or less.
4. 2. The hollow spherical particles according to claim 1, which are a population of hollow spherical particles made of lignin-saccharide complexes having an average particle size of 200 nm or more and a positive average zeta potential at pH 7 and room temperature.
5. 2. The hollow spherical particles of claim 1, comprising a population of hollow spherical particles of lignin-saccharide complexes having an average particle size of less than 200 nm and an average negative zeta potential at pH=7 and room temperature.
6. 2. The hollow spherical particles according to claim 1, having a number average particle size of 1 μm or less.
7. 2. The hollow spherical particle according to claim 1, which contains an active ingredient.
8. 8. The hollow spherical particle according to claim 7, wherein the active ingredient is at least one selected from the group consisting of dyes, pesticides, fertilizers, medicines, cosmetic ingredients, fragrances, fluorescent agents, paints, proteins, antibodies, nucleic acids, vaccines, lipids, hormones, sugars, glycosides, surfactants, adhesives, vitamins, coenzymes, minerals, cells, organelles, low molecular weight compounds, high molecular weight compounds, metal complexes, liposomes, and hydrogels.
9. The hollow spherical particle according to claim 1, which exhibits long wavelength fluorescence of 450 nm or more.
10. A drug delivery or introduction agent comprising the hollow spherical particles according to any one of claims 1 to 9.
11. The drug delivery or introduction agent of claim 10 , wherein the drug is a nucleic acid.
12. An ultraviolet absorber comprising the hollow spherical particles according to any one of claims 1 to 9.
13. A light resistance imparting agent comprising the hollow spherical particles according to any one of claims 1 to 9.
14. An anti-Stokes fluorescent agent comprising the hollow spherical particle according to any one of claims 1 to 9.