Rubber composition
A rubber composition with a rubber component, softener, and filler achieves a balance of flexibility and mechanical strength, addressing the limitations of existing compositions by enhancing both properties in rubber molded articles.
Patent Information
- Application Number
- JP2021174485
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2021-10-26
- Publication Date
- 2024-12-04
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing flexible rubber compositions, such as those made from silicone and urethane rubbers, lack mechanical strength, while olefin elastomers, which are mechanically strong, lack flexibility, making it difficult to achieve a balance between these properties in rubber molded articles.
A rubber composition comprising a rubber component, a softener, and a filler, with specific ratios and properties, including a range for the number of fillers per unit volume and average primary particle diameter, to enhance both flexibility and mechanical strength.
The rubber composition achieves a balanced combination of flexibility and mechanical strength, suitable for forming rubber molded articles with improved properties.
Smart Images

Figure 2024167455000001 
Figure 2024167455000002 
Figure 2024167455000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a rubber composition. [Background technology]
[0002] Conventionally, flexible rubber compositions have been used in various applications such as seals, packings, O-rings, etc. A flexible rubber composition is a rubber composition with a low hardness, the A hardness of which is less than 30 when measured with a hardness meter, and for example, Patent Document 1 discloses a rubber composition obtained by mixing an olefin-based rubber composition containing ethylene-propylene rubber and / or ethylene-propylene-diene rubber and conductive carbon black with a silicone rubber composition containing a specific organopolysiloxane.
[0003] Patent Document 2 discloses a thermoplastic elastomer resin composition comprising 100 parts by weight of (a) a block copolymer consisting of at least two polymer blocks A mainly made of a vinyl aromatic compound and at least one polymer block B mainly made of a conjugated diene compound, and / or a hydrogenated block copolymer obtained by hydrogenating the same, (b) 150 to 400 parts by weight of a non-aromatic rubber softener, (c) 1 to 20 parts by weight of a vinyl aromatic resin, (d) 5 to 20 parts by weight of a hydrogenated petroleum resin, and (e) 0.1 to 5.0 parts by weight of an acrylic processing aid, the thermoplastic elastomer resin composition being obtained by melt-kneading and crosslinking the components (a), (b), (c), (d), and (e) in the presence of an organic peroxide. Patent Document 3 discloses a thermoplastic elastomer composition containing (a) 100 parts by weight of a hydrogenated block copolymer (a-1) obtained by hydrogenating a block copolymer consisting of at least two polymer blocks A mainly composed of an aromatic vinyl compound and at least one polymer block B mainly composed of a conjugated diene compound and / or a hydrogenated product of a conjugated diene compound block copolymer (a-2), (b) 30 to 150 parts by weight of a non-aromatic rubber softener, and (c) 3 to 100 parts by weight of a thermoplastic resin having a melting point of 70 to 140°C and a melt viscosity at 140°C of 400 to 100,000 cps as measured by DSC. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Japanese Patent Application Publication No. 3-195752 [Patent Document 2] JP 2000-034389 A [Patent Document 3] JP 2003-192868 A Summary of the Invention [Problem to be solved by the invention]
[0005] Silicone-based rubber and urethane-based rubber are used as materials for flexible rubber compositions, but these rubbers generally have low mechanical strength. Thermoplastic elastomer compositions also have low mechanical strength. On the other hand, olefin-based elastomers that can be injection molded have been proposed as rubbers with high mechanical strength, but the olefin-based elastomers lack flexibility.
[0006] Therefore, one aspect of the present invention provides a rubber composition capable of forming a rubber molded article having an excellent balance between flexibility and mechanical strength. [Means for solving the problem]
[0007] One aspect of the present invention relates to a rubber composition containing (A) a rubber component, (B) a softener, and (C) a filler.
number
[0008] According to one aspect of the present invention, there is provided a rubber composition capable of forming a rubber molded article having an excellent balance between flexibility and mechanical strength. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] Hereinafter, several embodiments of the present invention will be described in detail. However, the present invention is not limited to the following embodiments.
[0010] A rubber composition according to one embodiment contains at least (A) a rubber component, (B) a softener, and (C) a filler.
[0011] (A) Rubber component The rubber component includes one or more kinds of rubber, and may be one kind of rubber or a mixture of two or more kinds of rubber. Examples of the rubber include ethylene-propylene-diene copolymer rubber (EPDM), styrene-butadiene copolymer rubber (SBR), natural rubber (NR), polyisoprene rubber (IR), polybutadiene rubber (BR), chloroprene rubber (CR), acrylonitrile-butadiene copolymer rubber (NBR), isoprene-isobutylene copolymer rubber (IIR), and halogenated butyl rubber (HR). The rubber may be a rubber having a carbon-carbon double bond, and may be EPDM, SBR, NR, or CR.
[0012] The EPDM may have an ethylene unit content of 30% by mass or more, 50% by mass or more, or 60% by mass or more, and 85% by mass or less, 80% by mass or less, or 75% by mass or less, based on the mass of the EPDM. The EPDM may have a propylene unit content of 10% by mass or more, 15% by mass or more, or 20% by mass or more, and 40% by mass or less, 35% by mass or less, or 30% by mass or less, based on the mass of the EPDM. The EPDM may have a non-conjugated diene unit content of 1% by mass or more, 3% by mass or more, or 4% by mass or more, and 15% by mass or less, 10% by mass or less, or 8% by mass or less, based on the mass of the EPDM.
[0013] During the production of the rubber composition, the Mooney viscosity ML of the rubber component 1+4,100℃ From the viewpoint of providing a torque that facilitates kneading in a Banbury mixer, the Mooney viscosity ML of the rubber may be 20 or more, 40 or more, or 50 or more. 1+4,100℃ From the viewpoint of obtaining excellent affinity with the softener during kneading with a Banbury mixer, the Mooney viscosity ML of the rubber component may be 100 or less, 80 or less, or 70 or less. 1+4,100℃ The Mooney viscosity ML of the rubber component may be 20 to 100. 1+4,100℃ In the case where the rubber component is extended by an extender oil during the production of the rubber composition, the above range may be used when the rubber component is extended by the extender oil. In the case where the rubber component is not extended by an extender oil during the production of the rubber composition, the above range may be used when the rubber component is not extended by the extender oil.
[0014] The content of the rubber component may be 5 mass% or more, 8 mass% or more, or 10 mass% or more, and may be 90 mass% or less, 88 mass% or less, or 85 mass% or less, based on the total mass of the rubber composition. The content of the rubber component may be 5 to 90 mass% based on the total mass of the rubber composition.
[0015] (B) Softener The softener can be selected from those that are commonly used as softeners in rubber compositions. Examples of the softener include mineral oil-based softeners and vegetable oil-based softeners. Examples of the mineral oil-based softener include process oils such as paraffin oil, naphthene oil, and aromatic oil; low molecular weight polymers such as terpene resin, petroleum resin, coumarone-indene resin, atactic polypropylene, ethylene-propylene random copolymer, liquid diene (co)polymer, modified liquid diene (co)polymer, and liquid thiokol; plasticizers such as dioctyl phthalate, dioctyl adipate, and dioctyl sebacate; waxes such as paraffin wax, microcrystalline wax, petrolatum, and polyolefin wax; and liquid paraffin, petroleum asphalt, petrolatum, and coal tar pitch. Examples of vegetable oil-based softeners include fatty oils such as castor oil, linseed oil, rapeseed oil, soybean oil, coconut oil, and tall oil; waxes such as beeswax, carnauba wax, and lanolin; unsaturated fatty acids such as oleic acid, linoleic acid, and ricinoleic acid or metal salts thereof; naphthenic acid or metal soaps thereof; pine oil, rosin or derivatives thereof, terpene (terpenoid), and factice (sub). These may be used alone or in combination of two or more. In addition, these softeners may be added in advance as extender oils in the rubber manufacturing process to improve the processability of the rubber.
[0016] The kinetic viscosity of the softener at 40°C is set to 50mm from the viewpoint of suppressing exudation from the rubber composition and the rubber molded product obtained by crosslinking the rubber composition. 2 / s or more, 55mm 2 / s or more, or 60 mm 2 The kinetic viscosity of the softener at 40° C. may be 100,000 mm / s or more from the viewpoint of facilitating workability during kneading. 2 / s or less, 80000mm 2 / s or less, or 60000mm 2 The kinetic viscosity of the softener at 40°C may be 50 to 100,000 mm 2 When the rubber composition contains two or more softeners, the kinematic viscosity of a mixture thereof may be within the above range.
[0017] The density of the softener is set to 0.80 g / cm3 in order to obtain excellent vibration-damping properties in rubber molded products. 3 More than 0.81g / cm 3 or more than 0.82 g / cm 3 The density of the softener may be 1.20 g / cm or more from the viewpoint of reducing the weight of the rubber molded product. 3 Below, 1.18g / cm 3 or less than 1.15g / cm 3 From these viewpoints, the density of the softener may be 0.80 to 1.20 g / cm 3 When the rubber composition contains two or more softeners, the density of a mixture thereof may be within the above range.
[0018] The content of the softener may be 20 parts by mass or more, 50 parts by mass or more, 100 parts by mass or more, or 150 parts by mass or more, and may be 600 parts by mass or less, 500 parts by mass or less, 400 parts by mass or less, or 300 parts by mass or less, based on 100 parts by mass of the (A) rubber component. The content of the softener may be 20 to 600 parts by mass, based on 100 parts by mass of the (A) rubber component.
[0019] (C) Filler The filler may be an inorganic filler, an organic filler, or a combination thereof. The filler may be a filler with excellent reinforcing properties. Examples of inorganic fillers include silica, carbon black, glass, silicate minerals, alumina, silicon dioxide, titanium oxide, iron oxide, aluminum oxide, antimony oxide, barium ferrite, strontium ferrite, and beryllium oxide. Examples of organic fillers include polyester, aromatic polyamide, cellulose, and vinylon. The filler may include silica, carbon black, or both. These may be used alone or in combination of two or more.
[0020] The average primary particle diameter of the filler may be 5 nm or more, 7 nm or more, 9 nm or more, or 10 nm or more, from the viewpoint of obtaining excellent compression set in the rubber molded article. The average primary particle diameter of the filler may be 500 nm or less, 450 nm or less, 400 nm or less, or 350 nm or less, from the viewpoint of obtaining excellent mechanical strength in the rubber molded article. The average primary particle diameter of the filler may be 5 to 500 nm.
[0021] The primary particle diameter of the filler means the diameter of the smallest circle circumscribing each primary particle when the primary particle of the filler is observed in a plan view. The average primary particle diameter of the filler is calculated by, for example, observing 100 primary particles using a transmission electron microscope H-7100 manufactured by Hitachi, Ltd., measuring the primary particle diameters of the 100 primary particles, and averaging the measurements.
[0022] In the rubber composition according to one embodiment, X calculated by the following formula (1) is 3.0 × 10 8 ~5.2×10 8 In the formula (1), Y is the rubber composition 1m 3 Number of fillers per unit (pcs / m 3 ), and Z represents the average primary particle size (nm) of the filler. The parameter X is a value that reflects the volume ratio of the filler in the rubber composition. From the viewpoint of the filler exhibiting sufficient mechanical strength in a crosslinked molded product, the parameter X is set to 3.5×10 8 That's it, 3.8 x 10 8 or more than 4.0 x 10 8 From the viewpoint of the filler exhibiting sufficient flexibility in the crosslinked molded product, the parameter X may be 5.0×10 8 Below, 4.7 x 10 8 or less, or 4.5 x 10 8 It may be the following.
number
[0023] Rubber composition 1m 3 The number of fillers per unit (Y) is calculated using the following formula: Y = R / (4 / 3×π×(Z / 2×10 -9 ) 3 ) In the formula, Y is the rubber composition 1m 3 Number of fillers per unit (pcs / m 3 ), R represents the volume fraction of the filler in the entire rubber composition, and Z represents the average primary particle diameter (nm) of the filler.
[0024] The amount of the filler may be 1 part by mass or more, 10 parts by mass or more, 20 parts by mass or more, or 30 parts by mass or more based on 100 parts by mass of the (A) rubber component. The amount of the filler may be 210 parts by mass or less, 150 parts by mass or less, 100 parts by mass or less, or 50 parts by mass or less based on 100 parts by mass of the (A) rubber component. The amount of the filler may be 1 to 210 parts by mass based on 100 parts by mass of the (A) rubber component.
[0025] (A) Based on 100 parts by mass of the rubber component, (B) the content of the softener is W B (C) The filler content is W c When the ratio W C / W B From the viewpoint of exhibiting sufficient mechanical strength in a rubber molded article, the ratio W may be 0.05 or more, 0.08 or more, or 0.10 or more. C / W B From the viewpoint of exhibiting sufficient flexibility in the crosslinked molded article, the ratio W may be 0.35 or less, 0.30 or less, or 0.25 or less. C / W B may be 0.05 to 0.35.
[0026] (D) Coupling Agent The rubber composition may further contain a coupling agent (D) in order to improve the dispersibility of the filler in the rubber or to form a chemical bond with the filler directly with the rubber molecules or via various additives such as a crosslinking agent described later. Examples of the coupling agent include a silane coupling agent, a carbon coupling agent, a titanium coupling agent, and a phosphate coupling agent. The coupling agent may be a silane coupling agent. The content of the coupling agent in the rubber composition may be 0.1 to 10 parts by mass, or 0.1 to 5 parts by mass, based on 100 parts by mass of the (A) rubber component.
[0027] Specific examples of coupling agents include bis(3-triethoxysilylpropyl)tetrasulfide (e.g., trade name "Si-69" manufactured by EVONIK), bis(3-triethoxysilylpropyl)disulfide (e.g., trade name "Si-75" manufactured by EVONIK), bis(3-diethoxymethylsilylpropyl)tetrasulfide, bis(3-diethoxymethylsilylpropyl)disulfide, 3-octanoylthiopropyltriethoxysilane (also known as "octanethioic acid S-[3-(triethoxysilyl)propyl]ester", e.g., trade name "NXT Silane"), Octanethioic acid S-[3-{(2-methyl-1,3-propanedialkoxy)ethoxysilyl}propyl] ester, Octanethioic acid S-[3-{(2-methyl-1,3-propanedialkoxy)methylsilyl}propyl] ester, Methyltrimethoxysilane, Methyltriethoxysilane, Methyltriacetoxysilane, Methyltributoxysilane, Ethyltrimethoxysilane, Ethyltriethoxysilane, Isobutyltrimethoxysilane, Isobutyltriethoxysilane, N-Octyltrimethoxysilane, N-Octyltriethoxysilane, Vinyltrimethoxysilane, Vinyltriethoxysilane, Vinyltris(methoxyethoxy)silane, Phenyltrimethoxysilane, Phenyltriethoxysilane , phenyltriacetoxysilane, 3-methacryloxypropyltrimethoxysilane, 3-methacryloxypropyltriethoxysilane, 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, N-(2-aminoethyl)-3-aminopropyltrimethoxysilane, N-(2-aminoethyl)-3-aminopropyltriethoxysilane, (3-glycidoxypropyl)trimethoxysilane, (3-glycidoxypropyl)triethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltriethoxysilane, 3-isocyanatopropyltrimethoxysilane, and 3-isocyanatopropyltriethoxysilane. These may be used alone or in combination of two or more.
[0028] Examples of carbon coupling agents include S-(3-aminopropyl)thiosulfuric acid (e.g., trade name "Sumilink 100" manufactured by Sumitomo Chemical Co., Ltd.), sodium (2Z)-4-[(4-aminophenyl)amino]-4-oxo-2-butenoate (e.g., trade name "Sumilink 200" manufactured by Sumitomo Chemical Co., Ltd.), N'-(1,3-dimethylbutylidene)-3-hydroxy-2-naphthoic acid hydrazide, and isophthalic acid dihydrazide. These may be used alone or in combination of two or more kinds.
[0029] (E) Crosslinking agent The rubber composition may further include a crosslinking agent (E) for crosslinking the rubber. The crosslinking agent may include, for example, an organic peroxide, sulfur, a sulfur compound, a resin crosslinking agent, an oxime compound, a nitroso compound, a polyamine compound, an alkylphenol-formaldehyde condensate, or a combination of two or more selected from these. The content of the crosslinking agent in the rubber composition may be 0.1 to 10 parts by mass, or 0.1 to 5 parts by mass, based on 100 parts by mass of the (A) rubber component.
[0030] Examples of organic peroxides include ketone peroxides, diacyl peroxides, hydroperoxides, dialkyl peroxides, peroxyketals, alkyl peresters, percarbonates, peroxydicarbonates, and peroxyesters.
[0031] Specific examples of organic peroxides include dicumyl peroxide, 2,5-dimethyl-2,5-di(t-butylperoxy)hexane, 2,5-dimethyl-2,5-di(t-butylperoxy)hexyne, 1,3-bis(t-butylperoxyisopropyl)benzene, t-butylcumyl peroxide, di-t-butyl peroxide, 2,2,4-trimethylpentyl-2-hydroperoxide, diisopropylbenzohydroperoxide, cumene peroxide, t-butyl peroxide, 1,1-di(t-butylperoxy)3,5,5-trimethylcyclohexane, 1,1-di-t-butylperoxycyclohexane, isobutyl peroxide, 2,4-dichlorobenzoyl peroxide, o-methylbenzoyl peroxide, bis-3,5,5-trimethylhexanoyl peroxide, lauroyl peroxide, benzoyl peroxide, and p-chlorobenzoyl peroxide. These may be used alone or in combination of two or more. The content of the organic peroxide in the rubber composition may be 0.01 to 10 parts by mass, or 0.1 to 5 parts by mass, based on 100 parts by mass of the (A) rubber component.
[0032] Specific examples of sulfur and sulfur-based compounds include powdered sulfur, precipitated sulfur, colloidal sulfur, surface-treated sulfur, and insoluble sulfur. These may be used alone or in combination of two or more. The content of sulfur and sulfur-based compounds in the rubber composition may be 0.01 to 10 parts by mass, or 0.1 to 5 parts by mass, based on 100 parts by mass of the (A) rubber component.
[0033] Specific examples of the resin crosslinking agent include the Tackirol series manufactured by Taoka Chemical Co., Ltd. The content of the resin crosslinking agent in the rubber composition may be 0.01 to 10 parts by mass, or 0.1 to 5 parts by mass, based on 100 parts by mass of the (A) rubber component.
[0034] (F) Crosslinking promoter The rubber composition may further contain (F) a crosslinking accelerator. Examples of the crosslinking accelerator include zinc oxide (zinc oxide), magnesium oxide, saturated fatty acids such as palmitic acid and stearic acid, saturated fatty acid metal salts such as zinc laurate, zinc stearate, barium stearate and calcium stearate, saturated fatty acid esters, and glycols such as ethylene glycol and polyethylene glycol. These may be used alone or in combination. The content of the crosslinking accelerator in the rubber composition may be 0.1 to 20 parts by mass, or 0.2 to 10 parts by mass, based on 100 parts by mass of the (A) rubber component.
[0035] (G) Crosslinking aid The rubber composition may further include a crosslinking aid (G). The crosslinking aid may be a vulcanization accelerator that accelerates sulfur crosslinking, a peroxide crosslinking accelerator that accelerates peroxide crosslinking, etc. The content of the crosslinking aid in the rubber composition may be 0.05 to 20 parts by mass, or 0.1 to 10 parts by mass, based on 100 parts by mass of the rubber component (A).
[0036] Specific examples of vulcanization accelerators include tetramethylthiuram monosulfide, tetramethylthiuram disulfide, tetraethylthiuram disulfide, tetrabutylthiuram disulfide, dipentamethylenethiuram monosulfide, dipentamethylenethiuram disulfide, dipentamethylenethiuram tetrasulfide, N,N'-dimethyl-N,N'-diphenylthiuram disulfide, N,N'-dioctadecyl-N,N'-diisopropylthiuram disulfide, N-cyclohexyl-2-benzothiazole sulfenamide, N-oxydiethylene-2-benzothiazole sulfenamide, N,N-diisopropyl-2-benzothiazole sulfenamide, 2-mercaptobenzothiazole, 2-(2,4-dinitrophenyl)mercaptobenzothiazole, 2-(2,6-diethyl-4-morpholinothio)benzol, Examples of the thiocarbamate include zothiazole, dibenzothiazyl disulfide, diphenyl guanidine, triphenyl guanidine, di-orthotolyl guanidine, orthotolyl-bi-guanide, diphenyl guanidine-phthalate, n-butylaldehyde aniline, hexamethylenetetramine, acetaldehyde ammonia, 2-mercaptoimidazoline, thiocarbanilide, diethylthiourea, dibutylthiourea, trimethylthiourea, di-orthotolylthiourea, zinc dimethyldithiocarbamate, zinc diethylthiocarbamate, zinc di-n-butyldithiocarbamate, zinc ethylphenyldithiocarbamate, zinc butylphenyldithiocarbamate, sodium dimethyldithiocarbamate, selenium dimethyldithiocarbamate, tellurium diethyldithiocarbamate, zinc dibutylxanthogenate, and ethylenethiourea. These may be used alone or in combination of two or more.
[0037] Specific examples of peroxide crosslinking accelerators include triallyl isocyanurate, N,N'-m-phenylene bismaleimide, methacrylic acid, methyl methacrylate, ethyl methacrylate, propyl methacrylate, isopropyl methacrylate, n-butyl methacrylate, i-butyl methacrylate, sec-butyl methacrylate, t-butyl methacrylate, 2-ethylhexyl methacrylate, cyclohexyl methacrylate, isodecyl methacrylate, lauryl methacrylate, tridecyl methacrylate, stearyl methacrylate, 2-hydroxyethyl methacrylate, hydroxypropyl methacrylate, polyethylene glycol monomethacrylate, polypropylene glycol monomethacrylate, 2-ethoxyethyl methacrylate, tetrahydrofurfuryl methacrylate, allyl methacrylate, glycidyl methacrylate, benzyl methacrylate, dimethylaminoethyl methacrylate, diethyl methacrylate, ... Aminoethyl methacrylate, methacryloxyethyl phosphate, 1,4-butanediol diacrylate, ethylene glycol dimethacrylate, 1,3-butylene glycol dimethacrylate, neopentyl glycol dimethacrylate, 1,6-hexanediol dimethacrylate, diethylene glycol dimethacrylate, triethylene glycol dimethacrylate, polyethylene glycol dimethacrylate, dipropylene glycol dimethacrylate, polypropylene glycol dimethacrylate, trimethylolethane trimethacrylate, trimethylolpropane trimethacrylate, allyl glycidyl ether, N-methylol methacrylamide, 2,2-bis(4-methacryloxypolyethoxyphenyl)propane, aluminum methacrylate, zinc methacrylate, calcium methacrylate, magnesium methacrylate, and 3-chloro-2-hydroxypropyl methacrylate. These may be used alone or in combination of two or more.
[0038] The rubber composition according to one embodiment has an excellent balance between flexibility and mechanical strength. Specifically, the rubber composition according to one embodiment has a breaking strength (tensile strength, TB) of 6 MPa or more and a hardness (Duro-A) of 30 or less, and has an excellent balance between flexibility and mechanical strength.
[0039] The rubber composition according to one embodiment can be molded and crosslinked (or vulcanized) to form various molded rubber products. The molded rubber products can be, for example, industrial parts such as seals, packings, and O-rings. EXAMPLES
[0040] The present invention will be described in detail below with reference to examples, although the present invention is not limited to the following examples.
[0041] [material] In the examples and comparative examples, the materials shown below were used. (A) Rubber component A-1: EPDM, Sumitomo Chemical Co., Ltd. "Esprene EPDM 600F", Mooney viscosity ML 1+4,100℃ = 63, rubber component / extending oil = 100 / 100 (mass ratio), ethylene unit content = 66 mass%, propylene unit content = 30 mass%, non-conjugated diene unit content = 4.0 mass% A-2: EPDM, Sumitomo Chemical Co., Ltd. "Esprene EPDM 6101", Mooney viscosity ML 1+4,125℃ = 52, rubber component / extending oil = 100 / 70 (mass ratio), ethylene unit content = 70 mass%, propylene unit content = 23.5 mass%, non-conjugated diene unit content = 6.5 mass% A-3: Styrene butadiene rubber (SBR), "SE-6233" manufactured by ZS Elastomers Co., Ltd., rubber component / extending oil = 100 / 37.5 (mass ratio) A-4: Hydrogenated styrene-based thermoplastic elastomer (SEBS), Asahi Kasei Corporation "Tuftec H1221", MFR 230℃,2.16kg = 4.5, styrene / ethylene-butylene ratio = 12 / 88 (mass ratio) (B) Softener B-1: Paraffin-based process oil, Idemitsu Kosan Co., Ltd. "Diana Process Oil PW-380", density (15°C) = 0.887g / cm 3 , kinematic viscosity (40℃)=438.1mm 2 / s B-2: Synthetic oil, ethylene-propylene random copolymer, Mitsui Chemicals "Lucant HC-3000X", kinematic viscosity (40℃) = 50000mm 2 / s, kinematic viscosity (100℃)=2880mm 2 / s, weight average molecular weight 15000 B-3: Sulfur chloride factice, "White Sub 1" manufactured by Tenma Sub Chemical Co., Ltd. (acetone extract 2-5%) B-4: Aromatic process oil, H&R "VivaTec500", density (15°C) = 0.950g / cm 3 , kinematic viscosity (40℃)=410.0mm 2 / s B-5. Polyolefin wax: Clariant Japan "Ricosene PP1302", ethylene-propylene copolymer, viscosity at 170°C 200 mPa s, softening point 90°C, density (15°C) = 0.88 g / cm 3 (C) Filler C-1: Silica, "Nipsil VN3" manufactured by Tosoh Silica Corporation, average primary particle size 16 nm C-2: Silica, "Nipsil ER" manufactured by Tosoh Silica Corporation, average primary particle diameter 32 nm C-3: Silica, Tosoh Silica Corporation "Nipsil E-74P", average primary particle size 80 nm C-4: Silica, Evonik "7000GR", nitrogen adsorption specific surface area 165m 2 / g, average primary particle size 32nm (D) Coupling Agent D-1: Silane coupling agent, Evonik's "Dynasylan MTMO", 3-mercaptopropyltrimethoxysilane D-2: Silane coupling agent, Evonik "Si69", bis(3-triethoxysilylpropyl)tetrasulfide (E) Crosslinking agent E-1: Sulfur, Tsurumi Chemical Industry Co., Ltd. "Kinkajirushi Fine Sulfur 200 Mesh" E-2: Resin crosslinking agent, "Takkiroll 250-1" manufactured by Taoka Chemical Co., Ltd. E-3: Dicumyl peroxide, NOF Corp. "Percumyl D-40 MB" (F) Crosslinking promoter F-1: Zinc oxide, Seido Chemical Industry Co., Ltd. "Zinc oxide type 2" F-2: Stearic acid, "Stearic acid 50S" manufactured by New Japan Chemical Co., Ltd. F-3: Polyethylene glycol, Sanyo Chemical Industries "PEG-4000S" F-4: N-phenyl-N'-1,3-dimethylbutyl-p-phenylenediamine (Kawaguchi Chemical Industry Co., Ltd., "ANTAGE 6C" (G) Crosslinking aid G-1: Zinc dibutyldithiocarbamate (masterbatch), Rhenogran ZDBC-80 by Rhein Chemie Japan G-2: 2-Mercaptobenzothiazole (master batch), Rhenogran MBT-80 manufactured by Rhein Chemie Japan G-3: Tetramethylthiuram disulfide (masterbatch), Rhenogran TMTD-80 manufactured by Rhein Chemie Japan G-4: Dipentamethylene thiuram tetrasulfide (master batch), Rhenogran DPTT-70 manufactured by Rhein Chemie Japan G-5: N-cyclohexylbenzothiazole-2-sulfenamide vulcanization accelerator, "Soxinol CZ" manufactured by Sumitomo Chemical Co., Ltd. G-6: 1,3-diphenylguanidine, "Soxinol D" manufactured by Sumitomo Chemical Co., Ltd. G-7: Ethylene glycol dimethacrylate, "Acryester ED" manufactured by Mitsubishi Chemical Corporation
[0042] [Preparation of rubber composition] The components (A) to (D) and (G) shown in Tables 1 to 3 were kneaded in the amounts shown in Tables 1 to 3 using a Banbury mixer (manufactured by Kobe Steel, Ltd., 1700 mL) under conditions of a mixer temperature of 100°C and a rotor rotation speed of 80 rpm. After the torque peak appeared, the kneading temperature was kept at 150 to 155°C for another 4 minutes to obtain a kneaded product. Next, using a 10-inch open roll machine with a roll temperature set to 40°C, the kneaded product obtained and the components (E) and (F) shown in Tables 1 to 3 were kneaded in the amounts shown in Tables 1 to 3 to obtain a rubber composition. In Comparative Examples 7 and 8, the torque did not rise in the kneader, and the rubber component and the oil component were discharged in a separated state after 30 minutes of kneading, so kneading was not possible. The amount of each component shown in Tables 1 to 3 means the amount (unit: parts by mass) excluding the extender oil for component (A) (rubber), and means the amount (unit: parts by mass) based on 100 parts by mass of component (A) for components (B) to (G). "Parameter X" in Tables 1 to 3 means X calculated by the following formula (1). "W C / W B " is the mass-based content W of the softener (B) B (C) Filler mass content W C This means the ratio of
number
[0043] [Tensile test] The rubber composition was molded and vulcanized by hot pressing under the pressing conditions shown in Tables 1 to 3 to prepare a vulcanized rubber sheet having a thickness of 2 mm. In accordance with JIS K6251, a dumbbell-shaped No. 3 test piece was cut out from the prepared rubber sheet, and the tensile strength (100% modulus (M100), 300% modulus (M300), breaking strength (TB), and breaking elongation (EB)) of the rubber sheet was measured using a tensile tester (Ueshima Seisakusho Co., Ltd., QUICK READER P-57) under test conditions of an ambient temperature of 23°C and a tensile speed of 500 mm / min. The measurement results are shown in Tables 1 to 3.
[0044] [Hardness (Duro-A)] The rubber composition was molded and vulcanized by hot pressing under the pressing conditions shown in Tables 1 to 3 to prepare a vulcanized rubber sheet having a thickness of 2 mm. Dumbbell-shaped No. 3 test pieces were cut out from the prepared rubber sheet in accordance with JIS K6253. The hardness of the measurement sample was measured at an ambient temperature of 23°C using an automatic hardness tester (RH-105A, manufactured by Excel Co., Ltd.) equipped with a durometer type A. The measurement results are shown in Tables 1 to 3.
[0045] [Table 1]
[0046] [Table 2]
[0047] [Table 3]
Claims
1. A rubber composition comprising (A) a rubber component, (B) a softener, and (C) a filler, The following formula (1): [0010] The calculated X is 3.0 x 10 8 ~5.2 x 10 8 and In the formula, Y is the rubber composition 1m 3 The number of fillers per m 3 ) and Z represents the average primary particle diameter (nm) of the filler; Rubber composition.
2. (A) based on 100 parts by mass of the rubber component, (B) the content of the softener is W B (C) The content of the filler is W C When W B is 20 to 600 parts by mass, W C is 1 to 210 parts by mass, W C / W B The rubber composition according to claim 1, wherein the β-
3. 3. The rubber composition according to claim 1 or 2, wherein the filler (C) comprises silica, carbon black or both.
4. The rubber composition according to any one of claims 1 to 3, wherein the rubber component (A) contains a rubber having a carbon-carbon double bond.
5. The rubber composition further contains (D) a coupling agent and (E) a crosslinking agent, The content of the coupling agent (D) is 0.1 to 10 parts by mass based on 100 parts by mass of the rubber component (A), The rubber composition according to any one of claims 1 to 4, wherein the content of the crosslinking agent (E) is 0.1 to 10 parts by mass based on 100 parts by mass of the rubber component (A).
Citation Information
Patent Citations
Rubber composition and production thereof
JP1991195752A
Thermoplastic elastomer resin composition and its production
JP2000034389A
Thermoplastic elastomer composition, and molded product and composite molded product using the same