Polyester resin emulsion for toner, resin particle, and toner
The polyester resin emulsion for toner with a specific OHV/AV ratio and alcohol composition ensures uniform shell layer formation on core particles, enhancing mechanical durability and cohesiveness, addressing issues of non-uniformity and peeling in existing core-shell toners.
Patent Information
- Application Number
- JP2023084943
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-23
- Publication Date
- 2024-12-05
AI Technical Summary
Existing toners with a core-shell structure face issues with mechanical durability due to non-uniform distribution and peeling of the shell layer, which affects cohesiveness and uniformity with core particles, especially under high temperature and humidity conditions.
A polyester resin emulsion for toner is developed with a specific hydroxyl value (OHV) to acid value (AV) ratio of 0.20 to 0.60, using trivalent or tetravalent alcohols with a linear or branched saturated fatty acid skeleton of 4 to 6 carbon atoms, ensuring uniform aggregation and adhesion of shell particles on core particles.
The solution results in a toner with excellent mechanical durability and cohesiveness, maintaining a uniform shell layer even under harsh conditions, thereby improving image quality and stability.
Smart Images

Figure 2024168362000011 
Figure 2024168362000001 
Figure 2024168362000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a polyester resin emulsion for a toner, a resin particle, and a toner. [Background technology]
[0002] Toners used in electrophotographic image forming apparatuses are required to have excellent low-temperature fixing properties in response to market demands for energy saving. In addition, toners with excellent blocking resistance, which prevents toner particles from fusing together even in harsh environments such as high temperature and humidity, and toners with excellent mechanical durability that can fully withstand the stress associated with high-speed output of image forming apparatuses are also required. In recent years, in order to provide heat resistance and mechanical durability, toners having a so-called core-shell structure, in which a shell layer is provided on the surface of the toner, have been developed. Various techniques for forming a core-shell toner have been proposed and put to practical use, but chemical toners in which polyester resins with excellent low-temperature fixing properties are used for both the core particles and the shell particles are mainstream.
[0003] For example, a toner for electrostatic charge development has been proposed in which polyethylene terephthalate (PET) is blended with respect to the resin in the core portion and the shell portion (see, for example, Patent Document 1). Summary of the Invention [Problem to be solved by the invention]
[0004] An object of the present invention is to provide a polyester resin emulsion for toner which has a core-shell structure and can provide a toner having excellent mechanical durability, and which is excellent in the cohesion of shell particles to core particles and in the uniformity thereof. [Means for solving the problem]
[0005] The polyester resin emulsion for toner of the present invention as a means for solving the above problems is as follows: A polyester resin emulsion for toner, comprising resin particles (S) containing a polyester resin (A) obtained by polycondensation of an alcohol component and a carboxylic acid component, dispersed in an aqueous medium, The alcohol component contains a trihydric or tetrahydric alcohol having a linear or branched saturated fatty acid skeleton having 4 to 6 carbon atoms, The polyester resin (A) has a characteristic that a ratio (OHV / AV) of a hydroxyl value (OHV) of the polyester resin (A) to an acid value (AV) of the polyester resin (A) is 0.20 or more and 0.60 or less. Effect of the Invention
[0006] According to the present invention, it is possible to obtain a toner having a core-shell structure and excellent mechanical durability, and it is also possible to provide a polyester resin emulsion for a toner which is excellent in the cohesion of shell particles to core particles and in the uniformity thereof. [Brief description of the drawings]
[0007] [Figure 1] FIG. 1 is a schematic diagram showing an example of an image forming apparatus according to the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0008] It is known that in a toner having a core-shell structure, it is very important that the shell layer formed on the surface of the core particle is uniformly arranged and has no defective portions from the viewpoint of the low-temperature fixing property, heat-resistant storage stability, and mechanical durability of the toner. More specifically, if the shell particles (shell layer) are not arranged uniformly and without defective portions on the surface of the core particle, the mechanical durability of the toner is reduced, and the shell layer may peel off from the core particle due to development stress in an image forming device, etc., and each toner performance may be significantly deteriorated.
[0009] In the conventional technology described in Patent Document 1, polyethylene terephthalate (PET) is introduced into the shell portion of a toner having a core-shell structure to improve the durability of the toner and suppress exposure of wax on the toner surface. However, there is concern that when polyethylene terephthalate (PET) is introduced into the shell particles that form the shell portion, the hydrophobicity of the shell particles is reduced, which reduces the cohesiveness of the core particles and shell particles, making it difficult to form a uniform shell layer on the surface of the core particles.
[0010] As a result of intensive research, the present inventors have found that when forming a core-shell structure, i.e., when aggregating shell particles to the surface of a core particle, by using an emulsion in which a polyester resin having a specific ratio (hydroxyl value (OHV) / acid value (AV)) is dispersed in an aqueous medium, the aggregability and aggregating uniformity of shell particles to core particles are improved, and a toner with excellent mechanical durability can be obtained. Specifically, this is as follows.
[0011] When preparing a toner having a core-shell structure by aggregating shell particles on the surface of a core particle, a resin emulsion containing shell particles is dispersed in a dispersion liquid in which the core particles are dispersed, and aggregation is carried out by utilizing collision energy between particles caused by stirring, thermal energy caused by heating, and aggregating agents such as inorganic metal salts and surfactants. Here, the characteristics of the resin constituting the shell particles not only affect the stability of the emulsion and the aggregability with the core particles, but also affect the adhesion with the core particles when the shell particles are heat-fused to form a shell layer. Representative properties of the resin constituting the shell particles include acid value (AV), hydroxyl value (OHV), hydrophilicity / hydrophobicity, affinity with solvent, melt viscosity, etc. Among these, it has been found that when the ratio (OHV / AV) of the hydroxyl value (OHV) to the acid value (AV) in the resin constituting the shell particles is 0.20 to 0.60, the shell particles have good cohesion to the core particles, are easily cohere and arranged uniformly on the surface of the core particles (cohesion uniformity), and the shell particles can form a shell layer without peeling off even during heat fusion. The ratio (OHV / AV) can be controlled by using a trihydric or tetrahydric alcohol having a skeleton of a linear or branched saturated fatty acid having 4 to 6 carbon atoms as the alcohol component in the resin.
[0012] The present invention will now be described in detail.
[0013] (Polyester resin emulsion for toner) The polyester resin emulsion for toner of the present invention is an emulsion in which resin particles (S) containing a polyester resin (A) are dispersed in an aqueous medium, and may contain other resins and other components as necessary.
[0014] <Resin particles (S)> The resin particles (S) contain a polyester resin (A) and may contain other components as necessary.
[0015] <<Polyester resin (A)>> The polyester resin (A) is a polyester resin obtained by polycondensation of an alcohol component and a carboxylic acid component, and may contain other alcohols, repeating units derived from polyethylene terephthalate (PET), and other components as necessary.
[0016] <<<Alcohol content>>> The alcohol component contains a trihydric or tetrahydric alcohol having a linear or branched saturated fatty acid skeleton having 4 to 6 carbon atoms. In this specification, "a trihydric or tetrahydric alcohol having a carbon number of 4 to 6 linear or branched saturated fatty acid as a skeleton" may be simply referred to as "alcohol". Note that alcohols that do not fall under the category of "a trihydric or tetrahydric alcohol having a carbon number of 4 to 6 linear or branched saturated fatty acid as a skeleton" may be referred to as "other alcohols". In this specification, the term "straight-chain" refers to a structure that has no bonds between carbon atoms other than a carbon chain (hereinafter sometimes referred to as the "main chain") that connects the minimum number of two oxygen atoms appropriately selected from among the oxygen atoms derived from the hydroxyl group in the monomer unit of the alcohol component. In this specification, the term "branched" refers to a structure having a carbon-carbon bond in addition to the main chain.
[0017] When the polyester resin (A) contains, as an alcohol component, a trihydric or tetrahydric alcohol having a linear or branched saturated aliphatic backbone having 4 to 6 carbon atoms, the hydroxyl value (OHV) of the polyester resin (A) can be controlled and the cohesiveness and adhesion to the core particles can be improved.
[0018] The alcohol is not particularly limited as long as it has a linear or branched saturated fatty acid skeleton having 4 to 6 carbon atoms and is trivalent or tetravalent, and can be appropriately selected depending on the purpose. Examples of the alcohol include trivalent aliphatic alcohols having 4 to 6 carbon atoms and tetravalent aliphatic alcohols having 4 to 6 carbon atoms. Examples of the trihydric aliphatic alcohol having 4 to 6 carbon atoms include 1,2,3-butanetriol, 1,2,4-butanetriol, trimethylolethane, 1,2,3-pentanetriol, 1,2,4-pentanetriol, 1,2,5-pentanetriol, 1,3,5-pentanetriol, 2,3,4-pentanetriol, trimethylolpropane, 1,2,3-hexanetriol, 1,2,6-hexanetriol, 1,3,5-hexanetriol, and 2-isopropylpropane-1,2,3-triol. Examples of the tetrahydric aliphatic alcohol having 4 to 6 carbon atoms include pentaerythritol, 1,2,3,4-butanetetraol, 1,2,3,4-pentanetetraol, 1,2,3,5-pentanetetraol, 1,2,4,5-pentanetetraol, 1,2,4,5-hexanetetraol, and 1,2,5,6-hexanetetraol. These alcohols may be used alone or in combination of two or more.
[0019] The content of the alcohol is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 0.5 mol % to 10 mol % and more preferably 2 mol % to 5 mol % based on the total amount of alcohol components in the polyester resin (A). When the content of the alcohol is 0.5 mol % or more based on the total amount of alcohol components in the polyester resin (A), this is advantageous in that it can solve the problem that the cohesion of the shell particles to the core particles is insufficient, resulting in an increase in shell particles that are not incorporated into the shell layer. When the content of the alcohol is 10 mol % or less based on the total amount of alcohol components in the polyester resin (A), the branched chains of the polyester resin (A) are increased, and the melt viscosity of the shell layer in the toner is reduced, which causes problems such as insufficient heat-resistant storage stability and hot offset resistance to be obtained, and this is preferable.
[0020] <<<Carboxylic Acid>>> The carboxylic acid is not particularly limited and can be appropriately selected depending on the purpose. For example, aliphatic dicarboxylic acids or anhydrides such as succinic acid, adipic acid, sebacic acid, azelaic acid, dodecanedioic acid, maleic acid, citraconic acid, itaconic acid, alkenylsuccinic acid, and fumaric acid; 1,2,4-butanetricarboxylic acid, 1,2,5-hexanetricarboxylic acid, 1,3-dicarboxy-2-methyl-2-methylenecarboxypropane, tetra(methylenecarboxy)methane, 1,2,7,8-octyloxy-2-methyl-2-methylenecarboxypropane, tetra(methylenecarboxy)methane ... Examples of the aromatic dicarboxylic acids include trivalent or higher aliphatic carboxylic acids or their anhydrides, such as butanetetracarboxylic acid; phthalic acid, isophthalic acid, terephthalic acid, naphthalenedicarboxylic acid, and the like; and trivalent or higher aromatic carboxylic acids or their anhydrides, such as trimellitic acid, pyromellitic acid, 1,2,4-benzenetricarboxylic acid, 1,2,5-benzenetricarboxylic acid, 2,5,7-naphthalenetricarboxylic acid, 1,2,4-naphthalenetricarboxylic acid, and the like, and partial lower alkyl esters. These carboxylic acids may be used alone or in combination of two or more.
[0021] The method for polycondensation of the alcohol component and the carboxylic acid component is not particularly limited and can be appropriately selected depending on the purpose. For example, the method can be performed at a temperature of 180°C to 250°C in an inert gas atmosphere in the presence of an esterification catalyst.
[0022] The esterification catalyst is not particularly limited and can be appropriately selected depending on the purpose. Examples of the esterification catalyst include titanium compounds and tin(II) compounds that do not have an Sn-C bond. These esterification catalysts may be used alone or in combination of two or more kinds.
[0023] The titanium compound is not particularly limited and can be appropriately selected depending on the purpose. Examples thereof include titanium diisopropylate bistriethanol aminate, titanium diisopropylate bistriethanol aminate, titanium dipentylate bistriethanol aminate, titanium diethylate bistriethanol aminate, titanium dihydroxyoctylate bistriethanol aminate, titanium distearate bistriethanol aminate, titanium triisopropylate triethanol aminate, titanium monopropylate tris(triethanol aminate), tetra-n-butyl titanate, tetrapropyl titanate, tetrastearyl titanate, tetramyristyl titanate, tetraoctyl titanate, dioctyl dihydroxyoctyl titanate, and dimyristyl dioctyl titanate. Among these, from the viewpoint of high activity and ability to reduce low molecular weight components in the polyester resin, titanium compounds having a Ti-O bond are preferred, and compounds having an alkoxy group, alkenyloxy group, or acyloxy group having a total of 1 to 28 carbon atoms are more preferred.
[0024] The content of the titanium compound is not particularly limited and can be appropriately selected depending on the purpose. From the viewpoint of controllability of the reaction rate in the polymerization and ensuring the quality of the polyester resin, the content is preferably 0.01 parts by mass or more and 1.0 parts by mass or less, and more preferably 0.1 parts by mass or more and 0.5 parts by mass or less, relative to 100 parts by mass of the total amount of the alcohol component and the carboxylic acid component.
[0025] The tin(II) compound not having an Sn-C bond is not particularly limited and can be appropriately selected depending on the purpose, but a tin(II) compound having an Sn-O bond or a tin(II) compound having an Sn-X (X represents a halogen atom) bond is preferred, and a tin(II) compound having an Sn-O bond is more preferred. Examples of tin(II) compounds having an Sn-O bond include tin(II) oxalate, tin(II) acetate, tin(II) octanoate, tin(II) 2-ethylhexanoate, tin(II) laurate, tin(II) stearate, tin(II) oleate, and other tin(II) carboxylates having a carboxylic acid group having 2 to 28 carbon atoms; alkoxytin(II) having an alkoxy group having 2 to 28 carbon atoms, such as octyloxytin(II), lauroxytin(II), stearoxytin(II), and oleyloxytin(II); tin(II) oxide; and tin(II) sulfate. Examples of the tin(II) compound having the Sn-X bond include tin(II) halides such as tin(II) chloride and tin(II) bromide.
[0026] The content of the tin(II) compound is not particularly limited and can be appropriately selected depending on the purpose. From the viewpoint of controllability of the reaction rate in the polymerization and ensuring the quality of the polyester resin, the content is preferably 0.01 parts by mass or more and 1.0 parts by mass or less, and more preferably 0.1 parts by mass or more and 0.5 parts by mass or less, relative to 100 parts by mass of the total amount of the alcohol component and the carboxylic acid component.
[0027] When the titanium compound and the tin (II) compound are used in combination, the total content of the titanium compound and the tin (II) compound is not particularly limited and can be appropriately selected depending on the purpose. From the viewpoint of controllability of the reaction rate in the polymerization and ensuring the quality of the polyester resin, however, the total content of the titanium compound and the tin (II) compound is preferably 0.01 parts by mass or more and 1.0 parts by mass or less, and more preferably 0.1 parts by mass or more and 0.5 parts by mass or less, per 100 parts by mass of the total amount of the alcohol component and the carboxylic acid component.
[0028] <<<Other alcohol>>> The polyester resin (A) in the present invention may contain other alcohols in addition to the above alcohols. The other alcohol is not particularly limited and can be appropriately selected depending on the purpose. For example, aliphatic diols such as ethylene glycol, 1,2-propanediol, 1,3-propanediol, 1,4-butanediol, 2,3-butanediol, 3-methyl-1,5-pentanediol, 1,6-hexanediol, neopentyl glycol, 2-ethyl-1,3-hexanediol, 1,8-octanediol, 1,10-decanediol, and 1,12-dodecanediol; diols having an oxyalkylene group such as diethylene glycol, triethylene glycol, dipropylene glycol, polyethylene glycol, polypropylene glycol, and polytetramethylene glycol; alicyclic diols such as 1,4-cyclohexanedimethanol, 1,4-sorbitan, and hydrogenated bisphenol A; Examples of the alkylene oxide adducts include those obtained by adding alkylene oxides such as ethylene oxide, propylene oxide, and butylene oxide to cyclic diols; bisphenols such as bisphenol A, bisphenol F, and bisphenol S; alkylene oxide adducts of bisphenols such as those obtained by adding alkylene oxides such as ethylene oxide, propylene oxide, and butylene oxide to the above bisphenols; tri- or higher hydric aliphatic alcohols such as heptanetriol, octanetriol, decanetriol, sorbitol, and dipentaerythritol; polyphenols such as trisphenol, phenol novolac, and cresol novolac; and alkylene oxide adducts of polyphenols such as those obtained by adding alkylene oxides such as ethylene oxide, propylene oxide, and butylene oxide to the above polyphenols. Among these, 1,2-propanediol, 1,3-propanediol, 1,4-butanediol, and 2,3-butanediol are preferred. By using these diols as other alcohol components in the polyester resin (A), a shell layer having a good balance between low-temperature fixability and mechanical durability can be formed, and the cohesiveness of the shell particles to the core particles and the uniformity thereof are favorable, which is preferable. In addition, from the viewpoint of reducing the amount of carbon dioxide emitted when the obtained toner is finally incinerated and disposed of, it is more preferable that these diols are derived from biomass. In this specification, "1,2-propanediol, 1,3-propanediol, 1,4-butanediol, and 2,3-butanediol" may be referred to as "diol (D)". These other alcohols may be used alone or in combination of two or more.
[0029] When 1,2-propanediol, 1,3-propanediol, 1,4-butanediol, and 2,3-butanediol are used as the other alcohols, at least one selected from these diols is preferably contained in an amount of 30 mol% or more, more preferably 50 mol% or more, and even more preferably 80 mol% or more, based on the total amount of the alcohol components in the polyester resin (A). In other words, the total content of these diols is preferably 30 mol% or more, more preferably 50 mol% or more, and even more preferably 80 mol% or more, based on the total amount of the alcohol components in the polyester resin (A). It is preferable that the total content of 1,2-propanediol, 1,3-propanediol, 1,4-butanediol, and 2,3-butanediol is 30 mol % or more based on the total amount of alcohol components in the polyester resin (A), since low-temperature fixability, mechanical durability, and an effect of reducing the environmental load can be obtained.
[0030] <<<Repeating units derived from polyethylene terephthalate (PET)>>> In addition to the above components, the polyester resin (A) of the present invention may contain a repeating unit derived from so-called polyethylene terephthalate (PET), which is a condensate of terephthalic acid and ethylene glycol. In this specification, the "repeating unit derived from polyethylene terephthalate (PET)" may be referred to as the "PET repeating unit." The polyester resin (A) containing the PET repeating unit has excellent mechanical durability and can be suitably applied to the shell layer of a toner having a core-shell structure. From the viewpoint of reducing the environmental load, such as reducing the consumption of petroleum resources, it is preferable to use recycled PET as the raw material.
[0031] The polyester resin (A) containing the PET repeating unit can be obtained by polycondensation while causing an ester exchange reaction with the above-mentioned polyester resin (A) material.
[0032] As described above, in the conventional technology, when PET is introduced into shell particles forming a shell layer, the hydrophobicity of the shell particles is reduced, which leads to a concern that the cohesiveness of the core particles and the shell particles is reduced, making it difficult to form a uniform shell layer on the surface of the core particles. On the other hand, the polyester resin emulsion for toner of the present invention has a ratio (OHV / AV) of the polyester resin (A) of 0.20 to 0.60, so that the hydrophobicity is maintained appropriately and hetero-coagulation with the core particles is preferentially likely to occur, and even if PET is introduced into the shell particles, the cohesiveness and adhesion with the core particles are not impaired, which is preferable.
[0033] The content of the PET repeating unit is not particularly limited and can be appropriately selected depending on the purpose, but is preferably from 10% by weight to 70% by weight, and more preferably from 30% by weight to 60% by weight, based on the total amount of the polyester resin (A). It is preferable that the content of the PET repeating unit is 10% by weight or more based on the total amount of the polyester resin (A) because this provides excellent mechanical durability. If the content of the PET repeating unit is 70% by weight or less based on the total amount of the polyester resin (A), this is preferable because it improves the solubility in organic solvents and the low-temperature fixability.
[0034] [Ratio of polyester resin (A) (OHV / AV)] In the present invention, the ratio (OHV / AV) of the hydroxyl value (OHV) of the polyester resin (A) to the acid value (AV) of the polyester resin (A) is 0.20 to 0.60, and preferably 0.35 to 0.50. In this specification, the "ratio (OHV / AV) of the hydroxyl value (OHV) of the polyester resin (A) to the acid value (AV) of the polyester resin (A)" may be referred to as the "ratio (OHV / AV)". The ratio (OHV / AV) of 0.20 or more and 0.60 or less can solve problems such as poor cohesion of the shell particles to the core particles, failure to uniformly distribute the shell particles on the surfaces of the core particles, resulting in defects in the formed shell layer, or an increase in the proportion of shell particles that do not cohere to the core particles, which remain as fine powder in the toner, resulting in a decrease in toner quality. Also, when the shell particles are heated and melted to form a shell layer, the adhesion of the shell particles to the core particles is improved, which makes the shell layer less likely to peel off, which is preferable.
[0035] The acid value (AV) of the polyester resin (A) is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 15 mgKOH / g or more and 30 mgKOH / g or less, and more preferably 18 KOH / g or more and 25 mgKOH / g or less. When the oxidation (AV) is 15 mgKOH / g or more, the emulsion has good stability, which can solve the problem of difficulty in emulsification, and the coagulation of the shell particles with respect to the core particles is also good, which is preferable. When the oxidation value (AV) is 30 mgKOH / g or less, the charge stability of the toner against environmental fluctuations is good, and the cohesion of the shell particles to the core particles is good, which is preferable.
[0036] The method for measuring the acid value (AV) of the polyester resin (A) is not particularly limited and may be appropriately selected depending on the purpose. For example, it may be measured by the method according to JIS K0070.
[0037] The hydroxyl value (OHV) of the polyester resin (A) is not particularly limited and can be appropriately selected depending on the purpose. When the acid value (AV) is 15 mgKOH / g or more and 30 mgKOH / g or less, the hydroxyl value (OHV) is preferably 3 mgKOH / g or more and 18 mgKOH / g or less.
[0038] The method for measuring the hydroxyl value (OHV) of the polyester resin (A) is not particularly limited and may be appropriately selected depending on the purpose. For example, the OHV may be measured by the method according to JIS K0070.
[0039] [Glass transition temperature (Tg) of polyester resin (A)] The glass transition temperature (Tg) of the polyester resin (A) at the second heating step measured by differential scanning calorimetry (DSC) is not particularly limited and may be appropriately selected depending on the purpose, but is preferably from 50° C. to 80° C., and more preferably from 60° C. to 75° C. In this specification, the "glass transition temperature (Tg) at the second heating step measured by differential scanning calorimetry (DSC)" may be referred to as "Tg2nd". If the Tg2nd of the polyester resin (A) is 60° C. or higher, the heat-resistant storage stability of the toner is improved, which is preferable. If the Tg2nd of the polyester resin (A) is 75° C. or less, the low-temperature fixability of the toner is improved, which is preferable.
[0040] The method for measuring the glass transition temperature (Tg) of the polyester resin (A) is not particularly limited, but for example, it can be measured using a differential scanning calorimeter (DSC) (e.g., Q-200 (manufactured by TA Instruments)). An example of the method for measuring the glass transition temperature (Tg) is as follows. --An example of how to measure glass transition temperature (Tg)-- 5.0 mg of polyester resin (A) is placed in an aluminum sample pan, placed on a holder unit, and set in an electric furnace. 10 mg of alumina is used as a reference, placed in an aluminum sample pan. In a nitrogen atmosphere, the sample is heated from 0°C to 150°C at a heating rate of 10°C / min (first heating), then cooled from 150°C to 0°C at a heating rate of 10°C / min (cooling process), and heated again to 150°C at a heating rate of 10°C / min (second heating). The endothermic and exothermic changes in the above process are measured, a graph of temperature and endothermic and exothermic amounts is drawn, a DSC curve is created, and the analysis is performed using the analysis program in the Q-200 system. The DSC curve in the second heating is selected, and the glass transition temperature of polyester resin (A) is calculated from the intersection of the extension line of the baseline of the DSC curve at a temperature lower than the enthalpy relaxation of the endothermic amount and the tangent line showing the maximum slope in the enthalpy relaxation.
[0041] [Weight average molecular weight of polyester resin (A)] The weight average molecular weight (Mw) of the polyester resin (A) measured by gel permeation chromatography (GPC) is not particularly limited and can be appropriately selected depending on the purpose. 4 More than 1×10 5 It is preferable that the value is less than 1×10 4 5×10 or more 4 It is more preferable that the weight average molecular weight (Mw) is equal to or less than 1. In this specification, the "weight average molecular weight (Mw) measured by gel permeation chromatography (GPC)" may be simply referred to as the "weight average molecular weight (Mw)". The weight average molecular weight (Mw) of the polyester resin (A) is 0.8×10 4 If the amount is more than this, the mechanical durability of the toner becomes good, which is preferable. The weight average molecular weight (Mw) of the polyester resin (A) is 5×10 4 If it is equal to or less, the low-temperature fixing property of the toner becomes good, which is preferable.
[0042] The method for measuring the weight average molecular weight (Mw) is not particularly limited, but it can be measured using a gel permeation chromatography (GPC) measuring device (e.g., HLC-8220GPC (manufactured by Tosoh Corporation)). An example of the method for measuring the weight average molecular weight (Mw) is as follows. --An example of how to measure weight-average molecular weight (Mw)-- As the column, a TSKgel SuperHZM-H 15 cm triple column (manufactured by Tosoh Corporation) is used. The polyester resin (A) to be measured is made into a 0.15 mass% solution using tetrahydrofuran (THF) (containing stabilizer, manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.), filtered through a 0.2 μm filter, and the filtrate is used as the sample. 100 μl of the THF sample solution is injected into the measuring device and measured at a flow rate of 0.35 ml / min under an environment of 40°C. The molecular weight is calculated using a calibration curve prepared using a monodisperse polystyrene standard sample. As the polystyrene standard sample, ShowdexSTANDARD series manufactured by Showa Denko Co., Ltd. is used to prepare THF solutions (solutions A to C) of the following three types of monodisperse polystyrene standard samples, and measurements are performed under the above conditions, and a calibration curve is prepared with the retention time of the peak top as the light scattering molecular weight of the monodisperse polystyrene standard sample. As the detector, an RI (refractive index) detector is used. Solution A: S-7300 2.5mg, S-602 2.5mg, S-46 2.5mg, S-2.8 2.5mg, THF 50mL Solution B: S-3500 2.5mg, S-277 2.5mg, S-18 2.5mg, S-1.3 2.5mg, THF 50mL Solution C: S-1700 2.5mg, S-136 2.5mg, S-6.7 2.5mg, toluene 2.5mg, THF 50mL
[0043] [Volume average particle size of polyester resin (A)] The volume average particle size of the resin particles (S) in the polyester resin emulsion for toner is not particularly limited and can be appropriately selected depending on the purpose. The median diameter (D50) is preferably 0.05 μm or more and 0.8 μm or less, more preferably 0.1 μm or more and 0.5 μm or less, and even more preferably 0.15 μm or more and 0.3 μm or less. When the volume average particle size of the resin particles (S) is 0.05 μm or more in terms of median diameter (D50), the aggregation efficiency of the shell particles relative to the core particles becomes good, and a shell layer with sufficient thickness can be formed on the toner surface, which is preferable. When the volume average particle size of the resin particles (S) is 0.8 μm or less in terms of median diameter (D50), the aggregation of the shell particles to the core particles becomes uniform, and a sufficiently uniform shell layer can be formed, which is preferable.
[0044] The method for measuring the median diameter (D50) is not particularly limited and can be appropriately selected depending on the purpose. For example, the median diameter can be measured using a laser type particle size distribution measuring device LA-920 (manufactured by Horiba, Ltd.).
[0045] <Other resins> The polyester resin emulsion for toner may contain other resins in addition to the polyester resin (A) as long as the effects of the present invention are not impaired. The other resins are not particularly limited and can be appropriately selected depending on the purpose. For example, homopolymers of styrene or its substitutes such as polystyrene, poly-p-styrene, and polyvinyltoluene, styrene-p-chlorostyrene copolymers, styrene-propylene copolymers, styrene-vinyltoluene copolymers, styrene-methyl acrylate copolymers, styrene-ethyl acrylate copolymers, styrene-methacrylic acid copolymers, styrene-methyl methacrylate copolymers, styrene-ethyl methacrylate copolymers, styrene-butyl methacrylate copolymers, styrene-α-chloromethyl methacrylate copolymers, styrene-acrylonitrile copolymers, and styrene-vinyl methyl Examples of the resin include styrene-based copolymers such as ether copolymers, styrene-vinyl methyl ketone copolymers, styrene-butadiene copolymers, styrene-isopropyl copolymers, and styrene-maleic acid ester copolymers; polymethyl methacrylate resins, polybutyl methacrylate resins, polyvinyl chloride resins, polyvinyl acetate resins, polyethylene resins, polyester resins, polyurethane resins, epoxy resins, polyvinyl butyral resins, polyacrylic acid resins, rosin resins, modified rosin resins, terpene resins, phenolic resins, aliphatic or aromatic hydrocarbon resins, aromatic petroleum resins, and these resins modified to have a functional group capable of reacting with an active hydrogen group such as an isocyanate group. These other resins may be used alone or in combination of two or more.
[0046] The solid content concentration in the polyester resin emulsion for toner is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 5% by mass or more and 50% by mass or less, and more preferably 30% by mass or more and 45% by mass or less. When the solid content concentration in the polyester resin emulsion for toner is 5% by mass or more, the aggregation efficiency of the shell particles relative to the core particles is good, and the productivity of the toner is preferably improved. It is preferable that the solid content concentration in the polyester resin emulsion for toner is 50% by mass or less since this leads to good emulsion stability.
[0047] The method for measuring the solid content concentration in the polyester resin emulsion for toner is not particularly limited and may be appropriately selected depending on the purpose. For example, the solid content concentration can be calculated by drying an emulsion sample weighed on an aluminum cup in a thermostatic chamber set at 150° C. for 3 hours, and weighing the emulsion sample before and after drying.
[0048] Although details will be described later, the polyester resin emulsion for toner is preferably a shell resin emulsion used for producing a toner having a core-shell structure consisting of core particles containing a binder resin and shell particles covering the core particles.
[0049] [Method for producing polyester resin emulsion for toner] The method for producing the polyester resin emulsion for toner is not particularly limited and may be appropriately selected depending on the purpose. For example, a shear emulsification method, a phase inversion emulsification method, or other known dispersion methods may be used. An example of the shear emulsification method includes dissolving the polyester resin (A) in an organic solvent, adding it to an aqueous medium, and dispersing it by mechanical shear force using a low-speed shear type, high-speed shear type, friction type, high-pressure jet type, ultrasonic type homomixer, homogenizer, ball mill with media, sand mill, dyno mill, or the like. An example of the phase inversion emulsification method is a method in which the polyester resin (A) is dissolved in an organic solvent, and then an aqueous medium is added to cause phase inversion. Among these, the phase inversion emulsification method is preferred from the viewpoint of obtaining a homogeneous emulsion with a sharp particle size distribution.
[0050] <Phase inversion emulsification method> The phase inversion emulsification method is a method in which an aqueous medium is added to a resin solution obtained by dissolving the polyester resin (A) in an organic solvent, thereby causing phase inversion emulsification.
[0051] --Organic solvent-- The organic solvent used in the phase inversion emulsification method is not particularly limited and can be appropriately selected depending on the purpose. Examples of the organic solvent include ethanol, isopropanol, isobutanol, acetone, methyl ethyl ketone, methyl isobutyl ketone, diethyl ketone, dibutyl ether, tetrahydrofuran, dioxane, methyl acetate, ethyl acetate, isopropyl acetate, toluene, xylene, benzene, carbon tetrachloride, methylene chloride, 1,2-dichloroethane, 1,1,2-trichloroethane, trichloroethylene, chloroform, monochlorobenzene, and dichloroethylidene. Of these, methyl ethyl ketone, ethyl acetate and isopropyl acetate are preferred from the viewpoints of solvent removability and polyester resin solubility. These may be used alone or in combination of two or more.
[0052] From the viewpoint of dispersion stability, it is preferable to quickly remove the organic solvent from the emulsion consisting of the resin solution and the aqueous medium.The method for removing the organic solvent is not particularly limited and can be selected from known desolvation methods according to the purpose, and examples thereof include a method of gradually increasing the temperature of the emulsion while stirring, and evaporating and removing the organic solvent in the system, a method of spraying the emulsion into a dry atmosphere such as air or nitrogen while stirring, and a method of reducing the pressure while stirring the emulsion, and evaporating and removing the organic solvent in the system. These methods for removing the solvent may be used alone or in combination of two or more.
[0053] -Aqueous medium- The aqueous medium used in the phase inversion emulsification method is not particularly limited and can be appropriately selected depending on the purpose. Examples of the aqueous medium include water and a mixture of water and an organic solvent miscible with water. The content of the aqueous medium is not particularly limited and may be appropriately selected depending on the purpose, and is preferably 80 parts by mass or more and 150 parts by mass or less with respect to 100 parts by mass of the resin solution. In the phase inversion emulsification method, the rate of addition of the aqueous medium until the resin solution undergoes phase inversion and is completed is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 0.1 parts by mass / min or more and 60 parts by mass / min or less, and more preferably 1 part by mass / min or more and 3 parts by mass / min or less, relative to 100 parts by mass of the resin solution. It is preferable that the addition rate of the aqueous medium is 0.1 parts by mass / minute or more relative to 100 parts by mass of the resin solution, since this improves the productivity of the toner. When the addition rate of the aqueous medium is 60 parts by mass / min or less per 100 parts by mass of the resin solution, the particle size distribution becomes sharp and the cohesion of the shell particles to the core particles becomes good, so that the shell layer can be formed uniformly, which is preferable.
[0054] In the phase inversion emulsification method, a neutralizing agent, a surfactant, a polymer protective colloid, and the like can be added to the resin solution or the aqueous medium within a range that does not impair the effects of the present invention.
[0055] -Neutralizer- The neutralizing agent is not particularly limited and can be appropriately selected depending on the purpose, and examples of the neutralizing agent include basic substances such as ammonia, trimethylamine, ethylamine, diethylamine, triethylamine, diethanolamine, triethanolamine, tributylamine, lithium hydroxide, sodium hydroxide, and potassium hydroxide. Among these, ammonia and sodium hydroxide are preferably used from the viewpoint of ensuring the quality of the emulsion.
[0056] The neutralization ratio (r), which is the molar ratio of the neutralizer to the acid value (AV) of the polyester resin (A), is not particularly limited and can be appropriately selected depending on the purpose. It is preferably 30% or more and 150% or less, and more preferably 60% or more and 100% or less. When the neutralization rate (r) is 30% or more, phase inversion emulsification proceeds easily, and an emulsion with a uniform particle size can be obtained, which is preferable. If the neutralization rate (r) is 150% or less, phase inversion emulsification is likely to proceed, which is preferable.
[0057] The amount of the neutralizing agent used is not particularly limited and can be appropriately selected depending on the purpose, and can be calculated, for example, by the following formula (1): In the formula, AV is the acid value of the resin (mgKOH / g), M is the amount of the resin used (g), and r is the neutralization rate (%). Amount of neutralizing agent used (mol / g) = (AV / 56,110) × M × (r / 100) Equation (1)
[0058] -Surfactants- The surfactant is not particularly limited and can be appropriately selected depending on the purpose. Examples of the surfactant include anionic surfactants such as alkylbenzenesulfonate, α-olefinsulfonate, and phosphate ester; cationic surfactants of amine salt type such as alkylamine salt, aminoalcohol fatty acid derivative, polyamine fatty acid derivative, and imidazoline, and quaternary ammonium salt type such as alkyltrimethylammonium salt, dialkyldimethylammonium salt, alkyldimethylbenzylammonium salt, pyridinium salt, alkylisoquinolinium salt, and benzethonium chloride; nonionic surfactants such as fatty acid amide derivatives and polyhydric alcohol derivatives; and alanine, dodecyldi(aminoethyl)glycine, di(octylaminoethyl)glycine, and N-alkyl-N,N-dimethylammonium betaine.
[0059] -Polymer protective colloid- The polymer protective colloid is not particularly limited and can be appropriately selected depending on the purpose. For example, acids such as acrylic acid, methacrylic acid, α-cyanoacrylic acid, α-cyanomethacrylic acid, itaconic acid, crotonic acid, fumaric acid, maleic acid, and maleic anhydride; (meth)acrylic monomers containing a hydroxyl group such as β-hydroxyethyl acrylate, β-hydroxyethyl methacrylate, β-hydroxypropyl acrylate, β-hydroxypropyl methacrylate, γ-hydroxypropyl acrylate, γ-hydroxypropyl methacrylate, 3-chloro-2-hydroxypropyl acrylate, 3-chloro-2-hydroxypropyl methacrylate, diethylene glycol monoacrylate, diethylene glycol monomethacrylate, glycerin monoacrylate, glycerin monomethacrylate, N-methylol acrylamide, and N-methylol methacrylamide; vinyl alcohol; vinyl alcohol such as vinyl methyl ether, vinyl ethyl ether, and vinyl propyl ether. esters of vinyl alcohol and compounds containing a carboxyl group, such as vinyl acetate, vinyl propionate, and vinyl butyrate; acrylamide, methacrylamide, diacetone acrylamide, and methylol compounds thereof; acid chlorides, such as acrylic acid chloride and methacrylic acid chloride; homopolymers or copolymers having a nitrogen atom or a heterocyclic ring thereof, such as vinylpyridine, vinylpyrrolidone, vinylimidazole, and ethyleneimine; polyoxyethylene-based copolymers, such as polyoxyethylene, polyoxypropylene, polyoxyethylene alkylamines, polyoxypropylene alkylamines, polyoxyethylene alkylamides, polyoxypropylene alkylamides, polyoxyethylene nonylphenyl ether, polyoxyethylene lauryl phenyl ether, polyoxyethylene stearyl phenyl ester, and polyoxyethylene nonyl phenyl ester; and celluloses, such as methyl cellulose, hydroxyethyl cellulose, and hydroxypropyl cellulose.
[0060] (Resin particles (T) and toner) The resin particles (T) of the present invention are resin particles (T) having a core-shell structure consisting of a core particle containing a binder resin and a shell particle covering the core particle, and the shell particle is formed from a polyester resin emulsion for a toner, and may contain an external additive and other components as necessary. The toner of the present invention has a core-shell structure consisting of core particles containing a binder resin and shell particles covering the core particles. The shell particles are formed from a polyester resin emulsion for toners, and may contain external additives and other components as necessary. The "polyester resin emulsion for toner" is the same as that described in the above section (Polyester resin emulsion for toner), and therefore a description thereof will be omitted. Moreover, the resin particles (S) contained in the polyester resin emulsion for a toner and the resin particles (T) made of the polyester resin emulsion for a toner are different from each other.
[0061] <Core-shell structure> The core-shell structure may, for example, be (1) a structure in which a shell particle made of a resin is disposed on the outermost surface of a core particle containing a binder resin, thereby coating the surface of the core particle, or (2) a structure in which a shell layer made of a resin is formed on the outermost surface of a core particle containing a binder resin, thereby coating the surface of the core particle. Among these, the structure (2) is preferred from the viewpoints of providing a toner with excellent homogeneity, heat-resistant storage stability, and mechanical durability, and of making the shell layer less likely to peel off due to stress.
[0062] In the resin particles (T) and toner having a core-shell structure, the surface of the core particle does not need to be completely covered with the shell particle or the shell layer. However, from the viewpoints of toner homogeneity, heat-resistant storage stability, and mechanical durability, it is preferable that the covering area is 90% or more of the total surface area of the core particle.
[0063] <<Core particle>> The core particles contain a binder resin, and may contain, as necessary, a crystalline resin as a fixing aid, a coloring agent, a releasing agent, a charge control agent, and the like.
[0064] --Binding resin-- The binder resin is not particularly limited and can be appropriately selected depending on the purpose. For example, homopolymers of styrene or its substitutes such as polystyrene, poly-p-styrene, and polyvinyltoluene, styrene-p-chlorostyrene copolymers, styrene-propylene copolymers, styrene-vinyltoluene copolymers, styrene-methyl acrylate copolymers, styrene-ethyl acrylate copolymers, styrene-methacrylic acid copolymers, styrene-methyl methacrylate copolymers, styrene-ethyl methacrylate copolymers, styrene-butyl methacrylate copolymers, styrene-α-chloromethyl methacrylate copolymers, styrene-acrylonitrile copolymers, styrene-vinyl methyl ether copolymers, Examples of the resin include styrene-based copolymers such as styrene-vinyl methyl ketone copolymers, styrene-butadiene copolymers, styrene-isopropyl copolymers, and styrene-maleic acid ester copolymers; polymethyl methacrylate resins, polybutyl methacrylate resins, polyvinyl chloride resins, polyvinyl acetate resins, polyethylene resins, polyester resins, polyurethane resins, epoxy resins, polyvinyl butyral resins, polyacrylic acid resins, rosin resins, modified rosin resins, terpene resins, phenolic resins, aliphatic or aromatic hydrocarbon resins, aromatic petroleum resins, and these resins modified to have a functional group capable of reacting with an active hydrogen group such as an isocyanate group. These may be used alone or in combination of two or more.
[0065] The binder resin preferably contains at least one amorphous polyester resin (B) from the viewpoint of increasing the adhesion of the core particles to the shell particles and obtaining a toner having excellent mechanical durability. The polyester resin in the amorphous polyester resin (B) is not particularly limited and can be appropriately selected depending on the purpose, and for example, the same polyester resin as described in the above item <<Polyester resin (A)>> can be used.
[0066] -Crystalline resin- The crystalline resin is not particularly limited as long as it has crystallinity and can be appropriately selected depending on the purpose, and examples thereof include polyester resin, polyurethane resin, polyurea resin, polyamide resin, polyether resin, vinyl resin, modified crystalline resin, etc. Among these, polyester resin is preferred from the viewpoint of achieving excellent compatibility between low-temperature fixability and heat-resistant storage stability. These may be used alone or in combination of two or more.
[0067] The crystalline resin is preferably one that melts at about the fixing temperature of the toner. By including such a crystalline resin in the toner, the crystalline resin becomes compatible with the binder resin as it melts at the fixing temperature, improving the sharp melting property of the toner and exhibiting an excellent effect of low-temperature fixing property, which is preferable. The melting point of the crystalline resin is not particularly limited, but is preferably 60°C or higher and 100°C or lower. If the melting point of the crystalline resin is 60° C. or higher, the crystalline resin is likely to melt at a low temperature, and the heat-resistant storage stability of the toner is favorable. If the melting point of the crystalline resin is 100° C. or lower, the low-temperature fixing property of the toner is favorable.
[0068] -Coloring agent- The colorant is not particularly limited and can be appropriately selected depending on the purpose. Examples of the colorant include carbon black, nigrosine dye, iron black, naphthol yellow S, Hansa yellow (10G, 5G, G), cadmium yellow, yellow iron oxide, yellow ocher, yellow lead, titanium yellow, polyazo yellow, oil yellow, Hansa yellow (GR, A, RN, R), pigment yellow L, benzidine yellow (G, GR), permanent yellow (NCG), Balkan fast yellow (5G, R), tartrazine lake, quinoline yellow lake, and anthrazan yellow BG. L, Isoindolinone Yellow, Bengala, Red Lead, Cinnabar, Cadmium Red, Cadmium Mercury Red, Antimony Vermilion, Permanent Red 4R, Para Red, Phaysee Red, Parachlor Orthonitroaniline Red, Lithol Fast Scarlet G, Brilliant Fast Scarlet, Brilliant Carmine BS, Permanent Red (F2R, F4R, FRL, FRLL, F4RH), Fast Scarlet VD, Belkan Fast Rubin B, Brilliant Scarlet G, Lithol Rubin GX, Permanent Red F5R, Brilliant Carmine 6B, Pigment Scarlet 3B, Bordeaux 5B, Toluidine Maroon, Permanent Bordeaux F2K, Helio Bordeaux BL, Bordeaux 10B, Bon Maroon Light, Bon Maroon Medium, Eosin Lake, Rhodamine Lake B, Rhodamine Lake Y, Alizarin Lake, Thioindigo Red B, Thioindigo Maroon, Oil Red, Quinacridone Red, Pyrazolone Red, Polyazo Red, Chrome Vermilion, Benzidine Orange, Perinone Orange, Oil Orange, Cobalt Blue, Cerulean Blue, Alkaline Blue Lake, Peacock Blue Lake, Victoria Blue Lake, Metal-free Phthalocyanine Blue, Phthalocyanine Blue, Fast Sky Blue, Indanthrene Blue (RS, BC), Indigo, Ultramarine Blue, Prussian Blue, Anthraquinone Blue, Fast Violet B, Methyl Violet Lake, Cobalt Purple, Manganese Purple, Dioxane Violet, Anthraquinone Violet, Chrome Green, Zinc Green, Chromium Oxide, Pyridian, Emerald Green, Pigment Green B, Naphthol Green B, Green Gold, Acid Green Lake,Examples include malachite green lake, phthalocyanine green, anthraquinone green, titanium oxide, zinc oxide, and lithopone. These may be used alone or in combination of two or more.
[0069] The content of the colorant is not particularly limited and can be appropriately selected depending on the purpose, but is preferably from 1 to 15% by mass, and more preferably from 3 to 10% by mass, based on the total amount of the resin particles (T) or the total amount of the toner. If the content of the colorant is 1% by mass or more based on the total amount of the resin particles (T) or the total amount of the toner, the coloring power of the toner becomes good, which is suitable. When the content of the colorant is 15% by mass or less relative to the total amount of the resin particles (T) or the total amount of the toner, the pigment is well dispersed in the toner, and the coloring power and charging characteristics of the toner are good, which is preferable.
[0070] The colorant may be used as a masterbatch in which it is combined with a masterbatch resin. The masterbatch resin is not particularly limited and can be appropriately selected depending on the purpose. Examples of the resin include a polymer of styrene or a substituted product thereof, a styrene-based copolymer, a polymethyl methacrylate resin, a polybutyl methacrylate resin, a polyvinyl chloride resin, a polyvinyl acetate resin, a polyethylene resin, a polypropylene resin, a polyester resin, an epoxy resin, an epoxy polyol resin, a polyurethane resin, a polyamide resin, a polyvinyl butyral resin, a polyacrylic acid resin, rosin, modified rosin, a terpene resin, an aliphatic hydrocarbon resin, an alicyclic hydrocarbon resin, an aromatic petroleum resin, chlorinated paraffin, and paraffin. These may be used alone or in combination of two or more.
[0071] --Release agent-- The release agent is not particularly limited and can be appropriately selected according to the purpose, and examples thereof include carnauba wax, rice wax, montan wax, trimethylolpropane tribehenate, pentaerythritol tetrabehenate, pentaerythritol diacetate dibehenate, glycerin tribehenate, icosanoic acid stearyl, behenic acid esters such as icosyl behenate, behenyl behenate, stearyl behenate, behenyl stearate, and stearyl stearate; polyalkanol esters such as tristearyl trimellitate and distearyl maleate; polyalkanoic acid amides such as dibehenylamide; polyalkylamides such as tristearyl trimellitate amide; dialkyl ketones such as distearyl ketone; polyolefin waxes such as polyethylene wax and polypropylene wax; and waxes such as long-chain hydrocarbons such as paraffin wax, microcrystalline wax, and sazol wax. Among these, waxes of alkanoic acid esters are preferred. These may be used alone or in combination of two or more.
[0072] The melting point of the release agent is not particularly limited and can be appropriately selected depending on the purpose, but is preferably from 40°C to 160°C, more preferably from 50°C to 120°C, and even more preferably from 60°C to 90°C. It is preferable for the melting point of the release agent to be 40° C. or higher, since this provides good heat-resistant storage stability. If the melting point of the release agent is 160° C. or lower, the occurrence of cold offset during low-temperature fixing can be suppressed, which is preferable.
[0073] The content of the release agent is not particularly limited and can be appropriately selected depending on the purpose, but is preferably from 1% by mass to 20% by mass, more preferably from 3% by mass to 15% by mass, and even more preferably from 3% by mass to 7% by mass, based on the total amount of the resin particles (T) or the total amount of the toner. If the content of the release agent is 20% by mass or less based on the total amount of the resin particles (T) or the total amount of the toner, the flowability of the toner is favorable, which is preferable.
[0074] -Charge control agent- The charge control agent is not particularly limited and can be appropriately selected depending on the purpose. Examples of the charge control agent include nigrosine dyes, triphenylmethane dyes, chromium-containing metal complex dyes, molybdic acid chelate pigments, rhodamine dyes, alkoxy amines, quaternary ammonium salts, alkylamides, phosphorus simple substances or compounds, tungsten simple substances or compounds, fluorine-based activators, metal salts of salicylic acid, and metal salts of salicylic acid derivatives.
[0075] The content of the charge control agent is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 0.1 parts by mass or more and 10 parts by mass or less, and more preferably 0.2 parts by mass or more and 5 parts by mass or less, relative to 100 parts by mass of the resin particles (T) or 100 parts by mass of the toner. When the content of the charge control agent is 10 parts by mass or less relative to 100 parts by mass of the resin particles (T) or 100 parts by mass of the toner, the charging characteristics of the toner become good, and a decrease in the fluidity of the developer and a decrease in the image density can be suppressed, which is preferable.
[0076] [Volume average particle diameter of core particles (Dv)] The volume average particle size (Dv) of the core particles is not particularly limited and can be appropriately selected depending on the purpose. From the viewpoints of granularity, sharpness, and fine line reproducibility, the median diameter (D50) is preferably 4 μm or more and 7 μm or less. The method for measuring the median diameter (D50) is not particularly limited and can be appropriately selected depending on the purpose. For example, the median diameter can be measured using a laser type particle size distribution measuring device LA-920 (manufactured by Horiba, Ltd.).
[0077] [Average circularity of core particles] The average circularity of the core particles is not particularly limited and can be appropriately selected depending on the purpose. From the viewpoints of transfer efficiency, fine line reproducibility, and cleaning properties of toner remaining on the photoreceptor or transfer belt, it is preferable that the average circularity is 0.940 or more and 0.990 or less. The method for measuring the average circularity of the core particles is not particularly limited and can be appropriately selected depending on the purpose. For example, the average circularity can be measured using a flow type particle image analyzer FPIA-3000 (manufactured by SYSMEX Corporation).
[0078] The method for producing the core particles is not particularly limited and may be appropriately selected depending on the purpose. Examples of the method include a kneading and grinding method and a so-called chemical method in which particles are granulated in an aqueous medium.
[0079] Examples of the chemical method include a suspension polymerization method, an emulsion polymerization method, a seed polymerization method, a dispersion polymerization method, and the like, which use a monomer as a starting material for production; a dissolution suspension method in which a resin or a resin precursor is dissolved in an organic solvent or the like and dispersed or emulsified in an aqueous medium; a phase inversion emulsification method in which water is added to a solution consisting of a resin or a resin precursor and a suitable emulsifier to invert the phase; and an aggregation method in which resin particles obtained by these methods are aggregated in a dispersed state in an aqueous medium and granulated into particles of a desired size by heating and melting, etc. Among these, the dissolution suspension method, phase inversion emulsification method, and aggregation method are preferred, because they allow easy handling of polyester resins having excellent low-temperature fixing properties.
[0080] From the viewpoint of agglomeration with the polyester resin emulsion for toner, the core particles are preferably in the form of an aqueous dispersion, and more preferably in the form of an aqueous dispersion of core particles obtained by a chemical process.
[0081] When using core particles obtained by the kneading and pulverizing method, the core particles are preferably subjected to a spheroidizing treatment and a surface smoothing treatment by a heat treatment or the like, from the viewpoint of forming a uniform shell layer.
[0082] From the viewpoint of agglomerating the shell particles onto the surface of the core particles, it is preferable that the core particles are particles to which no external additives, flow improvers, etc. are added.
[0083] <<Shell layer>> The shell layer can be obtained by a process in which a polyester resin emulsion consisting of the resin particles (S) is aggregated on the outermost surface of the core particles, and then the aggregate is heated and fused. It is preferable that the core particles and the shell particles (or shell layers) are in close contact with each other, or are not completely compatible with each other, with regions consisting of only the core particles or the shell particles (or shell layers) existing.
[0084] The average thickness of the shell layer is not particularly limited and can be appropriately selected depending on the purpose, but is preferably from 50 nm to 500 nm, and more preferably from 100 nm to 200 nm. When the average thickness of the shell layer is 50 nm or more, the function of protecting the core particles by the shell layer is improved, and the heat-resistant storage stability and mechanical durability are improved, which is preferable. When the average thickness of the shell layer is 500 nm or less, low-temperature fixability is favorable.
[0085] The method for measuring the average thickness of the shell layer is not particularly limited and can be appropriately selected depending on the purpose. For example, a sample in which toner particles are embedded in an epoxy resin or the like is cut with a micromicrotome or an ultramicrotome, and the ultrathin sliced sample is examined with a transmission electron microscope (TEM). In this case, it is preferable to stain the ultrathin slices with a staining agent such as ruthenium tetroxide or osmium tetroxide, as the core-shell structure can be easily visually observed. Specifically, the method is as follows. A sample of toner particles embedded in epoxy resin is cut into ultrathin slices using an ultramicrotome, and the cross-sectional images are photographed at 20,000x magnification using a TEM (field emission electron microscope JEM-2100F / JEOL). The photographed images are then imported into an image analyzer (LuzexAP / Nireco). The thickness of the shell layer is measured at five points on each of 30 toner particles, and the thickness can be calculated from the average value of these measurements.
[0086] The volume average particle size (Dv) of the resin particles (T) and the toner is not particularly limited and can be appropriately selected depending on the purpose. From the viewpoint of obtaining a high-quality image excellent in granularity, sharpness, and fine line reproducibility, the volume average particle size (Dv) is preferably 3 μm or more and 10 μm or less, and more preferably 4 μm or more and 7 μm or less. If the resin particles (T) and the toner have a volume average particle size (Dv) of 3 μm or more, the toner has good fluidity and transferability, which is preferable.
[0087] The ratio (Dv / Dn) of the volume average particle size (Dv) of the resin particles (T) and the toner to the number average molecular weight (Dn) of the resin particles (T) and the toner represents the particle size distribution of the resin particles (T) and the toner, and the closer the value is to 1, the sharper the particle size distribution. From the viewpoints of sharpness and fine line reproducibility, the ratio (Dv / Dn) is preferably 1.20 or less, and more preferably 1.15 or less.
[0088] The method for measuring the volume average particle size (Dv) and number average molecular weight (Dn) of the resin particles (T) and the toner is not particularly limited, but can be measured, for example, using a Coulter Multisizer III (aperture diameter 100 μm) (manufactured by Beckman Coulter, Inc.).
[0089] The average circularity of the resin particles (T) and the toner is not particularly limited and may be appropriately selected depending on the purpose, but is preferably 0.940 to 0.990.More preferably, the average circularity of the resin particles (T) and the toner is 0.960 to 0.985, and the content of the resin particles (T) and the toner having an average circularity of less than 0.94 is 15% by mass or less based on the total amount of the resin particles (T) and the toner. A toner having an average circularity within the above range, i.e., a substantially spherical toner, is effective for forming a high-definition image with excellent transfer efficiency and appropriate density and reproducibility. It is also suitable for obtaining a good image with few transfer defects in fine line images. This is believed to be because the toner surface is sufficiently smooth, so that the contact points with the image support are reduced, and the transfer failure of the toner to the transfer material is reduced. When the average circularity of the resin particles (T) and the toner is 0.940 or more, transferability becomes good, which is preferable. If the average circularity of the resin particles (T) and the toner is 0.990 or less, in a system using blade cleaning or the like, the problem of poor cleaning occurring on the photoconductor and transfer belt, etc., causing stains on the image can be eliminated, which is preferable. For example, in development or transfer with a low image area ratio, there is little residual toner after transfer, and poor cleaning is not a particular problem, but in the case of a high image area ratio such as a color photo image, toner that has not been transferred due to poor paper feed or the like may remain on the photoconductor as residual toner after transfer, and if this accumulates, it will cause background staining of the image. In addition, there is a problem that the charging roller that contact-charges the photoconductor is also contaminated, and the original charging ability is not exerted, but the present invention can solve this problem, which is preferable.
[0090] The method for measuring the average circularity of the resin particles (T) and the toner is not particularly limited and can be appropriately selected depending on the purpose. For example, the average circularity can be measured using a flow type particle image analyzer FPIA-3000 (manufactured by SYSMEX Co., Ltd.). Specifically, the circularity can be calculated from the two-dimensional image area of each particle captured by a CCD camera, and the circularity of each particle is added up and divided by the total number of particles. The circularity of each particle can be calculated by dividing the perimeter of a circle having the same projected area as the particle image by the perimeter of the particle projected image.
[0091] <External additives> The external additives are not particularly limited and can be appropriately selected depending on the purpose. Examples of the external additives include inorganic fine particles, polymer fine particles, flow improvers, cleaning assistants, and the like.
[0092] -Inorganic fine particles- Examples of the inorganic fine particles include silica, alumina, titanium oxide, barium titanate, magnesium titanate, calcium titanate, strontium titanate, zinc oxide, tin oxide, silica sand, clay, mica, wollastonite, diatomaceous earth, chromium oxide, cerium oxide, pengalla, antimony trioxide, magnesium oxide, zirconium oxide, barium sulfate, barium carbonate, calcium carbonate, silicon carbide, and silicon nitride.
[0093] The primary particle size of the inorganic fine particles is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 5 nm or more and 2 μm or less, and more preferably 5 nm or more and 500 nm or less. The inorganic fine particles having a primary particle diameter of 5 nm or more are preferably capable of suppressing embedding in the toner particle surface due to mechanical stress, and the inorganic fine particles having a primary particle diameter of 2 μm or less are preferably capable of suppressing detachment from the toner particle. The specific surface area of the inorganic fine particles according to the BET method is 20 m 2 / g or more 500m 2 / g or less is preferable. The content of the inorganic fine particles is preferably 0.01% by mass or more and 5% by mass or less based on the total amount of the resin particles (T) and the toner.
[0094] -Polymer-based fine particles- Examples of the polymeric fine particles include polymer particles of polycondensation systems such as polystyrene, methacrylate, acrylate copolymers, silicone, benzoguanamine, nylon, etc. obtained by soap-free emulsion polymerization, suspension polymerization, or dispersion polymerization, and polymer particles of thermosetting resins.
[0095] -Flow improver- The flow improver is not particularly limited and may be appropriately selected depending on the purpose as long as it is capable of increasing hydrophobicity by performing surface treatment and preventing deterioration of flow characteristics and charging characteristics even under high humidity conditions. Examples of the flow improver include silane coupling agents, silylating agents, silane coupling agents having a fluorinated alkyl group, organic titanate coupling agents, aluminum coupling agents, silicone oils, and modified silicone oils. The inorganic fine particles, ie, silica and titanium oxide, are preferably surface-treated with the flowability improving agent and used as hydrophobic silica and hydrophobic titanium oxide.
[0096] -Cleaning aid- The cleaning aid is not particularly limited as long as it is added to the toner in order to remove the developer remaining on the photoconductor or the primary transfer medium after transfer. Examples of the cleaning aid include fatty acid metal salts such as zinc stearate, calcium stearate, and stearic acid, polymer fine particles produced by soap-free emulsion polymerization such as polymethyl methacrylate fine particles and polystyrene fine particles. The polymer fine particles preferably have a relatively narrow particle size distribution, and the volume average particle size is preferably from 0.01 μm to 1 μm.
[0097] The external additive is attached to the particle surfaces by a process of adding and mixing the external additive with the resin particles (T) and the toner. The mixing method is not particularly limited, and examples of the method include a method of applying an impact force to the mixture with a blade rotating at high speed, a method of introducing the mixture into a high-speed air current, accelerating the mixture, and causing the particles to collide with each other or the composite particles to collide with an appropriate collision plate, etc. Specifically, examples of the mixing means include an Angmill (manufactured by Hosokawa Micron Corporation), a device modified from an I-type mill (manufactured by Japan Pneumatic Mfg. Co., Ltd.) with reduced grinding air pressure, a hybridization system (manufactured by Nara Machinery Works), a Kryptron system (manufactured by Kawasaki Heavy Industries, Ltd.), an automatic mortar, etc.
[0098] [Volume average particle size of toner (Dv)] The volume average particle diameter (Dv) of the toner is not particularly limited and can be appropriately selected depending on the purpose. From the viewpoints of granularity, sharpness, and fine line reproducibility, it is preferable that the median diameter (D50) is 4 μm or more and 7 μm or less. The method for measuring the median diameter (D50) is not particularly limited and can be appropriately selected depending on the purpose. For example, the median diameter can be measured using a laser type particle size distribution measuring device LA-920 (manufactured by Horiba, Ltd.).
[0099] [Average circularity of toner] The average circularity of the toner is not particularly limited and can be appropriately selected depending on the purpose. However, from the viewpoints of transfer efficiency, fine line reproducibility, and cleaning properties of toner remaining on the photoconductor or transfer belt, it is preferably 0.940 or more and 0.990 or less. The method for measuring the average circularity of the toner is not particularly limited and may be appropriately selected depending on the purpose. For example, the average circularity of the toner may be measured using a flow type particle image analyzer FPIA-3000 (manufactured by SYSMEX Corporation).
[0100] [Method of producing resin particles (T) having a core-shell structure and toner] The method for producing the resin particles (T) and the toner is not particularly limited, but may include, for example, an aggregation step and a fusion step, and may also include a washing step, a drying step, and an annealing step, as necessary.
[0101] <Agglomeration process> The aggregation step is a step in which shell particles are added to a dispersion of core particles dispersed in an aqueous medium, and the shell resin is aggregated on the surfaces of the core particles while stirring. The "dispersion of core particles dispersed in an aqueous medium" can be a polyester resin emulsion comprising the resin particles (S) of the present invention.
[0102] The aggregation step may be carried out under heating. The temperature of the aqueous medium in the aggregation step is not particularly limited and can be appropriately selected depending on the purpose. From the viewpoint of efficient aggregation, however, the temperature is preferably 20° C. or higher and the glass transition temperature (Tg) of the polyester resin (A) or lower.
[0103] In the aggregation step, from the viewpoint of promoting aggregation, an aggregating agent may be added or the pH may be adjusted. The flocculant is not particularly limited and can be appropriately selected depending on the purpose, and examples thereof include aluminum chloride, zinc sulfate, magnesium sulfate, aluminum sulfate, potassium aluminum sulfate, sodium chloride, sodium bromide, sodium iodide, sodium fluoride, sodium acetate, sodium acetoacetate, lithium chloride, lithium bromide, lithium iodide, lithium fluoride, lithium acetate, lithium acetoacetate, potassium chloride, potassium bromide, potassium iodide, potassium fluoride, potassium acetoacetate, magnesium bromide, magnesium chloride, magnesium iodide, and magnesium fluoride. Examples of the iron ore include magnesium, magnesium acetate, magnesium acetoacetate, calcium chloride, calcium bromide, barium bromide, barium chloride, barium iodide, barium fluoride, barium acetate, barium acetoacetate, strontium bromide, strontium chloride, strontium iodide, strontium fluoride, strontium acetate, strontium acetoacetate, zinc bromide, zinc chloride, zinc iodide, zinc fluoride, zinc acetate, zinc acetoacetate, copper bromide, copper chloride, copper iodide, copper fluoride, copper acetate, copper acetoacetate, iron bromide, iron chloride, iron iodide, iron fluoride, iron acetate, and iron acetoacetate. These may be used alone or in combination of two or more.
[0104] The content of the aggregating agent is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 0.1 parts by mass or more and 20 parts by mass or less, and more preferably 0.5 parts by mass or more and 10 parts by mass or less, relative to 100 parts by mass of the total amount of the core particles and the shell particles. The flocculant is preferably used as an aqueous solution from the viewpoint of uniform flocculation in the reaction system. When the flocculant is used as an aqueous solution, the content of the flocculant is preferably 1% by mass or more and 50% by mass or less, more preferably 5% by mass or more and 20% by mass or less, based on the total amount of the aqueous solution.
[0105] The addition speed of the aggregate to the aqueous medium is not particularly limited and can be appropriately selected depending on the purpose. The addition speed is preferably 0.1 parts by mass / min or more and 5 parts by mass / min or less, and more preferably 0.5 parts by mass / min or more and 2 parts by mass / min or less, relative to 100 parts by mass of the aqueous medium containing the core particles and the shell particles.
[0106] The aggregation reaction in the aggregation step can be terminated as necessary. The method for terminating the aggregation reaction is not particularly limited, and examples thereof include a method of adding a salt with a low ionic valence, a chelating agent, a surfactant, etc., a method of adjusting the pH, a method of lowering the temperature of the dispersion liquid, a method of adding a large amount of an aqueous medium to dilute the concentration, and the like. Examples of the chelating agent include metal salts such as sodium ethylenediaminetetraacetate, sodium gluconate, sodium tartrate, sodium citrate, potassium citrate, and nitrotriacetate salts, and polymer electrolytes.
[0107] <Fusing process> The fusion step is a step of heat-fusion of the aggregated particles, which are composed of the core particles and the shell particles obtained in the aggregation step, to form a shell layer.
[0108] In the fusion step, the dispersion of the aggregated particles is preferably heated while being stirred. The temperature in the fusion step is not particularly limited, but is preferably equal to or higher than the glass transition temperature (Tg) of the polyester resin (A).
[0109] <Cleaning process> The washing step is a step of washing the resin particles (T) and the toner obtained in the fusion step. The washing method in the washing step is not particularly limited and can be appropriately selected depending on the purpose, and examples thereof include centrifugation, reduced pressure filtration, and filter press. If washing cannot be performed sufficiently in one operation, the cake obtained in the washing step may be dispersed again in an aqueous solvent to form a slurry, and the step of extracting the resin particles (T) and the toner by any of the above methods may be repeated. When washing is performed by reduced pressure filtration or filter press, the washing method may be performed by penetrating the aqueous solvent into the cake. The aqueous solvent used for the washing is not particularly limited, and examples thereof include water and mixed solvents in which water is mixed with an alcohol such as methanol or ethanol, etc. Among these, water is preferred from the viewpoints of cost and environmental load due to wastewater treatment, etc.
[0110] <Drying process> The drying step is a step of drying the cake obtained in the washing step. The drying method in the drying step is not particularly limited and can be appropriately selected depending on the purpose. Examples of the drying method include drying methods using dryers such as a spray dryer, a vacuum freeze dryer, a reduced pressure dryer, a stationary shelf dryer, a mobile shelf dryer, a fluidized bed dryer, a rotary dryer, and an agitator dryer. The drying is preferably carried out until the moisture content in the cake becomes less than 1%. The resin particles (T) and toner obtained after drying may be crushed using a device such as a jet mill, a Henschel mixer, a super mixer, a coffee mill, an Oster blender, or a food processor to break up aggregates.
[0111] <Annealing> The annealing is suitably carried out when the core particles contain the crystalline polyester resin. The annealing is preferably performed at a temperature not lower than the glass transition temperature and not higher than the melting point of the crystalline polyester resin, and the annealing is preferably performed for a period of not less than 3 hours and not more than 24 hours, more preferably not less than 6 hours and not more than 15 hours.
[0112] <Developer> The toner of the present invention can be used as a developer containing other components, such as a carrier, which are appropriately selected. The developer may be a one-component developer or a two-component developer. However, when used in high-speed printers that correspond to the recent improvements in information processing speed, a two-component developer is preferred because it has a longer life. In the case of a one-component developer using the above toner, even if there is a toner balance, i.e., even if toner is supplied to the developer and consumed by development, there is little fluctuation in the particle size of the toner, and there is no toner filming on the developing roller or toner fusion to layer thickness regulating members such as blades for thinning the toner layer, and good and stable developability and images can be obtained even with long-term use (stirring) of the developing means. In the case of the two-component developer using the toner, even if the toner is balanced over a long period of time, there is little fluctuation in the toner particle size in the developer, and good and stable developability can be obtained even with long-term stirring in the developing means.
[0113] The carrier is not particularly limited and can be appropriately selected depending on the purpose, but is preferably one having a core material and a resin layer covering the core material. The material of the core material is not particularly limited and can be appropriately selected according to the purpose, for example, manganese-strontium (Mn-Sr)-based material and manganese-magnesium (Mn-Mg)-based material having a density of 50 emu / g or more and 90 emu / g or less are preferable, and from the viewpoint of ensuring image density, highly magnetized materials such as iron powder (100 emu / g or more) and magnetite (75 emu / g or more and 120 emu / g or less) are preferable. In addition, weakly magnetized materials such as copper-zinc (Cu-Zn)-based materials (30 emu / g or more and 80 emu / g or less) are preferable because they can weaken the contact of the toner with the electrostatic latent image carrier in a standing state, which is advantageous for improving image quality. These may be used alone or in combination of two or more.
[0114] The particle diameter of the core material is preferably 10 μm or more and 200 μm or less, and more preferably 40 μm or more and 100 μm or less, in terms of average particle diameter (weight average particle diameter (D50)). When the average particle size (weight average particle size (D50)) is 10 μm or more, the distribution of the carrier particles contains a large amount of fine powder, which is preferable because it can solve the problem of carrier scattering due to low magnetization per particle. When the average particle size (weight average particle size (D50)) is 200 μm or less, the specific surface area decreases, causing toner scattering, and in the case of full color toner with many solid areas, the reproduction of the solid areas becomes poor, which is particularly problematic. This is preferable.
[0115] The material of the resin layer is not particularly limited and can be appropriately selected from known resins according to the purpose, and examples thereof include amino resins, polyvinyl resins, polystyrene resins, halogenated olefin resins, polyester resins, polycarbonate resins, polyethylene resins, polyvinyl fluoride resins, polyvinylidene fluoride resins, polytrifluoroethylene resins, polyhexafluoropropylene resins, copolymers of vinylidene fluoride and acrylic monomers, copolymers of vinylidene fluoride and vinyl fluoride, fluoro terpolymers (fluorinated triple (multiple) copolymers) such as terpolymers of tetrafluoroethylene, vinylidene fluoride and non-fluorinated monomers, and silicone resins. Among these, silicone resins are preferred. These may be used alone or in combination of two or more.
[0116] The silicone resin is not particularly limited and can be appropriately selected from commonly known silicone resins depending on the purpose. Examples of the silicone resin include straight silicone resins consisting only of organosiloxane bonds, and silicone resins modified with alkyd resins, polyester resins, epoxy resins, acrylic resins, urethane resins, etc. The silicone resin may be a synthetic product or a commercially available product, such as straight silicone resin KR271, KR255, and KR152 manufactured by Shin-Etsu Chemical Co., Ltd., and SR2400, SR2406, and SR2410 manufactured by Dow Corning Toray Silicone Co., Ltd.
[0117] The modified silicone resin may be a synthetic product or a commercially available product. Commercially available modified silicone resins include, for example, KR206 (alkyd modified), KR5208 (acrylic modified), ES1001N (epoxy modified), and KR305 (urethane modified) manufactured by Shin-Etsu Chemical Co., Ltd., and SR2115 (epoxy modified) and SR2110 (alkyd modified) manufactured by Dow Corning Toray Silicone Co., Ltd.
[0118] The silicone resin may be used alone, or may be used together with a crosslinking component, a charge amount adjusting component, etc.
[0119] The resin layer may contain conductive powder or the like as required. Examples of the conductive powder include metal powder, carbon black, titanium oxide, tin oxide, and zinc oxide. The average particle size of the conductive powder is preferably 1 μm or less, from the viewpoint of facilitating control of the electrical resistance.
[0120] The resin layer can be formed, for example, by dissolving the silicone resin or the like in a solvent to prepare a coating solution, uniformly coating the coating solution on the surface of the core material by a known coating method, drying, and then baking. Examples of the coating method include a dipping method, a spraying method, and a brush coating method. The solvent is not particularly limited and can be appropriately selected depending on the purpose. Examples of the solvent include toluene, xylene, methyl ethyl ketone, methyl isobutyl ketone, cellosolve, and butyl acetate. The baking method is not particularly limited, and may be an external heating method or an internal heating method, such as a method using a fixed electric furnace, a flow type electric furnace, a rotary type electric furnace, a burner furnace, or the like, or a method using microwaves.
[0121] The content of the carrier is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 0.01% by mass or more and 5.0% by mass or less with respect to the total amount of the resin layer. If the content of the carrier is 0.01% by mass or more based on the total amount of the resin layer, a uniform resin layer can be formed on the surface of the core material, which is preferable. When the content of the carrier is 5.0% by mass or less relative to the total amount of the resin layer, the thickness of the resin layer increases, and the carrier particles are granulated together, which makes it difficult to obtain uniform carrier particles. This is preferable.
[0122] When the developer is a two-component developer, the content of the carrier is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 90% by mass or more and 98% by mass or less, and more preferably 93% by mass or more and 97% by mass or less, based on the total amount of the two-component developer. The mixture ratio of the toner and the carrier in the two-component developer is preferably 1 part by mass or more and 10.0 parts by mass or less of the toner per 100 parts by mass of the carrier.
[0123] [Image forming apparatus and image forming method] The image forming apparatus according to the present invention is not particularly limited and may be appropriately selected depending on the purpose as long as the toner of the present invention is used. For example, the image forming apparatus may have an electrostatic latent image carrier, an electrostatic latent image forming means, and a developing means, and may have other means as necessary. The image forming method according to the present invention is not particularly limited and may be appropriately selected depending on the purpose as long as the toner of the present invention is used. For example, the image forming method may include a process for forming an electrostatic latent image and a development process, and may include other processes as necessary.
[0124] <Electrostatic latent image carrier> The latent image carrier is not particularly limited in terms of its material, shape, structure, size, etc., and can be appropriately selected from known ones. A preferred shape is a drum shape, and examples of its material include inorganic photoreceptors such as amorphous silicon and selenium, and organic photoreceptors such as polysilane and phthalopolymethine. Examples of the organic photoreceptor include a laminated type photoreceptor having a laminated structure in which a layer (charge generation layer) in which a charge generation material such as metal-free phthalocyanine or titanyl phthalocyanine is dispersed in a binder resin and a layer (charge transport layer) in which a charge transport material is dispersed in a binder resin are stacked on a support such as an aluminum drum, and a single-layer type photoreceptor having a single-layered photosensitive layer in which both a charge generation material and a charge transport material are dispersed in a binder resin on a support. In the single-layer type photoreceptor, a hole transport material and an electron transport material can also be added to the photosensitive layer as charge transport materials. An undercoat layer may be provided between the support and the multi-layer charge generating layer or the single-layer photosensitive layer. The linear speed of the electrostatic latent image bearing member is preferably 300 mm / s or more.
[0125] <Electrostatic latent image forming means and electrostatic latent image forming process> The electrostatic latent image forming means is not particularly limited as long as it is a means for forming an electrostatic latent image on the electrostatic latent image carrier, and may be appropriately selected depending on the purpose. For example, there may be mentioned a means having at least a charging member that charges the surface of the electrostatic latent image carrier, and an exposure member that exposes the surface of the electrostatic latent image carrier to light in an imagewise manner. The electrostatic latent image forming step is not particularly limited as long as it is a step of forming an electrostatic latent image on the electrostatic latent image bearing member, and can be appropriately selected depending on the purpose. For example, the electrostatic latent image forming step can be performed by charging the surface of the electrostatic latent image bearing member and then exposing it to light in an imagewise manner, using the electrostatic latent image forming means.
[0126] <<Charging materials and charging>> The charging member is not particularly limited and may be appropriately selected depending on the purpose, and examples thereof include a contact charger known per se having a conductive or semiconductive roller, brush, film, rubber blade, etc., a non-contact charger utilizing corona discharge such as a corotron, a scorotron, etc. Among these, it is preferable to use a contact-type charging member, since it is possible to obtain an image forming apparatus in which the amount of ozone generated from the charging member is reduced. The shape of the charging member may be any shape such as a roller, a magnetic brush, a fur brush, etc., and can be selected according to the specifications and shape of the image forming apparatus.
[0127] The charging can be carried out, for example, by applying a voltage to the surface of the electrostatic latent image bearing member using the charging member.
[0128] <<Exposure materials and exposure>> The exposure member is not particularly limited as long as it can expose the surface of the electrostatic latent image carrier charged by the charging member in the shape of an image to be formed, and can be appropriately selected depending on the purpose. Examples of the exposure member include various exposure members such as a copying optical system, a rod lens array system, a laser optical system, and a liquid crystal shutter optical system.
[0129] The light source used in the exposure member is not particularly limited and can be appropriately selected depending on the purpose. Examples of the light source include fluorescent lamps, tungsten lamps, halogen lamps, mercury lamps, sodium lamps, light-emitting diodes (LEDs), semiconductor lasers (LDs), electroluminescence (EL), and other light-emitting materials. In addition, the light source used in the exposure member may include various filters such as a sharp cut filter, a band pass filter, a near infrared cut filter, a dichroic filter, an interference filter, and a color temperature conversion filter in order to irradiate only light in a desired wavelength range.
[0130] The exposure can be carried out, for example, by exposing the surface of the electrostatic latent image bearing member imagewise using the exposure member. In the present invention, a light back system may be adopted in which exposure is performed imagewise from the back side of the electrostatic latent image bearing member.
[0131] <Developing means and developing process> The developing unit is not particularly limited as long as it is a developing unit equipped with a toner that develops the electrostatic latent image formed on the electrostatic latent image carrier to form a toner image that is a visible image, and can be appropriately selected depending on the purpose. The developing step is not particularly limited as long as it is a step of forming a toner image, which is a visible image, by developing the electrostatic latent image formed on the electrostatic latent image carrier with a toner, and can be appropriately selected depending on the purpose. For example, the developing step can be performed by the developing unit. The developing means is preferably a developing device having an agitator that frictionally agitates the toner to charge it, and a magnetic field generating means fixed inside, and having a developer carrier that can rotate and carries a developer containing the toner on its surface.
[0132] <Other means and other steps> Examples of the other means include a transfer means, a fixing means, a cleaning means, a discharging means, and a recycling means. Examples of the other steps include a transfer step, a fixing step, a cleaning step, a static elimination step, and a recycling step.
[0133] <<Transfer means and transfer process>> The transfer means is not particularly limited as long as it is a means for transferring a visible image onto a recording medium, and can be appropriately selected depending on the purpose. However, a preferred embodiment has a primary transfer means for transferring the visible image onto an intermediate transfer body to form a composite transfer image, and a secondary transfer means for transferring the composite transfer image onto a recording medium. The transfer step is not particularly limited as long as it is a step of transferring a visible image onto a recording medium, and may be appropriately selected depending on the purpose. However, a preferred embodiment is one in which an intermediate transfer body is used, a visible image is primarily transferred onto the intermediate transfer body, and then the visible image is secondarily transferred onto a recording medium. The transfer step can be carried out by, for example, charging the visible image on the photoconductor using a transfer charger, and can be carried out by the transfer unit.
[0134] Here, when the image to be secondarily transferred onto the recording medium is a color image made up of toners of multiple colors, the transfer means can be configured to sequentially overlay toners of each color on the intermediate transfer body to form an image on the intermediate transfer body, and the intermediate transfer means can be configured to secondarily transfer the image on the intermediate transfer body onto the recording medium all at once. The intermediate transfer body is not particularly limited and can be appropriately selected from known transfer bodies depending on the purpose. For example, a transfer belt is preferably used.
[0135] The transfer means (the primary transfer means and the secondary transfer means) preferably has at least a transfer device that peels and charges the visible image formed on the photoreceptor onto the recording medium. Examples of the transfer device include a corona transfer device using corona discharge, a transfer belt, a transfer roller, a pressure transfer roller, and an adhesive transfer device. The recording medium is typically plain paper, but is not particularly limited as long as it is capable of transferring an unfixed image after development, and can be appropriately selected depending on the purpose. For example, a PET base for an OHP can also be used.
[0136] <<Fixing means and fixing process>> The fixing means is not particularly limited as long as it is a means for fixing the transferred image transferred onto the recording medium, and can be appropriately selected depending on the purpose. For example, a known heating and pressing member is preferable. Examples of the heat and pressure member include a combination of a heat roller and a pressure roller, and a combination of a heat roller, a pressure roller and an endless belt. The fixing step is not particularly limited as long as it is a step of fixing the visible image transferred to the recording medium, and can be appropriately selected depending on the purpose, and for example, it may be performed for each color toner each time it is transferred to the recording medium, or it may be performed simultaneously for each color toner in a laminated state. The fixing step can be performed by the fixing means. The heating temperature in the heating and pressing member is preferably 80°C to 200°C.
[0137] In the present invention, depending on the purpose, for example, a known optical fixing device may be used together with or instead of the fixing means. The surface pressure in the fixing step is not particularly limited and can be appropriately selected depending on the purpose. 2 ~80N / cm 2 It is preferable that:
[0138] <<Cleaning means and cleaning process>> The cleaning means is not particularly limited as long as it is capable of removing the toner remaining on the photoreceptor, and can be appropriately selected depending on the purpose. Examples of the cleaning means include a magnetic brush cleaner, an electrostatic brush cleaner, a magnetic roller cleaner, a blade cleaner, a brush cleaner, and a web cleaner. The cleaning step is not particularly limited as long as it is a step that can remove the toner remaining on the photoreceptor, and can be appropriately selected depending on the purpose. For example, the cleaning step can be performed by the cleaning unit.
[0139] <<Static charge removal means and static charge removal process>> The charge removing means is not particularly limited as long as it is a means for removing electricity by applying a charge removing bias to the photoconductor, and may be appropriately selected depending on the purpose. For example, a charge removing lamp may be used. The charge removing step is not particularly limited as long as it is a step of removing electricity by applying a charge removing bias to the photoconductor, and may be appropriately selected depending on the purpose. For example, the charge removing step may be performed by the charge removing unit.
[0140] <<Recycling methods and processes>> The recycling means is not particularly limited as long as it is a means for recycling the toner removed in the cleaning step to the developing device, and can be appropriately selected depending on the purpose. For example, a known transport means can be used. The recycling process is not particularly limited as long as it is a process for recycling the toner removed by the cleaning process back into the developing device, and can be appropriately selected depending on the purpose. For example, the recycling process can be performed by the recycling means.
[0141] Here, the image forming apparatus according to the present invention will be described with reference to the drawings. Note that the present invention is not limited to the following embodiment, and can be modified within the scope of what a person skilled in the art can imagine, such as other embodiments, additions, modifications, deletions, etc., and any aspect is included in the scope of the present invention as long as it achieves the functions and effects of the present invention.
[0142] One embodiment of a method for forming an image by the image forming apparatus of the present invention will be described with reference to Fig. 1. Although a printer is shown as an example of the image forming apparatus of this embodiment, the image forming apparatus of the present invention is not particularly limited as long as it is capable of forming an image using toner in a copier, facsimile, multifunction machine, etc.
[0143] FIG. 1 is a schematic diagram showing an example of an image forming apparatus according to the present invention. The image forming apparatus includes a paper feed section 210, a conveying section 220, an image creating section 230, a transfer section 240, and a fixing unit 250. The paper feed section 210 includes a paper feed cassette 211 in which the paper P to be fed is stacked, and a paper feed roller 212 that feeds the paper P stacked in the paper feed cassette 211 one sheet at a time.
[0144] The conveying section 220 includes a roller 221 that conveys the paper P fed by the paper feed roller 212 toward the transfer section 240, a pair of timing rollers 222 that hold the leading end of the paper P conveyed by the roller 221 and wait to send the paper to the transfer section 240 at a predetermined timing, and a paper discharge roller 223 that discharges the paper P with the color toner image fixed thereto onto a paper discharge tray 224.
[0145] The image creating section 230 includes, spaced at a predetermined interval from left to right in FIG. 1, an image forming unit 180Y that forms an image using a developer containing yellow toner, an image forming unit 180C that uses a developer containing cyan toner, an image forming unit 180M that uses a developer containing magenta toner, an image forming unit 180K that uses a developer containing black toner, and an exposure device 233.
[0146] The image forming unit 180 (180Y, 180C, 180M, 180K) is arranged to be rotatable clockwise in FIG. 1, and includes a photoconductor drum 231 (231Y, 231C, 231M, 231K) on which an electrostatic latent image and a toner image are formed, a charger 232 (232Y, 232C, 232M, 232K) that uniformly charges the surface of the photoconductor drum 231 (231Y, 231C, 231M, 231K), and a cleaner 236 (236Y, 236C, 236M, 236K) that removes toner remaining on the surface of the photoconductor drum 231 (231Y, 231C, 231M, 231K).
[0147] Image forming units 180 (180Y, 180C, 180M, 180K) are equipped with toner bottles 234 (234Y, 234C, 234M, 234K) that contain toner of each color, and sub-hoppers 160 (160Y, 160C, 160M, 160K) for replenishing the toner supplied from toner bottles 234 (234Y, 234C, 234M, 234K).
[0148] Incidentally, when referring to any one of the image forming units 180 (180Y, 180C, 180M, 180K), it will be referred to as the image forming unit.
[0149] The exposure unit 233 irradiates the photosensitive drum 231 with laser light L emitted from a light source 233a based on image information by reflecting the light on a polygon mirror 233b (233bY, 233bC, 233bM, 233bK) that is rotated by a motor. The developer contains toner and carrier. The four image forming units 180 (180Y, 180C, 180M, 180K) have substantially the same mechanical configuration, except for the developer used therein.
[0150] The transfer unit 240 includes a drive roller 241 and a driven roller 242, an intermediate transfer belt 243 that can rotate counterclockwise in FIG. 1 as the drive roller 241 is driven, primary transfer rollers 244 (244Y, 244C, 244M, 244K) arranged opposite the photosensitive drums 231 (231Y, 231C, 231M, 231K) across the intermediate transfer belt 243, and secondary opposing rollers 245 and 246 arranged opposite each other across the intermediate transfer belt 243 at the transfer position of the toner image to paper.
[0151] The fixing device 250 has a heater installed inside and includes a pressure roller 252 that forms a nip by rotatably pressing a fixing belt 251 that heats the paper P against the fixing belt 251. This applies heat and pressure to the color toner image on the paper P, and the color toner image is fixed. The paper P on which the color toner image has been fixed is discharged onto a paper discharge tray 224 by a paper discharge roller 223, completing a series of image forming processes. EXAMPLES
[0152] EXAMPLES Examples and comparative examples of the present invention will be described below, but the present invention is not limited to these examples in any way.
[0153] First, each measurement method will be described.
[0154] [Measurement of glass transition temperature (Tg) and melting point] The glass transition temperature (Tg) of the resin was measured using a differential scanning calorimeter (DSC) Q-200 (manufactured by TA Instruments). 5.0 mg of the resin sample was placed in an aluminum sample pan, placed on a holder unit, and set in an electric furnace. 10 mg of alumina (aluminum oxide, Fujifilm Wako Pure Chemical Industries, Ltd.) was used as a reference, placed in an aluminum sample pan like the sample. In a nitrogen atmosphere, the sample was heated from 0°C to 150°C at a heating rate of 10°C / min (first heating), then cooled from 150°C to 0°C at a heating rate of 10°C / min (cooling down process), and heated again to 150°C at a heating rate of 10°C / min (second heating). The heat absorption and heat generation changes during the above process were measured, and a graph of the temperature and heat absorption and generation was drawn to obtain a DSC curve. The obtained DSC curve was analyzed using an analysis program in the Q-200 system. The DSC curve in the second heating step was selected, and the glass transition temperature of the resin sample was calculated from the intersection of the extension of the baseline of the DSC curve at a temperature lower than the enthalpy relaxation of the endotherm and the tangent showing the maximum slope of the enthalpy relaxation. Similarly, the DSC curve in the second heating step was selected, and the peak temperature of the endotherm was determined as the melting point of the crystalline resin or wax sample.
[0155] [Measurement of weight average molecular weight (Mw)] The weight average molecular weight (Mw) of the resin was measured using a gel permeation chromatography (GPC) measuring device HLC-8220GPC (manufactured by Tosoh Corporation). As the column, a TSKgel SuperHZM-H 15 cm triple column (manufactured by Tosoh Corporation) was used. The resin to be measured was dissolved in tetrahydrofuran (THF) (containing stabilizer, manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) at 0.15% by mass, filtered through a 0.2 μm filter, and the filtrate was used as a sample. 100 μl of the THF sample solution was injected into the measuring device and measured at a flow rate of 0.35 ml / min under an environment of a temperature of 40° C. The molecular weight was calculated using a calibration curve prepared using a monodisperse polystyrene standard sample. As the polystyrene standard sample, ShowdexSTANDARD series manufactured by Showa Denko was used to prepare THF solutions (solutions A to C) of the following three types of monodisperse polystyrene standard samples, and measurements were performed under the above conditions. A calibration curve was prepared by using the retention time of the peak top as the light scattering molecular weight of the monodisperse polystyrene standard sample. An RI (refractive index) detector was used as the detector. ·Solution A: S-7300 2.5mg, S-602 2.5mg, S-46 2.5mg, S-2.8 2.5mg, THF 50mL ·Solution B: S-3500 2.5mg, S-277 2.5mg, S-18 2.5mg, S-1.3 2.5mg, THF 50mL ·Solution C: S-1700 2.5mg, S-136 2.5mg, S-6.7 2.5mg, toluene 2.5mg, THF 50mL
[0156] [Measurement of acid value (AV) and hydroxyl value (OHV)] The acid value (AV) and hydroxyl value (OHV) of the resin were measured according to the method specified in JIS K0070. The acid value was measured using a mixed solvent (acetone:methanol:toluene=12.5:12.5:75) of acetone (manufactured by Fuji Film Wako Pure Chemical Industries, Ltd.), methanol (manufactured by Fuji Film Wako Pure Chemical Industries, Ltd.), and toluene (manufactured by Fuji Film Wako Pure Chemical Industries, Ltd.), and the hydroxyl value was measured using tetrahydrofuran (THF) (manufactured by Fuji Film Wako Pure Chemical Industries, Ltd.).
[0157] [Measurement of volume average particle size (Dv)] The volume average particle diameter (Dv) of the resin particles and toner was measured using a Coulter Multisizer III (aperture diameter 100 μm, manufactured by Beckman Coulter) and an analysis software, Beckman Coulter Multisizer 3 (version 3.51, manufactured by Beckman Coulter). 10 mg of the measurement sample was added to 5 mL of 10 mass % surfactant (alkylbenzene sulfonate, Neogen SC-A, manufactured by Daiichi Kogyo Seiyaku Co., Ltd.), and dispersed for 1 minute with an ultrasonic disperser. Then, an arbitrary amount of 25 mL of electrolyte, Isoton III (manufactured by Beckman Coulter), was added and dispersed for 1 minute with an ultrasonic disperser to prepare a sample dispersion. Next, an appropriate amount of the electrolyte 100 mL and the sample dispersion were added to a beaker, and 30,000 particles were measured at a concentration at which the particle diameter of 30,000 particles could be measured in 20 seconds, and the volume average particle diameter (Dv) was obtained from the particle size distribution.
[0158] [Average circularity and amount of fine powder below 2μm] The average circularity of the resin particles and toner, and the amount of fine powder of 2 μm or less were measured using a flow type particle image analyzer FPIA-3000 (manufactured by SYSMEX Co., Ltd.). After preparing a 1% NaCl aqueous solution using first-class sodium chloride (manufactured by Fuji Film Wako Pure Chemical Industries, Ltd.), 0.1 to 5 ml of alkylbenzene sulfonate (Neogen, manufactured by Daiichi Kogyo Seiyaku Co., Ltd.) was added as a dispersant to 50 to 100 ml of the liquid that had been passed through a 0.45 μm filter, and 1 to 10 mg of the sample was added. This was dispersed for 1 minute using an ultrasonic disperser, and the measurement was performed using the dispersion liquid with the particle concentration adjusted to 5,000 to 15,000 particles / μl.
[0159] (Production Examples 1 to 20 of Polyester Resin (A)) -Production of polyester resins (A-1) to (A-20)- In a reaction vessel equipped with a cooling tube, a stirrer, and a nitrogen inlet tube, the materials shown in Tables 1 to 4 were added so that the molar ratio of hydroxyl groups to carboxylic acid (OH / COOH) was 1.2, and 1,000 ppm of tetrabutoxytitanate (titanium dihydroxybis(triethanolamine), manufactured by Tokyo Chemical Industry Co., Ltd.) was added as a condensation catalyst relative to the total monomer amount. The temperature was raised to 200°C over 2 hours under a nitrogen stream, and the temperature was further raised to 230°C over 8 hours, and the reaction was carried out for 5 hours while distilling off the water produced. After that, the reaction was carried out for 1 hour under a reduced pressure of 5mmHg to 15mmHg, and after cooling to 200°C, trimellitic anhydride (manufactured by Tokyo Chemical Industry Co., Ltd.) was added and the reaction was carried out at 200°C at normal pressure for 1 hour, and then the reaction was carried out under a reduced pressure of 5mmHg to 20mmHg until the desired molecular weight was reached, to obtain polyester resin (A) [polyester resin (A-1) to (A-20)]. The obtained [polyester resins (A-1) to (A-20)] were measured for glass transition point (Tg), weight average molecular weight, acid value (AV), hydroxyl value (OHV), and ratio (OHV / AV), and the results are shown in Tables 1 to 4.
[0160] (Polyester Resin Emulsion Production Examples 1 to 20) -Production of polyester resin emulsions (EM-1) to (EM-20)- In a 500 ml separable flask equipped with a stirrer, 150 parts by mass of [polyester resin (A-1)] and 150 parts by mass of methyl ethyl ketone (manufactured by Fuji Film Wako Pure Chemical Industries, Ltd.) were added, and sodium hydroxide (0.3 N) (manufactured by Fuji Film Wako Pure Chemical Industries, Ltd.) was added in an amount equivalent to a neutralization rate of 80% relative to the acid value of [polyester resin (A-1)] to prepare a resin mixture. Next, while stirring the resin mixture, 400 parts of ion-exchanged water was gradually added to perform phase inversion emulsification. Thereafter, the solvent was removed while reducing the pressure with an evaporator, and ion-exchanged water was added so that the solid content concentration was 25% by mass, to obtain [polyester resin emulsion (EM-1)]. [Polyester resins (A-2) to (A-20)] were treated in the same manner to obtain [polyester resin emulsions (EM-2) to (EM-20)]. The median diameter (D50) of the obtained polyester resin emulsions (EM-1) to (EM-20) was measured, and the results are shown in Tables 1 to 4.
[0161] (Production Examples 1 and 2 of Amorphous Polyester Resin (B)) -Production of amorphous polyester resins (B-1) and (B-2)- In a reaction vessel equipped with a cooling tube, a stirrer, and a nitrogen inlet tube, the acid monomer and alcohol monomer shown in Table 4 were added so that the molar ratio of hydroxyl group to carboxylic acid (OH / COOH) was 1.2, and 1,000 ppm of tetrabutoxy titanate was added as a condensation catalyst relative to the total monomer amount. The temperature was raised to 200°C over 2 hours under a nitrogen stream, and then the temperature was raised to 230°C over 8 hours, and the reaction was carried out for 5 hours while distilling off the water produced. After that, the reaction was carried out for 1 hour under a reduced pressure of 5mmHg to 15mmHg, and then the reaction was carried out for 1 hour at 200°C under normal pressure, and then the reaction was carried out further under a reduced pressure of 5mmHg to 20mmHg until the desired molecular weight was reached, thereby obtaining amorphous polyester resin (B) [amorphous polyester resin (B-1) to (B-2)]. The obtained [amorphous polyester resins (B-1) to (B-2)] were subjected to measurement of the glass transition point (Tg), weight average molecular weight, acid value (AV), and hydroxyl value (OHV). The results are shown in Table 4.
[0162] (Production Example of Crystalline Polyester Resin) -Production of crystalline polyester resin (C)- In a reaction vessel equipped with a cooling tube, a stirrer and a nitrogen inlet tube, 1,6-hexanediol (manufactured by Tokyo Chemical Industry Co., Ltd.) and sebacic acid (manufactured by Tokyo Chemical Industry Co., Ltd.) as a dicarboxylic acid component were added so that the molar ratio of hydroxyl group to carboxylic acid (OH / COOH) was 1.1, and titanium dihydroxybis(triethanolamine) (manufactured by Tokyo Chemical Industry Co., Ltd.) was added as a condensation catalyst at 500 ppm relative to the total monomer amount, and the mixture was heated to 180°C over 2 hours under a nitrogen stream, and reacted for 8 hours while distilling off the water produced. Next, the mixture was gradually heated to 220°C, and reacted for 5 hours under a nitrogen stream while distilling off the water produced, and then further reduced pressure of 5mmHg to 20mmHg was used to obtain [crystalline polyester resin (C)] having a melting point of 68°C, an acid value of 10.5mgKOH / g and a weight average molecular weight of 11,000.
[0163] (Production Example 1 of Crystalline Polyester Resin Dispersion) -Production of crystalline polyester resin dispersion (C-1)- In a reaction vessel equipped with a cooling tube, a thermometer and a stirrer, 10 parts by mass of [crystalline polyester resin (C)] and 90 parts by mass of ethyl acetate (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) were placed, heated to 77 ° C. to dissolve thoroughly, and cooled to 30 ° C. over 1 hour while stirring. Then, wet pulverization was performed using Ultraviscomill (manufactured by Imex) under conditions of a liquid delivery speed of 1.0 kg / hr, a disk peripheral speed of 10 m / sec, a 0.5 mm zirconia bead filling amount of 80 volume %, and 6 passes, and ethyl acetate was added to adjust the solid concentration to 10 wt %, to obtain a [crystalline polyester resin dispersion (C-1)] having a median diameter (D50) of 0.3 μm measured with a laser particle size distribution measuring device LA-920 (manufactured by Horiba, Ltd.).
[0164] (Crystalline polyester resin dispersion production example 2) -Production of crystalline polyester resin dispersion (C-2)- In a 500 ml separable flask equipped with a stirrer, 150 parts by mass of [crystalline polyester resin (C)], 75 parts by mass of methyl ethyl ketone (manufactured by Fuji Film Wako Pure Chemical Industries, Ltd.), and 75 parts by mass of isopropyl alcohol (manufactured by Fuji Film Wako Pure Chemical Industries, Ltd.) were placed, and the mixture was heated to 65 ° C. and dissolved. Then, an aqueous ammonia solution (manufactured by Fuji Film Wako Pure Chemical Industries, Ltd.) was added in an amount equivalent to a neutralization rate of 60% relative to the acid value of [crystalline polyester resin (C)] to prepare a resin mixture. Next, while stirring the resin mixture at 65 ° C., 400 parts of ion-exchanged water was gradually added to perform phase inversion emulsification. Thereafter, the solvent was removed while reducing the pressure with an evaporator, and ion-exchanged water was added so that the solid content concentration was 25 mass%, and a [crystalline polyester resin dispersion (C-2)] consisting of a crystalline polyester resin emulsion having a median diameter (D50) of 0.3 μm was obtained.
[0165] (Colorant masterbatch manufacturing examples 1-2) -Manufacture of colorant master batches (MB-1) to (MB-2)- 100 parts by mass of [amorphous polyester resin (B-1)], 100 parts by mass of cyan pigment (Pigment Blue 15:3), and 50 parts by mass of ion-exchanged water were thoroughly mixed and kneaded in an open roll type kneader (Kneadex / Mitsui Mining Co., Ltd.). The kneading temperature was 80°C, and then the temperature was raised to 120°C to remove water, thereby obtaining [colorant master batch (MB-1)] with a resin to pigment ratio (mass ratio) of 1:1. [Amorphous polyester resin (B-2)] was treated in the same manner to obtain [colorant master batch (MB-2)].
[0166] (Production Example of Colorant Dispersion) A container was charged with 30 parts by mass of cyan pigment (Pigment Blue 15:3), 3 parts by mass of anionic surfactant (linear alkylbenzenesulfonate sodium (Neogen), manufactured by Daiichi Kogyo Seiyaku Co., Ltd.), and 67 parts by mass of ion-exchanged water, which were dispersed for 30 minutes at 6,000 rpm using a TK Homomixer (manufactured by Tokushu Kika Co., Ltd.), and then a dispersion treatment was performed for 20 passes at a pressure of 245 MPa using a high-pressure disperser Ultimizer (Starburst, manufactured by Sugino Machine Co., Ltd.). Thereafter, ion-exchanged water was added so that the solid content concentration was 25% by mass, and a [colorant dispersion] was obtained.
[0167] (Wax Dispersion Production Example 1) -Production of wax dispersion (W-1)- In a reaction vessel equipped with a cooling tube, a thermometer and a stirrer, 20 parts by mass of ester wax (WE-11, manufactured by NOF Corp.) with a melting point of 70°C and 80 parts by mass of ethyl acetate were placed, heated to 77°C to dissolve thoroughly, and cooled to 30°C over 1 hour while stirring. Then, using an Ultraviscomill (manufactured by Imex), the mixture was wet-pulverized under the conditions of a liquid delivery rate of 1.0 kg / hr, a disk circumferential speed of 10 m / sec, a 0.5 mm zirconia bead filling amount of 80% by volume, and 6 passes, and ethyl acetate was added to adjust the solid concentration to 20% by mass, to obtain a wax dispersion (W-1) having a median diameter (D50) of 0.6 μm as measured by a laser particle size distribution analyzer LA-920 (manufactured by Horiba, Ltd.).
[0168] (Wax Dispersion Production Example 2) -Production of wax dispersion (W-2)- A container was charged with 30 parts by mass of ester wax (WE-11, NOF Corp.) with a melting point of 70°C, 2 parts by mass of anionic surfactant (sodium linear alkylbenzene sulfonate (Neogen), Daiichi Kogyo Seiyaku Co., Ltd.), and 68 parts by mass of ion-exchanged water, and the container was cooled with ice water while being dispersed at 8,000 rpm for 2 hours using a TK homomixer (Tokushu Kika Co., Ltd.). Thereafter, ion-exchanged water was added so that the solid content concentration was 25% by mass, and a wax dispersion (W-2) with a median diameter (D50) of 0.6 μm was obtained, as measured by a laser particle size distribution analyzer LA-920 (Horiba, Ltd.).
[0169] (Production Examples 1 and 2 of Core Particle Dispersion) -Production of core particle dispersions (CR-1) to (CR-2) by dissolution suspension method- In a container equipped with a stirrer and thermometer, 68 parts by mass of ion-exchanged water, 1 part by mass of sodium carboxymethylcellulose (Dai-ichi Kogyo Seiyaku Co., Ltd.), 16 parts by mass of a 48% aqueous solution of sodium dodecyl diphenyl ether disulfonate (Eleminol MON-7, Sanyo Chemical Industries, Ltd.), and 5 parts by mass of ethyl acetate were mixed and stirred, and 10 parts by mass of a particle size control emulsion consisting of a copolymer of styrene-methacrylic acid-butyl acrylate-ethylene oxide methacrylic acid adduct sulfate sodium salt (solid concentration 20%, median diameter 50 nm, Sanyo Chemical Industries, Ltd.) was added to prepare an [aqueous phase solution]. Next, in another container equipped with a stirrer and a thermometer, 76 parts by mass of [amorphous polyester resin (B-1)], 60 parts by mass of [crystalline polyester resin dispersion (C-1)], 30 parts by mass of [wax dispersion (W-1)], and 12 parts by mass of [colorant master batch (MB-1)] were added, and ethyl acetate was added so that the solid content concentration became 50% by mass, and the mixture was stirred and thoroughly dissolved. Next, the mixture was dispersed at a rotation speed of 8,000 rpm for 2 hours using a TK homomixer (manufactured by Tokushu Kika Co., Ltd.), and the mixture was uniformly dissolved and dispersed to prepare the [oil phase]. 50 parts by mass of the [oil phase] was added to a vessel containing 75 parts by mass of the [aqueous phase solution], and mixed at a liquid temperature of 30°C to 40°C with a TK Homomixer (manufactured by Tokushu Kika Co., Ltd.) at a rotation speed of 12,000 rpm for 1 minute to obtain an emulsified slurry. The obtained emulsified slurry was transferred to another container equipped with a stirrer, a nitrogen inlet tube, and a thermometer, and the temperature was raised to 50°C while stirring, and ethyl acetate was distilled off under a nitrogen stream. Next, a 10% by mass aqueous solution of sodium hydroxide (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was added to adjust the pH of the emulsified slurry to 12, and the mixture was heated in a 45°C environment for 10 hours to dissolve and remove the particle size control emulsion adhering to the particle surfaces in the emulsified slurry, and the solid content was obtained by suction filtration. The obtained solid content was reslurried in ion-exchanged water in an amount equivalent to 40 times the mass of the solid content, and a washing process was performed twice in which the solid content was thoroughly stirred and then filtered. After that, ion-exchanged water was added to the solid content again to obtain a core particle dispersion liquid (C-1) with a solid content concentration adjusted to 25 mass%. [Polyester resin (B-2)] was treated in the same manner, except that [colorant master batch (MB-1)] was changed to [colorant master batch (MB-2)], to obtain [core particle dispersion (CR-2)]. The resulting [core particle dispersions (CR-1) to (CR-2)] were subjected to measurement of the volume average particle size and the average circularity. The results are shown in Table 5.
[0170] (Production Example 3 of Core Particle Dispersion) -Production of core particle dispersion (CR-3) by emulsion aggregation method- In a container equipped with a stirrer, 150 parts by mass of [amorphous polyester resin (B-1)] and 150 parts by mass of methyl ethyl ketone were added, and sodium hydroxide (0.3N) was added in an amount equivalent to a neutralization rate of 70% relative to the acid value of [amorphous polyester resin (B-1)] to prepare a resin mixture. Next, while stirring the resin mixture, 400 parts of ion-exchanged water was gradually added to perform phase inversion emulsification. Thereafter, the solvent was removed while reducing the pressure with an evaporator, and ion-exchanged water was added so that the solid content concentration was 25% by mass, and a [polyester resin (B) emulsion] having a median diameter (D50) of 0.2 μm measured with a laser particle size distribution analyzer LA-920 (manufactured by Horiba, Ltd.) was obtained. Next, in another container equipped with a stirrer and a thermometer, 328 parts by mass of [polyester resin (B) emulsion], 24 parts by mass of [crystalline polyester resin dispersion (C-2)], 24 parts by mass of [wax dispersion (W-2)], and 24 parts by mass of [colorant dispersion] were placed, and 20 parts by mass of a 20% by mass aqueous magnesium sulfate solution (manufactured by Fuji Film Wako Pure Chemical Industries, Ltd.) was dropped at 2 parts by mass / min while stirring, and then the temperature was raised to 55 ° C. Then, when the volume average particle size (Dv) of the emulsion became 5 μm, 120 parts by mass of a 10% by mass aqueous sodium chloride solution (manufactured by Fuji Film Wako Pure Chemical Industries, Ltd.) was added, the temperature was raised to 60 ° C. and stirred for 1 hour, and then cooled to room temperature, and ion-exchanged water was added to obtain [core particle dispersion (CR-3)] adjusted to a solid concentration of 25%. The volume average particle diameter and average circularity of the obtained [core particle dispersion (CR-3)] were measured. The results are shown in Table 5.
[0171] (Production Example 4 of Core Particle Dispersion) - Manufacturing of core particle dispersion (CR-4) by melt kneading method - 76 parts by mass of [amorphous polyester resin (B-1)], 6 parts by mass of [crystalline polyester resin (C)], 6 parts by mass of ester wax (WE-11, NOF Corp.) with a melting point of 70°C, and 12 parts by mass of [colorant master batch (MB-1)] were premixed using a Henschel mixer (FM10B, Mitsui Miike Chemical Engineering Co., Ltd.), and then melted and kneaded at 85°C in a twin-screw kneader (PCM-30, Ikegai Corp.). The kneaded product obtained was cooled to room temperature and then coarsely pulverized to 200μm to 300μm using a hammer mill. Next, the mixture was finely ground using a counter jet mill (200AFG, manufactured by Hosokawa Micron Corporation) while appropriately adjusting the grinding air pressure so that the weight average particle size was 5.6±0.3μm, and then classified using an air classifier (MDS-I, manufactured by Nippon Pneumatic Mfg. Co., Ltd.) while appropriately adjusting the louver opening so that the weight average particle size was 6.0±0.2μm and the amount of fine powder of 4μm or less was 10% or less by number, thereby obtaining [classified particles]. Next, 25 parts by mass of [classified particles], 73 parts by mass of ion-exchanged water, and 2 parts by mass of anionic surfactant (sodium linear alkylbenzene sulfonate (Neogen), manufactured by Daiichi Kogyo Seiyaku Co., Ltd.) were placed in another container equipped with a stirrer, and thoroughly stirred to obtain [core particle dispersion (CR-4)] adjusted to a solid content concentration of 25%. The volume average particle diameter and average circularity of the obtained [core particle dispersion (CR-4)] were measured. The results are shown in Table 5.
[0172] (Carrier manufacturing example) As the core material, 5,000 parts by mass of Mn ferrite particles (weight average particle size: 35 μm) were used. A coating liquid was used that was prepared by dispersing 300 parts by mass of toluene (manufactured by Fuji Film Wako Pure Chemical Industries, Ltd.) as a coating material, 300 parts by mass of butyl cellosolve (manufactured by Fuji Film Wako Pure Chemical Industries, Ltd.), 60 parts by mass of acrylic resin solution (composition ratio methacrylic acid:methyl methacrylate:2-hydroxyethyl acrylate=5:9:3, solid content 50 mass% in toluene solution, Tg 38°C), 15 masses of N-tetramethoxymethylbenzoguanamine resin solution (degree of polymerization 1.5, solid content 77 mass% in toluene solution), and 15 masses of alumina particles (average primary particle diameter 0.30 μm) with a stirrer for 10 minutes. The core material was coated with the coating liquid by a coating device that was equipped with a rotating bottom plate disk and stirring blades in a fluidized bed to form a swirling flow. The resulting coating was baked in an electric furnace at 220°C for 2 hours to obtain the [carrier].
[0173] <Example 1> -Evaluation of the coagulation properties of shell particles against coagulating salts- In a container equipped with a stirrer and a thermometer, 320 parts by mass of core particle dispersion (CR-1) (solid concentration 25% by mass) and 80 parts by mass of polyester resin emulsion (EM-1) (solid concentration 25% by mass) were placed and stirred, and a 20% by mass aqueous magnesium sulfate solution was dropped at a rate of 2 parts by mass / min in an amount such that magnesium sulfate was 1% by mass relative to the total solid content, and then the temperature was raised to 55°C and stirring was performed for 30 minutes. Thereafter, 100 parts by mass of a 10% by mass aqueous sodium chloride solution was added, the temperature was raised to 70°C and stirring was performed for 1 hour, and then sampling was performed to measure the volume average particle size (Dv), average circularity, and amount of fine powder with Dv of 2 μm or less of the particles after the aggregation of shell particles. Evaluation was performed based on the following evaluation criteria. Similarly, the amount of the 20% by mass aqueous magnesium sulfate solution added was changed to amounts such that magnesium sulfate was 2%, 3%, and 4% by mass relative to the total solid content, and similar treatment and evaluation were performed. Here, the smaller the amount of fine powder having a Dv of 2 μm or less, the better the aggregability of the shell particles to the core particles. Even if the amount of fine powder having a Dv of 2 μm or less is small, if the volume average particle size of the shell particles after aggregation is 1 μm or more larger than the volume average particle size of the core particles, the aggregation stability can be said to be poor. Here, ΔDv is the volume average particle diameter of the particles after the shell particles are aggregated minus the volume average particle diameter of the core particles. The best rank evaluation result among the levels of the amount of magnesium sulfate added as the aggregating salt was taken as the overall evaluation result of the aggregability of the shell particles, and the results are shown in Tables 6 to 10. Tables 6 to 10 also show the amount of fine powder (number %) with Dv of 2 μm or less. [Evaluation Criteria] ◎: ΔDv is less than 1 μm and the amount of fine powder with Dv of 2 μm or less is less than 0.5% by number ○: ΔDv is less than 1 μm, and the amount of fine powder with Dv of 2 μm or less is 0.5% by number or more and less than 3% by number. △: ΔDv is less than 1 μm and the amount of fine powder with Dv of 2 μm or less is between 3% and 10% by number. ×: ΔDv is less than 1 μm and the amount of fine powder with Dv of 2 μm or less is 10% by number or more -: ΔDv is 1μm or more
[0174] -Production of resin particles (T) or toner- After the coagulation of the shell particles against the coagulated salt, the average circularity was measured for the sample with the best coagulation of the shell particles under the condition of the amount of coagulated salt added. For samples with an average circularity of less than 0.970, stirring was further performed at 70°C until the average circularity reached 0.970. The container was then transferred to an ice water bath and cooled to room temperature, and the solid content was obtained by suction filtration. To the obtained solid content, 800 parts by mass of ion-exchanged water was added, and the mixture was stirred to reslurry, and then suction filtered to obtain a solid content. This process was repeated five times, and then the mixture was dried in a circulating air dryer at 45° C. for 48 hours. The mixture was then sieved through a 75 μm mesh to obtain resin particles (T) [resin particles (T-1)]. 100 parts by mass of the obtained [resin particles (T-1)] were mixed with 1.0 part by mass of hydrophobic silica (HDK-2000, manufactured by Wacker Chemie) and 0.3 part by mass of titanium oxide (MT-150AI, manufactured by Teika Co., Ltd.) using a Henschel mixer, and then sieved through a 25 μm mesh to obtain [toner (TN-1)]. The volume average particle size (Dv) and average circularity of the obtained toner were measured, and the results are shown in Tables 6 to 10.
[0175] -Evaluation of the aggregation uniformity of shell particles- [Resin particles (T-1)] were embedded in a commercially available epoxy resin (S-31, DEVCON) and cured, and then ultrathinly sliced with a diamond knife using an ultrasonic ultramicrotome (Leica EM UC7, Leica). The thickness of the slices was adjusted to about 100 nm using the interference color of the epoxy resin. The slices were then placed on a copper grid mesh and steam stained using a 5% aqueous solution of commercially available ruthenium tetroxide (Fujifilm Wako Pure Chemical Industries, Ltd.). Observation was performed using a transmission electron microscope (JEM-2100F, JEOL Ltd.), and an image of the cross section of the resin particles in the slice was recorded. The cross section of the toner particles on which the shell layer is formed is determined by whether or not the crystalline polyester resin, wax, and colorant are exposed on the particle surface, so that the state of shell layer formation is determined by whether or not these components are exposed on the outermost surface of the resin particles. Specifically, the resin particle surfaces of 30 randomly selected resin particles were observed in cross-sectional images, and the ratio (P) of the number of particles in which the crystalline polyester resin, wax, and colorant were not exposed at all was calculated. It can be said that the higher the ratio (P), the higher the uniformity of the aggregation state between shell particles. Evaluation was performed based on the following evaluation criteria, and the results are shown in Tables 6 to 10. [Evaluation Criteria] ◎: Proportion (P) is 90% or more ○: Proportion (P) is 80% or more but less than 90% △: Proportion (P) is 60% or more but less than 80% ×: Proportion (P) is less than 60%
[0176] -Manufacture of developer- 100 parts by weight of [carrier] and 7 parts by weight of [toner (TN-1)] were mixed uniformly for 5 minutes at 48 rpm using a turbulent mixer (manufactured by Willy & Bachofen (WAB)) that rotates the container to mix, to obtain a two-component developer [developer (D-1)].
[0177] -Evaluation of the mechanical durability of toner- [Developer (D-1)] was loaded into the development unit of a digital color multifunction printer RICOH IM C5500 (manufactured by Ricoh Co., Ltd.), and after running 30,000 blank prints in monochrome mode, the developer was removed and placed in a gauge with a mesh of 32 μm opening, and an air blow was performed to separate the toner and carrier. Next, 10 g of the obtained carrier was placed in a 50 ml glass bottle, 10 ml of methyl ethyl ketone was added, and the bottle was shaken 50 times and left to stand for 10 minutes. After that, the supernatant methyl ethyl ketone solution was placed in a glass cell, and the transmittance of the methyl ethyl ketone solution was measured using a turbidity meter. Evaluation was performed based on the following evaluation criteria, and the results are shown in Tables 6 to 10. [Evaluation Criteria] ◎: Transmittance is 95% or more ○: Transmittance is 90% or more and less than 95% △: Transmittance is 80% or more but less than 90% ×: Transmittance is less than 80%
[0178] <Examples 2 to 19 and Comparative Examples 1 to 7> [Resin particles (T-2) to (T-25)], [Toners (TN-2) to (TN-25)], and [Developers (D-2) to (D-25)] were obtained in the same manner as in Example 1, except that the combinations of [Core particle dispersions (CR-1) to (CR-4)] and [Polyester resin emulsions (EM-1) to (EM-20)] shown in Tables 6 to 10 were changed. Each evaluation was performed in the same manner as in Example 1, and the results are shown in Tables 6 to 10.
[0179] [Table 1]
[0180] [Table 2]
[0181] [Table 3]
[0182] [Table 4]
[0183] [Table 5]
[0184] [Table 6]
[0185] [Table 7]
[0186] [Table 8]
[0187] [Table 9]
[0188] [Table 10]
[0189] For example, aspects of the present invention are as follows. <1> A polyester resin emulsion for a toner, comprising resin particles (S) containing a polyester resin (A) obtained by polycondensation of an alcohol component and a carboxylic acid component, dispersed in an aqueous medium, The alcohol component contains a trihydric or tetrahydric alcohol having a linear or branched saturated fatty acid skeleton having 4 to 6 carbon atoms, The polyester resin emulsion for toner is characterized in that the ratio (OHV / AV) of the hydroxyl value (OHV) of the polyester resin (A) to the acid value (AV) of the polyester resin (A) is 0.20 or more and 0.60 or less. <2> The acid value (AV) of the polyester resin (A) is 15 mgKOH / g or more and 30 mgKOH / g or less. <1> 2. The polyester resin emulsion for toner according to claim 1, <3> The shell resin emulsion is used for producing a toner having a core-shell structure composed of core particles containing a binder resin and shell particles covering the core particles. <1> From the above <2> 2. The polyester resin emulsion for toner according to claim 1, <4> The binder resin contains an amorphous polyester resin (B). <3> 2. The polyester resin emulsion for toner according to claim 1, <5> The alcohol component contains at least one selected from 1,2-propanediol, 1,3-propanediol, 1,4-butanediol, and 2,3-butanediol in an amount of 30 mol % or more based on the total amount of the alcohol component. <1> From the above <4> 2. The polyester resin emulsion for toner according to claim 1, <6> The polyester resin (A) contains a repeating unit derived from polyethylene terephthalate (PET) which is a condensate of terephthalic acid and ethylene glycol. <1> From the above <5> 2. The polyester resin emulsion for toner according to claim 1, <7> The glass transition temperature (Tg) of the resin particles (S) at the second heating stage in differential scanning calorimetry (DSC) is 60° C. or higher and 75° C. or lower. <1> From the above <6> 2. The polyester resin emulsion for toner according to claim 1, <8> Resin particles (T) having a core-shell structure composed of core particles containing a binder resin and shell particles covering the core particles, The shell particles are <1> From the above <7> The present invention relates to resin particles formed from the polyester resin emulsion for toner according to any one of the above items. <9> A toner having a core-shell structure composed of core particles containing a binder resin and shell particles covering the core particles, The shell particles are <1> From the above <7> 2. A toner comprising the polyester resin emulsion for toner according to claim 1.
[0190] The above <1> From the above <7> The polyester resin emulsion for toner according to any one of the preceding claims. <8> The resin particles according to <9> According to the toner described in the above, the conventional problems can be solved and the object of the present invention can be achieved. [Explanation of symbols]
[0191] 160Y Sub hopper (yellow) 160C Sub hopper (cyan) 160M Sub Hopper (Magenta) 160K Subhopper (Black) 180Y Image forming unit (yellow) 180C Image forming unit (cyan) 180M Image forming unit (magenta) 180K Image Forming Unit (Black) 210 Paper feed section 211 Paper feed cassette 212 Paper feed roller 220 Conveyor 221 Lola 222 Timing roller 223 Paper ejection roller 224 Output tray 230 Image creation section 231Y Photoconductor drum (yellow) 231C Photoconductor drum (cyan) 231M Photoconductor Drum (Magenta) 231K Photoconductor drum (black) 232Y Charger (Yellow) 232C Charger (cyan) 232M Charger (Magenta) 232K Charger (Black) 233 Exposure device 233a light source 233bY Polygon mirror (yellow) 233bC Polygon mirror (cyan) 233bM Polygon Mirror (Magenta) 233bK Polygon Mirror (Black) 234Y Toner bottle (yellow) 234C Toner bottle (cyan) 234M Toner Bottle (Magenta) 234K Toner Bottle (Black) 236Y Cleaning machine (yellow) 236C Cleaning Machine (Cyan) 236M Cleaner (Magenta) 236K Cleaner (Black) 240 Transcription Unit 241 Drive roller 242 Driven roller 243 Intermediate transfer belt 244 Primary transfer roller 244Y Primary transfer roller (yellow) 244C Primary transfer roller (cyan) 244M Primary transfer roller (magenta) 244K Primary transfer roller (black) 245 Secondary opposing roller 246 Secondary transfer roller 250 Fixing unit 251 Fixing belt 252 Pressure roller L Laser P paper [Prior art documents] [Patent documents]
[0192] [Patent Document 1] Patent No. 6632066
Claims
1. A polyester resin emulsion for a toner, comprising resin particles (S) containing a polyester resin (A) obtained by polycondensing an alcohol component and a carboxylic acid component, dispersed in an aqueous medium, The alcohol component contains a trihydric or tetrahydric alcohol having a linear or branched saturated fatty acid skeleton having 4 to 6 carbon atoms, A polyester resin emulsion for toner, characterized in that a ratio (OHV / AV) of a hydroxyl value (OHV) of the polyester resin (A) to an acid value (AV) of the polyester resin (A) is 0.20 or more and 0.60 or less.
2. 2. The polyester resin emulsion for toner according to claim 1, wherein the acid value (AV) of the polyester resin (A) is 15 mgKOH / g or more and 30 mgKOH / g or less.
3. 3. The polyester resin emulsion for toner according to claim 1, which is a shell resin emulsion used in the production of a toner having a core-shell structure consisting of core particles containing a binder resin and shell particles covering the core particles.
4. The polyester resin emulsion for toner according to claim 3 , wherein the binder resin contains an amorphous polyester resin (B).
5. 3. The polyester resin emulsion for toner according to claim 1, wherein the alcohol component contains at least one selected from the group consisting of 1,2-propanediol, 1,3-propanediol, 1,4-butanediol, and 2,3-butanediol in an amount of 30 mol % or more based on the total amount of the alcohol component.
6. 3. The polyester resin emulsion for toner according to claim 1, wherein the polyester resin (A) contains a repeating unit derived from polyethylene terephthalate (PET) which is a condensate of terephthalic acid and ethylene glycol.
7. 3. The polyester resin emulsion for toner according to claim 1, wherein the resin particles (S) have a glass transition temperature (Tg) of 60° C. or more and 75° C. or less in a second heating run in differential scanning calorimetry (DSC).
8. Resin particles (T) having a core-shell structure composed of core particles containing a binder resin and shell particles covering the core particles, 3. A resin particle, wherein the shell particle is formed from the polyester resin emulsion for toner according to claim 1.
9. A toner having a core-shell structure composed of core particles containing a binder resin and shell particles covering the core particles, 3. A toner, wherein the shell particles are formed from the polyester resin emulsion for toner according to claim 1.
Citation Information
Patent Citations
Method for producing toner for developing electrostatic images
JP6632066B2