Fastening method, method for manufacturing aluminum member, and aluminum member

The fastening method for aluminum members uses an intermediate layer and contact layer with unevenness to enhance friction and prevent corrosion, addressing the issues of reduced friction and corrosion in aluminum fastening systems.

JP2024168679APending Publication Date: 2024-12-05SINTOKOGIO LTD +1
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023085555
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-24
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

Aluminum members experience reduced frictional force and are prone to corrosion when fastened due to lower friction and potential electrochemical reactions with target members, especially when coated with fluoropolymer-based coatings.

Method used

A fastening method involving the formation of an aluminum member with an intermediate layer containing amorphous materials and a contact layer of aluminum hydroxide, featuring unevenness that pierces through a resin film on the target member, enhancing friction and preventing corrosion by interposing an insulating layer.

Benefits of technology

The method achieves high frictional properties and corrosion resistance by stabilizing the fastening interface through the anchor effect of unevenness and insulating intermediate layers, preventing electrochemical reactions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024168679000001_ABST
    Figure 2024168679000001_ABST
Patent Text Reader

Abstract

To provide a fastening method of an object member and an aluminum member having high friction property and high corrosion resistance.SOLUTION: A fastening method includes a preparing step, a forming step, and a fastening step. In the preparing step, an object member and an aluminum member are prepared. The object member has a resin film on a surface thereof. In the forming step, a middle layer and a contact layer which is arranged on the middle layer and has an irregularity capable of contacting the object member are formed on a surface of the aluminum member. In the fastening step, the aluminum member and the object member are fastened while thrusting the irregularity of the aluminum member into the resin film of the object member. The middle layer has an amorphous substance including aluminum atoms and oxygen atoms, or a layered double hydroxide including an amorphous substance, aluminum atoms, and oxygen atoms. The contact layer contains aluminum hydroxide. The irregularity has a small projection length compared to a thickness of the resin film of the object member.SELECTED DRAWING: Figure 10
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a fastening method, a manufacturing method for an aluminum member, and an aluminum member. [Background technology]

[0002] US Patent No. 5,399,633 discloses a method for improving the thread surface of a pipe joint. The method includes the steps of surface treating the entire surface of the female and male wedge threads, applying a fluoropolymer-based coating to designated areas of the female and male wedge threads, and applying a resin coating to the entire threads of the female and male wedge threads. The resin coating adheres to the areas lacking the fluoropolymer-based coating. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] Special table number 2013-507588 Summary of the Invention [Problem to be solved by the invention]

[0004] Aluminum can be used for fastening members because it is lighter than iron. In some cases, the fastening member and the target member fastened by the fastening member may be easily released as the frictional force between the members decreases. In addition, corrosion such as galvanic corrosion and stray current corrosion may occur between the members. According to the method described in Patent Document 1, the fastening member can be given corrosion resistance by coating the thread surface of the fastening member. On the other hand, the coating may not contribute to improving the frictional force, and may not ensure both the high frictional property and the high corrosion resistance required for the fastening member. Therefore, there is a demand for a fastening method, a manufacturing method for an aluminum member, and an aluminum member that can exhibit high frictional property and high corrosion resistance when fastening an aluminum member and a target member. [Means for solving the problem]

[0005] The fastening method according to the present disclosure includes a preparation step, a formation step, and a fastening step. In the preparation step, a target member and an aluminum member are prepared. The target member has a resin film on its surface. In the formation step, an intermediate layer and a contact layer, which is disposed on the intermediate layer and has irregularities that can come into contact with the target member, are formed on the surface of the aluminum member. In the fastening step, the aluminum member and the target member are fastened together while the irregularities of the aluminum member penetrate the resin film of the target member. The intermediate layer has both an amorphous substance containing aluminum atoms and oxygen atoms, or an amorphous substance and a layered double hydroxide containing aluminum atoms and oxygen atoms. The contact layer contains aluminum hydroxide. The irregularities have a protruding length that is smaller than the thickness of the resin film of the target member.

[0006] A manufacturing method for an aluminum member according to another aspect of the present disclosure is a manufacturing method for an aluminum member to be fastened to a target member having a resin film on its surface. The manufacturing method for an aluminum member includes a forming step. The forming step forms, on the surface of the aluminum member, an intermediate layer and a contact layer disposed on the intermediate layer and having irregularities capable of contacting the target member. The intermediate layer has both an amorphous substance containing aluminum atoms and oxygen atoms, or an amorphous substance and a layered double hydroxide containing aluminum atoms and oxygen atoms. The contact layer includes aluminum hydroxide. The irregularities have a protruding length smaller than the thickness of the resin film on the target member.

[0007] An aluminum member according to another aspect of the present disclosure is an aluminum member to be fastened to a target member having a resin film on its surface. The aluminum member includes an intermediate layer formed on the surface, and a contact layer. The contact layer is disposed on the intermediate layer and has a first irregularity capable of contacting the target member. The intermediate layer includes an amorphous substance containing aluminum atoms and oxygen atoms, or both an amorphous substance and a layered double hydroxide containing aluminum atoms and oxygen atoms. The contact layer includes aluminum hydroxide. The first irregularity has a protruding length smaller than the thickness of the resin film of the target member. Effect of the Invention

[0008] According to the present disclosure, high friction properties and high corrosion resistance can be exhibited when fastening an aluminum member to a target member. [Brief description of the drawings]

[0009] [Figure 1] 1 is a cross-sectional view showing a fastening unit including an aluminum member according to a first embodiment. [Diagram 2] 9 is an enlarged view of a fastening unit within a dashed line indicated by II in FIG. 1 and FIG. 8. [Diagram 3] FIG. 2 is a conceptual diagram of a blast processing device used in the manufacturing method of the aluminum member according to the first and second embodiments. [Figure 4] FIG. 2 is a diagram illustrating the configuration of a blast processing device used in the manufacturing method of the aluminum member according to the first and second embodiments. [Diagram 5] FIG. 5 is a cross-sectional view of the injection nozzle of FIG. [Figure 6] 1 is a flowchart of a fastening method including a manufacturing method of an aluminum member according to a first embodiment and a second embodiment. [Figure 7] FIG. 11 is a top view showing a fastening unit including an aluminum member according to a second embodiment. [Figure 8] FIG. 11 is a cross-sectional view showing a fastening unit including an aluminum member according to a second embodiment. [Figure 9] 13 is an enlarged view of an aluminum member and a fastening unit according to a modified example. FIG. [Figure 10] 5 shows the results of a friction test and a corrosion resistance test under processing conditions according to the embodiment. [Figure 11] 5 shows the results of a friction test and a corrosion resistance test under processing conditions according to the embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] [Outline of the first and second embodiments of the present disclosure] First, an overview of the first and second embodiments of the present disclosure will be described.

[0011] (Clause 1) A fastening method according to one aspect of the present disclosure includes a preparation step, a formation step, and a fastening step. In the preparation step, a target member having a resin film on its surface and an aluminum member are prepared. In the formation step, an intermediate layer and a contact layer, which is disposed on the intermediate layer and has irregularities capable of coming into contact with the target member, are formed on the surface of the aluminum member. In the fastening step, the aluminum member and the target member are fastened together while the irregularities of the aluminum member penetrate the resin film of the target member. The intermediate layer has both an amorphous substance containing aluminum atoms and oxygen atoms, or an amorphous substance and a layered double hydroxide containing aluminum atoms and oxygen atoms. The contact layer contains aluminum hydroxide. The irregularities have a protruding length smaller than the thickness of the resin film of the target member.

[0012] According to this fastening method, unevenness is formed in the contact layer on the surface of the aluminum member after the forming step. The contact layer contains aluminum hydroxide. Then, the unevenness of the aluminum member penetrates the resin film of the target member by the fastening step. Here, "piercing" includes the unevenness of the aluminum member penetrating into the resin film of the target member. The unevenness penetrating the resin film of the target member exerts an anchor effect in fastening with the target member. Therefore, high friction between the aluminum member and the target member can be stably maintained. In addition, an intermediate layer is formed on the surface of the aluminum member. The intermediate layer contains both an amorphous substance containing aluminum atoms and oxygen atoms, or an amorphous substance and a layered double hydroxide containing aluminum atoms and oxygen atoms. Therefore, even if the unevenness of the contact layer of the aluminum member penetrates the resin film of the target member, the intermediate layer is interposed between the fastened aluminum member and the target member. Therefore, corrosion of the aluminum member due to electrochemical action is suppressed, and this fastening method can stably maintain high corrosion resistance in fastening with the target member. In this manner, this fastening method can exhibit high friction and high corrosion resistance when fastening an aluminum member to an object member.

[0013] (Clause 2) In the fastening method described in Clause 1, the forming step may include a surface hydroxylation step of reacting the surface of the aluminum member with saturated water vapor under a pressure higher than atmospheric pressure and not more than 4.30 MPa to modify the surface of the aluminum member into aluminum hydroxide and form an intermediate layer and a contact layer. In this case, since the aluminum member reacts with water vapor under the above-mentioned pressure, this fastening method can form an intermediate layer and a contact layer having irregularities on the surface of the aluminum member.

[0014] (Clause 3) In the fastening method described in Clause 2, the surface hydroxylation step may involve reacting the surface of the aluminum member with saturated water vapor by applying heat of 100°C or more and 250°C or less. In this case, this fastening method can easily modify the surface of the aluminum member to aluminum hydroxide by reacting the aluminum member with water vapor by applying heat of more than 100°C. Also, this fastening method can form projections and recesses having appropriate rigidity by reacting the aluminum member with water vapor by applying heat of 100°C or more and 250°C or less.

[0015] (Clause 4) In the fastening method according to clause 2 or clause 3, the surface hydroxylation step may involve reacting the surface of the aluminum member with saturated water vapor for a treatment time of 30 minutes to 48 hours. In this case, this fastening method can form an aluminum hydroxide layer of an appropriate thickness on the surface of the aluminum member.

[0016] (Clause 5) In the fastening method according to any one of clauses 1 to 4, at least one of the maximum height and ten-point average roughness as defined in JIS-B0601: 1994 may be 0.5 μm or more on the surface of the aluminum member on which the unevenness is formed in the forming step. In this case, in this fastening method, unevenness having a maximum height and ten-point average roughness of 0.5 μm or more is formed on the surface of the aluminum member, and therefore unevenness that greatly contributes to friction is formed.

[0017] (Clause 6) In the fastening method according to any one of clauses 1 to 5, on the surface of the aluminum member on which the unevenness is formed in the forming step, the ratio of the maximum height defined in JIS-B0601:1994 to the ten-point average roughness defined in JIS-B0601:1994 may be 1.0 or more and 2.0 or less. In this case, this fastening method can form unevenness that can exhibit high friction properties and high corrosion resistance.

[0018] (Clause 7) In the fastening method according to any one of Clauses 1 to 6, the surface of the aluminum member on which the irregularities are formed in the forming step may have a developed interface area ratio of a contour curved surface defined in JIS-B0681-2: 2018 of 10% or more. In this case, in this fastening method, an appropriate number of irregularities can be formed on the surface of the aluminum member, and high friction can be exhibited when fastening the aluminum member to a target member.

[0019] (Clause 8) In the fastening method described in any one of clauses 1 to 7, the thickness of the resin film of the target member may be 5 μm or more and 50 μm or less. In this case, in this fastening method, since the thickness of the resin film is 5 μm or more, the unevenness of the contact layer of the aluminum member can be properly inserted into the resin film of the target member. In addition, in this fastening method, since the thickness of the resin film is 50 μm or less, the degree to which the resin film is deformed relative to the aluminum member when friction occurs between the aluminum member and the target member is reduced, and breakage can be suppressed. As a result, this fastening method can properly exert a high frictional force between the aluminum member and the target member.

[0020] (Clause 9) A manufacturing method for an aluminum member according to another aspect of the present disclosure is a manufacturing method for an aluminum member to be fastened to a target member having a resin film on its surface. The manufacturing method for an aluminum member includes a forming step. The forming step forms, on the surface of the aluminum member, an intermediate layer and a contact layer disposed on the intermediate layer and having irregularities capable of coming into contact with the target member. The intermediate layer has both an amorphous substance containing aluminum atoms and oxygen atoms, or an amorphous substance and a layered double hydroxide containing aluminum atoms and oxygen atoms. The contact layer contains aluminum hydroxide. The irregularities have a protruding length smaller than the thickness of the resin film on the target member.

[0021] According to this method for manufacturing an aluminum member, unevenness is formed in the contact layer on the surface of the aluminum member after the forming step. The contact layer includes aluminum hydroxide. The unevenness of the aluminum member can penetrate the resin film of the target member. The unevenness penetrating the resin film of the target member provides an anchor effect when fastening with the target member. Therefore, this method for manufacturing an aluminum member can manufacture an aluminum member that can stably maintain high friction between the aluminum member and the target member. In addition, an intermediate layer is formed on the surface of the aluminum member. The intermediate layer has both an amorphous substance containing aluminum atoms and oxygen atoms, or an amorphous substance and a layered double hydroxide containing aluminum atoms and oxygen atoms. Therefore, even if the unevenness of the contact layer of the aluminum member penetrates the resin film of the target member, the intermediate layer is interposed between the aluminum member to be fastened and the target member, so that corrosion of the aluminum member due to electrochemical action is suppressed. As a result, this method for manufacturing an aluminum member can manufacture an aluminum member that can stably maintain high corrosion resistance when fastening with the target member. In this manner, this method for manufacturing an aluminum component can produce an aluminum component that exhibits high friction properties and high corrosion resistance when fastened to an object component.

[0022] (Clause 10) In the manufacturing method of the aluminum member according to Clause 9, the forming step may include a surface hydroxylation step of reacting a surface of the aluminum member with saturated steam under a pressure higher than atmospheric pressure and lower than 4.30 MPa to modify the surface of the aluminum member into aluminum hydroxide and form the intermediate layer and the contact layer. In this case, the manufacturing method of the aluminum member has the same effects as the fastening method according to Clause 2.

[0023] (Clause 11) In the method for producing an aluminum member according to Clause 10, the surface hydroxylation step may involve reacting the surface of the aluminum member with saturated water vapor by applying heat of 100° C. or more and 250° C. or less. In this case, the method for producing an aluminum member has the same effects as the fastening method according to Clause 3.

[0024] (Clause 12) In the method for producing an aluminum member according to Clause 10 or 11, the surface hydroxylation step may involve reacting the surface of the aluminum member with saturated water vapor for a treatment time of 30 minutes to 48 hours. In this case, the method for producing an aluminum member has the same effects as the fastening method according to Clause 4.

[0025] (Clause 13) In the method for manufacturing an aluminum member according to any one of Clauses 9 to 12, at least one of the maximum height and the ten-point average roughness defined in JIS-B0601:1994 on the surface of the aluminum member on which the irregularities are formed in the forming step may be 0.5 μm or more. In this case, the method for manufacturing an aluminum member has the same effect as the fastening method according to Clause 5.

[0026] (Clause 14) In the method for manufacturing an aluminum member according to any one of Clauses 9 to 13, on the surface of the aluminum member on which the irregularities are formed in the forming step, the ratio of the maximum height defined in JIS-B0601:1994 to the ten-point average roughness defined in JIS-B0601:1994 may be 1.0 or more and 2.0 or less. In this case, the method for manufacturing an aluminum member has the same effect as the fastening method according to Clause 6.

[0027] (Clause 15) In the manufacturing method of an aluminum member according to any one of Clauses 9 to 13, a developed interface area ratio of a contour curved surface defined in JIS-B0681-2:2018 on the surface of the aluminum member on which the irregularities are formed in the forming step may be 10% or more. In this case, the manufacturing method of the aluminum member has the same effect as the fastening method according to Clause 7.

[0028] (Clause 16) An aluminum member according to another aspect of the present disclosure is an aluminum member to be fastened to a target member having a resin film on its surface. The aluminum member includes an intermediate layer formed on the surface, and a contact layer. The contact layer is disposed on the intermediate layer and has a first irregularity capable of contacting the target member. The intermediate layer includes an amorphous substance containing aluminum atoms and oxygen atoms, or both an amorphous substance and a layered double hydroxide containing aluminum atoms and oxygen atoms. The contact layer includes aluminum hydroxide. The first irregularity has a protruding length smaller than the thickness of the resin film of the target member.

[0029] This aluminum member is a member for fastening to a target member. Since the contact layer of the aluminum member has a first unevenness, it exerts an anchor effect in fastening to the target member. Therefore, high friction between the aluminum member and the target member is stably maintained. In addition, an intermediate layer is formed on the surface of the aluminum member. The intermediate layer has both an amorphous substance containing aluminum atoms and oxygen atoms, or an amorphous substance and a layered double hydroxide containing aluminum atoms and oxygen atoms. Therefore, even if the unevenness of the contact layer of the aluminum member penetrates the resin film of the target member, the intermediate layer is interposed between the aluminum member to be fastened and the target member, so that corrosion of the aluminum member due to electrochemical action is suppressed. As a result, this aluminum member can stably maintain high corrosion resistance when fastened to the target member. In this way, this aluminum member can exhibit high friction and high corrosion resistance when fastened to the target member.

[0030] (Clause 17) In the aluminum member according to Clause 16, at least one of the maximum height and the ten-point average roughness as defined in JIS-B0601:1994 on the surface of the aluminum member on which the first irregularities are formed may be 0.5 μm or more. In this case, the aluminum member has the same effect as the fastening method according to Clause 5.

[0031] (Clause 18) In the aluminum member according to Clause 16 or 17, the ratio of the maximum height, as defined in JIS-B0601:1994, to the ten-point average roughness, as defined in JIS-B0601:1994, on the surface of the aluminum member on which the first irregularities are formed may be 1.0 or more and 2.0 or less. In this case, the aluminum member has the same effect as the fastening method according to Clause 6.

[0032] (Clause 19) In the aluminum member according to any one of Clauses 16 to 18, on the surface of the aluminum member on which the first irregularities are formed, a developed interface area ratio of a contour curved surface defined in JIS-B0681-2:2018 may be 10% or more. In this case, the aluminum member has the same effect as the fastening method according to Clause 7.

[0033] (Clause 20) The aluminum member according to any one of clauses 16 to 19 may further include a second asperity of micro order formed on the surface of the aluminum member, and the first asperity may be formed on the surface of the second asperity. In this case, the second asperity contributes to an anchor effect. Even if the second asperity is an acute-angled protrusion, the surface of the aluminum member is covered with the intermediate layer and the contact layer by forming the first asperity on the surface of the second asperity. This makes the second asperity rounded. According to this aluminum member, the second asperity does not become an acute-angled protrusion that can become a starting point for breaking the resin film of the target member, so that high friction between the aluminum member and the target member can be stably maintained.

[0034] (Clause 21) The corrosion current density of the aluminum member according to any one of clauses 16 to 20 may be 1 / 130 or less of the corrosion current density of an aluminum material having neither an intermediate layer nor a contact layer. This aluminum member has higher corrosion resistance than the aluminum material having neither an intermediate layer nor a contact layer.

[0035] [Example of the first embodiment of the present disclosure] Hereinafter, a first embodiment of the present disclosure will be described with reference to the drawings. In the following description, the same or equivalent elements are given the same reference numerals, and overlapping descriptions will not be repeated. The dimensional ratios in the drawings do not necessarily match those in the description. Terms such as "upper", "lower", "left", and "right" are based on the illustrated state and are for convenience. The abrasive material in this embodiment is a member that is sprayed during blast processing, and is, for example, abrasive grains of ceramics (alumina, silicon carbide, etc.). Unless otherwise specified, the particle diameter of the abrasive material in this embodiment is expressed as the average particle diameter (D50).

[0036] [Aluminum parts] FIG. 1 is a perspective view showing a fastening unit including an aluminum member according to an embodiment. In the figure, the X and Y directions are horizontal directions, and the Z direction is vertical. The X, Y, and Z directions are mutually orthogonal axial directions in a Cartesian coordinate system in a three-dimensional space. Hereinafter, the direction along the XY plane is also referred to as the horizontal direction, and the Z direction is also referred to as the up-down direction. Hereinafter, the positive direction of the Z axis is also referred to as the up direction, and the negative direction of the Z axis is also referred to as the down direction. As shown in FIG. 1, the fastening unit 1 is a member in which a plurality of members are integrated by fastening. For example, the fastening unit 1 includes an aluminum member 2, a fastening member 3, and a target member 4. The aluminum member 2 of this embodiment is fastened to the target member 4 by the fastening member 3. That is, the aluminum member 2 is pressed downward toward the target member 4 by the fastening member 3, and comes into contact with the contact surface 4b of the target member 4.

[0037] The aluminum member 2 of this embodiment is, for example, an annular plate member extending in the horizontal direction. The aluminum member 2 is, for example, a washer. The aluminum member 2 is provided with, for example, an opening 2a penetrating in the vertical direction. The aluminum member 2 has a front surface 2b exposed downward and a back surface 2c exposed upward. The material of the aluminum member 2 is not limited, and may be, for example, A1100, A2024, A3003, A4032, A5052, A6061, A7075, ADC12, etc.

[0038] The fastening member 3 is inserted into the opening 2a of the aluminum member 2 and is screwed into the target member 4. The fastening member 3 is, for example, a male screw. The fastening member 3 has a head 3a and an insertion portion 3b. In the horizontal direction, the head 3a is larger than the opening diameter of the opening 2a and is thicker than the insertion portion 3b. The insertion portion 3b is provided on a surface 3c exposed downward from the head 3a. A part of the surface 3c of the head 3a where the insertion portion 3b is not provided contacts the back surface 2c of the aluminum member 2. In the horizontal direction, the insertion portion 3b is thinner than the opening diameter of the opening 2a. The insertion portion 3b extends in the vertical direction, and at least the lower end is threaded.

[0039] In this embodiment, the target member 4 is fastened to the aluminum member 2 by the fastening member 3. The target member 4 is screwed into the fastening member 3. The target member 4 is a member into which the fastening member 3 is inserted. The target member 4 has, for example, an opening 4a that is threaded so that it can be screwed into the insertion portion 3b of the fastening member 3.

[0040] A case where the aluminum member 2 and the fastening member 3 are fastened will be described. As an example, the aluminum member 2 is fastened to the target member 4 by the fastening member 3. The aluminum member 2 is placed on the contact surface 4b of the target member 4 so that the position of the opening 2a and the position of the opening 4a overlap. The aluminum member 2 is placed so that the front surface 2b of the aluminum member 2 contacts the contact surface 4b of the target member 4. The insertion portion 3b of the fastening member 3 is inserted into the aluminum member 2 and the target member 4 from above the aluminum member 2 and the target member 4. Specifically, the insertion portion 3b of the fastening member 3 is inserted into the opening 2a and screwed into the opening 4a. As the fastening member 3 screwed into the opening 4a of the target member 4, the front surface 3c of the fastening member 3 comes into contact with the back surface 2c of the aluminum member 2, and the head 3a of the fastening member 3 presses the aluminum member 2 toward the target member 4 (downward). As a result, the surface 2b of the aluminum member 2 comes into contact with and is pressed against the contact surface 4b of the target member 4. When the entire insertion portion 3b is inserted into the openings 2a and 4a, the surface 2b of the aluminum member 2 properly penetrates the contact surface 4b of the target member 4. In this manner, the aluminum member 2 is sandwiched between the head 3a of the fastening member 3 and the target member 4, and the aluminum member 2 is fastened to the target member 4 by the fastening member 3. Here, fastening includes a state in which certain members are rotated and twisted relative to one another to fix a member sandwiched between the two members to the certain member without loosening.

[0041] FIG. 2 is an enlarged view of the fastening unit within the dashed line indicated by II in FIG. 1. As shown in FIG. 2, the surface 2b of the aluminum member 2 is formed with a first unevenness 7a and a second unevenness 2d, which will be described later. Hereinafter, the surface 2b of the aluminum member 2 refers to the outermost surface layer of the aluminum member 2, regardless of whether the surface has been processed or modified. Note that the surface 2b of the aluminum member 2 is also referred to as the surface 2b of the second unevenness 2d when specifically describing the surface layer of the second unevenness 2d. The second unevenness 2d is a micro-order unevenness. The micro-order unevenness is an unevenness having a height difference of 1 μm or more and less than 1000 μm. The second unevenness 2d is formed with an inclined portion that is inclined from the convex portion to the concave portion of the second unevenness 2d. The inclined portion contributes to the fastening of the fastening member 3 to the target member 4, and serves as a stress concentration portion that contributes to shear strength and frictional force.

[0042] The aluminum member 2 includes a main body portion 5, an intermediate layer 6, and a contact layer 7. The contact layer 7 is located on the outermost side (the side facing the target member 4), and the main body portion 5 is located at a position farthest from the surface (the surface in contact with the target member 4). The intermediate layer 6 is provided between the main body portion 5 and the contact layer 7. The second irregularities 2d are formed on the surface of the main body portion 5. The main body portion 5 is mainly composed of aluminum atoms.

[0043] The intermediate layer 6 is formed on the surface 2b of the second irregularities 2d of the main body 5. The intermediate layer 6 has an amorphous substance containing aluminum atoms and oxygen atoms, or both an amorphous substance and a layered double hydroxide containing aluminum atoms and oxygen atoms. The amorphous substance here refers to a substance having an amorphous structure. The amorphous substance of the intermediate layer 6 refers to a substance in which the arrangement of solid substances containing aluminum atoms and oxygen atoms is irregular. The intermediate layer 6 may have a form having an amorphous substance without having a layered double hydroxide. The intermediate layer 6 may have a form having only an amorphous substance. The intermediate layer 6 is composed of, for example, dense alumina (Al2O3). The intermediate layer 6 is located on the upper layer of the second irregularities 2d (outside the main body 5), and has a thickness of, for example, several tens of nm to several μm.

[0044] The contact layer 7 includes aluminum hydroxide and is a layer capable of directly contacting the target member 4. The contact layer 7 is located on the upper layer of the intermediate layer 6 (outside the intermediate layer 6). The aluminum hydroxide is an aluminum compound having a hydroxyl group. The aluminum hydroxide includes at least one of diaspore, boehmite, pseudoboehmite, bayerite, norstlandite, gibbsite, and doillite. The aluminum hydroxide may include any one of diaspore, boehmite, pseudoboehmite, bayerite, norstlandite, gibbsite, and doillite. The aluminum hydroxide may include a plurality of types of aluminum hydroxide selected from diaspore, boehmite, pseudoboehmite, bayerite, norstlandite, gibbsite, and doillite.

[0045] The contact layer 7 has a first unevenness 7a that can come into contact with the target member 4. The contact layer 7 has, for example, a first unevenness 7a of at least one of micro-order and nano-order that can come into contact with the target member 4. Nano-order unevenness is unevenness having a height difference of 1 nm or more and less than 1000 nm. The contact layer 7 has, for example, a first unevenness 7a of 10 μm or less that can come into contact with the target member 4. At least one of the maximum height Ry and the ten-point average roughness Rz defined in JIS-B0601:1994 on the surface 2b of the aluminum member 2 on which the first unevenness 7a is formed is 0.5 μm or more. At least one of the maximum height Ry and the ten-point average roughness Rz defined in JIS-B0601:1994 may be less than the thickness of a resin film 8 of the target member 4, which will be described later. At least one of the maximum height Ry and the ten-point average roughness Rz defined in JIS-B0601:1994 may be, for example, less than 50 μm or 45 μm or less. The maximum height Ry defined in JIS B0601(1994) of the aluminum member 2 on which only the first asperities 7a are formed may be 0.5 μm or more. The ten-point average roughness Rz defined in JIS B0601(1994) of the aluminum member 2 on which the first asperities 7a and the second asperities 2d are formed may be 0.5 μm or more.

[0046] In the surface 2b of the aluminum member 2 on which the first irregularities 7a are formed, the ratio of the maximum height defined in JIS-B0601:1994 to the ten-point average roughness defined in JIS-B0601:1994 is 1.0 or more and 2.0 or less. In addition, in the surface 2b of the aluminum member 2 on which the first irregularities 7a are formed, the developed interface area ratio Sdr of the contour curved surface defined in JIS-B0681-2:2018 is 10% or more. Note that, in the surface 2b of the aluminum member 2 on which the first irregularities 7a are formed, the developed interface area ratio Sdr of the contour curved surface defined in JIS-B0681-2:2018 may be 20% or more.

[0047] The aluminum member 2 may have a precipitation layer formed between the main body portion 5 and the intermediate layer 6. The precipitation layer is a layer formed by precipitation of aluminum alloy elements such as silicon (Si) or magnesium (Mg) from the main body portion 5 of the aluminum member 2 by heat treatment. For example, the main body portion 5 located near the intermediate layer 6 may have the precipitation layer.

[0048] The target member 4 has a resin film 8 on its surface. For example, the resin film 8 is provided on a contact surface 4b that can come into contact with the contact layer 7 of the aluminum member 2. The target member 4 has a target main body portion 9 located inside the resin film 8 (at a lower position farther from the aluminum member 2). The resin film 8 is provided so as to cover the target main body portion 9 and is exposed toward the outside. The resin film 8 is an electrodeposition coating film or coating. The material of the resin film 8 is not limited, and may be, for example, epoxy, polyurethane, polyester, silicone, acrylic, fluororesin, polybutylene terephthalate, polyphenylene sulfide, polyamide, liquid crystal polymer, polypropylene, acrylonitrile butadiene styrene, or a combination thereof.

[0049] The resin film 8 has a thickness greater than, for example, at least one of the maximum height Ry and the ten-point mean roughness Rz on the surface 2b of the aluminum member 2 on which the first asperities 7a are formed. The resin film 8 has a thickness greater than, for example, at least one of the maximum height Ry and the ten-point mean roughness Rz on the surface 2b of the aluminum member 2 on which the first asperities 7a and the second asperities 2d of the aluminum member 2 are formed. The resin film 8 is, for example, 5 μm or more and 50 μm or less.

[0050] The material of the target body 9 of the target member 4 is not limited, and may be metal or resin. The target body 9 may be made of a material that has a potential difference with respect to the aluminum member 2, or may not be made of a material that does not have a potential difference. The material of the target body 9 is, for example, iron, aluminum, titanium, copper, resin (carbon fiber reinforced resin, etc.), ceramic, or a combination of these. There may be a potential difference between the aluminum member 2 and the target member 4 at least after fastening.

[0051] As described above, the aluminum member 2 according to the first embodiment is a member for fastening to a target member 4 having a resin film 8 on its surface. The aluminum member 2 includes a contact layer 7. The contact layer 7 has a first asperity 7a that can come into contact with the target member 4. The contact layer 7 has, for example, a first asperity 7a of at least one of a micro-order and a nano-order that can come into contact with the target member 4. The contact layer 7 includes aluminum hydroxide. When the aluminum member 2 and the target member 4 are fastened by the fastening member 3, the first asperity 7a of the aluminum member 2 penetrates the resin film 8 of the target member 4. The first asperity 7a increases the contact surface area between the aluminum member 2 and the resin film 8 compared to when there are no asperities on the surface. Therefore, the first asperity 7a that penetrates the resin film 8 of the target member 4 exerts an anchor effect in fastening to the target member 4. Therefore, high friction between the aluminum member 2 and the target member 4 can be stably maintained.

[0052] The aluminum member 2 also includes an intermediate layer 6. The intermediate layer 6 includes both an amorphous substance containing aluminum atoms and oxygen atoms, or an amorphous substance and a layered double hydroxide containing aluminum atoms and oxygen atoms. Here, when at least the main body 5 of the aluminum member 2 and the target member 4 are in direct contact with each other, corrosion of the aluminum member 2 may occur due to electrochemical action. For example, when the material of the aluminum member 2 and the material of the target member 4 are different types of metal, bimetallic corrosion (galvanic corrosion) defined in JIS-Z0103 may occur between the aluminum member 2 and the target member 4. In addition, when the aluminum member 2 and the target member 4 include the same material or the target member 4 includes a conductive material, stray current corrosion (electrolytic corrosion) defined in JIS-Z0103 may occur between the aluminum member 2 and the target member 4. In this embodiment, even if the first irregularities 7a of the contact layer 7 of the aluminum member 2 pierce the resin film 8 of the target member 4, the intermediate layer 6 is interposed between the fastened aluminum member 2 and the target member 4. The intermediate layer 6 has insulating properties, and therefore prevents contact between the main body 5 of the aluminum member 2 and the resin film 8 and the target main body 9 of the target member 4. Even if the target member 4 has a conductive material or a dielectric, contact between the target member 4 and the main body 5 of the aluminum member 2 is prevented, and therefore corrosion of the aluminum member 2 due to electrochemical action is prevented. Therefore, the aluminum member 2 can stably maintain high corrosion resistance when fastened to the target member 4. In this way, the aluminum member 2 can exhibit high friction properties and high corrosion resistance when fastened to the target member 4.

[0053] In addition, in the aluminum member 2, at least one of the maximum height Ry and ten-point mean roughness Rz defined in JIS-B0601:1994 is 0.5 μm or more on the surface 2b of the aluminum member 2 on which the first asperities 7a (and the second asperities 2d) are formed. Since asperities having a maximum height Ry and ten-point mean roughness Rz of 0.5 μm or more are formed on the surface of the aluminum member, asperities that greatly contribute to frictional properties are formed.

[0054] Furthermore, in the surface 2b of the aluminum member 2 on which the first asperities 7a (and the second asperities 2d) are formed, the ratio of the maximum height Ry defined in JIS-B0601:1994 to the ten-point average roughness Rz defined in JIS-B0601:1994 is 1.0 or more and 2.0 or less. In this case, the aluminum member 2 has asperities that can exhibit high friction properties and high corrosion resistance.

[0055] In addition, in the surface 2b of the aluminum member 2 on which the first irregularities 7a (and the second irregularities 2d) are formed, the developed interface area ratio Sdr of the contour curved surface defined in JIS-B0681-2:2018 is 10% or more. In this case, an appropriate number of first irregularities 7a are formed on the surface 2b of the aluminum member 2. Therefore, high friction can be exhibited when fastening the aluminum member 2 to the target member 4. In addition, in the surface 2b of the aluminum member 2 on which the first irregularities 7a (and the second irregularities 2d) are formed, the developed interface area ratio Sdr of the contour curved surface defined in JIS-B0681-2:2018 may be 20% or more. In this case, more first irregularities 7a are formed on the surface 2b of the aluminum member 2. Therefore, even higher friction can be exhibited when fastening the aluminum member 2 to the target member 4. The developed interface area ratio Sdr of the contour curved surface is 0 for a completely flat surface, and increases as the surface shape becomes denser and the undulations become larger. For this reason, the larger the developed interface area ratio Sdr of the contour curved surface defined in JIS-B0681-2:2018 on the surface 2b of the aluminum member 2 on which the first irregularities 7a (and the second irregularities 2d) are formed, the more first irregularities 7a are formed, thereby enabling even higher frictional properties to be exhibited when fastening the aluminum member 2 to the target member 4.

[0056] The aluminum member 2 further includes a second asperity 2d of the micro order formed on the surface 2b of the aluminum member 2. The first asperity 7a is formed on the surface 2b of the second asperity 2d. In this case, the second asperity 2d contributes to an anchor effect. Even if the second asperity 2d is an acute-angled protrusion, the surface 2b of the aluminum member 2 is covered with the intermediate layer 6 and the contact layer 7 by forming the first asperity 7a on the surface 2b of the second asperity 2d. As a result, the second asperity 2d is rounded. According to this aluminum member 2, the second asperity 2d cannot be an acute-angled protrusion that can become a starting point for breaking the resin film 8 of the target member 4, so that high friction between the aluminum member 2 and the target member 4 can be stably maintained.

[0057] Moreover, the corrosion current density of the aluminum member 2 is 1 / 130 or less of the corrosion current density of an aluminum material not having the intermediate layer 6 and the contact layer 7. This aluminum member 2 has higher corrosion resistance than an aluminum material not having the intermediate layer 6 and the contact layer 7. Moreover, the corrosion current density of the aluminum member 2 may be 1 / 140 or less of the corrosion current density of an aluminum material not having the intermediate layer 6 and the contact layer 7. In this case, the aluminum member 2 has higher corrosion resistance than an aluminum material not having the intermediate layer 6 and the contact layer 7, and an aluminum member in which the intermediate layer 6 and the contact layer 7 are not sufficiently formed. The corrosion current density of the aluminum member 2 may be 1 / 160 or less, or 1 / 180 or less of the corrosion current density of an aluminum material not having the intermediate layer 6 and the contact layer 7. In this case, since the aluminum member 2 has the intermediate layer 6 and the contact layer 7 formed with sufficient thickness, the aluminum member 2 has higher corrosion resistance than an aluminum material not having the intermediate layer 6 and the contact layer 7, and an aluminum member in which the intermediate layer 6 and the contact layer 7 are not sufficiently formed.

[0058] [Fastening method and manufacturing method for aluminum members] An outline of an apparatus used in the manufacturing method of the aluminum member 2 will be described. First, an apparatus for performing blast processing on the surface 2b of the aluminum member 2 will be described. The blast processing apparatus may be any type, such as a gravity type (suction type) air blasting apparatus, a direct pressure type (pressurized type) air blasting apparatus, or a centrifugal type blasting apparatus. The manufacturing method according to this embodiment uses, as an example, a so-called direct pressure type (pressurized type) air blasting apparatus. FIG. 3 is a conceptual diagram of a blast processing apparatus used in the manufacturing method of the aluminum member. The blast processing apparatus 10 includes a processing chamber 11, an injection nozzle 12, a storage tank 13, a pressurized chamber 14, a compressed gas supplier 15, and a dust collector (not shown).

[0059] A spray nozzle 12 is housed inside the treatment chamber 11, and blast processing is performed on a workpiece (here, an aluminum member 2) in the treatment chamber 11. The abrasives sprayed by the spray nozzle 12 fall to the bottom of the treatment chamber 11 together with dust. The fallen abrasives are supplied to a storage tank 13, and the dust is supplied to a dust collector. The abrasives stored in the storage tank 13 are supplied to a pressurizing chamber 14, and the pressurizing chamber 14 is pressurized by a compressed gas supply machine 15. The abrasives stored in the pressurizing chamber 14 are supplied to the spray nozzle 12 together with the compressed gas. In this manner, the workpiece is blast processed while the abrasives are circulated.

[0060] Fig. 4 is a diagram illustrating the configuration of a blast processing device used in the manufacturing method of an aluminum member according to the embodiment. The blast processing device 10 shown in Fig. 4 is the direct pressure type blasting device shown in Fig. 3. In Fig. 4, the wall surface of the treatment chamber 11 is partially omitted.

[0061] As shown in Figure 4, the blast processing device 10 includes a storage tank 13 for abrasives and a pressurized chamber 14 formed into an airtight structure to which a compressed gas supplier 15 is connected, a constant-volume supply section 16 connected to the storage tank 13 within the pressurized chamber 14, a spray nozzle 12 connected to the constant-volume supply section 16 via a connecting pipe 17, a processing table 18 that moves while holding a workpiece below the spray nozzle 12, and a control section 19.

[0062] The control unit 19 controls the components of the blast processing device 10. The control unit 19 includes a display unit and a processing unit, for example. The processing unit is a general computer having a CPU, a storage unit, and the like. The control unit 19 controls the supply amount of the compressed gas supplying device 15 that supplies compressed gas to the storage tank 13 and the pressurizing chamber 14 based on the set injection pressure and injection speed. The control unit 19 also controls the injection position of the injection nozzle 12 based on the set distance between the workpiece and the nozzle, and the scanning conditions of the workpiece (speed, feed pitch, number of scans, etc.). As a specific example, the control unit 19 controls the position of the injection nozzle 12 using the scanning speed (X direction) and feed pitch (Y direction) set before the blast processing. The control unit 19 controls the position of the injection nozzle 12 by moving the processing table 18 that holds the workpiece.

[0063] FIG. 5 is a cross-sectional view of the injection nozzle of FIG. 4. The injection nozzle 12 has an injection tube holder 120 which is a main body. The injection tube holder 120 is a cylindrical member having a space therein through which the injection material and compressed gas pass. One end of the injection tube holder 120 is an injection material inlet 123, and the other end is an injection material outlet 122. An inner wall surface tapered from the injection material inlet 123 side toward the injection material outlet 122 is formed inside the injection tube holder 120, and a cone-shaped convergence acceleration section 121 having an inclination angle is formed. A cylindrical injection tube 124 is provided in communication with the injection tube holder 120 on the injection material outlet 122 side. The convergence acceleration section 121 tapers from the middle of the cylindrical section of the injection tube holder 120 toward the injection tube 124. This forms a compressed gas flow 115.

[0064] The connecting pipe 17 of the blast processing device 10 is connected to the abrasives inlet 123 of the injection nozzle 12. As a result, the storage tank 13, the constant quantity supply unit 16 in the pressurized chamber 14, the connecting pipe 17, and the injection nozzle 12 are sequentially connected to form an abrasives path.

[0065] In the blast processing device 10 configured in this manner, compressed gas is supplied from the compressed gas supply machine 15 to the storage tank 13 and the pressurized chamber 14 at an amount controlled by the control unit 19. Then, the abrasives in the storage tank 13 are metered in the constant pressure flow force by the constant supply unit 16 in the pressurized chamber 14, supplied to the injection nozzle 12 via the connecting pipe 17, and injected from the injection pipe 124 of the injection nozzle 12 onto the processing surface of the workpiece. In this way, a constant amount of abrasives is always injected onto the processing surface of the workpiece. Then, the injection position of the injection nozzle 12 on the processing surface of the workpiece is controlled by the control unit 19, and the workpiece is blasted.

[0066] The sprayed abrasives and cutting powder generated during the blasting process are sucked up by a dust collector (not shown). A classifier (not shown) is arranged on the path from the processing chamber 11 to the dust collector, and separates the abrasives into reusable abrasives and other fine powder (abrasives that have become too large to be reused and cutting powder generated during the blasting process). The reusable abrasives are stored in a storage tank 13 and are supplied to the spray nozzle 12 again. The fine powder is collected by the dust collector.

[0067] Next, a series of flows of the fastening method of the fastening unit 1 and the manufacturing method of the aluminum member 2 will be described. FIG. 6 is a flowchart of the fastening method MT including the manufacturing method of the aluminum member according to the embodiment. As shown in FIG. 6, first, as a preparation step (S10), a target member 4 having a resin film 8 on its surface and an aluminum member 2 are prepared. The preparation step (S10) may include at least a determination step of determining the target member 4. By determining in advance the target member 4 to be used in the fastening step (S14) described later, it is possible to determine the processing content for the aluminum member 2 according to the target member 4. In the determination step, for example, a target member 4 on which a resin film 8 of 5 μm or more and 50 μm or less is formed on a contact surface 4b is determined as the target member 4 to be used in the fastening step (S14) described later.

[0068] In addition, as a preparation step (S10), a predetermined abrasive is filled into the blasting device 10. The particle diameter of the abrasive is, for example, 30 μm or more and 1000 μm or less. The smaller the particle diameter of the abrasive, the smaller the mass, and therefore the lower the inertial force. For this reason, when the particle diameter of the abrasive is smaller than 30 μm, it is difficult to form the second irregularities 2d of a desired shape. Also, when the particle diameter of the abrasive is smaller than 30 μm, the fluidity of the abrasive is poor, and the spraying in the blasting device 10 may become unstable. When the abrasive having a particle diameter exceeding 1000 μm is sprayed onto the aluminum member, the maximum height Ry and the ten-point average roughness Rz of the aluminum member may exceed the thickness of the resin film of the target member. Also, when the abrasive having a particle diameter exceeding 1000 μm is sprayed toward the aluminum member, the number of the abrasives that are lost increases, and the particle size distribution of the abrasives that hit the surface of the aluminum member changes significantly in a short time. In this case, it becomes impossible to perform a uniform treatment on the surface of the aluminum member. Therefore, the particle diameter of the abrasive material that can stably form the second irregularities 2d is 30 μm or more and 1000 μm or less. The particle diameter of the abrasive material may be, for example, 30 μm or more and 710 μm or less. The material of the abrasive material is, for example, alumina. The abrasive material has, for example, acute-angled protrusions.

[0069] The control unit 19 of the blast processing device 10 acquires blast processing conditions as a preparation step (S10). The control unit 19 acquires the blast processing conditions based on the operation of the operator or information stored in the memory unit. The blast processing conditions include the injection pressure, injection speed, nozzle distance, and workpiece scanning conditions (speed, feed pitch, number of scans). The injection pressure is, for example, 0.3 MPa or more and 2.0 MPa or less. The smaller the injection pressure, the lower the inertial force. Therefore, when the injection pressure is less than 0.3 MPa, it is difficult to form the second irregularities 2d of the desired shape. The higher the injection pressure, the higher the inertial force. Therefore, the abrasives are more likely to be crushed by collision with the aluminum member 2. As a result, problems such as (1) poor processing efficiency because the collision energy is dispersed to places other than the formation of the second irregularities 2d, and (2) the abrasives are worn out significantly, making it uneconomical, etc. occur. Such problems become more pronounced when the injection pressure exceeds 2.0 MPa. The control unit 19 manages the blasting conditions to precisely control the size and number of the second irregularities 2d on the surface 2b of the aluminum member 2 on the order of microns. The blasting conditions may include conditions for specifying the region to be blasted. In this case, selective surface treatment is possible.

[0070] Next, in a forming step (S12), a second unevenness 2d is formed on the surface 2b of the aluminum member 2. The forming step (S12) includes, for example, a blasting step. The blasting device 10 performs the following series of processes as the blasting step. First, the aluminum member 2 to be blasted is set on the processing table 18 in the processing chamber 11. Next, the control unit 19 operates a dust collector (not shown). The dust collector reduces the pressure inside the processing chamber 11 to a negative pressure state based on a control signal from the control unit 19. Next, the injection nozzle 12 injects the abrasive material as a two-phase solid-gas flow of compressed air at an injection pressure in the range of 0.3 MPa to 2.0 MPa based on a control signal from the control unit 19. Next, the control unit 19 operates the processing table 18 to move the aluminum member 2 into the injection flow of the two-phase solid-gas flow (below the injection nozzle in FIG. 5). Here, the control unit 19 continues the operation of the processing table 18, and operates it so that the jet of water flows along a preset trajectory relative to the aluminum member 2.

[0071] By performing blasting processing at a range of 0.3 MPa to 2.0 MPa using abrasives having a particle diameter of 30 μm to 1000 μm, the second irregularities 2d of the desired micro order are formed on the surface 2b of the aluminum member 2. The arithmetic mean roughness Ra of the second irregularities 2d as specified in JIS B0601 (1994) may be 0.7 μm to 5.0 μm as a result of the blasting processing. The arithmetic mean slope RΔa of the second irregularities 2d as specified in JIS B0601 (1994) may be 0.17 to 0.50 as a result of the blasting processing. The root mean square slope RΔq of the second irregularities 2d as specified in JIS B0601 (1994) may be 0.27 to 0.60 as a result of the blasting processing. After the operation of the blasting processing device 10 is stopped, the aluminum member 2 is taken out and the blasting processing is completed. By carrying out the above blasting process, the second asperities 2d on the micro-order are formed. Note that by carrying out the blasting process, scratches on the surface 2b of the aluminum member 2 and deposits and the like attached to the surface 2b of the aluminum member 2 are appropriately scraped off.

[0072] Subsequently, in the formation step (S12), the intermediate layer 6 and the contact layer 7 are formed on the surface 2b of the aluminum member 2 on which the second irregularities 2d are formed. The formation step (S12) includes, for example, a surface hydroxylation step. In the surface hydroxylation step, the surface 2b of the aluminum member 2 is reacted with water vapor to modify the surface 2b of the aluminum member 2 into aluminum hydroxide, thereby forming the intermediate layer 6 and the contact layer 7. In the surface hydroxylation step, the surface 2b of the aluminum member 2 on which the second irregularities 2d are formed is reacted with water vapor under a pressure that is higher than atmospheric pressure and is 4.30 MPa or less. In the surface hydroxylation step, the surface 2b of the aluminum member 2 on which the second irregularities 2d are formed is reacted with water vapor under a pressure that is higher than atmospheric pressure and is 4.30 MPa or less. The above-mentioned 4.30 MPa is a value obtained by rounding off the fourth significant digit of the saturated water vapor pressure at 250°C. Alternatively, in the surface hydroxylation step, the surface 2b of the aluminum member 2 on which the second irregularities 2d are formed may be reacted with water vapor by applying heat of 100° C. or more and 250° C. or less. This temperature is the temperature of the space (atmosphere) within the device in which the surface 2b of the aluminum member 2 is reacted with the water vapor. In this case, in the surface hydroxylation step, the surface 2b of the aluminum member 2 is reacted with the water vapor for a treatment time of 30 minutes or more and 48 hours or less.

[0073] As a result, an intermediate layer 6 is formed on the surface 2b of the second irregularities 2d, and a contact layer 7 having a first irregularity 7a is formed on the intermediate layer 6. The intermediate layer 6 has an amorphous substance containing aluminum atoms and oxygen atoms, or both an amorphous substance and a layered double hydroxide containing aluminum atoms and oxygen atoms. The amorphous substance here refers to a substance that contains aluminum atoms and oxygen atoms and has an amorphous structure. The intermediate layer 6 may have an amorphous substance without a layered double hydroxide. The intermediate layer 6 is composed of, for example, dense alumina (Al2O3). The intermediate layer 6 is located on the upper layer of the second irregularities 2d (outside the main body portion 5), and has a thickness of, for example, several tens of nm to several μm.

[0074] The contact layer 7 includes an aluminum hydroxide. The contact layer 7 is located on the upper layer of the intermediate layer 6. The aluminum hydroxide is a compound of aluminum having a hydroxyl group. The aluminum hydroxide includes at least one of diaspore, boehmite, pseudoboehmite, bayerite, nostrandite, gibbsite, and doillite. The aluminum hydroxide may include any one of diaspore, boehmite, pseudoboehmite, bayerite, nostrandite, gibbsite, and doillite. The aluminum hydroxide may include a plurality of types of aluminum hydroxide selected from diaspore, boehmite, pseudoboehmite, bayerite, nostrandite, gibbsite, and doillite. By forming the contact layer 7, the contact layer 7 is formed on the sharp portions (acute protrusions) of the second irregularities 2d formed by the blasting process, via the intermediate layer 6, and is modified to aluminum hydroxide, which has the additional effect of making it less likely that the resin film 8 of the target member 4 described below, which penetrates into the second irregularities 2d, will break starting from the sharp portions.

[0075] The contact layer 7 has a first unevenness 7a that can come into contact with the target member 4. The contact layer 7 has, for example, the first unevenness 7a of at least one of the micro-order and nano-order that can come into contact with the target member 4. The first unevenness 7a has a protruding length smaller than the thickness of the resin film 8 of the target member 4. The protruding length of the first unevenness 7a is, for example, less than 50 μm. On the surface 2b of the aluminum member 2 on which the first unevenness 7a is formed, at least one of the maximum height Ry and the ten-point average roughness Rz defined in JIS-B0601:1994 is 0.5 μm or more. At least one of the maximum height Ry and the ten-point average roughness Rz defined in JIS-B0601:1994 may be less than the thickness of the resin film 8 of the target member 4. That is, the protruding length of the first unevenness 7a may be expressed by at least one of the maximum height Ry and the ten-point average roughness Rz defined in JIS-B0601:1994. At least one of the maximum height Ry and ten-point mean roughness Rz defined in JIS-B0601:1994 may be, for example, less than 50 μm. The above-mentioned values ​​are, for example, the maximum height Ry and ten-point mean roughness Rz on the surface 2b of the aluminum member 2 on which the first asperities 7a and the second asperities 2d are formed. The above-mentioned values ​​may also be, for example, the maximum height Ry and ten-point mean roughness Rz on the surface 2b of the aluminum member 2 on which only the first asperities 7a are formed.

[0076] On the surface 2b of the aluminum member 2 on which the first irregularities 7a are formed, the ratio of the maximum height defined in JIS-B0601:1994 to the ten-point average roughness defined in JIS-B0601:1994 is 1.0 or more and 2.0 or less.

[0077] In the surface hydroxylation step of the formation step (S12), acute-angled crystals of aluminum hydroxide of nano-order are formed on the surface 2b of the aluminum member 2 for a predetermined period of time after the start of the step. Thereafter, the reaction between the aluminum member 2 and water vapor in the surface hydroxylation step continues, thereby forming first irregularities 7a of at least one of micro-order and nano-order. As the first irregularities 7a, for example, irregularities in which micro-order irregularities and nano-order irregularities are mixed are formed on the surface 2b of the aluminum member 2. Note that when the blast processing step of the formation step (S12) is performed and second irregularities 2d are formed on the surface 2b of the aluminum member 2, the first irregularities 7a have the effect of rounding the second irregularities 2d.

[0078] Next, in the fastening step (S14), the aluminum member 2 and the target member 4 are fastened together while the first unevenness 7a and the second unevenness 2d of the aluminum member 2 are pierced into the resin film 8 of the target member 4. For example, the worker places the aluminum member 2 on the contact surface 4b of the target member 4 so that the position of the opening 2a and the position of the opening 4a overlap. The aluminum member 2 is placed so that the surface 2b of the aluminum member 2 contacts the contact surface 4b of the target member 4. The aluminum member 2 is inserted into the aluminum member 2 and the target member 4 from above. Specifically, the worker inserts the insertion portion 3b of the fastening member 3 into the opening 2a and screws it into the opening 4a of the target member 4. As the fastening member 3 is screwed into the opening 4a of the target member 4, the surface 3c of the head 3a of the fastening member 3 can be brought into contact with the back surface 2c of the aluminum member 2, and the aluminum member 2 can be pressed toward the target member 4 (downward). As a result, the surface 2b of the aluminum member 2 sandwiched between the head 3a of the fastening member 3 and the target member 4 is pierced into the resin film 8 provided on the contact surface 4b of the target member 4. When the entire insertion portion 3b is inserted into the opening 2a and the opening 4a, the surface 2b of the aluminum member 2 is properly pierced into the contact surface 4b of the target member 4. In this manner, the aluminum member 2 is sandwiched between the head 3a of the fastening member 3 and the target member 4, and the aluminum member 2 is fastened to the target member 4 by the fastening member 3. Note that in the fastening step (S14), the aluminum member 2 and the target member 4 may be fastened automatically by a fastening device (not shown) or the like, instead of by an operator as described above. When the fastening step (S14) is completed, the flowchart shown in FIG. 6 is completed.

[0079] As described above, according to the fastening method MT and the aluminum manufacturing method, the second asperities 2d are formed on the surface 2b of the aluminum member 2 after the forming step (S12), and the first asperities 7a are formed in the contact layer 7. Since the contact layer 7 contains aluminum hydroxide, the surface of the second asperities 2d of the aluminum member 2 is rounded by the first asperities 7a. Then, the first asperities 7a and the second asperities 2d of the aluminum member 2 penetrate the resin film 8 of the target member 4 by the fastening step (S14). The first asperities 7a and the second asperities 2d that penetrate the resin film 8 of the target member 4 have an anchor effect in fastening to the target member 4. Therefore, high friction between the aluminum member 2 and the target member 4 can be stably maintained.

[0080] In addition, an intermediate layer 6 is formed on the surface of the aluminum member 2. The intermediate layer 6 has both an amorphous substance containing aluminum atoms and oxygen atoms, or an amorphous substance and a layered double hydroxide containing aluminum atoms and oxygen atoms. Here, when at least the main body 5 of the aluminum member 2 and the target member 4 are in direct contact with each other, corrosion of the aluminum member 2 may occur due to electrochemical action. For example, when the material of the aluminum member 2 and the material of the target member 4 are different types of metal, bimetallic corrosion (galvanic corrosion) defined in JIS-Z0103 may occur between the aluminum member 2 and the target member 4. In addition, for example, when the aluminum member 2 and the target member 4 contain the same material or when the target member 4 contains a conductive substance, stray current corrosion (electrolytic corrosion) defined in JIS-Z0103 may occur between the aluminum member 2 and the target member 4. In this embodiment, even if the first unevenness 7a of the contact layer 7 of the aluminum member 2 penetrates the resin film 8 of the target member 4, the intermediate layer 6 is interposed between the fastened aluminum member 2 and the target member 4. Since the intermediate layer 6 has insulating properties, contact between the main body 5 of the aluminum member 2 and the resin film 8 and the target main body 9 of the target member 4 is suppressed. Even if the target member 4 has a conductive material or a dielectric, contact between the target member 4 and the main body 5 of the aluminum member 2 is suppressed, so corrosion of the aluminum member 2 due to electrochemical action is suppressed. Therefore, the aluminum member 2 can stably maintain high corrosion resistance when fastened to the target member 4. In this way, high friction and high corrosion resistance are exhibited in this fastening method MT. In addition, this manufacturing method for an aluminum member can manufacture an aluminum member 2 that can exhibit high friction and high corrosion resistance when fastened to the target member 4.

[0081] Moreover, according to the fastening method MT and the manufacturing method for the aluminum member 2, the forming step (S12) includes a surface hydroxylation step of reacting the surface 2b of the aluminum member 2 with saturated water vapor under a pressure that is higher than atmospheric pressure and is equal to or lower than approximately 4.30 MPa, thereby modifying the surface 2b of the aluminum member 2 to aluminum hydroxide, and forming the intermediate layer 6 and the contact layer 7. In this case, since the aluminum member 2 reacts with the water vapor under the above-mentioned pressure, the fastening method MT and the manufacturing method for the aluminum member 2 can form the intermediate layer 6 and the contact layer 7 having the first unevenness 7a on the surface of the aluminum member 2.

[0082] Moreover, according to the fastening method MT and the manufacturing method of the aluminum member 2, the surface hydroxylation step involves reacting the surface 2b of the aluminum member 2 with saturated water vapor by applying heat of 100°C or more and 250°C or less. In this case, the fastening method MT and the manufacturing method of the aluminum member 2 can easily modify the surface 2b of the aluminum member 2 to aluminum hydroxide by reacting the aluminum member with saturated water vapor by applying heat of more than 100°C. Furthermore, the fastening method MT and the manufacturing method of the aluminum member 2 can form the first asperities 7a having appropriate rigidity by reacting the aluminum member 2 with saturated water vapor by applying heat of 100°C or more and 250°C or less. In the fastening method MT and the manufacturing method of the aluminum member 2, the heat for reacting the aluminum member with saturated water vapor is preferably higher than 100°C as long as it is 250°C or less. In the fastening method MT and the manufacturing method for the aluminum member 2, by reacting the aluminum member 2 with saturated water steam by applying heat of 120°C or more and 250°C or less, sufficient water steam pressure and heat are applied to the aluminum member, forming a contact layer and intermediate layer of an appropriate thickness, and an aluminum member that can exhibit higher friction properties and higher corrosion resistance can be manufactured.In the fastening method MT and the manufacturing method for the aluminum member 2, by reacting the aluminum member 2 with saturated water steam by applying heat of 180°C or more and 250°C or less, even higher water steam pressure and heat are applied to the aluminum member, forming a contact layer and intermediate layer of a more appropriate thickness, and an aluminum member that can exhibit even higher friction properties and higher corrosion resistance can be manufactured.

[0083] Moreover, according to the fastening method MT and the manufacturing method of the aluminum member 2, the surface hydroxylation step involves reacting the surface of the aluminum member with saturated water vapor for a treatment time of 30 minutes or more and 48 hours or less. In this case, the fastening method MT and the manufacturing method of the aluminum member 2 can form an aluminum hydroxide layer of an appropriate thickness on the surface 2b of the aluminum member 2, and can manufacture an aluminum member with good corrosion resistance. In the fastening method MT and the manufacturing method of the aluminum member 2, the time for reacting the aluminum member with saturated water vapor is preferably longer than 30 minutes, as long as it is 48 hours or less. In the fastening method MT and the manufacturing method of the aluminum member 2, the aluminum member 2 is reacted with saturated water vapor for a treatment time of 2 hours or more and 48 hours or less, so that sufficient pressure and heat of the water vapor are applied to the aluminum member, and contact layers and intermediate layers of appropriate thicknesses are formed, and an aluminum member that can exhibit higher friction and corrosion resistance can be manufactured. This fastening method MT and manufacturing method for the aluminum member 2 involves reacting the aluminum member 2 with saturated water vapor for a treatment time of 4 hours, 8 hours, 16 hours or 24 hours or more and not exceeding 48 hours, so that the pressure and heat of the water vapor are applied to the aluminum member for a longer period of time, forming a contact layer and intermediate layer of a more appropriate thickness, and an aluminum member can be manufactured that can further exhibit high friction properties and high corrosion resistance.

[0084] Furthermore, according to the fastening method MT and the manufacturing method for the aluminum member 2, on the surface 2b of the aluminum member 2 on which the first asperities 7a (and the second asperities 2d) are formed in the forming step (S12), at least one of the maximum height and ten-point mean roughness defined in JIS-B0601:1994 is 0.5 μm or more. In this case, in this fastening method MT and the manufacturing method for the aluminum member 2, the first asperities 7a (and the second asperities 2d) having a maximum height and ten-point mean roughness of 0.5 μm or more are formed on the surface 2b of the aluminum member 2, and therefore asperities that greatly contribute to frictional properties are formed.

[0085] Furthermore, according to the fastening method MT and the manufacturing method for the aluminum member 2, on the surface of the aluminum member on which the first asperities 7a (and the second asperities 2d) are formed in the forming step (S12), the ratio of the maximum height defined in JIS-B0601:1994 to the ten-point average roughness defined in JIS-B0601:1994 is 1.0 or more and 2.0 or less. In this case, the fastening method MT and the manufacturing method for the aluminum member 2 can form the first asperities 7a (and the second asperities 2d) that can exhibit high friction properties and high corrosion resistance.

[0086] Moreover, according to the fastening method MT and the manufacturing method of the aluminum member 2, the surface 2b of the aluminum member 2 on which the first irregularities 7a (and the second irregularities 2d) are formed in the forming step (S12) has a developed interface area ratio Sdr of the contour curved surface defined in JIS-B0681-2:2018 of 10% or more. In this case, an appropriate number of first irregularities 7a are formed on the surface 2b of the aluminum member 2. Therefore, high friction can be exhibited when fastening the aluminum member 2 and the target member 4. Moreover, according to the fastening method MT and the manufacturing method of the aluminum member 2, the surface 2b of the aluminum member 2 on which the first irregularities 7a (and the second irregularities 2d) are formed in the forming step (S12) has a developed interface area ratio Sdr of the contour curved surface defined in JIS-B0681-2:2018 of 20% or more. In this case, more first irregularities 7a are formed on the surface 2b of the aluminum member 2. Therefore, even higher friction can be exhibited when fastening the aluminum member 2 and the target member 4.

[0087] According to the fastening method MT, the thickness of the resin film 8 of the target member 4 is 5 μm or more and 50 μm or less. In this case, in the fastening method MT, since the thickness of the resin film 8 is 5 μm or more, the first asperities 7a and the second asperities 2d of the contact layer 7 of the aluminum member 2 can be appropriately inserted into the resin film 8 of the target member 4. Also, in the fastening method MT, since the thickness of the resin film 8 is 50 μm or less, the degree to which the resin film 8 deforms relative to the aluminum member 2 when friction occurs between the aluminum member 2 and the target member 4 is reduced, and breakage can be suppressed. As a result, the fastening method MT can appropriately exert a high frictional force between the aluminum member 2 and the target member 4. Also, since the second asperities 2d are formed before the first asperities 7a are formed in the forming step (S12), the surface 2b of the aluminum member 2 can be made to have an appropriate roughness corresponding to the thickness of the resin film 8.

[0088] Furthermore, according to the fastening method MT and the manufacturing method of the aluminum member 2, an aluminum member 2 can be manufactured in which the maximum height and ten-point average roughness of the surface 2b of the aluminum member 2 as specified in JIS-B0601:1994 are 0.5 μm or more, and are small relative to the thickness of the resin film 8, and the developed interface area ratio Sdr of the contour curved surface of the surface 2b of the aluminum member 2 as specified in JIS-B0681-2:2018 is 10% or more. This aluminum member 2 can stably exhibit high frictional properties. An aluminum member 2 can be manufactured in which the maximum height and ten-point average roughness of the surface 2b of the aluminum member 2 as specified in JIS-B0601:1994 are 0.5 μm or more, and are small relative to the thickness of the resin film 8, and the developed interface area ratio Sdr of the contour curved surface of the surface 2b of the aluminum member 2 as specified in JIS-B0681-2:2018 is 20% or more. This aluminum member 2 can stably exhibit even higher frictional properties.

[0089] Furthermore, according to the fastening method MT and the manufacturing method for the aluminum member 2, by performing the blasting process in the forming step (S12), scratches on the surface 2b of the aluminum member 2 and deposits attached to the surface 2b of the aluminum member 2 are appropriately scraped off, and uniform second irregularities 2d are formed. Therefore, the variation in the frictional force exerted is reduced when the aluminum member 2 subjected to the blasting process and surface hydroxylation process is fastened to the target member 4. The fastening unit 1 can stably exert high frictional properties.

[0090] [Second embodiment] Next, an aluminum member, a manufacturing method for the aluminum member, and a fastening method according to a second embodiment will be described with reference to Fig. 8. The fastening unit 1A according to the second embodiment has a different number of fastening members 3 and target members 4 from the fastening unit 1 according to the first embodiment. In the following description, descriptions that overlap with the first embodiment will be omitted as appropriate.

[0091] FIG. 7 is a top view showing a fastening unit including an aluminum member according to an embodiment. FIG. 8 is a cross-sectional view showing a fastening unit including an aluminum member according to an embodiment. In the example shown in FIG. 7 and FIG. 8, the fastening unit 1 is a member in which a plurality of members are integrated by fastening. For example, the fastening unit 1 includes an aluminum member 2, a pair of fastening members 3A, and a pair of target members 4A. The aluminum member 2 of the second embodiment is fastened to the pair of target members 4A by the pair of fastening members 3A. That is, the aluminum member 2 is sandwiched between the pair of target members 4A by the pair of fastening members 3A, and contacts the contact surfaces 4b of each of the target members 4A.

[0092] The aluminum member 2 of this embodiment is, for example, a plate member extending in the horizontal direction. The aluminum member 2 is provided with, for example, an opening 2a penetrating in the vertical direction. The aluminum member 2 has a surface 2b exposed at least toward the top and bottom.

[0093] The fastening unit 1 includes a first fastening member 31 and a second fastening member 32 as a pair of fastening members 3A. The first fastening member 31 and the second fastening member 32 sandwich the aluminum member 2 and the pair of target members 4A in the vertical direction. The first fastening member 31 is inserted through the aluminum member 2 and the pair of target members 4A, and is screwed into the second fastening member 32. The first fastening member 31 is provided above the second fastening member 32. The first fastening member 31 is, for example, a bolt. The first fastening member 31 is inserted through an opening 2a of the aluminum member 2. The first fastening member 31 has a head 3a and an insertion portion 3b. In the horizontal direction, the head 3a is larger than the opening diameter of the opening 2a and is thicker than the insertion portion 3b. The insertion portion 3b is provided on a surface 3c exposed toward the bottom of the head 3a. A part of the surface 3c of the head 3a on which the insertion portion 3b is not provided contacts the first target member 41 of the pair of target members 4A, which will be described later. In the horizontal direction, the insertion portion 3b is narrower than the opening diameter of the opening 2a. The insertion portion 3b extends in the vertical direction, and at least the lower end portion is threaded. The second fastening member 32 is, for example, a nut. The second fastening member 32 screws into the threaded insertion portion 3b of the first fastening member 31.

[0094] In this embodiment, a pair of target members 4A are fastened to the aluminum member 2 by a pair of fastening members 3A. Each target member 4A is a member into which a first fastening member 31 is inserted. The fastening unit 1 includes a first target member 41 and a second target member 42 as a pair of target members 4A. The first target member 41 and the second target member 42 sandwich the aluminum member 2 between them in the vertical direction. The first target member 41 and the second target member 42 are each provided with an opening 4a that penetrates in the vertical direction, for example. In the fastening unit 1, the first target member 41 is provided above the aluminum member 2. In the fastening unit 1, the upper surface 4c of the first target member 41 contacts the surface 3c of the head 3a of the first fastening member 31, and the contact surface 4b, which is the lower surface of the first target member 41, contacts the surface 2b, which is the upper surface of the aluminum member 2. The second target member 42 is provided below the aluminum member 2. In the fastening unit 1, the contact surface 4b which is the upper surface of the second target member 42 contacts the surface 2b which is the lower surface of the aluminum member 2, and the lower surface 4d of the second target member 42 contacts the upper surface 3d of the second fastening member 32.

[0095] A case where an aluminum member 2 and a pair of fastening members 3A are fastened to a pair of target members 4A will be described. As an example, the aluminum member 2 is fastened to a pair of target members 4A by the pair of fastening members 3A. The aluminum member 2 is placed between a first target member 41 and a second target member 42 so that the position of the opening 2a and the position of the opening 4a of the pair of target members 4A overlap. The aluminum member 2 is placed so that the surface 2b of the aluminum member 2 contacts each of the contact surfaces 4b of the first target member 41 and the second target member 42. An insertion portion 3b of a first fastening member 31 of the pair of fastening members 3A is inserted into the aluminum member 2 and the target member 4 from above the aluminum member 2 and the pair of target members 4A. Specifically, the insertion portion 3b of the first fastening member 31 is inserted into the opening 2a and the two openings 4a and screwed into the second fastening member 32. As the first fastening member 31 is screwed into the second fastening member 32, the surface 3c of the first fastening member 31 comes into contact with the upper surface 4c of the first target member 41, and the head 3a of the first fastening member 31 presses the first target member 41 toward the second target member 42 (downward). As the first fastening member 31 is screwed into the second fastening member 32, the upper surface 3d of the second fastening member 32 comes into contact with the lower surface 4d of the second target member 42, and the second fastening member 32 presses the second target member 42 toward the first target member 41 (upward). That is, the pair of target members 4A are pressed toward the aluminum members 2 by the pair of fastening members 3A. As a result, the surfaces 2b, which indicate the upper and lower surfaces of the aluminum member 2, come into contact with the contact surfaces 4b of the pair of target members 4A, respectively, and are sandwiched and pressed. When all of the insertion portions 3b are inserted into the opening 2a and the two openings 4a and screwed into the second fastening member 32, the surface 2b of the aluminum member 2 properly pierces the contact surface 4b of the first target member 41 and the contact surface 4b of the second target member 42. In this manner, the aluminum member 2 is sandwiched between the first target member 41 and the second target member 42, and the aluminum member 2 is fastened to the pair of target members 4A by the fastening member 3. Here, fastening includes a state in which certain members are rotated and twisted relatively to one another, so that a plurality of members sandwiched between the two members are fixed together without loosening.

[0096] The enlarged view shown in Fig. 2 is an enlarged view of the fastening unit within the dashed line shown in Fig. 8 when the target member 4 of the fastening unit 1 of the first embodiment is replaced with the second target member 42. Note that, although the contact between the aluminum member 2 and the second target member 42 is given as an example of contact between the aluminum member 2 and the pair of target members 4A, contact between the aluminum member 2 and the first target member 41 is also performed in the same manner. That is, the target member 4 in Fig. 2 may be replaced with either the first target member 41 or the second target member 42, and the description of the target member 4 in the first embodiment applies to either the first target member 41 or the second target member 42.

[0097] As described above, the aluminum member 2 according to the second embodiment is a member for fastening a pair of target members 4A having a resin film 8 on its surface. The aluminum member 2 includes a contact layer 7. The contact layer 7 has a first asperity 7a that can contact the target member 4. The contact layer 7 includes aluminum hydroxide. When the aluminum member 2 and the pair of target members 4A are fastened by a pair of fastening members 3A, the first asperity 7a of the aluminum member 2 penetrates into the resin film 8 of each of the pair of target members 4A. Compared to a case where there is no asperity on the surface, the first asperity 7a increases the contact surface area between the aluminum member 2 and the resin film 8. Therefore, the first asperity 7a that penetrates into the resin film 8 of each of the pair of target members 4A exerts an anchor effect in fastening the pair of target members 4A. Therefore, high friction between the aluminum member 2 and the pair of target members 4A can be stably maintained.

[0098] The aluminum member 2 also includes an intermediate layer 6. The intermediate layer 6 includes both an amorphous substance containing aluminum atoms and oxygen atoms, or an amorphous substance and a layered double hydroxide containing aluminum atoms and oxygen atoms. When at least the main body 5 of the aluminum member 2 and each of the pair of target members 4A are in direct contact with each other, corrosion of the aluminum member 2 may occur due to electrochemical action. For example, when the material of the aluminum member 2 and each of the pair of target members 4A have different types of metals, bimetallic corrosion (galvanic corrosion) defined in JIS-Z0103 may occur between the aluminum member 2 and each of the pair of target members 4A. In addition, when the aluminum member 2 and each of the pair of target members 4A contain the same material or when each of the pair of target members 4A contains a conductive material, stray current corrosion (electrolytic corrosion) defined in JIS-Z0103 may occur between the aluminum member 2 and each of the pair of target members 4A. In this embodiment, even if the first unevenness 7a of the contact layer 7 of the aluminum member 2 penetrates the resin film 8 of each of the pair of target members 4A, the intermediate layer 6 is interposed between the fastened aluminum member 2 and each of the pair of target members 4A. Since the intermediate layer 6 has insulating properties, contact between the main body 5 of the aluminum member 2 and the resin film 8 and the target main body 9 of each of the pair of target members 4A is suppressed. Even if each of the pair of target members 4A has a conductive material or a dielectric, contact between each of the pair of target members 4A and the main body 5 of the aluminum member 2 is suppressed, so corrosion of the aluminum member 2 due to electrochemical action is suppressed. Therefore, the aluminum member 2 can stably maintain high corrosion resistance when fastened to each of the pair of target members 4A. In this way, the aluminum member 2 can exhibit high friction and high corrosion resistance when fastened to each of the pair of target members 4A.

[0099] The aluminum member 2 further includes a second asperity 2d of the micro order formed on the surface 2b of the aluminum member 2. The first asperity 7a is formed on the surface 2b of the second asperity 2d. In this case, the second asperity 2d contributes to an anchor effect. Even if the second asperity 2d is an acute-angled protrusion, the surface 2b of the aluminum member 2 is covered with the intermediate layer 6 and the contact layer 7 by forming the first asperity 7a on the surface 2b of the second asperity 2d. As a result, the second asperity 2d is rounded. According to this aluminum member 2, the second asperity 2d cannot be an acute-angled protrusion that can become a starting point for breaking the resin film 8 of each of the pair of target members 4A, so that high friction between the aluminum member 2 and each of the pair of target members 4A can be stably maintained.

[0100] [Fastening method and manufacturing method for aluminum members] A description will be given of a series of flows of the fastening method of the fastening unit 1A and the manufacturing method of the aluminum member 2. In the fastening method of the fastening unit 1A and the manufacturing method of the aluminum member 2 according to the second embodiment, the same processes as those in the flowchart of the fastening method MT including the manufacturing method of the aluminum member shown in Fig. 6 according to the first embodiment are carried out. Descriptions of the processes that overlap with those in the first embodiment will be omitted.

[0101] In the preparation step (S10), a pair of target members 4A having a resin film 8 on their surfaces and an aluminum member 2 are prepared. The preparation step (S10) may include a determination step of determining at least a pair of target members 4A. By determining in advance the pair of target members 4A to be used in the fastening step (S14) described later, it is possible to determine the processing content for the aluminum member 2 in accordance with the pair of target members 4A. In the determination step, for example, a pair of target members 4A on which a resin film 8 of 5 μm or more and 50 μm or less is formed on each contact surface 4b is determined as a pair of target members 4A to be used in the fastening step (S14) described later. In this embodiment, a first target member 41 and a second target member 42 to be used in the fastening step (S14) described later are determined as the multiple target members 4.

[0102] In the fastening step (S14), the aluminum member 2 and each of the pair of target members 4A are fastened to each other while the first unevenness 7a and the second unevenness 2d of the aluminum member 2 are pierced into the resin film 8 of each of the pair of target members 4A. For example, the worker places the aluminum member 2 on each of the contact surfaces 4b of the pair of target members 4A so that the position of the opening 2a and the position of the opening 4a overlap. The aluminum member 2 is placed so that the surface 2b of the aluminum member 2 contacts each of the contact surfaces 4b of the pair of target members 4A. That is, the aluminum member 2 is placed so as to be sandwiched between the first target member 41 provided above and the second target member 42 provided below. The first fastening member 31 of the pair of fastening members 3A is inserted into the aluminum member 2 and the pair of target members 4A from above the aluminum member 2 and the pair of target members 4A. At this time, the second fastening member 32 of the pair of fastening members 3A is placed below the aluminum member 2 and the pair of target members 4A. Specifically, for example, the worker inserts the insertion portion 3b of the first fastening member 31 from above through the opening 4a of the first target member 41, the opening 2a of the aluminum member 2, and the opening 4a of the second target member 42, in that order, and screws it into the second fastening member 32 arranged below the second target member 42. As the first fastening member 31 screws into the second fastening member 32, the surface 3c of the head 3a of the first fastening member 31 comes into contact with the upper surface 4c of the first target member 41, and the upper surface 3d of the second fastening member 32 comes into contact with the lower surface 4d of the second fastening member 32, so that the first target member 41 and the second target member 42 can be pressed toward the aluminum member 2. As a result, the surface 2b of the aluminum member 2 sandwiched between the first target member 41 and the second target member 42 pierces the resin film 8 provided on each contact surface 4b of the first target member 41 and the second target member 42. When the insertion portion 3b of the first fastening member 31 is inserted into the opening 2a and each opening 4a and is screwed into the second fastening member 32, the surface 2b of the aluminum member 2 properly pierces each contact surface 4b of the first target member 41 and the second target member 42. In this manner, the aluminum member 2 is sandwiched between the first target member 41 and the second target member 42 by the screwing of the first fastening member 31 and the second fastening member 32, and the aluminum member 2 is fastened to the pair of target members 4A by the pair of fastening members 3A.In the fastening step (S14), the aluminum member 2 and the pair of target members 4A may be fastened together automatically by a fastening device (not shown) or the like, instead of by a worker as described above.

[0103] As described above, according to the fastening method and aluminum manufacturing method of the second embodiment, the first asperities 7a and second asperities 2d of the aluminum member 2 penetrate into the resin films 8 of the pair of target members 4A in the fastening step (S14). The first asperities 7a and second asperities 2d that penetrate into the resin films 8 of the pair of target members 4A provide an anchor effect in fastening to each of the pair of target members 4A. This makes it possible to stably maintain high friction between the aluminum member 2 and the multiple target members 4.

[0104] In addition, an intermediate layer 6 is formed on the surface of the aluminum member 2. The intermediate layer 6 has both an amorphous substance containing aluminum atoms and oxygen atoms, or an amorphous substance and a layered double hydroxide containing aluminum atoms and oxygen atoms. When at least the main body 5 of the aluminum member 2 and each of the pair of target members 4A are in direct contact with each other, corrosion of the aluminum member 2 may occur due to electrochemical action. For example, when the material of the aluminum member 2 and each of the pair of target members 4A have different types of metals, bimetallic corrosion (galvanic corrosion) defined in JIS-Z0103 may occur between the aluminum member 2 and each of the pair of target members 4A. In addition, for example, when the aluminum member 2 and each of the pair of target members 4A contain the same material or when each of the pair of target members 4A contains a conductive material, stray current corrosion (galvanic corrosion) defined in JIS-Z0103 may occur between the aluminum member 2 and each of the pair of target members 4A. In this embodiment, even if the first unevenness 7a of the contact layer 7 of the aluminum member 2 penetrates the resin film 8 of each of the pair of target members 4A, the intermediate layer 6 is interposed between the fastened aluminum member 2 and each of the pair of target members 4A. Since the intermediate layer 6 has insulating properties, contact between the main body 5 of the aluminum member 2 and the resin film 8 and the target main body 9 of each of the pair of target members 4A is suppressed. Even if each of the pair of target members 4A has a conductive material or a dielectric, contact between each of the pair of target members 4A and the main body 5 of the aluminum member 2 is suppressed, so corrosion of the aluminum member 2 due to electrochemical action is suppressed. Therefore, the aluminum member 2 can stably maintain high corrosion resistance when fastened to each of the pair of target members 4A. In this way, high friction and high corrosion resistance are exhibited in this fastening method MT. In addition, this manufacturing method for an aluminum member can manufacture an aluminum member 2 that can exhibit high friction and high corrosion resistance when fastened to a pair of target members 4A.

[0105] According to the fastening method MT and the manufacturing method of the aluminum member 2, the forming step (S12) includes a surface hydration step in which the surface 2b of the aluminum member 2 is reacted with saturated water vapor under a pressure higher than atmospheric pressure and not higher than about 4.30 MPa to modify the surface 2b of the aluminum member 2 into aluminum hydroxide, thereby forming the intermediate layer 6 and the contact layer 7. When the second irregularities 2d are formed on the surface 2b of the aluminum member 2, the second irregularities 2d are covered with the intermediate layer 6 and the contact layer 7 by the surface hydration step, and therefore change from acute irregularities that may be the starting point of breakage of the resin films 8 of the pair of target members 4A to rounded irregularities. Furthermore, since the aluminum member 2 reacts with water vapor due to the above-mentioned pressure, the fastening method MT and the manufacturing method of the aluminum member 2 can form the intermediate layer 6 and the contact layer 7 having the first irregularities 7a on the surface of the aluminum member 2.

[0106] According to the fastening method MT, the thickness of the resin film 8 of each of the pair of target members 4A is 5 μm or more and 50 μm or less. In this case, in the fastening method MT, since the thickness of the resin film 8 is 5 μm or more, the first asperities 7a and the second asperities 2d of the contact layer 7 of the aluminum member 2 can be appropriately inserted into the resin film 8 of each of the pair of target members 4A. Also, in the fastening method MT, since the thickness of the resin film 8 is 50 μm or less, the degree to which the resin film 8 deforms with respect to the aluminum member 2 when friction occurs between the aluminum member 2 and each of the pair of target members 4A is reduced, and breakage can be suppressed. As a result, the fastening method MT can appropriately exert a high frictional force between the aluminum member 2 and each of the pair of target members 4A. Also, since the second asperities 2d are formed before the first asperities 7a are formed in the forming step (S12), the surface 2b of the aluminum member 2 can be made to have an appropriate roughness corresponding to the thickness of the resin film 8.

[0107] Although the first and second embodiments have been described above, the present invention is not limited to the above-described first and second embodiments, and it goes without saying that the present invention can be implemented in various modified forms other than the first and second embodiments without departing from the spirit of the present invention.

[0108] [Modifications of aluminum and resin materials] A washer is shown as an example of the aluminum member 2 according to the first embodiment, and a plate-shaped member is shown as an example of the aluminum member 2 according to the second embodiment, but the aluminum member 2 is not limited to washers and plate-shaped members and can be applied to various parts used for fastening. A male screw is shown as an example of the fastening member 3, but the fastening member 3 is not limited to male screws and can be applied to various parts used for fastening to the aluminum member 2.

[0109] For example, the aluminum member 2 may be a washer, a bolt, a nut, a rivet, a pin, a key, or a retaining ring. For example, when the aluminum member 2 is a bolt, the target member 4 may be a base material that is directly fastened without a washer or the like. For example, when the aluminum member 2 is a bolt, the target member 4 may be a fastening member such as a washer or a nut. For example, when the aluminum member 2 is a fastening member such as a washer or a nut, the target member 4 may be a fastening member such as a bolt. The term "fastening" here may include fixing without loosening by rotating and twisting the members relative to each other. When the aluminum member 2 or the target member 4, 4A is a fastening member, the first fastening member 31 or the second fastening member 32 of the second embodiment may be replaced with the aluminum member 2 or the target member 4.

[0110] The fastening unit 1 may, for example, include a plurality of fastening members 3, and the fastening unit 1A may, for example, include one or three or more fastening members 3. Also, the fastening unit 1 may, for example, include a plurality of target members 4, and the fastening unit 1A may, for example, include one or three or more target members 4.

[0111] In the fastening method MT and the manufacturing method of the aluminum member 2, the forming step (S12) does not have to include a blasting process step. The forming step (S12) may include a mirror polishing step (mirror polishing step) instead of the blasting process step. The mirror polishing step is carried out before the surface hydroxylation step. In this case, as the preparation step (S10), instead of the preparation related to the blasting device 10, preparation of devices to be used in the mirror polishing step is carried out.

[0112] In the mirror polishing step, the aluminum member 2B (see FIG. 9 described later) to be mirror polished is buffed by a buffing machine in the forming step (S12). The forming step (S12) may include a step of washing the surface of the aluminum member 2B with ethanol after the buffing. As a result, the surface of the aluminum member 2 is smoothed after the mirror polishing step in the forming step (S12) and before the surface hydroxylation step is performed, so that the number of irregularities on the surface of the aluminum member before the forming step (S12) is reduced. In addition, by performing the mirror polishing step, scratches formed on the surface of the aluminum member before the surface hydroxylation step and deposits attached to the surface of the aluminum member before the surface hydroxylation step are scraped off. In the aluminum member that has been subjected to the mirror polishing step and the surface hydroxylation step in the forming step (S12), the maximum height Ry and the ten-point average roughness Rz, which indicate the surface roughness, are reduced. By carrying out the mirror polishing step before carrying out the surface hydroxylation step, the first irregularities formed on the surface of the aluminum member are prevented from breaking through the resin film. Therefore, the aluminum member that has been subjected to the mirror polishing step in the formation step (S12) can ensure appropriate high frictional properties against various target members.

[0113] FIG. 9 is an enlarged view of an aluminum member and a fastening unit according to a modified example. FIG. 9 shows a state in which an aluminum member 2B included in a fastening unit 1B is pierced into a target member 4. A main body portion 5B of the aluminum member 2B is processed into a flat shape. An intermediate layer 6 is formed on the surface of the flat main body portion 5B, and a contact layer 7 is formed at the lower end of the intermediate layer 6. In this case, the aluminum member 2B has a contact layer 7 that can pierce the resin film 8 of the target member 4 (second target member 42) formed thereon, similar to the first and second embodiments described above. Note that the aluminum member 2B can also have a contact layer 7 that can pierce the resin film 8 of the first target member 41 formed thereon, similar to the second embodiment described above. EXAMPLES

[0114] [Confirmation of friction and corrosion resistance of aluminum components by carrying out surface hydration process] Fig. 10 shows the results of a friction test and a corrosion resistance test for the processing conditions according to the examples. In Examples 1 to 10 and Comparative Examples 1 to 4 shown in Fig. 10, a fastening unit similar to the fastening unit 1A of the second embodiment including an aluminum member that had not been subjected to blast processing was prepared, and the slip resistance as a friction force was confirmed. In addition, in Examples 1 to 10 and Comparative Examples 1 to 4, an aluminum member that had been subjected to a surface hydroxylation process under the same conditions as the aluminum member used in the above-mentioned fastening unit was prepared, and the corrosion current density as a corrosion resistance was confirmed.

[0115] [Example 1] As the aluminum members of Example 1, an aluminum member for a slip resistance test and an aluminum member for a corrosion resistance test were prepared. In the preparation step (S10), an aluminum member, a pair of fastening members, and a pair of target members were prepared as members capable of producing a fastening unit for a slip resistance test. An aluminum plate (JIS: A5052) having a width of 50 mm, a depth of 30 mm, and a thickness of 5 mm was used as the aluminum member. In the aluminum member, a through hole into which an M12 bolt can be inserted was formed as an opening in the thickness direction. The through hole was formed so that the center of the through hole was located 15 mm away from the two long sides and 15 mm away from one short side. Of the pair of fastening members, an aluminum M12 hexagonal bolt was used as the first fastening member. Of the pair of fastening members, an aluminum M12 hexagonal nut was used as the second fastening member. As the pair of target members, a first target member and a second target member were prepared. As the first and second target members, aluminum plates (JIS: A5052) with a width of 50 mm, a depth of 30 mm, and a thickness of 5 mm were used. In the first and second target members, through holes into which M12 bolts could be inserted were formed in the thickness direction as openings. The through holes were formed at a location 15 mm from one short side toward the other short side. The first and second target members were resin-coated to form resin films. Each resin film was mainly composed of epoxy. As shown in FIG. 10, the resin film of the target member had a thickness of 5 μm. In addition, in the preparation step (S10), an aluminum plate (JIS: A5052) with a width of 15 mm, a depth of 15 mm, and a thickness of 1.5 mm was prepared as an aluminum member for the corrosion resistance test. Subsequently, a surface hydroxylation step was performed in a formation step (S12) on the aluminum member for the slip resistance test and the aluminum member for the corrosion resistance test.Specifically, the following steps were carried out in sequence: (1) washing each aluminum component with ethanol (special grade, Kishida Chemical Co., Ltd.) for 2 minutes; (2) placing the base, aluminum components, and 10 ml of pure water in a Teflon (registered trademark) container; (3) sealing the Teflon container in an autoclave container (HUTc-100, San-Ai Scientific Co., Ltd.); (4) placing the autoclave container in a constant temperature dryer (SONW-300S, AS ONE Co., Ltd.) that had been preheated to 180°C; (5) reacting the aluminum components with the water vapor generated by heating the pure water in the Teflon container for 24 hours; and (6) after 24 hours had passed, removing the autoclave container from the constant temperature dryer, removing the Teflon container from the autoclave container, and removing the aluminum components from the Teflon container. In the above-mentioned process (5), when the temperature is 180°C, the pressure of the water vapor in the Teflon container is equal to the value of the saturated water vapor pressure, so that the absolute pressure of the water vapor in the Teflon container is 1.05 MPa, which is higher than the atmospheric pressure. Hereinafter, the pressure of the water vapor is described in terms of absolute pressure, with the vacuum state being 0 MPa and the state under atmospheric pressure being 0.1013 MPa. As a result of reacting each aluminum member with the saturated water vapor as described above, as shown in FIG. 10, Ry was 2.7 μm, Rz was 1.9 μm, and the ratio of Ry to Rz was 1.4. Thereafter, as a fastening step (S14), the aluminum member for the slip resistance test and a pair of target members were fastened with a pair of fastening members to form a fastening unit. Specifically, the aluminum member for the slip resistance test was sandwiched between the first target member and the second target member, and the aluminum member, the first target member, and the second target member were positioned so that their openings overlapped with each other. At this time, the aluminum member, the first target member, and the second target member were positioned at the same position in the depth direction. The aluminum member and the first target member and the aluminum member and the second target member were overlapped so that the overlapping width was 30 mm each. Then, the insertion portion of the first fastening member was inserted from above into the opening of the aluminum member and the openings of the first target member and the second target member, and the portion of the insertion portion of the first fastening member protruding from the opening of the second target member was fastened with the second fastening member.As a result, the aluminum member for the slip resistance test and the multiple target members are sandwiched between the first fastening member and the second fastening member, and are pressed in a direction in which they come into contact with each other, thereby fastening them together.

[0116] [Example 2] In Example 2, the temperature was set to 100° C. in the surface hydroxylation step of the formation step (S12). When the temperature was 100° C., the pressure of the water vapor in the autoclave container was equal to the saturated water vapor pressure, so the pressure of the water vapor in the container was 0.102 MPa, which is higher than atmospheric pressure. The other conditions were the same as in Example 1.

[0117] [Example 3] In Example 3, the temperature was set to 120° C. in the surface hydroxylation step of the formation step (S12). When the temperature was 120° C., the water vapor pressure in the autoclave container was equal to the saturated water vapor pressure, and therefore the water vapor pressure in the container was 0.202 MPa, which is higher than atmospheric pressure. The other conditions were the same as in Example 1.

[0118] [Example 4] In Example 4, the temperature was set to 250° C. in the surface hydroxylation step of the formation step (S12). When the temperature was 250° C., the pressure of the water vapor in the autoclave container was equal to the saturated water vapor pressure, so the pressure of the water vapor in the container was 4.30 MPa, which is higher than atmospheric pressure. The other conditions were the same as in Example 1.

[0119] [Example 5] In Example 5, the aluminum member was reacted with saturated water vapor for 0.5 hours in the surface hydroxylation step of the formation step (S12). The other conditions were the same as those in Example 1.

[0120] [Example 6] In Example 6, the aluminum member was reacted with saturated water vapor for 2 hours in the surface hydroxylation step of the formation step (S12). The other conditions were the same as those in Example 1.

[0121] [Example 7] In Example 7, the aluminum member was reacted with saturated water vapor for 8 hours in the surface hydroxylation step of the formation step (S12). The other conditions were the same as those in Example 1.

[0122] [Example 8] In Example 8, the aluminum member was reacted with saturated water vapor for 16 hours in the surface hydroxylation step of the formation step (S12). The other conditions were the same as those in Example 1.

[0123] [Example 9] In Example 9, the aluminum member was reacted with saturated water vapor for 48 hours in the surface hydroxylation step of the formation step (S12). The other conditions were the same as those in Example 1.

[0124] [Example 10] In Example 10, aluminum plates (JIS: A6061) were prepared as the aluminum members for the slip resistance test and the aluminum members for the corrosion resistance test in the preparation step (S10). The other conditions were the same as those in Example 1.

[0125] [Comparative Example 1] In Comparative Example 1, the surface hydroxylation step was not performed in the formation step (S12). The other conditions were the same as those in Example 1.

[0126] [Comparative Example 2] In Comparative Example 2, the temperature was set to 90° C. in the surface hydroxylation step of the formation step (S12). When the temperature was 90° C., the water vapor pressure in the autoclave container was equal to the saturated water vapor pressure, and therefore the water vapor pressure in the container was 0.0705 MPa, which is lower than atmospheric pressure. The other conditions were the same as in Example 1.

[0127] [Comparative Example 3] In Comparative Example 3, the temperature was set to 300° C. in the surface hydroxylation step of the formation step (S12). When the temperature was 300° C., the water vapor pressure in the autoclave container was equal to the saturated water vapor pressure, so the water vapor pressure in the container was 9.41 MPa, which was higher than atmospheric pressure. The other conditions were the same as in Example 1.

[0128] [Comparative Example 4] In Comparative Example 4, the aluminum member was reacted with saturated water vapor for 0.25 hours in the surface hydroxylation step of the formation step (S12). The other conditions were the same as those in Example 1.

[0129] [Comparative Example 5] In Comparative Example 5, the aluminum member was reacted with saturated water vapor for 72 hours in the surface hydroxylation step of the formation step (S12). The other conditions were the same as those in Example 1.

[0130] [Composition and crystal structure analysis of the intermediate layer] The diffracted X-ray intensity at each diffraction angle was measured by XRD (X-ray diffraction) for the aluminum members before and after the surface hydroxylation step in Examples 1 to 10 and Comparative Examples 2 to 5. The diffracted X-ray intensity at each diffraction angle was also measured by XRD for the aluminum member after the preparation step (S10) in Comparative Example 1. The diffraction angle indicates the angle of the scanning axis. The diffracted X-ray intensity is the intensity (CPS) indicating the number of diffracted X-rays taken in by the detector per second. The composition and crystal structure of the surface layer (intermediate layer) of the aluminum member were confirmed based on the characteristics of the peaks shown in the measurement results of the diffracted X-ray intensity versus the diffraction angle. From the XRD measurement results, it was confirmed that the surface layer of the aluminum member before the surface hydroxylation step in Examples 1 to 10 and Comparative Examples 2 to 5 did not contain an amorphous substance containing aluminum atoms and oxygen atoms, and a layered double hydroxide containing aluminum atoms and oxygen atoms. The XRD measurement results confirmed that the surface layer of the aluminum component after the preparation step (S10) of Comparative Example 1 did not contain amorphous substances containing aluminum atoms and oxygen atoms, or layered double hydroxides containing aluminum atoms and oxygen atoms.

[0131] From the XRD measurement results, it was confirmed that the intermediate layer of the aluminum member after the surface hydroxylation process of Example 1 contains an amorphous substance containing aluminum atoms and oxygen atoms and a layered double hydroxide containing aluminum atoms and oxygen atoms, as shown by "A" in FIG. 10. From the XRD measurement results, it was confirmed that the intermediate layer of the aluminum member after the surface hydroxylation process of Examples 2 to 10 and Comparative Examples 3 and 5 does not contain a layered double hydroxide containing aluminum atoms and oxygen atoms, but contains an amorphous substance containing aluminum atoms and oxygen atoms, as shown by "B" in FIG. 10. From the XRD measurement results, it was confirmed that the surface layer of the aluminum member after the surface hydroxylation process of Comparative Examples 2 and 4 does not contain an amorphous substance containing aluminum atoms and oxygen atoms, and a layered double hydroxide containing aluminum atoms and oxygen atoms, as shown by "C" in FIG. 10.

[0132] [Friction force evaluation] The slip resistance was measured as the friction force in the fastening units of Examples 1 to 10 and Comparative Examples 1 to 5 produced under the above conditions. In Fig. 7 and Fig. 8, a tensile force was applied to the aluminum member in the positive direction of the Y axis, and to the first and second target members in the negative direction of the Y axis. In the fastening units of Examples 1 to 10 and Comparative Examples 1 to 5, the slip resistance is expressed as "very good" in Fig. 10 when it is twice or more the test result of the fastening unit of Comparative Example 1, which uses an aluminum member that has not been subjected to the blast processing process and the surface hydroxylation process, and the slip resistance is expressed as "good" in Fig. 10 when it is more than once and less than twice the slip resistance of Comparative Example 1, and the slip resistance is expressed as "poor" in Fig. 10 when it is once or less the slip resistance of Comparative Example 1. The evaluation values ​​of Examples 1, 3, 4, 6 to 10 and Comparative Examples 3 and 5 are "very good". The evaluation values ​​of Examples 2 and 5 are "good". The evaluation values ​​of Comparative Examples 1, 2 and 4 are "poor".

[0133] By comparing Examples 1 and 2 with Comparative Example 1, it was confirmed that the surface hydroxylation process in the forming process (S12) contributes to the generation of slip resistance. If the surface hydroxylation process is not performed, the developed interface area ratio Sdr of the contour curved surface will be less than 10%, and no unevenness will be generated on the surface of the aluminum member, which will not contribute to friction, and therefore the evaluation of the slip resistance will be poor.

[0134] By comparing Examples 1 to 4 and Comparative Example 3 with Comparative Example 2, it was confirmed that the slip resistance improves when the temperature of the surface hydroxylation step in the formation step (S12) is set to 100°C or higher. When the temperature of the surface hydroxylation step is 100°C or higher, a pressure exceeding atmospheric pressure is applied compared to when the temperature of the surface hydroxylation step is 90°C, so that a sufficient reaction takes place, the developed interface area ratio Sdr of the contour curved surface becomes 10% or more, and the first unevenness is appropriately formed on the surface of the aluminum member in the contact layer. For this reason, it is considered that a change is observed in the slip resistance (friction force) of the aluminum member before and after the reaction. In Comparative Example 2, in which the temperature of the surface hydroxylation step is 90°C, a pressure exceeding atmospheric pressure is not applied, so that it is considered that the formation of the contact layer (first unevenness) was insufficient.

[0135] Furthermore, by comparing Example 2 with Examples 1, 3, and 4 and Comparative Example 3, it was confirmed that the slip resistance was significantly improved when the temperature in the surface hydroxylation step was 120°C or higher. When the temperature in the surface hydroxylation step was 120°C or higher, the reaction proceeded more sufficiently than when the temperature in the surface hydroxylation step was 100°C, the developed interface area ratio Sdr of the contour curved surface was 20% or higher, and more first projections and recesses were appropriately formed on the surface of the aluminum member in the contact layer. For this reason, a large change was observed in the slip resistance (friction force) of the aluminum member before and after the reaction, and it is believed that the evaluation value improved significantly.

[0136] Furthermore, from the results of Examples 1 to 4 and Comparative Example 3, it was confirmed that the sliding resistance was significantly improved even when the temperature in the surface hydroxylation step was higher than 250°C. It is considered that when the temperature in the surface hydroxylation step is 250°C or higher, the reaction proceeds sufficiently, the developed interface area ratio Sdr of the contour curved surface becomes 30% or more, and the first irregularities in the contact layer are largely developed and formed on the surface of the aluminum member. For this reason, it is considered that a change in the sliding resistance (friction force) of the aluminum member before and after the reaction is observed.

[0137] From the results of Examples 1, 5 to 9 and Comparative Example 4, it was confirmed that the slip resistance improves when the reaction time of the surface hydroxylation step in the formation step (S12) is 0.5 hours or more. Unlike when the reaction time of the surface hydroxylation step is 0.25 hours, when the reaction time of the surface hydroxylation step is 0.5 hours or more, a sufficient reaction takes place, the developed interface area ratio Sdr of the contour curved surface becomes 10% or more, and the first unevenness is formed on the surface of the aluminum member in the contact layer, and therefore it is considered that a change is observed in the slip resistance (friction force) of the aluminum member before and after the reaction.

[0138] Furthermore, by comparing Example 5 with Examples 1, 6 to 9, it was confirmed that the slip resistance was significantly improved when the reaction time of the surface hydroxylation step was 2 hours or more. When the reaction time of the surface hydroxylation step was 2 hours or more, the reaction proceeded more sufficiently than when the reaction time of the surface hydroxylation step was 0.5 hours, the developed interface area ratio Sdr of the contour curved surface was 20% or more, and it is considered that more first projections and recesses are appropriately formed on the surface of the aluminum member in the contact layer.

[0139] Furthermore, from the results of Examples 1, 5 to 9 and Comparative Example 5, it was confirmed that the sliding resistance was significantly improved even when the reaction time of the surface hydroxylation step was longer than 48 hours. When the reaction time of the surface hydroxylation step was longer than 48 hours, it is considered that the reaction took place sufficiently, the developed interface area ratio Sdr of the contour curved surface was 40% or more, and the first unevenness in the contact layer was largely developed and formed on the surface of the aluminum member. For this reason, it is considered that a change was observed in the sliding resistance (frictional force) of the aluminum member before and after the reaction.

[0140] From the results of Examples 1 and 10, it was confirmed that very good slip resistance can be ensured by carrying out the surface hydroxylation step in the formation step (S12), regardless of the material of the aluminum member.

[0141] Although not shown in Fig. 10, Example 4 had the largest slip resistance among Examples 1 to 10. This is thought to be because the temperature of the surface hydroxylation step in the formation step (S12) was set high, thereby forming first irregularities of sufficient thickness on the surface of the aluminum member, and the area of ​​contact with the target member was increased, thereby contributing to an increase in the friction force (slip resistance).

[0142] [Corrosion resistance evaluation] The corrosion current density as corrosion resistance was measured for the aluminum members for corrosion resistance testing of Examples 1 to 10 and Comparative Examples 1 to 5 prepared under the above conditions. Using a potentiostat, the aluminum members for corrosion resistance testing of Examples 1 to 10 and Comparative Examples 1 to 5 were immersed in an H2SO4 aqueous solution of pH 3 at room temperature, and polarization measurements were performed while nitrogen bubbling was performed. The corrosion current density was calculated for the aluminum members for corrosion resistance testing of Examples 1 to 10 and Comparative Examples 1 to 5 by Tafel extrapolation from the obtained polarization curves. In Comparative Example 1, where the blasting process and surface hydroxylation process were not performed, the corrosion current density was 6.80×10 -7 A / cm 210 shows the ratio of the corrosion current density of Comparative Example 1 to the corrosion current densities of Examples 1 to 10 and Comparative Examples 1 to 5 as corrosion resistance (corrosion resistance performance). The larger this ratio is than 1, the smaller the corrosion current density is than Comparative Example 1, indicating better corrosion resistance. Hereinafter, when this ratio is 140 or more, the corrosion resistance is evaluated as very good (very high), when this ratio is 130 or more and less than 140, the corrosion resistance is evaluated as good (high), and when this ratio is less than 130, the corrosion resistance is evaluated as poor (low).

[0143] By comparing Examples 1 and 2 with Comparative Example 1, it was confirmed that the surface hydroxylation step in the formation step (S12) contributes to improving corrosion resistance. When the surface hydroxylation step is performed, an intermediate layer is formed on the surface of the aluminum member compared to when the surface hydroxylation step is not performed, so it is believed that the corrosion current density is reduced and the corrosion resistance is improved. The corrosion current density of Example 2 is 1 / 130 of the corrosion current density of Comparative Example 1. It is believed that the formation of an intermediate layer having a passivation function on the surface of the aluminum member in the surface hydroxylation step leads to a reduction in the current density on the surface of the aluminum member, resulting in high (very improved) corrosion resistance.

[0144] By comparing Example 2 and Comparative Example 2, it was confirmed that when the temperature in the surface hydroxylation step in the formation step (S12) is 100°C or higher, the corrosion resistance is improved and contributes to the improvement of the corrosion resistance. When the temperature in the surface hydroxylation step is 100°C or higher, a pressure exceeding atmospheric pressure is applied compared to when the temperature in the surface hydroxylation step is 90°C, so that a sufficient reaction takes place and an intermediate layer is appropriately formed on the surface of the aluminum member (between the aluminum member and the contact layer), and therefore it is considered that a change in the corrosion resistance of the aluminum member before and after the reaction is observed. In Comparative Example 2, where the temperature in the surface hydroxylation step is 90°C, it is considered that the formation of the intermediate layer was insufficient because no pressure exceeding atmospheric pressure was applied.

[0145] Furthermore, by comparing Examples 1, 3, and 4 with Example 2, it was confirmed that when the temperature in the surface hydroxylation step in the formation step (S12) is 120°C or higher, the corrosion resistance is significantly improved, which contributes greatly to the improvement of corrosion resistance. It is believed that when the temperature in the surface hydroxylation step is 120°C or higher, the reaction proceeds more sufficiently than when the temperature in the surface hydroxylation step is 100°C, and the intermediate layer is appropriately formed on the surface of the aluminum member. For this reason, a large change was observed in the corrosion resistance of the aluminum member before and after the reaction, and it is believed that the corrosion resistance was significantly improved.

[0146] Furthermore, by comparing Examples 1 to 4 with Comparative Example 3, it was confirmed that when the temperature of the surface hydroxylation step in the formation step (S12) is set to 250°C or less, the corrosion resistance is significantly improved, which contributes greatly to the improvement of the corrosion resistance. When the temperature of the surface hydroxylation step is 250°C or less, at least one of the contact layer and the intermediate layer does not grow too hard compared to when the temperature of the surface hydroxylation step is 300°C, and the occurrence of cracks in at least one of the contact layer and the intermediate layer due to thermal shock during cooling is suppressed, so it is believed that the corrosion resistance of the aluminum member is maintained at a high level. In Comparative Example 3, where the temperature of the surface hydroxylation step is 300°C, it is believed that the corrosion resistance was deteriorated because cracks occurred in at least one of the contact layer and the intermediate layer due to thermal shock.

[0147] From the results of Examples 1, 5 to 9 and Comparative Example 4, it was confirmed that when the reaction time of the surface hydroxylation step in the formation step (S12) is 0.5 hours or more, the corrosion resistance is improved and contributes to the improvement of the corrosion resistance. Unlike when the reaction time of the surface hydroxylation step is 0.25 hours, when the reaction time of the surface hydroxylation step is 0.5 hours or more, a sufficient reaction takes place and an intermediate layer is formed on the surface of the aluminum member, so it is considered that a change in the corrosion resistance of the aluminum member before and after the reaction is observed.

[0148] In addition, by comparing Example 5 with Examples 1, 6 to 9, it was confirmed that the corrosion resistance was significantly improved when the reaction time of the surface hydroxylation step was 2 hours or more. It is considered that when the reaction time of the surface hydroxylation step was 2 hours or more, the reaction proceeded more sufficiently than when the reaction time of the surface hydroxylation step was 0.5 hours, and the intermediate layer was appropriately formed on the surface of the aluminum component.

[0149] By comparing Examples 1, 4 to 7 with Comparative Example 5, it was confirmed that when the reaction time of the surface hydroxylation step in the formation step (S12) is 48 hours or less, the corrosion resistance is very good, which contributes greatly to the improvement of the corrosion resistance. When the reaction time of the surface hydroxylation step is 48 hours or less, at least one of the contact layer and the intermediate layer does not grow too hard, and cracks are suppressed in at least one of the contact layer and the intermediate layer due to thermal shock when cooled, compared with the case where the reaction time of the surface hydroxylation step is 72 hours, so that the corrosion resistance of the aluminum member is thought to be maintained at a high level. In Comparative Example 4, where the reaction time of the surface hydroxylation step is 72 hours, cracks are generated in at least one of the contact layer and the intermediate layer due to thermal shock, which is thought to have deteriorated the corrosion resistance. However, by comparing Comparative Example 1 with Comparative Example 4, it was confirmed that better corrosion resistance can be obtained if the reaction time of the surface hydroxylation step is 0.5 hours or more.

[0150] From the results of Examples 1 and 10, it was confirmed that very good corrosion resistance can be ensured by carrying out the surface hydroxylation process, regardless of the material of the aluminum member.

[0151] As described above, it has been confirmed that the aluminum members of Examples 1 to 10 manufactured by the fastening method MT and the manufacturing method for an aluminum member described in the above embodiment exhibit both high friction properties and high corrosion resistance when fastened to the target member 4, compared to the aluminum members of Comparative Examples 1 to 5.

[0152] [Confirmation of friction and corrosion resistance of aluminum components by performing blast processing and surface hydroxylation processes] Fig. 11 shows the results of a friction test and a corrosion resistance test for the processing conditions according to the examples. In Examples 11 to 15 and Comparative Examples 6 to 8 shown in Fig. 11, a fastening unit similar to the fastening unit 1A of the second embodiment was prepared, and slip resistance as a friction force was confirmed. In addition, in Examples 11 to 15 and Comparative Examples 6 to 8, an aluminum member was prepared that had been subjected to a blasting process and a surface hydroxylation process under the same conditions as the aluminum member used in the above-mentioned fastening unit, and the corrosion current density as corrosion resistance was confirmed.

[0153] [Example 11] In the preparation step (S10), an aluminum member, a pair of fastening members, and a pair of target members were prepared under the same conditions as in Example 1 as members capable of producing a fastening unit for a slip resistance test. In addition, in the preparation step (S10), an aluminum plate was prepared under the same conditions as in Example 1 as an aluminum member for a corrosion resistance test. Then, a mirror polishing step was performed on the aluminum member for the slip resistance test and the aluminum member for the corrosion resistance test in the formation step (S12). In the mirror polishing step, buffing was performed using a precision sample automatic polishing machine (Tegramin-30, Struers), and the aluminum member was washed for 2 minutes using ethanol (special grade, Kishida Chemical Co., Ltd.). Then, a surface hydroxylation step was performed in the formation step (S12) under the same conditions as in Example 1, except that the reaction time between each aluminum member and saturated water vapor was set to 2 hours for the mirror polished aluminum member for the slip resistance test and the aluminum member for the corrosion resistance test. In the aluminum member after the mirror polishing step and the surface hydroxylation step, as shown in Fig. 11, Ry was 0.5 µm, Rz was 0.25 µm, and the ratio of Ry to Rz was 2. Thereafter, the fastening step (S14) was performed under the same conditions as in Example 1 on the aluminum member for the slip resistance test to form a fastening unit.

[0154] [Example 12] In Example 12, the aluminum members were reacted with saturated water vapor for 4 hours in the surface hydroxylation step of the formation step (S12). The other conditions were the same as those in Example 11. As a result of reacting each aluminum member with saturated water vapor as described above for the aluminum members after the mirror polishing step and the surface hydroxylation step, as shown in FIG. 11, Ry was 0.9 μm, Rz was 0.5 μm, and the ratio of Ry to Rz was 1.8.

[0155] [Example 13] In Example 13, the aluminum member was reacted with saturated water vapor for 24 hours in the surface hydroxylation step of the formation step (S12). The other conditions were the same as those in Example 11. As shown in Fig. 11, the aluminum member after the mirror polishing step and the surface hydroxylation step had Ry of 1.4 µm, Rz of 0.9 µm, and the ratio of Ry to Rz of 1.5.

[0156] [Example 14] In Example 14, a first target member and a second target member with a resin film thickness of 20 μm were prepared in the preparation step (S10). Unlike Example 11, a gravity-type blasting device was used to perform a blasting process in the formation step (S12) instead of the mirror polishing process. For the blasting process, alumina with acute-angled protrusions and abrasives with a central particle diameter of 106 μm to 125 μm were used. The blasting pressure was 0.3 MPa. In FIG. 11, the above-mentioned blasting conditions are represented as "blasting (A)". Next, a surface hydroxylation process was performed under the same conditions as in Example 1 in the formation step (S12) for the blasted aluminum members for the sliding resistance test and the aluminum members for the corrosion resistance test. The other conditions were the same as in Example 11. As shown in FIG. 11, in the aluminum member after the blast processing step and the surface hydroxylation step, Ry was 17.7 μm, Rz was 12.5 μm, and the ratio of Ry to Rz was 1.4.

[0157] [Example 15] In Example 15, a first target member and a second target member with a resin film thickness of 50 μm were prepared in the preparation step (S10). Unlike Example 11, a blasting process was performed in the formation step (S12) using a direct pressure blasting device shown in FIG. 4 to FIG. 6 instead of the mirror polishing process. For the blasting process, alumina with acute protrusions and abrasives with a central particle diameter of 420 μm to 590 μm were used. The blasting pressure was 0.3 MPa. In FIG. 11, the above-mentioned blasting conditions are represented as "blasting (B)". Next, a surface hydroxylation process was performed in the formation step (S12) under the same conditions as in Example 1 for the blasted aluminum members for the sliding resistance test and the aluminum members for the corrosion resistance test. The other conditions were the same as in Example 11. As shown in FIG. 11, in the aluminum member after the blast processing step and the surface hydroxylation step, Ry was 45.0 μm, Rz was 43.3 μm, and the ratio of Ry to Rz was 1.0.

[0158] [Comparative Example 6] In Comparative Example 6, the aluminum member was reacted with saturated water vapor for 0.25 hours in the surface hydroxylation step of the formation step (S12). The other conditions were the same as those in Example 11. As shown in FIG. 11, the aluminum member after the mirror polishing step and the surface hydroxylation step had Ry of 0.2 μm, Rz of 0.1 μm, and the ratio of Ry to Rz of 2.

[0159] [Comparative Example 7] In Comparative Example 7, the blasting pressure was 0.5 MPa in the blasting process of the forming step (S12). The other conditions were the same as those in Example 15. As shown in Fig. 11, in the aluminum member after the blasting process and the surface hydroxylation process, Ry was 71.5 µm, Rz was 55.0 µm, and the ratio of Ry to Rz was 1.3.

[0160] [Comparative Example 8] In Comparative Example 8, the blasting pressure was 1.0 MPa in the blasting process of the forming step (S12). The other conditions were the same as those in Example 15. As shown in Fig. 11, in the aluminum member after the blasting process and the surface hydroxylation process, Ry was 94.5 µm, Rz was 45.0 µm, and the ratio of Ry to Rz was 2.1.

[0161] [Composition and crystal structure analysis of the intermediate layer] The diffracted X-ray intensity at each diffraction angle was measured by XRD for the aluminum members before and after the surface hydroxylation step in Examples 11 to 15 and Comparative Examples 6 to 8. The composition and crystal structure of the surface layer (intermediate layer) of the aluminum member were confirmed based on the peak characteristics shown in the measurement results of the diffracted X-ray intensity versus diffraction angle. The XRD measurement results confirmed that the surface layers of the aluminum members before the surface hydroxylation step in Examples 11 to 15 and Comparative Examples 6 to 8 did not contain amorphous substances containing aluminum atoms and oxygen atoms, and layered double hydroxides containing aluminum atoms and oxygen atoms.

[0162] From the XRD measurement results, it was confirmed that the intermediate layer of the aluminum member after the surface hydroxylation process in Examples 13 to 15 and Comparative Examples 7 and 8 contained an amorphous substance containing aluminum atoms and oxygen atoms and a layered double hydroxide containing aluminum atoms and oxygen atoms, as shown by "A" in FIG. 11. From the XRD measurement results, it was confirmed that the intermediate layer of the aluminum member after the surface hydroxylation process in Examples 11 and 12 did not contain a layered double hydroxide containing aluminum atoms and oxygen atoms, as shown by "B" in FIG. 11, but contained an amorphous substance containing aluminum atoms and oxygen atoms. From the XRD measurement results, it was confirmed that the surface layer of the aluminum member after the surface hydroxylation process in Comparative Example 6 did not contain an amorphous substance containing aluminum atoms and oxygen atoms, and a layered double hydroxide containing aluminum atoms and oxygen atoms, as shown by "C" in FIG. 11.

[0163] [Friction force evaluation] The slip resistance was measured as the friction force in the fastening units of Examples 11 to 15 and Comparative Examples 6 to 8 produced under the above conditions. The measurement method and the evaluation values ​​in Fig. 11 were the same as those described above and those in Fig. 10.

[0164] By comparing Examples 11 to 13 with Comparative Example 6, it was confirmed that the sliding resistance is significantly improved when the reaction time of the surface hydroxylation step in the formation step (S12) is 2 hours or more. When the reaction time of the surface hydroxylation step is 2 hours or more, the maximum height Ry and the ten-point average roughness Rz of the aluminum member are higher than when the reaction time of the surface hydroxylation step is 0.25 hours or more. Therefore, when the reaction time of the surface hydroxylation step is 2 hours or more, the reaction is sufficient compared to when the reaction time of the surface hydroxylation step is 0.25 hours or more, the developed interface area ratio Sdr of the contour curved surface is 20% or more, and the first unevenness is formed on the surface of the aluminum member in the contact layer. For this reason, it is considered that a change in the sliding resistance (friction force) generated by the aluminum member is observed before and after the reaction.

[0165] By comparing Example 6 with Example 11, and Example 1 with Example 13, it was shown that the maximum height Ry and ten-point average roughness, which indicate the surface roughness of the aluminum member, are reduced by performing the mirror polishing process. In the mirror polishing process, the surface is smoothed by performing buff polishing, so the number of irregularities on the surface of the aluminum member before the forming process (S12) is performed is reduced. In addition, by performing the mirror polishing process, scratches formed on the surface of the aluminum member before performing the surface hydroxylation process, and deposits attached to the surface of the aluminum member before performing the surface hydroxylation process are scraped off. For this reason, it is considered that the surface roughness of the surface of the aluminum member on which the mirror polishing process was performed is reduced. From this, the aluminum members according to Examples 11 and 13 have smaller maximum height Ry and ten-point average roughness Rz than the aluminum members according to Examples 6 and 1, respectively, so that it is considered that even when fastened to a target member having a thin resin film, the first irregularities on the surface of the aluminum member do not break through the resin film. For this reason, the aluminum members of the examples can appropriately ensure high frictional properties for various target members.

[0166] Comparison is made between Example 1, Example 13, Example 14, and Example 15. When the blasting process is performed, the maximum height Ry and the ten-point mean roughness indicating the surface roughness of the aluminum member are significantly larger than when the blasting process is not performed and when the mirror polishing process is performed instead of the blasting process, and the developed interface area ratio Sdr of the contour curved surface is 140% or more. It is considered that the second micro-order irregularities are formed on the surface in the blasting process, and the surface roughness of the aluminum member before the surface hydroxylation process is increased. For this reason, it is shown that the blasting process and the surface hydroxylation process can form irregularities of appropriate thickness including the first irregularities and the second irregularities on the aluminum member depending on the thickness of the resin film of the target member.

[0167] By comparing Example 15 with Comparative Examples 7 and 8, it was confirmed that the slip resistance is significantly improved when both the maximum height Ry and the ten-point mean roughness Rz are smaller than the thickness of the resin film of the target member. It is considered that when both the maximum height Ry and the ten-point mean roughness Rz are smaller than the thickness of the resin film of the target member, gaps are less likely to occur between the aluminum member and the target member, adhesion is improved, and friction is more likely to occur.

[0168] [Corrosion resistance evaluation] The corrosion current density as corrosion resistance was measured for the aluminum members for corrosion resistance testing of Examples 11 to 15 and Comparative Examples 6 to 8, which were prepared under the above conditions. The measurement method and the evaluation values ​​in Fig. 11 were the same as those described above and those in Fig. 10.

[0169] By comparing Examples 11 to 13 with Comparative Example 6, it was confirmed that setting the reaction time of the surface hydroxylation step to 2 hours or more in the formation step (S12) contributes to improving corrosion resistance. When the reaction time of the surface hydroxylation step is 2 hours or more, a sufficient reaction takes place and an intermediate layer is formed on the surface of the aluminum member, compared with when the reaction time of the surface hydroxylation step is 0.25 hours or more, so it is considered that the corrosion current density is reduced and the corrosion resistance is improved. The corrosion current density of Example 11 is 1 / 140 of the corrosion current density of Comparative Example 1. It is considered that the formation of an intermediate layer having a passivation function on the second irregularities on the surface of the aluminum member in the surface hydroxylation step leads to a reduction in the current density on the surface of the aluminum member, resulting in high (very improved) corrosion resistance.

[0170] As described above, it has been confirmed that the aluminum members of Examples 11 to 15 manufactured by the fastening method MT and the manufacturing method for an aluminum member described in the above embodiment exhibit both high friction properties and high corrosion resistance when fastened to the target member 4, compared to the aluminum members of Comparative Examples 6 to 8. [Explanation of symbols]

[0171] 1, 1A, 1B...fastening unit, 2, 2B...aluminum member, 2b...surface, 2d...second irregularity, 3, 3A...fastening member, 4, 4A...target member, 4b...contact surface, 5, 5B...main body, 6...intermediate layer, 7...contact layer, 7a...first irregularity, 8...resin film, 9...target main body, 10...blasting device, 31...first fastening member (an example of a fastening member), 32...second fastening member (an example of a fastening member), 41...first target member (an example of a target member), 42...second target member (an example of a target member), MT...fastening method.

Claims

1. A preparation step of preparing a target member having a resin film on a surface thereof and an aluminum member; a forming step of forming an intermediate layer on a surface of the aluminum member, and a contact layer disposed on the intermediate layer and having projections and recesses capable of coming into contact with the target member; a fastening process of fastening the aluminum member and the target member while penetrating the unevenness of the aluminum member into the resin film of the target member; Including, the intermediate layer comprises an amorphous material containing aluminum atoms and oxygen atoms, or both the amorphous material and a layered double hydroxide containing aluminum atoms and oxygen atoms; the contact layer comprises aluminum hydroxide; The projections and recesses have a length smaller than the thickness of the resin film of the target member. Fastening method.

2. 2. The fastening method according to claim 1, wherein the forming step includes a surface hydroxylation step of reacting a surface of the aluminum member with saturated water vapor under a pressure higher than atmospheric pressure and not higher than 4.30 MPa to modify the surface of the aluminum member into aluminum hydroxide, thereby forming the intermediate layer and the contact layer.

3. 3. The fastening method according to claim 2, wherein the surface hydroxylation step comprises reacting the surface of the aluminum member with saturated water vapor by applying heat of 100° C. or more and 250° C. or less.

4. 4. The fastening method according to claim 2, wherein the surface hydroxylation step comprises reacting the surface of the aluminum member with saturated water vapor for a treatment time of 30 minutes to 48 hours.

5. The fastening method according to any one of claims 1 to 3, wherein at least one of a maximum height and a ten-point average roughness defined in JIS-B0601:1994 on a surface of the aluminum member on which the unevenness is formed in the forming step is 0.5 µm or more.

6. The fastening method according to any one of claims 1 to 3, wherein, on a surface of the aluminum member on which the irregularities are formed in the forming step, a ratio of a maximum height defined in JIS-B0601:1994 to a ten-point average roughness defined in JIS-B0601:1994 is 1.0 or more and 2.0 or less.

7. The fastening method according to any one of claims 1 to 3, wherein a developed interface area ratio of a contour curved surface defined in JIS-B0681-2:2018 on a surface of the aluminum member on which the unevenness is formed in the forming step is 10% or more.

8. The fastening method according to any one of claims 1 to 3, wherein the thickness of the resin film on the target member is 5 µm or more and 50 µm or less.

9. A method for manufacturing an aluminum component to be fastened to a target component having a resin film on its surface, comprising the steps of: The method includes a forming step of forming an intermediate layer on a surface of the aluminum member, and a contact layer disposed on the intermediate layer and having projections and recesses capable of coming into contact with the target member, the intermediate layer comprises an amorphous material containing aluminum atoms and oxygen atoms, or both the amorphous material and a layered double hydroxide containing aluminum atoms and oxygen atoms, the contact layer comprises aluminum hydroxide, The projections and recesses have a length smaller than the thickness of the resin film of the target member. A method for manufacturing an aluminum component.

10. The method for producing an aluminum member according to claim 9, wherein the formation step includes a surface hydroxylation step of reacting a surface of the aluminum member with saturated water vapor under a pressure higher than atmospheric pressure and not higher than 4.30 MPa to modify the surface of the aluminum member into aluminum hydroxide and form the intermediate layer and the contact layer.

11. The method for producing an aluminum member according to claim 10, wherein the surface hydroxylation step comprises reacting the surface of the aluminum member with saturated water vapor by applying heat at a temperature of 100°C or higher and 250°C or lower.

12. The method for producing an aluminum member according to claim 10 or 11, wherein the surface hydroxylation step comprises reacting the surface of the aluminum member with saturated water vapor for a treatment time of 30 minutes or more and 48 hours or less.

13. The method for manufacturing an aluminum member according to any one of claims 9 to 11, wherein at least one of a maximum height and a ten-point average roughness defined in JIS-B0601:1994 on the surface of the aluminum member on which the unevenness is formed in the forming step is 0.5 μm or more.

14. The method for manufacturing an aluminum member according to any one of claims 9 to 11, wherein, on the surface of the aluminum member on which the unevenness is formed in the forming step, a ratio of a maximum height defined in JIS-B0601:1994 to a ten-point average roughness defined in JIS-B0601:1994 is 1.0 or more and 2.0 or less.

15. The method for manufacturing an aluminum member according to any one of claims 9 to 11, wherein the surface of the aluminum member on which the unevenness is formed in the forming step has a developed interface area ratio of a contour curved surface defined in JIS-B0681-2:2018 of 10% or more.

16. An aluminum member to be fastened to a target member having a resin film on its surface, An intermediate layer formed on the surface; a contact layer disposed on the intermediate layer and having a first projection and recess capable of coming into contact with the target member; Equipped with the intermediate layer comprises an amorphous material containing aluminum atoms and oxygen atoms, or both the amorphous material and a layered double hydroxide containing aluminum atoms and oxygen atoms, the contact layer comprises aluminum hydroxide, The first irregularities have a protruding length smaller than a thickness of the resin film of the target member. Aluminum components.

17. The aluminum member according to claim 16, wherein at least one of the maximum height and the ten-point average roughness defined in JIS-B0601:1994 on the surface of the aluminum member on which the first irregularities are formed is 0.5 μm or more.

18. The aluminum member according to claim 16 or 17, wherein the ratio of the maximum height defined in JIS-B0601:1994 to the ten-point average roughness defined in JIS-B0601:1994 on the surface of the aluminum member on which the first irregularities are formed is 1.0 or more and 2.0 or less.

19. The aluminum member according to claim 16 or 17, wherein the surface of the aluminum member on which the first irregularities are formed has a developed interface area ratio of a contour curved surface defined in JIS-B0681-2:2018 of 10% or more.

20. The aluminum member further includes a second unevenness of a micro order formed on the surface thereof, The aluminum member according to claim 16 or 17, wherein the first irregularity is formed on a surface of the second irregularity.

21. The aluminum member according to claim 16 or 17, wherein the corrosion current density of the aluminum member is 1 / 130 or less of the corrosion current density of an aluminum material not having the intermediate layer and the contact layer.

Citation Information

Patent Citations

  • Tubular joint with wedge-shaped threads having a surface coating

    JP2013507588A