Method for producing carbon dioxide-fixed hydraulic hardened body

By employing a non-cement kneading process with CO2-absorbing materials and additives, followed by a cement kneading step, the method effectively addresses the slump reduction issue in CO2 fixation, achieving enhanced CO2 absorption and strength in hydraulic cured bodies.

JP2024169084APending Publication Date: 2024-12-05KAJIMA CORP
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2023086273
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-25
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

Existing methods for fixing carbon dioxide in concrete result in significant reduction of slump due to cement hydration reactions, limiting the amount of CO2 that can be fixed and requiring prolonged standing times, which further decreases slump.

Method used

A method involving a non-cement kneading step with a carbon dioxide-absorbing mixture containing water reducers and additives, followed by a cement kneading step to produce a fluid composition, which is then hardened to form a carbon dioxide-immobilized hydraulic cured body, using absorbents like γ-C2S, blast furnace slag, and fly ash.

Benefits of technology

This method significantly suppresses the decrease in slump of the fluid composition and enhances CO2 fixation, allowing for higher CO2 absorption and improved compressive strength of the hydraulic cured body.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024169084000001_ABST
    Figure 2024169084000001_ABST
Patent Text Reader

Abstract

To provide a method for producing a carbon dioxide-fixed hydraulic hardened body with a high CO2 fixation amount, capable of suppressing a slump decrease in a fluid composition accompanying the supply of a CO2 source.SOLUTION: A method according to the present invention for producing a carbon dioxide-fixed hydraulic hardened body includes: a non-cement kneading step of kneading a cement-free CO2 absorbent that absorbs CO2 and does not contain cement, a CO2 source, and an additive comprising one or more selected from the group consisting of a water-reducing agent, an AE agent, and a high-performance AE water-reducing agent, to obtain a carbon dioxide-fixed non-cement kneaded material in which the carbon dioxide is fixed; a cement kneading step of kneading the carbon dioxide-fixed non-cement kneaded material obtained in the non-cement kneading step with cement to obtain a fluid composition; and a hardening step of casting and hardening the fluid composition obtained in the cement kneading step to obtain a carbon dioxide-fixed hydraulic hardened body.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing a carbon dioxide gas-immobilized hydraulic hardened product. [Background technology]

[0002] The cement used in concrete emits large amounts of carbon dioxide (carbon dioxide, CO2) during its production due to fuel combustion and decarbonation reactions, and therefore the CO2 emission intensity of concrete is large. In recent years, with the growing threat of global warming and climate change, there has been a demand for innovative and easy-to-apply methods to efficiently fix CO2 in concrete.

[0003] There are various methods for fixing CO2 in concrete, such as carbon dioxide gas and dry ice, which are methods for supplying a CO2 source. For example, Patent Document 1 describes a method for producing a cement composition that contains cement, fine aggregate, and water and fixes carbon dioxide. The method for producing a cement composition in Patent Document 1 includes a first mixing step in which a predetermined amount of cement, a predetermined amount of fine aggregate, a predetermined amount of water, and dry ice, which is a CO2 source, are mixed while stirring to obtain a cement-containing mixture, a settling step in which the cement-containing mixture is left to stand for a predetermined time to obtain a mixture, and a second mixing step in which the mixture, the remainder of the cement, the remainder of the fine aggregate, and the remainder of the water are mixed while stirring to obtain a cement composition.

[0004] However, when a CO2 source is supplied to the cement component as in Patent Document 1, the slump of the flowable composition such as the above-mentioned cement-containing mixture is significantly reduced due to the reaction between the cement and CO2 in addition to the setting associated with the hydration reaction of the cement, making it difficult to obtain the desired fresh properties of the flowable composition. In addition, in order to suppress the reduction in slump, the amount of the CO2 source supplied to the cement component must be reduced, and as a result, there is a limit to the amount of CO2 fixed in the hydraulic hardened body such as concrete. Furthermore, in Patent Document 1, a standing step must be performed for a predetermined time to fix CO2 in the cement component, so that a waiting time must be performed, and further reduction in slump progresses during standing, resulting in a further reduction in slump. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2023-18308 A Summary of the Invention [Problem to be solved by the invention]

[0006] An object of the present invention is to provide a method for producing a carbon dioxide gas-immobilized hydraulic hardened body which can fix a large amount of CO2 and suppress a decrease in slump of a flowable composition caused by the supply of a CO2 source. [Means for solving the problem]

[0007] [1] A method for producing a carbon dioxide-immobilized hydraulic hardened body, comprising: a non-cement kneading step of kneading non-cement components containing a cement-free CO2 absorbent that absorbs CO2 and does not contain cement, a CO2 source, and an additive containing one or more selected from the group consisting of a water reducing agent, an air entraining agent, and a high-performance air entraining water reducing agent, to obtain a carbon dioxide-immobilized non-cement kneaded product in which carbon dioxide is immobilized; a cement kneading step of kneading the carbon dioxide-immobilized non-cement kneaded product obtained in the non-cement kneading step with cement to obtain a flowable composition; and a hardening step of pouring and hardening the flowable composition obtained in the cement kneading step to obtain a carbon dioxide-immobilized hydraulic hardened body. [2] The method for producing a carbon dioxide-immobilized hydraulic hardened body described in [1] above, wherein the cement-free CO2 absorbent contains one or more selected from the group consisting of γ-C2S, ground granulated blast furnace slag, steelmaking slag and fly ash. [3] The method for producing a carbon dioxide gas-immobilized hydraulic hardened body according to the above [1] or [2], wherein the CO2 source is dry ice. [4] The method for producing a carbon dioxide gas immobilized hydraulic hardened body according to any one of the above [1] to [3], wherein the non-cement components further include aggregate. [5] The method for producing a carbon dioxide gas-immobilized hydraulic hardened material according to any one of the above [1] to [4], wherein in the non-cement kneading step, the non-cement components are kneaded with water to obtain the carbon dioxide gas-immobilized non-cement kneaded product. [6] The method for producing a carbon dioxide-immobilized hydraulic hardened product according to any one of the above [1] to [5], wherein in the cement kneading step, in addition to the carbon dioxide-immobilized non-cement kneaded product and cement, at least one of water and the additive is further kneaded to obtain the flowable composition. [7] The method for producing a carbon dioxide-immobilized hydraulic hardened product according to any one of the above [1] to [5], wherein in the cement kneading step, water and the additive are added to a cement kneaded product obtained by kneading the carbon dioxide-immobilized non-cement kneaded product, cement, water and the additive, and the flowable composition is obtained by kneading the mixture. Effect of the Invention

[0008] According to the present invention, a method for producing a carbon dioxide gas fixed hydraulic hardened body can be provided, which fixes a large amount of CO2 and can suppress a decrease in slump of a flowable composition that accompanies the supply of a CO2 source. [Brief description of the drawings]

[0009] [Figure 1] FIG. 1 is a flow chart showing an example of a method for producing a carbon dioxide gas-immobilized hydraulic hardened material according to an embodiment. [Diagram 2] FIG. 2 is a graph showing the results of a slump test carried out on the flowable compositions of Example 1 and Comparative Examples 1, 3 and 4. [Diagram 3] FIG. 3 is a graph showing the ratio of the compressive strength of Example 1 and Comparative Examples 2 to 4 to the compressive strength of Comparative Example 1. [Figure 4] FIG. 4 is a graph showing the results of measuring the amount of CO2 fixed in the hydraulic hardened products of Examples 2 to 4 and Comparative Example 5 and the flowable composition of Comparative Example 6. [Diagram 5] FIG. 5 is a graph showing the results of measuring the amount of CO2 fixed in γ-C2S or ground granulated blast furnace slag. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] Hereinafter, a detailed description will be given based on an embodiment.

[0011] As a result of extensive research, the inventors have found that by kneading cement with a carbon dioxide fixation non-cement mixture obtained by kneading a non-cement component containing a cement-free CO2 absorbent, a CO2 source, and an additive, a large amount of CO2 is fixed in the hydraulic hardened body and a decrease in slump of the flowable composition due to the supply of a CO2 source can be suppressed, and the present disclosure has been completed based on this finding.

[0012] The method for producing a carbon dioxide-immobilized hydraulic hardened body of the present invention includes a non-cement kneading step of kneading non-cement components containing a cement-free CO2 absorbent that absorbs CO2 and does not contain cement, a CO2 source, and an additive containing one or more selected from the group consisting of a water-reducing agent, an air-entraining agent, and a high-performance air-entraining water-reducing agent, to obtain a carbon dioxide-immobilized non-cement kneaded product in which carbon dioxide is immobilized; a cement kneading step of kneading the carbon dioxide-immobilized non-cement kneaded product obtained in the non-cement kneading step with cement to obtain a flowable composition; and a hardening step of pouring and hardening the flowable composition obtained in the cement kneading step to obtain a carbon dioxide-immobilized hydraulic hardened body.

[0013] The method for producing a carbon dioxide gas-immobilized hydraulic hardened material (hereinafter, simply referred to as a hydraulic hardened material) of the present invention includes a non-cement kneading step S10, a cement kneading step S20, and a hardening step S30. The hydraulic hardened material produced by this method is concrete or mortar in which carbon dioxide gas is immobilized.

[0014] In the non-cement mixing step S10 in the manufacturing method of the carbon dioxide gas immobilized hydraulic hardened body, non-cement components not containing cement are mixed to obtain a carbon dioxide gas immobilized non-cement mixture in which carbon dioxide gas (CO2) is immobilized. The non-cement components include a cement-free CO2 absorbent, a CO2 source, and additives.

[0015] The cement-free CO2 absorbent contained in the non-cement component does not contain cement. Furthermore, the cement-free CO2 absorbent absorbs CO2, is carbonated, and fixes CO2. From the viewpoint of increasing the amount of carbon dioxide fixed in the hydraulic hardened body, the cement-free CO2 absorbent preferably contains one or more selected from the group consisting of γ-C2S (γ-2CaO·SiO2, also called γ-belite), ground granulated blast furnace slag, steelmaking slag, and fly ash, more preferably contains γ-C2S, and even more preferably is γ-C2S.

[0016] By replacing part of the cement mixed with the carbon dioxide gas fixation non-cement mixture in the cement mixing step S20 described below with a cement-free CO2 absorbent, the amount of cement used can be reduced. This allows for a reduction in the amount of cement used, which emits a lot of CO2 during production, and therefore a reduction in CO2 emissions. Furthermore, the inclusion of γ-C2S can increase the compressive strength of the hydraulic hardened body, which also reduces the amount of cement used.

[0017] Ground granulated blast furnace slag is a fine powder as specified in JIS A 6206:2013 "Ground granulated blast furnace slag for concrete". Granulated blast furnace slag is made by quenching molten blast furnace slag, which is produced at the same time as shear iron in a blast furnace, with water or air, and has a basicity of 1.60 or more. Ground granulated blast furnace slag is made by drying and pulverizing this granulated blast furnace slag, or by adding gypsum to it. By replacing part of the Portland cement with ground granulated blast furnace slag, it is possible to reduce carbon dioxide emissions during the cement manufacturing stage.

[0018] The properties of the CO2 source contained in the non-cement component are not particularly limited as long as it contains CO2. For example, the CO2 source may be gaseous CO2 (carbon dioxide gas), liquid CO2 (liquefied carbon dioxide, liquid carbon dioxide gas), solid CO2 (dry ice), a gas containing CO2, a liquid containing CO2, or a solid containing CO2. An example of a liquid containing CO2 is an aqueous solution containing CO2 (carbonated water). An example of a solid containing CO2 is carbonated ice. One type of CO2 source may be used, or two or more types may be used in combination. As described later, when the CO2 source is an aqueous solution containing CO2, CO2 can be efficiently fixed in the non-cement-containing CO2 absorbent.

[0019] In addition, when the CO2 source is dry ice or a solid containing CO2, a CO2 source container may be used that is made of a water-soluble material and contains the CO2 source inside. The CO2 source container may further contain a non-cement-containing CO2 absorbent. When the CO2 source container is dissolved by the moisture in the non-cement component, the contained CO2 source and other contained items are released.

[0020] The lower limit of the ratio of the CO2 source to the total weight of the cement-free CO2 absorbent and the cement is preferably 0.3% or more, more preferably 0.6% or more, and even more preferably 1.0% or more, and the upper limit is preferably 20.0% or less, more preferably 10.0% or less, and even more preferably 5.0% or less. When the CO2 source ratio is 0.3% or more, a sufficient amount of CO2 can be fixed in the hydraulic hardened body. Also, when the CO2 source ratio is 20.0% or less, the slump decrease of the flowable composition due to the supply of the CO2 source can be suppressed.

[0021] In addition, from the viewpoint of efficiently reducing CO2 in the atmosphere, the source of CO2 is preferably exhaust gas from a thermal power plant, exhaust gas from a boiler, exhaust gas containing CO2 emitted in the manufacturing process of other products, high-concentration CO2 gas in which the CO2 concentration in the exhaust gas has been increased, etc. In addition, the humidity and temperature of these gases may be adjusted.

[0022] When the hydraulically set body is concrete, the non-cement components further include aggregate. The aggregate includes at least one of fine aggregate and coarse aggregate.

[0023] Fine aggregate is an aggregate defined in JIS A 5308, JIS A 5005, JIS A 5002 and JIS A 5011. Examples of fine aggregate include crushed sand, sand, river sand, sea sand, crushed lime sand, recycled aggregate, lightweight aggregate, heavy aggregate and the like.

[0024] Coarse aggregate is defined in JIS A 5308, JIS A 5005, JIS A 5002 and JIS A 5011. It is distinguished from the above fine aggregates by the size of the particles, and is classified by whether it passes through a 5mm sieve or not. In practice, fine aggregate is defined as aggregate that passes entirely through a 10mm sieve and 85% or more of its weight passes through a 5mm sieve, and coarse aggregate is defined as aggregate that is 85% or more of its weight retained on a 5mm sieve.

[0025] When the cement-free CO2 absorbent or aggregate in the non-cement component is wet with water, i.e., when the cement-free CO2 absorbent or aggregate contains water, or when the CO2 source contains water, such as an aqueous solution containing CO2, the cement-free CO2 absorbent is ionized by the water in the non-cement component, and can fix (carbonate) CO2 efficiently in a short period of time.

[0026] When the non-cement component contains little water or no water, adding water to the non-cement component increases the amount of cement-free CO2 absorbent that ionizes, so the carbon dioxide gas immobilizing non-cement mixture can fix more CO2 in a short time. In other words, by mixing the non-cement component with water, the amount of CO2 fixed in the carbon dioxide gas immobilizing non-cement mixture can be increased.

[0027] The additives contained in the non-cement component include one or more selected from the group consisting of a water reducing agent, an air entraining agent, and a high-performance air entraining water reducing agent. The additives suppress a decrease in the slump of the flowable composition caused by a reaction between the cement and CO2 that is not fixed (carbonated) in the non-cement-containing CO2 absorbent, among the CO2 contained in the carbon dioxide gas immobilized non-cement kneaded product, in the cement kneading step S20 described later.

[0028] Furthermore, so long as there is no decrease in the slump of the flowable composition and no decrease in the amount of CO2 fixed in the hydraulic hardened body, the carbon dioxide gas immobilizing non-cement kneaded product may contain various optional components in addition to the above-mentioned cement-free CO2 absorbent, CO2 source, additives and aggregate, depending on the desired properties of the flowable composition and hydraulic hardened product. In the non-cement kneading step S10, the optional components may be kneaded together with the non-cement components, or the optional components may be added to the carbon dioxide gas immobilizing non-cement kneaded product and kneaded.

[0029] In the cement mixing step S20 carried out after the non-cement mixing step S10, the carbon dioxide gas fixed non-cement mixture obtained in the non-cement mixing step S10 is mixed with cement to obtain a flowable composition. The flowable composition is a cement composition and has flowability.

[0030] The cement used in the cement mixing step S20 is preferably Portland cement. Portland cement includes ordinary Portland cement (OPC), as well as early strength, super early strength, moderate heat, low heat, sulfate resistance, and other types, which are specified in JIS R 5210:2019. In the fluid composition, one or more of these various Portland cements may be blended. Among these, it is preferable to use one or two of ordinary Portland cement and early strength Portland cement.

[0031] The water contained in the carbon dioxide gas fixed non-cement mixture obtained in the non-cement mixing step S10 reacts with the cement to cause a hydration reaction. When the water content in the carbon dioxide gas fixed non-cement mixture is low, water may be added before or during the cement mixing step S20.

[0032] The CO2 that is fixed in the flowable composition includes CO2 that is fixed in a cement-free CO2 absorbent and CO2 that is fixed in cement.

[0033] In the cement mixing step S20, the CO2 contained in the carbon dioxide fixation non-cement mix that is not fixed in the cement-free CO2 absorbent reacts with the cement, and the CO2 is fixed in the cement. Meanwhile, when the CO2 reacts with the cement, the slump of the flowable composition decreases.

[0034] Here, in the conventional technology such as Patent Document 1, CO2 is supplied to a system containing cement. On the other hand, in the present invention, CO2 is fixed in a cement-free CO2 absorbent in a non-cement kneading step S10. However, if all of the CO2 is not fixed in the cement-free CO2 absorbent, the CO2 that is not fixed in the cement-free CO2 absorbent reacts with cement in the subsequent cement kneading step S20.

[0035] Thus, the present invention and the prior art differ in the object to which the CO2 source is supplied. Furthermore, compared to the present invention, in the prior art where CO2 is supplied to a system containing cement, a large amount of cement reacts with CO2. Thus, in the present invention, the amount of cement that reacts with CO2 can be significantly reduced, so that a decrease in slump of the flowable composition can be suppressed. Furthermore, in the present invention, the carbon dioxide gas fixation non-cement kneaded product contains an additive, so that a decrease in slump of the flowable composition caused by a reaction between cement and CO2 can be further suppressed.

[0036] Furthermore, as long as there is no decrease in the slump of the flowable composition and no decrease in the amount of CO2 fixed in the hydraulic hardened body, the flowable composition may contain various optional components in addition to the carbon dioxide gas fixing non-cement mixture and cement described above, depending on the desired properties of the flowable composition and the hydraulic hardened body. In the cement kneading step S20, the optional components may be kneaded together with the carbon dioxide gas fixing non-cement mixture and cement, or the optional components may be added to the flowable composition and kneaded.

[0037] In addition, in the cement kneading step S20, in addition to the carbon dioxide gas fixed non-cement kneaded product and cement, water and at least one of the above-mentioned additives may be further kneaded to prepare a flowable composition. The above-mentioned additives are one or more selected from the group consisting of a water reducing agent, an air entraining agent, and a high-performance air entraining water reducing agent. Thus, in the present invention, water and additives may be supplied in the cement kneading step S20.

[0038] In addition, in the cement kneading step S20, water and additives may be added to the cement kneaded product obtained by kneading the carbon dioxide gas fixed non-cement kneaded product, cement, water, and the above-mentioned additives, and kneaded to prepare a flowable composition. In this way, in the present invention, water and additives may be supplied multiple times in the cement kneading step S20.

[0039] In the hardening step S30 carried out after the cement mixing step S20, the flowable composition obtained in the cement mixing step S20 is poured and hardened to obtain a carbon dioxide-fixed hydraulic hardened body. The flowable composition can be easily poured into a formwork in the same working process as a flowable composition that does not fix CO2. The method of hardening the flowable composition in the hardening step S30 is not particularly limited. For example, a known method used in the fields of concrete and mortar can be applied.

[0040] From the viewpoint of increasing the amount of CO2 fixed in the hydraulic hardened body and suppressing a decrease in the slump of the flowable composition, the CO2 source in the non-cement kneading step S10 is preferably dry ice. Also, from the same viewpoint, in this case, it is preferable to knead the non-cement components with water in the non-cement kneading step S10 to obtain a carbon dioxide gas fixed non-cement kneaded product.

[0041] According to the embodiment described above, by kneading cement with a carbon dioxide gas fixing non-cement mixture obtained by kneading a non-cement component containing a cement-free CO2 absorbent, a CO2 source, and an additive, the amount of CO2 fixed in the hydraulic hardened body is large and a decrease in slump of the flowable composition due to the supply of a CO2 source can be suppressed.

[0042] Although the embodiments have been described above, the present invention is not limited to the above embodiments, but includes all aspects included in the concept and scope of the claims of the present disclosure, and can be modified in various ways within the scope of the present disclosure. EXAMPLES

[0043] Next, examples and comparative examples will be described, but the present invention is not limited to these examples.

[0044] The raw materials used in the examples and comparative examples are shown in Table 1.

[0045] [Table 1]

[0046] Example 1 First, γ-CS (γ), dry ice (D), fine aggregate (S) and coarse aggregate (G) in the amounts shown in Table 2 were mixed for 20 seconds, and then tap water (W), water reducing agent (AD) and air entraining agent (AE) in amounts of 70% of the values ​​shown in Table 2 were added to the mixture and mixed for 30 seconds to obtain a carbon dioxide-immobilized non-cement mixture in which carbon dioxide had been immobilized.

[0047] Next, ordinary Portland cement (C) in the amounts shown in Table 2, as well as tap water, water reducing agent, and air entraining agent in amounts 15% of the values ​​shown in Table 2, were added to the carbon dioxide-fixed non-cement mixture, and the mixture was mixed for 60 seconds. Next, tap water, water reducing agent, and air entraining agent in amounts 15% of the values ​​shown in Table 2 were added to the mixture, and the mixture was mixed for 30 seconds to obtain a flowable composition. Next, the flowable composition was cast into a formwork, and sealed cured for 7 days to obtain a carbon dioxide-fixed hydraulic hardened body. As shown in Table 2, the amount of dry ice was 0.6% of the powder amount P (the total weight of C and γ).

[0048] (Comparative Examples 1 to 2) A flowable composition was obtained by kneading the raw materials shown in Table 2. Next, the flowable composition was cast into a formwork and sealed and cured for 7 days to obtain a hydraulically hardened body. That is, in Comparative Examples 1 and 2, no CO2 source was used and no forced CO2 addition was performed.

[0049] Comparative Example 3 First, ordinary Portland cement, fine aggregate, and coarse aggregate in the amounts shown in Table 2 were mixed for 30 seconds. Next, tap water, dry ice, water reducing agent, and AE agent in the amounts shown in Table 2 were added to the cement mixture and mixed for 60 seconds to obtain a flowable composition with fixed carbon dioxide. Next, the flowable composition was cast into a formwork and sealed and cured for 7 days to obtain a carbon dioxide-fixed hydraulic hardened body. That is, in Comparative Example 3, water and a CO2 source were added simultaneously to the cement mixture. Also, in Comparative Example 3, no cement-free CO2 absorbent was used.

[0050] Comparative Example 4 First, ordinary Portland cement, fine aggregate, and coarse aggregate in the amounts shown in Table 2 were mixed for 30 seconds. Next, tap water, water reducing agent, and AE agent in the amounts shown in Table 2 were added to the cement mixture and mixed for 60 seconds. Next, dry ice and γ-C2S in the amounts shown in Table 2 were added to the cement mixture and mixed for 30 seconds to obtain a flowable composition with fixed carbon dioxide. Next, the flowable composition was cast into a formwork and sealed and cured for 7 days to obtain a carbon dioxide-fixed hydraulic hardened body. That is, in Comparative Example 4, water was added to the cement mixture, and then a CO2 source was added. Also, in Comparative Example 4, a CO2 source and a cement-free CO2 absorbent were added simultaneously.

[0051] For Example 1 and Comparative Examples 1, 3 and 4, a slump test was conducted on the flowable compositions in accordance with JIS A 1101:2005 "Slump test method for concrete" to evaluate the fresh properties of the flowable compositions, and the results are shown in Figure 2. As shown in Figure 2, Example 1, in which cement was added to a carbon dioxide gas immobilized non-cement mixture in which carbon dioxide gas was immobilized, was able to suppress a decrease in slump, compared to Comparative Example 3, in which water and a CO2 source were added simultaneously to a cement mixture, and Comparative Example 4, in which water was added to a cement mixture and then a CO2 source was added.

[0052] In addition, the hydraulic hardened bodies of Example 1 and Comparative Example 1 were subjected to thermogravimetric analysis to measure the amount of CO2 fixed in the hydraulic hardened bodies. As a result, the amount of CO2 fixed in the hydraulic hardened body of Example 1 was greater than that of Comparative Example 1.

[0053] In addition, the compressive strength of the hydraulic hardened bodies of Example 1 and Comparative Examples 1 to 4 was measured according to JIS A 1108:2018 "Method of testing compressive strength of concrete", and the results are shown in Table 2. The compressive strength of Comparative Example 1 (32.3 N / mm 2 The ratio of compressive strength of Example 1 and Comparative Examples 2 to 4 to the total amount of cement is shown in Figure 3. As shown in Table 2 and Figure 3, comparing Example 1 and Comparative Examples 3 and 4 in which a CO2 source was added, the compressive strength of Example 1 was the highest. Furthermore, the compressive strength of Example 1 was equivalent to that of Comparative Example 1 in which no CO2 source was added and in which the amount of cement was large.

[0054] [Table 2]

[0055] (Examples 2 to 4) In Examples 2 to 4, the properties of hydraulic hardened bodies obtained by changing the amount of dry ice were investigated.

[0056] First, γ-CS and dry ice in the amounts shown in Table 3 were mixed for 20 seconds, and then tap water, a water reducing agent and an air entraining agent in amounts 70% of the values ​​shown in Table 3 were added to the mixture and mixed for 30 seconds to obtain a carbon dioxide-immobilized non-cement mixture in which carbon dioxide had been immobilized.

[0057] Next, ordinary Portland cement in the amounts shown in Table 3, as well as tap water, a water reducing agent, and an air entraining agent in amounts 15% of the values ​​shown in Table 3, were added to the carbon dioxide-fixed non-cement mixture, and the mixture was kneaded for 60 seconds. Next, tap water, a water reducing agent, and an air entraining agent in amounts 15% of the values ​​shown in Table 3 were added to the mixture, and the mixture was kneaded for 30 seconds to obtain a flowable composition. Next, the flowable composition was cast into a formwork and sealed and cured for 7 days to obtain a carbon dioxide-fixed hydraulic hardened body.

[0058] Comparative Example 5 In Comparative Example 5, the properties of the hydraulic hardened body obtained without using dry ice were investigated. First, γ-C2S in the amounts shown in Table 3, tap water in amounts of 70% of the values ​​shown in Table 3, a water reducing agent, and an air-enhancing agent were mixed for 30 seconds to obtain a non-cement mixture.

[0059] Next, ordinary Portland cement in the amounts shown in Table 3, as well as tap water, water reducing agent, and air entraining agent in amounts 15% of the values ​​shown in Table 3, were added to the non-cement mixture, and the mixture was kneaded for 60 seconds. Next, tap water, water reducing agent, and air entraining agent in amounts 15% of the values ​​shown in Table 3 were added to the mixture, and the mixture was kneaded for 30 seconds to obtain a fluid composition. Next, this fluid composition was cast into a formwork, and sealed cured for 7 days to obtain a hydraulic hardened body. That is, in Comparative Example 5, no CO2 source was used, and no forced CO2 addition was performed.

[0060] Comparative Example 6 In Comparative Example 6, the properties of a flowable composition obtained without using cement were investigated. First, γ-C2S and dry ice in the amounts shown in Table 3 were mixed for 20 seconds, and then tap water, a water reducing agent, and an AE agent in amounts 70% of the values ​​shown in Table 3 were added to the mixture, which was then mixed for 30 seconds to obtain a carbon dioxide gas-immobilized non-cement mixture in which carbon dioxide gas had been immobilized.

[0061] Next, tap water, a water reducing agent, and an air entraining agent in amounts 15% of the values ​​shown in Table 3 were added to the carbon dioxide-fixed non-cement mixture, and the mixture was kneaded for 60 seconds. Next, tap water, a water reducing agent, and an air entraining agent in amounts 15% of the values ​​shown in Table 3 were added to the mixture, and the mixture was kneaded for 30 seconds to obtain a flowable composition.

[0062] [Table 3]

[0063] The flowable composition was subjected to a slump test and the hydraulically hardened body was subjected to compressive strength measurement in the same manner as in Example 1. As a result, in Examples 2 to 4, the decrease in slump could be suppressed in the same manner as in Example 1. Furthermore, in Examples 2 to 4, the compressive strength was excellent in the same manner as in Example 1.

[0064] The hydraulic hardened bodies of Examples 2 to 4 and Comparative Example 5, and the flowable composition of Comparative Example 6 were subjected to thermogravimetric analysis to measure the amount of CO2 fixed in the hydraulic hardened bodies or the flowable composition, and the results are shown in Figure 4. As shown in Figure 4, by increasing the amount of the CO2 source as in Examples 2 to 4, the amount of CO2 fixed in the hydraulic hardened body could be increased.

[0065] Additionally, samples obtained by kneading the cement-free CO2 absorbent γ-C2S or ground granulated blast furnace slag with dry ice were subjected to thermogravimetric analysis to measure the amount of CO2 fixed in γ-C2S or ground granulated blast furnace slag. The results are shown in Figure 5. As shown in Figure 5, similar to γ-C2S, a large amount of CO2 could be fixed in the ground granulated blast furnace slag by kneading it with dry ice. Thus, it was found that CO2 can be fixed even when the type of cement-free CO2 absorbent is changed.

Claims

1. CO 2 Cement-free CO 2 An absorbent and CO 2 a non-cement kneading step of kneading a non-cement component containing a source and one or more additives selected from the group consisting of a water reducing agent, an air entraining agent, and a high-performance air entraining water reducing agent to obtain a carbon dioxide gas-immobilized non-cement kneaded product in which carbon dioxide gas is immobilized; a cement kneading step of kneading the carbon dioxide gas-immobilized non-cement kneaded product obtained in the non-cement kneading step with cement to obtain a flowable composition; a hardening step of casting and hardening the flowable composition obtained in the cement kneading step to obtain a carbon dioxide gas-immobilized hydraulic hardened body; The present invention relates to a method for producing a carbon dioxide gas immobilized hydraulic hardened body.

2. The cement-free CO 2 The absorbent is γ-C 2 2. The method for producing a carbon dioxide gas immobilized hydraulic hardened body according to claim 1, further comprising the step of: mixing the carbon dioxide gas immobilized hydraulic hardened body with the hydraulic hardened body;

3. The CO 2 2. The method for producing a carbon dioxide gas-immobilized hydraulic hardened body according to claim 1, wherein the source is dry ice.

4. The method for producing a carbon dioxide gas immobilized hydraulic hardened body according to claim 1 , wherein the non-cement components further include aggregate.

5. 2. The method for producing a carbon dioxide gas-immobilized hydraulic hardened body according to claim 1, wherein in the non-cement kneading step, the non-cement components are kneaded with water to obtain the carbon dioxide gas-immobilized non-cement kneaded product.

6. The method for producing a carbon dioxide gas-immobilized hydraulic hardened product according to any one of claims 1 to 5, wherein in the cement kneading step, in addition to the carbon dioxide gas-immobilized non-cement kneaded product and cement, at least one of water and the additive is further kneaded to obtain the flowable composition.

7. The method for producing a carbon dioxide-immobilized hydraulic hardened product according to any one of claims 1 to 5, wherein in the cement kneading step, water and the additive are added to a cement kneaded product obtained by kneading the carbon dioxide-immobilized non-cement kneaded product, cement, water and the additive, and the flowable composition is obtained by kneading the mixture.

Citation Information

Patent Citations

  • Method for solidification of fly ash

    JP2001259597A

  • Waterproof cement admixture and cement composition

    JP2012111640A

  • Landscaping products and manufacturing methods thereof

    JP2020500820A

  • Method for producing cement composition

    JP2023009794A

  • Production method of cement composition

    JP2023018308A