Polyamide composition and molded article

A polyamide composition with aliphatic and semi-aromatic polyamides addresses the challenges of heat resistance and toughness in rolling bearings, ensuring rigidity and surface quality even under moisture exposure.

JP2024168254APending Publication Date: 2024-12-05ASAHI KASEI KOGYO KABUSHIKI KAISHA
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023084761
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-23
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

Existing polyamide compositions for rolling bearings fail to provide sufficient heat resistance, rigidity, and toughness, especially during high-speed rotation, leading to potential deformation and seizing due to centrifugal force and frictional heat, with elastomer addition compromising elastic modulus.

Method used

A polyamide composition comprising aliphatic and semi-aromatic polyamides with specific monomer units and a difference in melting and crystallization temperatures, along with optional additives like acid-modified elastomers and fillers, to enhance heat resistance, rigidity, and toughness.

Benefits of technology

The composition maintains excellent heat resistance, rigidity, and surface appearance while suppressing rigidity and toughness degradation upon moisture absorption, suitable for high-performance rolling bearings.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024168254000001
    Figure 2024168254000001
Patent Text Reader

Abstract

To provide a polyamide composition which excels in heat resistance and rigidity during molding, and which suppresses the decrease in rigidity and toughness when absorbing moisture, and which excels in surface appearance.SOLUTION: There is provided a polyamide composition comprising an aliphatic polyamide and a semiaromatic polyamide, wherein the aliphatic polyamide comprises aliphatic dicarboxylic acid units and aliphatic diamine units, the semiaromatic polyamide comprises aromatic dicarboxylic acid units and aliphatic diamine units, the aliphatic diamine units of the semiaromatic polyamide comprise at least one unit selected from the group consisting of ethylenediamine unit, trimethylenediamine unit, tetramethylenediamine unit and pentamethylenediamine unit, and wherein a difference (Tm2-Tc) between a melting peak temperature Tm2 and a crystallization temperature Tc, measured when raising temperature at 20°C / min in differential scanning calorimetry in accordance with JIS-K7121 is 35°C or more and less than 45°C.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a polyamide composition and a molded article. [Background technology]

[0002] In recent years, electric vehicles that do not emit carbon dioxide while driving have been attracting attention due to the growing environmental awareness. New technology development is underway to further reduce the environmental impact, and while each component is required to be smaller in size in order to improve power efficiency through weight reduction, higher output is also required. In particular, the rolling bearings that support the motor are required to have higher speed rotation performance than ever before.

[0003] A rolling bearing is composed of an outer ring, an inner ring, balls and a cage, and the cage is required to have high heat resistance and toughness.

[0004] Polyamide resins are widely used as materials with excellent heat resistance and toughness. The melting point of commonly used aliphatic polyamides is about 200°C to 280°C, and they do not have heat resistance in the above-mentioned usage environment. Semi-aromatic polyamides such as those disclosed in Patent Document 1 are known as semi-aromatic polyamides with excellent rigidity and high-temperature physical properties. Furthermore, in order to achieve both heat resistance and toughness, attempts have been made to impart toughness in addition to heat resistance by adding an elastomer to semi-aromatic polyamides having rigidity and heat resistance (Patent Document 2). [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Patent No. 7188706 [Patent Document 2] Patent No. 5270106 Summary of the Invention [Problem to be solved by the invention]

[0006] To obtain a rolling bearing with superior high-speed rotation performance, it is necessary to provide the cage with sufficient rigidity to prevent it from coming into contact with the outer ring even if it is deformed by centrifugal force during high-speed rotation, and with sufficient heat resistance to prevent the cage from melting and seizing to the outer ring due to frictional heat. On the other hand, since a large distortion occurs when the balls are fitted into the cage, toughness at room temperature is also required.

[0007] However, in the technique disclosed in Patent Document 2, the elastic modulus is reduced by adding an elastomer, and therefore the results are not sufficient.

[0008] Therefore, an object of the present invention is to provide a polyamide composition which is excellent in heat resistance and rigidity during molding, which is inhibited from decreasing in rigidity and toughness upon moisture absorption, and which is excellent in surface appearance, and to provide a molded article obtained by molding the polyamide composition. [Means for solving the problem]

[0009] That is, the present invention includes the following aspects. [1] aliphatic polyamides and semi-aromatic polyamides, The aliphatic polyamide contains an aliphatic dicarboxylic acid unit and an aliphatic diamine unit, The semi-aromatic polyamide comprises an aromatic dicarboxylic acid unit and an aliphatic diamine unit, The aliphatic diamine unit of the semi-aromatic polyamide contains at least one or more units selected from the group consisting of an ethylenediamine unit, a trimethylenediamine unit, a tetramethylenediamine unit, and a pentamethylenediamine unit, A polyamide composition, in which the difference (Tm2-Tc) between the melting peak temperature Tm2 and the crystallization temperature Tc measured at a heating rate of 20°C / min in differential scanning calorimetry according to JIS-K7121 is 35°C or more and less than 45°C. [2] The polyamide composition according to [1], wherein the aromatic dicarboxylic acid units consist only of terephthalic acid units. [3] The polyamide composition according to [1] or [2], wherein a ratio of the mass of the aliphatic polyamide to a total mass of the aliphatic polyamide and the semi-aromatic polyamide is 30 to 50 mass %. [4] The polyamide composition according to any one of [1] to [3], wherein the aliphatic dicarboxylic acid units consist only of adipic acid units. [5] The polyamide composition according to any one of [1] to [4], wherein the aliphatic diamine units of the semi-aromatic polyamide further contain hexamethylenediamine units. [6] The polyamide composition according to any one of [1] to [5], wherein the aliphatic diamine units of the semi-aromatic polyamide contain tetramethylenediamine units. [7] The polyamide composition according to any one of [1] to [6], comprising an acid-modified elastomer in an amount of 1 to 20 mol % based on the total mass of the polyamide composition. [8] The polyamide composition according to any one of [1] to [7], further comprising a filler, the filler being a fibrous filler. [9] The polyamide composition according to [8], wherein the fibrous filler comprises glass fiber or carbon fiber.

[10] The polyamide composition according to [8], wherein the fibrous filler comprises carbon fiber.

[11] The polyamide composition according to any one of [1] to

[10] , wherein the melting peak temperature Tm2 is 300° C. or higher.

[12] The polyamide composition according to any one of [1] to

[11] , which has a tan δ peak temperature of 100 to 140° C. in differential scanning calorimetry according to JIS-K7121.

[13] A molded article obtained by molding the polyamide composition according to any one of [1] to

[12] .

[14] The molded article according to

[13] , wherein the molded article is a rolling bearing. Effect of the Invention

[0010] The polyamide composition of the present invention has excellent heat resistance, rigidity, surface appearance during molding, and suppression of decrease in rigidity upon moisture absorption when formed into a molded article. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] Hereinafter, an embodiment for carrying out the present invention (hereinafter, referred to as "the present embodiment") will be described in detail. The present embodiment is an example for explaining the present invention, and is not intended to limit the present invention to the following content. The present invention can be carried out with appropriate modifications within the scope of its gist.

[0012] In this specification, polyamide means a polymer having an amide bond (-NHCO-) ​​in the main chain.

[0013] Unless otherwise specified, the materials, components, compounds, resins and solvents described in this specification may be used alone or in combination of two or more.

[0014] In this specification, unless otherwise specified, any numerical range is intended to include the upper and lower limits of the range, for example, 1 to 20 mol% means a range of 1 mol% or more and 20 mol% or less.

[0015] Polyamide Composition The polyamide composition of the present embodiment is aliphatic polyamides and semi-aromatic polyamides, The aliphatic polyamide contains an aliphatic dicarboxylic acid unit and an aliphatic diamine unit, The semi-aromatic polyamide comprises an aromatic dicarboxylic acid unit and an aliphatic diamine unit, The aliphatic diamine unit of the semi-aromatic polyamide contains at least one or more units selected from the group consisting of an ethylenediamine unit, a trimethylenediamine unit, a tetramethylenediamine unit, and a pentamethylenediamine unit, The difference (Tm2-Tc) between the melting peak temperature Tm2 and the crystallization temperature Tc measured at a heating rate of 20°C / min in differential scanning calorimetry according to JIS-K7121 is 35°C or more and less than 45°C.

[0016] Properties of polyamide compositions The tan δ peak temperature of the polyamide composition of the present embodiment can be as follows, and specifically, can be measured by the method described in the examples described later.

[0017] Tan δ peak temperature of polyamide composition The tan δ peak temperature of the polyamide composition in differential scanning calorimetry according to JIS-K7121 is 80 to 160°C, preferably 90 to 150°C, more preferably 90 to 140°C, more preferably 100 to 140°C, even more preferably 100 to 130°C, and particularly preferably 110 to 130°C. In general, a water-based temperature regulator is used in a molding die for ease of introduction, and the die is heated to a maximum of 100 to 120°C before use. For this reason, when the tan δ peak temperature of the polyamide composition is within the range of 80 to 160°C, the appearance of the molded product is improved.

[0018] Melting peak temperature Tm2 and crystallization peak temperature Tc of polyamide composition The difference (Tm2-Tc) between the melting peak temperature Tm2 and the crystallization temperature Tc of the polyamide composition in differential scanning calorimetry according to JIS-K7121 is 35° C. or more and less than 45° C., and preferably 35° C. or more and less than 40° C. When Tm2-Tc is in the range of 35° C. or more and less than 45° C., the appearance of the molded article is improved.

[0019] In one embodiment, the polyamide composition has a melting peak temperature Tm2 of 290° C. or more, 300° C. or more, or 310° C. or more. In another embodiment, the polyamide composition has a melting peak temperature Tm2 of 360° C. or less, 350° C. or less, or 340° C. or less. In yet another embodiment, the polyamide composition has a melting peak temperature Tm2 of 300 to 335° C.

[0020] Hereinafter, each component of the polyamide composition of the present embodiment will be described in detail.

[0021] polyamide The polyamide composition of the present embodiment contains an aliphatic polyamide and a semi-aromatic polyamide.

[0022] Aliphatic Polyamide The aliphatic polyamide contains aliphatic dicarboxylic acid units and aliphatic diamine units.

[0023] Aliphatic dicarboxylic acid unit Examples of the aliphatic dicarboxylic acid constituting the aliphatic dicarboxylic acid unit include linear or branched saturated aliphatic dicarboxylic acids having 3 to 20 carbon atoms. Examples of linear saturated aliphatic dicarboxylic acids having 3 to 20 carbon atoms include malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, dodecanedioic acid, tetradecanedioic acid, hexadecanedioic acid, octadecanedioic acid, eicosane diacid, and diglycolic acid. Examples of branched saturated aliphatic dicarboxylic acids having 3 to 20 carbon atoms include dimethylmalonic acid, 2,2-dimethylsuccinic acid, 2,3-dimethylglutaric acid, 2,2-diethylsuccinic acid, 2,3-diethylglutaric acid, 2,2-dimethylglutaric acid, 2-methyladipic acid, and trimethyladipic acid.

[0024] The aliphatic dicarboxylic acid is preferably a linear saturated aliphatic dicarboxylic acid having 6 or more carbon atoms. Examples of linear saturated aliphatic dicarboxylic acids having 6 or more carbon atoms include adipic acid, sebacic acid, dodecanedioic acid, tetradecanedioic acid, hexadecanedioic acid, octadecanedioic acid, and eicosane diacid. The linear saturated aliphatic dicarboxylic acid having 6 or more carbon atoms is preferably adipic acid, sebacic acid, or dodecanedioic acid. In one embodiment, the aliphatic dicarboxylic acid unit is composed of only adipic acid units.

[0025] Aliphatic diamine units Examples of the aliphatic diamine constituting the aliphatic diamine unit include linear saturated aliphatic diamines having 2 to 20 carbon atoms, and branched saturated aliphatic diamines having 3 to 20 carbon atoms. Examples of linear saturated aliphatic diamines having 2 to 20 carbon atoms include ethylenediamine, trimethylenediamine, tetramethylenediamine, pentamethylenediamine, hexamethylenediamine, heptamethylenediamine, octamethylenediamine, nonamethylenediamine, decamethylenediamine, undecamethylenediamine, dodecamethylenediamine, and tridecamethylenediamine. Examples of branched saturated aliphatic diamines having 3 to 20 carbon atoms include 2-methylpentamethylenediamine, 2,2,4-trimethylhexamethylenediamine, 2,4,4-trimethylhexamethylenediamine, 2-methyl-1,8-octanediamine, and 2,4-dimethyloctamethylenediamine.

[0026] The aliphatic polyamide may further contain a unit derived from a trivalent or higher polyvalent aliphatic amine, if necessary, within a range that does not impair the effect of the polyamide composition of the present embodiment. Examples of the trivalent or higher polyvalent aliphatic amine include bishexamethylenetriamine.

[0027] In one embodiment, the aliphatic polyamide comprises polyamide 66. In another embodiment, the aliphatic polyamide is polyamide 66. Polyamide 66 is a copolymer of hexamethylenediamine and adipic acid.

[0028] Weight average molecular weight Mw of aliphatic polyamide The weight average molecular weight Mw of the aliphatic polyamide is preferably 10,000 to 50,000, more preferably 17,000 to 45,000, still more preferably 20,000 to 45,000, even more preferably 25,000 to 45,000, particularly preferably 30,000 to 45,000, and most preferably 35,000 to 40,000.

[0029] Semi-aromatic polyamide Semi-aromatic polyamides contain aromatic dicarboxylic acid units and aliphatic diamine units.

[0030] Aromatic dicarboxylic acid unit The aromatic dicarboxylic acid unit includes a terephthalic acid unit and an isophthalic acid unit, and is preferably a terephthalic acid unit. In one embodiment, the aromatic dicarboxylic acid unit is composed of only a terephthalic acid unit.

[0031] Examples of aromatic dicarboxylic acids constituting aromatic dicarboxylic acid units other than terephthalic acid units include dicarboxylic acids having an aromatic group such as a phenyl group, a naphthyl group, etc. The aromatic group of the aromatic dicarboxylic acid may be unsubstituted or may have a substituent.

[0032] Examples of the substituent include an alkyl group having 1 to 4 carbon atoms, an aryl group having 6 to 10 carbon atoms, an arylalkyl group having 7 to 10 carbon atoms, an alkylaryl group having 7 to 10 carbon atoms, a halogen group, a silyl group having 1 to 6 carbon atoms, a sulfonic acid group, and a salt thereof (such as a sodium salt).

[0033] Examples of the alkyl group having 1 to 4 carbon atoms include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an isobutyl group, and a tert-butyl group.

[0034] Examples of the aryl group having 6 to 10 carbon atoms include a phenyl group and a naphthyl group.

[0035] An example of the arylalkyl group having 7 to 10 carbon atoms is a benzyl group.

[0036] Examples of the alkylaryl group having 7 to 10 carbon atoms include a tolyl group and a xylyl group.

[0037] Examples of the halogen group include a fluoro group, a chloro group, a bromo group, and an iodo group.

[0038] Examples of the silyl group having 1 to 6 carbon atoms include a trimethylsilyl group and a tert-butyldimethylsilyl group.

[0039] The aromatic dicarboxylic acid constituting the aromatic dicarboxylic acid unit other than the isophthalic acid unit is preferably an aromatic dicarboxylic acid having 8 to 20 carbon atoms which is unsubstituted or substituted with a predetermined substituent.

[0040] Examples of the aromatic dicarboxylic acid having 8 to 20 carbon atoms which is unsubstituted or substituted with a predetermined substituent include terephthalic acid, naphthalenedicarboxylic acid, 2-chloroterephthalic acid, 2-methylterephthalic acid, 5-methylisophthalic acid, and 5-sodium sulfoisophthalic acid.

[0041] The dicarboxylic acid constituting the aromatic dicarboxylic acid unit may be any dicarboxylic acid capable of forming the aromatic dicarboxylic acid unit described above, and may be an anhydride of a dicarboxylic acid or a halide of a dicarboxylic acid.

[0042] The semi-aromatic polyamide may or may not contain a dicarboxylic acid unit other than the aromatic dicarboxylic acid unit. Examples of the dicarboxylic acid unit other than the aromatic dicarboxylic acid unit include an aliphatic dicarboxylic acid unit and an alicyclic dicarboxylic acid unit.

[0043] Alicyclic dicarboxylic acid unit Examples of alicyclic dicarboxylic acids constituting the alicyclic dicarboxylic acid unit include alicyclic dicarboxylic acids having an alicyclic structure with 3 to 10 carbon atoms.

[0044] The alicyclic dicarboxylic acid is preferably an alicyclic dicarboxylic acid having an alicyclic structure with a carbon number of 5 to 10. Examples of such alicyclic dicarboxylic acids include 1,4-cyclohexanedicarboxylic acid, 1,3-cyclohexanedicarboxylic acid, and 1,3-cyclopentanedicarboxylic acid.

[0045] The alicyclic group of the alicyclic dicarboxylic acid may be unsubstituted or may have a substituent, which is the same as the substituent explained in the aromatic dicarboxylic acid unit.

[0046] In addition, the semi-aromatic polyamide may further contain units derived from a trivalent or higher polyvalent carboxylic acid, if necessary, within a range that does not impair the effects of the polyamide composition of the present embodiment. Examples of the trivalent or higher polyvalent carboxylic acid include trimellitic acid, trimesic acid, and pyromellitic acid.

[0047] The dicarboxylic acid units preferably contain terephthalic acid units in an amount of 50 mol % or more, more preferably 65 to 100 mol %, 75 to 100 mol %, 80 to 100 mol %, or 100 mol %, based on the total moles of the dicarboxylic acid units.

[0048] Aliphatic diamine units The aliphatic diamine units of the semi-aromatic polyamide include at least one unit selected from the group consisting of ethylenediamine units, trimethylenediamine units, tetramethylenediamine units, and pentamethylenediamine units. In one embodiment, the aliphatic diamine units of the semi-aromatic polyamide further include hexamethylenediamine units. In another embodiment, the aliphatic diamine units of the semi-aromatic polyamide include tetramethylenediamine units. The ethylenediamine units, trimethylenediamine units, tetramethylenediamine units, pentamethylenediamine units, and hexamethylenediamine units are represented by -NH(CH2)2NH-, -NH(CH2)3NH-, -NH(CH2)4NH-, -NH(CH2)5NH-, and -NH(CH2)6NH-, respectively.

[0049] Otherwise, the aliphatic diamine units of the semi-aromatic polyamide are similar to the aliphatic diamine units of the aliphatic polyamide. The semi-aromatic polyamide preferably contains 20 to 80 mol %, 30 to 70 mol %, or 40 to 60 mol % of aromatic dicarboxylic acid units based on all constituent units of the semi-aromatic polyamide.

[0050] The semi-aromatic polyamide is preferably a polyamide containing dicarboxylic acid units containing 50 mol % or more of terephthalic acid units relative to the total dicarboxylic acid units of the semi-aromatic polyamide, and diamine units containing diamine units having 4 to 10 carbon atoms. In this case, the total content of the terephthalic acid units and the diamine units having 4 to 10 carbon atoms in the semi-aromatic polyamide is preferably 50 mol % or more, more preferably 80 to 100 mol %, further preferably 90 to 100 mol %, and particularly preferably 100 mol %, relative to the total constituent units of the semi-aromatic polyamide.

[0051] The proportion of a predetermined monomer unit constituting the semi-aromatic polyamide can be measured by nuclear magnetic resonance spectroscopy (NMR) or the like.

[0052] Diamine Unit Examples of the diamine unit constituting the semi-aromatic polyamide include an aliphatic diamine unit and an alicyclic diamine unit.

[0053] Aliphatic diamine units Examples of the aliphatic diamine constituting the aliphatic diamine unit include linear saturated aliphatic diamines having 2 to 20 carbon atoms, and branched saturated aliphatic diamines having 3 to 20 carbon atoms. The aliphatic diamine unit contains at least one unit selected from the group consisting of an ethylenediamine unit, a trimethylenediamine unit, a tetramethylenediamine unit, and a pentamethylenediamine unit.

[0054] Examples of linear saturated aliphatic diamines having 2 to 20 carbon atoms include ethylenediamine, propylenediamine, tetramethylenediamine, pentamethylenediamine, hexamethylenediamine, heptamethylenediamine, octamethylenediamine, nonamethylenediamine, decamethylenediamine, undecamethylenediamine, dodecamethylenediamine, and tridecamethylenediamine.

[0055] Examples of branched saturated aliphatic diamines having 3 to 20 carbon atoms include 2-methylpentamethylenediamine (also referred to as 2-methyl-1,5-diaminopentane), 2,2,4-trimethylhexamethylenediamine, 2,4,4-trimethylhexamethylenediamine, 2-methyl-1,8-octanediamine (also referred to as 2-methyloctamethylenediamine), and 2,4-dimethyloctamethylenediamine.

[0056] Alicyclic diamine unit The semi-aromatic polyamide only needs to contain an aliphatic diamine unit, and may or may not further contain an alicyclic diamine unit.

[0057] Examples of alicyclic diamines constituting the alicyclic diamine unit include 1,4-cyclohexanediamine, 1,3-cyclohexanediamine, and 1,3-cyclopentanediamine.

[0058] As the semi-aromatic polyamide, polyamide 4T (PA4T) using terephthalic acid and tetramethylenediamine as main raw materials is preferable. In one embodiment, the semi-aromatic polyamide is polyamide 4T / 6T. Polyamide 4T / 6T has tetramethylenediamine units, hexamethylenediamine units, and terephthalic acid units.

[0059] The ratio of the aliphatic polyamide to the total mass of the aliphatic polyamide and the semi-aromatic polyamide is, for example, 10 to 60 mass%, 15 to 50 mass%, 20 to 50 mass%, or 30 to 50 mass%. By setting the ratio of the aliphatic polyamide to the total mass of the aliphatic polyamide and the semi-aromatic polyamide to be 10 to 60 mass%, a molded product with excellent surface appearance can be obtained.

[0060] End-capping agent The terminals of the polyamide contained in the polyamide composition of the present embodiment may be capped with a known terminal capping agent. Such a terminal capping agent can also be added as a molecular weight regulator when producing a polyamide from a dicarboxylic acid and a diamine, or from at least one selected from the group consisting of a lactam and an aminocarboxylic acid.

[0061] Examples of the terminal blocking agent include monocarboxylic acid, monoamine, acid anhydride (phthalic anhydride, etc.), monoisocyanate, monoesters, monoalcohols, etc. The terminal blocking agent is preferably monocarboxylic acid or monoamine. By blocking the terminals of the polyamide with a terminal blocking agent, the thermal stability of the molded article obtained from the polyamide composition tends to be superior.

[0062] The monocarboxylic acid that can be used as the terminal blocking agent may be any one that is reactive with the amino group that may be present at the terminal of the polyamide. The monocarboxylic acid is not limited to the following, but may be, for example, an aliphatic monocarboxylic acid, an alicyclic monocarboxylic acid, or an aromatic monocarboxylic acid. The aliphatic monocarboxylic acid may be, for example, formic acid, acetic acid, propionic acid, butyric acid, valeric acid, caproic acid, caprylic acid, lauric acid, tridecyl acid, myristic acid, palmitic acid, stearic acid, pivalic acid, or isobutyric acid. The alicyclic monocarboxylic acid may be, for example, cyclohexane carboxylic acid. The aromatic monocarboxylic acid may be, for example, benzoic acid, toluic acid, α-naphthalene carboxylic acid, β-naphthalene carboxylic acid, methylnaphthalene carboxylic acid, or phenyl acetic acid. In particular, it is preferable that the terminals of the semi-aromatic polyamide are blocked with acetic acid from the viewpoint of fluidity and mechanical strength.

[0063] The monoamine that can be used as the end-capping agent may be any monoamine that is reactive with a carboxyl group that may be present at the end of the polyamide. Examples of the monoamine include aliphatic monoamines, alicyclic monoamines, and aromatic monoamines.

[0064] Examples of the aliphatic monoamine include methylamine, ethylamine, propylamine, butylamine, hexylamine, octylamine, decylamine, stearylamine, dimethylamine, diethylamine, dipropylamine, and dibutylamine.

[0065] Examples of the alicyclic monoamine include cyclohexylamine and dicyclohexylamine.

[0066] Examples of aromatic monoamines include aniline, toluidine, diphenylamine, and naphthylamine.

[0067] Polyamide compositions containing polyamide end-capped with an end-capping agent tend to have better heat resistance, flowability, toughness, low water absorption, and rigidity.

[0068] Polyamide manufacturing method When producing the polyamides (aliphatic polyamides and semi-aromatic polyamides) contained in the polyamide composition of the present embodiment, the amount of dicarboxylic acid added and the amount of diamine added are preferably approximately the same molar amount. Taking into consideration the amount of diamine that escapes to the outside of the reaction system during the polymerization reaction in the molar ratio, the molar amount of the total diamines relative to the molar amount of the total dicarboxylic acids is preferably 0.9 to 1.2, more preferably 0.95 to 1.1, and even more preferably 0.98 to 1.05.

[0069] The method for producing polyamide includes, for example, the following polymerization step (1) or (2). (1) A step of polymerizing a combination of a dicarboxylic acid constituting a dicarboxylic acid unit and a diamine constituting a diamine unit to obtain a polymer. (2) A step of polymerizing one or more members selected from the group consisting of lactam constituting the lactam unit and aminocarboxylic acid constituting the aminocarboxylic acid unit to obtain a polymer.

[0070] The method for producing polyamide preferably further includes, after the polymerization step, an increasing step of increasing the degree of polymerization of the polyamide. If necessary, the method may include, after the polymerization step and the increasing step, a capping step of capping the ends of the obtained polymer with a terminal capping agent.

[0071] Specific examples of the method for producing polyamide include various methods such as the following first to fourth methods. The first method is to heat an aqueous solution or suspension of one or more selected from the group consisting of a dicarboxylic acid-diamine salt, a mixture of a dicarboxylic acid and a diamine, a lactam, and an aminocarboxylic acid, and polymerize the resulting solution while maintaining the molten state (hereinafter, this may be referred to as the "thermal melt polymerization method"). Second: A method in which the degree of polymerization of polyamide obtained by the hot melt polymerization method is increased while maintaining the polyamide in a solid state at a temperature below the melting point (hereinafter sometimes referred to as "hot melt polymerization / solid-state polymerization method"). Third: A method of polymerizing one or more selected from the group consisting of dicarboxylic acid-diamine salts, mixtures of dicarboxylic acids and diamines, lactams, and aminocarboxylic acids while maintaining the solid state (hereinafter, sometimes referred to as "solid-state polymerization method"). Fourth: A method of polymerization using a dicarboxylic acid halide component equivalent to a dicarboxylic acid and a diamine component (hereinafter, sometimes referred to as a "solution method").

[0072] A specific method for producing polyamide is preferably a method including a hot melt polymerization method. When producing polyamide by hot melt polymerization, it is preferable to maintain the molten state until the polymerization is completed. In order to maintain the molten state, it is necessary to produce the polyamide composition under polymerization conditions suitable for the composition. Examples of the polymerization conditions include the following conditions. First, the polymerization pressure in the hot melt polymerization method is set to 14 to 25 kg / cm. 2 (gauge pressure) and continue heating. Next, the pressure in the vessel is controlled to atmospheric pressure (gauge pressure is 0 kg / cm 2 ) over 30 minutes or more until the blood pressure drops to 0.

[0073] In the method for producing polyamide, the polymerization form is not particularly limited, and may be a batch type or a continuous type. A known apparatus may be used as the polymerization apparatus used for producing polyamide. Specific examples of the polymerization apparatus include an autoclave type reactor, a tumbler type reactor, and an extruder type reactor (such as a kneader).

[0074] As a method for producing polyamide, a method for producing polyamide by a batch-type hot melt polymerization method will be specifically exemplified below.

[0075] First, raw material components of polyamide (a combination of dicarboxylic acid and diamine, and, if necessary, at least one selected from the group consisting of lactam and aminocarboxylic acid) are mixed with An aqueous solution containing about 40-60% by mass is prepared. The aqueous solution is then concentrated to about 65-90% by mass in a concentration tank operated at a temperature of 110-180°C and a pressure of about 0.035-0.6 MPa (gauge pressure) to obtain a concentrated solution. The concentrated solution obtained is then transferred to an autoclave, and heating is continued until the pressure in the autoclave reaches about 1.2-2.2 MPa (gauge pressure). The pressure in the autoclave is then maintained at about 1.2-2.2 MPa (gauge pressure) while removing at least one of water and gas components. When the temperature reaches about 220-260°C, the pressure is reduced to atmospheric pressure (gauge pressure: 0 MPa). After the pressure in the autoclave is reduced to atmospheric pressure, the pressure can be reduced as necessary to effectively remove by-product water. The autoclave is then pressurized with an inert gas such as nitrogen, and the polyamide melt is extruded from the autoclave as a strand. The extruded strand is cooled and cut to obtain polyamide pellets.

[0076] Polyamide properties Polyamide polymer end The polymer ends of the polyamide contained in the polyamide composition of the present embodiment are not particularly limited, but can be classified and defined as follows into the following first to fourth types: First: amino end, Second: carboxy end, Third: end due to a capping agent, Fourth: other end. The first: amino terminus is a polymer terminus having an amino group (-NH2 group) and is derived from a diamine unit. The second: carboxyl end is a polymer end having a carboxy group (-COOH group) and is derived from a dicarboxylic acid unit. The third terminal formed by a capping agent is a terminal formed when a capping agent is added during polymerization. Examples of the capping agent include the above-mentioned terminal capping agents. Fourth: Other terminals are polymer terminals that are not classified into the above-mentioned first to third types. Specific examples of other terminals include terminals generated by deammonia reaction of amino terminals, terminals generated by decarboxylation of carboxyl terminals, etc.

[0077] Acid-modified elastomer The polyamide composition of the present embodiment may further contain an acid-modified elastomer in addition to the polyamide. By containing the acid-modified elastomer, the polyamide composition can be made more excellent in toughness and appearance.

[0078] The acid-modified elastomer is, for example, an elastomer such as ethylene vinyl acetate (EVA), ethylene acrylate copolymer (EEA), polyethylene (PE), polypropylene (PP), or a styrene-based elastomer (styrene-ethylene-butylene-styrene copolymer: SEBS, styrene-ethylene-propylene-styrene copolymer: SEPS, etc.) modified with maleic anhydride. From the viewpoint of heat resistance, polyolefin, SEBS, or SEPS modified with acid is particularly preferred. In one embodiment, the acid-modified elastomer is one or more types of acid-modified elastomers selected from the group consisting of EVA, EEA, PE, PP, SEBS, and SEPS. In another embodiment, the acid-modified elastomer is one or more types of maleic anhydride-modified elastomers selected from the group consisting of EVA, EEA, PE, PP, SEBS, and SEPS.

[0079] The content of the acid-modified elastomer is preferably 1 to 20 mol%, more preferably 2 to 10 mol%, further preferably 2 to 6 mol%, and particularly preferably 2 to 5 mol% based on the total mass of the entire polyamide composition. By making the content of the acid-modified elastomer 1 mol% or more, it is possible to obtain a polyamide composition that suppresses excessive moisture absorption. On the other hand, by making the content of the acid-modified elastomer 20 mol% or less, it is possible to obtain a molded product with better surface appearance.

[0080] filling material The polyamide composition of the present embodiment may further contain a filler in addition to the polyamide and the acid-modified elastomer. By containing the filler, the polyamide composition can have more excellent mechanical properties such as toughness and rigidity.

[0081] Examples of the filler contained in the polyamide composition of the present embodiment include fibrous fillers such as glass fiber and carbon fiber. In addition, for example, the fillers described in JP-A-2023-035802 may be used. As the filler, glass fiber or carbon fiber is preferable.

[0082] The number average fiber diameter and weight average fiber length of the filler can be measured using the method described in JP 2023-035802 A.

[0083] The content of the filler in the polyamide composition is preferably 1 to 80 mass%, more preferably 5 to 70 mass%, further preferably 10 to 60 mass%, particularly preferably 15 to 55 mass%, and most preferably 20 to 50 mass%, based on the total mass of the polyamide composition. When the content of the filler is 1 mass% or more, the mechanical properties such as strength and rigidity of the polyamide composition tend to be further improved. On the other hand, when the content of the filler is 80 mass% or less, a polyamide composition having better moldability tends to be obtained.

[0084] Other additives The polyamide composition of the present embodiment may contain other additives commonly used in polyamides, such as moldability improvers, deterioration inhibitors, nucleating agents, and heat stabilizers, within the range that does not impair the effects of the polyamide composition of the present embodiment.

[0085] Moldability improver Examples of the moldability improver include those described in JP-A-2022-115097.

[0086] Deterioration inhibitor Examples of the deterioration inhibitor include those described in JP-A-2021-050323.

[0087] Nucleating Agent Examples of nucleating agents include those described in JP-A-2021-050323.

[0088] Heat stabilizer Examples of the heat stabilizer include those described in JP-A-2023-028935 and JP-A-2021-050323.

[0089] Method for producing polyamide composition The method for producing the polyamide composition of the present embodiment is not particularly limited as long as it is a method for mixing an aliphatic polyamide, a semi-aromatic polyamide, and an optional component. For example, the method described in JP 2023-035802 A can be mentioned. The blending amount of each component when producing the polyamide composition of the present embodiment is the same as the content of each component in the polyamide composition described above.

[0090] The temperature of the melt kneading is preferably about 1°C to 100°C higher than the melting point of the semi-aromatic polyamide, and more preferably about 10°C to 50°C higher than the melting point of the semi-aromatic polyamide. The shear rate in the kneader is 100 sec -1 The average residence time during kneading is preferably about 0.5 minutes or more and 5 minutes or less. The melt kneading apparatus may be any known apparatus, for example, the method described in JP-A-2023-028935.

[0091] molded product The molded article of the present embodiment is obtained by molding the polyamide composition of the above embodiment. That is, the molded article of the present embodiment is a molded body using the polyamide composition of the present embodiment.

[0092] The method for obtaining a molded product is not particularly limited, and a known molding method can be used. Examples of the known molding method include the method described in JP-A-2022-115097.

[0093] Purpose The molded article of the present embodiment contains the polyamide composition of the above embodiment, and is excellent in heat resistance, toughness, appearance of the molded article, and rigidity retention when absorbing moisture, and can be used in various applications. The molded article of the present embodiment can be preferably used in, for example, the automotive field, the electrical and electronic field, the mechanical and industrial field, the office equipment field, and the aviation and space field. The molded article of the present embodiment can be preferably used for a rolling bearing. In one embodiment, the molded article is a rolling bearing. EXAMPLES

[0094] The present invention will be described in detail below with reference to specific examples and comparative examples, but the present invention is not limited to the following examples.

[0095] Each of the components of the polyamide composition used in the present examples and comparative examples will be described below.

[0096] polyamide Polyamide 4T / 6T, synthesized as described below, indicated as "4T / 6T" in the table Polyamide 9T / 2Me8T (Kuraray, Genestar TM N1000, indicated as "9T / 2Me8T" in the table Polyamide 6T / 6I (Mitsui Chemicals, Arlen A3000), indicated as "6T / 6I" in the table Polyamide 6I, synthesized by the method described below, is indicated as "6I" in the table. Polyamide 66, synthesized as described below, indicated as "66" in the table

[0097] Acid-modified elastomer Acid-modified polyolefin resin (manufactured by Mitsui Chemicals, Inc., model number: TAFMER (registered trademark) MH5020), indicated as "MH5020" in the table

[0098] filling material Carbon fiber (manufactured by Teijin Ltd., product name "HT C413"), indicated as "HT C413" in the table

[0099] Polyamide manufacturing The methods for producing the semi-aromatic polyamides are described in detail below. The aliphatic polyamides and semi-aromatic polyamides obtained by the methods described below were dried in a nitrogen stream to adjust the moisture content to about 0.2% by mass, and then used as raw materials for the polyamide compositions in the examples and comparative examples described below.

[0100] Synthesis Example 1: Synthesis of polyamide 4T / 6T The heating time was adjusted with reference to PA-2 in paragraph

[0052] of JP2020-513438A, and a semi-aromatic polyamide (polyamide 4T / 6T) was obtained. The content of terephthalic acid units in the dicarboxylic acid units of the obtained polyamide 4T / 6T was 100 mol%.

[0101] Synthesis Example 2: Synthesis of Polyamide 6I A semi-aromatic polyamide (polyamide 6I) was obtained in the same manner as in the synthesis of polyamide 6I described in paragraph

[0247] of JP 2023-011541 A. The content of isophthalic acid units in the dicarboxylic acid units of the obtained polyamide 6I was 100 mol%.

[0102] Synthesis Example 3: Synthesis of Polyamide 66 An aliphatic polyamide (polyamide 66) was obtained in the same manner as in the synthesis of polyamide 66 described in paragraph

[0147] of JP2020-056003A.

[0103] Properties and Evaluation The polyamide composition pellets obtained in the Examples and Comparative Examples were dried in a nitrogen stream to reduce the moisture content in the polyamide composition to 500 ppm or less. Next, the pellets of each polyamide composition with the adjusted moisture content were used to measure various physical properties and perform various evaluations using the following methods.

[0104] Melting peak temperatures Tm1 and Tm2 of polyamide composition (℃) The measurement was performed using Diamond-DSC manufactured by PERKIN-ELMER in accordance with JIS-K 7121. The measurement conditions were as follows: under a nitrogen atmosphere, about 10 mg of the polyamide composition was heated to 280°C or more and 370°C or less according to the melting point (Tm) of the sample at a heating rate of 20°C / min (first heating), and the highest endothermic peak (melting peak) melting peak temperature was defined as Tm1 (°C). The melting peak temperature Tm2 of the polyamide was measured as follows. After the first heating, the temperature was kept in the molten state at the highest temperature of the heating for 1 minute, then the temperature was lowered to 30°C at a heating rate of 20°C / min, and held at 30°C for 1 minute. After that, the temperature was raised in the same manner at a heating rate of 20°C / min (second heating), and the highest endothermic peak temperature was defined as the melting peak temperature Tm2 of the polyamide composition.

[0105] ΔT Under the same conditions as above, the temperature of the exothermic peak (crystallization peak) appearing when the temperature was decreased at a rate of 20° C. / min was defined as the crystallization peak temperature Tc (° C.), and the difference between Tm2 and Tc was defined as ΔT.

[0106] tan δ peak temperature Using a PS40E injection molding machine manufactured by Nissei Kogyo Co., Ltd., a molded product was molded according to JIS-K7139 under the injection molding conditions of a cylinder temperature of 340°C, a mold temperature of 120°C, injection for 10 seconds, and cooling for 10 seconds. The molded product was measured under the following conditions using a dynamic viscoelasticity evaluation device (EPLEXOR500N manufactured by GABO Co., Ltd.).

[0107] (Measurement conditions) Measurement mode: Tensile Measurement frequency: 8.00Hz Heating rate: 3℃ / min Temperature range: -100℃ to 250℃

[0108] The ratio of the storage modulus E1 to the loss modulus E2 (E2 / E1) was defined as tan δ, and the highest temperature was defined as the tan δ peak temperature.

[0109] Evaluation 1: Surface gloss Using a Toshiba Machine IS150E injection molding machine, the cylinder temperature was set at 330° C., the mold temperature was set at 120° C., and the injection pressure and speed were appropriately adjusted so that the filling time was approximately 1.5 seconds to obtain an injection molded plate of 100×90×3 mm. The 60° gloss of this plate was measured using a gloss meter (HORIBA IG320) in accordance with JIS-K7150.

[0110] Evaluation 2: Flexural modulus A multipurpose test piece (type A) was cut to prepare a bending test piece (80 mm x 10 mm x 4 mm strip). The bending modulus of elasticity of the test piece was measured in accordance with ASTM D790 using a bending tester (Toyo Seiki Co., Ltd.: UTM25) at 23°C and a crosshead speed of 5 mm / min.

[0111] Evaluation 3: Elasticity retention rate A multipurpose test piece (A type) was conditioned in accordance with JIS K-7143 and subjected to bending test measurement according to the method described therein. The elastic modulus retention was calculated using the following formula. Flexural modulus retention rate (%) = (flexural modulus of test piece when hydrated / flexural modulus of test piece when completely dry) x 100

[0112] Evaluation 4: Bending strain retention rate A multipurpose test piece (A type) was conditioned in accordance with JIS K-7143 and subjected to bending test measurement according to the method described therein. The elastic modulus retention was calculated using the following formula. Bending strain retention rate (%) = (bending strain of test piece when hydrated / bending strain of test piece when completely dry) x 100

[0113] Preparation of polyamide compositions Example 1 Using a TEM 35 mm twin-screw extruder (set temperature: 350°C, screw rotation speed: 300 rpm) manufactured by Toshiba Machine Co., Ltd., polyamide was fed from a top feed port provided at the most upstream part of the extruder. In addition, a filler was fed from a side feed port on the downstream side of the extruder (in a state where the resin fed from the top feed port was fully melted). Next, the molten kneaded material extruded from the die head was cooled in a strand shape and pelletized to obtain pellets of a polyamide composition. The blending amounts were as shown in Table 1.

[0114] In addition, the obtained polyamide composition pellets with the adjusted moisture content were molded into multipurpose test pieces (A-type, dumbbell-shaped tensile test pieces) in accordance with ISO3167 using an injection molding machine (PS-40E, manufactured by Nissei Plastics Co., Ltd.). The dimensions of the multipurpose test piece are: total length ≧170 mm, distance between tabs 109.3±3.2 mm, length of parallel part 80±2 mm, radius of shoulder 24±1 mm, width of end 20±0.2 mm, width of central parallel part 10±0.2 mm, and thickness 4±0.2 mm. Specific injection molding conditions were set as follows: injection and pressure holding time: 5 seconds, cooling time: 5 seconds, mold temperature: 120°C, and cylinder temperature: 350°C.

[0115] The physical properties of the molded products produced were measured and evaluated. The evaluation results are shown in Table 1.

[0116] [Table 1]

[0117] Examples 2 to 4, Comparative Examples 1 to 6 Except for using the composition shown in Table 1, the production was carried out in the same manner as in Example 1. The evaluation results are shown in Table 1.

[0118] As can be seen from Table 1, the polyamide compositions containing PA4T / 6T and PA66 in Examples 1 to 3 gave molded articles having good gloss values, flexural modulus, flexural modulus after absorbing moisture, and flexural strain retention.

[0119] In the case of the polyamide composition containing the acid-modified elastomer of Example 4, a molded article having an even higher gloss value was obtained.

[0120] Among the polyamide compositions having a ratio of terephthalic acid:aliphatic dicarboxylic acid of 7:3 to 5:5 among the polyamide components, the gloss value, flexural modulus retention rate after moisture absorption, and flexural strain retention rate after moisture absorption were improved in Example 2, and the gloss value, flexural modulus, and flexural strain retention rate after moisture absorption were improved in Example 3.

[0121] On the other hand, in the compositions not containing PA66 (Comparative Examples 1 to 3), good results were not obtained in terms of toughness, gloss value, and elastic modulus retention rate when absorbing moisture. Also, in Comparative Example 2, in which only the acid-modified elastomer was added, the improvement in gloss value as in Example 4 was not observed.

[0122] In Comparative Example 4, in which the ratio of the aliphatic dicarboxylic acid to the total mass of terephthalic acid and the aliphatic dicarboxylic acid was outside the range of 30 to 50% by mass, the flexural modulus retention rate upon moisture absorption decreased.

[0123] From Comparative Examples 5 and 6, in the case of a skeleton not containing tetramethylenediamine in the aromatic polyamide, good results were not obtained even when the ratio of terephthalic acid:aliphatic dicarboxylic acid was 7:3 to 5:5.

[0124] From the above, it is clear that the polyamide composition of the present embodiment can provide a molded product that is excellent in heat resistance, rigidity, suppression of deterioration in rigidity and toughness upon moisture absorption, and surface appearance during molding. [Industrial Applicability]

[0125] According to the polyamide composition of the present embodiment, it is possible to provide a polyamide composition which, when formed into a molded article, is excellent in heat resistance, rigidity, suppression of deterioration in rigidity and toughness upon moisture absorption, and surface appearance upon molding. Therefore, the molded article of the present embodiment can be used for rolling bearings, etc.

Claims

1. aliphatic polyamides and semi-aromatic polyamides, The aliphatic polyamide contains an aliphatic dicarboxylic acid unit and an aliphatic diamine unit, The semi-aromatic polyamide comprises an aromatic dicarboxylic acid unit and an aliphatic diamine unit, The aliphatic diamine unit of the semi-aromatic polyamide includes at least one unit selected from the group consisting of an ethylenediamine unit, a trimethylenediamine unit, a tetramethylenediamine unit, and a pentamethylenediamine unit, A polyamide composition, in which the difference (Tm2-Tc) between a melting peak temperature Tm2 and a crystallization temperature Tc measured at a heating rate of 20°C / min in differential scanning calorimetry according to JIS-K7121 is 35°C or more and less than 45°C.

2. 2. The polyamide composition of claim 1, wherein said aromatic dicarboxylic acid units consist exclusively of terephthalic acid units.

3. 2. The polyamide composition according to claim 1, wherein a ratio of the mass of the aliphatic polyamide to a total mass of the aliphatic polyamide and the semi-aromatic polyamide is 30 to 50 mass%.

4. 2. The polyamide composition of claim 1, wherein said aliphatic dicarboxylic acid units consist exclusively of adipic acid units.

5. 2. The polyamide composition of claim 1, wherein the aliphatic diamine units of the semi-aromatic polyamide further comprise hexamethylene diamine units.

6. 2. The polyamide composition of claim 1, wherein the aliphatic diamine units of the semi-aromatic polyamide comprise tetramethylene diamine units.

7. 2. The polyamide composition according to claim 1, comprising 1 to 20 mol % of the acid-modified elastomer based on the total mass of the polyamide composition.

8. 10. The polyamide composition of claim 1, further comprising a filler, said filler being a fibrous filler.

9. 9. The polyamide composition of claim 8, wherein the fibrous filler comprises glass fiber or carbon fiber.

10. 9. The polyamide composition of claim 8, wherein the fibrous filler comprises carbon fiber.

11. The polyamide composition according to claim 1, wherein the melting peak temperature Tm2 is 300°C or higher.

12. 2. The polyamide composition according to claim 1, which has a tan δ peak temperature of 100 to 140° C. in differential scanning calorimetry according to JIS-K7121.

13. A molded article obtained by molding the polyamide composition according to any one of claims 1 to 12.

14. The molded article according to claim 13, wherein the molded article is a rolling bearing.

Citation Information

Patent Citations

  • Apparatus for recovering pulp fiber in pulp sludge

    JP1977070106A

  • Polyamide copolymers, preparation process and molded parts made therefrom

    JP7188706B2