Skin material

JP2024167712AInactive Publication Date: 2024-12-04ASAHI KASEI KOGYO KABUSHIKI KAISHA
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023083967
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-22
Publication Date
2024-12-04
Estimated Expiration
Not applicable · inactive patent

Smart Images

  • Figure 2024167712000001
    Figure 2024167712000001
Patent Text Reader

Abstract

To provide a skin material with superior deodorant performance and wear resistance.SOLUTION: A skin material includes a surface layer and a sheet material bonded to one side of the surface layer. The surface layer is at least one selected from the group consisting of woven fabric, knitted fabric, natural leather, artificial leather, synthetic leather, and resin. The air permeability of the surface layer is 30 cc / cm2 / sec or more. The sheet material has deodorant inorganic particles held between two nonwoven fabrics, where the two nonwoven fabrics are fused together.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a skin material, and more particularly to a skin material having excellent deodorizing properties and abrasion resistance. [Background technology]

[0002] Conventionally, as a deodorizing material with excellent deodorizing function that can be used in fields such as automobiles and building wall materials, a deodorizing sound-absorbing material has been known that includes a short-fiber nonwoven fabric layer and an inorganic porous material-containing layer, and that is characterized in that the inorganic porous material-containing layer has an inorganic porous material sandwiched between melt-blown nonwoven fabrics or between a melt-blown nonwoven fabric and another long-fiber nonwoven fabric (see Patent Document 1 below). [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2009-275309 A Summary of the Invention [Problem to be solved by the invention]

[0004] However, the deodorizing material described in Patent Document 1 cannot fully exhibit deodorizing properties because the fine pores of the inorganic particles that are required to exhibit deodorizing properties are blocked by a binder resin or adhesive. In addition, when the deodorizing material described in Patent Document 1 is applied to parts that are touched and worn by people, such as car seats and carpets, there is a problem that the bag breaks due to the low abrasion resistance of the nonwoven fabric.

[0005] In view of the above-mentioned problems of the conventional techniques, an object of the present invention is to provide a covering material having excellent deodorizing properties and abrasion resistance. [Means for solving the problem]

[0006] The present inventors conducted intensive research and repeated experiments to solve the above problems, and as a result, discovered a skin material comprising a surface layer and a sheet material bonded to one side of the surface layer, the surface layer being at least one selected from the group consisting of woven fabrics, knitted fabrics, natural leather, artificial leather, synthetic leather, and resins, and the surface layer having an air permeability of 30 cc / cm 2 / sec or more, and the sheet material is a surface material in which deodorizing inorganic particles are sandwiched between two nonwoven fabrics and the two nonwoven fabrics are fused together. The inventors unexpectedly found that this problem can be solved, and have completed the present invention.

[0007] That is, the present invention is as follows. [1] A skin material including a surface layer and a sheet material bonded to one side of the surface layer, The surface layer is at least one selected from the group consisting of woven fabric, knitted fabric, natural leather, artificial leather, synthetic leather, and resin, and The air permeability of the surface layer is 30cc / cm 2 / sec or more, and The sheet material has deodorizing inorganic particles sandwiched between two sheets of nonwoven fabric, and the two sheets of nonwoven fabric are fused together. A skin material characterized by: [2] The skin material according to [1] above, wherein the nonwoven fabric is composed of three layers: a thermoplastic synthetic fiber layer (A), an ultrafine fiber layer (B), and a thermoplastic fiber layer (C) containing a component having a melting point 40°C or more lower than the melting point of the fibers constituting the thermoplastic synthetic fiber layer (A), and the thermoplastic fiber layers (C) of the nonwoven fabric are bonded to each other in the sheet material. [3] The nonwoven fabric has a basis weight of 15 to 120 g / m 2 The skin material according to the above [1] or [2], [4] The skin material according to any one of [1] to [3] above, wherein the nonwoven fabric has a formation index of 300 or less. [5] The skin material according to any one of [1] to [4] above, wherein the deodorant inorganic particles have a particle size of 1000 μm or less. [6] The skin material according to any one of the above [1] to [5], wherein the deodorizing inorganic particles are activated carbon. [7] The skin material according to [6], wherein the activated carbon is obtained by carbonizing at least one material selected from the group consisting of rice husks, straw, coffee beans, tea leaves, sugar cane, corn, fruit skins, reeds, and wakame stems. [8] The weight of the deodorant inorganic particles is 50 g / m 2 The skin material according to any one of the above [1] to [7], which is as follows: [9] The breathability of the nonwoven fabric is 0.1 to 100 cc / cm 2 The skin material according to any one of the above [1] to [8], wherein the viscosity is 100 / sec.

[10] The skin material according to [2] above, wherein the thermoplastic synthetic fiber layer (A) is a fiber layer having an average fiber diameter of 10 μm or more and 30 μm or less, and the ultrafine fiber layer (B) is a fiber layer having an average fiber diameter of 0.3 μm or more and 7 μm or less.

[11] The skin material according to [2] or

[10] , wherein at least a portion of the components in the thermoplastic fiber layer (C) having a melting point 40°C or more lower than the melting point of the fibers constituting the plastic synthetic fiber layer (A) is made of composite fibers having a core-sheath structure.

[12] The covering material according to any one of [1] to

[11] above, which is used for at least one application selected from the group consisting of a seat, a ceiling, an instrument panel, a console, an armrest, a door trim, a carpet, and a flooring material. Effect of the Invention

[0008] The covering material of the present invention is excellent in deodorizing property and abrasion resistance. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] Hereinafter, an embodiment of the present invention will be described in detail. In this embodiment, A skin material including a surface layer and a sheet material bonded to one side of the surface layer, The surface layer is at least one selected from the group consisting of woven fabric, knitted fabric, natural leather, artificial leather, synthetic leather, and resin, and The surface layer has a permeability of 30cc / cm 2 / sec or more, and The sheet material has deodorizing inorganic particles sandwiched between two sheets of nonwoven fabric, and the two sheets of nonwoven fabric are fused together. The skin material is characterized by the above.

[0010] <Skin material> The skin material of the present embodiment includes a surface layer and a sheet material bonded to one side of the surface layer. The surface layer of the skin material is made of at least one material selected from the group consisting of woven fabric, knitted fabric, natural leather, artificial leather, synthetic leather, and resin, and the nonwoven fabric is not exposed on the surface, so that the skin material has excellent abrasion resistance.

[0011] The sheet material is bonded to one side of the surface layer. The bonding method can be appropriately selected depending on the materials of the surface layer and the sheet material, but a method that does not prevent the odor components from contacting the deodorant inorganic particles is preferable. Specific examples of the bonding method include heat pressing, ultrasonic fusion, sewing, needle punching, etc. Also, the surface layer and the sheet material may be molded integrally and bonded to each other.

[0012] <Surface layer> The surface layer is at least one selected from the group consisting of woven fabric, knitted fabric, natural leather, artificial leather, synthetic leather, and resin. When the surface layer includes woven fabric, knitted fabric, artificial leather, synthetic leather, or resin, the material is not particularly limited and may include, for example, polyester, polyamide, polyurethane, polyvinyl chloride, and polypropylene. When the surface layer is a woven fabric, the weave structure is not particularly limited and may include, for example, plain weave, twill weave, satin weave, and the like. When the surface layer is a knitted fabric, it may be either weft knitted or warp knitted, or may be a three-dimensional knitted fabric, and the knitting structure is not particularly limited.

[0013] The surface layer has an air permeability of 30cc / cm to facilitate contact of odorous components with the deodorizing inorganic particles. 2 / sec or more, preferably 50cc / cm 2The surface layer may be unprocessed, or may be perforated or otherwise processed to achieve the above-mentioned air permeability.

[0014] <Sheet material> The sheet material has deodorizing inorganic particles sandwiched between two sheets of nonwoven fabric, and the two sheets of nonwoven fabric are fused together. By fusing the two sheets of nonwoven fabric together, the sheet material can sandwich the deodorizing inorganic particles without using a binder or adhesive, and since the deodorizing inorganic particles are not covered by the binder or adhesive, the sheet material can exhibit its inherent deodorizing properties.

[0015] The sheet material may contain particles other than the deodorant inorganic particles in order to impart a desired effect.

[0016] <Deodorizing inorganic particles> The deodorant inorganic particles are not particularly limited as long as they have a deodorant function, and examples thereof include various types of charcoal such as activated charcoal, silica gel, porous glass, zeolite, hydrotalcite, hydroxyapatite, clay minerals, etc. In the present embodiment, the deodorant inorganic particles are preferably activated charcoal from the viewpoints of light weight, large specific surface area, and antibacterial properties, and more preferably from the viewpoint of environmental consideration, are carbonized from at least one material selected from the group consisting of rice husks, straw, coffee beans, tea leaves, sugar cane, corn, fruit skins, reeds, and wakame stems.

[0017] The deodorant inorganic particles have a specific surface area of ​​100 m2 as measured by the nitrogen BET method. 2 The activated carbon preferably has a pore size distribution of at least one peak within a diameter range of 3 nm to 20 nm and a volume of pores within the same range of at least 30% of the total volume of pores. The activated carbon can be produced, for example, by using a silicon-containing plant-derived material as a raw material, carbonizing it, and then removing the silicon component from the plant-derived material after carbonization by treatment with an acid or alkali.

[0018] The shape of the deodorant inorganic particles is not particularly limited, and can be granular or plate-like, but granular ones are preferably used.When the deodorant inorganic particles are granular, their particle size is preferably 1000 μm or less from the viewpoint of increasing the surface area and improving deodorant properties, and more preferably 1 μm or more and 1000 μm or less, and even more preferably 10 μm or more and 500 μm or less from the viewpoint of achieving both deodorant properties and handling properties.

[0019] The basis weight of the deodorant inorganic particles is preferably 50 g / m from the viewpoint that the effect can be exhibited with a smaller content. 2 Less than 15g / m 2 Less than 7 g / m, more preferably 2 The following is the result.

[0020] <Nonwoven fabric> The nonwoven fabric is preferably composed of three layers: a thermoplastic synthetic fiber layer (A), an ultrafine fiber layer (B), and a thermoplastic fiber layer (C) containing a component having a melting point 40°C or more lower than the melting point of the fiber constituting the thermoplastic synthetic fiber layer (A). By adopting such a configuration, the thermoplastic fiber layers (C) are fused to each other, making it easier to sandwich the deodorant inorganic particles and also easier to suppress leakage of the deodorant inorganic particles. Furthermore, by having the ultrafine fiber layer in the nonwoven fabric, sound absorption can be improved.

[0021] When the nonwoven fabric is composed of the above three layers, from the viewpoint of preventing leakage of the deodorant inorganic particles and achieving good breathability, it is preferable that the thermoplastic synthetic fiber layer (A) is a fiber layer having an average fiber diameter of 10 μm to 30 μm, and the ultrafine fiber layer (B) is a fiber layer having an average fiber diameter of 0.3 μm to 7 μm. Examples of the constituent fibers include synthetic fibers such as polyolefin fibers (polyethylene, polypropylene, copolymerized polypropylene, etc.), aromatic polyester fibers (polyethylene terephthalate (PET), polybutylene terephthalate, polytrimethylene terephthalate), aliphatic polyester fibers (poly-D-lactic acid, poly-L-lactic acid, copolymers of D-lactic acid and L-lactic acid, copolymers of D-lactic acid and hydroxycarboxylic acid, copolymers of L-lactic acid and hydroxycarboxylic acid, copolymers of D-lactic acid, L-lactic acid and hydroxycarboxylic acid, and blends thereof), polyamide resins (polyamide 6, polyamide 66, copolymerized polyamide, etc.), and polyphenylene sulfide fibers.

[0022] When the nonwoven fabric is composed of the above three layers, from the viewpoint of fusion between the nonwoven fabrics, it is preferable that at least a part of the components in the thermoplastic fiber layer (C) having a melting point 40°C or more lower than the melting point of the fibers constituting the plastic synthetic fiber layer (A) is a composite fiber composed of two components having a low melting point component such as a core-sheath structure or a side-by-side structure, for example, a composite fiber in which the core has a high melting point and the sheath has a low melting point. For example, it is preferable that the core is a high melting point fiber such as polyethylene terephthalate (PET), polybutylene terephthalate, nylon 6, nylon 66, copolymerized polyamide, etc., and the sheath is a low melting point fiber such as low density polyethylene, high density polyethylene, polypropylene, copolymerized polyethylene, copolymerized polypropylene, copolymerized polyester (co-PET), aliphatic polyester, etc.

[0023] The weight of the nonwoven fabric is preferably 15 to 120 g / m from the viewpoint of preventing the deodorant inorganic particles from leaking and ensuring good breathability. 2 It is.

[0024] The formation index of the nonwoven fabric is preferably 300 or less from the viewpoint of preventing leakage of the deodorant inorganic particles.

[0025] The air permeability of the nonwoven fabric is preferably 0.1 to 100 cc / cm from the viewpoint of exhibiting high deodorizing properties. 2 / sec. The breathability of the nonwoven fabric is 1 to 50cc / cm 2 By setting the range of 1 / sec, excessive adsorption to the deodorizing inorganic particles can be suppressed, and the deodorizing effect can be maintained for a long period of time.

[0026] <Application> The skin material of the present embodiment has excellent deodorizing properties and abrasion resistance, and can be used as a skin material in various industrial fields. Specifically, the skin material of the present embodiment can be suitably used as a skin material for automobile seats, ceilings, instrument panels, consoles, armrests, door trims, carpets, flooring, etc. The skin material of the present embodiment can also be used for air filters. EXAMPLES

[0027] The present invention will be specifically described below with reference to examples and comparative examples, but the present invention is not limited to these. The physical properties in the following examples were measured by the following methods. In principle, the various physical properties of the present invention are measured by the following methods, but if there are circumstances that make it impossible to measure them by the following methods, they can be measured by an appropriate and reasonable alternative method.

[0028] (1) Air permeability (cc / cm 2 / sec) In accordance with JIS-L-1096, 1018 breathability test method (method A air volume), the air permeability from one side of a nonwoven fabric or skin material to the other side is measured using a Takayama Reed Co., Ltd. breathability tester FX3300 Laboair IV.

[0029] (2) Abrasion resistance According to JASOM403 A method (Taber rotary abrader method), a Taber type abrasion tester is used to abrade the test piece 1000 times at a load of 4.9N and a speed of 70rpm using a CS-10 abrasive wheel. After the test, the abrasion state of the test piece surface is observed and the following grade is given. The grade is given in 0.5 grade increments. (Grade assessment criteria) Grade 5: No change in surface condition Grade 4: Somewhat frayed Grade 3: Lots of fluff Grade 2: Lots of fuzz and thin threads Grade 1: Thread breakage.

[0030] (3) Market sentiment index (%) Using a formation tester FMT-MIII (manufactured by Nomura Shoji Co., Ltd.), measurements were taken at 4 points per meter in the CD direction to obtain a formation index. The smaller this value, the more uniform and free of spots the formation.

[0031] (4) Average fiber diameter (μm) A 500x magnified photograph is taken using a Keyence VHX-700F microscope, and the average value of 10 fibers in focus within the observation field is calculated.

[0032] (5) Thickness (mm) Based on JIS L 1913 B method. Measure the thickness at three or more points under a load of 0.02 kPa and calculate the average value.

[0033] (6) Weight (g / m 2 ) The basis weight of the nonwoven fabric layer is measured in accordance with JIS L 1913.

[0034] (7) Sound absorption performance (sound absorption rate (%)) In accordance with JIS A 1405, measurements are taken using a normal incidence measuring device (Brüel & Kjær Type 4206T) with 10 mm of air space behind the prototype skin material, and the sound absorption coefficients (%) are calculated at frequencies of 1500 Hz, 3000 Hz, and 5000 Hz as representative values.

[0035] (8) Deodorizing performance <Evaluation of deodorizing performance> Deodorizing performance: Evaluated using ammonia gas in accordance with Method II-2 Deodorizer Efficacy Test Method (chemical deodorization) set out in the Voluntary Standards for Consumer Use by the Japan Association of Air Fresheners, Air Fresheners, and Air Fresheners. Bag used: Freck Sampler 10L Dilution gas: Odorless air Detector tube used: Gastec 3La (for ammonia) <Measurement of deodorizing performance> After sealing a 100 x 100 mm sample in a 10 L gas bag, the initial ammonia gas concentration was adjusted to 100 ppm. The ammonia gas concentration after leaving it for 1 hour was measured using a detector tube. The value was calculated using the following formula. {(Measured concentration of blank test - Measured concentration of actual test) ÷ (Measured concentration of blank test)} x 100 (%)

[0036] (9) Antibacterial performance Use a sample 5cm x 5cm square and follow the JIS-L-1902 quantitative test (bacterial liquid absorption method). Test strain: Moraxella viable count measurement method: Pour plate culture method Culture time: 18 hours (ultraviolet intensity during culture 0.1mV / cm 2 (The sample was then exposed to UV light for 10 min.) The results were expressed as bacteriostatic activity values. A bacteriostatic activity value of 2.2 or higher is considered to have antibacterial effects.

[0037] (10) Average particle size of deodorant inorganic particles In accordance with JIS-Z-8815:1994 General rules for sieving test methods, a test sieve was used, and the opening (μm) of the test sieve when the passing percentage of inorganic activated carbon was 50% was taken as the average particle size.

[0038] (11) Specific surface area Measurements are made using an automatic specific surface area measuring device (Shimadzu Corporation, Gemini 2360). Since activated carbon has countless micropores and a large specific surface area, it is preferable to add a small sample weight of about 0.05 to 0.10 g. The measurement time must also be long. The cell containing the sample is degassed and dried under vacuum at 150°C or higher. After returning to room temperature, the cell is set in the specific surface area measuring device, and the adsorption of nitrogen gas onto the sample surface is measured according to the following BET equation: P / {V(P0-P)}=1 / (Vm×C)+{(C-1) / (Vm×C)}(P / P0) {In the formula, P0: saturated water vapor pressure (Pa), V: nitrogen adsorption amount (mg / g), Vm: monolayer adsorption amount (mg / g), C: parameter related to heat of adsorption etc. (-)<0.} The specific surface area was calculated using the following formula.

[0039] [Example 1] The lower nonwoven fabric and the upper nonwoven fabric are an SMS type nonwoven fabric (Pressise (registered trademark) α Seal, manufactured by Asahi Kasei Corporation, basis weight 70.5 g / m) composed of three layers: a spunbond layer (A) made of polyester fibers, a microfiber layer (B) made of polyester fibers, and a spunbond layer (C) made of core-sheath structure fibers containing, as a sheath component, a copolymer polyester having a melting point 40° C. or more lower than the melting point of the fibers constituting the A layer. 2 , thickness 0.23 mm) was used. On top of the layer containing the low melting point component of the lower nonwoven fabric, activated carbon (derived from coconut shells, average particle size 32 μm, specific surface area 820 m) is used as a deodorizing inorganic particle. 2 / g) uniformly at 10g / m 2 The layer containing the low melting point component of the upper nonwoven fabric was placed on top of the sprayed deodorant inorganic particles, and the nonwoven fabrics were bonded together with a heat press roll heated to 120° C. to obtain a sheet material. Next, a polyester fabric (basis weight 411 g / m) was applied as a surface layer onto the obtained sheet material. 2 , thickness 2mm, breathability 86cc / cm 2 The sheet material and the woven fabric were bonded together using a hot press roll heated to 220°C to obtain the skin material. The properties are shown in Table 1 below.

[0040] [Example 2] The lower and upper nonwoven fabrics have a basis weight of 41.3 g / m 2 , and the thickness is 0.23 mm, and the activated carbon weight is 20 g / m 2 The surface layer is polyester knit (weight 332g / m 2 , thickness 1.5mm, breathability 120cc / cm 2 A skin material was obtained in the same manner as in Example 1, except that the surface abrasion resistance was changed to Class 4 (surface abrasion resistance: Class 4 / sec). The properties are shown in Table 1 below.

[0041] [Example 3] The lower and upper nonwoven fabrics have a basis weight of 24.6 g / m 2 , 0.15mm thick, activated carbon derived from rice husk, average particle size 125μm, specific surface area 2046m 2 / g, and its basis weight is 5g / m 2 The surface layer is made of polyester fabric (466g / m 2 , thickness 2.2mm, air permeability 65cc / cm 2 A skin material was obtained in the same manner as in Example 1, except that the surface abrasion resistance was changed to Class 4 (surface abrasion resistance: Class 4 / sec). The properties are shown in Table 1 below.

[0042] [Example 4] The surface layer is polyester knit (460g / m 2 , thickness 1.3mm, air permeability 75cc / cm 2 A deodorizing skin material was obtained in the same manner as in Example 3, except that the temperature was changed to 100° C. / sec, and surface abrasion resistance was grade 4. The properties are shown in Table 1 below.

[0043] [Example 5] The lower nonwoven fabric was the same as that in Example 1, and the activated carbon was made from rice husks, with an average particle size of 355 μm and a specific surface area of ​​1753 m. 2 / g, and its basis weight is 5g / m 2 The surface layer is made of polyester three-dimensional knit fabric (weight 711g / m 2 , thickness 5.7mm, breathability 60cc / cm 2A skin material was obtained in the same manner as in Example 3, except that the surface roughness was changed to 1.0 mm / sec, and the surface abrasion resistance was 3.5 grade. The properties are shown in Table 1 below.

[0044] [Example 6] Deodorizing inorganic particles are silica (average particle size 355 μm, specific surface area 455 m 2 / g) and the basis weight is 10g / m 2 The surface layer is polyester suede (Dinamica (registered trademark), Asahi Kasei Corporation, dot pattern perforated product (circular 1 mm diameter holes, hole spacing 5.45 mm), basis weight 513 g / m 2 , thickness 1.6mm, breathability 36cc / cm 2 A skin material was obtained in the same manner as in Example 3, except that the sheet material was bonded to the surface layer using ultrasonic welding, and the surface layer had a surface abrasion resistance of 3.5 (fibers per 1000 mm / sec, surface abrasion resistance of 3.5). The properties are shown in Table 1 below.

[0045] [Comparative Example 1] The lower nonwoven fabric and the upper nonwoven fabric were spunbond nonwoven fabrics (Eltas (registered trademark), model number E05070, manufactured by Asahi Kasei Corporation, basis weight 70.0 g / m 2 , thickness 0.21 mm) was used. The same activated carbon as in Example 1 and an EVA-based hot melt adhesive with a melting point of 83°C and classified into particle sizes of 75 to 200 μm were mixed in a rotary powder mixer at a weight ratio of 1:1 to obtain a mixture of activated carbon and hot melt adhesive. This mixture was evenly applied at 200 g / m on the lower nonwoven fabric. 2 The upper nonwoven fabric was placed on the sprayed mixture, and the nonwoven fabrics were bonded together with a heat press roll heated to 120° C. to obtain a sheet material. Next, a polyester woven fabric (basis weight 467 g / m) was applied as a surface layer onto the obtained sheet material. 2 , thickness 1.8mm, breathability 28cc / cm 2 The sheet material and the surface layer were bonded together using a hot press roll heated to 220°C to obtain the skin material. The properties are shown in Table 1 below.

[0046] [Comparative Example 2] The lower and upper nonwoven fabrics were made of an SMS type nonwoven fabric that did not contain a low-melting point thermoplastic fiber layer (Pressise (registered trademark), manufactured by Asahi Kasei Corporation, basis weight 41.3 g / m 2 , thickness 0.23 mm) was used. Activated carbon (derived from coconut shells: average particle size 32 μm, specific surface area 820 m 2 The activated carbon and hot melt adhesive were mixed in a rotary powder mixer at a weight ratio of 1:10 with an EVA-based hot melt adhesive with a melting point of 83°C and classified into particle sizes of 75 to 200 μm, to obtain a mixture of activated carbon and hot melt adhesive. This mixture was then uniformly applied at 220 g / m2 onto the lower nonwoven fabric. 2 The upper nonwoven fabric was placed on the sprayed mixture, and the nonwoven fabrics were bonded together with a heat press roll heated to 120° C. to obtain a sheet material. No surface layer was used, and the sheet material was used as the skin material. The properties are shown in Table 1 below.

[0047] [Comparative Example 3] The same nonwoven fabric as in Example 3 was used as the lower nonwoven fabric, and the same nonwoven fabric as in Comparative Example 1 was used as the upper nonwoven fabric. Activated carbon (derived from coconut shells: average particle size 32 μm, specific surface area 820 m 2 The activated carbon and hot melt adhesive were mixed in a rotary powder mixer at a weight ratio of 1:10 with an EVA-based hot melt adhesive with a melting point of 83°C and classified into particle sizes of 75 to 200 μm to obtain a mixture of activated carbon and hot melt adhesive. This was then uniformly applied at 220 g / m2 onto the layer of the lower nonwoven fabric containing a low melting point component. 2 The upper nonwoven fabric was placed on the sprayed mixture, and the nonwoven fabrics were bonded together with a heat press roll heated to 120° C. to obtain a sheet material. Next, a polyester knit fabric (weight 585 g / m2) was applied as a surface layer onto the obtained sheet material. 2 , thickness 3.6mm, air permeability 15cc / cm 2 The sheet material and the surface layer were bonded together using a hot press roll heated to 220°C to obtain the skin material. The properties are shown in Table 1 below.

[0048] [Table 1] [Industrial Applicability]

[0049] The covering material according to the present invention has excellent deodorizing properties and abrasion resistance, and can therefore be used as a covering material in various industrial fields. Specifically, the covering material according to the present invention can be suitably used as a covering material for automobile seats, ceilings, instrument panels, consoles, armrests, door trims, carpets, flooring, etc. The covering material according to the present invention can also be used for air filters.

Claims

1. A skin material including a surface layer and a sheet material bonded to one side of the surface layer, The surface layer is at least one selected from the group consisting of woven fabric, knitted fabric, natural leather, artificial leather, synthetic leather, and resin, and The air permeability of the surface layer is 30 cc / cm 2 / sec or more, and The sheet material has deodorizing inorganic particles sandwiched between two sheets of nonwoven fabric, and the two sheets of nonwoven fabric are fused together. A skin material characterized by:

2. 2. The skin material according to claim 1, wherein the nonwoven fabric is composed of three layers: a thermoplastic synthetic fiber layer (A), an ultrafine fiber layer (B), and a thermoplastic fiber layer (C) containing a component having a melting point that is 40° C. or more lower than the melting point of the fibers that constitute the thermoplastic synthetic fiber layer (A), and the thermoplastic fiber layers (C) of the nonwoven fabric are bonded to each other in the sheet material.

3. The nonwoven fabric has a basis weight of 15 to 120 g / m 2 The skin material according to claim 1 or 2,

4. 3. The skin material according to claim 1, wherein the nonwoven fabric has a formation index of 300 or less.

5. 3. The skin material according to claim 1, wherein the deodorant inorganic particles have a particle size of 1000 μm or less.

6. 3. The skin material according to claim 1, wherein the deodorizing inorganic particles are activated carbon.

7. 3. The skin material according to claim 1 or 2, wherein the activated carbon is obtained by carbonizing at least one material selected from the group consisting of rice husks, straw, coffee beans, tea leaves, sugar cane, corn, fruit skins, reeds, and wakame stems.

8. The weight of the deodorant inorganic particles is 50 g / m 2 3. The skin material according to claim 1 or 2, wherein:

9. The nonwoven fabric has a breathability of 0.1 to 100 cc / cm 2 The skin material according to claim 1 or 2, wherein the surface tension is 1 / sec.

10. 3. The skin material according to claim 2, wherein the thermoplastic synthetic fiber layer (A) is a fiber layer having an average fiber diameter of 10 μm or more and 30 μm or less, and the ultrafine fiber layer (B) is a fiber layer having an average fiber diameter of 0.3 μm or more and 7 μm or less.

11. 11. The skin material according to claim 2 or 10, wherein at least a part of the components in the thermoplastic fiber layer (C) having a melting point 40° C. or more lower than the melting point of the fibers constituting the thermoplastic synthetic fiber layer (A) is made of composite fibers having a core-sheath structure.

12. 3. The covering material according to claim 1 or 2, which is used for at least one application selected from the group consisting of a seat, a ceiling, an instrument panel, a console, an armrest, a door trim, a carpet, and a floor material.

Citation Information

Patent Citations

  • Deodorant and sound-absorbing material