Aqueous ink composition for writing boards

The aqueous ink composition with isobutylene/maleic anhydride copolymer and additives addresses the issue of line quality on glass surfaces in low-temperature, high-humidity environments, ensuring erasability and writing performance.

JP2024168921AInactive Publication Date: 2024-12-05MITSUBISHI PENCIL CO LTD

Patent Information

Application Number
JP2023085981
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-25
Publication Date
2024-12-05
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing water-based ink compositions for writing instruments fail to maintain good line quality and writing performance on non-absorbent surfaces like glass in low-temperature, high-humidity environments, leading to issues such as cracking, peeling, and smudging due to condensation.

Method used

An aqueous ink composition containing a neutralized isobutylene/maleic anhydride copolymer, water-soluble resin, trehalose, pentaerythritol, and sorbitol, with specific particle sizes and surface tensions, to enhance erasability and writing quality under low-temperature, high-humidity conditions.

Benefits of technology

The composition ensures sufficient erasability and excellent line drawing quality on non-absorbent surfaces, preventing cracking and peeling, even in challenging environmental conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024168921000001
    Figure 2024168921000001
  • Figure 2024168921000002
    Figure 2024168921000002
  • Figure 2024168921000003
    Figure 2024168921000003
Patent Text Reader

Abstract

To provide an aqueous ink composition for writing boards that ensures erasability even when applied to non-absorbent surfaces, while offering excellent quality of drawn lines and writing performance even when exposed to environments with low temperatures and high humidity levels.SOLUTION: An aqueous ink composition for writing boards contains at least a colorant, a neutralized product of an isobutylene-maleic anhydride copolymer, a water-soluble resin and / or resin emulsion, at least one selected from trehalose, pentaerythritol, and sorbitol, and water.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an aqueous ink composition for writing boards, which can be used on writing boards with non-absorbent surfaces such as glass surfaces, whiteboards, or blackboards, particularly glass surfaces, and which allows drawn lines to be easily erased by wiping with water, and which achieves both good line quality and writability even in low-temperature, high-humidity environments. [Background technology]

[0002] Conventional aqueous ink compositions for writing instruments and the like that have good erasability, water-resistant adhesion, etc. include, for example, [1] An ink composition for a marking pen containing water, a colorant, and a resin, characterized in that the resin is a water-soluble polyvinyl acetal resin (see, for example, Patent Document 1). [2] An aqueous pigment composition that aims to provide an aqueous pigment ink composition that, when used as a storefront sign or the like on a whiteboard or blackboard, the lines drawn on the non-absorbent surface can be easily erased by wiping with water despite having excellent water-resistant adhesion, and furthermore does not leave any residual image (see, for example, Patent Document 2). [3] A water-based marking pen ink composition for a writing board, which contains, as essential components in a solvent mainly composed of water, a pigment as a colorant, a resin, and a release agent, and the release agent is a phosphoric acid ester compound represented by the general formula 1 (see, for example, Patent Document 3). [4] A water-based ink composition for a writing board, comprising at least a pigment, a pigment dispersing resin, a masking agent, and modified polyvinyl alcohol or polyvinyl alcohol having a degree of saponification of 40 to 84% (see, for example, Patent Document 4). etc. are known.

[0003] However, the aqueous ink compositions for writing instruments described in the above Patent Documents 1 to 4 are suitable for use as window glass paint for decorating storefront window surfaces and the like with an aqueous marking pen, as has been in demand in recent years. Although the aqueous ink compositions have the ability to be erased by wiping with water, they are not yet excellent in line drawing quality and writability in low-temperature, high-humidity environments such as those caused by condensation in winter. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP-A-5-171092 (Claims, Examples, etc.) [Patent Document 2] JP 2015-48437 A (Claims, Examples, etc.) [Patent Document 3] JP 6-184486 A (claims, examples, etc.) [Patent Document 4] JP 2021-91815 A (Claims, Examples, etc.) Summary of the Invention [Problem to be solved by the invention]

[0005] In recent years, window glass painting, etc., is sometimes used to decorate window glass surfaces in storefronts with water-based marking pens, but while it is required that the drawn lines be easily erasable by wiping with water when they are dry, in winter, condensation on the window glass surface exposes the drawn lines to a low-temperature, high-humidity environment, which causes the drawn lines to crack and peel off on non-absorbent surfaces, especially on glass surfaces, making it difficult to maintain good line quality. Furthermore, when writing on a glass surface wet with condensation, there is a problem that the drawn lines tend to bleed and the ink hardens at the pen tip, making them more likely to be rubbed off, adversely affecting the writing properties. The present invention has been made in consideration of the above-mentioned development process of the conventional technology, the problems associated with it, the current situation, etc., and aims to solve these problems, and has an object to provide an aqueous ink composition for writing boards which has excellent erasability even when written on a non-absorbent surface, particularly a glass surface, and which also has good line drawing quality and writability even in a low-temperature, high-humidity environment. [Means for solving the problem]

[0006] In view of the above-mentioned problems in the prior art, the present inventors have conducted intensive research and have found that the above-mentioned aqueous ink composition for writing boards can be obtained by containing at least a colorant, a neutralized product of an isobutylene-maleic anhydride copolymer, a water-soluble resin and / or resin emulsion, at least one selected from trehalose, pentaerythritol, and sorbitol, and water, thereby completing the present invention.

[0007] That is, the aqueous ink composition for writing boards of the present invention is characterized by containing at least a colorant, a neutralized product of isobutylene-maleic anhydride copolymer, a water-soluble resin and / or resin emulsion, at least one selected from trehalose, pentaerythritol, and sorbitol, and water. The aqueous ink composition for a writing board preferably contains modified polyvinyl alcohol or polyvinyl alcohol having a degree of saponification of 40 to 84 mol %. The aqueous ink composition for a writing board preferably has a static surface tension measured at a temperature of 25° C. of 15 to 50 (mN / m). Effect of the Invention

[0008] According to the present invention, there is provided an aqueous ink composition for writing boards which has sufficient erasability of lines drawn on a non-absorbent surface, particularly a glass surface, and further has excellent line drawing quality and writability even in a low-temperature, high-humidity environment. The objects and advantages of the invention will be realized and obtained by means of the elements and combinations particularly pointed out in the claims. Both the foregoing general description and the following detailed description are exemplary and explanatory but are not restrictive of the invention as claimed. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] The following describes in detail the embodiments of the present invention. However, please note that the technical scope of the present invention is not limited to the embodiments described in detail below, but extends to the inventions described in the claims and their equivalents. The present invention can be implemented based on the contents disclosed in this specification and common technical knowledge in the relevant field (including design matters and obvious matters).

[0010] <Water-based ink composition for writing board> The aqueous ink composition for a writing board of the present invention is characterized by containing at least a colorant, a neutralized product of an isobutylene-maleic anhydride copolymer, a water-soluble resin and / or a resin emulsion, at least one selected from trehalose, pentaerythritol, and sorbitol, and water.

[0011] <Coloring material> The coloring materials used in the present invention include all dyes that dissolve or disperse in water, conventionally known inorganic and organic pigments such as titanium oxide, resin particle pigments containing pigments, pseudopigments in which resin emulsions are colored with dyes, white plastic pigments, hollow resin pigments (particles), pigments in which the surface is multi-layer-coated with iron oxide or titanium oxide or the like on a substrate of silica or mica, glittering pigments such as aluminum pigments, thermochromic pigments (particles), photochromic pigments (particles), and composite pigments (particles) thereof. Commercially available aluminum pigments that can be used include, for example, the WXM series in which the aluminum surface is rust-proofed with a phosphorus compound, the WL series in which the aluminum surface is rust-proofed with a molybdenum compound, the EMR series in which the surface of aluminum flakes is coated with high-density silica (all manufactured by Toyo Aluminum Co., Ltd.), SW-120PM (all manufactured by Asahi Kasei Chemicals Co., Ltd.), and the like, which can be used alone or in a mixture of two or more kinds. In the case where titanium oxide is added, it is desirable to use, for example, titanium oxide that has been treated with alumina or silica, or with zirconia or zinc, and it is preferable to use rutile or anatase type titanium oxide. Examples of dyes include acid dyes such as eosin, fuoxin, water yellow #6-C, acid red, water blue #105, brilliant blue FCF, and nigrosine NB; direct dyes such as direct black 154, direct sky blue 5B, and violet BB; and basic dyes such as rhodamine and methyl violet.

[0012] Examples of inorganic pigments include azo lakes, insoluble azo pigments, chelate azo pigments, phthalocyanine pigments, perylene and perinone pigments, and nitroso pigments. More specifically, inorganic pigments such as carbon black, titanium black, zinc oxide, red iron oxide, aluminum, chromium oxide, iron black, cobalt blue, iron oxide yellow, viridian, zinc sulfide, lithopone, cadmium yellow, vermilion, cadmium red, yellow lead, molybdate orange, zinc chromate, strontium chromate, white carbon, clay, talc, ultramarine blue, precipitated barium sulfate, baryte powder, calcium carbonate, lead white, navy blue, Prussian blue, manganese violet, aluminum powder, and brass powder; CI Pigment Blue 17, CI Pigment Blue 15, CI Pigment Blue 17, CI Pigment Blue 27, CI Pigment Red 5, CI Pigment Red 22, CI Pigment Red 38, CI Pigment Red 48, CI Pigment Red 49, CI Pigment Red 53, CI Pigment Red 57, C I Pigment Red 81, CI Pigment Red 104, CI Pigment Red 146, CI Pigment Red 245, CI Pigment Yellow 1, CI Pigment Yellow 3, CI Pigment Yellow 12, CI Pigment Yellow 13, CI Pigment Yellow 14, CI Pigment Yellow 17, CI Pigment Yellow 34, CI Pigment Yellow 55, CI Pigment Yellow 74, CI Pigment Yellow 95, CI Pigment Yellow 166, CI Pigment Yellow 167, CI Pigment Orange 5, CI Pigment Orange 13, CI Pigment Orange 16, CI Pigment Violet 1, CI Pigment Violet 3, CI Pigment Violet 19, CI Pigment Violet 23, CI Pigment Violet 50, CI Pigment Green 7, etc.

[0013] Examples of thermochromic pigments (particles) include thermochromic pigments produced by microencapsulating a thermochromic composition containing at least a leuco dye that functions as a color former, a color developer that is a component capable of causing the leuco dye to develop color, and a color change temperature regulator that can control the color change temperature in the color development of the leuco dye and the color developer, so as to have a predetermined average particle size (e.g., 0.1 to 10 μm). Examples of photochromic pigments (particles) include photochromic particles composed of at least one selected from photochromic dyes (compounds), fluorescent dyes, etc., and a resin such as a terpene phenol resin; and photochromic pigments (particles) produced by microencapsulating a photochromic composition containing at least one selected from photochromic dyes (compounds), fluorescent dyes, etc., an organic solvent, and additives such as an antioxidant, a light stabilizer, and a sensitizer, so as to have a predetermined average particle size (for example, 0.1 to 10 μm). In the present invention (including examples), the "average particle size" is a value measured by laser diffraction or dynamic light scattering, and in the case of laser diffraction, it is a value of D50 calculated on a volume basis. This measurement can be performed using, for example, a particle size distribution analyzer HRA9320-X100 manufactured by Nikkiso Co., Ltd., and the average particle size measured using dynamic light scattering is, for example, the average particle size value calculated using a concentrated particle size analyzer FPAR-1000 (manufactured by Otsuka Electronics Co., Ltd.) by cumulant method analysis in scattering intensity distribution.

[0014] These coloring materials can be used either alone or in combination of two or more (hereinafter simply referred to as "at least one"). Furthermore, with regard to these coloring materials, from the viewpoint of the erasability of drawn lines, it is desirable to use pigments, that is, colored resin pigments such as the above-mentioned inorganic pigments, organic pigments, resin particle pigments containing pigments, or pseudo-pigments obtained by coloring resin emulsions with dyes, white plastic pigments, hollow resin pigments (particles), pigments having a base material of silica or mica and a surface layer coated with a multilayer of iron oxide or titanium oxide, photochromic pigments such as aluminum pigments, thermochromic pigments (particles), photochromic pigments (particles), etc., and composite pigments (particles) of these.

[0015] The (total) content of these coloring materials is preferably 0.5 to 50 mass %, more preferably 2 to 40 mass %, and particularly preferably 5 to 30 mass %, based on the total amount of the aqueous ink composition for writing boards (hereinafter simply referred to as "total amount of ink composition"). By making the content of this coloring material 0.5% by mass or more, it is possible to improve the quality of the drawn lines, even in low-temperature and high-humidity environments, and to realize the formation of good drawn lines that do not crack or peel off, while by making the content 50% by mass or less, it is preferable in that the erasability is good, an increase in viscosity is suppressed, and the fluidity of the ink is good.

[0016] The neutralized product of isobutylene-maleic anhydride copolymer used in the present invention is a neutralized product of a copolymer of isobutylene and maleic anhydride, and in the present invention, when used in combination with a water-soluble resin (including a resin emulsion) described below, it becomes a component that exhibits the functions of improving the erasability of drawn lines and the quality of drawn lines and writability in low-temperature, high-humidity environments. In the neutralized product of isobutylene-maleic anhydride copolymer used, the basic structure of the isobutylene-maleic anhydride copolymer is represented by the following formula (I), and the following formula (II) is an ammonia-neutralized product (modified product) of isobutylene-maleic anhydride copolymer that can be preferably used in the present invention.

[0017] [ka]

[0018] [ka]

[0019] In the present invention, in addition to the ammonia-neutralized product of the above formula (II), sodium hydroxide-neutralized product and amine-neutralized product may be used. The values ​​of n in the above formula (I), l and m in (II), and j and k in the following formula (III) vary depending on the weight-average molecular weight described below, and the preferred ranges are determined. In the present invention, the copolymer may be a neutralized product obtained by imidizing (imide-modifying) an isobutylene-maleic anhydride copolymer represented by the following formula (III) and neutralizing the copolymer with ammonia, sodium hydroxide, an amine, or the like. [ka]

[0020] The weight-average molecular weight of each neutralized product of the isobutylene-maleic anhydride copolymer of the above formula (II), formula (III) or the like is preferably 3,000 to 400,000, more preferably 5,000 to 200,000, particularly preferably 30,000 to 100,000, and most preferably 50,000 to 70,000. This weight-average molecular weight is a value calculated in terms of polystyrene by aqueous gel permeation chromatography (GPC) analysis. The above isobutylene-maleic anhydride copolymer and its neutralized product can be a commercially available product, for example, "ISOBAM" manufactured by Kuraray Co., Ltd., and examples thereof include neutralized products of ISOBAM-04, 06, 10, and 18, and ISOBAM-104 and 110, which are commercially available products of ammonia neutralization (modification) of the isobutylene-maleic anhydride copolymer in the above formula (II), and further examples include neutralized products of ISOBAM-304, 306, and 310. When preparing a neutralized product of the isobutylene-maleic anhydride copolymer [from the above formula (I) etc.] to be used, for example, when all the carboxyl groups of the isobutylene-maleic anhydride copolymer are neutralized, the degree of neutralization is set to 1, and each neutralized product can be obtained by calculating and preparing the necessary amounts of ammonia, sodium hydroxide, amine, etc. to be used for neutralization.

[0021] The content of the neutralized product of the isobutylene-maleic anhydride copolymer is preferably 0.01 to 4 mass %, more preferably 0.05 to 3 mass %, and particularly preferably 0.1 to 2 mass %, based on the total amount of the ink composition. If the content of the neutralized product of this isobutylene-maleic anhydride copolymer is less than 0.01% by mass, the quality of the drawn lines will decrease in low-temperature, high-humidity environments, and the drawn lines will be prone to cracking and peeling. On the other hand, if the content exceeds 4% by mass, the viscosity will increase, causing a decrease in ink discharge properties, which will have an adverse effect on writing properties and lead to a decrease in erasability.

[0022] The water-soluble resin and resin emulsion used in the present invention function as a fixing agent, dispersant and stabilizer, and examples thereof include at least one type selected from water-soluble resins having a hydrophobic portion in the molecule, such as polyacrylic acid, acrylic resins, water-soluble styrene-acrylic resins, water-soluble styrene-maleic acid resins, polyvinyl alcohol, polyvinylpyrrolidone, water-soluble maleic acid resins, water-soluble styrene resins, water-soluble ester-acrylic resins, ethylene-maleic acid copolymers, polyethylene oxide and water-soluble urethane resins, and resin emulsions, such as acrylic emulsions, vinyl acetate emulsions, polyolefin emulsions, urethane emulsions, vinyl chloride emulsions, styrene-butadiene emulsions, styrene-acrylonitrile emulsions, silicone resin emulsions and silicone-acrylic copolymer emulsions.

[0023] Preferably, from the viewpoints of dispersibility of coloring materials, viscosity adjustment, and fixing power improvement, it is desirable to use water-soluble resins such as acrylic resins, water-soluble styrene-acrylic resins, styrene-maleic acid, and urethane resins, or acrylic resin emulsions, styrene-acrylic, styrene-maleic acid, and urethane resin emulsions, each of which has an acid value of 240 or less. The lower limit of the acid value is desirably 10 or more from the viewpoint of storage stability of the ink. By adjusting the acid value of the resin to 240 or less, it is possible to form a uniform coating film with good erasability, and further to maintain good line quality even in a low-temperature, high-humidity environment.

[0024] The mass average molecular weight of the resin having an acid value of 240 or less is preferably 2,000 or more, more preferably 3,000 to 300,000, and particularly preferably 5,000 to 200,000. By using a resin having a mass average molecular weight of 2,000 or more, a strong line drawing coating film can be formed, and good line drawing quality can be achieved without cracking or peeling even in a low-temperature, high-humidity environment. In the present invention, the "acid value of a resin" refers to the number of milligrams of KOH required to neutralize 1 g of resin, and is a value measured, for example, in accordance with JIS-K3054.

[0025] The water-soluble resins and resin emulsions having an acid value of 240 or less can be commercially available. For example, water-soluble resins such as BASF's PDX6157 (acid value: 205), JDX6500 (acid value: 85), and PDX-6137A (acid value: 240), and Seiko PMC's M-30 (acid value: 155) can be used. Resin emulsions such as BASF's PDX-7741 (acid value: 52), PDX-7787 (acid value: 100), and PDX-7158 (acid value: 54), Taisei Fine Chemical's WBR-016 (acid value: 7), and Mitsui Chemicals MC's Takelac W-5661 (acid value: 48) can be used.

[0026] The content of the water-soluble resin and resin emulsion having these characteristics (total: solid content) is preferably 0.1 to 20 mass % and more preferably 0.5 to 15 mass % based on the total amount of the ink composition, separate from the neutralized product of the isobutylene-maleic anhydride copolymer. If the content of water-soluble resin or resin emulsion having these characteristics is less than 0.1% by mass, the quality of the drawn lines will decrease in a low-temperature, high-humidity environment, which is not preferred. On the other hand, if the content exceeds 20% by mass, the viscosity will increase, which will have a negative effect on the ink ejection properties, which is also not preferred.

[0027] Pentaerythritol [C(CH2OH)4] used in the present invention is used as an inhibitor for preventing lines drawn on non-absorbent surfaces, particularly glass surfaces, from cracking or peeling due to condensation, etc., and when added to an aqueous ink composition for writing boards, it does not cause a decrease in ink performance, etc. The content of this pentaerythritol is desirably 0.1 to 5%, preferably 0.5 to 4%, of the total amount of the ink composition for writing boards. If the content is less than 0.1%, the effect of inhibiting cracking and peeling of drawn lines in low-temperature, high-humidity environments will be low, which is undesirable. On the other hand, if the content exceeds 5%, the viscosity of the aqueous ink composition for writing boards will increase and crystals will precipitate from the pen tip or the surface of the drawn lines at low temperatures, etc., which will result in a decrease in the quality of the drawn lines and problems with the storage stability of the ink, which is undesirable.

[0028] The trehalose used in the present invention is used as an agent for suppressing cracking and peeling of drawn lines due to condensation, etc., and does not cause a decrease in ink performance, etc., even when it is added to the writing board aqueous ink composition. The content of trehalose is desirably 0.1 to 15%, and preferably 0.5 to 8%, based on the total amount of the ink composition. If this content is less than 0.1%, the effect of inhibiting cracking and peeling of drawn lines will be low, which is undesirable. On the other hand, if it exceeds 15%, the viscosity of the aqueous ink composition for writing boards will increase, and crystals will precipitate from the pen tip or the surface of the drawn lines at low temperatures, etc., which will result in a decrease in the quality of the drawn lines and problems with the storage stability of the ink, which are also undesirable.

[0029] The sorbitol used in the present invention is used as an agent for suppressing cracking and peeling of drawn lines caused by condensation, etc., and does not cause a decrease in ink performance, etc., when it is added to the writing board aqueous ink composition. The content of sorbitol is desirably 0.1 to 15%, and preferably 0.5 to 8%, based on the total amount of the ink composition.

[0030] The pentaerythritol, trehalose, and sorbitol used in the present invention may be used alone or in combination of two or more types (hereinafter simply referred to as "at least one type") in the aqueous ink composition for writing boards, within the scope of the effects of the present invention.

[0031] The modified polyvinyl alcohol used in the present invention, that is, polyvinyl alcohol having a degree of saponification of 40 to 84 mol %, is a component that exerts the effects of the present invention; it does not affect the erasability of drawn lines, and even under low temperature and high humidity conditions, it forms a strong coating film for drawn lines, maintains good line quality without cracking or peeling of drawn lines, and further provides good writing properties without bleeding of drawn lines or rubbing due to hardening of the ink at the pen tip, even on surfaces wet with water such as condensation.

[0032] The polyvinyl alcohol (hereinafter simply referred to as "PVA") used in the aqueous ink composition for writing boards of the present invention is represented by the general formula -[CH2-CH(OH)]m-[CH2-CH(OCOCH3)n-, and in the present invention, the degree of saponification {[m / (m+n)]×100} used is 40 to 84 mol%, preferably 60 to 80 mol%, and particularly preferably 70 to 80 mol%. Regarding the saponification degree of the PVA, if the PVA has a saponification degree of less than 40 mol%, the ink becomes unstable and has a negative effect on the writing properties, while if the PVA has a saponification degree of more than 84 mol%, the effect of improving the erasability becomes insufficient, which is undesirable.

[0033] Specifically, PVA that can be used is selected from commercially available A-type Gohsenol series, G-type Gohsenol series, K-type Gohsenol series (trade name of Nippon Synthetic Chemical Industry Co., Ltd.), J-poval series (trade name of Nippon Synthetic Chemical Industry Co., Ltd.) manufactured by Nippon Vacuum Acetate & Poval Co., Ltd., KURARAY poval PVA series (trade name of Kuraray Co., Ltd.), etc. PVA having these saponification degrees may be used alone or in combination of two or more kinds.

[0034] In addition to the PVA having the above-mentioned properties, modified PVA can be used alone or in combination with the PVA having the above-mentioned properties in the present invention. The modified PVA that can be used includes PVA in which the hydroxyl group or acetate group has been modified with a modifying group such as a carboxyl group, a sulfonic acid group, an acetyl group, or an ethylene oxide group, or PVA having the above modifying groups on its side chain. In addition, a PVA-acrylic acid-methyl methacrylate copolymer in which acrylic acid and methyl methacrylate are copolymerized with partially saponified PVA can also be used as the modified PVA of the present invention.

[0035] Preferably, in order to further exert the effects of the present invention, it is desirable to use a modified PVA having the above-mentioned degree of saponification (40 to 84 mol%). Specifically, modified PVA that can be used is selected from among commercially available Gohsenx L series and Gohsenx WO series (trade name of Nippon Synthetic Chemical Industry Co., Ltd.) manufactured by Mitsubishi Chemical Corporation, anion-modified PVA (A series) (trade name of Nippon Vinyl Acetate & Poval Co., Ltd.) manufactured by Nippon Vinyl Acetate & Poval Co., Ltd., and Exeval 1713 (trade name of Kuraray Co., Ltd.) manufactured by Kuraray Co., Ltd., etc. As the PVA-acrylic acid-methyl methacrylate copolymer, a suitable one is selected from among POVACOAT (trade name of Daido Chemical Industry Co., Ltd.) manufactured by Daido Chemical Industry Co., Ltd., etc. These modified PVAs may be used alone or in combination of two or more. The modified PVA used is effective for writing on glass surfaces that have condensed in low-temperature, high-humidity environments without bleeding or rubbing of the pen tip. In particular, carboxyl-, sulfonic-, and acetyl-modified types are preferable because they have excellent stability.

[0036] The total content of such PVA and modified PVA is preferably 0.05 to 5%, and more preferably 0.1 to 3%, based on the total amount of the ink composition. If the content of these is less than 0.05%, the effects of the present invention cannot be achieved, and writing on non-absorbent surfaces such as glass surfaces becomes insufficient and the drawn lines tend to bleed. On the other hand, if the content exceeds 5%, the stability of the ink becomes unstable, which is not preferable.

[0037] The aqueous ink composition for writing boards of the present invention is more preferable in that if the measured static surface tension at 25° C. is 15 to 50 (mN / m), uniform lines can be easily drawn on a glass surface, and therefore cracks or peeling of the drawn lines are unlikely to occur even in a low-temperature, high-humidity environment, resulting in good writing properties. The static surface tension (25° C.) of the ink composition for writing boards of the present invention is a value measured using a surface tension measuring device: CBVP-Z manufactured by Kyowa Interface Science Co., Ltd.

[0038] Furthermore, the aqueous ink composition for writing boards of the present invention preferably contains hollow particles, provided that the effect of the present invention is not impaired. For example, commercially available products include Ropeake OP-62 (average particle size 450 nm, hollow ratio 33%), Ropeake OP-91, Ropeake HP-1055 (average particle size 1000 nm, hollow ratio 55%), Ropeake HP-91 (average particle size 1000 nm, hollow ratio 50%), Ropeake ULTRA (average particle size 380 nm, hollow ratio 45%), Ropeake ULTRA E (average particle size 380 nm, hollow ratio 45%), Ropeake ULTRA At least one of the following may be used: DUAL (average particle size 380 nm, hollow ratio 45%) (all manufactured by BASF), SX-863(A), SX-864(B), SX-866(A), SX-866(B) (average particle size 300 nm, hollow ratio 30%), SX-868 (average particle size 500 nm) (all manufactured by JSR), Nipol MH5055 (average particle size 500 nm), Nipol MH8101 (average particle size 1 μm) (all manufactured by Zeon Corporation). The content of these hollow particles is preferably 0.1 to 10% in terms of solids concentration, and more preferably 0.5 to 8%, of the total amount of the aqueous ink composition for writing boards. This is preferred in that it allows the formation of a flexible line coating film, resulting in better erasability.

[0039] The aqueous ink composition for writing boards of the present invention contains at least the neutralized product of the above-mentioned colorant and isobutylene-maleic anhydride copolymer, a water-soluble resin and / or resin emulsion, and at least one selected from trehalose, pentaerythritol, and sorbitol, as well as water (tap water, purified water, distilled water, ion-exchanged water, pure water, etc.) as the solvent as the remainder, and may also contain dispersants, lubricants, pH adjusters, rust inhibitors, preservatives or antibacterial agents, thickeners, etc., as appropriate, within the scope of the invention not impairing its effects.

[0040] Usable dispersants include nonionic and anionic surfactants and water-soluble resins other than the water-soluble resins mentioned above, and preferably water-soluble polymers. Examples of lubricants include nonionic lubricants such as fatty acid esters of polyhydric alcohols, higher fatty acid esters of sugars, polyoxyalkylene higher fatty acid esters, and alkyl phosphate esters, which are also used as surface treatment agents for pigments, anionic lubricants such as alkyl sulfonates and alkyl aryl sulfonates of higher fatty acid amides, derivatives of polyalkylene glycols, fluorine-based surfactants, acetylene-based activators, and polyether-modified silicones. Among these, from the viewpoint of writing properties and fixation of the drawn line coating film, it is preferable to use acetylene-based activators, and examples of commercially available products include the Surfynol series, such as Surfynol 104H (manufactured by Nissin Chemical Industry Co., Ltd.), and it is more preferable to contain 0.01 to 2% by mass of the aqueous ink composition for writing boards of the present invention based on the total amount of the composition.

[0041] Examples of pH adjusters include ammonia, urea, monoethanolamine, diethanolamine, triethanolamine, alkali metal salts of carbonates and phosphoric acids such as sodium tripolyphosphate and sodium carbonate, and hydrates of alkali metals such as sodium hydroxide. Examples of rust inhibitors include benzotriazole, tolyltriazole, dicyclohexylammonium nitrite, and saponins, while examples of preservatives or antibacterial agents include phenol, sodium omadine, sodium benzoate, and benzimidazole-based compounds. Examples of the thickener that can be used include cellulose derivatives, such as hydroxyalkyl celluloses such as hydroxyethyl cellulose, carboxymethyl cellulose (CMC) or a salt thereof, fermented cellulose, crystalline cellulose, polysaccharides, etc. Examples of polysaccharides that can be used include xanthan gum, guar gum, hydroxypropylated guar gum, casein, gum arabic, gelatin, amylose, agarose, agaropectin, arabinan, curdlan, callose, carboxymethyl starch, chitin, chitosan, quince seed, glucomannan, gellan gum, tamarind seed gum, dextran, nigeran, hyaluronic acid, pustulan, funoran, HM pectin, porphyran, laminaran, lichenan, carrageenan, alginic acid, tragacanth gum, alkaloid gum, succinoglycan, locust bean gum, tara gum, etc. Examples of synthetic polymers include polyacrylic acids, polyvinyl alcohol, polyethylene oxide, polyvinylpyrrolidone, polyvinyl methyl ether, bisacrylamide methyl ether, polyacrylamide, polyethyleneimine, polyethylene glycol, polydioxolane, polystyrene sulfonic acid, and polypropylene oxide. These may be used alone or in combination of two or more. If commercially available products of these are available, they may be used.

[0042] The aqueous ink composition for writing boards of the present invention is prepared by appropriately combining at least the above-mentioned colorant, a neutralized product of an isobutylene-maleic anhydride copolymer, a water-soluble resin and / or resin emulsion, at least one selected from trehalose, pentaerythritol and sorbitol, water and other components depending on the application of the ink for writing boards (for ballpoint pens, marking pens, etc.), stirring and mixing them with a stirrer such as a homomixer, homogenizer or disper, and further, if necessary, removing coarse particles from the ink composition by filtration or centrifugation, thereby obtaining an aqueous ink composition for writing boards with excellent color development. The pH (25°C) of the aqueous ink composition for writing boards of the present invention is preferably adjusted to 5 to 10 using a pH adjuster or the like from the viewpoints of usability, safety, the stability of the ink itself, and compatibility with the ink container, and is more preferably adjusted to 6 to 9.5.

[0043] The aqueous ink composition for writing boards of the present invention thus constituted contains at least the above-mentioned colorant, a neutralized product of isobutylene-maleic anhydride copolymer, a water-soluble resin and / or resin emulsion, at least one selected from trehalose, pentaerythritol and sorbitol, and water, and provides excellent erasability of drawn lines and good line drawing quality in low-temperature, high-humidity environments. Furthermore, by containing modified polyvinyl alcohol or polyvinyl alcohol with a degree of saponification of 40 to 84 mol%, it is possible to achieve both erasability and good line drawing quality in low-temperature, high-humidity environments, and good writability without bleeding or rubbing of drawn lines when writing on a glass surface that is wet with water due to condensation.

[0044] <Writing instruments> The writing instrument of the present invention is equipped with an aqueous ink composition for writing boards having the above-mentioned characteristics, and even when writing on a non-absorbent surface, particularly a glass surface, a writing instrument having excellent abrasion resistance, color development, erasability, etc. is obtained. As a writing instrument, for example, it is mounted on a ballpoint pen, a marking pen, etc., having a pen tip portion such as a ballpoint tip, a fiber tip, a felt tip, a plastic tip, a fiber core, or a porous core.

[0045] In the present invention, a "marking pen" refers to a pen having a mechanism for supplying ink stored in an ink reservoir to a resin writing part by capillary action, and includes pens referred to as "felt-tip pens." Additionally, a "ballpoint pen" refers to a pen having a mechanism for exuding ink stored in an ink reservoir by the rotation of a ball provided in the writing part. For a ballpoint pen, the aqueous ink composition for writing boards having the above composition is contained in a ballpoint pen ink container (refill) equipped with a ball having a diameter of 0.18 to 2.0 mm, and an ink follower is added. The ink follower is a liquid that is incompatible with the aqueous ink composition for writing boards having the above characteristics contained in the ink container and has a smaller specific gravity than the aqueous ink composition, such as polybutene, silicone oil, mineral oil, etc. The structure of the ballpoint pen, marking pen, etc. is not particularly limited, and may be, for example, a direct ink type ballpoint pen or marking pen having a collector structure (ink retention mechanism) in which the barrel itself serves as an ink container and is filled with the aqueous ink composition for writing boards having the above-mentioned configuration. In the aqueous ink composition for writing boards of the present invention, a direct ink marking pen having a fiber core is preferred, and a writing flow rate on the surface of a glass plate (15 cm long × 30 cm wide × 1 cm thick, ordinary plate glass) of 20 to 400 mg / m (straight line writing) is preferred, as this allows easy erasure and provides both good line drawing quality and writability even in a low-temperature, high-humidity environment. EXAMPLES

[0046] Next, the present invention will be described in more detail with reference to examples and comparative examples, but the present invention is not limited to the following examples.

[0047] [Examples 1 to 8 and Comparative Examples 1 to 5] Each aqueous ink composition for writing boards was prepared by a conventional method according to the formulation shown in Table 1. The pH of each aqueous ink composition for writing boards at room temperature (25°C) was measured with a pH meter (HORIBA Corporation) and was within the range of 7.9 to 8.2. For each of the aqueous ink compositions for writing boards obtained above, writing implements (marking pens) were prepared by the following method, and the scratch resistance, color development, and erasability of drawn lines were evaluated by the following evaluation methods. The glass plate used for the tests was an ordinary glass plate measuring 15 cm long x 30 cm wide x 1 cm thick. The results are shown in Table 1 below.

[0048] (Making a marking pen) A marking pen was prepared using each of the ink compositions obtained above. Specifically, a marking pen (manufactured by Mitsubishi Pencil Co., Ltd., product name: PXW-200-5M, shaft material: recycled PP resin, pen core: PET fiber) was used, and the ink composition for writing board was loaded to prepare each direct ink marking pen. It was confirmed that each marking pen had a writing flow rate on a glass plate (length 15 cm x width 30 cm x thickness 1 cm, ordinary plate glass) in the range of 20 to 400 mg / m. Using the marking pens of Examples 1 to 8 and Comparative Examples 1 to 5 obtained as described above, evaluations were carried out.

[0049] (Method of evaluating erasability) Each pen was used to draw three spiral lines of a circle approximately 2 cm in diameter on a glass plate. The resulting lines were allowed to dry for one hour, then erased with a tissue moistened with water and evaluated according to the following criteria. Evaluation criteria: ○: The drawn lines are erased cleanly. △: Compared to the above ○, there are some areas where the drawn lines remain slightly. ✕: Compared to the above ○, most of the lines remain.

[0050] (Evaluation method for line quality) Each pen was used to draw five spirals, each approximately 30 mm in diameter, on a glass plate in an environment at 25°C. The drawn lines were then allowed to dry thoroughly and stored in a test environment at a temperature of 5°C and a relative humidity of 85% for 24 hours, after which the condition of the drawn lines was visually observed. The evaluation was based on the following criteria. Evaluation criteria: ◯: There were no cracks or peeling in the drawn lines and the result was good. △: Some cracking or peeling of the lines is observed. ✕: Significant cracks and peeling of lines are observed.

[0051] (Writability evaluation method) Each pen was placed in a test environment of 5°C and 85% relative humidity, and after confirming that water droplets (condensation) had formed on the surface of a glass plate and that it was wet, five spirals with a diameter of approximately 30 mm were drawn on the glass plate. The state of the drawn lines was then visually observed and evaluated according to the following criteria. Evaluation criteria: ◯: The drawn lines were good with no bleeding or rubbing observed. △: Slight bleeding or rubbing was observed in the lines. X: There was noticeable bleeding or rubbing in the lines.

[0052] [Table 1]

[0053] As is clear from the results in Table 1 above, the aqueous ink compositions for writing boards of Examples 1 to 8 of the present invention are erasable and have good line drawing quality and excellent writability, even when exposed to low temperature and high humidity conditions, compared to the aqueous ink compositions for writing boards of Comparative Examples 1 to 5, which are outside the scope of the present invention. [Industrial Applicability]

[0054] The ink can be suitably used in aqueous ink compositions for writing boards such as ballpoint pens and marking pens.

Claims

1. An aqueous ink composition for a writing board, comprising at least a colorant, a neutralized product of an isobutylene-maleic anhydride copolymer, a water-soluble resin and / or a resin emulsion, at least one selected from trehalose, pentaerythritol, and sorbitol, and water.

2. 2. The aqueous ink composition for a writing board according to claim 1, which contains modified polyvinyl alcohol or polyvinyl alcohol having a degree of saponification of 40 to 84 mol %.

3. 3. The aqueous ink composition for a writing board according to claim 1, wherein the static surface tension measured at a temperature of 25° C. is 15 to 50 (mN / m).

Citation Information

Patent Citations

  • Ink composition for marking pen

    JP1993171092A

  • Aqueous marking pen ink composition for writing board

    JP1994184486A

  • Watercolor pigment ink composition

    JP2015048437A

  • Marking ink composition for writing board

    JP2021091815A

Cited By

  • Method for producing water-absorbent resin particles and water-absorbent resin particles

    US12359028B2