Method for producing rubber foam, rubber foam, and application of the rubber foam
A two-stage foaming process with EVA and controlled vulcanization techniques addresses the challenge of low hardness and smoothness in rubber foam production, resulting in high-quality rubber foams for various applications.
Patent Information
- Application Number
- JP2023084376
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-23
- Publication Date
- 2024-12-05
AI Technical Summary
Existing methods for producing rubber foams face challenges in achieving low hardness and high smoothness, leading to reduced thickness and poor manufacturing quality.
A two-stage foaming process using ethylene-vinyl acetate copolymer (EVA) in combination with press and oven vulcanization techniques to produce a rubber foam with low Asker F hardness of less than 74, incorporating specific resin content and conditions to enhance smoothness and reduce pinhole defects.
The method results in a rubber foam with low hardness and high smoothness, suitable for applications such as sealing, cushioning, sound absorption, and insulation, while minimizing defects and improving manufacturing efficiency.
Smart Images

Figure 2024168003000001
Abstract
Description
[Technical field]
[0001] The present technology relates to a method for producing a rubber foam. More specifically, the present technology relates to a method for producing a rubber foam using a rubber component and an ethylene-vinyl acetate copolymer (EVA), a rubber foam, and a sealing material, a cushioning material, a sound absorbing material, a heat insulating material, a vibration insulating material, a dust-proofing material, and a filler using the rubber foam. [Background technology]
[0002] Foams using rubber components are widely used in various fields, including construction, machinery, home appliances, transportation, packaging, daily necessities, toys, and miscellaneous goods. Various developments are being carried out to improve quality and impart new functions according to each field and purpose.
[0003] For example, Patent Document 1 discloses a sealing material comprising a vulcanized foam of a rubber composition containing a rubber component including a copolymer rubber of ethylene, an α-olefin having 3 or more carbon atoms, and a non-conjugated diene, a vulcanizing agent, and a foaming agent, wherein the rubber composition further contains 7 to 15 parts by mass of calcium oxide, 3 to 5 parts by mass of stearic acid, and 3 to 5 parts by mass of zinc stearate per 100 parts by mass of the rubber component, thereby providing a low-density sealing material that does not cause a decrease in water-stopping properties and does not deteriorate foam-breaking processability.
[0004] Also, for example, Patent Document 2 discloses a sealing material that is obtained by vulcanizing and foaming an admixture containing a rubber component including a copolymer rubber of ethylene, an α-olefin having 3 or more carbon atoms, and a non-conjugated diene, a vulcanizing agent, a foaming agent, and a thermoplastic resin, the admixture containing 2 to 4 parts by mass of stearic acid and 5 to 7 parts by mass of calcium oxide per 100 parts by mass of the rubber component, and the sealing material has a 50% compressive stress of 100 kPa or less, and has low hardness, low density, and excellent sealing properties. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2011-252125 A [Patent Document 2] International Publication No. 2013 / 161920 Summary of the Invention [Problem to be solved by the invention]
[0006] As described above, much development has been conducted on foams using rubber components that are used in various fields. However, depending on the production method, there have been problems such as difficulty in producing a rubber foam with low hardness, or poor smoothness, resulting in a reduced thickness of the rubber foam that can be commercialized.
[0007] Therefore, a main object of the present technology is to provide a technology for producing a rubber foam having low hardness and high smoothness. [Means for solving the problem]
[0008] As a result of extensive research into technology for improving the quality of rubber foam, the inventors of the present application have succeeded in producing a rubber foam having low hardness and high smoothness by using a specific resin and performing two-stage foaming under specific conditions, thereby completing the present technology. That is, in the present technology, first, a primary vulcanization and foaming process is performed in which a composition for producing a rubber foam containing a rubber component and an ethylene-vinyl acetate copolymer (EVA) is press-vulcanized and foamed; a secondary vulcanization and foaming step in which the composition for producing a rubber foam that has been subjected to the primary vulcanization and foaming step is oven-vulcanized and foamed; The present invention provides a method for producing a rubber foam having an Asker F hardness of less than 74. In the production method according to the present technology, the content of the ethylene-vinyl acetate copolymer in the composition for producing a rubber foam can be 50 parts by mass or less per 100 parts by mass of the rubber component.
[0009] Next, the present technology provides a rubber foam having an Asker F hardness of less than 74, which is produced by vulcanizing and foaming a composition for producing a rubber foam, which contains a rubber component and an ethylene-vinyl acetate copolymer (EVA: Ethylene-Vinyl Acetate). The content of the ethylene-vinyl acetate copolymer in the rubber foam-producing composition used in producing a rubber foam according to the present technology can be 50 parts by mass or less per 100 parts by mass of the rubber component. The rubber foam according to the present technology can be used as a sealing material, a cushioning material, a sound absorbing material, a heat insulating material, a vibration insulating material, a dust-proofing material, and a filling material. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] A preferred embodiment for carrying out the present technology will be described below. The embodiments described below are examples of typical embodiments of the present technology, and any of the embodiments can be combined. In addition, the scope of the present technology is not narrowly interpreted by these.
[0011] 1. Manufacturing method of rubber foam The method for producing a rubber foam according to the present technology is a method for carrying out a first vulcanization foaming step and a second vulcanization foaming step using a rubber foam production composition. In addition, as necessary, steps carried out in general rubber foam production methods, such as a kneading step and a molding step, can be freely combined as long as the action and effect of the present technology are not impaired. Each material and each step used in the production method according to the present technology will be described in detail below.
[0012] (1) Composition for producing rubber foam The composition for producing a rubber foam used in the present technology (hereinafter also referred to as the "composition for producing a rubber foam related to the present technology") can contain a rubber component, a resin component, a foaming agent, a foaming aid, a crosslinking agent, a crosslinking accelerator, a crosslinking accelerator aid, a filler, a softener, a processing aid, and various other components that can be used in producing a rubber foam depending on the purpose.
[0013] (1-1) Rubber component The rubber component used in this technology is a vulcanizable resin component, and as the rubber component that can be used in this technology, one or more rubber components that can be used in rubber foams can be freely selected and used as long as the action and effect of this technology are not impaired. Examples include natural rubber (NR), styrene-butadiene rubber (SBR), chloroprene rubber (CR), ethylene-propylene-diene rubber (EPDM), acrylonitrile-butadiene rubber (NBR), silicone rubber (SI), etc. Among these, in this technology, it is preferable to use a rubber component containing ethylene-propylene-diene rubber (EPDM) as the rubber component from the viewpoint of environmental consideration.
[0014] (1-2) Resin components (excluding rubber components) The composition for producing a rubber foam according to the present technology is characterized in that it uses ethylene-vinyl acetate copolymer (EVA) as a resin component other than the rubber component. In the present technology, a rubber foam having low hardness and high smoothness can be produced by carrying out a primary vulcanization foaming process of press vulcanization and a secondary vulcanization foaming process of oven vulcanization using EVA, which will be described later. In addition, since EVA has a low softening point, it is less likely to remain dissolved in the composition for producing a rubber foam according to the present technology during the production of the rubber foam, and as a result, the occurrence of pinhole defects in the produced rubber foam can be suppressed.
[0015] The vinyl acetate ratio of EVA is not particularly limited as long as it does not impair the action and effect of the present technology. The lower limit of the vinyl acetate ratio of EVA is, for example, 1% or more, preferably 5% or more, more preferably 10% or more, and even more preferably 20% or more. By setting the lower limit of the vinyl acetate ratio of EVA within this range, a rubber foam with lower hardness can be produced, and the occurrence of pinhole defects in the rubber foam caused by unmelted EVA can be suppressed. The upper limit of the vinyl acetate ratio of EVA is, for example, 60% or less, preferably 40% or less. By setting the upper limit of the vinyl acetate ratio of EVA within this range, it is possible to prevent a decrease in compatibility with the rubber component, and also to prevent a decrease in foamability due to a decrease in compatibility. In addition, it is possible to prevent a decrease in roll processability.
[0016] The content of EVA in the rubber foam according to the present technology can be freely set as long as it does not impair the function and effect of the present technology. In the present technology, the lower limit of the content of EVA in the rubber foam is, for example, 1 part by mass or more, preferably 5 parts by mass or more, and more preferably 10 parts by mass or more, per 100 parts by mass of the rubber component. By setting the lower limit of the content of EVA in the rubber foam within this range, it is possible to improve the foamability during foam production, as well as the physical properties and slicing processability of the rubber foam.
[0017] The upper limit of the EVA content in the rubber foam, per 100 parts by mass of the rubber component, is, for example, 50 parts by mass or less, preferably 45 parts by mass or less, more preferably 40 parts by mass or less, even more preferably 30 parts by mass or less, and particularly preferably less than 30 parts by mass. By setting the upper limit of the EVA content in the rubber foam within this range, the occurrence of pinhole defects in the rubber foam can be suppressed.
[0018] The composition for producing rubber foam according to the present technology may contain, in addition to EVA, other resins (excluding rubber components) and elastomers and other resins other than EVA, as long as the action and effect of the present technology are not impaired. Examples of resins and elastomers other than EVA include thermoplastic resins such as polyolefin resins other than EVA, polystyrene resins, polyamide resins, and polyester resins, olefin thermoplastic elastomers, and styrene thermoplastic elastomers.
[0019] (1-3) Foaming agent A foaming agent can be used in the composition for producing a rubber foam according to the present technology. As the foaming agent that can be used in the present technology, one or more foaming agents that can be used in a rubber foam can be freely selected and used as long as the action and effect of the present technology are not impaired.
[0020] Examples of the blowing agent that can be used in the present technology include organic or inorganic thermal decomposition type chemical blowing agents. Examples of organic blowing agents include azo compounds such as azodicarbonamide (ADCA), azodicarboxylate metal salts (e.g., barium azodicarboxylate), azobisisobutyronitrile (AIBN), etc.; nitroso compounds such as N,N'-dinitrosopentamethylenetetramine (DPT), etc.; hydrazine derivatives such as hydrazodicarbonamide, 4,4'-oxybis(benzenesulfonylhydrazide), toluenesulfonylhydrazide (TSH), etc.; and semicarbazide compounds such as toluenesulfonylsemicarbazide, etc. Examples of inorganic blowing agents include ammonium carbonate, sodium carbonate, ammonium hydrogen carbonate, sodium hydrogen carbonate, ammonium nitrite, sodium borohydride, anhydrous monosodium citrate, etc.
[0021] Among these, in the present technology, it is preferable to use an organic blowing agent as the blowing agent, and among the organic blowing agents, it is preferable to use azodicarbonamide (ADCA) because ADCA is easy to handle and has little impact on the human body and the environment.
[0022] The amount of the foaming agent used in the rubber foam production composition according to the present technology can be freely set as long as it does not impair the action and effect of the present technology. In the present technology, the lower limit of the amount of the foaming agent in the rubber foam production composition is, for example, 1.0 part by mass or more, preferably 3.0 parts by mass or more, and more preferably 5.0 parts by mass or more, per 100 parts by mass of the rubber component. By setting the lower limit of the amount of the foaming agent used within this range, the density of the foam can be reduced.
[0023] In the present technology, the upper limit of the amount of the foaming agent in the composition for producing a rubber foam is, for example, 40 parts by mass or less, preferably 35 parts by mass or less, and more preferably 30 parts by mass or less, per 100 parts by mass of the rubber component. Setting the upper limit of the amount of the foaming agent used within this range can suppress molding defects due to excessive foaming and also contribute to cost reduction.
[0024] (1-4) Foaming assistant A foaming aid can be used in the composition for producing a rubber foam according to the present technology. As the foaming aid that can be used in the present technology, one or more foaming aids that can be used in a rubber foam can be freely selected and used as long as the action and effect of the present technology are not impaired.
[0025] Examples of the foaming assistant that can be used in the present technology include urea-based assistants such as urea, metal oxides, and fatty acid metal salts. Examples of the metal oxides include zinc oxide, zinc chloride, zinc acetate, zinc nitrate, lead oxide, dibasic lead phosphite, and tribasic lead sulfate. Examples of the fatty acid metal salts include zinc stearate, lead stearate, magnesium stearate, and calcium stearate. Among these, in the present technology, it is preferable to use urea as the foaming assistant.
[0026] The amount of the foaming aid used in the rubber foam production composition according to the present technology can be freely set as long as it does not impair the action and effect of the present technology. The lower limit of the amount of the foaming aid in the rubber foam production composition is, for example, 0.1 parts by mass or more, preferably 0.2 parts by mass or more, and more preferably 0.3 parts by mass or more, per 100 parts by mass of the rubber component. By setting the lower limit of the amount of the foaming aid within this range, the foaming speed during production can be adjusted, thereby improving the foamability.
[0027] The upper limit of the amount of the foaming aid in the composition for producing a rubber foam is, for example, 8.0 parts by mass or less, preferably 7.0 parts by mass or less, and more preferably 6.0 parts by mass or less, per 100 parts by mass of the rubber component. Setting the upper limit of the amount of the foaming aid used within this range can improve the foamability by adjusting the foaming rate during production, and can also contribute to cost reduction.
[0028] (1-5) Crosslinking agent A crosslinking agent can be used in the composition for producing a rubber foam according to the present technology. As the crosslinking agent that can be used in the present technology, one or more crosslinking agents that can be used in rubber foams can be freely selected and used as long as the action and effect of the present technology are not impaired.
[0029] As the crosslinking agent that can be used in the present technology, a sulfur-based crosslinking agent for sulfur crosslinking can be used. As the sulfur-based crosslinking agent that can be used in the present technology, for example, sulfur such as powdered sulfur, oil-treated powdered sulfur, precipitated sulfur, colloidal sulfur, and dispersible sulfur, and organic sulfur-containing compounds such as tetramethylthiuram disulfide and N,N-dithiobismorpholine that can release active sulfur under crosslinking conditions to crosslink rubber can be mentioned. Among these, it is preferable to use sulfur as the sulfur-based crosslinking agent in the present technology.
[0030] The amount of the crosslinking agent used in the rubber foam production composition according to the present technology can be freely set as long as it does not impair the action or effect of the present technology. The lower limit of the amount of the crosslinking agent in the rubber foam production composition is, for example, 0.2 parts by mass or more, preferably 0.4 parts by mass or more, and more preferably 0.6 parts by mass or more, per 100 parts by mass of the rubber component. By setting the lower limit of the amount of the crosslinking agent within this range, sufficient crosslink density is obtained, and therefore foamability can be improved. In addition, the mechanical properties of the rubber foam can be improved.
[0031] The upper limit of the amount of the crosslinking agent in the composition for producing a rubber foam is, for example, 10.0 parts by mass or less, preferably 8.0 parts by mass or less, and more preferably 6.0 parts by mass or less, per 100 parts by mass of the rubber component. By setting the upper limit of the amount of the crosslinking agent within this range, blooming of the molded article can be suppressed.
[0032] (1-6) Crosslinking accelerator A crosslinking accelerator can be used in the composition for producing a rubber foam according to the present technology. As the crosslinking accelerator that can be used in the present technology, one or more crosslinking accelerators that can be used in rubber foams can be freely selected and used as long as the action and effect of the present technology are not impaired.
[0033] Examples of crosslinking accelerators that can be used in the present technology include thiazoles (e.g., 2-mercaptobenzothiazole, dibenzothiazyl disulfide, etc.), dithiocarbamic acids (e.g., sodium dimethyldithiocarbamate, sodium diethyldithiocarbamate, zinc dimethyldithiocarbamate, zinc diethyldithiocarbamate, etc.), guanidines (e.g., diphenylguanidine, di-o-tolylguanidine, etc.), sulfenamides (e.g., benzothiazyl-2-diethylsulfenamide, N-cyclohexyl-2-benzothiazylsulfene, etc.), and the like. amides, etc.), thiurams (e.g., tetramethylthiuram monosulfide, tetramethylthiuram disulfide, etc.), xanthogenic acids (e.g., sodium isopropyl xanthogenate, zinc isopropyl xanthogenate, etc.), aldehyde ammonias (e.g., acetaldehyde ammonia, hexamenthylenetetramine, etc.), aldehyde amines (e.g., n-butylaldehyde aniline, butylaldehyde monobutylamine, etc.), thioureas (e.g., diethylthiourea, trimethylthiourea, etc.), dithiophosphide crosslinking accelerators, etc. Among these, in the present technology, from the viewpoint of timing adjustment of the foaming rate and the vulcanization rate, it is preferable to use thiazoles, thioureas, dithiocarbamic acids, and sulfenamides.
[0034] The amount of the crosslinking accelerator used in the rubber foam production composition according to the present technology can be freely set as long as it does not impair the action or effect of the present technology. The lower limit of the amount of the crosslinking accelerator in the rubber foam production composition is, for example, 0.1 parts by mass or more, preferably 0.2 parts by mass or more, and more preferably 1.0 parts by mass or more, per 100 parts by mass of the rubber component. By setting the lower limit of the amount of the crosslinking accelerator within this range, the crosslinking speed can be increased, gas leakage can be suppressed, and foamability during production can be improved. In addition, the mechanical properties of the rubber foam can be improved.
[0035] The upper limit of the amount of crosslinking accelerator in the composition for producing a rubber foam, per 100 parts by mass of the rubber component, is, for example, 15 parts by mass or less, preferably 10 parts by mass or less, and more preferably 8 parts by mass or less. By setting the upper limit of the amount of crosslinking accelerator within this range, it is possible to prevent non-foaming due to an excessive increase in crosslinking speed, and to improve moldability.
[0036] (1-7) Crosslinking accelerator A crosslinking accelerator can be used in the rubber foam production composition for producing the rubber foam according to the present technology. As the crosslinking accelerator that can be used in the present technology, one or more crosslinking accelerators that can be used in rubber foam can be freely selected and used as long as the action and effect of the present technology are not impaired.
[0037] Examples of crosslinking accelerators that can be used in the present technology include metal oxides such as zinc oxide (zinc oxide), magnesium oxide, etc. Among these, in the present technology, it is preferable to use zinc oxide from the viewpoint of adjusting the timing of the foaming rate and the vulcanization rate.
[0038] The amount of the crosslinking promoter used in the rubber foam production composition according to the present technology can be freely set as long as it does not impair the action or effect of the present technology. The lower limit of the amount of the crosslinking promoter in the rubber foam production composition is, for example, 0.1 parts by mass or more, preferably 0.5 parts by mass or more, and more preferably 1.0 parts by mass or more, per 100 parts by mass of the rubber component. By setting the lower limit of the amount of the crosslinking promoter in this range, the crosslinking speed can be increased, gas leakage can be suppressed, and foamability during production can be improved. In addition, the mechanical properties of the rubber foam can be improved.
[0039] The upper limit of the amount of the crosslinking-accelerating aid in the composition for producing a rubber foam is, for example, 15 parts by mass or less, preferably 10 parts by mass or less, and more preferably 8 parts by mass or less, based on 100 parts by mass of the rubber component. By setting the upper limit of the amount of the crosslinking-accelerating aid within this range, it is possible to prevent non-foaming due to an excessive increase in the crosslinking rate, and to improve moldability. It can also contribute to cost reduction.
[0040] (1-8) Filler A filler can be used in the composition for producing a rubber foam according to the present technology. As the filler that can be used in the present technology, one or more fillers that can be used in a rubber foam can be freely selected and used as long as the action and effect of the present technology are not impaired.
[0041] Examples of fillers that can be used in the present technology include inorganic fillers such as calcium carbonate such as heavy calcium carbonate, magnesium carbonate, calcium hydroxide, silicic acid and its salts, clay, talc, mica powder, bentonite, silica, alumina, aluminum silicate, aluminum powder, etc. Among these, it is preferable to use calcium carbonate in the present technology.
[0042] The amount of filler used in the rubber foam production composition according to the present technology can be freely set as long as it does not impair the action and effect of the present technology. The lower limit of the amount of filler in the rubber foam production composition is, for example, 5 parts by mass or more, preferably 20 parts by mass or more, and more preferably 40 parts by mass or more, per 100 parts by mass of the rubber component. Setting the lower limit of the amount of filler within this range can contribute to cost reduction.
[0043] The upper limit of the amount of filler in the composition for producing a rubber foam, per 100 parts by mass of the rubber component, is, for example, 250 parts by mass or less, preferably 200 parts by mass or less, and more preferably 180 parts by mass or less. By setting the upper limit of the amount of filler within this range, the mechanical properties of the rubber foam can be improved and a decrease in foamability, etc. can be suppressed.
[0044] (1-9) Pigments A pigment can be used in the composition for producing a rubber foam according to the present technology. As the pigment that can be used in the present technology, one or more pigments that can be used in a rubber foam can be freely selected and used as long as the action and effect of the present technology are not impaired. Examples of the pigment that can be used in the present technology include carbon black such as acetylene black, furnace black, and channel black.
[0045] The amount of pigment used in the rubber foam production composition according to the present technology can be freely set as long as it does not impair the action and effect of the present technology. The lower limit of the amount of pigment in the rubber foam production composition is, for example, 10 parts by mass or more, preferably 25 parts by mass or more, and more preferably 40 parts by mass or more, per 100 parts by mass of the rubber component. By setting the lower limit of the amount of pigment within this range, it is possible to improve the kneadability during production and to improve the mechanical strength of the rubber foam.
[0046] The upper limit of the amount of the pigment in the composition for producing a rubber foam, per 100 parts by mass of the rubber component, is, for example, 90 parts by mass or less, preferably 80 parts by mass or less, and more preferably 70 parts by mass or less. By setting the upper limit of the amount of the pigment within this range, the hardness can be reduced.
[0047] (1-10) Softener A softener can be used in the composition for producing a rubber foam according to the present technology. As the softener that can be used in the present technology, one or more softeners that can be used in rubber foams can be freely selected and used as long as the action and effect of the present technology are not impaired.
[0048] Examples of softeners that can be used in the present technology include plasticizers, paraffin-based process oils, naphthene-based process oils, waxes, liquid paraffin, rosin, chroman resins, polybutene, asphalt, etc. Among these, it is preferable to use paraffin-based process oils in the present technology.
[0049] The amount of the softener used in the rubber foam production composition according to the present technology can be freely set as long as it does not impair the action and effect of the present technology. The lower limit of the amount of the softener in the rubber foam production composition is, for example, 10 parts by mass or more, preferably 15 parts by mass or more, and more preferably 20 parts by mass or more, per 100 parts by mass of the rubber component. By setting the lower limit of the amount of the softener within this range, a rubber foam with lower hardness can be produced.
[0050] The upper limit of the amount of the softener in the composition for producing a rubber foam is, for example, 100 parts by mass or less, preferably 95 parts by mass or less, and more preferably 90 parts by mass or less, per 100 parts by mass of the rubber component. By setting the upper limit of the amount of the softener within this range, kneadability during production can be improved.
[0051] (1-11) Processing aids The composition for producing a rubber foam according to the present disclosure may contain a processing aid. The use of the processing aid can improve processability during production.
[0052] The processing aid that can be used in the present technology can be freely selected from one or more processing aids that can be used in general rubber compositions, as long as the purpose and effect of the present technology are not impaired. Examples of processing aids that can be used in the present technology include fatty acids such as stearic acid, fatty acid esters, fatty acid amides, fatty alcohols, and metal salts of fatty acids.
[0053] The amount of the processing aid used in the rubber foam production composition according to the present technology can be freely set as long as it does not impair the purpose and effect of the present technology. The lower limit of the amount of the processing aid in the rubber foam production composition can be set to, for example, 0.1 parts by mass or more, preferably 0.5 parts by mass or more, and more preferably 1.0 parts by mass or more, per 100 parts by mass of the rubber component. By setting the lower limit of the amount of the processing aid within this range, it is possible to further improve the kneading processability during production.
[0054] The upper limit of the amount of processing aid in the composition for producing rubber foam can be set, for example, to 10 parts by mass or less, preferably 7 parts by mass or less, and more preferably 5 parts by mass or less, per 100 parts by mass of the rubber component. Setting the upper limit of the content of the processing aid within this range can prevent a decrease in the strength of the produced rubber foam.
[0055] (1-12)Other In the rubber foam-producing composition for producing the rubber foam according to the present technology, one or more components that can be used in rubber foams can be freely selected and used as other components depending on the purpose, as long as the action and effect of the present technology is not impaired.
[0056] Examples of components that can be used in the rubber foam according to the present technology include foam stabilizers, stabilizers, colorants, antioxidants, dispersants, UV absorbers, and flame retardants.
[0057] (2) Mixing process In the production method according to the present technology, a kneading step can be performed. The kneading step is a step of kneading the raw materials of the composition for producing a rubber foam described above. Specifically, all or a part of the raw materials of the composition for producing a rubber foam can be kneaded using a kneading machine such as a kneader, a Banbury mixer, or a roll mixer.
[0058] The kneading step can be performed in a plurality of stages. Specifically, for example, the components other than the crosslinking agent, crosslinking accelerator, foaming agent, foaming assistant, etc. are first kneaded, and then the crosslinking agent, crosslinking accelerator, crosslinking assistant, foaming agent, foaming assistant, etc. are added to the obtained primary kneaded product and second kneaded.
[0059] When kneading is performed in two separate steps, the conditions for the first kneading can be set to, for example, a temperature of 50° C. to 180° C. and a kneading time of 3 to 30 minutes, etc. The conditions for the second kneading can be set to, for example, a temperature of 20° C. to 80° C. and a kneading time of 3 to 30 minutes, etc.
[0060] (3) Primary vulcanization and foaming process The primary vulcanization and foaming step is a step of press-vulcanizing and foaming the rubber foam production composition. In the present technology, "press vulcanization" refers to a process of vulcanizing the rubber foam production composition under pressure. In the production method according to the present technology, a rubber foam with high smoothness can be produced by carrying out press vulcanization in the primary vulcanization and foaming step. Note that press vulcanization and foaming can be carried out simultaneously or sequentially under different conditions.
[0061] Various conditions in the primary vulcanization and foaming process can be freely set as long as they do not impair the action and effect of the present technology. The temperature condition is, for example, 100°C or higher, preferably 120°C or higher, and more preferably 125°C or higher. By setting the lower limit of the temperature within this range, it is possible to contribute to improving the ease of production. In addition, the upper limit of the temperature is, for example, 200°C or lower, preferably 180°C or lower, and more preferably 160°C or lower. By setting the upper limit of the temperature within this range, it is possible to contribute to energy reduction. The heating method is not particularly limited as long as it can perform press vulcanization and foaming. For example, heating methods such as heating using a hot air vulcanization tank (HAV), heating using a glass bead fluidized bed, heating using a microwave vulcanization device (UHF), and steam heating can be freely combined and used.
[0062] The pressure condition is, for example, 0.1 MPa or more, preferably 0.2 MPa or more, more preferably 0.5 MPa or more, and even more preferably 0.6 MPa or more. By setting the lower limit of the pressure in this range, it is possible to improve the foaming property and ease of production. The upper limit of the pressure is, for example, 20 MPa or less, preferably 18 MPa or less, and more preferably 17 MPa or less. By setting the upper limit of the pressure in this range, it is possible to contribute to energy reduction.
[0063] The time condition is, for example, 1 minute or more, preferably 2 minutes or more, more preferably 5 minutes or more, and even more preferably 6 minutes or more. By setting the lower limit of the time within this range, it is possible to improve the foaming property and ease of production. The upper limit of the time is, for example, 100 minutes or less, preferably 50 minutes or less, more preferably 40 minutes or less, even more preferably 30 minutes or less, and particularly preferably 10 minutes or less. By setting the upper limit of the time within this range, it is possible to improve the production efficiency and produce a rubber foam with lower hardness.
[0064] (4) Secondary vulcanization and foaming process The secondary vulcanization and foaming step is a step of oven vulcanizing and foaming the rubber foam production composition. In the present technology, "oven vulcanization" refers to a process in which the rubber foam production composition is vulcanized without applying pressure in a tank heated to a high temperature with steam. In the production method according to the present technology, a rubber foam with low hardness can be produced by performing oven vulcanization in the secondary vulcanization and foaming step. Note that oven vulcanization and foaming can be performed simultaneously or sequentially under different conditions.
[0065] Various conditions in the secondary vulcanization foaming process can be freely set as long as they do not impair the action and effect of the present technology. The temperature condition is, for example, 100°C or higher, preferably 120°C or higher, and more preferably 125°C or higher. By setting the lower limit of the temperature within this range, it is possible to contribute to lowering the density of the rubber foam to be produced. In addition, the upper limit of the temperature is, for example, 220°C or lower, preferably 210°C or lower, and more preferably 200°C or lower. By setting the upper limit of the temperature within this range, it is possible to contribute to energy reduction. The heating method is the same as that of the above-mentioned primary vulcanization foaming process, so a description thereof will be omitted here.
[0066] The time condition is, for example, 1 minute or more, preferably 2 minutes or more, more preferably 5 minutes or more, and even more preferably 6 minutes or more. By setting the lower limit of the time in this range, it is possible to improve the foaming property and ease of production. The upper limit of the time is, for example, 70 minutes or less, preferably 60 minutes or less, and more preferably 50 minutes or less. By setting the upper limit of the time in this range, it is possible to improve the production efficiency.
[0067] (5) Molding process In the manufacturing method according to the present technology, a molding process can be carried out. The molding process is a process in which the rubber foam that has undergone the above-mentioned primary vulcanization foaming process and secondary vulcanization foaming process is processed into a desired shape by cutting or slicing the edges. The rubber foam manufactured through the above-mentioned primary vulcanization foaming process and secondary vulcanization foaming process has a high smoothness, and therefore has the characteristic of being able to reduce loss in the molding process.
[0068] The specific method for the molding step is not particularly limited as long as it does not impair the action and effect of the present technology, and any molding method that can be used for producing general rubber foams can be freely combined.
[0069] 2. Rubber foam The rubber foam according to the present technology is a rubber foam obtained by vulcanizing and foaming the above-mentioned rubber foam-producing composition according to the present technology. Note that the rubber foam-producing composition for producing the rubber foam according to the present technology is the same as that described above, and therefore description thereof will be omitted here.
[0070] (1) Asker hardness The rubber foam according to the present technology is characterized in that it has an Asker F hardness of less than 74. The Asker F hardness of the rubber foam according to the present technology may be less than 74, but is preferably 70 or less, more preferably 65 or less, even more preferably 60 or less, and particularly preferably 50 or less. The lower limit of the Asker F hardness of the rubber foam according to the present technology can be freely set according to the application or purpose. In the present technology, the Asker F hardness is a value measured in accordance with a method based on JIS K7312:1996.
[0071] (2) Density The density of the rubber foam according to the present technology can be freely set as long as it does not impair the function and effect of the present technology. The lower limit of the density of the rubber foam according to the present technology is, for example, 0.01 g / cm 3 More than 0.03 g / cm 3 More preferably, 0.05 g / cm 3 The upper limit of the density of the rubber foam according to the present technology is, for example, 0.20 g / cm 3 Less than 0.17 g / cm 3 Less than or equal to 0.15 g / cm 3 In this technology, the density is a value measured in accordance with a method based on JIS K6767:1999.
[0072] 3. Applications of rubber foam The high quality of the rubber foam according to the present technology allows it to be used in a wide variety of fields for a wide variety of purposes. For example, it can be used as a sealing material, a cushioning material, a sound absorbing material, a heat insulating material, a vibration-proofing material, a dust-proofing material, a filler, etc. It can be used in a wide variety of fields, including the construction field, the vehicle field, the aircraft field, the transportation field, the home appliance field, the electronic device field, the packaging field, the packaging field, the daily necessities field, the clothing field, the medical field, the furniture field, the bedding field, the household goods field, the cosmetics field, etc. EXAMPLES
[0073] The present technology will be described in more detail below based on examples. Note that the examples described below are representative examples of the present technology, and the scope of the present technology is not to be interpreted narrowly by these examples.
[0074] In this example, the effects of differences in manufacturing methods and raw materials used on the physical properties of rubber foams were examined.
[0075] (1) Manufacturing of rubber foam [Examples 1] to [Examples 10], [Comparative Example 1] The rubber foam raw materials shown in Table 1 below were mixed and roll kneaded, and then heated and pressurized under the conditions shown in Table 1 below to carry out primary vulcanization and foaming for vulcanization and foaming. Next, the rubber foam was produced by heating under the conditions shown in Table 1 below to carry out secondary vulcanization and foaming for vulcanization and foaming.
[0076] [Comparative Example 2] The rubber foam raw materials shown in Table 1 below were mixed and roll kneaded, and then heated and pressurized under the conditions shown in Table 1 below to carry out primary vulcanization and foaming, whereby the mixture was vulcanized and foamed. Next, heated and pressurized under the conditions shown in Table 1 below to carry out secondary vulcanization and foaming, whereby the mixture was vulcanized and foamed, to produce a rubber foam.
[0077] [Reference example 1] The rubber foam raw materials shown in Table 1 below were mixed and roll-kneaded, and then heated under the conditions shown in Table 1 below to vulcanize and foam, thereby producing a rubber foam.
[0078] (2) Measurement of physical properties The produced rubber foams were evaluated for various physical properties using the following methods.
[0079] [density] The density was measured in accordance with the method based on JIS K6767:1999.
[0080] [Asker F hardness] The Asker F hardness was measured in accordance with the method based on JIS K7312:1996.
[0081] [25% compression load] The 25% compressive load was measured by the following method. (a) Three test pieces were prepared by slicing to a thickness of 12 mm or more and cutting to dimensions of 100 x 100 mm so that opposing surfaces were parallel. (b) Load-deflection: Using an autograph that can take chart graphs, the load required to compress the specimen by 25% was determined. The compression speed was 50 mm / min. (c) The compressive load was calculated using the following formula. 25% compression load (kPa) = (F25 (N) / S (cm 2 ))×10 F25: Full load at 25% compression (N) (chart graph read) S: Area of the compressed surface of the test piece (cm 2 ) (d) The measured value was the average of the compressive loads of three test pieces.
[0082] (3) Evaluation The foaming property, low hardness, smoothness, pinhole defects, and ease of production were evaluated based on the following evaluation criteria.
[0083] [Foaming] The state of the molded product after foaming was visually confirmed. A: No problem. B: Small or warped C: The surface is uneven due to air intrusion. D: Not inflated at all
[0084] [Low hardness] A: Asker F hardness 60 or less B: Asker F hardness 61-70 C: Asker F hardness 71~80 D: Asker F hardness 81 or higher
[0085] [Smoothness] A: The difference in thickness between the center and the edge is 3.0 mm or less B: The difference in thickness between the center and the edge is 3.1 to 6.0 mm. C: Thickness difference between the center and the edge is 6.1 to 9.0 mm D: The difference in thickness between the center and the edge is 9.1 mm or more
[0086] [Pinhole defect] 1m of the produced rubber foam 2 The size and number of pinholes were evaluated according to the following criteria. 1. There are no pinholes larger than φ4mm 2. Pinholes with a size of φ3mm or more and less than φ4mm: 6 or less on both sides 3. Pinholes with a size of φ1mm or more and less than φ3mm: 12 or less on both sides 4. There are a total of 14 pinholes or less on both sides A: All 1 to 4 are met B: 1-2 are met, but 3-4 are not met C: 1 is satisfied, but 2-4 are not satisfied D: None satisfied
[0087] [Production difficulty] A: No problem. B: The release properties are poor when removing the mold after the first vulcanization and foaming, but it can be removed without using a spatula. C: The mold release is very poor when removing the product after the first vulcanization and foaming, and a spatula must be used, resulting in defective products. D: Cannot foam
[0088] (4) Results The results are shown in Table 1 below. [Table 1]
[0089] (5) Discussion As shown in Table 1, Comparative Example 1, which did not use EVA, had an Asker F hardness of 74 or more. Even when EVA was used, Comparative Example 2, which was press-vulcanized in both the first vulcanization and foaming process and the second vulcanization and foaming process, had a very high Asker F hardness. On the other hand, Reference Example 1, which was oven-vulcanized in both the first vulcanization and foaming process and the second vulcanization and foaming process, was able to reduce the Asker F hardness, but lost smoothness. In contrast, Examples 1 to 10, which used EVA and were press-vulcanized in the first vulcanization and foaming process and oven-vulcanized in the second vulcanization and foaming process, had an Asker F hardness of less than 74 and good smoothness.
[0090] Comparing Examples 1 to 10, Example 1, which used EVA with a vinyl acetate ratio of 28%, had a lower hardness than Example 2, which used EVA with a vinyl acetate ratio of 5%. This result shows that the hardness of the manufactured rubber foam can be further reduced by using EVA with a relatively high vinyl acetate ratio.
[0091] Example 1, which used 20 parts by mass of EVA per 100 parts by mass of the rubber component, showed a higher pinhole defect evaluation than Example 3, which used 30 parts by mass of EVA per 100 parts by mass of the rubber component. This result shows that pinhole defects can be further reduced by setting the EVA content to less than 30 parts by mass per 100 parts by mass of the rubber component.
[0092] Example 4, in which the pressure in the primary vulcanization foaming step was set lower than that in Example 1, and Example 5, in which the time was set shorter than that in Example 1, were rated inferior in foamability and ease of production compared to Example 1. This result shows that lowering the pressure or shortening the time in the primary vulcanization foaming step may reduce ease of production. On the other hand, Example 6, in which the time of the primary vulcanization foaming step was set longer than that in Example 1, had a higher hardness compared to Example 1. This result shows that extending the time of the primary vulcanization foaming step may increase the hardness of the produced rubber foam.
[0093] In Examples 7 and 8, in which the temperature in the primary vulcanization foaming process was increased, all evaluations were equivalent to and excellent than those of Example 1. From these results, it was found that increasing the temperature in the primary vulcanization foaming process by about 6 degrees has little effect on the quality and ease of production of the produced rubber foam. On the other hand, in Examples 9 and 10, in which the temperature in the primary vulcanization foaming process was set lower than that of Example 1, the evaluation of the ease of production was lower. From these results, it was found that setting the temperature in the primary vulcanization foaming process lower may result in a decrease in ease of production.
Claims
1. a primary vulcanization and foaming step of press-vulcanizing and foaming a rubber foam production composition containing a rubber component and an ethylene-vinyl acetate copolymer (EVA); a secondary vulcanization and foaming step in which the composition for producing a rubber foam that has been subjected to the primary vulcanization and foaming step is oven-vulcanized and foamed; The method for producing a rubber foam having an Asker F hardness of less than 74.
2. 2. The method for producing a rubber foam according to claim 1, wherein a content of the ethylene-vinyl acetate copolymer in the composition for producing a rubber foam is 50 parts by mass or less per 100 parts by mass of the rubber component.
3. A rubber foam having an Asker F hardness of less than 74 is obtained by vulcanizing and foaming a composition for producing a rubber foam, which contains a rubber component and an ethylene-vinyl acetate copolymer (EVA).
4. The rubber foam according to claim 3, wherein the content of the ethylene-vinyl acetate copolymer in the composition for producing a rubber foam is 50 parts by mass or less per 100 parts by mass of the rubber component.
5. 5. A sealing material, a cushioning material, a sound absorbing material, a heat insulating material, a vibration insulating material, a dust-proofing material, or a filler, which uses the rubber foam according to claim 3 or 4.
Citation Information
Patent Citations
Sealing material and method of manufacturing the same
JP2011252125A
Sealing material
WO2013161920A1