Colloidal silica and method for manufacturing the same
By employing organopolysiloxane dispersants with acid anhydride structures and sol-gel silica treated with trifunctional silanes, the viscosity issues of colloidal silica in semiconductor polishing are addressed, ensuring effective long-term use as a polishing abrasive.
Patent Information
- Application Number
- JP2023085592
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-24
- Publication Date
- 2024-12-05
AI Technical Summary
Colloidal silica used in semiconductor polishing processes experiences increased viscosity at high concentrations and over time, leading to reduced effectiveness as an abrasive, and existing methods to improve dispersibility introduce additional issues like metal impurity contamination or pH-related aggregation.
The use of an organopolysiloxane with an acid anhydride structure or a hydrolyzed acid anhydride group as a dispersant, combined with sol-gel silica particles treated with a trifunctional silane compound, to maintain low viscosity even at high concentrations and over long periods, without surface treatment.
The colloidal silica maintains low viscosity at high concentrations and shows minimal increase over time, making it effective as a polishing abrasive for semiconductor devices, particularly in CMP processes.
Smart Images

Figure 2024168700000001 
Figure 2024168700000002 
Figure 2024168700000003
Abstract
Description
[Technical field]
[0001] The present invention relates to colloidal silica and a method for producing the same. [Background technology]
[0002] With the remarkable miniaturization of semiconductor devices in recent years, colloidal silica, which has small silica particles, is used in processes such as silicon wafer polishing and chemical mechanical polishing (hereinafter referred to as "CMP") of semiconductor devices.
[0003] As colloidal silica for CMP process, high purity colloidal silica with very little metal impurities is required for the reason of preventing contamination of silicon wafers, etc. Patent Document 1 discloses a method for producing colloidal silica modified with a silane coupling agent having a cationic group, which has a low content of metal impurities. However, the presence of cationic groups on the silica surface may cause hydrogen bonds between the cationic groups and silanol groups, or the cationic groups may act as a condensation catalyst between silanol groups, causing aggregation of silica particles.
[0004] In addition, producing colloidal silica having a high silica concentration is preferable not only because it improves production efficiency but also because it improves storage and transportation efficiency and allows the blending of the abrasive used in polishing to be freely adjusted, thereby increasing the degree of freedom in blending. On the other hand, when colloidal silica is used in the CMP process, there is a problem that the viscosity of the colloidal silica increases when it is reused, and therefore the effectiveness of the colloidal silica as an abrasive cannot be fully demonstrated. Therefore, there is a demand for colloidal silica that is highly concentrated and has a small increase in viscosity over a long period of time.
[0005] Therefore, Patent Documents 2 and 3 disclose a method of adding an inorganic or organic acid dispersant, such as sulfuric acid, nitric acid, or citric acid, to colloidal silica in order to improve the dispersibility of high-concentration colloidal silica. By using these dispersants, it is possible to improve the dispersibility of colloidal silica while preventing the inclusion of metal impurities, but there are cases in which silica aggregates or viscosity increases due to changes in pH value during long-term storage.
[0006] Patent Document 4 discloses a method for producing a surface-treated water-dispersed colloidal silica that is free of metal impurities and dispersants, is highly concentrated, and shows little increase in viscosity over a long period of time, by treating a part of the surface of water-dispersed colloidal silica obtained by a sol-gel method in the presence of a hydrophilic organic solvent with a trifunctional silane compound or the like, and then replaces the dispersion medium with water. However, since this method requires surface treatment of the silica, a more convenient method has been desired. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] JP 2005-162533 A [Patent Document 2] Patent No. 5270344 [Patent Document 3] JP 2019-172558 A [Patent Document 4] JP 2023-5414 A Summary of the Invention [Problem to be solved by the invention]
[0008] Therefore, an object of the present invention is to provide a colloidal silica which has a low viscosity even at a high concentration and which is less susceptible to an increase in viscosity during long-term storage. [Means for solving the problem]
[0009] As a result of intensive research conducted by the present inventors in order to achieve the above-mentioned object, it was discovered that by using an organopolysiloxane having a group with an acid anhydride structure, a group having a structure obtained by hydrolysis of an acid anhydride, or both, as a dispersant, it is possible to obtain colloidal silica that has a low viscosity even at high concentrations and that is only slightly affected by an increase in viscosity during long-term storage, even without surface treatment of the silica, and thus completed the present invention.
[0010] That is, the present invention provides the following colloidal silica and method for producing colloidal silica. [1] Silica particles, A dispersant comprising an organopolysiloxane having a group having an acid anhydride structure, a group having a structure formed by hydrolysis of an acid anhydride, or both. and water Colloidal silica containing [2] The colloidal silica according to [1], wherein the silica particles are sol-gel silica particles that have been surface-treated with a trifunctional silane compound represented by the following formula (II): R 2 Si(OR 3 )3(II) (In the formula, R 2 represents a substituted or unsubstituted monovalent hydrocarbon group having 1 to 20 carbon atoms, R 3 each independently represents a monovalent hydrocarbon group having 1 to 6 carbon atoms. [3] The colloidal silica according to [1] or [2], wherein the Z-average particle size of the silica particles as measured by a dynamic light scattering method is 5 to 300 nm. [4] The colloidal silica according to any one of [1] to [3], wherein the dispersant is at least one selected from the group consisting of organopolysiloxanes represented by the following general formula (1) and organopolysiloxanes represented by the following general formula (2): [ka] (In the formula, R 4are independently a substituted or unsubstituted alkyl group having 1 to 4 carbon atoms or a group represented by the following formula (3) or the following formula (4), R 4 At least two of the groups are represented by the following formula (3) or (4), and k is an integer of 0 to 150. [ka] (In the formula, R 6 each independently represents a substituted or unsubstituted alkyl group having 1 to 4 carbon atoms; R 5 are independently a group represented by the following formula (3) or (4), m is an integer of 2 to 5, n is an integer of 0 to 3, and the sum of m and n is 4 or 5. The order of arrangement of the siloxane units is arbitrary. [ka] (In the formula, the wavy line represents a bond.) [5] The colloidal silica according to any one of [1] to [4], wherein the amount of the dispersant is 10 to 3,000 ppm by mass relative to the silica particles. [6] The colloidal silica according to any one of [1] to [5], having a metal impurity concentration of 0 to 1 ppm by mass. [7] The colloidal silica according to any one of [1] to [6], wherein the concentration of the hydrophilic organic solvent is 0 to 1 mass %. [8] The colloidal silica according to any one of [1] to [7], having a solid content concentration of 30 to 50 mass %. [9] Dynamic viscosity at 25℃ is 1 to 100mm 2 The colloidal silica according to any one of [1] to [8], wherein the total amount of the colloidal silica is 0.1 to 0.5 wt %.
[10] A chemical mechanical polishing liquid containing the colloidal silica according to any one of [1] to [9].
[11] The method for producing colloidal silica according to any one of [1] and [3] to [9], comprising the following steps (A1), (A3') and (A4'): Step (A1): A step of obtaining colloidal silica (A1) by hydrolyzing and condensing a tetrafunctional silane compound represented by the following formula (I), a partial hydrolysis condensate thereof, or a mixture thereof in a mixed liquid containing a hydrophilic organic solvent and water in the presence of a basic substance. Si(OR 1 )4(I) (In the formula, R 1 each independently represents a monovalent hydrocarbon group having 1 to 6 carbon atoms. Step (A3'): A step of adding a dispersant comprising an organopolysiloxane having a group having an acid anhydride structure, a group having a structure obtained by hydrolysis of an acid anhydride, or both, to the colloidal silica (A1) obtained in step (A1) to obtain a dispersant-containing colloidal silica (A3'). Step (A4'): A step of replacing the hydrophilic organic solvent in the dispersion medium of the dispersant-containing colloidal silica (A3') obtained in step (A3') with water.
[12] The method for producing colloidal silica according to any one of [2] to [9], comprising the following steps (A1), (A2), (A3) and (A4): Step (A1): A step of obtaining colloidal silica by hydrolyzing and condensing a tetrafunctional silane compound represented by the following formula (I), a partial hydrolysis condensate thereof, or a mixture thereof in a mixed liquid containing a hydrophilic organic solvent and water in the presence of a basic substance. Si(OR 1 )4(I) (In the formula, R 1 each independently represents a monovalent hydrocarbon group having 1 to 6 carbon atoms. Step (A2): A trifunctional silane compound represented by the following formula (II), a partial hydrolysis condensate thereof, or a mixture thereof is added to the colloidal silica (A1) obtained in step (A1), and R is formed on the surface of the colloidal silica. 2 SiO 3 / 2 A step of introducing units to obtain surface-treated colloidal silica (A2) R 2 Si(OR 3 )3(II) (In the formula, R 2 represents a substituted or unsubstituted monovalent hydrocarbon group having 1 to 20 carbon atoms, R3 each independently represents a monovalent hydrocarbon group having 1 to 6 carbon atoms. Step (A3): A step of adding a dispersant comprising an organopolysiloxane having a group having an acid anhydride structure, a group having a structure obtained by hydrolysis of an acid anhydride, or both, to the surface-treated colloidal silica (A2) obtained in step (A2) to obtain a dispersant-containing surface-treated colloidal silica (A3). Step (A4): A step of replacing the hydrophilic organic solvent in the dispersion medium of the dispersant-containing surface-treated colloidal silica (A3) obtained in step (A3) with water.
[13] The method for producing colloidal silica according to
[12] , wherein in the step (A2), the trifunctional silane compound represented by the formula (II), its partial hydrolysis condensate, or a mixture thereof is added in an amount of 0.001 to 1 mol per 1 mol of SiO units in the colloidal silica (A1) obtained in the step (A1).
[14] The method for producing colloidal silica according to any one of
[11] to
[13] , wherein the dispersant is at least one selected from the group consisting of organopolysiloxanes represented by the following general formula (1) and organopolysiloxanes represented by the following general formula (2): [ka] (In the formula, R 4 are independently a substituted or unsubstituted alkyl group having 1 to 4 carbon atoms or a group represented by the following formula (3) or the following formula (4), R 4 At least two of the groups are represented by the following formula (3) or (4), and k is an integer of 0 to 150. [ka] (In the formula, R 6 each independently represents a substituted or unsubstituted alkyl group having 1 to 4 carbon atoms; R 5 are independently a group represented by the following formula (3) or (4), m is an integer of 2 to 5, n is an integer of 0 to 3, and the sum of m and n is 4 or 5. The order of arrangement of the siloxane units is arbitrary. [ka] (In the formula, the wavy line represents a bond.) Effect of the Invention
[0011] The colloidal silica of the present invention has a low viscosity even at high concentrations and shows little increase in viscosity during long-term storage, making it extremely useful as an abrasive for polishing silicon wafers, CMP processes for semiconductor devices, and the like. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] The present invention will be described in detail below. The colloidal silica of the present invention is A dispersant comprising an organopolysiloxane having a group having an acid anhydride structure, a group having a structure obtained by hydrolysis of an acid anhydride, or both, and water. It contains:
[0013] [Silica particles] The silica particles contained in the colloidal silica of the present invention are not particularly limited as long as they are silica dispersible in water, but sol-gel silica is preferred, and sol-gel silica particles surface-treated with a trifunctional silane compound represented by the following formula (II) are more preferred. R 2 Si(OR 3 )3(II) (In the formula, R 2 represents a substituted or unsubstituted monovalent hydrocarbon group having 1 to 20 carbon atoms, R 3 each independently represents a monovalent hydrocarbon group having 1 to 6 carbon atoms.
[0014] In the above formula (II), R 2 R is a monovalent hydrocarbon group having 1 to 20 carbon atoms, preferably 1 to 10 carbon atoms, and particularly preferably 1 to 3 carbon atoms. 2Examples of the monovalent hydrocarbon group represented by the formula (I) include alkyl groups such as methyl, ethyl, propyl, isopropyl, butyl, hexyl, octyl, and decyl, and particularly preferred are methyl, ethyl, and propyl. Some or all of the hydrogen atoms in these monovalent hydrocarbon groups may be substituted with halogen atoms such as fluorine, chlorine, and bromine, preferably fluorine atoms.
[0015] In the above formula (II), R 3 R is a monovalent hydrocarbon group having 1 to 6 carbon atoms, preferably having 1 to 4 carbon atoms, and particularly preferably having 1 or 2 carbon atoms. 3 Examples of the monovalent hydrocarbon group represented by the formula (I) include a methyl group, an ethyl group, a propyl group, a butyl group, and a phenyl group. Of these, a methyl group, an ethyl group, a propyl group, and a butyl group are preferred, and a methyl group and an ethyl group are particularly preferred.
[0016] Specific examples of the trifunctional silane compound represented by the above formula (II) include methyltrimethoxysilane, methyltriethoxysilane, ethyltrimethoxysilane, ethyltriethoxysilane, n-propyltrimethoxysilane, n-propyltriethoxysilane, i-propyltrimethoxysilane, i-propyltriethoxysilane, butyltrimethoxysilane, butyltriethoxysilane, hexyltrimethoxysilane, 3,3,3-trifluoropropyltrimethoxysilane, (heptadecafluoro-1,1,2,2-tetrahydrodecyl)trimethoxysilane, and the like.
[0017] The silica particles contained in the colloidal silica of the present invention preferably have a Z-average particle size of 5 to 300 nm, more preferably 10 to 150 nm, as measured by dynamic light scattering. The Z-average particle size as measured by dynamic light scattering can be measured, for example, using a Zetasizer Ultra (manufactured by Malvern Instruments).
[0018] [Dispersant] The colloidal silica of the present invention contains, as a dispersant, an organopolysiloxane having a group having an acid anhydride structure, a group having a structure formed by hydrolysis of an acid anhydride, or both.
[0019] Such organopolysiloxanes include linear, branched, cyclic and three-dimensional network organopolysiloxanes, and particularly preferred are organopolysiloxanes represented by the following general formula (1) and organopolysiloxanes represented by the following general formula (2).
[0020] [ka] (In the formula, R 4 are independently a substituted or unsubstituted alkyl group having 1 to 4 carbon atoms or a group represented by the following formula (3) or the following formula (4), R 4 At least two of the groups are represented by the following formula (3) or (4), and k is an integer of 0 to 150.
[0021] [ka] (In the formula, R 6 each independently represents a substituted or unsubstituted alkyl group having 1 to 4 carbon atoms; R 5 are independently a group represented by the following formula (3) or (4), m is an integer of 2 to 5, n is an integer of 0 to 3, and the sum of m and n is 4 or 5. The order of arrangement of the siloxane units is arbitrary.
[0022] [ka] (In the formula, the wavy line represents a bond.)
[0023] In the above formulas (3) and (4), R 4 and R 6Examples of the alkyl group having 1 to 4 carbon atoms include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, a sec-butyl group, a tert-butyl group, etc., and particularly preferred are a methyl group, an ethyl group, and an n-propyl group. In addition, some or all of the hydrogen atoms of these monovalent hydrocarbon groups may be substituted with halogen atoms such as fluorine atoms, chlorine atoms, and bromine atoms, preferably fluorine atoms.
[0024] In the above formula (1), k is an integer of 0 to 150, and preferably 1 to 30 from the viewpoints of viscosity and solubility in water.
[0025] In the above formula (2), m is an integer of 2 to 5, and preferably an integer of 2 to 4. n is an integer of 0 to 3, and preferably an integer of 0 to 2. m+n is 4 or 5, and preferably 4.
[0026] Specific examples of preferred dispersants include organopolysiloxanes represented by the following formulas and organopolysiloxanes in which the acid anhydride structure contained therein has been partially or completely hydrolyzed.
[0027] [ka]
[0028] [ka]
[0029] [ka]
[0030] [ka]
[0031] These organopolysiloxanes can be produced, for example, by the hydrosilylation reaction of an organohydrogenpolysiloxane with allylsuccinic anhydride under known hydrosilylation reaction conditions.
[0032] These dispersants may be used alone or in combination of two or more kinds.
[0033] In general, it is believed that as the concentration of silica particles in colloidal silica increases, the distance between silica particles decreases, hydrogen bonds are formed between the silanol groups between the silica particles, and the viscosity increases; however, it is believed that these dispersants act on the particles to block the hydrogen bonds between the silica particles, so that aggregation does not occur even when the silica concentration becomes high, and the increase in viscosity of the colloidal silica is suppressed.
[0034] The amount of the dispersant is preferably from 10 to 3000 ppm by mass, and more preferably from 500 to 2000 ppm by mass, relative to the silica particles.
[0035] [Dispersion medium] The colloidal silica of the present invention contains water as a dispersion medium.Other than water, the dispersion medium may contain a hydrophilic organic solvent, and the hydrophilic organic solvent may be, for example, alcohols such as methanol, ethanol, 1-propanol, 2-propanol, t-butanol, etc.; ethers such as tetrahydrofuran, dioxane, etc.; glycols such as diethylene glycol, dipropylene glycol, etc., and alcohols are preferred.
[0036] The concentration of the hydrophilic organic solvent in the colloidal silica of the present invention is preferably from 0 to 1 mass %, more preferably from 0 to 100 mass ppm, and particularly preferably from 0 to 10 mass ppm.
[0037] The total concentration of metal impurities such as sodium, potassium, iron, calcium, magnesium, titanium, nickel, chromium, and copper in the colloidal silica of the present invention is preferably 0 to 1 ppm by mass, and more preferably 0 to 0.5 ppm by mass, relative to the total mass of the colloidal silica.
[0038] The solids concentration (concentration of silica particles) of the colloidal silica of the present invention is preferably 30% by mass or more, and more preferably 30 to 50% by mass.
[0039] The kinematic viscosity of the colloidal silica of the present invention at 25° C. is 1 to 100 mm 2 / s is preferably 5 to 20 mm 2 Within this range, the powder is suitable for use as an abrasive.
[0040] The colloidal silica of the present invention may contain other components as long as they do not impair the dispersion stability of silica.For example, preservatives, bactericides, and biocides can be added to prevent bacterial growth, and examples of such compounds include hydrogen peroxide, ammonia, quaternary ammonium hydroxides, quaternary ammonium salts, ethylenediamine, glutaraldehyde, hydrogen peroxide, methyl p-hydroxybenzoate, 2-methyl-4-isothiazolin-3-one, 5-chloro-2-methyl-4-isothiazolin-3-one, isothiazoline compounds such as 1,2-benzoisothiazoline, and phenoxyethanol.
[0041] [Method of manufacturing colloidal silica] The colloidal silica of the present invention can be obtained by a production method including the following steps (A1), (A3') and (A4'). Step (A1): Synthesis step for obtaining colloidal silica Step (A3'): Addition of dispersant Step (A4'): Dispersion medium replacement step
[0042] The method for producing colloidal silica of the present invention preferably includes a production method having the following steps (A1), (A2), (A3), and (A4). Step (A1): Synthesis step for obtaining colloidal silica Step (A2): Surface treatment step using a trifunctional silane compound Step (A3): Addition of dispersant Step (A4): Dispersion medium replacement step
[0043] Step (A1): Synthesis step for obtaining colloidal silica This step is a step of obtaining colloidal silica (A1) by hydrolyzing and condensing a tetrafunctional silane compound represented by the following formula (I), a partial hydrolysis condensate thereof, or a mixture thereof in the presence of a basic substance in a mixed liquid containing a hydrophilic organic solvent and water. Si(OR 1 )4(I) (In the formula, R 1 each independently represents a monovalent hydrocarbon group having 1 to 6 carbon atoms.
[0044] In the above formula (I), R 1 R is a monovalent hydrocarbon group having 1 to 6 carbon atoms, preferably having 1 to 4 carbon atoms, and particularly preferably having 1 or 2 carbon atoms. 1 Examples of the monovalent hydrocarbon group represented by the formula (I) include a methyl group, an ethyl group, a propyl group, a butyl group, and a phenyl group. Of these, a methyl group, an ethyl group, a propyl group, and a butyl group are preferred, and a methyl group and an ethyl group are particularly preferred.
[0045] Examples of the tetrafunctional silane compound represented by the above formula (I) include tetraalkoxysilanes such as tetramethoxysilane, tetraethoxysilane, tetrapropoxysilane, and tetrabutoxysilane, and tetraphenoxysilane, and preferably tetramethoxysilane, tetraethoxysilane, tetrapropoxysilane, and tetrabutoxysilane, and particularly preferably tetramethoxysilane and tetraethoxysilane. Examples of the hydrolysis condensation product of the tetrafunctional silane compound represented by the above formula (I) include methyl silicate, ethyl silicate, and the like.
[0046] Examples of the basic substance include ammonia, dimethylamine, diethylamine, etc., and preferably ammonia and diethylamine, and particularly preferably ammonia. These basic substances can be used after dissolving the required amount in water.
[0047] The hydrophilic organic solvent is not particularly limited as long as it dissolves the compound represented by the above formula (I) and / or its partial hydrolysis condensate and water, and examples thereof include alcohols such as methanol, ethanol, 1-propanol, 2-propanol, t-butanol, etc.; ethers such as tetrahydrofuran, dioxane, etc.; glycols such as diethylene glycol, dipropylene glycol, etc., and alcohols are preferred. Since the particle size of the silica particles produced increases as the number of carbon atoms in the alcohol increases, the type of alcohol can be selected depending on the particle size of the desired silica particles.
[0048] The amount of water used in this step is preferably 0.5 to 5 moles, more preferably 0.6 to 2 moles, and particularly preferably 0.7 to 1 mole, per mole of the total of hydrocarbyloxy groups of the tetrafunctional silane compound represented by the above formula (I) and / or its partial hydrolysis condensate. When the above-mentioned basic substance is used by dissolving it in water, the water in which the basic substance is dissolved is also included in the "water" in this step. The ratio of the hydrophilic organic solvent to water is preferably 0.2 to 10, and more preferably 0.3 to 5, in terms of the affinity between the silica particles and the mixed solvent and ease of production. In terms of the size of the resulting silica particles, the amount of the basic substance is preferably 0.01 to 2 mol, and more preferably 0.03 to 0.5 mol, per 1 mol of the total of the hydrocarbyloxy groups of the tetrafunctional silane compound represented by the above formula (I) and / or its partial hydrolysis condensation product.
[0049] The reaction conditions for the hydrolysis and condensation in this step are preferably a reaction temperature of 20 to 120° C. and a reaction time of 1 to 8 hours, more preferably a reaction temperature of 20 to 100° C. and a reaction time of 1 to 6 hours.
[0050] The concentration of silica particles in the colloidal silica (A1) obtained in the step (A1) is preferably from 2 to 20 mass %, particularly preferably from 3 to 10 mass %.
[0051] Step (A2): Surface treatment step using a trifunctional silane compound This step is an optional step, in which a trifunctional silane compound represented by the following formula (II), a partial hydrolysis condensate thereof, or a mixture thereof is added to the colloidal silica (A1) obtained in step (A1), and R is formed on the surface of the colloidal silica. 2 SiO 3 / 2 This is a step of introducing the units to obtain surface-treated colloidal silica (A2). R 2 Si(OR 3 )3(II) (In the formula, R 2 represents a substituted or unsubstituted monovalent hydrocarbon group having 1 to 20 carbon atoms, R 3 each independently represents a monovalent hydrocarbon group having 1 to 6 carbon atoms.
[0052] In the above formula (II), R 2 R is a monovalent hydrocarbon group having 1 to 20 carbon atoms, preferably 1 to 10 carbon atoms, and particularly preferably 1 to 3 carbon atoms. 2Examples of the monovalent hydrocarbon group represented by the formula (I) include alkyl groups such as methyl, ethyl, propyl, isopropyl, butyl, hexyl, octyl, and decyl, and particularly preferred are methyl, ethyl, and propyl. Some or all of the hydrogen atoms in these monovalent hydrocarbon groups may be substituted with halogen atoms such as fluorine, chlorine, and bromine, preferably fluorine atoms.
[0053] In the above formula (II), R 3 R is a monovalent hydrocarbon group having 1 to 6 carbon atoms, preferably having 1 to 4 carbon atoms, and particularly preferably having 1 or 2 carbon atoms. 3 Examples of the monovalent hydrocarbon group represented by the formula (I) include a methyl group, an ethyl group, a propyl group, a butyl group, and a phenyl group. Of these, a methyl group, an ethyl group, a propyl group, and a butyl group are preferred, and a methyl group and an ethyl group are particularly preferred.
[0054] Specific examples of the trifunctional silane compound represented by the above formula (II) include methyltrimethoxysilane, methyltriethoxysilane, ethyltrimethoxysilane, ethyltriethoxysilane, n-propyltrimethoxysilane, n-propyltriethoxysilane, i-propyltrimethoxysilane, i-propyltriethoxysilane, butyltrimethoxysilane, butyltriethoxysilane, hexyltrimethoxysilane, 3,3,3-trifluoropropyltrimethoxysilane, (heptadecafluoro-1,1,2,2-tetrahydrodecyl)trimethoxysilane, and the like.
[0055] The amount of the trifunctional silane compound represented by the above formula (II) used is preferably 0.001 to 1 mol, more preferably 0.01 to 0.1 mol, and particularly preferably 0.01 to 0.05 mol, per mol of SiO units (Si atoms derived from the above formula (I)) in the colloidal silica obtained in step (A1).
[0056] In this step (A2), the trifunctional silane compound represented by the above formula (II) is added to the colloidal silica (A1) obtained in the step (A1), and a surface treatment reaction of the silica with the trifunctional silane compound is carried out under the following reaction conditions: The reaction conditions in this step (A2) are preferably a reaction temperature of 40 to 60°C and a reaction time of 1 to 10 hours, more preferably a reaction temperature of 50 to 60°C and a reaction time of 1 to 8 hours.
[0057] The surface-treated colloidal silica (A2) obtained in this step preferably has a Z-average particle size, as measured by dynamic light scattering, of 5 to 300 nm, more preferably 10 to 150 nm.
[0058] Step (A3') and Step (A3): Addition of Dispersant This step is a step of adding one or more dispersants selected from organopolysiloxanes having acid anhydride groups and organopolysiloxanes having groups obtained by hydrolyzing at least a portion of the acid anhydride groups to the colloidal silica (A1) obtained in step (A1) or the surface-treated colloidal silica (A2) obtained in step (A2).
[0059] Such organopolysiloxanes include linear, branched, cyclic and three-dimensional network organopolysiloxanes, and particularly preferred are organopolysiloxanes represented by the following general formula (1) and organopolysiloxanes represented by the following general formula (2).
[0060] [ka] (In the formula, R 4 are independently a substituted or unsubstituted alkyl group having 1 to 4 carbon atoms or a group represented by the following formula (3) or the following formula (4), R 4 At least two of the groups are represented by the following formula (3) or (4), and k is an integer of 0 to 150.
[0061] [ka] (In the formula, R6 each independently represents a substituted or unsubstituted alkyl group having 1 to 4 carbon atoms; R 5 are independently a group represented by the following formula (3) or (4), m is an integer of 2 to 5, n is an integer of 0 to 3, and the sum of m and n is 4 or 5. The order of arrangement of the siloxane units is arbitrary.
[0062] [ka] (In the formula, the wavy line represents a bond.)
[0063] In the above formulas (3) and (4), R 4 and R 6 Examples of the alkyl group having 1 to 4 carbon atoms include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, a sec-butyl group, a tert-butyl group, etc., and particularly preferred are a methyl group, an ethyl group, and an n-propyl group. In addition, some or all of the hydrogen atoms of these monovalent hydrocarbon groups may be substituted with halogen atoms such as fluorine atoms, chlorine atoms, and bromine atoms, preferably fluorine atoms.
[0064] In the above formula (1), k is an integer of 0 to 150, and preferably 1 to 30 from the viewpoints of viscosity and solubility in water.
[0065] In the above formula (2), m is an integer of 2 to 5, and preferably an integer of 2 to 4. n is an integer of 0 to 3, and preferably an integer of 0 to 2. Furthermore, the sum of m and n is 4 or 5, and preferably 4.
[0066] These dispersants may be used alone or in combination of two or more kinds.
[0067] The amount of the dispersant added is preferably from 10 to 3000 ppm by mass, and more preferably from 500 to 2000 ppm by mass, relative to the silica particles.
[0068] Step (A4') and Step (A4): Dispersion Medium Replacement Step This step is a step of replacing the hydrophilic organic solvent in the dispersion medium of the dispersant-containing colloidal silica (A3') obtained in step (A3') and the dispersant-containing surface-treated colloidal silica (A3) obtained in step (A3) with water. The hydrophilic organic solvent includes the hydrophilic organic solvent used in step (A1) and volatile by-products such as alcohol generated by condensation. As a replacement method, a heat concentration method in which the dispersant-containing colloidal silica (A3') obtained in step (A3') and the dispersant-containing surface-treated colloidal silica (A3) obtained in step (A3) are heated and concentrated while adding water in an amount equal to or greater than the amount of the distillate obtained by heating, or ultrafiltration using a filter can be used.
[0069] The amount of water added is preferably 0.5 to 4 times, more preferably 1.8 to 3.0 times by weight the total amount of the hydrophilic organic solvent used and the alcohol produced, from the viewpoint of the stability of colloidal silica. Furthermore, when the dispersion medium replacement step is carried out by a heat concentration method, the amount of the hydrophilic organic solvent to be distilled off may be adjusted, the amount of water to be added in the dispersion medium replacement step may be appropriately adjusted, or water may be added after the dispersion medium replacement step, so that the finally obtained colloidal silica satisfies the above-mentioned desired solid content concentration (concentration of silica particles) or kinetic viscosity. EXAMPLES
[0070] The present invention will be specifically described below using examples and comparative examples. Note that the following examples do not limit the present invention in any way. The colloidal silica obtained in each example and comparative example was evaluated as follows, and the results are shown in Tables 1 and 2.
[0071] [Particle size (Z-average particle size) and polydispersity index (PDI) measured by dynamic light scattering] Colloidal silica was diluted with ion-exchanged water to a silica particle concentration of 0.1% by mass, and the particle size distribution after irradiating with ultrasound for 10 minutes was measured using a Zetasizer Ultra (Malvern Panalytical). The Z-average particle size and PDI were calculated using dynamic light scattering. A PDI value of 0.1 or less indicates high monodispersity.
[0072] [Solid content concentration] 1.5 g of colloidal silica was precisely weighed and placed in an aluminum petri dish, and dried at 105°C for 3 hours. The residue (X) g was precisely weighed and the silica solids concentration was calculated using the following formula. Silica solid concentration (mass%) = (X / 1.5) x 100
[0073] [Measurement of remaining methanol amount] The amount of remaining methanol in the water-dispersed colloidal silica was measured by analyzing the gas phase of the vial while heating it at 60°C for 30 minutes using a headspace gas chromatography measuring device (HP6890 Series GC system, 5975 Mass Selective Detector, G1888 Network headspace Sampler, all manufactured by Agilent Technologies, Inc.).
[0074] [Measurement of metal impurity amount] Metal elements were measured using an ICP optical emission spectrometer (Agilent 5110 ICP-OES, manufactured by Agilent Technologies, Inc.), and the amount of metal impurities in the water-dispersed colloidal silica was calculated.
[0075] [Kinematic viscosity] The kinetic viscosity of the colloidal silica at 25°C was measured using a Cannon-Fenske viscometer. In addition, 80 g of colloidal silica was placed in a 100 ml polyethylene bottle, which was then sealed and stored at 60° C., and the kinetic viscosity at 25° C. was measured after 14 days, 30 days, and 60 days.
[0076] [Example 1] ·Process (A1) In a 3-liter glass reactor equipped with a stirrer, a dropping funnel and a thermometer, 793.0 g of methanol, 32.1 g of ion-exchanged water and 40.6 g of 28% aqueous ammonia were mixed. The solution was adjusted to 46°C, and while stirring, 646.5 g of tetramethoxysilane and 160.9 g of 5.5% aqueous ammonia were simultaneously added dropwise, the former over 6 hours and the latter over 4 hours. After the dropwise addition of tetramethoxysilane was completed, stirring was continued for another 0.5 hours to carry out hydrolysis and condensation, thereby obtaining colloidal silica (A1). The concentration of silica particles in this colloidal silica (A1) was 15.5% by mass.
[0077] ·Process (A2): To the colloidal silica (A1) obtained in the above step (A1), 5.8 g of methyltrimethoxysilane (0.01 mole equivalent to 1 mole of SiO units in the colloidal silica) was added at 25° C., and the mixture was stirred at 55° C. for 1 hour to obtain a surface-treated colloidal silica (A2). ·Process (A3): To the surface-treated colloidal silica (A2) obtained in the above step (A2), 0.46 g (1,800 mass ppm relative to the silica) of an organopolysiloxane represented by the following formula (1a) was added with stirring at 25° C., to obtain a dispersant-containing surface-treated colloidal silica (A3).
[0078] [ka]
[0079] ·Process (A4): 840 g of ion-exchanged water was added to the dispersant-containing surface-treated colloidal silica (A3) obtained in the step (A3) at 25° C., and then methanol was distilled off so that the solid content became 35 mass % or more, thereby obtaining 662 g of colloidal silica (i).
[0080] [Example 2] In the step (A2) of Example 1, the amount of methyltrimethoxysilane added was changed to 28.9 g (equivalent to 0.05 moles per mole of SiO units of the colloidal silica), and in the step (A3) of Example 1, the amount of organopolysiloxane represented by the above formula (1a) added was changed to 0.15 g (600 mass ppm relative to silica), except that, in the same manner as in Example 1, 689 g of colloidal silica (ii) was obtained.
[0081] [Example 3] 700 g of colloidal silica (iii) was obtained in the same manner as in Example 1, except that in step (A2) of Example 1, methyltrimethoxysilane was changed to 6.9 g of propyltrimethoxysilane (equivalent to 0.01 mole per mole of SiO units of the colloidal silica), and in step (A3) of Example 1, the organopolysiloxane represented by the above formula (1a) was changed to 0.46 g of organopolysiloxane represented by the following formula (2a) (1800 mass ppm relative to silica).
[0082] [ka]
[0083] [Example 4] Colloidal silica (iv) 705 g was obtained in the same manner as in Example 1, except that in step (A2) of Example 1, methyltrimethoxysilane was changed to 9.2 g of 3,3,3-trifluoropropyltrimethoxysilane (equivalent to 0.01 mole per mole of SiO units of the colloidal silica), and in step (A3) of Example 1, the organopolysiloxane represented by the above formula (1a) was changed to 0.46 g of organopolysiloxane represented by the following formula (2b) (1800 mass ppm relative to silica). [ka]
[0084] [Example 5] In the step (A1) of Example 1, the reaction temperature was changed to 38° C., and in the step (A3) of Example 1, the amount of the organopolysiloxane represented by the above formula (1a) added was changed to 0.15 g, and 0.05 g of the organopolysiloxane represented by the above formula (2a) was further added (a total of 800 ppm by mass relative to the silica), and the same procedure as in Example 1 was repeated to obtain 660 g of colloidal silica (v).
[0085] [Example 6] Colloidal silica (vi) 690 g was obtained in the same manner as in Example 1, except that in the step (A1) of Example 1, the reaction temperature was changed to 30° C., and in the step (A3) of Example 1, the organopolysiloxane represented by the above formula (1a) was changed to 0.51 g (2000 ppm by mass relative to silica) of an organopolysiloxane represented by the following formula (2a):
[0086] [Example 7] Colloidal silica (vii) 690 g was obtained in the same manner as in Example 1, except that in the step (A1) of Example 1, the reaction temperature was changed to 20° C., and in the step (A3) of Example 1, the organopolysiloxane represented by the above formula (1a) was changed to 0.51 g (2000 ppm by mass relative to silica) of an organopolysiloxane represented by the following formula (1b):
[0087] [ka]
[0088] [Example 8] ·Process (A1) In a 3-liter glass reactor equipped with a stirrer, a dropping funnel, and a thermometer, 793.0 g of methanol, 32.1 g of ion-exchanged water, and 40.6 g of 28% aqueous ammonia were mixed. The solution was adjusted to 46°C, and while stirring, 646.5 g of tetramethoxysilane and 160.9 g of 5.5% aqueous ammonia were simultaneously added dropwise, the former over 6 hours and the latter over 4 hours. After the dropwise addition of tetramethoxysilane was completed, stirring was continued for another 0.5 hours to carry out hydrolysis and condensation, thereby obtaining colloidal silica (A1). The concentration of silica particles in this colloidal silica (A1) was 15.5% by mass.
[0089] ·Process (A3'): 0.46 g (1800 ppm by mass relative to silica) of the organopolysiloxane represented by the above formula (1a) was added to the colloidal silica (A1) obtained in the above step (A1) with stirring at 25° C. to obtain a dispersant-containing colloidal silica (A3′).
[0090] ·Process (A4'): 840 g of ion-exchanged water was added to the dispersant-containing surface-treated colloidal silica (A3') obtained in the above step (A3') at 25°C, and then methanol was distilled off so that the solid content was 35 mass% or more, thereby obtaining 662 g of colloidal silica (viii).
[0091] [Comparative Example 1] The same procedure as in Example 8 was carried out except that the step (A3') in Example 8 was not carried out, thereby obtaining 655 g of colloidal silica (ix).
[0092] [Comparative Example 2] Colloidal silica (x) 675 g was obtained in the same manner as in Example 8, except that in the step (A1) of Example 8, the reaction temperature was changed to 20° C. and the step (A3′) of Example 8 was not performed.
[0093] [Comparative Example 3] In step (A3') of Example 8, 690 g of colloidal silica (xi) was obtained in the same manner as in Example 8, except that the organopolysiloxane represented by the above formula (1a) was changed to 0.17 g of ammonium benzoate (600 mass ppm relative to silica).
[0094] [Comparative Example 4] Colloidal silica (xii) 695 g was obtained in the same manner as in Example 8, except that in step (A3') of Example 8, the organopolysiloxane represented by the above formula (1a) was changed to 0.09 g of citric acid (300 ppm by mass relative to silica).
[0095] [Comparative Example 5] Colloidal silica (xiii) 6 was prepared in the same manner as in Example 1, except that in step (A3) of Example 1, the organopolysiloxane represented by the above formula (1a) was replaced with 0.46 g (1800 ppm by mass relative to silica) of organopolysiloxane represented by the following formula (5). 77g was obtained.
[0096] [ka]
[0097] [Table 1]
[0098] [Table 2]
[0099] From the above results, it was found that the colloidal silica obtained by the production method of the present invention has a low viscosity even at a high concentration, and the increase in viscosity during long-term storage is small. [Industrial Applicability]
[0100] The colloidal silica of the present invention has a low viscosity even at a high concentration and shows little increase in viscosity during long-term storage, and therefore can be suitably used as abrasive grains in the polishing of silicon wafers, the CMP process of semiconductor devices, and the like.
Claims
1. Silica particles, A dispersant comprising an organopolysiloxane having a group having an acid anhydride structure, a group having a structure formed by hydrolysis of an acid anhydride, or both. and water Colloidal silica containing
2. 2. The colloidal silica according to claim 1, wherein the silica particles are sol-gel silica particles which have been surface-treated with a trifunctional silane compound represented by the following formula (II): R 2 Si (OR 3 ) 3 (II) (In the formula, R 2 represents a substituted or unsubstituted monovalent hydrocarbon group having 1 to 20 carbon atoms; R 3 each independently represents a monovalent hydrocarbon group having 1 to 6 carbon atoms.
3. 2. The colloidal silica according to claim 1, wherein the Z-average particle size of the silica particles as measured by a dynamic light scattering method is from 5 to 300 nm.
4. 2. The colloidal silica according to claim 1, wherein the dispersant is at least one selected from the group consisting of organopolysiloxanes represented by the following general formula (1) and organopolysiloxanes represented by the following general formula (2): 【Chemistry 1】 (In the formula, R 4 are independently a substituted or unsubstituted alkyl group having 1 to 4 carbon atoms or a group represented by the following formula (3) or (4), R 4 At least two of the groups are represented by the following formula (3) or (4). k is an integer of 0 to 150. 【Chemistry 2】 (In the formula, R 6 each independently represents a substituted or unsubstituted alkyl group having 1 to 4 carbon atoms; R 5 are independently a group represented by the following formula (3) or (4), m is an integer of 2 to 5, n is an integer of 0 to 3, and the sum of m and n is 4 or 5. The order of arrangement of the siloxane units is arbitrary. 【Chemistry 3】 (In the formula, the wavy line represents a bond.)
5. 2. The colloidal silica according to claim 1, wherein the amount of the dispersant is 10 to 3,000 ppm by mass based on the silica particles.
6. 2. The colloidal silica according to claim 1, having a metal impurity concentration of 0 to 1 ppm by mass.
7. 2. The colloidal silica according to claim 1, wherein the concentration of the hydrophilic organic solvent is 0 to 1% by mass.
8. 2. The colloidal silica according to claim 1, having a solids concentration of 30 to 50 mass%.
9. Kinematic viscosity at 25°C is 1 to 100 mm 2 2. The colloidal silica according to claim 1, wherein
10. A chemical mechanical polishing liquid containing the colloidal silica according to any one of claims 1 to 9.
11. 2. The method for producing colloidal silica according to claim 1, comprising the following steps (A1), (A3′) and (A4′): Step (A1): A step of obtaining colloidal silica (A1) by hydrolyzing and condensing a tetrafunctional silane compound represented by the following formula (I), a partial hydrolysis condensate thereof, or a mixture thereof in a mixed liquid containing a hydrophilic organic solvent and water in the presence of a basic substance: Si(OR 1 ) 4 (I) (In the formula, R 1 each independently represents a monovalent hydrocarbon group having 1 to 6 carbon atoms. Step (A3'): A step of adding a dispersant comprising an organopolysiloxane having a group having an acid anhydride structure, a group having a structure obtained by hydrolysis of an acid anhydride, or both, to the colloidal silica (A1) obtained in step (A1) to obtain a dispersant-containing colloidal silica (A3'). Step (A4'): A step of replacing the hydrophilic organic solvent in the dispersion medium of the dispersant-containing colloidal silica (A3') obtained in step (A3') with water.
12. 3. A method for producing colloidal silica according to claim 2, comprising the following steps (A1), (A2), (A3) and (A4): Step (A1): A step of obtaining colloidal silica by hydrolyzing and condensing a tetrafunctional silane compound represented by the following formula (I), a partial hydrolysis condensate thereof, or a mixture thereof in a mixed liquid containing a hydrophilic organic solvent and water in the presence of a basic substance: Si(OR 1 ) 4 (I) (In the formula, R 1 each independently represents a monovalent hydrocarbon group having 1 to 6 carbon atoms. Step (A2): A trifunctional silane compound represented by the following formula (II), a partial hydrolysis condensate thereof, or a mixture thereof is added to the colloidal silica (A1) obtained in step (A1), and R is formed on the surface of the colloidal silica. 2 SiO 3 / 2 A step of introducing a unit to obtain surface-treated colloidal silica (A2) R 2 Si (OR 3 ) 3 (II) (In the formula, R 2 represents a substituted or unsubstituted monovalent hydrocarbon group having 1 to 20 carbon atoms; R 3 each independently represents a monovalent hydrocarbon group having 1 to 6 carbon atoms. Step (A3): A step of adding a dispersant comprising an organopolysiloxane having a group having an acid anhydride structure, a group having a structure obtained by hydrolysis of an acid anhydride, or both, to the surface-treated colloidal silica (A2) obtained in step (A2) to obtain a dispersant-containing surface-treated colloidal silica (A3). Step (A4): A step of replacing the hydrophilic organic solvent in the dispersion medium of the dispersant-containing surface-treated colloidal silica (A3) obtained in step (A3) with water.
13. In step (A2), the amount of the trifunctional silane compound represented by formula (II), its partial hydrolysis condensate, or a mixture thereof added is such that the amount of SiO in the colloidal silica (A1) obtained in step (A1) is 2 The method for producing colloidal silica according to claim 11, wherein the amount is 0.001 to 1 mol per 1 mol of the unit.
14. The method for producing colloidal silica according to any one of claims 11 to 13, wherein the dispersant is at least one selected from the group consisting of organopolysiloxanes represented by the following general formula (1) and organopolysiloxanes represented by the following general formula (2): 【Chemistry 4】 (In the formula, R 4 are independently a substituted or unsubstituted alkyl group having 1 to 4 carbon atoms or a group represented by the following formula (3) or (4), R 4 At least two of the groups are represented by the following formula (3) or (4). k is an integer of 0 to 150. 【Chemistry 5】 (In the formula, R 6 each independently represents a substituted or unsubstituted alkyl group having 1 to 4 carbon atoms; R 5 are independently a group represented by the following formula (3) or (4), m is an integer of 2 to 5, n is an integer of 0 to 3, and the sum of m and n is 4 or 5. The order of arrangement of the siloxane units is arbitrary. 【Chemistry 6】 (In the formula, the wavy line represents a bond.)
Citation Information
Patent Citations
Method for producing silica sol, polishing method, method for producing semiconductor wafer and method for producing semiconductor device
JP2023043024A
Negative phase sequence filter
JP1977070344A
Method for producing modified colloidal silica
JP2005162533A
Method for producing silica sol
JP2019172558A
Method for producing water-dispersed surface-treated colloidal silica
JP2023005414A