Integrated type sealing sheet, light-emitting type electronic component, and method for manufacturing light-emitting type electronic component
The integrated sealing sheet with a transparent curable resin and translucent film layer addresses brightness loss and manufacturing inefficiencies in mini LED and micro LED components by providing uniform sealing and maintaining brightness, enhancing display quality.
Patent Information
- Application Number
- JP2023085625
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-24
- Publication Date
- 2024-12-05
AI Technical Summary
Existing methods for manufacturing mini LED and micro LED components face challenges such as increased manufacturing costs due to time-consuming etching processes, difficulty in completely removing resin on light-emitting elements, and potential brightness loss or uneven brightness due to residual adhesive layers, leading to spots and overall brightness reduction.
An integrated sealing sheet comprising a transparent curable resin layer and a translucent film layer, laminated in sequence, is used to fill spaces between light-emitting elements without etching, ensuring uniform application and maintaining blackness while preventing brightness loss, achieved through specific transmittance and storage modulus properties.
The integrated sealing sheet allows for efficient sealing without appearance defects, maintaining overall brightness and improving contrast by ensuring uniform application and preventing residual adhesive layers, thus simplifying the manufacturing process and enhancing display quality.
Smart Images

Figure 2024168724000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to an integrated encapsulating sheet, a light-emitting electronic component, and a method for manufacturing a light-emitting electronic component. [Background technology]
[0002] In recent years, display technologies that use extremely small light-emitting diodes, known as mini-LED and micro-LED, have been attracting attention. Mini LEDs and micro LEDs can be used in two ways. One is a technology that allows the brightness of a liquid crystal backlight to be controlled locally by configuring a large number of LEDs arranged on a substrate. The other system uses LEDs of the respective colors to emit the R (red), G (green), and B (blue) that make up a pixel, and the high-purity colors emitted by the LEDs of each color reach the eye as is.
[0003] Mini LEDs and micro LEDs use electronic components in which multiple light-emitting elements are arranged on a substrate. In such electronic components, a dry film is used to fill the spaces between the multiple light-emitting elements with a resin that prevents light diffusion (Patent Document 1). A dry film is a resin film obtained by applying and drying a curable resin composition onto a protective film, which is then pressed onto the surface of the substrate on which the light-emitting elements are arranged, filling the spaces between the light-emitting elements, and then cured.
[0004] When the dry film is pressure-bonded to the surface of the substrate on which the light-emitting elements are arranged, a resin layer having light diffusion preventing properties is inevitably formed not only between the light-emitting elements but also on the light-emitting elements. If the resin layer having light diffusion prevention properties formed on the light emitting elements is left as it is, not only will light be diffused between the light emitting elements, but light that should be emitted toward the viewer will also be blocked. Therefore, Patent Document 1 describes that after the dry film is pressed, the resin on the light-emitting element is removed by etching such as plasma treatment, and the exposed light-emitting element is covered with a light-transmitting sealant.
[0005] Patent document 2 claims that by using a dry film having a two-layer structure consisting of a black adhesive layer that is lower than the height of the light-emitting element and a transparent adhesive layer that has a higher melting point than the black adhesive layer, it is possible to prevent the black adhesive layer from remaining on the light-emitting element. In Patent Document 2, after the dry film is cured, a semi-transparent dry film is further pressure-bonded and cured, thereby completing the sealing. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] Patent Publication No. 2022-22562 [Patent Document 2] China Patent Application Publication No. 115084320 Summary of the Invention [Problem to be solved by the invention]
[0007] However, when etching such as plasma treatment is performed as in Patent Document 1, it takes a lot of time, which is a factor in increasing manufacturing costs. In addition, it is difficult to completely remove the resin on the light-emitting element by etching, and there is a risk of partial reduction in brightness and unevenness. Furthermore, in order to provide a sealant layer on the outermost surface, an additional step of laminating a dry film of the sealant is required.
[0008] In Patent Document 2, etching is not required, but a work of laminating a translucent dry film is necessary to compensate for the blackness. However, when mounting the light-emitting element with solder, the inclination and height of the light-emitting element vary from one light-emitting element to another, so the transparent adhesive layer cannot wash away the black adhesive layer evenly, and the black adhesive layer remains on some of the light-emitting elements, causing a partial decrease in brightness and resulting in spots. In addition, when a translucent dry film, a transparent adhesive layer, and a black adhesive layer are laminated and pressed together to omit a process, the translucent dry film deforms without being cured, so that the stress during thermocompression cannot be sufficiently transmitted, and the black adhesive layer is likely to remain on the light-emitting element, resulting in a large loss of overall brightness.
[0009] In view of the above circumstances, an object of the present invention is to provide an integrated encapsulating sheet that can not only fill resin between multiple light-emitting elements but also complete the sealing process with a single compression bonding without causing appearance defects such as air bubbles or surface irregularities, and that can ensure blackness while suppressing loss of overall brightness without causing spots due to partial reduction in brightness, and a light-emitting electronic component using this integrated encapsulating sheet, and a method for manufacturing a light-emitting electronic component. [Means for solving the problem]
[0010] In order to achieve the above object, the present invention employs the following configuration. [1] An integrated encapsulating sheet that is pressure-bonded to a surface of an element-mounted substrate on which a plurality of light-emitting elements are arranged, the surface comprising the element-mounted substrate and the light-emitting elements arranged on the surface of the element-mounted substrate, An integrated encapsulating sheet comprising a transparent curable resin layer and a translucent film layer, which are laminated in this order from the side that is to be placed in direct contact with the element-mounted substrate during the pressure bonding. [2] The integrated encapsulating sheet according to [1], wherein the translucent film layer has a total light transmittance of 20 to 80%. [3] The integrated encapsulating sheet according to [1] or [2], wherein the transparent curable resin layer has a total light transmittance of 50% or more and is higher than the total light transmittance of the translucent film layer. [4] The storage modulus of the transparent curable resin layer at 100° C. is 1.0×107 The integrated encapsulating sheet according to any one of [1] to [3], wherein the elastic modulus is 0.01 Pa or less. [5] The storage modulus of the transparent curable resin layer at 100° C. is 1.0×10 5 The integrated encapsulating sheet according to [4], wherein the elastic modulus is 0.01 Pa or less. [6] The integrated encapsulating sheet according to any one of [1] to [5], wherein the transparent curable resin layer contains a high molecular weight resin having a weight average molecular weight of 20,000 to 1,000,000. [7] The integral encapsulating sheet according to [6], wherein the high molecular weight resin has a weight average molecular weight of 100,000 to 500,000. [8] The integrated encapsulating sheet according to [6] or [7], wherein the transparent curable resin layer contains a polyfunctional curable resin capable of forming a crosslinked structure with the high molecular weight resin. [9] The integrated encapsulating sheet according to any one of [6] to [8], wherein the content of the high molecular weight resin relative to 100 mass % of the transparent curable resin layer is 5 to 100 mass %.
[10] The integrated encapsulating sheet according to any one of [1] to [9], wherein the translucent film layer comprises a support film layer and a hard coat layer provided on the opposite side of the support film layer to the transparent curable resin layer.
[11] The translucent film layer includes a support film layer and at least one translucent resin layer; The integrated encapsulating sheet according to any one of [1] to
[10] , wherein the semitransparent resin layer has a total light transmittance of 20 to 80%.
[12] The integrated encapsulating sheet according to any one of claims [1] to
[11] , wherein the translucent film layer includes one or more layers containing carbon black.
[13] The storage modulus of the semi-transparent film layer at 100° C. is 1.0×10 8 The integrated encapsulating sheet according to any one of [1] to
[12] , wherein the elastic modulus is 1.0 Pa or more.
[14] The integrated encapsulating sheet according to any one of [1] to
[13] , wherein the gloss of an outermost surface of the translucent film layer opposite to the transparent curable resin layer is 0.01 to 35.
[15] An element-mounted substrate having a plurality of light-emitting elements arranged on a substrate, and the integrated encapsulating sheet according to any one of [1] to
[14] , which is pressure-bonded to a surface of the element-mounted substrate on which the plurality of light-emitting elements are arranged, A light-emitting electronic component, characterized in that at least a portion of the transparent curable resin layer is filled between the plurality of light-emitting elements.
[16] An integrated encapsulating sheet according to any one of [1] to
[14] is disposed on a surface of an element-mounted substrate on which a plurality of light-emitting elements are disposed, so that the transparent curable resin layer is in contact with the surface; filling a portion of the transparent curable resin layer between the plurality of light emitting elements by thermocompression bonding; The method for producing a light-emitting electronic component further comprises curing the transparent curable resin layer by heating. Effect of the Invention
[0011] According to the integrated encapsulating sheet of the present invention, not only can resin be filled between multiple light-emitting elements, but also the encapsulating process can be completed with a single compression bonding operation, and further, no spots occur due to partial reduction in brightness, and blackness can be ensured while suppressing loss of overall brightness. Furthermore, according to the light-emitting electronic component and the method for producing a light-emitting electronic component of the present invention, a light-emitting electronic component can be easily obtained. [Brief description of the drawings]
[0012] [Figure 1] FIG. 1 is a schematic cross-sectional view of an integrated encapsulating sheet according to a first embodiment of the present invention. [Diagram 2] 1A to 1C are schematic explanatory diagrams of a method for manufacturing a light-emitting electronic component according to a first embodiment of the present invention. [Diagram 3] 1A to 1C are schematic explanatory diagrams of a method for manufacturing a light-emitting electronic component according to a first embodiment of the present invention. [Figure 4] 1A to 1C are schematic explanatory diagrams of a method for manufacturing a light-emitting electronic component according to a first embodiment of the present invention. [Diagram 5] 1A to 1C are schematic explanatory diagrams of a method for manufacturing a light-emitting electronic component according to a first embodiment of the present invention. [Figure 6]FIG. 4 is a schematic cross-sectional view of an integrated encapsulating sheet according to a third embodiment of the present invention. [Figure 7] 11A to 11C are schematic explanatory diagrams of a method for producing a light-emitting electronic component according to a third embodiment of the present invention. [Figure 8] 11A to 11C are schematic explanatory diagrams of a method for producing a light-emitting electronic component according to a third embodiment of the present invention. [Figure 9] 11A to 11C are schematic explanatory diagrams of a method for producing a light-emitting electronic component according to a third embodiment of the present invention. [Figure 10] 11A to 11C are schematic explanatory diagrams of a method for producing a light-emitting electronic component according to a third embodiment of the present invention. [Figure 11] FIG. 11 is a schematic cross-sectional view of an integrated encapsulating sheet according to a fourth embodiment of the present invention. [Figure 12] 11A to 11C are schematic explanatory diagrams of a method for producing a light-emitting electronic component according to a fourth embodiment of the present invention. [Figure 13] 11A to 11C are schematic explanatory diagrams of a method for producing a light-emitting electronic component according to a fourth embodiment of the present invention. [Figure 14] 11A to 11C are schematic explanatory diagrams of a method for producing a light-emitting electronic component according to a fourth embodiment of the present invention. [Figure 15] 11A to 11C are schematic explanatory diagrams of a method for producing a light-emitting electronic component according to a fourth embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] In this specification and claims, a numerical range expressed by "to" means a numerical range with the numerical values before and after "to" as the lower and upper limits.
[0014] First Embodiment <Integrated sealing sheet> An integrated encapsulating sheet 1A according to the first embodiment will be described with reference to Figures 1 and 2. As shown in Figure 1, the integrated encapsulating sheet 1A is basically configured by laminating a transparent curable resin layer 2 and a semitransparent film layer 3A.
[0015] The integrated encapsulating sheet 1A of the present embodiment may further have a protective film on the surface of either or both of the transparent curable resin layer 2 and the semitransparent film layer 3A for ease of handling. 1 shows an example in which protective films are provided on the surfaces of both the transparent curable resin layer 2 and the semitransparent film layer 3A. Specifically, the transparent curable resin layer 2, the semitransparent film layer 3A, and the second protective film 7 are laminated in this order on the first protective film 6. If the surface hardness of the semi-transparent film layer 3A is sufficient, the second protective film 7 can be omitted.
[0016] 2, the integrated encapsulating sheet 1A is used to fill spaces between a plurality of light-emitting elements (light-emitting element 12, light-emitting element 13, light-emitting element 14) of an element-mounted substrate 10 in which a plurality of light-emitting elements are arranged on a substrate 11. The details of the element-mounted substrate 10 will be described later. The integrated encapsulating sheet 1A is used such that the transparent curable resin layer 2 is in direct contact with the element-mounted substrate 10 during pressure bonding, as shown in FIG. A specific method for obtaining a light-emitting electronic component by pressure-bonding the integrated encapsulating sheet 1A to the element-mounted substrate 10 will be described later.
[0017] <Semi-transparent film layer> The semi-transparent film layer 3A is a layer for protecting the light-emitting element from external physical impact, humidity, moisture, etc. It is also a layer for increasing the blackness of the display and improving the contrast.
[0018] The semitransparent film layer 3A in this embodiment is composed of a support film layer 4 and a hard coat layer 5 laminated on the side of the support film layer 4 opposite to the transparent curable resin layer 2, the support film layer 4 being semitransparent and the hard coat layer 5 being transparent. The hard coat layer 5 may be omitted.
[0019] [Total light transmittance] The total light transmittance of the semi-transparent film layer 3A as a whole (in this embodiment, the combined total of the support film layer 4 and the hard coat layer 5) is preferably 20 to 80%, more preferably 20 to 65%, and even more preferably 20 to 55%. When the total light transmittance of the semitransparent film layer 3A is equal to or greater than the lower limit, the light is not prevented from reaching the viewer's side. When the total light transmittance of the semitransparent resin layer 8 is equal to or less than the upper limit, the degree of blackness is more easily ensured. When the total light transmittance is within the above range, the contrast is further improved.
[0020] [Storage modulus] The storage modulus of the semi-transparent film layer 3A as a whole (in this embodiment, the combination of the support film layer 4 and the hard coat layer 5) at 100° C. is 1.0×10 8 Pa or more, 1.0×10 10 Pa or less, and 1.0×10 9 Pa or higher, 9.0×10 9 Pa or less, and 3.0×10 9 Pa or higher, 8.0×10 9 It is more preferable that the pressure is 0.1 Pa or less.
[0021] By having the storage modulus of the translucent film layer 3A at 100°C be equal to or less than the preferred upper limit, appropriate flexibility is obtained that does not hinder the flow of the transparent curable resin layer 2 when it is pressure-bonded to the element-mounted substrate 10, improving workability and preventing cracks due to pressure.
[0022] Since the storage modulus of the semi-transparent film layer 3A at 100°C is equal to or greater than the preferred lower limit, the semi-transparent film layer 3A is less likely to deform when pressed against the element-mounted substrate 10, and pressure can be reliably transmitted to the transparent curable resin layer 2, preventing defects such as cracks and deformation in the semi-transparent resin layer 8 and the hard coat layer 5.
[0023] <Support film layer> The support film layer 4 in the semitransparent film layer 3A is a layer for protecting the light-emitting element from external physical impact, humidity, moisture, etc. In this embodiment, the support film layer 4 is made semitransparent so that the entire semitransparent film layer 3A can improve the contrast of the display.
[0024] [Total light transmittance] The support film layer 4 in the semitransparent film layer 3A is preferably adjusted so that the total light transmittance of the entire semitransparent film layer 3A is in the above-mentioned preferred range. The total light transmittance of the support film layer 4 alone in this embodiment is preferably 20 to 80%, more preferably 20 to 65%, and even more preferably 20 to 55%.
[0025] Since the total light transmittance of the support film layer 4 alone is within the above range, the total light transmittance of the entire translucent film layer 3A can be set within an appropriate range without specially adjusting the total light transmittance of the hard coat layer 5. When the semitransparent film layer 3A does not have the hard coat layer 5 and is composed of only the support film layer 4, the preferred range of the total light transmittance of the support film layer 4 is the same as that of the semitransparent film layer 3A.
[0026] [Storage modulus] The storage modulus of the support film layer 4 at 100° C. is 1.0×10 9 Pa or more, 1.0×10 10 Pa or less, and 2.0×10 9 Pa or higher, 9.0×10 9 Pa or less, and 3.0×10 9 Pa or higher, 8.0×10 9 It is more preferable that the pressure is 0.1 Pa or less.
[0027] When the storage modulus of the support film layer 4 at 100° C. is equal to or less than the preferred upper limit, appropriate flexibility is obtained, workability is improved, and cracks due to pressure can be prevented. When the storage modulus of the support film layer 4 at 100° C. is equal to or greater than the preferred lower limit, the support film layer 4 is less likely to deform when pressure-bonded to the element-mounted substrate 10, and pressure can be uniformly transmitted to the transparent curable resin layer 2. Furthermore, defects such as cracks and deformations are prevented from occurring in the hard coat layer 5.
[0028] [resin] The support film layer 4 may be made of a thermoplastic resin or a thermosetting resin. Examples of the resin constituting the support film layer 4 include polyethylene terephthalate resin, polyethylene 2,6-naphthalate resin, polycarbonate resin, triacetyl cellulose resin, polymethylpentene resin, phenoxy resin, syndiotactic polystyrene resin, polyimide resin, etc., and it is preferable that the support film layer 4 contains at least one resin selected from polyethylene terephthalate resin, polyethylene 2,6-naphthalate resin, and polycarbonate resin in terms of heat resistance, weather resistance, availability, cost, etc. By including these resins, deformation during compression bonding can be prevented.
[0029] [Black pigment or black dye] The support film layer 4 of the present embodiment is made semi-transparent. In order to make it semi-transparent, it preferably contains a black pigment or a black dye, more preferably contains a black pigment, and further preferably contains carbon black.
[0030] The particle size of the carbon black is preferably 10 to 500 nm, more preferably 10 to 300 nm, and particularly preferably 10 to 100 nm. The particle size refers to the average particle size, and can be determined by a measuring device using the dynamic light scattering method. An example of a measuring device using the dynamic light scattering method is NanotracWave II UT151 manufactured by Microtrack Bell.
[0031] The pH of carbon black based on ISO 787-9 is preferably 5 or less, more preferably 1 to 4.5, and even more preferably 2 to 4. By setting the pH of the carbon black to the preferred upper limit or lower, good dispersibility can be obtained and the blackness can be improved. By setting the pH of the carbon black to the preferred lower limit or higher, the dispersion treatment can be easily performed.
[0032] As the carbon black, one or more of known carbon blacks such as gas black, channel black, furnace black, thermal black, lamp black, etc. may be used. Resin-coated carbon black may also be used. Furthermore, carbon nanofibers and carbon nanotubes may also be used.
[0033] Among these, gas black, which is an acidic carbon, is preferred because it has a large amount of surface functional groups, has high dispersibility, and exhibits sufficient light diffusion prevention function even with a small amount added. Furthermore, when the support film layer 4 contains a high molecular weight resin having a weight average molecular weight of 20,000 or more and has functional groups, the dispersibility is further improved due to the interaction between the surface functional groups of the gas black and the functional groups of the epoxy resin and the high molecular weight resin, thereby ensuring good blackness.
[0034] The blending amount of carbon black is preferably 0.01 to 10 mass %, and more preferably 0.01 to 5 mass %, based on the total solid content of the support film layer 4. When the blending amount of carbon black is within the above range, an appropriate total light transmittance can be obtained.
[0035] [Dispersant] In order to improve the dispersibility of carbon black, it is preferable to blend a dispersant in the support film layer 4. When the pH of carbon black is 5 or less, it is preferable to blend a cationic dispersant from the viewpoint of stronger interaction with the functional groups on the surface of the carbon black and further improving dispersibility. Examples of cationic dispersants include polymer-type dispersants such as polyalkylene polyamines and cationic group-containing acrylic polymers, and surfactant-type dispersants such as quaternary ammonium salts and alkyl polyamines. Among them, polymer-type dispersants are preferable from the viewpoint of high dispersion stability. In particular, by blending a curable resin composition for forming a hard coat layer having a carboxy group, a sulfo group, a phosphate group, or an acid anhydride group thereof, carbon black having a pH of 5 or less, and a cationic dispersant, it is possible to exhibit higher dispersibility and dispersion stability of the carbon black.
[0036] When a cationic dispersant is used, the amount of the cationic dispersant added is preferably 10 to 200 parts by mass per 100 parts by mass of carbon black. When a cationic dispersant is used, the amine value of the dispersant is preferably from 10 to 150 mgKOH / g, and more preferably from 13 to 100 mgKOH / g.
[0037] [Other ingredients] The support film layer 4 may contain an inorganic filler in order to improve flame retardancy and heat resistance and to adjust the refractive index.
[0038] [Film thickness] The thickness of the support film layer 4 is preferably from 10 to 250 μm, more preferably from 20 to 200 μm, and further preferably from 25 to 150 μm. When the thickness of the support film layer 4 is equal to or greater than the preferred lower limit, the layer has sufficient strength to protect the element. When the thickness of the support film layer 4 is equal to or less than the preferred upper limit, the layer has improved visibility and costs can be reduced.
[0039] <Hard coat layer> The hard coat layer 5 in the semi-transparent film layer 3A is a layer for protecting the light-emitting electronic component from scratches.
[0040] [hardness] The pencil hardness of the surface of the hard coat layer 5 is preferably H or higher, more preferably 2H or higher, and even more preferably 3H or higher.
[0041] [Surface roughness] The surface roughness Ra of the hard coat layer 5 is preferably from 0.1 to 1.5 μm, more preferably from 0.2 to 1 μm, and even more preferably from 0.3 to 1 μm. By setting the surface roughness of the hard coat layer 5 to the preferred lower limit or more, it is possible to reduce the reflectance of the surface of the hard coat layer 5. By setting the surface roughness of the hard coat layer 5 to the preferred upper limit or less, production becomes easy.
[0042] [Total light transmittance] The hard coat layer 5 of the present embodiment is preferably prepared so that the total light transmittance is 30 to 99%, more preferably 50 to 99%, and even more preferably 60 to 99%. When the total light transmittance of the hard coat layer 5 is equal to or greater than the lower limit, light is not prevented from reaching the viewer's side.
[0043] [Curable resin composition] The hard coat layer 5 is composed of a curable resin composition. Examples of the curable resin composition constituting the hard coat layer 5 include a thermosetting resin composition, an ultraviolet curable resin composition, and an electron beam curable resin composition. Among them, an ultraviolet curable resin composition is preferred. Examples of the ultraviolet-curable resin composition include acrylic resin, urethane resin, silicone resin, and the like, and the composition may contain one or more of these. Examples of the thermosetting resin composition include acrylic resin, urethane resin, silicone resin, melamine resin, and the like, and the composition may contain one or more of these.
[0044] [Fine particles] The hard coat layer 5 preferably contains fine particles. As the fine particles, one or both of inorganic fine particles and organic fine particles can be used. Examples of inorganic fine particles include silica fine particles and titanium fine particles, and examples of organic fine particles include polymethyl methacrylate resin (PMMA resin) and urethane resin. Among these, silica fine particles are preferable. By including the fine particles, it is possible to adjust the surface roughness and improve the surface hardness.
[0045] [Film thickness] The thickness of the hard coat layer 5 is preferably from 1 to 20 μm, more preferably from 2 to 10 μm, and further preferably from 3 to 8 μm. When the thickness of the hard coat layer 5 is equal to or greater than the preferred lower limit, sufficient hardness can be ensured. When the thickness of the hard coat layer 5 is equal to or less than the preferred upper limit, defects such as curling do not occur. The hard coat layer 5 may contain a black pigment or black dye in order to suppress uneven light emission or color unevenness.
[0046] <Transparent curable resin layer> The transparent curable resin layer 2 is a layer that is filled between a plurality of light emitting elements arranged on the element-mounted substrate 10 and serves to protect the light emitting elements.
[0047] [Total light transmittance] The transparent curable resin layer 2 has a high total light transmittance. The total light transmittance of the transparent curable resin layer 2 is measured in a cured state. The transparent curable resin layer 2 is preferably prepared so that the total light transmittance in a cured state is 50% or more and is higher than the total light transmittance of the semitransparent film layer 3A, more preferably is prepared so that the total light transmittance is more than 75% and is higher than the total light transmittance of the semitransparent film layer 3A, and further preferably is prepared so that the total light transmittance is more than 80% and is 99.5% or less. When the total light transmittance of the transparent curable resin layer 2 in a cured state is equal to or greater than the lower limit, even if the transparent curable resin layer 2 in a cured state remains on the light emitting element, the light is not prevented from reaching the viewer.
[0048] [Storage modulus] Before being pressure-bonded to the element-mounted substrate 10 and cured, the transparent curable resin layer 2 is in an uncured or semi-cured state. The storage modulus of the transparent curable resin layer 2 before curing is 1.0×107 Pa or less, and 1.0×10 2 Pa or more, 1.0×10 6 Pa or less, and more preferably 1.0×10 3 Pa or more, 1.0×10 5 It is more preferable that the pressure is 0.1 Pa or less.
[0049] Since the storage modulus at 100°C of the transparent curable resin layer 2 before curing is within a preferred range, appropriate fluidity is obtained when the layer is pressed against the element-mounted substrate 10, and the layer can conform to the unevenness of the element-mounted substrate 10 caused by the multiple light-emitting elements and sufficiently fill in the gaps between the multiple light-emitting elements. When the storage modulus at 100°C of the transparent curable resin layer 2 before curing exceeds the preferred upper limit, the fluidity of the transparent curable resin layer 2 is insufficient, making it difficult to sufficiently fill spaces between a plurality of light emitting elements, and cracks are likely to occur in the transparent curable resin layer 2 during thermocompression bonding, resulting in crack-like defects. Furthermore, a large amount of the transparent curable resin layer 2 that has not flowed remains above the light emitting elements, and the surface of the integrated encapsulating sheet is likely to have an uneven shape in accordance with the light emitting elements, resulting in poor appearance.
[0050] When the storage modulus at 100°C of the transparent curable resin layer 2 before curing is below the preferable lower limit, the fluidity of the transparent curable resin layer 2 is too high, and the film thickness after thermocompression bonding is not uniform, and the integrated encapsulating sheet is likely to have an appearance defect such as an uneven shape on its surface.
[0051] [Curable resin composition] (High molecular weight resin) The curable resin composition constituting the transparent curable resin layer 2 preferably contains a high molecular weight resin having a weight average molecular weight of 20,000 to 1,000,000. The weight average molecular weight of the high molecular weight resin in the curable resin composition constituting the transparent curable resin layer 2 is more preferably 100,000 to 1,000,000, and further preferably 120,000 to 500,000.
[0052] Examples of the high molecular weight resin include epoxy resin, acrylic resin, polyester resin, polyurethane resin, polycarbonate resin, polyimide resin, acrylonitrile butadiene copolymer, styrene butadiene copolymer, vinyl acetate resin, and silicone resin. The high molecular weight resin preferably has flexibility that allows the cured product to have both toughness and chemical resistance, and is preferably an acrylic resin, an acrylonitrile butadiene copolymer, a styrene butadiene copolymer, a vinyl acetate resin, or a silicone resin, more preferably an elastomer thereof. These high molecular weight resins may be used alone or in combination of two or more.
[0053] The amount of the high molecular weight resin in the transparent curable resin layer 2 is preferably 5 to 100% by mass, more preferably 0 to 70% by mass, further preferably 1 to 70% by mass, and particularly preferably 5 to 50% by mass, relative to 100% by mass of the total resin solid content of the transparent curable resin layer 2. Within the above range, the storage modulus can be controlled, and appropriate fluidity during thermocompression bonding can be ensured. In addition, pressure unevenness during thermocompression bonding can be prevented, and a uniform appearance can be maintained. In addition, outflow of the resin outside the range can be prevented, and the film thickness after compression bonding can be ensured. When the content is equal to or more than the above lower limit, the film-formability is improved, and the distribution of film thickness can be narrowed when the curable resin composition is applied to form a film.
[0054] (curable resin) The curable resin in the transparent curable resin layer 2 may be at least one curable resin composition selected from epoxy resin, acrylic resin, polyester resin, and polyurethane resin. Among them, epoxy resin is preferred because it can be thermally cured at low temperature and has excellent heat resistance and reliability. The transparent curable resin layer 2 preferably contains a polyfunctional curable resin capable of forming a crosslinked structure with a high molecular weight resin.
[0055] In this specification and claims, an epoxy resin is a compound having an epoxy group in the molecule. The epoxy resin used in the present invention is preferably one having two or more epoxy groups in one molecule and corresponding to a multifunctional curing resin. This is because a crosslinked structure is formed by reaction with a modified resin having a functional group capable of reacting with an epoxy group, and the cured product can exhibit high heat resistance. In addition, when an epoxy resin having two or more epoxy groups is used, the degree of crosslinking with a curing agent having a functional group capable of reacting with an epoxy group is sufficient, and sufficient heat resistance can be obtained in the cured product.
[0056] Examples of epoxy resins having two or more epoxy groups in one molecule include bifunctional epoxy resins having two epoxy groups in the molecule, polyfunctional epoxy resins having three or more epoxy groups in the molecule, and high molecular weight epoxy resins having a weight average molecular weight of 10,000 or more. Epoxy resins obtained by hydrogenating these may also be used.
[0057] In this specification and claims, high molecular weight epoxy resins are not classified as difunctional epoxy resins or polyfunctional epoxy resins, but as high molecular weight epoxy resins, regardless of the number of epoxy groups in the molecule. In the present specification and claims, high molecular weight epoxy resins having a weight average molecular weight of 20,000 to 1,000,000 are classified as high molecular weight resins. The weight average molecular weight of the epoxy resin is a polystyrene-equivalent molecular weight measured by gel permeation chromatography.
[0058] Examples of epoxy resins include bisphenol-based epoxy resins such as bisphenol A type epoxy resins, bisphenol F type epoxy resins, or phenoxy type epoxy resins obtained by polymerizing these resins, and hydrogenated versions of these resins; novolac type epoxy resins such as phenol novolac epoxy resins, o-cresol novolac epoxy resins, bisphenol A novolac epoxy resins, xylene structure-containing novolac epoxy resins, and naphthol novolac type epoxy resins; glycidyl ester-based epoxy resins such as phthalic acid diglycidyl ester, isophthalic acid diglycidyl ester, terephthalic acid diglycidyl ester, p-hydroxybenzoic acid glycidyl ester, tetrahydrophthalic acid diglycidyl ester, succinic acid diglycidyl ester, adipic acid diglycidyl ester, sebacic acid diglycidyl ester, and trimellitic acid triglycidyl ester; ethylene glycol diglycidyl ether, propylene glycol diglycidyl ether, 1,4-butanediol diglycidyl ether, 1,6-hexanediol diglycidyl ether, glycidyl ether-based epoxy resins such as tetraglycidyl diglycidyl ether, trimethylolpropane triglycidyl ether, pentaerythritol tetraglycidyl ether, tetraphenyl glycidyl ether ethane, triphenyl glycidyl ether ethane, polyglycidyl ether of sorbitol, and polyglycidyl ether of polyglycerol; glycidyl amine-based epoxy resins such as triglycidyl isocyanurate and tetraglycidyl diaminodiphenylmethane; linear aliphatic epoxy resins such as epoxidized polybutadiene and epoxidized soybean oil; and special skeleton epoxy resins such as brominated bisphenol A type epoxy resins, phosphorus-containing epoxy resins, fluorine-containing epoxy resins, dicyclopentadiene skeleton-containing epoxy resins, naphthalene skeleton-containing epoxy resins, anthracene type epoxy resins, tertiary butyl catechol type epoxy resins, triphenylmethane type epoxy resins, tetraphenylethane type epoxy resins, biphenyl type epoxy resins, and bisphenol S type epoxy resins. However, the epoxy resins are not limited to these.
[0059] As the high molecular weight epoxy resin, a phenoxy type epoxy resin, an epoxy modified polybutadiene, a copolymer of glycidyl methacrylate and methyl methacrylate, a modified polymer obtained by epoxy modifying other resins, and the like can be used. These epoxy resins may be used alone or in combination of two or more.
[0060] From the viewpoint of being able to impart an appropriate viscosity during compression to the transparent curable resin layer 2, the transparent curable resin layer 2 preferably contains a high molecular weight epoxy resin having a weight average molecular weight of 10,000 to 100,000 (however, resins having a weight average molecular weight of 20,000 or more are classified as high molecular weight resins; the same applies below). From the viewpoint of having good compatibility with other resin components and being able to dissolve without mixing with a high boiling point solvent that may remain in the dry film even after drying, it is more preferable for the transparent curable resin layer 2 to contain a high molecular weight epoxy resin having a weight average molecular weight of 10,000 to 35,000.
[0061] By including a high molecular weight epoxy resin having a weight average molecular weight of 10,000 to 100,000 as the epoxy resin used in the transparent curable resin layer 2, the transparent curable resin layer 2 has an appropriate viscosity when heated, and therefore the storage modulus of the transparent curable resin layer 2 in the range of 100°C to 150°C can be adjusted to a preferred range. The high molecular weight epoxy resin used in the transparent curable resin layer 2 is preferably a phenoxy type epoxy resin because it has good compatibility with other epoxy resins.
[0062] Phenoxy type epoxy resin has a relatively large molecular weight among epoxy resins and has an appropriate viscosity when heated, so that the storage modulus of the transparent curable resin layer 2 can be adjusted to a preferred range in the range of 100°C to 150°C. In addition, unlike other thermoplastic resins such as polyester, phenoxy type epoxy resin can be cured as an epoxy resin, so that the crosslink density can be increased and the heat resistance of the cured product and the reliability of performance for long-term use are not impaired.
[0063] From the viewpoint of preventing uneven pressure during thermocompression bonding, the glass transition temperature of the phenoxy type epoxy resin used in the transparent curable resin layer 2 is preferably 100° C. or higher.
[0064] Specific examples of phenoxy type epoxy resins include "1256", "YX7200", "YX8100", and "YX7180" manufactured by Mitsubishi Chemical Corporation, "YP-50", "YP-50S", and "YP-70" manufactured by Nippon Steel Chemical & Material Co., Ltd., "N-690" manufactured by DIC Corporation, and "H-157" and "EXA-192" manufactured by DIC Corporation.
[0065] The content of the high molecular weight epoxy resin in the transparent curable resin layer 2 is preferably 30 to 80 mass%, more preferably 40 to 70 mass%, and even more preferably 45 to 60 mass%, relative to 100 mass% of the total resin solid content of the transparent curable resin layer 2. The preferred content of the phenoxy type epoxy resin in the transparent curable resin layer 2 is also the same.
[0066] Within the above range, the storage modulus can be controlled, and the storage modulus can be secured to compress the transparent curable resin layer 2 during thermocompression bonding. In addition, flow during thermal curing can be suppressed, and poor appearance after curing due to the generation of bubbles can be suppressed. In addition, toughness is improved, and crack-like defects are less likely to occur during thermocompression bonding. Furthermore, when it is equal to or less than the above upper limit, the crosslink density of the transparent curable resin layer 2 in a cured state can be increased, and the heat resistance and chemical resistance can be improved.
[0067] Furthermore, it is preferable that the epoxy resin used in the transparent curable resin layer 2 contains a polyfunctional epoxy resin. The polyfunctional epoxy resin can increase the crosslink density, thereby further improving the stability of the performance of the cured product of the epoxy resin composition for long-term use and also improving the heat resistance. In addition, since the viscosity in the range of 100°C to 150°C is lower than that of the phenoxy type epoxy resin, the storage modulus of the transparent curable resin layer 2 can be adjusted by combining it with the phenoxy type epoxy resin.
[0068] Specific examples of polyfunctional epoxy resins include "YX7700", "157S70", and "1032S60" manufactured by Mitsubishi Chemical Corporation, "NC7000L", "XD1000", and "EOCN-1020" manufactured by Nippon Kayaku Co., Ltd., "ESN485" manufactured by Nippon Steel Chemical & Material Co., Ltd., and "N-690", "N-695", and "HP-7200H" manufactured by DIC Corporation.
[0069] The blending amount of the polyfunctional epoxy resin in the transparent curable resin layer 2 is preferably 90% by mass or less, more preferably 10 to 80% by mass, and even more preferably 35 to 70% by mass, relative to 100% by mass of the total resin solid content of the transparent curable resin layer 2. Within the above range, the storage modulus of the transparent curable resin layer 2 during thermocompression bonding can be controlled, and heat resistance and chemical resistance can be imparted in the cured state.
[0070] From the viewpoint of ensuring sufficient fluidity during thermocompression bonding, the transparent curable resin layer 2 preferably contains an epoxy resin having a softening point or melting point of 120° C. or less. From the viewpoint of handleability and heat resistance of the cured product, it is more preferable that the transparent curable resin layer 2 contains an epoxy resin having a softening point or melting point of 50 to 105° C. By containing an epoxy resin having a softening point or melting point within the above range, it becomes possible to control the storage modulus.
[0071] The total amount of epoxy resin in the transparent curable resin layer 2 is preferably 10 to 100% by mass, more preferably 30 to 99% by mass, and even more preferably 50 to 95% by mass, relative to 100% by mass of the total resin solid content of the transparent curable resin layer 2. Within the above range, the storage modulus can be controlled. Furthermore, flow during thermal curing can be suppressed, and poor appearance after curing due to the generation of bubbles can be suppressed. Furthermore, when the amount is equal to or greater than the above lower limit, heat resistance in the cured state is improved.
[0072] (Elastomer) The elastomer corresponds to the high molecular weight resin in this specification. As the elastomer, a thermosetting elastomer, generally called "rubber", is preferable because it can provide excellent heat resistance. Examples of the thermosetting elastomer include acrylonitrile butadiene rubber (NBR), which is a random copolymer of butadiene and acrylonitrile, acrylic rubber, styrene butadiene rubber, vinyl acetate resin, silicone resin, and the like. Among them, NBR is preferable because it has good compatibility with epoxy resin, can control the fluidity of the transparent curable resin layer 2 at about 100°C, and has good adhesion to the element-mounted substrate 10.
[0073] The weight average molecular weight of the elastomer is preferably 100,000 to 1,000,000, more preferably 120,000 to 500,000, and further preferably 150,000 to 300,000. When the weight average molecular weight of the elastomer is within the above range, the storage modulus of the transparent curable resin layer 2 can be controlled, and the flowability during thermocompression bonding can be ensured. When the weight average molecular weight of the elastomer is equal to or less than the above upper limit, the compatibility with the epoxy resin is improved, and the flowability during thermal curing can be more effectively controlled.
[0074] In particular, when the curable resin constituting the transparent curable resin layer 2 is an epoxy resin, it is preferable to include a modified elastomer having a functional group capable of reacting with an epoxy group. A modified elastomer having a functional group capable of reacting with an epoxy group also acts as a curing agent for the epoxy resin. In addition, since it can react and bond with the epoxy resin, the heat resistance and reliability against thermal shock are improved. Furthermore, the difference in polarity between the functional group capable of reacting with the epoxy resin and the resin skeleton has a favorable effect on dispersibility, and good dispersibility can be obtained when carbon black is contained in the transparent curable resin layer 2.
[0075] Examples of functional groups capable of reacting with an epoxy group include acid groups such as a carboxy group, a sulfo group, a nitro group, and a phosphoric acid group, as well as their acid anhydride groups, a hydroxyl group, and an amino group. Among these, an acid group or an acid anhydride group is preferred, and a carboxy group or a carboxylic acid anhydride group is particularly preferred, since they can be cured at low temperatures and can ensure a long pot life.
[0076] That is, when the curable resin constituting the transparent curable resin layer 2 is an epoxy resin, it preferably contains an acid-modified elastomer having an acid group or an acid anhydride group, more preferably contains an acid-modified elastomer having a carboxy group, and particularly preferably contains modified NBR having a carboxy group.
[0077] The modified NBR having a carboxy group is preferably a carboxylated acrylonitrile rubber into which acrylic acid, methacrylic acid, maleic anhydride, etc. are introduced. Commercially available products of the carboxylated acrylonitrile rubber include Nipol (registered trademark) NX775 and Nipol 1072CGJ manufactured by Zeon Corporation. Two or more types of modified elastomers having a functional group capable of reacting with an epoxy group may be used in combination.
[0078] The preferred content of the elastomer in the transparent curable resin layer 2 is the same as the preferred content of the high molecular weight resin in the transparent curable resin layer 2 .
[0079] (hardening agent) When the thermosetting resin constituting the transparent curable resin layer 2 is an epoxy resin, it may contain a curing agent for epoxy resin other than the modified elastomer having a functional group capable of reacting with an epoxy group. Examples of the other curing agent include known curing agents such as phenol-based curing agents, acid anhydride-based curing agents, and amine-based curing agents. Two or more types of the other curing agents may be used in combination.
[0080] (curing catalyst) When the transparent curable resin layer 2 is made of an epoxy resin composition, it may contain a curing catalyst that promotes the curing reaction of the epoxy resin. Examples of the curing catalyst include imidazole-based, tertiary amine-based, phosphorus compound-based, etc. Among them, imidazole-based catalysts are preferred because they have good compatibility with epoxy resins and are less likely to cause yellowing. Among imidazole-based curing catalysts, those having a cyanoethyl group are particularly preferred because they are easily soluble in epoxy resins.
[0081] The blending amount of the curing catalyst is preferably 0.01 to 5 parts by mass, more preferably 0.05 to 4 parts by mass, and further preferably 0.1 to 3 parts by mass, relative to 100 parts by mass of the total resin solid content of the transparent curable resin layer 2. When it is within the above range, curing can be sufficiently promoted and the pot life of the integrated encapsulating sheet 1A can be ensured. Two or more types of curing catalysts may be used in combination.
[0082] (Other Ingredients) The transparent curable resin layer 2 may contain a black pigment or black dye in order to suppress uneven light emission or color unevenness. From the viewpoint of increasing the total light transmittance, when the transparent curable resin layer 2 contains carbon black, the blending amount thereof is preferably less than 5 parts by mass, more preferably 1 part by mass or less, and even more preferably 0.1 part by mass or less, relative to 100 parts by mass of the total resin solid content. The transparent curable resin layer 2 may further contain, as necessary, a resin other than the epoxy resin and the elastomer, a thickener, a defoaming agent and / or a leveling agent, an adhesion imparting agent such as a coupling agent, and a flame retardant.
[0083] <Optical properties of the entire integrated laminate sheet> [Total light transmittance] The total light transmittance of the entire integrated laminate sheet, which in this embodiment is the total light transmittance of the three layers consisting of the transparent curable resin layer 2, the support film layer 4 in the semi-transparent film layer 3A, and the hard coat layer 5, is preferably 10 to 80%, more preferably 15 to 70%, and even more preferably 20 to 55%. By setting the total light transmittance of the three layers to be equal to or greater than the lower limit, light is not prevented from reaching the viewer's side. By setting the total light transmittance of the three layers to be equal to or less than the upper limit, the effect of improving the contrast of the display is enhanced.
[0084] [Glossiness] The gloss of the outermost surface of the integrated laminate sheet (in this embodiment, the outermost surface of the semi-transparent film layer 3A opposite the transparent curable resin layer 2 (the surface on the hard coat layer 5 side)) measured with a gloss meter (JIS-Z-8741) is preferably 0.01 to 35, more preferably 3 to 30, and even more preferably 5 to 25. When the gloss of the outermost surface is equal to or higher than the lower limit, the production is easy. When the gloss of the outermost surface is equal to or lower than the preferable upper limit, the visibility of the display is improved.
[0085] <Protective film> The first protective film 6 and the second protective film 7 (hereinafter, the first protective film 6 and the second protective film 7 may be collectively referred to simply as "protective films") have a role of protecting the integrated encapsulating sheet 1A, and can also be used as a film onto which a coating liquid of a curable resin composition is applied when forming the integrated encapsulating sheet 1A.
[0086] Examples of the protective film that can be used include polyester films such as polyethylene terephthalate and polyethylene naphthalate, films made of thermoplastic resins such as polyimide films, polyamideimide films, polyethylene films, polytetrafluoroethylene films, polypropylene films, and polystyrene films, as well as surface-treated paper.
[0087] Among these, polyester films can be preferably used from the viewpoints of heat resistance, mechanical strength, ease of handling, etc. The thickness of the protective film is not particularly limited, but is appropriately selected from the range of about 10 to 150 μm depending on the application. The surface of the protective film on which the resin layer is provided may be subjected to a release treatment.
[0088] <Manufacturing method of integrated encapsulating sheet> To obtain the integrated encapsulating sheet 1A, first, a first protective film 6 is coated with a coating liquid of a curable resin composition for the transparent curable resin layer 2 and dried, and a support film layer 4 on which a hard coat layer 5 has been formed in advance is prepared.
[0089] These are then stacked and laminated so that the transparent curable resin layer 2 and the support film layer 4 are in contact with each other, thereby obtaining a laminate in which the transparent curable resin layer 2, the support film layer 4, and the hard coat layer 5 are sequentially laminated on the first protective film 6. If necessary, the second protective film 7 is laminated on the surface of this hard coat layer 5. If the hardness of the hard coat layer 5 is sufficient, the second protective film 7 does not need to be laminated. The hard coat layer 5 formed on the support film layer 4 can be obtained by applying a coating agent for the hard coat layer to the surface of the support film layer 4, drying and curing the coating agent.
[0090] The hard coat layer 5 formed on the support film layer 4 can be obtained by applying a coating liquid of a curable resin composition for forming a hard coat layer to the surface of the support film layer 4, drying and curing the coating liquid. The coating liquid of the curable resin composition for forming a hard coat layer can be cured by heat curing, ultraviolet curing, electron beam curing, or the like.
[0091] Examples of methods for applying the coating liquid of the coating agent for the hard coat layer and the curable resin composition for the transparent curable resin layer 2 include various coaters such as a die coater, a gravure coater, a roll coater, a curtain flow coater, a spin coater, a bar coater, a reverse coater, a kiss coater, a fountain coater, a rod coater, an air doctor coater, a knife coater, a blade coater, a cast coater, and a screen coater. The drying temperature is preferably from 60 to 160°C, more preferably from 80 to 130°C, and further preferably from 90 to 120°C.
[0092] The coating agent for the hard coat layer and the coating liquid of the curable resin composition for the transparent curable resin layer 2 preferably contain an organic solvent in an amount that gives a viscosity that allows coating to be carried out without hindrance. The organic solvent is not particularly limited, and examples thereof include ketones, aromatic hydrocarbons, glycol ethers, glycol ether acetates, esters, alcohols, aliphatic hydrocarbons, petroleum-based solvents, etc. Specific examples of the organic solvent include ketones such as methyl ethyl ketone, cyclohexanone, methyl butyl ketone, and methyl isobutyl ketone; aromatic hydrocarbons such as toluene, xylene, and tetramethylbenzene; glycol ethers such as cellosolve, methyl cellosolve, butyl cellosolve, carbitol, methyl carbitol, butyl carbitol, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol monobutyl ether, propylene glycol monomethyl ether, dipropylene glycol monomethyl ether, dipropylene glycol diethyl ether, and triethylene glycol monoethyl ether; ethyl acetate, butyl acetate, isobutyl acetate, ethylene glycol diethyl ether, and triethylene glycol monoethyl ether; Examples of the solvent include esters such as propylene glycol monoethyl ether acetate, dipropylene glycol methyl ether acetate, propylene glycol methyl ether acetate, propylene glycol ethyl ether acetate, and propylene glycol butyl ether acetate; alcohols such as ethanol, propanol, 2-methoxypropanol, n-butanol, isobutyl alcohol, isopentyl alcohol, ethylene glycol, and propylene glycol; aliphatic hydrocarbons such as octane and decane; petroleum solvents such as petroleum ether, petroleum naphtha, hydrogenated petroleum naphtha, and solvent naphtha, as well as N,N-dimethylformamide (DMF), tetrachloroethylene, and turpentine.
[0093] When carbon black is blended into the coating liquid, carbon black powder or a carbon black dispersion may be added.
[0094] The temperature during lamination is preferably 20 to 120° C., more preferably 30 to 100° C., and even more preferably 40 to 80° C. By setting the temperature during lamination to a preferable lower limit or higher, it is possible to ensure adhesion between the transparent curable resin layer 2 and the support film layer 4 that allows handling even in an uncured or semi-cured state. In addition, by setting the temperature during lamination to a preferable upper limit or lower, it is possible to prevent the formation of air bubbles and wrinkles. The lamination can be carried out using a roll laminator, a press, a vacuum press, or the like.
[0095] <Substrate with elements> As shown in Fig. 2, the element-mounted substrate 10 has a plurality of light-emitting elements arranged on a substrate 11. Fig. 2 and other figures show a schematic view of a portion where three light-emitting elements (light-emitting element 12, light-emitting element 13, and light-emitting element 14) are arranged.
[0096] There is no limitation on the material of the substrate 11, but a known printed circuit board can be suitably used. Examples of known printed circuit boards include a glass epoxy board, a fluororesin board, and a ceramic board. The light emitting element is typically a light emitting diode, and the present invention is particularly suitable for use in cases where the light emitting element is extremely small.
[0097] For example, a light emitting diode having a height of 1000 nm to 200 μm and a side length of 0.001 to 0.5 mm can be used. In the element-mounted substrate 10 for obtaining mini LEDs or micro LEDs, light-emitting diodes of three colors R, G, and B can be used as the light-emitting elements, or a blue light-emitting diode can be used as the light-emitting element.
[0098] <Method of manufacturing light-emitting electronic components> The method for manufacturing the light-emitting electronic component of this embodiment is a method in which the integrated encapsulating sheet 1A of this embodiment is placed on the surface of an element-mounted substrate on which a plurality of light-emitting elements are arranged, so that the transparent curable resin layer 2 is in contact with the surface, and the sheet is thermocompressed to fill a portion of the transparent curable resin layer 2 between the plurality of light-emitting elements, and the transparent curable resin layer 2 is cured by heating. Hereinafter, a method for producing a light-emitting electronic component according to one embodiment of the present invention will be described with reference to FIGS.
[0099] In the manufacturing method of this embodiment, first, as shown in FIG. 2, an integrated encapsulating sheet 1A from which the first protective film 6 has been peeled off to expose the transparent curable resin layer 2 is placed on the surface of the element-mounted substrate 10 on which the light-emitting elements 12, 13, and 14 are arranged, so that the transparent curable resin layer 2 is in contact with the surface.
[0100] At this time, that is, before pressure bonding, the thickness of the transparent curable resin layer 2 is preferably 110 to 550% of the height of the light emitting element, preferably 120 to 400%, and more preferably 150 to 300%.
[0101] If the thickness of the transparent curable resin layer 2 is equal to or greater than the above-mentioned lower limit with respect to the height of the light emitting element, the curable resin can be sufficiently embedded between the light emitting elements. If the thickness of the transparent curable resin layer 2 is equal to or less than the above upper limit relative to the height of the light emitting element, unevenness in thickness is unlikely to occur during compression bonding, and poor appearance is unlikely to occur.
[0102] In this state shown in FIG. 2, the sheets are thermocompression bonded to each other, so that parts of the transparent curable resin layer 2 of the integrated encapsulating sheet 1A are embedded between the light emitting elements as shown in FIG. In this case, it is preferable that the transparent curable resin layer 2 has a relatively low storage modulus and ensures fluidity, since it can easily fill between the light emitting elements while conforming to the irregularities caused by the light emitting elements.
[0103] The temperature in thermocompression bonding is preferably 80 to 120° C., and more preferably 90 to 110° C. By setting the temperature in thermocompression bonding to 80° C. or higher, the fluidity of the transparent curable resin layer 2 is easily ensured. Furthermore, by setting the temperature in thermocompression bonding to 120° C. or lower, the light emitting element is less likely to be damaged. By setting the temperature in thermocompression bonding to 90 to 110° C., the fluidity can be controlled more precisely, and the occurrence of unevenness or crack-like defects can be suppressed.
[0104] The pressure in the thermocompression bonding is preferably 0.05 to 1.0 MPa, and more preferably 0.1 to 0.5 MPa. By setting the pressure in the thermocompression bonding to the preferred lower limit or more, the transparent curable resin layer can be sufficiently filled between the light emitting elements. By setting the pressure to the preferred upper limit or less, the light emitting elements are less likely to be damaged.
[0105] The thermocompression bonding is preferably carried out using a vacuum press capable of molding in a vacuum state, which makes it easier to avoid defects caused by air being mixed into the obtained light-emitting electronic component.
[0106] After the pressure bonding, the second protective film 7 is peeled off as shown in Fig. 4, and then the resultant is thermally cured to convert the transparent curable resin layer 2 of the integrated encapsulating sheet 1A into a transparent curable resin cured product layer 22 (the transparent curable resin layer 2 in a cured state) as shown in Fig. 5. In this way, a light-emitting electronic component 30A is obtained.
[0107] The curing temperature is 100 to 160° C., and preferably 120 to 150° C. By setting the curing temperature to 100° C. or higher, the transparent curable resin layer 2 can be cured. By setting the curing temperature to 120° C. or higher, the curing time of the transparent curable resin layer 2 can be shortened. Furthermore, by setting the curing temperature to the above upper limit temperature or lower, the light emitting element is less likely to be damaged.
[0108] The curing time varies depending on the curing temperature, but is preferably from 30 to 360 minutes, and more preferably from 45 to 180 minutes. It is preferable that the transparent curable resin layer 2 has a relatively high storage modulus and reduced fluidity at the curing temperature, since this reduces defects in appearance after curing. As a result, a light-emitting electronic component 30A is obtained in which the integrated encapsulating sheet 1A is pressure-bonded to the surface of the element-mounted substrate 10, in which a plurality of light-emitting elements are arranged on the substrate 11, on which the light-emitting elements are arranged.
[0109] In the obtained light-emitting electronic component 30A, the transparent cured resin layer 2 is cured to become a transparent cured resin layer 22, and a part of the transparent cured resin layer 22 fills spaces between a plurality of light-emitting elements.
[0110] Second Embodiment <Semi-transparent film layer> The second embodiment is similar to the first embodiment, except that the hard coat layer 5 in the semitransparent film layer 3A is semitransparent. The total light transmittance and storage modulus at 100° C. of the entire semitransparent film layer 3A are also similar to those of the first embodiment. Similarly to the first embodiment, the integrated encapsulating sheet 1A of this embodiment is used such that the transparent curable resin layer 2 is in direct contact with the element-mounted substrate 10 during pressure bonding, as shown in FIG.
[0111] <Support film layer> [Total light transmittance] The total light transmittance of the support film layer 4 alone is preferably from 30 to 99%, more preferably from 50 to 95%, and even more preferably from 70 to 95%. When the total light transmittance of the support film layer 4 alone is equal to or greater than the above lower limit, an inexpensive commercially available film can be used.
[0112] The preferred storage modulus of the support film layer 4, the resin constituting the support film layer 4, and other components are the same as those of the support film layer 4 in the first embodiment.
[0113] <Hard coat layer> The hard coat layer 5 in the semi-transparent film layer 3A is a layer for protecting the light-emitting electronic component from scratches. The hard coat layer 5 in this embodiment is semi-transparent.
[0114] [Total light transmittance] The hard coat layer 5 of this embodiment is preferably prepared so that the total light transmittance of the entire semitransparent film layer 3A is in the above-mentioned preferred range of 20 to 80%. The total light transmittance of the hard coat layer 5 alone is preferably prepared so as to be 20 to 80%, more preferably 30 to 65%, and further preferably 20 to 55%. When the total light transmittance of the hard coat layer 5 alone is equal to or greater than the lower limit, light is not prevented from reaching the viewer's side. When the total light transmittance of the hard coat layer 5 alone is equal to or less than the upper limit, a transparent, inexpensive, commercially available film can be used as the support film layer 4.
[0115] [Overall haze] The hard coat layer 5 of this embodiment preferably has an overall haze based on JIS K 7136 of 50% or more, more preferably 60 to 95%, and even more preferably 70 to 90%. When the overall haze of the hard coat layer 5 is equal to or more than the preferred lower limit, the ability to conceal diffuse reflection of external light in the support film layer 4 is improved. When the overall haze of the hard coat layer 5 is equal to or less than the preferred upper limit, light is not prevented from reaching the viewer's side.
[0116] The preferred hardness, surface roughness and thickness of the hard coat layer 5 are the same as those in the first embodiment. The curable resin composition constituting the hard coat layer 5 is similar to the curable resin composition constituting the hard coat layer 5 in the first embodiment, except that it contains a black pigment or black dye to achieve an appropriate total light transmittance.
[0117] The black pigment or black dye is the same as the black pigment or black dye described in the first embodiment as being blended in the support film layer 4, and the preferred embodiments are also the same. The blending amount of carbon black is preferably 0.01 to 10 mass %, and more preferably 0.01 to 5 mass %, based on the total solid content of the hard coat layer 5. When the blending amount of carbon black is within the above range, an appropriate total light transmittance can be obtained.
[0118] The total light transmittance of the entire integrated laminate sheet, i.e., the preferred total light transmittance of the entire three layers, i.e., the transparent curable resin layer 2, the support film layer 4 in the semitransparent film layer 3A, and the hard coat layer 5, is the same as in the first embodiment. The preferred range of the gloss of the outermost surface of the integrated laminate sheet, i.e., the gloss of the outermost surface (the surface on the hard coat layer 5 side) of the semitransparent film layer 3A opposite to the transparent curable resin layer 2, measured with a gloss meter (JIS-Z-8741) is also the same as in the first embodiment. In addition, the first protective film 6 and the second protective film 7 can be the same as in the first embodiment.
[0119] The manufacturing method of the integrated encapsulating sheet of the second embodiment is similar to the manufacturing method of the integrated encapsulating sheet 1A of the first embodiment. Moreover, a method for manufacturing a light-emitting electronic component using the integrated encapsulating sheet of the second embodiment is similar to the method for manufacturing a light-emitting electronic component using the integrated encapsulating sheet 1A of the first embodiment.
[0120] Third Embodiment The third embodiment will be described below. In the description of the third embodiment, the same components as those in the first embodiment are denoted by the same reference numerals, and detailed description thereof will be omitted.
[0121] <Integrated sealing sheet> An integrated encapsulating sheet 1B according to a third embodiment will be described with reference to Figures 6 and 7. As shown in Figure 6, the integrated encapsulating sheet 1B is similar to the integrated encapsulating sheet 1A of the first embodiment, except that the semitransparent film layer 3A is changed to a semitransparent film layer 3B. Like the integrated encapsulating sheet 1A, the integrated encapsulating sheet 1B is used such that the transparent curable resin layer 2 is in direct contact with the element-mounted substrate 10 during pressure bonding, as shown in FIG.
[0122] <Semi-transparent film layer> The semi-transparent film layer 3B of this embodiment is a layer for protecting the light-emitting element from external physical impact, humidity, moisture, etc. It is also a layer for increasing the blackness of the display and improving the contrast.
[0123] The semitransparent film layer 3B is composed of a support film layer 4, a semitransparent resin layer 8 and a hard coat layer 5, which are laminated in this order on the side of the support film layer 4 opposite to the side in contact with the transparent curable resin layer 2. The hard coat layer 5 may be omitted. The preferred ranges of the total light transmittance and storage modulus at 100° C. of the entire semitransparent film layer 3B are similar to those of the semitransparent film layer 3A of the first embodiment.
[0124] <Support film layer> The preferred total light transmittance of the support film layer 4 is the same as the preferred total light transmittance of the support film layer 4 in the second embodiment.
[0125] The preferred storage modulus of the support film layer 4 at 100° C. is the same as that of the support film layer 4 in the first embodiment. The resin constituting the support film layer 4 may be the same as that of the support film layer 4 in the first embodiment. From the viewpoint of increasing the total light transmittance, when the support film layer 4 contains carbon black, the amount of carbon black blended is preferably less than 5 parts by mass, more preferably 1 part by mass or less, and even more preferably 0.1 part by mass or less, per 100 parts by mass of the total resin solids.
[0126] <Translucent resin layer 8> The semitransparent resin layer 8 of the present embodiment is a layer that increases the blackness of the display and improves the contrast. In addition, it is a layer for making diffuse reflection of external light from the support film layer 4 less visible.
[0127] [Total light transmittance] The total light transmittance of the semitransparent resin layer 8 is preferably 20 to 80%, more preferably 30 to 65%, and further preferably 20 to 55%. When the total light transmittance of the semitransparent resin layer 8 is equal to or greater than the lower limit, light is not prevented from reaching the viewer's side. When the total light transmittance of the semitransparent resin layer 8 is equal to or less than the upper limit, the light diffusion prevention effect and the contrast improvement effect are further improved.
[0128] [Overall haze] The semitransparent resin layer 8 preferably has an overall haze based on JIS K 7136 of 7% or more, more preferably 10 to 70%, and even more preferably 15 to 65%. When the overall haze of the semitransparent resin layer 8 is equal to or greater than the preferred lower limit, the ability to conceal diffuse reflection of external light in the support film layer 4 is improved. When the overall haze of the semitransparent resin layer 8 is equal to or less than the preferred upper limit, the degree of blackness is increased. The overall haze of the semitransparent resin layer 8 can be adjusted by the compatibility of the carbon black, filler, and resin contained in the semitransparent resin composition.
[0129] [Storage modulus] The storage modulus of the semi-transparent resin layer 8 at 100° C. is 1.0×10 6 Pa or more, and 1.0×10 6 Pa or more, 1.0×10 10 Pa or less, and more preferably 1.0×10 7 Pa or more, 5.0×10 9 More preferably, the pressure is 1.0×10 Pa or less. 8 Pa or more, 5.0×10 9 It is particularly preferable that the pressure is 0.1 Pa or less.
[0130] If the thickness of the semitransparent resin layer 8 varies, the degree of blackness may become non-uniform in the surface direction, which may cause spots. By having the storage modulus of the semitransparent resin layer 8 at 100°C be equal to or greater than the preferable lower limit, the semitransparent resin layer 8 is less likely to deform when pressure-bonded to the element-mounted substrate 10, and the thickness is less likely to vary. Therefore, uneven light emission and color can be suppressed.
[0131] When the storage modulus at 100° C. of the semitransparent resin layer 8 is equal to or less than the preferred upper limit, it is easy to prevent the occurrence of cracks during pressure bonding to the element-mounted substrate 10. In addition, it is easy to ensure adhesion between the semitransparent resin layer 8 and the support film layer 4 or the hard coat layer 5.
[0132] [Translucent resin composition] The semitransparent resin layer 8 can be composed of a coating film of a semitransparent resin composition containing carbon black or the like, or a cured product thereof. The semitransparent resin composition is a thermoplastic resin composition or a curable resin composition, and is preferably a curable resin composition from the viewpoint of being less likely to deform during durability tests under thermal shock or high humidity. When the semitransparent resin composition is a curable resin composition, it is preferably a cured film from the viewpoints of being less prone to deformation and having stable coloration. In other words, it is preferably cured before being pressure-bonded to the element-mounted substrate 10.
[0133] The semitransparent resin composition preferably contains the aforementioned high molecular weight resin having a weight average molecular weight of 20,000 to 1,000,000. By containing the high molecular weight resin, the coatability is improved when the coating liquid for forming the semitransparent resin layer 8 is applied to the support film layer 4. Therefore, the uniformity of the blackness is further improved. When the translucent resin composition is a curable resin composition, it may contain, in addition to the high molecular weight resin, a curable resin in which a crosslinking reaction proceeds by heat and / or light.
[0134] The weight average molecular weight of the high molecular weight resin contained in the semitransparent resin composition constituting the semitransparent resin layer 8 is 20,000 to 1,000,000, preferably 100,000 to 500,000, and more preferably 150,000 to 300,000.
[0135] When the weight average molecular weight of the high molecular weight resin is 20,000 or more, the coating property of the semi-transparent resin layer is improved, and color unevenness caused by unevenness in the film thickness due to dripping or the like can be prevented. When the weight average molecular weight of the high molecular weight resin is 100,000 or more, the film-forming property of the semi-transparent resin layer is improved, and color loss caused by pinholes can be prevented. When the weight average molecular weight of the high molecular weight resin is 150,000 or more, toughness can be imparted to the semi-transparent resin layer, and cracks caused by pressure during thermocompression bonding can be prevented. When the weight average molecular weight of the high molecular weight resin is equal to or less than the upper limit, compatibility with other components is improved, light scattering caused by phase separation of the resin can be suppressed, and total light transmittance is stabilized.
[0136] The high molecular weight resin used in the semitransparent resin layer 8 preferably has at least one functional group selected from the group consisting of a carboxy group, a sulfo group, a phosphoric acid group, and an acid anhydride group thereof, as well as a hydroxyl group, an amino group, an acrylic group, a methacrylic group, a vinyl group, an ester group, a urethane group, a urea group, and an imide group. When the resin has such a functional group, the difference in polarity between the functional group and the resin skeleton acts favorably on dispersibility, and good dispersibility can be obtained when carbon black is contained in the semitransparent resin layer 8. Among these, those having a carboxy group, an acid anhydride group, an amino group, an acrylic group, a methacrylic group, or a vinyl group are preferred, since they can form a crosslinked structure with the curable resin when cured, and are less likely to deform when pressed and cause thickness variations.
[0137] The blending amount of the high molecular weight resin in the translucent resin composition constituting the translucent resin layer 8 is preferably 10% by mass or more, and more preferably 20 to 80% by mass, relative to 100% by mass of the total resin solid content of the translucent resin composition. When the blending amount of the high molecular weight resin is equal to or more than the above lower limit, the film-formability is improved, and the distribution of the film thickness can be narrowed when a coating liquid of the translucent resin composition is applied to form a film. In addition, when the high molecular weight resin has the above-mentioned preferred functional group, when the blending amount is equal to or more than the above lower limit, the dispersibility of carbon black is improved.
[0138] Examples of the high molecular weight resin in the translucent resin composition constituting the translucent resin layer 8 include epoxy resin, acrylic resin, polyester resin, polyurethane resin, polycarbonate resin, polyimide resin, acrylonitrile butadiene copolymer, styrene butadiene copolymer, vinyl acetate resin, and silicone resin. When the translucent resin composition is a thermoplastic resin composition, the high molecular weight resin preferably has an elastic modulus that does not deform when pressed, and is preferably an acrylic resin, a polyester resin, or a polyimide resin.
[0139] When the translucent resin composition is a curable resin composition, the high molecular weight resin preferably has flexibility that allows the cured product to have both toughness and chemical resistance, and is preferably an acrylic resin, an acrylonitrile butadiene copolymer, a styrene butadiene copolymer, a vinyl acetate resin, or a silicone resin, more preferably an elastomer thereof. These high molecular weight resins may be used alone or in combination of two or more.
[0140] (Elastomer) When the translucent resin composition is a curable resin composition, the elastomer is preferably a thermosetting elastomer, generally called "rubber", because it has excellent heat resistance. Examples of the thermosetting elastomer include acrylonitrile butadiene rubber (NBR), which is a random copolymer of butadiene and acrylonitrile, acrylic rubber, styrene butadiene rubber, vinyl acetate resin, silicone resin, etc. When the curable resin is an epoxy resin, it is preferably NBR, which has good compatibility.
[0141] The weight average molecular weight of the elastomer is preferably 100,000 to 1,000,000, and more preferably 150,000 to 300,000. When the weight average molecular weight of the elastomer is within the above range, the compatibility with the curable resin can be increased while maintaining sufficient flexibility, thereby imparting high toughness to the cured product.
[0142] In particular, when the curable resin is an epoxy resin, it is preferable to include a modified elastomer having a functional group capable of reacting with an epoxy group. A modified elastomer having a functional group capable of reacting with an epoxy group also acts as a curing agent for the epoxy resin. In addition, since it can react and bond with the epoxy resin, reliability against thermal shock is improved. Furthermore, the difference in polarity between the functional group capable of reacting with the epoxy resin and the resin skeleton has a favorable effect on dispersibility, and good dispersibility can be obtained when carbon black is contained in the translucent resin layer 8.
[0143] The functional group capable of reacting with the epoxy group is preferably a carboxy group, an acid anhydride group, or an amino group. In particular, since it is possible to cure at low temperatures and the change in viscosity of the coating liquid over time is suppressed, an acid group or an acid anhydride group is preferred, and a carboxy group or a carboxylic anhydride group is more preferred. In other words, it is particularly preferred to contain a modified NBR having a carboxy group.
[0144] The modified NBR having a carboxy group is preferably a carboxylated acrylonitrile rubber into which acrylic acid, methacrylic acid, maleic anhydride, etc. are introduced. Commercially available products of the carboxylated acrylonitrile rubber include Nipol (registered trademark) NX775 and Nipol 1072CGJ manufactured by Zeon Corporation.
[0145] (curable resin) The curable resin forms a crosslinked structure by heat and / or light, and can impart a storage modulus that does not deform when pressed to the cured product of the translucent resin composition and reliability in durability tests. Examples of the curable resin include epoxy resin, acrylic resin, isocyanate, melamine resin, silicone resin, etc. Among them, epoxy resin or acrylic resin is preferred because it can be cured at low temperature and has excellent heat resistance and reliability.
[0146] The epoxy resin may be the same as those mentioned in the description of the transparent curable resin in the first embodiment. Among these, the epoxy resin used in the translucent resin composition is preferably a multifunctional epoxy resin, from the viewpoints of obtaining a sufficient crosslink density after curing and being less susceptible to cracking during thermocompression bonding. Among the polyfunctional epoxy resins, novolac-type epoxy resins are particularly preferred because they are epoxy resins to which an appropriate flexible skeleton can be introduced and which enable the storage modulus of the cured product to be adjusted within an appropriate range.
[0147] Specific examples of novolac-type epoxy resins used in the translucent resin composition include "YX7700" manufactured by Mitsubishi Chemical Corporation, "NC7000L", "XD1000", and "EOCN-1020" manufactured by Nippon Kayaku Co., Ltd., "ESN485" manufactured by Nippon Steel Chemical & Material Co., Ltd., and "N-690" and "N-695" manufactured by DIC Corporation.
[0148] (hardening agent) The translucent resin composition may contain a curing agent capable of curing the curable resin. When the curable resin is an epoxy resin, the curing agent may be a known curing agent such as a phenol-based curing agent, an acid anhydride-based curing agent, or an amine-based curing agent. When the curable resin is an acrylic resin, the curing agent may be a known curing agent such as a photoradical initiator or a peroxide. Two or more types of curing agents may be used in combination.
[0149] (curing catalyst) The translucent resin composition may contain a curing catalyst that accelerates the curing reaction of the curable resin. The curing catalyst may be an imidazole type, a tertiary amine type, a phosphorus compound type, or the like. Two or more types of curing catalysts may be used in combination.
[0150] (Black pigment or black dye) The semitransparent resin layer 8 is semitransparent. In order to make it semitransparent, the semitransparent resin composition preferably contains a black pigment or a black dye, more preferably contains a black pigment, and further preferably contains carbon black. The preferred aspects of the carbon black are the same as those in the support film layer 4 of the first embodiment.
[0151] The amount of carbon black is preferably 0.01 to 10 mass % based on the total solid content of the translucent resin composition, and more preferably 0.01 to 5 mass %. When the amount of carbon black is within the above range, an appropriate total light transmittance can be obtained.
[0152] The translucent resin composition may contain a cationic dispersant to enhance the dispersibility of carbon black. Examples of the cationic dispersant include those similar to those described for the support film layer 4 of the first embodiment. When a cationic dispersant is used, the amount of the cationic dispersant added is preferably 10 to 150% by mass relative to the carbon black.
[0153] (Other Ingredients) The translucent resin composition may contain an inorganic filler in order to improve flame retardancy and heat resistance and to adjust the refractive index. The translucent resin composition may further contain, as necessary, a resin other than the epoxy resin and the elastomer, a thickener, a defoamer and / or a leveling agent, an adhesion imparting agent such as a coupling agent, and a flame retardant.
[0154] [Film thickness] The thickness of the semitransparent resin layer 8 is preferably 0.1 to 50 μm, more preferably 2 to 30 μm, and further preferably 5 to 15 μm. By making the thickness of the semitransparent resin layer 8 equal to or greater than the preferred lower limit, it is possible to suppress variations in the film thickness during film formation. By making the thickness of the semitransparent resin layer 8 equal to or less than the preferred upper limit, it is possible to suppress costs.
[0155] <Hard coat layer> The hard coat layer 5 is a layer for protecting the light-emitting electronic component from scratches. As the hard coat layer 5, the same one as the hard coat layer 5 in the first embodiment can be used, and the preferred aspects are also the same.
[0156] <Transparent curable resin layer> The transparent curable resin layer 2 in this embodiment can be the same as the transparent curable resin layer 2 in the first embodiment, and the preferred aspects are also the same.
[0157] <Optical properties of the entire integrated laminate sheet> [Total light transmittance] The total light transmittance of the entire integrated laminate sheet, which in this embodiment is the total light transmittance of the four layers, namely the transparent curable resin layer 2, the support film layer 4, the semitransparent resin layer 8, and the hard coat layer 5, is preferably 10 to 80%, more preferably 15 to 70%, and even more preferably 20 to 55%. By setting the total light transmittance of the four layers to be equal to or greater than the lower limit, light is not prevented from reaching the viewer's side. By setting the total light transmittance of the four layers to be equal to or less than the upper limit, the effect of improving the contrast of the display is enhanced.
[0158] [Glossiness] The gloss of the outermost surface of the integrated laminate sheet (in this embodiment, the outermost surface of the semi-transparent film layer 3B opposite the transparent curable resin layer 2 (the surface on the hard coat layer 5 side)) measured with a gloss meter (JIS-Z-8741) is preferably 0.01 to 35, more preferably 3 to 30, and even more preferably 5 to 25. When the gloss of the outermost surface is equal to or higher than the lower limit, the production is easy. When the gloss of the outermost surface is equal to or lower than the preferable upper limit, the visibility of the display is improved.
[0159] <Protective film> As the first protective film 6 and the second protective film 7, the same protective films as those in the first embodiment can be used, and the preferred aspects are also the same.
[0160] <Manufacturing method of integrated encapsulating sheet> To obtain the integrated encapsulating sheet 1B, first, a first protective film 6 is coated with a coating liquid of a curable resin composition for the transparent curable resin layer 2 and dried, and a support film layer 4 is provided on which a translucent resin layer 8 and a hard coat layer 5 are sequentially formed in advance.
[0161] These are then stacked and laminated so that the transparent curable resin layer 2 and the support film layer 4 are in contact with each other, thereby obtaining a laminate in which the transparent curable resin layer 2, the support film layer 4, the translucent resin layer 8, and the hard coat layer 5 are sequentially stacked on the first protective film 6. If necessary, the second protective film 7 is laminated on the surface of this hard coat layer 5. If the hardness of the hard coat layer 5 is sufficient, the second protective film 7 does not need to be laminated.
[0162] The support film layer 4 having the translucent resin layer 8 and the hard coat layer 5 formed in sequence can be obtained by applying and drying a coating liquid of a translucent resin composition for the translucent resin layer 8 on the surface of the support film layer 4, applying and drying a coating agent for the hard coat layer, and then curing the coating agent. The coating agent for the hard coat layer may be applied after the semi-transparent resin composition is cured.
[0163] The application methods of the coating liquid of the translucent resin composition for the translucent resin layer 8, the coating liquid of the curable resin composition for the transparent curable resin layer 2, and the coating agent for the hard coat layer are similar to the application methods of the coating agent for the hard coat layer and the coating liquid of the curable resin composition for the transparent curable resin layer 2 in the first embodiment. The curing method for the coating liquid of the curable resin composition for the semitransparent resin layer 8 and the coating agent for the hard coat layer may be heat curing, ultraviolet curing, electron beam curing, or the like.
[0164] As in the first embodiment, the coating liquid of the curable resin composition for the transparent curable resin layer 2 preferably contains an organic solvent in an amount that gives a viscosity that allows coating to be carried out without hindrance. As the organic solvent, the same ones as those exemplified in the first embodiment can be used. The coating liquid of the curable resin composition for the transparent curable resin layer 2 can be applied in the same manner as described in the first embodiment.
[0165] <Method of manufacturing light-emitting electronic components> The method for producing a light-emitting electronic component of the present invention is a method in which the integrated encapsulating sheet 1B of the present invention is placed on the surface of an element-mounted substrate on which a plurality of light-emitting elements are arranged, so that the transparent curable resin layer 2 is in contact with the surface, and the sheet is thermocompressed to fill a portion of the transparent curable resin layer 2 between the plurality of light-emitting elements, and the transparent curable resin layer 2 is cured by heating. Hereinafter, a method for producing a light-emitting electronic component according to one embodiment of the present invention will be described with reference to FIGS.
[0166] In the manufacturing method of this embodiment, first, as shown in Figure 7, an integrated encapsulating sheet 1B from which the first protective film 6 has been peeled off to expose the transparent curable resin layer 2 is placed on the surface of the element-mounted substrate 10 on which the light-emitting elements 12, 13, and 14 are arranged, so that the transparent curable resin layer 2 is in contact with the surface. At this time, that is, before pressure bonding, the preferred ratio of the thickness of the transparent curable resin layer 2 to the height of the light emitting element is the same as that in the first embodiment.
[0167] 7, thermocompression bonding is performed to embed a part of the transparent curable resin layer 2 of the integrated encapsulating sheet 1B between the light emitting elements as shown in Fig. 8. The preferable temperature and pressure in the thermocompression bonding are the same as those in the first embodiment.
[0168] After the pressure bonding, the second protective film 7 is peeled off as shown in Fig. 9, and then the resultant is thermally cured to convert the transparent curable resin layer 2 of the integrated encapsulating sheet 1B into a transparent curable resin cured product layer 22 (the transparent curable resin layer 2 in a cured state) as shown in Fig. 10. In this way, a light-emitting electronic component 30B is obtained. The preferred aspects of the curing temperature and curing time are the same as those in the first embodiment.
[0169] In the obtained light-emitting electronic component 30B, the transparent cured resin layer 2 is cured to become a transparent cured resin layer 22, and a part of the transparent cured resin layer 22 fills spaces between a plurality of light-emitting elements.
[0170] Fourth Embodiment The fourth embodiment will be described below. In the description of the fourth embodiment, the same components as those in the first embodiment are denoted by the same reference numerals, and detailed description thereof will be omitted.
[0171] <Integrated sealing sheet> An integrated encapsulating sheet 1C according to a fourth embodiment will be described with reference to Figures 11 and 12. As shown in Figure 11, the integrated encapsulating sheet 1B is similar to the integrated encapsulating sheet 1A of the first embodiment, except that the semitransparent film layer 3A is changed to a semitransparent film layer 3C. The integrated encapsulating sheet 1C is used in a manner that the transparent curable resin layer 2 is in direct contact with the element-mounted substrate 10 during pressure bonding, as shown in FIG.
[0172] <Semi-transparent film layer> The semi-transparent film layer 3C of this embodiment is a layer for protecting the light-emitting element from external physical impact, humidity, moisture, etc. It is also a layer for increasing the blackness of the display and improving the contrast.
[0173] The semitransparent film layer 3C is composed of a support film layer 4, a semitransparent resin layer 8 provided on the transparent curable resin layer 2 side of the support film layer 4, and a hard coat layer 5 provided on the side opposite to the side in contact with the transparent curable resin layer 2. The hard coat layer 5 may be omitted. The total light transmittance and storage modulus at 100° C. of the entire semitransparent film layer 3C are similar to those of the semitransparent film layer 3A of the first embodiment.
[0174] <Support film layer> As the support film layer 4, the same material as the support film layer 4 in the third embodiment can be used, and the preferred aspects are also the same.
[0175] <Translucent resin layer 8> The semitransparent resin layer 8 of this embodiment is a layer that prevents light diffusion between light emitting elements and improves the contrast of the display. The preferred total light transmittance and overall haze of the semitransparent resin layer 8 are similar to those of the semitransparent resin layer 8 of the third embodiment.
[0176] The preferred storage modulus of the semitransparent resin layer 8 at 100° C. is similar to that of the semitransparent resin layer 8 in the third embodiment, and the preferred range is also similar. The storage modulus of the semi-transparent resin layer 8 at 25° C. is 1.0×10 9 Pa or less, and 1.0×10 6 Pa or more, 1.0×10 9 Pa or less, and more preferably 1.0×10 7 Pa or more, 1.0×10 9 It is more preferable that the pressure is 0.1 Pa or less.
[0177] Since the storage modulus at 25°C is equal to or less than the preferred upper limit, the semitransparent resin layer 8 can exert a primer effect of enhancing the adhesion of the transparent curable resin layer 2 to the support film layer 4. This can prevent whitening, which is a decrease in the degree of blackness caused by the occurrence of lifting between the support film layer 4 and the transparent curable resin layer 2, when cutting off unnecessary parts of the substrate end portion of the light-emitting electronic component on which the integrated encapsulating sheet is mounted. In addition, since the storage modulus at 25°C is equal to or more than the preferred lower limit, whitening due to the occurrence of burrs in the support film layer 4 can be prevented when cutting off unnecessary parts.
[0178] The semitransparent resin layer 8 can be made of the same curable resin composition or thermoplastic resin composition as the semitransparent resin layer 8 of the third embodiment.
[0179] The semitransparent resin layer 8 is semitransparent. To make it semitransparent, it preferably contains a black pigment or a black dye, more preferably contains a black pigment, and even more preferably contains carbon black. The preferred aspects and preferred blending amount of carbon black are the same as those of the semitransparent resin layer 8 in the third embodiment. Also, as in the semitransparent resin layer 8 in the third embodiment, a cationic dispersant may be blended to enhance the dispersibility of carbon black. The preferred thickness of the semitransparent resin layer 8 is similar to the preferred thickness of the semitransparent resin layer 8 in the third embodiment.
[0180] <Hard coat layer> The hard coat layer 5 is a layer for protecting the light-emitting electronic component from scratches. As the hard coat layer 5, the same one as the hard coat layer 5 in the first embodiment can be used, and the preferred aspects are also the same.
[0181] <Transparent curable resin layer> The transparent curable resin layer 2 in this embodiment can be the same as the transparent curable resin layer 2 in the first embodiment, and the preferred aspects are also the same.
[0182] <Optical properties of the entire integrated laminate sheet> [Total light transmittance] The total light transmittance of the entire integrated laminate sheet, which in this embodiment is the total light transmittance of the four layers, namely the transparent curable resin layer 2, the semitransparent resin layer 8, the support film layer 4, and the hard coat layer 5, is preferably 10 to 80%, more preferably 15 to 70%, and even more preferably 20 to 55%. By setting the total light transmittance of the four layers to be equal to or greater than the lower limit, light is not prevented from reaching the viewer's side. By setting the total light transmittance of the four layers to be equal to or less than the upper limit, the effect of improving the contrast of the display is enhanced.
[0183] [Glossiness] The gloss of the outermost surface of the integrated laminate sheet (in this embodiment, the outermost surface of the semi-transparent film layer 3C opposite the transparent curable resin layer 2 (the surface on the hard coat layer 5 side)) measured with a gloss meter (JIS-Z-8741) is preferably 0.01 to 35, more preferably 3 to 30, and even more preferably 5 to 25. When the gloss of the outermost surface is equal to or higher than the lower limit, the production is easy. When the gloss of the outermost surface is equal to or lower than the preferable upper limit, the visibility of the display is improved.
[0184] <Protective film> As the first protective film 6 and the second protective film 7, the same protective films as those in the first embodiment can be used, and the preferred aspects are also the same.
[0185] <Manufacturing method of integrated encapsulating sheet> To obtain the integrated encapsulating sheet 1C, first, a first protective film 6 is coated with a coating liquid of a curable resin composition for the transparent curable resin layer 2 and dried, and a support film layer 4 is prepared having a semi-transparent resin layer 8 formed on one surface thereof and a hard coat layer 5 formed on the other surface thereof.
[0186] Then, these are stacked and laminated so that the transparent curable resin layer 2 and the translucent resin layer 8 are in contact with each other, thereby obtaining a laminate in which the transparent curable resin layer 2, the translucent resin layer 8, the support film layer 4, and the hard coat layer 5 are stacked in that order on the first protective film 6. If necessary, the second protective film 7 is laminated on the surface of this hard coat layer 5. If the hardness of the hard coat layer 5 is sufficient, the second protective film 7 does not need to be laminated.
[0187] A film having a translucent resin layer 8 on one surface of a support film layer 4 and a hard coat layer 5 on the other surface thereof can be obtained by applying and drying a coating liquid of a translucent resin composition for the translucent resin layer 8 on one surface of the support film layer 4, applying and drying a coating agent for the hard coat layer on the other surface, and then curing these two layers. The application of the coating agent for the hard coat layer may be performed after curing the translucent resin composition for the translucent resin layer 8. The application of the coating liquid of the translucent resin composition for the translucent resin layer 8 may be performed after curing the coating agent for the hard coat layer.
[0188] The application method of the coating liquid of the translucent resin composition for the translucent resin layer 8, the coating agent for the hard coat layer, and the coating liquid of the curable resin composition for the transparent curable resin layer 2 is the same as the application method of the coating agent for the hard coat layer and the coating liquid of the curable resin composition for the transparent curable resin layer 2 in the first embodiment. The coating liquid of the semitransparent resin composition for the semitransparent resin layer 8 and the coating agent for the hard coat layer may be cured by heat curing, ultraviolet curing, electron beam curing, or the like.
[0189] As in the first embodiment, the coating liquid of the translucent resin composition, the coating liquid of the curable resin composition for the transparent curable resin layer 2, and the coating agent for the hard coat layer preferably contain an organic solvent in an amount that gives a viscosity that allows for unhindered application. As the organic solvent, the same ones as those exemplified in the first embodiment can be used.
[0190] <Method of manufacturing light-emitting electronic components> The method for producing a light-emitting electronic component of the present invention is a method in which the integrated encapsulating sheet 1C of the present invention is placed on the surface of an element-mounted substrate on which a plurality of light-emitting elements are arranged, so that the transparent curable resin layer 2 is in contact with the surface, and the sheet is thermocompressed to fill a portion of the transparent curable resin layer 2 between the plurality of light-emitting elements, and the transparent curable resin layer 2 is cured by heating. Hereinafter, a method for manufacturing a light-emitting electronic component according to one embodiment of the present invention will be described with reference to FIGS.
[0191] In the manufacturing method of this embodiment, first, as shown in Figure 12, an integrated encapsulating sheet 1C from which the first protective film 6 has been peeled off to expose the transparent curable resin layer 2 is placed on the surface of the element-mounted substrate 10 on which the light-emitting elements 12, 13, and 14 are arranged, so that the transparent curable resin layer 2 is in contact with the surface. At this time, that is, before pressure bonding, the preferred ratio of the thickness of the transparent curable resin layer 2 to the height of the light emitting element is the same as that in the first embodiment.
[0192] 12, thermocompression bonding is performed to embed a part of the transparent curable resin layer 2 of the integrated encapsulating sheet 1C between the light emitting elements as shown in Fig. 13. The preferable temperature and pressure in the thermocompression bonding are the same as those in the first embodiment.
[0193] The thermocompression bonding is preferably carried out using a vacuum press capable of molding in a vacuum state, which makes it easier to avoid defects caused by air being mixed into the obtained light-emitting electronic component.
[0194] After the pressure bonding, the second protective film 7 is peeled off as shown in Fig. 14, and then the resultant is thermally cured to make the transparent curable resin layer 2 of the integrated encapsulating sheet 1C into a transparent curable resin cured product layer 22 (the transparent curable resin layer 2 in a cured state) as shown in Fig. 15. In this way, a light-emitting electronic component 30C is obtained.
[0195] In the obtained light-emitting electronic component 30C, the transparent cured resin layer 2 is cured to become a transparent cured resin layer 22, and a part of the transparent cured resin layer 22 fills spaces between a plurality of light-emitting elements.
[0196] Other Aspects The translucent film layer in the integrated sealing sheet of the present invention may be a single layer, or may be only a translucent support film layer. In the case of a multi-layer structure, the number of layers is not limited. For example, the hard coat layer may be omitted. In addition, other functional layers such as an anti-reflection layer may be laminated. In the case of a multi-layered film, it is sufficient to have one or more semi-transparent layers. For example, a semi-transparent resin layer may be provided on both sides of a support film layer. In addition, both the support film layer and the hard coat layer may be semi-transparent film layers. Alternatively, one or both of the support film layer and the hard coat layer may be semi-transparent, and a semi-transparent resin layer may be provided on one or both sides of the support film layer.
[0197] <Action and Effect> According to the integrated encapsulating sheet of the present invention, the resin layer filled between the light emitting elements is a transparent curable resin layer, so that etching of the black curable resin layer on the light emitting elements is not required. Furthermore, by providing a semi-transparent film layer, the degree of blackness can be increased when the light emitting element is turned off, and contrast can be improved.
[0198] The translucent film layer is unlikely to vary in thickness in the surface direction even when pressed together with an uncured or semi-cured transparent curable resin layer, so that there is no risk of localized reduction in brightness resulting in spots. Furthermore, according to the light-emitting electronic component and the method for producing a light-emitting electronic component of the present invention, a light-emitting electronic component can be easily obtained. EXAMPLES
[0199] The present invention will be described in detail below with reference to examples, but the present invention is not limited to the description of these examples. Note that the blend amounts in the following description are all calculated on a solid content basis.
[0200] <Raw materials> Details of the raw materials used in each of the examples and comparative examples are as follows. [Epoxy resin] EOCN (registered trademark)-1020-55: Manufactured by Nippon Kayaku Co., Ltd., cresol novolac type multifunctional epoxy resin (solid), softening point 55.7°C, epoxy equivalent 195g / eq. EPICLON(registered trademark) HP-7200H: Manufactured by DIC, cyclopentadiene novolac type multifunctional epoxy resin (solid), softening point 82°C, epoxy equivalent 227g / eq.
[0201] [High molecular weight resin] jER (registered trademark) YX7200B35: Manufactured by Mitsubishi Chemical Corporation, a phenoxy-type epoxy resin (MEK solution, solid content 35 mass%), an epoxy resin having a glass transition temperature of 150°C, an epoxy equivalent of 8750 g / eq., and a weight average molecular weight of 27,218. · Nipol NX775: Manufactured by Zeon Corporation, carboxy-modified nitrile rubber, elastomer with a weight average molecular weight of 208,000.
[0202] [Curing catalyst] Curesol (registered trademark) 2PZ-CN: 1-cyanoethyl-2-phenylimidazole, manufactured by Shikoku Chemical Industry Co., Ltd. · Curesol 2E4MZ: Shikoku Chemical Industry Co., Ltd., 2-ethyl-4-methylimidazole.
[0203] [Carbon black] Special Black 4: ORION ENGINEERED CARBONS, gas black, pH 3, average particle size 25 nm.
[0204] [solvent] MEK: Methyl ethyl ketone, manufactured by Junsei Chemical Co., Ltd. PGM: Propylene glycol monomethyl ether, manufactured by Junsei Chemical Co., Ltd.
[0205] [Support film layer] -Cosmoshine (registered trademark) A4300: Toyobo Co., Ltd., PET film, thickness 75 μm. Film 1: Polycarbonate film containing 0.075% by mass of carbon black (Special Black 4), manufactured by Shin-Etsu Polymer, thickness 75 μm. Film 2: Polycarbonate film containing 0.04% by mass of carbon black (Special Black 4), manufactured by Shin-Etsu Polymer, thickness 75 μm.
[0206] [Removable PET] · 1-E: Made by Nippa, thickness 50μm.
[0207] [Resin for hard coat layer] 8KX-078: Taisei Fine Chemical Co., Ltd., solid content 40% by mass, UV-curable acrylic polymer, weight average molecular weight 40,000. 8KQ-2001: Taisei Fine Chemical Co., Ltd., solid content 40% by mass, UV-curable acrylic polymer having carboxyl, hydroxyl and methacrylic groups, weight average molecular weight 20,000, acid value 130 mgKOH / g.
[0208] [Fine particles] Chemisnow (registered trademark) MX-500L: manufactured by Soken Chemical & Engineering Co., Ltd., cross-linked acrylic monodisperse particles, average particle diameter 5 μm. [Photoradical polymerization initiator] Omnirad(R) TPO H: Manufactured by IGM Resins BV.
[0209] <Preparation of coating solution> [Coating agent for hard coat layer] The raw materials having the composition shown in Table 1 were mixed in a solvent of MEK / PGM=80 / 20 (volume ratio) to prepare coating agents (raw materials 1-1 to 1-2) for the hard coat layer having a solid content concentration of 25 mass %.
[0210] [Table 1]
[0211] [Coating liquid of semi-transparent resin composition] The raw materials having the composition shown in Table 2 were mixed in a solvent of MEK / PGM=80 / 20 (volume ratio) to prepare a coating liquid of a semitransparent resin composition (raw materials 2-1 to 2-2) for a semitransparent resin layer having a solid content concentration of 25 mass %. That is, the total amount of the raw materials having the composition shown in Table 2 (converted into solid content) was 25 mass % with respect to the entire coating liquid obtained.
[0212] [Table 2]
[0213] [Coating liquid for transparent curable resin layer] 40 parts by mass of epoxy resin EOCN-1020-55 (manufactured by Nippon Kayaku Co., Ltd.), 40 parts by mass of epoxy resin jER YX7200B35 (manufactured by Mitsubishi Chemical Corporation), 20 parts by mass of elastomer Nipol NX775 (manufactured by Nippon Zeon Co., Ltd.), and 3 parts by mass of curing catalyst Curesol 2PZ-CN (manufactured by Shikoku Kasei Co., Ltd.) were mixed in a solvent of MEK / PGM = 80 / 20 (volume ratio) to prepare a coating liquid for transparent curable resin layer with a solids concentration of 50 mass% as raw material 3-1. The glass transition temperature of Raw Material 3-1 after curing was 54.1°C.
[0214] In addition, 50 parts by mass of epoxy resin EOCN-1020-55 (manufactured by Nippon Kayaku Co., Ltd.), 30 parts by mass of epoxy resin jER YX7200B35 (manufactured by Mitsubishi Chemical Corporation), 20 parts by mass of elastomer Nipol NX775 (manufactured by Nippon Zeon Co., Ltd.), and 3 parts by mass of curing catalyst Curesol 2PZ-CN (manufactured by Shikoku Kasei Co., Ltd.) were mixed in a solvent of MEK / PGM = 80 / 20 (volume ratio) to prepare a coating liquid for transparent curable resin layer with a solids concentration of 50 mass% as raw material 3-2. The glass transition temperature of Raw Material 3-2 after curing was 44.7°C.
[0215] [Coating liquid for black curable resin layer] 70 parts by mass of epoxy resin EPICLON HP-7200H (manufactured by DIC Corporation), 30 parts by mass of elastomer Nipol NX775 (manufactured by Nippon Zeon Corporation), 3 parts by mass of curing catalyst Curesol 2PZ-CN (manufactured by Shikoku Kasei Corporation), and 4 parts by mass of carbon black Special Black 4 (manufactured by Orion Engineered Carbons) were mixed in a solvent of MEK / PGM = 80 / 20 (volume ratio) to prepare a coating liquid for a black curable resin layer with a solids concentration of 50 mass% as raw material 4. The glass transition temperature of Raw Material 4 after curing was 37.4°C.
[0216] <Total light transmittance> [Support film layer] The total light transmittance of Cosmoshine A4300 (manufactured by Toyobo Co., Ltd.) was measured in accordance with JIS K 7361 using a haze meter NDH5000 manufactured by Nippon Denshoku Industries Co., Ltd. The same measurement was also carried out for Film 1 and Film 2.
[0217] [Hard coat layer] The total light transmittance of the hard coat layer in each example described later was measured by applying the coating agent for the hard coat layer to Cosmoshine A4300 using a bar coater so that the dry film thickness was as shown in Table 3, drying at 120°C for 5 minutes, and then measuring 400 mJ / cm 2 The coating agent for the hard coat layer was cured by irradiation with ultraviolet light of 1000 nm to obtain a film with a hard coat layer.
[0218] The total light transmittance of the obtained film with a hard coat layer was measured using a haze meter NDH5000 manufactured by Nippon Denshoku Industries Co., Ltd. in accordance with JIS K 7361, with the transmitted light of Cosmoshine A4300 being taken as 100%.
[0219] [Translucent resin layer] The total light transmittance of the translucent resin layer in each example described below was measured by applying a coating solution of the translucent resin composition to Cosmoshine A4300 (manufactured by Toyobo Co., Ltd.) using an applicator so that the dry film thickness was the film thickness shown in Table 3, drying at 120°C for 5 minutes, and then heating in a hot air circulating oven at 80°C for 72 hours to harden the translucent resin composition and obtain a film with a translucent resin layer. The total light transmittance of the obtained film with a semi-transparent resin layer was measured in the same manner as for the film with a hard coat layer, with the transmitted light through Cosmoshine A4300 being set as 100%.
[0220] [Transparent curable resin layer] The total light transmittance of the transparent curable resin layer in each example described below was measured by applying the coating liquid for the transparent curable resin layer to Cosmoshine A4300 (manufactured by Toyobo Co., Ltd.) using an applicator so that the dry film thickness was 80 μm (30 μm in Comparative Example 1), drying at 120° C. for 5 minutes, and then heating in a hot air circulating oven at 150° C. for 1 hour to cure the coating liquid for the transparent curable resin layer, thereby obtaining a film with a cured transparent curable resin layer. The total light transmittance of the obtained cured film with a transparent curable resin layer was measured in the same manner as for the film with a hard coat layer, with the transmitted light through Cosmoshine A4300 being set as 100%. The measurement results of the total light transmittance of the support film layer and each layer are shown in Table 3.
[0221] <Storage modulus> The coating liquid for the transparent curable resin layer was applied to the release surface of release PET 1-E (Nippa Corporation, 50 μm) using an applicator so that the dry film thickness was 40 μm. After drying at 120° C. for 5 minutes, the release PET 1-E was peeled off to obtain a single-layer sheet of the transparent curable resin layer and the black curable resin layer.
[0222] The storage modulus at 100°C of each of the obtained monolayer sheets and the storage modulus at 100°C of the film layer (Cosmoshine A4300: manufactured by Toyobo Co., Ltd.) were measured using a viscoelasticity measuring device (RSA-G2 manufactured by TA Instruments Co., Ltd.) at a measurement frequency of 1 Hz and a heating rate of 5°C / min according to JIS K7244. The results are shown in Table 3.
[0223] <Example> [Example 1] A coating solution of the translucent resin composition (raw material 2-1) was applied to the first surface of a support film layer (Cosmoshine A4300: manufactured by Toyobo Co., Ltd.) using a bar coater so that the dry film thickness was as shown in Table 3. The coating was then dried at 120°C for 5 minutes and then heated in a hot air circulating oven at 80°C for 72 hours to harden the translucent resin composition and form a lower translucent resin layer. Next, a corona treatment was performed on the second surface of the support film layer opposite to the lower semi-transparent resin layer, and a coating agent for a hard coat layer (raw material 1-1) was applied using a bar coater so that the dry film thickness was as shown in Table 3. Then, after drying at 120°C for 5 minutes, 400 mJ / cm 2 The coating agent for the hard coat layer was cured by irradiating it with ultraviolet light of 1000 nm to obtain a first sheet in which the lower semitransparent resin layer and the hard coat layer were supported by the support film layer.
[0224] Further, the coating liquid for the transparent curable resin layer (raw material 3-1) was applied to the lower semi-transparent resin layer on the first surface of the support film layer of this first sheet using an applicator so that the dry film thickness was 80 μm. Then, it was dried at 120° C. for 5 minutes to obtain a second sheet in which the lower semi-transparent resin layer and the transparent curable resin layer were supported on the first surface of the support film layer and the hard coat layer was supported on the second surface of the support film layer.
[0225] The obtained second sheet and release PET 1-E (manufactured by Nippa Corporation, 50 μm) were overlapped so that the transparent curable resin layer was in contact with the release surface of the release PET 1-E, and laminated with a roll laminator at 60°C to obtain an integrated sealing sheet of Example 1.
[0226] [Example 2] A coating solution of a translucent resin composition (raw material 2-1) was applied to the first surface of a support film layer (Cosmoshine A4300: manufactured by Toyobo Co., Ltd.) using a bar coater so that the dry film thickness was the thickness shown in Table 3, and after drying at 120°C for 5 minutes, the translucent resin composition was cured by heating in a hot air circulating oven at 80°C for 72 hours to form an upper translucent resin layer. Next, a corona treatment was performed on the surface of the upper translucent resin layer opposite the support film layer, and a coating agent for a hard coat layer (raw material 1-1) was applied using a bar coater so that the dry film thickness was the thickness shown in Table 3. Then, after drying at 120°C for 5 minutes, 400 mJ / cm 2 The coating agent for the hard coat layer was cured by irradiating it with ultraviolet light of 1000 nm to obtain a third sheet in which the upper semitransparent resin layer and the hard coat layer were supported by the support film layer.
[0227] Further, the coating solution for the transparent curable resin layer was applied to the second surface of the support film layer of the third sheet using an applicator so that the dry thickness was 80 μm, and then dried at 120° C. for 5 minutes to obtain a fourth sheet having an upper semi-transparent resin layer and a hard coat layer supported on the first surface of the support film layer and a transparent curable resin layer supported on the second surface of the support film layer. The obtained fourth sheet and release PET 1-E (manufactured by Nippa Corporation, 50 μm) were overlapped so that the transparent curable resin layer was in contact with the release surface of the release PET 1-E, and laminated with a roll laminator at 60°C to obtain an integrated encapsulating sheet of Example 2.
[0228] [Example 3] A coating agent for a hard coat layer (raw material 1-2) was applied to the first surface of a support film layer (Cosmoshine A4300: manufactured by Toyobo Co., Ltd.) using a bar coater so that the dry film thickness was as shown in Table 3. Then, after drying at 120°C for 5 minutes, 400 mJ / cm 2 The coating agent for the hard coat layer was cured by irradiation with ultraviolet light of 1000 nm to obtain a fifth sheet having a hard coat layer supported by a support film layer.
[0229] The coating solution for the transparent curable resin layer was applied to the second surface of the support film layer of the fifth sheet using an applicator so that the dry thickness was 80 μm, and then dried at 120° C. for 5 minutes to obtain a sixth sheet having a hard coat layer supported on the first surface of the support film layer and a transparent curable resin layer supported on the second surface of the support film layer. The obtained sixth sheet and release PET 1-E (manufactured by Nippa Corporation, 50 μm) were stacked so that the transparent curable resin layer was in contact with the release surface of the release PET 1-E, and laminated with a roll laminator at 60°C to obtain an integrated encapsulating sheet of Example 3.
[0230] [Example 4] An integrated encapsulating sheet of Example 4 was obtained in the same manner as in Example 1, except that Raw material 3-2 was used as the coating liquid for the transparent curable resin layer.
[0231] [Example 5] A coating agent for a hard coat layer (raw material 1-1) was applied to the first surface of a support film layer (film 1: manufactured by Shin-Etsu Polymer Co., Ltd.) using a bar coater so that the dry film thickness was as shown in Table 3. Then, after drying at 120°C for 5 minutes, 400 mJ / cm 2 The coating agent for the hard coat layer was cured by irradiation with ultraviolet light of 1000 nm to obtain a seventh sheet having a hard coat layer supported by a support film layer.
[0232] The coating solution for the transparent curable resin layer was applied to the second surface of the support film layer of the fifth sheet using an applicator so that the dry thickness was 80 μm, and then dried at 120° C. for 5 minutes to obtain an eighth sheet having a hard coat layer supported on the first surface of the support film layer and a transparent curable resin layer supported on the second surface of the support film layer. The obtained eighth sheet and release PET 1-E (manufactured by Nippa Corporation, 50 μm) were stacked so that the transparent curable resin layer was in contact with the release surface of the release PET 1-E, and laminated with a roll laminator at 60°C to obtain an integrated sealing sheet of Example 5.
[0233] [Example 6] A coating solution of the translucent resin composition (raw material 2-2) was applied to the first surface of the support film layer (film 1: manufactured by Shin-Etsu Polymer Co., Ltd.) using a bar coater so that the dry film thickness was the thickness shown in Table 3. The coating was then dried at 120°C for 5 minutes and then heated in a hot air circulating oven at 80°C for 72 hours to harden the translucent resin composition and form a lower translucent resin layer. Using a bar coater, a coating solution of the translucent resin composition (raw material 2-2) was applied to the second surface of the support film layer so that the dry film thickness was as shown in Table 3. The coating was then dried at 120°C for 5 minutes and then heated in a hot air circulating oven at 80°C for 72 hours to harden the translucent resin composition and form an upper translucent resin layer. Next, a corona treatment was performed on the surface of the upper semi-transparent resin layer opposite to the support film layer, and a coating agent for a hard coat layer (raw material 1-2) was applied using a bar coater so that the dry film thickness was as shown in Table 3. Then, after drying at 120°C for 5 minutes, 400 mJ / cm 2 The coating agent for the hard coat layer was cured by irradiation with ultraviolet light of 1000 nm to obtain a ninth sheet in which the upper semitransparent resin layer and the hard coat layer were supported by the support film layer.
[0234] Further, the coating liquid for the transparent curable resin layer (raw material 3-1) was applied to the lower semi-transparent resin layer on the first surface of the support film layer of the ninth sheet using an applicator so that the dry film thickness was 80 μm. Then, it was dried at 120° C. for 5 minutes to obtain a tenth sheet in which the lower semi-transparent resin layer and the transparent curable resin layer were supported on the first surface of the support film layer, and the lower semi-transparent resin layer and the hard coat layer were supported on the second surface of the support film layer.
[0235] The obtained tenth sheet and release PET 1-E (manufactured by Nippa Corporation, 50 μm) were stacked so that the transparent curable resin layer was in contact with the release surface of the release PET 1-E, and laminated with a roll laminator at 60°C to obtain an integrated sealing sheet of Example 6.
[0236] [Comparative Example 1] A coating solution for semi-transparent dry film (solid content 60%) was applied to a mud release PET PTHY-25 manufactured by Unitika Ltd. to a dry film thickness of 80 μm and dried to obtain an eleventh sheet. The coating liquid for transparent curable resin layer was applied to release PET 1-E (manufactured by Nippa Corporation, 50 μm) to a dry film thickness of 30 μm, and then dried to obtain a twelfth sheet. The eleventh sheet and the twelfth sheet were overlapped so that the semi-transparent dry film layer and the transparent curable resin layer were in contact with each other, and after lamination, the release PET 1-E was peeled off to obtain a thirteenth sheet. Furthermore, the coating liquid for the black curable resin layer was applied to release PET 1-E in a dry thickness of 50 μm and dried to obtain a fourteenth sheet. The thirteenth sheet and the fourteenth sheet were laminated together so that the transparent curable resin layer and the black curable resin layer were in contact with each other, thereby obtaining an integrated encapsulating sheet of Comparative Example 1.
[0237] <Total light transmittance of the entire semi-transparent film layer> The total light transmittance of the first sheet (Examples 1 and 4), the third sheet (Example 2), the fifth sheet (Example 3), the seventh sheet (Example 5), the ninth sheet (Example 6), and the eleventh sheet (Comparative Example 1) from which the release PET PTHY-25 was peeled off was measured using a haze meter NDH5000 manufactured by Nippon Denshoku Industries Co., Ltd. in accordance with JIS K 7361. The results are shown in Table 3.
[0238] <Storage modulus of the entire semi-transparent film layer> The storage modulus at 100°C of the first sheet (Examples 1 and 4), the third sheet (Example 2), the fifth sheet (Example 3), the seventh sheet (Example 5), the ninth sheet (Example 6), and the eleventh sheet (Comparative Example 1) from which the release PET PTHY-25 was peeled off was measured using a viscoelasticity measuring device (TA Instruments RSA-G2) under conditions of a measurement frequency of 1Hz and a heating rate of 5°C / min according to JIS K7244. The results are shown in Table 3.
[0239] <Total light transmittance of integrated laminated sheet> The second sheet (Examples 1 and 4), the fourth sheet (Example 2), the sixth sheet (Example 3), the eighth sheet (Example 5), the tenth sheet (Example 6), and the integrated encapsulating sheet of Comparative Example 1 from which the release PET PTHY-25 and the release PET 1-E were peeled off were each heated in a hot air circulating oven at 150°C for 1 hour to cure the transparent curable resin layer, thereby obtaining an integrated laminate sheet after curing. The total light transmittance of the obtained integrated laminate sheet was measured in accordance with JIS K 7361 using a haze meter NDH5000 manufactured by Nippon Denshoku Industries Co., Ltd.
[0240] <Substrate with evaluation element> A substrate with LED light emitting elements for evaluation was prepared by arranging multiple LED light emitting elements, each of which was 0.1×0.2 mm and 65 μm high, on an epoxy glass substrate.
[0241] <Evaluation of integrated encapsulating sheet> The release PET of the integrated encapsulating sheet of each example was peeled off, and the transparent curable resin layer (black curable resin layer in Comparative Example 1) was placed in contact with the LED light emitting element of the evaluation element-mounted substrate. Then, a transparent curable resin layer, or a black curable resin layer and a transparent curable resin layer, were filled between the light-emitting elements using a vacuum press under conditions of a vacuum of 100 hPa, 100°C, 0.36 MPa, and 3 minutes, and the layers were thermally cured by heating in an oven at 150°C for 1 hour to obtain 10 light-emitting electronic components of each example.
[0242] [Lab] The Lab values on the hard coat layer side of the 10 light-emitting electronic components obtained for each example were measured using a spectrophotometer CM-5 manufactured by Konica Minolta in accordance with JIS K 8722. The average Lab values of the 10 light-emitting electronic components for each example are shown in Table 2.
[0243] [Variation coefficient of L value] For each example, the coefficient of variation of the L value was calculated from the Lab values of 10 light-emitting electronic components. The results are shown in Table 3.
[0244] [Glossiness] The gloss of the surface of the hard coat layer was measured at 60° in accordance with JIS Z 8741 using a gloss meter VG8000 manufactured by Nippon Denshoku Industries Co., Ltd. The results are shown in Table 3.
[0245] [Brightness after mounting / Brightness before mounting] For ten light-emitting electronic components in each example, the luminance of the light-emitting electronic components before and after mounting the integrated encapsulant sheet was measured using a Konica Minolta CA-410 luminance meter, and the luminance after mounting was divided by the luminance before mounting to calculate the ratio of luminance after mounting / luminance before mounting. The average value of the results for the ten light-emitting electronic components is shown in Table 3.
[0246] [Surface smoothness] The surface waviness of the 10 light-emitting electronic components obtained for each example was measured using a stylus surface roughness tester, Surfcorder SE500, manufactured by Kosaka Laboratory Co., Ltd., and the difference between the maximum and minimum values was averaged to calculate the average. The calculated results were evaluated according to the following criteria. The results are shown in Table 3. ◎: Waviness is less than 10 μm. ○: Waviness is 10 to 20 μm. ×: Waviness exceeds 20 μm.
[0247] [Table 3]
[0248] As shown in Table 3, it was confirmed that the integrated encapsulating sheet according to the present invention can provide a light-emitting electronic component with little variation in blackness while suppressing the loss of overall brightness. It was also confirmed that no defects in appearance such as air bubbles or surface irregularities were observed. [Explanation of symbols]
[0249] 1A Integrated encapsulating sheet 1B Integrated encapsulating sheet 1C Integrated encapsulating sheet 2 Transparent curable resin layer 3A Semi-transparent film layer 3B Semi-transparent film layer 3C semi-transparent film layer 4 Support film layer 5 Hard Coat Layer 6 First protective film 7 Second protective film 8 Translucent resin layer 10 Substrate with element 11 Substrate 12 Light emitting element 13 Light emitting element 14 Light emitting element 22 Transparent curable resin cured material layer 30A Light-emitting electronic components 30B Light-emitting electronic components 30C Light-emitting electronic components
Claims
1. An integrated encapsulating sheet that is pressure-bonded to a surface of an element-mounted substrate on which a plurality of light-emitting elements are arranged, the surface being formed with the plurality of light-emitting elements, An integrated encapsulating sheet comprising a transparent curable resin layer and a translucent film layer, which are laminated in this order from the side that is to be placed in direct contact with the element-mounted substrate during the pressure bonding.
2. The integrated encapsulating sheet according to claim 1, wherein the total light transmittance of the translucent film layer is 20 to 80%.
3. The integrated encapsulating sheet according to claim 1 , wherein the transparent curable resin layer has a total light transmittance of 50% or more and is higher than a total light transmittance of the translucent film layer.
4. The storage modulus of the transparent curable resin layer is 1.0×10 7 The integrated encapsulating sheet according to claim 1, wherein the elastic modulus is 0.01 Pa or less.
5. The storage modulus of the transparent curable resin layer is 1.0×10 5 The integrated encapsulating sheet according to claim 1, wherein the elastic modulus is 0.01 Pa or less.
6. The integrated sealing sheet according to claim 1 or 2, wherein the transparent curable resin layer contains a high molecular weight resin having a weight average molecular weight of 20,000 to 1,000,000.
7. The integrated encapsulating sheet according to claim 6, wherein the high molecular weight resin has a weight average molecular weight of 100,000 to 500,000.
8. The integrated encapsulating sheet according to claim 6 , wherein the transparent curable resin layer contains a polyfunctional curable resin capable of forming a crosslinked structure with the high molecular weight resin.
9. The integrated sealing sheet according to claim 6, wherein the content of the high molecular weight resin relative to 100% by mass of the transparent curable resin layer is 5 to 100% by mass.
10. 2. The integrated encapsulating sheet according to claim 1, wherein the translucent film layer comprises a support film layer and a hard coat layer provided on the opposite side of the support film layer to the transparent curable resin layer.
11. the translucent film layer includes a support film layer and at least one translucent resin layer; The integrated encapsulating sheet according to claim 1, wherein the translucent resin layer has a total light transmittance of 20 to 80%.
12. 12. The integral encapsulant sheet of claim 1, 10, or 11, wherein the translucent film layer comprises one or more layers comprising carbon black.
13. The storage modulus of the semi-transparent film layer is 1.0×10 at 100° C. 8 The integrated encapsulating sheet according to claim 1 , 10 , or 11 , wherein the elastic modulus is 1 Pa or more.
14. The integral encapsulating sheet according to any one of claims 1, 10, and 11, wherein the gloss of the outermost surface of the translucent film layer opposite the transparent curable resin layer is 0.01 to 35.
15. A substrate having a plurality of light-emitting elements arranged on a substrate, and the integrated encapsulating sheet according to claim 1 or 2, which is pressure-bonded to a surface of the substrate having the light-emitting elements arranged thereon, A light-emitting electronic component, characterized in that at least a portion of the transparent curable resin layer is filled between the plurality of light-emitting elements.
16. The integrated encapsulating sheet according to claim 1 or 2 is disposed on a surface of an element-mounted substrate on which a plurality of light-emitting elements are arranged, so that the transparent curable resin layer is in contact with the surface of the element-mounted substrate, filling a portion of the transparent curable resin layer between the plurality of light emitting elements by thermocompression bonding; The method for producing a light-emitting electronic component further comprises curing the transparent curable resin layer by heating.
Citation Information
Patent Citations
LED packaging method, LED lamp and LED display
CN115084320A
Curable resin composition, dry film, cured product, and electronic component