Laminate sheet and production method of the same, printed matter, and molding

A laminated sheet with a methacrylic resin base and styrene copolymer surface layer addresses ink adhesion and machinability issues, ensuring high transparency and sustainability through controlled triad chain ratios and recycled material usage.

JP2024167952AActive Publication Date: 2024-12-05KURARAY CO LTD
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
JP2023084294
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-23
Publication Date
2024-12-05
Estimated Expiration
2043-05-23

AI Technical Summary

Technical Problem

Methacrylic resins exhibit poor ink adhesion with UV curable inks and styrenic copolymers with aromatic rings cause odor and poor laser machinability due to evaporated gas, while laminated sheets with methacrylic and styrene copolymers have compatibility issues leading to reduced transparency.

Method used

A laminated sheet with a base layer of methacrylic resin and a surface layer of styrene copolymer, specifically a binary copolymer with controlled triad chain ratios, ensuring good ink adhesion and laser machinability, and allowing for the use of recycled materials.

Benefits of technology

The laminated sheet achieves excellent ink adhesion, laser machinability, and sustainability by minimizing odor and maintaining transparency, even with recycled materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024167952000001_ABST
    Figure 2024167952000001_ABST
Patent Text Reader

Abstract

To provide a laminate sheet good in ink adhesion and laser machinability, and excellent in sustainability.SOLUTION: A laminate sheet (16X) has a substrate layer (21), and a surface layer (31) laminated on at least a single side of the substrate layer (21), where the substrate layer (21) includes a methacrylic resin (M) including 80 mass% or more of a methyl methacrylate unit, the surface layer (31) includes a styrenic copolymer (SX) which is a binary copolymer of a styrenic monomer unit (S) and another monomer unit (X), and the styrenic copolymer (SX) has a ratio of a triad chain (SSS) of 0 to 40 mol%, and a ratio of a triad chain (XSX) of 5 to 34 mol% to 100 mol% of a total of the triad chain (SSS), a triad chain (XSS), and the triad chain (XSX).SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a laminated sheet, a manufacturing method thereof, a printed matter, and a molded article. [Background technology]

[0002] Inkjet printing, which can process digital images on a print medium using a computer, is becoming more and more popular as more types of printable media are being used. For example, it is now widely used in a variety of fields, including printing, advertising, sign displays, events, amusement, architecture, and interior design. Resin sheets are an example of a printing medium other than paper. Unlike paper, resin sheets are highly water-resistant and durable, and can also be made transparent. After inkjet printing, the resin sheet for inkjet printing can be cut using a laser and an NC router, etc., as necessary, to form it into a desired shape. The molded product thus obtained can be preferably used for miscellaneous goods and fixtures such as key holders. A method for cutting a resin sheet using a laser is disclosed in claim 1 of Patent Document 1, for example. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2016-055348 A [Patent Document 2] JP 2018-94843 A [Patent Document 3] JP 2021-160119 A Summary of the Invention [Problem to be solved by the invention]

[0004] In applications such as miscellaneous goods and fixtures such as key holders, methacrylic resins are preferably used as the base resin of the resin sheet for inkjet printing from the viewpoints of transparency and ink color development. As the ink for inkjet printing, ultraviolet (UV) curable inks and the like are preferably used. However, methacrylic resins tend not to have good adhesion to inkjet printing inks such as UV curable inks. Examples of components that have good adhesion to inkjet printing inks such as UV curable inks include styrene copolymers.

[0005] In general, in laser cutting, depending on the material of the workpiece, when the workpiece is melted and evaporated by the irradiation of laser light, the evaporated gas may cause an unpleasant odor or smoke. In addition, after the laser cutting is completed, when the melted part cools and solidifies again, the evaporated gas may adhere to the cut surface, resulting in poor appearance of the cut surface. Methacrylic resins are less likely to cause the above problems due to evaporated gas (unpleasant odor or smoke due to evaporated gas, and poor appearance of the cut surface due to the adhesion of evaporated gas), and tend to have good laser cutting processability. In contrast, styrene copolymers having an aromatic ring structure in the molecule are more likely to cause the above problems due to evaporated gas (unpleasant odor or smoke due to evaporated gas, and poor appearance of the cut surface due to the adhesion of evaporated gas), and tend to have poor laser cutting processability.

[0006] Patent Documents 2 and 3 disclose a laminate sheet having a base layer containing a methacrylic resin and a surface layer containing a styrene copolymer such as a methyl methacrylate-styrene copolymer (MS resin), and having good ink adhesion and laser cutting processability (Claim 1 in Patent Document 2, Claim 1 in Patent Document 3). This laminate sheet can be preferably produced by coextrusion molding.

[0007] In general, in the production of (co)extrusion molded sheets and molded products using the same, there are defective products that arise when the extrusion molding production line is started up, scraps generated by trimming both ends of the sheet, defective products that are determined not to meet product standards in quality inspections for defects and foreign bodies, and scraps generated by cutting the sheet. In recent years, efforts toward a sustainable society have been progressing, and it is preferable to effectively reuse the above-mentioned defective products and scraps as rework materials rather than disposing of them.

[0008] In the laminated sheets disclosed in Patent Documents 2 and 3, it is considered that a laminated sheet manufactured in the past containing a methacrylic resin and a styrene copolymer such as MS resin is used as a base layer material as a rework material. However, in general, a styrene copolymer such as MS resin is not compatible with a methacrylic resin, and there is a refractive index difference between these resins, so that a laminated sheet using the above-mentioned rework material as a base layer material may have a low transparency and become cloudy. In fact, Patent Document 3 describes that "in order to suppress the occurrence of cloudiness and maintain transparency, the styrene content in the base layer is preferably 1 mass% or less, more preferably 0.85 mass% or less" (paragraph 0171). In Patent Document 3, the preferred styrene content in the base layer is very low. In addition, this document does not disclose an example in which a laminated sheet manufactured in the past containing a methacrylic resin and a styrene copolymer such as MS resin is used as a rework material. It is preferable to be able to use more rework material as a base layer material.

[0009] The present disclosure has been made in consideration of the above-mentioned problems, and aims to provide a laminate sheet that has good ink adhesion and laser cutting processability and is highly sustainable. [Means for solving the problem]

[0010] The present disclosure provides the following laminate sheets [1] to

[14] , a manufacturing method thereof, a printed matter, and a molded article. [1] A laminated sheet having a base layer and a surface layer laminated on at least one side of the base layer, The base layer contains a methacrylic resin (M) containing 80% by mass or more of methyl methacrylate units, The surface layer contains a styrene-based copolymer (SX) which is a binary copolymer of a styrene-based monomer unit (S) and another monomer unit (X), Styrene copolymer (SX) is measured under the following conditions: Measurement mode: Inverse gated decoupling method 13 When the ratios of the triad chain (SSS) of a styrene-based monomer unit (S)-styrene-based monomer unit (S), the triad chain (XSS) of another monomer unit (X)-styrene-based monomer unit (S)-styrene-based monomer unit (S), and the triad chain (XSX) of another monomer unit (X)-styrene-based monomer unit (S)-another monomer unit (X) are determined from the C-NMR spectrum, the ratio of the triad chain (SSS) is 0 to 40 mol% and the ratio of the triad chain (XSX) is 5 to 34 mol% relative to the total of the triad chain (SSS), the triad chain (XSS), and the triad chain (XSX) being 100 mol%. Laminated sheet.

[0011] [2] The laminate sheet of [1], wherein the styrene copolymer (SX) is one or more styrene copolymers selected from the group consisting of acrylonitrile-styrene copolymer (AS) and styrene-maleic anhydride copolymer (SMA). [3] The laminate sheet of [2], wherein the styrene-based copolymer (SX) is one or more styrene-based copolymers selected from the group consisting of acrylonitrile-styrene copolymers (AS) containing 70 to 95% by mass of styrene units and styrene-maleic anhydride copolymers (SMA) containing 60 to 95% by mass of styrene units.

[0012] [4] The laminate sheet according to any one of [1] to [3], wherein the average styrene-based monomer unit concentration in the entire laminate sheet is 0.1 to 20 mass %. [5] The laminate sheet according to any one of [1] to [4], wherein the base layer is made of a methacrylic resin composition (MR) containing a methacrylic resin (M) and a styrene copolymer (SX). [6] The laminate sheet according to any one of [1] to [5], wherein a concentration of a styrene-based monomer unit in the base layer is 0 to 10.0 mass %. [7] The laminate sheet according to [6], wherein the concentration of styrene-based monomer units in the base layer is 1.2 to 10.0 mass %.

[0013] [8] The laminate sheet of [5], wherein at least a portion of the total raw materials of the base material layer is a recycled resin composition (R) consisting of pulverized material of the laminate sheet produced in the past or a processed product of the pulverized material. [9] The laminate sheet according to any one of [1] to [8], wherein the laminate sheet has a total thickness of 1 to 10 mm.

[10] A laminate sheet according to any one of [1] to [9], which is for inkjet printing and / or laser cutting.

[11] A laminate sheet of any one of [1] to

[10] , which is a coextrusion molding sheet.

[0014]

[12] A printed matter, obtained by subjecting the surface layer of the laminate sheet according to any one of [1] to

[11] to inkjet printing.

[13] A molded product obtained by applying inkjet printing and laser cutting to any of the laminated sheets [1] to

[11] .

[14] A method for producing a laminate sheet according to [5], comprising co-extrusion molding the laminate sheet using a recycled resin composition (R) consisting of pulverized material of the laminate sheet previously produced or a processed product of the pulverized material, as at least a portion of the total raw material of the base material layer. Effect of the Invention

[0015] According to the present disclosure, it is possible to provide a laminate sheet that has good ink adhesion and laser cutting processability and is highly sustainable. [Brief description of the drawings]

[0016] [Figure 1] 1 is a schematic cross-sectional view of a laminate sheet according to a first embodiment of the present invention. [Diagram 2] FIG. 4 is a schematic cross-sectional view of a laminate sheet according to a second embodiment of the present invention. [Diagram 3] 1 is a schematic diagram of a laminated sheet manufacturing apparatus according to an embodiment of the present invention. [Figure 4] Measurement mode: This is an example of a 13C-NMR spectrum of a styrene copolymer (SX) measured under the inverse gated decoupling method. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0017] [Laminated sheet] The laminate sheet of the present disclosure has a base layer and a surface layer laminated on at least one side of the base layer. The base layer contains a methacrylic resin (M) containing 80 mass% or more of methyl methacrylate (MMA) units, and the surface layer contains a styrene copolymer (SX) which is a binary copolymer of a styrene monomer unit (S) and another monomer unit (X). The laminate sheet of the present disclosure is suitable for inkjet printing and / or laser cutting.

[0018] The laminated structure of the laminated sheet of the present disclosure may be a two-layer structure having a surface layer on one side of the base layer of the first embodiment shown in FIG. 1. In the figure, reference numeral 16X denotes the laminated sheet, reference numeral 21 denotes the base layer, and reference numeral 31 denotes the surface layer. The laminated sheet of the present disclosure may include any layer other than the base layer and the surface layer as necessary. However, the surface 31S of the surface layer 31 opposite the base layer does not have any other layer thereon and is an exposed surface. This exposed surface may be a printing surface on which printing is performed.

[0019] The laminated structure of the laminated sheet of the present disclosure may be a three-layer structure having surface layers on both sides of the base layer of the second embodiment shown in FIG. 2. In the figure, reference numeral 16Y denotes a laminated sheet, reference numeral 21 denotes a base layer, reference numeral 32 denotes a first surface layer, and reference numeral 33 denotes a second surface layer. The second laminated sheet of the present disclosure may include any other layer other than the base layer and the surface layer, as necessary. However, the surface 32S of the first surface layer 32 opposite the base layer and / or the surface 33S of the second surface layer 33 opposite the base layer have no other layer thereon and are exposed surfaces. This exposed surface may be a printing surface on which printing is applied. In a three-layer laminated sheet, the thickness and composition of the two surface layers may be the same or different.

[0020] The laminated sheet of the present disclosure is suitable as a resin sheet for inkjet printing. Examples of inkjet printing methods include an electrostatic suction method, a method in which a piezoelectric element such as a piezo element is used to apply mechanical vibration or displacement to ink, a method in which ink is heated to foam and the resulting pressure is utilized, and a method in which ultraviolet (UV) curable ink is used. The laminate sheet of the present disclosure can be inkjet printed on the surface layer. The laminate sheet of the present disclosure can also be cut using a laser, an NC router, or the like, as necessary, after inkjet printing, to form into a desired shape. The molded product thus obtained can be preferably used for miscellaneous goods and fixtures such as key holders. In such applications, a UV-curable ink or the like is preferably used as the inkjet printing ink.

[0021] In general, styrene copolymers having an aromatic ring structure in the molecule have good permeability and good adhesion to inkjet printing inks such as UV-curable inks. However, styrene copolymers having an aromatic ring structure do not have good laser cutting processability, and when the resin melts and evaporates due to laser light irradiation, the evaporated gas may cause an unpleasant odor or smoke. In addition, when the melted part cools and solidifies again after the laser cutting process is completed, the evaporated gas may adhere to the cut surface, causing a poor appearance of the cut surface. Methacrylic resins (M) generally suppress the above problems caused by evaporated gas (unpleasant odor or smoke caused by evaporated gas, and poor appearance of the cut surface caused by adhesion of evaporated gas) and have good laser cutting processability. However, they tend to have poor permeability for inkjet printing inks such as UV-curable inks, and poor adhesion for inkjet printing inks.

[0022] The laminate sheet of the present disclosure has a surface layer containing a styrene-based copolymer (SX) having an aromatic ring structure in the molecule, and therefore has good permeability to inkjet printing inks such as UV-curable inks and good adhesion to inkjet printing inks. The laminate sheet of the present disclosure has a laminated structure of a base layer containing a methacrylic resin (M) and a surface layer containing a styrene copolymer (SX), and the proportion of styrene monomer units in the entire laminate sheet is reduced, thereby suppressing the above-mentioned problems caused by evaporated gas during laser cutting (unpleasant odor or smoke caused by evaporated gas, and poor appearance of the cut surface caused by adhesion of evaporated gas) and improving laser cutting processability.

[0023] In the laminate sheet of the present disclosure, the ratio of the total thickness of the surface layer to the total thickness of the laminate sheet is not particularly limited, and is preferably 1 to 20%. The lower limit is more preferably 2%, and particularly preferably 3%. The upper limit is more preferably 15%, and particularly preferably 10%. When the ratio of the total thickness of the surface layer is equal to or greater than the above lower limit, the thickness of the surface layer containing the styrene copolymer (SX) is sufficiently ensured, and good ink adhesion can be ensured. In addition, when the ratio of the total thickness of the surface layer is equal to or less than the above upper limit, the ratio of the styrene monomer unit in the entire laminate sheet can be reduced, and unpleasant odors or smoke due to evaporated gas during laser cutting and poor appearance of the cut surface due to adhesion of evaporated gas can be suppressed.

[0024] In this specification, the "average styrene monomer unit concentration in the entire laminate sheet" refers to the ratio of the total mass of the styrene monomer units in the laminate sheet to the total mass of the laminate sheet. This average styrene monomer unit concentration is not particularly limited, and is preferably 0.1 to 20 mass%. The lower limit is more preferably 0.5 mass%, particularly preferably 1.0 mass%, and most preferably 2.0 mass%. The upper limit is more preferably 15 mass%, particularly preferably 10 mass%. When the average styrene monomer unit concentration in the entire laminate sheet is equal to or higher than the lower limit, good ink adhesion can be ensured, and when it is equal to or lower than the upper limit, odor or smoke due to evaporated gas during laser cutting and poor appearance of the cut surface due to adhesion of evaporated gas can be suppressed.

[0025] In the laminate sheet of the present disclosure, the total thickness of the laminate sheet is not particularly limited, and is preferably 1 to 10 mm, more preferably 1 to 5 mm, in order to improve inkjet printability and laser cutting processability. For example, when the total thickness of the laminate sheet is 3 mm, the thickness of the base layer is preferably 2.4 to 2.9 mm, the thickness of one surface layer is preferably 50 to 200 μm, and the total thickness of the surface layers is preferably 50 to 400 μm.

[0026] The haze value of the 3.0 mm thick monolayer molded sheet of the pulverized laminate sheet of the present disclosure is not particularly limited, and is preferably 5% or less, more preferably 4% or less, even more preferably 3% or less, particularly preferably 2% or less, and most preferably 1% or less. The haze value of the monolayer molded sheet can be realized by using a styrene copolymer (SX) having good compatibility with the methacrylic resin (M) as the styrene copolymer contained in the surface layer. If the haze value of the monolayer molded sheet is 5% or less, the laminate sheet of the present disclosure having excellent transparency can be manufactured using a recycled resin composition (R) consisting of a pulverized laminate sheet of the present disclosure manufactured in the past or a processed product of the pulverized product as at least a part of the total raw material of the base layer. The laminate sheet of the present disclosure having the above characteristics can be used as a rework material or can contain a rework material, and is excellent in sustainability. In this specification, unless otherwise specified, "transparent" is defined as a haze value of 5% or less.

[0027] The laminated sheets of the present disclosure are preferably coextruded sheets. A 3.0 mm thick single-layer molded sheet of the pulverized laminate sheet of the present disclosure can be obtained by a known method, for example, as follows. The laminated sheet of the present disclosure is pulverized using a known resin pulverizer. The pulverized material obtained is melt-kneaded using an extruder and a kneading / extrusion tester ("Labo Plastomill (registered trademark)" manufactured by Toyo Seiki Seisakusho) to obtain a uniform resin composition. The molten kneaded material obtained is molded by a known method such as hot press molding to obtain a single-layer molded sheet having a thickness of 3.0 mm. The melt-kneading temperature and molding temperature in molding the monolayer molded sheet are preferably within the range of suitable melt-kneading temperatures of the base layer material when molding (preferably co-extrusion molding) the laminated sheet of the present disclosure, and may be, for example, the maximum temperature in the extruder used for melt-kneading the base layer material when molding (preferably co-extrusion molding) the laminated sheet of the present disclosure. The melt-kneading temperature and molding temperature in molding the monolayer molded sheet are preferably 190 to 280°C, more preferably 210 to 270°C, particularly preferably 230 to 260°C, and for example, 240 to 250°C.

[0028] (Surface layer) The surface layer contains one or more styrene copolymers (SX) which are binary copolymers of styrene monomer units (S) and other monomer units (X). Examples of the styrene monomer units (S) contained in the styrene copolymers (SX) include styrene, α-methylstyrene, o-, m- or p-methylstyrene, and combinations thereof, with styrene being preferred. As described above, in the present disclosure, the styrene copolymer (SX) having good compatibility with the methacrylic resin (M) is used as the styrene copolymer.

[0029] Styrene-based copolymers (SX) include triad chains (SSS) of styrene-based monomer unit (S)-styrene-based monomer unit (S), triad chains (XSS) of other monomer units (X)-styrene-based monomer unit (S)-styrene-based monomer unit (S), and triad chains (XSX) of other monomer units (X)-styrene-based monomer unit (S)-other monomer units (X). The ratio of each triad chain is measured under the following conditions: Measurement mode: Inverse gated decoupling method. 13 It can be determined from the C-NMR spectrum.

[0030] In the laminate sheet of the present disclosure, from the viewpoint of compatibility with the methacrylic resin (M), a styrene-based copolymer (SX) is used in which the ratio of triad chains (SSS) is 0 to 40 mol % and the ratio of triad chains (XSX) is 5 to 34 mol % relative to a total of 100 mol % of triad chains (SSS), triad chains (XSS) and triad chains (XSX).

[0031] The lower limit of the ratio of triad sequences (SSS) is preferably 10 mol%, more preferably 15 mol%. The upper limit of the ratio of triad sequences (SSS) is preferably 37 mol%, more preferably 35 mol%. The lower limit of the ratio of triad linkages (XSX) is preferably 10 mol%, more preferably 15 mol%, particularly preferably 20 mol%. The upper limit of the ratio of triad linkages (XSX) is preferably 32 mol%, more preferably 30 mol%. The ratio of triad chains (XSS) is not particularly limited, and is preferably 40 to 80 mol%. The lower limit of the ratio of triad chains (XSS) is more preferably 50 mol%, and particularly preferably 55 mol%. The upper limit of the ratio of triad chains (XSS) is more preferably 75 mol%, and particularly preferably 70 mol%.

[0032] The other monomer unit (X) contained in the styrene copolymer (SX) is not particularly limited. The styrene copolymer (SX) may be one or more styrene copolymers selected from the group consisting of acrylonitrile-styrene copolymer (AS resin), styrene-maleic anhydride copolymer (SMA resin), and methyl methacrylate-styrene copolymer (MS resin). Among them, one or more styrene copolymers selected from the group consisting of acrylonitrile-styrene copolymer (AS resin) and styrene-maleic anhydride copolymer (SMA resin) are preferred because of their excellent compatibility with the methacrylic resin (M).

[0033] From the viewpoint of compatibility with the methacrylic resin (M), the styrene unit concentration in the AS resin is preferably 70 to 95% by mass. The lower limit is more preferably 73% by mass, and particularly preferably 75% by mass. The upper limit is more preferably 90% by mass, particularly preferably 88% by mass, and most preferably 85% by mass. Commercially available AS resins include "LiTac-A100PCF" and "120PCF" manufactured by Nippon A&L Co., Ltd.; "Sunrex SAN-C", "SAN-R", and "SAN-H" manufactured by Techno UMG; "Denka ASAS-C-800" and "AS-C-820" manufactured by Denka Co., Ltd.; "Toyolac" manufactured by Toray Industries, Inc.; and "Cevian N" manufactured by Daicel Miraize Co., Ltd. When the styrene copolymer (SX) is an acrylonitrile-styrene copolymer (AS resin), the styrene monomer unit (S) is a styrene unit, and the other monomer unit (X) is an acrylonitrile unit. In the present disclosure, as the styrene copolymer (SX), an AS resin having a ratio of triad chains (SSS) of 0 to 40 mol% and a ratio of triad chains (XSX) of 5 to 34 mol% can be preferably used.

[0034] From the viewpoint of compatibility with the methacrylic resin (M), the styrene unit concentration in the styrene-maleic anhydride copolymer (SMA resin) is preferably 60 to 95% by mass. The lower limit is more preferably 65% ​​by mass, particularly preferably 70% by mass, and most preferably 75% by mass. The upper limit is more preferably 90% by mass, particularly preferably 85% by mass, and most preferably 80% by mass. Commercially available SMA resins include "XIRAN" and "XIBOND" manufactured by Polyscope; "SMA-700" manufactured by Jiaxing Huawen Chemical; and "SAM-020" manufactured by Fine-blend Polymer. When the styrene copolymer (SX) is a styrene-maleic anhydride copolymer (SMA resin), the styrene monomer unit (S) is a styrene unit, and the other monomer unit (X) is a maleic anhydride unit. In the present disclosure, as the styrene copolymer (SX), an SMA resin having a ratio of triad chains (SSS) of 0 to 40 mol% and a ratio of triad chains (XSX) of 5 to 34 mol% can be preferably used.

[0035] Methyl methacrylate-styrene copolymer (MS resin) can be used in small amounts because it is compatible with the methacrylic resin (M). When using a methyl methacrylate-styrene copolymer (MS resin), it is preferable to use it in combination with a styrene copolymer that has excellent compatibility with the methacrylic resin (M), such as an acrylonitrile-styrene copolymer (AS resin), a styrene-maleic anhydride copolymer (SMA resin), or a styrene-maleic anhydride-methyl methacrylate copolymer (SMM resin). The amount of methyl methacrylate-styrene copolymer (MS resin) in the surface layer is preferably 0 to 1.5 mass%, more preferably 0 to 1.2 mass%, particularly preferably 0 to 1.0 mass%, and most preferably 0 to 0.85 mass%. From the viewpoint of compatibility with the methacrylic resin (M), the styrene unit concentration in the methyl methacrylate-styrene copolymer (MS resin) is preferably 35 to 50 mass%. The upper limit is more preferably 45 mass%. Commercially available MS resins include "Toyo MS MS600" manufactured by Toyo Styrene Co., Ltd.; "Denka TX Polymer TX-100S" manufactured by Denka Co., Ltd.; and "Cevian NAS" manufactured by Daicel Miraize Co., Ltd. When the styrene copolymer (SX) is a methyl methacrylate-styrene copolymer (MS resin), the styrene monomer unit (S) is a styrene unit, and the other monomer unit (X) is a methyl methacrylate unit. In the present disclosure, as the styrene copolymer (SX), an MS resin having a ratio of triad chains (SSS) of 0 to 40 mol% and a ratio of triad chains (XSX) of 5 to 34 mol% can be used.

[0036] Acrylonitrile-butadiene-styrene copolymer (ABS resin), methyl methacrylate-butadiene-styrene copolymer (MBS resin), and high impact polystyrene graft-copolymerized with butadiene (HIPS resin) are not preferably used as the styrene copolymer because they have poor compatibility with the methacrylic resin (M). The laminate sheet of the present disclosure is a binary copolymer of a styrene-based monomer unit (S) and another monomer unit (X), and preferably does not contain any styrene-based copolymer other than the styrene-based copolymer (SX) having a ratio of triad chains (SSS) of 0 to 40 mol% and a ratio of triad chains (XSX) of 5 to 34 mol%.

[0037] Within the range where the haze value of a 3.0 mm thick single-layer molded sheet of the pulverized laminate sheet of the present disclosure is 5% or less, the surface layer may contain one or more methacrylic resins (M) and / or one or more other acrylic resins (A) other than the methacrylic resin (M) as necessary. Examples of the optional other acrylic resins (A) are the same as those of the base layer. The methacrylic resin (M) in the surface layer may be the same or different from the methacrylic resin (M) in the base layer. The same applies to the optional other acrylic resins (A).

[0038] Within the range where the haze value of a 3.0 mm thick monolayer molded sheet of the pulverized laminate sheet of the present disclosure is 5% or less, the surface layer may contain one or more other polymers other than the styrene copolymer (SX), methacrylic resin (M), and other acrylic resin (A) as necessary. The other polymers are not particularly limited, and include other thermoplastic resins such as polyolefins such as polyethylene and polypropylene, polyamide, polyphenylene sulfide, polyether ether ketone, polyester, polysulfone, polyphenylene oxide, polyimide, polyetherimide, and polyacetal; and thermosetting resins such as phenolic resin, melamine resin, silicone resin, and epoxy resin. The content of the other polymers in the surface layer is preferably 10% by mass or less, more preferably 5% by mass or less, and particularly preferably 2% by mass or less. The surface layer may not contain other polymers other than the styrene copolymer (SX), methacrylic resin (M), and other acrylic resin (A).

[0039] The surface layer may contain various additives as necessary within a range that satisfies the characteristic that the haze value of a 3.0 mm thick single-layer molded sheet of the pulverized laminate sheet of the present disclosure is 5% or less. Examples of additives include colorants, antioxidants, heat deterioration inhibitors, ultraviolet absorbers, light stabilizers, lubricants, release agents, polymer processing aids, antistatic agents, flame retardants, light diffusing agents, matting agents, rubber components (impact resistance modifiers) such as core-shell particles and block copolymers, and fluorescent materials. The content of the additives can be appropriately set within a range that does not impair the effects of the present invention. For example, the content of the antioxidant is preferably 0.01 to 1 part by mass, the content of the ultraviolet absorber is preferably 0.01 to 3 parts by mass, the content of the light stabilizer is preferably 0.01 to 3 parts by mass, and the content of the lubricant is preferably 0.01 to 3 parts by mass, relative to 100 parts by mass of the constituent resin of the surface layer (100 parts by mass in total in the case of multiple types). When other polymers and / or additives are added to the surface layer, the timing of addition may be during or after polymerization of the styrene-based copolymer (SX).

[0040] The glass transition temperature (Tg) of the constituent resin of the surface layer (a mixed resin composition when multiple types are used) is not particularly limited, and is preferably 80 to 160°C, more preferably 100 to 110°C. The melt-kneading temperature of the surface layer material during molding of the laminate sheet of the present disclosure is not particularly limited, and is preferably 150 to 280°C, more preferably 170 to 270°C, and particularly preferably 190 to 260°C.

[0041] (base material layer) The substrate layer contains one or more methacrylic resins (M). The methacrylic resins (M) are homopolymers or copolymers containing methyl methacrylate (MMA) units. From the viewpoint of transparency, the content of MMA units in the methacrylic resins (M) is 80% by mass or more, preferably 90% by mass or more, more preferably 95% by mass or more, and may be 100% by mass.

[0042] The methacrylic resin (M) may contain one or more (meth)acrylic acid ester units other than MMA units. Examples of (meth)acrylic acid esters other than MMA include methyl acrylate (MA), ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, t-butyl (meth)acrylate, hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, nonyl (meth)acrylate, decyl (meth)acrylate, dodecyl (meth)acrylate, stearyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, and the like. Examples of the acrylates include acrylate, 4-hydroxybutyl (meth)acrylate, cyclohexyl (meth)acrylate, 2-methoxyethyl (meth)acrylate, 3-methoxybutyl (meth)acrylate, trifluoromethyl (meth)acrylate, trifluoroethyl (meth)acrylate, pentafluoroethyl (meth)acrylate, glycidyl (meth)acrylate, allyl (meth)acrylate, phenyl (meth)acrylate, toluyl (meth)acrylate, benzyl (meth)acrylate, isobornyl (meth)acrylate, and 3-dimethylaminoethyl (meth)acrylate. Among these, MA is preferred from the viewpoint of transparency. For example, a copolymer of MMA and MA is preferred because it has excellent transparency. In this specification, (meth)acrylic is a general term for acrylic and methacrylic, and the same applies to (meth)acrylic acid, (meth)acrylonitrile, and the like.

[0043] The substrate layer may contain one or more other acrylic resins (A) other than the methacrylic resin (M) as necessary. In this specification, the "other acrylic resins (A)" refer to methacrylic resins having an MMA unit content of less than 80 mass% and (meth)acrylic resins that do not contain MMA units and contain one or more (meth)acrylic acid ester units other than MMA units.

[0044] The methacrylic resin (M) and the other acrylic resin (A) may contain structural units derived from one or more other monomers other than (meth)acrylic acid esters. Examples of the other monomers include (meth)acrylic acid, (meth)acrylic acid metal salts, (meth)acrylonitrile, (meth)acrylamide, vinyl monomers such as vinyl chloride and vinyl acetate, acid anhydrides such as maleic anhydride, maleimides such as phenylmaleimide and cyclohexylmaleimide, and styrene monomers such as styrene, α-methylstyrene, and vinyltoluene. The content of structural units derived from monomers other than (meth)acrylic acid esters in the methacrylic resin (M) and the other acrylic resin (A) (the total amount in the case of multiple types) is preferably 10 mass % or less, more preferably 5 mass % or less, and particularly preferably 2 mass % or less. The content of styrene monomer units in the methacrylic resin (M) and the other acrylic resin (A) (when multiple types are used, the total amount) is preferably 0 to 1.5 mass%, more preferably 0 to 1.2 mass%, particularly preferably 0 to 1.0 mass%, and most preferably 0 to 0.85 mass%.

[0045] The methacrylic resin (M) and the other acrylic resin (A) are obtained by polymerizing one or more (meth)acrylic acid esters and, if necessary, other monomers. When using multiple types of monomers, the multiple types of monomers are usually mixed to prepare a monomer mixture, and then polymerization is performed. There are no particular limitations on the polymerization method, and from the viewpoint of productivity, radical polymerization methods such as bulk polymerization, suspension polymerization, solution polymerization, and emulsion polymerization are preferred.

[0046] Within the range where the haze value of a 3.0 mm thick single-layer molded sheet of the pulverized laminate sheet of the present disclosure is 5% or less, the base layer may contain one or more styrene copolymers (SX) as necessary. That is, the base layer may be made of a methacrylic resin composition (MR) containing a methacrylic resin (M) and a styrene copolymer (SX). The styrene copolymer (SX) in the base layer may be the same or different from the styrene copolymer (SX) in the surface layer. When the base layer contains a styrene-based monomer unit, there is a tendency that the amount of change in warpage of the laminate sheet after being left standing in a high-humidity environment can be effectively reduced.

[0047] In general, in the production of (co)extrusion molded sheets and molded products using the same, there are defective products that arise when the extrusion molding production line is started up, scraps generated by trimming both ends of the sheet, defective products that are determined not to meet product standards in quality inspections for defects and foreign bodies, and scraps generated by cutting the sheet. In recent years, efforts toward a sustainable society have been progressing, and it is preferable to effectively reuse the above-mentioned defective products and scraps as rework materials rather than disposing of them. In this specification, a "virgin material" is a molding material that has never been subjected to molding processing in the past, and a "rework material" is a molding material that has been molded into a molded product at least once in the past. At least a part of the total raw material of the base material layer can be a recycled resin composition (R) (also called a rework material) consisting of a crushed product of the laminate sheet of the present disclosure that was previously manufactured or a processed product of the crushed product. The form of the processed product can be a strand, a pellet, or the like. As described above, the pulverized laminate sheet of the present disclosure can have a haze value of 5% or less when formed into a 3.0 mm-thick single-layer molded sheet, and a laminate sheet of the present disclosure having excellent transparency can be produced by using a recycled resin composition (R) consisting of pulverized material of a laminate sheet of the present disclosure previously produced or a processed product of the pulverized material as at least a portion of the total raw material for the base layer.

[0048] The concentration of the styrene-based monomer unit in the base layer is not particularly limited, and is preferably 0 to 10.0% by mass. Patent Document 3, listed in the [Background Art] section, states that "in order to suppress the occurrence of cloudiness and maintain transparency, the styrene content in the base layer is preferably 1 mass % or less, and more preferably 0.85 mass % or less" (paragraph 0171). In the technology of the present disclosure, the styrene-based monomer unit concentration in the base layer can be made higher than the range described in Patent Document 3, and can be made 1.2 mass% or more, 1.5 mass% or more, 2.0 mass% or more, 2.5 mass% or more, 3.0 mass% or more, 3.5 mass% or more, or 4.0 mass% or more. The upper limit is more preferably 9.0 mass%, particularly preferably 8.5 mass%, and most preferably 8.0 mass%.

[0049] Within the range that satisfies the characteristic that the haze value of a 3.0 mm thick single-layer molded sheet of the pulverized laminate sheet of the present disclosure is 5% or less, the base layer may contain one or more other polymers other than the methacrylic resin (M), other acrylic resin (A), and styrene copolymer (SX) as necessary. The base layer may contain various additives as necessary. Examples of the types of other polymers and additives and the preferred amounts of addition are the same as those of the surface layer.

[0050] The glass transition temperature (Tg) of the constituent resin of the substrate layer (a mixed resin composition when multiple resins are used) is not particularly limited and is preferably 100 to 140°C, more preferably 105 to 135°C, and particularly preferably 105 to 125°C. The melt-kneading temperature of the base layer material during molding of the laminate sheet of the present disclosure is not particularly limited, and is preferably 190 to 280°C, more preferably 210 to 270°C, and particularly preferably 230 to 260°C.

[0051] [Manufacturing method of laminated sheet] The laminate sheet of the present disclosure can be manufactured by a known sheet molding method, and from the viewpoint of production efficiency and interlayer adhesion, an extrusion molding method or the like is preferable. In the case of the extrusion molding method, a co-extrusion molding is preferable in which a base layer material containing a methacrylic resin (M) and a surface layer material containing a styrene copolymer (SX) that are melt-kneaded using different extruders are co-extruded from a common extrusion die (such as a T-die). In other words, the laminate sheet of the present disclosure is preferably a co-extrusion molded sheet.

[0052] Co-extrusion die types include a multi-manifold die type and a field block type. In the feed block type, a molten base material layer material containing a methacrylic resin (M) and a molten surface layer material containing a styrene copolymer (SX) are laminated in a feed block, then guided to a T-die or the like to be formed into a sheet and co-extruded. In the multi-manifold die type, a molten base material layer material containing a methacrylic resin (M) and a molten surface layer material containing a styrene copolymer (SX) are guided to a T-die or the like to be formed into a sheet, then guided to a T-die or the like to be formed into a sheet, then laminated and co-extruded. In the laminate sheet of the present disclosure, the surface layer is designed to be relatively thin. In this case, the multi-manifold die type is preferred. In either method, the thermoplastic resin laminate extruded from a T-die or the like is cooled by passing through a gap between at least a pair of cooling pressure rolls, and then taken up by a take-up roll. The above co-extrusion, cooling, and take-up steps are carried out continuously. In this specification, the heated and molten state is mainly referred to as a "thermoplastic resin laminate" and the solidified state is referred to as a "laminate sheet", but there is no clear boundary between the two.

[0053] 3 shows, as one embodiment, a schematic diagram of a production apparatus including a T-die 11, first to third cooling rolls 12 to 14, and a pair of take-up rolls 15. The thermoplastic resin laminate coextruded from the T-die 11 is cooled using the first to third cooling rolls 12 to 14, and the obtained laminate sheet 16 is taken up by the pair of take-up rolls 15. The configuration of the production apparatus can be appropriately modified in design.

[0054] In the co-extrusion molding of the laminated sheet of the present disclosure, the T die temperature (Td) is preferably 190 to 280°C. If Td is less than 190°C, the melt viscosity of the methacrylic resin (M) and the styrene copolymer (SX) may be too high, making it difficult to extrude these resins satisfactorily. If Td is more than 280°C, the styrene copolymer (SX) may decompose due to the high temperature. Td is more preferably 210 to 270°C, particularly preferably 230 to 260°C. The lip thickness of the T-die is designed according to the desired total thickness of the laminate sheet (preferably 1 to 10 mm, more preferably 1 to 5 mm). The take-up speed (V) of the laminated sheet by the pair of take-up rolls is not particularly limited, and is preferably 0.5 to 2.0 m / min.

[0055] In the manufacturing method of the laminate sheet of the present disclosure, the laminate sheet of the present disclosure can be co-extrusion molded using a recycled resin composition (R) consisting of pulverized material of a laminate sheet of the present disclosure previously manufactured or a processed product of the pulverized material, as at least a portion of the total raw material of the base layer. The proportion of the recycled resin composition (R) in the total raw materials of the base layer is not particularly limited and can be, for example, 1 to 100% by mass. In the technology of the present disclosure, the proportion of the recycled resin composition (R) in the total raw materials of the base layer can be increased, and can be 10 to 100% by mass, 20 to 100% by mass, 30 to 100% by mass, 40 to 100% by mass, or 50 to 100% by mass.

[0056] Generally, when the same material is repeatedly reworked, the quality of the rework material may deteriorate, and the haze value of the laminated sheet using the rework material may increase. It is preferable to adjust the proportion of the rework material used within a range that satisfies the characteristic that the haze value of a 3.0 mm-thick laminated sheet using the crushed laminated sheet of the present disclosure as the base layer is 5% or less, taking into consideration the number of reworks or the quality of the rework material. Even when at least a portion of the total raw materials of the base layer is a recycled resin composition (R) consisting of pulverized material of a laminate sheet of the present disclosure that was previously manufactured or a processed product of the pulverized material, the laminate sheet of the present disclosure has excellent transparency and can have a haze value at a thickness of 3.0 mm of 5% or less, 4% or less, 3% or less, 2% or less, or 1% or less.

[0057] [Printed materials, molded products] The laminate sheet of the present disclosure can be preferably used as a resin sheet for inkjet printing. By performing inkjet printing on the surface layer containing the styrene copolymer (SX) contained in the laminate sheet of the present disclosure, a printed matter can be provided. The laminate sheet of the present disclosure can also be cut using a laser and an NC router, etc., as necessary, after inkjet printing, to form it into a desired shape. The laminated sheet of the present disclosure has good laser cutting processability, so that fine cutting can be performed. For example, a molded product having a curved cut portion with a radius of 0.5 to 2 mm can be manufactured with good shape accuracy. The laminated sheet of the present disclosure has good laser cutting processability, so that a high-power laser processing machine can be used to perform cutting at high speed with good productivity. For example, the laminated sheet of the present disclosure can be cut at a speed of 350 cm / min or more with a laser processing machine with an output of 100 W or more to manufacture a molded product.

[0058] As described above, according to the present disclosure, it is possible to provide a laminate sheet that has good ink adhesion and laser cutting processability, and is highly sustainable.

[0059] [Application] The laminated sheets, printed matter, and molded articles of the present disclosure can be used in a variety of fields, such as printing, advertising, sign and display, events, amusement, architecture, and interior design. The laminated sheet, printed matter, and molded article of the present disclosure can be preferably used for miscellaneous goods such as key holders, figurines, and character panels; fixtures, and the like. EXAMPLES

[0060] Examples and comparative examples according to the present invention will be described below. [Evaluation items and evaluation methods] (Styrene monomer unit concentration in styrene copolymer (SX)) Using a nuclear magnetic resonance spectrometer (Bruker's "ULTRA SHIELD 400 PLUS"), the styrene copolymer (SX) 1H-NMR spectrum was measured. The concentration of styrene monomer units was calculated from the integral value of the peaks derived from hydrogen atoms bonded to carbon atoms at positions 2 to 6 of the aromatic ring contained in the styrene monomer units. The styrene monomer units contained in the styrene copolymer (SX) used in the [Examples] section were specifically styrene units.

[0061] (Ratio of each triad chain in styrene copolymer (SX)) A styrene copolymer (SX) was dissolved in deuterated chloroform, and 0.5% by mass of chromium (III) acetylacetonate was added as a relaxation promoter to prepare a sample solution. The obtained sample solution was measured using a nuclear magnetic resonance apparatus (Bruker's "ULTRA SHIELD 400 PLUS") under the conditions of temperature: 50°C, measurement mode: reverse gated decoupling method. 13 C-NMR spectrum was measured. From the integral value of the peak (136-148 ppm) derived from the carbon atom at the 1st position of the aromatic ring contained in the styrene-based monomer unit, the ratio of the triad chain (SSS) of the styrene-based monomer unit (S)-styrene-based monomer unit (S), the triad chain (XSS) of the other monomer unit (X)-styrene-based monomer unit (S)-styrene-based monomer unit (S), and the triad chain (XSX) of the other monomer unit (X)-styrene-based monomer unit (S)-other monomer unit (X) was calculated. The total amount of the triad chain (SSS), triad chain (XSS), and triad chain (XSX) was set to 100 mol%. When the styrene copolymer (SX) is an acrylonitrile-styrene copolymer (AS resin), the styrene monomer unit (S) is a styrene unit, and the other monomer unit (X) is an acrylonitrile unit. When the styrene copolymer (SX) is a styrene-maleic anhydride copolymer (SMA resin), the styrene monomer unit (S) is a styrene unit, and the other monomer unit (X) is a maleic anhydride unit. When the styrene copolymer (SX) is a methyl methacrylate-styrene copolymer (MS resin), the styrene monomer unit (S) is a styrene unit, and the other monomer unit (X) is a methyl methacrylate unit.

[0062] (Haze value of laminated sheet) A 50 mm x 50 mm test piece was cut out from the center of the width direction of a 3.0 mm thick laminated sheet, and the haze value was measured using "HM-150" manufactured by Murakami Color Research Laboratory.

[0063] (Ink adhesion) The ink adhesion was evaluated for the inkjet-printed laminated sheet. In the printed layer consisting of the cured product of white and black UV-curable ink, a 10 mm square evaluation area was cross-cut into 100 squares (10 squares vertically x 10 squares horizontally) at 1 mm intervals vertically and horizontally. Cellophane tape was applied to the entire evaluation area, and the tape was rubbed with an eraser to ensure that the tape was sufficiently adhered to the printed surface, after which the tape was peeled off at a 90° angle. Observation was performed with a 10x magnifying glass, and the number of squares in which the ink had peeled off from the resin sheet was counted out of the 100 squares to be evaluated. The evaluation criteria are as follows: A (Excellent): No ink peeling was observed in any of the squares. B (Good): Ink peeling was observed in squares with 1 or more and less than 10. C (Acceptable): Ink peeling was observed in 10 or more but less than 50 squares. D (Fail): Ink peeling was observed in 50 or more squares.

[0064] (Laser cutting processability) The inkjet-printed laminated sheet was evaluated for laser cutting processability. <Appearance of cutting surface> The ten molded products obtained after the laser cutting process were evaluated for defects on the cutting surface of the 30 cm straight cut section by optical microscope observation and finger touch inspection. The main defects are as follows: Roughness: The cutting surface was not uniform overall and felt rough to the touch. Rough corners: The corners of the cut surface were partially rough and felt rough to the touch. Resin pool: Molten resin pool was observed on some parts of the cutting surface. Foreign matter: Colored foreign matter was found on the cutting surface. The evaluation criteria are as follows: A (Excellent): The number of molded products with defects is 0 to 1. B (Good): The number of molded products with defects is 2 to 4. C (Fail): The number of molded products with defects is 5 to 10.

[0065] <Whether or not smoke or odor is generated> The presence or absence of smoke or odor generation during laser cutting was evaluated sensorily. The evaluation criteria are as follows: A (Good): There was some smoke or odor, but it was not noticeable. B(Acceptable): Between A and C. C (bad): There was noticeable smoke or odor.

[0066] [material] The materials used are as follows: (Methacrylic resin (M)) <pmma1>Methyl methacrylate-methyl acrylate copolymer, "Parepet" manufactured by Kuraray, methyl methacrylate unit content: 94 mass%, methyl acrylate unit content: 6 mass%, styrene unit content: 0 mass%.

[0067] (Acrylonitrile-styrene copolymer (AS resin)) <as1>Nippon A&L "Lytac-A 100PCF", styrene unit content: 77% by mass, <as2>Techno UMG's "Sunrex SAN-C", styrene unit content: 76% by mass, <as3>Denka AS AS-C-820, styrene unit content: 82% by mass, <as4>"Cevian-N 020SF" manufactured by Daicel Miraize Co., Ltd., styrene unit content: 74% by mass.

[0068] (Styrene-maleic anhydride copolymer (SMA resin)) <sma1>"XIRAN23110" manufactured by Polyscope (styrene unit content: 77% by mass).

[0069] (Methyl methacrylate-styrene copolymer (MS resin)) <ms200>"Toyo MS MS200" manufactured by Toyo Styrene Co., Ltd., styrene unit content: 80 mass%.

[0070] [Laminated sheet manufacturing] (Examples (EV1-1) to (EV4-1), Comparative Examples (ECV11-1), (ECV12-1)) As the base layer material, virgin methacrylic resin (M) was melted using a 150 mmφ single screw extruder (maximum temperature of the cylinder part: 240°C) manufactured by Toshiba Machine Co., Ltd. As the surface layer material, virgin styrene copolymer (SX) was melted using a 65 mmφ single screw extruder (maximum temperature of the cylinder part: 240°C) manufactured by Toshiba Machine Co., Ltd. Using a multi-manifold type die, the molten styrene copolymer (SX), the molten methacrylic resin (M), and the molten styrene copolymer (SX) were laminated in this order, extruded from a T-die, cooled using four adjacent cooling rolls, and taken up by a take-up roll. By the above co-extrusion molding, the styrene copolymer (SX) was extruded from a T-die, cooled using four adjacent cooling rolls, and taken up by a take-up roll. Two types of three-layer laminated sheets (LV1-1) to (LV4-1), (LCV11-1), and (LCV12-1) were manufactured: acrylic copolymer (SX) (first surface layer, 0.05 mm thick) / methacrylic resin (M) (base layer, 2.9 mm thick) / styrene copolymer (SX) (second surface layer, 0.05 mm thick). The first surface layer and the second surface layer had the same composition and thickness. The main manufacturing conditions and various parameter values ​​are shown in Tables 1 and 2. In Tables 1 to 4, conditions not listed in the tables were common conditions.

[0071] (Example (EV1-2), Comparative Example (ECV11-2)) Except for changing the thickness of the first and second surface layers to 0.15 mm and the thickness of the base layer to 2.7 mm, laminate sheets (LV1-2) and (LCV11-2) were obtained in the same manner as in Example (EV1-1) or Comparative Example (ECV11-1). The main manufacturing conditions and various parameter values ​​are shown in Tables 1 and 2.

[0072] (Examples (E1-1) to (E1-4)) Laminated sheets (L1-1) to (L1-4) were obtained in the same manner as in Example (EV1-1) or (EV1-2), except that at least a portion (30 mass%, 50 mass%, or 100 mass%) of the base layer material was replaced with the pulverized laminated sheet (LV1-1) or (LV1-2) as a rework material. The main manufacturing conditions and various parameter values ​​are shown in Table 3. The virgin methacrylic resin (M) and the rework material were mixed by dry blending. The same applies to the other examples.

[0073] (Examples (E2-1) to (E4-1)) Laminated sheets (L2-1) to (L4-1) were obtained in the same manner as in Examples (EV2-1), (EV3-1), or (EV4-1), except that a part (50 mass%) of the base material layer material was replaced with the pulverized laminated sheets (LV2-1), (LV3-1), or (LV4-1) as rework materials. The main manufacturing conditions and various parameter values ​​are shown in Table 3.

[0074] (Comparative examples (EC11-1)~(EC11-4), (EC12-1)) Laminated sheets (LC11-1) to (LC11-4) and (LC12-1) were obtained in the same manner as in Comparative Example (ECV11-1), (ECV11-2) and (ECV12-1), except that at least a portion (30 mass%, 50 mass%, or 100 mass%) of the base layer material was replaced with the pulverized laminated sheets (LCV11-1), (LCV11-2), or (LCV12-1) as the rework material. The main manufacturing conditions and various parameter values ​​are shown in Table 4.

[0075] [Evaluation Results] The evaluation results are shown in Tables 1 to 4.

[0076] [Table 1]

[0077] [Table 2]

[0078] [Table 3]

[0079] [Table 4]

[0080] [Summary of results] In Examples (EV1-1), (EV1-2), (EV2-1) to (EV4-1), only virgin materials were used as the materials for the base layer and the surface layer, and laminate sheets were produced in which a base layer containing a methacrylic resin (M) and surface layers containing a styrene copolymer (SX), which is a binary copolymer of a styrene monomer unit (S) and another monomer unit (X), were laminated on both sides of the base layer. In these examples, the ratio of the total thickness of the surface layer to the total thickness of the laminate sheet was 1 to 20%. In these examples, an acrylonitrile-styrene copolymer (AS resin) containing 70 to 95 mass% of styrene units, or a styrene-maleic anhydride copolymer (SMA resin) containing 60 to 95 mass% of styrene units was used as the styrene copolymer (SX). The styrene copolymers (SX) used in these examples all had a ratio of triad chains (SSS) of 0 to 40 mol%, and a ratio of triad chains (XSX) of 5 to 34 mol%. As an example, the measurement mode was set to the inverse gate decoupling method. 13 The C-NMR spectrum is shown in Figure 4. In Figure 4, the peaks (136 to 148 ppm) derived from the carbon atom at position 1 of the aromatic ring contained in the styrene unit are shown for the triad chain (SSS), triad chain (ASS), and triad chain (ASA). Here, the symbol A represents an acrylonitrile unit, which is the other monomer unit (X). The laminate sheets obtained in these examples all had good ink adhesion and laser cutting processability, a haze value of 1% or less, and good transparency.

[0081] In Examples (E1-1) to (E1-4), laminate sheets were obtained in the same manner as in Examples (EV1-1) or (EV1-2), except that 30 to 100% by mass of the total raw material of the base layer was replaced with a rework material made of a pulverized laminate sheet (LV1-1) or (LV1-2). All of the obtained laminate sheets had good ink adhesion and laser cutting processability, a haze value of 1% or less, and good transparency. In these examples, the compatibility between the styrene-based copolymer (SX) and the methacrylic resin (M) used was good, and even when a large amount of rework material was used, a high-quality laminate sheet was obtained as in the examples using only virgin material. In these examples, a laminate sheet with excellent sustainability including the rework material was obtained. Similar results were obtained in Examples (E2-1) to (E4-1).

[0082] In the comparative examples (ECV11-1), (ECV11-2), and (ECV12-1), only virgin materials were used as the materials for the base layer and the surface layer, and laminated sheets were produced in which a base layer containing a methacrylic resin (M) and surface layers containing a styrene copolymer (SX), which is a binary copolymer of a styrene monomer unit (S) and another monomer unit (X), were laminated on both sides of the base layer. In these examples, the ratio of the total thickness of the surface layer to the total thickness of the laminate sheet was 1 to 20%. In the comparative examples (ECV11-1) and (ECV11-2), an acrylonitrile-styrene copolymer (AS resin) with a ratio of triad chains (XSX) exceeding 34 mol% was used as the styrene copolymer (SX).In the comparative example (ECV12-1), a methyl methacrylate-styrene copolymer (MS resin) with a ratio of triad chains (SSS) exceeding 40 mol% was used as the styrene copolymer (SX). The laminate sheets obtained in these examples all had good ink adhesion and laser cutting processability, a haze value of 1% or less, and good transparency.

[0083] In Comparative Examples (EC11-1) to (EC11-4) and (EC12-1), 30 to 100 mass% of the total raw material of the base layer was replaced with a rework material made of the pulverized laminate sheet (LCV11-1), (LCV11-2), or (LCV12-1), and the laminate sheet was obtained in the same manner as in Comparative Example (ECV11-1), (ECV11-2), or (ECV12-1). The haze value of each of the obtained laminate sheets was extremely high at 4.7 to 45.0%, and the transparency was extremely poor. In these examples, the compatibility between the styrene-based copolymer (SX) and the methacrylic resin (M) used was poor, and a laminate sheet with excellent transparency and excellent sustainability was not obtained even if the rework material was included.

[0084] The present invention is not limited to the above-described embodiment and examples, and appropriate design changes are possible without departing from the spirit of the present invention. [Explanation of symbols]

[0085] 11 T-die 16X, 16Y laminated sheet 21 Base material layer 31, 32, 33 surface layer

Claims

1. A laminated sheet having a base layer and a surface layer laminated on at least one surface of the base layer, The base layer contains a methacrylic resin (M) containing 80% by mass or more of methyl methacrylate units, the surface layer contains a styrene-based copolymer (SX) which is a binary copolymer of a styrene-based monomer unit (S) and another monomer unit (X), Styrene copolymer (SX) is measured under the following conditions: Measurement mode: Inverse gated decoupling method 13 When the ratios of the triad chain (SSS) of a styrene-based monomer unit (S)-styrene-based monomer unit (S), the triad chain (XSS) of another monomer unit (X)-styrene-based monomer unit (S)-styrene-based monomer unit (S), and the triad chain (XSX) of another monomer unit (X)-styrene-based monomer unit (S)-other monomer unit (X) are respectively determined from the C-NMR spectrum, the ratio of the triad chain (SSS) is 0 to 40 mol% and the ratio of the triad chain (XSX) is 5 to 34 mol% relative to 100 mol% in total of the triad chain (SSS), the triad chain (XSS), and the triad chain (XSX), Laminated sheet.

2. The laminate sheet according to claim 1, wherein the styrene-based copolymer (SX) is one or more styrene-based copolymers selected from the group consisting of acrylonitrile-styrene copolymers (AS) and styrene-maleic anhydride copolymers (SMA).

3. The styrene copolymer (SX) is one or more styrene copolymers selected from the group consisting of acrylonitrile-styrene copolymers (AS) containing 70 to 95% by mass of styrene units and styrene-maleic anhydride copolymers (SMA) containing 60 to 95% by mass of styrene units. The laminate sheet according to claim 2.

4. 2. The laminate sheet according to claim 1, wherein the average styrene monomer unit concentration in the entire laminate sheet is 0.1 to 20% by mass.

5. 2. The laminate sheet according to claim 1, wherein the base layer is made of a methacrylic resin composition (MR) containing a methacrylic resin (M) and a styrene copolymer (SX).

6. 2. The laminate sheet according to claim 1, wherein the concentration of the styrene-based monomer unit in the base layer is 0 to 10.0% by mass.

7. The laminate sheet according to claim 6, wherein the concentration of the styrene-based monomer unit in the base layer is 1.2 to 10.0 mass %.

8. The laminate sheet according to claim 5, wherein at least a portion of the total raw materials of the base layer is a recycled resin composition (R) consisting of crushed material of the laminate sheet produced in the past or a processed product of the crushed material.

9. The laminate sheet according to claim 1, wherein the total thickness of the laminate sheet is 1 to 10 mm.

10. 2. The laminate sheet according to claim 1, which is adapted for inkjet printing and / or laser cutting.

11. The laminate sheet of claim 1 which is a coextruded sheet.

12. A printed matter, obtained by inkjet printing on the surface layer of the laminate sheet according to claim 1.

13. A molded article obtained by subjecting the laminate sheet according to claim 1 to inkjet printing and laser cutting.

14. 6. The method for producing a laminate sheet according to claim 5, wherein the laminate sheet is co-extruded using a recycled resin composition (R) consisting of crushed material of the laminate sheet produced in the past or a processed product of the crushed material as at least a part of the total raw material of the base layer.

Citation Information

Patent Citations

  • Thermoplastic-resin multilayer structure

    JP1984012850A

  • Antistatic multilayer sheet and antistatic thermoformed article

    JP2008221839A

  • Heat-shrinkable multi-layer film

    JP2009285892A

  • A multilayer optical film layer containing a blend of methyl methacrylate polymer and styrene acrylonitrile polymer.

    JP2011528450A

  • Laminate and novelty goods

    JP2021160119A