Decorative sheet
A non-chlorine-based decorative sheet with specific layer configurations addresses yield and assembly issues, offering improved scratch and impact resistance through a layered structure with ionizing radiation-curable resin and additives.
Patent Information
- Application Number
- JP2023083589
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-22
- Publication Date
- 2024-12-04
AI Technical Summary
Decorative sheets using melamine boards face issues with size regulations leading to poor yields and require labor-intensive assembly, lacking sufficient scratch and impact resistance.
A decorative sheet composed of non-chlorine-based resins with specific layer configurations, including a pattern layer, adhesive layers, and a transparent thermoplastic resin layer with a surface protection layer, featuring a total thickness range of 200-300 μm and containing ionizing radiation-curable resin, nucleating agents, and inorganic fillers.
The solution provides enhanced scratch and impact resistance without using melamine boards, ensuring flexibility and mechanical strength while maintaining processability.
Smart Images

Figure 2024167491000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a decorative sheet. [Background technology]
[0002] Conventionally, decorative sheets used in areas requiring resistance to scratches and impacts were mainly polyvinyl chloride resin films with printed patterns. In recent years, in consideration of environmental issues, decorative sheets using non-chlorine resins that are less likely to generate harmful substances such as hydrogen chloride or dioxins when burned have been developed and are now widely used. As such decorative sheets using non-chlorine resins, those using melamine boards have been proposed (see Patent Document 1 below, etc.). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2014-188941 A Summary of the Invention [Problem to be solved by the invention]
[0004] However, decorative sheets using melamine boards have certain regulations regarding the size of the melamine boards, which means that many parts of the melamine boards must be cut out, resulting in poor yields. Also, decorative sheets using melamine boards are difficult to work with because they must be attached one heavy sheet at a time during construction. For this reason, there is a demand in the market for decorative sheets that do not use melamine boards.
[0005] In view of the above, an object of the present invention is to provide a decorative sheet which is made of a non-chlorine-based resin and which exhibits sufficient scratch resistance and impact resistance without using a melamine plate. [Means for solving the problem]
[0006] In order to solve the above-mentioned problems, the decorative sheet according to the present invention is a decorative sheet in which a picture pattern layer, a first adhesive layer, a polyester-based resin layer, a second adhesive layer, a transparent thermoplastic resin layer, and a surface protective layer are laminated in this order on a base sheet made of a thermoplastic resin, the sum of the thickness of the polyester-based resin layer and the thickness of the transparent thermoplastic resin layer being in the range of 200 μm to 300 μm, and the polyester-based resin layer has a Martens hardness of 40 N / mm 2 More than 190N / mm 2 The surface protective layer is characterized in that it contains an ionizing radiation curable resin.
[0007] Furthermore, the decorative sheet of the present invention is preferably the decorative sheet described above, wherein the transparent thermoplastic resin layer is provided on the polyester-based resin layer side and comprises a first resin layer formed containing a first resin, and a second resin layer is provided on the first resin layer and formed containing a second resin different from the first resin, and the first resin is a transparent maleic acid-modified polypropylene resin, and the second resin is a transparent polypropylene resin.
[0008] Furthermore, the decorative sheet according to the present invention is preferably such that, in the decorative sheet described above, the thickness of the first resin layer is 10 μm or more and 20% or less of the total thickness of the transparent thermoplastic resin layer.
[0009] In the decorative sheet according to the present invention, it is preferable that the surface protective layer in the decorative sheet described above contains at least one of a nucleating agent and an inorganic filler. Effect of the Invention
[0010] The decorative sheet according to the present invention can exhibit sufficient scratch resistance and impact resistance by using a non-chlorine-based resin without using a melamine board. [Brief description of the drawings]
[0011] [Figure 1] 1 is a schematic cross-sectional view of a first embodiment of a decorative sheet according to the present invention. [Diagram 2] FIG. 2 is a schematic cross-sectional view of a second embodiment of a decorative sheet according to the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] The embodiments of the decorative sheet according to the present invention will be described with reference to the drawings. Note that the present invention is not limited to the following embodiments described with reference to the drawings, and the technical matters described in each embodiment can be appropriately combined and applied as necessary.
[0013] [First embodiment] A first embodiment of a decorative sheet according to the present invention will be described with reference to FIG.
[0014] <Composition of decorative sheet> The decorative sheet of this embodiment is an olefin-based decorative sheet or polyester-based decorative sheet that is bonded to substrates such as wood-based substrates, inorganic substrates, synthetic resin substrates, metal substrates, etc., and is particularly used in areas where scratch resistance and impact resistance are required.
[0015] As shown in Fig. 1, the decorative sheet 10 is formed by laminating, in this order, a picture pattern layer 12, a first adhesive layer 13, a polyester-based resin layer 14, a second adhesive layer 15, a transparent thermoplastic resin layer 16, and a surface protection layer 17 on a base sheet 11 made of a thermoplastic resin. An embossment 10a is formed on at least the transparent thermoplastic resin layer 16. The base sheet 11 having the above layers 12 to 17 laminated thereon is laminated on an undercoat layer 19.
[0016] <Base sheet 11> As the thermoplastic resin base sheet 11, various materials other than polyvinyl chloride resin can be used. For example, taking into consideration non-polluting properties, price, performance, ease of coloring, etc., polyolefin-based materials to which fillers and coloring pigments have been added are preferably used.
[0017] Resins applicable to the base sheet 11 include, for example, polyolefin-based resins such as polyethylene resin, polypropylene resin, polybutene resin, and polymethylpentene resin; polyolefin-based copolymer resins such as ethylene-vinyl acetate copolymer or its saponification product, and ethylene-(meth)acrylic acid (ester) copolymer; polyethylene terephthalate resin, polybutylene terephthalate resin, polyethylene naphthalate resin, polyarylate resin, polycarbonate resin, and copolymer polyester resin (typically, 1,4-cyclohexanedimethanol copolymerized polyethylene terephthalate resin, commonly known as PE). Examples of the resin that can be used include polyester resins such as polymethyl methacrylate (T-G), acrylic resins such as polymethyl methacrylate, polyamide resins such as nylon 6, nylon 6,6, nylon 6,10, and nylon 12, styrene resins such as polystyrene, AS resin, and ABS resin, cellulose resins such as cellulose acetate and nitrocellulose, chlorine-containing resins such as polyvinyl chloride and polyvinylidene chloride, fluorine-containing resins such as polyvinyl fluoride, polyvinylidene fluoride, polytetrafluoroethylene, and ethylene-tetrafluoroethylene copolymers, and copolymers or mixtures of two or more of these resins.
[0018] The base sheet 11 can also be prepared by adding color pigments, fillers, stabilizers, etc. to the above-mentioned resin components, dispersing them uniformly, and forming the mixture into a sheet.
[0019] <Pattern layer 12> A picture pattern layer 12 on which an arbitrary picture pattern is printed is provided on the surface of the base sheet 11. The type of picture pattern of the picture pattern layer 12 is not particularly limited, and may be, for example, a wood grain pattern, a stone pattern, a cloth pattern, a sand pattern, an abstract pattern, a geometric figure, letters or symbols, or a combination thereof. The type of printing ink used to form the picture pattern layer 12 is not particularly limited, and any known printing ink used in forming decorative sheets may be used.
[0020] Specifically, for example, a printing ink can be applied which is prepared by adding an organic or inorganic dye or pigment, and if necessary, an extender pigment, a filler, a tackifier, a dispersant, an antifoaming agent, a stabilizer or other additives to a binder resin such as a polyvinyl chloride resin, a vinyl chloride-vinyl acetate copolymer resin, a butyral, an acrylic, a urethane, a polyester, an epoxy, an alkyd, or a polyamide, and then adjusting the viscosity to the desired level with a suitable diluting solvent.
[0021] Examples of the printing method for the picture pattern layer 12 include gravure printing, inkjet printing, flexographic printing, screen printing, etc. As the printing ink, a printing ink suitable for each printing method can be used.
[0022] <First adhesive layer 13> A first adhesive layer 13 is provided on the picture pattern layer 12. The first adhesive layer 13 can be provided by, for example, applying a composition for forming the first adhesive layer 13 onto the picture pattern layer 12. The adhesive contained in the first adhesive layer 13 can be arbitrarily selected from, for example, urethane-based, acrylic-based, polyester-based, etc., depending on the combination with the transparent thermoplastic resin contained in the transparent thermoplastic resin layer 16.
[0023] <Polyester-based resin layer 14> For example, polyethylene terephthalate, polybutylene terephthalate, polycyclohexylene dimethylene terephthalate, polyethylene naphthalate, polylactic acid, etc. are used for the polyester-based resin layer 14. In particular, polyethylene terephthalate and polybutylene terephthalate are preferably used. In addition, in order to improve adhesion, it is also possible to appropriately perform corona treatment, etc.
[0024] The polyester-based resin layer 14 is preferably a layer that has been subjected to a biaxial stretching treatment. The thickness of the polyester-based resin layer 14 is preferably within a range of 100 μm to 200 μm. When the thickness of the polyester-based resin layer 14 is within the above range, cutting workability can be improved with respect to cutting using a circular saw or a hand router.
[0025] The polyester resin layer 14 has a Martens hardness (HM) of 40 N / mm 2 More than 190N / mm 2 The Martens hardness (MH) of the polyester resin layer 14 is 40 N / mm 2 If it is less than 190N / mm 2 If the hardness exceeds this value, the material will be prone to cracking, and sufficient scratch resistance and impact resistance will not be obtained. The Martens hardness (MH) is determined in accordance with the international standard "ISO 14577".
[0026] <Second adhesive layer 15> A second adhesive layer 15 is provided on the polyester-based resin layer 14. The second adhesive layer 15 can also be provided by, for example, applying a composition for forming the second adhesive layer 15 onto the polyester-based resin layer 14. The adhesive contained in the second adhesive layer 15 can be arbitrarily selected from, for example, urethane-based, acrylic-based, polyester-based, etc., depending on the combination of transparent thermoplastic resins contained in the transparent thermoplastic resin layer 16.
[0027] <Transparent thermoplastic resin layer 16> The transparent thermoplastic resin layer 16 is a layer on which the embossment 10a is formed, and is, for example, a sheet-like layer consisting of multiple layers. Each layer forming the transparent thermoplastic resin layer 16 is made of, for example, a transparent thermoplastic resin so that the pattern of the picture pattern layer 12 can be seen through. The thermoplastic resin contained in the transparent thermoplastic resin layer 16 can be, for example, various transparent resins other than vinyl chloride resin. The resins of the layers forming the transparent thermoplastic resin layer 16 can be variously combined depending on the desired characteristics.
[0028] Examples of thermoplastic resins that can be used for the transparent thermoplastic resin layer 16 include polyolefin-based resins such as low-density polyethylene resin (LDPE), high-density polyethylene resin (HDPE), linear low-density polyethylene resin (LLDPE), polypropylene resin (PP), and polyolefin-based elastomers; polyester-based resins such as polyethylene terephthalate resin (PET), polybutylene terephthalate resin (PBT), and polyethylene naphthalate resin (PEN); polymethyl methacrylate resin (PMMA), ethylene-vinyl acetate copolymer resin (EVA), ionomer resin, polybutene resin, polyacrylonitrile resin, polyamide-based resins such as nylon-6 and nylon-66, polystyrene resin (PS), polyvinyl chloride resin (PVC), polyvinylidene chloride resin (PVDC), polycarbonate resin (PC), fluorine-based resin, and synthetic resins such as urethane-based resin.
[0029] In addition, when the picture pattern layer 12 has a wood grain, the embossments 10a may be formed to represent the vessels of natural wood by depressions, and even when the picture pattern layer 12 has a grain other than wood, the design can be enhanced by roughness of a sand grain or a geometric pattern. In this way, by forming the embossments 10a, a three-dimensional effect can be imparted to the surface of the decorative sheet 10, improving the design. Also, the embossments 10a can be formed not only in the transparent thermoplastic resin layer 16 but also in other layers.
[0030] The embossment 10a can be formed by a post-embossing method in which the layers are laminated together, the whole is heated, and an embossing roll is pressed against the laminate, or a simultaneous extrusion and embossing method in which the transparent thermoplastic resin layer 16 is extruded from a T-die and pressed against an embossing roll. In this way, the embossment 10a can be formed before or after the surface protective layer 17 is provided.
[0031] The thickness of the transparent thermoplastic resin layer 16 is preferably in the range of 50 μm to 150 μm, more preferably in the range of 100 μm to 120 μm. If the thickness of the transparent thermoplastic resin layer 16 is within the above range, there is no problem in forming the unevenness by the embossment 10a, and sufficient abrasion resistance can be obtained. In addition, in terms of design, the presence of the transparent thermoplastic resin layer 16 in combination with the picture pattern layer 12 can produce an effect of making the user feel greater depth and profundity.
[0032] That is, if the thickness of the transparent thermoplastic resin layer 16 is less than 50 μm, there is a risk that sufficient abrasion resistance, etc. cannot be obtained, and if the thickness of the transparent thermoplastic resin layer 16 exceeds 150 μm, productivity during manufacturing is likely to decrease, which may be disadvantageous in terms of cost.
[0033] In addition, the total thickness of the polyester-based resin layer 14 and the transparent thermoplastic resin layer 16 is preferably within a range of 200 μm to 300 μm. When the total thickness of the polyester-based resin layer 14 and the transparent thermoplastic resin layer 16 is within the above range, sufficient scratch resistance and impact resistance can be obtained. Furthermore, the decorative sheet 10 does not lose both its flexibility and mechanical strength, and does not interfere with the processability into a decorative board such as in-line roll lamination, or the processability as a decorative board, thereby improving usability.
[0034] The transparent thermoplastic resin layer 16 may contain various additives such as an ultraviolet absorbing agent, a light stabilizer, etc. Examples of the ultraviolet absorbing agent include benzotriazole-based, triazine-based, and benzophenone-based agents.
[0035] As the benzotriazole system, for example, 2-(2-hydroxy-5-t-butylphenyl)-2H-benzotriazole, 2-(5-methyl-2-hydroxyphenyl)benzotriazole, 2-[2-hydroxy-3,5-bis(α,α-dimethylbenzyl)phenyl]-2H-benzotriazole, 2-(3,5-di-t-butyl-2-hydroxyphenyl)benzotriazole, 2-(3-t-butyl-5-methyl-2-hydroxyphenyl)-5-chlorobenzotriazole, 2-(3,5-di-t-butyl-2-hydroxyphenyl)-5-chlorobenzotriazole, 2-(3,5-di-t-amyl-2-hydroxyphenyl)benzotriazole, 2-(2'-hydroxy-5'-t-octylphenyl)benzotriazole, and the like, and mixtures, modified products, polymers, derivatives, and the like thereof can be applied.
[0036] Examples of triazines include 2-(4,6-diphenyl-1,3,5-triazine-2-yl)-5-[(hexyl)oxy]-phenol, 2-[4-[(2-hydroxy-3-dodecyloxypropyl)oxy]-2-hydroxyphenyl]-4,6-bis(2,4-dimethylphenyl)-1,3,5-triazine, 2-[4-[(2-hydroxy-3-tridecyloxypropyl)oxy]-2-hydroxyphenyl]-4,6-bis(2,4-dimethylphenyl)-1,3,5-triazine, 2,4-bis(2,4-dimethylphenyl)-6-(2-hydroxy-4-iso-octyloxyphenyl)-s-triazine, and mixtures, modified products, polymers, and derivatives thereof can be used.
[0037] As the benzophenone-based agent, for example, octabenzone, modified products, polymers, derivatives, etc. can be applied. Here, the ultraviolet absorbent having a hydroxyl group is particularly effective because it can be bonded to the resin component by crosslinking accompanying the addition of isocyanate. The amount of the added part can be appropriately set according to the desired weather resistance, but is preferably within the range of 0.1% to 50% and more preferably within the range of 1% to 30% of the resin solid content.
[0038] Examples of light stabilizers include bis(1,2,2,6,6-pentamethyl-4-piperidyl)[[3,5-bis(1,1-dimethylethyl)-4-hydroxyphenyl]methyl]butyl malonate, bis(1,2,2,6,6-pentamethyl-4-piperidinyl)sebacate, methyl(1,2,2,6,6-pentamethyl-4-poperidinyl)sebacate, decanedioic acid bis(2,2,6,6-tetramethyl-1(octyloxy)-4-piperidinyl)ester, and mixtures, modified products, polymers, and derivatives thereof. The number of parts added can be appropriately set according to the desired weather resistance, but is preferably in the range of 0.1% to 50% and more preferably in the range of 1% to 30% of the resin solid content.
[0039] Examples of other additives include heat stabilizers, flame retardants, and antiblocking agents. Examples of heat stabilizers include pentaerythrityl-tetrakis[3-(3,5-di-t-butyl-4-hydroxyphenyl)]-propionate, 2,4-bis-(n-octylthio)-6-(4-hydroxy-3,5-di-t-butylanilino)-1,3,5-triazine, octadecyl-3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate, 1,3,5-trimethyl-2,4,6-tris(3,5-t-butyl-4-hydroxybenzyl)benzene, 1,3,5- Examples of antioxidants that can be used include hindered phenol-based antioxidants such as tris(4-t-butyl-3-hydroxy-2,6-dimethylbenzyl)isocyanuric acid, phenol-based antioxidants such as 2,2'-methylenebis(4-ethyl-6-t-butylphenol) and 2,2'-methylenebis(4-methyl-6-t-butylphenol), and phosphorus-based antioxidants such as tris(2,4-di-t-butylphenyl)phosphite, and mixtures of these, that is, a combination of one or more of these, can be used.
[0040] Examples of the flame retardant that can be used include inorganic compounds such as aluminum hydroxide, magnesium hydroxide, calcium carbonate, magnesium carbonate, and phosphate flame retardants, etc. Examples of the anti-blocking agent that can be used include inorganic compounds such as aluminum silicate, silicon oxide, hydrotalcite, calcium carbonate, and organic compounds such as fatty acid amides, etc.
[0041] <Surface protective layer 17> The surface protective layer 17 is located on the outermost surface of the decorative sheet 10, and serves to protect the decorative sheet 10 from direct external forces, such as collisions with objects or rubbing during movement. In other words, the surface protective layer 17 improves the surface properties of the decorative sheet 10, imparting scratch resistance, impact resistance, stain resistance, slipperiness, etc. to the surface of the decorative sheet 10, and also affects the gloss, feel, etc.
[0042] The surface protective layer 17 contains an ionizing radiation curable resin such as an ultraviolet curable resin. Specifically, the material of the surface protective layer 17 is preferably, for example, a mixture (blend resin) of a thermosetting resin and an ultraviolet curable resin (UV curable resin). In this way, the surface protective layer 17 contains a thermosetting resin and an ultraviolet curable resin, i.e., a resin with high hardness, and by being exposed to the surface, the scratch resistance of the decorative sheet 10 can be improved.
[0043] As the thermosetting resin, it is preferable to use a thermosetting resin having a urethane bond, such as a two-component curing urethane resin, in consideration of the deformation conformability and scratch resistance of the decorative sheet 10. As the two-component curing urethane resin, for example, a urethane resin mainly composed of polyol and using isocyanate as a crosslinking agent (curing agent) can be used. In addition, examples of the solvent include ethyl acetate and n-butyl acetate.
[0044] The polyol has two or more hydroxyl groups in the molecule, and examples of the polyol that can be used include polyethylene glycol, polypropylene glycol, acrylic polyol, polyester polyol, polyether polyol, polycarbonate polyol, and polyurethane polyol.
[0045] As the isocyanate, polyvalent isocyanates having two or more isocyanate groups in the molecule can be used. As the polyvalent isocyanate, for example, aromatic isocyanates such as 2,4-tolylene diisocyanate, xylylene diisocyanate, 4,4'-diphenylmethane diisocyanate, or aliphatic (or alicyclic) isocyanates such as 1,6-hexamethylene diisocyanate, isophorone diisocyanate, hydrogenated tolylene diisocyanate, hydrogenated diphenylmethane diisocyanate, can be used. In addition, adducts or multimers of the above various isocyanates can also be used. For example, adducts of tolylene diisocyanate, tolylene diisocyanate trimer, etc. can be mentioned. Among the above isocyanates, aliphatic (or alicyclic) isocyanates are preferable because they are good in weather resistance and heat yellowing resistance, and for example, 1,6-hexamethylene diisocyanate, etc. can be mentioned.
[0046] Examples of the ultraviolet-curable resin that can be used include (meth)acrylic resins, silicone resins, polyester resins, urethane resins, amide resins, and epoxy resins.
[0047] The surface protective layer 17 is preferably formed by adding a dispersant or the like as a nano-sized additive (hereinafter also referred to as "dispersant nano specification"). The surface protective layer 17 may also be one to which a weathering agent has been added. The surface protective layer 17 preferably contains the above-mentioned resin material and a nucleating agent that improves the crystallinity of the resin material, and has an uneven surface. The nucleating agent is preferably added to the resin material in the form of a nucleating agent vesicle that is encapsulated in an outer membrane and turned into a vesicle.
[0048] The surface protective layer 17 preferably contains a nucleating agent as a nano-sized additive. The nano-sized nucleating agent is preferably used by being added to the above-mentioned resin material in the form of a nucleating agent vesicle, which is encapsulated in a vesicle having a single-layer outer membrane. The nucleating agent in the resin material constituting the surface protective layer 17 may also be encapsulated in a vesicle with a part of the nucleating agent exposed. By including a nucleating agent, the surface protective layer 17 can improve the crystallization degree and improve the scratch resistance of the decorative sheet 10.
[0049] The nano-sized nucleating agent preferably has an average particle size of 1 / 2 or less of the wavelength range of visible light. Specifically, since the wavelength range of visible light is 400 nm or more and 750 nm or less, the average particle size is preferably 375 nm or less.
[0050] Nano-sized nucleating agents have extremely small particle sizes, so the number of nucleating agents present per unit volume and their surface area increase inversely proportional to the cube of the particle diameter. As a result, the distance between each nucleating agent particle becomes closer, so that when crystal growth occurs from the surface of one nucleating agent particle added to the resin, the end of the growing crystal immediately comes into contact with the end of the crystal growing from the surface of another nucleating agent particle adjacent to the one nucleating agent particle, and the ends of the crystals hinder each other's growth, stopping the growth of each crystal.
[0051] Therefore, the average particle size of the spherulites in the crystalline portion of the crystalline resin can be reduced, for example, the size of the spherulites can be reduced to 1 μm or less. As a result, a resin film with high crystallinity and high hardness can be obtained, and stress concentration between the spherulites that occurs during bending can be efficiently dispersed, thereby realizing a resin film that suppresses cracking and whitening during bending.
[0052] When a nucleating agent is simply added, the particle size becomes larger due to secondary aggregation of the nucleating agent in the resin. On the other hand, when a nucleating agent vesicle is added, the dispersibility in the resin is improved, so the number of crystal nuclei per amount of nucleating agent added is significantly increased compared to when a nucleating agent is simply added. As a result, the average particle size of the spherulites in the crystalline part of the resin becomes smaller, and the occurrence of cracks and whitening during bending processing can be suppressed. Therefore, by adding a nucleating agent vesicle, the degree of crystallization can be further increased, and it is possible to achieve both improved elastic modulus and processability.
[0053] The amount of the nucleating agent added to the surface protective layer 17 is, for example, preferably 0.05 parts by mass to 0.5 parts by mass, more preferably 0.1 parts by mass to 0.3 parts by mass, relative to 100 parts by mass of the resin material. When a nucleating agent vesicle is used, the amount of the nucleating agent added to the resin material is the amount of the nucleating agent added converted into the amount of the nucleating agent in the nucleating agent vesicle.
[0054] If the amount of nucleating agent added is less than 0.05 parts by mass, the crystallinity of the resin material may not be improved sufficiently, and the scratch resistance of the surface protective layer 17 may not be improved sufficiently. If the amount of nucleating agent added is more than 0.5 parts by mass, the spherulite growth of the resin material may be inhibited due to an excess of crystal nuclei, and as a result, the crystallinity of the resin material may not be improved sufficiently, and the scratch resistance of the surface protective layer 17 may not be improved sufficiently.
[0055] Methods for nano-sizing a nucleating agent include, for example, a solid-phase method in which the nucleating agent is primarily subjected to mechanical grinding to obtain nano-sized particles, a liquid-phase method in which nano-sized particles are synthesized or crystallized in a nucleating agent or a solution in which the nucleating agent is dissolved, and a gas-phase method in which nano-sized particles are synthesized or crystallized from a nucleating agent or a gas or vapor comprising the nucleating agent.
[0056] Examples of the solid phase method include a ball mill, a bead mill, a rod mill, a colloid mill, a conical mill, a disk mill, a hammer mill, a jet mill, etc. Examples of the liquid phase method include a crystallization method, a coprecipitation method, a sol-gel method, a liquid phase reduction method, a hydrothermal synthesis method, etc. Examples of the gas phase method include an electric furnace method, a chemical flame method, a laser method, a thermal plasma method, etc.
[0057] The method of nano-sizing the nucleating agent is preferably the supercritical reverse phase evaporation method. The supercritical reverse phase evaporation method is a method of producing a capsule (nano-sized vesicle) encapsulating a target substance using carbon dioxide in a supercritical state or under temperature or pressure conditions above the critical point. Carbon dioxide in a supercritical state means carbon dioxide in a supercritical state above the critical temperature (30.98°C) and critical pressure (7.3773±0.0030MPa). Carbon dioxide under temperature or pressure conditions above the critical point means carbon dioxide under conditions where only the temperature or only the pressure exceeds the critical condition.
[0058] In the specific nano-processing by the supercritical reverse phase evaporation method, first, an aqueous phase is injected into a mixed fluid of supercritical carbon dioxide, phospholipids as an outer membrane forming substance, and a nucleating agent as an encapsulating substance, and an emulsion of supercritical carbon dioxide and aqueous phase is generated by stirring. Next, the pressure is reduced, causing the carbon dioxide to expand and evaporate, resulting in phase inversion, and generating nanocapsules (nanovesicles) in which the phospholipids cover the surface of the nucleating agent particles with a single layer membrane. By using this supercritical reverse phase evaporation method, unlike the conventional encapsulation method in which the outer membrane on the surface of the nucleating agent particles becomes multiple membranes, it is possible to easily generate capsules with a single layer membrane, and therefore to prepare capsules with a smaller diameter.
[0059] The nucleating agent vesicle is prepared, for example, by the Bangham method, the extrusion method, the hydration method, the surfactant dialysis method, the reverse phase evaporation method, the freeze-thaw method, the supercritical reverse phase evaporation method, etc. Among these, the nucleating agent vesicle is preferably prepared by using the supercritical reverse phase evaporation method.
[0060] The outer membrane constituting the nucleating agent vesicle is, for example, composed of a monolayer membrane. The outer membrane is composed of a substance containing a biological lipid such as a phospholipid. In this specification, the nucleating agent vesicle whose outer membrane is composed of a substance containing a biological lipid such as a phospholipid is referred to as a nucleating agent liposome.
[0061] Examples of phospholipids constituting the outer membrane include glycerophospholipids such as phosphatidylcholine, phosphatidylethanolamine, phosphatidylserine, phosphatidic acid, phosphatidylglycerol, phosphatidylinositol, cardiopin, yolk egg lecithin, hydrogenated yolk egg lecithin, soybean lecithin, and hydrogenated soybean lecithin; sphingophospholipids such as sphingomyelin, ceramide phosphorylethanolamine, and ceramide phosphorylglycerol.
[0062] Other substances that form the outer membrane of the vesicle include dispersants such as nonionic surfactants and mixtures of these with cholesterols or triacylglycerols.
[0063] As the nonionic surfactant, for example, one or more of polyglycerin ether, dialkyl glycerin, polyoxyethylene hydrogenated castor oil, polyoxyethylene alkyl ether, polyoxyethylene sorbitan fatty acid ester, sorbitan fatty acid ester, polyoxyethylene polyoxypropylene copolymer, polybutadiene-polyoxyethylene copolymer, polybutadiene-poly(2-vinylpyridine), polystyrene-polyacrylic acid copolymer, polyethylene oxide-polyethylethylene copolymer, polyoxyethylene-polycaprolactam copolymer, etc. can be used.
[0064] Examples of cholesterols that can be used include cholesterol, α-cholestanol, β-cholestanol, cholestane, desmosterol (5,24-cholestadiene-3β-ol), sodium cholate, and cholecalciferol.
[0065] The outer membrane of the liposome may be formed from a mixture of a phospholipid and a dispersant. The nucleating agent vesicle is preferably a radical scavenger liposome having an outer membrane made of a phospholipid, and by forming the outer membrane from a phospholipid, the compatibility between the resin material of the surface protective layer 17 and the vesicle can be improved.
[0066] The nucleating agent is not particularly limited as long as it is a substance that is the starting point of crystallization when the resin crystallizes. Examples of the nucleating agent include metal phosphate salts, metal benzoates, metal pimelate salts, metal rosin salts, benzylidene sorbitol, quinacridone, cyanine blue, and talc. In particular, in order to maximize the effect of the nano-processing, it is preferable to use metal phosphate salts, metal benzoates, metal pimelate salts, and metal rosin salts that are non-melting and can be expected to have good transparency, but if the material itself can be made transparent by the nano-processing, colored quinacridone, cyanine blue, talc, etc. can also be used. It is also possible to appropriately mix melting benzylidene sorbitol with a non-melting nucleating agent.
[0067] In this embodiment, a nucleating agent encapsulated in vesicles is added to a resin material to crystallize the resin material when forming the surface protective layer 17. By adding the nucleating agent encapsulated in vesicles to the resin composition, it is possible to achieve an effect of dramatically improving the dispersibility of the nucleating agent in the resin material, i.e., in the surface protective layer 17.
[0068] However, it may be difficult or impractical to directly identify the nucleating agent encapsulated in the vesicles based on the structure and properties of the finished decorative sheet 10, depending on the circumstances. The reasons for this are as follows.
[0069] The nucleating agent added in the form of vesicles is in a dispersed state with high dispersibility, and is also highly dispersed in the surface protective layer 17 in the form of the laminate, which is the precursor of the produced decorative sheet 10. However, in the process of producing the decorative sheet 10, the laminate is usually subjected to various treatments such as compression treatment and hardening treatment, and such treatments may cause the outer membrane of the vesicles encapsulating the nucleating agent to break down or cause a chemical reaction.
[0070] For this reason, depending on the processing steps of the decorative sheet 10, there is variation in the state in which the outer membrane of the nucleating agent in the completed decorative sheet 10 is broken or a chemical reaction occurs, and there is a high possibility that the nucleating agent is not encapsulated (enveloped) by the outer membrane. If the nucleating agent is not encapsulated by the outer membrane, it is difficult to specify the physical properties of the nucleating agent itself within a numerical range, and it is also expected that it may be difficult to determine whether the constituent material of the broken outer membrane is the outer membrane of the vesicle or a material added separately from the nucleating agent.
[0071] Thus, although the present invention differs from the prior art in that the nucleating agent is highly dispersed in the decorative sheet 10, it is anticipated that there may be cases in which it is impractical to determine within a numerical range a structure or characteristics of the decorative sheet 10 that are analyzed based on measurements, whether this is because the nucleating agent is added in the form of vesicles encapsulating the nucleating agent.
[0072] <Base layer 19> For example, a polyester resin, a polyurethane resin, a mixture thereof, etc. can be used as the undercoat layer 19. Furthermore, by making the undercoat layer 19 a two-liquid type of polyol and isocyanate, the adhesion to the base sheet 11 and the cohesive force of the undercoat layer 19 itself can be improved.
[0073] Examples of the polyol that can be used include acrylic polyols and polyester polyols. Examples of the isocyanates that can be used include aromatic isocyanates such as tolylene diisocyanate and 4,4'-diphenylmethane diisocyanate, and aliphatic isocyanates such as hexamethylene diisocyanate, isophorone diisocyanate, and xylene diisocyanate. Among these, aromatic isocyanates are preferred in view of their rapid reactivity and heat resistance.
[0074] The thickness of the underlayer 19 is preferably 1 μm or more and 10 μm or less. If the thickness of the underlayer 19 is less than 1 μm, it may be dissolved and disappear depending on the type of solvent used in the adhesive, and may not contribute to improving adhesion.
[0075] Effects of this embodiment In the decorative sheet 10 according to this embodiment, the total thickness of the polyester-based resin layer 14 and the transparent thermoplastic resin layer 16 is within a range of 200 μm or more and 300 μm or less, and the Martens hardness of the polyester-based resin layer 14 is 40 N / mm 2 More than 190N / mm 2 Since the surface protective layer 17 contains an ionizing radiation curable resin, sufficient scratch resistance and impact resistance can be achieved without using a melamine board made of a non-chlorine based resin.
[0076] Furthermore, since the surface protective layer 17 contains at least one of a nucleating agent and an inorganic filler, scratch resistance can be further improved.
[0077] [Second embodiment] A second embodiment of the decorative sheet according to the present invention will be described with reference to Fig. 2. However, for parts similar to those in the above-mentioned embodiment, the same reference numerals as those used in the description of the above-mentioned embodiment will be used, and descriptions of parts that overlap with the description of the above-mentioned embodiment will be omitted.
[0078] <Transparent thermoplastic resin layer> As shown in FIG. 2, the decorative sheet 20 of this embodiment has a transparent thermoplastic resin layer 26 formed by laminating, in this order from the polyester resin layer 14 side, two layers: a first resin layer 26a formed containing a predetermined resin (hereinafter referred to as the "first resin"), and a second resin layer 26b formed containing a resin different from the first resin (hereinafter referred to as the "second resin").
[0079] The transparent thermoplastic resin layer 26 has the first resin layer 26a and the second resin layer 26b, and thus the necessary functions can be shared, thereby expanding the types of materials that can be used. For example, the first resin layer 26a is responsible for adhesion to the polyester-based resin layer 14, and the second resin layer 26b is responsible for various other functions.
[0080] Specifically, taking into consideration various functions such as scratch resistance, impact resistance, weather resistance, stain resistance, light resistance, transparency, foldability, thermoformability, etc., as well as material costs, etc., it is preferable that the first resin be a transparent maleic acid-modified polypropylene resin, and the second resin be a transparent polypropylene resin.
[0081] Thereby, the first resin layer 26a containing the first resin can improve adhesiveness, etc., and the second resin layer 26b containing the second resin can improve embrittlement resistance, etc. The second resin layer 26b can also contain at least one of an ultraviolet absorbing agent and a light stabilizer.
[0082] In addition, the mass content (mass%) of the transparent maleic acid-modified polypropylene resin, which is the first resin in the first resin layer 26a, can be made greater than the mass content (mass%) of the transparent polypropylene resin, which is the second resin in the second resin layer 26b.
[0083] Specifically, the mass content of the transparent maleic acid modified polypropylene resin, which is the first resin in the first resin layer 26a, can be set to 80 mass% or more, which is greater than the mass content of the transparent polypropylene resin, which is the second resin in the second resin layer 26b. Even with such a mass content, it is possible to reliably maintain the overall surface strength of the decorative sheet 20 while maintaining adhesion stability.
[0084] The first resin layer 26a preferably has a thickness of 10 μm or more, and preferably has a thickness of 20% or less of the total thickness of the transparent thermoplastic resin layer 26. In particular, the first resin layer 26a more preferably has a thickness of 50 μm or more, and more preferably has a thickness of 10% or less of the total thickness of the transparent thermoplastic resin layer 26.
[0085] If the thickness of the first resin layer 26a is less than 10 μm, it may cause a decrease in adhesion stability, and if it exceeds 20% of the total thickness of the transparent thermoplastic resin layer 26, it may cause a decrease in the overall surface strength of the decorative sheet 20. In other words, if the thickness of the first resin layer 26a is 10 μm or more and 20% or less of the total thickness of the transparent thermoplastic resin layer 26, it is possible to reliably maintain the overall surface strength of the decorative sheet 20 while maintaining adhesion stability.
[0086] The transparent thermoplastic resin layer 26 consisting of two layers, the first resin layer 26a and the second resin layer 26b, is preferably produced by simultaneously extruding and bonding the first resin layer 26a and the second resin layer 26b using a twin-screw extruder.
[0087] Although the transparent thermoplastic resin layer may have four or more layers, the extruder would have a complicated structure, and the manufacturing process would be complicated, so up to three layers is preferable. In practice, it is most practical to have the transparent thermoplastic resin layer 26 consisting of two layers, a first resin layer 26a and a second resin layer 26b, as shown in FIG.
[0088] Also, as the transparent polypropylene resin, for example, a mixture of polypropylene resin (a) with free terminal long chain branching and polypropylene resin (b) without free terminal long chain branching, in which the molecular weight distribution Mw / Mn, defined as the mass average molecular weight / number average molecular weight of the mixture, is in the range of 1 to 5, and the isotactic index, defined as the boiling heptane soluble residue, of the mixed resin of polypropylene resin (a) and polypropylene resin (b) is in the range of 1 to 90%. This makes it possible to suppress the occurrence of whitening and cracking when the decorative sheet 20 is bonded to a base material such as a steel plate via the undercoat layer 19 and then bent.
[0089] Here, the molecular weight distribution is defined as the ratio Mw / Mn, where Mn=Σ(Mi×Ni) / ΣNi and Mw=Σ(Ni×Mi2) / Σ(Ni×Mi), where Mw / Mn is the number average molecular weight when there are Ni molecules with molecular weight Mi. The closer to 1, the narrower the molecular weight distribution and the higher the uniformity. If this molecular weight distribution is kept below 5, the molecular weight can be made to a necessary and sufficient size, which helps to suppress whitening and cracking. Generally, the molecular weight distribution can be measured by gel permeation chromatography (GPC).
[0090] The isotactic index, defined as the boiling heptane soluble residue, is useful as an index for examining the crystallinity of polypropylene resin. Specifically, a sample is extracted with boiling n-heptane for a certain period of time, and the mass (%) of the unextracted portion is calculated to calculate the isotactic index.
[0091] Specifically, dry the cylindrical filter paper at 110±5°C for 2 hours, leave it in a constant temperature and humidity room for at least 2 hours, then place 8g to 10g of sample (powder or flake form) into the cylindrical filter paper and weigh it precisely using a weighing cup and tweezers. Place this on top of an extractor containing about 80cc of heptane, and assemble the extractor and cooler. Heat this in an oil bath or electric heater and extract for 12 hours. Adjust the heating so that the number of drops from the cooler is 130 or more per minute.
[0092] Next, the cylindrical filter paper containing the extraction residue is taken out and placed in a vacuum dryer to dry for 5 hours at 80°C and a reduced pressure of 100 mmHg or less. After drying, it is left in a constant temperature and humidity environment for 2 hours, and then precisely weighed and the isotactic index is calculated by (P / Po) x 100, where Po is the sample mass (g) before extraction and P is the sample mass (g) after extraction.
[0093] By setting the isotactic index at 90% or less, the sheet stiffness caused by polypropylene crystals can be suppressed. Methods for lowering the isotactic index include, for example, using an amorphous polypropylene component (syndiotactic polypropylene, adactic polypropylene, etc.) in part, randomly copolymerizing one or more olefin monomers such as ethylene or α-olefin, and adding various rubber components (for example, ethylene-propylene rubber (EPR), ethylene-propylene-diene rubber (EPDM), styrene-butadiene rubber (SBR), acrylonitrile-butadiene rubber (NBR), butadiene rubber (BR), isoprene rubber (IR), etc.).
[0094] The melt tension of the mixed resin of polypropylene resin (a) and polypropylene resin (b) is preferably in the range of 100 mN to 500 mN, more preferably in the range of 300 mN to 400 mN. If it exceeds 500 mN, the melt viscosity becomes too high, making it difficult to form a stable film, and if it is less than 100 mN, the long chain branched components are insufficient, making it difficult to obtain the desired performance. The melt tension is the tension when extruded at 60 mm / min and taken up at 2 mm / min at a temperature of 230°C using a rheometer with a nozzle capillary of 2.0 mm diameter.
[0095] In addition, it is preferable that the melt flow rate at 230°C of the mixture of polypropylene resin (a) and polypropylene resin (b) as specified in the Japanese Industrial Standard "JIS K6760" is in the range of 5 g / 10 min to 50 g / 10 min, since a stable film formation state can be easily maintained even at a molecular weight of a certain value or more. More preferably, it is in the range of 10 g / 10 min to 30 g / 10 min, and even more preferably, it is in the range of 10 g / 10 min to 25 g / 10 min.
[0096] If the melt flow rate exceeds 50 g / 10 min, the effect of the resin melt-extruded from the T-die gathering in the center (neck-in) becomes too large during melt extrusion through the T-die, and the thickness of the end of the resin melt-extruded from the T-die becomes too large. If the thickness of the end of the resin becomes too large in this way, the cooling efficiency decreases and the thickness in the width direction becomes unstable, making it difficult to maintain a stable film formation state.
[0097] On the other hand, if the melt flow rate is less than 5 g / 10 min, the draw resonance of the molten resin is likely to decrease, and the gap between the speed (initial speed) of the molten resin immediately after it leaves the T-die and the speed of the resin immediately after it touches the cooling roll becomes large, making it difficult for the molten resin to follow the initial speed, and therefore making it difficult to maintain a stable film formation state.
[0098] Effects of this embodiment In the decorative sheet 20 of this embodiment, the transparent thermoplastic resin layer 26 is provided on the polyester resin layer 14 side and comprises a first resin layer 26a containing a first resin, transparent maleic acid-modified polypropylene, and a second resin layer 26b provided on the first resin layer 26a and containing a second resin, transparent polypropylene resin. Therefore, not only can the same effects as those of the decorative sheet 10 of the embodiment described above be obtained, but also adhesion can be improved while embrittlement resistance can be reduced.
[0099] Furthermore, since the thickness of the first resin layer 26a is 10 μm or more and 20% or less of the total thickness of the transparent thermoplastic resin layer 26, it is possible to reliably maintain the overall surface strength of the decorative sheet 20 while maintaining adhesion stability.
[0100] [Other embodiments] In the above-mentioned embodiment, the decorative sheets 10, 20 having a surface protective layer 17 containing at least one of a nucleating agent and an inorganic filler have been described, but the present invention is not limited thereto. As another embodiment, for example, a decorative sheet having a surface protective layer that does not contain a nucleating agent and an inorganic filler is also possible. However, as in the above-mentioned embodiment, the decorative sheets 10, 20 having a surface protective layer 17 containing at least one of a nucleating agent and an inorganic filler are highly preferable because scratch resistance and the like can be further improved. EXAMPLES
[0101] Examples of the decorative sheet according to the present invention will be specifically described below, but the present invention is not limited to only the following examples that are specifically described.
[0102] [Preparation of test specimens and comparison specimens] Test specimen 1 A polyolefin inorganic filling sheet "OW (product number)" (thickness 55 μm) manufactured by Riken Technos Corporation was used as the base sheet 11, and a wood grain pattern was printed on the front side thereof by gravure printing to form a picture pattern layer 12.
[0103] Next, a biaxially oriented polyethylene terephthalate "Lumirror (registered trademark) T60 (product number)" manufactured by Toray Industries, Inc. (thickness: 200 μm, Martens hardness: 190 N / mm) that had been previously subjected to corona treatment was used. 2 ) was dry laminated onto the picture pattern layer 12 via a first adhesive layer 13 to provide a polyester resin layer 14. The Martens hardness (HM) was determined in accordance with the international standard "ISO 14577."
[0104] Next, a urethane resin adhesive was applied onto the polyester resin layer 14 and dried with hot air to provide a second adhesive layer 15, and then two layers of molten transparent thermoplastic resin were extruded from a T-die using a multi-screw extruder to provide a transparent thermoplastic resin layer 26 (thickness 100 μm) on the second adhesive layer 15. At the same time, all layers were nipped with a conduit embossing plate and a rubber roll to form embossments 10a, and then the transparent thermoplastic resin layer 26 was subjected to a surface treatment.
[0105] The transparent thermoplastic resin layer 26 was formed as a first resin layer 26a (thickness 15 μm) using a transparent maleic acid modified polypropylene resin "Rikeaid (registered trademark)" manufactured by Riken Vitamin Co., Ltd. As a second resin, 0.2 parts by mass of a phenolic antioxidant "Irganox (registered trademark) 1010 (product number)" manufactured by BASF Japan Ltd., 0.3 parts by mass of a hindered amine light stabilizer "Tinuvin (registered trademark) 622 (product number)" manufactured by BASF Japan Ltd., and 0.5 parts by mass of a benzotriazole ultraviolet absorber "Tinuvin (registered trademark) 326 (product number)" manufactured by BASF Japan Ltd. were added and mixed with 100 parts by mass of polypropylene resin to form a second resin layer 26b (thickness 85 μm).
[0106] Next, 10 parts by mass of a hardener "UR150B Varnish (product number)" manufactured by Toyo Ink Co., Ltd., 0.5 parts by mass of a benzotriazole-based ultraviolet absorber "Tinuvin (registered trademark) 326 (product number)" manufactured by BASF Japan Ltd., and 1 part by mass of a hindered amine-based light stabilizer "Tinuvin (registered trademark) 622 (product number)" manufactured by BASF Japan Ltd. were added to 100 parts by mass of a urethane-based resin "URV238 Varnish (product number)" manufactured by Toyo Ink Co., Ltd., and the coating amount after drying was 5 g / m 2 The transparent thermoplastic resin layer 26 was coated with the solution by gravure coating so that the solution had a thickness of 100 μm and a thickness of 100 μm. The solution was then immediately irradiated with ultraviolet light to cause curing, thereby providing the surface protective layer 17.
[0107] Next, after surface treatment was performed on the back surface of the base sheet 11, 10 parts by mass of silica and 3 parts by mass of isocyanate "LPNYB hardener" manufactured by Toyo Ink Co., Ltd. were added to 100 parts by mass of polyol "Laminstar (registered trademark) EM (product number)" manufactured by Toyo Ink Co., Ltd. to prepare a coating liquid, and the coating amount after drying was 3 g / m. 2 The undercoat layer 19 was formed by applying the above-mentioned solution to the back surface of the base sheet 11 by gravure coating and drying it.
[0108] A 6 mm-thick medium-density wood fiberboard (MDF) base material was then attached to the undercoat layer 19 via an ethylene-vinyl acetate copolymer resin emulsion adhesive to produce a decorative board specimen 1.
[0109] Test specimen 2 Thickness 100μm, Martens hardness 40N / mm 2 A decorative board specimen 2 was produced in the same manner as specimen 1, except that the polyester-based resin layer 14 was made of the above polyester-based resin layer 14.
[0110] Test specimen 3 Decorative board specimen 5 was produced in the same manner as specimen 2, except that the first resin layer 26a of the transparent thermoplastic resin layer 26 had a thickness of 20 μm and the second resin layer 26b had a thickness of 80 μm.
[0111] Test specimen 4 Decorative board specimen 6 was produced in the same manner as specimen 2, except that the first resin layer 26a of the transparent thermoplastic resin layer 26 had a thickness of 10 μm and the second resin layer 26b had a thickness of 90 μm.
[0112] Test specimen 5 A decorative board specimen 7 was prepared in the same manner as specimen 3, except that a surface protective layer 17 was formed by adding 0.5 parts by mass of nucleating agent vesicles to 100 parts by mass of the resin material.
[0113] Test specimen 6 A decorative board specimen 8 was produced in the same manner as specimen 3, except that a surface protective layer 17 was formed by adding 0.05 parts by mass of nucleating agent vesicles to 100 parts by mass of the resin material.
[0114] Comparison body 1 Thickness 250μm, Martens hardness 200N / mm 2 A comparative decorative board specimen 1 was prepared in the same manner as test specimen 1, except that the polyester-based resin layer 14 was made of the above polyester-based resin layer 14.
[0115] Comparison body 2 Thickness 50μm, Martens hardness 35N / mm 2 A comparative decorative board sample 2 was prepared in the same manner as test sample 1, except that the polyester-based resin layer 14 was made of the above polyester-based resin.
[0116] [Test Contents] Scratch resistance test In accordance with the pencil hardness test specified in the Japanese Industrial Standard "JIS K5600," test specimens 1 to 6 and comparative specimens 1 and 2 were subjected to a scratch resistance test using a pencil of hardness "H," and the degree of scratching was visually confirmed. The results are shown in Table 1 below. In Table 1, "○" indicates no scratches, "△" indicates slight scratches, and "×" indicates dent scratches, with "○" and "△" being pass marks and "×" being fail marks.
[0117] Impact resistance test In accordance with the DuPont impact test stipulated in the Japanese Industrial Standard "JIS K5400," test specimens 1 to 6 and comparative specimens 1 and 2 were subjected to impact by dropping a 500g weight from a height of 500mm, and the degree of denting was visually confirmed. The results are shown in Table 1 below. In Table 1, "○" indicates no dent, "△" indicates slight dent (less than 1.0mm), and "×" indicates dent (1.0mm or more) or cracking of the base material, with "○" and "△" being pass and "×" being fail.
[0118] [Test Results] The results of the above tests are shown in Table 1 below.
[0119] [Table 1]
[0120] As can be seen from Table 1, sufficient impact resistance was not obtained in Comparative Sample 1. Furthermore, sufficient scratch resistance was not obtained in Comparative Sample 2. In contrast, it was confirmed that sufficient scratch resistance and impact resistance were obtained in Samples 1 to 6, and in particular, it was confirmed that Samples 1, 5, and 6 were excellent in both scratch resistance and impact resistance. [Industrial Applicability]
[0121] The decorative sheet according to the present invention is made of a non-chlorine-based resin and can exhibit sufficient scratch resistance and impact resistance without using a melamine board, and therefore can be used industrially in an extremely beneficial manner. [Explanation of symbols]
[0122] 10 Decorative Sheet 10a Emboss 11 Base sheet 12 Pattern layer 13 First adhesive layer 14 Polyester resin layer 15 Second adhesive layer 16 Transparent thermoplastic resin layer 17 Surface protective layer 19 Base layer 20 Decorative Sheet 26 Transparent thermoplastic resin layer 26a First resin layer 26b Second resin layer
Claims
1. A decorative sheet comprising a base sheet made of a thermoplastic resin, and a picture pattern layer, a first adhesive layer, a polyester resin layer, a second adhesive layer, a transparent thermoplastic resin layer, and a surface protective layer laminated in this order on the base sheet made of a thermoplastic resin, the sum of the thickness of the polyester-based resin layer and the thickness of the transparent thermoplastic resin layer is in the range of 200 μm or more and 300 μm or less; The polyester resin layer has a Martens hardness of 40 N / mm 2 190N / mm or more 2 is as follows: The surface protective layer contains an ionizing radiation curable resin. A decorative sheet characterized by:
2. the transparent thermoplastic resin layer is provided on the polyester-based resin layer side and includes a first resin layer formed containing a first resin, and a second resin layer is provided on the first resin layer and formed containing a second resin different from the first resin, the first resin is a transparent maleic acid modified polypropylene resin, The second resin is a transparent polypropylene resin.
2. The decorative sheet according to claim 1.
3. The thickness of the first resin layer is 10 μm or more and is 20% or less of the total thickness of the transparent thermoplastic resin layer.
3. The decorative sheet according to claim 2.
4. The surface protective layer contains at least one of a nucleating agent and an inorganic filler. The decorative sheet according to any one of claims 1 to 3.