Gas separation membrane and method of manufacturing the same

A gas separation membrane with a 0.2 μm to 5.0 μm thick gas separation layer of organic polymer nanofibers and porous polymers addresses the low permeability issue, achieving high permeability and strength with minimal damage and improved selectivity.

JP2024167739APending Publication Date: 2024-12-04NISSAN MOTOR CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023084013
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-22
Publication Date
2024-12-04

AI Technical Summary

Technical Problem

Existing gas separation membranes with a crosslinked cellulose resin and cellulose nanofibers exhibit low gas permeability despite their thickness, failing to adequately enhance permeability and strength.

Method used

The gas separation membrane is designed with a thickness of 0.2 μm to 5.0 μm, incorporating a gas separation layer made of organic polymer nanofibers and porous polymers such as intrinsic microporous polymers or polyimide, supported by a porous layer, using a manufacturing method that involves applying a coating liquid containing a porous polymer onto a nanofiber layer and removing the solvent.

Benefits of technology

The membrane achieves excellent gas permeability and strength, with improved selectivity and reduced membrane damage, as demonstrated by permeability rates exceeding 10 GPU and minimal permeability increase.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024167739000001_ABST
    Figure 2024167739000001_ABST
Patent Text Reader

Abstract

To provide a gas separation membrane with high gas permeability and strength and a method of manufacturing the same.SOLUTION: A gas separation membrane includes: a gas separation layer; and a porous layer supporting the gas separation layer. The gas separation layer includes: a nanofiber made of an organic polymer; and a porous polymer with gas separation ability. The porous polymer contains at least one kind selected from the group consisting of an intrinsic micro porous polymer, a polytrimethylsilylpropyne and polyimide. A thickness of the gas separation layer is 0.2 μm or more and 5.0 μm or less.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a gas separation membrane and a method for manufacturing the same, and more particularly to a gas separation membrane having excellent gas permeability and strength and a method for manufacturing the same. [Background technology]

[0002] Conventionally, Patent Document 1 discloses a gas separation membrane that exhibits excellent gas permeability and excellent gas separation selectivity, has excellent gas separation performance even when used under high temperature, high pressure and high humidity conditions, and is less susceptible to the influence of impurities such as toluene present in natural gas. The gas separation membrane disclosed in Patent Document 1 is a gas separation membrane having a gas separation layer containing a crosslinked cellulose resin, has a predetermined connection structure in the crosslinked structure, and contains a predetermined amount of organic solvent. In addition, in the gas separation membrane disclosed in Patent Document 1, the gas separation layer contains cellulose nanofibers. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] International Publication No. 2016 / 136294 Summary of the Invention [Problem to be solved by the invention]

[0004] However, as disclosed in Example 32 of Patent Document 1, the gas separation membrane has a gas separation layer containing a crosslinked cellulose resin and has a predetermined linking structure in the crosslinked structure, and the gas separation layer contains a predetermined amount of organic solvent and cellulose nanofibers, so the thickness of the gas separation layer is as thick as 40 μm. As a result, there was a problem that the effect of improving gas permeability was not fully exhibited even if the gas separation layer contained cellulose nanofibers. In addition, the present inventors further studied the porous polymer of the gas separation layer and found that the gas permeability of the gas separation membrane containing a cellulose resin was low.

[0005] The present invention has been made in consideration of the problems associated with the conventional techniques, and an object of the present invention is to provide a gas separation membrane having excellent gas permeability and strength, and a method for producing the same. [Means for solving the problem]

[0006] As a result of extensive research into achieving the above-mentioned object, the inventors discovered that the above-mentioned object can be achieved by setting the thickness of the specified gas separation layer to be 0.2 μm or more and 5.0 μm or less, and thus completed the present invention.

[0007] That is, the gas separation membrane of the present invention has a gas separation layer and a porous layer supporting the gas separation layer. The gas separation layer includes nanofibers made of an organic polymer and a porous polymer having gas separation performance. The porous polymer contains at least one selected from the group consisting of polymers of intrinsic microporosity, polytrimethylsilylpropyne, and polyimides. The thickness of the gas separation layer is 0.2 μm or more and 5.0 μm or less.

[0008] In addition, the method for producing a gas separation membrane of the present invention is a method for producing a gas separation membrane having a gas separation layer and a porous layer supporting the gas separation layer, the gas separation layer containing nanofibers made of an organic polymer and a porous polymer having gas separation performance, the porous polymer containing at least one selected from the group consisting of polymers of intrinsic microporosity, polytrimethylsilylpropyne, and polyimide, and the gas separation layer having a thickness of 0.2 μm or more and 5.0 μm or less. In this manufacturing method, a coating liquid containing a porous polymer having gas separation performance and a solvent is applied to a nanofiber layer containing nanofibers made of an organic polymer formed on a porous layer to impregnate the nanofiber layer with the coating liquid, and then the solvent is removed from the coating liquid. Effect of the Invention

[0009] According to the present invention, since the thickness of the above-mentioned gas separation layer is set to be 0.2 μm or more and 5.0 μm or less, it is possible to provide a gas separation membrane having excellent gas permeability and strength, and a method for producing the same. [Brief description of the drawings]

[0010] [Figure 1] 1 is a cross-sectional view that diagrammatically illustrates a first embodiment of a gas separation membrane of the present invention. [Diagram 2] FIG. 4 is a cross-sectional view that illustrates a gas separation membrane of a second embodiment. [Diagram 3] FIG. 1 is an explanatory diagram illustrating a schematic diagram of one embodiment of a method for producing a gas separation membrane of the present invention. [Figure 4] FIG. 2 is an explanatory diagram showing a schematic view of a stainless steel gas separation membrane module used for evaluating gas separation membranes. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] The gas separation membrane and the method for producing the gas separation membrane of the present invention will be described in detail below with reference to the drawings. Note that the dimensional ratios of the drawings cited below are exaggerated for the convenience of explanation and may differ from the actual ratios.

[0012] [Gas separation membrane] (First embodiment) 1, the gas separation membrane 1 of this embodiment has a gas separation layer 10 and a porous layer 20 formed of a nonwoven fabric that supports the gas separation layer 10. The thickness of this gas separation layer 10 is 0.2 μm or more and 0.5 μm or less. The gas separation layer 10 also contains nanofibers made of an organic polymer and polymers of intrinsic microporosity (PIM) as a porous polymer having gas separation performance (not shown).

[0013] Here, in the present invention, the gas separation layer 10 is a layer that separates a gas containing one or more components from a mixed gas containing two or more components. The gas separation layer 10 can be used, for example, as a layer that separates O2 from air containing oxygen (O2) and nitrogen (N2), or as a layer that separates CO2 or water vapor (H2O) from air containing carbon dioxide (CO2) or water vapor (H2O).

[0014] Furthermore, in the present invention, as long as the porous layer 20 can support the gas separation layer 10 and ensure the permeability of the gas separated by the gas separation layer 10, its structure is not particularly limited to one formed from a nonwoven fabric.

[0015] Furthermore, in the present invention, the thickness of the gas separation layer 10 is defined as the distance from the surface (portion) of the porous layer 20 in contact with the surface 20a to the surface 10a of the gas separation layer 10.

[0016] In the present invention, the thickness of the gas separation layer can be measured and calculated as follows. First, the gas separation membrane is cut in the thickness direction at an arbitrary position of the gas separation membrane. Next, the obtained cut surface is observed with a scanning electron microscope (SEM) or a transmission electron microscope (TEM) or the like, and if necessary, further observed with energy dispersive X-ray spectroscopy (EDS), X-ray photoelectron spectroscopy (XPS) or Fourier transform infrared spectroscopy (FT-IR), and the distance from the part in contact with the surface of the porous layer to the surface of the gas separation layer is measured at any five points. Then, the average value of the distances at these five points is calculated to be the thickness of the gas separation layer.

[0017] Next, advantages of this embodiment will be described. According to this embodiment, the thickness of the gas separation layer is 0.2 μm or more and 5.0 μm or less, so that excellent gas permeability and strength can be achieved.

[0018] For example, when the porous polymer is made of cellulose, excellent gas permeability cannot be achieved. On the other hand, when the porous polymer is made of the above-mentioned polymer of intrinsic microporosity (PIM), polytrimethylsilylpropyne (PTMSP), or polyimide, excellent gas permeability can be achieved, although to a greater or lesser extent. These can be used alone or in combination of two or more.

[0019] Furthermore, if the thickness of the gas separation layer is less than 0.2 μm, excellent strength cannot be achieved. On the other hand, if the thickness of the gas separation layer is more than 5.0 μm, excellent gas permeability cannot be achieved. Furthermore, from the viewpoint of achieving better gas permeability and strength, the thickness of the gas separation layer is preferably 0.5 μm or more, more preferably 4.0 μm or less, and more preferably 3.0 μm or less.

[0020] 2 to 4 are diagrams for explaining embodiments of the gas separation membrane and the manufacturing method thereof of the present invention. In the following embodiments, the same components as those in the first embodiment described above are denoted by the same reference numerals, and detailed descriptions of the invention are omitted.

[0021] Second embodiment 2, the gas separation membrane 2 of this embodiment has a structure similar to that of the gas separation membrane 1 of the first embodiment, except that the gas separation layer 10 has a gas separation inner layer 11 containing nanofibers made of an organic polymer and a porous polymer having gas separation performance, and a gas separation surface layer 12 containing only a porous polymer having gas separation performance. The compositions of the porous polymer having gas separation performance contained in the gas separation inner layer 11 and the gas separation surface layer 12 may be the same or different.

[0022] Next, advantages of this embodiment will be described. According to this embodiment, since the gas separation layer 10 has the above-mentioned gas separation inner layer 11 and gas separation outer layer 12, in addition to the advantages of the first embodiment, there is an advantage that gas selectivity can be improved.

[0023] The specifications, materials, etc. of the components in the gas separation membrane of the above-mentioned embodiment will be described in more detail below.

[0024] (Gas separation layer 10) Suitable examples of the porous polymer include polymers of intrinsic microporosity (PIM) such as PIM-1, and polyimides such as aromatic polyimides and fluorine-containing polyimides. Among them, it is more preferable to use PIM-1. PIM-1 has, for example, a structural unit represented by the following formula (I).

[0025] [ka]

[0026] In the above formula (I), R 1 is a hydrogen atom or a linear or branched alkyl group having 1 to 4 carbon atoms, and R 2 is a hydrogen atom, a linear or branched alkyl group having 1 to 4 carbon atoms, or a cyano group; R 3 is a hydrogen atom, a linear or branched alkyl group having 1 to 4 carbon atoms, or a cyano group. 1 , R 2 and R 3 may be the same or different.

[0027] As shown in formula (I), PIM-1 is a polymer that has a rigid ladder structure and a bent backbone and can form micropores inside the layer, so that the gas separation layer 10 containing PIM-1 has excellent gas permeability.

[0028] Suitable examples of organic polymers that form nanofibers include fluororesins such as polyvinylidene fluoride (PVDF) and polytetrafluoroethylene (PTFE). Among these, it is more preferable to use polyvinylidene fluoride (PVDF).

[0029] The average fiber diameter of the nanofibers is usually 500 nm or less, and from the viewpoint of realizing better gas permeability and strength, the average fiber diameter of the nanofibers is preferably 1 to 100 nm, more preferably 5 to 80 nm, and more preferably 10 to 50 nm. Furthermore, such nanofibers are preferably formed into a nonwoven fabric.

[0030] Here, in the present invention, the average fiber diameter of the nanofibers can be measured and calculated as follows. First, the gas separation membrane is cut in the thickness direction at an arbitrary position of the gas separation membrane. Next, the obtained cut surface is observed by SEM, TEM, etc., and further observed by EDS or XPS as necessary, and the width in the direction perpendicular to the axial direction of the nanofibers is measured at any five positions as the fiber diameter. Then, the average value of these fiber diameters is calculated to be the average fiber diameter of the nanofibers.

[0031] (Porous layer 20) As the material for forming the porous layer, either an organic material or an inorganic material can be used, but it is preferable to use an organic material. As the organic material, for example, olefin resins such as polyethylene (PE) and polypropylene (PP), and polyester resins such as polyethylene terephthalate (PET) and polybutylene terephthalate (PBT) are preferably used. These can be used alone or in combination of two or more. Among them, it is more preferable to use polyethylene terephthalate (PET).

[0032] From the viewpoint of imparting high mechanical strength, the thickness of the porous layer is preferably from 1 μm to 3000 μm, more preferably from 5 μm to 500 μm, and even more preferably from 5 μm to 200 μm.

[0033] Here, in the present invention, the thickness of the porous layer can be measured and calculated as follows. First, the gas separation membrane is cut in the thickness direction at an arbitrary position of the gas separation membrane. Next, the obtained cut surface is observed by SEM, TEM, etc., and further observed by EDS, XPS or FT-IR as necessary, and the distance from the front surface 20a to the back surface 20b of the porous layer is measured at any five points (see FIG. 1, etc.). Then, the average value of the distances at these five points is calculated to be the thickness of the porous layer.

[0034] [Method of manufacturing gas separation membrane] The method for producing a gas separation membrane of this embodiment is one embodiment of the method for producing the gas separation membrane of the present invention described above.

[0035] First, as shown in the upper diagram of Fig. 3, a substrate is prepared in which a nanofiber layer 30 is formed on a porous layer 20. Such a substrate can be obtained, for example, by laminating the nanofiber layer 30 on the above-mentioned porous layer 20 by lamination processing.

[0036] As the nanofiber layer 30, for example, a nonwoven fabric containing the nanofibers described above can be used. From the viewpoint of realizing excellent strength, the thickness of the nanofiber layer is preferably 0.2 μm or more, and more preferably 0.5 μm or more. From the viewpoint of realizing excellent gas permeability, the thickness of the nanofiber layer is preferably 5.0 μm or less, more preferably 4.0 μm or less, and even more preferably 3.0 μm or less. The basis weight of the nonwoven fabric is, for example, 0.8 to 1.2 g / m 2 It is preferable that:

[0037] In addition, the contact angle of the coating liquid 40, which will be described later, with the nanofiber layer 30 is preferably smaller than the contact angle of the coating liquid 40 with the porous layer 20. Furthermore, the contact angle of the coating liquid, which will be described later, with the nanofiber layer is preferably less than 90°.

[0038] In the present invention, the contact angle of the coating liquid with respect to the nanofiber layer or the porous layer can be measured and calculated as follows: In accordance with the Japanese Industrial Standards, Testing Method for Wettability of Glass Substrate Surfaces (JIS R 3257), the coating liquid described below is dropped onto the surface of the nanofiber layer or the porous layer, and the contact angle is measured and calculated by the θ / 2 method.

[0039] Next, as shown in the central diagram of Figure 3, the coating liquid 40 is applied to the above-mentioned nanofiber layer 30 using a coating device 60 such as a die coater that does not pressurize the coating liquid 40 supplied to the nanofiber layer 30, and the coating liquid 40 is impregnated into the nanofiber layer 30 to form a coating liquid-impregnated layer 50.

[0040] The coating liquid 40 contains the above-mentioned porous polymer and a solvent (not shown). Examples of such solvents include tetrahydrofuran, chloroform, dichloromethane, N-methyl-2-pyrrolidone, toluene, isopropyl alcohol, and tetralin. These can be used alone or in combination of two or more. For example, tetrahydrofuran (THF) is a suitable solvent for PIM-1 and polyimide, in view of the high solubility of PIM-1 and polyimide.

[0041] Moreover, the arrow A in the figure indicates the traveling direction of the coating device 60. As the coating device 60, a gravure coater having a gravure roll can also be used instead of a die coater.

[0042] Thereafter, as shown in the lower diagram of Figure 3, the solvent is removed from the coating liquid 40 impregnated into the above-mentioned coating liquid-impregnated layer 50, and if necessary, the impregnation of the nanofiber layer 30 with the coating liquid 40 and the removal of the solvent from the coating liquid 40 impregnated into the coating liquid-impregnated layer 50 are repeated to obtain the gas separation membrane of the present embodiment described above.

[0043] The coating fluid 40 may be removed from the coating fluid-impregnated layer 50 by drying in the air at a temperature of 10° C. or higher and 40° C. or lower for 1 hour or higher and 8 hours or lower.

[0044] Next, the advantages of this embodiment will be described. According to this embodiment, when the coating liquid is applied to the nanofiber layer using a coating device such as a die coater or gravure coater that does not pressurize the coating liquid instead of a coating device (e.g., a roll coater or a bar coater) that pressurizes the coating liquid supplied to the nanofiber layer, a gas separation membrane having excellent gas permeability and strength can be obtained with a good yield. In particular, by making the contact angle of the coating liquid with respect to the nanofiber layer smaller than the contact angle of the coating liquid with respect to the porous layer or by making the contact angle of the coating liquid with respect to the nanofiber layer less than 90°, the coating liquid penetrates only into the nanofiber layer and does not penetrate into the underlying porous layer, so that the thickness of the gas separation layer can be controlled by the thickness of the nanofiber layer. In addition, since the gas separation layer contains a nanofiber layer, excellent strength can be achieved. Furthermore, since the underlying porous layer contains almost no porous polymer, excellent gas permeability can be achieved. EXAMPLES

[0045] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples. Each example and comparative example was carried out under atmospheric pressure, at room temperature (25°C), and at a relative humidity of 50% RH, unless otherwise specified.

[0046] Example 1 In the first coating process, a nanofiber layer (material: PVDF, shape: nanofiber nonwoven fabric, average nanofiber fiber diameter: 50 nm, basis weight: 0.59 g / m) was applied on a porous layer (material: PET, shape: nonwoven fabric, thickness: 100 μm). 2 The nanofiber layer of the substrate on which the porous polymer (material: PIM-1 (R in formula (I)) was laminated) was applied with a coating solution (porous polymer (material: PIM-1 (R in formula (I)) 1 is a methyl group, R 2 is a cyano group, R 3 is a hydrogen atom.) Weight average molecular weight (Mw) = 3.1 × 10 5 The porous polymer was coated with a mixture of 100% polyaniline (POW), weight average molecular weight (Mw) / number average molecular weight (Mn) = 5.4, solvent (material: THF), and porous polymer concentration: 4% by mass using a gravure coater equipped with a gravure roll (plate and line count: 150 L / inch).

[0047] The coating solution applied to the nanofiber layer was then dried in a fume hood at room temperature (25° C.) for 4 hours to remove the solvent from the coating solution, thereby forming a gas separation layer having an uncoated nanofiber layer.

[0048] Furthermore, in the second coating step, the same coating liquid was coated onto the uncoated nanofiber layer using the same gravure coater.

[0049] Thereafter, it was dried in a draft at room temperature (25°C) for 4 hours to remove the solvent from the coating liquid applied to the uncoated nanofiber layer, forming a gas separation layer and obtaining the gas separation membrane of this example.

[0050] (Examples 2 to 8) The same procedure as in Example 1 was repeated except that the basis weight of the nanofiber layer and the thickness of the gas separation layer were changed as shown in Table 1, to obtain gas separation membranes of each example.

[0051] Example 9 In the first coating process, a nanofiber layer (material: PVDF, shape: nanofiber nonwoven fabric, average fiber diameter of nanofiber: 50 nm) was laminated on a porous layer (material: PET, shape: nonwoven fabric, thickness: 100 μm). The coating liquid (porous polymer (material: PTMSP, weight average molecular weight (Mw) = 5.4 × 10 5 The porous polymer was coated with a mixture of 100% polyaniline (POW), weight average molecular weight (Mw) / number average molecular weight (Mn) = 6.13, solvent (material: THF), and porous polymer concentration: 4% by mass using a gravure coater equipped with a gravure roll (plate / line count: 150 L / inch).

[0052] The coating solution applied to the nanofiber layer was then dried in a fume hood at room temperature (25° C.) for 4 hours to remove the solvent from the coating solution, thereby forming a gas separation layer having an uncoated nanofiber layer.

[0053] Furthermore, in the second coating step, the same coating liquid was coated onto the uncoated nanofiber layer using the same gravure coater.

[0054] Thereafter, it was dried in a draft at room temperature (25°C) for 4 hours to remove the solvent from the coating liquid applied to the uncoated nanofiber layer, forming a gas separation layer and obtaining the gas separation membrane of this example.

[0055] Example 10 Furthermore, the same coating liquid was applied to the gas separation layer of Example 9 using the same gravure coater, and then dried in a draft at room temperature (25°C) for 4 hours to remove the solvent from the coating liquid applied to the gas separation layer, thereby forming a gas separation layer of the thickness shown in Table 1. The same operations as in Example 9 were repeated, except that the gas separation membrane of this example was obtained.

[0056] Example 11 The porous polymer in the coating liquid was polyimide (6FDA-3MPA, number average molecular weight (Mn) = 2.5 × 10 5 The same procedure as in Example 10 was repeated, except that the weight average molecular weight (Mw) / number average molecular weight (Mn) was changed to 1.7, to obtain a gas separation membrane of this example.

[0057] Example 12 The porous polymer in the coating liquid was polyimide (6FDA-3MPA, number average molecular weight (Mn) = 2.5 × 10 5 The same procedure as in Example 9 was repeated, except that the weight average molecular weight (Mw) / number average molecular weight (Mn) was changed to 1.7, to obtain a gas separation membrane of this example.

[0058] Comparative Example 1 The same procedure as in Example 1 was repeated except that the basis weight of the nanofiber layer and the thickness of the gas separation layer were changed as shown in Table 1, to obtain a gas separation membrane of this example.

[0059] Comparative Example 2 In the first coating process, a nanofiber layer (material: PVDF, shape: nanofiber nonwoven fabric, average fiber diameter of nanofiber: 50 nm) was laminated on a porous layer (material: PET, shape: nonwoven fabric, thickness: 100 μm) of a substrate. A coating liquid (porous polymer (material: PIM-1 (R in formula (I)) 1 is a methyl group, R 2 is a cyano group, R 3 is a hydrogen atom.) Weight average molecular weight (Mw) = 3.1 × 10 5 The porous polymer was coated with a mixture of 100% polyaniline (POW), weight average molecular weight (Mw) / number average molecular weight (Mn) = 5.4, solvent (material: THF), and porous polymer concentration: 4% by mass using a gravure coater equipped with a gravure roll (plate and line count: 150 L / inch).

[0060] The coating solution applied to the nanofiber layer was then dried in a fume hood at room temperature (25° C.) for 4 hours to remove the solvent from the coating solution, thereby forming a gas separation layer having an uncoated nanofiber layer.

[0061] Furthermore, in the second coating step, the same coating liquid was coated onto the uncoated nanofiber layer using the same gravure coater.

[0062] Thereafter, the coating was dried in a draft at room temperature (25° C.) for 4 hours to remove the solvent from the coating liquid applied to the uncoated nanofiber layer, thereby forming a gas separation layer.

[0063] Furthermore, the same coating liquid was applied to the above gas separation layer using the same gravure coater, and then it was dried in a draft at room temperature (25°C) for 4 hours to remove the solvent from the coating liquid applied to the gas separation layer. This coating and drying process was repeated to obtain the gas separation membrane of this example.

[0064] Comparative Example 3 In the first coating process, a nanofiber layer (material: PVDF, shape: nanofiber nonwoven fabric, average fiber diameter of nanofibers: 50 nm) was laminated on a porous layer (material: PET, shape: nonwoven fabric, thickness: 100 μm) of the substrate. The nanofiber layer was then coated with a coating liquid (porous polymer (cellulose (cellulose acetate (product name: L-70, Daicel Corporation, acetylation degree: 0.55 (acetylation degree means the weight percentage of bound acetic acid per unit weight))), solvent (material: THF), concentration of porous polymer: 4% by mass)) using a gravure coater equipped with a gravure roll (plate / line count: 150 L / inch).

[0065] The coating solution applied to the nanofiber layer was then dried in a fume hood at room temperature (25° C.) for 4 hours to remove the solvent from the coating solution, thereby forming a gas separation layer having an uncoated nanofiber layer.

[0066] Furthermore, in the second coating step, the same coating liquid was coated onto the uncoated nanofiber layer using the same gravure coater.

[0067] Thereafter, the coating solution was dried in a draft at room temperature (25°C) for 4 hours to remove the solvent from the coating solution applied to the uncoated nanofiber layer, forming a gas separation layer and obtaining the gas separation membrane of this example. Some of the specifications of the above examples are shown in Table 1.

[0068] [Table 1]

[0069] In Table 1, the "basis weight of the nanofiber layer" is the weight of the nanofiber nonwoven fabric per square meter. 2The weight of each layer was measured and calculated. The "thickness of the gas separation layer" was determined by cutting the gas separation membrane in the thickness direction at an arbitrary position of the gas separation membrane. The cut surface was then observed by SEM, TEM, etc., and further observed by EDS, XPS, or FT-IR as necessary, and the distance from the part in contact with the surface of the porous layer to the surface of the gas separation layer was measured at any five points. The average value of the distances at these five points was then calculated to determine the thickness of the gas separation layer. In addition, although not shown in Table 1, in each example, the contact angle of the coating liquid with respect to the nanofiber layer and the contact angle of the coating liquid with respect to the porous layer were measured and calculated by the θ / 2 method. This confirmed that the contact angle of the coating liquid with respect to the nanofiber layer (54°) was smaller than the contact angle of the coating liquid with respect to the porous layer (80°) and that the contact angle of the coating liquid with respect to the nanofiber layer was 80°, less than 90°.

[0070] [Performance evaluation] As for the permeability test, for the gas separation membrane of each of the above examples, N2 permeability measurement (first time), then O2 permeability measurement (first time), and then N2 permeability measurement (second time) were performed in that order. The permeability obtained in the first N2 permeability measurement was taken as the N2 permeability of the gas separation membrane. The results are also shown in Table 1. In addition, the permeability obtained in the first N2 permeability measurement was taken as the "N2 permeability 1" of the gas separation membrane. The same applies below.

[0071] The increase rate of permeability obtained by the following formula (1) was used as an index of strength. The results are shown in Table 1. In Table 1, "A" in "Strength" indicates that the increase rate is 3% or less, "B" indicates that the increase rate is 10% or less, and "C" indicates that the increase rate is more than 10%. Increase rate (%) = |N2 permeability 1 - N2 permeability 2| / N2 permeability 2 × 100 (1)

[0072] The "N2 permeability", "O2 permeability" and "O2 / N2 selectivity" of the gas separation membranes of the above examples were measured and calculated as follows. Specifically, the gas separation membranes were evaluated based on a differential pressure method using a stainless steel gas separation membrane module 71 shown in the left and right diagrams of FIG. 4. More specifically, as shown in the left diagram of FIG. 4, a sample 73 cut out from the gas separation membranes prepared in the examples and comparative examples was fixed between the gas supply side 75 and the permeation side 77 of the gas separation membrane module 71. Thereafter, as shown in the left diagram of FIG. 4, the inlet 75A of the gas supply side 75 was closed, and the outlet 77A of the permeation side 77 was connected to a vacuum device and evacuated to create a vacuum inside the gas separation membrane module 71. Thereafter, as shown in the right diagram of FIG. 4, a (predetermined amount) of gas (N2, O2, and a mixed gas thereof) was supplied from the inlet 75A to the supply side 75, and the time until the pressure difference with the permeation side 77 disappeared (with the inlet 75A and outlet 77A closed after the gas supply) was measured to calculate the permeation rate and permeability (permeability coefficient) of N2 and O2. Selectivity (unitless (-)) was calculated from selectivity = (permeability coefficient of O2) / (permeability coefficient of N2), and the gas permeability coefficient was calculated as permeability (unit (GPU): 1 GPU = 3.35 × 10 -10 mol m -2 ·s -1 ·Pa -1 ) was decided.

[0073] The component composition of the mixed gas was the same as that of normal air, with 79% by volume of N2 and 21% by volume of O2. The pressure (or pressure difference) between the supply side and the permeation side was continuously measured by pressure gauges installed inside the supply side 75 and the permeation side 77. Furthermore, the internal pressure for determining a vacuum was set to 0.1 MPa (or less).

[0074] More specifically, the permeation rates and permeabilities (permeability coefficients) of N2 and O2 and the selectivity based thereon were calculated using the following formulas (2) to (4).

[0075] The pressure difference over time on the permeation side is calculated using the following formula (2). Pressure difference: dP / dt=(Pe-Ps) / t (2) Here, Pe in equation (2) is the pressure on the permeation side when it reaches 0 kPa, Ps is the pressure on the permeation side at the start of measurement, and t is the time it takes to reach 0 kPa.

[0076] The gas permeation rate is calculated by the following formula (3). Transmission rate: q=V / RT dP / dt (3) In the formula (3), V is the permeation volume, R is the molar gas constant, T is the absolute temperature during the experiment, and dP / dt is the pressure difference calculated by formula (2). The temperature during the experiment was 25°C.

[0077] The transmission coefficient is calculated by the following formula (4). Transmission coefficient: P / δ=q / Ph / A (4) Here, in formula (4), q is the permeation rate, Ph is the pressure on the supply side when the gas is supplied, A is the effective area of ​​the gas separation layer, P is the permeability coefficient (Pa), and δ is the thickness of the gas separation layer (μm).

[0078] From Table 1, it can be seen that Examples 1 to 12, which are within the scope of the present invention, have superior gas permeability and strength compared to Comparative Examples 1 to 3, which are outside the scope of the present invention. Specifically, Examples 1 to 12 exhibit N2 permeability of 10 GPU or more, preferably 100 GPU or more, and the increase rate of N2 permeability associated with microscopic damage to the membrane is suppressed to 10% or less. Furthermore, by suppressing microscopic damage to the membrane, excellent gas selectivity can also be achieved.

[0079] Although the present invention has been described above with reference to some embodiments and examples, the present invention is not limited to these, and various modifications are possible within the scope of the gist of the present invention.

[0080] The present invention provides a gas separation membrane having excellent gas permeability and strength, and a method for producing the same, with a main feature that the thickness of the above-mentioned gas separation layer is 0.2 μm or more and 5.0 μm or less.

[0081] Therefore, for example, the above-mentioned components are not limited to the configurations shown in each embodiment or example, and it is possible to change the details of the specifications and materials of the gas separation layer, porous layer, etc., or to replace or combine the components of one embodiment with the components of another embodiment. [Explanation of symbols]

[0082] 1, 2 Gas separation membrane 10 Gas separation layer 10a surface 11 Gas separation inner layer 12 Gas separation surface layer 20 Porous layer 20a surface 20b back side 30 nanofiber layers 40 Coating Fluid 50 Coating fluid impregnated layer 60 Coating equipment 71 Stainless steel gas separation membrane module 73 Gas separation membrane sample 75 Gas supply side 75A Gas supply inlet 77 Gas permeation side 77A Gas permeation outlet

Claims

1. A gas separation membrane having a gas separation layer and a porous layer supporting the gas separation layer, The gas separation layer includes nanofibers made of an organic polymer and a porous polymer having a gas separation performance, The porous polymer contains at least one selected from the group consisting of intrinsic microporosity polymer, polytrimethylsilylpropyne, and polyimide; The thickness of the gas separation layer is 0.2 μm or more and 5.0 μm or less. A gas separation membrane characterized by:

2. A gas separation layer and a porous layer supporting the gas separation layer, The gas separation layer includes nanofibers made of an organic polymer and a porous polymer having a gas separation performance, The porous polymer contains at least one selected from the group consisting of intrinsic microporosity polymer, polytrimethylsilylpropyne, and polyimide; The thickness of the gas separation layer is 0.2 μm or more and 5.0 μm or less.

1. A method for producing a gas separation membrane, comprising: A coating liquid containing a porous polymer having gas separation properties and a solvent is applied to a nanofiber layer containing nanofibers made of an organic polymer formed on the porous layer, so that the coating liquid is impregnated into the nanofiber layer, and then the solvent is removed from the coating liquid. A method for producing a gas separation membrane comprising the steps of:

3. 3. The method for producing a gas separation membrane according to claim 2, wherein a contact angle of the coating liquid with respect to the nanofiber layer is smaller than a contact angle of the coating liquid with respect to the porous layer.

4. 4. The method for producing a gas separation membrane according to claim 3, wherein a contact angle of the coating liquid with respect to the nanofiber layer is less than 90°.

Citation Information

Patent Citations

  • Gas separation membrane, gas separation module, gas separation device, gas separation method, and method for producing gas separation asymmetric membrane