Optical film

A resin composition with specific polycarbonate and acrylic structures addresses incompatibility issues, enhancing heat resistance and transparency in optical films, suitable for polarizing plates and display protection.

JP2024169074APending Publication Date: 2024-12-05MITSUBISHI CHEM CORP
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
JP2023086263
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-25
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

Existing resin compositions using ISB polycarbonate and acrylic resins for polarizing plates suffer from incompatibility, leading to significant haze and insufficient heat resistance when deformed, which affects transparency and durability in optical applications.

Method used

A resin composition comprising a polycarbonate resin with a specific structure and an acrylic resin with a specific structure, where the polycarbonate resin contains 65% to 90% of a structural unit derived from isosorbide and the acrylic resin contains 50% to 100% of a (meth)acrylate structural unit, with specific molecular weights and glass transition temperatures, ensuring compatibility and improved heat resistance.

Benefits of technology

The optical film exhibits excellent heat resistance, transparency, and mechanical properties, making it suitable for polarizing plate protective films and display front protective films.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024169074000001
    Figure 2024169074000001
  • Figure 2024169074000002
    Figure 2024169074000002
  • Figure 2024169074000003
    Figure 2024169074000003
Patent Text Reader

Abstract

To provide an optical film composed of a resin composition containing an ISB-based polycarbonate resin and an acrylic resin, which has low birefringence and good heat resistance and transparency.SOLUTION: An optical film uses a resin composition containing a polycarbonate resin containing 65 wt.% or more and 90 wt.% or less of a structural unit (1), and an acrylic resin containing 50 wt.% or more and 100 wt.% or less of a structural unit (2).SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an optical film and a polarizing plate using the optical film. [Background technology]

[0002] Due to concerns about global warming due to the depletion of petroleum resources and the increase in carbon dioxide emissions, there is a demand for the development of plastics made from plant-derived monomers. In response, polycarbonate resins using the plant-derived raw material isosorbide (hereinafter sometimes referred to as "ISB") have been developed and are beginning to be used in automotive interior and exterior components, as a glass replacement, and for optical applications (see, for example, Patent Documents 1 and 2).

[0003] Polarizing plates are used in liquid crystal displays and organic EL displays, and generally, polarizing plates are used in which a polarizer protective film is attached to a linear polarizer made of a polyvinyl alcohol-based film containing iodine via an adhesive or pressure-sensitive adhesive. The resin used in this polarizer protective film is required to have a small phase difference and high heat resistance, and resins such as acetyl cellulose, acrylic, and cycloolefin are used. Patent documents 3 and 4 propose a resin composition with low birefringence by mixing an ISB-based polycarbonate resin and an acrylic resin. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] International Publication No. 2004 / 111106 [Patent Document 2] International Publication No. 2007 / 148604 [Patent Document 3] JP 2018-131587 A [Patent Document 4] Patent Publication No. 2021-88651 Summary of the Invention [Problem to be solved by the invention]

[0005] In Patent Documents 3 and 4, a highly transparent resin composition is obtained by matching the refractive index of an ISB-based polycarbonate resin with an acrylic resin. According to the study by the present inventors, it was found that the acrylic resins in Patent Documents 3 and 4 are incompatible with an ISB-based polycarbonate resin, and that when a film made by molding an incompatible alloy is subjected to a large deformation such as stretching or bending, a large haze occurs in the film, and transparency is impaired. This is a serious drawback for use in optical applications. In addition, the materials reported in Patent Documents 3 and 4 also have insufficient heat resistance.

[0006] In view of the above circumstances, an object of the present invention is to provide an optical film made of a resin composition containing an ISB-based polycarbonate resin and an acrylic resin, which has low birefringence as well as good heat resistance and transparency. [Means for solving the problem]

[0007] As a result of intensive research aimed at solving the above problems, the present inventors have found that a film made of a resin composition containing a polycarbonate resin having a specific structure and an acrylic resin having a specific structure satisfies both the properties of heat resistance and low birefringence.

[0008] [1] A polycarbonate resin containing 65% by weight or more and 90% by weight or less of a structural unit represented by the following formula (1): and an acrylic resin containing 50% by weight or more and 100% by weight or less of a (meth)acrylate structural unit represented by the following formula (2):

[0009] [ka]

[0010] [ka]

[0011] (In formula (2), R 1 R is a hydrogen atom or an alkyl group having 1 to 10 carbon atoms which may have a substituent. 2 represents an alkyl group or a cycloalkyl group that contains a cyclohexane structure and may further have a substituent.

[0012] [2] The optical film according to [1], wherein the polycarbonate resin has a glass transition temperature of 130° C. or higher and 160° C. or lower.

[0013] [3] The optical film according to [1] or [2], wherein the polycarbonate resin contains a structural unit derived from an aliphatic dihydroxy compound or an alicyclic dihydroxy compound.

[0014] [4] The optical film according to any one of [1] to [3], wherein the acrylic resin has a weight average molecular weight (Mw) of 10,000 or more and 500,000 or less.

[0015] [5] The optical film according to any one of [1] to [4], wherein the acrylic resin contains 0.1 wt % or more and 10 wt % or less of an acrylate structural unit represented by the following formula (3):

[0016] [ka]

[0017] (In formula (3), R 3 is a hydrogen atom, an alkyl group having 1 to 10 carbon atoms which may have a substituent, a cycloalkyl group, or an aryl group.

[0018] [6] The optical film according to any one of [1] to [5], comprising 50% by weight or more and 99% by weight or less of the polycarbonate resin and 1% by weight or more and 50% by weight or less of the acrylic resin.

[0019] [7] A polarizing plate comprising the optical film according to any one of [1] to [6] and a linear polarizer, which are laminated together. Effect of the Invention

[0020] The optical film of the present invention, which is made using a specified resin composition, has excellent heat resistance and optical properties, and also has excellent mechanical properties such as stretchability, and can therefore be suitably used for applications such as polarizing plate protective films and display front protective films. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0021] The present invention will be described in detail below, but the present invention is not limited to the following description, and can be modified in any manner without departing from the gist of the present invention.

[0022] In this specification, when "~" is used with a numerical value or a physical property value enclosed therein, the values ​​before and after the "~" are included in the expression.

[0023] In this specification, the term "repeated structural unit" refers to a structural unit in which the same structure appears repeatedly in a resin, and each of the structural units is linked to form the resin. For example, in the case of a polycarbonate resin, the carbonyl group is also referred to as the repeating structural unit. In addition, the term "structural unit" refers to a partial structure that constitutes a resin, and a specific partial structure contained in the repeating structural unit. For example, it refers to a partial structure sandwiched between adjacent linking groups in a resin, or a partial structure sandwiched between a polymerizable reactive group present at the end of a polymer and a linking group adjacent to the polymerizable reactive group. More specifically, in the case of a polycarbonate resin, a carbonyl group is a linking group, and a partial structure sandwiched between adjacent carbonyl groups is referred to as a structural unit.

[0024] [Optical film] The optical film of the present invention is a film made using a resin composition containing a polycarbonate resin containing 65% by weight or more and 90% by weight or less of a structural unit represented by the following formula (1) and an acrylic resin containing 50% by weight or more and 100% by weight or less of a (meth)acrylate structural unit represented by the following formula (2). That is, as described below, it is a film made by molding the resin composition. Hereinafter, the structural unit represented by formula (1) may be referred to as "structural unit (1)", and the (meth)acrylate structural unit represented by formula (2) may be referred to as "structural unit (2)". The weight ratios of the various structural units may be, for example, 1 By analyzing H-NMR, the area ratio of the peaks originating from each structural unit and the molecular weight of each structural unit can be calculated.

[0025] [ka]

[0026] [ka] (In formula (2), R 1 R is a hydrogen atom or an alkyl group having 1 to 10 carbon atoms which may have a substituent. 2 represents an alkyl group or a cycloalkyl group that contains a cyclohexane structure and may further have a substituent.

[0027] <Polycarbonate resin> The resin composition constituting the optical film of the present invention contains a polycarbonate resin containing 65% by weight or more and 90% by weight or less of the structural unit represented by the formula (1). Hereinafter, this polycarbonate resin may be referred to as the "polycarbonate resin in the present invention."

[0028] (Dihydroxy Compounds) Dihydroxy compounds forming the structural unit (1) include isosorbide (ISB), isomannide, and isoidet, which are stereoisomers. These may be used alone or in combination of two or more. Among them, isosorbide obtained by dehydration condensation of sorbitol produced from various starches, which are abundant and easily available as a plant-derived resource, is most preferred in terms of availability, ease of production, and properties of the resulting molded product (for example, heat resistance, impact resistance, surface hardness, carbon neutrality).

[0029] The lower limit of the content of the structural unit (1) in the polycarbonate resin is more preferably 68% by weight or more, and even more preferably 70% by weight or more. The upper limit is more preferably 85% by weight or less, and even more preferably 80% by weight or less. Since the structural unit (2) in the acrylic resin in the present invention described later has high compatibility with the structural unit (1), within the above range, a resin composition with high transparency can be obtained. In addition, the structural unit (1) is also a structure with a high glass transition temperature, and a resin with high heat resistance can be obtained. In this specification, the content of the structural unit (1) in the polycarbonate resin means the content (weight %) of the structural unit (1) when the total weight of all the structural units and linking groups constituting the polycarbonate resin is 100% by weight. The contents of other structural units in the polycarbonate resin are defined in the same manner.

[0030] The polycarbonate resin in the present invention may contain structural units other than the structural unit (1). Hereinafter, structural units other than the structural unit (1) may be referred to as "other structural units". Examples of compounds forming other structural units include aliphatic dihydroxy compounds, alicyclic dihydroxy compounds, ether-containing dihydroxy compounds, acetal-containing dihydroxy compounds, aromatic-containing dihydroxy compounds, and diester compounds. A polycarbonate resin partially incorporating a structural unit derived from a diester compound is referred to as a polyester carbonate resin. In this specification, the term "polycarbonate resin" includes polyester carbonate resins.

[0031] Examples of the aliphatic dihydroxy compound include the following dihydroxy compounds: straight-chain aliphatic dihydroxy compounds such as ethylene glycol, 1,3-propanediol, 1,2-propanediol, 1,4-butanediol, 1,5-heptanediol, 1,6-hexanediol, 1,9-nonanediol, 1,10-decanediol, and 1,12-dodecanediol; and branched-chain aliphatic dihydroxy compounds such as 1,3-butanediol, 1,2-butanediol, neopentyl glycol, and hexylene glycol.

[0032] Examples of the alicyclic dihydroxy compound include the following dihydroxy compounds: dihydroxy compounds which are primary alcohols of alicyclic hydrocarbons, such as 1,2-cyclohexanedimethanol, 1,3-cyclohexanedimethanol, 1,4-cyclohexanedimethanol, tricyclodecane dimethanol, pentacyclopentadecane dimethanol, 2,6-decalin dimethanol, 1,5-decalin dimethanol, 2,3-decalin dimethanol, 2,3-norbornane dimethanol, 2,5-norbornane dimethanol, 1,3-adamantanedimethanol, and dihydroxy compounds derived from terpene compounds such as limonene; dihydroxy compounds which are secondary or tertiary alcohols of alicyclic hydrocarbons, such as 1,2-cyclohexanediol, 1,4-cyclohexanediol, 1,3-adamantanediol, hydrogenated bisphenol A, and 2,2,4,4-tetramethyl-1,3-cyclobutanediol.

[0033] Examples of the ether-containing dihydroxy compound include oxyalkylene glycols and dihydroxy compounds containing an acetal ring. Examples of the oxyalkylene glycol that can be used include diethylene glycol, triethylene glycol, tetraethylene glycol, polyethylene glycol, polypropylene glycol, and polytetramethylene glycol.

[0034] Examples of acetal-containing dihydroxy compounds that can be used include spiroglycol (also known as 3,9-bis(1,1-dimethyl-2-hydroxyethyl-2,4,8,10-tetraoxaspiro[5,5]undecane) and dioxane glycol (also known as 2-(1,1-dimethyl-2-hydroxyethyl)-5-ethyl-5-hydroxymethyl-1,3-dioxane).

[0035] As the aromatic dihydroxy compound, for example, the following dihydroxy compounds can be used: 2,2-bis(4-hydroxyphenyl)propane, 2,2-bis(3-methyl-4-hydroxyphenyl)propane, 2,2-bis(4-hydroxy-3,5-dimethylphenyl)propane, 2,2-bis(4-hydroxy-3,5-diethylphenyl)propane, 2,2-bis(4-hydroxy-(3-phenyl)phenyl)propane, 2,2-bis(4-hydroxy-(3,5-diphenyl)phenyl)propane, 2,2-bis(4-hydroxy-3,5-dibromophenyl)propane, bis(4-hydroxyphenyl)propane, )methane, 1,1-bis(4-hydroxyphenyl)ethane, 2,2-bis(4-hydroxyphenyl)butane, 2,2-bis(4-hydroxyphenyl)pentane, 1,1-bis(4-hydroxyphenyl)-1-phenylethane, bis(4-hydroxyphenyl)diphenylmethane, 1,1-bis(4-hydroxyphenyl)-2-ethylhexane, 1,1-bis(4-hydroxyphenyl)decane, bis(4-hydroxy-3-nitrophenyl)methane, 3,3-bis(4-hydroxyphenyl)pentane, 1,3-bis(4-hydroxyphenyl)pentane, Bis(2-(4-hydroxyphenyl)-2-propyl)benzene, 1,3-bis(2-(4-hydroxyphenyl)-2-propyl)benzene, 2,2-bis(4-hydroxyphenyl)hexafluoropropane, 1,1-bis(4-hydroxyphenyl)cyclohexane, bis(4-hydroxyphenyl)sulfone, 2,4'-dihydroxydiphenyl sulfone, bis(4-hydroxyphenyl)sulfide, bis(4-hydroxy-3-methylphenyl)sulfide, bis(4-hydroxyphenyl)disulfide, 4, Aromatic bisphenol compounds such as 4'-dihydroxydiphenyl ether and 4,4'-dihydroxy-3,3'-dichlorodiphenyl ether; dihydroxy compounds having an ether group bonded to an aromatic group such as 2,2-bis(4-(2-hydroxyethoxy)phenyl)propane, 2,2-bis(4-(2-hydroxypropoxy)phenyl)propane, 1,3-bis(2-hydroxyethoxy)benzene, 4,4'-bis(2-hydroxyethoxy)biphenyl, and bis(4-(2-hydroxyethoxy)phenyl)sulfone;9,9-bis(4-(2-hydroxyethoxy)phenyl)fluorene, 9,9-bis(4-hydroxyphenyl)fluorene, 9,9-bis(4-hydroxy-3-methylphenyl)fluorene, 9,9-bis(4-(2-hydroxypropoxy)phenyl)fluorene, 9,9-bis(4-(2-hydroxyethoxy)-3-methylphenyl)fluorene, 9,9-bis(4-(2-hydroxypropoxy)-3-methylphenyl)fluorene, 9,9-bis(4-(2-hydroxypropoxy)-3-methylphenyl)fluorene, 9,9-bis(4-(2-hydroxyethoxy)-3-isopropylphenyl)fluorene, 9,9-bis(4-(2-hydroxyethoxy)-3-isobutylphenyl)fluorene , 9,9-bis(4-(2-hydroxyethoxy)-3-tert-butylphenyl)fluorene, 9,9-bis(4-(2-hydroxyethoxy)-3-cyclohexylphenyl)fluorene, 9,9-bis(4-(2-hydroxyethoxy)-3-phenylphenyl)fluorene, 9,9-bis(4-(2-hydroxyethoxy)-3,5-dimethylphenyl)fluorene, 9,9-bis(4-(2-hydroxyethoxy)-3-tert-butyl-6-methylphenyl)fluorene, 9,9-bis(4-(3-hydroxy-2,2-dimethylpropoxy)phenyl)fluorene and other dihydroxy compounds having a fluorene ring;

[0036] Examples of diester compounds include the following dicarboxylic acids: aromatic dicarboxylic acids such as terephthalic acid, phthalic acid, isophthalic acid, 4,4'-diphenyldicarboxylic acid, 4,4'-diphenyletherdicarboxylic acid, 4,4'-benzophenonedicarboxylic acid, 4,4'-diphenoxyethanedicarboxylic acid, 4,4'-diphenylsulfonedicarboxylic acid, and 2,6-naphthalenedicarboxylic acid; alicyclic dicarboxylic acids such as 1,2-cyclohexanedicarboxylic acid, 1,3-cyclohexanedicarboxylic acid, and 1,4-cyclohexanedicarboxylic acid; and aliphatic dicarboxylic acids such as malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, and sebacic acid. These dicarboxylic acid components can be used as raw materials for polyester carbonate resins as dicarboxylic acids themselves, but dicarboxylic acid esters such as methyl esters and phenyl esters, and dicarboxylic acid derivatives such as dicarboxylic acid halides can also be used as raw materials depending on the production method.

[0037] Among the above other structural units, it is preferable to contain a structural unit derived from an aliphatic dihydroxy compound or an alicyclic dihydroxy compound from the viewpoint of mechanical properties and heat resistance, and among these, 1,4-cyclohexanedimethanol and tricyclodecanedimethanol are more preferable.

[0038] The lower limit of the content of the other structural units in the polycarbonate resin of the present invention is preferably 1% by weight or more, more preferably 3% by weight or more. The upper limit is preferably 30% by weight or less, more preferably 25% by weight or less, and even more preferably 20% by weight or less. Within the above range, the excellent properties of the structural unit (1) are not significantly impaired, and the balance with other physical properties can be improved.

[0039] By using aromatic dihydroxy compounds or diester compounds such as bisphenol compounds as copolymerization components, the heat resistance of polycarbonate resins can be improved in some cases, but on the other hand, when the polycarbonate resin contains a large amount of aromatic structures, the weather resistance tends to decrease. In addition, since there is a large difference in the polymerization reactivity between bisphenol compounds or diester compounds and dihydroxy compounds forming the structural unit (1), it becomes difficult to obtain a polycarbonate resin with a high molecular weight, and mechanical properties such as impact resistance tend to decrease when the bisphenol compounds or diester compounds remain in the terminal groups. If the reaction temperature is raised to promote the reaction, the structural unit (1) is thermally decomposed, and the obtained polycarbonate resin tends to become colored. For these reasons, the content ratio of the structural unit derived from aromatic dihydroxy compounds or diester compounds is preferably 10% by weight or less, more preferably 5% by weight or less.

[0040] (Compound for introducing a linking group (carbonic acid diester)) The linking group contained in the polycarbonate resin in the present invention is introduced by using a compound for introducing a linking group (e.g., a carbonyl diester or a carbonyl halide) in a polycondensation reaction. The linking group introduced into the polycarbonate resin by the carbonyl diester or the carbonyl halide is a carbonyl group.

[0041] From the viewpoint of being usable in the melt polymerization method described later, it is preferable to use a carbonate diester represented by the following formula (5).

[0042] [ka]

[0043] (In formula (5), A 1 and A 2 each represents an aliphatic hydrocarbon group having 1 to 18 carbon atoms which may have a substituent, or an aromatic hydrocarbon group which may have a substituent, 1 and A 2 may be the same or different.)

[0044] A 1 and A 2 is preferably a substituted or unsubstituted aromatic hydrocarbon group, more preferably an unsubstituted aromatic hydrocarbon group. Examples of the substituent of the aliphatic hydrocarbon group include an ester group, an ether group, an amide group, and a halogen atom, and examples of the substituent of the aromatic hydrocarbon group include an alkyl group such as a methyl group or an ethyl group.

[0045] Examples of the carbonic acid diester represented by the formula (5) include diphenyl carbonate (hereinafter sometimes abbreviated as DPC), substituted diphenyl carbonates such as ditolyl carbonate, and dialkyl carbonates such as dimethyl carbonate, diethyl carbonate, and di-tert-butyl carbonate. From the viewpoint of reactivity, preferred are diphenyl carbonate and substituted diphenyl carbonates, and particularly preferred is diphenyl carbonate.

[0046] The carbonate diester may contain impurities such as chloride ions, and these impurities may inhibit the polymerization reaction or deteriorate the hue of the resulting resin. Therefore, it is preferable to use a diester that has been purified, as necessary, by distillation or the like.

[0047] In the polycondensation reaction, the reaction rate and the molecular weight of the resin obtained can be controlled by strictly adjusting the molar ratio of all dihydroxy compounds used in the reaction to all compounds for introducing linking groups (e.g., carbonic acid diester). In the case of polycarbonate, the molar ratio of carbonic acid diester to all dihydroxy compounds is preferably adjusted to 0.90 to 1.10, more preferably adjusted to 0.96 to 1.05, and particularly preferably adjusted to 0.98 to 1.03. When a compound for introducing a linking group other than a carbonic acid diester is mixed and used, the total amount of the carbonic acid diester and the compound for introducing another linking group is adjusted to the above-mentioned molar ratio range with respect to the total dihydroxy compounds. When the molar ratio is within the above-mentioned range, a resin with a desired molecular weight can be produced at a good reaction rate, and the amount of low molecular weight compounds remaining in the resin can be reduced, so that a resin with excellent color tone, thermal stability, and moldability can be obtained.

[0048] <Production method of polycarbonate resin in the present invention> The polycarbonate resin of the present invention can be produced by a commonly used polymerization method. For example, it can be produced by a solution polymerization method or an interfacial polymerization method using phosgene or a carboxylic acid halide, or a melt polymerization method in which a reaction is carried out without using a solvent. Among these production methods, it is preferable to produce the polycarbonate resin by the melt polymerization method, which is excellent in productivity and can reduce the environmental load because it does not use a solvent or a highly toxic compound.

[0049] In the melt polymerization method, the above-mentioned dihydroxy compound and a compound for introducing a linking group (e.g., a carbonic acid diester) are polycondensed by transesterification to obtain a polycarbonate resin. More specifically, the polycarbonate resin can be obtained by removing the monohydroxy compound and the like that are by-produced in the transesterification reaction from the system.

[0050] The transesterification reaction proceeds in the presence of a transesterification catalyst (hereinafter, the transesterification catalyst is referred to as a "polymerization catalyst.") The type of polymerization catalyst can have a significant effect on the reaction rate of the transesterification reaction and the quality of the resulting polycarbonate resin.

[0051] The polymerization catalyst is not particularly limited as long as it satisfies the transparency, color tone, heat resistance, weather resistance, and mechanical properties of the resulting polycarbonate resin. For example, metal compounds of Group I or Group II (hereinafter simply referred to as "Group 1" and "Group 2") in the long-form periodic table, as well as basic compounds such as basic boron compounds, basic phosphorus compounds, basic ammonium compounds, and amine compounds can be used as the polymerization catalyst, and among these, Group 1 metal compounds and / or Group 2 metal compounds are preferred.

[0052] Examples of Group 1 metal compounds include the following compounds: sodium hydroxide, potassium hydroxide, lithium hydroxide, cesium hydroxide, sodium hydrogen carbonate, potassium hydrogen carbonate, lithium hydrogen carbonate, cesium hydrogen carbonate, sodium carbonate, potassium carbonate, lithium carbonate, cesium carbonate, sodium acetate, potassium acetate, lithium acetate, cesium acetate, sodium stearate, potassium stearate, lithium stearate, cesium stearate, sodium borohydride, potassium borohydride, lithium borohydride, cesium borohydride, sodium phenylborohydride, and boron phenylide. Potassium, lithium phenyl boron, cesium phenyl boron, sodium benzoate, potassium benzoate, lithium benzoate, cesium benzoate, disodium hydrogen phosphate, dipotassium hydrogen phosphate, dilithium hydrogen phosphate, dicesium hydrogen phosphate, disodium phenylphosphate, dipotassium phenylphosphate, dilithium phenylphosphate, dicesium phenylphosphate, alcoholates, phenolates of sodium, potassium, lithium, and cesium, and disodium salts, dipotassium salts, dilithium salts, and dicesium salts of bisphenol A. As the Group 1 metal compound, lithium compounds are preferred from the viewpoints of polymerization activity and the color tone of the resulting polycarbonate resin.

[0053] Examples of Group 2 metal compounds include the following compounds: calcium hydroxide, barium hydroxide, magnesium hydroxide, strontium hydroxide, calcium hydrogen carbonate, barium hydrogen carbonate, magnesium hydrogen carbonate, strontium hydrogen carbonate, calcium carbonate, barium carbonate, magnesium carbonate, strontium carbonate, calcium acetate, barium acetate, magnesium acetate, strontium acetate, calcium stearate, barium stearate, magnesium stearate, and strontium stearate. As the Group 2 metal compound, magnesium compounds, calcium compounds, or barium compounds are preferred, and from the viewpoints of polymerization activity and color tone of the resulting polycarbonate resin, magnesium compounds and / or calcium compounds are more preferred, and calcium compounds are even more preferred.

[0054] Although it is possible to use a basic compound such as a basic boron compound, a basic phosphorus compound, a basic ammonium compound, or an amine compound in combination with the Group 1 metal compound and / or the Group 2 metal compound, it is preferable to use only the Group 1 metal compound and / or the Group 2 metal compound, and more preferably to use only the Group 2 metal compound from the viewpoint of the color tone of the resulting polycarbonate resin.

[0055] The amount of the polymerization catalyst used is preferably 0.1 μmol or more, more preferably 0.5 μmol or more, and even more preferably 1 μmol or more per mol of the total dihydroxy compounds used in the reaction, and is preferably 50 μmol or less, more preferably 20 μmol or less, and even more preferably 10 μmol or less per mol of the total dihydroxy compounds used in the reaction.

[0056] By adjusting the amount of the polymerization catalyst used within the above range, the polymerization rate can be increased, so that it is possible to obtain a polycarbonate resin with a desired molecular weight without necessarily increasing the polymerization temperature, and the deterioration of the color tone of the polycarbonate resin can be suppressed. In addition, it is possible to prevent the unreacted raw materials from volatilizing during the polymerization, which would cause the molar ratio of the dihydroxy compound and the carbonic acid diester to be lost, so that a resin with a desired molecular weight and copolymerization ratio can be obtained more reliably. Furthermore, it is possible to suppress the occurrence of side reactions, so that the deterioration of the color tone of the polycarbonate resin or coloring during molding can be further prevented.

[0057] Considering the adverse effects of sodium, potassium, and cesium among the group 1 metals on the color tone of the polycarbonate resin and the adverse effects of iron on the color tone of the polycarbonate resin, the total content of sodium, potassium, cesium, and iron in the polycarbonate resin is preferably 1 weight ppm or less. In this case, the deterioration of the color tone of the polycarbonate resin can be further prevented, and the color tone of the polycarbonate resin can be further improved. From the same viewpoint, the total content of sodium, potassium, cesium, and iron in the polycarbonate resin is more preferably 0.5 weight ppm or less. Note that these metals may be mixed in not only from the catalyst used, but also from the raw materials or reaction equipment. Regardless of the source, the content of these metals in the polycarbonate resin is preferably within the above-mentioned range as the total content of sodium, potassium, cesium, and iron.

[0058] The method of polycondensing a dihydroxy compound and a carbonic acid diester is carried out in multiple stages using multiple reactors in the presence of the above-mentioned catalyst. The reaction may be carried out in a batchwise manner, a continuous manner, or a combination of a batchwise manner and a continuous manner, but it is preferable to adopt a continuous manner, which is excellent in productivity and can obtain a polycarbonate resin with less heat history.

[0059] From the viewpoint of controlling the polymerization rate and the quality of the resulting polycarbonate resin, it is important to appropriately select the jacket temperature, the internal temperature, and the pressure in the reaction system according to the reaction stage. Specifically, it is preferable to obtain a prepolymer at a relatively low temperature and low vacuum in the early stage of the polycondensation reaction, and to increase the molecular weight to a predetermined value at a relatively high temperature and high vacuum in the later stage of the reaction. In this case, the distillation of unreacted monomers is suppressed, and it becomes easier to adjust the molar ratio of the dihydroxy compound and the carbonate diester to a desired ratio. As a result, the decrease in the polymerization rate can be suppressed. In addition, it becomes possible to more reliably obtain a polymer having a desired molecular weight and terminal group.

[0060] By adjusting the temperature of the polycondensation reaction, it is possible to improve productivity and prevent the increase of the heat history of the product. Furthermore, it is possible to further prevent the volatilization of the monomer and the decomposition and coloration of the polycarbonate resin. Specifically, the following conditions can be adopted as the reaction conditions in the first stage reaction. That is, the maximum temperature inside the polymerization reactor is set in the range of usually 160 to 230°C, preferably 170 to 220°C, and more preferably 180 to 210°C. In addition, the pressure of the polymerization reactor (hereinafter, pressure refers to absolute pressure) is set in the range of usually 1 to 110 kPa, preferably 5 to 50 kPa, and more preferably 7 to 30 kPa. In addition, the reaction time is set in the range of usually 0.1 to 10 hours, preferably 1 to 5 hours. It is preferable that the first stage reaction is carried out while distilling off the generated monohydroxy compound outside the reaction system.

[0061] From the second stage onwards, it is preferable to gradually reduce the pressure of the reaction system from the pressure of the first stage, and to finally reduce the pressure (absolute pressure) of the reaction system to 1 kPa or less while removing the monohydroxy compound that is subsequently generated from the reaction system. The maximum internal temperature of the polymerization reactor is usually set in the range of 200 to 260° C., preferably 210 to 240° C., and more preferably 215 to 230° C. The reaction time is usually set in the range of 0.1 to 10 hours, preferably 0.5 to 5 hours, and more preferably 1 to 3 hours.

[0062] Using the stirring power as an indicator, once it has been confirmed that the specified reduced viscosity (molecular weight) has been reached, the polycondensation reaction is stopped by introducing nitrogen into the reactor to return the pressure to normal pressure, or by withdrawing the molten resin from the reactor. The molten resin is discharged from the die head in the form of strands, cooled and solidified, and pelletized using a rotary cutter or the like. If necessary, extrusion devolatilization, extrusion kneading, and extrusion filtration processes may be added before pelletization. In these processes, additives are mixed into the resin, low molecular weight components are devolatilized using a vacuum vent, and foreign matter is removed using a polymer filter.

[0063] <Characteristics of the polycarbonate resin in the present invention> (molecular weight) The molecular weight of the polycarbonate resin in the present invention is determined by the reduced viscosity and 1 It can be expressed as the number average molecular weight measured by H-NMR, etc. The higher the value obtained by these measurement methods, the higher the molecular weight. 1 The number average molecular weight measured by H-NMR is preferably 8,000 or more and 30,000 or less. The lower limit is more preferably 9,000 or more, and even more preferably 10,000 or more. The upper limit is more preferably 25,000 or less, and even more preferably 20,000 or less. The reduced viscosity of the polycarbonate resin in the present invention is preferably 0.3 dL / g or more and 1.0 dL / g or less. The lower limit is more preferably 0.35 dL / g or more, and even more preferably 0.38 dL / g or more. The upper limit is more preferably 0.8 dL / g or less, and even more preferably 0.7 dL / g or less. Within the above range, sufficient mechanical strength can be obtained, and the fluidity during melt molding can also be adjusted to a preferred range. In this specification, 1 The number average molecular weight measured by H-NMR is 1 When the term "number average molecular weight (Mn)," "number average molecular weight," or "Mn" is used, it refers to the number average molecular weight measured by GPC, which will be described later.

[0064] (glass transition temperature) The glass transition temperature of the polycarbonate resin in the present invention is preferably 130° C. or higher and 160° C. or lower. The lower limit is more preferably 135° C. or higher, and even more preferably 140° C. or higher. The upper limit is more preferably 155° C. or lower, and even more preferably 150° C. or lower. Within the above range, the polycarbonate resin has sufficient heat resistance and mechanical properties, and is also excellent in melt processability.

[0065] (Melt Viscosity) The melt viscosity of the polycarbonate resin in the present invention at 240°C is preferably 1000 Pa·s or more and 5000 Pa·s or less. The lower limit is more preferably 1500 Pa·s or more, and even more preferably 2000 Pa·s or more. The upper limit is more preferably 4000 Pa·s or less, and even more preferably 3000 Pa·s or less. Within the above range, sufficient mechanical strength can be obtained and fluidity during melt molding can be ensured. Furthermore, in this case, coloring and foaming caused by an increase in resin temperature due to shear heat can be further prevented. In this specification, the melt viscosity is the melt viscosity measured using a capillary rheometer (manufactured by Toyo Seiki Seisakusho Co., Ltd.) at a temperature of 240°C and a shear rate of 91.2 sec -1 The method for measuring the melt viscosity will be described in detail later.

[0066] <Acrylic resin> The resin composition constituting the optical film of the present invention contains an acrylic resin containing 50% by weight or more and 100% by weight or less of the structural unit (2). Hereinafter, this acrylic resin may be referred to as the "acrylic resin in the present invention." In this specification, the content of the structural unit (2) in the acrylic resin means the content (wt%) of each of the structural units (2) when the total weight of all the structural units constituting the acrylic resin is taken as 100% by weight. The contents of other structural units in the acrylic resin are defined in the same manner.

[0067] The acrylic resin in the present invention preferably has compatibility with the polycarbonate resin in the present invention. From this viewpoint, R 1R is preferably a hydrogen atom or a methyl group, and more preferably a methyl group which has higher heat resistance. 2 is a structure containing a cyclohexane structure, and this structure enhances compatibility with the polycarbonate resin in the present invention. Examples of vinyl compounds forming the structural unit (2) include cyclohexyl acrylate, cyclohexyl methacrylate, cyclohexyl methyl acrylate, cyclohexyl methyl methacrylate, 1-ethylcyclohexyl acrylate, 1-ethylcyclohexyl methacrylate, 2-cyclohexylpropyl-2-yl acrylate, 2-cyclohexylpropyl-2-yl methacrylate, hydroxycyclohexyl acrylate, hydroxycyclohexyl methacrylate, cyclohexanedimethanol monoacrylate, cyclohexanedimethanol monomethacrylate, 3,4-epoxycyclohexylmethyl acrylate, 3,4-epoxycyclohexylmethyl methacrylate, etc. These may be used alone or in combination of two or more. Among these, from the viewpoints of availability and physical properties such as heat resistance and low birefringence of the resulting acrylic resin, it is more preferable to use cyclohexyl methacrylate, hydroxycyclohexyl methacrylate, and cyclohexane monomethacrylate, and cyclohexyl methacrylate is even more preferable.

[0068] The lower limit of the content of the structural unit (2) in the acrylic resin in the present invention is preferably 70% by weight or more, more preferably 80% by weight or more, and particularly preferably 85% by weight or more. The upper limit is preferably 99% by weight or less. Within the above range, compatibility with the polycarbonate resin in the present invention is good, and heat resistance and optical properties are also excellent.

[0069] The acrylic resin in the present invention preferably contains a structural unit other than the structural unit (2), and more preferably an acrylate structural unit represented by the following formula (3) is introduced. By introducing the acrylate structural unit represented by the following formula (3), thermal decomposition of the main chain can be suppressed, and the thermal stability of the acrylic resin can be improved.

[0070] [ka] (In formula (3), R 3 is a hydrogen atom, an alkyl group having 1 to 10 carbon atoms which may have a substituent, a cycloalkyl group, or an aryl group.

[0071] The vinyl compound forming the structural unit (3) is not particularly limited as long as it satisfies the above definition and has a structure in which the main chain is an acrylate structural unit, but from the viewpoint of improving thermal stability without changing the desired resin properties, the vinyl compound forming the structural unit (3) is preferably one having a relatively small molecular weight or a structure similar to that of the structural unit (2), and more preferably methyl acrylate, ethyl acrylate, or cyclohexyl acrylate is used. The lower limit of the content of the structural unit (3) is preferably 0.1% by weight or more, more preferably 0.5% by weight or more. The upper limit is preferably 10% by weight or less, more preferably 5% by weight or less. Within the above range, sufficient thermal stability for use in melt molding can be imparted without impairing compatibility with the polycarbonate resin in the present invention.

[0072] When the acrylic resin in the present invention contains a (meth)acrylate structural unit containing an ether group or a hydroxyl group, the compatibility with the polycarbonate resin in the present invention can be improved. Examples of vinyl compounds forming a (meth)acrylate structural unit containing an ether group or a hydroxyl group include 2-hydroxyethyl acrylate, 2-hydroxyethyl methacrylate, methoxyethyl acrylate, methoxyethyl methacrylate, 2-hydroxyethoxyethyl acrylate, 2-hydroxyethoxyethyl methacrylate, glycerin monoacrylate, glycerin monomethacrylate, polyethylene glycol monoacrylate, polyethylene glycol monomethacrylate, methoxypolyethylene glycol acrylate, methoxypolyethylene glycol acrylate, polypropylene glycol monoacrylate, polypropylene glycol monomethacrylate, polytrimethylene glycol monoacrylate, polytrimethylene glycol monomethacrylate, polycaprolactone-modified 2-hydroxyethyl acrylate, and polycaprolactone-modified 2-hydroxyethyl methacrylate. These may be used alone or in combination of two or more. From the viewpoint of balancing various physical properties, the content of this component is preferably 1% by weight or more and 20% by weight or less.

[0073] The acrylic resin in the present invention may further contain another structural unit, and examples of the vinyl compounds forming the other structural units include acrylonitrile, styrene, α-methylstyrene, butadiene, and polyfunctional (meth)acrylates. By appropriately combining these, it is possible to improve the thermal stability of the acrylic resin, adjust the refractive index of the acrylic resin, and improve the transparency of the resin composition. From the viewpoint of ensuring compatibility with the polycarbonate resin, it is preferable that the content of the component is relatively small, and it is preferably 0.1% by weight or more and 10% by weight or less. The lower limit is more preferably 0.3% by weight or more, and more preferably 0.5% by weight or more. The upper limit is more preferably 7% by weight or less, and more preferably 5% by weight or less.

[0074] <Characteristics of the acrylic resin in the present invention> (molecular weight, molecular weight distribution) Various molecular weights of the acrylic resin in the present invention can be measured by GPC, which will be described later. The weight average molecular weight (Mw) of the acrylic resin in the present invention is preferably 10,000 or more and 500,000 or less. The lower limit of the weight average molecular weight is more preferably 20,000 or more, and even more preferably 30,000 or more. The upper limit is more preferably 400,000 or less, and even more preferably 300,000 or less. Within the above range, compatibility with the polycarbonate resin in the present invention is good, and mechanical properties are also excellent.

[0075] The number average molecular weight (Mn) is preferably 10,000 or more and 200,000 or less. The molecular weight distribution (Mw / Mn) is preferably 1.0 or more and 5.0 or less. The molecular weight of the acrylic resin can be adjusted by the ratio of the amount of the monomer used in the polymerization to the amount of the radical polymerization initiator and the chain transfer agent.

[0076] (glass transition temperature) The glass transition temperature of the acrylic resin in the present invention is preferably 30°C or higher and 120°C or lower. The lower limit is more preferably 40°C or higher, and even more preferably 50°C or higher. The upper limit is more preferably 110°C or lower, and even more preferably 100°C or lower. Within the above range, the acrylic resin becomes solid at room temperature and has excellent handleability. In addition, it can be melt-processed at the same temperature as the polycarbonate resin in the present invention.

[0077] <Method of producing acrylic resin in the present invention> Examples of the method for producing the acrylic resin in the present invention include bulk polymerization, solution polymerization, and aqueous dispersion polymerization such as suspension polymerization and emulsion polymerization. Among these, aqueous dispersion polymerization is preferred from the viewpoint of simplifying the recovery process of the resin after polymerization and controlling the heat generated by polymerization, and suspension polymerization is particularly preferred. In the suspension polymerization, the resin after polymerization is obtained as spherical particles with an average particle size of about 5 μm to 1 mm, so that the flowability is good when used in processing operations such as extrusion and molding, and also, there is little concern about dust scattering, so that the handling is excellent.

[0078] <Resin composition> The resin composition constituting the optical film of the present invention preferably contains 50% by weight or more and 99% by weight or less of the polycarbonate resin of the present invention, and 1% by weight or more and 50% by weight or less of the acrylic resin of the present invention. The lower limit of the content of the polycarbonate resin of the present invention is more preferably 60% by weight or more, and even more preferably 70% by weight or more. The upper limit is more preferably 95% by weight or less, and even more preferably 90% by weight or less. The lower limit of the content of the acrylic resin of the present invention is more preferably 5% by weight or more, and even more preferably 10% by weight or more. The upper limit is more preferably 40% by weight or less, and even more preferably 30% by weight or less. By keeping it within the above range, various physical properties such as heat resistance, low birefringence, and mechanical properties can be balanced at a high level.

[0079] (Additives) The resin composition constituting the film of the present invention may contain other components such as additives in addition to the polycarbonate resin and acrylic resin. Within the scope of not impairing the effects of the present invention, additives that can be used include antioxidants, heat stabilizers, light stabilizers, ultraviolet absorbers, fillers such as fillers, neutralizing agents, lubricants, antifogging agents, antiblocking agents, slip agents, dispersants, colorants, flame retardants, antistatic agents, conductivity imparting agents, crosslinking agents, crosslinking assistants, metal deactivators, molecular weight regulators, antibacterial agents, antifungal materials, fluorescent brightening agents, organic diffusing agents, inorganic diffusing agents, and the like.

[0080] Furthermore, within a range that does not impair the effects of the present invention, the composition may further contain one or more types of resins, such as synthetic resins such as aromatic polycarbonates, aromatic polyesters, aliphatic polyesters, polyamides, polystyrenes, polyolefins, amorphous polyolefins, acrylonitrile-butadiene-styrene copolymers (ABS resins), and acrylonitrile-styrene copolymers (AS resins); elastomers such as acrylic rubbers, butadiene rubbers, and silicone rubbers; and biodegradable resins such as polylactic acid and polybutylene succinate.

[0081] <Method of producing resin composition> The resin composition constituting the film of the present invention can be produced, for example, by a method of mechanically melt-kneading each of the above-mentioned components constituting the resin composition. As the melt-kneader, a single-screw extruder, a twin-screw extruder, a Brabender, a Banbury mixer, a kneader blender, a roll mill, etc. can be used. When kneading, each component may be kneaded at once, or a multi-stage division kneading method in which an arbitrary component is kneaded and then the remaining components are added and kneaded may be used. Among them, a method in which each component is continuously charged using a twin-screw extruder equipped with a vacuum vent and a resin composition is continuously obtained is preferable from the viewpoint of productivity and quality uniformity. The lower limit of the kneading temperature is usually 150°C or more, preferably 180°C or more, and more preferably 200°C or more. The upper limit of the kneading temperature is usually 280°C or less, preferably 260°C or less, more preferably 250°C or less, and even more preferably 240°C or less. Within this range, productivity (processing speed of kneading) is also increased while suppressing heat deterioration due to heating by the kneader and heat generation due to shear.

[0082] <Characteristics of resin composition> (transparency) The resin composition constituting the film of the present invention preferably has a haze value of 7% or less, more preferably 6% or less, and even more preferably 5% or less, as measured by the method described below. If the haze value is within the above range, the film can be applied to applications requiring high transparency.

[0083] (Heat resistance) The resin composition constituting the film of the present invention preferably has a glass transition temperature of 130° C. or more and 160° C. or less, as measured by the method described below. The lower limit is more preferably 135° C. or more, and even more preferably 140° C. or more. The upper limit is more preferably 155° C. or less, and even more preferably 150° C. or less. Within the above range, the film has practical heat resistance and is also excellent in mechanical properties such as stretchability and melt processability.

[0084] <Molded products> The resin composition constituting the film of the present invention can be processed into various molded products by molding methods such as injection molding (insert molding, two-color molding, sandwich molding, gas injection molding, etc.), extrusion molding, inflation molding, T-die film molding, lamination molding, blow molding, hollow molding, compression molding, calendar molding, etc. The shape of the molded product is not particularly limited, and examples thereof include sheets, films, plates, particles, lumps, fibers, rods, porous bodies, foams, etc.

[0085] (Application) The applications of the molded products are not particularly limited, but the resin composition constituting the optical film of the present invention has excellent optical properties, heat resistance, and moldability, and also has high transparency, and is therefore suitable for optical applications such as optical films, optical disks, optical prisms, and lenses, and is particularly suitable for applications requiring low birefringence, such as polarizing plate protective films and display front protective films.

[0086] [Method of Manufacturing the Optical Film of the Present Invention] As a method for forming an unstretched film using the above-mentioned resin composition, a casting method in which the resin composition is dissolved in a solvent and cast, and then the solvent is removed, or a melt film-forming method in which the resin is melted without using a solvent to form a film can be adopted.Specific examples of the melt film-forming method include melt extrusion using a T-die, calendar molding, heat pressing, co-extrusion, co-melting, multilayer extrusion, and inflation molding.The film-forming method for an unstretched film is not particularly limited, but since the casting method may cause problems due to residual solvent, the melt film-forming method is preferable, and among them, the melt extrusion method using a T-die is preferable from the viewpoint of ease of subsequent stretching treatment.

[0087] When forming an unstretched film by the melt film-forming method, the forming temperature is preferably 270°C or less, more preferably 265°C or less, and particularly preferably 260°C or less. If the forming temperature is too high, defects due to the generation of foreign matter or bubbles in the obtained film may increase, or the film may become discolored. However, if the forming temperature is too low, the melt viscosity of the resin composition becomes too high, making it difficult to form, and it may be difficult to produce an unstretched film with a uniform thickness, so the lower limit of the forming temperature is usually 200°C or more, preferably 210°C or more, and more preferably 220°C or more. Here, the forming temperature of the unstretched film is the temperature during forming in the melt film-forming method, and is usually the value measured by measuring the temperature at the die outlet from which the molten resin is extruded.

[0088] If foreign matter is present in the film, it will be recognized as a defect such as light leakage when used as a polarizing plate. In order to remove foreign matter in the resin composition, a method is preferred in which a polymer filter is attached after the extruder, the resin composition is filtered, and then extruded through a die to form a film. In this case, it is necessary to connect the extruder, the polymer filter, and the die with piping to transfer the molten resin composition, but in order to minimize thermal deterioration in the piping, it is important to arrange each piece of equipment so that the residence time is minimized. In addition, the process of transporting and winding the film after extrusion is performed in a clean room, and the utmost care is required to prevent foreign matter from adhering to the film.

[0089] The thickness of the original film (unstretched film) before stretching is determined according to the design of the film thickness after stretching and the stretching conditions such as the stretching ratio. If the film is too thick, thickness unevenness is likely to occur, and if the film is too thin, it may break during stretching. Therefore, the thickness is usually 30 μm or more, preferably 40 μm or more, and more preferably 50 μm or more, and is usually 200 μm or less, preferably 160 μm or less, and more preferably 120 μm or less.

[0090] The length of the unstretched film in the longitudinal direction is preferably 500 m or more, more preferably 1000 m or more, and particularly preferably 1500 m or more. From the viewpoints of productivity and quality, it is preferable to perform continuous stretching when producing the optical film of the present invention, but usually, condition adjustment is required to match a predetermined retardation at the start of stretching, and if the length of the film is too short, the amount of the product that can be obtained after condition adjustment is reduced.

[0091] By stretching the unstretched film, the area can be increased and the thickness unevenness can be reduced. Alternatively, by orienting the polymer chains by stretching, an optical film can be obtained by providing a predetermined phase difference. As the stretching method, known methods such as longitudinal uniaxial stretching, transverse uniaxial stretching using a tenter or the like, or a combination of these, simultaneous biaxial stretching, sequential biaxial stretching, etc. can be used. Since the resin composition constituting the film of the present invention has low birefringence characteristics, it is preferable to use the unstretched film as a product or to use a stretching method that does not develop an in-plane phase difference by simultaneous biaxial stretching. Stretching may be performed in a batch manner, but a continuous manner is preferable in terms of productivity and the quality of the obtained stretched film.

[0092] The stretching temperature is preferably in the range of (Tg-20°C) to (Tg+30°C) with respect to the glass transition temperature (Tg) of the resin used as the raw material. The lower limit of the stretching temperature is more preferably (Tg-10°C) or more, and even more preferably (Tg-5°C) or more. The upper limit is more preferably (Tg+25°C) or less, and even more preferably (Tg+20°C) or less. The stretching ratio is determined according to the target retardation value, and is 1.2 times to 4 times, more preferably 1.5 times to 3.5 times, and even more preferably 2 times to 3 times in each of the longitudinal and transverse directions. If the stretching ratio is too small, the productivity is poor, while if the stretching ratio is too large, the film may break or wrinkles may occur during stretching. When the optical film of the present invention is stretched and used, it is preferable that the maximum stretching ratio when stretched by the method described below is 2.7 times or more because the stretching process is stable.

[0093] The stretching speed is also appropriately selected depending on the purpose, and can be selected so that the strain rate represented by the following formula is usually 30% / min to 2000% / min, preferably 50% / min to 1000% / min, more preferably 70% / min to 500% / min, and particularly preferably 100% / min to 400% / min. If the stretching speed is too high, it may cause breakage during stretching or the optical properties may fluctuate greatly due to long-term use under high temperature conditions. In addition, if the stretching speed is too low, not only will the productivity decrease, but the orientation of the polymer molecular chains may relax during stretching, making it difficult to obtain the desired orientation. Distortion rate (% / min) = {stretching rate (mm / min) / original film length (mm)} x 100

[0094] After stretching the unstretched film, a heat setting process may be performed in a heating furnace as necessary, or a relaxation process may be performed by controlling the width of the tenter or adjusting the roll peripheral speed. The heat setting temperature is in the range of 60°C to (Tg), preferably 70°C to (Tg-5°C) relative to the glass transition temperature (Tg) of the resin used in the unstretched film. If the heat treatment temperature is too high, the desired retardation may be significantly reduced or wrinkles may occur. In addition, when a relaxation process is provided, the film may be contracted to 95% to 100% of the width of the film expanded by stretching, thereby removing the stress generated in the film. The treatment temperature applied to the film at this time is the same as the heat setting temperature. By performing the heat setting process or relaxation process as described above, the birefringence can be further reduced and the fluctuation of optical properties due to long-term use under high temperature conditions can be suppressed.

[0095] Although the thickness required varies depending on the application, the optical film of the present invention has excellent toughness and is therefore advantageous in applications where a thin film is particularly required, so that the thickness of the final product, both the unstretched film and the stretched film, is preferably 50 μm or less. More preferably, it is 45 μm or less, and even more preferably, it is 40 μm or less. On the other hand, if the thickness is too thin, the film becomes difficult to handle, and wrinkles or breakage occurs during production, so the lower limit of the thickness of the optical film of the present invention is preferably 3 μm or more, more preferably 5 μm or more.

[0096] The optical film of the present invention is suitable for applications requiring low birefringence, and preferably has an in-plane birefringence (Δn) of 0.010 or less at a wavelength of 590 nm measured by the method described below. More preferably, it is 0.009 or less, and even more preferably, it is 0.008 or less. If it is within the above range, it has a property that birefringence is unlikely to occur due to stress or deformation, and a low birefringence film can be stably produced in the film production.

[0097] The optical film of the present invention has an absolute value of a photoelastic coefficient of 14×10 -12 Pa -1 It is preferable that the value is less than 13×10 -12 Pa -1 It is more preferable that the photoelastic coefficient is 0.1 to 1.0 times or less. If the photoelastic coefficient is too large, when the film of the present invention is incorporated into an image display device, degradation of image quality such as white blurring of the periphery of the screen may occur. This problem is particularly noticeable when the film is used in a large display device or a bendable (bendable, rollable, foldable) display device.

[0098] [Polarizing plate] The optical film of the present invention becomes a polarizing plate by laminating and pasting with a known linear polarizer. As the linear polarizer, a polarizing film or a liquid crystal compound having an absorption axis in either the width direction or the length direction can be adopted. Specific examples of the polarizing film include a film obtained by uniaxially stretching a dichroic substance such as iodine or a dichroic dye adsorbed on a hydrophilic polymer film such as a polyvinyl alcohol film, a partially formalized polyvinyl alcohol film, or an ethylene-vinyl acetate copolymer partially saponified film, and a polyene-based oriented film such as a dehydrated product of polyvinyl alcohol or a dehydrochlorinated product of polyvinyl chloride. Among these, a long polarizing film obtained by uniaxially stretching a dichroic substance such as iodine adsorbed on a polyvinyl alcohol film is particularly preferred because it has a high polarized dichroic ratio.

[0099] The optical film of the present invention and the polarizing film may be laminated via a pressure-sensitive adhesive. As the pressure-sensitive adhesive, any known pressure-sensitive adhesive may be used as long as it does not impair the optical properties of the laminated film (polarizing plate).

[0100] As described above, the polarizing plate has sufficient heat resistance and optical properties, and is configured so as to be suitable for use in devices that require precision, thinness, and uniformity. Therefore, the polarizing plate can be suitable for use in, for example, liquid crystal panels used in liquid crystal displays, organic EL panels used in organic EL displays, and the like. EXAMPLES

[0101] The present invention will be described in more detail below using examples, but the present invention is not limited to the following examples as long as the gist of the present invention is not exceeded.

[0102] [Measurement method] Various physical properties were measured according to the following methods.

[0103] <Measurement of polycarbonate resin> (reduced viscosity) A polycarbonate resin sample was dissolved in methylene chloride to prepare a resin solution with a concentration of 0.6 g / dL. Using an Ubbelohde viscometer (manufactured by Moritomo Rika Kogyo Co., Ltd.), the solvent transit time t0 and the solution transit time t were measured at a temperature of 20.0°C ± 0.1°C. The relative viscosity η was calculated using the obtained t0 and t values ​​according to the following formula (i). rel The relative viscosity η rel Using the concentration c [g / dL], the reduced viscosity η is calculated using the following equation (ii): sp The higher this value, the larger the molecular weight. η rel =t / t0(i) η sp / c=(η rel -1) / c (ii)

[0104] ( 1 (number average molecular weight measured by H-NMR) Approximately 15 mg of a polycarbonate resin sample was weighed out and dissolved in approximately 0.7 mL of deuterated chloroform. This was then placed in an NMR tube with an inner diameter of 5 mm. 1 H-NMR spectrum was measured. From the intensity ratio of the signals based on each repeating structural unit of the polycarbonate resin and the signals of various terminal groups, 1 The number average molecular weight was calculated using H-NMR. The equipment and conditions used are as follows: Equipment: JNM-ECZ400S (manufactured by JEOL Ltd.) ·Measurement temperature: 30℃ Relaxation time: 6 seconds Number of times accumulated: 64

[0105] For example, the copolymer polycarbonate resin of ISB (isosorbide) and CHDM (1,4-cyclohexanedimethanol) 1 The H-NMR analysis is carried out as follows. The ISB double bond end and the CHDM double bond end are end group structures formed by a thermal decomposition reaction during the polymerization reaction.

[0106] (Range for calculating integral value) (a): 5.6-4.4 ppm: All derived from ISB repeating structural units (proton number: 4, molecular weight: 172.14) (b): 2.2-0.5 ppm: All derived from CHDM repeating structural units (proton number: 10, molecular weight: 170.21) (c): 4.4 ppm: from the hydroxyl end group of ISB (proton number: 1) (d): 3.6-3.5 ppm: derived from ISB hydroxy end group (proton number: 1) and CHDM hydroxy end group (proton number: 2) (e): 3.5-3.4 ppm: derived from CHDM hydroxyl end groups (proton count: 2) and ISB double bond end groups (proton count: 1) (f): 2.6 ppm: from ISB hydroxyl end group (proton number: 1) (g): 6.7-6.5 ppm: ISB double bond end group (proton number: 1) (h): 2.3 ppm: derived from CHDM double bond end group (proton number: 2) (i): 7.4 ppm: DPC (diphenyl carbonate) end group (proton number: 2, molecular weight: 93.10)

[0107] (Calculation of the value equivalent to the number of moles of each structure) Total ISB repeating units (a´): (a) integral value / 4 Total CHDM repeating unit (b´): (b) integral value / 10 ISB hydroxyl end group (c´): (c) integral value + (f) integral value CHDM hydroxy end group (d´): {(d) integral value - (f) integral value} / 2 + {(e) integral value - (g) integral value} / 2 ISB double bond end group (e´): (g) integral value ·CHDM double bond end group (f´): (h) integral value / 2 DPC end group (i´): (i) integral value / 2

[0108] ( 1 Calculation of number average molecular weight measured by H-NMR) (a´×172.14+b´×170.21+i´×93.10) / {(c´+d´+e´+f´+i´) / 2}

[0109] (Melt Viscosity) The polycarbonate resin sample was vacuum dried at 90° C. for 5 hours or more. Then, the melt viscosity was measured using a capillary rheometer (manufactured by Toyo Seiki Seisakusho Co., Ltd.). The measurement temperature was 240° C., and the shear rate was 6.08 to 1824 sec -1 The shear rate was set to 91.2 sec -1 The value at was used as the melt viscosity of the resin to be measured. The orifice used was 1 mmφ×10 mmL.

[0110] (glass transition temperature) The glass transition temperature of polycarbonate resin was measured using a differential scanning calorimeter DSC6220 (manufactured by SII Nano Technology Co., Ltd.). Approximately 10 mg of resin was placed in an aluminum pan manufactured by the same company and sealed. Measurement was started at 200°C under a nitrogen gas flow of 50 mL / min, and the temperature was cooled to 0°C at a rate of 20°C / min. The sample was held at 0°C for 3 minutes and then heated again to 200°C at a rate of 20°C / min. From the DSC data during the temperature rise, the extrapolated glass transition onset temperature was calculated, which is the temperature at the intersection of a straight line extending the low-temperature baseline to the high-temperature side and a tangent drawn at the point where the gradient of the curve of the step-like change in the glass transition is maximum, and this was taken as the glass transition temperature.

[0111] <Measurement of acrylic resin> (GPC) The number average molecular weight (Mn), weight average molecular weight (Mw), and molecular weight distribution (Mw / Mn) of the acrylic resin were measured using gel permeation chromatography (GPC). Approximately 10 mg of the resin sample was dissolved in 10 mL of tetrahydrofuran, and the solution filtered through a 0.45 μm filter was used as a sample for GPC measurement. A polymer measurement guard column TSK-GUARD COLUMN SUPER HH (manufactured by Tosoh Corporation) and two polymer measurement columns TSK-GEL SUPER HM-H (manufactured by Tosoh Corporation) were connected in series to a gel permeation chromatography measurement device HLC-8320 (manufactured by Tosoh Corporation). A differential refractometer (RI) was used as a detector. The measurements were performed under the following conditions: separation column temperature: 40°C, mobile phase: tetrahydrofuran, mobile phase flow rate: 0.6 mL / min, sample injection amount: 10 μL. A calibration curve was prepared using polymethyl methacrylate (manufactured by Polymer Laboratories) with a known molecular weight and a peak molecular weight of 1,560 to 19,500,000 as the standard polymer, and Mn, Mw and Mw / Mn were determined.

[0112] (glass transition temperature) The glass transition temperature of the acrylic resin was measured in the same manner as for the polycarbonate resin.

[0113] <Measurement of resin composition> (glass transition temperature) The glass transition temperature of the resin composition was measured in the same manner as for the polycarbonate resin.

[0114] (Haze) Approximately 4 g of a resin sample that had been dried in a vacuum dryer at 90°C for more than 5 hours was placed in a mold 7 cm long, 7 cm wide, and 0.5 mm thick, with polyimide films laid on the top and bottom of the sample, preheated at 210-230°C for approximately 3 minutes, pressurized at 10 MPa for approximately 3 minutes, removed from the mold, and cooled to produce a sheet. The haze of the sheet molded product was measured using a haze meter NDH4000 (manufactured by Nippon Denshoku Industries Co., Ltd.) under a D65 light source in accordance with JIS K7136.

[0115] <Measurement of unstretched film> (Forming of unstretched film) Approximately 4 g of a resin sample that had been dried in a hot air dryer at 100°C for more than 6 hours was placed in a mold 14 cm long, 14 cm wide, and 0.1 mm thick. Polyimide films were placed on the top and bottom of the sample, and the sample was preheated at a temperature of 210 to 230°C for 3 minutes and pressurized at a pressure of 10 MPa for 5 minutes. The mold was then removed and cooled to produce an unstretched film.

[0116] (Photoelastic Coefficient) The measurements were performed using a combination of a birefringence measuring device consisting of a He-Ne laser, a polarizer, a compensator, an analyzer, and a photodetector, and a vibration type viscoelasticity measuring device (DVE-3 manufactured by Rheology Co., Ltd.) (for details, see Journal of the Society of Rheology, Japan, Vol. 19, p. 93-97 (1991)). A sample with a width of 5 mm and a length of 20 mm was cut out from the unstretched film produced by the above-mentioned method, and fixed to the viscoelasticity measuring device, and the storage modulus E' was measured at a frequency of 96 Hz at room temperature of 25°C. At the same time, the emitted laser light was passed through the polarizer, the sample, the compensator, and the analyzer in that order, and picked up by a photodetector (photodiode). The amplitude and phase difference with respect to the strain were obtained for the waveform of angular frequency ω or 2ω through a lock-in amplifier, and the strain optical coefficient O' was obtained. At this time, the directions of the absorption axes of the polarizer and the analyzer were adjusted to be perpendicular to each other and to form an angle of π / 4 with respect to the stretching direction of the sample. The photoelastic coefficient C was calculated from the storage modulus E' and the strain optical coefficient O' according to the following formula. C=O' / E' The smaller the photoelastic coefficient, the less likely the film is to exhibit birefringence when stress is applied to it, and the higher the quality and reliability of the device incorporating the film.

[0117] (Stretchability (maximum stretching ratio)) A film piece measuring 70 mm in length and 100 mm in width was cut out from the unstretched film produced by the above-mentioned method, and free-end uniaxial stretching was performed using a batch-type biaxial stretching device (Island Industrial Co., Ltd. BIX-277-AL) to obtain a stretched film. The stretching conditions were an oven temperature set to the glass transition temperature of the resin + 20°C, a stretching speed of 250% / min, and a stretching ratio of 2 times. If stretching was successful under these conditions, the stretching ratio was gradually increased to 2.1 times, 2.2 times, and so on, and stretching was repeated until the stretching ratio at which the film broke was reached. The stretching ratio just before the stretching ratio at which the film broke was taken as the maximum stretching ratio. The higher this ratio, the better the stretching.

[0118] <Measurement of stretched film> (Phase difference, birefringence (Δn)) The stretched film was stretched by the above method, and the central part of the stretched film obtained at a stretch ratio of 2.6 was cut out to a width of 4 cm and a length of 4 cm. The retardation was measured using a retardation measuring device (KOBRA-WPR manufactured by Oji Scientific Instruments). The birefringence (Δn) was calculated from the following formula using the retardation at 590 nm (R590) and the thickness of the retardation film. Birefringence (Δn) = R590 [nm] / (film thickness [mm] × 10 6 ) In applications where low birefringence is required, the smaller this birefringence value, the more preferable.

[0119] [Raw materials used] The abbreviations and manufacturers of the compounds used in the following Examples and Production Examples are as follows.

[0120] ISB: Isosorbide (manufactured by Rocket Fleuret) CHDM: 1,4-cyclohexanedimethanol (SK Chemical) DPC: Diphenyl carbonate (manufactured by Mitsubishi Chemical Corporation) Phosphonic acid (Tokyo Chemical Industry Co., Ltd.) Irganox 1010: Pentaerythritol-tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] (BASF) CHMA: Cyclohexyl methacrylate (Mitsubishi Chemical Corporation) HEMA: 2-hydroxyethyl methacrylate (manufactured by Mitsubishi Chemical Corporation) ·MA: Methyl acrylate (manufactured by Mitsubishi Chemical Corporation) AMBN: 2,2'-azobis(2-methylbutyronitrile) (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.), product name V59 Sodium sulfate (Tokyo Chemical Industry Co., Ltd.) 1-Octanethiol (Tokyo Chemical Industry Co., Ltd.) Dispersants

[0121] An aqueous dispersant solution containing 8% by weight of polymer was prepared by the method described in WO 2022 / 114157 and used as a dispersant for suspension polymerization.

[0122] <Production example 1 / Reference example 1> PC-1 Polycarbonate resin was polymerized using a continuous polymerization system consisting of three vertical stirring reactors, one horizontal stirring reactor, and a twin-screw extruder. ISB, CHDM, and DPC were melted in tanks and continuously fed to the first vertical stirring reactor at flow rates of 38.3 kg / hr for ISB, 4.2 kg / hr for CHDM, and 62.9 kg / hr for DPC (molar ratio ISB / CHDM / DPC=0.900 / 0.100 / 1.010). At the same time, an aqueous solution of calcium acetate monohydrate, a polymerization catalyst, was fed to the first vertical stirring reactor in an amount such that 1.5 μmol of calcium acetate monohydrate was added to 1 mol of all dihydroxy compounds. The internal temperature, internal pressure, and residence time of each reactor were respectively: first vertical stirring reactor: 190°C, 25kPa, 120 minutes, second vertical stirring reactor: 195°C, 10kPa, 90 minutes, third vertical stirring reactor: 205°C, 4kPa, 45 minutes, fourth horizontal stirring reactor: 230°C, 0.1-1.0kPa, 120 minutes. The internal pressure of the fourth horizontal stirring reactor was finely adjusted so that the reduced viscosity of the resulting polycarbonate resin was 0.45dL / g. The polycarbonate resin extracted from the fourth horizontal stirring reactor was supplied in a molten state to a vented twin-screw extruder TEX30α (manufactured by Japan Steel Works, Ltd.). The extruder had three vacuum vents, where residual low molecular weight components in the resin were removed by volatilization, and phosphonic acid was added as a catalyst deactivator just before the first vent at 0.64 ppm by weight relative to the polycarbonate resin, and Irganox 1010 was added just before the third vent at 1000 ppm by weight relative to the polycarbonate resin. The polycarbonate resin that had passed through the extruder was still in a molten state and passed through a 10 μm Ultipleats candle filter (PALL) to filter out foreign matter. The polycarbonate resin was then extruded in a strand shape from the die, cooled with water, solidified, and cut with a rotary cutter to pelletize. The polycarbonate resin thus obtained was designated "PC-1". The analysis results of this polycarbonate resin are shown in Table 1 as Reference Example 1.

[0123] <Production example 2 / Reference example 2> PC-2 The same procedure as in Production Example 1 was repeated except that the raw materials were fed at flow rates of ISB 29.8 kg / hr, CHDM 12.6 kg / hr, and DPC 62.9 kg / hr (ISB / CHDM / DPC=0.700 / 0.300 / 1.008 in molar ratio). The analysis results of this polycarbonate resin are shown in Table 1 as Reference Example 2.

[0124] [Table 1]

[0125] <Production Example 3 / Reference Example 3> Acrylic-1 In a polymerization apparatus equipped with a stirrer, a cooling tube, and a thermometer, 450 parts of deionized water, 0.1 parts of sodium sulfate, and 1 part of a dispersant aqueous solution were added and stirred to obtain a uniform aqueous solution. Next, 198 parts of CHMA, 2 parts of MA, 0.1 parts of 1-octanethiol, and 0.2 parts of AMBN as a polymerization initiator were added and stirred to obtain an aqueous dispersion. Next, the inside of the polymerization apparatus was fully replaced with nitrogen, and the aqueous dispersion was heated to 75°C and held for 3 hours, and then heated to 90°C and held for 1 hour. Thereafter, the reaction solution was cooled to 40°C to obtain an aqueous suspension of an acrylic resin. This aqueous suspension was filtered with a filter cloth, and the filtrate was washed with deionized water and dried in a hot air dryer at 60°C for 10 hours to obtain an acrylic resin (Acryl-1). The analysis results of this acrylic resin are shown in Table 2 as Reference Example 3.

[0126] <Production Example 4 / Reference Example 4> Acrylic-2 An acrylic resin (Acryl-2) was obtained in the same manner as in Production Example 3, except that 178 parts of CHMA, 20 parts of HEMA, and 2 parts of MA were used. The analysis results of this acrylic resin are shown in Table 2 as Reference Example 4.

[0127] <Reference Example 5> Acryl-3 Acrypet VH001 (manufactured by Mitsubishi Chemical Corporation) was used. The analysis results of this acrylic resin are shown in Table 2 as Reference Example 5.

[0128] [Table 2]

[0129] <Example 1> 90 parts by weight of PC-1 and 10 parts by weight of Acryl-1 were blended and dried in a vacuum dryer at 90°C for 5 hours or more, and then melt-kneaded for 3 minutes at a temperature of 220°C and a screw rotation speed of 100 rpm using a kneading device, Labo Plastomill (manufactured by Toyo Seiki Seisakusho Co., Ltd.) to obtain a resin composition. The obtained resin composition was subjected to the various evaluations described above. The results are shown in Table 3.

[0130] <Examples 2 to 3, Comparative Examples 1 to 4> A resin composition was obtained in the same manner as in Example 1, except that the formulation was as shown in Table 3. The obtained resin composition was subjected to the above-mentioned various evaluations. The results are shown in Table 3. Note that for Comparative Example 3, the haze of the molded product was large, so that it was not possible to measure Δn and the photoelastic coefficient.

[0131] [Table 3]

[0132] From the above results, it was found that the optical films of the present invention are excellent in transparency, glass transition temperature, birefringence, and stretchability (Examples 1 to 3). In contrast, the optical films of the comparative examples are inferior in performance to the examples, with one or more of haze, glass transition temperature, birefringence, and photoelastic coefficient being outside the preferred range (Comparative Examples 1 to 4). [Industrial Applicability]

[0133] Since the optical film of the present invention has both high heat resistance and low birefringence, it is particularly suitable for use as a polarizing plate protective film, a display front protective film, and the like.

Claims

1. A polycarbonate resin containing 65% by weight or more and 90% by weight or less of a structural unit represented by the following formula (1): and an acrylic resin containing 50% by weight or more and 100% by weight or less of a (meth)acrylate structural unit represented by the following formula (2): [Formula 1] [chemical 2] (In formula (2), R 1 R is a hydrogen atom or an alkyl group having 1 to 10 carbon atoms which may have a substituent. 2 represents an alkyl group or cycloalkyl group containing a cyclohexane structure and which may further have a substituent.)

2. The optical film according to claim 1 , wherein the polycarbonate resin has a glass transition temperature of 130° C. or more and 160° C. or less.

3. 3. The optical film according to claim 1, wherein the polycarbonate resin contains a structural unit derived from an aliphatic dihydroxy compound or an alicyclic dihydroxy compound.

4. The optical film according to claim 1 , wherein the acrylic resin has a weight average molecular weight (Mw) of 10,000 or more and 500,000 or less.

5. 5. The optical film according to claim 1, wherein the acrylic resin contains 0.1% by weight or more and 10% by weight or less of an acrylate structural unit represented by the following formula (3): [C3] (In formula (3), R 3 is a hydrogen atom, an alkyl group having 1 to 10 carbon atoms which may have a substituent, a cycloalkyl group, or an aryl group.

6. 5. The optical film according to claim 1, comprising 50% by weight or more and 99% by weight or less of the polycarbonate resin and 1% by weight or more and 50% by weight or less of the acrylic resin.

7. A polarizing plate comprising the optical film according to claim 1 , 2 or 4 and a linear polarizer, which are laminated together.

Citation Information

Patent Citations

  • Polymer composition

    JP1993009359A

  • Methacrylic copolymer, method for producing the same, and methacrylic resin composition using the same

    JP2011500914A

  • Resin composition

    JP2015232091A

  • Resin composition, and film comprising resin composition

    JP2018131587A

  • Polycarbonate resin composition and molded article

    JP2021088651A