Three-dimensional QR code on surface of resin molded body, resin molding die, and method for manufacturing the same
By integrating a QR code as a concavo-convex aggregate of fine area cells on resin molded products through three-dimensional additive manufacturing and compression molding, the method addresses labor-intensive label application issues, enhancing information density and durability.
Patent Information
- Application Number
- JP2023096561
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-25
- Publication Date
- 2024-12-05
AI Technical Summary
Conventional methods for displaying information on resin molded products using barcodes or QR codes require additional processes like printing or pasting labels, which are labor-intensive and prone to environmental degradation, and are limited in durability and information capacity.
A method involving three-dimensional additive manufacturing and compression molding to directly form a QR code as a concavo-convex aggregate of fine area cells on a resin molding surface using a metal-resin composite powder, eliminating the need for manual label application and enhancing information density.
Enables direct integration of a QR code on resin molded products with increased information capacity and durability, reducing labor and equipment costs while maintaining shape fidelity and thermal conductivity.
Smart Images

Figure 2024169252000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a QR code that is three-dimensionally shaped as an uneven aggregate of fine area cells on a resin molding surface, a resin molding die that uses three-dimensional additive manufacturing and compression molding technology to form a block for imprinting the QR code using metal-resin composite powder, and a manufacturing method thereof. [Background technology]
[0002] Conventionally, as a means for indicating various information for production management on resin molded products, bar codes or QR codes have been printed on the surface of the molded product as a separate process after molding, or printed labels have been attached. Furthermore, since there is a need to display a large amount of management information, barcodes have their limitations and QR codes are increasingly being used.
[0003] These conventional methods require the introduction of dedicated equipment as a separate process after molding and increase the number of labor hours. Furthermore, whether direct printing or attaching a printed label, there are limitations to how long the marking can be maintained due to changes in the environment and depending on the ink and printed material. [Prior art documents]
[0004] [Patent Document 1] JP 2017-136666 A Summary of the Invention [Problem to be solved by the invention]
[0005] However, as shown in Patent Document 1, as a means of indicating various information such as product specifications, handling precautions, or model numbers, labels indicating various information during the assembly process are printed as barcodes and affixed to limited positions on the product. Furthermore, due to an increase in the amount of information and restrictions on the shape of the product part and the area where the QR code must be attached, affixing the label printed as the QR code becomes an additional task, resulting in increased man-hours.
[0006] The object of the present invention is to eliminate the manual work of attaching labels by directly forming a QR code cell as a collection of concave-convex micro-area cells during the molding process, which is capable of presenting a large amount of information within the limited area of the resin molded body, and to provide a resin molding mold and its manufacturing method that incorporates a QR code pattern as an uneven collection of fine area cells, which is difficult to process with ordinary injection molding molds, as an engraved block.
[0007] The cell size and number of cells (version) of the QR code format are selected based on the amount of information to be stored and the level of error correction; in version 1, which is a commonly printed method, the cell size is around 0.6 mm and the dimension between both ends of the finder pattern is 13 mm square; by making the cell size smaller, the version can be made larger, making it possible to increase the amount of information to be stored. [Means for solving the problem]
[0008] In order to achieve the above object, the resin molding mold of the present invention provides a manufacturing method for a resin molding concave mold in which an engraved block is formed, the manufacturing method including a surface treatment step of coating the surface of a metal powder with a predetermined particle size with a coupling agent, a step of mixing and solidifying a thermosetting resin and the surface-treated metal powder, followed by crushing and classifying the resulting metal-resin composite powder, a step of using a three-dimensional modeling device to create a convex mold in the shape of a resin molded product onto which a QR code pattern based on three-dimensional data is transferred, and a step of feeding the metal-resin composite powder into the upper space of the convex mold placed on the lower punch in a die, heating it to a B-stage temperature at which the resin component is in a plastic state, and compression molding it together with the upper punch to form a three-dimensional QR code as an uneven collection of fine area cells, which is then cooled and solidified in the mold, and after demolding, hardened in an atmosphere at the hardening temperature of the thermosetting resin.
[0009] The 3D modeling equipment used in the convex processing to form the 3D QR code cell, which is modeled as an assembly of micro-area cell-sized concaves and convexes, uses a method in which photocurable resin is photocured and layered, or a method in which molten resin is layered and cooled to form the molded product shape.
[0010] The resin molding concave mold is made using the convex mold that forms the QR code cell created by the 3D modeling device. In order to ensure strength and thermal conductivity during resin molding, the concave mold for resin molding uses a metal-resin composite powder obtained through a surface treatment process in which the surface of metal powder with a specified particle size is coated with a coupling agent, and a process in which the thermosetting resin that has the property of finally becoming in a hardened state after passing through the B stage (semi-hardened state) and the surface-treated metal powder are compositely solidified and then crushed and classified.
[0011] The metal powder may contain one or more metals selected from iron, aluminum, tungsten, stainless steel, titanium, zinc, tin, copper, lead, magnesium, chromium, cobalt, nickel, zirconium, molybdenum, silver, neodymium, platinum, gold, and samarium. The above metals are granulated by reduction, electrolysis, atomization, or other methods depending on the intended use, and coarse and fine powders of a certain particle size are removed to achieve a specified particle size distribution. The maximum particle size is generally controlled to be 105 to 212 μm.
[0012] In order to improve the bonding strength of the thermosetting metal compact, the metal powder of the present invention is classified to remove coarse powder with a particle size of 100 μm or more, preferably 63 μm or more, and is surface-treated with a surface treatment agent having multiple different reactive groups in its molecule to improve the bonding strength with the thermosetting resin that is mixed to form the thermosetting metal compact.
[0013] The surface-treated metal powder is given high fluidity during molding, and in order to increase shape reproducibility and solidification after molding, resulting in a high-density structure, a resin component consisting of epoxy resin or polyester resin as the main component, amine-based or isocyanate-based hardeners, and additives is added and mixed at a ratio of 20 wt% or less, and the kneaded composite material in a paste state plasticized at a certain heating temperature is crushed and classified to produce a metal-resin composite powder.
[0014] Alternatively, surface-treated metal powder is mixed with epoxy resin or polyester resin as the main component, and an amine or isocyanate curing agent and additives are added to a solvent such as methyl ethyl ketone, which vaporizes at a low temperature of around 100°C, and the mixture is homogeneously mixed to obtain a slurry. The slurry is then flattened using a doctor blade or similar wet mixing method, and the solvent is removed by vaporization to obtain a plate-shaped solidified material, which is then crushed and classified to produce a metal-resin composite powder.
[0015] The obtained metal-resin composite powder is poured into a convex mold in which a three-dimensional QR code cell made of a collection of micro-area cell-sized protrusions and recesses has been created using a three-dimensional modeling device set in a space formed by a lower punch and die, and then low-pressure molding is performed using the upper and lower punches at or above the B-stage temperature, after which it is cooled.
[0016] The equipment used for pressure molding is equipped with a mechanism for controlling the heating and cooling of the mold. A mold containing metal-resin composite powder is installed, and the mechanism controls the temperature range above and below the heat distortion temperature at which the thermosetting resin enters a plastic state (B-stage region), applying pressure at the upper limit and cooling at the lower limit, allowing the solidified molded body to be released from the mold. After pressure molding, the concave mold of the resin molded product is cooled to a temperature at which it can be released from the compression molding die and then removed. It is also effective to provide a mechanism that allows forced cooling in addition to natural cooling.
[0017] The upper limit temperature for pressure molding is desirably 10°C above the heat distortion temperature and 30°C below the curing start temperature, and the lower limit temperature for demolding is desirably 20°C below the heat distortion temperature, and these are determined based on the shape and dimensions of the molded product to be formed in the mold and productivity.
[0018] In the compression molding process used in general powder metallurgy, in order to increase the final sintering strength, the usual rate is 5 to 9 ton / cm for iron-based materials. 2 However, the strength after molding is very low, and there is a limit to the molding of fine uneven shapes, whereas the process of the present invention requires a high pressure of 2 to 3 tons / cm 2 The strength after molding is high, and there is no need to use a large press or worry about damage to the mold.
[0019] During hot compression molding, the thermosetting resin first flows and fills the spaces between the metal particles in the mold in a fluid state, and then becomes a binder between the metal particles as it is cooled from the pressurized temperature range.The resin is then released from the compression molding mold as a solidified molded product that maintains its molded shape. After compression molding, the thermosetting resin is first cooled from its fluid state temperature and solidified, becoming a bonding material between the metal particles. It is then released from the compression molding die while maintaining its molded shape, and in the next step it is hardened at around 200°C to complete the concave mold.
[0020] The resulting concave mold is pressurized in a plasticized state, faithfully reproducing the three-dimensional shape of the QR code formed with fine area cells, and the resin molded product obtained using the concave mold has a surface condition with three-dimensional QR code cells that cannot be obtained with ordinary metal molds, making it an effective technology for processing ultra-fine patterns and shapes onto the surface of ordinary resin molding molds.
[0021] In general powder metallurgy molded products, sintering is carried out with a temperature profile ranging from 500°C to 1200°C for approximately 4 to 6 hours in order to chemically bond after molding depending on the metal composition, but in the present invention, the solidified molded product is removed from the mold in a solidified state where the resin component functions as an adhesive, and is then left to rest in a constant temperature bath heated to a hardening temperature of around 200°C for approximately 10 to 30 minutes.After the resin component has completely hardened, the product is removed from the bath and cooled, and a hardened concave molded product is obtained for the purpose of forming a QR code into the resin molded product.
[0022] The thermostatic bath used in the hardening process of the present invention can be a batch-type general-purpose drying device or the like, into which the molded bodies are all charged at once. This allows for a significant reduction in the equipment cost, installation area, and energy input compared to conventional powder metallurgy molding, and also eliminates the need for temperature profile setting and atmosphere control in the sintering furnace.
[0023] In the present invention, the metal powder with a specified particle size is coated with a coupling agent for surface treatment, and the thermosetting resin is combined with the metal composite resin powder obtained in the process of compounding with the thermosetting resin. The thermosetting resin is plasticized at a temperature range of about 60 to 130°C together with a convex mold for forming a QR code cell created by a three-dimensional modeling device, and in the B-stage state, it is compressed in a compression molding die at a rate of 2 to 3 tons / cm2 per square centimeter. 2 The resin is pressed at 100°C, and the hardening resin is cooled and solidified to maintain its shape, after which the mold is released. Finally, a hardening process is carried out at 160-220°C for 10-30 minutes to obtain a resin molding die that can form a 3D QR code cell directly on the surface of the molded product during molding.
[0024] The resin molding concave mold after the curing reaction, in which the resulting three-dimensional QR code cell made of a collection of concave and convex portions with fine cell area size is formed, has sufficient strength to withstand the transfer and demolding processes with the convex mold obtained with the 3D additive manufacturing device due to the curable resin used as a binder between the metal powder particles, and is strong enough to withstand the molding pressure and temperature when used as a resin molding die after the curing process, and also has properties that are effective for temperature control.
[0025] QR codes are difficult to process using molds assembled by cutting and machining blocks of metal used in ordinary resin molding. As such, it is impossible to mold them three-dimensionally as a collection of minute dots. This is impossible unless the dot dimensions are enlarged, and if a concave mold is directly created using three-dimensional modeling, the thermal conductivity and mechanical strength will be significantly inferior to those of molds assembled by cutting and machining blocks of metal, making it impractical. Effect of the Invention
[0026] In the present invention, metal powder is combined with curable resin particles that go through the B stage and ultimately become a thermosetting molded product, and then, via a convex object obtained by three-dimensional modeling, a heat compression molding device equipped with heating and cooling mechanisms before and after the B stage, and a thermostatic bath are used to form a resin molding die in which a QR code, which is an aggregate of fine cells, is transferred as concave and convex parts.This makes it possible to directly mold a three-dimensional QR code onto the surface of the resin molding product, and further makes it possible to provide resin molding dies that can produce ultra-fine patterns and shaped molded products on the surface of general resin molding dies, at significantly reduced cost and in a short period of time. Furthermore, this technology can be easily used not only to create three-dimensional QR code cells using a collection of micro-area cell-sized projections and recesses, but also to create embossed molds with special patterns applied to the surface of resin molds. [Brief description of the drawings]
[0027] [Figure 1] 1 is a process diagram illustrating a method for producing a metal-resin composite powder according to an embodiment of the present invention. [Diagram 2] This is a manufacturing process diagram of a resin molding concave mold using a QR code convex mold made by three-dimensional modeling technology based on CAD data according to an embodiment of the present invention. [Diagram 3] 1 is a photograph of an example of a convex mold including a three-dimensional QR code formed by a three-dimensional modeling technique based on CAD data according to an embodiment of the present invention. [Figure 4] 1 is a photograph of an example of a resin molded concave mold to which a QR code has been transferred, the concave mold being obtained by molding and curing the metal resin composite powder according to an embodiment of the present invention through a convex mold containing a QR code. [Diagram 5] 1 is a photograph of an example of a resin molded product that is injection molded using a concave mold including a QR code for resin molding according to an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0028] Hereinafter, the present embodiment will be described with reference to the drawings, in which: Fig. 1 is a process diagram of a method for producing a metal-resin composite powder according to the present embodiment. First, in order to make the metal powder suitable for molding into a fine shape, coarse particles are removed using a sieve or the like to obtain a specified particle size. The surface of the metal powder is then coated with a coupling agent in order to enhance the bond with the resin to be compounded. The two components, the surface-treated metal powder and the thermosetting resin, are then compounded, and the resulting mixture is crushed and classified to produce the metal-resin composite powder used in the process shown in Figure 2.
[0029] FIG. 2 provides a method for manufacturing a resin molding concave die in which an engraving block is formed by a process in which a convex die onto which a QR code pattern is transferred based on three-dimensional data is created using a three-dimensional modeling device, the metal-resin composite powder obtained in FIG. 1 is poured into the space above the convex die placed on the lower punch in a die, and the powder is heated up to a B-stage temperature at which the resin component reaches a plastic state and compressed together with the upper punch to form a three-dimensional QR code as an uneven collection of fine area cells, which is then cooled and solidified within the die, and after demolding, is hardened in an atmosphere at the hardening temperature of the thermosetting resin to obtain an engraving block.
[0030] FIG. 3 is a photograph of an example of a convex mold including a three-dimensional QR code portion formed by a three-dimensional modeling technique based on the metal-resin composite powder obtained through the process shown in FIG. 1 of the present invention and the 3D CAD data shown in FIG. 2.
[0031] Figure 4 is a photograph showing an example of a resin molding concave mold obtained by heating a three-dimensional QR code convex mold created by three-dimensional modeling technology based on the 3D CAD data shown in Figure 2 to the B-stage temperature at which the resin component becomes plastic and compressing it together with the upper punch using a metal-resin composite powder, cooling and solidifying it, releasing it from the mold, and then curing it in an atmosphere at the curing temperature of the thermosetting resin.
[0032] FIG. 5 is a photograph of an example of a resin molded body injection-molded by mounting the resin molding concave mold shown in FIG. 4 on an injection molding machine.
[0033] (Major Effects Obtained by the Present Embodiment) In this embodiment, a metal resin composite powder is produced, in which coarse powders larger than a specified particle size have been removed, and the powder is surface-treated with a coupling agent having two or more different reactive groups in its molecule, and a thermosetting resin is used as a binder that plasticizes in a specific temperature range (B stage) to increase the fluidity of the metal powder. The powder is then shaped using a three-dimensional modeling device and introduced into a convex mold space attached to a compression molding device. After heat and pressure molding, a curing process is performed to obtain a three-dimensional QR code cell and a concave mold of the cell pattern, and the three-dimensional QR code cell can be directly formed on the surface of the resin molded product, without the need for special equipment or high energy.
[0034] The surface-treated metal powder is compounded in advance by methods such as paste mixing in a plasticized state of B-stage thermosetting resin or wet mixing sheet formation using a solvent, and then crushed and the resulting powder with the coarse particles removed is put into the compression molding process.The high fluidity during molding transfers the fine unevenness inside the mold, and the mold has ample strength when released from the mold.After final heat curing, a resin molding mold is obtained that has sufficient strength as an injection molding mold and thermal conductivity roughly equivalent to that of a normal metal mold.
[0035] The pressure required for compression molding of the composite thermosetting resin with metal powder in the plasticized temperature range is 2 to 3 tons / cm. 2 In contrast, in conventional powder metallurgy manufacturing, a large amount of lubricant is added and pressures of 5 to 7 tons / cm are required. 2 However, applying even greater pressure is limited due to the strength of the mold and equipment. The strength of the unsintered part after molding is insufficient to form objects with fine areas, such as 3D QR codes, which are an assembly of concave and convex micro-area cells, and it is not possible to release the molded object while maintaining the molded shape.
[0036] In addition, in this embodiment, the heating temperature during compression molding can be in the range of 60 to 130°C depending on the plasticization temperature of the thermosetting polymer, and the final hardening temperature after molding and cooling is 160 to 220°C. It is sufficient to leave it to stand for about 10 to 30 minutes. In this embodiment, small equipment such as a normal dryer can be used, and energy costs can be significantly reduced compared to powder metallurgy processes in which large-scale sintering furnaces are indispensable, which greatly contributes to decarbonization. Furthermore, the sintering shrinkage is smaller than that in powder metallurgy, and dimensional accuracy can be improved.
[0037] Furthermore, in this embodiment, the convex mold on which the three-dimensional QR code is formed, which is a concave-convex aggregate of fine area cells obtained by three-dimensional additive manufacturing, can be designed and manufactured in just one or two days. Furthermore, the concave mold obtained using this through powder molding and hardening processes can be manufactured in a similar number of days, and the resin molding die attached to the die base as a nest can be provided at low cost in a significantly shorter period of time.
[0038] (Other forms) The manufacturing method of the resin molding die of the present embodiment described above is one example of a preferred form of the present invention, but it is not limited to this and various modifications are possible within the scope that does not change the gist of the present invention.
[0039] In order to improve the bonding strength with the thermosetting resin to form a thermosetting molded body, it is possible to use a titanate-based, silane-based, graphene oxide, or other surface treatment agent for the metal powder.
[0040] The thermosetting resin having a B stage to be added to the metal powder desirably has a plasticization temperature of about 90°C and a hardening temperature of about 200°C.
[0041] In this embodiment, the metal-resin composite powder obtained by crushing and classifying after dry mixing or wet mixing is put into the upper space of the convex mold on which the three-dimensional QR code is formed, which is installed on the lower punch in the die, and compressed. The pressure during compression molding is 2 to 3 tons / cm. 2However, depending on the combination of metal powder and added thermosetting particles, the compression pressure can reach 2 tons / cm. 2 It may be less than 3 tons / cm 2 It is okay to exceed that.
[0042] In this embodiment, the plasticization temperature is about 100° C., and the curing temperature is about 200° C. However, depending on the combination of the metal powder and the added thermosetting resin, the temperature during compression molding in the B stage is preferably in the range of 10° C. or more higher than the heat distortion temperature, and 30° C. lower than the curing temperature, and the curing time during which the material is left to stand in a thermostatic chamber set at the curing temperature is 10 to 30 minutes.
[0043] Furthermore, the concave mold in which the three-dimensional QR code is formed can be modularized and used as a nesting piece to be attached to a part of a general resin molding die manufactured by machining a block of metal, and this embodiment can be applied to molding methods other than injection molding, such as vacuum molding and blow molding. EXAMPLES
[0044] The metal powder used is iron-based particles (Höganäs Somaloy: ASC100.29), which are commonly used in powder metallurgy and produced by the atomization method. The present invention contains a large amount of coarse powder, but it is possible to refine it during the metal powder production process. TIFF2024169252000002.tif23148
[0045] The surface treatment of the metal powder used to form the three-dimensional QR code cell and cell pattern, which are shaped as an uneven aggregate with fine cell size and have improved bonding with the thermosetting resin, is carried out by feeding iron powder, from which coarse particles of 63 μm or more have been removed, into a stirring mixer, dropping a coupling agent diluted with alcohol into the mixed state, and evaporating the alcohol with the shear heat generated during mixing to perform the surface treatment. The coupling treatment was carried out under the conditions of putting 6,500 g of iron powder into a Henschel mixer, and dropping a treatment solution prepared by dissolving 12.5 g of Ajinomoto Co.'s Plenact 46B, a titanate-based material, in 62.5 g of ethanol into the mixer at a low speed. In order to evaporate the alcohol with the help of shear heat and heating from the mixing equipment, the mixture was mixed by rotation at 130°C for 45 minutes, then cooled to 40°C using the equipment's cooling device before being discharged and collected.
[0046] The thermosetting resin is E-150BK14S, a Towa Gosei product made of epoxy- and amine-based hardeners, heated above its softening point on a hot plate to form a paste. The titanate-surface-treated iron powder is added in portions until the desired ratio is reached, and the mixture is mixed and kneaded before cooling. The kneading temperature was 130°C, 40°C higher than the softening point of the thermosetting resin E-150BK14S, which is 90°C, and the ratio of thermosetting resin added was 8 parts by weight per 100 parts by weight of iron powder.
[0047] In order to increase the bonding strength between the iron powder and thermosetting resin, they were compounded by mixing and kneading in a paste state. After cooling, they were crushed at room temperature using a grinding device to create three-dimensional QR code cells and cell patterns shaped as an uneven aggregate of fine cell size, and coarse powder was removed using a 63 μm sieve to obtain a particle size equivalent to that of the original iron powder.
[0048] On the other hand, in order to create the three-dimensional QR code cell shaped as an uneven aggregate of minute cell size and the cell pattern as well as the embossing that assumes a fine pattern, three-dimensional CAD data of the molded body shape was created. Based on the obtained CAD data, a three-dimensional modeling device was used to create a convex mold to which the QR code pattern and multiple fine patterns were transferred based on the three-dimensional data. The 3D modeling device used was the fomlabs-Form3, and the material used was Rigid 10K Resin with a layer pitch of 0.025 mm. The photograph shown in Figure 3 is a convex mold containing a three-dimensional QR code created using three-dimensional modeling technology.
[0049] Metal-resin composite powder is placed in the upper space of the convex mold placed on the lower punch in the die, and the temperature is raised to 140°C, the B-stage temperature range where the resin component becomes plastic, and then 2.5 tons / cm 2 After cooling and lowering the temperature in the mold, the mixture was released from the mold and left to stand in a thermostatic chamber at 200°C for 20 minutes to prepare a completely hardened concave mold for resin molding. A thermostatic bath is a common type of equipment, and is simpler than the sintering furnaces used in powder metallurgy processes, and requires significantly less heat energy. The photograph shown in Figure 4 shows a convex mold in which a three-dimensional QR code and the like are formed, and a concave mold for resin molding obtained using metal-resin composite powder.
[0050] The obtained concave mold was machined with ejector pin guide holes to allow the mold to be opened after injection molding and the resin molded body to be removed. The mold was then mounted as a nest in the resin molding mold base and attached to the BabyPlast 6t / 12 molding machine to carry out the molding process. ABS pellets were used as the molding resin, and the cooling time was 20 seconds. The obtained resin molding is shown in FIG.
[0051] We confirmed that the information written on the 3D QR code shown in Figure 5 can be read using a smartphone QR code reader.
Claims
1. A resin molding die incorporating a three-dimensional QR code cell formed as a collection of micro-area cell-sized irregularities on the surface of a resin molded body, and an engraving block corresponding to the formed portion of the cell pattern, and a method for manufacturing the same.
2. The resin molding die and its manufacturing method described in claim 1, wherein a convex mold having an engraving block surface shape of the same pattern as the QR code cell pattern is created using three-dimensional modeling equipment, and a concave mold to which the obtained convex mold is transferred is manufactured using a process of compression molding and hardening a metal-resin composite powder.
3. 2. A resin molding die and a method for manufacturing the same according to claim 1, comprising: a surface treatment step of coating the surface of a metal powder having a predetermined particle size with a coupling agent; and a step of mixing and solidifying a plasticized thermosetting resin and the surface-treated metal powder, followed by crushing and classifying the resulting metal-resin composite powder, which is charged into a convex die, heated to a B-stage temperature at which the resin component is in a plastic state, and compression-molded, followed by cooling and solidification within the die, and after demolding, curing in an atmosphere at the curing temperature of the thermosetting resin.
Citation Information
Patent Citations
Power tool