Silica-based particle dispersion liquid for polishing, and method for producing the same
A silica-based particle dispersion with concave-shaped particles addresses the inefficiencies of existing polishing methods by achieving high polishing rates and smooth surfaces, using a controlled production process.
Patent Information
- Application Number
- JP2023085610
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-24
- Publication Date
- 2024-12-05
AI Technical Summary
Existing polishing compositions face challenges in achieving both high polishing rates and maintaining surface flatness and smoothness without scratches, with methods like using large abrasive grains or alkyl silicate-based particles being inefficient or economically unviable.
A silica-based particle dispersion with concave-shaped particles, characterized by specific particle size distribution and pore volume, is produced by controlled addition of acidic silicic acid and alkali halide to an alkali silicate solution, resulting in a high polishing rate and reduced waviness.
The dispersion achieves a high polishing rate while minimizing waviness and surface roughness, enhancing the smoothness of polished substrates.
Smart Images

Figure 2024168713000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a silica-based particle dispersion for polishing, which is suitable for a polishing slurry for polishing magnetic disk substrates or a polishing composition for polishing magnetic disk substrates, and to a method for producing the same. [Background technology]
[0002] Conventionally, silica sol, fumed silica, fumed alumina, etc. have been used as polishing particles. In the manufacture of semiconductor integrated circuit-attached substrates, aluminum wiring is formed on a silicon wafer, and an oxide film such as silica is provided thereon as an insulating film. In this case, unevenness is generated by the wiring, so this oxide film is polished to flatten it. In polishing such substrates, it is required that the surface after polishing is flat without steps or unevenness, smooth without microscopic scratches, etc., and a high polishing rate.
[0003] A method for obtaining a high polishing rate is generally to use abrasive grains of large size. However, if the particle size of the abrasive grains becomes too large, the flatness of the substrate surface after polishing tends to deteriorate. Therefore, it is known that it is effective to make the abrasive grains non-spherical, that is, to make the abrasive grains irregularly shaped particles (irregular particles), in order to obtain a high polishing rate without deteriorating the flatness of the surface. As a method for obtaining large irregularly shaped particles, as in Patent Document 1, a method is known in which porous silica gel is pulverized by a bead mill or the like to prepare an irregularly shaped porous gel, and the irregularly shaped porous gel is grown by silicic acid or the like to obtain irregularly shaped particles of large size and high irregularity.
[0004] Another method for achieving a high polishing rate is a method for producing silica particles in which at least four primary particles are clustered together, as described in Patent Document 2, by adding an alkali halide to an aqueous alkali silicate solution and an acidic silicic acid solution, setting the molar ratio of the alkali halide to silica to 0.01 to 0.5, heating and stirring the solution, and adding an acidic silicic acid solution while stirring at a Reynolds number in the range of 2000 to 1,000,000.
[0005] As yet another method for obtaining a high polishing rate, Patent Document 3 discloses a method in which a hydrolyzed liquid obtained by hydrolyzing an alkyl silicate is added to a liquid containing an alkali catalyst and water, and the pH of the mixed liquid is controlled to obtain non-spherical silica particles having a bent and / or branched structure, i.e., irregularly shaped silica particles. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2018-177576 A [Patent Document 2] Patent No. 6207345 [Patent Document 3] International Publication No. 2010 / 035613 Summary of the Invention [Problem to be solved by the invention]
[0007] However, the polishing composition described in Patent Document 1 has a high polishing rate, but when a high flatness is to be obtained on the substrate surface after polishing, it is necessary to prepare the particle size of the irregular particles smaller. When trying to reduce the particle size using the method of Patent Document 1, it is necessary to repeatedly grind the porous silica gel used as the raw material to further reduce the size. Although the size of the irregular porous gel can be reduced by repeatedly grinding, the irregularity of the irregular porous gel is also reduced at the same time. As a result, the irregularity of the irregular silica particles after particle growth using silicic acid or the like is also reduced, which causes a problem of a decrease in the polishing rate. In addition, in order to grind the irregular porous gel to a predetermined size, it is necessary to repeatedly grind it, which is inefficient and uneconomical.
[0008] In addition, although the silica particles described in Patent Document 2 have a higher polishing rate than spherical silica particles, a higher polishing rate is required for primary polishing of hard disks, and while achieving a higher polishing rate, it is also required to reduce the flatness of the surface of the polished substrate, such as waviness. That is, although the silica particles described in Patent Document 2 have a high polishing rate, there is a problem in that they cannot achieve both a high polishing rate and low waviness at the same time.
[0009] In addition, the colloidal silica described in Patent Document 3 is disclosed as particles having a bent structure and / or a branched structure, which are obtained by using a hydrolysis liquid obtained by hydrolyzing an alkyl silicate, but since the colloidal silica uses an alkyl silicate as a raw material, it is very expensive and very uneconomical, and therefore cannot be used for hard disks. Furthermore, when the authors actually carried out a reproduction experiment, although a bent or branched structure was obtained, there was also a problem that the polishing speed was significantly slower than that of irregular silica particles made from an alkali silicate, possibly due to the lack of hardness of the particles.
[0010] An object of the present invention is to provide a silica-based particle dispersion liquid for polishing, which, when used as a polishing slurry, can reduce waviness and increase the polishing rate, and a method for producing the same. [Means for solving the problem]
[0011] The present inventors have conducted extensive research to solve the above problems and have completed the present invention. The present invention relates to the following (1) to (4). (1) A dispersion of silica-based particles for polishing, comprising a particle group including depression-type silica-based particles having a depression toward the inside of the particle, which satisfies the following [1] to [5], dispersed in a solvent. [1] The average particle size (Dd) of the particle group as measured by dynamic light scattering is within the range of 40 to 300 nm. [2] In the weight-converted particle size distribution of the particle group, the cumulative 10% particle size from the smallest particle size (D 10 ), cumulative 90% particle diameter (D 90) and cumulative 50% particle size (D 50 ) satisfies the following formula: Formula: 1.6≦(D 90 -D 10 ) / D 50 <=5 [3] The particle group has a pore volume measured by a nitrogen adsorption method within a range of 0.1 to 0.35 ml / g. [4] In the electron microscope photograph or image, the dented silica-based particles have a particle outline that has a concave portion toward the inside of the particle, and when the maximum length L from a tangent M that touches two points on the particle outline that sandwich the concave portion to a line drawn perpendicularly to the tangent M to a point where the tangent M intersects with the particle outline, L is 3 nm or more. [5] The ratio (La / De) of La to the specific surface area converted particle diameter De of the particle group is 0.15 or more (where La represents the number average value of the length L of the depression type silica-based particles in the particle group). (2) The silica-based particle dispersion liquid for polishing according to the above (1), wherein the content of the dent-type silica-based particles in the particle group is 25 to 90 mass %. (3) The dispersion liquid of silica-based particles for polishing according to the above (1) or (2), wherein the average major axis / minor axis ratio of the dented silica-based particles is in the range of 1.34 to 5. (4) A method for producing a dispersion liquid of silica-based particles for polishing, comprising the following steps (a) to (c): Step (a): A step of adding and mixing an acidic silicic acid liquid and an alkali halide to an aqueous solution of alkali silicate, thereby preparing a precursor dispersion in which the ratio of the number of moles of silica (MTS) to the number of moles of alkali halide (MH), ((MTS) / (MH)), is 2 to 100 and the silica concentration is within the range of 10 to 18 mass%. Step (b): A step of holding the precursor dispersion at 50 to 95° C., and then continuously or intermittently adding the acidic silicic acid liquid while maintaining the same temperature range to prepare a seed particle dispersion. Step (c): A step of adding the acidic silicic acid liquid containing 2 to 100 times the molar number of SiO2 relative to the SiO2 contained in the seed particle dispersion liquid to the seed particle dispersion liquid to obtain a silica-based particle dispersion liquid. Effect of the Invention
[0012] For example, when the silica-based particle dispersion liquid for polishing of the present invention is used as a polishing slurry or a polishing composition for polishing a magnetic disk substrate, it shows a sufficient polishing speed and can also suppress the occurrence of "waviness" on the substrate to be polished. The present invention provides such a silica-based particle dispersion liquid for polishing, and further provides a method for producing the same. [Brief description of the drawings]
[0013] [Figure 1] FIG. 1 is a conceptual diagram of a photograph or image obtained by observing a dimple-type silica-based particle using an electron microscope (scanning electron microscope or the like). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] The present invention will now be described. The present invention provides a silica-based particle dispersion for polishing in which a particle group including depression-type silica-based particles having a portion depression toward the inside of the particle is dispersed in a solvent, and satisfies the following [1] to [5]. [1] The average particle size (Dd) of the particle group as measured by dynamic light scattering is within the range of 40 to 300 nm. [2] In the weight-converted particle size distribution of the particle group, the cumulative 10% particle size from the smallest particle size (D 10 ), cumulative 90% particle diameter (D 90 ) and cumulative 50% particle size (D 50 ) satisfies the following formula: Formula: 1.6≦(D 90 -D 10 ) / D 50 <=5 [3] The particle group has a pore volume measured by a nitrogen adsorption method within a range of 0.1 to 0.35 ml / g. [4] In the electron microscope photograph or image, the dented silica-based particles have a particle outline that has a concave portion toward the inside of the particle, and when the maximum length L from a tangent M that touches two points on the particle outline that sandwich the concave portion to a line drawn perpendicularly to the tangent M to a point where the tangent M intersects with the particle outline, L is 3 nm or more. [5] The ratio (La / De) of La to the specific surface area converted particle diameter De of the particle group is 0.15 or more (where La represents the number average value of the length L of the depression type silica-based particles in the particle group). Such a silica-based particle dispersion is hereinafter also referred to as the "dispersion of the present invention."
[0015] Moreover, the particle group contained in the dispersion liquid of the present invention will hereinafter be referred to as “particle group of the present invention.” In the present invention, the term “particle group” means an assembly of a large number of particles.
[0016] The present invention also provides a method for producing a silica particle dispersion liquid for polishing, comprising the following steps (a) to (c): Step (a): A step of adding and mixing an acidic silicic acid liquid and an alkali halide to an aqueous solution of alkali silicate, thereby preparing a precursor dispersion in which the ratio of the number of moles of silica (MTS) to the number of moles of alkali halide (MH), ((MTS) / (MH)), is 2 to 100 and the silica concentration is within the range of 10 to 18 mass%. Step (b): A step of holding the precursor dispersion at 50 to 95° C., and then continuously or intermittently adding the acidic silicic acid liquid while maintaining the same temperature range to prepare a seed particle dispersion. Step (c): A step of adding the acidic silicic acid liquid containing 2 to 100 times the molar number of SiO2 relative to the SiO2 contained in the seed particle dispersion liquid to the seed particle dispersion liquid to obtain a silica-based particle dispersion liquid. Such a production method will be hereinafter referred to as the "production method of the present invention."
[0017] The dispersion of the present invention is preferably produced by the production method of the present invention.
[0018] <Depression-type silica particles> The depression-type silica particles will now be described. The hollow silica-based particles have a hollow portion toward the inside of the particle.
[0019] The depression-type silica-based particles will be explained with reference to FIG. FIG. 1 is a conceptual diagram of a photograph or image obtained by observing a dimple-type silica-based particle using an electron microscope (scanning electron microscope or the like). As shown in Figure 1, in the part of the particle that is concave toward the inside, a tangent line M is drawn that touches two points (points A and B) on the particle contour, and a straight line is drawn perpendicular to the tangent line M from the tangent line M to the particle contour. The length of the straight line (the length from the tangent line M to the particle contour) is L. Particles for which L ≥ 3 nm are considered to be concave-type silica-based particles.
[0020] Potentially recessed silica-based particles include non-spherical particles, inter-particle type particles, plate-like particles, curved particles, elongated particles, and branched particles.
[0021] The fact that the pitted silica-based particles are made of silica can be confirmed, for example, by an ICP apparatus (inductively coupled plasma emission spectrometry apparatus). 1 g of an aqueous dispersion containing pitted silica-based particles is collected in a 30 ml zirconia bowl with a lid, dried (200°C, 20 minutes), and baked (700°C, 5 minutes), and then 2 g of Na2O2 and 1 g of NaOH are added and melted for 15 minutes. Furthermore, 50 ml of HCl and 200 ml of water are added to dissolve the mixture, and then the mixture is diluted with pure water to 500 ml to obtain a sample. The silicon content of the obtained sample can be measured using an ICP apparatus (Shimadzu Corporation, ICPS-8100, analysis software ICPS-8000). If the silicon content is 90 mass% or more, the particles are deemed to be made of silica.
[0022] When used as polishing particles, the recessed silica-based particles are difficult to roll due to their shape, so the coefficient of dynamic friction between the substrate and the abrasive grains is high, and the polishing speed is high. In addition, the recessed shape means irregular particles or linked type. Therefore, the contact area with the substrate is high, and the polishing speed is high. On the other hand, because the contact area between the substrate and the abrasive grains is high, the local stress concentration on the substrate is alleviated, that is, the polishing is performed with relatively dispersed stress, and the surface roughness and waviness of the substrate tend to improve. In addition, the dimpled silica particles of the present invention have a diameter of 1.6≦(D 90 -D 10 ) / D 50 ≦5. In other words, since the particle size distribution is wide, it also contains many small-sized particles. In addition, the content of the recessed silica-based particles is preferably 25 to 90% by mass, and in that case, in addition to the recessed type, it also contains many spherical and small-sized silica-based particles. Therefore, when the abrasive grains are pressed against the substrate by the polishing pad during polishing, and the abrasive grains are concentrated on the surface of the pad, that is, when the abrasive grains form a dense structure on the protruding parts of the pad, the recessed parts of the recessed silica-based particles contain small particles such as spherical particles, so that the polishing is performed while forming a structure in which the silica-based particles are packed with fewer voids between the polishing pad and the substrate. Therefore, the contact area between the polishing substrate and the abrasive grains is increased. In addition, it is considered that the rolling of the abrasive grains or the abrasive grains is suppressed when a structure in which the fine particles enter the recessed parts of the recessed particles or a structure of dense silica-based particle groups is formed due to the formation of the structure. It is estimated that such an effect results in a high contact area with the substrate and stress dispersion, which results in a high polishing rate and improved surface roughness and waviness of the substrate.
[0023] The depression-type silica-based particles constitute at least a part of the particle group of the present invention. The particle group of the present invention dispersed in a solvent constitutes the dispersion liquid of the present invention. When the dispersion of the present invention is used as an abrasive, it is possible to achieve a high removal rate while reducing the waviness and surface roughness of the substrate to be polished, that is, to make the surface smooth.
[0024] The particle group of the present invention is composed of silica, but may contain 10 mass % or less of components other than silica, such as Al, Ti, Fe, Ca, Mg, Cr, Ni, Cu, Zn, K, or Na, or oxides thereof. As described above, it can be confirmed that the particle group of the present invention is made of silica using, for example, an ICP apparatus. In addition, the content of components other than silica that the particle group of the present invention may contain can be specified and quantified, for example, using an inductively coupled plasma emission spectrometer. Note that, Ni, Cu, K and Na can be specified and quantified using an atomic absorption spectrophotometer.
[0025] The content of the dimpled silica particles in the particle group of the present invention will be described below. The silica-based particle dispersion is observed at a magnification of 200,000 times using an electron microscope (scanning electron microscope photograph, etc.), and an image is taken so that 200 or more particles are included in the same visual field, and the particles in the obtained photograph or image are confirmed as to whether or not they correspond to depression-type silica-based particles by the method described above using Figure 1. Specifically, 200 particles randomly selected within the same visual field are confirmed as to whether or not they correspond to depression-type silica-based particles, and the number ratio (content) of the particles that correspond to depression-type silica-based particles among the 200 particles is calculated.
[0026] The content of dimpled silica-based particles in the particle group calculated in this manner is preferably 25 to 90 mass %, more preferably 30 to 85 mass %, and most preferably 40 to 80 mass %. When the content of the dented silica-based particles in the particle group is within this range, when the dispersion of the present invention is used as polishing particles, the fine particles can easily enter the dented portions of the dented silica-based particles, and as a result, a high polishing rate can be achieved while mitigating waviness and surface roughness of the substrate surface, i.e., making it smooth. Among the 200 particles, the number average value of the length (L) of the particles corresponding to the dented silica-based particles is calculated, and this value is defined as the number average value La.
[0027] <Average particle diameter (Dd)> The average particle size (Dd) of the particle group of the present invention as measured by dynamic light scattering is preferably from 40 to 300 nm, more preferably from 80 to 250 nm, further preferably from 100 to 200 nm, and most preferably from 120 to 170 nm. When the average particle size (Dd) is in the range of 40 to 300 nm, when the dispersion liquid of the present invention is used as an abrasive, a high polishing rate can be obtained, and furthermore, the residue of abrasive grains on the object to be polished can be suppressed. In addition, the occurrence of scratches on the object to be polished can be suppressed, and waviness and surface roughness can also be suppressed, making the surface of the object to be polished smoother. If the average particle size (Dd) is too low, the polishing rate tends to be low when the dispersion of the present invention is used as an abrasive, whereas if the average particle size (Dd) is too high, waviness and surface roughness tend to worsen, and scratches tend to occur more easily.
[0028] The average particle size (Dd) of the particle group of the present invention means a value obtained by measurement using the dynamic light scattering method described below. Specifically, a silica particle dispersion with a silica concentration of 1% by mass was prepared and measured using a particle size distribution measuring device (Otsuka Electronics' "nanoSAQLA") Ammonia water with a concentration of 0.58% by mass was used as the dispersion medium.
[0029] <Weight-equivalent particle size distribution of particle groups> The particle size distribution by weight of the particle group of the present invention is the cumulative 10% particle size (D 10 ), cumulative 90% particle diameter (D 90 ) and cumulative 50% particle size (D 50 ) satisfies the following equation: Formula: 1.6≦(D 90 -D 10 ) / D 50 <=5
[0030] Here, (D 90 -D 10 ) / D 50The range of 1.6 to 5 is preferable. Weight-converted particle size distribution (D 90 -D 10 ) / D 50 The value of indicates the width of the particle size distribution, (D 90 -D 10 ) / D 50 The larger the value of D, the wider the particle size distribution. 90 -D 10 ) / D 50 When the value of is large, it means that the particle group of the present invention has both small and large particles. Since the particle group of the present invention includes both the large pitted silica-based particles and the fine particles that can enter the pitted parts, the fine particles enter the pitted parts of the pitted silica-based particles. Therefore, when the dispersion of the present invention is used as an abrasive, it tends to achieve a high polishing rate while reducing waviness and surface roughness. Furthermore, although large-diameter particles alone exhibit a high removal rate, they also tend to worsen waviness, but the presence of small particles together with them has the effect of repairing the worsened waviness. The particle group of the present invention exhibits such an effect since the weight-converted particle size distribution satisfies the above formula. Weight-equivalent particle size distribution of particle groups (D 90 -D 10 ) / D 50 If the value of (D) is less than 1.6, the polishing rate tends to be slow when the dispersion of the present invention is used as an abrasive. 90 -D 10 ) / D 50 If the value of exceeds 5, when the dispersion of the present invention is used as an abrasive, the distribution becomes too broad and the number of coarse particles increases, which tends to cause waviness and surface roughness of the polished surface to deteriorate. (D 90 -D 10 ) / D 50 The value is more preferably in the range of 1.6 to 4, and further preferably in the range of 1.6 to 3.0.
[0031] <Pore volume> The pore volume of the particle group of the present invention as measured by a nitrogen adsorption method is preferably in the range of 0.1 to 0.35 ml / g, and more preferably in the range of 0.1 to 0.3 ml / g. Here, the pore volume in the present invention is the pore volume of the dried powder obtained by drying the silica-based fine particle dispersion at 105°C as described later, and this indicates the density of the packing structure of the silica-based particle group formed on the polishing pad when the silica-based fine particles of the present invention are pressed against the substrate by the polishing pad during polishing. Therefore, when the pore volume is small, it is considered that a denser packing structure is formed on the polishing pad. That is, it is considered that a structure is formed in which the fine particles enter the depressions of the depression-type silica-based fine particles. When the pore volume is large, it is considered that the packing structure is sparse and the small particles are not sufficiently filled in the depressions of the depression particles. When the packing structure is dense, the contact area between the abrasive grains and the substrate increases, the polishing speed increases, stress is dispersed, and the surface roughness and waviness of the substrate tend to improve.
[0032] <Ratio (La / De)> In the particle group of the present invention, the ratio (La / De) of the average value La determined as above to the specific surface area converted particle diameter De of the particle group of the present invention is preferably 0.15 or more, more preferably 0.15 to 1.00, and even more preferably 0.2 to 0.8. As described above, in the present specification, L represents the absolute value of the depth of the recessed portion of the hollow silica-based particle, La represents its number average value, and the ratio (La / De) is an index of the ratio of the depth of the recessed portion to the particle size of the hollow silica-based particle. When the value of the ratio (La / De) is less than 0.15, the ratio of the depth of the recess to the particle size is small, so that microparticles are difficult to enter the recess, and the packing structure tends to be sparse. On the other hand, the ratio of the depth of the recess to the particle size is large in proportion to the increase in the value of the ratio (La / De), so that more microparticles can enter the recess, but the particle with a large ratio of the depth of such a recess tends to be large in size, and as a result, scratches are easily generated and the surface roughness and waviness of the substrate tend to deteriorate.
[0033] The specific surface area converted particle diameter De of the particle group of the present invention is a value converted from the specific surface area. Specific details will be described later.
[0034] <Average long axis / short axis ratio of hollow-type silica particles> The average major axis / minor axis ratio of the dented silica-based particles of the present invention is preferably in the range of 1.34 to 5.0. If the average major axis / minor axis ratio of the dented silica-based particles is in this range, a practically sufficient polishing rate can be obtained when the dispersion of the present invention is applied to polishing purposes. If the average major axis / minor axis ratio of the dented silica-based particles is less than 1.34, it is difficult to obtain a sufficient polishing rate. If the average major axis / minor axis ratio of the dented silica-based particles is more than 5.0, the polishing rate is improved, but scratches are more likely to be generated on the polished surface.
[0035] The method for measuring the average major axis / minor axis value of the dented silica particles of the present invention is as described below.
[0036] As described above, the dispersion of the present invention is obtained by dispersing the particle group of the present invention in a solvent. Examples of the solvent include water, alcohols such as methyl alcohol, ethyl alcohol, and isopropyl alcohol, and water-soluble organic solvents such as ethers, esters, and silicones. A mixed solvent consisting of water and an organic solvent may also be used.
[0037] The content of the particle group of the present invention contained in the dispersion of the present invention is preferably from 1 to 50% by mass, and more preferably from 10 to 50% by mass. Here, the content of the particle group of the present invention contained in the dispersion of the present invention is calculated by subjecting the dispersion of the present invention to ignition loss at 1000°C, weighing the obtained solid content, and subtracting the separately calculated alkali content converted into an oxide (such as Na2O) to obtain the content of the particle group of the present invention.
[0038] <Polishing composition for magnetic disk substrates> The polishing composition for magnetic disk substrates will now be described. The polishing composition for magnetic disk substrates contains the dispersion liquid of the present invention or the particle group of the present invention. A polishing composition for magnetic disk substrates is a concept that includes a polishing slurry. A polishing composition for magnetic disk substrates that has a low solid content concentration, or a polishing composition for magnetic disk substrates that is diluted with water or the like, is usually called a polishing slurry. A polishing composition for magnetic disk substrates containing the dispersion of the present invention is hereinafter also referred to as the "composition of the present invention."
[0039] The composition of the present invention may further contain other components in addition to the dispersion of the present invention. As the other components, one or more components selected from a polishing accelerator, a surfactant, a hydrophilic compound, a heterocyclic compound, a pH adjuster, and a pH buffering agent can be used.
[0040] Examples of the polishing accelerator include acids such as sulfuric acid, nitric acid, phosphoric acid, oxalic acid, and hydrofluoric acid, or the sodium salts, potassium salts, and ammonium salts of these acids, and mixtures thereof. When the composition of the present invention contains these polishing accelerators, when polishing a material to be polished that is composed of multiple components, the polishing rate of a specific component of the material to be polished can be accelerated, and a flat polished surface can be finally obtained.
[0041] When the composition of the present invention contains a polishing accelerator, the content thereof is preferably from 0.1 to 10 mass %, and more preferably from 0.5 to 5 mass %. In order to improve the dispersibility and stability of the polishing composition of the present invention, a cationic, anionic, nonionic or amphoteric surfactant or a hydrophilic compound can be added.
[0042] Both the surfactant and the hydrophilic compound have the effect of reducing the contact angle with the surface to be polished and promoting uniform polishing. As the surfactant and / or hydrophilic compound, for example, those selected from the following group can be used.
[0043] Examples of anionic surfactants include carboxylates, sulfonates, sulfates, and phosphates. Examples of carboxylates include soaps, N-acylamino acid salts, polyoxyethylene or polyoxypropylene alkyl ether carboxylates, and acylated peptides. Examples of sulfonates include alkylsulfonates, alkylbenzene and alkylnaphthalenesulfonates, naphthalenesulfonates, sulfosuccinates, α-olefinsulfonates, and N-acylsulfonates. Examples of sulfate ester salts include sulfated oils, alkyl sulfates, alkyl ether sulfates, polyoxyethylene or polyoxypropylene alkyl allyl ether sulfates, and alkyl amide sulfates. Examples of phosphate ester salts include alkyl phosphates, polyoxyethylene or polyoxypropylene alkyl allyl ether phosphates, and the like.
[0044] Examples of cationic surfactants include aliphatic amine salts, aliphatic quaternary ammonium salts, benzalkonium chloride salts, benzethonium chloride, pyridinium salts, and imidazolinium salts. Examples of amphoteric surfactants include carboxybetaine type, sulfobetaine type, aminocarboxylate salts, imidazolinium betaine, lecithin, and alkylamine oxide.
[0045] Examples of nonionic surfactants include ether type, ether ester type, ester type, and nitrogen-containing type, and examples of ether type include polyoxyethylene alkyl and alkylphenyl ether, alkylaryl formaldehyde condensed polyoxyethylene ether, polyoxyethylene polyoxypropylene block polymer, and polyoxyethylene polyoxypropylene alkyl ether, examples of ether ester type include polyoxyethylene ether of glycerin ester, polyoxyethylene ether of sorbitan ester, and polyoxyethylene ether of sorbitol ester, examples of ester type include polyethylene glycol fatty acid ester, glycerin ester, polyglycerin ester, sorbitan ester, propylene glycol ester, and sucrose ester, and examples of nitrogen-containing type include fatty acid alkanolamide, polyoxyethylene fatty acid amide, and polyoxyethylene alkylamide. Other examples include fluorine-based surfactants, etc.
[0046] The surfactant is preferably an anionic surfactant or a nonionic surfactant, and the salt includes ammonium salts, potassium salts, sodium salts, etc., and ammonium salts and potassium salts are particularly preferred.
[0047] Further, other surfactants, hydrophilic compounds, etc., include esters (glycerin esters, sorbitan esters, alanine ethyl esters, etc.), ethers (polyethylene glycol, polypropylene glycol, polytetramethylene glycol, polyethylene glycol alkyl ethers, polyethylene glycol alkenyl ethers, alkyl polyethylene glycols, alkyl polyethylene glycol alkyl ethers, alkyl polyethylene glycol alkenyl ethers, alkenyl polyethylene glycols, alkenyl polyethylene glycol alkyl ethers, alkenyl polyethylene glycol alkenyl ethers, polypropylene glycol alkyl ethers, polypropylene glycol alkenyl ethers, alkyl polypropylene glycols, alkyl polypropylene glycol alkyl ethers, alkyl polypropylene glycol alkenyl ethers, alkenyl polypropylene glycols, etc.), polysaccharides (alginic acid, pectinic acid, carboxymethylcellulose, curdlan, pullulan, etc.), amino acid salts (glycine ammonium salt, glycine sodium salt, etc.), polysaccharides (alginic acid, pectinic acid, carboxymethylcellulose, curdlan, pullulan, etc.), amino acid salts (glycine ammonium salt, glycine sodium salt, etc.), polysaccharides (alginic acid, pectinic acid, carboxymethylcellulose, curdlan, pullulan, etc.), polysaccharides (alginic acid, pectinic acid, carboxymethylcellulose, curdlan, pullulan, etc.), polysaccharides (alginic acid, pectinic acid, carboxymethylcellulose, curdlan, pullulan, etc.), polysaccharides (alginic acid, pectinic acid, polysaccharides ... Polycarboxylic acids and their salts (polyaspartic acid, polyglutamic acid, polylysine, polymalic acid, polymethacrylic acid, ammonium salts of polymethacrylic acid, sodium salts of polymethacrylic acid, polyamic acid, polymaleic acid, polyitaconic acid, polyfumaric acid, poly(p-styrene carboxylic acid), polyacrylic acid, polyacrylamide, aminopolyacrylamide, ammonium salts of polyacrylic acid, sodium salts of polyacrylic acid, polyamic acid, ammonium salts of polyamic acid, sodium salts of polyamic acid, and polyglyoxylic acid, etc.), vinyl polymers (polyvinyl chloride, polyvinyl alcohol, polyvinyl ether, polyvinyl alcohol ... alcohol, polyvinylpyrrolidone and polyacrolein, etc.), sulfonic acids and their salts (ammonium methyl taurate, sodium methyl taurate, sodium methyl sulfate, ethyl ammonium sulfate, butyl ammonium sulfate, sodium vinyl sulfonate, sodium 1-allyl sulfonate, sodium 2-allyl sulfonate, sodium methoxymethyl sulfonate, ammonium ethoxymethyl sulfonate, sodium 3-ethoxypropyl sulfonate, etc.), and amides (propionamide, acrylamide,methylurea, nicotinamide, succinamide, sulfanilamide, etc.
[0048] When the substrate to be polished is a glass substrate or the like, any surfactant can be suitably used. However, when the substrate is a silicon substrate for a semiconductor integrated circuit or the like, and the influence of contamination by alkali metals, alkaline earth metals, halides, or the like must be avoided, it is preferable to use an acid or an ammonium salt-based surfactant.
[0049] When the composition of the present invention contains a surfactant and / or a hydrophilic compound, the total content thereof is preferably from 0.001 g to 10 g, more preferably from 0.01 g to 5 g, and particularly preferably from 0.1 g to 3 g, per 1 L of the composition of the present invention.
[0050] The surfactant or hydrophilic compound may be used alone or in combination with two or more kinds.
[0051] The composition of the present invention may contain a heterocyclic compound in order to form a passivation layer or a dissolution-suppressing layer on the metal when the substrate to be polished contains a metal, thereby suppressing the erosion of the substrate to be polished. Here, the term "heterocyclic compound" refers to a compound having a heterocycle containing one or more heteroatoms. The term "heteroatom" refers to an atom other than a carbon atom or a hydrogen atom. The term "heterocycle" refers to a cyclic compound having at least one heteroatom. The term "heteroatom" refers only to atoms that form a part of the ring system of the heterocycle, and does not refer to atoms that are located outside the ring system, that are separated from the ring system by at least one non-conjugated single bond, or that are part of a further substituent of the ring system. Preferred examples of heteroatoms include, but are not limited to, nitrogen atoms, sulfur atoms, oxygen atoms, selenium atoms, tellurium atoms, phosphorus atoms, silicon atoms, and boron atoms. Examples of heterocyclic compounds that can be used include imidazole, benzotriazole, benzothiazole, tetrazole, and the like. More specific examples include 1,2,3,4-tetrazole, 5-amino-1,2,3,4-tetrazole, 5-methyl-1,2,3,4-tetrazole, 1,2,3-triazole, 4-amino-1,2,3-triazole, 4,5-diamino-1,2,3-triazole, 1,2,4-triazole, 3-amino-1,2,4-triazole, and 3,5-diamino-1,2,4-triazole, but are not limited to these.
[0052] When the composition of the present invention contains a heterocyclic compound, the content is preferably from 0.001% by mass to 1.0% by mass, more preferably from 0.001% by mass to 0.7% by mass, and even more preferably from 0.002% by mass to 0.4% by mass.
[0053] In order to enhance the effects of the above-mentioned additives, etc., the pH of the polishing composition can be adjusted by adding an acid or a base as necessary.
[0054] When the composition of the present invention is adjusted to a pH of 7 or higher, an alkaline pH adjuster is used. Preferably, sodium hydroxide, aqueous ammonia, ammonium carbonate, or an amine such as ethylamine, methylamine, triethylamine, or tetramethylamine is used.
[0055] When the polishing composition is adjusted to a pH of less than 7, an acidic pH adjuster is used, such as hydroxy acids such as lactic acid, citric acid, malic acid, tartaric acid, and glyceric acid.
[0056] In order to keep the pH value of the composition of the present invention constant, a pH buffer may be used. Examples of pH buffers that can be used include phosphates and borates such as ammonium dihydrogen phosphate, diammonium hydrogen phosphate, and ammonium tetraborate tetrahydrate, or organic acids.
[0057] The concentration of the polishing particles in the composition of the present invention is preferably 0.5 to 50 mass%, more preferably 5 to 30 mass%. If the concentration is less than 0.5 mass%, depending on the type of substrate or insulating film, the concentration is too low, and the polishing speed is slow, which may cause productivity problems. If the concentration of the polishing particles exceeds 50 mass%, the stability of the polishing material becomes insufficient, and the polishing speed and polishing efficiency are not further improved, and dried matter may be generated and adhered during the process of supplying a dispersion liquid for polishing treatment, which may cause scratches.
[0058] <Production Method of the Present Invention> The manufacturing method of the present invention will now be described. The production method of the present invention includes the following steps (a) to (c).
[0059] <Process (a)> In step (a), an acidic silicic acid liquid and an alkali halide are added to and mixed with an aqueous alkali silicate solution to prepare a precursor dispersion having a ratio ((MTS) / (MH)) of the number of moles of silica (MTS) to the number of moles of alkali halide (MH) of 2 to 100 and a silica concentration in the range of 10 to 18 mass%.
[0060] Here, the sum of the number of moles of silica contained in the alkali silicate aqueous solution (MWG) and the number of moles of silica contained in the acidic silicic acid solution (MSA1) is the number of moles of silica contained in the precursor dispersion (MTS).
[0061] Here, the amount of alkali silicate aqueous solution, acidic silicic acid solution and alkali halide added is preferably such that the amount of alkali halide added (moles) (MH) is 2 to 100 times the number of moles of silica (MTS), which is the sum of the number of moles of silica contained in the alkali silicate aqueous solution (MWG) and the number of moles of silica contained in the acidic silicic acid solution (MSA1). In other words, it is preferable that the ratio (MTS) / (MH) is 2 to 100. It is more preferable that the value of (MTS) / (MH) is 5 to 60. Here, the alkali halide plays the role of a structure control agent or a flocculating agent for forming a dimple-type structure. An alkali silicate or an acidic silicic acid solution is added to adjust the silica to alkali molar ratio and silica concentration to a predetermined range, and the solution is heated and stirred to prepare a precursor. Here, the precursor is mainly a polymer of silicic acid, and is not yet clearly granulated. The precursor is the source of the generation of core particles and seed particles (which are formed by the aggregation of core particles and further particle growth) by the reaction with an acidic silicic acid liquid in the subsequent step (b). In the present invention, in step (b), the core particles generated by the reaction of the precursor with the acidic silicic acid liquid are partially aggregated by an alkali halide, and three or more core particles are aggregated to form a bent aggregate structure, or particles having such an aggregate structure are further grown. Such aggregate structures and further grown particles become seed particles of pit-shaped particles. While pit-shaped seed particles are generated, pit-shaped seed particles also coexist with non-aggregated core particles, so the seed particle dispersion is in a form in which pit-shaped seed particles and spherical particles such as pit-shaped particles coexist. In step (c), the inventors of the present application presume that pit-shaped silica-based particles are generated by subsequently adding an acidic silicic acid liquid to the seed particle dispersion to grow the seed particles. Incidentally, it is difficult to directly observe the generation or aggregation process of core particles because the size of the core particles is small and the reaction proceeds rapidly. However, from the particle size distribution and shape of the particles of the present invention, it is presumed that new core particles are generated while core particles are agglomerating, and that although some core particles further agglomerate to become seed particles, the majority of core particles remain unaggregated. It is difficult to clearly distinguish between core particles and seed particles, but as described above, the seed particle dispersion is a mixture of seed particles consisting of aggregated core particles and non-aggregated core particles, and the precursor dispersion in this specification can be considered to be a dispersion of the precursors that are the source of the core particles and the seed particles. If the MTS / MH value is less than 2, i.e., if the amount of flocculant is large, the core particles will aggregate and become larger in size, causing sedimentation or making it difficult to obtain the desired size of the silica-based particles obtained through steps (b) and (c). If the value of MTS / MH exceeds 100, the aggregation of the core particles will not proceed easily, making it difficult to obtain the desired dimple-shaped particles.
[0062] [Alkaline silicate solution] Examples of the aqueous alkali silicate solution that can be used in step (a) include sodium silicate, potassium silicate, lithium silicate, and quaternary ammonium silicate. As the aqueous alkali silicate solution, it is preferable to use sodium silicate or potassium silicate, which are commercially available under the names of No. 1 water glass, No. 2 water glass, No. 3 water glass, etc. As the aqueous alkali silicate solution, it is preferable to use one obtained by hydrolyzing a hydrolyzable organic compound such as tetraethyl orthosilicate (TEOS) with an excess of NaOH or the like.
[0063] The concentration of the aqueous alkali silicate solution is preferably 15 to 30 mass %, and more preferably 15 to 25 mass %, calculated as SiO2.
[0064] [Acidic silicic acid liquid] The acidic silicic acid solution that can be used is one obtained by dealkalizing an aqueous alkali silicate solution with a cation exchange resin. The concentration of the acidic silicic acid liquid is preferably 0.1 to 10 mass %, and more preferably 1 to 7 mass %, calculated as SiO2. The pH of the acidic silicic acid solution is preferably 1-3.
[0065] [Alkali halide] The alkali halide is preferably used in the form of an aqueous solution. Examples of the aqueous alkali halide solution include an aqueous potassium chloride solution, an aqueous sodium chloride solution, and an aqueous lithium chloride solution. The concentration of the alkali halide in the aqueous alkali halide solution is preferably 1 to 30% by mass.
[0066] The stirring conditions when mixing the aqueous alkali silicate solution, the acidic silicic acid solution, and the alkali halide are not particularly limited, provided that the aqueous alkali silicate solution, the acidic silicic acid solution, and the alkali halide can be mixed almost uniformly. The temperature when mixing the aqueous alkali silicate solution, the acidic silicic acid solution, and the alkali halide is not particularly limited, but may be room temperature.
[0067] In step (a), the alkali silicate aqueous solution, the acidic silicic acid solution, and the alkali halide are mixed under the above-mentioned conditions, and stirred and mixed until homogeneous to obtain a precursor dispersion liquid. Here, the silica concentration of the precursor dispersion liquid is 10 to 18% by mass, and preferably 10 to 15% by mass. When the silica concentration of the precursor dispersion is within this range, the core particles generated in and after step (a) are appropriately aggregated, making it easy to obtain the desired recessed particles, and ultimately, the manufacturing method of the present invention makes it easy to obtain a silica-based particle dispersion that has a high polishing rate and is less likely to produce waviness. If the silica concentration is less than 10% by mass, the core particles do not aggregate, making it difficult to obtain dimpled particles.If the silica concentration is more than 18% by mass, the core particles aggregate and dimpled particles are easily obtained, but the particles tend to be large and easily aggregate, and when used as polishing abrasives, scratches tend to occur, and the surface roughness and waviness of the substrate tend to worsen.
[0068] <Process (b)> In step (b), the precursor dispersion obtained in step (a) is held at 50 to 95°C, and then, while maintaining the same temperature range, an acidic silicic acid liquid is added continuously or intermittently to prepare a seed particle dispersion.
[0069] The precursor dispersion liquid is maintained at 50 to 95° C., whereby aging proceeds, and core particles are generated in a later step. If the maintenance temperature is within the range of 50 to 95° C. (preferably 60 to 90° C., and more preferably 60 to 88° C.), depression-type particles having the desired size and shape are easily obtained. If the holding temperature exceeds 95° C., the ratio of coarse particles in the silica-based microparticle dispersion obtained after step (c) tends to increase, possibly because the core particles formed later will aggregate too much. If the holding temperature is less than 50° C., the core particles formed later will not aggregate easily, and the aggregation of the core particles will be insufficient, possibly making it difficult to obtain the desired dimple-shaped particles.
[0070] The time for which the mixture is held at 50 to 95°C varies depending on the holding temperature or the silica concentration in the precursor dispersion, but is preferably within 24 hours, and practically, a time within the range of 10 to 300 minutes is recommended.
[0071] After the precursor dispersion has been kept at 50 to 95° C., an acidic silicic acid liquid is added continuously or intermittently while maintaining the same temperature range to obtain a seed particle dispersion.
[0072] Here, the acidic silicic acid solution used can be the same as that mentioned in step (a). It is also preferable to use the same acidic silicic acid liquid in step (b) as that used in step (a).
[0073] By such step (b), a seed particle dispersion liquid is obtained.
[0074] <Process (c)> In the step (c), an acidic silicic acid liquid is added to the seed particle dispersion liquid obtained in the step (b). Here, an acidic silicic acid liquid containing 2 to 100 times the molar number of SiO2 relative to the SiO2 contained in the seed particle dispersion liquid is added. In step (c), the seed particles grow to produce silica-based particles.
[0075] Here, the acidic silicic acid solution used can be the same as that mentioned in step (a). It is also preferable to use the same acidic silicic acid liquid in step (c) as that used in steps (a) and (b).
[0076] The amount (number of moles) of SiO2 contained in the acidic silicic acid liquid to be added is 2 to 100 times, and preferably 3 to 80 times, the number of moles of SiO2 contained in the seed particle dispersion liquid. If this value is less than 2 times, the particle size of the silica particles in the silica-based microparticle dispersion liquid obtained by the manufacturing method of the present invention is small, and the polishing speed may be insufficient even when used as an abrasive. Conversely, if this value exceeds 100 times, the particle size of the silica-based particles in the silica-based microparticle dispersion liquid obtained by the manufacturing method of the present invention is large, and the shape of the silica-based particles approaches a sphere, making it difficult to obtain desired dimple-shaped particles, and therefore the polishing speed may be insufficient even when used as an abrasive.
[0077] The temperature of the prepared liquid when the acidic silicic acid liquid is added is preferably in the range of 50 to 95°C, more preferably 60 to 95°C. If the temperature is less than 50°C, the acidic silicic acid liquid added to grow the seed particles does not dissolve sufficiently and is difficult to deposit on the surface of the seed particles, which causes self-nucleation by the acidic silicic acid liquid, making it difficult to obtain the desired depression-shaped particles. If the temperature exceeds 98°C, the mixture approaches its boiling point, causing an increase in coarse particles, which may result in scratches (grinding marks) when used as an abrasive.
[0078] The pH of the preparation when the acidic silicic acid solution is added is preferably in the range of 9 to 12.5, and more preferably in the range of 10 to 12.0. If the pH is less than 9, the acidic silicic acid solution added for particle growth does not dissolve sufficiently and does not deposit on the surface of the seed particles, which tends to cause self-nucleation by silicic acid. On the other hand, if the pH is higher than 12.5, the ionic strength in the preparation becomes too high, which reduces the dispersion stability of the seed particles and may cause excessive aggregation, resulting in the formation of coarse particles.
[0079] In the step (c), when the acidic silicic acid liquid is added, an acid or a base can be added as a pH adjuster, if necessary, to adjust the pH of the dispersion to the above range. The acid that can be used is a mineral acid such as hydrochloric acid, nitric acid, or sulfuric acid. As the base, a basic nitrogen compound such as an alkali metal hydroxide such as NaOH or KOH, a metal carbonate such as potassium oxide, sodium carbonate or ammonium carbonate, an amine such as ammonia, monoethanolamine or piperazine, or a quaternary ammonium hydroxide such as tetramethylammonium can be used.
[0080] After the step (c), washing may also be carried out. By washing, impurities remaining in the silica-based particle dispersion, such as Na, K, and the like derived from the raw materials, cations and anions used for agglomeration or deformation of precursors, and acids or bases used for pH adjustment, can be removed, and adverse effects during polishing or adverse effects when the polished substrate is used for an electronic device, etc. can be suppressed. As the washing method, a conventionally known method such as an ultrafiltration membrane method or an ion exchange resin method can be used.
[0081] Furthermore, in the manufacturing method of the present invention, following the step (c) or after the cleaning, if there are particles other than the desired particle size (especially coarse particles with an excessively large particle size) or particles other than the desired shape, they can be separated and removed as necessary. If such particles remain, depending on the remaining amount, the polishing speed may be insufficient, scratches may occur, or the smoothness of the polished substrate may deteriorate. The separation method is not particularly limited as long as it can remove particles other than the desired particle size and shape, and any method known in the art can be used, such as various filters and centrifuges.
[0082] After the step (c), a concentration treatment may be carried out, if desired. The silica concentration after concentration is recommended to be in the range of, for example, 10 to 50 mass %. EXAMPLES
[0083] The silica-based particle dispersions obtained in each Example and Comparative Example were evaluated as follows. The results are shown in Table 1. Table 2 also shows the conditions for the production process of the silica-based fine particle dispersions in each Example and Comparative Example.
[0084] 1) Identification of pitted silica particles, and calculation of their content and [La] / [De] A scanning electron microscope photograph (S-2000 model manufactured by Hitachi, Ltd., magnification 200,000 times, containing 200 or more particles in the same field of view) of the silica-based particle dispersion was taken, and whether or not the particles in the photograph corresponded to dent-type silica-based particles was confirmed by the following method. First, in the concave portion of one particle, a tangent line M was drawn that touched two points (points A and B) on the particle contour that sandwiched the concave portion, and the maximum length of the straight line perpendicular to the tangent line M from the tangent line M to the particle contour was determined. If the length (L) was 3 nm or more, the particle was determined to be a concave-type silica-based particle. Note that, if a particle has multiple concave portions and multiple concaves with a length L of 3 nm or more, the length L of the particle means the maximum L. In this way, 200 particles randomly selected within the field of view were examined to see whether they were dented silica-based particles, and the number ratio (content) of the dented silica-based particles among the 200 particles was calculated.
[0085] Next, the number average value of the length (L) of each of the particles that were determined to be dimpled silica-based particles by the above-mentioned method was determined, and this was taken as the number average value La.
[0086] Next, the specific surface area converted particle diameter De of the silica-based particle group was determined by the method described below, and the value of [La] / [De] was then calculated.
[0087] 2) Average long / short diameter ratio of hollow silica particles A scanning electron microscope photograph (Hitachi S-2000, 200,000x magnification, containing 200 or more particles in the same field of view) of the silica-based particle dispersion is taken, and depression-type silica-based particles are confirmed in the same manner as in 1) above, to prepare a scanning electron microscope photograph in which 50 or more depression-type silica-based particles are confirmed. Then, for 50 depression-type silica-based particles randomly selected from the depression-type silica-based particles, the major axis / minor axis ratio of each circumscribed rectangle is taken as the maximum, and the average of the 50 particles is calculated to obtain the average major axis / minor axis ratio of the depression-type silica-based particles.
[0088] 3) Weight-converted particle size distribution and weight-average particle size (D 50 ) Measurement The silica-based particle dispersion was diluted with a 0.05% by mass aqueous solution of sodium dodecyl sulfate to a solid content of 2% by mass, and 0.1 mL of the diluted solution was injected with a syringe into a known disk centrifugal particle size distribution analyzer (manufactured by CPS Instruments) and measured in a density gradient solution of 8% to 24% sucrose at 18,000 rpm to obtain a weight-equivalent particle size distribution. In the weight-converted particle size distribution obtained, the cumulative 10% particle size (D 10 )[nm], cumulative 50% particle diameter (D 50 )[nm], cumulative 90% particle diameter (D 90 ) [nm] and calculate the value of (D 90 -D 10 ) / D 50 The value was calculated. In addition, the cumulative particle size of the smallest particle size (D 50 ) [nm] was taken as the weight average particle diameter.
[0089] 4) Method for measuring the pore volume of particle groups 10 g of sample powder obtained by drying the silica-based particle dispersion was placed in a crucible and dried at 105°C for 1 hour, then placed in a desiccator and cooled to room temperature. Next, 1 g of sample was weighed and placed in a well-cleaned cell, vacuum degassed at 300°C for 2 hours, and then set in a MicrotrackBell BELSORP-mini to adsorb N2 to obtain an adsorption isotherm. Here, the value at relative pressure (P / P0): 0.990 was taken as the pore volume. The pore volume was calculated from the following formula. Pore volume (mL / g) = (0.001567 × (V-Vc) / W) In the above formula, V is the adsorption amount (mL) under standard conditions at a pressure of 735 mmHg, Vc is the volume (mL) of the cell blank at a pressure of 735 mmHg, and W is the mass (g) of the sample. The density ratio of nitrogen gas to liquid nitrogen was set to 0.001567.
[0090] 5) Particle size converted into specific surface area (De) The particle size in terms of specific surface area can be obtained by measuring the specific surface area Sa of the silica fine particles and using the following formula: (De) (nm) = 6000 / (ρ × Sa). (Here, ρ represents the density of the silica fine particles, 2.2 [g / cm 3 .) When the specific surface area of the silica fine particles is 100 m 2 / g or more, sintering progresses during firing in the BET method. In this case, the specific surface area (SA) was determined by the titration method, and the particle size in terms of specific surface area (De) was calculated from the formula (De) = 6000 / (SA × ρ).
[0091] <BET method> For a 50 mL silica particle dispersion containing silica-based particles (silica concentration 40 mass%) adjusted to pH 3.5 with HNO3, 40 mL of 1-propanol was added, and the sample dried at 110°C for 16 hours was pulverized in a mortar and then fired in a muffle furnace at 500°C for 1 hour to obtain a measurement sample. Then, using a specific surface area measuring device (manufactured by Yuasa Ionics, model number Multi-Sorb 12), the specific surface area was calculated by the BET one-point method from the nitrogen adsorption amount using the nitrogen adsorption method (BET method).
[0092] Specifically, 0.5 g of the sample was placed in the measurement cell, degassed at 300°C for 20 minutes in a mixed gas stream of 30 v% nitrogen and 70 v% helium, and then the sample was maintained at liquid nitrogen temperature in the above mixed gas stream to allow nitrogen to be adsorbed on the sample in equilibrium. Next, while flowing the above mixed gas, the sample temperature was gradually raised to room temperature, and the amount of nitrogen desorbed during that time was detected, and the specific surface area of the silica-based particles was calculated using a calibration curve prepared in advance. Then, the obtained specific surface area (Sa) was substituted into the conversion formula from the specific surface area to the particle size described above to obtain the particle size in terms of specific surface area (De).
[0093] <Titration method> Here, the titration method is as follows. First, a sample equivalent to 1.5 g of SiO2 was placed in a beaker, then transferred to a thermostatic reaction tank (25°C), and pure water was added to make the liquid volume 90 ml. The following operations were carried out in the thermostatic reaction tank maintained at 25°C. Next, 0.1 mol / L hydrochloric acid solution was added to this to adjust the pH to 3.6, and 30 g of sodium chloride was added, diluted with pure water to 150 ml, and stirred for 10 minutes. Then, a pH electrode was set, and 0.1 mol / L sodium hydroxide solution was added dropwise while stirring to adjust the pH to 4.0. Furthermore, the sample adjusted to pH 4.0 was titrated with 0.1 mol / L sodium hydroxide solution, and the titration amount and pH value in the range of pH 8.7 to 9.3 were recorded at four or more points, and a calibration curve was created by setting the titration amount of 0.1 mol / L sodium hydroxide solution as X and the pH value at that time as Y. The consumption amount V (ml) of 0.1 mol / L sodium hydroxide solution required to change the pH from 4.0 to 9.0 per 1.5 g of SiO2 was calculated from the equation V = (A × f × 100 × 1.5) / (W × C), and the specific surface area was calculated using this amount according to the equation SA = 29.0V-28. In the above formula, A is the titration amount (ml) of 0.1 mol / L sodium hydroxide solution required per 1.5 g of SiO2 to change the pH to 4.0 to 9.0, f is the titer of the 0.1 mol / L sodium hydroxide solution, C is the SiO2 concentration of the sample (%), and W is the amount of sample taken (g).
[0094] 6) Measurement of mean particle size (Dd) of particle groups by dynamic light scattering method For a silica-based particle dispersion (SiO2 concentration 0.1 to 5 mass%, aqueous solvent), the average particle size was measured by dynamic light scattering using a particle size distribution measuring device (Otsuka Electronics Co., Ltd.: nanoSAQLA).
[0095] 7) Measurement of silica concentration in silica-based particle dispersions 2 mL of 50% aqueous sulfuric acid solution is added to 10 g of a sample consisting of a silica-based particle dispersion liquid, and the mixture is evaporated to dryness on a platinum dish. The solid obtained is baked at 1000°C for 1 hour, cooled, and weighed. The weighed solid is then dissolved in a small amount of 50% aqueous sulfuric acid solution, and 20 mL of hydrofluoric acid is added. The mixture is evaporated to dryness on a platinum dish, baked at 1000°C for 15 minutes, cooled, and weighed. The solid content is calculated from the difference in weight, and the solid concentration relative to the mass (10 g) of the sample can be calculated. Next, the concentration obtained by subtracting the separately calculated alkali content converted into oxide (Na2O, etc.) is calculated as the content of the particle group of the present invention. In addition, the content of components other than silica that the particle group of the present invention may contain can be specified and quantified, for example, using an inductively coupled plasma emission spectrometer. Note that, Ni, Cu, K and Na can be specified and quantified using an atomic absorption spectrophotometer.
[0096] 8) Polishing test method (polishing speed ratio and waviness ratio) An aluminum substrate coated with nickel plating for hard disks (nickel-plated substrate manufactured by Toyo Kohan Co., Ltd.) was prepared as the substrate to be polished. This substrate to be polished was set in a polishing device (NF300 manufactured by Nanofactor Co., Ltd.) and polished 1 μm using a polishing pad (Bellatrix NO178 manufactured by FILWEL) with a substrate load of 0.05 MPa, a platen rotation speed of 50 rpm, a head rotation speed of 50 rpm, and a polishing slurry supplied at a rate of 40 g / min.
[0097] <Polishing speed ratio> The polishing rate was determined from the difference in weight of the polished substrate before and after polishing and the polishing time, and a relative value was calculated with Comparative Example 1 taken as 100.
[0098] <Waviness ratio> In a polished doughnut-shaped aluminum substrate, the amplitude of minute irregularities with a waviness wavelength of several tens to several hundreds of μm was measured at any point that equally bisects the diameter between the outer and inner circles. Next, the amplitude of minute irregularities with a waviness wavelength of several tens to several hundreds of μm was similarly measured at a point on a line connecting the measurement point and the center point of the doughnut-shaped aluminum substrate, where the center point bisects the measurement point.The average of these two values was then calculated as the "waviness value," and the relative value (waviness ratio) was calculated with Comparative Example 1 taken as 100. The measurement conditions for the amplitude of the unevenness are as follows. Equipment:ZygoNewView7200 Lens: 2.5x Zoom ratio: 1.0 Filter: 50~500μm Measurement area: 3.75mm x 2.81mm
[0099] <Preparation of acidic silicic acid solution> Pure water was added to a sodium silicate aqueous solution (silica concentration 24.06% by mass, Na2O concentration 7.97% by mass) to obtain a sodium silicate aqueous solution (silica concentration 5% by mass). 18 kg of the obtained sodium silicate aqueous solution was added to 6 L of a strong acid cation exchange resin (SK1BH, manufactured by Mitsubishi Chemical Corporation) at a space velocity of 3.0 h -1 The solution was passed through a filter at 1000 rpm, and 18 kg (silica concentration: 4.5 mass %, pH: 2.7) was obtained. In the following Examples and Comparative Examples, this acidic silicic acid solution or an acidic silicic acid solution equivalent to this acidic silicic acid solution was used as the raw material.
[0100] [Example 1] (Step a) 790 g of a sodium silicate aqueous solution (silica concentration: 24.3% by mass) was added to 637 g of water and stirred until homogenous, and then 80 g of an acidic silicic acid solution (silica concentration: 4.5% by mass) and 61 g of a potassium chloride aqueous solution (concentration: 20% by mass) were added and stirred until homogenous, to obtain a precursor dispersion (silica concentration: 12.5% by mass).
[0101] (Step b) Next, the obtained precursor dispersion liquid was heated to 85°C and maintained at 85°C for 40 minutes. While maintaining the temperature at 85°C, 6,158 g of acidic silicic acid liquid (silica concentration: 4.5% by mass) was added over 5 hours, and then 2,230 g of water was added and cooled to obtain a seed particle dispersion liquid (1).
[0102] (Step c) 4,400 g of the obtained seed particle dispersion (1) was added to 8,828 g of water, and then the temperature was raised to 98° C. While maintaining the temperature at 98° C., 26,441 g of an acidic silicic acid liquid (silica concentration: 4.5% by mass) was added over 15 hours to obtain a silica-based particle dispersion (1). The average particle diameter (Dd) of the obtained silica-based particle dispersion (1) was measured by the dynamic light scattering method described in 6) above and found to be 170 nm.
[0103] [Example 2] (Step a) 600 g of a sodium silicate aqueous solution (silica concentration: 24.3% by mass) was added to 642 g of water and stirred until homogenous, and then 60 g of an acidic silicic acid solution (silica concentration: 4.5% by mass) and 46 g of a potassium chloride aqueous solution (concentration: 20% by mass) were added and stirred until homogenous, to obtain a precursor dispersion (silica concentration: 11% by mass).
[0104] (Step b) Next, the obtained precursor dispersion liquid was heated to 85°C and maintained at 85°C for 40 minutes. While maintaining the temperature at 85°C, 4,710 g of acidic silicic acid liquid (silica concentration: 4.5% by mass) was added over 5 hours. Then, 1,748 g of water was added and cooled to obtain seed particle dispersion liquid (2).
[0105] (Step c) The obtained seed particle dispersion liquid (2) 4,589 g was added to 8,834 g of water, and then the temperature was raised to 98° C. While maintaining the temperature at 98° C., 26,832 g of an acidic silicic acid liquid (silica concentration: 4.5% by mass) was added over 15 hours to obtain a silica-based particle dispersion liquid (2). The average particle diameter (Dd) of the obtained silica-based particle dispersion (2) was measured by the dynamic light scattering method described in 6) above, and was found to be 144 nm.
[0106] [Comparative Example 1] (Step a) 790 g of a sodium silicate aqueous solution (silica concentration: 24.3% by mass) was added to 2,278 g of water and stirred until homogenous, and then 78 g of an acidic silicic acid solution (silica concentration: 4.5% by mass) and 61 g of a potassium chloride aqueous solution (concentration: 20% by mass) were added and stirred until homogenous, to obtain a precursor dispersion (silica concentration: 6.1% by mass).
[0107] (Step b) Next, the obtained precursor dispersion liquid was heated to 98°C and maintained at 98°C for 40 minutes. While maintaining the temperature at 98°C, 5,984 g of acidic silicic acid liquid (silica concentration: 4.5% by mass) was added over 5 hours, and then 2,655 g of water was added and cooled to obtain a seed particle dispersion liquid (3).
[0108] (Step c) 4,000 g of the obtained seed particle dispersion (3) was added to 5,900 g of water, and then the temperature was raised to 98° C., and 26,451 g of an acidic silicic acid liquid (silica concentration: 4.5% by mass) was added over 18 hours while maintaining the temperature at 98° C., to obtain silica-based particle dispersion (3). The average particle diameter (Dd) of the obtained silica-based particle dispersion (3) was measured by the dynamic light scattering method described in 6) above, and was found to be 155 nm.
[0109] [Comparative Example 2] 3,500 g of the seed particle dispersion (3) obtained in step b of Comparative Example 1 was added to 5,163 g of water to obtain a silica solution. The obtained silica solution was heated to 98° C., and while maintaining the temperature at 98° C., 29,181 g of an acidic silicic acid liquid (silica concentration: 4.5% by mass) was added over 22 hours to obtain a silica-based particle dispersion (4). The average particle diameter (Dd) of the obtained silica-based particle dispersion (4) was measured by the dynamic light scattering method described in 6) above, and was found to be 154 nm.
[0110] [Comparative Example 3] The silica fine particle dispersion obtained by carrying out the same procedure as in Example 1 of Patent Document 2 was used for evaluation.
[0111] [Table 1]
[0112]
Table 2
Claims
1. A dispersion of silica-based particles for polishing, comprising a particle group including hollow-type silica-based particles having a hollow portion facing toward the inside of the particle, which satisfies the following [1] to [5], dispersed in a solvent. [1] The average particle size (Dd) of the particle group as measured by dynamic light scattering is within the range of 40 to 300 nm. [2] In the weight-converted particle size distribution of the particle group, the cumulative 10% particle size from the smallest particle size (D 10 ), cumulative 90% particle diameter (D 90 ) and cumulative 50% particle size (D 50 ) satisfies the following formula: Formula: 1.6≦(D 90 -D 10 ) / D 50 ≦5 [3] The particle group has a pore volume measured by a nitrogen adsorption method within a range of 0.1 to 0.35 ml / g. [4] In the above-mentioned depression type silica-based particles, in an electron microscope photograph or image, the particle contour has a concave portion that is depressed toward the inside of the particle, and when the maximum length L from the tangent M to a point where a straight line drawn perpendicularly from a tangent M that touches two points on the particle contour that sandwich the concave portion intersects with the particle contour, L satisfies L≧3 nm. [5] The ratio (La / De) of La to the specific surface area converted particle diameter De of the particle group is 0.15 or more (where La represents the number average value of the length L of the depression type silica-based particles in the particle group).
2. 2. The silica-based particle dispersion liquid for polishing according to claim 1, wherein the content of said dent-type silica-based particles in said particle group is 25 to 90 mass %.
3. 3. The silica-based particle dispersion for polishing according to claim 1, wherein the average major axis / minor axis ratio of said depression-type silica-based particles is in the range of 1.34 to 5.
4. A method for producing a dispersion liquid of silica-based particles for polishing, comprising the following steps (a) to (c): Step (a): A step of adding and mixing an acidic silicic acid liquid and an alkali halide to an aqueous alkali silicate solution to prepare a precursor dispersion having a ratio ((MTS) / (MH)) of the number of moles of silica (MTS) to the number of moles of alkali halide (MH) of 2 to 100 and a silica concentration in the range of 10 to 18 mass %. Step (b): A step of holding the precursor dispersion at 50 to 95° C., and then continuously or intermittently adding the acidic silicic acid liquid while maintaining the same temperature range to prepare a seed particle dispersion. Step (c): The SiO contained in the seed particle dispersion 2 2 to 100 times the molar amount of SiO 2 to the seed particle dispersion to obtain a silica-based particle dispersion.
Citation Information
Patent Citations
Manufacture of multilayer seat coil
JP1987007345A
Method of manufacturing irregular shape silica particle
JP2018177576A
Colloidal silica containing silica secondary particles having bent structure and / or branched structure, and method for producing same
WO2010035613A1