Sputtering device
The film forming apparatus addresses non-uniform target erosion and contamination issues in sputtering by using a plasma diffusion prevention plate and inductively coupled plasma to achieve high-quality, reproducible thin films with enhanced plasma density and reduced impurities.
Patent Information
- Application Number
- JP2024147157
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2020-06-23
- Filing Date
- 2024-08-29
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2041-06-22
AI Technical Summary
Conventional sputtering methods, including magnetron and inductively coupled plasma (ICP) sputtering, face issues such as non-uniform target erosion, target cracking, localized plasma concentration leading to thermal stress, and contamination from impurities like oxygen molecules and moisture, which affect film quality and reproducibility.
A film forming apparatus with a plasma diffusion prevention plate and inductively coupled plasma generation, which confines plasma near the target, uses a negative pulse voltage, and includes a configuration to prevent impurities from entering the deposition chamber, allowing for higher plasma density and uniform film deposition.
This configuration enhances film quality by preventing plasma spread, reducing impurity incorporation, and increasing sputtering rates, resulting in high-density, reproducible thin films with improved thermal stability and reduced contamination.
Smart Images

Figure 2024167324000001_ABST
Abstract
Description
[Technical field]
[0001] One embodiment of the present invention uses inductively coupled plasma (ICP). This relates to the film forming apparatus used. [Background technology]
[0002] Sputtering is a type of physical vapor deposition (PVD) method used to deposit thin films. The sputtering method generates plasma in a vacuum and ions in the plasma are spun at high speed. Sputtering is caused by colliding with a sputtering target, and the target A thin film is formed by depositing particles (atoms or molecules) of the film-forming material that constitutes the surface of a substrate. This is known as a technique for
[0003] The sputtering device has a magnetron placed behind the sputtering target. The magnetron method is well known, but there are also other methods such as inductively coupled plasma (ICP). A sputtering apparatus using induction is also disclosed (see, for example, Patent Document 1). An antenna structure for generating a coupled plasma has also been disclosed (see Patent Document 2). [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2016-065299 A [Patent Document 2] JP 2016-072168 A Summary of the Invention [Problem to be solved by the invention]
[0005] In the magnetron sputtering method, the magnetic field (magnetic field strength) generated by a magnet is Since the sputtering target is not uniform, the erosion of the sputtering target is not uniform. The effective utilization rate of the target material is low, and nodules are easily generated. The plasma is concentrated locally due to the magnetic field, so the target material is easily subjected to thermal stress. There is a problem that cracks are easily generated in the get material.
[0006] In addition, when forming a metal film by magnetron sputtering, the magnet A strong magnetic field can increase the density of the deposited film. However, for oxide materials (e.g. For example, when forming an oxide semiconductor film or an oxide conductive film, oxygen gas is decomposed. Only the area with a strong magnetic field near the sputtering target is left, and unreacted oxygen molecules ( O2) is adsorbed on the deposition surface and is incorporated into the film in the form of oxygen molecules, However, there is a problem in that the density of the material decreases.
[0007] In addition, in conventional sputtering equipment using inductively coupled plasma (ICP), In order to generate a combined plasma efficiently, the antenna body and the antenna are placed inside the deposition chamber. A cylindrical tube of insulating material was installed, but the deposition chamber was enlarged to over 3m. In this case, the antenna body and the cylindrical insulating tube that covers the antenna can be stably held. It has become extremely difficult to do so.
[0008] Furthermore, inductively coupled plasma (ICP) sputtering as disclosed in Patent Document 1 is also used. In the deposition equipment, the generated inductively coupled plasma diffuses throughout the entire interior of the deposition chamber, Plasma is confined near the sputtering target like in magnetron sputtering equipment. Therefore, the deposition chamber is smaller than that of the magnetron sputtering device. Moisture (H2O), oxygen (O2), and hydrocarbons adsorbed on the inner wall at the start of film formation In principle, they are easily detached in large quantities from the inner walls of the deposition chamber and are easily incorporated into the coating during deposition. In order to increase the plasma density near the sputtering target, The only way to do this is to increase the current flowing through the tenna body, which in turn moves it away from the inner wall of the deposition chamber. This increases the amount of contaminant gases that escape, reducing the reproducibility of the film quality of the deposited film. It is as follows.
[0009] In view of such problems, one embodiment of the present invention provides a method for forming a film by sputtering, comprising the steps of: To provide a film forming method and apparatus capable of forming high-quality thin films with good reproducibility and efficiency. The purpose of this document is to [Means for solving the problem]
[0010] The film formation apparatus according to one embodiment of the present invention includes a film formation chamber in which a sputtering target is installed. The chamber covers the sputtering target and overlaps the surface of the sputtering target. a plasma diffusion prevention plate having an opening at a position adjacent to the sputtering target; An inductively coupled plasma detector that protrudes into the area surrounded by the plasma diffusion prevention plate. The antenna for plasma generation and the plasma diffusion prevention plate are placed inside the plate to introduce gas into the deposition chamber. A negative pulse voltage is applied to the sputtering target. will be added. Effect of the Invention
[0011] According to one embodiment of the present invention, the plasma diffusion prevention plate is an antenna for inductively coupled plasma generation. The nozzle is provided to cover the nozzle and the sputtering target, thereby enabling inductively coupled plasma It is possible to prevent the gas from spreading throughout the entire inner space of the deposition chamber, and the gas can be prevented from spreading to the thin film being deposited. It is possible to prevent impurities from being taken in. Furthermore, the sputtering target The plasma density in the vicinity can be increased, so the sputtering rate can also be increased. It is Noh. [Brief description of the drawings]
[0012] [Figure 1] 1 shows an overall configuration of a film forming apparatus according to an embodiment of the present invention. [Diagram 2] FIG. 1 is a diagram showing the configuration of a film formation apparatus according to one embodiment of the present invention, illustrating the main components provided in or connected to a pre-treatment chamber, a transfer chamber, and a film formation chamber, excluding a load / unload chamber. [Diagram 3] 1 is a schematic partial cross-sectional view of a film formation chamber of a film formation apparatus according to an embodiment of the present invention, as viewed from above; [Figure 4] 2 shows a detailed cross-sectional structure of an antenna for generating inductively coupled plasma used in a film formation apparatus according to one embodiment of the present invention. [Diagram 5] 2 shows a detailed cross-sectional structure of an antenna for generating inductively coupled plasma used in a film formation apparatus according to one embodiment of the present invention. [Figure 6] 1 is a schematic diagram showing a plasma diffusion prevention plate provided in a film formation chamber of a film formation apparatus according to an embodiment of the present invention, as viewed from the front. [Figure 7] 1 is a schematic diagram showing a plasma diffusion prevention plate provided in a film formation chamber of a film formation apparatus according to an embodiment of the present invention, as viewed from the front. [Figure 8A] 1 is a diagram for explaining the influence of an antenna for generating inductively coupled plasma provided in a film formation chamber on a substrate surface, showing a case in which there is no plasma diffusion prevention plate. [Figure 8B] 1A and 1B are diagrams for explaining the influence of an antenna for generating inductively coupled plasma provided in a film formation chamber on a substrate surface, showing the case where a plasma diffusion prevention plate is provided. [Figure 9] FIG. 1 is a diagram for explaining the effect of an antenna for generating inductively coupled plasma installed in a deposition chamber on the substrate surface, and is a diagram for explaining the problem of non-uniformity of the deposited thin film that can occur when there is no plasma diffusion prevention plate. [Figure 10A] 1 shows an example of a film formation target mounted in a film formation apparatus according to an embodiment of the present invention, in which two types of target materials are used. [Figure 10B] 1 shows an example of a film formation target mounted in a film formation apparatus according to an embodiment of the present invention, in which three types of target materials are used. [Figure 11] 1 is a diagram illustrating a configuration of an antenna for generating inductively coupled plasma provided in a film formation chamber of a film formation apparatus according to an embodiment of the present invention. FIG. [Figure 12] 2 shows a cross-sectional structure of an antenna coupling region of an antenna body for generating coupled plasma used in a film formation apparatus according to one embodiment of the present invention. [Figure 13] 1 is a diagram showing waveforms of an AC voltage applied to an antenna for generating inductively coupled plasma provided in a film formation chamber of a film formation apparatus according to one embodiment of the present invention, and a pulse voltage applied to a film formation target. FIG. [Figure 14] 13 is a schematic diagram showing the relationship between the target voltage and the film density when an InGaZnO film is formed as an oxide semiconductor film. [Figure 15] 1 is a schematic cross-sectional view showing a configuration of a pretreatment chamber of a film forming apparatus according to an embodiment of the present invention; [Figure 16A] 1 is a front view of an antenna for generating inductively coupled plasma provided in a deposition chamber of a deposition apparatus according to an embodiment of the present invention; [Figure 16B] 16B is a cross-sectional view of an antenna for generating inductively coupled plasma provided in a film formation chamber of a film formation apparatus according to one embodiment of the present invention, showing a cross-sectional structure corresponding to the section A1-A2 shown in FIG. 16A. [Figure 17A]1 is a front view of an antenna for generating inductively coupled plasma provided in a deposition chamber of a deposition apparatus according to an embodiment of the present invention; [Figure 17B] 17B is a cross-sectional view of an antenna for generating inductively coupled plasma provided in a film formation chamber of a film formation apparatus according to one embodiment of the present invention, showing a cross-sectional structure corresponding to the section B1-B2 shown in FIG. 17A. [Figure 18A] 1 shows an example of an element fabricated using a film formation apparatus according to an embodiment of the present invention. [Figure 18B] 2 shows a detailed structure of an oxide semiconductor layer in an element manufactured using a film formation apparatus according to one embodiment of the present invention. [Figure 18C] 2 shows a detailed structure of an oxide semiconductor layer in an element manufactured using a film formation apparatus according to one embodiment of the present invention. [Figure 19] 1 shows an overall configuration of a film forming apparatus according to an embodiment of the present invention. [Figure 20] FIG. 1 is a diagram showing the configuration of a film formation apparatus according to one embodiment of the present invention, illustrating the main components provided in or connected to a pre-treatment chamber, a transfer chamber, and a film formation chamber, excluding a load / unload chamber. [Figure 21] 1 shows an example of an element fabricated using a film formation apparatus according to an embodiment of the present invention. [Figure 22A] 1 is a schematic partial cross-sectional view of a film formation chamber of a film formation apparatus according to an embodiment of the present invention, as viewed from above; [Figure 22B] 22B is a front view of a ceramic member used in the film formation chamber shown in FIG. 22A. [Figure 23A] 1 is a schematic partial cross-sectional view of a film formation chamber of a film formation apparatus according to an embodiment of the present invention, as viewed from above; [Figure 23B] 23B is a front view of a ceramic member used in the film formation chamber shown in FIG. 23A. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] Hereinafter, an embodiment of the present invention will be described with reference to the drawings. The present specification includes the following embodiments, and is not to be construed as being limited to the following embodiments. In order to make the explanation clearer, the width, thickness, shape, etc. of each part in the accompanying drawings may be distorted compared to the actual embodiment. Although the state of the present invention may be shown in a schematic manner, it is merely an example and should not be construed as limiting the scope of the present invention. The present invention is not necessarily limited to the specific embodiments shown in the drawings. When an element in one drawing has the same or corresponding relationship with a specific element shown in another drawing, the same element is used. A single code (or a code with a, b, etc., added after the number written as the code) is added, and The explanation of the return may be omitted as appropriate. In addition, each element is labeled "first" or "second". The letters are convenient symbols used to distinguish each element, and unless otherwise specified, Unless otherwise stated, it has no further meaning.
[0014] As used herein, one element or region may be "on (or under)" another element or region. Unless otherwise specified, this applies when it is directly above (or directly below) another component or area. This includes not only cases where the component or area is located above (or below) other components or areas. There is another component between a certain member or region and above (or below) the member or region. This also includes cases where
[0015] [First embodiment] FIG. 1 is a general view of a film formation apparatus 100 for performing sputtering film formation according to an embodiment of the present invention. The film forming apparatus 100 has a load / unloader for storing substrates before and after film formation. a substrate pre-treatment chamber 104 for pre-treatment of the substrate, and a transfer robot 116. A first transfer chamber 106a is provided, a second transfer chamber 106b is provided with a platen mechanism 118, and 106b, a first deposition chamber 108a and a second deposition chamber 108b for performing sputtering deposition. These chambers are connected by a gate valve and are connected to a vacuum (not shown). An exhaust means is provided.
[0016] The substrate on which the thin film is to be formed is held in a cassette and placed in the load-unload chamber 1. The substrate is, for example, a glass substrate. The substrate stored in the transfer chamber 102 is transferred to the transfer robot 116 provided in the first transfer chamber 106a. The substrate is then transferred to the pre-treatment chamber 104. The pre-treatment chamber 104 is a chamber for The pretreatment chamber 104 is connected to a high frequency power source 120. The pretreatment includes a stage equipped with a heating mechanism and a high-frequency discharge electrode. The high-frequency discharge plasma generated by the electrodes is used to degas the substrate. 1 shows an embodiment in which two pre-treatment chambers 104 are installed on either side of a first transfer chamber 106a. However, the number of pre-treatment chambers 104 is not limited. By providing two pre-treatment chambers 104, the degassing process can be performed sufficiently and the time can be shortened. The sputtering deposition can be performed continuously with a sufficient margin. The number of pre-treatment chambers 104 is not limited to the form shown in FIG. 1, and may be one, three or more. It may be provided on the
[0017] The substrate that has been pre-processed in the pre-processing chamber 104 is transferred to the second transfer chamber by the transfer robot 116. The substrate is transferred from the load / unload chamber 102 to the pre-processing chamber 106b. The second transfer chamber 106b is a platen mechanism. 118, and the substrate that is brought in horizontally is conveyed by a conveying carrier (not shown in FIG. 1). The device is held vertically or tilted at a range of about 20 degrees from the vertical. It can be said.
[0018] The first deposition chamber 108a and the second deposition chamber 108b are for generating inductively coupled plasma. The antenna 126 is provided, and the sputtering target 124 is attached. The chamber 108a and the second deposition chamber 108b are provided with an antenna for generating inductively coupled plasma. Sputtering deposition is performed using inductively coupled plasma (ICP) generated by 126. A pulse power supply 123 is connected to the sputtering target 124, and the ion acceleration energy The film forming apparatus 100 is capable of controlling the energy by using such a mechanism. It is possible to control the density of the thin film deposited on the substrate.
[0019] The first deposition chamber 108a and the second deposition chamber 108b are provided with different materials (components, compositions, etc.). A sputtering target 124 having a different composition can be mounted in the vacuum. In addition, the first film forming chamber 108a and the second film forming chamber 108b can be used to continuously deposit a thin film. The chamber 108b is equipped with a sputtering target 124 of the same type (component, composition, density). The thin films may be deposited on the substrate, so that different film formation conditions can be applied to deposit thin films of different film properties. Although FIG. 1 shows two deposition chambers 108, the deposition apparatus 100 may include The configuration of the film forming chamber 108 is not limited to this, and may be changed depending on the structure and type of the thin film to be formed. The number of the film forming apparatuses 100 may be changed as appropriate. The number of deposition chambers 108 may be one, or three or more if a multi-layer thin film is to be formed. The deposition chamber 108 may be connected to the deposition chamber 106 .
[0020] FIG. 2 is a diagram showing the configuration of the film forming apparatus 100, excluding the load / unload chamber. Processing chamber 104, first transfer chamber 106a, second transfer chamber 106b, first film formation Main components provided in or connected to the chamber 108a and the second deposition chamber 108b Each chamber is connected to a vacuum exhaust system 110. The vacuum exhaust system 110 is a turbocharger. It consists of vacuum pumps such as a sub-pump (TMP) and a dry pump (DRP). The system 110 is configured with a first transfer chamber 106a, a second transfer chamber 106b, and a first component. The film chamber 108a and the second film deposition chamber 108b may be different or the same. The first deposition chamber 108a and the second deposition chamber 108b may be provided with a pressure controller. A conductance valve for the roll may be provided. Also, the pre-treatment chamber 1 04, a gas supply system 112 is connected to the first film formation chamber 108a and the second film formation chamber 108b. The gas supply system 112 is composed of a mass flow controller, a filter, and the like.
[0021] The pretreatment chamber 104 is provided with a substrate stage 114 and a high-frequency discharge electrode 115. The high-frequency discharge electrode 115 is connected to a high-frequency power supply 120. In the pre-treatment chamber 104, The high-frequency discharge plasma generated by the substrate stage 114 and the high-frequency discharge electrode 115 This allows pre-treatment of the substrate.
[0022] A transfer robot 116 is provided between the pretreatment chamber 104 and the first film formation chamber 108a. A first transfer chamber 106a and a second transfer chamber 106b are provided with a platen mechanism 118. The substrate is subjected to a desorption process of adsorbed molecules in the pre-processing chamber 104. The first transfer chamber 106a and the second transfer chamber 106b are passed through the first transfer chamber 106a and the second transfer chamber 106b without being exposed to the atmosphere. The wafer is transferred to the first deposition chamber 108a via the pretreatment chamber 104. The substrate is transferred to the second transfer chamber 10 by the transfer robot 116 of the first transfer chamber 106a. The transfer robot 116 transfers the substrate while keeping it horizontal. The substrate transferred to chamber 106b is tilted vertically or 2x vertically by platen mechanism 118. The substrate is tilted at an angle of about 0 degrees and is then carried into the first film formation chamber 108a.
[0023] In the deposition by sputtering, the substrate is set so that pinholes are not formed in the deposited thin film. It may be preferable to deposit the film with the plate in an upright position rather than horizontally. When the size of the substrate increases, such as in the case of display applications (e.g., liquid crystal processes), The 8th generation glass substrate is 2200mm x 2400mm, and it is warped by its own weight. Therefore, it is difficult to transport the substrates in a vertical position. In a device that forms a film by keeping the substrate horizontal, such as a sputtering device, the size of the substrate The floor space required for the equipment increases due to the mold (i.e., the floor space required for the clean room increases). To address this issue, the film forming apparatus 100 has a platen on the substrate transport path. A tilt mechanism 118 is provided to handle the substrate horizontally until the stage before the film formation, and to handle the substrate vertically or The board is tilted about 20 degrees from the vertical, so Furthermore, the film forming apparatus 100 requires a small floor space for installation. This has the advantage that:
[0024] The first deposition chamber 108a is provided with an antenna 126 for generating inductively coupled plasma. A sputtering target 124 is attached. Antenna for inductively coupled plasma generation 126 is connected to a high frequency power source 120 that outputs a high frequency in the megahertz band. The antenna 126 for generating the combined plasma transmits an AC power in the kilohertz range so as to be superimposed on the high frequency power. An AC power source 122 may be connected to the sputtering heater 120 so that a voltage can be applied. The get 124 is connected to the pulse power supply 123 as described above. A heater 127 for heating the substrate may be provided in 108a.
[0025] Although detailed description is omitted, the second film formation chamber 108b is the same as the first film formation chamber 108a. Although not shown in FIG. 2, the first film formation chamber 108a and the second film formation chamber 108b have the same configuration. In the deposition chamber 108b, the substrate is placed vertically or tilted within a range of about 20 degrees from the vertical. A transport mechanism is provided for transporting the material.
[0026] FIG. 3 shows the deposition chambers 108 (first deposition chamber 108a, second deposition chamber 108b The film-forming chamber 108 has an internal space of It is constructed to form a closed space isolated from the atmosphere, but FIG. 3 shows two walls (the first chamber 1 shows a schematic structure between a first chamber wall 109a and a second chamber wall 109b.
[0027] The deposition chamber 108 is provided with a plate that covers the sputtering target 124. The plasma diffusion prevention plate 140 and the plasma diffusion prevention plate 140 are provided so as to protrude into the area surrounded by the plasma diffusion prevention plate 140. The antenna 126 for generating inductively coupled plasma (first antenna 126a, second antenna The deposition apparatus 100 includes a nozzle 126b and a gas introduction pipe 138 for introducing a sputtering gas. The deposition chamber 108 is used with a sputtering target 124 attached thereto. However, the sputtering target 124 is a consumable item and is fixed to the deposition apparatus 100. The deposition chamber 108 is not a component, but an accessory that can be replaced as needed. The ring target 124, the antenna 126 for generating inductively coupled plasma, and other components are attached. However, sealing members such as O-rings and gaskets are provided at the mounting parts of each component.
[0028] The sputtering target 124 comprises a target material 132 and a backing plate 130. The target material 132 is a bar made of a metal such as copper (Cu) or titanium (Ti). The substrate 130 is bonded to a bonding plate 130 using a bonding material such as an indium alloy. The target material 132 is preferably a one-piece molded product. 4 is attached to a first chamber wall 109a of the deposition chamber 108. The first through hole 128a is provided in the first through hole 109a, and the sputtering target 124 is The support plate 130 is attached so as to be fitted into the first through hole 128a. A bias voltage is applied to the sputtering target 124, so that the backing plate An insulating piece 136 is provided between 130 and the first chamber wall 109a.
[0029] When viewed from the front, the sputtering target 124 has a rectangular shape with the longitudinal direction being vertical. The target material 132 is made of various sputterable materials. For example, the target material 132 may be a transparent conductive film, an oxide semiconductor film, or the like. A sintered body of a metal oxide can be applied to form the target material 132. The temperature rises due to ion collisions during sputtering deposition. 100 includes a backing plate 130 to suppress the temperature rise of the target material 132. FIG. 3 shows an example of a cooling mechanism for the backing plate 130. The figure shows a structure with a drainage hole for cooling water.
[0030] When the sputtering target 124 is attached to the first chamber wall 109a, the target The get material 132 is exposed to the internal space of the deposition chamber 108. A shield plate 134 is provided to cover the periphery of the target material 132. 34 is a backing exposed in the region between the target material 132 and the first chamber wall 109a. The backing plate 130 is provided so as to cover the surface of the backing plate 130. This prevents the plate 130 from being exposed to the inductively coupled plasma and being sputtered. Cut.
[0031] The deposition chamber 108 includes an antenna 126 (first antenna 12) for generating inductively coupled plasma. 6a, and a second antenna 126b) are provided. Antenna 126 for generating inductively coupled plasma The sputtering target 124 is aligned along the longitudinal direction of the sputtering target 124 and is aligned along the longitudinal direction of the sputtering target 124. In other words, the antenna 126 for generating inductively coupled plasma is arranged between the The first antenna 126a and the second antenna 126b are arranged to face the sputtering target. They are placed on either side of 124.
[0032] The first antenna 126a and the second antenna 126b are used as the antenna 126 for generating inductively coupled plasma. The antenna 126b includes an antenna body 148 (first antenna body 14) for generating inductively coupled plasma. 8a, second antenna body 148b), and a U-shaped groove-shaped insulating member 146 (first insulating member The first antenna body 148a includes a first insulating member 146a and a second insulating member 146b. The second antenna body 148b is provided in the second insulating member 146a. The antenna 126 for generating inductively coupled plasma is connected to the first chamber wall by an insulating member 146. 109a, and protrudes from both sides of the sputtering target 124. In this manner, the insulating member 146 is provided with a heat source for generating inductively coupled plasma. The antenna body 148 is provided to generate an inductively coupled plasma. This can prevent the sputtered material from adhering to the target material 132. Furthermore, the antenna body 148 for generating inductively coupled plasma is exposed to the inductively coupled plasma. It is possible to make this happen.
[0033] The antenna 126 for generating inductively coupled plasma is an antenna body for generating inductively coupled plasma. 148 is located at a position higher than the surface of the target material 132 (closer to the center of the deposition chamber 108). For example, the inductively coupled plasma is provided so as to protrude toward the substrate 200 side. The antenna body 148 for generating the ion beam protrudes from the surface of the target material 132 by a length D2. In this manner, the antenna body 148 for generating inductively coupled plasma is provided as a target. By providing the protruding portion 134 on the surface of the target material 132, the protruding portion 134 is The plasma density can be increased.
[0034] FIG. 22A shows the deposition chamber 108 (first deposition chamber 108a, second deposition chamber 10 FIG. 22A shows another configuration of the deposition chamber 108 as seen from above, similar to FIG. The deposition chamber 108 shown in FIG. 22A is an inductively coupled plasma deposition chamber. Antenna 126 for generating the marker (first antenna 126a, second antenna 126b) and A part of the first chamber wall 109a on which the printing target 124 is attached is made of ceramic. FIG. 22B shows a front view of the ceramic member 180a. The figure is shown.
[0035] As shown in FIGS. 22A and 22B, the ceramic member 180a is A first through hole 128a for mounting the target 124 is provided. Since 180a has insulating properties, the sputtering target 124 can be directly attached. That is, the sputtering target 124 is attached to the deposition chamber 108. In this case, the insulating part 136 as shown in FIG. 3 can be omitted. The material 180a includes antennas 126 (first antenna 126a, second antenna 126b) for generating inductively coupled plasma. A second through hole 128b is provided for mounting the second antenna 126b. The insulating member 146 (first insulating member 146a, second insulating member 146b) is 2 is inserted through the through hole 128b and is secured to the back surface of the ceramic member 180a by an O-ring. The ceramic member 180a is vacuum sealed. Since the ceramic member 180a is insulating, the target A shield plate 134 that covers the peripheral portion of the support material 132 can be integrated.
[0036] FIG. 23A shows the deposition chamber 108 (first deposition chamber 108a, second deposition chamber 10 8b), a portion of the first chamber wall 109a is inductively coupled to the ceramic member 180b. Antenna body 148 for plasma generation (first antenna body 148a, second antenna body 1 The insulating member 146 (first insulating member 146a, second insulating member 48b) is U-shaped and covers the insulating member 146. FIG. 23B shows a structure in which the ceramic member 180b is integrated. As shown in FIG. 23A and FIG. 23B, a U-shaped insulating member 146 ( The first insulating member 146a and the second insulating member 146b are integral with a part of the first chamber wall 109a. By molding, the number of parts can be reduced and leaks (vacuum airtightness) can be prevented. In addition, the insulating member (first insulating member) having a U-shaped groove shape of the ceramic member 180b can be 146a, the second insulating member 146b) on the atmospheric side (for generating inductively coupled plasma) A glass layer may be formed on the side where the antenna body 148 is provided. This can further reduce leakage from the atmosphere.
[0037] The ceramic members 180a and 180b are not only excellent in insulation but also have a high heat resistance. It has a very small thermal expansion coefficient, can be precisely machined, and emits little gas, making it ideal for use in deposition chambers. The material can be suitably used as a wall material for the wall of the bath 108. Antenna 1 for generating inductively coupled plasma By using ceramic members 180a and 180b as the wall material near 26, inductive coupling plasma This can reduce the power loss of the antenna 126 for generating the target signal. The plasma density near the surface of the support material 132 can be increased.
[0038] As shown in FIG. 22A and FIG. 23A, the sputtering target 124 is attached. The chamber wall 109a is made of ceramic members 180a and 180b. The amount of gas desorbed from the inner wall of the chamber can be reduced, and the plasma density can be increased. The periphery of the target material 132 is covered with insulating ceramic members 180a and 180b. By configuring the target material 132 as above, a region where a vertical electric field is generated with respect to the surface of the target material 132 is It can be expanded and denser films can be made.
[0039] 4 shows a detailed cross-sectional structure of the antenna 126 for generating inductively coupled plasma. The antenna body 148 for plasma generation is formed of a hollow metal tube 150. The antenna body 148 for generating the coupled plasma is made of copper (Cu), brass, or aluminum (Al). The antenna body 148 for inductively coupled plasma generation is formed of a hollow metal tube 150 such as A rod-shaped antenna is formed from such a metal tube, and cooling water is passed through the hollow portion. The inner surface of the tube 150 is plated with nickel (Ni) or tin (Sn) to prevent corrosion. It is preferable that the insulating member 146 is provided with a conductive layer 151 formed of a plating film. Quartz, or alumina, yttria (Y2O3), forsterite (Mg2SiO4), The insulating member 146 is made of ceramics such as steatite (MgO·SiO2). A U-shaped groove-shaped member in which the antenna body 148 for generating inductively coupled plasma is placed. The insulating member 146 is disposed so as to separate the air from the air. A glass layer 147 is provided to increase the sealing property (to prevent leakage). It is preferable that the antenna body 148 for generating inductively coupled plasma is inserted into the insulating member 146. In this way, the antenna for generating inductively coupled plasma is placed on the atmospheric side. By arranging the main body 148 on the atmospheric side, the accuracy of the installation position can be improved, and the target The uniformity of the plasma density in the vicinity of the pad material 132 can be improved. The holding mechanism for the antenna body 148 for generating the magnet can also be freely designed.
[0040] As shown in FIG. 5, the antenna 126 for generating inductively coupled plasma is The antenna body 148 for generating the Zuma may be configured to include a plurality of antenna bodies 148. The antenna body 148 for plasma generation includes a plurality of antenna bodies 1 for inductively coupled plasma generation. 48 and may be disposed on the atmospheric side of the insulating member 146. The metal tube 150 constituting the antenna body 148 for use in the antenna is Therefore, the AC resistance becomes high. For example, when 13.56MHz high frequency power is applied to an inductively coupled plasma generator, When the voltage is applied to the antenna body 148, the thickness of the metal tube 150 is 5 mm. However, the current flows only in a region about 17.7 μm deep from the surface of the metal tube 150. In order to prevent power loss due to the skin effect, the antenna 12 for inductively coupled plasma generation is 6, as shown in FIG. 5, a plurality of antenna bodies 148 for generating inductively coupled plasma are arranged in parallel. It may be placed.
[0041] As shown in FIG. 3, the gas introduction pipe 138 is located in the area inside the plasma diffusion prevention plate 140. The gas introduction pipe 138 is disposed adjacent to the first antenna 126a. The gas introduction tube 138 is provided for introducing gas into the deposition chamber 108. In the same manner as the antenna 126 for generating plasma, the sputtering target 124 is arranged in the longitudinal direction. The gas introduction pipe 138 is a metal pipe with a shower nozzle. However, it may be formed of an insulating porous body, for example, a ceramic porous body tube. By using a porous body for the gas introduction pipe 138, sputtering The sputtering gas can be introduced uniformly along the longitudinal direction of the target 124 .
[0042] The plasma diffusion prevention plate 140 surrounds the area in which the sputtering target 124 is disposed. The plasma diffusion prevention plate 140 is a box-shaped member and is provided in the deposition chamber 10. A space surrounded by the first chamber wall 109a and the plasma diffusion prevention plate 140 is formed inside the chamber 8. The plasma diffusion prevention plate 140 is provided so as to be substantially flush with the surface of the first chamber wall 109a. A first surface 142 is parallel to the first chamber wall 109a, and a second surface 143 is parallel to the first surface 142 and faces the first chamber wall 109a. In addition, in the area surrounded by the plasma diffusion prevention plate 140, the first chamber wall 10 The plasma diffusion prevention plate 140 is provided so as to cover the surface of the plasma diffusion prevention plate 140. The first opening 144 is provided in the target material 132. It is provided at a position overlapping with.
[0043] FIG. 6 is a schematic diagram showing the structure of the plasma diffusion prevention plate 140 when viewed from the front. The stripping target 124 is provided in an area surrounded by a plasma diffusion prevention plate 140. When the sputtering target 124 is viewed from the front, the target material 132 is a plasma diffusion It is exposed from the first opening 144 of the prevention plate 140.
[0044] Antenna 126 for generating inductively coupled plasma (first antenna 126a, second antenna 12 6b) is disposed in a position covered by the plasma diffusion prevention plate 140. 8a, a first metal tube 150a and a second metal tube 150b are connected via a first capacitor 152a. The second antenna body 148b has a structure in which the third metal tube 150c and the fourth metal tube 150b are connected to each other. 50d are connected via a second capacitor 152b.
[0045] The plasma diffusion prevention plate 140 has a slit-shaped portion extending from the second surface 143 to the first surface 142. A second opening 154 is provided. The second opening 154 is an antenna for generating inductively coupled plasma. The second opening 154 is provided in a plurality of portions, each of which extends in a direction intersecting with the longitudinal direction of the first opening 126. , an orifice for sputter gas, surrounded by a plasma diffusion prevention plate 140 The second opening 1 has a function of controlling the flow of the sputtering gas supplied to the space. 54 is a space surrounded by a plasma diffusion prevention plate 140 in which sputtering gas remains for a predetermined period of time. The conductance of the gas flow is controlled to form a uniform gas pressure in the deposition area. Furthermore, the second slit-shaped opening 154 has a function of generating an inductively coupled plasma. The function of preventing an induced current generated in the plasma diffusion prevention plate 140 by the antenna 126 is as follows. and an antenna 126 for generating inductively coupled plasma supplies energy to the inductively coupled plasma. Transmission efficiency can be improved.
[0046] The plasma diffusion prevention plate 140 is preferably made of a material having a secondary electron emission rate of greater than 1. For example, the plasma diffusion prevention plate 140 is made of magnesium mainly composed of aluminum. It is preferable that the alloy is made of aluminium alloy, barium alloy or calcium alloy. The plasma diffusion prevention plate 140 made of the above metal material is disposed in contact with the sputtering target 12. It is preferable that the inner surface of the plasma diffusion prevention plate 140 facing the plasma diffusion prevention plate 140 is anodized. An anodic oxide film of magnesium alloy, barium alloy, or calcium alloy is formed on the inner surface. By doing so, the secondary electron emission ratio can be made larger than 1. The surface is positively charged, and the argon ion (positive ion) plasma diffusion prevention plate 140 In other words, it is possible to prevent the incidence and collision of argon ions (positive ions). The plasma diffusion prevention plate 140 is prevented from being sputtered, and the film is formed in the film formation chamber 108. This can reduce impurities that are introduced into the thin film that is to be formed.
[0047] When the carrier concentration of the n-type oxide semiconductor film is precisely controlled by sputtering, It is necessary to prevent the inclusion of impurities that cause the Lectron Killer effect. The inner surface of the plasma diffusion prevention plate 140 exposed to the inductively coupled plasma is treated with an electron killer. It is preferable to cover the insulating film with a material that does not cause the electron killer effect. The insulating film may be, for example, silicon oxide (SiO2), magnesium oxide (MgO), or aluminum. In particular, magnesium oxide, which has a high secondary electron emission rate, is used as an insulating film. Magnesium oxide (MgO) is preferred, and silicon oxide containing magnesium oxide (MgO) is also preferred. It is preferable to cover the surface of the plasma diffusion prevention plate 140 with aluminum oxide or the like.
[0048] The plasma diffusion prevention plate 140 is formed by the antenna 126 for inductively coupled plasma generation. The inductively coupled plasma is prevented from spreading throughout the deposition chamber 108. By forming a physical wall called the plasma diffusion prevention plate 140, This can prevent the inductively coupled plasma from spreading unnecessarily within 108. The deposition chamber 108 is surrounded by a plasma diffusion prevention plate 140 and an adhesion prevention plate 141. The structure is such that inductively coupled plasma is generated and does not spread to other areas. The plasma diffusion prevention plate 140 and the adhesion prevention plate 141 have an anodic oxide film formed on their surfaces. This enhances the plasma confinement effect and increases the plasma density. do.
[0049] In the conventional magnetron sputtering apparatus, the film density of the oxide semiconductor film is improved. In order to achieve this, it is necessary to keep the gas pressure at 0.5 Pa or less during film formation. Not only impurity gases that escape from the inner wall of the chamber, but also the materials inside the deposition chamber are sputtered. It is necessary to take care that the ions are not absorbed into the film as impurities.
[0050] InGaSnO x Oxide semiconductors, such as those shown in Figure 1, have n-type conductivity, so they are Stainless steel containing iron (Fe), chromium (Cr), manganese (Mn), etc., which have a large Lonkiller effect. When the deposition chamber is made of stainless steel, the chamber wall is prevented from coming into contact with the plasma. When forming an oxide semiconductor film, it is necessary to completely prevent the water adsorbed on the substrate surface. If no treatment is performed to remove hydrocarbons such as H2O, the film density will not increase. Therefore, it is impossible to manufacture a highly reliable thin film transistor.
[0051] The substrate temperature is kept below 150°C even during the degassing process and transfer to the deposition chamber. If the sensor is not held above the surface, the moisture (H2O) in the vacuum chamber will be re-adsorbed, which will result in poor reproducibility. Furthermore, it is difficult to improve the film density of the as-deposited oxide semiconductor film. To achieve this, it is necessary to increase the substrate temperature to 200°C or higher to improve the crystallization rate. By adding a small amount of hydrogen gas (H2) to the Ar+O2 gas, the inside of the deposition chamber Contamination caused by impurity gases escaping from the walls can be reduced, and heat treatment after film formation can be omitted. In the case of thin-film transistors, the heat treatment temperature after element completion can be reduced to about 200°C. This allows for a significant reduction in manufacturing costs.
[0052] In this manner, the deposition chamber 108 is protected by the plasma diffusion prevention plate 140 and the adhesion prevention plate 141. Since the inductively coupled plasma is confined by the chamber wall 109 (first chamber Impurities (water (H2O), hydrogen ( Prevents H2) and hydrocarbons from being incorporated into the thin film deposited on the substrate. The deposition chamber 108 is made of stainless steel (SUS304). Even in such a case, problems of contamination by iron (Fe), chromium (Cr), etc. can be prevented.
[0053] As shown in FIG. 7, a mesh 170 may be provided in the first opening 144. By providing the mesh 170, the confinement effect of the inductively coupled plasma can be improved. The mesh 170 is preferably made of a metal material that does not have an electron killer effect. For example, the mesh 170 may be made of titanium (Ti), tungsten (W), nickel (Ni), or the like. It is preferable that the electrode is made of a metal material selected from the group consisting of nickel (Ni) and tantalum (Ta). This reliably prevents the plasma from spreading into the deposition chamber 108 and also prevents the oxide semiconductor from When a conductive film is deposited, impurities that act as electron killers are incorporated into the film. By installing Mesh 170, negative oxygen ions can be prevented from being mixed in. This makes it easier for the ions to be perpendicularly incident on the substrate 200, and promotes crystallization of the formed oxide semiconductor film. It is possible.
[0054] The mesh 170 preferably has an opening ratio of 70% or more. The wire (or mesh pattern) is aligned in the direction of the substrate movement (horizontal direction) as shown in FIG. The mesh is arranged so that it intersects with the mesh at an angle of 30 to 60 degrees. This can prevent the pattern of 170 from being transferred to the deposited film.
[0055] The plasma diffusion prevention plate 140 also supports an antenna 126 (first The first antenna 126a and the second antenna 126b are provided so as to be interposed between the substrate 200. If there is no plasma diffusion prevention plate 140, as shown in FIG. The antenna 126 for generating inductively coupled plasma (first antenna 126a, second antenna 126b) is 26b) affects the quality of the thin film deposited on the substrate 200. The antenna 126 for generating inductively coupled plasma (first antenna 126a, second antenna 126b) 26b) is connected to the surface 202 of the substrate 200, which is adjacent to the antenna 12 for generating inductively coupled plasma. 6 (the first antenna 126a and the second antenna 126b) are affected by the self-bias. As a result, the quality of the deposited thin film varies greatly. , an antenna 126 for generating inductively coupled plasma (first antenna 126a, second antenna 12 6b) and the substrate 200, the plasma diffusion prevention plate 140 is interposed, and the self-bias Since the influence is shielded, the quality of the thin film deposited on the substrate 200 can be kept constant. Also, an antenna 126 for generating inductively coupled plasma is connected to the coupling region (two conductors are capacitively coupled). In the case where the plasma diffusion prevention plate 140 has a thickness of 100 nm, the thickness of the plasma diffusion prevention plate 140 is 100 nm. By having the above, the problem of plasma non-uniformity can be solved.
[0056] In addition, when the plasma diffusion prevention plate 140 is not provided, the substrate 200 is In the moving type deposition method in which the front of the part 144 is moved in one direction, as shown in FIG. The metal tube 150 (first metal tube 150a and second metal tube 150b) constitutes the antenna body 148 for generating plasma. A capacitor 152 connecting the second metal tube 150b, the third metal tube 150c, and the fourth metal tube 150d The film quality of the area overlapping with the first capacitor 152a and the second capacitor 152b is different. This becomes a problem.
[0057] That is, if the plasma diffusion prevention plate 140 is not provided, the first antenna 12 A first capacitor 152a and a second capacitor 152b are provided on the first antenna 126a and the second antenna 126b, respectively. The plasma density in the capacitor 152b is different, and the antenna connection area 2 overlaps with this area. 04, it affects the quality of the thin film deposited on the substrate 200. In contrast, when the plasma diffusion prevention plate 140 is provided, In this case, there is no region corresponding to the antenna connection region 204, and the plasma becomes non-uniform. Since the influence of the temperature is eliminated, a uniform film can be formed over the entire surface of the substrate 200.
[0058] The film forming apparatus 100 is of a moving film forming type. As shown in FIG. The substrate 200 is attached to the sputtering plate 60 and transported in front of the sputtering target 124. The target material is conveyed to a position adjacent to the plasma diffusion prevention plate 140. As shown in FIG. The distance from the surface of 132 to the surface of the substrate 200 is D1. The distance between the surface of the diffusion prevention plate 140 and the substrate is set to D3. In this case, the distance D3 is 5 times the distance D1. The plasma diffusion prevention plate 140 and the carrier tray 160 are arranged so that the difference between the plasma diffusion prevention plate 140 and the carrier tray 160 is equal to or less than one of the above. For example, if the distance D1 is 55 mm, then the interval D3 has a length of 5 mm.
[0059] In this way, by transporting the substrate 200 close to the plasma diffusion prevention plate 140, The sputtering gas supplied to the area surrounded by the plasma diffusion prevention plate 140 passes through the first opening 144. The conductance when the gas flows through the deposition chamber 108 can be reduced. Furthermore, this configuration prevents impurities (water (H2O), hydrogen (H 2) It has the effect of preventing foreign substances (e.g., hydrocarbons) from diffusing and flowing into the film formation region, This provides the effect of improving the reproducibility of the physical properties of the thin film to be formed.
[0060] 10A and 10B show a sputtering target 124 that can be applied to the moving deposition method. FIG. 10A shows an example of a backing plate 130 having two types of target materials 132. (First target material 132a, second target material 132b) are fixed with bonding material 131. The bonding material 131 is indium or an indium alloy. I can.
[0061] The first target material 132a and the second target material 132b are different in composition or material. For example, when the target material is an oxide semiconductor, the first target material 132a is a ternary system containing indium (In), gallium (Ga), and tin (Sn). An oxide semiconductor target is used, and the first target is used as the second target material 132b. An oxide semiconductor target having a higher concentration of gallium (Ga) than that of the material 132a is used. In this way, by arranging two types of target materials in the same direction along the substrate transport direction, Two different layers can be deposited in succession.
[0062] The first target material 132a and the second target material 132b are formed to prevent damage due to thermal expansion. The gap G1 is 0. In this case, the backing plate 130 or The first target material 132a and the second target material 132b are disposed so as not to expose the bonding material 131. The end of the material 132b is tapered in cross section. As shown in FIG. 1, the first target material 132a has a top surface that is slightly larger than the bottom surface that is in contact with the bonding material 131. The second target material 132b has a tapered surface formed so that the end portion on the upper surface side protrudes. The bottom surface of the casing is tapered so that the two tapered surfaces fit together. By disposing the first target material 132a and the second target material 132b, sputtering When the target 124 is viewed in plan, the backing plate 130 and the bonding material 1 In other words, one backing plate 130 is not exposed. Even if two types of target materials are placed on the same plate, the boundary area between the backing plate 130 The bonding material 131 can be prevented from being sputtered, and impurities can be prevented from being deposited. This can prevent the particles from being incorporated into the membrane.
[0063] In the deposition chamber 108, the substrate 200 is moved toward the sputtering target 124 at a constant speed. Since the second target material 132a is transported in one direction in front of the first target material 132a, By narrowing the width of 32b, the thickness of the deposited thin film can be varied. For example, the width of the second target material 132b is narrower than the width of the first target material 132a. This increases the thickness of the thin film deposited on the first target material 132a, and The thickness of the thin film deposited in 132b can be reduced.
[0064] FIG. 10B shows three types of target materials 132 (a first target material 132a, a third target material 132b, a In this example, the first target material 132c and the second target material 132b are arranged as shown in FIG. As in the example shown, the side ends of the adjacent targets are tapered. Specifically, the third target is sandwiched between the first target material 132a and the second target material 132b. The third terminal 132c has a trapezoidal cross-sectional shape. The first target material 132a and the second target material 132b are tapered from both sides of the target material 132c. By disposing the get material 132b, the sputtering target 124 is The plate 130 and the bonding material 131 are structured so as not to be exposed in a plan view.
[0065] FIG. 11 shows an antenna 126 for generating inductively coupled plasma (first antenna 126a, second antenna The first antenna 126a is made up of a first insulating member 146a and The first antenna 126b includes a first antenna body 148a, and the second antenna 126b includes a second insulating member 146b and The first antenna body 148a includes a first metal tube 150a and a second antenna body 148b. The second metal tube 150b is connected to the antenna through a first capacitor 152a formed in the antenna connection region 204. The second antenna body 148b is a rod-shaped antenna connected to a third metal tube 150c. and the fourth metal tube 150d are formed in the antenna connection region 204. The first antenna body 148a and the second antenna body 148b are rod-shaped antennas connected via a The body 148b can reduce impedance by having such a structure. As a result, even if the antenna body 148 for generating inductively coupled plasma is lengthened, This prevents an increase in impedance, and the antenna body 148 for generating inductively coupled plasma can be This prevents a large potential difference from occurring at both ends. It can also accommodate larger models such as 124.
[0066] FIG. 12 shows the structure of the antenna coupling region 204 of the antenna body 148 for inductively coupled plasma generation. The cross-sectional structure is shown. The antenna connection region 204 is made up of a first metal tube 150a and a second metal tube 150b. (or the third metal tube 150c and the fourth metal tube 150d) are hollow tubes 17 made of insulating material. The hollow tube 172 is fitted into the first metal tube 150a and the second metal tube 150b. An O-ring 153 is provided at the part where it fits with Ob to maintain airtightness, and the cooling water flows through The O-ring 153 is preferably heat resistant, e.g. For example, a fluororubber-based material is used.
[0067] The inner surface of the hollow tube 172 is provided with a conductive layer 174 which serves as an electrode for the capacitor 152. The conductive layer 174 has a first conductive layer 174a formed of copper plating in order to reduce resistance. The second conductive layer 174b is made of nickel (Ni) to prevent corrosion of the copper plating film. As described above, the first metal tube 1 is formed by plating or tin (Sn) plating. A conductive layer 151 is also formed on the inner surfaces of the first metal tube 50a and the second metal tube 150b.
[0068] The conductive layer 174 is connected to the first metal tube 150a and the second metal tube 150b via a hollow tube 172 made of an insulating material. The second metal tube 150b is disposed opposite the first metal tube 150a to form a capacitor 152. That is, the first metal tube 150a and the second metal tube 150b have a conductive layer 174 on the inner surface. The hollow tube 172 is fitted with the capacitive coupling, and is used for generating inductively coupled plasma. The antenna body 148 is formed by the hollow tube 172 made of insulating material. By disposing the first metal tube 150a and the second metal tube 150b on the inner circumference thereof, inductively coupled plasma The unevenness of the antenna body 148 for generation can be reduced to make the inductively coupled plasma uniform. do.
[0069] In addition, the antenna body 148 for generating inductively coupled plasma is provided on the atmospheric side. A variable capacitor 176 may be provided in parallel with the capacitor 152. The impedance of the antenna body 148 for generating combined plasma can be adjusted precisely and over a wide range. As a result, the antenna 126 for generating inductively coupled plasma can receive high-frequency electric current. This makes it easier to match with the source 120.
[0070] Furthermore, the antenna body 148 for generating inductively coupled plasma has a capacitor 152 that is cooled by water. Since the condenser 152 is provided in the flow path of the cooling water (since the condenser 152 is in contact with the cooling water), With this configuration, the heat generation of the capacitor 152 can be effectively suppressed. The antenna 1 for generating inductively coupled plasma can be prevented from malfunctioning or being destroyed due to heat generated by the The high frequency power applied to 26 can also be increased.
[0071] As shown in FIG. 11, the antenna 126 for generating inductively coupled plasma is When applying high frequency power of 100 Hz, the length of the antenna body 148 for generating inductively coupled plasma is When the distance exceeds 3m, the problem of standing waves cannot be ignored. However, the problem of standing waves is caused by inductive coupling. The antenna body 148 for plasma generation is divided into two or more pieces as shown in FIG. 16 and FIG. 17. This can be eliminated by connecting the variable capacitor 176 for resonance in series.
[0072] The antenna body 148 for generating inductively coupled plasma has an oscillation frequency of 13.56 MHz or 2 The first antenna body 148a is connected to a 7 MHz high frequency power supply 120. The second antenna body 148b is connected to the first high frequency power source 120a, and the second antenna body 148b is connected to the second high frequency power source 120b. The first high frequency power supply 120a and the second high frequency power supply 120b are connected to The phases of the wave powers may be the same, but it is preferable that they are shifted by half a wavelength (180 degrees). This makes it possible to increase the plasma density on the surface of the target material 132. The first antenna body 148a is also connected to a first variable capacitor 158a. The tenna body 148b is connected to a second variable capacitor 158b. 158 (the first variable capacitor 158a and the second variable capacitor 158b) is an inductive Antenna body 148 for inductively coupled plasma generation (first antenna body 148a and second antenna The impedance of the power supply 120 (first high frequency power supply 120) is adjusted. a, the second high frequency power source 120b) is provided to facilitate impedance matching. .
[0073] Antenna body 148 for generating inductively coupled plasma (first antenna body 148a, second antenna The antenna body 148b) is also connected to an AC power source 122 having a frequency of 10 kHz to 1000 kHz. The antenna body 148 for generating inductively coupled plasma (first antenna body 148a, Between the second antenna body 148b and the AC power source 122, there is a coil for blocking high frequencies. 156 is inserted. In addition to high frequency power, AC voltage is applied to the antenna for inductively coupled plasma generation. By applying to the main body 148 (the first antenna main body 148a and the second antenna main body 148b), Therefore, the plasma density on the surface of the target material 132 can be increased.
[0074] Furthermore, by superimposing an AC voltage on the high frequency power, the deposits adhering to the insulating member 146 are (Products sputtered from the target material 132) are removed by the sputtering phenomenon. This makes it possible to suppress the deterioration of the discharge characteristics over time. When forming a transparent conductive film with a low resistance, the antenna for generating inductively coupled plasma shown in Figure 11 is used. The circuit configuration of the tenna 126 is advantageous in obtaining a stable discharge. In the case of forming a high-temperature oxide semiconductor film, the adhesion of deposits to the insulating member 146 does not have a large effect. Since the first antenna 126 is not affected by the power supply, the AC power supply 122 is not essential. When the distance between the first antenna 126a and the second antenna 126b becomes 300 mm or more, the sputtering temperature Since the plasma density in the central region of the target 124 is decreased, the first By applying an AC voltage between the antenna body 148a and the second antenna body 148b, The plasma density can be made uniform.
[0075] A pulse power supply 123 is connected to the sputtering target 124. 3. A negative power supply of -100V to -600V is applied to the sputtering target 124. As shown in Figure 13, a negative pulse voltage is applied to the inductively coupled plasma. The AC voltage applied to the antenna body 148 for generation is applied at a timing when the AC voltage becomes 0V. This makes it possible to emit sputtering particles in a direction perpendicular to the substrate. This allows for the deposition of a denser film.
[0076] FIG. 14 shows the results when an InGaZnO film was formed by sputtering as an oxide semiconductor film. The relationship between the target voltage and the film density is shown in the figure. The advantage of the ring method is that it requires a power source to generate and maintain the plasma and to control the sputtering deposition. The advantage of this is that it is possible to separate the two power sources and control them independently. In the DC magnetron method, the voltage applied to the sputtering target is -300V or less. If it is placed downwards, the plasma generation will be non-uniform and it will not be possible to maintain a stable discharge.
[0077] On the other hand, when using inductively coupled plasma, an antenna for generating inductively coupled plasma is used. By increasing the high frequency power applied to the plasma to increase the plasma density, negative oxygen ions and oxygen It is possible to generate a large amount of atomic radicals. The magnetic field of the magnet confines the plasma in the vicinity of the sputtering target. Since there is no contact between the metal and the substrate, the plasma can be uniformly brought into contact with the substrate surface. It is possible to promote the oxidation reaction with oxygen atoms.
[0078] When forming an InGaZnO film using the inductively coupled plasma sputtering method, By applying a voltage of about -200V to the sputtering target, The crystallization rate can be increased while minimizing damage to the deposited film. The film density of the InGaZnO film was 6.30 g / cm 3 This membrane tightness can be achieved. The theoretical value is 6.378g / cm 3 is close to the value.
[0079] In the conventional magnetron method, the target voltage must be increased to -300V or higher for stability. The inability to maintain a constant discharge increases damage to the film, reducing the film density by 6. 25g / cm 3 On the other hand, the inductively coupled plasma of the present embodiment The film formation apparatus 100 using the ZnO film is capable of forming oxide semiconductor films of various compositions, including InGaZnO films. It is possible to increase the film density and to reduce the shift in the threshold voltage Vth of the thin film transistor. In other words, the film forming apparatus using the inductively coupled plasma of this embodiment can reduce the The long-term reliability of the thin film transistor can be improved by the method according to claim 100.
[0080] FIG. 15 shows the configuration of the pre-treatment chamber 104. The pre-treatment chamber 104 contains a substrate stage. The substrate stage 114 is provided with a substrate 112 and a high-frequency discharge electrode 115. A lifting mechanism 164 for lifting the substrate 200 upward is added. 00, and the pins 162 are raised by a lifting mechanism 164. By protruding, the substrate 200 has a function of being raised up in a floating state.
[0081] The substrate stage 114 is made of a conductor so as to function as a ground electrode. The potential of the substrate stage 114 is set to be the same as that of the chamber wall of the chamber 104. The high-frequency discharge electrode 115 may include a built-in heater for heating a substrate (not shown). The high-frequency discharge electrode 115 and the substrate stage 114 are disposed opposite each other. The diode 114 is connected to a high-frequency power source 120 having an oscillation frequency of 13.56 MHz or 27 MHz. The pretreatment chamber 104 is also provided with a gas inlet pipe 166. From 166, a pre-treatment gas, for example, nitrogen (N2) gas, oxygen (O2) gas, or Nitrous oxide (N2O) gas is introduced. Also, instead of the gas introduction pipe 166, a shower A high-frequency discharge electrode 115 made of a plate is used, and gas is introduced from there. The pressure when generating plasma during pretreatment is 10 Pa to 10 3 Pa range is preferred.
[0082] The pre-treatment chamber 104 is a chamber in which a pre-treatment gas is introduced, and a high-frequency power is applied to a high-frequency discharge electrode 115. When the high frequency discharge plasma 168 is applied, the high frequency discharge plasma 168 is generated. After reaching a stable state, the substrate 200 is lifted by the pins 162 and the substrate stage 114 In this state, the high-frequency discharge plasma 168 is generated on the substrate 200. As a result, the surface of the substrate 200 is (the surface on which the thin film is deposited) as well as impurities and contaminants such as moisture adsorbed on the back and sides. The pin 162 is exposed to the plasma and does not emit impurities. For this reason, it is preferable that the insulating material is made of ceramics.
[0083] Up until now, plasma processing in a vacuum has been performed as a pre-processing of the substrate 200. However, usually, only the front side of the substrate 200 is plasma-treated, and the back side is not exposed to plasma. In this state, even if the front surface of the substrate 200 is cleaned, the back surface The moisture adsorbed on the substrate 200 remains on the substrate 200 even after the substrate 200 is transferred to the deposition chamber. Degassing from the back surface continues. In particular, in the case of sputtering deposition such as deposition of an oxide semiconductor film, When the gas pressure during degassing is low, degassing only on one side of the substrate 200 surface is insufficient. As a result, no matter how highly the deposition chamber is evacuated, the adsorbed particles are absorbed from the back side of the substrate 200. Since molecules (water (H2O), hydrogen (H2), hydrocarbons, etc.) continue to be released, the substrate The film quality is significantly different between the center and periphery of the oxide semiconductor film 200. When the film is formed by sputtering, the outgassing components released from the back surface of the substrate 200 are Due to the lack of control, the carrier concentration is large near the center of the substrate 200 compared to near the periphery. The larger the size of the substrate 200, the greater this problem becomes.
[0084] As a degassing process for the substrate 200, it is possible to heat the substrate 200 in a vacuum at a temperature of 200° C. or higher. However, it takes several hours to completely remove the adsorbed moisture, making this method unsuitable for mass production. When forming an oxide semiconductor film in a single-wafer process, a heat treatment is performed for several hours for each substrate 200. That is not realistic.
[0085] However, as shown in this embodiment, the substrate 200 is By floating the substrate and performing plasma treatment, not only the front surface but also the back surface is exposed to the plasma. Degassing of the entire surface is possible, and the entire surface of the substrate can be cleaned in a short time, and the carrier concentration This enables precise control of the
[0086] To reiterate, the important point in the film formation apparatus 100 for forming an oxide semiconductor film is that Before the sputtering film formation, adsorbed components (water (H2O), hydrogen (H2, hydrocarbons) are forcibly degassed with nitrogen plasma or oxygen plasma. As a result, a uniform oxidation with a constant carrier concentration is achieved over the entire surface of the substrate 200. It is possible to fabricate a semiconductor film.
[0087] The deposition chamber 108 of the deposition apparatus 100 described above is made of a metal that is less susceptible to outgassing. It is preferable that the insulating layer is made of a material such as an oxide for forming a thin film transistor. When forming a semiconductor film, it is necessary to increase the film density in order to improve the reliability. In order to increase the film density, the sputtering pressure during sputtering deposition should be increased from approximately 0.1 Pa to 1.5 Pa. In this pressure range, the inductively coupled plasma is required to be in the deposition chamber at about 1 Pa. Since the plasma spreads over the entire surface of the 108, the inner wall is exposed to the plasma. When the ions collide with the inner walls of the deposition chamber, they convert the adsorbed moisture (H2O), hydrogen (H2) These impurities are then released into the oxide semiconductor. This can affect the characteristics of transistors formed from conductive films.
[0088] The deposition chamber 108 of the deposition apparatus 100 shown in this embodiment is made of stainless steel in consideration of strength. However, the iron (Fe) and molybdenum (M) components of stainless steel are Elements such as manganese (Mn) and ZnO are poor electron killers for n-type oxide semiconductors. This is not desirable because it will result in a pure product. If the oxide semiconductor film is present in the oxide semiconductor film, the characteristics of the transistor including the oxide semiconductor film are adversely affected. In conventional sputtering equipment, the stainless steel is left exposed in the deposition chamber. Since the oxide semiconductor film is used in the manufacturing process, the manufacturing yield of the transistor using the oxide semiconductor film is decreased. This is a factor that reduces the reproducibility of the process.
[0089] In order to solve such a problem, the film forming apparatus 100 according to the present embodiment includes a film forming chamber Among 108, magnesium (Mg), aluminum (Al), titanium (Ti), tungsten A plasma diffusion prevention plate 140 made of a metal such as stainless steel (W) or nickel (Ni) is provided. In addition, the electron density in the plasma is increased to confine the plasma. In order to improve the stability of the charge, a plasma diffusion prevention plate 140 is provided on its surface with a high secondary electron emission rate. Magnesium oxide (MgO), barium oxide (BaO), and strontium oxide (SrO) , a film of an oxide of an alkaline earth metal such as calcium oxide (CaO), or a film containing these A structure is adopted in which an insulating film made of silicon oxide, aluminum oxide, yttrium oxide, etc. is provided. is.
[0090] As shown in FIG. 1 and FIG. 2, the film forming apparatus 100 includes a first film forming chamber 108a and a second film forming chamber 108b. The first deposition chamber 108a and the second deposition chamber 108b are provided. Depending on the configuration of the chamber 108b, two types of oxide semiconductor films having different film properties can be stacked. For example, a first oxide semiconductor film is deposited in the first deposition chamber 108a, and a second oxide semiconductor film is deposited in the second deposition chamber 108b. A second oxide semiconductor film can be deposited in film chamber 108b.
[0091] For example, in the first deposition chamber 108a, a sputtering process is performed using an oxide semiconductor target. The deposition was performed using argon (Ar) alone or argon (Ar) and oxygen (O2) as gas. In the second deposition chamber 108b, argon (Ar) and oxygen (O2) are used. The oxygen partial pressure is set higher than that in the first deposition chamber 108a, and deposition can be performed. In sputtering of an oxide semiconductor film, the oxygen partial pressure can be increased to The density of negative ions can be increased, and the negative ions of oxygen on the deposition surface of the thin film can be reduced. This allows the irradiation density of the ions to be increased. In contrast to the oxide semiconductor film deposited in the first deposition chamber 108b, the oxide semiconductor film deposited in the second deposition chamber 108c is The rear density can be reduced and the crystallinity can be improved.
[0092] Furthermore, by applying a negative pulse voltage to the sputtering target 124, Negative oxygen ions generated during discharge are deposited on the oxide semiconductor film surface during application of a pulse voltage. In this embodiment, the induced oxygen reaches the film, which promotes densification of the film and facilitates crystallization. The antenna 126 for generating coupled plasma can generate a large amount of oxygen radicals. When the inductively coupled plasma comes into contact with or is close to the surface of the substrate 200, the metal element reacts with oxygen. This reduces the probability of unreacted oxygen (O2) molecules being trapped in the film. can be done.
[0093] In this manner, the film forming apparatus 100 according to the present embodiment employs a moving film forming method. The first deposition chamber 108a and the second deposition chamber 108b are connected in series. By this, the carrier concentration can be precisely controlled when depositing the oxide semiconductor film. In this embodiment, an example in which an oxide semiconductor film is formed using the film forming apparatus 100 will be mainly described. However, the film forming apparatus 100 is not limited to this, and may be used for forming transparent conductive films, other semiconductor films, and metal films. This can also be applied to manufacturing.
[0094] In this embodiment, the front view of FIG. 16A and the cross-sectional view of FIG. 16B (A1 shown in FIG. 16A) As shown in the cross-sectional structure corresponding to the -A2 section, the first antenna 126a and the second antenna 12 6b extends in the same direction as the longitudinal direction of the sputtering target 124 and has approximately the same length. In this example, a first insulating member 146a having a U-shaped groove shape is used. The second insulating member 146b is surrounded by the first chamber wall 109a and the plasma diffusion prevention plate 140. The first antenna body 148a and the second antenna body 148b are provided so as to protrude inward from the area. 148b is surrounded by a first insulating member 146a and a second insulating member 146b having a U-shaped groove shape. It is set up so that
[0095] However, the first antenna 126a and the second antenna 126b are shown in FIG. 16A and FIG. The embodiment is not limited to the form shown in FIG. 1B, and the first antenna 126a and the second antenna 126b may be U-shaped. For example, the front view of FIG. 17A and the front view of FIG. 17B As shown in the cross-sectional view (cross-sectional structure corresponding to the line B1-B2 shown in FIG. 17A), Antenna bodies 148a_1 to 148a_3, a plurality of second antenna bodies 148b_1 to 14 8b_3 may be divided along the longitudinal direction of the sputtering target 124. With such an arrangement of the first antenna 126a and the second antenna 126b, This increases the plasma density, and allows a dense film to be deposited. FIG. 17B shows an arrangement of an inductively coupled plasma generating antenna in the longitudinal direction of the sputtering target 124. The antenna body 148 is divided into three parts for generating inductively coupled plasma. The first antenna 126a and the second antenna 126b are used for generating inductively coupled plasma. There is no limit to the number of divisions of the antenna body 148, and the antenna body 1 for generating inductively coupled plasma may be divided into any number of parts. An antenna for generating inductively coupled plasma may be arranged in which 48 is divided into three or more.
[0096] The present invention is not limited to the above-described embodiment, and may be modified as appropriate without departing from the spirit and scope of the present invention. In addition, the embodiments can be appropriately combined.
[0097] FIG. 18A shows an example of a device fabricated using the film forming apparatus 100. 18A shows a cross-sectional structure of the transistor 230. includes an oxide semiconductor layer 216 formed on a substrate 200 by a film formation apparatus 100.
[0098] Specifically, the transistor 230 is formed on a first insulating layer 210 on the surface of the substrate 200. On the first insulating layer 210, a first conductive layer 212a and The first conductive layer 212b forming the drain electrode is provided in pairs. a, 212b are, for example, indium tin oxide (ITO), indium zinc oxide (IZ The first conductive layers 212a and 212b are formed of a transparent conductive film such as a transparent insulating film. In order to achieve this, second conductive layers 214a and 214b are provided, which are made of a metal material such as aluminum (Al). It may be possible to use
[0099] The oxide semiconductor layer 216 is formed by the first conductive layers 212a and 212b (and the second conductive layers 214a and On the oxide semiconductor layer 216, a gate insulating layer is formed. A functional second insulating layer 218 is provided, and a gate insulating layer 218 is formed on the gate insulating layer 218 so as to overlap the oxide semiconductor layer 216. A port electrode 220 is provided.
[0100] The oxide semiconductor layer 216 may be formed of multiple layers having different compositions and crystallinity. For example, as shown in FIG. 18B, a first oxide semiconductor layer 216a and a second oxide semiconductor layer 216b The first oxide semiconductor layer 216a may have a stacked structure. n), gallium (Ga), and tin (Sn). The conductor layer 216b has a higher ratio of gallium (Ga) than the first oxide semiconductor layer 216a. The second oxide semiconductor layer 216b is preferably made of the first oxide semiconductor The second oxide semiconductor layer 216b is formed thinner than the second oxide semiconductor layer 216a. Since the concentration is high, the band gap is wider than that of the first oxide semiconductor layer 216a. For example, the first oxide semiconductor layer 216a has a thickness of 40 nm or less. The first oxide semiconductor layer 216b is formed to a thickness of 4 nm to 60 nm. It is formed with a film thickness of about one-tenth of that of the original thickness, m.
[0101] The transistor 230 is made up of a first oxide semiconductor layer 216a and a second insulating layer 218 (gate insulating layer). By providing such a second oxide semiconductor layer 216b between the first oxide semiconductor layer 216a and the second oxide semiconductor layer 216b, carriers can be A channel region in which current flows is formed in the first oxide semiconductor layer 216a, which is called a buried channel. That is, the transistor 230 is formed by the second insulating layer 218 (gate insulating layer) and The capacitance is not affected by defects formed at the interface with the oxide semiconductor layer 216. By having such a structure, the transistor 230 can This makes it possible to stabilize characteristics and reduce characteristic variations.
[0102] As shown in FIG. 18C, the oxide semiconductor layer 216 is a first oxide semiconductor layer 216a Even if a third oxide semiconductor layer 216c is provided between the first oxide semiconductor layer 216b and the second oxide semiconductor layer 216c, The third oxide semiconductor layer 216c is also a ternary oxide semiconductor, but is made of indium. The concentration of In is higher than that of the first oxide semiconductor layer 216a and the second oxide semiconductor layer 216b. By providing such a third oxide semiconductor layer 216c, The transistor 230 can enhance the field effect mobility.
[0103] According to the film formation apparatus 100 of this embodiment, the structure of the oxide semiconductor layer 216 shown in FIG. The structure can be produced by using a sputtering target 124 shown in FIG. 10A. The structure of the oxide semiconductor layer 216 shown in FIG. 18C is the same as that of the sputtering target shown in FIG. In other words, oxide semiconductors having different compositions and crystallinity can be fabricated using the get 124. Conductors can be deposited successively in a vacuum.
[0104] The composite segmented target shown in FIG. 10A and FIG. 10B is a conventional magnetron type. Sputtering equipment cannot be used because abnormal discharges tend to occur at the split parts. In the method without using a nozzle, positively charged argon is applied to the entire surface of the sputtering target. Since the ions are almost uniformly incident on the substrate, abnormal discharge is unlikely to occur. The entire surface of the target is sputtered uniformly, so the surface of the sputtering target Therefore, cracks due to thermal stress in the sputtering target are also prevented. It is unlikely to occur.
[0105] InGaSnO, which can be used to fabricate oxide semiconductor films with high electron mobility x Tar In conventional magnetron sputtering equipment, the get is a sputtering target. Fine cracks called hairline cracks are easily generated in the steel, and it is not used in mass production factories. In contrast, the film forming apparatus 100 according to the present embodiment does not use a magnet. Since no external heating is used, the plasma does not concentrate locally, and localized heat generation does not occur. This also makes hairline cracks caused by thermal stress less likely to occur.
[0106] In the film forming apparatus 100 according to this embodiment, the plasma diffusion prevention plate 140 is used. The ICP prevents the plasma from spreading throughout the interior area of the deposition chamber 108. By doing so, the deposition rate can be increased even in the moving deposition method, in which the substrate is moved while the sputtering deposition is performed. It is possible to form a film without any deterioration.
[0107] Furthermore, by applying a negative pulse voltage to the sputtering target 124, Even if the target material 132 is a high resistance material, stable sputtering film formation can be performed. Furthermore, negative oxygen ions can be made to be incident perpendicularly onto the substrate 200. Therefore, even when the deposition gas pressure is about 1.5 Pa, the decrease in the film density can be prevented. For example, Even on 11th generation glass substrates (3000mm x 3320mm), high mobility is achieved by increasing film density. Therefore, an oxide semiconductor film can be deposited with high reliability at high speed.
[0108] Note that the structure of the transistor 230 shown in FIG. 18A is an example, and the film formation according to this embodiment The device 100 can be used to fabricate oxide semiconductor transistors of various structures, regardless of whether they are top-gate or bottom-gate. It can be used to fabricate transistors.
[0109] [Second embodiment] In this embodiment, sputtering using inductively coupled plasma and vacuum deposition (and / or The following shows an example of a film forming apparatus capable of continuously performing the deposition of a thin film by electron beam evaporation. The film forming apparatus is, for example, an organic electroluminescence element (or an organic electroluminescence The present invention can be applied to the manufacture of a display device (a display device) and the like. In the following, the film formation shown in the first embodiment will be described. The following description will focus on the differences from the device 100.
[0110] FIG. 19 shows the overall configuration of a film forming apparatus 101 according to this embodiment. a load / unload chamber 102 in which substrates before and after film formation are stored; a pre-treatment chamber 104 for performing the treatment, a first transfer chamber 10 in which a transfer robot 116 is provided, 6a, a second transfer chamber 106b provided with a platen mechanism 118, and a sputtering film formation a first deposition chamber 108a in which the deposition is performed, a third transfer chamber 117 in which a platen mechanism 118 is provided, 06c, a fourth transfer chamber 106d in which a transfer robot 116 is provided, and an evaporation source 111 is provided. The third deposition chamber 108c, the fourth deposition chamber 108d and the fifth deposition chamber 1 These chambers are connected by gate valves and have a vacuum exhaust system (not shown). A ventilation means is provided.
[0111] The pre-treatment chamber 104, the first transfer chamber 106a, the second transfer chamber 106b, the third transfer chamber 106c, The transfer chamber 106c and the fourth transfer chamber 106d have the same configuration as in the first embodiment. In the first deposition chamber 108a, sputtering is performed by inductively coupled plasma. This is the chamber where the film is formed, and the electron injection layer described later is formed. The fourth film-forming chamber 108c and the fourth film-forming chamber 108d are provided with an evaporation source 111 and perform vacuum deposition. This is a chamber in which organic films such as a light-emitting layer and a hole transport layer, which will be described later, are formed. The fifth film formation chamber 106e is provided with an evaporation source 111, and is used for vacuum deposition (and This is a chamber in which the anode is deposited by deposition (described later) using a vacuum evaporation method (or an electron beam deposition method).
[0112] The film formation apparatus 101 shown in FIG. 19 performs sputtering film formation using inductively coupled plasma. and a chamber in which a film is formed by vacuum deposition (and / or electron beam deposition). The inorganic and organic films are deposited successively in a vacuum by connecting the two via a transfer chamber. In addition, the first deposition method includes the step of performing sputtering deposition using inductively coupled plasma. A second transfer chamber 106b in which a platen mechanism 118 is provided is disposed on either side of the chamber 108a. The third transfer chamber 106c is provided, so that the sputtering deposition can be performed on the substrate 20. The film was formed with the substrate held vertically or tilted about 20 degrees from the vertical, and then vacuum deposition (and / or electrochemical deposition) was performed. In the case of deposition by the electron beam deposition method, deposition is performed while the substrate 200 is held approximately horizontally. can.
[0113] The number of chambers in which the film is formed by vacuum deposition (and / or electron beam deposition) is arbitrary. The number of layers and the type of the deposited films can be appropriately determined.
[0114] FIG. 20 is a diagram showing the configuration of the film forming apparatus 101. Except for the pre-treatment chamber 104, the first transfer chamber 106a, the second transfer chamber 106b, The first film formation chamber 108a, the third transfer chamber 106c, the fourth transfer chamber 106d, The main components provided in or connected to the third deposition chamber 108c are shown. Except for chamber 108c, the configuration of the other chambers is similar to that of the first embodiment.
[0115] A third deposition chamber 10 in which deposition is performed by vacuum deposition (and / or electron beam deposition) 8c is equipped with a turbo molecular pump, dry pump, and cryopump as the vacuum exhaust system 110. Such a vacuum exhaust system 110 realizes high vacuum exhaust and removes the residual gas from the chamber. The deposition of the film by vacuum deposition is performed by using a linear evaporation source 11. Alternatively, a moving deposition method in which the substrate moves in front of the evaporation source 111 may be adopted. Alternatively, a scanning deposition method in which the substrate is moved in a scanning manner may be adopted.
[0116] The film forming apparatus 101 is a device for forming films by sputtering and vacuum deposition (and / or electron beam deposition). In the film deposition by the moving deposition method, a moving deposition method is adopted, so substrates of various sizes can be deposited. For example, the film forming apparatus 101 can be used for 11th generation glass substrates (300 It can be used to deposit films of dimensions 20.0 mm x 3320 mm.
[0117] FIG. 21 shows an example of a device fabricated using the film forming apparatus 101. The element shows a cross-sectional structure of an organic electroluminescent element 300. The light-emitting element 300 is provided on the substrate 200 with a carrier injection amount control electrode 302, a first insulating layer 303, and a second insulating layer 304. 04, a first electrode (cathode) 306, an electron transport layer 308, and a second insulating layer in which an opening 311 is formed layer 310, an electron injection layer 312, an emissive layer 314, a hole transport layer 316, a hole injection layer 318, The organic electroluminescence element 30 has a structure in which two electrodes (anodes) 320 are laminated. 0 indicates the area where the opening 311 is provided, in which the carrier injection amount control electrode 302 and the first insulating layer 303 are formed. An edge layer 304, an electron transport layer 308, an electron injection layer 312, an emissive layer 314, a hole transport layer 316, The hole injection layer 318 has an overlapping region with the second electrode (anode) 320 .
[0118] The carrier injection control electrode 302 is insulated from the electron transport layer 308 and is a positive valence. When a bias voltage is applied, electrons are emitted from the electron transport layer 308 through the electron injection layer 312. Controlling the amount of carriers (electrons) injected into the light emitting layer 314 and the light emitting position in the light emitting layer 314 The organic electroluminescence element 300 is a bottom transmission type. Therefore, the carrier injection amount control electrode 302 is formed of a transparent conductive film.
[0119] The electron transport layer 308 has a two-layer structure. The first electron transport layer 308a is a first insulating layer 304. The first electrode (cathode) 30 is provided on the substrate 301 and has a larger area than the carrier injection amount control electrode 302. The first electrode (6) is provided outside the opening 311 (the area overlapping with the second insulating layer 310). The cathode 306 is formed, for example, of a two-layer structure of a first conductive layer 306a and a second conductive layer 306b. The end of the first conductive layer 306a may overlap with the carrier injection amount control electrode 302. The first conductive layer 306a is formed of a transparent conductive film such as ITO or IZO. It has a function of forming an ohmic contact with the electron transport layer 308 and injecting electrons. The conductive layer 306b is appropriately provided to reduce the resistance of the first electrode (cathode) 306.
[0120] The first electron transport layer 308a is made of a metal oxide having semiconducting properties. Metal oxides include In2O3-Ga2O3-SnO2-ZnO oxide materials, In2 O3-Ga2O3-SnO2 oxide materials, In2O3-SnO2-ZnO oxide materials , In2O3-Al2O3-ZnO oxide materials, Ga2O3-SnO2-ZnO oxide materials Materials, Ga2O3-Al2O3-ZnO oxide materials, SnO2-Al2O3-ZnO In2O3-ZnO oxide materials, SnO2-ZnO oxide materials, Al 2O3-ZnO-based oxide materials, Ga2O3-SnO2-based oxide materials, Ga2O3-ZnO system oxide materials, Ga2O3-MgO system oxide materials, MgO-ZnO system oxide materials, SnO 2-MgO-based oxide materials, In2O3-MgO-based oxide materials, In2O3-based metal oxide materials materials, Ga2O3-based metal oxide materials, SnO2-based metal oxide materials, ZnO-based metal oxide materials Such a first electron transport layer 308a can be formed by using the same composition as that shown in the first embodiment. The film can be produced by a sputtering method using the film device 100.
[0121] A second insulating layer 310 is provided on the first electron transport layer 308a. An opening 311 is provided in the second electron transport layer 308a to expose the surface of the first electron transport layer 308a. The first electron transport layer 308b is made of a metal oxide material having semiconductor properties similar to the first electron transport layer 308a. The second electron transport layer 308b may be formed by a sputtering method. It may be formed in the region 311 by a coating method.
[0122] In this case, the second insulating layer 310 is preferably formed of an insulating film having polarity. Such a second insulating layer 310 can be formed using a straight-chain fluorine-based organic material. As a straight-chain fluorine-containing organic material, for example, a fluoroalkylsilane (FAS)-based material is used. Fluoroalkylsilane (FAS) materials include, for example, H, 1H, 2H ,2H-Perfluorodecyltrichlorosilane (FDTS), Tridecafluoro-1,1 ,2,2-Tetrahydrooctyltrichlorosilane (FOTS), etc. are used. The edge layer 310 is formed using a linear fluorine-containing organic material, and thus has a water-repellent surface. An opening 311 is formed in the second insulating layer 310. The water repellency of the surface of the opening 311 is strongly expressed on the surface, and the side wall surface of the opening 311 is hydrophilic in comparison with the surface. It becomes a state of mind.
[0123] When the second electron transport layer 308b is formed by a coating method, the above-mentioned quaternary oxide materials, ternary oxide materials, Compositions containing a cation-based oxide material, a binary oxide material, a monocation-based oxide material, or precursors thereof - Patents.com The solution is applied onto the second insulating layer 310 in which the opening 311 is formed, and then dried and baked. A specific example is zinc oxide (ZnO) with aluminum as a trivalent metallic element. By doping with tungsten (Al), indium (In), gallium (Ga), etc., the resistivity becomes 1 0 2 Ωcm~10 5 The second insulating layer 3 is baked to have a resistivity in the range of Ωcm. When the surface of 10 is water-repellent, the viscosity of the composition to be applied can be appropriately adjusted. The coating film is selectively formed in the opening 311. After baking, the second electron transport layer 308b is Since the side wall surface of the portion 311 is hydrophilic, the contact surface with the second insulating layer 310 is The cross-sectional shape has a gently tapered inclination toward the inside. The average thickness of the second electron transport layer 308b is preferably 200 nm or more. The second electron transport layer 308b has such a thickness. As a result, the occurrence of short-circuit defects in the organic electroluminescence element 300 is greatly reduced, improving the yield. It is possible.
[0124] The organic electroluminescent device 300 is formed by forming a first electron transport layer 314 before the light emitting layer 314 is formed. A second insulating layer 310 is provided, in which an opening 311 is formed to expose the upper surface of the transfer layer 308a. In this way, a light emitting region can be defined. The end of the electron transport layer 308b is formed into a tapered shape that is gently inclined from the wall surface of the opening 311. By having a planar shape, the electron injection layer 312 and the light emitting layer 314 to be formed in the next step can be formed. Step coverage can be improved.
[0125] The electron injection layer 312 is made of a material with a small work function to inject electrons into the light emitting layer 314. For example, the electron injection layer 312 is made of calcium (Ca) oxide, aluminum (A As an example, the electron injection layer 312 is made of a material containing C12A7(1 2Ca·7Al2O3) electride. C12A7 electride is a semiconductor. It has excellent thermal conductivity and can be controlled from high to low resistance. Its work function is 2.4 eV. Since the energy of the electron injection layer 312 is about the same as that of an alkali metal, it is preferably used as the electron injection layer 312. It is possible.
[0126] The electron injection layer 312 is made of Zn 0.7 Mg 0.3 O, Zn 0.75 S 0.25 O. These metal oxides have semiconducting properties and a work function of 3.1. Since the metal oxides are as small as 1.0 eV, electrons can be injected into the light-emitting layer 314. In addition, since the band gap is large at 3.9 eV to 4.1 eV, holes can pass through the light emitting layer 314. It is possible to prevent the Zn from passing through the electron transport layer 308. 0.7 Mg 0.3 O and Zn 0.75 S0.25 O and two metal oxides in the range of 1:4 to 1:10. A ternary metal oxide semiconductor material having a ternary structure may also be used as the electron injection layer 312. .
[0127] Such an electron injection layer 312 is formed by the film forming apparatus 101. The polycrystalline electride was used as the sputtering target 124, and the first deposition chamber was The electron injection layer 312 made of C12A7 electride is formed at 1n The electron injection layer 312 is made of C12A7 electride and has a thickness of 100 nm. It is formed as an amorphous thin film, but may also have crystallinity. Since lectride is stable in the air, it has been used as an electron injection layer. Lithium fluoride (LiF), lithium oxide (Li2O), sodium chloride (NaCl), Compared with alkali metal compounds such as potassium chloride (KCl), it is easy to handle and has a smooth surface. This has the advantage that the film can be formed by a deposition method.
[0128] Zinc 0.7 Mg 0.3 O, Zn 0.75 S 0.25 Sputtering of polycrystalline materials such as O The target 124 is used, and a sputtering method using inductively coupled plasma is used. The electron injection layer 312 can be formed by using Zn 0.7 Mg 0.3 O and Zn 0.75 S 0.25 Polycrystalline ternary metal oxide materials mixed with O in the range of 1:4 to 1:10 As a sputtering target 124, a film forming apparatus 1 using inductively coupled plasma was used. By performing sputtering deposition at 00, the electron injection layer 312 can be formed. 12A7 electride is stable in air, but is easily soluble in water, so it is not suitable as a target material. When used as a storage medium, moisture-proofing measures are required. 0.7 Mg 0.3 O and Zn 0.75 S 0.25 A ternary system of 1:4 to 1:10 mixed gold and O Metal oxide polycrystalline target material is difficult to dissolve in water, so it is easy to store and manage. .
[0129] Zn used as the electron injection layer 312 0.7 Mg 0.3 O and Zn 0.75 S 0.2 Since the resistivity of 5O is very high, it is difficult to sputter it using conventional DC magnetron sputtering equipment. The sputtering target is divided into two parts and the AC power supply is AC dual magnetron with alternating sputtering on each target using Although it is possible to use a sputtering device, in order to increase the film density and the crystallization rate, The discharge pressure during sputtering must be 0.3 Pa or less. However, the size of the substrate is For G8.5 (2500mm x 2200mm) and above, uniformity within the surface is achieved at 0.3Pa or less. In contrast, it becomes difficult to stably discharge the battery while maintaining the charge. In the method using inductively coupled plasma, the sputtering target 124 is It is possible to deposit a film by applying a pulse voltage, and the pressure during sputtering deposition is Even if the pressure is increased to around 1.3 Pa, crystallization can be promoted and the film density can be increased.
[0130] Before the electron injection layer 312 is formed in the first deposition chamber 108a, the electron transport layer 30 The substrate 200 formed up to step 8 may be subjected to a degassing process in the pre-processing chamber 104 . By carrying out the pretreatment, moisture and the like that are taken in the organic electroluminescence element 300 can be prevented. The amount of impurities can be reduced.
[0131] After the electron injection layer 312 is formed in the first deposition chamber 108a, the substrate 200 is transferred to the third The platen mechanism 118 of the chamber 106c returns the platen 118 to a horizontal position. 6d to the third deposition chamber 108c. The light-emitting layer 314 is formed by vacuum deposition (and / or electron beam deposition).
[0132] The light-emitting layer 314 is formed using a metal mask having through holes formed in accordance with the arrangement of the openings 311. The light-emitting layer 314 is formed by vacuum deposition using a material corresponding to each known light-emitting color. The thickness of the light-emitting layer 314 is appropriately set, for example, from 10 nm to 100 nm. When a white light emitting layer is to be formed as the light emitting layer 314, a metal The light emitting layer 314 may be formed on the entire surface of the element forming region without using a mask.
[0133] After the light-emitting layer 314 is formed, the substrate 200 is transferred to the fourth transfer chamber 106d. The substrate is transferred to the film chamber 108d, where a hole transport layer 316 and a hole injection layer 318 are formed. The hole transport layer 316 may be formed of an arylamine compound, an amine compound containing a carbazole group, Using known materials such as amine compounds including fluorene derivatives, a vacuum deposition method (and / or The hole injection layer 318 is formed by a method such as electron beam deposition. Metal oxides such as vanadium oxide, ruthenium oxide, tungsten oxide, and manganese oxide Vacuum deposition method (and / or) using phthalocyanine-based materials such as copper phthalocyanine or copper phthalocyanine For example, the hole transport layer 316 is formed to a thickness of 10 nm to 500 nm. The hole injection layer 318 is formed to a thickness of 1 nm to 100 nm.
[0134] In this embodiment, the hole transport layer 316 and the hole injection layer 318 are formed in the same deposition chamber. However, the present invention is not limited to this example, and the film forming apparatus 101 may be used in many other film forming processes. The hole transport layer 316 and the hole injection layer 318 are deposited in different deposition chambers. This is also fine.
[0135] After the hole transport layer 316 and the hole injection layer 318 are deposited, the substrate 200 is transferred to a fourth transfer chamber. The substrate is transferred to the fourth deposition chamber 108d via 106d, and a film is formed on the second electrode (anode) 320. The second electrode (anode) 320 is a metal film such as aluminum (Al) or an ITO The display is formed of a laminate of a transparent conductive film such as IZO and a metal film such as aluminum (Al). Such a second electrode (anode) 320 is formed in the fourth film-forming chamber 108d by vacuum deposition (and It is produced by a method called CVD (electron beam deposition and / or electron beam evaporation).
[0136] As described above, the organic electroluminescence element 300 is manufactured by the film forming apparatus 101. The film forming apparatus 101 is a device for performing sputtering film formation using inductively coupled plasma. The chamber where the film is deposited by vacuum deposition (and / or electron beam deposition) The electron injection layer 312 and the light emitting layer 313 are connected to each other via the transfer chamber 106. 14, the hole transport layer 316, the hole injection layer 318, and the second electrode (anode) 320 are connected in vacuum. By using the film forming apparatus 101 having such a configuration, The organic electroluminescence element 300 and the organic electroluminescence element 301 are highly reliable and highly practical. A display panel including the luminescent element 300 can be fabricated. [Explanation of symbols]
[0137] 100: film forming apparatus, 101: film forming apparatus, 102: load / unload chamber 104 a pre-treatment chamber, 106 a transfer chamber, 108 a deposition chamber 109: chamber wall; 110: vacuum exhaust system; 111: evaporation source; 112: 115...high frequency discharge electrode; 116... 118...transport robot, 118...platen mechanism, 120...high frequency power source, 122...exchanger current power source, 123...pulse power source, 124...sputtering target, 126... Antenna for inductively coupled plasma generation, 127, heater, 128, through hole, 13 0···Backing plate, 131···Bonding material, 132···Target material , 134 , shield plate, 136 , insulating part, 138 , gas introduction pipe, 140 , Plasma diffusion prevention plate, 141, adhesion prevention plate, 142, first surface, 143, second surface surface, 144 . . . first opening, 146 . . . insulating member, 147 . . . glass layer, 148 . . . Antenna body for generating inductively coupled plasma, 150, metal tube, 151, conductive layer , 152 , condenser, 153 , O-ring, 154 , second opening, 156 , Coil, 158 variable capacitor, 160 carrier tray, 162 Pin, 164... lifting mechanism, 166... gas introduction tube, 168... high frequency discharge plasma 170 mesh, 172 hollow tube, 174 conductive layer, 176 Variable capacitor, 180... ceramic member, 200... substrate, 202... surface, 204...antenna connection region; 210...first insulating layer; 212...first conductive layer; 14 second conductive layer, 216 oxide semiconductor layer, 218 second insulating layer, 220 Gate electrode, 230 Transistor, 300 Organic electroluminescent device 302 . . . carrier injection amount control electrode; 304 . . . first insulating layer; 306 . . . First electrode (cathode), 308 Electron transport layer, 310 Second insulating layer, 311 Open mouth portion, 312 , electron injection layer, 314 , light emitting layer, 316 , hole transport layer, 318 Hole injection layer, 320 Second electrode (anode)
Claims
1. a deposition chamber in which a sputtering target having a rectangular shape in a plan view is placed; A film that covers the sputtering target and overlaps the surface of the sputtering target. a plasma diffusion prevention plate having a rectangular opening at a position; The plasma diffusion prevention plate has a U-shaped groove shape in cross section and protrudes into the area surrounded by the plasma diffusion prevention plate. an insulating member extending along the longitudinal direction of the sputtering target; A rod for generating inductively coupled plasma extending along the longitudinal direction of the sputtering target. a shaped antenna; having The insulating member is arranged to separate a vacuum space of the deposition chamber from an atmospheric space. Located in The rod-shaped antenna is disposed on the atmospheric side of the insulating member and in the U-shaped groove. Placed, The rod-shaped antenna is not in contact with the insulating member having the U-shaped groove shape. A sputtering apparatus comprising:
2. the insulating member is inserted into a through hole provided in the film formation chamber from the atmosphere side; 2. The sputtering apparatus of claim 1.
3. The sputtering method according to claim 1 , wherein a glass layer is provided on a surface of the insulating member. Device.
4. The insulating member is provided with a vacuum seal portion in contact with the wall of the deposition chamber on the atmospheric side.
3. The sputtering apparatus according to claim 2 .
5. The insulating member is made of quartz, alumina, yttria (Y 2 O 3 ), forsterite (Mg 2 SiO 4 ), steatite (MgO.SiO 2 ) is made of a material selected from 2. The sputtering apparatus of claim 1 .
6. The rod-shaped antenna is provided at a position protruding from the surface of the sputtering target.
2. The sputtering apparatus of claim 1 .
7. The rod-shaped antenna is divided into a plurality of parts along the longitudinal direction of the sputtering target.
2. The sputtering apparatus of claim 1 .
8. The rod-shaped antenna is formed of a plurality of metal tubes, and the plurality of metal tubes are connected via a capacitor.
7. The sputtering apparatus of claim 6, wherein the first and second electrodes are connected to each other via a first electrode.
9. The rod-shaped antenna has a structure in which the plurality of metal tubes are connected by an insulating hollow tube. The sputtering apparatus of claim 8 .
10. The insulating member and the rod-shaped antenna are provided on both sides of the sputtering target.
2. The sputtering apparatus of claim 1 .
Citation Information
Patent Citations
Sputtering apparatus
JP2014037555A
Antenna cover and plasma generation device using the same
JP2015115172A
Film deposition method and film deposition apparatus
JP2019052345A
Antenna and plasma processing apparatus
JP2019160593A
Film deposition method and sputtering apparatus
JP2016065299A