Member for suppressing ice nucleation or suppressing icing

A member with a brush-like polymer chain aggregate and antifreeze water layer addresses the inadequacies of existing ice nucleation suppression methods, achieving effective icing prevention and improved heat exchange efficiency by maintaining a stable liquid layer that inhibits ice formation.

JP2024168817APending Publication Date: 2024-12-05NIPPON PAINT SURF CHEM CO LTD +3

Patent Information

Application Number
JP2023085782
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-24
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

Existing methods for suppressing ice nucleation and icing on cooling members in air conditioners and heat exchangers are inadequate, as they fail to effectively prevent the formation and growth of ice nuclei, leading to decreased heat exchange efficiency.

Method used

A member with a layer containing a brush-like polymer chain aggregate, where the liquid substance includes at least 15% antifreeze water by mass, and the polymer chain has a specific molecular weight ratio and surface occupancy, forming a stable liquid layer that inhibits ice nucleation and icing.

Benefits of technology

The member effectively suppresses ice nucleation and icing by maintaining a stable liquid layer, reducing freezing temperatures and preventing ice formation, even at extremely low temperatures, thus enhancing heat exchange efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024168817000009
    Figure 2024168817000009
  • Figure 2024168817000001
    Figure 2024168817000001
  • Figure 2024168817000002
    Figure 2024168817000002
Patent Text Reader

Abstract

To provide a member that can suppress ice nucleation and icing.SOLUTION: A member for suppressing ice nucleation or suppressing icing of the present invention has a layer including a brush-like polymer chain aggregate constituted of a plurality of polymer chains fixed to a substrate, the layer including a polymer chain aggregate holds a liquid substance, at least a part of the liquid substance is water, and a ratio of unfreezable water to the total mass of the water in the liquid substance is 15 mass% or more.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a component for inhibiting ice nucleation or ice accretion. [Background technology]

[0002] In heat exchangers used in air conditioners and freezers, rapid cooling of air can cause water droplets to adhere to the surface of the cooling member in the heat exchanger or cause frost to form, reducing the heat exchange efficiency. In particular, frost is formed through the formation and growth of ice nuclei and ice adhesion on the surface of the cooling member. As a method for suppressing the formation of frost, a method for forming a resin film on the surface of a component, as described in Patent Document 1, is known. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2019-158247 A Summary of the Invention [Problem to be solved by the invention]

[0004] The method described in Patent Document 1 can slow down the growth of frost by controlling the shape of water droplets that adhere to the surface of a component, but cannot sufficiently suppress ice nucleation or icing on the surface of the component, and further improvements were needed.

[0005] SUMMARY OF THE PRESENT EMBODIMENT An object of the present invention is to provide a member capable of suppressing ice nucleation and icing. [Means for solving the problem]

[0006] That is, the present invention is as follows. [1] a layer including a brush-like polymer chain assembly including a plurality of polymer chains fixed to a substrate; the layer containing the polymer chain assembly holds a liquid substance, A member for suppressing ice nucleation or icing, wherein at least a portion of the liquid substance is water, and the proportion of antifreeze water relative to the total mass of the water in the liquid substance is 15 mass % or more. [2] The member according to [1], wherein the polymer chain contains an antifreeze-forming unit composed of an antifreeze-forming monomer unit. [3] The member according to [1] or [2], wherein the ratio of the sum of the molecular weights of the nonfreeze-water-forming structural moieties contained in the nonfreeze-water-forming monomer units in the polymer chain to the molecular weight of the polymer chain (the sum of the molecular weights of the nonfreeze-water-forming structural moieties contained in the nonfreeze-water-forming monomer units / the molecular weight of the polymer chain) is 0.80 or more. [4] the substrate is a carrier made of a material different from the polymer chain assembly, The member according to [1] or [2], wherein the surface occupancy of the polymer chains on the surface of the base material is 0.08 to 0.65. [5] the member has a bottle brush structure in which the plurality of polymer chains are bonded as side chains to a polymer chain that is the base material, The member according to [1] or [2], wherein the surface occupancy rate of the side chains is 0.08 to 0.65. Effect of the Invention

[0007] Since the member of the present invention has the above-mentioned configuration, it is possible to suppress ice nucleation and icing. [Brief description of the drawings]

[0008] [Figure 1] FIG. 1 is a schematic diagram illustrating a test method for ice accretion stress. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] Hereinafter, an embodiment of the present invention (hereinafter, referred to as "the present embodiment") will be described in detail. The present invention is not limited to the following description, and can be practiced in various modifications within the scope of the gist of the present invention.

[0010] [Part] The member of this embodiment is a member for suppressing ice nucleation or icing, which has a layer including brush-like polymer chain assemblies composed of a plurality of polymer chains fixed to a substrate, and the layer including the polymer chain assemblies holds a liquid substance, at least a part of which is water, and the proportion of antifreeze water relative to the total mass of the water in the liquid substance is 15 mass% or more. The member may be a member consisting of only the substrate and the layer containing the polymer chain assembly, or may further include other layers or materials. The layer containing the polymer chain assembly may be a layer consisting of only the polymer chain assembly and a liquid substance, or may further contain other substances. In this specification, a layer containing brush-like polymer chain assemblies may be referred to as a "layer containing polymer chain assemblies".

[0011] The member of this embodiment has an excellent ice formation suppression effect and ice nucleation suppression effect. The detailed reason why such an effect is obtained is unclear, but it is presumed to be due to the following. It is presumed that in the member of this embodiment, the liquid substance is held by the polymer chain assemblies to form a stable liquid layer in which irreversible liquid leakage is unlikely to occur in the layer containing the polymer chain assemblies. It is also presumed that the mobility of the liquid substance held by the polymer chain assemblies is appropriately controlled by the polymer chain assemblies, making it easy to create a supercooled state or an unfrozen state. It is presumed that the member of this embodiment has an interface with high mobility against ice, snow, frost, etc. due to the presence of such a stable liquid layer. It is also presumed that the presence of such a stable liquid layer allows water to undergo thermal motion without solidifying even below the freezing point, so that the freezing temperature of water on the member surface can be further reduced. The present inventors further investigated the inhibition of ice formation, and surprisingly found that the proportion of non-freezing water that does not freeze even at temperatures below -90°C, which is much lower than the temperature at which ice formation occurs, is related to the inhibition of ice nucleation and the inhibition of ice formation. Since the member of this embodiment contains a large amount of non-freezing water in the liquid substance in the layer containing the polymer chain aggregate, water is unlikely to freeze on the member surface even at low temperatures, and ice, snow, frost, etc. are unlikely to form on the member surface. Furthermore, since the member has an interface with high mobility against ice, snow, frost, etc., even if ice, snow, frost, etc. form on the member surface, they have extremely excellent sliding properties, and therefore it is presumed that the member has an extremely excellent ice formation inhibition effect. In addition, the component of this embodiment can further lower the freezing temperature of water inside the component or on its surface, thereby lowering the temperature at which ice nuclei occur, and is presumably therefore capable of providing an extremely excellent effect of inhibiting ice nucleation.

[0012] The polymer chain aggregate used in this embodiment is an aggregate of a plurality of polymer chains, which has a brush-like shape as a whole, and is completely different from an organic film formed by simply applying a polymer solution. In this specification, the term "brush-like" may refer to a structure in which at least one end of a polymer chain is fixed to the surface of a substrate or a layer on the substrate, and there are multiple (e.g., two or more) polymer chains extending in a direction away from the substrate. When both ends of the polymer chain are fixed to the substrate, the structure may be U-shaped.

[0013] The fact that the layer containing the polymer chain assembly retains the liquid substance can be confirmed by differential scanning calorimetry. If it cannot be confirmed by differential scanning calorimetry, it can be confirmed by an indentation hardness test. The proportion of non-freezing water in the layer containing the polymer chain assembly can be measured by the method described in the Examples below.

[0014] In the member of this embodiment, the liquid substance refers to a substance that is held in the layer containing the polymer chain assembly and is liquid at room temperature. At least a part of the liquid substance preferably maintains a liquid state even at a temperature lower than the freezing point (preferably -10°C or lower, more preferably -18°C or lower, even more preferably -20°C or lower, and particularly preferably -30°C or lower). In addition, the liquid substance is preferably water. From the viewpoint of excellent suppression of ice nucleation and icing, the member of this embodiment preferably has a mass ratio of the substance confirmed to be in a liquid state at the above-mentioned temperature to 100 mass parts of polymer chains contained in the layer containing the polymer chain assembly at -18°C of 50 mass parts or more, more preferably 70 mass parts or more, even more preferably 80 mass parts or more, and particularly preferably 90 mass parts or more. The above ratio can be adjusted by the combination of the polymer chains and the liquid substance. The above ratio can be measured by an atomic force microscope, an ellipsometry method, or the like. The member of this embodiment preferably has a layer containing brush-like polymer chain assemblies composed of a plurality of polymer chains fixed to a substrate at −18° C., and the layer containing the polymer chain assemblies preferably holds a liquid substance.

[0015] The member of the present embodiment contains antifreeze water in the layer containing the polymer chain assembly. The nonfreezing water refers to water in the layer that is in a liquid state at −90° C., and refers to water in the polymer (hydration water) that does not freeze even at −90° C. due to a strong interaction with the polymer. The nonfreezing water can be measured, for example, by the method described in the Examples below.

[0016] In the member of this embodiment, the thickness of the layer containing the polymer chain assembly is preferably 50 nm or more, more preferably 100 nm or more, even more preferably 350 nm or more, even more preferably 500 nm or more, and particularly preferably 1000 nm or more, because this makes it easier to obtain a better ice adhesion suppression effect and ice nucleation suppression effect. There is no particular upper limit, but it can be, for example, 100 μm or less, or 50 μm or less. The thickness of the layer containing the polymer chain assembly can be measured by an ellipsometry method, etc. The film thickness may be a value measured at -18°C.

[0017] The members of this embodiment will be described in detail below.

[0018] [Polymer chain assembly] The polymer chain assembly in this embodiment is composed of multiple polymer chains and has a brush-like shape as a whole. In this specification, the term "polymer chain" refers to a molecule or a portion of a molecule having a structure in which multiple monomer units are linked in a chain. The multiple polymer chains constituting the polymer chain assembly may be the same or different from each other. In addition, the polymer chain may have a structure in which multiple identical or different monomer units are linked in a chain, and may be linear, have a side chain, or have a branched structure, and a cross-linked structure may be formed between the polymer chains or between the polymer chain and the substrate.

[0019] (polymer chain) The polymer chain may be a homopolymer obtained by polymerizing one type of monomer, or a copolymer obtained by polymerizing two or more types of monomers. Examples of the copolymer include random copolymers, block copolymers, gradient copolymers, and alternating copolymers. The monomers used to generate the polymer chains may be used alone or in combination of two or more kinds.

[0020] The polymer chain includes a non-freezing water-forming unit. The polymer chain may be composed of only the non-freezing water-forming unit, or may be composed of the non-freezing water-forming unit and a unit other than the non-freezing water-forming unit (sometimes referred to as other units). The non-freezing water-forming unit refers to one monomer unit or a chain of multiple monomer units composed of only the non-freezing water-forming monomer unit having the non-freezing water-forming structural portion described below. The mass ratio of the nonfreezing water forming units to 100 mass parts of the polymer chain is preferably 40 to 100 mass parts, more preferably 50 to 100 mass parts, and even more preferably 80 to 100 mass parts, from the viewpoint of retaining a large amount of nonfreezing water in the layer containing the polymer chain assembly. The ratio of the nonfreezing water forming units in the polymer chain refers to the ratio of the nonfreezing water forming monomer units in the polymer chain. The other units refer to a sequence of one or more monomer units consisting only of monomer units other than the nonfreezing water forming monomer units.

[0021] The non-freezing water forming structural portion refers to a structural portion in a monomer unit that has the property of forming and retaining non-freezing water in a polymer chain, and examples of such structural portions include functional groups capable of forming hydrogen bonds, structures derived from (poly)alkylene glycols and alkoxy(poly)alkylene glycols, etc. The structure derived from (poly)alkylene glycol refers to all alkylene oxide units and terminal hydroxyl groups, and the structure derived from alkoxy(poly)alkylene glycol refers to all alkylene oxide units and terminal alkoxy groups. The nonfreezing water-forming monomer unit may have one or more nonfreezing water-forming structural moieties.

[0022] Examples of the functional group capable of forming a hydrogen bond include a carboxy group, a group that can be converted into a salt of a carboxy group, a hydroxy group, a glycidyl group, a sulfonic acid group, a sulfonate salt, an amide group, a group containing quaternary ammonium, an imide group, a nitrile group, an alkoxy group, etc. The functional group capable of forming a hydrogen bond is preferably located at the end of the nonfreezing water-forming monomer.

[0023] Examples of the monomer constituting the nonfreezing water forming monomer unit having a carboxy group include (meth)acrylic acid, maleic acid, fumaric acid, itaconic acid, crotonic acid, etc. Also, it may be an ester of the monomer having a carboxy group, for example, a monoalkyl ester of maleic acid, a monoalkyl ester of fumaric acid, etc. In this specification, the alkyl group may be an alkyl group having 1 to 10 carbon atoms (preferably 2 to 5 carbon atoms).

[0024] Examples of the monomer constituting the nonfreezing water forming monomer unit having a group that can be converted into a salt of a carboxy group include tert-butyl (meth)acrylate.

[0025] Examples of monomers constituting the nonfreezing water-forming monomer unit having a hydroxy group include 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, and hydroxy-substituted alkyl (meth)acrylates (e.g., 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, and 2,3-dihydroxypropyl (meth)acrylate).

[0026] Examples of the monomer constituting the glycidyl group-containing nonfreezing water-forming monomer unit include glycidyl (meth)acrylate.

[0027] Examples of the monomer constituting the above-mentioned sulfonic acid group-containing nonfreezing water-forming monomer unit include p-styrene chlorosulfonic acid and styrene sulfonic acid.

[0028] Examples of the monomer that constitutes the nonfreezing water-forming monomer unit having the above-mentioned sulfonate include salts of the monomer that constitutes the nonfreezing water-forming monomer unit having the above-mentioned sulfonic acid group, anionic monomers such as potassium 3-sulfopropyl methacrylate, and the like.

[0029] Examples of the monomer that constitutes the nonfreezing water-forming monomer unit having an amide group include acrylamide, methacrylamide, N-methylacrylamide, N,N-dimethylacrylamide, and N-methylmethacrylamide.

[0030] Examples of monomers constituting the nonfreezing water-forming monomer unit having the above-mentioned quaternary ammonium-containing group include ionic liquid type monomers, cationic type monomers such as N-vinylpyrrolidone, N,N-dimethylaminoethyl (meth)acrylate, and methacryloyloxyethyl trimethylammonium chloride. The ionic liquid type monomer is not particularly limited, but examples thereof include compounds represented by the following formula (1). [ka] In formula (1), m represents an integer of 1 to 10, and n represents an integer of 1 to 5. 1 represents a hydrogen atom or an alkyl group having 1 to 3 carbon atoms, R 2 , R 3 and R 4 Each independently represents an alkyl group having 1 to 5 carbon atoms. 2 , R 3 and R 4 The alkyl group in the formula (I) may have a carbon atom or a hydrogen atom substituted with one or more heteroatoms selected from an oxygen atom, a sulfur atom, and a fluorine atom; 2 , R 3 and R 4 may be linked to form a cyclic structure. Y represents a monovalent anion. Examples of the monovalent anion represented by Y include BF4 - , PF6 - , AsF6 - , SbF6 - , AlCl4 - , NbF6 - , HSO4 - , ClO4 - , CH3SO3 - , CF3SO3 - , CF3CO2 - , (CF3SO2)2N - , Cl - , Br - , I - Considering the stability of the anion, BF4 - , PF6 - , (CF3SO2)2N- , CF3SO3 - , or CF3CO2 - It is preferable that: Of the compounds represented by formula (1), the ionic liquid type monomer is preferably a compound represented by any one of the following formulae (2) to (9). [ka] In formulas (2) to (9), m, n, R 1 , R 2 , Y is m, n, R in formula (1) 1 , R 2 , Y. Me represents a methyl group, and Et represents an ethyl group.

[0031] Examples of monomers constituting the above-mentioned imide group-containing antifreeze-forming monomer unit include maleimide, methylmaleimide, ethylmaleimide, propylmaleimide, butylmaleimide, hexylmaleimide, octylmaleimide, dodecylmaleimide, stearylmaleimide, phenylmaleimide, and cyclohexylmaleimide.

[0032] Examples of the monomer constituting the nonfreezing water-forming monomer unit having a nitrile group include acrylonitrile and methacrylonitrile.

[0033] Examples of the monomer constituting the above-mentioned alkoxy group-containing nonfreezing water-forming monomer unit include polyethoxyethyl (meth)acrylate and polyethoxypropyl (meth)acrylate.

[0034] Examples of monomers constituting the alkylene glycol-containing nonfreeze-water-forming monomer unit include nonionic monomers such as poly(alkylene glycol) mono(meth)acrylates (e.g., poly(ethylene glycol) monomethacrylate), alkoxypoly(alkylene glycol) (meth)acrylates (e.g., methoxypoly(ethylene glycol) methacrylate), phenoxypoly(alkylene glycol) (meth)acrylates (e.g., phenoxypoly(ethylene glycol) methacrylate), polyalkoxypoly(alkylene glycol) (meth)acrylates, 2-glucosyloxyethyl (meth)acrylate, and poly(ethylene glycol) monomethacrylate.

[0035] Examples of the monomer that constitutes the betaine-containing nonfreezing water-forming monomer unit include (3-[(3-acrylamidopropyl)dimethylammonio]propane-1-sulfonic acid, and the like.

[0036] Among these, as the nonfreezing water-forming monomer unit, from the viewpoint of retaining a larger amount of nonfreezing water in the layer containing the polymer chain assembly, a monomer having an alkylene glycol is preferred, and a polyalkoxypoly(alkylene glycol)(meth)acrylate is more preferred.

[0037] The monomer used for generating the polymer chain is preferably one that can bond the polymer chain obtained by polymerization to the substrate as a graft chain. Such a monomer can be a monomer having at least one addition polymerizable double bond, and is preferably a monofunctional monomer having one addition polymerizable double bond. Examples of the monofunctional monomer having one addition polymerizable double bond include (meth)acrylic acid monomers and styrene monomers. The monomer constituting the nonfreezing water forming monomer unit is preferably a monofunctional monomer having a nonfreezing water forming structure portion and further having one addition polymerizable double bond. For example, the monofunctional monomer having a nonfreezing water forming structure portion and further having one addition polymerizable double bond may be exemplified as the monomer having the above nonfreezing water forming structure portion and also as the monofunctional monomer having one addition polymerizable double bond described below.

[0038] Examples of (meth)acrylic acid monomers include (meth)acrylic acid, methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, isopropyl (meth)acrylate, butyl (meth)acrylate, isobutyl (meth)acrylate, tert-butyl (meth)acrylate, pentyl (meth)acrylate, hexyl (meth)acrylate, cyclohexyl (meth)acrylate, heptyl (meth)acrylate, octyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, and nonyl (meth)acrylate. (meth)acrylate, decyl (meth)acrylate, dodecyl (meth)acrylate, tridecyl (meth)acrylate, phenyl (meth)acrylate, toluyl (meth)acrylate, benzyl (meth)acrylate, 2-methoxyethyl (meth)acrylate, 3-methoxypropyl (meth)acrylate, 3-methoxybutyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, stearyl (meth)acrylate, glycidyl (meth)acrylate, 3-ethyl-3 -(meth)acryloyloxymethyloxetane, 2-(meth)acryloyloxyethyl isocyanate, (meth)acrylate-2-aminoethyl, 2-(2-bromopropionyloxy)ethyl (meth)acrylate, 2-(2-bromoisobutyryloxy)ethyl (meth)acrylate, 1-(meth)acryloxy-2-phenyl-2-(2,2,6,6-tetramethyl-1-piperidinyloxy)ethane, 1-(4-((4-(meth)acryloxy)ethoxyethyl)phenylethoxy)piperidine, γ-(methacryloyloxy) dimethylpropyl)trimethoxysilane, 3-(3,5,7,9,11,13,15-heptaethylpentacyclo[9.5.1.13,9.15,15.17,13]octasiloxan-1-yl)propyl (meth)acrylate, 3-(3,5,7,9,11,13,15-heptaisobutyl-pentacyclo[9.5.1.13,9.15,15.17,13]octasiloxan-1-yl)propyl (meth)acrylate, 3-(3,5,7,9,11,13,15-heptaisooctylpentacyclo[9.5.1.13,9.15,15.17,13]octasiloxan-1-yl)propyl (meth)acrylate, 3-(3,5,7,9,11,13,15-heptacyclopentyl pentacyclo[9.5.1.13,9.15,15.17,13]octasiloxan-1-yl)propyl (meth)acrylate, 3-(3,5,7,9,11,13,15-heptaphenyl pentacyclo[9.5.1. 13,9.15,15.17,13]octasiloxane-1-yl)propyl (meth)acrylate, 3-[(3,5,7,9,11,13,15-heptaethylpentacyclo[9.5.1.13,9.15,15.17,13]octasiloxane-1-yloxy)dimethylsilyl]propyl (meth)acrylate, 3-[(3,5,7,9,11,13,15-heptaethylpentacyclo[9.5.1.13,9.15,15.17,13]octasiloxane-1-yloxy)dimethylsilyl]propyl (meth)acrylate Butaisobutylpentacyclo[9.5.1.13,9.15,15.17,13]octasiloxane-1-yloxy)dimethylsilyl]propyl (meth)acrylate, 3-[(3,5,7,9,11,13,15-heptaisooctylpentacyclo[9.5.1.13,9.15,15.17,13]octasiloxane-1-yloxy)dimethylsilyl]propyl propyl (meth)acrylate, 3-[(3,5,7,9,11,13,15-heptacyclopentyl pentacyclo[9.5.1.13,9.15,15.17,13]octasiloxan-1-yloxy)dimethylsilyl]propyl (meth)acrylate, 3-[(3,5,7,9,11,13,15-heptaphenyl pentacyclo[9.5.1.13,9.15,15.17,13]Octasiloxane-1-yloxy)dimethylsilyl]propyl (meth)acrylate, ethylene oxide adduct of (meth)acrylic acid, trifluoromethyl methyl (meth)acrylate, 2-trifluoromethylethyl (meth)acrylate, 2-perfluoroethylethyl (meth)acrylate, 2-perfluoroethyl-2-perfluorobutylethyl (meth)acrylate, 2-perfluoroethyl (meth)acrylate, trifluoromethyl (meth)acrylate, diperfluoromethyl methyl (meth)acrylate, 2-perfluoromethyl-2-perfluoroethylethyl (meth)acrylate, 2-perfluorohexylethyl (meth)acrylate, 2-perfluorodecylethyl (meth)acrylate, 2-perfluorohexadecylethyl (meth)acrylate, and the like.

[0039] Styrenic monomers include styrene, vinyltoluene, α-methylstyrene, p-chlorostyrene, p-chloromethylstyrene, m-chloromethylstyrene, o-aminostyrene, p-styrene chlorosulfonic acid, styrenesulfonic acid and its salts, vinylphenylmethyldithiocarbamate, 2-(2-bromopropionyloxy)styrene, 2-(2-bromoisobutyryloxy)styrene, 1-(2-((4-vinylphenyl)methoxy)-1-phenylethoxy)-2,2,6,6-tetramethylpiperidine, 1-(4-vinylphenyl)- 3,5,7,9,11,13,15-heptaethylpentacyclo[9.5.1.13,9.15,15.17,13]octasiloxane, 1-(4-vinylphenyl)-3,5,7,9,11,13,15-heptaisobutylpentacyclo[9.5.1.13,9.15,15.17,13]octasiloxane, 1-(4-vinylphenyl)-3,5,7,9,11,13,15-heptaisooctylpentacyclo[9.5.1.13,9.15,15.17,13]octasiloxane, 1-(4-vinylphenyl)-3,5,7,9,11,13,15 -Heptacyclopentyl pentacyclo [9.5.1.13, 9.15, 15.17, 13] octasiloxane, 1- (4-vinylphenyl) -3,5,7,9,11,13,15-heptaphenyl pentacyclo [9.5.1.13, 9.15, 15.17, 13] octasiloxane, 3- (3,5,7,9,11,13,15-heptaethyl pentacyclo [9.5.1.13, 9.15, 15.17, 13] octasiloxane-1-yl) ethyl styrene, 3- (3,5,7,9,11,13,15-heptaisobutyl pentacyclo [9.5.1.13, 9.15,15.17,13]octasiloxan-1-yl)ethylstyrene, 3-(3,5,7,9,11,13,15-heptaisooctylpentacyclo[9.5.1.13,9.15,15.17,13]octasiloxan-1-yl)ethylstyrene, 3-(3,5,7,9,11,13,15-heptacyclopentylpentacyclo[9.5.1.13,9.15,15.17,13]octasiloxan-1-yl)ethylstyrene, 3-(3,5,7,9,11,13,15-heptaphenylpentacyclo[9.5.1.13,9.15,15.17,13]octasiloxan-1-yl)ethylstyrene, 3-((3,5,7,9,11,13,15-heptaethylpentacyclo[9.5.1.13,9.15,15.17,13]octasiloxan-1-yloxy)dimethylsilyl)ethylstyrene, 3-((3,5,7,9,11,13,15-heptaisobutylpentacyclo[9.5.1.13,9.15,15.17,13]octasiloxan-1-yloxy)dimethylsilyl)ethylstyrene, 3-((3,5,7,9,11,13,15-heptaisooctylpentacyclo[9 .5.1.13,9.15,15.17,13]octasiloxane-1-yloxy)dimethylsilyl)ethylstyrene, 3-((3,5,7,9,11,13,15-heptacyclopentyl pentacyclo[9.5.1.13,9.15,15.17,13]octasiloxane-1-yloxy)dimethylsilyl)ethylstyrene, 3-((3,5,7,9,11,13,15-heptaphenyl pentacyclo[9.5.1.13,9.15,15.17,13]octasiloxane-1-yloxy)dimethylsilyl)ethylstyrene, etc.

[0040] In addition, examples of monofunctional monomers having one addition-polymerizable double bond in one molecule include fluorine-containing vinyl monomers (perfluoroethylene, perfluoropropylene, vinylidene fluoride, etc.), silicon-containing vinyl monomers (vinyltrimethoxysilane, vinyltriethoxysilane, etc.), maleic anhydride, maleic acid, monoalkyl esters and dialkyl esters of maleic acid, fumaric acid, monoalkyl esters and dialkyl esters of fumaric acid, maleimide monomers (maleimide, methylmaleimide, ethylmaleimide, propylmaleimide, butylmaleimide, hexylmaleimide, octylmaleimide, dodecylmaleimide, stearylmaleimide, phenylmaleimide, cyclohexylmaleimide, etc.), nitrile group-containing monomers, Monomers (acrylonitrile, methacrylonitrile, etc.), amide group-containing monomers (acrylamide, methacrylamide, etc.), vinyl ester monomers (vinyl acetate, vinyl propionate, vinyl pivalate, vinyl benzoate, vinyl cinnamate, etc.), olefins (ethylene, propylene, etc.), conjugated diene monomers (butadiene, isoprene, etc.), vinyl halides (vinyl chloride, etc.), vinylidene halides (vinylidene chloride, etc.), allyl halides (allyl chloride, etc.), allyl alcohol, vinylpyrrolidone, vinylpyridine, N-vinylcarbazole, methyl vinyl ketone, vinyl isocyanate, macromonomers whose main chains are derived from styrene, (meth)acrylic acid esters, siloxanes, etc., can also be used.

[0041] The polymer chain may be a polymer obtained by reacting polymers having reactive groups with each other. Examples of the reactive groups include hydroxyl groups and isocyanate groups. Examples of the polymer having reactive groups include polymers of polyethylene glycol and dimethylsiloxane, and specifically, Silaplane FM-0421 (reactive silicone) (manufactured by Shin-Etsu Chemical Co., Ltd.) and the like. From the viewpoint of being particularly excellent in the effect of suppressing ice nucleation and icing, methoxypoly(ethylene glycol) methacrylate or a mixture of dodecyl methacrylate and tridecyl methacrylate is preferred, and from the viewpoint of suppressing snow accumulation outdoors, a mixture of dodecyl methacrylate and tridecyl methacrylate is particularly preferred.

[0042] The polymer chains are preferably hydrophilic polymer chains having affinity for a liquid substance to be held in the layer containing the polymer chain aggregate. For example, when the layer containing the polymer chain assembly is to retain water or a hydrophilic liquid substance, the polymer chains constituting the polymer chain assembly are preferably hydrophilic polymer chains. The hydrophilic polymer chains may be synthesized using hydrophilic monomers, or may be synthesized by synthesizing a polymer using hydrophobic monomers and then introducing a hydrophilic group into the polymer. In this specification, a polymer chain having high compatibility with water may be referred to as a "compatible polymer chain," and a polymer chain having low compatibility with water may be referred to as a "non-compatible polymer chain." Note that a polymer chain having high compatibility with water refers to a polymer chain having a swelling degree of 1.5 or more (preferably 2.0 or more, more preferably 2.5 or more) measured and calculated by a film thickness measurement method using an atomic force microscope, and a polymer chain having low compatibility with water refers to a polymer chain having a swelling degree of less than 1.5 (preferably 1.3 or less, more preferably 1.1 or less, even more preferably 1.08 or less, particularly preferably 1.05 or less). The swelling degree is a value measured by the following method. The test piece for measuring the layer thickness is scratched with the tip of tweezers, and the height of the step (i.e., the thickness of the layer in a dry state) is estimated at the boundary between the part where the substrate base is exposed and the part where the layer is present, using the atomic force microscope colloidal probe method (contact mode). Next, the same test piece is immersed overnight in a corresponding liquid substance (e.g., water), and then the height of the step (i.e., the thickness of the layer in a swollen state) is estimated at the same location in the liquid, using the atomic force microscope colloidal probe method (contact mode). The swelling degree is then calculated from the thickness of the layer in a swollen state / the thickness of the layer in a dry state.

[0043] It is preferable to use a hydrophilic monomer for producing the polymer chain, that is, the polymer chain preferably contains a monomer unit derived from a hydrophilic monomer. The monomer constituting the nonfreezing water forming monomer unit is preferably a monomer having a nonfreezing water forming structural part and further having hydrophilicity. Examples of the monomer having a nonfreezing water forming structural part and further having hydrophilicity include the monomers exemplified as the monomer having the nonfreezing water forming structural part described above and also exemplified as the hydrophilic monomer described below.

[0044] As the hydrophilic monomer, hydroxy-substituted alkyl (meth)acrylate (e.g., 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2,3-dihydroxypropyl (meth)acrylate, polyethoxyethyl (meth)acrylate, polyethoxypropyl (meth)acrylate, etc.), poly(alkylene glycol) mono(meth)acrylate (e.g., poly(ethylene glycol) monomethacrylate, etc.), alkoxy poly(alkylene glycol) (meth)acrylate (e.g., methoxy poly(ethylene glycol) methacrylate, etc.), phenoxy poly(alkylene glycol) (meth)acrylate (e.g., phenoxy poly(ethylene glycol) methacrylate, etc.), polyalkoxy poly(alkylene glycol) (meth)acrylate is more preferred. In addition, examples of hydrophilic monomers that can be used include (meth)acrylamide, N-alkyl (meth)acrylamide (for example, N-methylacrylamide, N,N-dimethylacrylamide, N-methylmethacrylamide, etc.), 2-glucosyloxyethyl (meth)acrylate, acrylic acid, methacrylic acid, fumaric acid, maleic acid, itaconic acid, crotonic acid, methacrylamide, N-vinylpyrrolidone, N,N-dimethylaminoethyl (meth)acrylate, and quaternary ammonium salts thereof.

[0045] To generate hydrophilic polymer chains, it is also preferable to use hydrophilic monomers having a side chain with a group that can be easily converted to a carboxy group or a salt of a carboxy group. Hydrophilicity can be imparted by converting the side chain group of the generated polymer chain to a carboxy group or a salt of a carboxy group. Examples of monomers having a side chain with a group that can be easily converted to a carboxy group or a salt of a carboxy group include tert-butyl (meth)acrylate.

[0046] In the member of this embodiment, at least a part of the liquid substance is water, and from the viewpoint of excellent effects of suppressing ice nucleation and icing, it is preferable that the polymer chains are compatible polymer chains. The compatible polymer chain preferably contains a structural unit derived from at least one compatible monomer selected from the group consisting of nonionic monomers such as poly(ethylene glycol) monomethacrylate, anionic monomers such as potassium 3-sulfopropyl methacrylate, cationic monomers such as methacryloyloxyethyl trimethylammonium chloride, and betaine monomers such as 3-[(3-acrylamidopropyl)dimethylammonio]propane-1-sulfonic acid. Among them, a monomer having a (poly)alkylene glycol is preferred from the viewpoint of being particularly excellent in the effect of suppressing ice nucleation and icing. The compatible monomers may be used alone or in combination. The compatible polymer chain is a polymer chain in which the mass ratio of the structural unit derived from the compatible monomer to 100 parts by mass of the polymer chain is more than 50 parts by mass (preferably 70 parts by mass or more, more preferably 80 parts by mass or more, even more preferably 90 parts by mass or more, and particularly preferably 100 parts by mass). The mass ratio of the structural unit derived from the betaine monomer to 100 parts by mass of the polymer chain is preferably 70 parts by mass or more, more preferably 80 parts by mass or more, even more preferably 90 parts by mass or more, and particularly preferably 100 parts by mass. The compatible monomer refers to a monomer having a swelling degree of 1.1 or more when made into a homopolymer, and the incompatible monomer refers to a monomer having a swelling degree of less than 1.1 when made into a homopolymer. A part of the monomers constituting the compatible polymer chain may be an incompatible monomer. When the polymer chain contains a monomer having a (poly)alkylene glycol, the mass ratio of the nonfreezing water forming unit to 100 parts by mass of the polymer chain is preferably 80 to 100 parts by mass, from the viewpoint of being able to retain a large amount of nonfreezing water in the layer containing the polymer chain assembly.

[0047] In the member of this embodiment, a part of the liquid substance may be a substance that is incompatible with water, as long as the effect of the present invention is not impaired.

[0048] In the polymer chain assembly, a crosslinked structure may be formed between the polymer chains or between the polymer chain and the substrate. This allows the elastic modulus of the polymer chain assembly to be controlled. The crosslinked structure formed between the polymer chains may be either a physical crosslinked structure or a chemical crosslinked structure. The crosslinked structure may be formed simultaneously with the polymerization reaction for generating the polymer chain, or may be formed after the polymer chain is generated. The formation of the crosslinked structure performed simultaneously with the polymerization reaction for generating the polymer chain can be performed by adding an appropriate amount of a bifunctional monomer such as a divinyl monomer such as ethylene glycol dimethacrylate to the polymerization reaction solution in addition to the monofunctional monomer for generating the polymer chain. In addition, the formation of the crosslinked structure between the generated polymer chains or between the polymer chain and the substrate can be performed by introducing a crosslinked group into the polymer chain using a monomer having a crosslinked group, and reacting the crosslinked group with a reactive group of another polymer chain, or reacting the crosslinked group with a reactive group of the substrate. Examples of the crosslinked group include an azide group, a halogen group (preferably a bromo group), an alkoxysilyl group, an isocyanate group, a vinyl group, and a thiol group. Furthermore, when a polymer chain is produced by living radical polymerization, a reactive group remaining at the end of the graft chain can be used as a crosslinking group.

[0049] In the member of this embodiment, the polymer chains constituting the polymer chain assembly are fixed to a substrate. The substrate may be a carrier made of a substance different from the polymer chain assembly, or may be a linear or branched polymer chain that is the same as or different from the polymer chain contained in the polymer chain assembly. In this specification, the polymer chain serving as the substrate may be referred to as a "trunk polymer." When the substrate is a carrier, the polymer chain aggregate constitutes a "polymer brush." ​​The carrier may be flat, spherical, porous, or have a large surface area (e.g., 100 mm 2 The substrate may have a surface area of ​​at least 100 nm. Furthermore, when the substrate is a trunk polymer, the trunk polymer as the main chain and the polymer chain (side chain) bonded to the main chain as a whole constitute a “bottle brush structure.” When the substrate is a trunk polymer, the member of this embodiment includes the bottle brush structure adhered to the above-mentioned carrier. Furthermore, when the polymer chains constituting the polymer chain assembly are fixed to a carrier made of a different material from the polymer chain assembly, for example, when the polymer chain assembly constitutes a "polymer brush," only a part of the polymer chain (for example, one end or the center of the polymer chain) may be fixed to the substrate (carrier), or both ends of the polymer chain may be fixed to the substrate (carrier). When both ends of the polymer chain are fixed to the substrate (carrier), the polymer chain forms a loop structure, and such a polymer chain assembly constitutes a polymer brush with a loop structure. The brush-like polymer forming a loop structure may be a bottle brush. Here, the term "fixing" refers to direct chemical bonding between a polymer chain and a compound constituting the substrate or an initiator group introduced on the substrate surface, or between a layer provided on the substrate surface and a polymer, etc. Among these, from the viewpoint of excellent ice nucleation suppression and icing suppression at low temperatures, it is preferable that direct chemical bonding between a polymer chain and a compound constituting the substrate or an initiator group introduced on the substrate surface. In this specification, the term "substrate" refers to a material to which polymer chains are fixed. The term "carrier" refers to a material that can have a layer on its surface that includes a brush-like polymer chain assembly composed of a plurality of polymer chains. For example, in the member having the above-mentioned polymer brush structure, the substrate may be a material to which polymer chains are fixed, and the carrier may also be a material to which polymer chains are fixed. In the member having the above-mentioned bottle brush structure, the substrate may be a trunk polymer, and the carrier may be a material to which the trunk polymer is adhered.

[0050] In the member of this embodiment, when the polymer chain assembly constitutes the polymer brush, the thickness of the polymer brush layer, i.e., the thickness of the layer including the polymer chain assembly, is preferably 10 nm or more, more preferably 50 nm or more, even more preferably 100 nm or more, still more preferably 300 nm or more, even more preferably 500 nm or more, and particularly preferably 1000 nm or more. There is no particular upper limit, but it can be, for example, 100 μm or less, or it can be 50 μm or less. When the polymer chain assembly is formed by self-organization, this layer thickness is preferably 1 nm or more, more preferably 5 nm or more, more preferably 10 nm or more, and even more preferably 100 nm or more. There is no particular upper limit, but it can be, for example, 1 μm or less, or it can be 10 μm or less. The formation of the polymer chain assembly by self-organization means that the individual polymer chains spontaneously form the polymer chain assembly.

[0051] In the member of this embodiment, when the polymer chain assembly has the bottle brush structure, the thickness of the layer containing the polymer chain assembly is preferably 2 nm or more, more preferably 50 nm or more, even more preferably 100 nm or more, still more preferably 300 nm or more, even more preferably 500 nm or more, and particularly preferably 1000 nm or more. There is no upper limit, but it can be, for example, 100 μm or less, or 50 μm or less.

[0052] In the following, a method for forming a polymer chain assembly will be described for each of a polymer brush and a member having a bottle-brush structure.

[0053] [A] Polymer brush The polymer chain assembly of the polymer brush can be obtained by a graft polymerization method in which a plurality of polymer chains are bonded to a substrate, i.e., a carrier, as graft chains. This graft polymerization can be performed by the grafting-from method or the grafting-to method, of which the grafting-from method is preferred. Here, the grafting-from method is a method in which a polymerization initiator group is introduced to the substrate and a graft chain is allowed to grow from the polymerization initiator group, while the grafting-to method is a method in which a graft chain synthesized in advance is bonded to a reaction site introduced to the substrate. The polymer chain assembly can also be obtained by a method in which the hydrophobic portion of a polymer (block copolymer) having a hydrophobic block and a hydrophilic block is hydrophobically bonded to the surface of a hydrophobic substrate or a hydrophobized substrate. An example of the block copolymer is a copolymer having a polymethyl methacrylate (PMMA) structure as the hydrophobic block and a poly(sodium sulfonated glycidyl methacrylate) (PSGMA) structure as the hydrophilic block. Another polymer structure may be interposed between the PMMA structure and the PSGMA structure. For details of this method, see Nature, 425, 163-165 (2003), etc.

[0054] (Graft polymerization method) A method for producing a polymer chain assembly by graft polymerization will be specifically described below.

[0055] - Polymer chain formation - The method for producing the polymer chains used in the graft polymerization method is not particularly limited, but it is preferable to use a radical polymerization method, more preferably to use a living radical polymerization method (LRP) method, and even more preferably to use an atom transfer radical polymerization method (ATRP) method. The living radical polymerization method has the advantage that it is easy to control the molecular weight and molecular weight distribution of the polymer chain, and various types of copolymers (for example, random copolymers, block copolymers, compositionally gradient copolymers, etc.) can be produced as graft chains. In addition, according to the living radical polymerization method, by using high pressure conditions and an ionic liquid solvent, it is possible to produce a concentrated polymer brush described later with precisely controlled density and thickness. Here, the method of graft polymerization when using the living radical polymerization method may be either the grafting-from method or the grafting-to method, but the grafting-from method is preferable. For details of the graft polymerization method combining the living radical polymerization method and the grafting-from method, reference can be made to JP-A-11-263819 and the like. For details of the atom transfer radical polymerization method, reference can be made to J. Am. Chem. Soc., 117, 5614 (1995), Macromolecules, 28, 7901 (1995), Science, 272, 866 (1996), and Macromolecules, 31, 5934-5936 (1998). Polymer chains can also be produced by nitroxide-mediated polymerization (NMP), reversible addition-fragmentation chain transfer (RAFT) polymerization, reversible transfer catalyzed polymerization (RTCP), reversible complexation mediated polymerization (RCMP), etc.

[0056] The catalyst used in the radical polymerization method may be any catalyst capable of controlling radical polymerization, and is preferably a transition metal complex. A preferred example of the transition metal complex is a metal complex having a central metal of an element of Group 7, 8, 9, 10, or 11 of the periodic table, and among them, it is preferable to use a copper complex, a ruthenium complex, an iron complex, or a nickel complex, and it is more preferable to use a copper complex. The copper complex preferably contains a complex of a monovalent copper compound and an organic ligand, and more preferably contains both a complex of a monovalent copper compound and an organic ligand and a complex of a divalent copper compound and an organic ligand. Examples of the monovalent copper compound include cuprous chloride and cuprous bromide, and examples of the divalent copper compound include cupric chloride and cupric bromide. Examples of organic ligands include 2,2'-bipyridyl or its derivatives, 1,10-phenanthroline or its derivatives, polyamines (tetramethylethylenediamine, pentamethyldiethylenetriamine, hexamethyltris(2-aminoethyl)amine, etc.), polycyclic alkaloids such as L-(-)-sparteine, etc. When both a monovalent copper compound and a divalent copper compound are used, the ratio of non-frozen water in the layer containing the polymer chain aggregate can be further increased, and the molecular weight distribution index (Mw / Mn) can be well adjusted. Therefore, the molar ratio of the monovalent copper compound to the divalent copper compound is preferably 10 times or more, more preferably 20 times or more, and even more preferably 30 times or more. A tristriphenylphosphine complex of divalent ruthenium chloride (RuCl2(PPh3)3) is also suitable as a catalyst. When a ruthenium compound is used as a catalyst, it is preferable to add an aluminum alkoxide as an activator. Bistriphenylphosphine complex of divalent iron (FeCl2(PPh3)2), bistriphenylphosphine complex of divalent nickel (NiCl2(PPh3)2), bistributylphosphine complex of divalent nickel (NiBr2(PBu3)2) and the like are also suitable as catalysts. When a copper complex is mixed in radical polymerization, the copper complex may be formed in advance and then used in radical polymerization, or a copper compound and an organic ligand may be mixed in a ratio that forms a copper complex and then radical polymerization may be carried out.The ratio of the copper compound and the organic ligand to be blended in the radical polymerization is preferably such that the number of moles of the organic ligand is 2 or more times, more preferably 2.1 or more times, and most preferably 2.2 or more times the number of moles of the copper compound, so that the organic ligand is sufficiently coordinated to the copper compound and the copper complex is well dissolved.

[0057] The polymerization reaction is preferably carried out in a solvent. Examples of the solvent include hydrocarbon solvents (benzene, toluene, etc.), ether solvents (diethyl ether, tetrahydrofuran, diphenyl ether, anisole, dimethoxybenzene, etc.), halogenated hydrocarbon solvents (methylene chloride, chloroform, chlorobenzene, etc.), ketone solvents (acetone, methyl ethyl ketone, methyl isobutyl ketone, etc.), alcohol solvents (methanol, ethanol, propanol, isopropanol, butyl alcohol, t-butyl alcohol, etc.), nitrile solvents (acetonitrile, propionitrile, benzonitrile, etc.), ester solvents (ethyl acetate, butyl acetate, etc.), carbonate solvents (ethylene carbonate, propylene carbonate, etc.), etc. Examples of the solvent include amide solvents (N,N-dimethylformamide, N,N-dimethylacetamide, etc.), hydrochlorofluorocarbon solvents (1,1-dichloro-1-fluoroethane, dichloropentafluoropropane, etc.), hydrofluorocarbon solvents (hydrofluorocarbons having 2 to 5 carbon atoms, hydrofluorocarbons having 6 or more carbon atoms, etc.), perfluorocarbon solvents (perfluoropentane, perfluorohexane, etc.), alicyclic hydrofluorocarbon solvents (fluorocyclopentane, fluorocyclobutane, etc.), oxygen-containing fluorine-based solvents (fluoroethers, fluoropolyethers, fluoroketones, fluoroalcohols, etc.), and water. These solvents may be used alone or in combination of two or more.

[0058] -Introduction of polymerization initiating groups- To produce a polymer chain assembly using, for example, the grafting-from method, a polymerization initiator group that serves as the initiation point of the polymerization reaction is introduced into the substrate, and the polymer chain is grafted from the polymerization initiator group using the above-mentioned polymerization method. Examples of the polymerization initiator group include a halogenated alkyl group and a halogenated sulfonyl group. The polymerization initiator group is preferably physically or chemically bonded to the substrate surface, since the density of the graft chain (graft density) and the primary structure of the polymer chain obtained by graft polymerization (molecular weight, molecular weight distribution, monomer arrangement pattern) can be precisely controlled. Examples of methods for introducing (bonding) the polymerization initiator group to the substrate surface include the chemical adsorption method and the Langmuir-Blodgett (LB) method. For example, a chlorosulfonyl group (polymerization initiating group) can be introduced onto the surface of a silicon wafer (substrate) by chemical bonding by reacting 2-(4-chlorosulfonylphenyl)ethyltrimethoxysilane or 2-(4-chlorosulfonylphenyl)ethyltrichlorosilane with the oxide layer on the silicon wafer surface.

[0059] To introduce a polymerization initiator group by the LB method, a film-forming material containing a polymerization initiator group is dissolved in a suitable solvent (e.g., chloroform, benzene, etc.). Next, a small amount of this solution is spread on a clean liquid surface, preferably on the surface of pure water, and then the solvent is evaporated or diffused into an adjacent water phase to form a low-density film of film-forming molecules on the water surface. Then, a partition plate is mechanically swept over the water surface to reduce the surface area of ​​the water surface on which the film-forming molecules are spread, thereby compressing the film and increasing its density, thereby obtaining a dense monolayer on the water surface. Next, under suitable conditions, while keeping the surface density of the molecules constituting the monolayer on the water surface constant, the substrate on which the monolayer is deposited is immersed or pulled up in a direction across the monolayer on the water surface, thereby transferring the monolayer on the water surface onto the substrate, and the monolayer is deposited on the substrate. For details of the LB method, see "Kiyonari Fukuda et al., New Experimental Chemistry Lectures, Vol. 18 (Interfaces and Colloids), Chapter 6 (1977), Maruzen," "Kiyonari Fukuda, Michio Sugi and Hiroyuki Suzumebe (eds.), LB Films and Electronics (1986), CMC," or "Yoshio Ishii, Practical Techniques for Making Good LB Films (1989), Kyoritsu Shuppan."

[0060] When introducing a polymerization initiating group onto the surface of a substrate, it is preferable to treat the surface of the substrate with a surface treatment agent having at least one of a group that bonds to the substrate and a group that has affinity with the substrate, and at least one of a group that bonds to the polymerization initiating group and a group that has affinity with the polymerization initiating group. The surface treatment agent may be a low molecular weight compound or a high molecular weight compound. Examples of the surface treatment agent include compounds represented by the following formula (10). [ka] In formula (10), n is an integer of 1 to 10, and preferably an integer of 3 to 8. 11 , R 12 and R 13 R each independently represents a substituent. 11 , R 12 and R 13 At least one of R is preferably an alkoxyl group or a halogen atom. 11 , R 12and R 13 It is particularly preferred that all of R are methoxy groups or ethoxy groups. 14 and R 15 R each independently represents a substituent. 14 and R 15 are preferably each independently an alkyl group having 1 to 3 carbon atoms or an aromatic functional group, and R 14 and R 15 Most preferably, both of X are methyl groups. 11 represents a halogen atom, preferably a bromine atom.

[0061] As the surface treatment agent, it is preferable to use a silane coupling agent containing a polymerization initiator group (a polymerization initiator group-containing silane coupling agent). This allows the surface treatment and the introduction of a polymerization initiator group to be performed simultaneously. Examples of the polymerization initiator group-containing silane coupling agent include compounds represented by the above formula (10). For an explanation of the polymerization initiator group-containing silane coupling agent and its manufacturing method, reference can be made to the description in International Publication No. 2006 / 087839. Specific examples of the polymerization initiator group-containing silane coupling agent include (2-bromo-2-methyl)propionyloxyhexyltrimethoxysilane (BHM) and (2-bromo-2-methyl)propionyloxypropyltrimethoxysilane (BPM).

[0062] From the viewpoint of adjusting the graft density, when a polymerization initiator group-containing silane coupling agent is used as a surface treatment agent, it is preferable to use a silane coupling agent that does not contain a polymerization initiator group, for example, a known alkyl silane coupling agent in combination. This allows the graft density to be freely changed by adjusting the ratio of the polymerization initiator group-containing silane coupling agent and the silane coupling agent that does not contain a polymerization initiator group. For example, when all of the silane coupling agents are polymerization initiator group-containing silane coupling agents, the polymer chain can be grown with a surface occupancy rate exceeding 0.03 by performing graft polymerization by the grafting-from method after the surface treatment. In addition, when a polymerization initiator group-containing silane coupling agent is used as a surface treatment agent, the polymerization initiator group-containing silane coupling agent may be hydrolyzed in the presence of water to form a silanol, which may then be partially condensed to form an oligomer state, and then subjected to surface treatment. Specifically, the oligomer may be adsorbed on a substrate, such as silica, by hydrogen bonding, and then dried to cause a dehydration condensation reaction, thereby introducing a polymerization initiator group into the substrate.

[0063] (base material) In the polymer brush-type polymer chain assembly, the material constituting the substrate (carrier) to which the polymer chains are fixed is not particularly limited and can be appropriately selected from organic materials, inorganic materials, metal materials, and the like. The substrate is preferably a carrier made of a material different from the polymer chain assembly.

[0064] The organic material is not particularly limited, and various resins and rubbers can be used without restrictions. The resin may be either a thermosetting resin or a thermoplastic resin. Examples of the thermosetting resin include epoxy resin, phenol resin, amino resin, unsaturated polyester resin, polyurethane resin, urea resin, melamine resin, thermosetting polyimide resin, and diallyl phthalate resin. Examples of the thermoplastic resin include polyolefin resins such as polyethylene, polypropylene, polystyrene, and polycycloolefin; vinyl resins such as polystyrene, acrylic resin, polyvinyl chloride resin, and polyvinyl alcohol; fluorine resins such as polytetrafluoroethylene; polyester resins such as polyethylene terephthalate, polybutylene terephthalate, polytrimethylene terephthalate, and polyethylene naphthalate; and silicone resins such as polydimethylsiloxane. Examples of rubber include diene-based rubbers such as butadiene rubber, styrene butadiene rubber, chloroprene rubber, isoprene rubber, natural rubber, nitrile rubber, and butyl rubber; and rubbers other than diene-based rubbers such as ethylene propylene rubber, acrylic rubber, polyether rubber, polyurethane rubber, fluororubber, and silicone rubber.

[0065] The substrate may be a polymer monolith. Here, the polymer monolith refers to a polymeric porous body having a three-dimensional co-continuous structure formed by three-dimensionally interconnected continuous pores and a polymer skeleton. The polymer backbone of the polymer monolith is preferably a polymer of a polymerizable compound and a crosslinking agent.

[0066] The polymerizable compound may be any compound capable of forming a polymer skeleton by polymerization with a crosslinking agent, and examples of such compounds include epoxy compounds, (meth)acrylate compounds, and styrene compounds. Among these, epoxy compounds are preferred because they are highly flexible and can easily form a polymer monolith having a fine porous structure. Examples of the epoxy compounds include bisphenol A type epoxy resins, brominated bisphenol A type epoxy resins, bisphenol F type epoxy resins, bisphenol AD ​​type epoxy resins, stilbene type epoxy resins, biphenyl type epoxy resins, bisphenol A novolac type epoxy resins, cresol novolac type epoxy resins, diaminodiphenylmethane type epoxy resins, polyphenyl-based epoxy resins such as tetrakis(hydroxyphenyl)ethane-based epoxy resins, fluorene-containing epoxy resins, and 2,2,2-tri-(2,3-epoxypropyl)-isocyanate. Examples of the epoxy resin include epoxy resins containing heteroaromatic rings such as triglycidyl isocyanurate and triazine ring-containing epoxy resins, aromatic epoxy compounds containing carbon atoms derived from aromatic rings such as N,N,N',N'-tetraglycidyl-m-xylylenediamine, and aliphatic epoxy compounds not containing carbon atoms derived from aromatic rings such as aliphatic glycidyl ether type epoxy resins, aliphatic glycidyl ester type epoxy resins, alicyclic glycidyl ether type epoxy resins, alicyclic glycidyl ester type epoxy resins, and 1,3-bis(N,N'-diglycidylaminomethyl)cyclohexane. Among these, bifunctional or higher epoxy compounds are preferred, and compounds having two or more glycidyl groups in the molecule are more preferred. A preferred example is 1,3-bis(N,N'-diglycidylaminomethyl)cyclohexane.

[0067] Examples of the crosslinking agent include amine compounds, acid anhydrides, phenol compounds, and hydrazide compounds. Examples of the amine compound include aromatic amine compounds such as m-phenylenediamine, p-phenylenediamine, o-phenylenediamine, 4,4'-diaminodiphenylsulfone, 4,4'-methylene-bis(2-chloroaniline), benzyldimethylamine, and dimethylaminomethylbenzene; aromatic amine compounds having a heteroaromatic ring such as a triazine ring; ethylenediamine, diethylenetriamine, triethylenetetramine, tetraethylenepentamine, iminobispropylamine, bis(hexamethylene)triamine, 1,3,6-trisaminomethylhexane, polyamines, and the like. Alicyclic amine compounds such as dimethylaminoethylpiperazine, 3,9-bis(3-aminopropyl)2,4,8,10-tetraoxaspiro(5,5)undecane adduct, bis(4-aminocyclohexyl)methane, and modified products thereof; aliphatic polyamine hydrazide compounds such as 1,6-hexamethylenebis(N,N-dimethylsemicarbazide); and aliphatic polyamidoamines and polyaminoamides formed from polyamines and dimer acids. Examples of the acid anhydride include aromatic acid anhydrides such as phthalic anhydride, trimellitic anhydride, and pyromellitic anhydride. The phenol compound may, for example, be a novolac type phenol resin. Examples of the hydrazide compound include aromatic hydrazide compounds such as isophthalic acid dihydrazide; and aliphatic hydrazide compounds such as adipic acid dihydrazide, sebacic acid dihydrazide, and dodecanedioic acid dihydrazide.

[0068] It is preferable to select the crosslinking agent appropriately according to the type of polymerizable compound. When an epoxy compound is used as the polymerizable compound, the crosslinking agent is preferably an amine compound, more preferably a compound having two or more amino groups in the molecule, which is a bifunctional or higher amine compound. The bifunctional or higher amine compound is preferably an alicyclic amine compound. A preferred example is bis(4-aminocyclohexyl)methane.

[0069] As the polymer backbone of the polymer monolith, from the viewpoint of ease of forming the polymer monolith, it is preferable that it is a polymer of a difunctional or higher epoxy compound and a difunctional or higher amine compound, and it is more preferable that it is a polymer of a difunctional or higher aliphatic epoxy compound and a difunctional or higher alicyclic amine compound.

[0070] The blending ratio of the polymerizable compound and the crosslinking agent may be determined in consideration of the crosslinking density, etc. For example, when the polymerizable compound is a bifunctional or higher epoxy compound and the crosslinking agent is a bifunctional or higher amine compound, it is preferable to adjust the amine equivalent of the crosslinking agent to be in the range of 0.6 to 1.5 relative to 1 equivalent of the epoxy group of the polymerizable compound.

[0071] The polymer monolith can be formed, for example, by a composition for forming a polymer monolith, which contains a polymerizable compound, a crosslinking agent, and a pore-forming agent. More specifically, the composition for forming a polymer monolith is applied to a substrate as a carrier to form a coating film, and the coating film is cured. The polymer component increases with the polymerization of the polymerizable compound, and spinodal decomposition occurs to develop a co-continuous structure. The pore-forming agent is then removed from the cured film to form a polymer monolith.

[0072] The surface on which the polymer monolith is to be formed may be treated with a known coupling agent such as a silane coupling agent or may be subjected to plasma treatment in order to improve affinity with the composition for forming the polymer monolith.

[0073] The inorganic material is not particularly limited, and examples thereof include ceramics (e.g., alumina ceramics, bioceramics, composite ceramics such as zirconia-alumina composite ceramics, etc.), metals (e.g., iron, cast iron, steel, stainless steel, carbon steel, ferrous alloys such as high carbon chromium bearing steel material (SUJ2), non-ferrous and non-ferrous alloys such as aluminum, zinc, copper, titanium, etc.), silicon such as polycrystalline silicon, silicon oxide, silicon nitride, various types of glass, quartz, and composite materials thereof.

[0074] The type of the substrate is not particularly limited. Examples of the material include tubes, sheets, fibers, strips, films, plates, foils, membranes, pellets, powders, particles, molded products (e.g., extrusion molded products, casting molded products, etc.), etc. Furthermore, the article itself to which the member of the present embodiment is applied may be used as the substrate.

[0075] (Other manufacturing methods) The polymer chain assembly of polymer brushes can also be produced by the following production method. That is, the method includes a step of mixing, in a solvent, an organic material constituting a substrate (hereinafter also referred to as substrate polymer) with a plurality of block copolymers each including a polymer block A and a polymer block B having a lower affinity for the substrate polymer than the polymer block A and having the polymer block A at at least two locations to prepare a mixed solution, and a step of removing the solvent from the mixed solution to cause phase separation. This production method can produce a polymer chain assembly of polymer brushes having a loop structure in which both ends of the polymer chains constituting the polymer chain assembly are fixed to a substrate as a carrier.

[0076] The organic material constituting the base material, which is the base polymer, is not particularly limited, and examples thereof include those mentioned above.

[0077] The block copolymer is not particularly limited as long as it comprises polymer block A and polymer block B having lower affinity for the base polymer than polymer block A, and has polymer block A in at least two locations. From the viewpoint of favorable formation of a loop structure, however, it is preferable to use polymer block B that is incompatible with the base polymer, and a combination in which polymer block B is incompatible with the base polymer and polymer block A is compatible with the base polymer is more preferable.

[0078] Here, the polymer block A being compatible with the base polymer refers to the following state: That is, when a polymer consisting of only the polymer block A is mixed with the base polymer by hot melt mixing, co-solution mixing, or the like, and the mixture is then solidified by cooling or evaporating and removing the solvent, and the glass transition temperature (Tg) of the obtained sample is measured, it can be determined that the polymer block A is compatible with the base polymer when a Tg different from the Tg of the polymer consisting of only the polymer block A and the Tg of the base polymer is observed in a temperature range between these two. The immiscibility of the polymer block B with the base polymer refers to the following state: That is, when a polymer consisting of only the polymer block B is mixed with the base polymer by hot melt mixing, co-solution mixing, or the like, and the mixture is then solidified by cooling or evaporating and removing the solvent, and the glass transition temperature (Tg) of the obtained sample is measured, it can be determined that the polymer block B is immiscible when no Tg other than the Tg of the polymer consisting of only the polymer block B and the Tg of the base polymer is observed.

[0079] As the polymer block A and the polymer block B, those having the above-mentioned compatibility with the base polymer may be used. From the viewpoint of favorably forming a loop structure, the difference in SP value (solubility parameter) between the polymer block A and the polymer block B is preferably 1.5 (MPa). 0.5 It is preferable that the temperature is 3 (MPa) or more. 0.5 More preferably, it is 5 (MPa) or more. 0.5 It is more preferable that the difference between the SP value of the polymer block A and the SP value of the base polymer is 0.5 (MPa) or more. 0.5 It is preferable that the temperature is 0.3 (MPa) or less. 0.5 More preferably, it is 0.2 (MPa) or less. 0.5 It is more preferable that the difference between the SP value of the polymer block B and the SP value of the base polymer is 1.5 (MPa) or less. 0.5It is preferable that the temperature is 3 (MPa) or more. 0.5 More preferably, it is 5 (MPa) or more. 0.5 It is more preferable that the SP value is equal to or higher than that. For the SP values ​​of the polymer block A and the polymer block B, for example, values ​​disclosed in Polymer Handbook (4th edition, Wiley-Interscience) can be used.

[0080] The polymer block A is not particularly limited as long as it satisfies the above-mentioned characteristics and may be selected in relation to the base polymer used. Specific examples include those composed of polymer segments constituting the resins or rubbers exemplified as the resins or rubbers constituting the base polymer described above.

[0081] The molecular weight (weight average molecular weight (Mw)) of the polymer block A portion of the block copolymer is not particularly limited, but from the viewpoint of exhibiting sufficient interaction with the base polymer and thereby more appropriately supporting the loop structure formed by the polymer block B, thereby further enhancing durability, it is preferably 1,000 to 100,000, more preferably 1,000 to 50,000, even more preferably 1,000 to 20,000, still more preferably 2,000 to 20,000, and particularly preferably 2,000 to 6,000.

[0082] As the polymer block B, of the polymer chains described above, those which satisfy the above-mentioned properties between themselves and the base polymer are preferably used.

[0083] The solvent used when mixing the base polymer and the multiple block copolymer chains in a solvent is not particularly limited, and any solvent that can dissolve or disperse the base polymer and the block copolymer chains may be used. Examples of the solvent include aliphatic hydrocarbons such as n-pentane, n-hexane, and n-heptane; alicyclic hydrocarbons such as cyclopentane, cyclohexane, methylcyclohexane, dimethylcyclohexane, trimethylcyclohexane, ethylcyclohexane, diethylcyclohexane, decahydronaphthalene, bicycloheptane, tricyclodecane, hexahydroindene, and cyclooctane; aromatic hydrocarbons such as benzene, toluene, xylene, and mesitylene; nitrogen-containing hydrocarbons such as nitromethane, nitrobenzene, acetonitrile, propionitrile, and benzonitrile; ethers such as diethyl ether, tetrahydrofuran, and dioxane; ketones such as acetone, ethyl methyl ketone, methyl isobutyl ketone, cyclopentanone, and cyclohexanone; esters such as methyl acetate, ethyl acetate, ethyl propionate, and methyl benzoate; halogenated hydrocarbons such as chloroform, dichloromethane, 1,2-dichloroethane, chlorobenzene, dichlorobenzene, and trichlorobenzene; and alcohols such as methanol and ethanol.

[0084] In such a solvent, the base polymer and a plurality of block copolymer chains are mixed and dissolved or dispersed to obtain a mixed solution. Next, the obtained mixed solution is used to form a film by a casting method, a spin coating method, or the like, and then the solvent is removed from the mixed solution from which the film has been formed. By removing the solvent, a part of the plurality of block copolymer chains dispersed in the base polymer through the solvent is changed to a state in which the polymer block A remains in a compatible state with the base polymer, and the polymer block B constituting the block copolymer chain is phase-separated from the base polymer, so that the polymer block A is in the base polymer and the polymer block B is exposed from the base polymer, thereby forming a loop structure in which both ends of the polymer chains constituting the polymer chain assembly are fixed to a carrier.

[0085] The method for removing the solvent is not particularly limited and may be selected depending on the type of solvent used, but a method of heating at 50°C to 100°C is preferred, and a method of heating at 70°C to 80°C is more preferred.

[0086] The polymer chain assembly of polymer brushes can also be produced by the following production method. That is, the method includes a step of mixing a base polymer with a plurality of block copolymers, each of which comprises a polymer block A and a polymer block B having a lower affinity for the base polymer than the polymer block A and has the polymer block A at at least two locations, under heating to prepare a molten mixture, and a step of cooling the molten mixture to cause phase separation. This production method can also be used to produce a polymer chain assembly of polymer brushes having a loop structure in which both ends of the polymer chains constituting the polymer chain assembly are fixed to a substrate as a carrier.

[0087] The heating temperature when preparing a molten mixture by mixing the base polymer and multiple block copolymers under heating is not particularly limited and may be a temperature at which the base polymer or the block copolymers melt, preferably a temperature at which both the base polymer and the block copolymer chains melt, and is preferably 40 to 300°C, more preferably 80 to 200°C.

[0088] The resulting molten mixture is used to form a film by casting, spin coating, dip coating, or the like, and then cooled to cause phase separation during the solidification process. As a result of being melt-mixed, some of the block copolymers dispersed in the base polymer undergo a transition from a molten state to a solid state, during which polymer block A remains in a compatible state with the base polymer, while polymer block B constituting the block copolymer undergoes phase separation from the base polymer, thereby changing the state so that polymer block A is present in the base polymer and polymer block B is exposed from the base polymer, thereby forming a loop structure.

[0089] The method for cooling the molten mixture is not particularly limited, but examples include a method in which the molten mixture formed into a film is allowed to stand at room temperature, and a method in which the molten mixture is allowed to stand at a heated temperature lower than the melting temperature of each component constituting the molten mixture.

[0090] (Number average molecular weight and molecular weight distribution index of polymer chains) The number average molecular weight (Mn) of the polymer chains constituting the polymer chain assembly is preferably 500 to 10,000,000, and more preferably 100,000 to 10,000,000. The molecular weight distribution index (Mw / Mn) of the polymer chain assembly is preferably 1.0 to 2.0, more preferably 1.0 to 1.5, from the viewpoint of retaining a larger amount of antifreeze water in the layer containing the polymer chain assembly. If the molecular weight distribution index (Mw / Mn) is within the above range, it is expected that the polymer chains constituting the polymer chain assembly can maintain a high density state up to the outermost surface. For example, the molecular weight distribution index (Mw / Mn) can be adjusted by the ratio of the monovalent copper compound and the divalent copper compound in the copper catalyst used in the radical polymerization to form the polymer chain assembly, the number of moles of the organic ligand relative to the copper compound, etc. The number average molecular weight (Mn) and molecular weight distribution index (Mw / Mn) of a polymer chain aggregate can be measured by cutting out polymer chains from a substrate by treatment with hydrofluoric acid, and then subjecting the cut out polymer chains to molecular weight analysis by size exclusion chromatography such as gel permeation chromatography. In addition, when a polymer chain assembly is formed using a graft polymerization method, it is assumed that the free polymer generated during the polymerization reaction of the polymer chain has the same molecular weight as the polymer chain fixed to the substrate, and the number average molecular weight (Mn) and molecular weight distribution index (Mw / Mn) of the free polymer are measured by size exclusion chromatography, and the results are used as the number average molecular weight (Mn) and molecular weight distribution index (Mw / Mn) of the polymer chain. It has been confirmed that the number average molecular weight (Mn) and molecular weight distribution index (Mw / Mn) of the polymer chain fixed to the substrate are almost equal to those of the free polymer generated during the polymerization reaction.

[0091] The method for measuring molecular weight using free polymers will be specifically described. When polymer chains are synthesized by surface-initiated living radical polymerization, adding a free initiator to the polymerization solution makes it possible to obtain a free polymer with the same molecular weight and molecular weight distribution as the polymer chains that compose the polymer chain assembly. The number average molecular weight (Mn) and molecular weight distribution index (Mw / Mn) of this free polymer are determined by analyzing it using size exclusion chromatography.

[0092] The analysis by size exclusion chromatography involves a calibration method using available homogeneous monodisperse standard samples with known molecular weights, and absolute molecular weight evaluation using a multi-angle light scattering detector. In the examples of this specification, the values ​​of number average molecular weight (Mn) and weight average molecular weight (Mw) are shown as absolute values ​​appropriately calculated using a multi-angle light scattering detector and molecular weight calibration curves of various standard samples. Examples of standard samples include polystyrene standard samples, polymethyl methacrylate standard samples, and polyethylene glycol standard samples.

[0093] The density of polymer chains on the substrate surface is 0.01 chains / nm 2 More preferably, it is 0.05 chains / nm or more. 2 More preferably, it is 0.1 chains / nm or more. 2 More preferably, it is 0.2 chains / nm or more. 2 The upper limit is particularly preferably 1.0 chain / nm. 2 Can be less than 0.9 chains / nm 2 It can also be the following:

[0094] The density of the polymer chains can be calculated by measuring the graft amount (W) per unit area and the number average molecular weight (Mn) of the polymer chain aggregate, and using the following formula. Polymer chain density (chains / nm 2 )=W(g / nm 2 ) / Mn × (Avogadro's number) In the formula, W represents the graft amount per unit area, and Mn represents the number average molecular weight of the polymer chain assembly. When the substrate is a flat substrate such as a silicon wafer, the graft amount (W) per unit area can be determined by measuring the total thickness in a dry state, i.e., the thickness of the polymer chain assembly layer in a dry state, by an ellipsometry method, and calculating the graft amount (W) per unit area using the density of the bulk film. The number average molecular weight (Mn) of the polymer chain assembly can be measured by the method described above.

[0095] The surface occupancy of the polymer chains on the substrate surface (cross-sectional area of ​​the polymer × density of the polymer chains) is preferably 0.01 or more, more preferably 0.05 or more, and even more preferably 0.10 or more. The surface occupancy means the ratio of the substrate surface occupied by the graft points (first structural unit), and is 1 in close packing. The density of the polymer chains can be calculated by the method described above. The cross-sectional area of ​​the polymer can be calculated using the repeating unit length in the stretched form of the polymer and the bulk density of the polymer. When the polymer is a copolymer, it can be calculated as a number average value according to the ratio of the monomers that constitute the polymer. The surface occupancy rate of the polymer chains on the substrate surface is preferably 0.08 to 0.65, more preferably 0.10 to 0.40, and even more preferably 0.15 to 0.25 from the viewpoint of preventing snow from adhering outdoors.

[0096] In the member of this embodiment, when it has a polymer brush structure, from the viewpoint of obtaining an excellent ice formation suppression effect in a wide range of 0° C. to −18° C., it is preferable that the substrate is a carrier made of a substance other than the polymer chain assembly, and the surface occupancy of the polymer chains on the substrate surface is 0.08 to 0.65 (preferably 0.10 to 0.40, more preferably 0.15 to 0.40). In particular, when it has a polymer brush structure, if the surface occupancy is in the above range, the brush density is in an appropriate range, which improves the retention of liquid substances (particularly for liquid substances that are not phase with water, the retention is greatly improved), and the suppression of ice nucleation due to the size exclusion effect can be further improved.

[0097] [B] Member having a bottle brush structure Next, a member having a bottle brush structure will be described. The bottle brush structure refers to a branched polymer structure in which a plurality of side chains are branched from the main chain, forming a bottle brush-like shape as a whole. In the bottle brush structure, the main chain constitutes the base material, and the side chains constitute the polymer chain assembly, and further, the bottle brush structure may be bonded to a carrier to form a member having a bottle brush structure. Examples of the carrier include those mentioned above. In this case, both the bottle brush and the polymer brush may be fixed or bonded to the carrier. In this case, the polymer brush is preferably a dense polymer brush. The member of the present embodiment is preferably a member having a bottle brush structure in which the plurality of polymer chains are bonded as side chains to the base polymer chain.

[0098] A member having a bottle brush structure can also be obtained by graft polymerization. The graft polymerization can be performed using a grafting-to method in which a reactive side chain (graft chain) synthesized in advance is bonded to a trunk polymer that becomes a main chain, a grafting-from method in which a side chain (graft chain) grows from a polymerization initiator group of a macroinitiator (trunk polymer with a polymerization initiator group introduced therein), or a grafting-through method in which a macromonomer (a polymer having a polymerizable functional group at the end of a side chain constituent polymer) is polymerized. In addition, living anionic polymerization, ring-opening metathesis polymerization (ROMP), or the highly versatile living radical polymerization method (LRP) can be used to synthesize these side chains and trunk polymers. A preferred example of a member having a bottle brush structure can be a compound represented by formula (11). [ka] In formula (11), R 1 and R 2 each independently represents a hydrogen atom or a methyl group, R 3 R represents a substituent, and is preferably an alkyl group having 1 to 10 carbon atoms. 4 and R 5 represents an end group consisting of an atom or an atomic group, and examples thereof include a hydrogen atom, a halogen, and a functional group derived from a polymerization initiator. X represents O or NH, Y represents a divalent organic group, n represents an integer of 10 or more, and Polymer A represents a polymer chain. In the compound represented by formula (11), the repeating structure of the constitutional unit bounded by n corresponds to the main chain of the bottle brush structure, and Polymer A corresponds to the side chain of the bottle brush structure.

[0099] Examples of the organic group represented by Y include an alkylene group having 1 to 10 carbon atoms, an oxyalkylene group (RO) having 1 to 5 carbon atoms (R represents an alkylene group having 1 to 5 carbon atoms), a linking structure in which a plurality of such oxyalkylene groups are linked, or a divalent organic group consisting of a combination of at least two of such organic groups (an alkylene group having 1 to 10 carbon atoms, an oxyalkylene group having 1 to 5 carbon atoms, and a linking structure of an oxyalkylene group). Here, the alkylene group and the alkylene group of the oxyalkylene group may be linear or branched, and may have a cyclic structure. Specific examples of the alkylene group include an ethylene group, a propylene group, a butylene group, and a cyclohexylene group. The alkylene group and the alkylene group of the oxyalkylene group may be substituted with a substituent. Examples of the substituent include an alkyl group having 1 to 10 carbon atoms, an aryl group having 6 to 40 carbon atoms, and a heteroaryl group having 3 to 40 carbon atoms, and these substituents may be further substituted with a substituent. The above-mentioned polymer chain can be referred to for the description of Polymer A, its preferred range, and specific examples. In Polymer A, the constituent units of the main chain may be the same or different from each other.

[0100] In a component having a bottle brush structure, when the main chain is taken as the central axis, the side chains (graft chains) are extended in a straight line from the central axis, and a surface (virtual outer periphery) including the tips is imagined, the external shape of the component can be considered as a cylinder with the surface including the tips as the side. In a component having such an external shape, the longer the side chains (graft chains), the lower the density of the side chains (graft chains) on the side surface, and the higher the structural freedom of the side chains (graft chains). As a result, the side chains (graft chains) can be freely folded.

[0101] In materials with a bottle-brush structure, the surface occupancy rate of side chains (σ * ) can be calculated using the following formula:

number

[0102] The surface occupancy rate of the side chains of the member having a bottle-brush structure is preferably 0.01 or more, more preferably 0.05 or more, and even more preferably 0.10 or more. The surface occupancy rate of the side chains is preferably 0.08 to 0.65, more preferably 0.10 to 0.50, and further preferably 0.20 to 0.40.

[0103] The density of side chains in the bottle-brush structure is 0.01 chains / nm 2 More preferably, it is 0.05 chains / nm or more. 2 More preferably, it is 0.1 chains / nm or more. 2 More preferably, it is 0.2 chains / nm or more. 2 The upper limit is particularly preferably 1.0 chain / nm. 2 Can be less than 0.9 chains / nm 2It can also be the following:

[0104] The number average molecular weight of the member having a bottle brush structure is preferably 1,000 to 10,000,000, more preferably 1,000 to 1,000,000, and even more preferably 5,000 to 500,000.

[0105] The molecular weight distribution index (Mw / Mn) of the member having a bottle-brush structure is preferably 1.0 to 2.0, and more preferably 1.0 to 1.5. When the molecular weight distribution index is within the above range, it is expected that the polymer chains constituting the polymer chain assembly can maintain a high density state up to the outermost surface.

[0106] When the member of this embodiment is a member having a bottle brush structure, the member has a bottle brush structure in which the multiple polymer chains are bonded as side chains to the base polymer chain, and the member having the bottle brush structure preferably has a surface occupancy rate of the side chains of 0.08 to 0.50 (more preferably 0.10 to 0.50, and even more preferably 0.15 to 0.50).

[0107] [Liquid substance] The layer containing the polymer chain assembly of the member of the present embodiment holds a liquid substance, and the liquid substance contains at least water. The liquid substance may be only water, or may further contain other liquid substances. The liquid substance other than water is preferably a hydrophilic liquid substance. Examples of the hydrophilic liquid substance include hydrophilic ionic liquids, low molecular weight alcohols such as methanol and ethanol, acetonitrile, acetone, and ethylene glycol. The liquid substance may contain an additive.

[0108] Ionic liquids are also called ionic liquids or room temperature molten salts, and are salts with low melting points and ion conductivity. Most ionic liquids have relatively low melting points obtained by combining an organic onium ion as a cation and an organic or inorganic anion as an anion. The melting point of an ionic liquid is usually 100°C or lower, preferably room temperature (25°C) or lower. The melting point of an ionic liquid can be measured by a differential scanning calorimeter (DSC) or the like.

[0109] As the ionic liquid, a compound represented by the following formula (20) can be used: The melting point of this ionic liquid is preferably 50° C. or lower, and more preferably 25° C. or lower. [ka] In formula (20), R 21 , R 22 , R 23 and R 24 are each independently an alkyl group having 1 to 5 carbon atoms, or R'-O-(CH2) n -, R' represents a methyl group or an ethyl group, and n is an integer of 1 to 4. 21 , R 22 , R 23 and R 24 may be the same or different. 21 , R 22 , R 23 and R 24 Any two of R may be bonded to each other to form a cyclic structure. 21 , R 22 , R 23 and R 24 At least one of X is an alkoxyalkyl group. 21 represents a nitrogen atom or a phosphorus atom, and Y represents a monovalent anion.

[0110] R 21 , R 22 , R 23 and R 24Examples of the alkyl group having 1 to 5 carbon atoms in the formula (I) include a methyl group, an ethyl group, an n-propyl group, a 2-propyl group, an n-butyl group, and an n-pentyl group. R 21 , R 22 , R 23 and R 24 In the formula, R'-O-(CH2) n The alkoxyalkyl group represented by - is preferably a methoxymethyl group or an ethoxymethyl group, a 2-methoxyethyl group or a 2-ethoxyethyl group, a 3-methoxypropyl group or a 3-ethoxypropyl group, a 4-methoxybutyl group or a 4-ethoxybutyl group, or the like. R 21 , R 22 , R 23 and R 24 Compounds in which any two of the above are bonded to form a ring structure include X 21 When a nitrogen atom is used for X, a quaternary ammonium salt having an aziridine ring, an azetidine ring, a pyrrolidine ring, a piperidine ring, or the like is preferred. 21 When a phosphorus atom is used, a quaternary phosphonium salt having a pentamethylenephosphine (phosphorinane) ring or the like is preferred. As the quaternary ammonium salt, one having, as a substituent, a methyl group for R' and at least one 2-methoxyethyl group with n being 2 is preferred. The monovalent anion at Y is BF4 - , PF6 - , AsF6 - , SbF6 - , AlCl4 - , NbF6 - , HSO4 - , ClO4 - , CH3SO3 - , CF3SO3 - , CF3CO2 - , (CF3SO2)2N - , Cl - , Br - , I - BF4 - , PF6 - , (CF3SO2)2N - , CF3SO3- , or CF3CO2 - It is preferable that:

[0111] As the ionic liquid, R 21 is a methyl group, and R 23 and R 24 is an ethyl group, and R 24 is R'-O-(CH2) n Compounds having an alkoxyalkyl group structure represented by the formula - are preferably used.

[0112] Among the compounds represented by formula (20), specific examples of the quaternary ammonium salt and the quaternary phosphonium salt that can be suitably used include the compounds shown below. [ka]

[0113] As the ionic liquid, an ionic liquid containing an imidazolium ion or an ionic liquid containing an aromatic cation can also be used.

[0114] The method of holding a liquid substance in the layer containing polymer chain assemblies is not particularly limited. For example, a method of applying a liquid substance to the surface of the layer containing polymer chain assemblies and then leaving it to be held, or a method of immersing a substrate on which a layer containing polymer chain assemblies is formed in a liquid substance, etc. In addition, the polymer chain assemblies may take in moisture from the atmosphere and hold water as a liquid substance in the layer containing polymer chain assemblies.

[0115] The mass ratio of water relative to 100 parts by mass of the above liquid substance is preferably 80 parts by mass or more, more preferably 90 parts by mass or more, even more preferably 95 parts by mass or more, and particularly preferably 100 parts by mass. The water as the liquid substance includes nonfreezing water. The mass ratio of the nonfreezing water to the total mass of water in the liquid substance is 15 mass% or more as a lower limit, preferably 20 mass% or more, more preferably 25 mass% or more, and 50 mass% or less as an upper limit, preferably 40 mass% or less, more preferably 30 mass% or less. The mass ratio of the nonfreezing water to the total mass of water in the liquid substance can be adjusted by the monomer composition of the polymer chain, etc. The water in the layer containing the polymer chain aggregates includes bulk water and hydrated water (e.g., water in the polymer chains) contained in the layer, and the hydrated water includes free water and intermediate water that freeze at −90° C., and nonfreezing water that does not freeze at −90° C. The mass proportion of the nonfreezing water can be measured by the method described in the Examples below.

[0116] [Material characteristics] The member of this embodiment has an icing stress at -18°C of 150 kPa or less, preferably 100 kPa or less, more preferably 80 kPa or less, more preferably 65 kPa or less, even more preferably 50 kPa or less, still more preferably 35 kPa or less, and particularly preferably 20 kPa or less. The icing stress at -18°C can be measured by the method described in the Examples below. The above-mentioned ice adhesion stress at -18°C can be adjusted by the type of polymer chain, the type of liquid substance, the surface occupancy of the polymer chain, and the like.

[0117] The member of this embodiment has an ice accretion stress of preferably 10 to 50 kPa, more preferably 10 to 30 kPa, and even more preferably 0 to 20 kPa at -8°C. When the ice accretion stress at -8°C is within the above range, an excellent ice accretion suppression effect can be obtained in a wide range of 0°C to -18°C. The above-mentioned ice adhesion stress at -8°C can be adjusted by the type of polymer chain, the type of liquid substance, the surface occupancy of the polymer chain, etc.

[0118] The difference between the ice accretion stress of the member of this embodiment at -18°C and that at -8°C is preferably 100 kPa or less, more preferably 90 kPa or less, even more preferably 80 kPa or less, even more preferably 50 kPa or less, even more preferably 30 kPa or less, and particularly preferably 10 kPa or less. When the difference is within the above range, an excellent ice accretion suppression effect can be obtained in a wide range of 0°C to -18°C, and in particular, when a compatible polymer chain is used as the polymer chain, a particularly excellent ice accretion suppression effect can be obtained at 0°C to -20°C. The member of this embodiment preferably has a higher icing stress at -18°C than at -8°C. In this specification, the difference between the icing stress at -18°C and the icing stress at -8°C refers to the absolute value of the difference.

[0119] In this embodiment, the contact angle of the component surface with water at 25°C is preferably 10° or more, more preferably 20° or more, even more preferably 45° or more, even more preferably 48° or more, and particularly preferably 48 to 80°. If the contact angle is within the above range, a better water droplet adhesion suppression effect, ice formation suppression effect, and ice nucleation suppression effect can be obtained. In this specification, the value of the contact angle of the component surface with water is a value obtained by dropping 1 μL of water on the component surface at 23°C and measuring the contact angle of water on the component surface 1 second after the drop has landed.

[0120] In the member of this embodiment, from the viewpoint of being able to retain a larger amount of antifreeze water in the layer containing the polymer chain assembly, the ratio of the total molecular weight of the antifreeze-forming structural moieties contained in each antifreeze-forming monomer unit contained in the polymer chain to the number average molecular weight of the polymer chain in the layer containing the polymer chain assembly (total molecular weight of the antifreeze-forming structural moieties contained in the antifreeze-forming monomer unit / number average molecular weight of the polymer chain) is preferably 0.75 or more, more preferably 0.80 or more, and even more preferably 0.80 to 0.95. The above ratio can be adjusted by the mass ratio of the antifreeze-forming monomer unit, etc. The above ratio can be measured by the method described in the Examples below.

[0121] [Part Shape] The shape of the member of the present embodiment is not particularly limited, and may be a tube, sheet, fiber, strip, film, plate, foil, membrane, pellet, powder, particle, or the like.

[0122] [Application form of the material] The member of the present embodiment can be applied to various articles, such as window glass, vehicle glass, mirrors, piping, and containers. The member of this embodiment has an ice accretion stress that does not change significantly in the temperature range of 0°C to -20°C, and therefore can be suitably used in applications where ice accretion needs to be suppressed over a wide temperature range of 0°C to -20°C.

[0123] The present invention may be a member capable of retaining a liquid material containing at least water in a layer containing a polymer chain assembly, and capable of making the ratio of nonfreezing water to the total amount of water in the liquid material 15 mass % or more. For example, the member obtained by the above-mentioned method can be manufactured by drying the member and immersing it in water. Since the permeated water is likely to strongly interact with the polymer in the layer containing the polymer chain assembly, most of the permeated water becomes nonfreezing water that does not freeze even at -90°C. EXAMPLES

[0124] The present invention will be described in more detail below based on examples, but the present invention is not limited to these examples.

[0125] Example 1 The silicon wafer and DSC pan (made of aluminum) were ultrasonically cleaned in acetone for 30 minutes, in chloroform for 30 minutes, and in 2-propanol for 30 minutes, respectively, and then both sides of the silicon wafer and DSC pan were irradiated with UV ozone for 30 minutes. Next, only the DSC pan was coated with silica. Next, the silicon wafer and the silica-coated DSC pan were ultrasonically cleaned in ethanol for 30 minutes, and then immersed in a mixture of (2-bromo-2-methyl)propionyloxypropyltrimethoxysilane (BPM) / ethanol / ammonia water = 1 / 89 / 10 (mass ratio) for 24 hours to introduce polymerization initiator groups into the silicon wafer and DSC pan. Next, methoxypoly(ethylene glycol) methacrylate (manufactured by Aldrich, code 10001) was added to the DSC pan. 50 parts by mass of a mixture of ethyl 2-bromo-2-methylpropionate (EBIB), copper (I) bromide (CuBr(I), copper (II) bromide (CuBr(II)), and 4,4'-dinonyl-2,2'-bipyridine (diNbip) (PEGMA / EBIB / CuBr(I) / CuBr(II) / diNbip=200,000 / 0.1 / 1036.8 / 28.8 / 2344 (molar ratio)), and 50 parts by mass of anisole. The silicon wafer with the polymerization initiator group introduced and the DSC pan were placed in a fluororesin container containing the above. The container was sealed, covered with an aluminum bag, and placed in a high-pressure reactor to carry out the polymerization reaction at 400 MPa and 60°C for 4 hours. After the polymerization reaction was completed, the silicon wafer and the DSC pan were removed from the container and washed with tetrahydrofuran using a shaking device. After that, by drying, a brush-like polymer chain assembly (polymer brush layer) consisting of multiple polymer chains was formed on the silicon wafer surface, and a test specimen was obtained. The thickness of the layer of the obtained test specimen was measured using an atomic force microscope in both a dry state and when immersed in water. The results showed that the mass ratio of water was 50 parts by mass when the mass of polymer chains contained in the layer containing polymer chain assemblies was 100 parts by mass. Subsequent analysis revealed that the thickness of the polymer brush layer formed on the silicon wafer surface was 1102 nm, and the number average molecular weight was 6.2 × 10 6, molecular weight distribution index (Mw / Mn) is 1.4, polymerization rate is 3%, and density of polymer chain is 0.12 chains / nm 2 The surface occupancy rate of the polymer chains was 0.33. The film thickness of the polymer brush layer was measured by ellipsometry. The number average molecular weight and molecular weight distribution index of the polymer brush layer were calculated by gel permeation chromatography using dimethylformamide containing 10 mM lithium bromide as the developing solvent and a multi-angle light scattering detector as the detector. The polymer polymerization rate was 1 Measurements were performed by H-NMR. The obtained DSC pan was dried under reduced pressure at 40°C for 24 hours. Then, it was moistened with 0.03 mg of water (amount of water exceeding the water content (Wmax) in the layer in the saturated swollen state). It was confirmed by the method described below that the layer containing the polymer chain assembly contained 20% by mass of non-frozen water. In addition, it was confirmed by differential scanning calorimetry that water was retained in liquid form in the layer containing the polymer chain assembly even at -18°C.

[0126] Example 2 A member was obtained in the same manner as in Example 1, except that methoxypoly(ethylene glycol) methacrylate (manufactured by Aldrich, code (447951), number average molecular weight = 950) was used instead of methoxypoly(ethylene glycol) methacrylate (manufactured by Aldrich, code 447943, number average molecular weight = 500).

[0127] Example 3 A member was obtained in the same manner as in Example 1, except that a mixture of 50 parts by weight of methoxypoly(ethylene glycol)methacrylate (manufactured by Aldrich, code 447943, number average molecular weight = 500) and 50 parts by weight of methoxypoly(ethylene glycol)methacrylate (manufactured by Aldrich, code (447951), number average molecular weight = 950) was used instead of methoxypoly(ethylene glycol)methacrylate (manufactured by Aldrich, code 447943, number average molecular weight = 500).

[0128] Example 4 A member was obtained in the same manner as in Example 1, except that a mixture of 50 parts by weight of methoxypoly(ethylene glycol)methacrylate (manufactured by Aldrich, code (447935), number average molecular weight = 300) and 50 parts by weight of methoxypoly(ethylene glycol)methacrylate (manufactured by Aldrich, code (447951), number average molecular weight = 950) was used instead of methoxypoly(ethylene glycol)methacrylate (manufactured by Aldrich, code 447943, number average molecular weight = 500).

[0129] Example 5 A member was obtained in the same manner as in Example 1, except that a mixture of 50 parts by weight of methoxypoly(ethylene glycol)methacrylate (manufactured by Aldrich, code (447935), number average molecular weight = 300) and 50 parts by weight of methoxypoly(ethylene glycol)methacrylate (manufactured by Aldrich, code 447943, number average molecular weight = 500) was used instead of methoxypoly(ethylene glycol)methacrylate (manufactured by Aldrich, code 447943, number average molecular weight = 500).

[0130] Comparative Example 1 A member was obtained in the same manner as in Example 1, except that methoxypoly(ethylene glycol) methacrylate (manufactured by Aldrich, code (447935), number average molecular weight = 300) was used instead of methoxypoly(ethylene glycol) methacrylate (manufactured by Aldrich, code 447943, number average molecular weight = 500).

[0131] [evaluation] The members obtained in the above examples were subjected to the following measurements.

[0132] (Surface occupancy) Calculated using the method described above.

[0133] (mass fraction of water in the layer containing polymer chain aggregates) When producing the members in the examples and comparative examples, the thickness of the layer containing the polymer chain aggregates after drying under reduced pressure at 40°C for 24 hours and the difference in height between areas where the layer was present and where it was not present were measured using an atomic force microscope (product name (NanoWizard3, manufactured by JPK Instruments)) in contact mode. The thickness of the layer containing the polymer chain assemblies in a saturated swollen state, i.e., the state where the layer was immersed in ion-exchanged water at room temperature, was then measured in the same manner, and the amount of water (Wmax, unit (mg)) contained in the layer containing the polymer chain assemblies in a saturated swollen state was calculated from the difference between the layer thickness in the saturated swollen state and the layer thickness in the dry state. In addition, the layer containing the polymer chain assembly of the dry member produced in the same manner as above was moistened by adding ion-exchanged water in an amount (Wcal, unit (mg)) exceeding the above Wmax to obtain a member in a moist state. The member in the moist state was covered with a lid (Tzero Hermetic Lid, manufactured by TA Instruments) and sealed, and then cooled from 25°C to -90°C at a cooling rate of 3°C / min using a Discovery DSC 2500 type differential scanning calorimeter (manufactured by TA Instruments), and heated to 50°C at a heating rate of 3°C / min to perform differential scanning calorimetry, and the amount of frozen water (Wice, unit (mg)) in the layer containing the polymer chain assembly in the moist state was calculated by dividing the heat of fusion calculated from the DSC curve by the latent heat of fusion of ice (334J / g). The amount of unfrozen water Wf (unit: mg) was obtained by subtracting Wice from the amount of ion-exchanged water Wcal added to the layer containing the polymer chain assembly, and the proportion of unfrozen water Wf / Wmax × 100 (unit: mass %) was calculated. When an excess amount of water is added to a layer containing polymer chain assemblies, it becomes bulk water and hydrated water (water in the polymer). The hydrated water includes free water that freezes at 0°C, intermediate water that does not freeze at 0°C but freezes when cooled to -90°C, and unfrozen water that does not freeze even at -90°C. The free water and intermediate water are hydrated water in polymer chains that freezes at -90°C. In this specification, the total mass of water in the liquid substance when measuring the mass proportion of water in a layer containing polymer chain assemblies may be the total mass of hydrated water excluding bulk water.

[0134] (Molecular weight ratio of nonfreezing water forming structure part) Polymer chains were cut from the substrate of the layer containing the polymer chain aggregates by hydrofluoric acid treatment, and the number average molecular weight (Mn) of the cut polymer chains was measured by molecular weight analysis using size exclusion chromatography. In addition, the structure of the nonfreeze-water-forming monomer unit contained in the polymer chain assembly was analyzed, and the molecular weight was calculated from the composition of the nonfreeze-water-forming structural portion in the monomer unit. The molecular weight analysis by size exclusion chromatography was carried out as follows. The analysis by size exclusion chromatography was carried out using a multi-angle light scattering detector (product name (see Examples)) and a molecular weight calibration curve prepared using a polymethyl methacrylate standard sample, which is a homogeneous monodisperse standard sample with a known molecular weight. The size exclusion chromatography analysis was carried out under the following conditions. Name and model of the device used: Shodex GPC-101 Column product name and model number: Shodex, LF-804, KF-06L Eluent:DMF / LiBr(10mM) Eluent flow rate: 0.8mL / min Column temperature: 40℃ Detector name and model number: Wyatt Technology, DAWN-HELLO Table 1 shows the number average molecular weight Mn of the polymer chain cut out from the layer containing the polymer chain assembly, and the weight average molecular weight (Mw) / number average molecular weight (Mn). The ratio of the total molecular weight of the nonfreeze-water-forming structural portion contained in the nonfreeze-water-forming monomer unit constituting the nonfreeze-water-forming unit to the molecular weight of the polymer chain was calculated from the following formula (1). Sum of molecular weights of nonfreezable water-forming structural parts contained in each monomer unit constituting the nonfreezable water-forming unit / Sum of molecular weights of monomer units constituting the polymer chain (1)

[0135] (Icing Stress) The members obtained in the examples and comparative examples were set on a microscope-use extension stage with cooling function (manufactured by Japan Hightec Co., Ltd.) and ice adhesion stress measurements were performed. The icicles were made by injecting 60 μL of pure water into the inside of an aluminum cylinder (inner diameter 6 mm) with silicone grease applied to the edge, cooling it to -20°C at a rate of 5°C / min, and holding it for 30 minutes. The set temperature of the stage was then raised to -18°C at a rate of 5°C / min and held for 30 minutes, after which the test was performed. The L-shaped jig attached to the stage was set to push the aluminum cylinder as the extension stage moved, and the ice adhesion stress (kPa) was calculated from the load applied to the load cell of the extension stage when the icicle peeled off (Figure 1). Evaluation was performed according to the following criteria. The stage movement speed was 10 mm / min. ◎(Excellent):Icing stress is less than 50kPa ○ (Excellent): Ice stress is 50 kPa or more and less than 100 kPa △ (Good): Ice stress is 100kPa or more but less than 150kPa × (bad): Ice adhesion stress is 150 kPa or more

[0136] (Thickness of layer containing polymer chain aggregates) Measurements were performed at room temperature using a spectroscopic ellipsometric method (MASS-105, manufactured by Filab). The optical constants were measured using files prepared using each specimen according to the manufacturer's method.

[0137] (Swelling degree) The members prepared in the examples and comparative examples were dried under reduced pressure at 40°C for 24 hours. The layer containing the polymer chain aggregates of the members was scratched with the tip of tweezers. The height of the step (i.e., the thickness of the layer containing the polymer chain aggregates in a dry state) was measured at the boundary between the part where the substrate base was exposed and the part where the layer containing the polymer chain aggregates was present, using an atomic force microscope colloidal probe method (contact mode). Next, the same test body was immersed in ion-exchanged water at room temperature, and the height of the step in the swollen state was measured at the same location in the liquid using an atomic force microscope colloidal probe method (contact mode). The degree of swelling was calculated from the thickness of the layer in the swollen state / the thickness of the layer in the dry state.

[0138]

Table 1

Claims

1. a layer including a brush-like polymer chain assembly including a plurality of polymer chains fixed to a substrate; the layer containing the polymer chain assembly holds a liquid substance, A member for suppressing ice nucleation or icing, wherein at least a portion of the liquid substance is water, and the proportion of nonfreezing water relative to the total mass of the water in the liquid substance is 15 mass % or more.

2. The member according to claim 1 , wherein the polymer chain contains an antifreeze-forming unit composed of an antifreeze-forming monomer unit.

3. The member according to claim 1 or 2, wherein a ratio of the sum of the molecular weights of the nonfreeze-water-forming structural moieties contained in the nonfreeze-water-forming monomer units in the polymer chain to the molecular weight of the polymer chain (the sum of the molecular weights of the nonfreeze-water-forming structural moieties contained in the nonfreeze-water-forming monomer units / the molecular weight of the polymer chain) is 0.80 or more.

4. the substrate is a carrier made of a material different from the polymer chain assembly, 3. The member according to claim 1, wherein the surface occupancy of the polymer chains on the substrate surface is 0.08 to 0.

65.

5. the member has a bottle brush structure in which the plurality of polymer chains are bonded as side chains to a polymer chain that is the base material, 3. The member according to claim 1, wherein the surface occupancy of the side chains is from 0.08 to 0.65.

Citation Information

Patent Citations

  • Preparation and application of super-smooth coating with long-acting ice dredging characteristic

    CN113528010A

  • Heat exchanger and refrigeration cycle device

    JP2022020472A

  • Snow slip film or sheet

    WO2019181216A1

  • Member for fogging prevention, suppression of water droplet adhesion, suppression of icing, or suppression of ice nucleus formation

    WO2021117537A1

  • Heat exchanger

    JP2019158247A

Cited By

  • Rotary transformer

    CN121748146A