Adhesive sheet

The adhesive sheet addresses peel-off charging by incorporating a conductive polymer antistatic layer and release film with specific electrical resistances, ensuring transparency and strong adhesion, suitable for optical applications.

JP2024167827AInactive Publication Date: 2024-12-04OJI HLDG CORP
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023084177
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-22
Publication Date
2024-12-04
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing adhesive sheets face issues with peel-off charging when the release film is peeled off, leading to potential performance degradation of the target member due to electrification, and existing antistatic solutions compromise transparency for optical applications.

Method used

A pressure-sensitive adhesive sheet with a conductive polymer-based antistatic layer on one surface of the adhesive layer and a release film on the other, along with a base material, where the antistatic layer has a surface electrical resistance of 1.0×10^8 to 1.0×10^12 Ω/sq, and the release layer has a similar resistance, suppressing peel-off charging.

Benefits of technology

The adhesive sheet effectively suppresses peel-off charging, maintains high transparency, and ensures excellent adhesive strength, making it suitable for optical applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024167827000001
    Figure 2024167827000001
Patent Text Reader

Abstract

To provide an adhesive sheet having suppressed peeling charge.SOLUTION: There is provided an adhesive sheet which comprises a base material, an antistatic layer a, an adhesive layer and a release film, wherein the antistatic layer a is provided on one surface of the adhesive layer, the release film is provided on the other surface, the base material is provided on a surface of the antistatic layer opposite to a side of the adhesive layer, the antistatic layer a contains a conductive polymer and the surface electrical resistance of the antistatic layer is 1.0×108 to 1.0×1012 Ω / sq.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a pressure-sensitive adhesive sheet. [Background technology]

[0002] Adhesive sheets are used, for example, for bonding members (adherends) together, and are widely used in various fields, for example, in display devices such as liquid crystal displays (LCDs) and input devices such as touch panels.

[0003] A pressure-sensitive adhesive sheet usually has a pressure-sensitive adhesive layer, but if the pressure-sensitive adhesive layer is exposed, the pressure-sensitive adhesive layer may deteriorate during storage or transportation, or may stick to other materials. For this reason, the pressure-sensitive adhesive sheet is generally stored or transported with the pressure-sensitive adhesive layer protected by a release film. The release film is a film formed with a release layer, and is sometimes called a separator.

[0004] In the case of an adhesive sheet having a release film, the release film is peeled off to expose the adhesive layer, and the adhesive layer is attached to a target member (adherend). When the release film is peeled off from the adhesive sheet, peeling electrification may occur, and the adhesive layer may become charged. This electrification makes it easier for foreign matter to adhere to the adhesive layer, and when the charged adhesive layer is attached to a target member, it may also reduce the performance of the target member. For this reason, it is necessary to make the adhesive layer less likely to be charged by suppressing the peeling electrification of the adhesive sheet. From this perspective, for example, Patent Document 1 proposes a protective film with improved antistatic performance by providing an antistatic layer containing non-conductive metal oxide fine particles such as silica on an adhesive layer formed on a transparent support. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2008-087434 A Summary of the Invention [Problem to be solved by the invention]

[0006] However, as disclosed in Patent Document 1, when metal oxide fine particles are used to improve antistatic performance, the transparency of the film tends to decrease, which leaves a problem in fields such as optical applications where transparency is required. In addition, although the technology disclosed in Patent Document 1 can improve the antistatic performance of a transparent support provided with an antistatic layer, the antistatic performance of the adhesive layer side is insufficient. For this reason, for example, in a pressure-sensitive adhesive sheet in which a release film is attached to the pressure-sensitive adhesive layer, peeling electrification is likely to occur when the release film is peeled off.

[0007] The present invention has been made in view of the above, and has an object to provide a pressure-sensitive adhesive sheet in which peel-off static electricity is suppressed. [Means for solving the problem]

[0008] As a result of extensive research into achieving the above object, the present inventors have discovered that the above object can be achieved by providing a specific antistatic layer at a predetermined position, thereby completing the present invention.

[0009] That is, the present invention includes, for example, the subject matter described in the following sections. Item 1 A pressure-sensitive adhesive sheet comprising a substrate, an antistatic layer a, a pressure-sensitive adhesive layer, and a release film, the antistatic layer a is provided on one surface of the pressure-sensitive adhesive layer, and the release film is provided on the other surface of the pressure-sensitive adhesive layer; the base material is provided on the surface of the antistatic layer a opposite to the pressure-sensitive adhesive layer, The antistatic layer a contains a conductive polymer, The surface electrical resistance of the antistatic layer a is 1.0×10 8 ~1.0×10 12 Adhesive sheet with a resistance of Ω / sq. Section 2 Item 2. The pressure-sensitive adhesive sheet according to item 1, wherein an amount of peeling electrification generated when the release film is peeled off from the pressure-sensitive adhesive layer is −0.2 to 0.2 kV. Section 3 A release layer is formed on the release film, The surface electrical resistance of the release layer is 1.0×10 8 ~1.0×10 12 Item 3. The pressure-sensitive adhesive sheet according to item 1 or 2, wherein the surface area is Ω / sq. Section 4 Item 4. The pressure-sensitive adhesive sheet according to any one of items 1 to 3, wherein the pressure-sensitive adhesive layer a contains an acrylic polymer. Section 5 Item 5. The pressure-sensitive adhesive sheet according to any one of items 1 to 4, wherein the substrate is a resin film. Effect of the Invention

[0010] The pressure-sensitive adhesive sheet of the present invention is one in which peel-off static electricity is suppressed. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] Hereinafter, embodiments of the present invention will be described in detail. In this specification, the expressions "containing" and "comprise" include the concepts of "containing", "comprises", "consists essentially of" and "consists only of".

[0012] The pressure-sensitive adhesive sheet of the present invention is a pressure-sensitive adhesive sheet comprising a substrate, an antistatic layer a, a pressure-sensitive adhesive layer, and a release film, the pressure-sensitive adhesive layer having the antistatic layer a on one side thereof and the release film on the other side thereof, the substrate being provided on the side of the antistatic layer a opposite to the pressure-sensitive adhesive layer, the antistatic layer a containing a conductive polymer as an antistatic component, and the antistatic layer having a surface electrical resistance of 1.0×10 8 ~1.0×10 12 Ω / sq.

[0013] The pressure-sensitive adhesive sheet of the present invention comprises a substrate, an antistatic layer a, a pressure-sensitive adhesive layer, and a release film, and thus suppresses the generation of charge due to peeling when the release film is peeled off from the pressure-sensitive adhesive layer. Moreover, the pressure-sensitive adhesive sheet of the present invention has excellent adhesive strength and high transparency. Therefore, the pressure-sensitive adhesive sheet of the present invention can be suitably used as a protective film, a support film, etc. in various applications, and can be suitably used in optical applications in particular.

[0014] Base material The substrate is a member for supporting the pressure-sensitive adhesive layer in the pressure-sensitive adhesive sheet of the present invention. The type of substrate is not particularly limited, and for example, various films used in known pressure-sensitive adhesive sheets can be widely applied. Among them, the substrate is preferably a resin film.

[0015] Examples of the resin film include a wide range of films, such as a polyethylene terephthalate film, an acrylic film, a polycarbonate film, a polyolefin film, a triacetyl cellulose film, a cycloolefin polymer film, etc. Among these, the resin film is preferably a polyethylene terephthalate film.

[0016] The substrate may be transparent or translucent. The thickness of the substrate is not particularly limited and may be, for example, 10 to 200 μm.

[0017] Adhesive layer The adhesive layer is a layer for making the adhesive sheet exhibit adhesive performance. The type of the adhesive layer is not particularly limited, and for example, the adhesive layer used in the known adhesive sheet can be widely used in the present invention. For example, the adhesive layer is a layer mainly composed of an acrylic polymer. That is, the adhesive layer can contain an acrylic polymer.

[0018] The acrylic polymer preferably has a crosslinked structure. In this case, the adhesive strength of the pressure-sensitive adhesive sheet is likely to be increased. For example, the acrylic polymer preferably has a structure in which a crosslinkable acrylic polymer is crosslinked with a crosslinking agent described below.

[0019] The crosslinkable acrylic polymer may have a (meth)acrylic acid alkyl ester unit. In this specification, a "unit" is a repeating structural unit (also called a monomer unit) that constitutes a polymer. In this specification, "(meth)acrylic" means "acrylic" or "methacrylic", "(meth)acrylate" means "acrylate" or "methacrylate", and "(meth)allyl" means "allyl" or "methallyl".

[0020] The (meth)acrylic acid alkyl ester unit is a structural unit derived from a (meth)acrylic acid alkyl ester. Examples of the (meth)acrylic acid alkyl ester include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, t-butyl (meth)acrylate, n-pentyl (meth)acrylate, n-hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, n-octyl (meth)acrylate, isooctyl (meth)acrylate, n-nonyl (meth)acrylate, isononyl (meth)acrylate, n-decyl (meth)acrylate, isodecyl (meth)acrylate, n-undecyl (meth)acrylate, n-dodecyl (meth)acrylate, stearyl (meth)acrylate, methoxyethyl (meth)acrylate, ethoxyethyl (meth)acrylate, cyclohexyl (meth)acrylate, benzyl (meth)acrylate, and isobornyl (meth)acrylate. The (meth)acrylic acid alkyl ester unit contained in the acrylic polymer may be one type alone or may contain two or more types of units. Among them, the (meth)acrylic acid alkyl ester is preferably methyl (meth)acrylate, n-butyl (meth)acrylate, or the like.

[0021] The crosslinkable acrylic polymer may further contain one or more units selected from the group consisting of carboxyl group-containing monomer units and hydroxyl group-containing monomer units in addition to the (meth)acrylic acid alkyl ester units. In this case, the crosslinkable acrylic polymer is likely to form a crosslinked structure in the pressure-sensitive adhesive layer by reaction with a crosslinking agent described below.

[0022] The carboxyl group-containing monomer unit is a monomer unit formed by a carboxyl group-containing monomer, such as acrylic acid or methacrylic acid.

[0023] The hydroxyl group-containing monomer unit is a monomer unit formed by a hydroxyl group-containing monomer. Examples of the hydroxyl group-containing acrylic monomer include hydroxyalkyl (meth)acrylates such as 2-hydroxyethyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, and 2-hydroxypropyl (meth)acrylate, (meth)acrylic acid [(mono-, di-, or poly) alkylene glycol] such as mono(diethylene glycol) (meth)acrylate, and (meth)acrylic acid lactones such as monocaprolactone (meth)acrylate.

[0024] The crosslinkable acrylic polymer preferably contains (meth)acrylic acid alkyl ester units and hydroxyl group-containing monomer units. In this case, the pressure-sensitive adhesive layer is likely to have high transparency and adhesive strength, and peeling static electricity is also likely to be suppressed. The crosslinkable acrylic polymer may be composed only of (meth)acrylic acid alkyl ester units and hydroxyl group-containing monomer units.

[0025] The crosslinkable acrylic polymer preferably contains 50% by mass or more of (meth)acrylic acid alkyl ester units, more preferably 70% by mass or more, even more preferably 80% by mass or more, particularly preferably 90% by mass or more, and preferably 99% by mass or less, more preferably 98% by mass or less.

[0026] The crosslinkable acrylic polymer preferably contains 0.1% by mass or more of the hydroxyl group-containing monomer units, more preferably 0.5% by mass or more, even more preferably 0.8% by mass or more, and particularly preferably 1.0% by mass or more, and preferably 20% by mass or less, more preferably 15% by mass or less, and particularly preferably 10% by mass or less.

[0027] The mass average molecular weight of the crosslinkable acrylic polymer is not particularly limited, and can be, for example, 300,000 or more and 2,000,000 or less. The mass average molecular weight of the crosslinkable acrylic polymer is preferably 400,000 or more, more preferably 500,000 or more, and is preferably 1,800,000 or less, more preferably 1,600,000 or less, even more preferably 1,500,000 or less, and particularly preferably 1,300,000 or less.

[0028] The weight average molecular weight of the crosslinkable acrylic polymer is a value measured by gel permeation chromatography (GPC) and calculated in terms of standard polystyrene. The measurement conditions for gel permeation chromatography (GPC) are as follows. Solvent: Tetrahydrofuran Columns: Shodex KF801, KF803L, KF800L, KF800D (four columns made by Showa Denko Co., Ltd. were connected and used) Column temperature: 40℃ Sample concentration: 0.5% by mass Detector: RI-2031plus (JASCO) Pump: RI-2080plus (JASCO) Flow rate (flow rate): 0.8ml / min Injection volume: 10μL Calibration curve: A calibration curve using 10 samples of standard polystyrene (Shodex standard polystyrene, manufactured by Showa Denko) with Mw=1,320 to 2,500,000 is used.

[0029] The crosslinkable acrylic polymer can be produced, for example, by a known method, for example, by a polymerization reaction of a (meth)acrylic monomer. In this case, various polymerization methods can be adopted, for example, a solution polymerization method, an emulsion polymerization method, a suspension polymerization method, etc.

[0030] The pressure-sensitive adhesive layer can be formed using a pressure-sensitive adhesive composition. Such a pressure-sensitive adhesive composition can contain a crosslinkable acrylic polymer, and can also contain a crosslinking agent, a solvent, etc. The pressure-sensitive adhesive layer formed from the pressure-sensitive adhesive composition containing the crosslinkable acrylic polymer and the crosslinking agent is a layer containing an acrylic polymer having a crosslinked structure.

[0031] The type of crosslinking agent is not particularly limited, and may be any crosslinking agent used to form a known pressure-sensitive adhesive sheet. Examples of the crosslinking agent include epoxy compounds, isocyanate compounds, oxazoline compounds, aziridine compounds, metal chelate compounds, butylated melamine compounds, etc. The pressure-sensitive adhesive composition may contain one or more crosslinking agents.

[0032] Examples of epoxy compounds include ethylene glycol diglycidyl ether, polyethylene glycol diglycidyl ether, propylene glycol diglycidyl ether, polypropylene glycol diglycidyl ether, glycerin diglycidyl ether, neopentyl glycol diglycidyl ether, 1,6-hexanediol diglycidyl ether, tetraglycidylxylenediamine, 1,3-bis(N,N-diglycidylaminomethyl)cyclohexane, trimethylolpropane polyglycidyl ether, diglycerol polyglycidyl ether, polyglycerol polyglycidyl ether, sorbitol polyglycidyl ether, etc. Examples of commercially available epoxy compounds include "E-AX" manufactured by Soken Chemical Industries, Ltd.

[0033] The isocyanate compound preferably has two or more isocyanate groups, more preferably has three or more, and preferably has six or less. Examples of the isocyanate compound include polyisocyanates such as tolylene diisocyanate, isophorone diisocyanate, chlorophenylene diisocyanate, diphenylmethane diisocyanate, butylene diisocyanate, hexamethylene diisocyanate, tetramethylene diisocyanate, hydrogenated diphenylmethane diisocyanate, and xylylene diisocyanate; alicyclic isocyanates such as cyclopentylene diisocyanate and cyclohexylene diisocyanate; and aromatic isocyanates such as 2,4-tolylene diisocyanate, 2,6-tolylene diisocyanate, and 4,4'-diphenylmethane diisocyanate. The isocyanate compound may be used alone or in a mixture of two or more different types. Examples of commercially available isocyanate compounds include tolylene diisocyanate compounds (Coronate L, manufactured by Nippon Polyurethane Industry Co., Ltd.), xylylene diisocyanate compounds (Takenate D-110N, manufactured by Mitsui Chemicals, Inc.), and "Crosslinker N" manufactured by Lion Specialty Chemicals.

[0034] When the pressure-sensitive adhesive composition contains a crosslinking agent, the content ratio is not particularly limited.For example, the pressure-sensitive adhesive composition preferably contains 0.01 parts by mass or more of the crosslinking agent, more preferably contains 0.1 parts by mass or more, and even more preferably contains 0.3 parts by mass or more, and preferably contains 10 parts by mass or less, more preferably contains 5 parts by mass or less, and even more preferably contains 1 part by mass or less, based on 100 parts by weight of the crosslinking acrylic polymer.

[0035] The pressure-sensitive adhesive composition may contain a solvent, if necessary. When the pressure-sensitive adhesive composition contains a solvent, the coatability of the pressure-sensitive adhesive composition is improved, and the pressure-sensitive adhesive layer can be easily formed. Examples of the solvent include hydrocarbons such as hexane, heptane, octane, toluene, xylene, ethylbenzene, cyclohexane, and methylcyclohexane; halogenated hydrocarbons such as dichloromethane, trichloroethane, trichloroethylene, tetrachloroethylene, and dichloropropane; alcohols such as methanol, ethanol, propanol, isopropyl alcohol, butanol, isobutyl alcohol, and diacetone alcohol; ethers such as diethyl ether, diisopropyl ether, dioxane, and tetrahydrofuran; ketones such as acetone, methyl ethyl ketone, methyl isobutyl ketone, isophorone, and cyclohexanone; esters such as methyl acetate, ethyl acetate, butyl acetate, isobutyl acetate, amyl acetate, and ethyl butyrate; and polyols and derivatives thereof such as ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol monomethyl ether acetate, propylene glycol monomethyl ether, propylene glycol monoethyl ether, and propylene glycol monomethyl ether acetate.

[0036] The content of the solvent in the pressure-sensitive adhesive composition is not particularly limited, and is preferably 25 to 500 parts by mass, more preferably 30 to 400 parts by mass, relative to 100 parts by mass of the crosslinkable acrylic polymer. In addition, the content of the solvent relative to the total mass of the pressure-sensitive adhesive composition is preferably 10 to 90% by mass, more preferably 20 to 80% by mass. The pressure-sensitive adhesive composition may contain one or more solvents.

[0037] The adhesive composition may contain, as required, a tackifier, a silane coupling agent, a plasticizer, an antioxidant, a metal corrosion inhibitor, an ultraviolet absorber, a crosslinking accelerator, a crosslinking retarder, a light stabilizer such as a hindered amine compound, etc., within a range that does not impair the effects of the present invention. In addition, a dye or a pigment may be added for the purpose of coloring.

[0038] However, it is preferable that the pressure-sensitive adhesive composition does not contain an antistatic agent, that is, it is preferable that the pressure-sensitive adhesive layer does not contain an antistatic agent, which makes it easier to increase the adhesive strength of the pressure-sensitive adhesive layer.

[0039] The method for preparing the pressure-sensitive adhesive composition is not particularly limited, and for example, a wide variety of known methods for preparing pressure-sensitive adhesive compositions can be used.

[0040] The pressure-sensitive adhesive layer can be formed by curing the pressure-sensitive adhesive composition. That is, the pressure-sensitive adhesive layer can contain a cured product of the pressure-sensitive adhesive composition. Such a cured product contains a crosslinked structure obtained by crosslinking the crosslinkable acrylic polymer with a crosslinking agent.

[0041] The method for forming the adhesive layer using the adhesive composition (i.e., the method for curing the adhesive composition) is not particularly limited, and for example, known methods can be widely adopted. Among them, it is preferable to form the adhesive layer by a manufacturing method including a step of applying the adhesive composition to form a coating film and a step of heating the coating film. When the adhesive composition contains a solvent, the solvent is removed in the heating step and at the same time, the reaction between the crosslinkable acrylic polymer and the crosslinking agent proceeds to form a cured product.

[0042] The pressure-sensitive adhesive composition can be applied using a known coating device, such as an applicator, a blade coater, an air knife coater, a roll coater, a bar coater, a gravure coater, a microgravure coater, a rod blade coater, a lip coater, a die coater, or a curtain coater.

[0043] The pressure-sensitive adhesive composition can be applied directly to the area where the pressure-sensitive adhesive layer is to be formed. Thus, in the pressure-sensitive adhesive sheet of the present invention, for example, the pressure-sensitive adhesive composition can be applied onto an antistatic layer formed on a substrate, or onto the release layer side of a release film.

[0044] The thickness of the pressure-sensitive adhesive composition after coating is not particularly limited, and can be appropriately set depending on the desired thickness of the pressure-sensitive adhesive layer.

[0045] In the step of heating the coating film, the heating temperature is not particularly limited, and is preferably, for example, 50 to 150°C. This heating allows the curing reaction to proceed and removes as much volatile matter as possible, such as the solvent, from the adhesive composition. The heating time can be appropriately adjusted depending on the heating temperature, the thickness of the coating film, and the content of the solvent in the adhesive composition, and can be, for example, 1 to 60 minutes. A known heating device such as a heating furnace or an infrared lamp can be used to heat the coating film. After heating, it is preferable to carry out an aging treatment in which the adhesive sheet is left to stand at a constant temperature for a certain period of time. The aging treatment can be carried out, for example, by leaving the sheet to stand at 23°C for 7 days.

[0046] In the pressure-sensitive adhesive sheet of the present invention, the pressure-sensitive adhesive layer can have a single-layer structure, or can have a multi-layer structure in which a plurality of single-layer pressure-sensitive adhesive layers are laminated. The thickness of the pressure-sensitive adhesive layer can be appropriately set according to the application, and is not particularly limited. For example, the thickness of the pressure-sensitive adhesive layer can be 1 to 150 μm, preferably 3 to 100 μm, and more preferably 5 to 40 μm. In addition, when the pressure-sensitive adhesive layer has a multi-layer laminate structure, the thickness of the pressure-sensitive adhesive layer means the total thickness of each layer.

[0047] Antistatic layer a The antistatic layer a is a layer for imparting antistatic properties to the pressure-sensitive adhesive sheet, and is a layer provided on at least one side of the pressure-sensitive adhesive layer. In particular, in this specification, the antistatic layer a means an antistatic layer disposed between the pressure-sensitive adhesive layer and the substrate.

[0048] The antistatic layer a is a layer containing a conductive polymer as an antistatic component. The type of such conductive polymer is not particularly limited, and can be a wide variety of known conductive polymers. Examples of the conductive polymer include anionic polymers, cationic polymers, and other polymers having a π-conjugated system such as polythiophene, polyacetylene, polypyrrole, and polyaniline.

[0049] Examples of the anionic polymer include polystyrene sulfonic acid, polyvinyl sulfonic acid, polyacrylic acid, polyisoprene sulfonic acid, and polyethyl acrylate sulfonic acid. Examples of the anionic polymer include an alkali metal salt such as a sodium salt. Examples of the cationic polymer include a polymer having a quaternary ammonium cation.

[0050] The conductive polymer contained in the antistatic layer a preferably contains polystyrene sulfonic acid. The conductive polymer contained in the antistatic layer may be one type or two or more types. The antistatic layer a may be formed only from the conductive polymer.

[0051] The weight average molecular weight of the conductive polymer is not particularly limited and can be, for example, the same as the weight average molecular weight of known conductive polymers, specifically, 2,000 to 1,000,000, and preferably 5,000 to 500,000.

[0052] The method for forming the antistatic layer a is not particularly limited, and for example, a known method for forming an antistatic layer can be widely adopted. For example, the antistatic layer a can be formed using a conductive composition containing a conductive polymer. The conductive composition is not particularly limited in type as long as it contains a conductive polymer, and examples thereof include a dispersion or solution of the conductive polymer. In this case, the type of the solvent is not particularly limited, and examples thereof include water and alcohol compounds having 1 to 3 carbon atoms. In the dispersion or solution, the concentration of the conductive polymer is not particularly limited, and can be, for example, 0.1 to 5.0 mass%. The conductive composition can contain other components together with or instead of the solvent.

[0053] The conductive composition can be applied to the substrate to form a coating film of the conductive composition on the substrate, and the coating film can be obtained as an antistatic layer a. The coating method is not particularly limited, and any known coating means can be widely used. When forming the coating film, a heat treatment or the like can be appropriately performed.

[0054] The thickness of the antistatic layer a is not particularly limited as long as the desired antistatic effect is exhibited, and can be, for example, 0.1 to 2.0 μm.

[0055] The surface electrical resistance of the antistatic layer is 1.0×10 8 ~1.0×10 12 Ω / sq. (i.e. 1.0×10 8 Ω / sq. or more, 1.0×10 12 The surface electrical resistance of the antistatic layer is 1.0×10 8 If the thickness is less than 1.0×10, the adhesion to the adhesive layer is likely to decrease. 12 If the surface resistivity exceeds Ω / sq., charging is likely to occur, and it becomes difficult to suppress peeling charging. The surface resistivity of the antistatic layer is 1.2×10 8 It is preferable that the resistance is Ω / sq. or more, and 1.0×10 11 It is preferable that the resistance is 1.0×10 10 Ω / sq. or less is more preferable, and 1.0×10 9 It is more preferable that the resistance is Ω / sq. or less.

[0056] Release film The type of release film is not particularly limited, and for example, a wide variety of release films used in known pressure-sensitive adhesive sheets can be used. For example, a release laminate sheet having a release layer formed on one side of a film can be used as the release film.

[0057] Examples of the film for forming the release film include various resin films such as polyethylene terephthalate. Examples of the release layer include a layer formed of a general-purpose addition type or condensation type silicone-based release agent or a long-chain alkyl group-containing compound.

[0058] The thickness of the release film is not particularly limited and can be, for example, 38 to 100 μm.

[0059] The release layer is formed on the release film, and the surface electrical resistance of the release layer is 1.0×10 8 ~1.0×10 12 Ω / sq. (i.e. 1.0×10 8 Ω / sq. or more, 1.0×10 12 In this case, the amount of peeling electrification generated when the release film is peeled off from the adhesive sheet (adhesive layer) can be particularly reduced. The surface electrical resistance of the release layer is preferably 1×10 9 It is preferable that the resistance is Ω / sq. or more, and 1×10 11 It is preferable that the resistance is Ω / sq. or less.

[0060] The release film can have an antistatic layer. In this case, the antistatic layer can be provided between the release layer and the film in the release film, or can be provided on the opposite side of the film to the release layer. Preferably, the antistatic layer is provided between the release layer and the film. When the release film has an antistatic layer, the amount of peeling charge generated when the release film is peeled off from the adhesive sheet (adhesive layer) can be particularly reduced, and the surface electrical resistance of the release layer is likely to be in the above-mentioned range.

[0061] When the release film has an antistatic layer, the type of the antistatic layer is not particularly limited, and a wide variety of known antistatic layers can be applied. For example, the same antistatic layer as the antistatic layer a described above can also be applied to the release film.

[0062] The release film can be commercially available, and examples of such a release film include a heavy separator film that is a release-treated polyethylene terephthalate film manufactured by Toyobo Co., Ltd., and a light separator film that is a release-treated polyethylene terephthalate film manufactured by Toyobo Co., Ltd. In addition, a specific example of a release film having an antistatic layer is "75E0010KFAS" manufactured by Fujimori Kogyo Co., Ltd.

[0063] Adhesive sheet As described above, the pressure-sensitive adhesive sheet of the present invention has the antistatic layer a on one side of the pressure-sensitive adhesive layer, the release film on the other side, and the substrate on the surface of the antistatic layer a opposite to the pressure-sensitive adhesive layer. That is, the pressure-sensitive adhesive sheet of the present invention has a laminated structure in which the substrate, the antistatic layer a, the pressure-sensitive adhesive layer, and the release film are laminated in this order. In the pressure-sensitive adhesive sheet of the present invention, the surface of the release film facing the release layer is directly attached to the pressure-sensitive adhesive layer.

[0064] In the pressure-sensitive adhesive sheet of the present invention, the substrate, the antistatic layer a, the pressure-sensitive adhesive layer, and the release film can be directly laminated together without any other layers being interposed between them. Thus, for example, one side of the pressure-sensitive adhesive layer is directly laminated to the antistatic layer a, and the other side of the pressure-sensitive adhesive layer is directly laminated to the release layer of the release film. Also, the antistatic layer a is provided directly on the substrate.

[0065] The pressure-sensitive adhesive sheet of the present invention may also have an antistatic layer on the opposite side of the substrate to the pressure-sensitive adhesive layer. That is, the substrate may have antistatic layers on both sides. In this case, the pressure-sensitive adhesive sheet of the present invention can further reduce the amount of peeling charge generated when the release film is peeled off from the pressure-sensitive adhesive layer.

[0066] As described above, when an antistatic layer is provided on the opposite side of the substrate to the pressure-sensitive adhesive layer (i.e., when an antistatic layer is provided on the opposite side of the substrate to the antistatic layer a), the antistatic layer may be the same as the antistatic layer a, or may be an antistatic layer different from the antistatic layer a. It is preferable that the types of antistatic layers on both sides of the substrate are the same. Therefore, when antistatic layers are provided on both sides of the substrate, it is preferable that both antistatic layers are antistatic layers a. It is preferable that the antistatic layers on both sides of the substrate are layers containing polystyrene sulfonic acid. The thicknesses of the antistatic layers provided on both sides of the substrate may be the same or different.

[0067] One embodiment of the layer structure of the adhesive sheet of the present invention is substrate / antistatic layer a / adhesive layer / release film. Another embodiment of the layer structure of the adhesive sheet of the present invention is antistatic layer a / substrate / antistatic layer a / adhesive layer / release film. In any embodiment, the release film may have an antistatic layer, and in this case, it is preferable that an antistatic layer a is formed between the release layer in the release film and the film. In any embodiment, the release layer and the adhesive layer are bonded together.

[0068] The adhesive sheet of the present invention comprises a substrate, an antistatic layer a, an adhesive layer, and a release film, and thus generates a small amount of peeling charge when the release film is peeled off from the adhesive layer, i.e., peeling charge is unlikely to occur. Since peeling charge is unlikely to occur even when the release film is peeled off from the adhesive sheet, the adhesive layer is unlikely to be charged, and therefore adhesion of foreign matter to the adhesive layer is suppressed, and even when the adhesive layer is attached to a target member (adherend), the performance degradation of the target member is easily suppressed. Moreover, the adhesive sheet of the present invention can suppress peeling charge without containing an antistatic agent such as metal oxide fine particles as in the conventional adhesive sheet, so the transparency of the adhesive sheet is excellent, and there is no risk of the antistatic agent bleeding out from the adhesive sheet.

[0069] In the pressure-sensitive adhesive sheet of the present invention, the amount of peeling electrification generated when the release film is peeled off from the pressure-sensitive adhesive layer is preferably −0.2 to 0.2 kV (i.e., −0.2 kV or more and 0.2 kV or less), which makes the pressure-sensitive adhesive sheet of the present invention less susceptible to peeling electrification when the release film is peeled off from the pressure-sensitive adhesive layer.

[0070] The pressure-sensitive adhesive sheet of the present invention suppresses peeling static electricity, has excellent transparency, and has excellent adhesive strength, so it can be used for a variety of purposes and is particularly suitable for use as a protective film, support film, etc. for optical components.

[0071] In specifying the invention included in the present disclosure, the configurations (properties, structures, functions, etc.) described in each embodiment of the present disclosure may be combined in any manner. In other words, the present disclosure includes all subject matter consisting of all combinations of the configurations that can be combined as described in this specification. EXAMPLES

[0072] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the embodiments of these examples.

[0073] (Production Example 1-1: Acrylic Polymer A) A monomer mixture of butyl acrylate (BA) and hydroxylethyl acrylate (HEA) in a mass ratio of 95:5 was polymerized in ethyl acetate, a polymerization solvent, in the presence of AIBN (azobisisobutyronitrile), by heating to 60°C. This resulted in a solution of crosslinkable acrylic polymer A with a solid content concentration of 30% by mass. The mass average molecular weight (Mw) of the crosslinkable acrylic polymer A was 500,000.

[0074] (Production Example 1-2: Acrylic Polymer B) A solution of crosslinkable acrylic polymer B having a solid content of 30% by mass and Mw of 500,000 was obtained in the same manner as in Production Example 1-1, except that the mixed monomer was changed to a mixed monomer having a mass ratio of BA and HEA of 85:15.

[0075] (Production Example 1-3: Acrylic Polymer C) A solution of crosslinkable acrylic polymer C having a solid content of 30% by mass and Mw of 500,000 was obtained in the same manner as in Production Example 1-1, except that the mixed monomer was changed to a mixed monomer having a mass ratio of BA and HEA of 70:30.

[0076] (Production Example 2) A raw material containing 100 parts by mass of the crosslinkable acrylic polymer A obtained in Production Example 1 and 0.5 parts by mass of "E-AX" manufactured by Soken Chemical & Engineering Co., Ltd. as an epoxy crosslinking agent was added to ethyl acetate so that the concentration of the raw material became 25% by mass, and the mixture was stirred to prepare a pressure-sensitive adhesive composition.

[0077] (Production Example 3) A pressure-sensitive adhesive composition was prepared by adding raw materials containing 100 parts by mass of the acrylic polymer A obtained in Production Example 1, 0.5 parts by mass of "E-AX" manufactured by Soken Chemical & Engineering Co., Ltd. as an epoxy crosslinking agent, and 1.0 part by mass of "Colcoat PS169" manufactured by Colcoat Co., Ltd. as an antistatic agent, to ethyl acetate so that the concentration of the raw materials was 25% by mass, and stirring.

[0078] Example 1 A 1.0% by mass aqueous solution of polystyrene sulfonic acid was applied to the entire area of ​​one side of a 50 μm polyethylene terephthalate film ("U403" manufactured by Toray Industries, Inc.) as a substrate, and the entire area was treated at 100° C. to form an antistatic layer a having a thickness of 0.5 μm. The substrate thus obtained with the antistatic layer a formed on one side was designated as "substrate A". The adhesive composition obtained in Production Example 2 was applied onto the antistatic layer a of the substrate A, and uniformly coated with an applicator to form a coating film. The coating film was dried at 100° C. for 3 minutes in an air-circulating thermostatic oven to form an adhesive layer having a thickness of 25 μm. Next, the release layer side surface of a release film having a thickness of 75 μm (manufactured by Toyobo Co., Ltd.: E7002) was attached to the exposed surface of the adhesive layer, to obtain a laminate in which the substrate, the antistatic layer a, the adhesive layer, and the release film were laminated in this order as an adhesive sheet.

[0079] Example 2 A 0.5% by mass aqueous solution of polystyrene sulfonic acid was applied to the entire area of ​​both sides of a 50 μm polyethylene terephthalate film ("U403" manufactured by Toray Industries, Inc.) as a substrate, and treated at 100° C. to form an antistatic layer a having a thickness of 0.5 μm. The substrate thus obtained with the antistatic layer a formed on both sides was designated as "substrate B". The adhesive composition obtained in Production Example 2 was applied onto one of the antistatic layers a of the substrate B, and uniformly coated with an applicator to form a coating film. The coating film was dried at 100° C. for 3 minutes in an air-circulating thermostatic oven to form an adhesive layer having a thickness of 25 μm. Next, the release layer side surface of a release film having a thickness of 75 μm (manufactured by Toyobo Co., Ltd.: E7002) was attached to the exposed surface of the adhesive layer, to obtain a laminate having the antistatic layer a, substrate, antistatic layer a, adhesive layer, and release film laminated in this order as an adhesive sheet.

[0080] Example 3 The adhesive composition obtained in Production Example 2 was applied onto one of the antistatic layers a of the substrate B prepared in Example 2, and the coating was uniformly applied with an applicator to form a coating film. The coating film was dried at 100°C for 3 minutes in an air-circulating thermostatic oven to form an adhesive layer having a thickness of 25 μm. Next, the release layer side surface of an antistatic release film (manufactured by Fujimori Kogyo Co., Ltd.: 75E0010KFAS) having a thickness of 75 μm was attached to the exposed surface of the adhesive layer to obtain a laminate in which the antistatic layer a, substrate, antistatic layer a, adhesive layer, and antistatic release film were laminated in this order as an adhesive sheet. The antistatic release film used was one in which the release layer, antistatic layer (polystyrene sulfonic acid), and film were formed in this order.

[0081] Example 4 A laminate having a substrate, an antistatic layer a, an adhesive layer and a release film laminated in this order was obtained as an adhesive sheet in the same manner as in Example 1, except that a 0.5 mass% aqueous polythiophene solution was used instead of the aqueous polystyrene sulfonic acid solution.

[0082] Comparative Example 1 A laminate having a substrate, a pressure-sensitive adhesive layer and a release film laminated in this order was obtained as a pressure-sensitive adhesive sheet in the same manner as in Example 1, except that an antistatic layer was not provided on the substrate.

[0083] Comparative Example 2 A 0.5% by mass aqueous solution of polystyrene sulfonic acid was applied to the entire area of ​​one side of a 50 μm polyethylene terephthalate film ("U403" manufactured by Toray Industries, Inc.) as a substrate, and the entire area was treated at 100° C. to form an antistatic layer having a thickness of 0.5 μm. The substrate having an antistatic layer formed on one side thus obtained was designated as "Substrate C". The adhesive composition obtained in Production Example 2 was applied to the surface of the substrate C on which the antistatic layer was not formed, and uniformly coated with an applicator to form a coating film. The coating film was dried at 100° C. for 3 minutes in an air-circulating thermostatic oven to form an adhesive layer having a thickness of 25 μm. Next, a release film having a thickness of 75 μm (manufactured by Toyobo Co., Ltd.: E7002) was attached to the exposed surface of the adhesive layer, and a laminate having an antistatic layer, a substrate, an adhesive layer, and a release film laminated in this order was obtained as an adhesive sheet.

[0084] Comparative Example 3 A laminate having a colloidal silica-containing antistatic layer, a substrate, an adhesive layer and a release film laminated in this order was obtained as an adhesive sheet in the same manner as in Comparative Example 2, except that a colloidal silica dispersion having a concentration of 20% by mass ("Snowtex N" manufactured by Nissan Chemical Industries, Ltd.) was used instead of the aqueous solution of polystyrene sulfonic acid.

[0085] Comparative Example 4 A laminate having a substrate, a colloidal silica-containing antistatic layer, an adhesive layer and a release film laminated in this order was obtained as an adhesive sheet in the same manner as in Example 1, except that a colloidal silica dispersion having a concentration of 20% by mass ("Snowtex N" manufactured by Nissan Chemical Industries, Ltd.) was used instead of the aqueous solution of polystyrene sulfonic acid.

[0086] (Reference example 1) A laminate comprising a substrate, an antistatic agent-containing adhesive layer, and a release film laminated in this order was obtained as an adhesive sheet in the same manner as in Comparative Example 1, except that the adhesive composition obtained in Production Example 3 was used instead of the adhesive composition obtained in Production Example 2.

[0087] (Evaluation method) <Surface electrical resistance> The surface electrical resistance was measured using a resistivity meter (Mitsubishi Chemical Analytical, Hiresta MCP-HT800 type) in accordance with JIS-K-6911 under an atmosphere of temperature 23°C and humidity 50% RH. The measurement sample was left to stand for 60 minutes in an environment of 23°C x 50% RH.

[0088] <Amount of charge from peeling off> The pressure-sensitive adhesive sheets obtained in each Example and Comparative Example were previously destaticized, cut to a size of 70 mm wide and 130 mm long, and placed on a horizontal surface in an environment of 23° C. and 50% RH with the release film positioned on the upper side. The release film of this pressure-sensitive adhesive sheet was peeled off at a peeling angle of 90° and a peeling speed of 300 mm / min, and the charged voltage on the pressure-sensitive adhesive layer side of the substrate generated during this peeling was measured with an electrostatic potential meter (Shishido Electrostatic Corporation, STATIRON DZ4) fixed at a position 30 mm away, and the amount of charge from peeling was measured.

[0089] <Adhesive strength of adhesive sheet to glass> The adhesive strength was measured according to the method described in JIS Z 0237. First, the obtained adhesive sheet was cut to a size of 25 mm wide and 50 mm long, the release film was peeled off from the adhesive sheet, and the exposed adhesive layer side was attached to soda glass and pressed with a 2 kg roller. Then, 24 hours after pressing, the adhesive strength was measured at a peeling speed of 300 mm / min, and this adhesive strength was defined as the adhesive strength to glass.

[0090] [Table 1]

[0091] From Table 1, it is clear that the adhesive sheet having a substrate (resin film), an antistatic layer a containing a conductive polymer, an adhesive layer, and a release film, such as the adhesive sheets obtained in each Example, suppresses peeling electrification and has excellent transparency and adhesive performance. On the other hand, the adhesive sheet obtained in the comparative example had a large peeling electrification amount because the antistatic layer a was not formed at least between the adhesive layer and the substrate. In Reference Example 1, the adhesive layer contains an antistatic agent, so peeling electrification is suppressed, but the adhesive strength is insufficient.

Claims

1. A pressure-sensitive adhesive sheet comprising a substrate, an antistatic layer a, a pressure-sensitive adhesive layer, and a release film, the antistatic layer a is provided on one surface of the pressure-sensitive adhesive layer, and the release film is provided on the other surface of the pressure-sensitive adhesive layer; the base material is provided on the surface of the antistatic layer a opposite to the pressure-sensitive adhesive layer, The antistatic layer a contains a conductive polymer, The surface electrical resistance of the antistatic layer a is 1.0×10 8 ~1.0 x 10 12 An adhesive sheet having a surface area of ​​Ω / sq.

2. 2. The pressure-sensitive adhesive sheet according to claim 1, wherein the amount of peeling charge generated when the release film is peeled off from the pressure-sensitive adhesive layer is −0.2 to 0.2 kV.

3. A release layer is formed on the release film, The surface electrical resistance of the release layer is 1.0×10 8 ~1.0 x 10 12 The pressure-sensitive adhesive sheet according to claim 1 or 2, wherein the surface tension is Ω / sq.

4. The pressure-sensitive adhesive sheet according to claim 1 , wherein the pressure-sensitive adhesive layer contains an acrylic polymer.

5. The pressure-sensitive adhesive sheet according to claim 1 , wherein the substrate is a resin film.

Citation Information

Patent Citations

  • Surface protecting film

    JP2008087434A