Ni-BASED ALLOY FLUX-CORED WIRE
The Ni-based alloy flux-cored wire with controlled component ratios addresses issues of bead appearance and crack resistance by optimizing manganese and niobium contents, achieving superior weld metal quality and stability in multi-position welding.
Patent Information
- Application Number
- JP2024141752
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2019-11-29
- Filing Date
- 2024-08-23
- Publication Date
- 2024-12-03
AI Technical Summary
Ni-based alloy flux-cored wires experience issues with bead appearance, arc stability, spatter suppression, and crack resistance due to the accumulation of gas at the interface between the Ni-based alloy and solidified slag, and the limitations on manganese content to prevent slag removability deterioration.
A Ni-based alloy flux-cored wire with specific compositions and ratios of components, including 0.1-3.0wt% Mn, 0-2.9wt% Nb, 5.0-10.0wt% Mo, 3.0-9.0wt% Fe, and 0.5-3.0wt% SiO2, along with controlled oxide contents, to ensure favorable bead appearance, arc stability, and crack resistance.
The wire produces weld metal with excellent bead appearance, strength, defect resistance, and crack resistance, enabling multi-position welding with improved slag removability and arc stability.
Smart Images

Figure 2024167274000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a Ni-based alloy flux-cored wire, and more particularly to a Ni-based alloy flux-cored wire in which the contents of Mn and Nb are adjusted so that a weld metal having favorable bead appearance, arc stability, spatter suppression effect, excellent strength, defect resistance, and crack resistance can be obtained from the wire. [Background technology]
[0002] In the 20th century, superalloys (called superalloys) have been widely used as basic structural materials in high-tech industries such as aerospace, nuclear power, power plants, and petrochemical industries. Among them, Ni-base alloys are precipitation hardening alloys that use the precipitation phenomenon of austenite phase in face-centered cubic (FCC) lattice. Ni-base alloys have the best performance among superalloys and are widely used as structural materials for many parts that operate under high stress at high temperatures, such as gas turbine blades, disks, and combustion chambers. They have favorable stiffness, strength, and toughness at high temperatures such as 980°C, and are particularly resistant to oxidation and corrosion. They are also resistant to phosphoric acid solutions. Therefore, they are used in piping and offshore valve equipment in chemical processing and pollution control facilities.
[0003] Welding materials containing Ni-base alloys as components are used for welding highly corrosion-resistant austenitic stainless steels, or Ni-base alloys used in structural members of chemical plants and petroleum-related equipment, or for welding 9% nickel steels used as structural members of storage tanks for LNG, liquid nitrogen, liquid oxygen, etc.
[0004] Among many Ni-base alloys, Inconel 625 alloy (Ni-Cr-Mo-Nb alloy) has excellent weldability. Several welding techniques are often used for these alloys, including gas tungsten arc welding (GTAW), shielded metal arc welding (SMAW), gas metal arc welding (GMAW), submerged arc welding (SAW), and flux cored arc welding (FCAW).
[0005] The development of welding materials for FCAW has lagged behind other welding materials, but recently welding materials that can be used in the vertical upward welding position have been developed, and the frequency of use is gradually increasing. In recent years, in conjunction with special welding materials such as Ni-base alloys, the use of gas-coated metal arc welding using Ni-base alloy flux-cored wires, which provides relatively high work efficiency compared to coated metal arc welding and TIG welding, has been increasing.
[0006] However, in the case of gas-clad welding using Ni-based alloy flux-cored wire, since Ni-based alloy has a low melting point, the gas is likely to accumulate at the interface between itself and the solidified slag, resulting in pitting of the weld metal.Furthermore, there is a problem that the content of magnesium (Mn) must be limited to a very small amount to prevent the deterioration of slag removability, as disclosed in Korean Patent No. 10-1708997 and Korean Patent No. 10-1760828. Summary of the Invention [Problem to be solved by the invention]
[0007] An object of the present invention is to provide a Ni-based alloy flux-cored wire that solves the above problems. [Means for solving the problem]
[0008] In order to achieve the above object, the present invention provides a Ni-based alloy flux-cored wire having a Ni-based alloy sheath filled with flux, and the overall composition including the sheath components and the flux components provided in the sheath is 0.1 wt% or less (excluding 0 wt%) of C, 0.01-0.5 wt% of Si, 0.01-0.3 wt% of Mn, 15.0-22.0 wt% of Cr, 0-2.9 wt% of Nb (excluding 0%), 5.0-10 wt% of Mn, and 0.01-0.5 wt% of Mn, based on the total weight of the flux-cored wire. The Ni-based alloy flux-cored wire contains 0.0wt% Mo, 3.0-9.0wt% Fe, and the remainder including Ni and unavoidable impurities, contains SiO2 in an amount of 0.5-3.0wt%, at least one oxide selected from Na2O, K2O, MgO, and CaO in an amount of 0.1-3.0wt%, and at least one of Al2O3, TiO2, and ZrO2 in an amount of 5.0-12.0wt%, and satisfies [Relationship 1] and [Relationship 2]. [Equation 1] 0.1Na2O+{K2O+0.5(MgO+Al2O3)} / {CaO+1.6(TiO2+SiO2)+0.2(ZrO2)}<0.5 [Equation 2] 0.01Mn≦Nb≦(0.01Mn)+3.3
[0009] Furthermore, in order to achieve the above-mentioned object, the present invention provides a Ni-based alloy flux-cored wire having a Ni-based alloy sheath filled with flux, and a weld metal obtained from the flux-cored wire has a composition including 0.1 wt% or less (excluding 0 wt%) C, 0.01-0.5 wt% Si, 0.01-3.0 wt% Mn, 15.0-20.0 wt% Cr, 0-3.5 wt% (excluding 0 wt%) Nb, 5.0-15.0 wt% Mo, 3.0-9.0 wt% Fe, the balance being Ni and unavoidable impurities, and the composition of the weld metal satisfies [Relationship 3]. [Equation 3] [Fe+{15(2.8Nb+0.85Mn)}] / (Cr+Mo)<7.0 Effect of the Invention
[0010] The Ni-base alloy flux-cored wire of the present invention can produce a weld metal having excellent bead appearance in welding Ni-base alloys, 9% Ni steels, and highly corrosion-resistant austenitic stainless steels, and can produce a weld metal having favorable strength, defect resistance, and crack resistance. [Brief description of the drawings]
[0011] [Figure 1] FIG. 1 is a photograph showing cracks in a weld bead according to an exemplary composition of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] The present invention will be described in detail below.
[0013] In this document, the flux-cored wire is a Ni-based alloy flux-cored wire in which the Ni-based alloy sheath is filled with flux.
[0014] As used herein, the term "weld metal" refers to the metal resulting from solidification of a molten mixture of the weld metal and base metal during welding.
[0015] As used herein, the term "deposited metal" refers to metal transferred from the filler metal (i.e., wire), which is the metallic material added to the weld metal area during welding.
[0016] According to one aspect of the present invention, there is provided a flux-cored wire having an internal sheath. The flux cored wire is a Ni-based flux cored wire containing Ni, Cr, Mn and Ni in predetermined amounts expressed as weight percent with respect to the total weight of the wire.
[0017] More specifically, a Ni-based alloy flux-cored wire is provided having a Ni-based alloy sheath with flux therein, and the total wire composition including the sheath components and the flux components provided in the sheath includes, based on the total weight of the entire flux-cored wire, 0.05-0.5 wt% Si, 0.01-3.0 wt% Mn, 15.0-22.0 wt% Cr, 0-2.9 wt% (excluding 0%) Nb, 5.0-10.0 wt% Mo, 3.0-9.0 wt% Fe, the balance being Ni and unavoidable impurities. SiO2 is included in an amount of 0.5-3.0 wt%, at least one oxide of Na2O, K2O, MgO and CaO is included in an amount of 0.1-3.0 wt%, and at least one oxide of Al2O3, TiO2 and ZrO2 is included in an amount of 5.0-12.0 wt%. The composition satisfies [Relationship 1] and [Relationship 2]. [Equation 1] 0.1Na2O+{K2O+0.5(MgO+Al2O3)} / {CaO+1.6(TiO2+SiO2)+0.2(ZrO2)}<0.5 [Equation 2] 0.01Mn≦Nb≦(0.01Mn)+3.3
[0018] The reasons for limiting the composition of the flux-cored wire are explained below. Unless otherwise specified below, the content of each component in the composition is represented by "% by weight (wt%)". The content of each component includes the amount of the component initially contained in the alloy sheath and the amount of the component in the form of metal powder or alloy powder added from the flux.
[0019] Cr: 15.0-22.0wt% Chromium (Cr) is added to improve the strength and corrosion resistance of the weld metal. If the chromium content is less than 15.0wt%, the corrosion resistance decreases and it becomes difficult to obtain a certain strength of the weld metal. Meanwhile, Cr combines with C to form carbides. If the chromium content is more than 22.0wt%, excessive chromium carbides are generated, resulting in a decrease in the toughness of the weld metal. Therefore, the chromium content in the flux-cored wire is set to 15.0-22.0wt% based on the total weight of the wire. More specifically, the Cr content is 16-18wt%.
[0020] Mo: 5.0-10wt% Molybdenum (Mo) is a component that combines with carbon (C) to form carbides, and is an element that is advantageous in improving friction resistance, hardness, and corrosion resistance. If the Mo content is less than 5 wt%, it is difficult to obtain the above effects, while if the Mo content is more than 10.0 wt%, Mo precipitates as a Laves phase, resulting in a decrease in crack resistance.
[0021] Therefore, in the present invention, it is preferable to limit the Mo content to 5-10 wt% based on the total weight of the wire, and more specifically, the Mo content is set to 5-8 wt%.
[0022] C: 0.1wt% or less (excluding 0wt%) Carbon (C) has the effect of improving the strength of the weld metal, but if it is added in excess, there is a problem that carbides are formed and toughness is reduced. Therefore, the C content is set to 0.1 wt% or less based on the total weight of the wire. There is no particular lower limit for the C content. In order to prevent a decrease in the toughness of the weld metal, it is preferable that the C content be in the range of 0.1 wt% or less.
[0023] Mn: 0.01-3.0wt% Manganese (Mn) is added to improve the bead shape of the weld metal and to improve the defect resistance and crack resistance. If the manganese content is less than 1.0 wt%, it is not preferable because it does not provide sufficient deoxidization effect. If the manganese content is more than 10.0 wt%, the segregation of the weld metal accelerates in the final solidification region, thus lowering the melting point of the molten metal and reducing the hot crack resistance. Therefore, the manganese content is preferably limited to 1.0-10.0 wt%. In the existing Ni-base flux-cored wire, the Mn content is limited to prevent a sudden decrease in toughness. However, in the present invention, the Mn content is increased to improve the crack resistance, but the Nb content is limited to reduce the toughness as described below.
[0024] Mn has the effect of reducing crack resistance by combining with Ni, and reducing the harmful effect of S by combining with S. Mn also has the effect of improving mechanical properties by promoting deoxidation of the welded area. If the Mnmp content is less than 0.01wt%, Mn cannot combine with S sufficiently, so it is difficult to obtain the effect of improving crack resistance and sufficient deoxidation effect. Therefore, it is not preferable that the Mn content is less than 0.01wt%. Furthermore, if the Mn content exceeds 3.0wt%, it is not preferable because the melting point of the slag melting is lowered due to the formation of MnO, resulting in deterioration of multi-position work performance and slag removability. Therefore, the Mn content is set to be in the range of 0.01-3.0wt% based on the total weight of the wire. More specifically, Mn is included in an amount of 0.5-3.0wt%.
[0025] Nb: 0-2.9wt% or less (excluding 0wt%) Niobium (Nb) may be added to improve the strength of the weld metal. Niobium (Nb) combines with carbon or nitrogen to form carbides, nitrides, or carbonitrides, thereby having a precipitation hardening effect. However, if the content is increased excessively, there is a problem that it precipitates as Laves phase, resulting in a reduced crack resistance.
[0026] Therefore, in the present invention, Nb is not added at all or the Nb content is limited to 2.9wt% or less (i.e., Nb is 0-2.9wt%). Preferably, Nb is added in an amount of 2wt% or less, more preferably 0.5wt% or less. The present invention is characterized in that the workability and physical properties are ensured by adjusting the Mn content while limiting the Nb content.
[0027] Fe: 3.0-9.0wt% Iron (Fe) is an essential element in the raw materials for welding materials or Ni-based alloys, and is a component for obtaining ductility of the metal. If the Fe content is less than 3.0 wt%, the required ductility of the weld metal cannot be obtained, while if the Fe content exceeds 9.0 wt%, the high temperature crack resistance decreases. Therefore, in the present invention, it is preferable to limit the Fe content to the range of 3.0-9.0 wt% based on the total weight of the wire. Furthermore, if Cu is included, Fe forms a compound with Cu (copper) and causes cracks, so it is preferable to control the Cu content together with the Fe content.
[0028] Si: 0.01-0.5wt% Silicon (Si) is an ingredient that improves deoxidation and weldability. If the Si content is less than 0.01wt%, the deoxidation effect is insufficient. If the Si content is more than 0.5wt%, it is not preferable because it increases the cracking sensitivity due to the generation of Laves phase. Therefore, it is preferable to limit the Si content to the range of 0.01-0.5wt%.
[0029] P+S: 0.01wt% or less (excluding 0wt%) Phosphorus (P) and sulfur (S) are elements that affect hot cracking. P and S have low melting points, which cause hot cracking. In the present invention, P or S may be included, and the total content of P and S is preferably less than 0.01 wt%.
[0030] The remaining component of the present invention is nickel (Ni).
[0031] Ni stabilizes the austenite structure and combines with Nb to form precipitates, thereby improving tensile strength. Preferably, the Ni content is limited to the range of 45-60wt%. If the Ni content is less than 40wt%, the contents of other elements increase, making the structure unstable and reducing toughness. If the Ni content is more than 60wt%, the amounts of Cr, Mo, etc. decrease relatively, reducing corrosion resistance or strength. Therefore, the Ni content in the flux-cored wire is set to the range of 45-60wt% with respect to the total weight of the wire. More specifically, the Ni content is set to the range of 50-60wt%.
[0032] SiO 2 : 0.5-3.0wt% SiO2 is a slag-forming material and acts to increase the fluidity and ductility of the weld bead. For this effect, SiO2 is preferably added in an amount of 0.5 wt% or more. Furthermore, if the SiO2 content is more than 3.0wt%, the Si content in the weld metal will increase, resulting in a decrease in crack resistance. Therefore, it is preferable to limit the SiO2 content to the range of 0.5-3.0wt%.
[0033] Na 2 O and K 2 One or more oxides selected from O: 0.1-3.0 wt% It is advisable to add alkali metal oxides in an amount of 0.1 wt% or more to reduce the ionization potential of the arc during welding, making it easier to generate the arc, and maintaining a stable arc during welding. Furthermore, if the content of alkali metal oxides is more than 3.0 wt%, excessive welding fumes will be generated due to high vapor pressure. Therefore, it is preferable to limit the content of alkali metal oxides to 0.1-3.0 wt%. The alkali metal oxides may include either one or both of Na2O and K2O.
[0034] Al 2 O 3 , TiO 2 and ZrO 2 One or more oxides selected from the following: 5.0-12.0 wt% in total Al, Ti and Zr oxides may be added to increase the melting point of the slag and improve the workability of multi-spot welding. If the total content of Al, Ti and Zr oxides is less than 5.0wt%, the amount of slag will be insufficient, and therefore the slag coverage will be reduced. If it is more than 12.0wt%, slag inclusion defects may occur. Therefore, it is preferable to limit the total content of Al, Ti and Zr oxides to the range of 5.0-12.0wt%.
[0035] The flux-cored wire of the present invention may further contain titanium (Ti) in an amount of 0.2wt% or less. Ti can improve strength due to the effect of precipitation hardening in Ni-based alloys and reduce pore formation due to its action as a deoxidizing component. If the Ti content is more than 0.2wt%, it is not preferred because excessive precipitation reduces the low-temperature impact toughness and crack resistance of the welded area.
[0036] On the other hand, in the flux-cored wire of the present invention, it is preferable to control the content of each oxide so as to satisfy the following [Relationship 1]. In particular, it is preferable to control so that the value defined by [Relationship 1] is smaller than 0.5. If the value is 0.5 or more, the quality of the weld metal region is deteriorated due to the deterioration of weldability and cracking properties. [Equation 1] 0.1Na2O+{K2O+0.5(MgO+Al2O3)} / {CaO+1.6(TiO2+SiO2)+0.2(ZrO2)}<0.5
[0037] Furthermore, in the present invention, it is preferable to control the contents of Mn and Nb so as to satisfy [Relationship 2]. In the case of chemical compositions that do not satisfy [Relationship 2], harmful phases are generated according to the contents of Mn and Nb, so it is difficult to ensure desirable physical properties of the weld metal region. [Equation 2] 0.01Mn≦Nb≦(0.01Mn)+3.3
[0038] The flux composition of the flux-cored wire according to the present invention may further comprise up to 0.1 wt% MnO and 0.1-1.5 wt% fluorine compounds with respect to F. In addition to the above components, unintentional impurities from raw materials and the surrounding environment may be inevitably incorporated during normal manufacturing processes.
[0039] According to another aspect of the present invention, in a Ni-based alloy flux-cored wire in which a Ni-based alloy sheath is filled with flux, a weld metal obtained from the flux-cored wire contains 0.1 wt% or less (excluding 0 wt%) C, 0.01-0.5 wt% Si, 0.01 wt%-3.0 wt% Mn, 15.0-22.0 wt% Cr, 0-2.9 wt% (excluding 0 wt%) Nb, 5.0-10.0 wt% Mo, 3.0-9.0 wt% Fe and Ni, and the balance including unavoidable impurities, and the composition of the weld metal satisfies [Relationship 3], which is [Fe + {15 (2.8Nb + 0.85Mn)}] / (Cr + Mo) < 7.0.
[0040] The composition of the flux-cored wire alloy according to the present invention allows for multi-position welding and provides a weld metal with excellent strength and toughness. The content of each component includes the amount of the component originally contained in the alloy sheath and the amount of the component in the form of metal powder or alloy powder added from the flux.
[0041] The Cr content of the weld metal obtained from the flux-cored wire according to the present invention may be 15-20wt%. Chromium (Cr) is added to improve the strength and corrosion resistance of the weld metal. If the Cr content is less than 15wt%, the corrosion resistance decreases and it becomes difficult to obtain a certain strength of the weld metal. Meanwhile, Cr combines with C to form carbides. If the Cr content is more than 20wt%, the toughness of the weld metal decreases and the growth of carbides is suppressed.
[0042] The content of Mo may be in the range of 5-15wt%. Molybdenum (Mo) is a component that combines with carbon (C) to form carbides, and plays an advantageous role in improving wear resistance, hardness, and corrosion resistance. If the content of Mo is less than 5wt%, it is difficult to obtain the above-mentioned effects, while if the content of Mo is more than 15wt%, Mo precipitates, thereby reducing crack resistance. More specifically, the content of Mo may be in the range of 5-8wt%.
[0043] The C content may be 0.1 wt% or less. Carbon (C) has the effect of improving the strength of the weld metal, but if it is added in excess, carbides are formed, which causes a problem of reduced toughness. More preferably, in order to prevent a decrease in the toughness of the weld metal, the C content may be set to 0.1 wt% or less.
[0044] The Mn content may be in the range of 0.01-3.0wt%. Manganese (Mn) is added to improve the bead shape of the weld metal and to improve defect resistance and crack resistance. In the present invention, the crack resistance is improved by increasing the Mn content, and as described below, the toughness reduction is prevented by limiting the Nb content. In the present invention, if the Mn content is less than 0.01wt%, the bonding with S is insufficient, so the effect of improving the crack resistance is not obtained, and sufficient deoxidization effect is not obtained. Therefore, it is not preferable that the Mn content is less than 0.01wt%. Furthermore, if the Mn content is more than 3.0wt%, the peelability will be reduced. Therefore, it is not preferable that the Mn content is more than 3.0wt%. More preferably, the Mn content is in the range of 0.5-3.0wt%.
[0045] The Nb content may be in the range of 0-3.5wt% (excluding 0wt%). Niobium (Nb) may be added for the purpose of improving the strength of the weld metal. Niobium (Nb) combines with nitrogen or nitrogen to form carbides, nitrides or carbonitrides, thereby having a precipitation strengthening effect. However, if the content is excessively increased, there is a problem that crack resistance decreases. Therefore, in the present invention, Nb is not added at all or the Nb content is limited to 3.5wt% or less. Preferably, Nb is added in an amount of 2.9wt% or less, more preferably 2.0wt% or less. The present invention has the characteristic that the Nb content is limited and the Mn content is adjusted to an appropriate range to ensure a certain degree of strength.
[0046] The Fe content may be in the range of 3.0-9.0wt%. Fe is an essential element in Ni-based alloy welding materials or base materials. Iron (Fe) is an essential element in Ni-based alloy welding materials or base materials, and is a component for ensuring the ductility of the metal. If the Fe content is less than 3.0wt%, the required ductility of the weld metal cannot be obtained, while if the Fe content is more than 9.0wt%, the high temperature crack resistance decreases. Therefore, such a Fe content range is not preferable. Therefore, in the present invention, it is preferable to limit the Fe content to the range of 3.0-9.0wt% based on the total weight of the wire. Furthermore, if Cu is additionally contained, Fe forms a compound with Cu (copper) and causes cracks, so it is preferable to control the Fe content in addition to the Cu content.
[0047] The Si content may be in the range of 0.01-0.5wt%. If the Si content is less than 0.01wt%, the deoxidizing effect is insufficient. If the Si content is more than 0.5wt%, the crack susceptibility increases due to the formation of Laves phase, which is not preferable. Therefore, it is preferable to limit the Si content to 0.5wt% or less.
[0048] In addition, titanium (Ti) may be included in an amount of 0.2wt% or less. Ti can improve the strength in Ni-based alloys due to its precipitation hardening effect and reduce pore formation by acting as a deoxidizing component. If the Ti content is more than 0.2wt%, it is not preferred because excessive precipitation reduces the low-temperature impact toughness and crack resistance of the weld area.
[0049] The balance may be Ni and unavoidable impurities.
[0050] On the other hand, it is preferable that the components of the deposited metal obtained from the Ni-based alloy flux-cored wire of the present invention satisfy the following [Relationship 3]. [Equation 3] [Fe+{15(2.8Nb+0.85Mn)}] / (Cr+Mo)<7.0
[0051] Specifically, the composition of the weld metal is preferably determined so that the value defined by [Relationship 3] is less than 7.0. If the value is 7.0 or more, it becomes difficult to ensure excellent weld quality due to a decrease in weldability and crack resistance.
[0052] The Ni-based alloy flux-cored wire according to the present invention does not contain tungsten (W), but contains large amounts of chromium (Cr) and manganese (Mn), and a limited amount of niobium (Nb) to improve slag removability and crack resistance and to obtain desired physical properties such as strength.
[0053] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these examples.
[0054] A flux-cored wire was prepared containing the components shown in Table 1. Examples of each component will be described below. [Table 1]
[0055] Flux cored arc welding (FCAW) was performed with each welding material. For FCAW, welding was performed with a heat input of 8.0–12.0 kJ / cm in a 100% CO2 protective gas environment. A wire with a diameter of 1.2 mm was used for FCAW. A bevel was formed on an A36 steel plate with a thickness of 7 mm so that the bevel angle of the groove surface was 30°, and the groove was buttered with the test wire to form a buttered layer. The buttered base material was then aligned with a root gap of 12 mm, and a backing plate (steel material) with a similarly buttered surface was placed on the narrow side of the groove. Welding was performed at this bevel to form a welded joint.
[0056] After that, taking into consideration the arc stability and the slag removability of the obtained welded joints, the multi-position welds were visually compared and evaluated, and the weld quality was classified into four levels: ◎ (excellent), O (good), △ (passable), and X (unacceptable). The results are shown in Table 2. [Table 2]
[0057] Referring to Table 2, it was confirmed that the crack resistance and bead appearance were improved in the welded joint of the flux-cored wire in which the Mn and Nb contents were within the ranges proposed in the present invention. In particular, it is possible to determine the ranges of the manganese and niobium contents in which the bead appearance, slag removability, and crack resistance are improved.
[0058] With reference to Composition Examples 1-11, even when the niobium content was 2.5 wt% or more, increasing the manganese content improved the crack resistance and bead appearance.
[0059] With reference to Composition Examples 12-20, it was confirmed that even if the manganese content was more than 2 wt%, there were no problems with crack resistance and slag removability as long as the niobium content was limited to 2.9 wt% or less.
[0060] Further, with reference to Composition Example 24 in relation to Relation 1, when the value of Relation 1 is greater than 0.5, problems arise with respect to arc stability, bead appearance, and slag removability in addition to crack resistance.
[0061] Meanwhile, the crack ratio according to the niobium content was investigated. The crater crack ratio and bead crack ratio of beads according to composition examples 13-20 with different niobium contents are shown in Table 3 below. Figure 1 is a photograph showing cracks (cracks) in weld beads according to exemplary compositions of the present invention. In Figure 1, (a) is a photograph of a weld bead according to composition example 15, (b) is a photograph of a weld bead according to composition example 17, (c) is a photograph of a weld bead according to composition example 18, and (d) is a photograph of a weld bead according to composition example 20. [Table 3]
[0062] 1, the crack ratio can be significantly reduced by controlling the niobium content. In particular, when comparing the crack ratios of Composition Example 17 and Composition Example 18, it was found that the crack ratio differed by about 20% at a Nb content of 2.9 wt%, which is the upper limit of the niobium content range of the present invention.
[0063] Furthermore, the yield strength (YS, MPa), tensile strength (TS, MPa), elongation (EL, %), and Charpy impact energy (J) at -196°C of the obtained welded joints were measured. The results are shown in Table 4 below. [Table 4]
[0064] Referring to Table 4, it was confirmed that, unlike conventional Ni-based alloy flux-cored wires, physical properties such as strength are maintained even if the manganese content is increased and the niobium content is decreased. The addition of niobium provided the desired strength in the absence of tungsten, and it was determined that the problems caused by the relatively low niobium content compared to conventional flux-cored wires could be overcome by increasing the chromium content.
[0065] The Ni-based alloy flux-cored wire according to the present invention has excellent high-temperature crack resistance and satisfactory impact toughness and strength by controlling the contents of manganese and niobium. The Ni-based alloy flux-cored wire according to the present invention can solve the problems of conventional wires, including low crack resistance and low workability caused by Ni alloys.
[0066] The features and technical advantages of the present invention have been described above in a broad manner so that the appended claims may be better understood. Those skilled in the art will appreciate that the present invention may be embodied in other different forms without departing from the technical spirit or basic characteristics of the illustrated embodiments. It will therefore be understood that the above-described examples are for illustrative purposes only and are not limiting in all respects. The scope of the present invention is defined by the following claims, not the above detailed description, and all changes or modifications that come within the meaning and scope of the claims, and their equivalents, should be construed as being within the scope of the present invention.
Claims
1. A Ni-based alloy flux-cored wire having a Ni-based alloy sheath having flux therein, The total wire composition, including the sheath components and the flux components provided in the sheath, comprises, based on the total weight of the flux-cored wire, 0.1 wt% or less (except 0 wt%) C, 0.01-0.5 wt% Si, 0.01-3.0 wt% Mn, 15.0-22.0 wt% Cr, 0-2.9 wt% Nb (except 0 wt%), 5.0-10.0 wt% Mo, 3.0-9.0 wt% Fe, the balance being Ni, and unavoidable impurities; SiO 2 is included in an amount of 0.5-3.0 wt %, Na 2 O.K. 2 At least one oxide of O, MgO, and CaO is included in an amount of 0.1-3.0 wt %; A 2 O 3、 TiO 2 and ZrO 2 At least one oxide of is included in an amount of 5.0-12.0 wt %; The composition satisfies the following [Relationship 1] and [Relationship 2]: Ni-based alloy flux cored wire. [Relationship 1] 0.1Na 2 O+{K 2 O+0.5(MgO+Al 2 O 3 )} / {CaO+1.6(TiO 2 +SiO 2 )+0.2(ZrO 2 )}<0.5 [Relationship 2] 0.01Mn≦Nb≦(0.01Mn)+3.3
2. The flux components further comprise 0.1 wt % (except 0 wt %) MnO and a fluorine compound in the amount of 0.1-1.5 wt % F; The Ni-based alloy flux-cored wire according to claim 1.
3. A Ni-based alloy flux-cored wire having a Ni-based alloy sheath filled with flux, A weld metal obtained from the flux-cored wire has a composition comprising 0.1 wt% or less (excluding 0 wt%) C, 0.01-0.5 wt% Si, 0.01-3.0 wt% Mn, 15.0-22.0 wt% Cr, 0-2.9 wt% Nb (excluding 0 wt%), 5.0-10.0 wt% Mo, 3.0-9.0 wt% Fe, and the balance including Ni and unavoidable impurities; The composition of the deposited metal satisfies [Relationship 3], Ni-based alloy flux cored wire. [Relationship 3] [Fe+{15(2.8Nb+0.85Mn)}] / (Cr+Mo)<7.0
Citation Information
Patent Citations
Flux-cored wire for welding ni alloy
JP1997314382A
Ni-BASED ALLOY FLUX-CORED WIRE
JP2011140064A
Flux-cored wire for gas shield arc welding, and welding method
JP2019093428A